Copper alloy and component for electronic / electric devices
The Cu-Fe-P based copper alloy addresses the lack of anisotropy study in conventional alloys by optimizing composition and microstructure, enhancing longitudinal electrical conductivity and maintaining strength and thermal performance for electronic and electrical equipment.
Patent Information
- Application Number
- PCT/JP2024/011866
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional Cu-Fe-P alloys used in electronic and electrical equipment parts lack sufficient study on conductive anisotropy, particularly in electrical conductivity, which is crucial for applications where electric current flows in specific directions, such as bus bars.
A Cu-Fe-P based copper alloy with specific compositions and microstructural control, including Fe, P, Zn, Sn, and optional Mg, Co, Ni, Al, and Si, is developed to enhance electrical conductivity in the longitudinal direction while minimizing anisotropy and surface defects, by adjusting precipitate particle morphology and size.
The alloy achieves improved electrical conductivity in the longitudinal direction with a conductivity ratio greater than 100.1% and less than 105.0%, maintaining excellent strength and thermal conductivity, suitable for high-temperature and specific directional current applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Copper alloys and parts for electronic and electrical equipment
[0001] The present invention relates to a copper alloy suitable for electrical and electronic equipment components such as semiconductor components such as home appliances and lead frames, printed wiring boards, heat sinks, switch components, bus bars, and connectors, and to electrical and electronic equipment components made of this copper alloy. This application claims priority based on Japanese Patent Application No. 2023-053123, filed on March 29, 2023, the contents of which are incorporated herein by reference.
[0002] Conventionally, copper or copper alloys with excellent electrical conductivity have been used for electronic and electrical equipment components such as terminals, bus bars, lead frames, and heat dissipation members. Cu—Fe—P alloys containing Fe and P have been widely used as copper alloys for the various applications described above. Cu—Fe—P alloys are precipitation-strengthened alloys in which intermetallic compounds such as Fe or Fe—P are precipitated in a copper matrix. Due to their excellent strength, electrical conductivity, and thermal conductivity, they are widely used in a variety of applications. In recent years, with the expansion of applications for Cu—Fe—P alloys and the trend toward lighter, thinner, and smaller electrical and electronic devices, even higher strength, electrical conductivity, and good thermal conductivity are required for Cu—Fe—P alloys. For example, Patent Document 1 proposes a Cu—Fe—P alloy in which the crystal grains of the Cu matrix are equiaxed in order to reduce the anisotropy of mechanical properties.
[0003] Japanese Patent Application Publication No. 2013-057116 (A)
[0004] For example, electrical conductivity in the longitudinal direction is particularly required for applications such as bus bars in electrical and electronic equipment components where current flows in a specific direction. However, no conventional Cu-Fe-P alloys have been proposed in which the anisotropy of electrical conductivity has been fully considered. While Patent Document 1 examines the anisotropy of properties, it aims to reduce the anisotropy of mechanical properties, and does not pay attention to electrical conductivity.
[0005] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a Cu-Fe-P based copper alloy having superior electrical conductivity in a direction parallel to the longitudinal direction to that in a direction perpendicular to the longitudinal direction, and an electronic / electrical device component made of this copper alloy.
[0006] In order to solve the above problems, a copper alloy according to a first aspect of the present invention contains Fe; 1.5% by mass or more and 2.7% by mass or less, P; 0.008% by mass or more and 0.20% by mass or less, Zn; 0.01% by mass or more and 0.5% by mass or less, Sn; 0.01% by mass or more and 0.5% by mass or less, with the balance being Cu and inevitable impurities, and has a composition in which the electrical conductivity σ measured in a direction parallel to the longitudinal direction is P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ O is more than 100.1% and not more than 105.0%, and the particle diameter observed in the cross section including the longitudinal direction is 150 nm or more and less than 1000 nm, the particle length L in the direction perpendicular to the longitudinal direction is O and the particle length L in the direction parallel to the longitudinal direction P Relative to L O / L P The average value of is 0.8 or less.
[0007] According to the copper alloy of aspect 1 of the present invention, the copper alloy contains 1.5 mass% or more and 2.7 mass% or less of Fe, 0.008 mass% or more and 0.20 mass% or less of P, 0.01 mass% or more and 0.5 mass% or less of Zn, and 0.01 mass% or more and 0.5 mass% or less of Sn, with the balance being Cu and inevitable impurities. Therefore, the copper alloy has excellent strength and electrical conductivity, and can have good thermal conductivity.
[0008] In the copper alloy of the first embodiment of the present invention, the electrical conductivity σ measured in a direction parallel to the longitudinal direction P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ OSince the σ is greater than 100.1% and less than 105.0%, the material has good electrical conductivity, especially for applications where current flows in the longitudinal direction. Furthermore, the precipitate particles act as an obstacle to electrons flowing through the matrix, causing electrical resistance. Therefore, the particle length L of the precipitate particles in the direction perpendicular to the longitudinal direction O and the particle length L in the direction parallel to the longitudinal direction P When the particle length L is different from the particle length L, the conductivity becomes anisotropic. Therefore, the conductivity in the longitudinal direction can be improved by controlling the morphology of the precipitates. O and the particle length L in the direction parallel to the longitudinal direction P Relative to L O / L P To obtain small precipitates, coarse precipitates are necessary, and such coarse precipitates may cause surface defects. Furthermore, small precipitates are often spherical, and have little effect on anisotropy.
