All-solid-state battery
By integrating a softer resin within the all-solid-state battery structure to mitigate crack propagation, the issue of short circuits and cycle deterioration is addressed, enhancing the battery's performance and reliability, especially when using alloy materials with large expansion and contraction.
Patent Information
- Application Number
- PCT/JP2024/012283
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
All-solid-state batteries face issues with short circuits due to cracks caused by expansion and contraction during charging and discharging, particularly when alloy materials with large expansion and contraction are used for the negative electrode, which can lead to deteriorated cycle characteristics.
Incorporating a softer resin than the solid electrolyte at specific positions within the battery structure, such as between the electrode layers and the external terminals, to prevent cracks from propagating and enhance the battery's cycle characteristics.
The use of a softer resin effectively suppresses the occurrence of short circuits and improves the cycle performance of all-solid-state batteries, even when alloy materials with significant expansion and contraction are employed, resulting in batteries with excellent reliability and longevity.
Smart Images

Figure JP2024012283_03102024_PF_FP_ABST
Abstract
Description
All solid state battery
[0001] The present invention relates to an all-solid-state battery. This application claims priority to Japanese Patent Application No. 2023-055316, filed on March 30, 2023, the contents of which are incorporated herein by reference.
[0002] In recent years, electronics technology has made remarkable advances, with efforts being made to make portable electronic devices smaller, lighter, thinner, and more multifunctional. Accordingly, there is a strong demand for batteries, which serve as the power source for electronic devices, to be smaller, lighter, thinner, and more reliable.
[0003] In commonly used lithium-ion secondary batteries, electrolytes (electrolytic solutions) such as organic solvents have traditionally been used as a medium for ion migration. However, lithium-ion secondary batteries using electrolytic solutions have the risk of electrolyte leakage. Furthermore, since organic solvents and the like used in electrolytic solutions are flammable substances, there is a demand for safer energy storage devices.
[0004] In order to improve the safety of the energy storage element, attention has been focused on all-solid-state batteries that include a solid electrolyte instead of an electrolytic solution and that also have other solid components (for example, Patent Documents 1 and 2).
[0005] The all-solid-state batteries described in Patent Documents 1 and 2 include a laminate in which positive electrode layers each including a positive electrode active material layer and a positive electrode current collector, and negative electrode layers each including a negative electrode active material layer and a negative electrode current collector are alternately stacked with a solid electrolyte layer interposed therebetween, and a pair of external electrodes that are in contact with the side surfaces of the laminate and are arranged to face each other.
[0006] In an all-solid-state battery, there is a concern that peeling of electrode layers such as a positive electrode layer and a negative electrode layer may result in a deterioration in cycle characteristics. Specifically, in an all-solid-state battery, a positive electrode current collector and a negative electrode current collector are connected to a positive electrode external terminal and a negative electrode external terminal, respectively, and there is a concern that peeling of the positive electrode current collector from the positive electrode external terminal or peeling of the negative electrode current collector from the negative electrode external terminal due to expansion and contraction during charge and discharge may result in a deterioration in cycle characteristics.
[0007] In the all-solid-state battery of Patent Document 2, in order to prevent the positive electrode current collector and the negative electrode current collector from peeling off from the external terminals, it is proposed to increase the thickness of the portions of the positive electrode current collector and the negative electrode current collector that are bonded to the external terminals, and to increase the area of the regions where the positive electrode current collector and the negative electrode current collector are bonded to the external terminals.
[0008] JP 2021-108258 A International Publication No. 2020 / 105662
[0009] However, the all-solid-state batteries disclosed in Patent Documents 1 and 2 were unable to sufficiently prevent short circuits caused by expansion and contraction of the electrode layers during charging and discharging.
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an all-solid-state battery that can suppress the occurrence of short circuits caused by cracks in the all-solid-state battery due to expansion and contraction during charge and discharge, and can obtain excellent cycle characteristics.
[0011] The inventors of the present invention have found that cracks are likely to occur in a region of an all-solid-state battery stack extending from the tip of an electrode layer toward an electrode layer of opposite polarity adjacent to the electrode layer in the stacking direction. They have also found that cracks are particularly likely to occur at the tip of the negative electrode when an alloy-based material that exhibits large expansion and contraction during charging and discharging is used for the negative electrode. Even when such an alloy-based material exhibiting large expansion and contraction during charging and discharging is used for the negative electrode, it is desirable to prevent cracks from propagating from an electrode layer to an electrode layer adjacent to the electrode layer. That is, the present inventors provide the following means to solve the above problem.
[0012] (1) An all-solid-state battery according to one aspect of the present invention includes a cathode layer, an anode layer, and a solid electrolyte layer, wherein the solid electrolyte layer is a laminate disposed between the cathode layer and the anode layer, a cathode external terminal joined to the cathode layer at a first end surface of the laminate, and a cathode external terminal joined to the anode layer at a second end surface of the laminate opposite to the first end surface, and the all-solid-state battery further includes a resin softer than the solid electrolyte layer at a position in contact with at least one of an end of the cathode layer opposite the first end surface of the cathode layer and an end of the anode layer opposite the second end surface of the anode layer.
[0013] (2) In the all-solid-state battery of (1), the resin may fill either a first region sandwiched between the positive electrode layer and the second end surface or a second region sandwiched between the negative electrode layer and the first end surface.
[0014] (3) In the all-solid-state battery of (1) or (2), the resin may be a thermoplastic resin.
[0015] (4) In the all-solid-state batteries according to (1) to (3), the resin may have a Rockwell hardness of HRR115 or less.
[0016] (5) The all-solid-state batteries according to (1) to (4) above may include the resin at a position in contact with an end of the negative electrode layer.
[0017] (6) The all-solid-state batteries according to (1) to (5) above may include the resin at a position in contact with an end of the positive electrode layer.
[0018] (7) The all-solid-state batteries according to (1) to (6) above may include the resin at both a position in contact with the end of the positive electrode layer and a position in contact with the end of the negative electrode layer.
[0019] (8) In the all-solid-state batteries described in (1) to (7) above, the negative electrode active material layer provided in the negative electrode layer may be made of AgPd or Ag.
[0020] According to the present invention, it is possible to provide an all-solid-state battery that can suppress the occurrence of cracks that propagate from an electrode layer of the all-solid-state battery to an electrode layer adjacent to the electrode layer due to expansion and contraction during charge and discharge, and that can obtain excellent cycle characteristics.
