All-solid-state battery
The introduction of a porous body within the all-solid-state battery laminate addresses crack propagation issues by reducing stress between electrode layers, enhancing cycle characteristics and preventing short circuits, even with alloy-based materials that expand and contract significantly.
Patent Information
- Application Number
- PCT/JP2024/012285
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
All-solid-state batteries face issues with crack propagation from electrode layers due to expansion and contraction during charging and discharging, leading to deteriorated cycle characteristics and potential short circuits, especially when alloy-based materials with large expansion and contraction are used for the negative electrode.
Incorporating a porous body with a porosity of 20% to 99% and average void diameters of 0.1 μm to 10 μm within specific regions of the battery laminate, which alleviates stress and prevents crack propagation between electrode layers by increasing the distance between electrode layers and external terminals.
The solution effectively suppresses crack propagation and improves cycle characteristics, reducing the occurrence of short circuits and maintaining battery performance even with alloy-based materials that exhibit significant expansion and contraction.
Smart Images

Figure JP2024012285_03102024_PF_FP_ABST
Abstract
Description
All solid state battery
[0001] The present invention relates to an all-solid-state battery. This application claims priority to Japanese Patent Application No. 2023-055315, filed on March 30, 2023, the contents of which are incorporated herein by reference.
[0002] In recent years, electronics technology has made remarkable advances, with efforts being made to make portable electronic devices smaller, lighter, thinner, and more multifunctional. Accordingly, there is a strong demand for batteries, which serve as the power source for electronic devices, to be smaller, lighter, thinner, and more reliable.
[0003] In commonly used lithium-ion secondary batteries, electrolytes (electrolytic solutions) such as organic solvents have traditionally been used as a medium for ion migration. However, lithium-ion secondary batteries using electrolytic solutions have the risk of electrolyte leakage. Furthermore, since organic solvents and the like used in electrolytic solutions are flammable substances, there is a demand for safer energy storage devices.
[0004] In order to improve the safety of the energy storage element, attention has been focused on all-solid-state batteries that include a solid electrolyte instead of an electrolytic solution and that also have other solid components (for example, Patent Documents 1 and 2).
[0005] The all-solid-state batteries described in Patent Documents 1 and 2 include a laminate in which positive electrode layers each including a positive electrode active material layer and a positive electrode current collector, and negative electrode layers each including a negative electrode active material layer and a negative electrode current collector are alternately stacked with a solid electrolyte layer interposed therebetween, and a pair of external electrodes that are in contact with the side surfaces of the laminate and are arranged to face each other.
[0006] In an all-solid-state battery, there is a concern that peeling of electrode layers such as a positive electrode layer and a negative electrode layer may result in a deterioration in cycle characteristics. Specifically, in an all-solid-state battery, a positive electrode current collector and a negative electrode current collector are connected to a positive electrode external terminal and a negative electrode external terminal, respectively, and there is a concern that peeling of the positive electrode current collector from the positive electrode external terminal or peeling of the negative electrode current collector from the negative electrode external terminal due to expansion and contraction during charge and discharge may result in a deterioration in cycle characteristics.
[0007] In the all-solid-state battery of Patent Document 2, in order to prevent the positive electrode current collector and the negative electrode current collector from peeling off from the external terminals, it is proposed to increase the thickness of the portions of the positive electrode current collector and the negative electrode current collector that are bonded to the external terminals, and to increase the area of the regions where the positive electrode current collector and the negative electrode current collector are bonded to the external terminals.
[0008] JP 2021-108258 A International Publication No. 2020 / 105662
[0009] However, the all-solid-state batteries disclosed in Patent Documents 1 and 2 were unable to sufficiently prevent short circuits caused by expansion and contraction of the electrode layer during charge and discharge. Furthermore, the all-solid-state battery of Patent Document 2 was also concerned about short circuits caused by cracks propagating from an electrode layer to an adjacent electrode layer, resulting in a deterioration in cycle performance. Thus, it is considered desirable to prevent cracks from propagating from an electrode layer to an adjacent electrode layer.
[0010] The present invention has been made in view of the above circumstances, and aims to provide an all-solid-state battery that can suppress the occurrence of cracks that propagate from an electrode layer of the all-solid-state battery to an electrode layer adjacent to the electrode layer due to expansion and contraction during charge and discharge, and can obtain excellent cycle characteristics.
[0011] The inventors of the present invention have discovered that in a laminate of an all-solid-state battery, cracks tend to occur or propagate from the tip of an electrode layer toward an electrode layer adjacent to the electrode layer in the stacking direction and having a different polarity. They have also discovered that cracks tend to occur or propagate particularly from the tip of the negative electrode when an alloy-based material that exhibits large expansion and contraction during charge and discharge is used for the negative electrode. Even when such an alloy-based material that exhibits large expansion and contraction during charge and discharge is used for the negative electrode, it is desirable to suppress the occurrence of cracks propagating from an electrode layer to an electrode layer adjacent to the electrode layer. That is, the present inventors provide the following means to solve the above problem.
[0012] (1) An all-solid-state battery according to one aspect of the present invention includes a cathode layer, an anode layer, and a solid electrolyte layer, wherein the solid electrolyte layer is disposed between the cathode layer and the anode layer. The battery also includes: a cathode external terminal joined to the cathode layer at a first end surface of the laminate; and a cathode external terminal joined to the anode layer at a second end surface of the laminate opposite to the first end surface. The laminate further includes a porous body provided in either a first region sandwiched between the cathode layer and the second end surface or a second region sandwiched between the anode layer and the first end surface.
[0013] (2) In the all-solid-state battery of (1), the porosity of the porous body may be 20% or more and 99% or less.
[0014] (3) In the all-solid-state battery of (1) or (2) above, the porous body may have communicating holes formed in a direction intersecting the first end surface and the second end surface.