[0009] Therefore, in the copper alloy of the first embodiment of the present invention, the particle length L in the direction perpendicular to the longitudinal direction is measured for precipitate particles having an observed particle diameter of 150 nm or more and less than 1000 nm. O and the particle length L in the direction parallel to the longitudinal direction P Relative to L O / L P The average value of σ is 0.8 or less, which enables improvement of electrical conductivity in the longitudinal direction and suppression of surface defects. Note that the grain size of the precipitate particles in the present invention is the diameter of a circle (equivalent circle diameter) having an area equal to the area of the precipitate particle in microstructural observation, and the lengths of the precipitate particles in the directions parallel to the longitudinal direction and perpendicular to the longitudinal direction are the lengths of the precipitate particles measured in these directions.
[0010] The copper alloy of the second aspect of the present invention is the copper alloy of the first aspect of the present invention, wherein the electrical resistance ratio R measured in a direction parallel to the longitudinal direction is P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O The ratio R P / R O is more than 100.1% and not more than 105.0%.
[0011] According to the copper alloy of the second aspect of the present invention, the electrical resistance ratio R measured in a direction parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O R P / R O The electrical resistivity ratio (R) is calculated by measuring the electrical resistivity at 293 K (ρ293 K) and the electrical resistivity at liquid nitrogen temperature (77 K) (ρ77 K) as follows: R = ρ293 K / ρ77 K.
[0012] The copper alloy of Aspect 3 of the present invention is characterized in that, in the copper alloy of Aspect 1 or Aspect 2 of the present invention, it further contains one or two of Mg; 0.005% by mass or more and 0.5% by mass or less, and Co; 0.005% by mass or more and 0.5% by mass or less.
[0013] According to the copper alloy of Aspect 3 of the present invention, the copper alloy further contains one or two of Mg; 0.005% by mass or more and 0.5% by mass or less, and Co; 0.005% by mass or more and 0.5% by mass or less. Therefore, Mg and Co are solid-solved in the matrix and a portion thereof is solid-solved in the Fe-based and Fe—P-based precipitates, and the heat resistance and strength can be improved by solid-solution strengthening and a portion thereof is precipitation strengthening.
[0014] The copper alloy of Aspect 4 of the present invention is characterized in that, in the copper alloy of any one of Aspects 1 to 3 of the present invention, it further contains one or more of Ni; 0.005% by mass or more and 0.5% by mass or less, Al; 0.005% by mass or more and 0.5% by mass or less, and Si; 0.005% by mass or more and 0.5% by mass or less.
[0015] According to the copper alloy of Aspect 4 of the present invention, the copper alloy further contains one or more of Ni; 0.005% by mass or more and 0.5% by mass or less, Al; 0.005% by mass or more and 0.5% by mass or less, and Si; 0.005% by mass or more and 0.5% by mass or less, thereby making it possible to further improve the heat resistance and strength.
[0016] A copper alloy according to aspect 5 of the present invention is characterized in that the electrical conductivity in a direction parallel to the longitudinal direction is 55% IACS or more in any one of the copper alloys according to aspects 1 to 4 of the present invention. Since the copper alloy according to aspect 5 of the present invention has an electrical conductivity of 55% IACS or more in a direction parallel to the longitudinal direction, it can be used in applications requiring high electrical conductivity.
[0017] A copper alloy of Aspect 6 of the present invention is the copper alloy of any one of Aspects 1 to 5 of the present invention, characterized in that the content of C contained as the inevitable impurities is less than 5 ppm by mass, the content of Cr is less than 7 ppm by mass, the content of Mo is less than 5 ppm by mass, the content of W is less than 1 ppm by mass, the content of V is less than 1 ppm by mass, and the content of Nb is less than 1 ppm by mass.
[0018] According to the copper alloy of Aspect 6 of the present invention, the content of elements that have the effect of promoting liquid phase separation during melting and casting is reduced, so that it is possible to suppress the generation of coarse Fe-based crystals in the ingot and reduce the number of generated surface defects.
[0019] A component for electronic / electrical equipment according to Aspect 7 of the present invention is characterized in that it is made of the copper alloy according to any one of Aspects 1 to 6 of the present invention. According to the component for electronic / electrical equipment according to Aspect 7 of the present invention, since it is made of the copper alloy according to any one of Aspects 1 to 6 of the present invention, it can exhibit excellent properties even in a high-temperature environment.
[0020] It is possible to provide a Cu--Fe--P based copper alloy having better electrical conductivity in a direction parallel to the longitudinal direction than in a direction perpendicular to the longitudinal direction, and electronic / electrical equipment parts made of this copper alloy.
[0021] 1 is a photograph showing an example of precipitate particles in the copper alloy of the present embodiment. 2 is a flow chart showing a method for producing the copper alloy of the present embodiment.
[0022] A copper alloy according to one embodiment of the present invention will be described below. The copper alloy according to this embodiment contains 1.5% by mass to 2.7% by mass of Fe, 0.008% by mass to 0.20% by mass of P, 0.01% by mass to 0.5% by mass of Zn, and 0.01% by mass to 0.5% by mass of Sn, with the balance being Cu and inevitable impurities.
[0023] The copper alloy of this embodiment may further contain one or two of: Mg; 0.005% by mass to 0.5% by mass; Co; 0.005% by mass to 0.5% by mass. The copper alloy of this embodiment may further contain one or two or more of: Ni; 0.005% by mass to 0.5% by mass; Al; 0.005% by mass to 0.5% by mass; and Si; 0.005% by mass to 0.5% by mass.
[0024] Furthermore, in the copper alloy of the present embodiment, it is preferable that the content of C contained as the inevitable impurities is less than 5 ppm by mass, the content of Cr is less than 7 ppm by mass, the content of Mo is less than 5 ppm by mass, the content of W is less than 1 ppm by mass, the content of V is less than 1 ppm by mass, and the content of Nb is less than 1 ppm by mass.
