Photosensitive resin composition, photosensitive resin film, printed wiring board, and semiconductor package
The photosensitive resin composition, featuring a photopolymerizable compound and blocked isocyanate, addresses the inefficiencies in via formation and dielectric performance, enabling efficient high-density via formation and improved dielectric properties for printed wiring boards and semiconductor packages.
Patent Information
- Application Number
- PCT/JP2024/012289
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional methods for manufacturing printed wiring boards face inefficiencies in forming small-diameter vias due to the limitations of laser processing, and photosensitive resin compositions struggle to achieve both dielectric properties and developability, which are essential for high-density semiconductor packages.
A photosensitive resin composition containing a photopolymerizable compound with an ethylenically unsaturated group and an acidic substituent, a blocked isocyanate compound with a molecular weight of 3,000 or less, and other additives like a thermosetting resin and inorganic filler, which enables efficient via formation and dielectric performance.
The composition allows for the formation of small-diameter vias in high density and improves dielectric properties and developability, enhancing the manufacturing efficiency of printed wiring boards and semiconductor packages.
Smart Images

Figure JP2024012289_03102024_PF_FP_ABST
Abstract
Description
Photosensitive resin composition, photosensitive resin film, printed wiring board, and semiconductor package
[0001] The present embodiment relates to a photosensitive resin composition, a photosensitive resin film, a printed wiring board, and a semiconductor package.
[0002] In recent years, electronic devices have become smaller and more powerful, and printed wiring boards have become increasingly dense due to an increase in the number of circuit layers and finer wiring. In particular, the density of semiconductor package substrates, such as BGA (ball grid array) and CSP (chip size package), on which semiconductor chips are mounted, has increased significantly, and in addition to finer wiring, thinner insulating layers and smaller via diameters for interlayer connection are required.
[0003] A conventional method for manufacturing printed wiring boards is the build-up method (see, for example, Patent Document 1), in which an interlayer insulating layer and a conductor circuit layer are sequentially laminated. As wiring becomes finer, semi-additive processes, in which circuits are formed by plating, have become mainstream for printed wiring boards. Conventional semi-additive processes include, for example, (1) laminating a thermosetting resin film on a conductor circuit, and then curing the thermosetting resin film by heating to form an "interlayer insulating layer." (2) Next, vias for interlayer connection are formed by laser processing, followed by desmearing and roughening treatments such as alkaline permanganate treatment. (3) Subsequently, electroless copper plating is performed on the substrate, followed by pattern formation using a resist, followed by electrolytic copper plating to form a copper circuit layer. (4) Next, the resist is stripped, and the electroless plating layer is flash-etched to form a copper circuit.
[0004] As mentioned above, laser processing is the mainstream method for forming vias in interlayer insulating layers formed by curing thermosetting resin films, but the ability to reduce the diameter of vias using laser irradiation with a laser processing machine is reaching its limit. Furthermore, when forming vias using a laser processing machine, each via hole must be formed one by one, and when a large number of vias are required for high density, forming the vias takes a long time, resulting in poor manufacturing efficiency.
[0005] Under these circumstances, a method has been proposed as a method capable of forming a large number of vias at once, in which a photosensitive resin composition containing an acid-modified vinyl group-containing epoxy resin, a photopolymerizable compound, a photopolymerization initiator, an inorganic filler, and a silane compound, and in which the inorganic filler content is 10 to 80 mass %, is used to form a plurality of small diameter vias at once by photolithography (see, for example, Patent Document 2).
[0006] JP 7-304931 A JP 2017-116652 A
[0007] Meanwhile, with the trend toward faster signal speeds and larger capacities, substrate materials for printed wiring boards are required to have dielectric properties capable of reducing transmission loss of high-frequency signals (hereinafter, sometimes referred to as "high-frequency properties"). That is, low dielectric constant and low dielectric loss tangent are required. In photosensitive resin compositions, photosensitive resins having acidic substituents such as carboxyl groups are sometimes used from the viewpoint of photosensitivity. However, studies by the present inventors have revealed that it is difficult for photosensitive resin compositions containing such photosensitive resins to achieve both good dielectric properties and good developability.
[0008] In view of the current situation, an object of the present embodiment is to provide a photosensitive resin composition that can achieve both dielectric properties and developability, and a photosensitive resin film, a printed wiring board, and a semiconductor package that use the photosensitive resin composition.
[0009] The present inventors have conducted extensive research to solve the above-mentioned problems and have found that the present embodiment can solve the above-mentioned problems. Specifically, the present embodiment relates to the following items [1] to
[15] . [1] A photosensitive resin composition containing (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, and (B) a blocked isocyanate compound having a molecular weight of 3,000 or less. [2] The photosensitive resin composition according to item [1] above, in which the dissociation temperature of component (B) is 80 to 250°C. [3] The photosensitive resin composition according to item [1] or [2] above, in which component (B) is a compound containing an isocyanurate ring. [4] The photosensitive resin composition according to item [3] above, in which component (B) is a compound obtained by blocking a trifunctional isocyanate compound containing an isocyanurate ring with a blocking agent. [5] The photosensitive resin composition according to any one of [1] to [4] above, wherein the content of the component (B) is 1 to 40 mass % based on the total amount of the resin components. [6] The photosensitive resin composition according to any one of [1] to [5] above, wherein the component (A) contains an alicyclic skeleton represented by the following general formula (A-1): (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1is an integer of 0 to 6. * is a bonding site to another structure.) [7] The photosensitive resin composition according to any one of [1] to [6] above, further comprising (C) a thermosetting resin. [8] The photosensitive resin composition according to any one of [1] to [7] above, further comprising (D) a photopolymerization initiator. [9] The photosensitive resin composition according to any one of [1] to [8] above, further comprising (E) a crosslinking agent.
[10] The photosensitive resin composition according to any one of [1] to [9] above, further comprising (F) an elastomer.
[11] The photosensitive resin composition according to any one of [1] to
[10] above, further comprising (G) an inorganic filler.
[12] The photosensitive resin composition according to any one of [1] to
[11] above, which is used for forming photovias.
[13] A photosensitive resin film comprising the photosensitive resin composition according to any one of [1] to
[12] above.
[14] A printed wiring board comprising a cured product of the photosensitive resin composition according to any one of [1] to
[12] above.
[15] A semiconductor package comprising the printed wiring board according to
[14] above and a semiconductor element.
[0010] According to the present embodiment, it is possible to provide a photosensitive resin composition that can achieve both dielectric properties and developability, and a photosensitive resin film, a printed wiring board, and a semiconductor package that use the photosensitive resin composition.
[0011] 1 is a schematic diagram showing one embodiment of a manufacturing process for a printed wiring board using the photosensitive resin film of the present embodiment as a material for an interlayer insulating layer.
[0012] In the numerical ranges described herein, the lower and upper limits of the numerical ranges may be replaced with values shown in the examples. In addition, the lower and upper limits of the numerical ranges can be arbitrarily combined with the lower or upper limits of other numerical ranges. In the expression "AA to BB," the numerical values AA and BB at the ends are included as the lower and upper limits, respectively, of the numerical range.
[0013] In this specification, for example, the expression "10 or more" means 10 or a numerical value exceeding 10, and this also applies when the numerical values are different. Furthermore, for example, the expression "10 or less" means 10 or a numerical value less than 10, and this also applies when the numerical values are different.
[0014] In this specification, when there are multiple substances corresponding to each component, the content of each component means the total content of the multiple substances, unless otherwise specified.
[0015] In this specification, "solid content" refers to non-volatile content excluding volatile substances such as solvents. In other words, "solid content" refers to components that remain without volatilization when the resin composition is dried, and includes those that are liquid at room temperature. Here, in this specification, room temperature means 25°C.
[0016] As used herein, the term "number of ring carbon atoms" refers to the number of carbon atoms necessary to form a ring, and does not include the number of carbon atoms of substituents on the ring. For example, both a cyclohexane skeleton and a methylcyclohexane skeleton have 6 ring carbon atoms.
[0017] The expression "(meth)acrylic XX" means either or both of acrylic XX and the corresponding methacrylic XX. Furthermore, the expression "(meth)acryloyl group" means either or both of an acryloyl group and a methacryloyl group.
[0018] In this specification, when the term "layer" is used, for example, as in an interlayer insulating layer, the term "layer" includes not only a solid layer, but also a layer that is not a solid layer but has some islands, has holes, or has an unclear interface with an adjacent layer.
[0019] The weight average molecular weight (Mw) and number average molecular weight (Mn) in this specification refer to values measured in terms of polystyrene by gel permeation chromatography (GPC). Specifically, the weight average molecular weight (Mw) in this specification can be measured by the method described in the examples.
[0020] The mechanism of action described in this specification is speculation and does not limit the mechanism by which the effects of this embodiment are achieved.
[0021] Any combination of the features described in this specification is also included in this embodiment.
[0022] [Photosensitive Resin Composition] The photosensitive resin composition of the present embodiment is a photosensitive resin composition containing (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, and (B) a blocked isocyanate compound having a molecular weight of 3,000 or less.
[0023] The photosensitive resin composition of this embodiment is suitable for via formation (also referred to as photovia formation) by photolithography, and is therefore suitable for forming one or more layers selected from the group consisting of photovias and interlayer insulating layers. That is, the photosensitive resin composition of this embodiment is suitable for photovia formation. Furthermore, the photosensitive resin composition of this embodiment is suitable as a negative photosensitive resin composition.
