Positive electrode for secondary battery, and secondary battery

The positive electrode in secondary batteries, featuring olivine-type phosphoric acid compounds, acrylic ester polymers, carbon black, and carboxymethyl cellulose salt, addresses the insufficiency in battery characteristics by optimizing volume resistivity, resulting in enhanced conductivity and stability.

WO2024204452A1PCT designated stage expired Publication Date: 2024-10-03MURATA MFG CO LTD

Patent Information

Application Number
PCT/JP2024/012481
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Secondary batteries exhibit insufficient battery characteristics despite various studies on their configuration, necessitating the development of a positive electrode that can enhance performance.

Method used

A positive electrode comprising a positive electrode active material layer with phosphoric acid compounds having an olivine crystal structure, an acrylic ester polymer binder, carbon black conductive agent, and carboxymethyl cellulose salt, optimized to achieve a volume resistivity of 10 Ω·cm to 100 Ω·cm, facilitating improved conductivity and stability.

Benefits of technology

The optimized positive electrode active material layer enhances the conductivity and stability of the secondary battery, leading to superior battery characteristics, including stable battery capacity and safety, with the use of Ketjen black for extensive electronic network formation and appropriate content ratios of binder, conductive agent, and carboxymethyl cellulose salt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012481_03102024_PF_FP_ABST
    Figure JP2024012481_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a positive electrode for a secondary battery and a secondary battery, with which excellent battery characteristics can be obtained. This secondary battery comprises: a positive electrode including a positive electrode active material layer; a negative electrode; and an electrolyte. The positive electrode active material layer includes a plurality of positive electrode active material particles, a positive electrode binder, a positive electrode conductive agent, and a carboxymethyl cellulose salt. The positive electrode active material particles include a phosphoric acid compound having an olivine-type crystal structure, the positive electrode binder includes an acrylic acid ester polymer, and the positive electrode conductive agent includes carbon black. The volume resistivity of the positive electrode active material layer is 10-100 Ω·cm.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode for secondary battery and secondary battery

[0001] The present technology relates to a positive electrode for a secondary battery and a secondary battery.

[0002] Due to the widespread use of various electronic devices such as mobile phones, secondary batteries have been developed as small, lightweight power sources that can provide high energy density. These secondary batteries contain a positive electrode (a positive electrode for the secondary battery), a negative electrode, and an electrolyte solution, and various studies have been conducted on the configuration of these secondary batteries.

[0003] Specifically, the positive electrode mixture layer contains an electrode material, a conductive additive, and a binder, the electrode material contains an electrode active material (a transition metal lithium phosphate compound having an olivine structure) and a carbonaceous coating, and the volume resistivity of the positive electrode mixture layer after pressing is 5.0 Ω cm or less (see, for example, Patent Document 1).

[0004] Japanese Patent Application Laid-Open No. 2018-163763

[0005] Although various studies have been conducted on the configuration of secondary batteries, the battery characteristics of the secondary batteries are still insufficient and there is room for improvement.

[0006] There is a demand for a positive electrode for a secondary battery and a secondary battery that can provide excellent battery characteristics.

[0007] According to one embodiment of the present disclosure, a positive electrode for a secondary battery includes a positive electrode active material layer, the positive electrode active material layer including a plurality of positive electrode active material particles, a positive electrode binder, a positive electrode conductive agent, and a carboxymethyl cellulose salt. The positive electrode active material particles include a phosphate compound having an olivine crystal structure, the positive electrode binder includes an acrylic acid ester polymer, and the positive electrode conductive agent includes carbon black. The positive electrode active material layer has a volume resistivity of 10 Ω cm or more and 100 Ω cm or less.

[0008] A secondary battery according to an embodiment of the present technology includes a positive electrode, a negative electrode, and an electrolyte solution, and the positive electrode has a configuration similar to the configuration of the positive electrode for a secondary battery according to the embodiment of the present technology described above.

[0009] Here, the "acrylic acid ester polymer" refers to either or both of a homopolymer of an acrylic acid ester and a copolymer of an acrylic acid ester. Details of the acrylic acid ester polymer will be described later.

[0010] The "volume resistivity of the positive electrode active material layer" is a physical property value of the positive electrode active material layer measured using an electrode resistor. Details of the procedure for measuring the volume resistivity of the positive electrode active material layer will be described later.

[0011] According to the positive electrode for a secondary battery or the secondary battery of one embodiment of the present technology, the positive electrode active material layer contains a plurality of positive electrode active material particles (a phosphoric acid compound having an olivine-type crystal structure), a positive electrode binder (an acrylic acid ester polymer), a positive electrode conductive agent (carbon black), and a carboxymethyl cellulose salt, and the volume resistivity of the positive electrode active material layer is 10 Ω cm or more and 100 Ω cm or less, thereby enabling excellent battery characteristics to be obtained.

[0012] Note that the effects of the present technology are not necessarily limited to the effects described here, but may be any of a series of effects related to the present technology described below.

[0013] Fig. 1 is a cross-sectional view showing the configuration of a positive electrode for a secondary battery according to an embodiment of the present technology. Fig. 2 is a cross-sectional view showing the configuration of a secondary battery according to an embodiment of the present technology. Fig. 3 is a cross-sectional view showing the configuration of the battery element shown in Fig. 2. Fig. 4 is a block diagram showing the configuration of an application example of a secondary battery. Fig. 5 is a cross-sectional view showing the configuration of a test secondary battery.

[0014] Hereinafter, an embodiment of the present technology will be described in detail with reference to the drawings. The description will be made in the following order: 1. Positive electrode for secondary battery 1-1. Configuration 1-2. Operation 1-3. Manufacturing method 1-4. Action and effect 2. Secondary battery 2-1. Configuration 2-2. Operation 2-3. Manufacturing method 2-4. Action and effect 3. Modification 4. Use of secondary battery

[0015] 1. Positive Electrode for Secondary Battery First, a positive electrode for a secondary battery (hereinafter simply referred to as "positive electrode") according to an embodiment of the present technology will be described.

[0016] The positive electrode described here is used in a secondary battery, which is an electrochemical device. However, the positive electrode may also be used in electrochemical devices other than secondary batteries. Specific examples of other electrochemical devices include primary batteries and capacitors.

[0017] The positive electrode absorbs and releases an electrode reactant during operation of the electrochemical device (i.e., during the electrode reaction). The type of electrode reactant is not particularly limited, but specifically includes light metals such as alkali metals and alkaline earth metals. Specific examples of alkali metals include lithium, sodium, and potassium, and specific examples of alkaline earth metals include beryllium, magnesium, and calcium.

[0018] In the following, an example will be given in which the electrode reactant is lithium, whereby lithium is absorbed and released in an ionic state at the positive electrode during the electrode reaction.

[0019] 1 shows a cross-sectional structure of a specific example of a positive electrode, a positive electrode 100. As shown in FIG. 1, the positive electrode 100 includes a positive electrode current collector 100A and a positive electrode active material layer 100B.

[0020] [Positive Electrode Current Collector] The positive electrode current collector 100A is a conductive support that supports the positive electrode active material layer 100B, and has a pair of surfaces (upper and lower surfaces) on which the positive electrode active material layer 100B is provided. The positive electrode current collector 100A contains a conductive material such as a metal material, and a specific example of the conductive material is aluminum.

[0021] However, the positive electrode 100 does not necessarily have to include the positive electrode current collector 100A.

[0022] [Positive Electrode Active Material Layer] The positive electrode active material layer 100B is a layer that absorbs and releases lithium, and is provided on one surface (upper or lower surface) of the positive electrode current collector 100A. However, the positive electrode active material layer 100B may be provided on both surfaces (upper and lower surfaces) of the positive electrode current collector 100A.

[0023] This positive electrode active material layer 100B contains a plurality of particulate positive electrode active materials (hereinafter referred to as "plural positive electrode active material particles") that absorb and release lithium, a positive electrode binder, a positive electrode conductive agent, and a carboxymethyl cellulose salt.

[0024] (Multiple Positive Electrode Active Material Particles) The positive electrode active material particles are particles that absorb and release lithium, and contain one or more types of phosphate compounds having an olivine-type crystal structure (hereinafter referred to as "olivine-type phosphate compounds").

[0025] The positive electrode active material particles contain an olivine-type phosphate compound because the olivine-type phosphate compound has a strong and stable crystal structure, which prevents oxygen from being released from the olivine-type phosphate compound, thereby providing a stable battery capacity and improving safety in a secondary battery using the positive electrode 100.

[0026] Here, as described above, since the electrode reactant is lithium, the olivine-type phosphate compound contains lithium as a constituent element. In this case, the type of the olivine-type phosphate compound is not particularly limited as long as it is a phosphate compound containing lithium as a constituent element.

[0027] The olivine-type phosphate compound may further contain one or more metal elements (excluding lithium) as constituent elements, including, but not limited to, iron, manganese, cobalt, nickel, titanium, chromium, vanadium, zinc, tin, tungsten, zirconium, magnesium, and aluminum.