[0015] (4) The all-solid-state batteries according to (1) to (3) above may have the porous body in the second region.
[0016] (5) The all-solid-state batteries according to (1) to (4) above may have the porous body in the first region.
[0017] (6) In the all-solid-state batteries described in (1) to (5), the average diameter of the voids may be 0.1 μm or more and 10 μm or less.
[0018] (7) In the all-solid-state batteries described in (1) to (6) above, the porous body may be made of a solid electrolyte.
[0019] (8) The all-solid-state batteries according to (1) to (7) above may have the porous body in the first region and the second region.
[0020] According to the present invention, it is possible to provide an all-solid-state battery that can suppress the occurrence of cracks that propagate from an electrode layer of the all-solid-state battery to an electrode layer adjacent to the electrode layer due to expansion and contraction during charge and discharge, and that can obtain excellent cycle characteristics.
[0021] Fig. 1 is a cross-sectional view showing an example of the configuration of an all-solid-state battery according to an embodiment of the present invention. Fig. 2 is a cross-sectional view showing the configuration of an all-solid-state battery according to a modified example of Fig. 1. Fig. 3 is a cross-sectional view showing the configuration of an all-solid-state battery according to a modified example of Fig. 1.
[0022] Hereinafter, the embodiments will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may show characteristic portions enlarged for convenience in order to make the features easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate changes can be made within the scope of the effects of the present invention.
[0023] [All-Solid-State Battery] Fig. 1 is a cross-sectional view showing an example of the configuration of an all-solid-state battery according to one embodiment of the present invention. The all-solid-state battery 100A shown in Fig. 1 includes a cathode layer 1, an anode layer 2, and a solid electrolyte layer 3. The solid electrolyte layer 3 is disposed between the cathode layer 1 and the anode layer 2. The all-solid-state battery 100A includes a laminate 50A, a cathode external terminal 5 joined to the cathode layer 1 at a first end surface S1 of the laminate 50A, and a negative electrode external terminal 6 joined to the anode layer 2 at a second end surface S2 of the laminate 50A opposite to the first end surface S1. The laminate 50A further includes a porous body 10 provided in either a first region sandwiched between the cathode layer 1 and the second end surface S2 or a second region sandwiched between the anode layer 2 and the first end surface S1.
[0024] In this embodiment, the stacking direction of the positive electrode layer 1 and the negative electrode layer 2 in the laminate 50A shown in Fig. 1 is defined as the z direction, the direction perpendicular to the z direction and in which the positive electrode layer 1 and the negative electrode layer 2 extend in Fig. 1 is defined as the x direction, and the direction perpendicular to the x direction and the z direction is defined as the y direction. A positive electrode external terminal 5 and a negative electrode external terminal 6, which will be described in detail later, are formed to be spaced apart in the x direction.
[0025] [Laminate] The laminate 50A includes at least one positive electrode layer 1 and one negative electrode layer 2. The positive electrode layers 1 and the negative electrode layers 2 are alternately arranged with the solid electrolyte layer 3 interposed therebetween.
[0026] The laminate 50A is a substantially hexahedron having an upper surface and a lower surface, which are end surfaces in the stacking direction, and four side surfaces that are perpendicular to the upper and lower surfaces and parallel to the stacking direction. Of the four side surfaces, the side surface that is bonded to the positive electrode layer 1 is referred to as the first end surface S1, and the side surface that is bonded to the negative electrode layer 2 is referred to as the second end surface S2. In the laminate 50A, the first end surface S1 and the second end surface S2 are end surfaces of the laminate 50A in the x direction and are arranged opposite each other. In the laminate 50A, the distance between adjacent electrode layers is smaller than the distance from the positive electrode layer 1 to the second end surface S2 and the distance from the negative electrode layer 2 to the first end surface S1.
[0027] <Positive Electrode Layer> The positive electrode layer 1 includes a positive electrode current collector 1A and a positive electrode active material layer 1B. In the example shown in FIG. 1 , the positive electrode active material layer 1B is provided on at least one of the main surfaces of the positive electrode current collector 1A, and may be provided on both main surfaces. The positive electrode layer end portion E1 is formed on the surface of the positive electrode current collector 1A and the positive electrode active material layer 1B opposite to the first end surface S1. The positive electrode layer end portion E1 is not joined to the positive electrode external terminal 5, and is provided at a position closer to the negative electrode external terminal 6 than to the positive electrode external terminal 5.
[0028] The positive electrode current collector 1A is made of a highly conductive material, such as a metal or alloy containing at least one of silver (Ag), palladium (Pd), gold (Au), platinum (Pt), aluminum (Al), copper (Cu), and nickel (Ni), or carbon (C).
[0029] The positive electrode current collector 1A may be a foil or may be made of a plurality of conductive particles that are connected to each other and arranged in the xy plane so as to be electrically connected.
[0030] (Positive Electrode Active Material Layer) The positive electrode active material layer 1B contains, as a positive electrode active material, a compound capable of absorbing and releasing at least lithium ions. The positive electrode active material layer 1B may also contain a conductive additive or an ion-conducting additive. It is preferable that the positive electrode active material be capable of efficiently inserting and desorbing lithium ions.
[0031] Such a positive electrode active material is, for example, a transition metal oxide or a transition metal composite oxide. 2 Mn a Ma 1-a O 3 (0.8≦a≦1, Ma=Co, Ni), lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMn) having a spinel structure 2 O 4 ), general formula: LiNi x Co y Mn z O 2 a composite metal oxide represented by (x+y+z=1, 0≦x≦1, 0≦y≦1, 0≦z≦1), a lithium vanadium compound (LiV 2 O 5 ), olivine-type LiMbPO 4 (wherein Mb is one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, and Zr), lithium vanadium phosphate (Li 3 V 2 (P.O. 4 ) 3 or LiVOPO 4 ), Li 2 MnO 3 -LiMcO 2 Lithium-excess solid solution cathode represented by (Mc=Mn, Co, Ni), lithium titanate (Li 4 Ti 5 O 12 ), titanium oxide (TiO 2 ), Li s Ni t Co u Al v O 2 (0.9<s<1.3, 0.9<t+u+v<1.1), and the like.