[0025] In the copper alloy of this embodiment, the conductivity σ measured in a direction parallel to the longitudinal direction is P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ O In the copper alloy of this embodiment, as shown in FIG. 1, the particle length in the direction perpendicular to the longitudinal direction (particle diameter in the direction perpendicular to the longitudinal direction) L is measured for precipitate particles 12 having a particle diameter of 150 nm or more and less than 1000 nm when observed in a cross section including the longitudinal direction. O and the particle length in the direction parallel to the longitudinal direction (particle diameter in the longitudinal direction) L P Relative to L O / L P The average value is set to be 0.8 or less.
[0026] That is, in the copper alloy of this embodiment, as shown in FIG. 1 , precipitate particles 12 such as Fe and Fe—P are dispersed in a matrix phase 11, and the particle diameter of these precipitate particles 12 is specified as described above. The matrix phase 11 refers to a phase other than the precipitate particles 12 such as Fe and Fe—P, and is a phase containing Cu as the main component (Cu content exceeding 97% by mass) with some Fe, Zn, P, Sn, etc., in solid solution. Small precipitates with a particle diameter of less than 150 nm are often spherical and have little effect on anisotropy, so they were excluded. Furthermore, precipitate particles 12 with a particle diameter of 1000 nm or more were excluded because they may cause surface defects. The particle diameter of the precipitate particles 12 in this embodiment is the diameter (circle equivalent diameter) of a circle having an area equal to the area of the precipitate particles 12 in microstructural observation, and is the diameter of the particle length L in the direction perpendicular to the longitudinal direction. O , and the particle length L in the direction parallel to the longitudinal direction P are the lengths of the precipitate grains 12 measured in those directions.
[0027] Here, in the copper alloy of this embodiment, the electrical conductivity in the direction parallel to the longitudinal direction is preferably 55% IACS or more. Also, in the copper alloy of this embodiment, the strength is preferably 480 MPa or more. Furthermore, in the copper alloy of this embodiment, the Vickers hardness is preferably 100 HV or more.
[0028] The reasons for specifying the component composition, various properties, and crystalline structure of the copper alloy of this embodiment as described above will be explained below.
[0029] (Fe) Fe dissolves in the matrix 11 and generates Fe or Fe—P precipitate particles 12. The dispersion of these Fe or Fe—P precipitate particles 12 in the matrix 11 improves strength, hardness, and heat resistance without reducing electrical conductivity. If the Fe content is less than 1.5% by mass, the strength improvement effect is insufficient. On the other hand, if the Fe content exceeds 2.7% by mass, large crystals may form, impairing surface cleanliness. Furthermore, this may result in reduced electrical conductivity and workability. Therefore, in this embodiment, the Fe content is set to 1.5% by mass or more and 2.7% by mass or less. To ensure the above-described effects, the lower limit of the Fe content is preferably 1.8% by mass or more, and more preferably 2.1% by mass or more. In order to reliably suppress the formation of large crystallized particles, the upper limit of the Fe content is preferably set to 2.6 mass % or less, and more preferably set to 2.4 mass % or less.
[0030] (P) P is an element with a deoxidizing effect. As described above, P forms Fe—P precipitate particles 12 together with Fe, improving strength, hardness, and heat resistance without reducing electrical conductivity. Here, if the P content is less than 0.008% by mass, the effect of improving strength is insufficient. On the other hand, if the P content exceeds 0.20% by mass, electrical conductivity and workability are reduced. Therefore, in this embodiment, the P content is set to 0.008% by mass or more and 0.20% by mass or less. To ensure the above-described effects, the lower limit of the P content is preferably 0.01% by mass or more, and more preferably 0.02% by mass or more. To reliably suppress the reduction in electrical conductivity and workability, the upper limit of the P content is preferably 0.19% by mass or less, more preferably 0.15% by mass or less, and particularly preferably 0.12% by mass or less.
[0031] (Zn) Zn is an element that improves solder wettability and solder weather resistance. Here, if the Zn content is less than 0.01% by mass, the effect of improving solder wettability and solder weather resistance cannot be fully achieved. On the other hand, if the Zn content exceeds 0.5% by mass, the effect saturates. Therefore, in this embodiment, the Zn content is set to 0.01% by mass or more and 0.5% by mass or less. To ensure the above-mentioned effects, the lower limit of the Zn content is preferably 0.02% by mass or more, more preferably 0.05% by mass or more, and particularly preferably 0.07% by mass or more. Furthermore, the upper limit of the Zn content is preferably 0.44% by mass or less, more preferably 0.35% by mass or less, and particularly preferably 0.20% by mass or less.
[0032] (Sn) Sn is an element that improves heat resistance and strength by dissolving in the matrix 11. Here, if the Sn content is less than 0.01 mass%, the above-described effects cannot be fully achieved. On the other hand, if the Sn content exceeds 0.5 mass%, the electrical conductivity will be significantly reduced. Therefore, in this embodiment, the Sn content is set to 0.01 mass% or more and 0.5 mass% or less. To ensure the above-described effects, the lower limit of the Sn content is preferably 0.02 mass% or more, and more preferably 0.03 mass% or more. To further suppress the reduction in electrical conductivity, the upper limit of the Sn content is preferably 0.3 mass% or less, and more preferably 0.2 mass% or less.