[0021] Fig. 4 is a cross-sectional view showing an example of the configuration of an all-solid-state battery according to one embodiment of the present invention. Fig. 5 is a cross-sectional view showing a cross section along the cutting line A-A in Fig. 1. Fig. 6 is a cross-sectional view according to a modified example of Fig. 2. Fig. 7 is a cross-sectional view showing the configuration of an all-solid-state battery according to a modified example of Fig. 1. Fig. 8 is a cross-sectional view showing a cross section along the cutting line B-B in Fig. 4. Fig. 9 is a cross-sectional view showing the configuration of an all-solid-state battery according to a modified example of Fig. 1.
[0022] Hereinafter, the embodiments will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may show characteristic portions enlarged for convenience in order to make the features easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate changes can be made within the scope of the effects of the present invention.
[0023] [All-Solid-State Battery] Fig. 1 is a cross-sectional view showing an example of the configuration of an all-solid-state battery according to one embodiment of the present invention, and Fig. 2 is a cross-sectional view showing a cross section along the cutting line A-A in Fig. 1. The all-solid-state battery 100A shown in Fig. 1 includes a cathode layer 1, an anode layer 2, and a solid electrolyte layer 3. The solid electrolyte layer 3 is disposed between the cathode layer 1 and the anode layer 2. The all-solid-state battery 100A also includes a laminate 50A, a cathode external terminal 5 joined to the cathode layer 1 at a first end surface S1 of the laminate 50A, and a negative electrode external terminal 4 joined to the anode layer 2 at a second end surface S2 of the laminate 50A opposite to the first end surface S1. The laminate 50A further includes a resin 10, which is softer than the solid electrolyte layer, in a position in contact with at least one of a cathode layer end E1 opposite the first end surface S1 of the cathode layer 1 and a negative electrode layer end E2 opposite the second end surface S2 of the anode layer 2. 1 includes resin 10 at both a position in contact with a positive electrode layer end E1 opposite the second end face S2 of the positive electrode layer 1 and a position in contact with a negative electrode layer end E2 opposite the first end face S1 of the negative electrode layer 2. Hereinafter, for convenience of explanation, the resin in contact with the positive electrode layer end E1 may be referred to as a first resin 10a, and the resin in contact with the negative electrode layer end E2 may be referred to as a second resin 10b. In this embodiment, when there is no need to particularly distinguish between the first resin 10a and the second resin 10b, they will be simply referred to as resin 10.
[0024] In this embodiment, the stacking direction of the positive electrode layer 1 and the negative electrode layer 2 in the laminate 50A shown in Fig. 1 is defined as the z direction, the direction perpendicular to the z direction and in which the positive electrode layer 1 and the negative electrode layer 2 extend in Fig. 1 is defined as the x direction, and the direction perpendicular to the x direction and the z direction is defined as the y direction. The positive electrode external terminal 5 and the negative electrode external terminal 4, which will be described in detail later, are formed to be spaced apart in the x direction.
[0025] [Laminate] The laminate 50A includes at least one positive electrode layer 1 and one negative electrode layer 2. The positive electrode layers 1 and the negative electrode layers 2 are alternately arranged with the solid electrolyte layer 3 interposed therebetween.
[0026] The laminate 50A is a substantially hexahedron having an upper surface and a lower surface, which are end surfaces in the stacking direction, and four side surfaces that are perpendicular to the upper and lower surfaces and parallel to the stacking direction. Of the four side surfaces, the end surface that joins the positive electrode layer 1 is referred to as the first end surface S1, and the end surface that joins the negative electrode layer 2 is referred to as the second end surface S2. In the laminate 50A, the first end surface S1 and the second end surface S2 are end surfaces of the laminate 50A in the x direction and are arranged opposite each other. In the laminate 50A, the distance between adjacent electrode layers is, for example, smaller than the distance from the positive electrode layer 1 to the second end surface S2 and the distance from the negative electrode layer 2 to the first end surface S1.
[0027] <Positive Electrode Layer> The positive electrode layer 1 includes a positive electrode current collector 1A and a positive electrode active material layer 1B. In the example shown in FIG. 1 , the positive electrode active material layer 1B is provided on at least one of the main surfaces of the positive electrode current collector 1A, and may be provided on both of them. The positive electrode layer end portion E1 is formed on the surface of the positive electrode current collector 1A and the positive electrode active material layer 1B opposite to the first end surface S1. The positive electrode layer end portion E1 is not joined to the positive electrode external terminal 5, and is provided at a position closer to the negative electrode external terminal 4 than to the positive electrode external terminal 5.
[0028] (Positive Electrode Current Collector) The positive electrode current collector 1A is made of a material with high conductivity. For example, the positive electrode current collector 1A can be made of a metal or alloy containing at least one metal element selected from silver (Ag), palladium (Pd), gold (Au), platinum (Pt), aluminum (Al), copper (Cu), and nickel (Ni), or carbon (C).
[0029] The positive electrode current collector 1A may be a foil or may be made of a plurality of conductive particles that are connected to each other and electrically connected in the xy plane.
[0030] (Positive Electrode Active Material Layer) The positive electrode active material layer 1B contains, as a positive electrode active material, a compound capable of absorbing and releasing at least lithium ions. The positive electrode active material layer 1B may also contain a conductive additive or an ion-conducting additive. It is preferable that the positive electrode active material be capable of efficiently inserting and desorbing lithium ions.
[0031] Such a positive electrode active material is, for example, a transition metal oxide or a transition metal composite oxide. Specific examples of the positive electrode active material include lithium manganese composite oxide Li 2 Mn a Ma 1-a O 3 (0.8≦a≦1, Ma=Co, Ni), lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMn) having a spinel structure 2 O 4 ), general formula: LiNi x Co y Mn z O 2 a composite metal oxide represented by (x+y+z=1, 0≦x≦1, 0≦y≦1, 0≦z≦1), a lithium vanadium compound (LiV 2 O 5 ), olivine-type LiMbPO 4 (wherein Mb is one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, and Zr), lithium vanadium phosphate (Li 3 V 2 (P.O. 4 ) 3 or LiVOPO 4 ), Li 2 MnO 3 -LiMcO 2 Lithium-excess solid solution cathode represented by (Mc=Mn, Co, Ni), lithium titanate (Li 4 Ti 5 O 12 ), titanium oxide (TiO 2 ), Li s Ni t Co u Al v O 2(0.9<s<1.3, 0.9<t+u+v<1.1), and the like.
[0032] Furthermore, in these positive electrode active materials, some of the elements may be substituted with different elements, and the composition may be changed from the stoichiometric composition.
[0033] Examples of the conductive additive include carbon materials such as carbon black, acetylene black, ketjen black, carbon nanotubes, graphite, graphene, and activated carbon, and metal materials such as gold, silver, palladium, platinum, copper, and tin.
[0034] The ion-conducting aid is, for example, a solid electrolyte. As the solid electrolyte, for example, the same material as that used for the solid electrolyte layer 3 can be used.