[0032] Furthermore, in these positive electrode active materials, some of the elements may be substituted with different elements, and the composition may be changed from the stoichiometric composition.
[0033] Examples of the conductive additive include carbon materials such as carbon black, acetylene black, ketjen black, carbon nanotubes, graphite, graphene, and activated carbon, and metal materials such as gold, silver, palladium, platinum, copper, and tin.
[0034] The ion-conducting aid is, for example, a solid electrolyte. For the solid electrolyte, for example, the same material as that used for the solid electrolyte layer 3 can be used.
[0035] <Negative Electrode Layer> The negative electrode layer 2 includes a negative electrode current collector 2 A and a negative electrode active material layer 2 B. In the example shown in Fig. 1, the negative electrode active material layer 2 B is provided on at least one of the main surfaces of the negative electrode current collector 2 A.
[0036] (Negative electrode current collector) The negative electrode current collector 2A is made of, for example, a metal or alloy containing at least one metal element selected from silver (Ag), palladium (Pd), gold (Au), platinum (Pt), aluminum (Al), copper (Cu), and nickel (Ni), or a non-metal such as carbon (C).
[0037] The negative electrode current collector 2A may be a foil or may be made of a plurality of conductive particles, which are, for example, connected to each other and electrically connected in the xy plane.
[0038] (Negative Electrode Active Material Layer) The negative electrode active material layer 2B is formed, for example, on one or both surfaces of the negative electrode current collector 2A. The negative electrode active material layer 2B contains a negative electrode active material. The negative electrode active material layer 2B may contain a conductive additive and a solid electrolyte. When the negative electrode active material layer 2B contains a solid electrolyte, the space between an xy plane passing through the outermost portion of the negative electrode active material and the boundary surface with the negative electrode current collector 2A is considered to be the negative electrode active material layer 2B.
[0039] The negative electrode active material is a compound capable of absorbing and releasing ions. The negative electrode active material is a compound exhibiting a more base potential than the positive electrode active material. Materials similar to those exemplified as the materials for the positive electrode active material above, but exhibiting a more base potential than the positive electrode active material, can be used as the negative electrode active material. Thus, the negative electrode active material and the positive electrode active material used in the all-solid-state battery 100A are determined taking into consideration the potentials of the negative electrode active material and the positive electrode active material. Examples of the negative electrode active material include carbon materials, metals, alloys, or composite materials capable of combining with lithium, oxides, and metallic lithium. More specific examples include natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, fired organic compounds, Ag, Li, silicon, tin, zinc, lead, antimony, Si, Sn, aluminum, and alloys of these metals such as AgPd, and lithium titanate (Li 4 Ti 5 O 12 , LiTiO 2 , Li 2 TiO 3 ), Li 2 TiSiO 5 , Li 3 V 2 (P.O. 4 ) 3 , SiO x , SnO 2 , is.
[0040] The conductive additive improves the electronic conductivity of the negative electrode active material layer 2 B. As the conductive additive, the same materials as those used for the positive electrode active material layer 1 B can be used.
[0041] <Solid Electrolyte Layer> The solid electrolyte layer 3 includes a solid electrolyte. A solid electrolyte is a substance that can move ions by an externally applied electric field. For example, the solid electrolyte layer 3 conducts lithium ions and inhibits the movement of electrons. The solid electrolyte layer 3 is, for example, a sintered body obtained by sintering.
[0042] The solid electrolyte layer 3 is, for example, γ-Li 3 P.O. 4 The solid electrolyte includes a solid electrolyte having a crystalline structure of LiSiC type (LiSiC type) and a solid electrolyte having a crystalline structure of NaSiC type.3+x Si x P 1-x O 4 (LSPO, 0.4≦x≦0.8), Li 3+x Si x V 1-x O 4 (LSVO, 0.4≦x≦0.8), Li 3+x Ge x P 1-x O 4 (LGPO, 0.4≦x≦0.8), Li 3+x Ge x V 1-x O 4 (LGVO, 0.4≦x≦0.8) and other crystalline structures of lysicone type, LiTi 2 (P.O. 4 ) 3 (LTP), LiZr 2 (P.O. 4 ) 3 (LZP), Li 1+x A l x Ti 2-x (P.O. 4 ) 3 (LATP, 0<x≦0.6)), Li 1+x Al x Ge 2-x (P.O. 4 ) 3 (LAGP, 0<x≦0.6), Li 1+x Y x Zr 2-x (P.O. 4 ) 3 (LYZP, 0<x≦0.6) or the like. 0.5 Li 0.5 TiO 3 Perovskite compounds such as Li 14 Zn(GeO 4 ) 4 Lithium-type compounds such as Li 7 La 3 Zr 2 O 12 Garnet-type compounds such as Li 3.25 Ge 0.25 P 0.75 S 4 and Li 3 P.S.4 Thiolisicon-type compounds such as Li 2 S-P 2 S 5 and Li 2 O-V 2 O 5 -SiO 2 Glass compounds such as Li 3 P.O. 4 and Li 3.5 Si 0.5 P 0.5 O 4 and Li 2.9 P.O. 3.3 N 0.46 and the like.
[0043] The oxide-based solid electrolyte described above is harder than the sulfide-based solid electrolyte and is less likely to deform under pressure. Therefore, it is thought that cracks are more likely to occur due to expansion and contraction during charging and discharging of the battery. However, in this embodiment, as will be described in detail later, a porous body is formed at a predetermined position, thereby suppressing the occurrence of cracks that propagate from an electrode layer to an adjacent electrode layer. This makes it possible to provide an all-solid-state battery with excellent cycle characteristics that is less likely to cause short circuits even after repeated use.