[0024] <(A) Photopolymerizable Compound Having an Ethylenically Unsaturated Group and an Acidic Substituent> The component (A) is a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent. As the component (A), one type may be used alone, or two or more types may be used in combination.
[0025] Component (A) is a compound that exhibits photopolymerizability, particularly radical polymerizability, due to the presence of an ethylenically unsaturated group. Examples of the ethylenically unsaturated group contained in component (A) include photopolymerizable functional groups such as vinyl, allyl, propargyl, butenyl, ethynyl, phenylethynyl, maleimide, nadimide, and (meth)acryloyl groups. Among these, (meth)acryloyl groups are preferred from the viewpoints of reactivity and via resolution.
[0026] Component (A) has an acidic substituent to enable alkaline development. Examples of acidic substituents that component (A) has include carboxyl groups, sulfonic acid groups, and phenolic hydroxyl groups. Of these, carboxyl groups are preferred from the viewpoint of via resolution. The acid value of component (A) is preferably 20 to 200 mgKOH / g, more preferably 40 to 180 mgKOH / g, even more preferably 70 to 150 mgKOH / g, and particularly preferably 90 to 120 mgKOH / g. When the acid value of component (A) is equal to or greater than the above-mentioned lower limit, the solubility of the photosensitive resin film in dilute alkaline solutions tends to be excellent, while when the acid value is equal to or less than the above-mentioned upper limit, the dielectric properties tend to be excellent. The acid value of component (A) can be measured by the method described in the Examples. Two or more components (A) with different acid values may be used in combination. In this case, it is preferable that the weighted average acid value of the acid values of the two or more components (A) falls within one of the above-mentioned ranges.
[0027] The weight average molecular weight (Mw) of component (A) is preferably 600 to 30,000, more preferably 800 to 25,000, even more preferably 1,000 to 18,000, still more preferably 1,100 to 8,000, particularly preferably 1,200 to 5,000, and most preferably 1,200 to 3,500. When the weight average molecular weight (Mw) of component (A) is within the above range, the adhesive strength with copper plating, heat resistance, and insulation reliability tend to be excellent.
[0028] From the viewpoint of dielectric properties, component (A) preferably contains an alicyclic skeleton. From the viewpoints of via resolution, adhesive strength with copper plating, and electrical insulation reliability, the alicyclic skeleton of component (A) is preferably an alicyclic skeleton having 5 to 20 ring carbon atoms, more preferably an alicyclic skeleton having 5 to 18 ring carbon atoms, even more preferably an alicyclic skeleton having 6 to 18 ring carbon atoms, particularly preferably an alicyclic skeleton having 8 to 14 ring carbon atoms, and most preferably an alicyclic skeleton having 8 to 12 ring carbon atoms. Furthermore, from the viewpoints of via resolution, adhesive strength with copper plating, and electrical insulation reliability, the alicyclic skeleton preferably consists of two or more rings, more preferably two to four rings, and even more preferably three rings. Examples of alicyclic skeletons having two or more rings include a norbornane skeleton, a decalin skeleton, a bicycloundecane skeleton, and a saturated dicyclopentadiene skeleton. In this specification, a saturated dicyclopentadiene skeleton refers to a skeleton containing a ring structure in which the unsaturated bond contained in the dicyclopentadiene ring is saturated. Among these, a saturated dicyclopentadiene skeleton is preferred from the viewpoints of via resolution, adhesive strength with copper plating, and electrical insulation reliability. From the same viewpoint, it is preferable that component (A) contains an alicyclic skeleton represented by the following general formula (A-1):
[0029] (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1 is an integer from 0 to 6. * is a binding site to another structure.)
[0030] In the above general formula (A-1), R A1 Examples of the alkyl group having 1 to 12 carbon atoms represented by m include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group is even more preferred. 1 is an integer of 0 to 6, preferably an integer of 0 to 2, and more preferably 0. 1 is an integer from 2 to 6, a plurality of R A1may be the same or different. A1 may be substituted on the same carbon atom or different carbon atoms, to the extent possible. * represents a bonding site to another structure, and may be bonded to any carbon atom on the alicyclic skeleton, but is preferably bonded to the carbon atom at the site represented by 1 or 2 and the carbon atom at the site represented by 3 or 4 in the following general formula (A-1'):
[0031] (In the formula, R A1 , m 1 and * are the same as those in general formula (A-1).
[0032] From the viewpoints of via resolution and adhesive strength with copper plating, component (A) is preferably an acid-modified vinyl group-containing epoxy resin obtained by reacting (a3) a saturated or unsaturated group-containing polybasic acid anhydride with (a1) an epoxy resin modified with (a2) an ethylenically unsaturated group-containing organic acid [hereinafter sometimes referred to as component (A')]. Here, the term "acid-modified" in the acid-modified vinyl group-containing epoxy resin refers to the presence of an acidic substituent, "vinyl group" refers to an ethylenically unsaturated group, and "epoxy resin" refers to the use of an epoxy resin as a raw material. The acid-modified vinyl group-containing epoxy resin does not necessarily have to contain epoxy groups, and may not necessarily have epoxy groups. Below, preferred embodiments of component (A) obtained from (a1) an epoxy resin, (a2) an ethylenically unsaturated group-containing organic acid, and (a3) a saturated or unsaturated group-containing polybasic acid anhydride are described.
[0033] ((a1) Epoxy Resin) The (a1) epoxy resin is preferably an epoxy resin having two or more epoxy groups. The (a1) epoxy resin may be used alone or in combination of two or more types. The (a1) epoxy resin is classified into glycidyl ether type epoxy resin, glycidyl amine type epoxy resin, glycidyl ester type epoxy resin, etc. Among these, glycidyl ether type epoxy resin is preferred.
[0034] (a1) Epoxy resins can be classified into various epoxy resins depending on the difference in the main skeleton, and can be classified into epoxy resins having an alicyclic skeleton, novolac epoxy resins, bisphenol epoxy resins, aralkyl epoxy resins, other epoxy resins, etc. Among these, epoxy resins having an alicyclic skeleton and novolac epoxy resins are preferred.
[0035] -Epoxy resin having an alicyclic skeleton- The alicyclic skeleton of the epoxy resin having an alicyclic skeleton is explained in the same manner as the alicyclic skeleton of the component (A) described above, and preferred embodiments are also the same. As the epoxy resin having an alicyclic skeleton, an epoxy resin represented by the following general formula (A-2) is preferred.
[0036] (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. A2 represents an alkyl group having 1 to 12 carbon atoms. 1 is an integer from 0 to 6, m 2 is an integer from 0 to 3. n is a number from 0 to 50.
[0037] In general formula (A-2), R A1 represents R in general formula (A-1). A1 The preferred embodiments are also the same as those of the general formula (A-2). A2 Examples of the alkyl group having 1 to 12 carbon atoms represented by m include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group is even more preferred. 1 is m in general formula (A-1) 1 The preferred embodiments are also the same as those of the general formula (A-2). 2is an integer of 0 to 3, preferably 0 or 1, and more preferably 0. In general formula (A-2), n represents the repeating number of the structural unit in the parentheses and is a number of 0 to 50. Usually, epoxy resins are mixtures of structural units in the parentheses with different repeating numbers, and in such cases, n represents the average value of the mixture. Preferably, n is a number of 0 to 30.
[0038] As the epoxy resin having an alicyclic skeleton, commercially available products may be used, and examples of commercially available products include XD-1000 (trade name, manufactured by Nippon Kayaku Co., Ltd.) and EPICLON (registered trademark) HP-7200 (trade name, manufactured by DIC Corporation).
[0039] -Novolac-type epoxy resin- Examples of novolac-type epoxy resins include bisphenol novolac-type epoxy resins such as bisphenol A novolac-type epoxy resin, bisphenol F novolac-type epoxy resin, and bisphenol S novolac-type epoxy resin; phenol novolac-type epoxy resin, cresol novolac-type epoxy resin, biphenyl novolac-type epoxy resin, and naphthol novolac-type epoxy resin. Preferred novolac-type epoxy resins are epoxy resins having a structural unit represented by the following general formula (A-3):
[0040] (In the formula, R A3 represents a hydrogen atom or a methyl group, and Y A1 Each of R independently represents a hydrogen atom or a glycidyl group. A3 may be the same or different. A1 At least one of these represents a glycidyl group.
[0041] R A3 From the viewpoints of via resolution and adhesive strength with copper plating, it is preferable that Y be a hydrogen atom. A1are preferably glycidyl groups. The number of structural units in the (a1) epoxy resin having the structural unit represented by general formula (A-3) is 1 or more, preferably 10 to 100, more preferably 13 to 80, and even more preferably 15 to 70. When the number of structural units is within the above range, the adhesive strength with copper plating, heat resistance, and insulation reliability tend to be improved. In general formula (A-3), R A3 are all hydrogen atoms, and Y A1 In addition, those in which R is a glycidyl group are commercially available as EXA-7376 series (trade name, manufactured by DIC Corporation). A3 are all methyl groups, and Y A1 However, those having a glycidyl group are commercially available as EPON SU8 series (trade name, manufactured by Mitsubishi Chemical Corporation).