[0033] (Mg, Co) Mg and Co have the effect of improving heat resistance and strength by dissolving in the matrix 11 and solid-solution strengthening. Therefore, they may be added appropriately depending on the required characteristics. Here, if the Mg content is less than 0.005 mass% or the Co content is less than 0.005 mass%, the above-mentioned effects cannot be fully achieved. On the other hand, if the Mg content exceeds 0.5 mass% or the Co content exceeds 0.5 mass%, the electrical conductivity will be significantly reduced. Therefore, in this embodiment, when Mg and Co are added, it is preferable that the Mg content be 0.005 mass% or more and 0.5 mass% or less, and the Co content be 0.005 mass% or more and 0.5 mass% or less.
[0034] When Mg and Co are added, the lower limit of the Mg content is preferably 0.01 mass% or more, and the lower limit of the Co content is preferably 0.01 mass% or more. Furthermore, the lower limit of the Mg content is preferably 0.02 mass% or more, and the lower limit of the Co content is preferably 0.02 mass% or more. Furthermore, the upper limit of the Mg content is preferably 0.2 mass% or less, and the upper limit of the Co content is preferably 0.2 mass% or less. Note that when Mg and Co are contained as impurities, they may be contained in amounts less than the above-mentioned lower limits.
[0035] (Ni, Al, Si) Ni, Al, and Si have the effect of further improving heat resistance and strength. Therefore, they may be added appropriately depending on the required characteristics. Here, if the Ni content is less than 0.005 mass%, the Al content is less than 0.005 mass%, or the Si content is less than 0.005 mass%, the above-mentioned effects cannot be fully achieved. On the other hand, if the Ni content exceeds 0.5 mass%, the Al content exceeds 0.5 mass%, or the Si content exceeds 0.5 mass%, the electrical conductivity will be significantly reduced. Therefore, when Ni, Al, and Si are added in this embodiment, it is preferable that the Ni content be 0.005 mass% to 0.5 mass%, the Al content be 0.005 mass% to 0.5 mass%, and the Si content be 0.005 mass% to 0.5 mass%.
[0036] When Ni, Al, or Si is added, the lower limit of the Ni content is preferably 0.01 mass% or more, the lower limit of the Al content is preferably 0.01 mass% or more, and the lower limit of the Si content is preferably 0.01 mass% or more. Furthermore, the upper limit of the Ni content is preferably 0.1 mass% or less, the upper limit of the Al content is preferably 0.1 mass% or less, and the upper limit of the Si content is preferably 0.1 mass% or less. Note that when Ni, Al, or Si is contained as an impurity, it may be contained in an amount less than the above-mentioned lower limit.
[0037] (Inevitable impurities: C, Cr, Mo, W, V, and Nb) C, Cr, Mo, W, V, and Nb are contained in the above-mentioned copper alloy as inevitable impurities. Here, if the contents of C, Cr, Mo, W, V, and Nb are high, the surface defects of the copper alloy thin sheet will increase significantly. These surface defects are caused by iron alloy particles containing at least one of Cr, Mo, W, V, and Nb, as well as Fe and C.
[0038] Typically, when the above-mentioned copper alloy is melted and cast, the Fe element exists in a dissolved state in a liquid phase mainly composed of Cu. However, when a certain amount or more of C, Cr, Mo, W, V, and Nb is present, the molten copper alloy is separated into a liquid phase mainly composed of Cu and a liquid phase mainly composed of Fe and containing C and at least one of Cr, Mo, W, V, and Nb. As a result, coarse crystallized particles containing at least one of Cr, Mo, W, V, and Nb, Fe, and C are present in the ingot. It is believed that subsequent rolling of the ingot exposes iron alloy particles on the surface of the copper alloy thin plate, causing the above-mentioned surface defects. Furthermore, these iron alloy particles cause shape defects when press-forming, etching, or silver-plating are performed.
[0039] From the above, it is possible to suppress surface defects and defective product shapes caused by iron alloy particles by reducing the amounts of C, Cr, Mo, W, V, and Nb. Therefore, in this embodiment, in order to suppress the generation of coarse crystallized particles, it is preferable to limit the content of inevitable impurities, C to less than 5 ppm by mass, Cr to less than 7 ppm by mass, Mo to less than 5 ppm by mass, W to less than 1 ppm by mass, V to 1 ppm by mass, and Nb to less than 1 ppm by mass.
[0040] In order to further suppress the generation of coarse crystals, it is more preferable that the content of C, which is an inevitable impurity, is less than 4 ppm by mass, more preferably 3 ppm by mass or less, and even more preferably 2 ppm by mass or less. It is more preferable that the content of Mo, which is an inevitable impurity, is less than 1 ppm by mass, and even more preferably less than 0.6 ppm by mass. It is also preferable that the content of Cr, which is an inevitable impurity, is less than 5 ppm by mass, the content of W, the content of V, and the content of Nb are less than 0.6 ppm by mass.
[0041] In addition to the above elements and C, Cr, Mo, W, V, and Nb, inevitable impurities include Ca, Sr, Ba, rare earth elements, Zr, Be, Ti, H, Li, B, N, O, F, Na, S, Cl, K, Mn, Ga, Ge, As, Se, Br, Rb, Tc, Ru, Rh, Pd, Ag, Cd, In, Sb, Te, I, Cs, Hf, Ta, Re, Os, Ir, Pt, Au, Hg, Tl, Pb, and Bi. These inevitable impurities may be contained to a degree that does not affect the characteristics. Since these inevitable impurities may reduce the conductivity, the total amount is preferably 0.1% by mass or less, more preferably 0.05% by mass or less, even more preferably 0.03% by mass or less, and even more preferably 0.01% by mass or less.