[0044] <Porous Body> A porous body 10 is provided in either the first region R1 sandwiched between the positive electrode layer 1 and the second end face S2, or the second region R2 sandwiched between the negative electrode layer 2 and the first end face S1. Voids 20A are formed in the porous body 10. In the porous body 10, the voids 20A are distributed in the x direction from the interface with the electrode layer to the first end face S1 and the second end face S2.
[0045] 1 shows an example in which the porous body 10 is formed in all of the first region R1 and the second region R2, but the porous body 10 may be formed in only one of the first region R1 and the second region R2. Furthermore, it is sufficient that the porous body 10 is formed in at least one of the plurality of first regions R1, or the porous body 10 is formed in at least one of the plurality of second regions R2.
[0046] The ratio of the number of regions in which the porous body 10 is formed among the plurality of first regions R1 is referred to as the formation rate of the first regions R1. The formation rate of the first regions R1 is preferably 50% or more, and more preferably 80% or more. The ratio of the number of regions in which the porous body 10 is formed among the plurality of second regions R2 is referred to as the formation rate of the second regions. The formation rate of the second regions R2 is preferably 50% or more, and more preferably 80% or more.
[0047] The porosity of the porous body 10 is, for example, 20% or more, preferably more than 20% and 99% or less, more preferably 30% or more and 98% or less, and particularly preferably 50% or more and 95% or less.
[0048] The porosity of the porous body 10 is calculated from a cross-sectional SEM image. Specifically, it is calculated as the ratio of the area of voids to the area of a region between the electrode layer and the external electrode terminal, with the same thickness as the electrode layer adjacent to the porous body 10. In calculating the void area ratio, the cross-sectional SEM image is binarized by brightness to separate the voids and the solid electrolyte, allowing the ratio to be calculated accurately.
[0049] The material constituting the porous body 10 preferably contains the same material as that of the solid electrolyte layer 3. Therefore, the porous body 10 preferably uses a lithium ion conductor such as LSPO.
[0050] The porous body 10 is a structure in which voids are formed in a solid electrolyte. The average diameter of the voids formed in the porous body 10 is, for example, 0.1 μm or more and 20 μm or less, preferably 1 μm or more and 10 μm or less, and more preferably 1 μm or more and 5 μm or less. The diameter of the voids formed in the porous body 10 is calculated by image analysis of a cross-sectional SEM photograph and further converting it into a three-dimensional pore diameter. The average diameter is calculated as the average of the diameters of the voids.
[0051] The all-solid-state battery 100A according to this embodiment further includes a porous body 10 provided in either the first region R1, where the laminate 50A is sandwiched between the positive electrode layer 1 and the second end surface S2, or the second region R2, where the laminate 50A is sandwiched between the negative electrode layer 2 and the first end surface S1. According to the all-solid-state battery 100A according to this embodiment, the above-described configuration relieves stress in other regions during the charge / discharge process between an electrode layer and an external electrode terminal of a different polarity from the electrode layer, which is located at a greater distance than the distance between adjacent electrode layers. This suppresses cracks from forming from the end (tip) of the electrode layer toward the adjacent electrode layer of a different polarity during the charge / discharge process, thereby suppressing the occurrence of short circuits due to the cracks. Therefore, according to the present invention, an all-solid-state battery with excellent cycle characteristics can be obtained.
[0052] FIG. 2 is a cross-sectional view showing the configuration of an all-solid-state battery according to a modified example of FIG. 1 . The all-solid-state battery 100B shown in FIG. 2 differs from the all-solid-state battery 100A in the anode layer. In this modified example, components similar to those in the all-solid-state battery 100A of FIG. 1 are designated by the same reference numerals and will not be described again. In the all-solid-state battery 100B, the anode layer 2X serves as both an anode current collector and an anode active material layer. The anode layer 2X exhibits a lower potential than the cathode active material. The anode layer 2X preferably contains a metal selected from the group consisting of silver (Ag), palladium (Pd), gold (Au), and platinum (Pt). This is because Ag, Pd, Au, and Pt do not melt and are resistant to oxidation even when the sintering process for producing the laminate 50B is performed in an air atmosphere. The anode layer 2X may be made of any of the above metals or an alloy containing any of the above metals.
[0053] The negative electrode layer 2X preferably contains an AgPd alloy. Furthermore, the negative electrode layer 2X preferably contains an AgPd alloy, because this results in a solid-state battery with high energy density. For example, the AgPd alloy may contain Ag and Pd in a molar ratio of 8:2 (Ag:Pd).
[0054] The negative electrode layer 2X may contain metal particles made of any of the above metals and / or alloy particles made of an alloy containing any of the above metals, and one or more selected from a conductive additive and a solid electrolyte.
[0055] FIG. 3 is a cross-sectional view showing the configuration of an all-solid-state battery according to a modified example of FIG. 1 . In the laminate 50C of the all-solid-state battery 100C shown in FIG. 3 , a porous body 12 is formed in the first region R1 and the second region R2. The porous body 12 has a communication hole 20B that connects multiple voids adjacent in the x direction. That is, the communication hole 20B is formed so as to extend in a direction intersecting the yz plane, for example, in a direction perpendicular to the yz plane. FIG. 3 is a cross-sectional view of one cross section of the all-solid-state battery 100C, and additional voids that are not connected to the communication hole 20B may be provided in regions not shown. Furthermore, multiple communication holes may be provided within the porous body 12. The porous body 12 is preferably formed between the negative electrode layer 2 and the positive electrode external terminal 5.