[0035] <Negative electrode layer> The negative electrode layer 2 includes a negative electrode current collector 2A and a negative electrode active material layer 2B. In the example shown in Fig. 1 , the negative electrode active material layer 2B is provided on at least one of the main surfaces of the negative electrode current collector 2A. The negative electrode layer end portion E2 is formed on the surface of the negative electrode current collector 2A and the negative electrode active material layer 2B opposite to the second end surface S2. The negative electrode layer end portion E2 is not joined to the negative electrode external terminal 4, and is provided at a position closer to the positive electrode external terminal 5 than to the negative electrode external terminal 4.
[0036] (Negative electrode current collector) The negative electrode current collector 2A is made of, for example, a metal or alloy containing at least one metal element selected from silver (Ag), palladium (Pd), gold (Au), platinum (Pt), aluminum (Al), copper (Cu), and nickel (Ni), or a non-metal such as carbon (C).
[0037] The negative electrode current collector 2A may be a foil or may be made of a plurality of conductive particles, which are, for example, connected to each other and electrically connected in the xy plane.
[0038] (Negative Electrode Active Material Layer) The negative electrode active material layer 2B is formed, for example, on one or both surfaces of the negative electrode current collector 2A. The negative electrode active material layer 2B contains a negative electrode active material. The negative electrode active material layer 2B may contain a conductive additive and a solid electrolyte. When the negative electrode active material layer 2B contains a solid electrolyte, the space between an xy plane passing through the outermost portion of the negative electrode active material and the boundary surface with the negative electrode current collector 2A is considered to be the negative electrode active material layer 2B.
[0039] The negative electrode active material is a compound capable of absorbing and releasing ions. The negative electrode active material is a compound exhibiting a more base potential than the positive electrode active material. Materials similar to those exemplified as the materials for the positive electrode active material can also be used as the negative electrode active material, but exhibiting a more base potential than the positive electrode active material. The negative electrode active material and the positive electrode active material used in the all-solid-state battery 100A are determined taking into consideration the potentials of the negative electrode active material and the positive electrode active material. Examples of the negative electrode active material include carbon materials, metals, alloys, or composite materials capable of combining with lithium, oxides, and metallic lithium. More specific examples include natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, fired organic compounds, Ag, Li, silicon, tin, zinc, lead, antimony, Si, Sn, aluminum, and alloys of these metals such as AgPd, and lithium titanate (Li 4 Ti 5 O 12 , LiTiO 2 , Li 2 TiO 3 , Li 2 TiSiO 5 ) and Li 3 V 2 (P.O. 4 ) 3 , SiO x , SnO 2 , may be used. An alloy containing Ag other than AgPd may also be used.
[0040] The conductive additive improves the electronic conductivity of the negative electrode active material layer 2 B. As the conductive additive, the same materials as those used in the positive electrode active material layer 1 B can be used.
[0041] <Solid Electrolyte Layer> The solid electrolyte layer 3 includes a solid electrolyte. A solid electrolyte is a substance that can move ions by an externally applied electric field. For example, the solid electrolyte layer 3 conducts lithium ions and inhibits the movement of electrons. The solid electrolyte layer 3 is, for example, a sintered body obtained by sintering.
[0042] The solid electrolyte layer 3 is, for example, γ-Li 3 P.O. 4The solid electrolyte includes a solid electrolyte having a crystalline structure of LiSiC type (LiSiC type) and a solid electrolyte having a crystalline structure of NaSiC type. 3+x Si x P 1-x O 4 (LSPO, 0.4≦x≦0.8), Li 3+x Si x V 1-x O 4 (LSVO, 0.4≦x≦0.8), Li 3+x Ge x P 1-x O 4 (LGPO, 0.4≦x≦0.8), Li 3+x Ge x V 1-x O 4 (LGVO, 0.4≦x≦0.8) and other crystalline structures of lysicone type, LiTi 2 (P.O. 4 ) 3 (LTP), LiZr 2 (P.O. 4 ) 3 (LZP), Li 1+x Al x Ti 2-x (P.O. 4 ) 3 (LATP, 0<x≦0.6), Li 1+x Al x Ge 2-x (P.O. 4 ) 3 (LAGP, 0<x≦0.6), Li 1+x Y x Zr 2-x (P.O. 4 ) 3 (LYZP, 0<x≦0.6) or the like. 0.5 Li 0.5 TiO 3 Perovskite compounds such as Li 14 Zn(GeO 4 ) 4 Lithium-type compounds such as Li 7 La 3 Zr 2 O 12 Garnet-type compounds such as Li 3.25 Ge 0.25P 0.75 S 4 and Li 3 P.S. 4 Thiolisicon-type compounds such as Li 2 S-P 2 S 5 and Li 2 O-V 2 O 5 -SiO 2 Glass compounds such as Li 3 P.O. 4 and Li 3.5 Si 0.5 P 0.5 O 4 and Li 2.9 P.O. 3.3 N 0.46 and the like.
[0043] The oxide-based solid electrolyte described above is harder than the sulfide-based solid electrolyte and is less likely to deform under pressure. Therefore, it is thought that cracks are more likely to occur due to expansion and contraction during charging and discharging of the battery. However, in this embodiment, as will be described in detail later, the resin 10 is formed at a predetermined position, which suppresses cracks from propagating from an electrode layer to an adjacent electrode layer. This makes it possible to provide an all-solid-state battery with excellent cycle characteristics that is less likely to cause short circuits even after repeated use.
[0044] <Resin> The all-solid-state battery 100A includes a first resin 10a in contact with the positive electrode layer end E1 and a second resin 10b in contact with the negative electrode layer end E2. The all-solid-state battery 100A includes a resin 10 softer than the solid electrolyte layer 3, filling, for example, either a first region R1 sandwiched between the positive electrode layer 1 and the second end surface S2 or a second region R2 sandwiched between the negative electrode layer 2 and the first end surface S1. As shown in FIG. 2 , the second resin 10b formed in the second region R2 is, for example, aligned with the negative electrode layer 2 in the y direction and positioned between the negative electrode layer 2 and the first end surface S1 in the x direction so as to be in contact with the negative electrode layer end E2 and the first end surface S1. A margin layer made of, for example, a solid electrolyte or the like is aligned with the negative electrode layer 2 in the y direction.