[0028] Among these, the metal element is preferably iron. That is, the olivine-type phosphate compound preferably contains iron as a constituent element together with lithium. This is because oxygen release from the olivine-type phosphate compound is sufficiently suppressed, thereby obtaining a sufficient battery capacity and sufficiently improving safety.

[0029] More specifically, the olivine-type phosphate compound preferably contains one or more of the compounds represented by formula (1). When the olivine-type phosphate compound contains two or more metal elements (Me) as constituent elements, the mixing ratio (molar ratio) of the two or more metal elements can be set arbitrarily.

[0030] Li x  MeP.O. 4  ... (1) (Me is at least one of Fe, Mn, Co, Ni, Ti, Cr, V, Zn, Sn, W, Zr, Mg, and Al; and x satisfies 0.9≦x≦1.1.)

[0031] A specific example of an olivine-type phosphate compound is LiFePO 4  , LiMnPO 4  , LiFe 0.5  Mn 0.5  P.O. 4  and LiFe 0.5  Co 0.5  P.O. 4  And so on.

[0032] Here, the positive electrode active material particles are secondary particles formed by aggregation of a plurality of primary particles, and therefore the positive electrode active material layer 100B contains a plurality of positive electrode active material particles, which are a plurality of secondary particles. Here, the secondary particles are formed by aggregation of a plurality of primary particles.

[0033] The median diameter MD1 of the plurality of primary particles is preferably 1 μm or less, and the median diameter MD2 of the plurality of positive electrode active material particles (plurality of secondary particles) is preferably 4 μm to 20 μm. This is because the plurality of primary particles are more likely to be connected to one another within the secondary particles, and the plurality of secondary particles are also more likely to be connected to one another. This improves the electronic conductivity between the plurality of positive electrode active material particles, thereby improving the conductivity of the positive electrode active material layer 100B.

[0034] The procedure for calculating the median diameter MD1 is as follows. First, a scanning electron microscope (SEM) is used to observe the cross section of the positive electrode active material layer 100B (observation magnification = 10,000 times). This allows the observation of the multiple positive electrode active material particles contained in the positive electrode active material layer 100B, and therefore the multiple primary particles forming each positive electrode active material particle. Next, 50 primary particles whose entire outlines (outer edges) can be observed are arbitrarily selected from the multiple primary particles, and the particle size (major axis diameter) of each primary particle is measured. Finally, the average particle size of the 50 particles is calculated to obtain the median diameter MD1.

[0035] When measuring the median diameter MD2, a plurality of positive electrode active material particles are analyzed using a particle size measuring device, such as the LA-960 laser diffraction / scattering particle size distribution measuring device manufactured by Horiba, Ltd.

[0036] More specifically, when measuring the median diameter MD2, the positive electrode 100 is first placed in an aqueous solvent to peel the positive electrode active material layer 100B from the positive electrode current collector 100A. The type of aqueous solvent is not particularly limited, but specifically, pure water capable of dissolving the positive electrode binder and carboxymethyl cellulose salt is used. The details regarding the aqueous solvent described here will also apply hereinafter. Next, the positive electrode active material layer 100B is placed in the aqueous solvent, and the aqueous solvent is stirred, and then filtered. This dissolves and removes the positive electrode binder and dispersant, allowing the solid content (a plurality of positive electrode active material particles and positive electrode conductive agent) to be recovered.

[0037] Next, the solid content is introduced into the aqueous solvent, and then the solid content in the aqueous solvent is centrifuged using a centrifuge. This separates the positive electrode active material particles from the positive electrode conductive agent, and the positive electrode active material particles are recovered. Finally, the positive electrode active material particles are analyzed using a particle size measuring device to measure the median diameter MD2.

[0038] (Positive Electrode Binder) The positive electrode binder is a material that binds a plurality of positive electrode active material particles together, and contains a water-soluble polymer compound, more specifically, contains one or more types of acrylic acid ester polymers, because the binding properties of the positive electrode binder are ensured and decomposition of the positive electrode binder is suppressed even at high potentials.

[0039] As described above, the acrylic acid ester polymer is one or both of an acrylic acid ester homopolymer and an acrylic acid ester copolymer. The type of acrylic acid ester homopolymer may be one type or two or more types. The type of acrylic acid ester copolymer may be one type or two or more types.

[0040] A homopolymer of an acrylic acid ester is a so-called polyacrylic acid ester. Specific examples of the polyacrylic acid ester include polymethyl acrylate, polyethyl acrylate, and polybutyl acrylate.

[0041] An acrylic acid ester copolymer is a compound obtained by copolymerizing an acrylic acid ester with one or more types of monomers (excluding acrylic acid esters). Specific examples of acrylic acid esters include methyl acrylate, ethyl acrylate, and butyl acrylate. The type of monomer is not particularly limited, but a specific example is acrylonitrile.

[0042] The acrylic acid ester copolymer may be a binary copolymer in which an acrylic acid ester is copolymerized with one type of monomer, or a ternary copolymer in which an acrylic acid ester is copolymerized with two types of monomers. Of course, the acrylic acid ester copolymer may also be a quaternary or higher copolymer. The copolymerization amount of the monomers in the acrylic acid ester copolymer is not particularly limited and can be set arbitrarily.

[0043] Among these, it is preferable that the acrylic acid ester polymer contains a binary copolymer in which an acrylic acid ester and acrylonitrile are copolymerized, because this sufficiently improves the binding property when using a positive electrode binder and also sufficiently suppresses decomposition of the positive electrode binder even at a high potential.

[0044] The content of the positive electrode binder in the positive electrode active material layer 100B is not particularly limited, but is preferably 0.5% by weight to 4.0% by weight, because this prevents the conductivity of the positive electrode 100 from decreasing.

[0045] Specifically, if the content of the positive electrode binder in the positive electrode active material layer 100B is less than 0.5 wt %, the binding strength of the positive electrode active material particles using the positive electrode binder will be insufficient, which may cause the positive electrode active material layer 100B to collapse and peel off from the positive electrode current collector 100A, resulting in a decrease in the conductivity of the positive electrode 100.

[0046] On the other hand, if the content of the positive electrode binder in the positive electrode active material layer 100B is greater than 4.0 wt %, the proportion of the low-conductivity component (positive electrode binder) contained in the positive electrode active material layer 100B increases, which may fundamentally reduce the conductivity of the positive electrode 100.

[0047] The procedure for examining the content of the positive electrode binder in the positive electrode active material layer 100B is as follows.

[0048] First, the positive electrode current collector 100A is peeled from the positive electrode active material layer 100B, and the weight of the positive electrode active material layer 100B is measured. Next, the positive electrode active material layer 100B is analyzed using thermogravimetric analysis (TGA) to calculate the weight of the positive electrode binder contained in the positive electrode active material layer 100B. For example, when the thermal decomposition temperature of the positive electrode binder is approximately 300°C to 600°C, the positive electrode active material layer 100B is heated at a heating rate of 1°C / min, and the weight of the positive electrode binder is calculated based on the weight loss rate within the heating temperature range of approximately 300°C to 600°C. Finally, the content of the positive electrode binder in the positive electrode active material layer 100B is calculated based on the weight of the positive electrode active material layer 100B and the weight of the positive electrode binder.

[0049] (Positive Electrode Conductive Agent) The positive electrode conductive agent is a material that improves the conductivity of the positive electrode active material layer 100B, and contains one or more types of carbon black. This is because the conductivity of the positive electrode active material layer 100B is sufficiently improved. Specific examples of carbon black include ketjen black, acetylene black, furnace black, channel black, and thermal black.

[0050] Among these, it is preferable that the carbon black contains ketjen black. This is because ketjen black can retain a large amount of electrolyte due to its particle shape in a secondary battery using the positive electrode 100. Furthermore, since the specific gravity of ketjen black is smaller than that of acetylene black, etc., a large amount of positive electrode conductive agent is adsorbed to the surface of the positive electrode active material particles. This forms an extensive electronic network (electron conduction path) inside the positive electrode active material layer 100B and facilitates the movement of lithium ions.

[0051] The content of the positive electrode conductive agent in the positive electrode active material layer 100B is not particularly limited, but is preferably 0.5% by weight to 3.0% by weight, because this improves the stability over time of the positive electrode mixture slurry in the manufacturing process of the positive electrode 100 and also sufficiently improves the conductivity of the positive electrode 100.

[0052] In detail, if the content of the positive electrode conductive agent in the positive electrode active material layer 100B is less than 0.5 wt %, the proportion of the conductive component (positive electrode conductive agent) contained in the positive electrode active material layer 100B decreases, and therefore the conductivity of the positive electrode 100 may fundamentally decrease.

[0053] On the other hand, if the content of the positive electrode conductive agent in the positive electrode active material layer 100B is greater than 3.0 wt %, the fluidity of the positive electrode mixture slurry decreases in the manufacturing process of the positive electrode 100, and the stability of the positive electrode mixture slurry over time may decrease.