[0056] In the porous body 12, it is preferable that the voids closest to the electrode layers and the voids closest to the external electrode terminals are connected in a cross-sectional view. That is, it is preferable that the porous body 12 is connected in the x direction from the voids closest to the electrode layers to the voids closest to the external electrode terminals. By having voids connected in the x direction in the porous body 12, it is possible to obtain the effect of preventing cracks from occurring between the voids, suppressing the occurrence of short circuits caused by cracks propagating from an electrode layer to an adjacent electrode layer, and obtaining even better cycle characteristics.
[0057] 1, 2, and 3 show examples in which the porous bodies 10, 12 are provided in all of the first regions R1 and second regions R2, each having a void 20A or a through hole 20B connecting a plurality of voids. Preferably, the porous bodies 10, 12 are provided in all of the first regions R1 and second regions R2, as shown in Fig. 1 and 3. However, it is sufficient that the porous bodies 10, 12 are formed in either the first region R1 or the second region R2 of the all-solid-state batteries 100A, 100C, or the porous bodies 10, 12 may be formed in either the first region R1 or the second region R2.
[0058] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is an example, and additions, omissions, substitutions, and other modifications of the configurations are possible within the scope that does not deviate from the spirit of the present invention.
[0059] The upper and / or lower limits of the numerical ranges described herein can be arbitrarily combined to define a preferred range. For example, the upper and lower limits of the numerical ranges can be arbitrarily combined to define a preferred range, the upper limits of the numerical ranges can be arbitrarily combined to define a preferred range, and the lower limits of the numerical ranges can be arbitrarily combined to define a preferred range.
[0060] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0061] [Example 1] (Preparation of paste for positive electrode active material layer) LCO (LiCoO 2 100 parts of the powder, 15 parts of ethyl cellulose as a binder, and 65 parts of dihydroterpineol as a solvent were mixed and dispersed to prepare a paste for a positive electrode active material layer.
[0062] (Preparation of Positive Electrode Current Collector Paste) AgPd (Ag:Pd molar ratio of 8:2) and LCO were mixed to a volume ratio of 70 / 30, and then 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent were added to 100 parts of the mixed powder, and the mixture was mixed and dispersed to prepare a positive electrode current collector paste.
[0063] (Preparation of Paste for Solid Electrolyte Layer) Li 2 CO 3 and SiO 2 and Li 3 P.O. 4 These were used as starting materials and mixed in a molar ratio of 2:1:1. The mixture was wet mixed for 16 hours using a ball mill with water as a dispersion medium. The mixture was calcined at 950°C for 2 hours to obtain Li 3.5 Si 0.5 P 0.5 O 4 Then, 100 parts of this calcined powder, 100 parts of ethanol, and 200 parts of toluene were added to a ball mill and wet mixed. Then, 16 parts of a polyvinyl butyral binder and 4.8 parts of benzyl butyl phthalate were further added and mixed to prepare a paste for a solid electrolyte layer.
[0064] (Preparation of Solid Electrolyte Sheet) A solid electrolyte sheet having a thickness of 15 μm was prepared by forming a sheet on a PET film using the paste for a solid electrolyte layer by a doctor blade method.
[0065] (Preparation of Negative Electrode Layer Paste) In Example 1, the negative electrode layer served as both a negative electrode current collector and a negative electrode active material layer. A negative electrode layer paste was prepared by mixing and dispersing 100 parts of AgPd powder as a negative electrode current collector and negative electrode active material, 15 parts of ethyl cellulose as a binder, and 65 parts of dihydroterpineol as a solvent.
[0066] (Preparation of Porous Body Paste) The following porous body paste was prepared to form a porous body.
[0067] The paste for the porous body was prepared using the same method as that used for the solid electrolyte layer. 3.5 Si 0.5 P 0.5 O 4 ) powder and spherical acrylic resin powder with a particle diameter of 3 μm were mixed in a volume ratio of 20:80, and 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent were added to 100 parts of the LSPO powder, and the mixture was mixed and dispersed. In the firing step described below, the acrylic resin was thermally decomposed during firing, forming voids in the decomposed areas.
[0068] (Preparation of External Electrode Paste) Silver powder, a thermosetting resin, and a solvent were mixed and dispersed to prepare a thermosetting external electrode paste.
[0069] (Preparation of Positive Electrode Layer Unit) A positive electrode active material layer paste was formed on a solid electrolyte sheet by screen printing to a thickness of 10 μm and dried at 80°C for 10 minutes to form a positive electrode active material layer (hereinafter referred to as a first positive electrode active material layer). Next, a positive electrode current collector paste was formed on the positive electrode active material layer by screen printing to a thickness of 10 μm and dried at 80°C for 10 minutes to form a positive electrode current collector. Next, a positive electrode active material layer paste was formed on the positive electrode current collector by screen printing to a thickness of 10 μm and dried at 80°C for 10 minutes to form another positive electrode active material layer (hereinafter referred to as a second positive electrode active material layer). In this way, a 30 μm thick positive electrode layer was formed on the solid electrolyte sheet, in which the first positive electrode active material layer, the positive electrode current collector, and the second positive electrode active material layer were stacked in this order.
[0070] Next, a paste for a porous body was formed by screen printing on the outer periphery of one end of the positive electrode layer (the surface opposite to the surface to be later joined to the positive electrode external terminal), and dried for 10 minutes at 80° C. The paste for a porous body was formed to a thickness such that its surface was flush with the surface of the active material layer.
[0071] Next, the PET film was peeled off to produce a positive electrode layer unit in which a formation formed by drying the paste for porous body was formed on the positive electrode layer and on the outer periphery of the positive electrode layer in contact with the first end face of the positive electrode layer.
[0072] (Fabrication of Negative Electrode Layer Unit) The negative electrode layer unit was fabricated in the same manner as the positive electrode layer unit, that is, in the following procedure.