[0042] Examples of bisphenol-type epoxy resins include bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, and 3,3',5,5'-tetramethyl-4,4'-diglycidyloxydiphenylmethane. Examples of aralkyl-type epoxy resins include phenol aralkyl-type epoxy resins, biphenyl aralkyl-type epoxy resins, and naphthol aralkyl-type epoxy resins. Other examples of epoxy resins include stilbene-type epoxy resins, naphthalene skeleton-containing epoxy resins, biphenyl-type epoxy resins, dihydroanthracene-type epoxy resins, cyclohexanedimethanol-type epoxy resins, trimethylol-type epoxy resins, alicyclic epoxy resins, aliphatic linear epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, and rubber-modified epoxy resins.
[0043] ((a2) Ethylenically Unsaturated Group-Containing Organic Acid) The (a2) ethylenically unsaturated group-containing organic acid is preferably an ethylenically unsaturated group-containing monocarboxylic acid. Examples of the ethylenically unsaturated group contained in the component (a2) include the same ethylenically unsaturated groups as those contained in the component (A). Examples of the component (a2) include acrylic acid, acrylic acid dimer, methacrylic acid, β-furfurylacrylic acid, β-styrylacrylic acid, cinnamic acid, crotonic acid, α-cyanocinnamic acid and other acrylic acid derivatives; half-ester compounds which are reaction products of hydroxyl group-containing acrylates and dibasic acid anhydrides; and half-ester compounds which are reaction products of vinyl group-containing monoglycidyl ethers or vinyl group-containing monoglycidyl esters and dibasic acid anhydrides. One type of component (a2) may be used alone, or two or more types may be used in combination.
[0044] The half-ester compound can be obtained by reacting one or more ethylenically unsaturated group-containing compounds selected from the group consisting of hydroxyl group-containing acrylates, vinyl group-containing monoglycidyl ethers, and vinyl group-containing monoglycidyl esters with a dibasic acid anhydride. The reaction is preferably carried out by reacting the ethylenically unsaturated group-containing compound and the dibasic acid anhydride in equimolar amounts.
[0045] Examples of hydroxyl group-containing acrylates used in the synthesis of the above-mentioned semi-ester compounds include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, etc. Examples of vinyl group-containing monoglycidyl ethers include glycidyl (meth)acrylate, etc.
[0046] The dibasic acid anhydride used in the synthesis of the half ester compound may contain either a saturated group or an unsaturated group, and examples of the dibasic acid anhydride include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.
[0047] In the reaction between component (a1) and component (a2), the amount of component (a2) used relative to 1 equivalent of the epoxy group in component (a1) is preferably 0.6 to 1.05 equivalents, more preferably 0.7 to 1.02 equivalents, and even more preferably 0.8 to 1.0 equivalents. By reacting components (a1) and (a2) in the above ratio, the photopolymerizability of component (A) is improved, and the resulting photosensitive resin composition tends to have improved via resolution.
[0048] It is preferable that the (a1) component and the (a2) component are dissolved in an organic solvent and reacted. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. The organic solvent may be used alone or in combination of two or more.
[0049] The reaction between component (a1) and component (a2) preferably uses a catalyst to promote the reaction. Examples of such catalysts include amine-based catalysts such as triethylamine and benzylmethylamine; quaternary ammonium salt catalysts such as methyltriethylammonium chloride, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide and benzyltrimethylammonium iodide; and phosphine-based catalysts such as triphenylphosphine. Among these, phosphine-based catalysts are preferred, with triphenylphosphine being more preferred. One catalyst may be used alone, or two or more catalysts may be used in combination. When a catalyst is used, the amount used is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total of component (a1) and component (a2), from the viewpoint of obtaining an appropriate reaction rate.
[0050] In the reaction between component (a1) and component (a2), it is preferable to use a polymerization inhibitor to prevent polymerization during the reaction. Examples of polymerization inhibitors include hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol. One polymerization inhibitor may be used alone, or two or more polymerization inhibitors may be used in combination. When a polymerization inhibitor is used, the amount used is preferably 0.01 to 1 part by mass, more preferably 0.02 to 0.8 parts by mass, and even more preferably 0.1 to 0.5 parts by mass, per 100 parts by mass of the total of component (a1) and component (a2).
[0051] The reaction temperature between component (a1) and component (a2) is preferably 60 to 150°C, more preferably 80 to 120°C, and even more preferably 90 to 110°C, from the viewpoint of ensuring sufficient reactivity and allowing the reaction to proceed homogeneously.
[0052] As described above, when an ethylenically unsaturated group-containing monocarboxylic acid is used as component (a2), component (A') obtained by reacting components (a1) and (a2) has hydroxyl groups formed by a ring-opening addition reaction between the epoxy groups of component (a1) and the carboxyl groups of component (a2). Next, by further reacting component (A') with component (a3), an acid-modified vinyl group-containing epoxy resin can be obtained in which the hydroxyl groups of component (A') (including the hydroxyl groups originally present in component (a1)) and the acid anhydride groups of component (a3) are half-esterified.
[0053] ((a3) Saturated or Unsaturated Group-Containing Polybasic Acid Anhydride) The component (a3) may contain a saturated group or an unsaturated group. Examples of the component (a3) include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride. Among these, tetrahydrophthalic anhydride is preferred from the viewpoint of via resolution. One type of component (a3) may be used alone, or two or more types may be used in combination.
[0054] In the reaction between component (A') and component (a3), for example, the acid value of the acid-modified vinyl group-containing epoxy resin can be adjusted by reacting 0.1 to 1.0 equivalents of component (a3) with one equivalent of hydroxyl groups in component (A').
[0055] The reaction temperature between component (A') and component (a3) is preferably 50 to 150°C, more preferably 60 to 120°C, and even more preferably 70 to 100°C, from the viewpoint of ensuring sufficient reactivity and allowing the reaction to proceed homogeneously.
[0056] The content of the component (A) in the photosensitive resin composition of the present embodiment is not particularly limited, but from the viewpoints of heat resistance, dielectric properties, and chemical resistance, it is preferably 5 to 80 mass %, more preferably 10 to 60 mass %, even more preferably 12 to 50 mass %, particularly preferably 15 to 45 mass %, and most preferably 20 to 40 mass %, based on the total amount of resin components in the photosensitive resin composition.
[0057] <(B) Blocked Isocyanate Compound Having a Molecular Weight of 3,000 or Less> Component (B) is a blocked isocyanate compound having a molecular weight of 3,000 or less. Here, the "molecular weight" of the compound in this specification means the molecular weight that can be calculated from the structural formula when the compound is not a polymer and the structural formula of the compound can be identified, and means the number average molecular weight (Mn) when the compound is a polymer. Component (B) may be used alone or in combination of two or more types.
[0058] The photosensitive resin composition of this embodiment, containing component (B), achieves both excellent dielectric properties and developability. While the exact reason for this is unclear, it is speculated as follows: Hydroxyl groups generated during the curing process or unreacted acidic substituents may remain in the cured product of the photosensitive resin composition, and these functional groups can cause a deterioration in the dielectric dissipation factor (Df). On the other hand, the blocking agent contained in component (B) of this embodiment dissociates upon heating, and the generated isocyanate groups react with the functional groups that deteriorate the dielectric dissipation factor (Df), resulting in good dielectric properties. Furthermore, since the molecular weight of component (B) contained in the photosensitive resin composition of this embodiment is 3,000 or less, it is speculated that good developability is also maintained.
[0059] The molecular weight of component (B) is 3,000 or less, preferably 200 to 2,700, more preferably 350 to 2,500, even more preferably 400 to 2,300, and particularly preferably 600 to 2,000. When the molecular weight of component (B) is the above-mentioned upper limit or less, the developability of the photosensitive resin composition of this embodiment tends to be better. On the other hand, when the molecular weight of component (B) is the above-mentioned lower limit or more, the desmear resistance of the photosensitive resin composition of this embodiment tends to be better. From the above-mentioned viewpoints, the molecular weight of component (B) may be 1,500 or less, 1,200 or less, or 700 or more, or 800 or more.
[0060] The dissociation temperature of component (B) is not particularly limited, but is preferably 80 to 250°C, more preferably 90 to 200°C, even more preferably 100 to 180°C, and particularly preferably 110 to 150°C. When the dissociation temperature of component (B) is equal to or greater than the above-mentioned lower limit, the circuit embedding properties of the photosensitive resin film formed from the photosensitive resin composition of this embodiment tend to be better. Furthermore, when the dissociation temperature of component (B) is equal to or less than the above-mentioned upper limit, the effect of reducing the dielectric tangent tends to be more easily exhibited. The dissociation temperature of component (B) refers to the endothermic peak temperature associated with the deprotection reaction of the blocked isocyanate compound in differential scanning calorimetry.
[0061] The isocyanate compound (hereinafter also referred to as "isocyanate compound (b1)") that is a precursor of the blocked isocyanate compound may be a monoisocyanate compound, a diisocyanate compound, or a tri- or higher functional polyisocyanate compound, but is preferably a tri- or higher functional polyisocyanate compound, and more preferably a trifunctional isocyanate compound from the viewpoint of improving the dielectric properties.
[0062] The tri- or higher functional polyisocyanate compound is preferably a diisocyanate compound multimer. The diisocyanate compound multimer is preferably a trimer or tetramer or higher, and more preferably a trimer from the viewpoint of improving dielectric properties. The diisocyanate compound trimer has three isocyanate groups. From the viewpoint of improving dielectric properties, the diisocyanate compound trimer is preferably a trifunctional isocyanate compound having a biuret structure formed by trimerizing a diisocyanate compound, or a trifunctional isocyanate compound formed by trimerizing a diisocyanate compound to form an isocyanurate ring, and more preferably a trifunctional isocyanate compound formed by trimerizing a diisocyanate compound to form an isocyanurate ring. That is, from the viewpoint of improving dielectric properties, component (B) is preferably a compound containing an isocyanurate ring, and more preferably a compound obtained by blocking a trifunctional isocyanate compound containing an isocyanurate ring with a blocking agent.