[0054] The procedure for examining the content of the positive electrode conductive agent in the positive electrode active material layer 100B is as follows.

[0055] First, the positive electrode current collector 100A is peeled off from the positive electrode active material layer 100B, and then the weight of the positive electrode active material layer 100B is measured.

[0056] Next, the positive electrode active material layer 100B is immersed in an organic solvent to dissolve the positive electrode binder contained in the positive electrode active material layer 100B. Specific examples of the organic solvent include one or more of N-methyl-2-pyrrolidone, dimethylformamide, and dimethyl sulfoxide. Next, the dissolved material is filtered to recover the residue, which is then dried.

[0057] The residue is then immersed in an aqueous solvent to dissolve the carboxymethyl cellulose salt contained in the residue, and the residue is then filtered to recover the residue, which is then dried.

[0058] The residue is then subjected to carbon analysis to calculate the weight of the carbon component (positive electrode conductive agent) contained in the residue. An analytical device for carbon analysis may be an EMIA-920V2 carbon-sulfur analyzer (CS meter) manufactured by Horiba, Ltd.

[0059] Finally, the content of the positive electrode conductive agent in the positive electrode active material layer 100B is calculated based on the weight of the positive electrode active material layer 100B and the weight of the positive electrode conductive agent.

[0060] (Carboxymethylcellulose Salt) Carboxymethylcellulose salt is a material that appropriately increases the viscosity of the positive electrode mixture slurry when preparing the positive electrode mixture slurry in the manufacturing process of the positive electrode 100, thereby improving the dispersibility of a plurality of positive electrode active material particles, etc. In other words, carboxymethylcellulose salt is a so-called thickener.

[0061] The carboxymethyl cellulose salt contains one or more types of water-soluble carboxymethyl cellulose salts, because the dispersibility of a plurality of positive electrode active material particles and the like is improved while the fluidity of the positive electrode mixture slurry is ensured.

[0062] The type of carboxymethylcellulose salt is not particularly limited, but specific examples include alkali metal carboxymethylcellulose salts and alkaline earth metal carboxymethylcellulose salts. Specific examples of alkali metal carboxymethylcellulose salts include lithium carboxymethylcellulose, sodium carboxymethylcellulose, and potassium carboxymethylcellulose. Specific examples of alkaline earth metal carboxymethylcellulose salts include magnesium carboxymethylcellulose and calcium carboxymethylcellulose.

[0063] Among these, it is preferable that the carboxymethyl cellulose salt contains sodium carboxymethyl cellulose, because this sufficiently improves the fluidity of the positive electrode mixture slurry and also sufficiently improves the dispersibility of a plurality of positive electrode active material particles and the like.

[0064] The content of the carboxymethyl cellulose salt in the positive electrode active material layer 100B is not particularly limited, but is preferably 0.6% by weight to 2.0% by weight, because this improves the stability over time of the positive electrode mixture slurry in the manufacturing process of the positive electrode 100, and also improves the physical durability of the positive electrode active material layer 100B formed using the positive electrode mixture slurry.

[0065] In detail, if the content of carboxymethyl cellulose salt in the positive electrode active material layer 100B is less than 0.6 wt %, the fluidity of the positive electrode mixture slurry decreases during the manufacturing process of the positive electrode 100, and the stability of the positive electrode mixture slurry over time may decrease.

[0066] On the other hand, if the content of carboxymethyl cellulose salt in the positive electrode active material layer 100B is greater than 2.0 wt %, the positive electrode active material layer 100B formed using the positive electrode mixture slurry becomes excessively hard, which may reduce the physical durability of the positive electrode active material layer 100B. In this case, the positive electrode active material layer 100B may crack and may fall off from the positive electrode current collector 100A.

[0067] The procedure for determining the content of carboxymethyl cellulose salt in the positive electrode active material layer 100B is as follows.

[0068] First, the positive electrode current collector 100A is peeled from the positive electrode active material layer 100B, and the weight of the positive electrode active material layer 100B is measured. Next, the positive electrode active material layer 100B is analyzed using thermogravimetric analysis in a nitrogen atmosphere to calculate the weight of the carboxymethyl cellulose salt contained in the positive electrode active material layer 100B. For example, if the thermal decomposition temperature of the carboxymethyl cellulose salt is approximately 250°C, the positive electrode active material layer 100B is heated at a heating rate of 1°C / min, and the weight of the carboxymethyl cellulose salt is calculated based on the weight loss rate within a heating temperature range from room temperature to approximately 250°C. Finally, the content of the carboxymethyl cellulose salt in the positive electrode active material layer 100B is calculated based on the weight of the positive electrode active material layer 100B and the weight of the carboxymethyl cellulose salt.

[0069] (Volume Resistivity) The volume resistivity R of the positive electrode active material layer 100B is 10 Ω cm to 100 Ω cm. This is because an appropriate electronic network using a positive electrode conductive agent together with a plurality of positive electrode active material particles is formed inside the positive electrode active material layer 100B, thereby improving the conductivity of the positive electrode active material layer 100B.

[0070] Specifically, when the volume resistivity R is less than 10 Ω·cm, the positive electrode conductors tend to be connected to each other within the positive electrode active material layer 100B with almost no intervening positive electrode active material particles, making it easier for the positive electrode conductor to form an electronic network without the involvement of the positive electrode active material particles. In this case, it becomes difficult to form an appropriate electronic network using the positive electrode conductor together with the multiple positive electrode active material particles, and electrons are not sufficiently conducted to each positive electrode active material particle. This increases the electrical resistance within the positive electrode active material layer 100B, thereby reducing the conductivity of the positive electrode active material layer 100B.

[0071] On the other hand, if the volume resistivity R is greater than 100 Ω·cm, the electrical resistance increases excessively inside the positive electrode active material layer 100B, resulting in a fundamental decrease in the conductivity of the positive electrode active material layer 100B.

[0072] As described above, the volume resistivity R is measured using an electrode resistor. As this electrode resistor, an electrode resistance measurement system RM2610 manufactured by Hioki E.E. Corporation can be used. In this case, the volume resistivity R of the positive electrode active material layer 100B is measured by analyzing the positive electrode 100 using the electrode resistor.

[0073] <1-2. Operation> In this positive electrode 100, during an electrode reaction, lithium is released in an ionic state from the positive electrode active material layer 100B, and lithium is absorbed in an ionic state into the positive electrode active material layer 100B.

[0074] <1-3. Manufacturing Method> The positive electrode 100 is manufactured by the following example procedure.

[0075] First, a carboxymethyl cellulose salt, a powdered positive electrode conductive agent, and an aqueous solvent are mixed together to prepare a first mixed solution, which is then stirred (pre-mixed) until the positive electrode conductive agent swells.

[0076] The type of aqueous solvent is not particularly limited, but specifically, it is pure water or the like. The details regarding the aqueous solvent described here also apply hereinafter. When stirring the first mixture, a stirrer such as a planetary mixer may be used.

[0077] Here, when stirring the first mixture, the solids concentration is set to be higher than the solids concentration of the positive electrode mixture slurry prepared in a subsequent process, thereby intentionally stirring the first mixture in a high solids concentration state. The solids concentration of the first mixture is not particularly limited, but specifically, the solids concentration of the first mixture is set to be about 5% to 15% higher than the solids concentration of the positive electrode mixture slurry. In this case, the first mixture is continuously stirred until no aggregates are present in the first mixture.

[0078] The first mixed solution is intentionally stirred in a state where the solid content concentration is high in order to sufficiently disperse the positive electrode conductive agent in the positive electrode mixture slurry, thereby improving the conductivity of the positive electrode active material layer 100B formed using the positive electrode mixture slurry.

[0079] Specifically, the positive electrode conductive agent is hydrophobic and therefore difficult to disperse in the first mixed liquid containing the aqueous solvent. If the positive electrode conductive agent is not sufficiently dispersed in the first mixed liquid, it becomes difficult to form an appropriate electronic network using the positive electrode conductive agent together with the plurality of positive electrode active material particles inside the positive electrode active material layer 100B, and the conductivity of the positive electrode active material layer 100B decreases.

[0080] However, if the first mixed liquid is intentionally stirred in a state where the solids concentration is high, the water-soluble carboxymethyl cellulose salt tends to coat the surface of the positive electrode conductive agent, and the positive electrode conductive agent tends to be dispersed in the first mixed liquid containing the aqueous solvent. This makes it easier to form an electronic network using the positive electrode conductive agent together with the plurality of positive electrode active material particles inside the positive electrode active material layer 100B, thereby improving the conductivity of the positive electrode active material layer 100B.

[0081] Next, the positive electrode active material particles and the aqueous solvent are added to the first mixed solution to prepare a second mixed solution, and the second mixed solution is then stirred (main kneading). Note that, when stirring the second mixed solution, a stirrer may be used, as in the case of stirring the first mixed solution.