[0045] FIG. 3 is a cross-sectional view of a modified example of FIG. 2 . As shown in FIG. 3 , the second resin 10b formed in the second region R2 only needs to be provided in the region between the negative electrode layer 2 and the first end surface S1 in the y direction. It may also be provided across the entire region from end to end in the x direction beyond the second region R2. The first resin 10a aligned with the positive electrode layer 1 in the stacking direction may be arranged in the same manner as the second resin 10b aligned with the negative electrode layer 2. The second resin 10b formed in the second region R2 is, for example, aligned with the second end surface S2 in the y direction and is provided between the negative electrode layer 2 and the first end surface S1 in the x direction so as to contact the negative electrode layer end E2 and the first end surface S1. A margin layer made of, for example, a solid electrolyte may be provided in the y direction of the negative electrode layer 2, or a resin may be provided. The resin provided in the y direction relative to the negative electrode layer 2 may extend to a position sandwiching the second region R2. That is, the resin may be provided over the entire second region R2, which is the region between the negative electrode layer 2 and the first end surface S1 in the x direction.
[0046] The resin 10 may be a resin having a Rockwell hardness lower than that of the solid electrolyte layer 3. The resin 10 may be, for example, a thermoplastic resin or a thermosetting resin.
[0047] When the resin 10 is a thermoplastic resin, for example, a fluororesin, an acrylic resin (e.g., polymethyl acrylate, polymethyl methacrylate), polycarbonate, polyimide, polyamide, polyamideimide, polystyrene, polyvinyl chloride, polyethylene, polypropylene, an acrylonitrile-butadiene-styrene copolymer, an acrylonitrile-styrene copolymer, polyvinyl alcohol, polyvinylidene chloride, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyphenyl ether, polysulfone, polyethersulfone, polyphenyl sulfide, polyarylate, polyetherimide, polyetheretherketone, a liquid crystal polymer, an ultra-high molecular weight polyethylene, a urethane resin, polypropylene, an acrylic-nitrile-butadiene-styrene resin, polyphenylene ether, polyphenylene sulfite, polytetrafluoroethylene, etc. When the resin 10 is a thermosetting resin, for example, a phenolic resin, a urea resin, a melamine resin, an unsaturated polyester, an epoxy resin, a silicone resin, a polyurethane, etc. can be used.
[0048] The Rockwell hardness of the resin 10 is preferably HRR 115 or less, and more preferably HRR 100 or less. The "HR" in HRR indicates Rockwell hardness, and the "R" indicates the hardness scale. HRR is a hardness scale that is softer than HRM. The Rockwell hardness HR of the resin is measured by a method in accordance with JIS K7202-2:2001.
[0049] The resin 10 is provided so as to fill, for example, the first region R1 or the second region R2. The all-solid-state battery 100A shown in FIG. 1 illustrates an example in which the first resin 10a is formed in all of the first regions R1 and the second resin 10b is formed in all of the second regions R2. However, only one of the first resin 10a or the second resin 10b may be formed. Furthermore, it is sufficient that the first resin 10a is formed in at least one of the multiple first regions R1, or the second resin 10b is formed in at least one of the multiple second regions R2.
[0050] As described above, for example, a margin layer 15 is provided at the same position in the stacking direction as the positive electrode layer 1 and in the ±y direction with respect to the positive electrode layer 1. Similarly, for example, a margin layer 15 is provided at the same position in the stacking direction as the negative electrode layer 2 and in the ±y direction with respect to the negative electrode layer 2. The margin layer 15 is made of, for example, the same material as the solid electrolyte layer 3.
[0051] In the above example, the first region R1 is filled with the first resin 10a and the second region R2 is filled with the second resin 10b, but in the first region R1 and the second region R2, a layer made of another material such as a solid electrolyte may be formed on the first resin 10a or the second resin 10b or below the resin 10. Even when another material is formed on the first resin 10a or the second resin 10b or below the first resin 10a or the second resin 10b, it is preferable that the first resin 10a and the second resin 10b be provided so as to contact the end of the electrode layer and the end face of the opposing laminate.
[0052] The all-solid-state battery 100A according to this embodiment includes at least one of the first resin 10 a and the second resin 10 b, which suppresses the occurrence of short circuits caused by cracks propagating from an electrode layer to an adjacent electrode layer. Therefore, according to the present invention, an all-solid-state battery with excellent cycle characteristics can be obtained.
[0053] Although one embodiment of the present invention has been described above in detail with reference to the drawings, the configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible within the scope of the present invention. For example, the all-solid-state battery 100B shown in FIG. 4 may be used.
[0054] FIG. 4 is a cross-sectional view showing the configuration of an all-solid-state battery according to a modified example of FIG. 1 , and FIG. 5 is a cross-sectional view showing a cross section taken along the line B-B in FIG. 4 . The all-solid-state battery 100B shown in FIG. 4 includes a first resin 10c in contact with the positive electrode layer end E1 and a second resin 10d in contact with the negative electrode layer end E2. The lengths of the first resin 10c and the second resin 10d in the x direction of the all-solid-state battery 100B are different from those of the all-solid-state battery 100A. The lengths of the first resin 10c and the second resin 10d in the x direction are shorter than those of the first resin 10a and the second resin 10b, and the first resin 10c and the second resin 10d are not in contact with the second end surface S2 and the first end surface S1, respectively. Furthermore, the first resin 10c and the second resin 10d may be provided so as to be in contact with three of the side surfaces of the electrode layer exposed in a direction intersecting the stacking direction, other than the external electrode terminals of the same polarity, as shown in FIG. 5 . In the all-solid-state battery 100B, the same components as those in the all-solid-state battery 100A are denoted by the same reference numerals, and the description thereof will be omitted.
[0055] In the extension direction (x direction) of the positive electrode layer 1, the ratio of the length d2 of the first resin 10c to the distance d1 between the positive electrode layer end E1 and the second end surface S2 is, for example, 0.1 or more, preferably 0.5 or more. Similarly, in the extension direction (x direction) of the negative electrode layer 2, the ratio of the length of the second resin 10d to the distance between the negative electrode layer end E2 and the first end surface S1 is, for example, 0.1 or more, preferably 0.5 or more. A margin layer 15, for example, is formed in the region of the first region R1 excluding the first resin 10c and in the region of the second region R2 excluding the second resin 10d. When resin is formed in the first region R1 and the second region R2, the first resin filling rate and the second resin filling rate are, for example, 50 to 100%, preferably 80 to 100%. The first region resin filling rate represents the ratio of the area of the region in which resin is formed to the area of the first region R1 in the cross section of the laminate, and the second region resin filling rate represents the ratio of the area of the region in which resin is formed to the area of the second region R2.
[0056] The all-solid-state battery 100B according to the modified example can also suppress the occurrence of a short circuit caused by a crack propagating from an electrode layer to an electrode layer adjacent to the electrode layer.
