Production method for welded joint by gas-shielded arc welding of steel plate
The gas-shielded arc welding method for thick steel plates addresses the challenges of high heat input and narrow gap welding by using multiple electrodes and optimizing groove shape, achieving strong and tough welds with reduced defects and improved efficiency.
Patent Information
- Application Number
- PCT/JP2024/012427
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for welding thick steel plates, such as high heat input and narrow gap welding, face challenges in ensuring both high strength and low-temperature impact toughness, particularly in cold environments, and often result in weld defects like hot cracking and poor fusion.
A gas-shielded arc welding method using multiple electrodes with specific wire and shielding gas compositions, where the welding area per layer is controlled to prevent excessive heat input, and the groove shape is optimized to maintain a height-to-width ratio of 1.00 or less, ensuring efficient and defect-free welding of steel plates with thicknesses of 50 mm or more.
The method produces welds with high strength (yield strength of 325 MPa or more) and excellent low-temperature impact toughness (absorbed energy of 30J or more at -40°C), reducing the likelihood of hot cracking and improving welding efficiency.
Smart Images

Figure JP2024012427_03102024_PF_FP_ABST
Abstract
Description
Manufacturing method for welded joints by gas-shielded arc welding of steel plates
[0001] The present invention relates to a method for manufacturing a welded joint by gas-shielded arc welding using steel plate, particularly steel plate having a plate thickness of 50 mm or more.
[0002] With the growth of the energy industry, for example, to improve the efficiency of drilling marine resources and power generation, marine structures and offshore wind turbines constructed on the ocean are becoming larger. As these structures and turbines become larger, the foundations of these facilities must be strong, and the use of thick steel plates with thicknesses of 50 mm or more is being considered. Furthermore, in cold oceans, structures are likely to be hit by waves and drifting ice, so excellent toughness at -40°C is also required. When manufacturing marine structures and offshore turbines using thick plates, improving construction efficiency is an important issue, and highly efficient welding of such thick plates is particularly required.
[0003] High heat input welding has been proposed as a highly efficient welding method for thick plates. However, when high heat input welding is used, it is often difficult to ensure the toughness of the weld metal and the heat-affected zone of the base metal.
[0004] For example, Patent Document 1 discloses a "two-electrode, single-side, single-pass, large heat input submerged arc welding method with excellent toughness of the weld metal." The welding method disclosed in Patent Document 1 uses a specific flux and specific first and second electrode welding wires for a specific steel plate when performing single-side, single-pass welding using two-electrode submerged arc welding on a steel plate having a thickness of 40 mm or more. The steel plate contains, by mass%, 0.02 to 0.2% C, 0.01 to 1% Si, 0.1 to 2.5% Mn, 0.002 to 0.1% Al, and 0.001 to 0.015% N, with P limited to 0.02% or less, S limited to 0.01% or less, and O limited to 0.01% or less, with the balance being Fe and unavoidable impurities. The flux contains, by mass%, 10-25% SiO2, 5-20% MgO, 5-15% CaO, 1-10% CaF2, 5-25% Al2O3, 2-20% TiO2, 10-25% Fe, and 0.1-2.5% BO3. The welding wire contains, by mass%, 0.02-0.2% C, 0.01-1% Si, 0.5-2.5% Mn, 0.002-0.1% Al, 0.005-0.3% Ti, and 0.001-0.015% N, with P limited to 0.02% or less, S limited to 0.01% or less, and O limited to 0.01%, with the balance being Fe and unavoidable impurities. Furthermore, welding is performed under the conditions that the diameter of the welding wire of the second electrode is 6 to 8 mm and the ratio of the cross-sectional area of the welding wire of the first electrode to the cross-sectional area of the welding wire of the second electrode is 35 to 75%. Patent Document 1 describes this as a two-electrode, single-side, one-pass, large heat input submerged arc welding method that produces excellent toughness in the weld metal.
[0005] Furthermore, Patent Document 2 discloses a "two-electrode, large heat input submerged arc welding method." The welding method described in Patent Document 2 is a two-electrode, large heat input submerged arc welding method in which welding is performed using a specific wire and a specific flux. The wire contains, by mass%, 0.02 to 0.18% C, 0.02 to 0.5% Si, 1.15 to 2.2% Mn, 0.1 to 1.0% Mo, 0.1 to 1.5% Ni, and 0.005 to 0.05% Ti, 0.006% or less P, and 0.003% or less S, with the balance being Fe and unavoidable impurities. The flux consists of 13-25% SiO2, 8-20% MgO, 5-13% CaO, 1-7% CaF2, 9-23% Al2O3, 3-11% TiO2, 11-25% Fe, 0.1-0.6% BO3, 1-4.3% Mo, and 1-4.5% Ni. This welding method is said to provide excellent weld metal mechanical performance and good welding workability even in high-heat-input submerged arc welding with a welding heat input of 500 kJ / cm or more, significantly improving the safety of building structures while also significantly increasing welding efficiency.
[0006] For example, Patent Document 3 discloses a "high-efficiency welding method for thick steel plates." According to Patent Document 3, the method includes a processing step of forming an X-shaped groove in a pair of steel materials having a plate thickness of more than 50 mm and not more than 100 mm. Furthermore, the method includes a welding step of performing one pass of welding on each of the front and back surfaces of the pair of steel materials using a multi-electrode submerged arc welding method with two or more and six or less electrodes and a flux. In the welding step, the welding current for the first electrode is an AC current with a waveform ratio of 60% to 90%, and the welding current for the other electrodes is an AC current with a waveform ratio of 70% or more or a negative DC current. The flux used herein contains, by mass ratio relative to the total mass of the flux, 10% to 50% Al2O3 and 16% to 30% SiO2. The welding material also contains a total of 10% to 60% of one or more of MgO, TiO2, CaF2, and MnO, with MgO limited to 40% or less, TiO2 to 20% or less, CaF2 to 30% or less, and MnO to 20% or less. This submerged arc welding method is capable of producing a weld metal with excellent toughness even at low temperatures, and is therefore said to enable the efficient manufacture of foundations for wind power generation facilities to be installed in cold regions.
[0007] On the other hand, narrow gap welding has been proposed as a highly efficient welding method for thick plates. By reducing the cross-sectional area of the groove, it is possible to reduce the welding heat input and ensure the toughness of the weld metal and the base metal heat-affected zone. However, simply welding thick plates using narrow gap welding has the problem of being prone to hot cracking and incomplete fusion.
[0008] To address this issue, for example, Patent Document 4 discloses a "narrow-gap submerged arc welding method." The welding method disclosed in Patent Document 4 involves narrow-gap submerged arc welding of extra-thick steel plates, in which a backing material is abutted against the backside of a narrow groove with a groove angle of 1 to 5° and a root gap of 10 to 14 mm, and steel particles are scattered into the groove to a height of 10 to 15 mm from the backside of the groove. A molten flux is then used, containing, by mass % relative to the total mass of the flux, 50 to 70% AlO, TiO, and CaF, 10 to 20% SiO, with the remainder consisting of CaO, MnO, BaO, KO, NaO, and unavoidable impurities. This narrow-gap submerged arc welding method involves multi-pass welding with one layer per pass. Patent Document 4 achieves excellent welding workability, including good slag removability and bead shape, and enables narrow-gap submerged arc welding without back chipping. Patent Document 4 claims that a sound welded joint free from welding defects such as hot cracking, slag inclusion, and incomplete fusion can be obtained with high efficiency.
[0009] In the submerged arc welding method, which is a narrow gap welding method for thick steel plates as described above, flux must be sprayed in front of the weld before welding and then recovered after welding, requiring separate management of the flux. Furthermore, after welding, the slag formed in the weld must be removed, which reduces workability. In response to this, a narrow gap gas-shielded arc welding method has been proposed, which offers excellent workability during on-site construction.
[0010] For example, Patent Document 5 discloses a narrow-gap gas-shielded arc welding method for joining thick steel plates by narrow-gap multi-layer welding. In the technology described in Patent Document 5, the first layer welding is performed using multi-electrode welding with two or more electrodes, the first electrode and the second electrode are positioned along a predetermined parallel weld line, and the distance between the welding wire tips of the first electrode and the second electrode is controlled to a range of 5 mm to 16 mm. Furthermore, the angle of the line connecting the welding wire tips of the first electrode and the second electrode relative to the direction perpendicular to the weld line is controlled to a range of 45° or less. Furthermore, the fusion depth perpendicular to the weld line at the bottom of the steel is set to 1.5 mm or more. This is said to result in no defects and improved welding efficiency even when groove preparation such as gas cutting or plasma cutting is performed.
[0011] Japanese Patent No. 4673710 JP 2006-212676 A International Publication No. 2013 / 073565 JP 2021-126696 A Japanese Patent No. 6137053 A
[0012] However, the invention of Patent Document 1, which aims to achieve high-efficiency welding through large heat input, aims to provide a welding method that achieves high toughness, with a 2 mm V-notch Charpy absorbed energy of 70 J or more at 0°C. In other words, it is not suitable for use in cold environments of -40°C. Similarly, in Patent Document 2, toughness evaluation is performed at 0°C, and use in cold environments of -40°C is not anticipated. Furthermore, the invention of Patent Document 3 does not mention the low-temperature toughness value of the base metal heat-affected zone (hereinafter, the base metal heat-affected zone is also referred to as the "weld heat-affected zone"), making it unclear whether it can be used in cold environments of -40°C. Furthermore, the invention of Patent Document 4, which aims to achieve high-efficiency welding through narrow gap welding, does not mention the mechanical properties of the weld metal and the weld heat-affected zone. Furthermore, the narrow-gap gas-shielded arc welding method disclosed in Patent Document 5 may cause hot cracks to occur in the center of the weld metal when multi-electrode welding is performed using three or more electrodes.
[0013] The present invention aims to solve the problems of the prior art and to provide a method for manufacturing a narrow-gap welded joint using steel plate with a plate thickness of 50 mm or more by gas-shielded arc welding, which is free of weld defects, has high strength, and has excellent low-temperature impact toughness.
[0014] The term "high strength" as used herein means that the yield strength (0.2% proof stress) at room temperature of the weld metal produced in accordance with the provisions of JIS Z 3111 is 325 MPa or more, and the tensile strength is 520 MPa or more, and further the tensile strength of the welded joint is 520 MPa or more. Also, the term "excellent low-temperature impact toughness" means that the absorbed energy (vE) of the weld metal and the weld heat-affected zone of the welded joint produced in accordance with the provisions of JIS Z 3128 is 520 MPa or more at room temperature. -40 ) is 30J or more.
[0015] [Background to the Invention] In order to achieve the above-mentioned object, the inventors first conducted extensive research into a weld metal shape that enables highly efficient and sound welding of welded joints in steel plates having a plate thickness of 50 mm or more. The total weld length of the foundations of marine structures and offshore wind power plants can exceed 1.0 km per structure, and reducing the number of weld metal layers is effective for highly efficient welding. However, conventional welding methods distribute the welds along the groove walls, which results in low welding efficiency. In contrast, the present invention discovered that highly efficient welding is possible by constructing a multi-layer weld metal with one welding pass per weld metal layer without distributing the welds. However, it was noted that a large welding heat input reduces the low-temperature impact toughness of the weld metal and the base metal heat-affected zone.
[0016] Next, as a result of examining the above-mentioned problem, it was found that the welding area of the weld metal per layer was 120.0 mm 2 It was found that if the welding heat input is less than 120.0 mm, the heat effect on the base metal is sufficiently small, and excellent low-temperature toughness characteristics of the weld can be obtained. 2It was found that hot cracking is likely to occur when the ratio [H / W] of the height H (mm) to the width W (mm) of the weld metal of each weld layer is greater than 1.00, even if the ratio is less than 1.00. This occurs because hot cracking occurs at the junction of dendrites during the solidification process of the weld metal when the solidification direction and the direction of tensile strain during cooling coincide. Therefore, it was found that hot cracking can be suppressed by controlling the ratio [H / W] to 1.00 or less. Furthermore, after extensive research into groove shapes that satisfy the above, it was found that a groove angle of 20° or less and a gap between the base metals of 6 mm or less and 10 mm or less can be satisfied for single-sided welding and double-sided welding, respectively.