[0063] Examples of the isocyanate compound (b1) include aliphatic isocyanate compounds and aromatic isocyanate compounds. In this specification, an aliphatic isocyanate compound refers to an isocyanate compound having an isocyanate group directly bonded to an aliphatic group, and an aromatic isocyanate compound refers to an isocyanate compound having an isocyanate group directly bonded to an aromatic group. A compound having both an isocyanate group directly bonded to an aliphatic group and an isocyanate group directly bonded to an aromatic group is considered to belong to both the aliphatic isocyanate compound and the aromatic isocyanate compound. In addition, an alicyclic isocyanate compound is also included in the aliphatic isocyanate compound.
[0064] Examples of the aliphatic isocyanate compound include aliphatic diisocyanate compounds such as trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2,6-diisocyanate methylcaprate, xylylene diisocyanate, 1,3-cyclopentane diisocyanate, 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, methylenebis(cyclohexyl isocyanate), methylcyclohexane diisocyanate, norbornane diisocyanate, bis(isocyanatomethyl)cyclohexane, and isophorone diisocyanate; and polymers of the above-mentioned aliphatic diisocyanate compounds. Among these, multimers of aliphatic diisocyanate compounds are preferred, trimers of aliphatic diisocyanate compounds are more preferred, and trifunctional isocyanate compounds in which an isocyanurate ring is formed by trimerizing hexamethylene diisocyanate, trifunctional isocyanate compounds in which an isocyanurate ring is formed by trimerizing isophorone diisocyanate, and trifunctional isocyanate compounds having a biuret structure in which hexamethylene diisocyanate is trimerized are even more preferred.
[0065] Examples of aromatic isocyanate compounds include tolylene diisocyanate, phenylene diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-toluidine diisocyanate, and 4,4'-diphenyl ether diisocyanate.
[0066] Examples of blocking agents include oxime compounds, alcohol compounds, acid amide compounds, acid imide compounds, phenol compounds, amine compounds, active methylene compounds, imidazole compounds, and pyrazole compounds. Examples of oxime compounds include formaldoxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, 2-butanone oxime, and cyclohexanone oxime. Examples of alcohol compounds include methanol, ethanol, 2-propanol, n-butanol, sec-butanol, 2-ethyl-1-hexanol, 2-methoxyethanol, 2-ethoxyethanol, and 2-butoxyethanol. Examples of acid amide compounds include acetanilide, acetic acid amide, ε-caprolactam, δ-valerolactam, and γ-butyrolactam. Examples of acid imide compounds include succinimide and maleimide. Examples of phenolic compounds include phenol, cresol, ethylphenol, butylphenol, nonylphenol, dinonylphenol, styrenated phenol, and hydroxybenzoic acid esters. Examples of amine compounds include diphenylamine, aniline, carbazole, di-n-propylamine, diisopropylamine, and isopropylethylamine. Examples of active methylene compounds include dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone. Examples of imidazole compounds include imidazole and 2-methylimidazole. Examples of pyrazole compounds include pyrazole, 3-methylpyrazole, and 3,5-dimethylpyrazole.
[0067] The content of component (B) in the photosensitive resin composition of this embodiment is not particularly limited, but is preferably 1 to 40 mass%, more preferably 3 to 35 mass%, even more preferably 5 to 30 mass%, and particularly preferably 6 to 25 mass%, based on the total amount of resin components in the photosensitive resin composition. When the content of component (B) in the photosensitive resin composition of this embodiment is equal to or greater than the above-mentioned lower limit, the dielectric properties tend to be better. Furthermore, when the content of component (B) in the photosensitive resin composition of this embodiment is equal to or less than the above-mentioned upper limit, the adhesive strength with copper plating tends to be better.
[0068] <(C) Thermosetting Resin> The photosensitive resin composition of this embodiment preferably further contains a thermosetting resin as component (C). Component (C) does not include component (A). When the photosensitive resin composition of this embodiment contains a thermosetting resin (C), the heat resistance tends to be improved in addition to the adhesive strength with copper plating and the insulation reliability. One type of component (C) may be used alone, or two or more types may be used in combination.
[0069] Examples of the (C) thermosetting resin include epoxy resins, phenolic resins, unsaturated imide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins. Furthermore, the thermosetting resin is not particularly limited to these, and any known thermosetting resin can be used. Among these, epoxy resins are preferred from the viewpoints of adhesive strength with copper plating, insulation reliability, and heat resistance.
[0070] The epoxy resin is preferably an epoxy resin having two or more epoxy groups. Epoxy resins are classified into glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among these, glycidyl ether type epoxy resins are preferred.
[0071] Epoxy resins are also classified into various epoxy resins depending on the difference in the main skeleton, and each of the above types of epoxy resins is further classified as follows: Specifically, bisphenol-based epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and bisphenol S-type epoxy resins; bisphenol-based novolac-type epoxy resins such as bisphenol A-type novolac-type epoxy resins and bisphenol F-type novolac-type epoxy resins; novolac-type epoxy resins other than the above bisphenol-based novolac-type epoxy resins such as phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, and biphenyl novolac-type epoxy resins; phenol aralkyl-type epoxy resins; stilbene-type epoxy resins; naphtha-type epoxy resins; They are classified into naphthalene skeleton-containing epoxy resins such as novolac-type epoxy resins, naphthol-type epoxy resins, naphthol aralkyl-type epoxy resins, and naphthylene ether-type epoxy resins; biphenyl-type epoxy resins; biphenyl aralkyl-type epoxy resins; xylylene-type epoxy resins; dihydroanthracene-type epoxy resins; alicyclic epoxy resins such as saturated dicyclopentadiene-type epoxy resins; heterocyclic epoxy resins; spiro ring-containing epoxy resins; cyclohexanedimethanol-type epoxy resins; trimethylol-type epoxy resins; aliphatic linear epoxy resins; and rubber-modified epoxy resins.
[0072] Among these, the epoxy resin preferably contains at least one selected from the group consisting of bisphenol-based epoxy resins, naphthalene skeleton-containing epoxy resins, and biphenylaralkyl-type epoxy resins, particularly from the viewpoints of heat resistance, electrical insulation reliability, developability, and adhesive strength with copper plating, and more preferably contains at least one selected from the group consisting of naphthalene skeleton-containing epoxy resins and biphenylaralkyl-type epoxy resins.
[0073] In the photosensitive resin composition of this embodiment, the equivalent ratio of the acidic substituent in component (A) to the epoxy group in component (C) [epoxy group / acidic substituent] is not particularly limited, but from the viewpoints of insulation reliability, dielectric properties, heat resistance, and adhesive strength with copper plating, it is preferably 0.5 to 6.0, more preferably 0.7 to 4.0, even more preferably 0.8 to 2.0, and particularly preferably 0.9 to 1.8.
[0074] When the photosensitive resin composition of the present embodiment contains a thermosetting resin (C), the content of the thermosetting resin (C) is not particularly limited, but from the viewpoints of insulation reliability, dielectric properties, heat resistance, and adhesive strength with copper plating, it is preferably 1 to 50 mass %, more preferably 5 to 45 mass %, even more preferably 15 to 40 mass %, and particularly preferably 20 to 35 mass %, based on the total amount of resin components in the photosensitive resin composition.
[0075] <(D) Photopolymerization initiator> The photosensitive resin composition of this embodiment preferably further contains a photopolymerization initiator as component (D). By containing the photopolymerization initiator (D), the photosensitive resin composition of this embodiment tends to improve the resolution of vias. The photopolymerization initiator (D) may be used alone or in combination of two or more. From the viewpoint of the resolution of vias, the photosensitive resin composition of this embodiment preferably contains two or more types of photopolymerization initiator (D).
[0076] The (D) photopolymerization initiator is not particularly limited as long as it can photopolymerize an ethylenically unsaturated group, and can be appropriately selected from commonly used photopolymerization initiators. Examples of the (D) photopolymerization initiator include benzoin-based compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone-based compounds such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane, and N,N-dimethylaminoacetophenone; 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and the like. ketal compounds such as acetophenone dimethyl ketal and benzil dimethyl ketal; acridine compounds such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; acylphosphine oxide compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; and oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime].
[0077] Among these, oxime ester compounds and acylphosphine oxide compounds are preferred, with 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime) and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide being more preferred. Oxime ester compounds have the advantage of improving photocurability, while acylphosphine oxide compounds have the advantage of improving the degree of cure at the bottom of the cured product obtained by curing a photosensitive resin film and suppressing undercut. The combined use of an oxime ester compound and an acylphosphine oxide compound tends to further improve via resolution.
[0078] When the photosensitive resin composition of the present embodiment contains a (D) photopolymerization initiator, the content of the (D) photopolymerization initiator is not particularly limited, but from the viewpoint of easily obtaining an appropriate effect of promoting the polymerization reaction, the content is preferably 0.01 to 20 mass %, more preferably 0.02 to 10 mass %, even more preferably 0.03 to 3 mass %, and particularly preferably 0.05 to 1 mass %, based on the total amount of resin components of the photosensitive resin composition.