[0057] FIG. 6 is a cross-sectional view showing the configuration of an all-solid-state battery according to a modified example of FIG. 1 . The all-solid-state battery 100C shown in FIG. 6 differs from the all-solid-state battery 100A in the anode layer. In this modified example, components similar to those in the all-solid-state battery 100A of FIG. 1 are designated by the same reference numerals and will not be described again. In the all-solid-state battery 100C, the anode layer 2X serves as both an anode current collector and an anode active material layer. The anode layer 2X exhibits a lower potential than the cathode active material. The anode layer 2X preferably contains a metal selected from the group consisting of silver (Ag), palladium (Pd), gold (Au), and platinum (Pt). This is because Ag, Pd, Au, and Pt do not melt and are resistant to oxidation even when the sintering process for producing the laminate 50B is performed in an air atmosphere. The anode layer 2X may be made of any of the above metals or an alloy containing any of the above metals.
[0058] The negative electrode layer 2X preferably contains an AgPd alloy. Furthermore, the negative electrode layer 2X preferably contains an AgPd alloy, because this results in a solid-state battery with high energy density. For example, the AgPd alloy may contain Ag and Pd in a molar ratio of 8:2 (Ag:Pd).
[0059] The negative electrode layer 2X may contain metal particles made of any of the above metals and / or alloy particles made of an alloy containing any of the above metals, and one or more selected from a conductive additive and a solid electrolyte.
[0060] The upper and / or lower limits of the numerical ranges described herein can be arbitrarily combined to define a preferred range. For example, the upper and lower limits of the numerical ranges can be arbitrarily combined to define a preferred range, the upper limits of the numerical ranges can be arbitrarily combined to define a preferred range, and the lower limits of the numerical ranges can be arbitrarily combined to define a preferred range.
[0061] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0062] [Example 1] (Preparation of paste for positive electrode active material layer) LCO (LiCoO2 100 parts of the powder, 15 parts of ethyl cellulose as a binder, and 65 parts of dihydroterpineol as a solvent were mixed and dispersed to prepare a paste for a positive electrode active material layer.
[0063] (Preparation of Positive Electrode Current Collector Paste) AgPd and LCO were mixed to a volume ratio of 70 / 30, and then 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent were added to 100 parts of the mixed powder, and the mixture was mixed and dispersed to prepare a positive electrode current collector paste.
[0064] (Preparation of Paste for Solid Electrolyte Layer) Li 2 CO 3 and SiO 2 and Li 3 P.O. 4 These were used as starting materials and mixed in a molar ratio of 2:1:1. The mixture was wet mixed for 16 hours using a ball mill with water as a dispersion medium. The mixture was calcined at 950°C for 2 hours to obtain Li 3.5 Si 0.5 P 0.5 O 4 Then, 100 parts of this calcined powder, 100 parts of ethanol, and 200 parts of toluene were added to a ball mill and wet mixed. Then, 16 parts of a polyvinyl butyral binder and 4.8 parts by mass of benzyl butyl phthalate were further added and mixed to prepare a paste for a solid electrolyte layer.
[0065] (Preparation of Solid Electrolyte Sheet) A solid electrolyte sheet having a thickness of 15 μm was prepared by forming a sheet on a PET film using the paste for a solid electrolyte layer by a doctor blade method.
[0066] (Preparation of Negative Electrode Layer Paste) In Example 1, the negative electrode layer served as both a negative electrode current collector and a negative electrode active material layer. A negative electrode layer paste was prepared by mixing and dispersing 100 parts of AgPd powder as a negative electrode current collector and negative electrode active material, 15 parts of ethyl cellulose as a binder, and 65 parts of dihydroterpineol as a solvent.
[0067] (Preparation of Resin) In Example 1, an acrylic resin was prepared as the resin to be formed in the first region and the second region. The prepared acrylic resin was subjected to a heat treatment under the same conditions as those for producing the all-solid-state battery of Example 1, and then the Rockwell hardness was measured using a method in accordance with JIS K7202-2:2001, resulting in a result of HRR 110. The heat-resistant temperature based on the continuous use temperature of the acrylic resin used was 110°C. Here, the continuous use temperature refers to the upper limit temperature at which the strength of a test piece of the object is maintained at 50% or more of its initial value even when left in that temperature environment for 40,000 hours.
[0068] (Preparation of void paste) In the example, a structure laminated in a predetermined arrangement and order is heat-treated, and then a resin is formed in the structure by vacuum impregnation. In the areas where resin is to be formed by vacuum impregnation, a void paste is formed and heat-treated to create voids. The void paste was prepared by mixing and dispersing 100 parts of acrylic resin powder with a particle diameter of 200 nm, 15 parts of ethyl cellulose as a binder, and 65 parts of dihydroterpineol as a solvent. In the firing process described below, the acrylic resin is thermally decomposed when fired, forming voids in those areas.
[0069] (Preparation of Margin Paste) The margin paste was prepared using LSPO (Li 3.5 Si 0.5 P 0.5 O 4 The powder was prepared by mixing and dispersing 100 parts of the above powder, 15 parts of ethyl cellulose as a binder, and 65 parts of dihydroterpineol as a solvent.
[0070] (Preparation of Positive Electrode Layer Unit) A positive electrode active material layer paste was formed on a solid electrolyte sheet by screen printing to a thickness of 10 μm and dried at 80°C for 10 minutes to form a positive electrode active material layer (hereinafter referred to as a first positive electrode active material layer). Next, a positive electrode current collector paste was formed on the positive electrode active material layer by screen printing to a thickness of 10 μm and dried at 80°C for 10 minutes to form a positive electrode current collector. Next, a positive electrode active material layer paste was formed on the positive electrode current collector by screen printing to a thickness of 10 μm and dried at 80°C for 10 minutes to form another positive electrode active material layer (hereinafter referred to as a second positive electrode active material layer). In this way, a 30 μm thick positive electrode layer was formed on the solid electrolyte sheet, in which the first positive electrode active material layer, the positive electrode current collector, and the second positive electrode active material layer were stacked in this order.
[0071] Next, a gap paste was formed by screen printing on the outer periphery of the side surface of the positive electrode layer that would later face (be close to) the negative electrode external terminal, and dried at 80° C. for 10 minutes.
[0072] Next, a margin paste was formed by screen printing on the outer periphery of each side surface in the width direction of the positive electrode layer (two side surfaces excluding the surface to be joined later to the positive electrode external terminal and the surface opposite thereto), and dried for 10 minutes at 80° C. The margin paste was formed to a thickness such that its surface was flush with the surface of the positive electrode layer unit.