[0073] First, the paste for the negative electrode layer was applied to a solid electrolyte sheet by screen printing to form a layer having a thickness of 10 μm, and then dried at 80° C. for 10 minutes to form a negative electrode layer having a thickness of 10 μm.
[0074] Next, a paste for a porous body was formed by screen printing on the outer periphery of one end of the negative electrode layer (the surface opposite to the surface to be later joined to the external positive electrode terminal), and dried for 10 minutes at 80° C. The paste for a porous body was formed so that its surface was flush with the surface of the active material layer.
[0075] Next, the PET film was peeled off to produce a negative electrode layer unit, in which a laminate was formed on the negative electrode layer and the outer periphery of the negative electrode layer, in contact with the second end face of the negative electrode layer and in which the paste for porous body was dried.
[0076] Ten positive electrode layer units and ten negative electrode layer units were prepared and stacked in the order of the positive electrode layer units and the negative electrode layer units, with their ends alternately offset so as not to coincide with each other. Furthermore, a plurality of solid electrolyte sheets were stacked on the outer side of the electrode layer unit serving as the outermost layer in the stacking direction, to provide an outer layer having a thickness of 100 μm.
[0077] This was thermocompressed using a mold press and then cut to produce an unfired all-solid-state battery laminate. The laminate size was 5 mm and 4 mm in the x and y directions, respectively. Next, the unfired laminate was debindered and fired to produce an all-solid-state battery laminate. The laminate was heat-treated at 500°C for 10 hours in an air atmosphere to perform a binder removal treatment on the laminate. Firing was performed at 900°C for 1 hour in an air atmosphere.
[0078] (External Electrode Forming Step) An external electrode paste was applied to the end faces (first end face and second end face) of the fired all-solid-state battery laminate, and thermal curing was performed at 150°C for 30 minutes to form a pair of external electrodes, thereby producing an all-solid-state battery.
[0079] [Example 2] An all-solid-state battery was produced in the same manner as in Example 1, except that the volume ratio of the solid electrolyte powder to the acrylic resin in the paste for the porous body formed on the outer periphery of one end of the positive electrode layer unit and the negative electrode layer unit was adjusted to 5:95, and the porosity of the porous body formed in the laminate was increased.
[0080] [Examples 3, 4, and 5] All-solid-state batteries were produced in the same manner as in Example 1, except that the volume ratio of the solid electrolyte powder and the acrylic resin in the porous body paste formed on the outer periphery of one end of the positive electrode layer unit and the negative electrode layer unit was adjusted, and the porosity of the porous body formed in the laminate was adjusted.
[0081] [Examples 6, 7, and 8] All-solid-state batteries were fabricated in the same manner as in Example 1, except that the average pore size in the porous body was adjusted by adjusting the particle size of the acrylic resin powder mixed in the porous body paste.
[0082] Example 9 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the negative electrode active material was changed to Ag.
[0083] [Example 10] The negative electrode layer was changed to have a configuration including a negative electrode current collector and a negative electrode active material layer, and the negative electrode active material was changed to LTO (Li 4 Ti 5 O 12 An all-solid-state battery was fabricated in the same manner as in Example 9, except that the negative electrode layer was changed to AgPd, and AgPd was used as the negative electrode current collector. In Example 10, the negative electrode layer was fabricated by the following procedure.
[0084] (Preparation of negative electrode active material paste) LTO (Li 4 Ti 5 O 12 100 parts of the powder, 15 parts of ethyl cellulose as a binder, and 65 parts of dihydroterpineol as a solvent were mixed and dispersed to prepare a paste for a positive electrode active material layer.
[0085] (Preparation of a paste for a negative electrode current collector) AgPd and LTO were mixed to a volume ratio of 70 / 30, and then 100 parts of the mixed powder were mixed with 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent, followed by mixing and dispersing to prepare a paste for a negative electrode current collector.
[0086] First, a negative electrode active material paste was formed on a solid electrolyte sheet by screen printing to a thickness of 10 μm and dried at 80° C. for 10 minutes to form a negative electrode active material layer (hereinafter referred to as the first negative electrode active material layer). Next, a negative electrode current collector paste was formed on the negative electrode active material layer by screen printing to a thickness of 10 μm and dried at 80° C. for 10 minutes to form a negative electrode current collector. Next, a negative electrode active material layer paste was formed on the negative electrode current collector by screen printing to a thickness of 10 μm and dried at 80° C. for 10 minutes to form another negative electrode active material layer (hereinafter referred to as the second negative electrode active material layer). In this way, a 30 μm thick negative electrode layer was formed on the solid electrolyte sheet, in which the first negative electrode active material layer, the negative electrode current collector, and the second negative electrode active material layer were stacked in this order.
[0087] [Example 11] A negative electrode active material was LVP (Li 3 V 2 (P.O. 4 ) 3 An all-solid-state battery was produced in the same manner as in Example 9, except that the above-mentioned method was changed to the above-mentioned method.
[0088] [Example 12] The positive electrode active material was LTO (Li 4 Ti 5 O 12 An all-solid-state battery was produced in the same manner as in Example 1, except that the above-mentioned method was changed to the above-mentioned method.
[0089] [Example 13] The solid electrolyte was LATP (Li 1.4 Al 0.4 Ti 1.6 (P.O. 4 ) 3 An all-solid-state battery was produced in the same manner as in Example 1, except that the above-mentioned method was changed to the above-mentioned method.
[0090] [Example 14] The solid electrolyte was LZP (LiZr 2 (P.O. 4 ) 3 An all-solid-state battery was produced in the same manner as in Example 1, except that the above-mentioned method was changed to the above-mentioned method.