[0017] On the other hand, it was found that if the gap between the base materials exceeds 6 mm, there is a possibility that poor fusion may occur during welding of the first layer. From these findings, it was found that the groove shape that can weld steel plates with a thickness of 50 mm or more with high efficiency and soundness is preferably a gap between the base materials of 6 mm or less and a groove angle of 20° or less, regardless of whether single-sided or double-sided welding is used. It was also found that by performing double-sided welding, it is possible to further reduce the groove area.
[0018] [Summary of the present invention] The present invention was completed based on the above findings and further studies, and the gist of the present invention is as follows: [1] A method for manufacturing a welded joint by gas-shielded arc welding of steel plates, wherein the steel plates have a thickness T (mm) of 50 mm or more, the weld metal is made of multiple layers with one pass per layer, and the cross-sectional area A (mm) of the weld metal in the direction perpendicular to the weld line is 2 The ratio [A / p] of the number of weld layers p (layers) to the number of weld layers p (layers) is 120.0 mm 2a ratio [H / W] of a height H (mm) to a width W (mm) of each layer in the weld metal is 1.00 or less; the gas-shielded arc welding is multi-electrode welding using three or more electrodes; tips of the welding wires of first and second electrodes are arranged on different parallel weld lines; one of the first and second electrodes is a negative wire (positive polarity) and the other is a positive wire (reverse polarity); a distance a (mm) between the welding wire tips of the first and second electrodes is 5 to 16 mm; an angle α of a line connecting the welding wire tips of the first and second electrodes with respect to a perpendicular direction to the weld line is 60° or less; and a welding wire containing 0.015 to 0.100 mass % of REM is used for the negative (positive polarity) electrode. [2] The method for manufacturing a welded joint by gas-shielded arc welding of steel plates in [1], wherein an inclination angle Φ of a tip of each of the power feed tips of the first electrode and the second electrode toward the groove surface with respect to a perpendicular direction of the weld line is 0° to 15°, a distance d (mm) between a side end of a tip of each of the welding wires of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm, each of the welding wires is curved in advance to have a radius of curvature in a range of 150 to 300 mm, a third electrode and subsequent electrodes are positioned at the center of the groove behind the first electrode and the second electrode, and a gas containing 60% or more by volume of CO2 gas is used as the shielding gas. [3] In the above [1] or [2], the chemical composition of the steel plate includes, in mass%, C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, O: 0.0100% or less, and N: 0.0100% or less, with the balance consisting of Fe and inevitable impurities, and the chemical composition is such that Ceq and plate thickness (T) defined by the following formula (1) satisfy 0.0004T + 0.25 ≦ Ceq ≦ 0.0004T + 0.45, The dislocation density ρ at a position 1 mm below the surface of the steel plate is 4.0 × 10 14 m -2a method for manufacturing a welded joint by gas-shielded arc welding of steel plate, wherein the average grain size at a position 1 mm below the surface of the steel plate is 15.0 μm or less, and the average grain size at a position 1 mm below the surface of the steel plate is 20.0 μm or less. Ceq=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15 (1) where each element symbol in the above formula (1) represents the content (mass%) of the element, and if the element is not contained, it is set to 0. [4] The method for manufacturing a weld joint by gas-shielded arc welding of steel plates in [3], wherein the chemical composition of the steel plate further includes, in mass%, one or more elements selected from the group consisting of Cu: 2.000% or less, Ni: 2.500% or less, Cr: 1.500% or less, Mo: 1.000% or less, Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less. [5] In any one of [1] to [4] above, the chemical composition of the weld metal is, in mass %, C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, Cu: 0.001 to 2.000%, Ni: 0.001 to 2.500%, Cr: 0.001 to 1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B : 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less, with the balance consisting of Fe and unavoidable impurities.[6] In the above [5], the method for manufacturing a welded joint by gas-shielded arc welding of steel plates, wherein the chemical composition of the weld metal further includes, in mass%, one or more elements selected from the group consisting of W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less.
[0019] According to the present invention, a welded joint can be obtained by welding steel plates having a thickness of 50 mm or more. This narrow-gap welded joint has sound weld metal free from weld defects such as hot cracking and incomplete fusion, and combines high strength with excellent low-temperature impact toughness, and is therefore of great industrial value.
[0020] The welded joints of steel plates according to the present invention are not limited to marine structures and offshore wind turbines, but can also be applied to, for example, shipbuilding, line pipes, construction, and the like.
[0021] FIG. 1 is a schematic cross-sectional view showing the shape of the weld metal of a welded joint according to the present invention. FIG. 2 is a schematic cross-sectional view of the weld metal showing the welding process of a welded joint according to the present invention. FIG. 3 is a partially enlarged view of the schematic cross-sectional view of the weld metal showing the welding process using three electrodes. FIG. 4 is a schematic plan view showing the welding process using three electrodes. FIG. 5 is a schematic plan view showing the welding process using four electrodes. FIG. 6 is a schematic cross-sectional view showing the groove shapes of (a) a V-groove and (b) an X-groove. FIG. 7 is a side cross-sectional view showing the relationship between a gas supply nozzle and an electrode according to the present invention. FIG. 8 is a plan view showing the relationship between a gas supply nozzle and an electrode according to the present invention.
[0022] The present invention will be described in detail below, but the present invention is not limited to the following embodiments.
[0023] [Cross-sectional shape of welded joint] First, the welded joint of steel plates according to the present invention will be described. The welded joint of steel plates according to the present invention is a butt-welded joint of steel plates having a plate thickness T (mm) of 50 mm or more, and the weld metal is made of multiple layers with one pass per layer. In addition, the cross-sectional area A (mm 2 The ratio [A / p] of the number of weld layers p (layers) to the number of weld layers p (layers) is 120.0 mm 2 / layer or less, and the ratio [H / W] of the height H (mm) to the width W (mm) of each layer in the weld metal is 1.00 or less. In the present invention, the weld metal is formed by one welding pass per weld metal layer, without distributing the weld along the groove wall as in conventional welding methods, thereby enabling highly efficient welding.
[0024] Here, the thickness T of the steel plate is specified to be 50 mm or more for application to large structures, etc. There is no particular upper limit to the thickness T, but due to manufacturing constraints, it is preferably 200 mm or less, and more preferably 50 to 160 mm. Here, the weld line refers to an imaginary line when representing a bead or a welded portion as a single line.
[0025] The cross-sectional shape of the above-mentioned welded joint will be explained based on Fig. 1. The cross-sectional area A (mm 2 ) Regarding the welding layers, L1 (first layer) to L p When the number of layers p up to the (outermost surface layer) is applied, the cross-sectional area per layer [A / p] is 120.0 mm 2 That is, the deposition area of the weld metal per layer is 120.0 mm 2 If the ratio [A / p] is set to 80.0 mm or less, the welding heat input will not be excessive, the thermal effect on the base metal will be sufficiently small, and excellent low-temperature toughness characteristics of the weld metal will be obtained. 2 More preferably, the ratio [A / p] is 60.0 mm 2 The lower limit of this ratio [A / p] is not particularly specified, but from the viewpoint of welding efficiency, it is preferably 25.0 mm 2 / layer or more.
[0026] Furthermore, the ratio [H / W] of the height H (mm) to the width W (mm) of each layer in the weld metal is set to 1.00 or less. For example, the ith weld layer (L i ) is the height at H i , width is W i Then, the ratio [H i / W i] is 1.00 or less for all layers from the first layer (initial layer) to the pth layer (outermost layer). Here, the height H of the weld layer represents the distance between the top and bottom of each layer, and the width W represents the width of the weld metal at the center line of the height H (i.e., the distance between fusion lines). The height H of each layer can be determined by cross-sectional macroscopic observation or the like. i and width W i The ratio [H i / W i ] is calculated. If this ratio [H / W] is greater than 1.00, hot cracking is more likely to occur. This is because hot cracking occurs at the dendrite junctions when the solidification direction and the direction of tensile strain during cooling coincide during the solidification process of the weld metal. Therefore, hot cracking can be suppressed by controlling the maximum value of the ratio [H / W] of each layer to 1.00 or less. Preferably, the ratio [H / W] is 0.90 or less. There is no particular lower limit for this ratio [H / W], but from the viewpoint of welding efficiency, it is preferably 0.10 or more, and more preferably 0.20 or more.
[0027] [Groove Shape] The weld metal of the welded joint according to the present invention is a weld metal produced by multi-pass welding with a narrow groove, one layer at a time. In the present invention, the narrow groove means that the groove angle is 20° or less and the maximum groove width between the base materials is 50% or less of the plate thickness T.
[0028] In the case of single-sided welding, the occurrence of hot cracking can be suppressed if the gap between the base materials is 6 mm or less and the groove angle is 20° or less. In the case of double-sided welding, the gap between the base materials is 10 mm or less and the groove angle is 20° or less. However, if the gap between the base materials exceeds 6 mm, there is a possibility of insufficient fusion during the first layer welding. Therefore, the groove shape that can efficiently and soundly weld steel plates 50 mm or more is preferably a gap between the base materials of 6 mm or less and a groove angle of 20° or less, regardless of whether single-sided welding or double-sided welding is used. Furthermore, a groove angle of 4 to 20° is more preferable. Double-sided welding is more preferable because it allows for a smaller groove area. Furthermore, as shown in Figures 6(a) and 6(b), when the gap is 0 mm, i.e., when the base materials are in contact with each other, the width of the weld metal becomes smaller relative to the height of the weld metal, and the bead shape approaches a pear shape, as will be apparent from the examples described below. Therefore, impurities segregated in the final solidification portion of the weld metal lowered the melting point, causing welding strain to concentrate, resulting in hot cracking and poor fusion during welding. Therefore, it is preferable that the gap be greater than 0 mm. More preferably, the gap is 2 mm or greater.
[0029] [Chemical Composition of Steel Plate] Next, the steel plate that is the base material of the welded joint of the present invention will be described. First, the steel plate may be a carbon steel or a low-alloy steel. Next, the chemical composition will be described, and "%" in the chemical composition described below means "mass %" unless otherwise specified.
[0030] [Basic Composition of Steel Plate] The basic chemical composition of the steel plate of the welded joint according to the present invention is as follows.
[0031] Preferably, the steel sheet has a chemical composition containing C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, O: 0.0100% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities.
[0032] The reasons for specifying the above-mentioned chemical composition of the steel sheet in the present invention are explained below. [C: 0.04 to 0.14%] C is the element that can most inexpensively improve the strength of the steel sheet and also contributes to strengthening the austenite grain boundaries. If the C content is less than 0.04%, the austenite grain boundary strength decreases, causing hot tearing of the slab, significantly reducing manufacturability. Furthermore, the strength targeted by the present invention may not be achieved. On the other hand, if the C content exceeds 0.14%, weldability may decrease and toughness may also decrease. Therefore, the C content is preferably 0.04 to 0.14%. It is more preferable that the C content be 0.05 to 0.12%.
[0033] [Si: 0.03 to 0.70%] Si is an effective element for deoxidation, but if the Si content is less than 0.03%, it may not be possible to obtain a sufficient effect. On the other hand, if the Si content exceeds 0.70%, weldability may decrease. Therefore, the Si content is preferably 0.03 to 0.70%. The Si content is more preferably 0.04 to 0.60%.
[0034] [Mn: 0.30 to 2.50%] Mn is an element that can improve the hardenability and strength of steel at low cost. To achieve this effect, it is preferable to contain 0.30% or more of Mn. On the other hand, if the Mn content exceeds 2.50%, weldability may decrease. Therefore, the Mn content is preferably 0.30 to 2.50%. The Mn content is more preferably 0.50 to 2.20%.