[0073] Next, the PET film was peeled off to form a margin paste on the outside of the positive electrode layer in the y direction, and a gap paste was formed between the positive electrode layer end and the second end face to produce a positive electrode layer unit. The ratio of the length of the positive electrode layer in the x direction to the length of the positive electrode layer unit in the x direction was 0.9. Specifically, the x direction length of the positive electrode layer of the positive electrode layer unit was 4.5 mm + 0.5 mm of gap paste provided in the margin, and the y direction length of the positive electrode layer was 3.0 mm + 0.5 mm x 2 of margin paste provided in the margin.
[0074] (Fabrication of Negative Electrode Layer Unit) The negative electrode layer unit was fabricated in the same manner as in the fabrication of the positive electrode layer unit, that is, the negative electrode layer unit was fabricated in the following manner.
[0075] First, the paste for the negative electrode layer was applied to a solid electrolyte sheet by screen printing to form a layer having a thickness of 10 μm, and then dried at 80° C. for 10 minutes to form a negative electrode layer having a thickness of 10 μm.
[0076] Next, a gap paste was formed by screen printing on the outer periphery of the surface that would later face (be close to) the positive electrode external terminal, and dried at 80° C. for 10 minutes.
[0077] Next, a margin paste was formed by screen printing on the outer periphery of each side surface in the width direction of the negative electrode layer (two side surfaces excluding the surface to be joined later to the negative electrode external terminal and the surface opposite thereto), and dried for 10 minutes at 80° C. The margin paste was formed so that its surface was flush with the surface of the negative electrode layer unit.
[0078] Next, the PET film was peeled off to form a margin paste on the y-direction outer side of the negative electrode layer, and a gap paste was formed between the end of the negative electrode layer and the first end face to produce a negative electrode layer unit. The ratio of the length of the negative electrode layer in the x-direction to the length of the negative electrode layer unit in the x-direction was 0.9. Specifically, the x-direction length of the negative electrode layer of the negative electrode layer unit was 4.5 mm + 0.5 mm of gap paste provided in the margin, and the y-direction length of the negative electrode layer was 3.0 mm + 0.5 mm x 2 of margin paste provided in the margin.
[0079] (Fabrication of laminate structure for laminate) Ten positive electrode layer units and ten negative electrode layer units were prepared, and the positive electrode layer units and the negative electrode layer units were laminated in this order while being alternately offset so that one end of each unit did not coincide. Furthermore, multiple layers of solid electrolyte sheets were laminated on the outer side of the electrode layer unit that was to be the outermost layer in the stacking direction, to provide an outer layer with a thickness of 100 μm.
[0080] This was thermocompressed using a mold press and then cut to produce an unfired all-solid-state battery laminate. The laminate size was 5 mm and 4 mm in the x and y directions, respectively. Next, the unfired laminate was debindered and fired to produce an all-solid-state battery laminate. The laminate was heat-treated at 500°C for 10 hours in an air atmosphere to perform a binder removal treatment on the laminate. Firing was performed at 900°C for 1 hour in an air atmosphere.
[0081] (Resin Formation) In the laminated structure, the regions where the void-forming paste was formed by the previous firing were voids. In the regions where voids were formed in the laminated structure, acrylic resin was formed by vacuum impregnation using the following procedure.
[0082] First, a silicon jig for resin impregnation was prepared. Specifically, a silicon resin having the same length and thickness in the x direction as the positive electrode layer unit and the negative electrode layer unit was prepared, and holes were drilled inside the silicon resin, leaving the skeleton portion. This resin impregnation jig was then installed in a position corresponding to the void in the laminate structure.
[0083] Next, the laminated structure equipped with a jig for resin impregnation was placed in a pressure-resistant container. Next, resin heated to 260°C was dripped onto the area of the laminate aligned with the positive electrode layer, and the pressure-resistant container was evacuated using a rotary pump. By evacuating the pressure-resistant container, the resin was impregnated into the area (second area) where a void was formed at the tip of the negative electrode, forming a laminate. Next, excess resin adhering to the surface of the laminated structure was wiped off. Next, the area (first area) where a void was formed at the tip of the positive electrode was similarly impregnated with resin, the container was evacuated, and excess resin adhering to the surface of the laminated structure was wiped off. Next, the resin was cured at room temperature, and the end surfaces of the laminated structure were polished with #1200 abrasive paper to expose the electrodes. Of the side surfaces of the laminated structure, the surface where the positive electrode layer is exposed is referred to as the first end surface, and the surface where the negative electrode layer is exposed is referred to as the second end surface. The region sandwiched between the first end surface and the negative electrode layer is referred to as the “first region,” and the region sandwiched between the second end surface and the positive electrode layer is referred to as the “second region.” In Example 1, the acrylic resin was formed in both the first region and the second region by the above-described process.
[0084] (External electrode forming step) An external electrode paste was applied to the end faces (first end face and second end face) in the x direction of the fired all-solid-state battery laminate, and thermal curing was performed for 30 minutes at 150°C to form a pair of external electrodes, thereby producing an all-solid-state battery. As the external electrode paste, a thermosetting external electrode paste prepared by mixing and dispersing silver powder, a thermosetting resin, and a solvent was used.
[0085] (Example 2) An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to vinyl chloride. The Rockwell hardness of the vinyl chloride used was measured in the same manner as in Example 1 and was found to be HRR 110. The heat-resistant temperature of vinyl chloride, as defined in Example 1, is 90°C.
[0086] (Example 3) An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to polyethylene. The Rockwell hardness of the polyethylene used was measured in the same manner as in Example 1 and was found to be HRR 125. The heat-resistant temperature of polyethylene, as defined in Example 1, is 90°C.
[0087] Example 4 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to polypropylene. The Rockwell hardness of the polypropylene used was measured in the same manner as in Example 1 and was found to be HRR 100. The heat-resistant temperature of polypropylene, as defined in Example 1, was 110°C.
[0088] (Example 5) An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to polystyrene. The Rockwell hardness of the polystyrene used was measured in the same manner as in Example 1 and was found to be HRR 90. The heat-resistant temperature of polystyrene, as defined in Example 1, was 100°C.
[0089] (Example 6) An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to polycarbonate. The Rockwell hardness of the polycarbonate used was measured in the same manner as in Example 1 and was found to be HRR 115. The heat-resistant temperature of polycarbonate, as defined in Example 1, was 130°C.
[0090] Example 7 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to nylon 66. The Rockwell hardness of the nylon 66 used was measured in the same manner as in Example 1 and was found to be HRR 100. The heat-resistant temperature of nylon 66, as defined in Example 1, is 120°C.
[0091] Example 8 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to polyacetal. The Rockwell hardness of the polyacetal used was measured in the same manner as in Example 1 and was found to be HRR 100. The heat-resistant temperature of polyacetal, as defined in Example 1, was 120°C.
[0092] Example 9 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to acrylonitrile butadiene styrene resin (ABS). The Rockwell hardness of the ABS used was measured in the same manner as in Example 1 and was found to be HRR 105. The heat-resistant temperature of the ABS, as defined in Example 1, was 80°C.