[0042] (Ratio of particle length of precipitate particle) The precipitate particle 12 acts as an obstacle to the electrons flowing through the matrix 11. Therefore, the particle length L in the direction perpendicular to the longitudinal direction is Oand the particle length L in the direction parallel to the longitudinal direction P On the other hand, the particle length L in the direction perpendicular to the longitudinal direction O and the particle length L in the direction parallel to the longitudinal direction P The ratio L O / L P To obtain precipitates with small diameters, coarse precipitates are necessary, and such coarse precipitates may cause surface defects. Furthermore, small precipitates are often spherical, and have little effect on anisotropy. Therefore, in this embodiment, the particle length L in the direction perpendicular to the longitudinal direction of the precipitate particles 12 is measured for precipitate particles 12 with a particle diameter of 150 nm or more and less than 1000 nm observed in a cross section including the longitudinal direction. O and the particle length L in the direction parallel to the longitudinal direction P The ratio L O / L P In order to obtain the above-mentioned effects, the average value of the particle length ratio L of the precipitate particles 12 is set to 0.8 or less. O / L P The average value of is preferably 0.75 or less, and more preferably 0.7 or less.
[0043] (Electrical Conductivity) In the copper alloy of this embodiment, when the electrical conductivity in the direction parallel to the longitudinal direction is 55% IACS or more, it is particularly suitable as a material for electrical and electronic equipment components such as bus bars. The electrical conductivity in the direction parallel to the longitudinal direction of the copper alloy of this embodiment is preferably 57% IACS or more, and more preferably 60% IACS or more. In the copper alloy of this embodiment, the electrical conductivity σ measured in the direction parallel to the longitudinal direction is P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ O When the conductivity σ measured in the direction parallel to the longitudinal direction is more than 100.1%, the material is particularly suitable for use in electrical and electronic equipment components that pass current in a specific direction, such as bus bars. P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ OTo increase the aspect ratio, precipitates with a high aspect ratio are required, but such precipitates are coarse and may cause surface defects.
[0044] Therefore, in the copper alloy of this embodiment, the conductivity σ measured in a direction parallel to the longitudinal direction P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ O The conductivity σ measured in the direction parallel to the longitudinal direction is set to be more than 100.1% and not more than 105.0%. P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ O The lower limit of the conductivity σ measured in a direction parallel to the longitudinal direction is preferably 100.2% or more, and more preferably 100.3% or more. P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ O The upper limit of is preferably 103.0% or less, and more preferably 102.0% or less.
[0045] (Electrical Resistivity Ratio (R)) In the copper alloy of this embodiment, when the electrical resistance ratio (R), which is an index of electrical conductivity at low temperatures, measured in a direction parallel to the longitudinal direction is higher than the value measured in a direction perpendicular to the longitudinal direction, the copper alloy is particularly suitable as a material for parts for electrical and electronic devices that pass current in a specific direction, such as bus bars, even at low temperatures. That is, the electrical resistance ratio R measured in a direction parallel to the longitudinal direction is P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O The ratio R P / R O On the other hand, the electrical resistance ratio R measured in a direction parallel to the longitudinal direction is preferably set to be more than 100.1%. P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O The ratio R P / R O To increase the aspect ratio, precipitates with a high aspect ratio are required, but such precipitates are coarse and may cause surface defects.
[0046] Therefore, the electrical resistance ratio R measured in a direction parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O The ratio R P / R O It is preferable that the electrical resistance ratio R measured in a direction parallel to the longitudinal direction is more than 100.1% and not more than 105.0%. P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O The ratio R P / R O The lower limit of the electrical resistance ratio R measured in a direction parallel to the longitudinal direction is preferably 100.2% or more, and more preferably 100.3% or more. P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O The ratio R P / R O The upper limit of is preferably 103.0% or less, and more preferably 102.0% or less.
[0047] (Tensile strength) In the copper alloy of this embodiment, when the tensile strength is 400 MPa or more, the copper alloy is excellent in strength and is particularly suitable as a material for parts for electric and electronic devices such as bus bars. In this embodiment, the tensile strength when a tensile test is performed in a direction parallel to the rolling direction is set to 400 MPa or more. The tensile strength of the copper alloy of this embodiment is more preferably 415 MPa or more, and even more preferably 430 MPa or more.
[0048] (Vickers hardness) In the copper alloy of this embodiment, when the Vickers hardness is 100 HV or more, the copper alloy does not easily deform and is particularly suitable as a material for electrical and electronic equipment components such as bus bars, etc. The Vickers hardness of the copper alloy of this embodiment is preferably 110 HV or more, and more preferably 120 HV or more.
[0049] Next, an example of a method for producing the copper alloy according to this embodiment will be described with reference to the flow chart shown in FIG.
[0050] (Melting and Casting Step S01) First, the aforementioned elements are added to the molten copper obtained by melting a copper raw material to adjust the composition, thereby producing a molten copper alloy. The various elements can be added using simple elements or master alloys. Raw materials containing the aforementioned elements may also be melted together with the copper raw material. Recycled or scrap materials of this alloy may also be used. Here, the molten copper is preferably so-called 4NC Cu, which has a purity of 99.99% by mass or more, or so-called 5NC Cu, which has a purity of 99.999% by mass or more. The molten copper alloy with the adjusted composition is then poured into a mold to produce an ingot. When considering mass production, it is preferable to use a continuous casting method or a semi-continuous casting method.
[0051] (Homogenization step S02) Next, a heat treatment is performed to homogenize the obtained ingot. The ingot is preferably held at 850°C or higher and 1050°C or lower for 1 hour or longer. There is no upper limit to the holding time in the homogenization step S02, but considering costs and manufacturing efficiency, it is preferably 24 hours or shorter. There is also no particular limit to the cooling rate in the homogenization step S02, and air cooling or water cooling may be used.