[0035] [P: 0.030% or less] P is an element that has a strong effect of embrittling grain boundaries, and if contained in a large amount, it may reduce the toughness of the steel sheet. Therefore, the P content is preferably 0.030% or less. Furthermore, the P content is more preferably 0.025% or less. On the other hand, since a lower P content is preferable, the lower limit of the P content is not particularly limited and may be 0%. However, since P is an element that is inevitably contained in the steel sheet as an impurity, and excessively reducing the P content leads to an increase in refining time and cost, the P content is preferably 0.001% or more.
[0036] [S: 0.020% or less] Since S may reduce the toughness of the steel sheet, the S content is preferably 0.020% or less. Furthermore, the S content is more preferably 0.010% or less. On the other hand, since a lower S content is preferable, the lower limit of the S content is not particularly limited and may be 0%. However, S is an element that is inevitably contained in the steel sheet as an impurity, and excessive reduction in S content leads to an increase in refining time and an increase in costs, so the S content is preferably 0.0001% or more.
[0037] [Nb: 0.001 to 0.100%] Nb is an element that inhibits recrystallization when strain is applied to the austenite structure through solute Nb and finely precipitated NbC, and also has the effect of raising the non-recrystallization temperature range to the higher temperature side. To achieve this effect, the Nb content is preferably 0.001% or more. On the other hand, if the Nb content exceeds 0.100%, there is a possibility that weldability will deteriorate. Therefore, the Nb content is preferably 0.001 to 0.100%. The Nb content is more preferably 0.005 to 0.075%. Furthermore, the Nb content is particularly preferably 0.005 to 0.050%.
[0038] [Al: 0.001 to 0.100%] Al is an element that is effective as a deoxidizer and also has the effect of forming nitrides to reduce the austenite grain size. To achieve this effect, the Al content is preferably 0.001% or more. On the other hand, if the Al content exceeds 0.100%, the cleanliness of the steel material or steel plate may decrease, which may result in a decrease in ductility and toughness. Therefore, the Al content is preferably 0.001 to 0.100%. The Al content is more preferably 0.005 to 0.080% or less.
[0039] [O: 0.0100% or less] O is an element that reduces ductility and toughness, so the O content is preferably 0.0100% or less. On the other hand, since a lower O content is preferable, the lower limit of the O content is not particularly limited and may be 0%. However, O is an element that is inevitably contained in steel sheet as an impurity, and excessive reduction in O content leads to an increase in refining time and an increase in costs, so the O content is preferably 0.0005% or more.
[0040] [N: 0.0100% or less] N is an element that reduces ductility and toughness, so the N content is preferably 0.0100% or less. On the other hand, the lower the N content, the better, so the lower limit of the N content is not particularly limited and may be 0%. However, because N is an element that is inevitably contained in the weld metal as an impurity, excessively reducing the N content leads to increased refining time and higher costs. Therefore, the N content is preferably 0.0005% or more.
[0041] [Optional Composition of Steel Plate] The steel plate for the welded joint of the present invention has the above-mentioned basic composition to obtain the properties intended by the present invention. However, for the purpose of further improving strength and weldability (specifically, the toughness of the welded portion, welding workability, etc.), the steel plate may contain the following optional composition in addition to the above-mentioned basic composition, as necessary.
[0042] One or more elements selected from the group consisting of Cu: 2.000% or less, Ni: 2.500% or less, Cr: 1.500% or less, Mo: 1.000% or less, Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less. Since Cu, Ni, Cr, Mo, Ti, V, B, W, Ca, Mg, and REM are chemical compositions that can be contained arbitrarily, their contents may be 0%.
[0043] [Cu: 2.000% or less] Cu is an element that can improve the strength of a steel sheet without significantly deteriorating the toughness of the steel sheet. On the other hand, if the Cu content exceeds 2.000%, hot cracking due to a Cu-enriched layer formed directly below the scale may become a problem. Therefore, when Cu is contained, the Cu content is preferably 2.000% or less. More preferably, the Cu content is 0.010 to 1.500%.
[0044] [Ni: 2.500% or less] Ni is an element that has the effect of improving the hardenability and toughness of the steel sheet. On the other hand, if the Ni content exceeds 2.500%, an increase in manufacturing costs may become a problem. Therefore, when Ni is contained, the Ni content is preferably 2.500% or less. More preferably, the Ni content is 0.010 to 2.000%.
[0045] [Cr: 1.500% or less] Cr is an element that can improve the hardenability of a steel sheet, thereby improving the strength of the steel sheet. On the other hand, if the Cr content exceeds 1.500%, weldability may be reduced. Therefore, when Cr is contained, the Cr content is preferably 1.500% or less. More preferably, the Cr content is 0.010 to 1.200%.
[0046] [Mo: 1.000% or less] Mo is an element that can improve the hardenability of a steel sheet, thereby improving the strength of the steel sheet. On the other hand, if the Mo content exceeds 1.000%, weldability may be reduced. Therefore, when Mo is contained, the Mo content is preferably 1.000% or less. More preferably, the Mo content is 0.010 to 0.800%.
[0047] [Ti: 0.100% or less] Ti is an element that has the effect of pinning the movement of grain boundaries and suppressing grain growth by precipitating as TiN. On the other hand, if the Ti content exceeds 0.100%, the cleanliness of the steel sheet structure may decrease, resulting in decreased ductility and toughness. Therefore, when Ti is contained, the Ti content is preferably 0.100% or less. More preferably, the Ti content is 0.001 to 0.080%.
[0048] [V: 0.300% or less] V is an element that can improve the hardenability of a steel sheet and also improve the strength of the steel sheet by forming carbonitrides. On the other hand, if the V content exceeds 0.300%, weldability may be reduced. Therefore, when V is contained, the V content is preferably 0.300% or less. More preferably, the V content is 0.010 to 0.250%.
[0049] [B: 0.0100% or less] B is an element that has the effect of improving the hardenability by adding a very small amount, thereby improving the strength of the steel sheet. On the other hand, if the B content exceeds 0.0100%, weldability may be reduced. Therefore, when B is contained, the B content is preferably 0.0100% or less. More preferably, the B content is 0.0001 to 0.0070%.
[0050] [W: 0.500% or less] W is an element that can improve the hardenability of steel and thereby improve the strength of the steel sheet. On the other hand, if the W content exceeds 0.500%, weldability may be reduced. Therefore, when W is contained, the W content is preferably 0.500% or less. More preferably, the W content is 0.010 to 0.400%.
[0051] [Ca: 0.0200% or less] Ca is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Ca content exceeds 0.0200%, the cleanliness may decrease and the toughness of the steel plate may be impaired. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. More preferably, the Ca content is 0.0001 to 0.0180%.
[0052] [Mg: 0.0200% or less] Mg is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Mg content exceeds 0.0200%, the effect of adding Mg becomes saturated and no effect commensurate with the content can be expected, which may be economically disadvantageous. Therefore, if Mg is contained, the Mg content is preferably 0.0200% or less. More preferably, the Mg content is 0.0001 to 0.0180%.
[0053] [REM: 0.0500% or less] REM (rare earth metal) is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the REM content exceeds 0.0500%, the effect of adding REM saturates and no effect commensurate with the content can be expected, which can be economically disadvantageous. Therefore, if REM is contained, the REM content is preferably 0.0500% or less. More preferably, the REM content is 0.0001 to 0.0450%.
[0054] [Remainder of Steel Plate] The steel plate for the welded joint of the present invention has the above-mentioned chemical composition, and the remainder is Fe and inevitable impurities. Examples of inevitable impurities include H, Zn, Re, Co, Sb, and Bi, and a total of 0.0100% or less is acceptable. Furthermore, as long as the above-mentioned basic composition and optional composition are satisfied, elements other than these may be contained, and such embodiments are also within the technical scope of the present invention.
[0055] [Ceq] Furthermore, it is more preferable that the chemical composition of the above steel plate satisfies the following condition: The relationship between Ceq and plate thickness T (mm) satisfies 0.0004T + 0.25 ≦ Ceq ≦ 0.0004T + 0.45. Here, Ceq is defined by the following formula (1), and is an index of hardenability due to contained elements: Ceq = [C] + [Mn] / 6 + ([Cr] + [Mo] + [V]) / 5 + ([Cu] + [Ni]) / 15 (1) where each element symbol in formula (1) represents the content (mass%) of the element, and if the element is not contained, it is set to 0.
[0056] In the present invention, in order to obtain the desired high-strength structure, it is necessary to control the cooling rate and the amount of alloy addition according to the plate thickness T of a certain steel plate. If Ceq is less than (0.0004T + 0.25), the required strength cannot be obtained. On the other hand, if Ceq is greater than (0.0004T + 0.45), the strength becomes too high at the surface of the steel plate, where the cooling rate is faster than at the center of the plate thickness, and the low-temperature impact toughness becomes low. Therefore, it is preferable to satisfy the following relationship: 0.0004T + 0.25 ≦ Ceq ≦ 0.0004T + 0.45. More preferably, it is preferable to satisfy the following relationship: 0.0004T + 0.27 ≦ Ceq ≦ 0.0004T + 0.43.
[0057] [Steel Plate Properties] Here, the properties of the steel plate used in the welded joint according to the present invention will be described. The dislocation density ρ (m -2 ) is 4.0 × 10 14 m -2 It is preferable that the dislocation density ρ (m -2 ) refers to the dislocation length per unit volume present in a metal crystal. The reason for specifying the position 1 mm below the surface of the base material (i.e., "1 mm below the surface of the steel sheet") is from the perspective of the bending workability of the steel sheet. The bending workability of the steel sheet is determined by the ductility of the surface layer structure of the steel sheet. When the dislocation density of the surface layer structure increases due to processing strain during hot rolling, the deformation limit of the surface layer structure decreases, and therefore the bending workability decreases. Therefore, the dislocation density at a position 1 mm below the surface of the steel sheet is set to 4.0 x 10 14 m -2 In addition, since the steel structure usually inevitably contains dislocations, the dislocation density was set to 1.0 × 10 11 m -2 Therefore, the dislocation density is preferably 1.0×10 11 m -2 More preferably, 3.0 × 10 14 m -2 The following is the result.
[0058] It is also preferable that the average crystal grain size at a position 1 mm below the surface of the base material is 15.0 μm or less, and the average crystal grain size at the center position of the plate thickness of the base material is 20.0 μm or less.
[0059] The average grain size refers to the average of all grains at a position 1 mm below the surface of the steel sheet and at the center of the thickness of the steel sheet, where the region surrounded by boundaries with a crystal orientation difference of 15° or more is considered a grain. It can be measured by the method described in the examples below. The finer the grain size of the surface layer structure of the steel sheet, the more improved the toughness of the steel sheet surface. To achieve this effect, it is preferable that the average grain size at a position 1 mm below the surface of the steel sheet be 15.0 μm or less. More preferably, the average grain size at a position 1 mm below the surface of the steel sheet is 13.0 μm or less. Furthermore, the finer the grain size of the steel structure at the center of the thickness of the steel sheet, the more improved the toughness at the center of the thickness of the steel sheet. To achieve this effect, it is preferable that the average grain size at the center of the thickness of the steel sheet be 20.0 μm or less. More preferably, the average grain size at a position 1 mm below the surface of the steel sheet is 15.0 μm or less. Here, in the present invention, "1 mm below the surface of the steel sheet" refers to a depth of 1 mm in the thickness direction from the surface of the steel sheet. The "plate thickness center position" refers to the position at half the plate thickness of the steel plate.
[0060] [Method of manufacturing steel sheet] Next, a method of manufacturing the above-mentioned steel sheet will be described. The steel sheet to which the present invention is directed is obtained by heating, hot rolling, and cooling a slab (steel material) having the above-mentioned composition. After the cooling, an optional tempering step can be further carried out. Various preferable conditions will be described below. However, the manufacturing method is not limited to a specific one, and it is sufficient if it includes the above-mentioned steps.
[0061] In the following description of the manufacturing method, the temperature indicated in "°C" refers to the surface temperature of the slab or steel plate unless otherwise specified. The surface temperature can be measured, for example, with a radiation thermometer.