[0079] <(E) Crosslinking Agent> The photosensitive resin composition of this embodiment preferably further contains a crosslinking agent as component (E). The crosslinking agent is preferably a crosslinking agent having two or more ethylenically unsaturated groups and no acidic substituent. The crosslinking agent reacts with the ethylenically unsaturated groups of component (A) to increase the crosslink density of the photosensitive resin film after curing. Therefore, by including a crosslinking agent, the photosensitive resin composition of this embodiment tends to have improved heat resistance and dielectric properties. One type of (E) crosslinking agent may be used alone, or two or more types may be used in combination.
[0080] Examples of the (E) crosslinking agent include a bifunctional monomer having two ethylenically unsaturated groups and a polyfunctional monomer having three or more ethylenically unsaturated groups. The (E) crosslinking agent preferably contains the polyfunctional monomer. Examples of the ethylenically unsaturated groups contained in the (E) crosslinking agent include the same ethylenically unsaturated groups as those contained in the (A) component, and preferred embodiments are also the same.
[0081] Examples of the bifunctional monomer include aliphatic di(meth)acrylates such as trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; di(meth)acrylates having an alicyclic skeleton such as dicyclopentadiene di(meth)acrylate and tricyclodecane dimethanol di(meth)acrylate; and aromatic di(meth)acrylates such as 2,2-bis(4-(meth)acryloxypolyethoxypolypropoxyphenyl)propane and bisphenol A diglycidyl ether di(meth)acrylate. Among these, from the viewpoint of obtaining better dielectric properties, di(meth)acrylates having an alicyclic skeleton are preferred, and tricyclodecane dimethanol diacrylate is more preferred.
[0082] Examples of the polyfunctional monomer include (meth)acrylate compounds having a skeleton derived from trimethylolpropane, such as trimethylolpropane tri(meth)acrylate; (meth)acrylate compounds having a skeleton derived from tetramethylolmethane, such as tetramethylolmethane tri(meth)acrylate and tetramethylolmethane tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from pentaerythritol, such as pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from dipentaerythritol, such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; (meth)acrylate compounds having a skeleton derived from ditrimethylolpropane, such as ditrimethylolpropane tetra(meth)acrylate; and (meth)acrylate compounds having a skeleton derived from diglycerin. Among these, from the viewpoints of via resolution and adhesive strength with copper plating, (meth)acrylate compounds having a skeleton derived from dipentaerythritol are preferred, and dipentaerythritol hexa(meth)acrylate is more preferred. Here, the above-mentioned "(meth)acrylate compound having a skeleton derived from XXX" (where XXX is the name of the compound) refers to an esterification product of XXX and (meth)acrylic acid, and the esterification product also includes compounds modified with an alkyleneoxy group.
[0083] When the photosensitive resin composition of the present embodiment contains a crosslinking agent (E), the content of the crosslinking agent (E) is not particularly limited, but from the viewpoints of heat resistance and dielectric properties, it is preferably 10 to 85 parts by mass, more preferably 25 to 80 parts by mass, even more preferably 35 to 75 parts by mass, and particularly preferably 45 to 70 parts by mass per 100 parts by mass of the component (A).
[0084] <(F) Elastomer> The photosensitive resin composition of this embodiment preferably further contains an elastomer as component (F). By containing the (F) elastomer, the photosensitive resin composition of this embodiment tends to have improved adhesive strength with copper plating. One type of (F) elastomer may be used alone, or two or more types may be used in combination.
[0085] The (F) elastomer may have a reactive functional group at the molecular end or in the molecular chain. Examples of the reactive functional group include an acid anhydride group, an epoxy group, a hydroxyl group, a carboxyl group, an amino group, an amide group, an isocyanato group, an acrylic group, a methacrylic group, and a vinyl group. Among these, an acid anhydride group is preferred from the viewpoints of via resolution and adhesive strength with copper plating. As the acid anhydride group, an acid anhydride group derived from maleic anhydride is preferred. When the (F) elastomer has an acid anhydride group, from the viewpoints of via resolution and dielectric properties, the number of acid anhydride groups per molecule is preferably 1 to 10, more preferably 3 to 10, and even more preferably 6 to 10.
[0086] Examples of the (F) elastomer include polybutadiene-based elastomers, polyester-based elastomers, styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, polyamide-based elastomers, acrylic elastomers, silicone-based elastomers, and derivatives of these elastomers. Among these, polybutadiene-based elastomers are preferred from the viewpoints of improving adhesive strength with copper plating and further improving compatibility and solubility with resin components. From the viewpoint of via resolution, the polybutadiene-based elastomer is preferably a polybutadiene-based elastomer having an acid anhydride group that has been modified with an acid anhydride, and more preferably a polybutadiene-based elastomer having an acid anhydride group derived from maleic anhydride.
[0087] From the viewpoint of adhesive strength with copper plating, the polybutadiene elastomer may be a polybutadiene having an epoxy group [hereinafter, may be referred to as an epoxidized polybutadiene]. From the viewpoint of adhesive strength with copper plating and flexibility, the epoxidized polybutadiene is preferably an epoxidized polybutadiene represented by the following general formula (F-1):
[0088] (In the formula, a, b, and c each represent the ratio of the structural units in parentheses, where a is 0.05 to 0.40, b is 0.02 to 0.30, and c is 0.30 to 0.80, and further, a+b+c=1.00 and (a+c)>b are satisfied. y represents the number of structural units in square brackets and is an integer from 10 to 250.)
[0089] In the general formula (F-1), the structural units in the square brackets may be bonded in any order. In other words, the structural unit shown on the left, the structural unit shown in the center, and the structural unit shown on the right may be interchanged, and when they are represented as (a), (b), and (c), respectively, various bonding orders are possible, such as -[(a)-(b)-(c)]-[(a)-(b)-(c)-]-, -[(a)-(c)-(b)]-[(a)-(c)-(b)-]-, -[(b)-(a)-(c)]-[(b)-(a)-(c)-]-, -[(a)-(b)-(c)]-[(c)-(b)-(a)-]-, -[(a)-(b)-(a)]-[(c)-(b)-(c)-]-, -[(a)-(b)-(a)]-[(c)-(b)-(c)-]-, -[(c)-(b)-(c)]-[(b)-(a)-(a)-]-. From the viewpoints of adhesive strength with copper plating and flexibility, a is preferably 0.10 to 0.30, b is preferably 0.10 to 0.30, and c is preferably 0.40 to 0.80. From the same viewpoints, y is preferably an integer of 30 to 180.
[0090] The number average molecular weight (Mn) of the (F) elastomer is not particularly limited, but is preferably 10,000 to 80,000, and may be 20,000 to 70,000, 30,000 to 65,000, or 40,000 to 60,000.
[0091] When the photosensitive resin composition of the present embodiment contains the elastomer (F), the content of the elastomer (F) is not particularly limited, but from the viewpoints of heat resistance and adhesive strength with copper plating, it is preferably 0.5 to 15 mass %, more preferably 1 to 14 mass %, even more preferably 3 to 13 mass %, and particularly preferably 5 to 12 mass %, based on the total amount of resin components in the photosensitive resin composition.
[0092] <(G) Inorganic Filler> The photosensitive resin composition of this embodiment preferably further contains an inorganic filler as component (G). By containing the inorganic filler (G), the photosensitive resin composition of this embodiment tends to have better low thermal expansion, heat resistance, and flame retardancy. One type of (G) inorganic filler may be used alone, or two or more types may be used in combination.
[0093] (G) As inorganic filler, silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, molybdenum acid compound, talc, aluminum borate, silicon carbide etc. are enumerated.Among these, as inorganic filler, silica and alumina are preferred from the viewpoint of thermal expansion coefficient, heat resistance and flame retardancy, and silica is more preferred.As silica, crushed silica, fumed silica, fused silica etc. are enumerated.
[0094] (G) Volume average particle diameter (D 50 ) is not particularly limited, but is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, even more preferably 0.2 to 1 μm, and particularly preferably 0.3 to 0.8 μm. 50 The particle diameter can be determined as the particle diameter corresponding to an integrated value of 50% (volume basis) in the particle size distribution by measuring particles dispersed in a solvent at a refractive index of 1.38 using a submicron particle analyzer (manufactured by Beckman Coulter, Inc., product name: N5) in accordance with the international standard ISO 13321.
[0095] When the photosensitive resin composition of the present embodiment contains an inorganic filler (G), the content of the inorganic filler (G) is preferably 1 to 70 mass %, more preferably 5 to 60 mass %, even more preferably 15 to 55 mass %, and particularly preferably 25 to 50 mass %, based on the total solid content of the photosensitive resin composition, from the viewpoint of forming an interlayer insulating layer that is superior in low thermal expansion properties, heat resistance, flame retardancy, and conductor adhesion.
[0096] <(H) Curing Accelerator> The photosensitive resin composition of this embodiment preferably further contains a curing accelerator as component (H). By containing the curing accelerator (H), the photosensitive resin composition of this embodiment tends to have better heat resistance, dielectric properties, etc. One type of (H) curing accelerator may be used alone, or two or more types may be used in combination.