[0093] (Example 10) An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin formed in the first region and the second region was changed to a thermosetting polyimide. The Rockwell hardness of the polyimide used was measured in the same manner as in Example 1 and was found to be HRR 120. The heat-resistant temperature of the polyimide, as defined in Example 1, was 300°C.
[0094] (Example 11) An all-solid-state battery was fabricated in the same manner as in Example 1, except that the resin forming the first region and the second region was changed to epoxy resin. The Rockwell hardness of the epoxy resin used was HRM 100. The heat-resistant temperature of the epoxy resin, as defined in Example 1, was 200°C.
[0095] Example 12 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the negative electrode current collector and negative electrode active material was changed to Ag.
[0096] Example 13: The negative electrode layer was changed to a configuration having a negative electrode current collector and a negative electrode active material layer, and the negative electrode active material was changed to lithium titanate Li 4 Ti 5 O 12 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the negative electrode current collector was changed to AgPd (hereinafter referred to as LTO), the thickness of the negative electrode layer and the thickness of the resin adjacent to the negative electrode layer were changed to 30 μm.
[0097] Example 14: The negative electrode active material was a lithium vanadium compound Li 3 V 2 (P.O. 4 ) 3 An all-solid-state battery was produced in the same manner as in Example 1, except that the thickness of the negative electrode layer and the thickness of the resin provided adjacent to the negative electrode layer were changed to 30 μm.
[0098] Example 15 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the positive electrode active material was changed to LTO.
[0099] Example 16: Solid electrolyte: Lithium aluminum phosphate titanium Li 1.4 Al 0.4 Ti 1.6 (P.O. 4 ) 3 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the electrolyte was changed to (LATP).
[0100] Example 17: Solid electrolyte: Lithium zirconium phosphate LiZr 2 (P.O. 4 ) 3 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the PET film was changed to LZP.
[0101] (Example 18) An all-solid-state battery was produced in the same manner as in Example 1, except that no resin was formed in the second region. By doing so, the second region, which is the tip portion of the negative electrode, was not impregnated with resin, and a structure was formed in which the second region was a void.
[0102] Example 19 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the size of the resin formed in contact with the anode layer was reduced. In Example 19, the length of the resin formed in contact with the anode layer in the extension direction of the anode layer was 10% of the distance from the tip of the anode layer to the first end face. That is, in Example 19, the ratio of the length of the resin to the length of the second region in the extension direction of the anode layer was 10%, and the filling rate of the resin in the second region was 10%. The resin length ratio was adjusted using the following method. First, resin was dripped into the region (second region) of the laminate aligned with the cathode layer, and a predetermined amount of resin was impregnated by adjusting the time for vacuuming using a rotary pump. Next, the resin was solidified with the surface facing up. This resulted in the formation of a structure in which the resin was present in the portion in contact with the tip of the anode layer and voids were present on the end face side.
[0103] Example 20 An all-solid-state battery was fabricated in the same manner as in Example 19, except that the length of the resin formed so as to be in contact with the negative electrode layer was smaller than that in Example 1 and larger than that in Example 19, and the filling rate of the resin in the second region was 50%.
[0104] Example 21 An all-solid-state battery was fabricated in the same manner as in Example 1, except that no resin was formed in the first region. By doing so, the first region, which is the tip portion of the positive electrode, was not impregnated with resin, and a structure was formed in which the first region was a void.
[0105] Example 22 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the size of the resin formed in the first region was reduced. That is, in Example 22, the ratio of the length of the resin to the length of the first region in the extending direction of the positive electrode layer was set to 10%, and the filling rate of the resin in the first region was set to 10%.
[0106] Example 23 An all-solid-state battery was fabricated in the same manner as in Example 22, except that the filling rate of the resin in the first region was set to 50%.
[0107] In Examples 24 and 25, all-solid-state batteries were fabricated in the same manner as in Examples 19 and 20, respectively, except that the portion in contact with the positive electrode layer (first region) was not filled with resin but was left as a gap. That is, in Examples 24 and 25, the resin filling rate of the first region was 0%.
[0108] In Examples 26 and 27, all-solid-state batteries were fabricated in the same manner as in Examples 22 and 23, respectively, except that the portion in contact with the negative electrode layer (second region) was not filled with resin but was left as a void. That is, in Examples 26 and 27, the resin filling rate of the second region was 0%.
[0109] (Examples 28 and 29) In Examples 28 and 29, all-solid-state batteries were fabricated in the same manner as in Examples 24 and 25, respectively, except that a solid electrolyte was provided in the area (first region) in contact with the positive electrode layer. Specifically, a margin paste was applied instead of a void paste to form LSPO, which is a solid electrolyte, in the first region. That is, in Examples 28 and 29, the resin filling rate of the first region was 0%.
[0110] (Examples 30 and 31) In Examples 30 and 31, all-solid-state batteries were fabricated in the same manner as in Examples 26 and 27, respectively, except that a solid electrolyte was provided in the area (second region) in contact with the negative electrode layer. Specifically, a margin paste was applied instead of a void paste to form the second region using LSPO, which is a solid electrolyte. That is, in Examples 30 and 31, the resin filling rate of the second region was 0%.
[0111] Example 32 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the thickness of the negative electrode layer paste to be fabricated on the solid electrolyte sheet was changed to 1 μm. In Example 32, the resin had a thickness equal to or greater than the negative electrode layer at the stage of fabricating the all-solid-state battery. In Example 32, by reducing the thickness of the negative electrode layer paste in this way, the portion of silver exceeding the allowable amount precipitated as metallic lithium during charge and discharge and functioned as the negative electrode.
[0112] Examples 33 to 36 All-solid-state batteries were fabricated in the same manner as in Example 32, except that the resin used was changed.
[0113] (Comparative Example 1) An all-solid-state battery was fabricated in the same manner as in Example 1, except that all regions corresponding to the first region and the second region were filled with only margin paste without using any voids. That is, in Comparative Example 1, the filling rate of the resin in the first region and the second region was set to 0%.
[0114] Comparative Example 2 An all-solid-state battery was produced in the same manner as in Example 1, except that the step of vacuum impregnating a resin into the voids after producing a laminated structure having voids was omitted.
[0115] Comparative Example 3 An all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that the negative electrode active material was changed from AgPd to Ag.
[0116] Comparative Example 4: The negative electrode layer was changed to have a configuration including a negative electrode current collector and a negative electrode active material layer, and the negative electrode active material was changed to LTO (Li 4 Ti 5 O 12 An all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that the negative electrode layer was changed to AgPd) and that AgPd was used as the negative electrode current collector. In Comparative Example 4, the negative electrode layer was fabricated by the following procedure.