[0062] In the present invention, the method for producing the slab is not particularly limited, and any of the known methods such as converter, electric furnace, and vacuum melting furnace are suitable. The slab is produced to the desired dimensions by, for example, a continuous casting method. The molten steel may further be subjected to secondary refining such as ladle refining.
[0063] Heating Conditions As described above, it is preferable to heat the manufactured slab to a temperature of 1000 to 1200°C. If the slab heating temperature is less than 1000°C, the coarse NbC precipitated inside the slab during slab casting will not redissolve and will remain. As a result, the effect of raising the temperature of the non-recrystallization temperature range due to the dissolved Nb and the fine NbC reprecipitated during hot rolling will not be obtained. As a result, the effect of grain refinement by controlled rolling will be reduced, and toughness will decrease. On the other hand, if the slab heating temperature exceeds 1200°C, the grain size at the start of hot rolling will become coarse due to austenite grain growth, and therefore the grain size of the final structure after hot rolling will also become coarse, resulting in a decrease in toughness. Therefore, the slab heating temperature is preferably 1000 to 1200°C. The slab heating temperature is more preferably 1030°C or higher, and even more preferably 1170°C or lower.
[0064] Hot Rolling Conditions Next, the heated slab is preferably hot rolled. As described above, in the present invention, the dislocation density and average grain size at a position 1 mm below the steel sheet surface, and the average grain size at the center of the sheet thickness are important. In order to obtain various properties, it is preferable to roll under the following hot rolling conditions.
[0065] Here, the temperature range exceeding (8250 [Nb] + 770°C) at a temperature 1 mm below the surface of the steel plate or at the center of the plate thickness is referred to as the recrystallization temperature range. The temperature range between (8250 [Nb] + 770°C) and the Ar3 temperature at a temperature 1 mm below the surface of the steel plate or at the center of the plate thickness is referred to as the non-recrystallization temperature range. The temperature at the center of the plate thickness of the steel plate can be determined, for example, by measuring with a thermocouple attached to the center of the plate thickness, or by calculating the temperature distribution in the cross section of the steel plate by heat transfer analysis and correcting the result by the surface temperature of the steel plate. The above-mentioned [Nb] represents the content (mass%) of this element in the chemical composition of the steel plate.
[0066] First, the steel sheet temperature at a position 1 mm below the surface is temporarily cooled to Ar3 temperature or below, and then reheated to exceed Ac3 temperature. Next, reduction is performed at a rolling reduction rate of 25% or more in a temperature range where the steel sheet temperature at a position 1 mm below the surface is between (8250[Nb]+770°C) and Ar3 temperature. After that, reduction is performed at a total rolling reduction rate of 15% or less in a temperature range where the steel sheet temperature at a position 1 mm below the surface is less than Ar3 temperature.
[0067] During hot rolling of a heated slab, the surface layer of the steel sheet is once cooled to below the Ar3 temperature, thereby transforming it from austenite to a low-temperature structure such as ferrite. The surface layer of the steel sheet is then reheated to a temperature above the Ac3 temperature, thereby retransforming it to an austenite structure and forming fine austenite in the surface layer of the steel sheet.
[0068] The cooling in this hot rolling step can be performed by, for example, water cooling, air cooling, etc., and any method can be used as long as it can control the temperature to a predetermined level. For example, water cooling is used to cool the steel sheet to the Ar3 temperature or below, and the residence time during which the steel sheet reaches the Ar3 temperature or below at a position 1 mm below the surface is preferably 5 seconds or more and 300 seconds or less. To reheat the steel sheet after cooling, the steel sheet is held in the atmosphere, and the holding time is preferably 30 seconds or more and 600 seconds or less.
[0069] Next, a rolling reduction of 25% or more is applied in the temperature range from (8250 [Nb] + 770°C) to the Ar3 temperature, which is the non-recrystallization temperature range of the steel sheet surface, to introduce working strain into the austenite in the steel sheet surface. These act as transformation nuclei during final cooling, resulting in a microstructure with good toughness. Preferably, the rolling reduction in this temperature range is 30% or more. From the viewpoint of rolling efficiency, the rolling reduction in this temperature range is preferably 80% or less, and even more preferably 70% or less.
[0070] There is no particular upper limit to the number of passes in this temperature range, and as long as the above-mentioned rolling reduction condition is satisfied, the rolling may be performed in multiple passes, for example.
[0071] If the total reduction exceeds 15% in a temperature range where the temperature of the steel sheet surface layer is below the Ar3 temperature, processing strain is introduced into the ferrite structure and pearlite structure that have completed transformation in the steel sheet surface layer, resulting in a decrease in ductility and deterioration of bending workability. Therefore, it is preferable to set the total reduction in a temperature range where the temperature of the steel sheet surface layer is below the Ar3 temperature to 15% or less. More preferably, the total reduction in this temperature range is set to 6% or less.
[0072] By controlling the structure of the steel sheet surface layer under the above-mentioned rolling conditions, the steel sheet surface layer can have a structure with a low dislocation density, a small crystal grain size, and excellent bending workability and toughness.
[0073] Next, it is advisable to apply reduction to the center of the thickness of the steel plate so that the steel plate temperature at the center of the thickness is (8250 [Nb] + 770 ° C) or less and the total reduction rate in the temperature range above the Ar3 temperature is 25% or more.
[0074] While hot rolling the heated slab under the rolling conditions for the steel sheet surface layer described above, a reduction of 25% or more is applied in the temperature range from (8250[Nb]+770°C) to the Ar3 temperature, which is the non-recrystallization temperature range at the center of the thickness of the steel sheet. This introduces working strain into the austenite at the center of the thickness. These act as transformation nuclei during final cooling, resulting in a microstructure with excellent toughness. Therefore, it is preferable to set the total reduction rate at a temperature range below (8250[Nb]+770°C) at the center of the thickness of the steel sheet to 25% or more. More preferably, the total reduction rate in this temperature range is 30% or more. From the viewpoint of rolling efficiency, the total reduction rate in this temperature range is preferably 80% or less, and even more preferably 70% or less.
[0075] Furthermore, if the center of thickness of the steel plate is below the Ar3 temperature, processing strain is introduced into the generated ferrite, reducing toughness. Therefore, it is preferable that the center of thickness of the steel plate is at least the Ar3 temperature.
[0076] In the present invention, the two types of rolling, "rolling on the surface layer of the steel sheet" and "rolling on the center of the sheet thickness", may have overlapping temperature ranges within the respective rolling conditions. In this case, the reduction amounts in the overlapping temperature ranges are integrated as the reduction amounts for the "surface layer of the steel sheet" and the "center of the sheet thickness", and it is sufficient if this integrated reduction amount falls within the range of each rolling condition.
[0077] Here, the total reduction in the recrystallization temperature range at the surface layer of the steel sheet and at the center of the sheet thickness is calculated as follows: Total reduction = (r0 - r1) / r0 x 100 (%) in the temperature range exceeding (8250 [Nb] + 770°C). r0 is the sheet thickness at the start of the first rolling, and r1 is the sheet thickness after the final rolling. The Ar3 temperature and Ac3 temperature can be determined by a Formaster test or the like.
[0078] By controlling the structure through the above-described rolling conditions at the center of the thickness of the steel plate, the center of the steel plate can have a structure with small grain size and excellent toughness.
[0079] Cooling Conditions After the above-mentioned hot rolling, the obtained steel sheet is cooled. In the cooling, the average cooling rate in the temperature range of 700 to 550°C at the center of the thickness of the steel sheet is 2500 x T (where T is the thickness [mm]). -1.7 The cooling is carried out at a rate of °C / sec or more. Examples of the cooling method include water cooling in which water is sprayed from a nozzle at a large flow rate. In the present invention, it is preferable to perform the cooling operation (treatment) on both sides of the steel sheet so that both sides of the steel sheet are cooled under the same conditions.
[0080] The average cooling rate between 700 and 550°C at the center of the plate thickness after hot rolling is 2500 x T -1.7 If the cooling rate is less than 2500 × T / sec, the required strength targeted by the present invention cannot be obtained due to an insufficient cooling rate in the temperature range where transformation from austenite to a low-temperature transformed structure occurs. In addition, coarse ferrite is generated, resulting in a decrease in toughness. Therefore, the average cooling rate in the temperature range of 700 to 550°C at the center of the plate thickness should be 2500 × T -1.7 ° C. / sec or more is preferred.
[0081] In the present invention, after the cooling, tempering can be performed as necessary to further improve strength and toughness. In this case, the steel sheet is tempered at a tempering temperature of 650°C or less after cooling. If the tempering temperature is higher than 650°C, significant softening may occur and the required strength may not be ensured. Therefore, it is preferable to set the tempering temperature to 650°C or less. On the other hand, the lower limit of the tempering temperature is not particularly limited, but it is preferably 200°C or more. The tempering time can be adjusted as appropriate. The tempering temperature here refers to the temperature of the steel sheet surface.
[0082] [Chemical Composition of Weld Metal] Next, the chemical composition of the weld metal of the weld joint of the present invention will be described. Note that "%" regarding the chemical composition means "mass %" unless otherwise specified.
[0083] [Basic Composition of Weld Metal] The basic chemical composition of the weld metal of the weld joint according to the present invention is as follows. Preferably, the weld metal has a chemical composition containing C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, Cu: 0.001 to 2.000%, Ni: 0.001 to 2.500%, Cr: 0.001 to 1.500%, Mo: 0.001 to 1.000%, Ti: 0.001 to 0.100%, V: 0.001 to 0.300%, B: 0.001 to 0.020%, O: 0.050% or less, and N: 0.010% or less, with the balance being Fe and unavoidable impurities.
[0084] The reason why the chemical composition of the weld metal is specified as above in the present invention will now be explained. Note that each component can be added (contained) in the weld metal from either the steel plate or the wire, which is the welding material.
[0085] [C: 0.04 to 0.14%] C is an element that increases the strength of the weld metal through solid solution strengthening and also contributes to strengthening the austenite grain boundaries. If the C content is less than 0.04%, the austenite grain boundary strength decreases, and the strength targeted by the present invention may not be achieved. On the other hand, if the C content exceeds 0.14%, the occurrence of weld cracks may be promoted and the low-temperature impact toughness of the weld metal may also decrease. Therefore, the C content is preferably 0.04 to 0.14%. The C content is more preferably 0.05 to 0.12%.
[0086] [Si: 0.03 to 0.70%] Si acts as a deoxidizer and also has the effect of increasing the viscosity of the weld metal and stably maintaining the bead shape. To achieve this effect, a Si content of 0.03% or more is preferable. However, if the Si content exceeds 0.70%, the low-temperature impact toughness of the weld metal may be reduced. Furthermore, Si segregates during solidification and generates a liquid phase at the solidification cell interface, which may reduce weld crack resistance. Therefore, the Si content is preferably 0.03 to 0.70%. The Si content is more preferably 0.04 to 0.60%.
[0087] [Mn: 0.30 to 2.50%] Mn is an element that can improve the hardenability and strength of weld metal at low cost. To achieve this effect, it is preferable to contain 0.30% or more of Mn. On the other hand, if the Mn content exceeds 2.50%, Mn segregation occurs during solidification, inducing hot cracking, which may reduce weldability. Therefore, the Mn content is preferably 0.30 to 2.50%. The Mn content is more preferably 0.50 to 2.20%.
[0088] [P: 0.030% or less] P is an element that has a strong effect of embrittling grain boundaries. If contained in large amounts, it reduces the low-temperature impact toughness of the weld metal and may segregate at the interface during solidification, inducing hot cracking. Therefore, the P content is preferably 0.030% or less. Furthermore, the P content is more preferably 0.025% or less. On the other hand, since a lower P content is preferable, the lower limit of the P content is not particularly limited and may be 0%. However, since P is an element that is inevitably contained in the weld metal as an impurity, and excessively reducing the P content leads to increased costs, the P content is preferably 0.001% or more.