[0082] Here, when stirring the second mixed liquid, the solid content concentration is set to be higher than the solid content concentration of the positive electrode mixture slurry, as in the case of stirring the first mixed liquid, so that the second mixed liquid is stirred in an intentionally high solid content state. The details regarding the solid content concentration of the second mixed liquid are the same as the details regarding the solid content concentration of the first mixed liquid. In this case, the second mixed liquid is continuously stirred until no aggregates are present in the second mixed liquid.

[0083] The reason why the second mixed liquid is intentionally stirred in a state where the solid content concentration is high is to sufficiently disperse the plurality of positive electrode active material particles in the positive electrode mixture slurry, thereby improving the conductivity of the positive electrode active material layer 100B formed using the positive electrode mixture slurry.

[0084] Specifically, the hydrophobic positive electrode active material particles are difficult to disperse in the second mixed liquid containing the aqueous solvent, which makes it difficult to form an appropriate electronic network using the positive electrode conductive agent together with the positive electrode active material particles inside the positive electrode active material layer 100B, thereby reducing the conductivity of the positive electrode active material layer 100B.

[0085] However, if the second mixed liquid is intentionally stirred in a state where the solids concentration is high, the water-soluble carboxymethyl cellulose salt tends to coat the surfaces of the positive electrode active material particles, and thus the positive electrode active material particles tend to be dispersed in the second mixed liquid containing the aqueous solvent. This facilitates the formation of an electronic network using the positive electrode conductive agent together with the positive electrode active material particles inside the positive electrode active material layer 100B, thereby improving the conductivity of the positive electrode active material layer 100B.

[0086] After stirring the second mixed liquid, a positive electrode binder and an aqueous solvent are added to the second mixed liquid, and the second mixed liquid is stirred. As a result, the positive electrode active material particles and the positive electrode conductive agent are dispersed in the second mixed liquid, and the positive electrode binder is dissolved, thereby preparing a positive electrode mixture slurry. Note that, when stirring the second mixed liquid, a stirrer may be used, as described above.

[0087] In this case, in order to add the positive electrode binder to the second mixed liquid, a dispersion liquid (emulsion liquid) in which the positive electrode binder is dispersed in advance may be used, because the dispersibility of the positive electrode binder in the positive electrode mixture slurry is improved.

[0088] Finally, the positive electrode mixture slurry is applied to one surface of the positive electrode current collector 100A to form the positive electrode active material layer 100B. The positive electrode active material layer 100B may then be compression-molded using a molding machine such as a roll press. In this case, the positive electrode active material layer 100B may be heated, or the compression molding may be repeated multiple times.

[0089] As a result, the positive electrode active material layer 100B is formed on one surface of the positive electrode current collector 100A, and thus the positive electrode 100 is completed.

[0090] <1-4. Function and Effect> According to this positive electrode 100, the positive electrode active material layer 100B contains a plurality of positive electrode active material particles (olivine-type phosphate compound), a positive electrode binder (acrylic acid ester polymer), a positive electrode conductive agent (carbon black), and a carboxymethyl cellulose salt. The volume resistivity R of the positive electrode active material layer 100B is 10 Ω cm to 100 Ω cm.

[0091] In this case, the volume resistivity R is optimized in the positive electrode active material layer 100B containing a plurality of positive electrode active material particles (olivine-type phosphate compound), a positive electrode binder (acrylic acid ester polymer), a positive electrode conductor (carbon black), and a carboxymethyl cellulose salt. As a result, as described above, an appropriate electronic network is formed inside the positive electrode active material layer 100B using the positive electrode conductor together with the plurality of positive electrode active material particles.

[0092] Therefore, the conductivity of the positive electrode active material layer 100B is improved, and excellent battery characteristics can be obtained.

[0093] In particular, if the carbon black contains ketjen black, an extensive electronic network is formed inside the positive electrode active material layer 100B, and the movement of lithium ions is facilitated, so that a greater effect can be obtained.

[0094] Furthermore, if the content of the positive electrode conductive agent in the positive electrode active material layer 100B is 0.5% by weight to 3.0% by weight, the stability over time of the positive electrode mixture slurry is improved in the manufacturing process of the positive electrode 100, and the conductivity of the positive electrode 100 is sufficiently improved, thereby obtaining a greater effect.

[0095] Furthermore, if the olivine-type phosphate compound contains lithium and iron as constituent elements, the release of oxygen from the olivine-type phosphate compound is sufficiently suppressed, thereby achieving sufficient battery capacity and improving safety, resulting in even greater benefits.

[0096] Furthermore, if the acrylic acid ester polymer contains a copolymer of acrylic acid ester and acrylonitrile, the binding property using the positive electrode binder is sufficiently improved, and decomposition of the positive electrode binder is sufficiently suppressed even at a high potential, so that a greater effect can be obtained.

[0097] Furthermore, if the content of the positive electrode binder in the positive electrode active material layer 100B is 0.5% by weight to 4.0% by weight, the decrease in the conductivity of the positive electrode 100 is suppressed, and therefore a greater effect can be obtained.

[0098] Furthermore, if the carboxymethyl cellulose salt contains sodium carboxymethyl cellulose, the fluidity of the positive electrode mixture slurry is sufficiently improved, and the dispersibility of a plurality of positive electrode active material particles and the like is also sufficiently improved, thereby achieving a greater effect.

[0099] Furthermore, if the content of carboxymethyl cellulose salt in the positive electrode active material layer 100B is 0.6% by weight to 2.0% by weight, the stability over time of the positive electrode mixture slurry in the manufacturing process of the positive electrode 100 is improved, and the physical durability of the positive electrode active material layer 100B formed using the positive electrode mixture slurry is also improved, thereby achieving even greater effects.

[0100] Furthermore, if the median diameter MD1 is 1 μm or less and the median diameter MD2 is 4 μm to 20 μm, the electronic conductivity between the plurality of positive electrode active material particles is improved, and therefore a greater effect can be obtained.

[0101] 2. Secondary Battery Next, a secondary battery according to an embodiment of the present technology to which the positive electrode 100 is applied will be described.

[0102] The secondary battery described here is a secondary battery that obtains battery capacity by absorbing and releasing an electrode reactant, and includes a positive electrode, a negative electrode, and an electrolyte. Hereinafter, as described above, the case where the electrode reactant is lithium will be taken as an example. A secondary battery that obtains battery capacity by absorbing and releasing lithium is a so-called lithium-ion secondary battery. In this lithium-ion secondary battery, lithium is absorbed and released in an ionic state.

[0103] The charge capacity of the negative electrode is preferably larger than the discharge capacity of the positive electrode. That is, the electrochemical capacity per unit area of ​​the negative electrode is preferably larger than the electrochemical capacity per unit area of ​​the positive electrode. This is to prevent lithium from being deposited on the surface of the negative electrode during charging.

[0104] 2-1. Structure FIG. 2 shows a cross-sectional structure of a secondary battery, and FIG. 3 shows a cross-sectional structure of the battery element 20 shown in FIG.

[0105] 2 and 3, this secondary battery includes a battery can 11, a pair of insulating plates 12 and 13, a battery element 20, a positive electrode lead 25, and a negative electrode lead 26. The secondary battery described here is a cylindrical secondary battery in which the battery element 20 is housed inside the cylindrical battery can 11.

[0106] [Battery Can] The battery can 11 is a housing member that houses the battery element 20 and other components. The battery can 11 has an open end and a closed end, and thus has a hollow structure. The battery can 11 contains one or more metal materials such as iron, aluminum, iron alloys, and aluminum alloys. The surface of the battery can 11 may be plated with a metal material such as nickel.

[0107] At one open end of the battery can 11, a battery lid 14, a safety valve mechanism 15, and a PTC element 16, which is a thermosensitive resistor, are crimped via a gasket 17. This seals the battery can 11 with the battery lid 14. Here, the battery lid 14 contains the same material as the material from which the battery can 11 is formed. The safety valve mechanism 15 and the PTC element 16 are provided inside the battery lid 14, and the safety valve mechanism 15 is electrically connected to the battery lid 14 via the PTC element 16. The gasket 17 contains an insulating material, and the surface of the gasket 17 may be coated with asphalt or the like.

[0108] In the safety valve mechanism 15, when the internal pressure of the battery can 11 reaches a certain level due to an internal short circuit, external heating, or the like, the disk plate 15A reverses, thereby cutting off the electrical connection between the battery lid 14 and the battery element 20. To prevent abnormal heat generation due to a large current, the electrical resistance of the PTC element 16 increases with increasing temperature.

[0109] [Insulating Plates] The insulating plates 12 and 13 are arranged to face each other across the battery element 20. As a result, the battery element 20 is sandwiched between the insulating plates 12 and 13.

[0110] [Battery Element] The battery element 20 is a so-called power generating element, and includes a positive electrode 21, a negative electrode 22, a separator 23, and an electrolyte (not shown).