[0052] (Hot working step S03) Next, hot working is performed. This hot working step may also serve as the homogenizing step S02. After holding at 850°C or higher and 1050°C or lower for at least one hour, hot working is performed at 850°C or higher and 1050°C or lower, and then water cooling is performed. In this hot working step S03, there are no particular limitations on the processing method, and for example, rolling, wire drawing, extrusion, groove rolling, forging, pressing, etc. can be used. In this embodiment, rolling processing is performed.
[0053] (Roughing Step S04) After the hot working step S03, cold roughing is performed. In this processing, the hot-worked material is immersed in liquid nitrogen for at least one minute, and processing is performed while cooling the processing tool with liquid nitrogen. The processing rate is preferably in the range of 10% to 95%. This removes heat generated by processing, and processing at an extremely low temperature suppresses recovery and recrystallization due to processing heat. This allows the precipitates to be processed at a low temperature, thereby reducing the particle length ratio of the precipitate particles 12. Note that there are no particular limitations on the processing method in this roughing step S04, and methods such as rolling, wire drawing, extrusion, groove rolling, forging, and pressing can be used. Note that in this embodiment, rolling processing is performed.
[0054] (First precipitation heat treatment step S05) Next, a heat treatment is performed at 450°C or higher and 600°C or lower, maintaining the temperature for more than 1 hour and not more than 24 hours. It is preferable to shorten the maintenance time when performing heat treatment at a high temperature, and to lengthen the maintenance time when performing heat treatment at a low temperature. This first precipitation heat treatment step S05 improves electrical conductivity. The temperature increase rate and temperature decrease rate in the first precipitation heat treatment step S05 may be set appropriately, but it is preferable to set the temperature increase rate to 1°C / min or higher and the temperature decrease rate to 300°C to 0.1°C / min or higher.
[0055] (First Cold Working Step S06) After the first precipitation heat treatment step S05, a first cold working step is performed. In this step, the first precipitation heat-treated material is immersed in liquid nitrogen for at least one minute, and the processing is performed while the processing tool is cooled with liquid nitrogen. The processing rate is preferably in the range of 10% to 95%. Furthermore, the processing rate is preferably in the range of 20% to 95%, more preferably in the range of 30% to 95%, and even more preferably in the range of 40% to 95%. By removing processing-induced heat and processing at extremely low temperatures, recovery and recrystallization due to processing heat are suppressed, allowing the precipitate to be processed at low temperatures, thereby achieving an average particle length ratio of the precipitate particles 12 of 0.8 or less. In the first cold working step S06, there are no particular limitations on the processing method; for example, rolling, wire drawing, extrusion, groove rolling, forging, pressing, etc. can be used. In this embodiment, rolling processing is performed.
[0056] (Second precipitation heat treatment step S07) Next, a heat treatment is performed at 450°C or higher and 600°C or lower, maintaining the temperature for more than 1 hour and not exceeding 24 hours. It is preferable to shorten the maintenance time when performing heat treatment at a high temperature, and to lengthen the maintenance time when performing heat treatment at a low temperature. This second precipitation heat treatment step S07 further improves the electrical conductivity. It is preferable to set the electrical conductivity of the final product to 55% IACS or higher, taking into account the conditions of subsequent processes. The temperature increase rate and temperature decrease rate in the second precipitation heat treatment step S07 may be set as appropriate, but it is preferable to set the temperature increase rate to 1°C / min or higher and the temperature decrease rate to 300°C to 0.1°C / min or higher.
[0057] (Finishing Process S08) After the second precipitation heat treatment process S07, finishing is performed. The processing rate at this time is preferably in the range of 10% to 95%. In the finishing process S08, there are no particular limitations on the processing method, and for example, rolling, wire drawing, extrusion, groove rolling, forging, pressing, etc. can be used. In this embodiment, rolling is performed.
[0058] (Strain Removal Heat Treatment Step S09) Next, as necessary, a strain removal heat treatment is performed in which the material is held at 200° C. or higher but lower than 700° C. for 1 second or longer but shorter than 24 hours in order to remove residual strain generated in the finish processing step S08. When the heat treatment is performed at a high temperature, it is preferable to shorten the holding time, and when the heat treatment is performed at a low temperature, it is preferable to lengthen the holding time.
[0059] The copper alloy of this embodiment is produced by the steps described above. In this embodiment, rolling is performed as the processing method in the finishing step S08, so that a copper alloy plate strip material having a predetermined plate thickness is produced.
[0060] The copper alloy of this embodiment having the above-described configuration contains 1.5% by mass or more and 2.7% by mass or less of Fe, 0.008% by mass or more and 0.20% by mass or less of P, 0.01% by mass or more and 0.5% by mass or less of Zn, 0.01% by mass or more and 0.5% by mass or less of Sn, and the balance being Cu and inevitable impurities. Therefore, the copper alloy has excellent strength and electrical conductivity, and also has good thermal conductivity.
[0061] The conductivity measured in the direction parallel to the longitudinal direction is σ P and the conductivity σ measured in the direction perpendicular to the longitudinal direction O Ratio σ P / σ O Since the ratio of the length of the particle to the length of the longitudinal direction is more than 100.1% and less than 105.0%, the film has good conductivity, particularly for applications in which current is passed in the longitudinal direction. O and the particle length L in the direction parallel to the longitudinal direction P Relative to L O / L P Since the average value of is 0.8 or less, it is possible to improve the electrical conductivity in the longitudinal direction.