[0089] [S: 0.020% or less] S reduces the low-temperature impact toughness of the weld metal and may segregate at the interface during solidification, inducing hot cracking. Therefore, the S content is preferably 0.020% or less. Furthermore, the S content is more preferably 0.010% or less. On the other hand, since the lower the S content, the better, the lower limit of the S content is not particularly limited and may be 0%. However, S is an element that is inevitably contained in the weld metal as an impurity, and excessively reducing the S content leads to an increase in costs. Therefore, the S content is preferably 0.0001% or more.
[0090] [Nb: 0.001 to 0.100%] Nb is a carbide-forming element that precipitates carbides and contributes to improving the strength of the weld metal. Furthermore, Nb precipitates carbides at the solidification cell interface of the weld metal, contributing to the suppression of hot cracking. To achieve this effect, the Nb content is preferably 0.001% or more. On the other hand, if the Nb content exceeds 0.100%, the carbides may become coarse and become the starting point for fracture, potentially resulting in a decrease in cryogenic impact toughness. Therefore, the Nb content is preferably 0.001 to 0.100%. The Nb content is more preferably 0.005 to 0.075%. Furthermore, the Nb content is particularly preferably 0.005 to 0.050%.
[0091] [Al: 0.001 to 0.100%] Al acts as a deoxidizer, increases the viscosity of the molten metal, and has the important effect of stably maintaining the bead shape. To achieve this effect, the Al content is preferably 0.001% or more. On the other hand, if the Al content exceeds 0.100%, the cleanliness of the weld metal may decrease, resulting in decreased ductility and toughness. Furthermore, if the viscosity of the weld metal becomes too high, the bead may not spread, increasing defects such as incomplete fusion. Therefore, the Al content is preferably 0.001 to 0.100%. The Al content is more preferably 0.005 to 0.080%.
[0092] [Cu: 0.001 to 2.000%] Cu is an element that can improve the strength of the weld metal without significantly degrading the toughness of the weld metal. To achieve this effect, the Cu content is preferably 0.001% or more. On the other hand, if the Cu content exceeds 2.000%, segregation may occur during solidification, potentially inducing hot cracking. Therefore, when Cu is contained, the Cu content is preferably 2.000% or less. The Cu content is more preferably 0.005 to 1.500%. The Cu content is even more preferably 0.005 to 1.000%, and even more preferably 0.005 to 0.500%.
[0093] [Ni: 0.001 to 2.500%] Ni is an element that has the effect of increasing the hardenability of the weld metal and improving its toughness. To achieve this effect, the Ni content is preferably 0.001% or more. However, Ni is an expensive element, and a content of more than 2.500% is economically disadvantageous. Therefore, when Ni is contained, the Ni content is preferably 2.500% or less. The Ni content is more preferably 0.010 to 2.000%. The Ni content is even more preferably 0.010 to 1.500%, and even more preferably 0.010 to 1.000%.
[0094] [Cr: 0.001 to 1.500%] Cr is an element that can improve the hardenability of the weld metal and thereby improve the strength of the weld metal. To achieve this effect, the Cr content is preferably 0.001% or more. On the other hand, if the Cr content exceeds 1.500%, weldability may be reduced. Furthermore, Cr carbides may be formed, which may lead to a decrease in low-temperature impact toughness. Therefore, when Cr is contained, the Cr content is preferably 1.500% or less. The Cr content is more preferably 0.010 to 1.200%, and even more preferably 0.010 to 1.000%.
[0095] [Mo: 0.001 to 1.000%] Mo is an element that can improve the hardenability of the weld metal and thereby improve the strength of the weld metal. To achieve this effect, the Mo content is preferably 0.001% or more. On the other hand, if the Mo content exceeds 1.000%, the weldability may deteriorate. Therefore, when Mo is contained, the Mo content is preferably 1.000% or less. More preferably, the Mo content is 0.010 to 0.800%.
[0096] [Ti: 0.001 to 0.100%] Ti is an element that precipitates as fine carbonitrides in the weld metal and can improve the strength of the weld metal. To achieve this effect, the Ti content is preferably 0.001% or more. On the other hand, if the Ti content exceeds 0.100%, the cleanliness of the weld metal structure may decrease, resulting in decreased ductility and toughness. Therefore, if Ti is contained, the Ti content is preferably 0.100% or less. More preferably, the Ti content is 0.005 to 0.080%.
[0097] [V: 0.001 to 0.300%] V is an element that can improve the hardenability of the weld metal and also improve the strength of the weld metal by forming carbonitrides. To achieve this effect, the V content is preferably 0.001% or more. On the other hand, if the V content exceeds 0.300%, weldability may decrease. Therefore, when V is contained, the V content is preferably 0.300% or less. More preferably, the V content is 0.005 to 0.250%. The V content is even more preferably 0.005 to 0.150%, and even more preferably 0.005 to 0.100%.
[0098] [B: 0.001 to 0.020%] B is an element that has the effect of improving the hardenability by adding a very small amount, thereby improving the strength of the weld metal. To achieve this effect, the B content is preferably 0.001% or more. On the other hand, if the B content exceeds 0.020%, weldability may decrease. Therefore, when B is contained, the B content is preferably 0.020% or less. More preferably, the B content is 0.005 to 0.018%.
[0099] [O: 0.050% or less] O is an element that reduces ductility and toughness, so the O content is preferably 0.050% or less. On the other hand, the lower the O content, the better, so the lower limit of the O content is not particularly limited and may be 0%. However, O is an element that is inevitably contained in the weld metal as an impurity, and excessively reducing the O content leads to an increase in costs, so the O content is preferably 0.0005% or more.
[0100] [N: 0.010% or less] N is an element that reduces ductility and toughness, so the N content is preferably 0.010% or less. On the other hand, the lower the N content, the better, so the lower limit of the N content is not particularly limited and may be 0%. However, since N is an element that is inevitably contained in the weld metal as an impurity, excessively reducing the N content leads to an increase in costs, so the N content is preferably 0.0005% or more.
[0101] [Optionally Selected Composition of Weld Metal] The weld metal of the present invention can achieve the intended properties of the present invention by using the basic composition described above. However, for the purpose of further improving strength and weldability (specifically, the toughness of the welded portion, welding workability, etc.), the weld metal can contain the following optional selected composition as needed in addition to the basic composition described above.
[0102] One or more elements selected from the group consisting of W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less. W, Ca, Mg, and REM are compositions that can be contained arbitrarily, and therefore the contents of these elements may be 0%.
[0103] [W: 0.500% or less] W is an element that can improve the hardenability of the weld metal, thereby improving the strength of the weld metal. On the other hand, if the W content exceeds 0.500%, the weldability may deteriorate. Therefore, when W is contained, the W content is preferably 0.500% or less. Preferably, the W content is 0.001% or more. More preferably, the W content is 0.001 to 0.300%.
[0104] [Ca: 0.0200% or less] Ca is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Ca content exceeds 0.0200%, the cleanliness may decrease and the toughness of the weld metal may be impaired. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. More preferably, the Ca content is 0.0001 to 0.0180%. Even more preferably, the Ca content is 0.0001 to 0.0100%.
[0105] [Mg: 0.0200% or less] Mg is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the Mg content exceeds 0.0200%, the effect of adding Mg becomes saturated and no effect commensurate with the content can be expected, which may be economically disadvantageous. Therefore, when Mg is contained, the Mg content is preferably 0.0200% or less. More preferably, the Mg content is 0.0001 to 0.0180%. Even more preferably, the Mg content is 0.0001 to 0.0150%.
[0106] [REM: 0.0500% or less] REM (rare earth metal) is an element that improves weldability by forming oxysulfides that are highly stable at high temperatures. On the other hand, if the REM content exceeds 0.0500%, the effect of adding REM saturates and an effect commensurate with the content cannot be expected, which may be economically disadvantageous. Therefore, when REM is contained, the REM content is preferably 0.0500% or less. More preferably, the REM content is 0.0001 to 0.0450%.
[0107] [Remainder Composition of Weld Metal] The remainder of the weld metal of the present invention, other than the above chemical composition, is Fe and inevitable impurities. Incidentally, inevitable impurities refer to components that are mixed in from the welding wire, steel sheet, surrounding atmosphere, etc. during the welding process and are not intentionally included. Examples of inevitable impurities include H, Zn, Re, Co, Sb, and Bi, and a total of 0.0100% or less is acceptable. Furthermore, elements other than these may be contained as long as the above-mentioned basic composition and optional composition are satisfied, and such embodiments are also within the technical scope of the present invention.
[0108] [Mechanical Properties of Weld Metal] Here, preferred mechanical properties of the weld joint according to the present invention will be described. It is preferable that the weld metal having the above-mentioned chemical composition and produced in accordance with JIS Z 3111 has a room temperature yield strength (0.2% proof stress) of 325 MPa or more and a tensile strength of 520 MPa or more in a tensile test. It is also preferable that the room temperature tensile strength of the weld joint is 520 MPa or more. In the present invention, "room temperature" refers to 25.0°C.
[0109] Furthermore, the absorbed energy (vE) of a V-notch Charpy impact test at a test temperature of -40°C for the weld metal and weld heat affected zone of a welded joint prepared in accordance with the provisions of JIS Z 3128 was measured. -40 If the strength is less than 30 J, the toughness of the structure containing the joint will be low and fracture may occur more easily.
[0110] [Method for manufacturing a welded joint] Next, a method for manufacturing a welded joint according to the present invention will be described. That is, a method for manufacturing a welded joint formed by gas-shielded arc welding the above-described steel plates will be described. First, steel plates having the above-described chemical composition and a thickness of 50 mm or more are prepared. Then, groove preparation is performed so that the prepared steel plates form a predetermined groove shape. The groove shape to be formed does not need to be particularly limited, and examples of groove shapes that are commonly used for welded structures include V-grooves, square grooves, X-grooves, and K-grooves.
[0111] Next, the grooved steel plates are welded together to form a multi-layer weld metal, preferably three or more layers, with one welding pass per layer, to form a weld joint. If welding is performed with one or two layers of weld metal, the heat generated during welding will not spread uniformly within the groove, causing welding defects. The welding wire used is not particularly limited as long as it can form a weld metal with the desired properties.
[0112] [Gas-shielded arc welding method] The welding method used in the present invention is a multi-electrode gas-shielded arc welding method that can stably produce narrow-gap welded joints that have weld metal free of welding defects and that have high strength and excellent low-temperature impact toughness.
[0113] The gas-shielded arc welding method of the present invention requires proper control of the welding conditions described below with reference to the drawings.
[0114] [Welding Conditions (Basic Conditions and Optional Selective Conditions)] (1) Basic Welding Conditions (a) Multi-layer welding is performed using three or more electrodes. (b) The tips of the welding wires of the first and second electrodes are arranged on different parallel welding lines. (See FIG. 4) (c) One of the first and second electrodes is the negative wire (positive polarity), and the other is the positive wire (reverse polarity). (d) The distance a (mm) between the tips of the welding wires of the first and second electrodes is 5 to 16 mm. (See FIG. 4) (e) The angle α of the line connecting the tips of the welding wires of the first and second electrodes with respect to the perpendicular direction to the welding line is 60° or less. (See FIG. 4) (f) A welding wire containing 0.015 to 0.100 mass % of REM is used for the electrode that is the negative wire (positive polarity). (2) Optionally Selected Welding Conditions (g) The inclination angle Φ of the tip of each current contact tip of the first electrode and the second electrode toward the groove surface relative to the perpendicular direction of the weld line is 0° to 15° (see Figure 3). (h) The distance d (mm) between the side end of the tip of each welding wire of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm (see Figures 2 and 3). (i) Each welding wire is pre-bent to have a radius of curvature in the range of 150 to 300 mm. (j) The third and subsequent electrodes are positioned at the center of the groove behind the first and second electrodes (see Figures 4 and 5). (k) A gas containing 60% or more by volume of CO2 gas is used as a shielding gas.
[0115] [Individual Welding Conditions] The above welding conditions will be explained in more detail below.