[0097] (H) Examples of the curing accelerator include imidazole compounds such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, 2-phenyl-1-benzyl-1H-imidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and isocyanate-masked imidazole (an addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole); trimethylamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), and tetramethyl Examples of suitable curing agents include tertiary amines such as methylguanidine and m-aminophenol; organic phosphines such as tributylphosphine, triphenylphosphine and tris-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; the above-mentioned polybasic acid anhydrides; diphenyliodonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, and 2,4,6-triphenylthiopyrylium hexafluorophosphate. Among these, imidazole-based compounds are preferred from the viewpoint of obtaining excellent curing properties.
[0098] When the photosensitive resin composition of the present embodiment contains the curing accelerator (H), the content of the curing accelerator (H) is not particularly limited, but from the viewpoint of improving the heat resistance and dielectric properties, it is preferably 0.01 to 10 mass %, more preferably 0.05 to 5 mass %, and even more preferably 0.1 to 2 mass %, based on the total amount of the resin components of the photosensitive resin composition.
[0099] <(I) Other Components> The photosensitive resin composition of this embodiment may contain (I) other components as necessary. Examples of (I) other components include resins other than the above components; curing agents, organic fillers; photosensitizers; polymerization inhibitors; foam stabilizers; pigments; adhesion aids such as melamine; foam stabilizers such as silicone compounds; thickeners; flame retardants; and organic solvents. Each of these may be used alone or in combination of two or more. The content of (I) other components in the photosensitive resin composition of this embodiment may be adjusted appropriately depending on the purpose, and each may be 0.01 to 10% by mass, 0.05 to 5% by mass, or 0.1 to 1% by mass, based on the total solids content of the photosensitive resin composition.
[0100] <Method for Producing Photosensitive Resin Composition> The photosensitive resin composition of the present embodiment can be obtained by kneading and mixing the components using a roll mill, a bead mill, or the like.
[0101] [Photosensitive Resin Film] The photosensitive resin film of this embodiment contains the photosensitive resin composition of this embodiment. The photosensitive resin film is useful as a photosensitive layer for forming an interlayer insulating layer. The components and their contents in the photosensitive resin film of this embodiment are the same as those in the photosensitive resin composition of this embodiment.
[0102] The photosensitive resin film of this embodiment may be provided on a carrier film. Examples of the carrier film include polyesters such as polyethylene terephthalate and polybutylene terephthalate; and polyolefins such as polypropylene and polyethylene. The thickness of the carrier film is preferably 5 to 100 μm, more preferably 10 to 60 μm, and even more preferably 15 to 45 μm. The photosensitive resin film of this embodiment may also have a protective film on the surface opposite to the surface in contact with the carrier film.
[0103] The photosensitive resin film of this embodiment can be formed, for example, by applying the photosensitive resin composition of this embodiment to a carrier film using a known coating device such as a comma coater, bar coater, kiss coater, roll coater, gravure coater, or die coater, followed by drying. The coating film formed by applying the photosensitive resin composition can be dried using hot air drying, a dryer using far infrared rays, or a dryer using near infrared rays. The drying temperature is preferably 60 to 150°C, more preferably 70 to 120°C, and even more preferably 80 to 110°C. The drying time is preferably 1 to 60 minutes, more preferably 2 to 30 minutes, and even more preferably 5 to 20 minutes. The content of residual diluent in the photosensitive resin film after drying is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less, from the viewpoint of preventing diffusion of the diluent during the manufacturing process of a printed wiring board.
[0104] The thickness of the photosensitive resin film of this embodiment is not particularly limited, but from the viewpoint of thinning the printed wiring board, it is preferably 1 to 100 μm, more preferably 3 to 60 μm, and even more preferably 5 to 40 μm.
[0105] [Printed Wiring Board] The printed wiring board of this embodiment is a printed wiring board including a cured product of the photosensitive resin composition of this embodiment. The printed wiring board of this embodiment is preferably a printed wiring board having an interlayer insulating layer that is a cured product of the photosensitive resin film of this embodiment. Note that the "interlayer insulating layer" of the printed wiring board of this embodiment also includes a state after various processing or treatments such as via and wiring formation, roughening treatment, etc. have been performed.
[0106] The method for manufacturing a printed wiring board according to this embodiment is not particularly limited as long as it uses the photosensitive resin film according to this embodiment. However, a preferred method for manufacturing a printed wiring board includes the following steps (1) to (4). (1): Laminating the photosensitive resin film according to this embodiment on one or both sides of a circuit board (hereinafter also referred to as the "laminating step (1)"). (2): Forming an interlayer insulating layer having vias by exposing and developing the photosensitive resin film laminated in step (1) (hereinafter also referred to as the "via forming step (2)"). (3): Heat-curing the interlayer insulating layer having vias (hereinafter also referred to as the "heat-curing step (3)"). (4): Forming a circuit pattern on the interlayer insulating layer (hereinafter also referred to as the "circuit pattern forming step (4)"). The method for manufacturing a printed wiring board according to this embodiment will be described below with reference to FIG. 1 as appropriate. Note that, for convenience, a specific operation may be referred to as the "XX step" in this specification, but this "XX step" is not limited to the specific embodiments described herein.
[0107] (Laminating Step (1)) In the laminating step (1), the photosensitive resin film of this embodiment is laminated onto one or both sides of a circuit board. FIG. 1(a) illustrates a step of forming a photosensitive layer 103 on both sides of a substrate 101 having a circuit pattern 102. The photosensitive layer 103 can be formed by laminating the photosensitive resin film of this embodiment onto both sides of the substrate 101 so that the second surface becomes the attachment surface. Lamination can be performed, for example, by pressing the film together while applying pressure and heat using a vacuum laminator or the like. If a carrier film is attached to the photosensitive layer 103 after lamination, the carrier film may be peeled off before or after the exposure described below.
[0108] (Via Forming Step (2)) In the via forming step (2), the photosensitive layer formed in the laminating step (1) is exposed to light and developed to form an interlayer insulating layer having vias. FIG. 1(b) illustrates a step of forming an interlayer insulating layer 104 having vias 105 by exposing and developing the photosensitive layer 103. By exposing the photosensitive layer 103, a photoradical polymerization reaction is initiated, and the photosensitive resin film is cured.
[0109] The exposure method for the photosensitive layer 103 may be, for example, a mask exposure method in which actinic rays are irradiated imagewise through a negative or positive mask pattern known as artwork, or a method in which actinic rays are irradiated imagewise by a direct writing exposure method such as LDI (Laser Direct Imaging) exposure or DLP (Digital Light Processing) exposure. Examples of light sources for actinic rays include known light sources such as gas lasers such as carbon arc lamps, mercury vapor arc lamps, high-pressure mercury lamps, xenon lamps, and argon lasers; solid-state lasers such as YAG lasers; and semiconductor lasers that effectively emit ultraviolet or visible light. The exposure dose may be adjusted appropriately depending on the light source used, the thickness of the photosensitive layer, and the like. For example, when a photosensitive layer having a thickness of 1 to 100 μm is exposed to ultraviolet radiation from a high-pressure mercury lamp, the exposure dose is not particularly limited, but is preferably 10 to 1,000 mJ / cm. 2 , more preferably 50 to 700 mJ / cm 2 , more preferably 150 to 400 mJ / cm 2 is.
[0110] Next, if a carrier film is present on the photosensitive layer 103, the carrier film is removed before development. In development, the uncured portions of the photosensitive layer 103 are removed, and the photocured portions are formed on the substrate as the interlayer insulating layer 104. The development method may be wet development or dry development, but wet development is preferred. As a wet development method, a spray method is preferred from the viewpoint of improving resolution. Examples of the developer include an alkaline aqueous solution, a water-based developer, and an organic solvent-based developer, and among these, an alkaline aqueous solution is preferred. After exposure and development, post-exposure may be performed from the viewpoint of increasing the degree of curing of the interlayer insulating layer. The exposure dose in post-exposure is not particularly limited, but is preferably 0.2 to 10 J / cm. 2 , more preferably 0.5 to 5 J / cm 2 is.
[0111] The shape of the via is not particularly limited, and examples of cross-sectional shapes include a rectangle and an inverted trapezoid. An inverted trapezoid has a shape in which the upper side is longer than the lower side. Examples of planar shapes include a circle and a rectangle. Forming a via using the photolithography method of this embodiment allows for the formation of a via with an inverted trapezoid cross-sectional shape. Vias having such shapes are preferred because they have high adhesion of plated copper to the via wall surface. Forming a via using the photolithography method of this embodiment allows for the via diameter to be smaller than the diameter of a via fabricated by laser processing. The diameter of a via formed using the manufacturing method of this embodiment may be, for example, 40 μm or less, 35 μm or less, or 30 μm or less. There is no particular limit to the lower limit of the via diameter, but it may be, for example, 15 μm or more, or 20 μm or more.
[0112] (Heat Curing Step (3)) In the heat curing step (3), the interlayer insulating layer having vias is heat cured. That is, in the heat curing step (3), heating is used to promote the curing reaction of the thermosetting component contained in the photosensitive resin film of this embodiment. The heating temperature is not particularly limited, but is preferably 100 to 300°C, more preferably 120 to 200°C, and even more preferably 150 to 180°C. The heating time is not particularly limited, but is preferably 0.3 to 3 hours, more preferably 0.5 to 2 hours, and even more preferably 0.75 to 1.5 hours.
[0113] (Circuit Pattern Forming Step (4)) Next, a circuit pattern is formed on the interlayer insulating layer formed above. From the viewpoint of forming fine wiring, the circuit pattern is preferably formed by a semi-additive process in which roughening treatment, formation of a seed layer, formation of a resist pattern, formation of a copper circuit layer, and removal of the resist pattern are carried out in this order.