[0091] Example 15 differs from Example 1 in that no porous body was formed in the second region. In Example 15, a margin paste was prepared by adding 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent to 100 parts of LSPO powder prepared using the same method as that used for the solid electrolyte layer, and mixing and dispersing the mixture. Next, an all-solid-state battery was prepared in the same manner as Example 1, except that the entire second region located between the negative electrode layer and the positive electrode external terminal was coated with a margin paste without using a porous body paste, thereby forming a margin region without forming a porous body. That is, in Example 15, the porous body formation rate in the second region was 0%.
[0092] [Example 16] An all-solid-state battery was produced in the same manner as in Example 1, except that, of the ten second regions located between the negative electrode layer and the positive electrode external terminal, five second regions were formed as margin regions without forming a porous body by applying the same margin paste as in Example 15 without using the paste for porous body. That is, in Example 16, the formation rate of the porous body in the second regions was set to 50%.
[0093] [Example 17] An all-solid-state battery was produced in the same manner as in Example 1, except that the entire first region located between the positive electrode layer and the negative electrode external terminal was coated with the same margin paste as in Example 15 without using a paste for porous body, thereby forming a margin region without forming a porous body. That is, in Example 17, the formation rate of the porous body in the first region was set to 0%.
[0094] [Example 18] An all-solid-state battery was produced in the same manner as in Example 1, except that, of the ten first regions located between the positive electrode layer and the negative electrode external terminal, five first regions were formed as margin regions without forming a porous body by applying the same margin paste as in Example 15 without using the paste for porous body. That is, in Example 18, the formation rate of the porous body in the first regions was set to 50%.
[0095] [Example 19] The powder in the margin paste of Example 15 was changed from LSPO to Al 2 O 3 That is, in Example 18, the porous body was changed to Al.2 O 3 The structure is as follows.
[0096] [Example 20] A porous body paste and a pore-forming material paste were prepared, and an all-solid-state battery having a porous body with communicating pores was produced. The same porous body paste as in Example 1 was used. The pore-forming material paste was prepared by adding 100 parts of acrylic resin powder with a particle diameter of 200 nm, 10 parts of ethyl cellulose as a binder, and 50 parts of dihydroterpineol as a solvent, and mixing and dispersing them. A positive electrode layer was formed in the same manner as in Example 1, and then a porous body paste was formed to a thickness of 10 μm on the outer periphery of one end of the positive electrode layer (the surface opposite the surface that will later be joined to the positive electrode external terminal) by screen printing and dried at 80 ° C. for 10 minutes. Next, a pore-forming material paste was formed to a thickness of 10 μm on the dried porous body paste by screen printing and dried at 80 ° C. for 10 minutes.
[0097] Next, a porous body paste was formed on the dried pore-forming material paste by screen printing to a thickness of 10 μm and dried at 80 ° C. for 10 minutes to form a positive electrode layer unit. Furthermore, a negative electrode layer was formed in the same manner as in Example 1, and then a porous body paste was formed on the periphery of one end of the negative electrode layer (three side surfaces excluding the surface that will later be joined to the negative electrode external terminal) to a thickness of 3.3 μm by screen printing and dried at 80 ° C. for 10 minutes. Next, a pore-forming material paste was formed on the dried porous body paste by screen printing to a thickness of 3.3 μm and dried at 80 ° C. for 10 minutes. Next, a porous body paste was formed on the dried pore-forming material paste by screen printing to a thickness of 3.3 μm and dried at 80 ° C. for 10 minutes to form a negative electrode layer unit. Thereafter, an all-solid-state battery of Example 18 having a porous body having communicating pores was produced by producing it in the same manner as in Example 1.
[0098] [Example 21] An all-solid-state battery was fabricated in the same manner as in Example 1, except that the thickness of the negative electrode layer paste to be fabricated on the solid electrolyte sheet was changed to 1 μm. In Example 21, the porous body had a thickness equal to or greater than that of the negative electrode layer at the stage of fabricating the all-solid-state battery. In Example 21, by reducing the thickness of the negative electrode layer paste in this way, the portion of silver exceeding the allowable amount precipitates as metallic lithium during charge and discharge, functioning as the negative electrode.
[0099] [Examples 22 to 24] All-solid-state batteries were produced in the same manner as in Example 21, except that the volume ratio of the solid electrolyte powder and the acrylic resin in the porous body paste formed on the outer periphery of one end of the positive electrode layer unit and the negative electrode layer unit was adjusted, and the porosity of the porous body formed in the laminate was adjusted.
[0100] [Comparative Example 1] An all-solid-state battery was produced in the same manner as in Example 1, except that a margin paste was used in the region where the porous body paste had been used, and a solid electrolyte (LSPO) was filled in the region between the positive electrode layer and the negative electrode external terminal, and the region between the negative electrode layer and the positive electrode external terminal. That is, in Comparative Example 1, a porous body was not formed in the regions corresponding to the first region and the second region, and instead a layer composed of a solid electrolyte was formed.
[0101] Comparative Example 2 An all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that the negative electrode active material was changed from AgPd to Ag.
[0102] [Comparative Example 3] The negative electrode active material was changed from AgPd to LTO (Li 4 Ti 5 O 12 An all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that the negative electrode current collector was changed to AgPd.
[0103] [Comparative Example 4] The negative electrode active material was changed from AgPd to LVP (Li 3 V 2 (P.O. 4 ) 3 An all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that the negative electrode current collector was changed to AgPd.
[0104] Comparative Example 5: The positive electrode active material was changed from LCO to LTO (Li 4 Ti5 O 12 An all-solid-state battery was produced in the same manner as in Comparative Example 1, except that the above-mentioned material was changed to the above-mentioned material.
[0105] Comparative Example 6 The conditions were changed in the same manner as in Example 21 for Example 1. That is, an all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that the thickness of the negative electrode layer paste to be fabricated on the solid electrolyte sheet was changed to 1 μm.