[0116] (a) Multi-layer welding with three or more electrodes In multi-layer welding of narrow gaps, when one pass is performed per layer, heat tends to concentrate at the center of the groove with one electrode, resulting in insufficient melting of the steel at the groove surface, leading to defects due to poor fusion (cold lap) and spatter and slag entrapment on the groove surface. In particular, the temperature of the steel is low in the first layer welding, resulting in a small melting depth, making defects due to poor fusion more likely to occur. Furthermore, from the viewpoint of improving welding efficiency, multi-electrode welding with three or more electrodes is advantageous. However, from the viewpoint of welding efficiency, four or fewer electrodes are preferable. Three electrodes are most preferable.
[0117] (b) Electrode Arrangement The tips of the welding wires of the first electrode and the second electrode are arranged on different parallel welding lines. Fig. 4 shows an example of the arrangement of the welding wire tips in the case of three electrodes, and Fig. 5 shows an example of the arrangement of the welding wire tips in the case of four electrodes. As shown in these figures, the welding wire tip 5c of the first electrode 5 and the welding wire tip 6c of the second electrode 6 are arranged on different parallel welding lines 9. In this way, the arcs emitted from the welding wires of the first electrode and the second electrode spread in the width direction of the weld metal to be formed.
[0118] (c) Electrode Polarity One of the first electrode and the second electrode is wire-negative (positive polarity), and the other is wire-positive (reverse polarity). If the first electrode and the second electrode have the same polarity, for example, if both the first electrode and the second electrode are wire-positive, the arcs will be inward due to the electromagnetic force of attraction between them, causing heat to concentrate at the center of the groove and preventing sufficient melting at the groove surface. However, if the first electrode and the second electrode have different polarities and the tips of the welding wires described in (b) above are arranged on different lines parallel to the weld line, the magnetic fields due to the welding currents will generate strong outward electromagnetic forces, causing the arcs to repel each other. As a result, it is possible to obtain sufficient melting depth at the groove surface. Based on this result, in the present invention, the polarity of the first electrode and the second electrode is wire-negative (positive polarity) and the other is wire-positive (reverse polarity).
[0119] (d) Distance a between the tips of the first and second electrodes: 5 to 16 mm The distance a between the tips of the welding wires 5 b and 6 b supplied from the power feed tips 5 a and 6 a at the tip of each welding torch of the first electrode 5 and the second electrode 6 (hereinafter simply referred to as the "distance between the tips of the first and second electrodes") needs to be controlled within a range of 5 to 16 mm. Note that the distance a between the tips of the welding wires 5 b and 6 b here refers to the distance between the centers of the welding wire tips 5 c and 6 c of each electrode, as shown in FIG. 4.
[0120] If the distance a between the first and second electrode tips is less than 5 mm, the current (electrons) flowing between the electrodes reduces the heat of the arc itself, preventing sufficient melting of the groove surface. On the other hand, if the distance a exceeds 16 mm, the outward electromagnetic force between the electrodes decreases inversely proportional to the distance, and the arc repulsion force required to overcome the inward electromagnetic force generated by the current flowing through the groove surface is not obtained. As a result, the arcs are directed inward, and heat is concentrated at the center of the groove. As a result, sufficient melting of the groove surface is not achieved.
[0121] Furthermore, in narrow gap welding, suppressing welding defects due to adhesion of spatter to the groove surface is an issue, but by controlling the welding conditions (b), (c), and (d) described above, the spatter is absorbed into the respective molten metals. This suppresses adhesion of spatter to the groove surface, making it possible to obtain a sound weld.
[0122] From the above, the distance a between the first and second electrode tips is controlled to be in the range of 5 to 16 mm. However, in order to obtain a deeper and more stable melting depth of the groove face by a stronger repulsion of the arc, it is preferable to control the distance a between the first and second electrode tips to be in the range of 5 to 8 mm.
[0123] (e) First-Second Electrode Tip Arrangement Angle α: 60° or Less In the narrow-gap gas-shielded arc welding method of the present invention, melting of the groove surface is ensured by utilizing the repulsion of the arc. Here, referring to FIG. 4 , the angle α of the line connecting the welding wire tips 5c and 6c of the first electrode 5 and the second electrode 6 relative to the perpendicular direction of the weld line 9 (hereinafter, also simply referred to as the "first-second electrode tip arrangement angle") will be described. If this angle α exceeds 60°, sufficient repulsive force of the arc cannot be obtained, and sufficient melting cannot be achieved at the groove surface. Therefore, the angle α is limited to 60° or less. Preferably, the angle α is 45° or less. Note that the angle α may be 0° (i.e., parallel to the perpendicular direction of the weld line). More preferably, the angle α is 25° or greater.
[0124] (f) REM Content of Welding Wire Used for Positive Electrode: REM (rare earth element) is an element effective in reducing the size of inclusions during steelmaking and casting and improving the toughness of weld metal during welding. Furthermore, when welding is performed using a welding wire containing REM as the negative (positive) electrode, droplet size reduction and stable transfer can be achieved. This droplet transfer refinement suppresses spatter generation and enables stable gas-shielded arc welding even with positive polarity. For this reason, in the present invention, a steel wire containing 0.015 to 0.100 mass% of REM (rare earth element) is supplied to the positive electrode. Note that elements other than REM (rare earth element) are typically contained in appropriate amounts depending on the grade (steel type) of welding wire, as specified in JIS Z 3312. If the REM (rare earth element) content is less than 0.015 mass%, the droplet size reduction and stable transfer cannot be achieved. On the other hand, if the REM content exceeds 0.100 mass%, cracks occur during the wire manufacturing process, making it difficult to manufacture the welding wire. For this reason, the REM (rare earth element) content is limited to the range of 0.015 to 0.100 mass%. Preferably, the REM content is 0.025 to 0.050 mass%.
[0125] Welding wire for gas-shielded arc welding is generally manufactured with a diameter in the range of 0.6 to 2.0 mm. When welding with the same current, the thinner the wire diameter, the higher the deposition rate due to Joule heat. Therefore, to achieve highly efficient welding, it is preferable to select a relatively thin wire diameter. On the other hand, if the wire diameter is too thin, the wire will soften due to Joule heat, making welding unstable. For this reason, it is preferable to use a welding wire with a diameter in the range of 1.0 to 1.6 mm.
[0126] The above welding conditions are the basic welding conditions for gas-shielded arc welding according to the present invention, and by performing welding under the above-mentioned conditions, it is possible to obtain a narrow-gap welded joint that is free of weld defects, has high strength, and has excellent low-temperature impact toughness.
[0127] Furthermore, in the present invention, by satisfying the optional welding conditions described below in addition to the basic welding conditions described above, it becomes possible to more reliably obtain narrow gap welded joints that are free of welding defects, have high strength, and have excellent low-temperature impact toughness.
[0128] (g) Inclination angle Φ of the power feed tip: 0° to 15°. Arcs have directionality and tend to point in the direction of the electrode welding wire tip. To effectively utilize this arc directionality in melting the groove face, it is advantageous to orient the welding wire tip toward the groove face. The direction of the welding wire tip varies significantly depending on the feed angle of the welding wire supplied from the power feed tip at the electrode tip. Therefore, as shown in FIG. 3 , the feed angle of the welding wires 5b and 6b of the first and second electrodes 5 and 6 relative to the bottom of the weld metal 2 is the same as the inclination of the tips of the power feed tips 5a and 6a of the electrodes. Therefore, by adjusting the inclination angle Φ of the power feed tip tip toward the groove face 4 (hereinafter also referred to as the "inclination angle Φ of the power feed tip"), the feed angle of the welding wire supplied from each power feed tip relative to the bottom of the weld metal can be controlled. Here, the bottom of the weld metal refers to the bottom of each weld layer of the weld metal, near the boundary with the previous weld layer.
[0129] When the inclination angle Φ of the power feed tips of the first and second electrodes is less than 0° (i.e., when they are inclined away from the groove face), the current flows through a path with less resistance. As a result, the arc creeps up the electrode wire (i.e., this is also known as "arc creep"), making it difficult to maintain the desired fusion at the groove face, particularly at the bottom. On the other hand, when the inclination angle Φ of the power feed tip exceeds 15°, the arc is directed too far toward the groove face, resulting in a convex weld bead shape. This results in insufficient arc fusion in the first and subsequent layers of welding, making welding defects more likely to occur. For this reason, the inclination angle Φ of the power feed tip is preferably in the range of 0° to 15°. More preferably, the inclination angle Φ of the power feed tip is 5° to 12°.
[0130] (h) Distance d between the tip end of the welding wire and the groove surface: 0.5 to 3.0 mm In order to obtain a deeper and more stable fusion depth at the bottom of the weld metal, it is preferable to set the distance d between the side ends of the tips 5c and 6c of the welding wire of the first electrode 5 and the second electrode 6 and the groove surface 4 of the steel plate to 0.5 to 3.0 mm, as shown in Figures 2 and 3. This is because if this distance d is less than 0.5 mm, the arc will be generated not between the wire and the bottom of the weld metal but between the wire and the groove surface, and the previous weld layer and the groove surface will not be able to melt efficiently at the bottom of the weld metal.
[0131] On the other hand, if the distance d exceeds 3.0 mm, the arc will be separated from the groove surface, and the groove surface will not be melted efficiently. This distance d is more preferably in the range of 0.5 to 2.0 mm, and even more preferably in the range of 0.5 to 1.0 mm. Note that the "side end of the tip of the welding wire" referred to here refers to the side end closest to the groove surface of the steel sheet to be melted by each electrode, and the distance d refers to the shortest distance between that side end and the groove surface 4.
[0132] (i) Radius of curvature of the welding wire to be fed: 150 to 300 mm In the present invention, in order to control the feed angle (Φ) of the welding wires 5 b and 6 b fed from the power feed tips at the tips of the welding torches of the first electrode 5 and the second electrode 6, power feed tips 5 a and 6 a with their tips inclined toward the groove surface are used, as shown in Fig. 3. In this case, the welding wires 5 b and 6 b pass through the power feed tips with their tips inclined toward the groove surface, and in order to pass through them more smoothly, it is preferable to curve the welding wire to be fed in advance using a so-called three-point roller or the like (not shown).
[0133] The radius of curvature when pre-bending is preferably 150 to 300 mm. If the radius of curvature is less than 150 mm, the wire feed resistance increases, making it difficult to stably feed the welding wire and maintain an arc. On the other hand, if the radius of curvature of the welding wire exceeds 300 mm, the wire feed resistance is not effectively reduced when the tip of the power feed tip is bent, making it difficult to stably feed the welding wire and maintain an arc. Therefore, the radius of curvature of the welding wire fed to the power feed tips of the first and second electrodes is preferably 150 to 300 mm. More preferably, the radius of curvature of the welding wire is 175 to 275 mm.
[0134] (j) Arrangement of Third and Subsequent Electrodes In order to avoid the risk of hot cracking, it is effective to arrange the welding wire tips (7c and 8c) of the third and subsequent electrodes in the center of the groove behind the welding wire tips (5c and 6c) of the first and second electrodes, as shown in Figures 4 and 5. This also makes it possible to further reduce the number of layers, thereby significantly reducing the risk of stacking faults in multi-layer welding.
[0135] The distance b between the welding wire tip 6c of the second electrode and the welding wire tip 7c of the third electrode is preferably in the range of 10 to 100 mm, more preferably 10 to 60 mm, even more preferably 10 to 40 mm, and most preferably 10 to 25 mm. Furthermore, the distance c between the welding wire tip 7c of the third electrode and the welding wire tip 8c of the fourth electrode is also preferably in the range of 10 to 100 mm, more preferably 10 to 60 mm, even more preferably 10 to 40 mm, and most preferably 10 to 25 mm.
[0136] Furthermore, the polarity of the third electrode and thereafter is not particularly limited, and may be either wire negative (positive polarity) or wire positive (reverse polarity).
[0137] (k) Shielding Gas Composition Since the oxygen content in the weld metal is also greatly affected by the shielding gas composition, it is preferable to use a shielding gas containing 60% by volume or more of CO gas and the remainder as an inert gas such as Ar. More preferably, the shielding gas is 100% by volume of CO gas.