[0114] The roughening treatment is a treatment for roughening the surface of the interlayer insulating layer to form uneven anchors. If smears occur in the via formation step (2), roughening treatment and smear removal may be performed simultaneously using a roughening solution. Examples of the roughening solution include alkaline permanganate roughening solutions such as sodium permanganate roughening solutions; chromium / sulfuric acid roughening solutions; and sodium fluoride / chromium / sulfuric acid roughening solutions.
[0115] 1C illustrates the step of forming a seed layer 106. The seed layer 106 is used to form a power supply layer for electrolytic copper plating. The seed layer 106 can be formed by electroless copper plating using a palladium catalyst or the like on the via bottom, via wall surface, and the entire surface of the interlayer insulating layer.
[0116] 1(d) illustrates a step of forming a resist pattern 107 on the seed layer 106. The resist pattern 107 can be formed, for example, by thermocompressing a dry film resist onto the seed layer 106 using a roll laminator or the like, and then exposing and developing the resist. Commercially available dry film resists can be used.
[0117] The dry film resist may be exposed through a mask on which a desired wiring pattern is drawn. After exposure, the dry film resist is developed using an alkaline aqueous solution to remove the unexposed portions, forming a resist pattern 107. Thereafter, plasma treatment may be performed as necessary to remove development residues of the dry film resist.
[0118] FIG. 1( e) illustrates the step of forming a copper circuit layer 108. The copper circuit layer 108 is preferably formed by electrolytic copper plating. As the electrolytic copper plating solution used for electrolytic copper plating, for example, a commercially available electrolytic copper plating solution, such as an electrolytic copper plating solution containing copper sulfate, can be used. After electrolytic copper plating, the resist pattern 107 is removed using an alkaline aqueous solution or an amine-based stripper. Further, flash etching to remove the seed layer 106 between the wirings, removal of the palladium catalyst, or the like is appropriately performed by a known method. Furthermore, if necessary, a post-baking treatment may be performed to sufficiently thermally cure any unreacted thermosetting components.
[0119] 1(f) shows a multilayer printed wiring board 100A that is formed by repeating the above steps and has a solder resist layer 109 on the outermost surface. The solder resist layer 109 can be formed using a known photosensitive resin film for solder resist.
[0120] The method for manufacturing a printed wiring board in which vias are formed using the photosensitive resin film of this embodiment has been described above, but the photosensitive resin film of this embodiment has excellent pattern resolution, so it is also suitable for forming cavities for incorporating chips, passive elements, etc. The cavities can be suitably formed, for example, by using a drawing pattern that can form the desired cavities when forming a pattern by exposing the photosensitive resin film in the above description of the printed wiring board.
[0121] [Semiconductor Package] The semiconductor package of this embodiment is a semiconductor package including the printed wiring board of this embodiment and a semiconductor element. The semiconductor package of this embodiment can be manufactured, for example, by mounting a semiconductor element such as a semiconductor chip or memory at a predetermined position on the printed wiring board of this embodiment and sealing the semiconductor element with a sealing resin or the like.
[0122] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to these examples.
[0123] [Method for Measuring Acid Value] The acid value was calculated from the amount of aqueous potassium hydroxide solution required to neutralize the object to be measured.
[0124] [Method for measuring weight-average molecular weight (Mw)] The weight-average molecular weight (Mw) was measured using the following GPC measurement device and measurement conditions, and calculated using the calibration curve of standard polystyrene. The calibration curve was created using a set of five samples ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation) as standard polystyrene. (GPC measurement device) GPC device: high-speed GPC device "HCL-8320GPC", detector: differential refractometer or UV, manufactured by Tosoh Corporation Column: column TSKgel SuperMultipore HZ-H (column length: 15 cm, column inner diameter: 4.6 mm), manufactured by Tosoh Corporation (Measurement conditions) Solvent: tetrahydrofuran (THF) Measurement temperature: 40°C Flow rate: 0.35 ml / min Sample concentration: 10 mg / 5 ml THF Injection amount: 20 μl
[0125] [Production of Photosensitive Resin Compositions and Photosensitive Resin Films] Examples 1 to 8, Comparative Examples 1 to 5 (1) Production of Photosensitive Resin Compositions The components were mixed according to the formulations shown in Table 1 (the units of values in the table are parts by mass, and in the case of solutions, they are amounts converted to solid content), and kneaded using a three-roll mill and a planetary mixer. Thereafter, methyl ethyl ketone was added so that the solid content concentration became 65% by mass, thereby obtaining photosensitive resin compositions.
[0126] (2) Production of Photosensitive Resin Film A 16 μm thick polyethylene terephthalate film (manufactured by Teijin Limited, product name "G2-16") was used as the carrier film. The photosensitive resin composition prepared in each example was applied to the carrier film so that the film thickness after drying would be 25 μm, and a photosensitive resin film was formed by drying at 100°C for 10 minutes using a hot air convection dryer. Subsequently, a polyethylene film (manufactured by Tamapoly Corporation, product name "NF-15") was laminated as a protective film to the surface of the photosensitive resin film opposite the side in contact with the carrier film, and a photosensitive resin film with the carrier film and protective film laminated together was produced.
[0127] [Measurement of relative permittivity (Dk) and dielectric loss tangent (Df)] Two photosensitive resin films from which the protective films had been peeled off were bonded together, and with the carrier films on both sides still attached, they were exposed to 400 mJ / cm 2 using a flatbed exposure machine. 2 (wavelength 365 nm), 2 J / cm using a UV conveyor exposure machine 2 The specimen was irradiated with ultraviolet light (wavelength 365 nm). The specimen was then heat-treated at 170°C for 1 hour using a hot air circulation dryer, and cut into a size of 7 cm x 10 cm to prepare an evaluation sample. A desiccant was enclosed in the obtained evaluation sample, which was then dried for 10 hours or more. The dielectric constant (Dk) and dielectric loss tangent (Df) in the 10 GHz band were measured using a split post dielectric resonator (SPDR) method.
[0128] [Measurement of Minimum Development Time] The copper foil surface of a printed wiring board substrate (manufactured by Resonac Corporation, product name "MCL-E-679"), in which copper foil (thickness 12 μm) was laminated on a glass epoxy base material, was roughened pretreated with a roughening pretreatment solution (manufactured by MEC Co., Ltd., product name "CZ-8101"), followed by rinsing with water and drying. Next, a photosensitive resin film from which the protective film had been peeled was laminated onto the copper foil of the roughened pretreated printed wiring board substrate, with the photosensitive resin film serving as the attachment surface. Note that a press-type vacuum laminator (manufactured by Meiki Seisakusho Co., Ltd., product name "MVLP-500") was used for lamination, and the lamination conditions were a press hot plate temperature of 75°C, a vacuum evacuation time of 20 seconds, a lamination press time of 30 seconds, an atmospheric pressure of 4 kPa or less, and a pressure of 0.4 MPa. After lamination, the laminate was left at room temperature for at least 1 hour to obtain a laminate for evaluation in which a photosensitive resin film and a carrier film were laminated in this order on the copper foil surface of the substrate for printed wiring board. The carrier film of the laminate for evaluation obtained above was removed, and the photosensitive resin film was spray-developed using a 1% by mass aqueous solution of sodium carbonate at 30°C. The minimum development time was defined as the minimum development time.
[0129] [Measurement of Adhesion Strength with Copper Plating] (1) Preparation of Laminate for Evaluation and Measurement of Sensitivity of Photosensitive Resin Film A laminate for evaluation was prepared using the same procedure as in [Measurement of Minimum Development Time] above, and a 41-step tablet was placed on the carrier film of the laminate for evaluation. Next, exposure was carried out using a parallel light exposure machine (manufactured by ORC Manufacturing Co., Ltd., product name "EXM-1201") using an ultra-high pressure mercury lamp as a light source. After exposure, the laminate was left at room temperature for 30 minutes, and then the carrier film of the laminate for evaluation obtained above was removed, and the photosensitive resin film was spray-developed using a 1% by mass aqueous solution of sodium carbonate at 30°C. The amount of exposure energy at which the gloss remaining step number was 8.0 was determined, and this was used as the sensitivity (unit: mJ / cm) of the photosensitive resin film. 2) (2) Exposure Step and Development Step The entire surface of the evaluation laminate was exposed to light with the exposure energy amount corresponding to the sensitivity determined above, and the photosensitive resin film was cured. After exposure, the evaluation laminate was left at room temperature for 30 minutes, and then the carrier film was peeled off and removed, and the photosensitive resin film was spray-developed using a 1% by mass aqueous solution of sodium carbonate at 30°C for a development time twice the minimum development time. (3) Post-Cure Treatment Subsequently, using a UV conveyor device (manufactured by Oak Manufacturing Co., Ltd.) with a high-pressure mercury lamp irradiation type, the exposure dose was 2 J / cm 2 Post-UV curing was performed at a conveyor speed of 1000 rpm. Thereafter, the laminate was heated at 170°C for 1 hour using a hot air circulation dryer to obtain an evaluation laminate having an interlayer insulating layer formed by curing the photosensitive resin film. (4) Roughening Treatment The evaluation laminate after heating was treated with a swelling liquid "Swelling Dip Securigant P" at 70°C for 5 minutes, and then roughened with a roughening liquid "Dosing Securigant P500J" at 70°C for 10 minutes. Subsequently, a neutralization treatment was performed with a neutralizing liquid "Reduction Conditioner Securigant P500" at 50°C for 5 minutes. Then, a hydrofluoric acid treatment was performed at room temperature for 10 minutes using buffered hydrofluoric acid "LAL1800 SA High Purity Buffered Hydrofluoric Acid." The swelling liquid, roughening liquid, and neutralizing liquid were all manufactured by Atotech Japan Co., Ltd., and the buffered hydrofluoric acid was manufactured by Stella Chemifa Corporation. (5) Plating Treatment After the roughening treatment, the evaluation laminate was subjected to electroless plating treatment at 30°C for 15 minutes using an electroless plating solution "Prigant MSK-DK" (manufactured by Atotech Japan Co., Ltd.). Then, electroplating treatment was performed at 24°C and 2 A / dm using an electroplating solution "Cupracid HL" (manufactured by Atotech Japan Co., Ltd.). 2 The test was carried out at 400°C for 1.5 hours to form plated copper on the interlayer insulating layer. The thickness of the plated copper was 25 μm. (6) Measurement of Adhesion Strength with Plated Copper The adhesive strength with plated copper was measured by perpendicular peel strength at 23°C in accordance with JIS C6481:1996, and this was taken as the adhesive strength with the copper plating. In the table, "floating" refers to peeling between the copper plating and the interlayer insulating layer, or peeling between the interface of the interlayer insulating layer and the copper substrate.