[0117] (Preparation of negative electrode active material paste) LTO (Li 4 Ti 5 O 12 100 parts of the powder, 15 parts of ethyl cellulose as a binder, and 65 parts of dihydroterpineol as a solvent were mixed and dispersed to prepare a paste for a negative electrode active material layer.
[0118] (Preparation of negative electrode current collector paste) AgPd and LTO were mixed to a volume ratio of 70 / 30, and then 100 parts of the mixed powder were added with 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent, followed by mixing and dispersing to prepare a negative electrode current collector paste.
[0119] First, a negative electrode active material paste was formed on a solid electrolyte sheet by screen printing to a thickness of 10 μm and dried at 80° C. for 10 minutes to form a negative electrode active material layer (hereinafter referred to as the first negative electrode active material layer). Next, a negative electrode current collector paste was formed on the negative electrode active material layer by screen printing to a thickness of 10 μm and dried at 80° C. for 10 minutes to form a negative electrode current collector. Next, a negative electrode active material layer paste was formed on the negative electrode current collector by screen printing to a thickness of 10 μm and dried at 80° C. for 10 minutes to form another negative electrode active material layer (hereinafter referred to as the second negative electrode active material layer). In this way, a 30 μm thick negative electrode layer was formed on the solid electrolyte sheet, in which the first negative electrode active material layer, the negative electrode current collector, and the second negative electrode active material layer were stacked in this order.
[0120] Comparative Example 5 An all-solid-state battery was fabricated in the same manner as in Comparative Example 4, except that the negative electrode active material was changed from LTO to LVP.
[0121] Comparative Example 6 An all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that the positive electrode active material was changed from LCO to LTO.
[0122] Comparative Example 7 The conditions were changed in the same manner as in Example 32 for Example 1. That is, an all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that the thickness of the negative electrode layer paste to be formed on the solid electrolyte sheet was changed to 1 μm.
[0123] (Battery Evaluation) The charge / discharge cycle characteristics of the all-solid-state batteries of Examples 1 to 35 and Comparative Examples 1 to 7 were evaluated under the charge / discharge conditions shown below. First, 1,000 all-solid-state batteries corresponding to each Example and Comparative Example were prepared and subjected to constant current charging (CC charging) at a constant current of 0.2 C rate in an environment of 25°C until the battery voltage reached 1.6 V. Next, the batteries were discharged at a constant current of 0.2 C rate until the battery voltage reached 0 V (CC discharging). The CC charging and CC discharging constituted one cycle, and this cycle was repeated up to 100 cycles. The short-circuit occurrence rate was calculated from the number of short-circuited all-solid-state batteries among the 1,000 all-solid-state batteries after 100 cycles.
[0124] The fabrication conditions and measurement results for the all-solid-state batteries of Examples 1 to 35 and Comparative Examples 1 to 7 are summarized in Tables 1 to 4. In the tables, the resin filling rate of the first region represents the ratio of the area of the region where the resin is formed to the area of the first region in the cross section of the laminate, and the resin filling rate of the second region represents the ratio of the area of the region where the resin is formed to the area of the second region. Since Tables 1 and 3 show the conditions before charge and discharge, AgPd is listed as the negative electrode layer in Examples 32 to 35 and Comparative Example 7. However, in these Examples and Comparative Examples, as described above, Li precipitated during the charge and discharge process also functions as the negative electrode.
[0125]
[0126]
[0127]
[0128]
[0129] Tables 1 to 4 confirm that Examples 1 to 35, in which a resin was formed in at least one of the first and second regions, were able to suppress the incidence of short circuits compared to Comparative Examples 1 to 7, in which a resin was not formed in either the first or second region. In the tables, the resin filling rate in the first region and the resin filling rate in the second region represent the area ratio of the first resin in the first region and the area ratio of the second resin in the second region, respectively, in the cross section of the all-solid-state battery. Comparative Example 2 presents experimental data in which the entire first and second regions are voids. However, it was confirmed that Examples 1 to 27 and Examples 32 to 35 were able to reduce the incidence of short circuits compared to Comparative Example 2. Examples 28 to 31, in which a solid electrolyte was formed in one of the first and second regions and a resin was formed in the other to achieve a lower filling rate, also suppressed the incidence of short circuits compared to Comparative Example 1, which differs in that a solid electrolyte was formed without a resin. Furthermore, it was confirmed that among Examples 1 to 11, which had the same configuration except for the type of resin, the example using a resin with a Rockwell hardness of 115 or less had a lower incidence of short circuits.
[0130] 1: Positive electrode layer, 1A: Positive electrode current collector, 1B: Positive electrode active material layer, 2: Negative electrode layer, 2A: Negative electrode current collector, 2B: Negative electrode active material layer, 3: Solid electrolyte layer, 4: Negative electrode external terminal, 5: Positive electrode external terminal, 10: Resin, 50A, 50B: Laminated body, R1: First region, R2: Second region, S1: First end surface, S2: Second end surface
Claims
1. An all-solid-state battery comprising: a laminate having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer, the solid electrolyte layer being disposed between the positive electrode layer and the negative electrode layer; a positive electrode external terminal joining the positive electrode layer at a first end surface of the laminate; and a negative electrode external terminal joining the negative electrode layer at a second end surface of the laminate facing the first end surface, the all-solid-state battery further comprising a resin softer than the solid electrolyte layer at a position in contact with at least one of an end surface of the positive electrode layer opposite to the first end surface of the positive electrode layer and an end surface of the negative electrode layer opposite to the second end surface of the negative electrode layer.
2. The all-solid-state battery according to claim 1, wherein the resin fills either a first region sandwiched between the positive electrode layer and the second end surface, or a second region sandwiched between the negative electrode layer and the first end surface.
3. The all-solid-state battery according to claim 1 or 2, wherein the resin is a thermoplastic resin.
4. The all-solid-state battery according to claim 1, wherein the resin has a Rockwell hardness of HRR115 or less.
5. The all-solid-state battery according to claim 1 or 2, wherein the resin is provided at a position in contact with an end of the negative electrode layer.
6. The all-solid-state battery according to claim 1 or 2, wherein the resin is provided at a position in contact with an end of the positive electrode layer.
7. The all-solid-state battery according to claim 1 or 2, wherein the resin is provided on both an end portion of the positive electrode layer and an end portion of the negative electrode layer.
8. The all-solid-state battery according to claim 1 or 2, wherein the negative electrode active material layer provided in the negative electrode layer is composed of AgPd or Ag.
Citation Information
Patent Citations
All-solid-state lithium secondary battery
JP2020191202A
Laminate type solid battery