[0138] The nozzle for supplying the shielding gas is preferably arranged as follows.
[0139] In order to ensure good shielding in gas-shielded arc welding, which is the object of the present invention, suppress the inclusion of nitrogen from the atmosphere, and reduce the deterioration of the low-temperature toughness of the weld metal and the occurrence of welding defects, a shielding gas supply nozzle 11 is positioned in front of the welding direction of the first electrode 5 in the groove.
[0140] A detailed description will be given based on Figures 7 and 8. Figure 7 is a side cross-sectional view showing a schematic arrangement of the shielding gas supply nozzle and the electrodes, and Figure 8 is a plan view showing the same arrangement as in Figure 7, viewed from above. These figures show an example of three-electrode welding in which a first electrode 5, a second electrode 6, and a third electrode 7 are arranged. A shielding gas supply nozzle 11 is arranged in front of the first electrode 5 in the welding direction, and a gas outlet 11a from which the shielding gas is discharged is directed toward the first electrode 5. During welding, the shielding gas supply nozzle 11 moves along the welding direction in conjunction with the three electrodes, and arc welding is performed while supplying shielding gas.
[0141] The cross-sectional area N of the gas discharge port 11a is 100 mm 2 ~350mm 2 It is preferable that the range is:
[0142] The cross-sectional area N of the gas discharge port 11a is 100 mm 2 If the cross-sectional area N of the gas discharge port 11a is less than 350 mm, the area onto which the gas is blown becomes small, resulting in insufficient shielding. 2 If the cross-sectional area exceeds 100 mm, the gas will be dispersed to areas other than the bottom of the groove, resulting in insufficient shielding. 2 ~350mm 2 This cross-sectional area N is more preferably 125 mm 2 ~300mm 2 is.
[0143] The supply flow rate Q of the shielding gas is preferably in the range of 35 L / min to 70 L / min.
[0144] If the shielding gas supply flow rate Q is less than 35 L / min, the amount of gas supplied to the molten pool 12 will be insufficient, resulting in poor shielding performance. On the other hand, if the shielding gas supply flow rate Q exceeds 70 L / min, the shielding gas flow rate will be excessive, increasing the likelihood of welding defects. Therefore, the shielding gas supply flow rate Q is preferably set to 35 L / min to 70 L / min. This supply flow rate Q is more preferably set to 40 L / min to 65 L / min. The shielding gas flow rate varies depending on the combination of the shielding gas supply flow rate Q and the cross-sectional area N of the gas outlet, but a flow rate of 2 m / s to 7 m / s is preferred.
[0145] The preferred cross-sectional shape of the tip of the gas discharge port is as follows.
[0146] 7 and 8 show only the tip portion of the shielding gas supply nozzle 11, the cross-sectional shape of the tip of the gas discharge port 11 a is not particularly limited. However, because a nozzle with a larger cross-sectional area can be inserted into the groove when the cross-sectional shape of the tip is rectangular rather than circular, it is preferable that the cross-sectional shape of the tip of the gas discharge port be rectangular.
[0147] The angle X formed between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is preferably 40° to 80° (see FIG. 7).
[0148] If the angle X between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is less than 40°, the shielding gas does not sufficiently reach the third electrode 7, resulting in insufficient shielding. On the other hand, if the angle X exceeds 80°, the gas is dispersed to areas other than the bottom of the groove, resulting in insufficient shielding. Therefore, the angle X between the cross section of the gas discharge port 11a and the bottom of the groove to be welded is preferably 40° to 80°. This angle X is more preferably 45° to 75°.
[0149] Furthermore, the distance Y between the tip of the gas discharge port 11a and the welding wire tip 5c of the first electrode 5 is preferably 40 mm or less (see FIGS. 7 and 8). The distance between the gas discharge port 11a and the electrode is also effective for shielding. That is, if the distance Y between the tip of the gas discharge port 11a (specifically, the portion closest to the electrode) and the welding wire tip 5c of the first electrode 5 exceeds 40 mm, the shielding gas will not sufficiently reach the entire electrode, and the gas will disperse to areas other than the bottom of the groove, resulting in insufficient shielding. Therefore, the distance Y is preferably 40 mm or less. The distance Y is more preferably 5 mm to 35 mm.
[0150] Other welding conditions are not particularly specified except for the above-mentioned welding conditions, and may be, for example, a welding current of 280 to 360 A, a welding voltage of 32 to 37 V, a welding speed of 30 to 90 cm / min, a wire extension length of 15 to 30 mm, and a welding heat input per pass of 10 to 50 kJ / cm.
[0151] In addition, when multi-layer welding is performed using three electrodes, the following welding current conditions are more suitable. First, the current value I1 of the first electrode and the current value I2 of the second electrode are set to a range of 280 A to 360 A. If the current values I1 and I2 of the first and second electrodes are less than 280 A, the groove faces cannot be sufficiently melted, increasing the likelihood of incomplete fusion. On the other hand, if the current values I1 and I2 exceed 360 A, the height of the weld bead increases, resulting in a vertically elongated bead, increasing the risk of hot cracking. Therefore, the range of the current value I1 of the first electrode and the current value I2 of the second electrode is preferably 280 A to 360 A, and more preferably 280 A to 340 A.
[0152] Next, the current value I3 of the third electrode is controlled for each layer of the multi-layer welding based on the relationship with the width of the weld bead of each layer, thereby suppressing hot cracking that occurs in each weld layer, which is an object of the present invention. Specifically, the current value I3 of the third electrode for the i-th layer is i is set to a range that satisfies the following formula (2): I3 i ≦30×G i-1 -10 ... (2) Here, I3 i : current value of the third electrode of the i-th layer [A], G i-1 : Width [mm] of the weld bead formed by welding the layer immediately before the i-th layer (i.e., the (i-1)th layer), where i is a natural number of 2 or greater.
[0153] Current value I3 of the third electrode i When the weld bead width G becomes larger, the height of the weld bead becomes larger and the bead becomes longer, which increases the risk of hot cracking. i is the width G of the weld bead formed by welding one layer before (i.e., the i-1th layer). i-1 The width of the weld bead increases with the number of layers due to the influence of the third electrode current. Therefore, the relationship between the width of the weld bead and the current value of the third electrode was examined, and a favorable range was found, from which the above formula (2) was derived. In other words, within the range that satisfies formula (2), the formation of a vertically elongated weld bead is suppressed, and the excellent effect of preventing hot cracking can be obtained.
[0154] The present invention will be further described below with reference to examples. However, the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention.
[0155] First, molten steel having the chemical composition shown in Table 1 was melted, and a steel material (slab) was produced by continuous casting or the like. The composition in Table 1 becomes the chemical composition of the steel plate that becomes the base material. Note that the "-" column in Table 1 indicates that the element is not intentionally added, and includes not only cases where the element is not contained (0%), but also cases where the element is unavoidably contained.
[0156]
[0157] Next, the obtained slab was sequentially subjected to the steps of heating, hot rolling, and cooling to obtain steel plates having thicknesses T (mm) shown in Tables 2-1 and 2-2. The rolling start temperature in the hot rolling step was in the range of 990 to 1140°C at the surface layer of the steel plate, and the rolling finish temperature was in the range of 670 to 830°C at the surface layer of the steel plate. Regarding the above steel plate temperatures, the surface temperature was measured with an emissivity thermometer, and the temperature at the center of the plate thickness was measured by attaching a thermocouple at the center of the plate thickness. Furthermore, cooling after hot rolling was performed by spraying water at a large flow rate from the front and back surfaces of the steel plate.
[0158] On the other hand, molten steel was melted in a vacuum melting furnace and cast to obtain a steel ingot, which was then heated to 1200°C and then hot and cold worked to produce a 1.2 mm diameter gas-shielded arc welding wire. The wire steel types (grades) used were YGW18 and G 59J A 1.
[0159] Next, the above steel plates were grooved to obtain the groove shapes shown in Tables 2-1 and 2-2. Note that the groove shapes V (groove) in Tables 2-1 and 2-2 are the shapes shown in FIG. 6( a), and X (groove) are the shapes shown in FIG. 6( b). Furthermore, gas-shielded arc welding was performed using the welding wire obtained above to form weld metal in the above-mentioned groove, thereby obtaining a welded joint. The layering conditions at this time (specifically, whether one pass or two passes per layer was performed) are also shown.
[0160]
[0161]
[0162] The specific welding conditions for the gas-shielded arc welding were as follows: no preheating, flat welding, welding current: 180 to 390 A, welding voltage: 22 to 38 V, welding speed: 40 to 120 cm / min, and interpass temperature: 200° C. or less. The number of weld metal layers was three or more.
[0163] Tables 3-1 to 3-4 show the welding conditions for each electrode in gas-shielded arc welding. The welding electrodes were positioned as shown in Figures 4 and 5. The wire tip spacing b between the second and third electrodes was 18 mm, and the wire tip spacing c between the third and fourth electrodes was 10 mm. The "2 to 4 passes per layer" shown in the lamination conditions for Joint No. 35 in Table 3-3 specifically refers to one pass for the first and second layers, two passes for the subsequent third to eighth layers, three passes for the subsequent ninth to fourteenth layers, and four passes for the fifteenth to final layers. In the "Polarity" column of Tables 3-1 and 3-3, negative wire is listed as "positive polarity" and positive wire is listed as "reverse polarity."
[0164]
[0165]
[0166]
[0167]
[0168] [Evaluation of weld metal shape] Vertical cross-sectional macros were taken at positions 1 / 4D, 2 / 4D, and 3 / 4D in the weld line direction of the welded joint and observed. Here, D refers to the length from one end of the weld line to the other. The 1 / 4D position represents a position 1 / 4 of D away from one end of the weld line in the welding direction. Similarly, the 2 / 4D position is the center position of the weld line, and the 3 / 4D position represents a position 3 / 4 of D away in the welding direction.
[0169] Then, the cross-sectional area A (mm 2) was measured and divided by the number of weld layers p (layers), and the ratio [A / p] of the cross-sectional area A of the weld metal to the number of weld layers p was recorded.
[0170] The distance between the top and bottom of each layer of the weld metal was measured to determine the height H (mm) of each layer of the weld metal, and the width of the weld metal at the center line of each height H (i.e., the distance between the fusion lines) was measured to determine the width W (mm) of the weld metal. The ratio [H / W] between these was determined for each layer, and the maximum value of the ratio [H / W] for the entire weld metal was recorded. Furthermore, as mentioned above, a narrow groove means that the groove angle is 20° or less and the maximum groove width between the base metals is 50% or less of the plate thickness T, so the ratio [Wmax / T] of the maximum groove width Wmax to the plate thickness T was determined.
[0171] [Measurement of dislocation density of steel sheet] A sample was taken from each steel sheet at the center position in the longitudinal and width directions, 1 mm below the surface of the steel sheet, to be the evaluation surface. The surface of the sample was mirror-polished by mechanical polishing and electrolytic polishing, and the dislocation density ρ (m -2 (Reference 1) G. K. Williams and W. H. Hall: Acta Metall., 1 (1953), 22
[0172] [Average Grain Size] As described above, samples were taken from each steel sheet at a position 1 mm below the surface at the center of the longitudinal and width directions and at the longitudinal cross section of the steel sheet at the center of the sheet thickness, so that the evaluation surfaces were the test surfaces. The surfaces of the obtained samples were mirror-polished with a colloidal silica finish and measured by EBSP (electron backscattered beam diffraction) under the following conditions. The measurement area was 300 μm × 400 μm, and the measurement step size was 1 μm. From the obtained crystal orientation map, the circle-equivalent diameter of the structure surrounded by high-angle grain boundaries where the crystal orientation difference with adjacent grains was 15° or more was determined, and the average value of the circle-equivalent diameter in the measurement area was taken as the average grain size. Note that the steel sheets of the present invention had a structure mainly composed of bainite and pseudo-polygonal ferrite in both the surface layer and the center of the sheet thickness.