[0106] Cross sections of the all-solid-state batteries of Examples 1 to 24 and Comparative Examples 1 to 6, which were parallel to the lamination direction and perpendicular to the electrode external terminals, were observed with an electron microscope, and the porous body formation rate, porosity, and average pore diameter were measured.
[0107] (Porous body formation rate) The ratio of the number of porous bodies sandwiched between the positive electrode layer and the negative electrode external terminal to the number (10) of first regions of the all-solid-state battery is referred to as the first region porous body formation rate. Similarly, the ratio of the number of porous bodies sandwiched between the negative electrode layer and the positive electrode external terminal to the number (10) of second regions of the all-solid-state battery is referred to as the second region porous body formation rate. For example, if porous bodies are formed in five of the ten first regions, this is referred to as 50%.
[0108] (Porosity) The porosity of the porous body 10 was calculated from a cross-sectional SEM image. To calculate the void area ratio, 10 cross-sectional SEM images of the porous body were acquired at a magnification of 2000 times. The porous body portion was then binarized based on brightness to separate the voids and the solid electrolyte. The void area ratio per unit volume of the porous body portion was then calculated to determine the porosity.
[0109] Next, the average pore size in the porous body was calculated as follows.
[0110] (Average pore diameter) First, the number and area of pores per unit area in the cross section of the porous body were calculated using a binarized SEM image of the porous body. For interconnected pores, the maximum diameter of the interconnected pores was measured. Next, the three-dimensional particle diameter of the pores was calculated using the Schwartz-Saltykov method described in Foundry Engineering, Vol. 1, pp. 7-13, 1998. The obtained three-dimensional particle diameters were averaged to obtain the average diameter of the pores (average pore diameter).
[0111] (Battery Evaluation) The charge / discharge cycle characteristics were evaluated under the charge / discharge conditions shown below for the all-solid-state batteries of Examples 1 to 24 and Comparative Examples 1 to 6. First, 1000 all-solid-state batteries corresponding to each Example and Comparative Example were prepared, and in an environment of 60° C., constant current charging (CC charging) was performed at a constant current of 10 μA until the battery voltage reached 3.9 V, and then discharge (CC discharging) at a constant current of 10 μA until the battery voltage reached 0 V. This process was defined as one cycle, and the short-circuit occurrence rate was calculated from the number of short-circuited all-solid-state batteries among the 1000 all-solid-state batteries after repeating this process 100 times.
[0112] The fabrication conditions and measurement results of the all-solid-state batteries of Examples 1 to 24 and Comparative Examples 1 to 6 are summarized in Tables 1 to 4. Tables 1 and 3 show the conditions before charge and discharge, and therefore AgPd is listed as the negative electrode layer in Examples 21 to 24 and Comparative Example 6. However, in these Examples and Comparative Examples, as described above, Li deposited during the charge and discharge process also functions as the negative electrode.
[0113]
[0114]
[0115]
[0116]
[0117] Tables 1 to 4 confirm that Examples 1 to 4 and Examples 6 to 24, in which a porous body was formed in at least one of the first and second regions, had a reduced short-circuit occurrence rate compared to Comparative Examples 1 to 6, in which a porous body was not formed in either the first or second region. Comparing Examples 2 to 5, it was confirmed that Examples 2 and 3, in which the porosity of the porous body was 50% or more, exhibited particularly excellent cycle characteristics. It was also confirmed that Example 5, in which the porosity of the porous body was low, exhibited excellent cycle characteristics compared to Comparative Example 1, in which the conditions other than the porous body were similar. Examples 15 and 16, in which the second region porous body formation rate was low, exhibited a lower short-circuit occurrence rate after 100 cycles compared to Examples 17 and 18, in which the first region porous body formation rate was low. These results demonstrate that forming a larger number of porous bodies in the first region R1 is more effective than forming a larger number of porous bodies in the second region R2 in order to improve cycle characteristics. Examples 21 to 24, which used Li as the negative electrode active material, had a lower incidence of short circuits than Comparative Examples 1 to 6, and were confirmed to be effective in improving cycle characteristics.
[0118] 1: positive electrode layer, 1A: positive electrode current collector, 1B: positive electrode active material layer, 2: negative electrode layer, 2A: negative electrode current collector, 2B: negative electrode active material layer, 3: solid electrolyte layer, 5: positive electrode external terminal, 6: negative electrode External terminal, 10, 12: porous body, 20A: void, 20B: communication hole, 50A, 50B: laminate, R1: first region, R2: second region, S1: first end surface, S2: second end surface
Claims
1. An all-solid-state battery comprising: a laminate having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer, the solid electrolyte layer being disposed between the positive electrode layer and the negative electrode layer; a positive electrode external terminal joined to the positive electrode layer at a first end surface of the laminate; and a negative electrode external terminal joined to the negative electrode layer at a second end surface of the laminate opposite to the first end surface, the laminate further comprising a porous body provided in either a first region sandwiched between the positive electrode layer and the second end surface, or a second region sandwiched between the negative electrode layer and the first end surface.
2. The all-solid-state battery according to claim 1, wherein the porosity of the porous body is 20% or more and 99% or less.
3. The all-solid-state battery according to claim 1, wherein the porous body has communicating holes formed in a direction intersecting the first end face and the second end face.
4. The all-solid-state battery according to claim 1 or 2, wherein the second region has the porous body.
5. The all-solid-state battery according to claim 1 or 2, wherein the porous body is present in the first region.
6. The all-solid-state battery according to claim 1 or 2, wherein the average diameter of the voids formed in the porous body is 0.1 or more and 20 or less.
7. The all-solid-state battery according to claim 1 or 2, wherein the porous body is made of a solid electrolyte.
8. The all-solid-state battery according to claim 1 or 2, comprising the porous body in the first region and the second region.
Citation Information
Patent Citations
solid-state batteries
JP2022120181A
All solid state secondary battery
WO2020184476A1