[0111] This battery element 20 is a so-called wound electrode body, and therefore the positive electrode 21 and the negative electrode 22 are wound while facing each other with a separator 23 interposed therebetween. A center pin 24 is inserted into a space 20S provided at the center of the winding of the battery element 20. However, the center pin 24 may be omitted.

[0112] (Positive Electrode) The positive electrode 21 has the same configuration as the positive electrode 100 .

[0113] Specifically, the positive electrode 21 includes a positive electrode current collector 21A and a positive electrode active material layer 21B. The configuration of the positive electrode current collector 21A is similar to the configuration of the positive electrode current collector 100A, and the configuration of the positive electrode active material layer 21B is similar to the configuration of the positive electrode active material layer 100B. Here, the positive electrode active material layer 21B is provided on both sides of the positive electrode current collector 21A.

[0114] (Negative Electrode) The negative electrode 22 includes a negative electrode current collector 22A and a negative electrode active material layer 22B.

[0115] The negative electrode current collector 22A has a pair of surfaces on which the negative electrode active material layer 22B is provided. The negative electrode current collector 22A contains a conductive material such as a metal material, and a specific example of the conductive material is copper.

[0116] The negative electrode active material layer 22B includes one or more types of negative electrode active materials that absorb and release lithium. However, the negative electrode active material layer 22B may further include one or more types of other materials, such as a negative electrode binder and a negative electrode conductive agent. The method for forming the negative electrode active material layer 22B is not particularly limited, and specifically includes one or more types of a coating method, a vapor phase method, a liquid phase method, a thermal spraying method, and a firing method (sintering method).

[0117] Here, the anode active material layer 22B is provided on both sides of the anode current collector 22A. However, the anode active material layer 22B may be provided on only one side of the anode current collector 22A on the side where the anode 22 faces the cathode 21.

[0118] The type of negative electrode active material is not particularly limited, but specific examples include carbon materials and metal-based materials, because high energy density can be obtained.

[0119] Specific examples of carbon materials include graphitizable carbon, non-graphitizable carbon, and graphite (natural graphite and artificial graphite).

[0120] The metal-based material is a material containing, as a constituent element, one or more of metal elements and metalloid elements that can form an alloy with lithium, and specific examples of the metal elements and metalloid elements include silicon and tin. This metal-based material may be a simple substance, an alloy, a compound, a mixture of two or more of these, or a material containing two or more of these phases. However, since the simple substance may contain any amount of impurities, the purity of the simple substance is not necessarily limited to 100%. A specific example of the metal-based material is TiSi 2  and SiO x  (0<x≦2, or 0.2<x<1.4), etc.

[0121] The negative electrode binder contains one or more of materials such as synthetic rubber and polymer compounds. Specific examples of synthetic rubber include styrene-butadiene rubber, fluorine-containing rubber, and ethylene-propylene-diene. Specific examples of polymer compounds include polyvinylidene fluoride, polyimide, and carboxymethyl cellulose.

[0122] The negative electrode conductive agent contains one or more conductive materials such as a carbon material, a metal material, and a conductive polymer compound, and specific examples of the carbon material include graphite, carbon black, acetylene black, and ketjen black.

[0123] (Separator) The separator 23 is an insulating porous film interposed between the positive electrode 21 and the negative electrode 22, and allows lithium ions to pass through while preventing a short circuit caused by contact between the positive electrode 21 and the negative electrode 22. The separator 23 contains a polymer compound such as polyethylene.

[0124] (Electrolyte) The electrolyte is a liquid electrolyte, and is impregnated into each of the positive electrode 21, the negative electrode 22, and the separator 23. The electrolyte contains a solvent and an electrolyte salt.

[0125] The solvent contains one or more types of non-aqueous solvents (organic solvents), and the electrolyte containing the non-aqueous solvent is a so-called non-aqueous electrolyte.

[0126] The non-aqueous solvent is an ester, an ether, or the like, more specifically, a carbonate ester compound, a carboxylic acid ester compound, a lactone compound, or the like, because it improves the dissociation of the electrolyte salt and the mobility of ions.

[0127] The carbonate ester compounds include cyclic carbonate esters and chain carbonate esters. Specific examples of the cyclic carbonate esters include ethylene carbonate and propylene carbonate, and specific examples of the chain carbonate esters include dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0128] The carboxylic acid ester compound is a chain carboxylic acid ester, etc. Specific examples of the chain carboxylic acid ester include ethyl acetate, ethyl propionate, propyl propionate, and ethyl trimethylacetate.

[0129] The lactone compound is lactone, etc. Specific examples of lactone include γ-butyrolactone and γ-valerolactone.

[0130] The ethers may be 1,2-dimethoxyethane, tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, or the like.

[0131] The non-aqueous solvent may be an unsaturated cyclic carbonate, a fluorinated cyclic carbonate, a sulfonate, a phosphate, an acid anhydride, a nitrile compound, an isocyanate compound, or the like, because the electrochemical stability of the electrolyte solution is improved.

[0132] Specific examples of unsaturated cyclic carbonates include vinylene carbonate, vinylethylene carbonate, and methyleneethylene carbonate. Specific examples of fluorinated cyclic carbonates include monofluoroethylene carbonate and difluoroethylene carbonate. Specific examples of sulfonate esters include propane sultone and propene sultone. Specific examples of phosphate esters include trimethyl phosphate and triethyl phosphate. Specific examples of acid anhydrides include succinic anhydride, 1,2-ethanedisulfonic anhydride, and 2-sulfobenzoic anhydride. Specific examples of nitrile compounds include succinonitrile. Specific examples of isocyanate compounds include hexamethylene diisocyanate.

[0133] The electrolyte salt contains one or more types of light metal salts such as lithium salts.

[0134] A specific example of the lithium salt is lithium hexafluorophosphate (LiPF 6  ), lithium tetrafluoroborate (LiBF 4  ), lithium trifluoromethanesulfonate (LiCF 3  SO 3  ), lithium bis(fluorosulfonyl)imide (LiN(FSO 2  ) 2  ), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF 3  SO 2  ) 2  ), lithium tris(trifluoromethanesulfonyl)methide (LiC(CF 3  SO 2  ) 3  ), lithium bis(oxalato)borate (LiB(C 2  O 4  ) 2  ), lithium monofluorophosphate (Li 2  PFO 3  ) and lithium difluorophosphate (LiPF 2  O 2  ) etc. This is because a high battery capacity can be obtained.

[0135] The content of the electrolyte salt is not particularly limited, but specifically, it is 0.3 mol / kg to 3.0 mol / kg relative to the solvent, because high ionic conductivity can be obtained.

[0136] [Positive Electrode Lead and Negative Electrode Lead] The positive electrode lead 25 is connected to the positive electrode current collector 21A and contains a conductive material such as aluminum. The positive electrode lead 25 is electrically connected to the battery lid 14 via the safety valve mechanism 15.

[0137] The negative electrode lead 26 is connected to the negative electrode current collector 22A and contains a conductive material such as nickel. The negative electrode lead 26 is electrically connected to the battery can 11.

[0138] <2-2. Operation> The secondary battery operates as follows during charging and discharging.

[0139] During charging, lithium is released from the positive electrode 21 of the battery element 20 and is absorbed into the negative electrode 22 via the electrolyte. During discharging, lithium is released from the negative electrode 22 of the battery element 20 and is absorbed into the positive electrode 21 via the electrolyte. During charging and discharging, lithium is absorbed and released in an ionic state.

[0140] <2-3. Manufacturing Method> When manufacturing a secondary battery, the positive electrode 21 and the negative electrode 22 are fabricated and an electrolyte solution is prepared according to the procedure described below as an example, and then the secondary battery is assembled and subjected to a stabilization process after assembly.

[0141] [Fabrication of Positive Electrode] The positive electrode 21 is fabricated by forming the positive electrode active material layers 21B on both sides of the positive electrode current collector 21A using the same procedure as that for fabricating the positive electrode 100 described above.

[0142] [Fabrication of Negative Electrode] First, a paste-like negative electrode mixture slurry is prepared by adding a mixture (negative electrode mixture) of a negative electrode active material, a negative electrode binder, and a negative electrode conductive agent to a solvent. This solvent may be an aqueous solvent or an organic solvent. Next, the negative electrode mixture slurry is applied to both surfaces of the negative electrode current collector 22A to form the negative electrode active material layer 22B. Finally, the negative electrode active material layer 22B is compression-molded using a roll press or the like. In this case, the negative electrode active material layer 22B may be heated, or the compression molding may be repeated multiple times. As a result, the negative electrode active material layer 22B is formed on both surfaces of the negative electrode current collector 22A, thereby fabricating the negative electrode 22.

[0143] [Preparation of Electrolyte Solution] An electrolyte salt is added to a solvent, whereby the electrolyte salt is dispersed or dissolved in the solvent, thereby preparing an electrolyte solution.