[0062] Furthermore, in the copper alloy of this embodiment, the electrical resistance ratio R measured in a direction parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O R P / R O When the elongation ratio is more than 100.1% and not more than 105.0%, the longitudinal conductivity is excellent even at low temperatures, and therefore the material is particularly suitable as a material for parts of electronic and electrical devices used in low-temperature environments.
[0063] Furthermore, in the copper alloy of the present embodiment, when one or two of Mg; 0.005% by mass or more and 0.5% by mass or less and Co; 0.005% by mass or more and 0.5% by mass or less are further contained, it becomes possible to improve the heat resistance and strength by solid solution strengthening.
[0064] Furthermore, in the copper alloy of the present embodiment, when the copper alloy further contains one or more of Ni; 0.005% by mass or more and 0.5% by mass or less, Al; 0.005% by mass or more and 0.5% by mass or less, and Si; 0.005% by mass or more and 0.5% by mass or less, it becomes possible to further improve the heat resistance and strength.
[0065] Furthermore, in the copper alloy of the present embodiment, when the content of C contained as unavoidable impurities is less than 5 ppm by mass, the content of Cr is less than 7 ppm by mass, the content of Mo is less than 5 ppm by mass, the content of W is less than 1 ppm by mass, the content of V is less than 1 ppm by mass, and the content of Nb is less than 1 ppm by mass, elements having the effect of promoting liquid phase separation in the melting and casting step S01 are reduced, and it is possible to suppress the generation of coarse Fe-based crystals in the ingot and reduce the number of generated surface defects.
[0066] Furthermore, in the copper alloy of this embodiment, when the electrical conductivity in the direction parallel to the longitudinal direction is 55% IACS or more, it can be applied to applications requiring high electrical conductivity. Furthermore, in the copper alloy of this embodiment, when the tensile strength is 400 MPa or more, it can be applied to applications requiring high strength. Furthermore, in the copper alloy of this embodiment, when the Vickers hardness is 100 HV or more, it does not easily deform and is particularly suitable for use as parts for electrical and electronic devices.
[0067] Although the copper alloy according to the embodiment of the present invention has been described above, the present invention is not limited thereto and can be appropriately modified within the scope of the technical concept of the invention. In the above embodiment, an example of a method for manufacturing a copper alloy has been described, but the method for manufacturing a copper alloy is not limited to the one described in the embodiment and an existing manufacturing method may be appropriately selected to manufacture the copper alloy.
[0068] For example, in this embodiment, rolling is performed as a processing method to obtain a copper alloy plate strip material made of the copper alloy of the present invention, but when wire drawing, extrusion, groove rolling, etc. are performed as a processing method, a copper alloy wire rod material made of the copper alloy of the present invention can be obtained, and when forging, pressing, etc. are performed as a processing method, copper alloy members of various shapes made of the copper alloy of the present invention can be obtained.
[0069] First, in the melting and casting process, a copper raw material consisting of oxygen-free copper (ASTM B152 C10100) with a purity of 99.99% by mass or more was prepared and placed in an alumina crucible. This was then melted in a high-frequency melting furnace under an Ar gas atmosphere. To the resulting molten copper, Fe, P, Zn, Sn, Mg, Al, Si, Co, and Ni were added. These elements were added using a Cu master alloy. This resulted in a molten copper alloy with the composition shown in Table 1, which was then poured into a carbon mold to produce an ingot. The size of the ingot was approximately 25 mm thick, 70 mm wide, and 100 mm long.
[0070] Next, in the hot working step, the obtained ingot was heat treated for 4 hours at the hot rolling temperature shown in Table 2, and then hot worked at 900°C until the thickness reached 12 mm. Reheating was performed as necessary. After hot rolling, water cooling was performed. Surface grinding was performed to remove the oxide film formed on the surface after hot rolling. Next, in the rough processing step, the ingot was immersed in liquid nitrogen for 10 minutes or more, and then cold rolled to a thickness of 2 mm while cooling the rolling roll surface with liquid nitrogen.
[0071] Next, in the first precipitation heat treatment step, the sample was held for a predetermined time between 1 hour and 24 hours at the heat treatment temperature listed in Table 2 using an electric furnace, followed by air cooling, furnace cooling, or water cooling. Then, polishing was performed to remove the surface oxide film formed after the heat treatment. Next, in the first cold working step, the sample was immersed in liquid nitrogen for 10 minutes or more, and then cold rolling was performed until the thickness reached 0.7 mm while cooling the rolling roll surface with liquid nitrogen. Next, in the second precipitation heat treatment step, the sample was held for a predetermined time between 1 hour and 24 hours at the heat treatment temperature listed in Table 2 using an electric furnace. After the heat treatment, the sample was furnace cooled to 300°C, followed by air cooling or water cooling.
[0072] Then, as a finishing process, cold rolling was performed to a thickness of 0.5 mm for Inventive Examples 1 to 11 and Comparative Examples 1 and 2, and to a thickness of 0.2 mm for Inventive Examples 12 to 22, to prepare samples for evaluation and measurement. Thereafter, as shown in Table 2, some of the samples were subjected to strain relief heat treatment for 1 minute at the listed temperature using a salt bath furnace to prepare samples for evaluation and measurement.
[0073] The copper alloys of Examples 1 to 22 of the present invention and Comparative Examples 1 and 2 obtained as described above were evaluated as follows.