[0173] [Evaluation of Weld Defects] Furthermore, radiographic testing was carried out on the obtained welded joints in accordance with JIS Z 3104 to evaluate the presence or absence of weld defects. The weld defects were judged as falling under Class 1 of JIS Z 3104, as indicated by "○", Class 2 by "△", and Class 3 or 4 by "×". Here, Class 1 or 2 was considered to be pass, and Class 3 or 4 was considered to be fail.
[0174] [Evaluation of Mechanical Properties of Weld Metal] Tensile test pieces (parallel portion diameter 6 mm) and Charpy impact test pieces (V notch) were taken from the obtained weld joints in accordance with the provisions of JIS Z 3111, and tensile tests and impact tests were carried out. Tensile tests were carried out on three pieces each at room temperature (normal temperature), and the average values obtained (0.2% proof stress, tensile strength) were taken as the tensile properties of the weld metal of the weld joint. Charpy impact tests were also carried out on three pieces each, and the absorbed energy (vE -40 The average value was taken as the cryogenic impact toughness of the weld metal of the welded joint. A value of 30 J or more was evaluated as "Good", and a value less than this was evaluated as "Poor".
[0175] In addition, tensile tests were also conducted on the welded joints at room temperature in accordance with the provisions of JIS Z 3121. The test specimens were taken perpendicular to the weld axis so that the weld axis was at the center of the parallel length of the test specimen, and the thickness was a Type 1A test specimen, which was the full thickness of the welded joint. Three test specimens were taken, and the evaluation was given as "○" if the individual yield stress values were all 325 MPa or higher, "△" if the average was 325 MPa or higher but some individual values did not reach 325 MPa, and "×" if the individual tensile strength values were less than 520 MPa. The evaluation was given as "○" if the individual tensile strength values were all 520 MPa or higher, "△" if the average was 520 MPa or higher but some individual values did not reach 520 MPa, and "×" if the individual tensile strength values were less than 520 MPa.
[0176] Furthermore, a Charpy impact test was also carried out on the weld heat-affected zone of the welded joint in accordance with the provisions of JIS Z 3128. The V-notch direction of the test specimen was perpendicular to the steel plate surface, and the test specimens were taken from the center of the plate thickness, the center position of the weld metal, on the fusion line, and a position 1 mm from the fusion line. Three test specimens were taken, and the evaluation was given as "○" if all of the individual values were 30 J or more, "△" if the average was 30 J or more but some individual values did not reach 30 J, and "×" if they were less than 30 J.
[0177] As mentioned above, the target values in the present invention are a room temperature yield strength (0.2% proof stress) of the weld metal of 325 MPa or more, a tensile strength of the weld metal of 520 MPa or more, and a room temperature tensile strength of the welded joint of 520 MPa or more. Furthermore, the absorbed energy (vE -40 ) is set to 30J or more.
[0178] [Welding Efficiency] The wire diameter (mm) used during welding and the wire feed rate (mm / min) during welding were measured, and the deposition amount (g) divided by the unit welding time (min) was recorded as the deposition efficiency (g / min). A value of 250 g / min or more was evaluated as "Good", and a value less than this was evaluated as "Poor".
[0179] Of the above measurement and evaluation results, the results for the chemical composition of the weld metal are shown in Tables 4-1 and 4-2, and the results for the properties of the weld metal and steel plate, the performance of the welded joints, etc. are shown in Tables 5-1 and 5-2.
[0180]
[0181]
[0182]
[0183]
[0184] All of the examples of the present invention have sound welded joints free from weld defects such as hot cracking and incomplete fusion. Furthermore, all of the examples of the present invention have a room temperature yield strength (0.2% proof stress) of the weld metal of 325 MPa or more, a tensile strength of 520 MPa or more, and a room temperature tensile strength of the welded joint of 520 MPa or more. In addition, the absorbed energy (vE) of the weld metal and the weld heat affected zone in a Charpy impact test at a test temperature of -40°C was -40 ) is 30 J or more, and the weld metal has both high strength and excellent low-temperature impact toughness.
[0185] On the other hand, in Examples that are outside the preferred ranges for the steel plate and welded weld metal of the present invention, hot cracking occurs, reducing hot cracking resistance, or incomplete fusion occurs. In addition, the room temperature yield strength (0.2% proof stress) and tensile strength of the weld metal, the room temperature tensile strength of the welded joint, and the absorbed energy (vE) of the weld metal and weld heat affected zone in a Charpy impact test at a test temperature of -40°C were -40 ) and other mechanical properties were at slightly lower levels.
[0186] Although joints No. 5-2, No. 22-2, and No. 22-3 were economically disadvantageous due to the REM content of the welding wire or weld metal, they exhibited good results in the properties and performance shown in Tables 5-1 and 5-2. Also, joint No. 18-2 was economically disadvantageous due to the shielding gas composition, but it exhibited good results in the properties and performance shown in Tables 5-1 and 5-2.
[0187] REFERENCE SIGNS LIST 1 steel plate 2 weld metal 3 fusion line 4 groove surface 5 first electrode 6 second electrode 7 third electrode 8 fourth electrode 5a, 6a, 7a, 8a power feed tips of first electrode, second electrode, third electrode, fourth electrode 5b, 6b, 7b, 8b welding wire of first electrode, second electrode, third electrode, fourth electrode 5c, 6c, 7c, 8c welding wire tip of first electrode, second electrode, third electrode, fourth electrode 9 weld line 10 backing material 11 shielding gas supply nozzle 11a gas discharge port 12 molten pool T plate thickness A cross-sectional area of entire weld metal L iWelding layer (i = 1 to p layer), (L1: initial layer, L P : outermost layer) W i Width of weld layer (i = 1 to p layer) a Distance between welding wire tip 5c of the first electrode and welding wire tip 6c of the second electrode b Distance between welding wire tip 6c of the second electrode and welding wire tip 7c of the third electrode c Distance between welding wire tip 7c of the third electrode and welding wire tip 8c of the fourth electrode d Distance between welding wire tip end 5c or 6c and groove surface 4 α Angle of the straight line connecting the welding wire tips of the first electrode and second electrode with respect to the direction perpendicular to the weld line θ Groove angle, θ f Surface bevel angle, θ b Back bevel angle Φ Inclination angle of power supply tip tip G Gap T f Surface thickness, T m Intermediate thickness, T b Backside Thickness
Claims
1. A method for manufacturing a welded joint by gas-shielded arc welding of steel plates, wherein the thickness T (mm) of the steel plate is 50 mm or more, the weld metal is made of multiple layers with one pass per layer, and the cross-sectional area A (mm 2 The ratio [A / p] of the number of weld layers p (layers) to the number of layers p (layers) is 120.0 mm 2 a ratio [H / W] of a height H (mm) to a width W (mm) of each layer in the weld metal is 1.00 or less, the gas-shielded arc welding is a multi-electrode welding having three or more electrodes, tips of the welding wires of first and second electrodes are arranged on different parallel weld lines, one of the first and second electrodes is a negative wire (positive polarity) and the other is a positive wire (reverse polarity), a distance a (mm) between the welding wire tips of the first and second electrodes is 5 to 16 mm, an angle α of a straight line connecting the welding wire tips of the first and second electrodes with respect to a perpendicular direction to the weld line is 60° or less, and a welding wire containing 0.015 to 0.100 mass % of REM is used for the electrode serving as the negative wire (positive polarity).
2. A method for manufacturing a welded joint by gas-shielded arc welding of steel plate as set forth in claim 1, wherein the inclination angle Φ of the tip of each of the power tips of the first electrode and the second electrode toward the groove surface with respect to the perpendicular direction of the weld line is 0° to 15°, the distance d (mm) between the side end of the tip of each of the welding wires of the first electrode and the second electrode and the groove surface is 0.5 to 3.0 mm, each of the welding wires is curved in advance to have a radius of curvature in the range of 150 to 300 mm, a third electrode and subsequent electrodes are positioned in the center of the groove behind the first electrode and the second electrode, and a gas containing 60 volume % or more of CO2 gas is used as the shielding gas.
3. The chemical composition of the steel plate includes, in mass%, C: 0.04 to 0.14%, Si: 0.03 to 0.70%, Mn: 0.30 to 2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001 to 0.100%, Al: 0.001 to 0.100%, O: 0.0100% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities, and the Ceq and plate thickness (T) defined by the following formula (1) satisfy 0.0004T + 0.25 ≦ Ceq ≦ 0.0004T + 0.45, and the dislocation density ρ at a position 1 mm below the surface of the steel plate is 4.0 × 10 14 m -2 3. The method for manufacturing a welded joint by gas shielded arc welding of steel plate according to claim 1 or 2, wherein an average grain size at a position 1 mm below the surface of the steel plate is 15.0 μm or less, and an average grain size at a center position in the plate thickness is 20.0 μm or less. Ceq=[C]+[Mn] / 6+([Cr]+[Mo]+[V]) / 5+([Cu]+[Ni]) / 15... (1) where each element symbol in the above formula (1) represents the content (mass%) of the corresponding element, and if the corresponding element is not contained, it is set to 0.
4. A method for manufacturing a welded joint by gas-shielded arc welding of a steel plate as described in claim 3, wherein the chemical composition of the steel plate further includes, in mass%, one or more elements selected from the group consisting of Cu: 2.000% or less, Ni: 2.500% or less, Cr: 1.500% or less, Mo: 1.000% or less, Ti: 0.100% or less, V: 0.300% or less, B: 0.0100% or less, W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less.
5. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001-0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001-2.500%, Cr: 0.001-1.500%, Mo: 0.001-1.000%, Ti: 0.001-0.100%, V: 0.001-0.300%, B: 0.001-0.020%, O 3. The method for producing a welded joint by gas shielded arc welding of steel plates according to claim 1 or 2, comprising: C 0.050% or less; and N 0.010% or less, with the balance being Fe and unavoidable impurities.
6. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001-0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001-2.500%, Cr: 0.001-1.500%, Mo: 0.001-1.000%, Ti: 0.001-0.100%, V: 0.001-0.300%, B: 0.001-0.020%, O 4. The method for producing a welded joint by gas shielded arc welding of steel plates according to claim 3, comprising: C 0.050% or less; and N 0.010% or less, with the balance being Fe and unavoidable impurities.
7. The chemical composition of the weld metal is, in mass%, C: 0.04-0.14%, Si: 0.03-0.70%, Mn: 0.30-2.50%, P: 0.030% or less, S: 0.020% or less, Nb: 0.001-0.100%, Al: 0.001-0.100%, Cu: 0.001-2.000%, Ni: 0.001-2.500%, Cr: 0.001-1.500%, Mo: 0.001-1.000%, Ti: 0.001-0.100%, V: 0.001-0.300%, B: 0.001-0.020%, O 5. The method for producing a welded joint by gas shielded arc welding of steel plates according to claim 4, comprising: C: 0.050% or less; and N: 0.010% or less, with the balance consisting of Fe and unavoidable impurities.
8. A method for manufacturing a welded joint by gas-shielded arc welding of steel plates as described in claim 5, wherein the chemical composition of the weld metal further includes, in mass%, one or more elements selected from the group consisting of W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less.
9. A method for manufacturing a welded joint by gas-shielded arc welding of steel plates as described in claim 6, wherein the chemical composition of the weld metal further includes, in mass%, one or more elements selected from the group consisting of W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less.
10. A method for manufacturing a welded joint by gas-shielded arc welding of steel plates as described in claim 7, wherein the chemical composition of the weld metal further includes, in mass percent, one or more elements selected from the group consisting of W: 0.500% or less, Ca: 0.0200% or less, Mg: 0.0200% or less, and REM: 0.0500% or less.
Citation Information
Patent Citations
Shallow penetration submerged arc welding method
JP1980084278A
Three electrode two layer submerged arc welding of thick plate
JP1996257752A
Method and apparatus for submerged arc welding
JP2011200920A
Narrow groove gas-shield arc-welding method
JP2015223605A
Thick steel sheet, and method for producing thick steel sheet
WO2021054344A1