[0144] [Assembly of Secondary Battery] First, a positive electrode lead 25 is connected to the positive electrode current collector 21A using a joining method such as welding, and a negative electrode lead 26 is connected to the negative electrode current collector 22A of the negative electrode 22 using a joining method such as welding. Next, the positive electrode 21 and the negative electrode 22 are stacked together with the separator 23 interposed therebetween, and the positive electrode 21, the negative electrode 22, and the separator 23 are then wound to produce a wound body (not shown) having a space 20S. This wound body has a configuration similar to that of the battery element 20, except that the positive electrode 21, the negative electrode 22, and the separator 23 are not impregnated with an electrolyte. Next, a center pin 24 is inserted into the space 20S of the wound body.

[0145] Next, with the wound body sandwiched between insulating plates 12 and 13, the wound body and insulating plates 12 and 13 are housed inside battery can 11. In this case, the positive electrode lead 25 is connected to safety valve mechanism 15 using a joining method such as welding, and the negative electrode lead 26 is connected to battery can 11 using a joining method such as welding. Next, an electrolyte solution is injected into the battery can 11, thereby impregnating the wound body with the electrolyte solution. As a result, the positive electrode 21, the negative electrode 22, and the separator 23 are impregnated with the electrolyte solution, and battery element 20 is produced.

[0146] Finally, the battery lid 14, the safety valve mechanism 15, and the PTC element 16 are housed inside the battery can 11, and then the battery can 11 is crimped via the gasket 17. As a result, the battery lid 14, the safety valve mechanism 15, and the PTC element 16 are fixed to the battery can 11, and the battery element 20 is sealed inside the battery can 11, thereby assembling a secondary battery.

[0147] [Stabilization Treatment of Assembled Secondary Battery] The assembled secondary battery is charged and discharged. Various conditions, such as the ambient temperature, the number of charge / discharge cycles (number of cycles), and the charge / discharge conditions, can be set as desired. This forms a coating on the surface of each of the positive electrode 21 and the negative electrode 22, electrochemically stabilizing the state of the battery element 20. This completes the secondary battery.

[0148] <2-4. Actions and Effects> In this secondary battery, the positive electrode 21 has a configuration similar to that of the positive electrode 100. Therefore, for the reasons described above, the conductivity of the positive electrode active material layer 21B is improved, and excellent battery characteristics can be obtained.

[0149] In particular, if the secondary battery is a lithium ion secondary battery, a sufficient battery capacity can be stably obtained by utilizing the absorption and release of lithium, and therefore a greater effect can be obtained.

[0150] Other functions and effects of the secondary battery are the same as those of the positive electrode 100 .

[0151] 3. Modifications The configuration of the secondary battery described above can be modified as appropriate, as described below. However, the series of modifications described below may be combined with each other.

[0152] [Modification 1] A porous film separator 23 is used. However, although not specifically shown here, a laminated separator including a polymer compound layer may also be used.

[0153] Specifically, the laminated separator includes a porous membrane having a pair of surfaces and a polymer compound layer provided on one or both surfaces of the porous membrane. This is because the separator improves adhesion to the positive electrode 21 and the negative electrode 22, respectively, thereby suppressing misalignment of the battery element 20 (misalignment of the positive electrode 21, the negative electrode 22, and the separator 23). This suppresses swelling of the secondary battery even if a decomposition reaction of the electrolyte occurs. The polymer compound layer includes a polymer compound such as polyvinylidene fluoride. Polyvinylidene fluoride has excellent physical strength and is electrochemically stable.

[0154] One or both of the porous film and the polymer compound layer may contain a plurality of insulating particles. This is because the plurality of insulating particles promotes heat dissipation when the secondary battery generates heat, thereby improving the safety (heat resistance) of the secondary battery. The plurality of insulating particles contain one or more insulating materials, such as inorganic materials and resin materials. Specific examples of inorganic materials include aluminum oxide, aluminum nitride, boehmite, silicon oxide, titanium oxide, magnesium oxide, and zirconium oxide. Specific examples of resin materials include acrylic resin and styrene resin.

[0155] When a laminated separator is produced, a precursor solution containing a polymer compound and a solvent is prepared, and then the precursor solution is applied to one or both sides of a porous film. In this case, multiple insulating particles may be added to the precursor solution as needed.

[0156] Even when this laminated separator is used, the same effect can be obtained because lithium becomes movable between the positive electrode 21 and the negative electrode 22. In this case, as described above, the safety of the secondary battery is particularly improved, and therefore, a greater effect can be obtained.

[0157] [Modification 2] An electrolytic solution that is a liquid electrolyte is used. However, although not specifically shown here, an electrolyte layer that is a gel electrolyte may also be used.

[0158] In the battery element 20 using the electrolyte layer, the positive electrode 21 and the negative electrode 22 are wound facing each other with the separator 23 and the electrolyte layer interposed therebetween. The electrolyte layer is interposed between the positive electrode 21 and the separator 23, and also between the negative electrode 22 and the separator 23.

[0159] Specifically, the electrolyte layer contains a polymer compound together with an electrolytic solution, and the electrolytic solution is held by the polymer compound. This is because leakage of the electrolytic solution is prevented. The composition of the electrolytic solution is as described above. The polymer compound contains polyvinylidene fluoride, etc. When forming the electrolyte layer, a precursor solution containing the electrolytic solution, the polymer compound, a solvent, etc. is prepared, and then the precursor solution is applied to one or both surfaces of each of the positive electrode 21 and the negative electrode 22.

[0160] Even when this electrolyte layer is used, the same effect can be obtained because lithium can move between the positive electrode 21 and the negative electrode 22 via the electrolyte layer. In this case, particularly, as described above, leakage of the electrolyte solution is prevented, so that a greater effect can be obtained.

[0161] 4. Uses of Secondary Batteries There are no particular limitations on the uses (application examples) of secondary batteries. Secondary batteries used as power sources may be the main power source or auxiliary power source in electronic devices, electric vehicles, and the like. The main power source is a power source that is used preferentially regardless of the presence or absence of other power sources. The auxiliary power source may be a power source used in place of the main power source or a power source that can be switched from the main power source.

[0162] Specific examples of uses for secondary batteries are as follows: Electronic devices such as video cameras, digital still cameras, mobile phones, laptop computers, headphone stereos, portable radios, and portable information terminals. Storage devices such as backup power supplies and memory cards. Power tools such as power drills and power saws. Battery packs installed in electronic devices. Medical electronic devices such as pacemakers and hearing aids. Electric vehicles such as electric cars (including hybrid cars). Power storage systems such as home or industrial battery systems that store power in preparation for emergencies. In these uses, one secondary battery may be used, or multiple secondary batteries may be used.

[0163] The battery pack may use a single cell or a battery pack. The electric vehicle is a vehicle that runs on a secondary battery as a driving power source, and may be a hybrid vehicle that also has a driving source other than the secondary battery. In a home power storage system, power stored in a secondary battery, which is a power storage source, can be used to power home electrical appliances, etc.

[0164] Here, an example of an application of the secondary battery will be specifically described. The configuration of the application described below is merely an example and can be modified as appropriate.

[0165] Figure 4 shows the block diagram of a battery pack. The battery pack described here is a battery pack (a so-called soft pack) that uses one secondary battery, and is installed in electronic devices such as smartphones.

[0166] The battery pack includes a power source 51 and a circuit board 52. The circuit board 52 is connected to the power source 51 and includes a positive terminal 53, a negative terminal 54, and a temperature detection terminal 55.

[0167] The power source 51 includes one secondary battery. The positive electrode lead of this secondary battery is connected to a positive electrode terminal 53, and the negative electrode lead is connected to a negative electrode terminal 54. The power source 51 can be connected to the outside via the positive electrode terminal 53 and the negative electrode terminal 54, and is therefore capable of charging and discharging. The circuit board 52 includes a control unit 56, a switch 57, a PTC element 58, and a temperature detection unit 59. However, the PTC element 58 may be omitted.

[0168] The control unit 56 includes a central processing unit (CPU) and memory, and controls the operation of the entire battery pack. The control unit 56 detects and controls the usage state of the power source 51 as necessary.

[0169] When the voltage of the power supply 51 (secondary battery) reaches the overcharge detection voltage or the overdischarge detection voltage, the control unit 56 turns off the switch 57 to prevent the charging current from flowing through the current path of the power supply 51. The overcharge detection voltage is not particularly limited, but specifically, it is 4.20 V±0.05 V. The overdischarge detection voltage is not particularly limited, but specifically, it is 2.40 V±0.1 V.

[0170] Switch 57 includes a charge control switch, a discharge control switch, a charge diode, a discharge diode, etc., and switches between the connection and disconnection of power supply 51 and an external device in response to instructions from control unit 56. Switch 57 includes a metal oxide semiconductor field effect transistor (MOSFET), etc., and the charge / discharge current is detected based on the ON resistance of switch 57.