[0074] (Observation of Precipitate Particles) Observation of precipitate particles was carried out by the following method. The rolled surface of the sample for evaluation and measurement, i.e., the ND surface, was mechanically polished to a mirror finish, and then the surface was subjected to ion milling processing using Ar ions at an acceleration voltage of 4.0 kV using an IM-5000 manufactured by Hitachi High-Technologies Corporation. Then, observation was carried out using a field emission scanning electron microscope (SU7000 manufactured by Hitachi High-Technologies Corporation). The observation magnification was 5000 times and the field of view (approximately 450 μm 2 ) were image-processed to add contrast to only the precipitates. From the contrast-added images, the image analysis software "Win ROOF" was used to calculate the circle-equivalent diameter from the area of the precipitates. For precipitate particles with a particle diameter of 150 nm or more and less than 1000 nm, the aspect ratio was calculated from the lengths of the precipitate particle diameter in the direction perpendicular to the longitudinal direction and in the direction parallel to the longitudinal direction for each particle, and the average value of the aspect ratios for each particle was taken as the ratio of the precipitate particle lengths. Observations were performed in three or more fields of view.
[0075] (Conductivity) Test pieces measuring 10 mm wide x 350 mm long were taken from the samples for evaluation measurement, and the electrical resistance was determined by a four-terminal method. The dimensions of the test pieces were measured using a micrometer, and the volume of the test pieces was calculated. The electrical conductivity was then measured from the measured electrical resistivity and the calculated volume. The test pieces were taken so that their longitudinal directions were parallel and perpendicular to the rolling direction. The measurement results are shown in Table 3.
[0076] (Electrical Resistivity Ratio (R)) Test pieces measuring 5 mm wide x 200 mm long were taken from the samples for evaluation and measurement, and the electrical resistivity at 293 K (ρ293 K) and the electrical resistivity at liquid nitrogen temperature (77 K) (ρ77 K) were measured using the four-terminal method, and R = ρ293 K / ρ77 K was calculated. The test pieces were taken so that their longitudinal direction was parallel and perpendicular to the rolling direction. The evaluation results are shown in Table 3.
[0077] (Tensile strength) No. 13B test pieces were taken from the samples and the tensile strength was measured in accordance with JIS Z 2241. The test pieces were taken so that the tensile direction was parallel to the rolling direction. The evaluation results are shown in Table 3.
[0078] (Vickers Hardness) Vickers hardness was measured at a test load of 0.98 N in accordance with the micro Vickers hardness testing method specified in JIS Z 2244. The evaluation results are shown in Table 3.
[0079]
[0080]
[0081]
[0082] In Comparative Example 1, the first cold working step was performed at room temperature, so the average grain length ratio was large at 0.86 and the anisotropy was small.In Comparative Example 2, the rough working step was performed at room temperature, so the average grain length ratio was large at 0.88 and the anisotropy was small.
[0083] In contrast, in the examples of the present invention, it was confirmed that the electrical conductivity in the direction parallel to the longitudinal direction was superior to that in the direction perpendicular to the longitudinal direction. Furthermore, the tensile strength, electrical conductivity, and Vickers hardness were also excellent. From the above, it was confirmed that the examples of the present invention can provide a Cu—Fe—P-based copper alloy that has superior electrical conductivity in the direction parallel to the longitudinal direction to that in the direction perpendicular to the longitudinal direction.
[0084] The present invention makes it possible to provide a Cu--Fe--P based copper alloy having superior electrical conductivity in a direction parallel to the longitudinal direction to that in a direction perpendicular to the longitudinal direction.
[0085] 11 Mother phase 12 Precipitate particles L O Particle diameter in the direction perpendicular to the longitudinal axis L P Particle diameter parallel to the longitudinal axis
Claims
1. The composition is Fe; 1.5 mass% to 2.7 mass%, P; 0.008 mass% to 0.20 mass%, Zn; 0.01 mass% to 0.5 mass%, Sn; 0.01 mass% to 0.5 mass%, with the balance being Cu and unavoidable impurities, and the electrical conductivity σ measured in a direction parallel to the longitudinal direction P and the conductivity σ measured perpendicular to the longitudinal direction O Ratio to σ P / σ O is more than 100.1% and not more than 105.0%, and the particle length L in the direction perpendicular to the longitudinal direction is measured for precipitate particles having a particle diameter of 150 nm or more and less than 1000 nm observed in a cross section including the longitudinal direction. O and the particle length L in the direction parallel to the longitudinal direction P Relative to L O / L P The copper alloy is characterized in that the average value of is 0.8 or less.
2. Electrical resistance ratio R measured parallel to the longitudinal direction P and the electrical resistance ratio R measured in a direction perpendicular to the longitudinal direction O Ratio of R P / R O The copper alloy according to claim 1, characterized in that it has a C content of more than 100.1% and not more than 105.0%.
3. The copper alloy according to claim 1, further comprising one or two of Mg; 0.005% by mass or more and 0.5% by mass or less; and Co; 0.005% by mass or more and 0.5% by mass or less.
4. The copper alloy according to claim 1, further comprising one or more of the following: Ni; 0.005% by mass or more and 0.5% by mass or less; Al; 0.005% by mass or more and 0.5% by mass or less; and Si; 0.005% by mass or more and 0.5% by mass or less.
5. The copper alloy according to claim 1, characterized in that the electrical conductivity in the direction parallel to the longitudinal direction is 55% IACS or more.
6. The copper alloy according to claim 1, characterized in that the content of C contained as the unavoidable impurities is less than 5 ppm by mass, the content of Cr is less than 7 ppm by mass, the content of Mo is less than 5 ppm by mass, the content of W is less than 1 ppm by mass, the content of V is less than 1 ppm by mass, and the content of Nb is less than 1 ppm by mass.
7. A part for electronic or electrical equipment, comprising the copper alloy according to any one of claims 1 to 6.
Citation Information
Patent Citations
Copper alloy excellent in heat resistance
JP2016211053A
Copper alloy
JP2019173090A
Copper alloy
JP2019173091A