[0130] [Measurement of Desmear Weight Loss] A laminate for evaluation having an interlayer insulating layer was prepared in the same procedure as in the above [Measurement of Adhesion Strength with Copper Plating], and the laminate for evaluation was immersed in a swelling solution, "Swelling Dip Securigant P" (aqueous solution of glycol ethers and sodium hydroxide, manufactured by Atotech Japan Co., Ltd.), at 70°C for 10 minutes, and then washed with water at 25°C for 3 minutes. Next, a roughening solution, "Concentrate Compact P" (KMnO 4 The laminate was immersed in a neutralizing solution "Reduction Shoreusin Securigant P" (aqueous solution of sulfuric acid, manufactured by Atotech Japan Co., Ltd.) at 40°C for 5 minutes, and then washed with water at 25°C for 3 minutes. Thereafter, the laminate was dried at 105°C for 10 minutes to obtain a laminate for evaluation after the desmear treatment. The difference between the weight of the laminate for evaluation before the desmear treatment and the weight of the laminate for evaluation after the desmear treatment [before desmear treatment - after desmear treatment] was defined as the desmear weight loss.
[0131]
[0132] The components used in Table 1 are as follows: [(A) Photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent] A1: "ZXR-1935H" (manufactured by Nippon Kayaku Co., Ltd., acid value: 110 mg KOH / g, weight average molecular weight (Mw): 2,000), a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, which contains an alicyclic skeleton represented by the above general formula (A-1).
[0133] [(B) Blocked isocyanate compounds having a molecular weight of 3,000 or less] B1: "BI7951" (manufactured by LANXESS Corporation), molecular weight: 955, dissociation temperature: 120°C, a blocked isocyanate compound in which the isocyanate group of an isophorone diisocyanate trimer represented by the following formula is blocked with 3,5-dimethylpyrazole (DMP):
[0134] B2: "TPA-B80E" (manufactured by Asahi Kasei Corporation), molecular weight: 766, dissociation temperature: 130°C, a blocked isocyanate compound in which the isocyanate group of a trimer of 1,6-hexamethylene diisocyanate represented by the following formula is blocked with 2-butanone oxime.
[0135] B3: "Coronate 2554" (manufactured by Tosoh Corporation), molecular weight: 844, dissociation temperature: 160°C, a blocked isocyanate compound in which the isocyanate group of a 1,6-hexamethylene diisocyanate trimer represented by the following formula is blocked with ε-caprolactam.
[0136] B4: "MOI-MP" (manufactured by Resonac Corporation), molecular weight: 250, dissociation temperature: 170°C, blocked isocyanate compound obtained by blocking 2-isocyanatoethyl methacrylate with 1-methoxy-2-propanol
[0137] [(B') Blocked isocyanate compounds having a molecular weight of more than 3,000] B'5: "Blonate 1950" (manufactured by Daiei Sangyo Co., Ltd.), molecular weight: more than 3,000, dissociation temperature: 140°C, phenol-blocked polyisocyanate B'6: "Blonate 1901" (manufactured by Daiei Sangyo Co., Ltd.), molecular weight: more than 3,000, dissociation temperature: 140°C, phenol-blocked polyisocyanate B'7: "Blonate 1631V01" (manufactured by Daiei Sangyo Co., Ltd.), molecular weight: more than 3,000, dissociation temperature: 150°C, oxime-blocked polyisocyanate B'8: "Blonate 1227EV" (manufactured by Daiei Sangyo Co., Ltd.), molecular weight: more than 3,000, dissociation temperature: 80 to 100°C, active methylene-based polyisocyanate
[0138] [(C) Thermosetting Resin] C1: "Epotohto (registered trademark) ESN-475V" (manufactured by Nippon Steel Chemical & Material Co., Ltd.), α-naphthol aralkyl type epoxy resin, acid value: 110 mg KOH / g, weight average molecular weight (Mw): 2,000 C2: "NC-3000L" (manufactured by Nippon Kayaku Co., Ltd.), biphenyl aralkyl type epoxy resin, epoxy equivalent: 272 g / eq
[0139] [(D) Photopolymerization initiator] D1: "Irgacure OXE02" (manufactured by BASF Japan Ltd.), an oxime ester-based compound D2: "Omnirad 819" (manufactured by IGM Resins B.V.), an acylphosphine oxide-based compound
[0140] [(E) Crosslinking agent] E1: "DPHA" (dipentaerythritol hexaacrylate)
[0141] [(F) Elastomer] F1: "Ricon (registered trademark) 131MA17" (manufactured by Cray Valley Corporation), maleic acid-modified polybutadiene, number average molecular weight (Mn) 54,000 (catalog value)
[0142] [(G) Inorganic Filler] G1: Spherical fused silica (volume average particle diameter (D 50 ): 0.5 μm)
[0143] [(H) Curing Accelerator] H1: 1-benzyl-2-phenylimidazole
[0144] [(I) Other Components] I1: 4,4'-bis-(diethylamino)benzophenone (sensitizer) I2: t-butylcatechol (polymerization inhibitor)
[0145] As can be seen from Table 1, the photosensitive resin compositions of Examples 1 to 8 of this embodiment all had good compatibility between dielectric properties and developability. On the other hand, the photosensitive resin compositions of Comparative Examples 1 to 5, which did not satisfy the configuration of the photosensitive resin composition of this embodiment, were inferior in either dielectric properties or developability.
[0146] 100A Multilayer printed wiring board 101 Substrate 102 Circuit pattern 103 Photosensitive layer 104 Interlayer insulating layer 105 Via 106 Seed layer 107 Resist pattern 108 Copper circuit layer 109 Solder resist layer
Claims
1. A photosensitive resin composition comprising: (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent; and (B) a blocked isocyanate compound having a molecular weight of 3,000 or less.
2. The photosensitive resin composition according to claim 1, wherein the dissociation temperature of component (B) is 80 to 250°C.
3. The photosensitive resin composition according to claim 1 or 2, wherein the component (B) is a compound containing an isocyanurate ring.
4. The photosensitive resin composition according to claim 3, wherein the component (B) is a compound obtained by blocking a trifunctional isocyanate compound containing an isocyanurate ring with a blocking agent.
5. The photosensitive resin composition according to claim 1 or 2, wherein the content of the component (B) is 1 to 40 mass % based on the total amount of the resin components.
6. The photosensitive resin composition according to claim 1 or 2, wherein the component (A) contains an alicyclic skeleton represented by the following general formula (A-1): (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1 is an integer from 0 to 6. * is a binding site to other structures.) 7. The photosensitive resin composition according to claim 1 or 2, further comprising (C) a thermosetting resin.
8. The photosensitive resin composition according to claim 1 or 2, further comprising (D) a photopolymerization initiator.
9. The photosensitive resin composition according to claim 1 or 2, further comprising (E) a crosslinking agent.
10. The photosensitive resin composition according to claim 1 or 2, further comprising (F) an elastomer.
11. The photosensitive resin composition according to claim 1 or 2, further comprising (G) an inorganic filler.
12. The photosensitive resin composition according to claim 1 or 2, which is used for forming a photovia.
13. A photosensitive resin film comprising the photosensitive resin composition according to claim 1 or 2.
14. A printed wiring board comprising a cured product of the photosensitive resin composition according to claim 1 or 2.
15. A semiconductor package comprising the printed wiring board according to claim 14 and a semiconductor element.
Citation Information
Patent Citations
Thermosetting resin composition, multilayered printed wiring board, and preparation thereof
JP1995304931A
Photosensitive resin composition, and dry film, printed wiring board and method for manufacturing printed wiring board using the composition
JP2017116652A
Photosensitive resin composition, cured film, laminate, transfer film, and touch panel manufacturing method
JP2020056825A
Touch panel sensor and manufacturing method of touch panel sensor
JP2023020450A
Cited By
Photosensitive resin composition, photosensitive element, printed wiring board, and production method for printed wiring board