[0171] Temperature detection unit 59 includes a temperature detection element such as a thermistor. Temperature detection unit 59 measures the temperature of power supply 51 using temperature detection terminal 55 and outputs the temperature measurement result to control unit 56. The temperature measurement result measured by temperature detection unit 59 is used when control unit 56 performs charge / discharge control in the event of abnormal heat generation and when control unit 56 performs correction processing when calculating the remaining capacity.

[0172] An embodiment of the present technology will be described.

[0173] Examples 1 to 12 and Comparative Examples 1 to 3 As will be described below, secondary batteries were manufactured, and then the battery characteristics of the secondary batteries were evaluated.

[0174] [Manufacturing of Secondary Battery] FIG. 5 shows a cross-sectional structure of a test secondary battery, which is a so-called coin-type secondary battery (lithium ion secondary battery).

[0175] This secondary battery includes a test electrode 61, a counter electrode 62, a separator 63, an exterior cup 64, an exterior can 65, a gasket 66, and an electrolyte (not shown).

[0176] The test electrode 61 is housed in an exterior cup 64, and the counter electrode 62 is housed in an exterior can 65. The test electrode 61 and the counter electrode 62 are stacked together with a separator 63 interposed therebetween, and the test electrode 61, the counter electrode 62, and the separator 63 are impregnated with an electrolyte. The exterior cup 64 and the exterior can 65 are crimped together with a gasket 66, so that the test electrode 61, the counter electrode 62, and the separator 63 are sealed by the exterior cup 64 and the exterior can 65.

[0177] A coin-type secondary battery shown in FIG. 5 was fabricated according to the procedure described below.

[0178] (Preparation of Test Electrode) When preparing the test electrode 61, first, a carboxymethyl cellulose salt (thickener), a powdered positive electrode conductive agent, and an aqueous solvent (pure water) were mixed together to prepare a first mixed solution, and then the first mixed solution was stirred (pre-mixed) using a planetary mixer.

[0179] As the carboxymethyl cellulose salt, sodium carboxymethyl cellulose (CMCNa) was used. As the positive electrode conductive agent, carbon black, Ketjen black (KC, specific surface area = 800 m) was used. 2  / g) and acetylene black (AB, specific surface area = 133 m 2  / g) was used.

[0180] Subsequently, a plurality of positive electrode active material particles and an aqueous solvent (pure water) were added to the first mixed solution to prepare a second mixed solution, and the second mixed solution was then stirred (main kneading) using a planetary mixer.

[0181] The positive electrode active material particles are composed of a powder of lithium iron phosphate compound (LiFePO), which is an olivine-type phosphate compound. 4  (LFP), median diameter MD1 = 1.0 μm and median diameter MD2 = 9.0 μm) were used.

[0182] Next, the emulsion liquid of the positive electrode binder and an aqueous solvent (pure water) were added to the second mixed solution, and the second mixed solution was stirred using a planetary mixer to prepare a positive electrode mixture slurry containing a plurality of positive electrode active material particles, the positive electrode binder, the positive electrode conductive agent, and the carboxymethyl cellulose salt.

[0183] The positive electrode binder was a copolymer of methyl acrylate and acrylonitrile (PAA), which is an acrylic acid ester polymer (acrylic acid ester copolymer). In this case, the copolymerization amount of methyl acrylate was 50 wt % and the copolymerization amount of acrylonitrile was 50 wt %.

[0184] When preparing the positive electrode mixture slurry, the solid content concentrations of the first and second mixed liquids were set to 72%, and the solid content concentration of the positive electrode mixture slurry was set to 62%.

[0185] Next, the positive electrode mixture slurry was applied to one surface of a positive electrode current collector (aluminum foil having a thickness of 12 μm) using a coating device, and then the positive electrode mixture slurry was dried to form a positive electrode active material layer. In this case, the amount of the positive electrode mixture slurry applied was 22 mg / cm. 2  Subsequently, the positive electrode active material layer was compression-molded using a roll press. In this case, the volume density of the positive electrode active material layer was 2.1 g / cm 3  It was decided.

[0186] Finally, the positive electrode current collector on which the positive electrode active material layer was formed was punched out into a disk shape (diameter = 16.5 mm), thereby producing a test electrode 61.

[0187] After producing the test electrode 61, the content (wt %) of the positive electrode binder in the positive electrode active material layer 21B, the content (wt %) of the carboxymethyl cellulose salt in the positive electrode active material layer 21B, the content (wt %) of the positive electrode conductive agent in the positive electrode active material layer 21B, and the volume resistivity R (Ω cm) were examined.

[0188] In this case, the content of the positive electrode binder in the positive electrode active material layer 21B was 3.0 wt %, and the content of the carboxymethyl cellulose salt in the positive electrode active material layer 21B was 1.0 wt %. The content of the positive electrode conductor and the volume resistivity R in the positive electrode active material layer 21B were as shown in Table 1.

[0189] For comparison, a test electrode 61 was produced using the same procedure except that carbon nanotubes (CNT, average fiber length = 150 μm) were used as the positive electrode conductive agent instead of carbon black (Ketjen black). In Table 1, the symbol (*) before "CNT" indicates that carbon nanotubes, which do not fall under the category of carbon black, are exceptionally shown in the "Carbon Black" column.

[0190] (Fabrication of Counter Electrode) A lithium metal plate was punched out into a disk shape (diameter = 17 mm), thereby obtaining a counter electrode 62.

[0191] (Preparation of Electrolyte Solution) A solvent (ethylene carbonate, which is a cyclic carbonate ester, and diethyl carbonate, which is a chain carbonate ester) was dissolved in an electrolyte salt (lithium hexafluorophosphate (LiPF 6  )) was added, and the solvent was stirred. In this case, the mixing ratio (weight ratio) of the solvents was ethylene carbonate:diethyl carbonate=30:70, and the content of the electrolyte salt in the electrolytic solution was 1 mol / kg relative to the solvent. In this way, the electrolytic solution was prepared.

[0192] (Assembly of Secondary Battery) First, the test electrode 61 was placed in the exterior cup 64, and the counter electrode 62 was placed in the exterior can 65. Next, the test electrode 61 placed in the exterior cup 64 and the counter electrode 62 placed in the exterior can 65 were stacked together via a separator 63 (a microporous polyethylene film with a thickness of 20 μm and a diameter of 17.5 mm) impregnated with an electrolyte. In this case, the positive electrode active material layer and the counter electrode 62 faced each other via the separator 63. Next, with the test electrode 61 and the counter electrode 62 stacked together via the separator 63, the exterior cup 64 and the exterior can 65 were crimped together via a gasket 66. As a result, the test electrode 61 and the counter electrode 62 were sealed by the exterior cup 64 and the exterior can 65, thereby assembling a secondary battery. Finally, the assembled secondary battery was left to stand (standing time = 10 hours).

[0193] This completed the secondary battery.

[0194] [Evaluation of Battery Characteristics] When the electrical resistance characteristics were evaluated as the battery characteristics, the results shown in Table 1 were obtained.

[0195] When evaluating the electrical resistance characteristics, first, the secondary battery was charged in a room temperature environment (temperature = 23°C) until the battery voltage reached 3.5V.

[0196] Subsequently, in the same environment, the secondary battery was discharged at a current of 2.0 C while measuring the discharge capacity (mAh / g). 2.0 C is a current value at which the battery capacity (theoretical capacity) is fully discharged in 0.5 hours.

[0197] Finally, the battery voltage (V) was measured when the discharge capacity reached 100 mAh / g. Based on the battery voltage, the electrical state of the secondary battery, which is an index for evaluating the electrical resistance characteristics, was determined. The results of the determination of the electrical state of the secondary battery are shown in Table 1.

[0198] Specifically, when the battery voltage was 3.0 V or higher, the battery voltage was maintained almost without any significant drop, and was therefore rated as "A." When the battery voltage was 2.8 V or higher but less than 3.0 V, the battery voltage did not drop excessively but remained within the allowable range, and was therefore rated as "B." When the battery voltage was less than 2.8 V, the battery voltage dropped excessively, and was therefore rated as "C."

[0199]

[0200] [Discussion] As shown in Table 1, the electrical resistance characteristics varied depending on the physical property (volume resistivity R) of the test electrode 61 .

[0201] Specifically, even when carbon black was used as the positive electrode conductive agent, when the volume resistivity R was greater than 100 Ω cm (Comparative Example 1) and when the volume resistivity R was less than 10 Ω cm (Comparative Example 2), the battery voltage was excessively reduced, and the electrical resistance characteristics were deteriorated.

[0202] This tendency for the electrical resistance characteristics to deteriorate was also observed when carbon nanotubes were used as the positive electrode conductive agent (Comparative Example 3).

[0203] In contrast, when carbon black was used as the positive electrode conductive agent and the volume resistivity R was 10 Ω cm to 100 Ω cm (Examples 1 to 12), the battery voltage did not decrease excessively but decreased within an allowable range, and therefore the electrical resistance characteristics were improved.

[0204] In this case (Examples 1 to 12), when the carbon black was Ketjen black, the electrical resistance characteristics were further improved.

[0205] Examples 13 to 18 Secondary batteries were fabricated in the same manner as in Example 2, except that the content (wt %) of the positive electrode binder in the positive electrode active material layer 21B was changed as shown in Table 2, and then the battery characteristics of the secondary batteries were evaluated.

[0206]

[0207] As shown in Table 2, even when the content of the positive electrode binder in the positive electrode active material layer 21B was changed, results similar to those in Table 1 were obtained. In this case, particularly when the content of the positive electrode binder in the positive electrode active material layer 21B was 0.5 wt % to 4.0 wt %, the battery voltage was almost maintained with almost no decrease.

[0208] Examples 19 to 23 Secondary batteries were fabricated in the same manner as in Example 2, except that the content (wt %) of carboxymethyl cellulose salt in the positive electrode active material layer 21B was changed as shown in Table 3, and then the battery characteristics of the secondary batteries were evaluated.

[0209]

[0210] As shown in Table 3, even when the content of carboxymethyl cellulose salt in the positive electrode active material layer 21B was changed, results similar to those in Table 1 were obtained. In this case, particularly when the content of carboxymethyl cellulose salt in the positive electrode active material layer 21B was 0.6 wt % to 2.0 wt %, the battery voltage was almost maintained with almost no decrease.

[0211] Examples 24 to 31 Secondary batteries were fabricated in the same manner as in Example 2, except that the median diameters MD1 and MD2 were changed as shown in Table 4, and then the battery characteristics of the secondary batteries were evaluated.

[0212] Here, not only electrical resistance characteristics but also cycle characteristics were evaluated as battery characteristics. To evaluate cycle characteristics, first, the discharge capacity (discharge capacity at the first cycle) was measured by charging and discharging the secondary battery in a room temperature environment. Next, the discharge capacity (discharge capacity at the 100th cycle) was measured by repeatedly charging and discharging the secondary battery in the same environment until the total number of cycles reached 100. Finally, the cycle retention rate, which is an index for evaluating cycle characteristics, was calculated based on the formula: capacity retention rate (%) = (discharge capacity at the 100th cycle / discharge capacity at the first cycle) × 100.

[0213] During charging, the battery was charged at a constant current of 0.1 C until the voltage reached 3.6 V, and then charged at a constant voltage of 3.6 V until the current reached 0.05 C. During discharging, the battery was discharged at a constant current of 0.1 C until the voltage reached 2.0 V. 0.1 C is the current value at which the battery capacity (theoretical capacity) is fully discharged in 10 hours, and 0.05 C is the current value at which the battery capacity is fully discharged in 20 hours.

[0214]

[0215] As shown in Table 4, even when the median diameters MD1 and MD2 were changed, the same results as those in Table 1 were obtained. In this case, particularly when the median diameter MD1 was 1 μm or less and the median diameter MD2 was 4 μm to 20 μm, and the content of carboxymethyl cellulose salt in the positive electrode active material layer 21B was 0.6 wt % to 2.0 wt %, the battery voltage was almost maintained with almost no decrease, and the capacity retention rate increased.

[0216] [Summary] From the results shown in Tables 1 to 4, when positive electrode active material layer B contains a plurality of positive electrode active material particles (olivine-type phosphate compound), a positive electrode binder (acrylic acid ester polymer), a positive electrode conductor (carbon black), and a carboxymethyl cellulose salt, and when the volume resistivity R of positive electrode active material layer 100B is 10 Ω cm to 100 Ω cm or less, the electrical resistance characteristics are improved. Therefore, excellent battery characteristics are obtained in the secondary battery.

[0217] The present technology has been described above with reference to an embodiment and examples. However, the configuration of the present technology is not limited to the configuration described in the embodiment and examples, and can be modified in various ways.

[0218] Specifically, the battery structure of the secondary battery has been described as being cylindrical and coin-shaped. However, the battery structure of the secondary battery is not particularly limited, and may be a laminate film type, a square type, a button type, or the like.

[0219] The battery element has been described as having a wound structure. However, the structure of the battery element is not particularly limited, and may be a stacked structure or a zigzag structure. In the stacked structure, the positive and negative electrodes are stacked on top of each other, and in the zigzag structure, the positive and negative electrodes are folded in a zigzag pattern.

[0220] Furthermore, although the electrode reactant is lithium in the above description, the electrode reactant is not particularly limited. Specifically, as described above, the electrode reactant may be other alkali metals such as sodium and potassium, or alkaline earth metals such as beryllium, magnesium, and calcium. In addition, the electrode reactant may be other light metals such as aluminum.

[0221] The effects described in this specification are merely examples, and therefore the effects of the present technology are not limited to the effects described in this specification. Therefore, other effects may be obtained with respect to the present technology.

[0222] The present technology may also be configured as follows. <1> A secondary battery comprising: a positive electrode including a positive electrode active material layer; a negative electrode; and an electrolyte; wherein the positive electrode active material layer contains a plurality of positive electrode active material particles, a positive electrode binder, a positive electrode conductor, and a carboxymethyl cellulose salt; the positive electrode active material particles contain a phosphate compound having an olivine crystal structure; the positive electrode binder contains an acrylic acid ester polymer; the positive electrode conductor contains carbon black; and the volume resistivity of the positive electrode active material layer is 10 Ω·cm or more and 100 Ω·cm or less. <2> The secondary battery according to <1>, wherein the carbon black contains ketjen black. <3> The secondary battery according to <1> or <2>, wherein the content of the positive electrode conductor in the positive electrode active material layer is 0.5 wt % or more and 3.0 wt % or less. <4> The secondary battery according to any one of <1> to <3>, wherein the phosphate compound contains lithium and iron as constituent elements. <5> The secondary battery according to any one of <1> to <4>, wherein the acrylic acid ester polymer includes a copolymer of acrylic acid ester and acrylonitrile. <6> The secondary battery according to any one of <1> to <5>, wherein the content of the positive electrode binder in the positive electrode active material layer is 0.5% by weight or more and 4.0% by weight or less. <7> The secondary battery according to any one of <1> to <6>, wherein the carboxymethyl cellulose salt includes sodium carboxymethyl cellulose. <8> The secondary battery according to any one of <1> to <7>, wherein the content of the carboxymethyl cellulose salt in the positive electrode active material layer is 0.6% by weight or more and 2.0% by weight or less. <9> The secondary battery according to any one of <1> to <8>, wherein the positive electrode active material particles are secondary particles formed by aggregating a plurality of primary particles, wherein the median diameter of the plurality of primary particles is 1 μm or less, and wherein the median diameter of the plurality of positive electrode active material particles that are the plurality of secondary particles is 4 μm or more and 20 μm or less. <10> The secondary battery according to any one of <1> to <9>, which is a lithium ion secondary battery.<11> A positive electrode for a secondary battery, comprising: a positive electrode active material layer; the positive electrode active material layer comprising a plurality of positive electrode active material particles, a positive electrode binder, a positive electrode conductor, and a carboxymethyl cellulose salt; the positive electrode active material particles comprising a phosphate compound having an olivine crystal structure; the positive electrode binder comprising an acrylic acid ester polymer; and the positive electrode conductor comprising carbon black; and a volume resistivity of the positive electrode active material layer being 10 Ω cm or more and 100 Ω cm or less.

[0223] 20... Battery element, 21... Positive electrode, 21B... Positive electrode active material layer, 22... Negative electrode

Claims

1. A secondary battery comprising: a positive electrode including a positive electrode active material layer; a negative electrode; and an electrolyte; wherein the positive electrode active material layer contains a plurality of positive electrode active material particles, a positive electrode binder, a positive electrode conductor, and a carboxymethyl cellulose salt; the positive electrode active material particles contain a phosphate compound having an olivine type crystal structure; the positive electrode binder contains an acrylic acid ester polymer; the positive electrode conductor contains carbon black; and the volume resistivity of the positive electrode active material layer is 10 Ω·cm or more and 100 Ω·cm or less.

2. The secondary battery according to claim 1, wherein the carbon black includes Ketjen black.

3. The secondary battery according to claim 1 or 2, wherein the content of the positive electrode conductive agent in the positive electrode active material layer is 0.5% by weight or more and 3.0% by weight or less.

4. The secondary battery according to any one of claims 1 to 3, wherein the phosphate compound contains lithium and iron as constituent elements.

5. The secondary battery according to any one of claims 1 to 4, wherein the acrylic ester polymer includes a copolymer of acrylic ester and acrylonitrile.

6. The secondary battery according to claim 1, wherein the content of the positive electrode binder in the positive electrode active material layer is 0.5% by weight or more and 4.0% by weight or less.

7. The secondary battery according to any one of claims 1 to 6, wherein the carboxymethylcellulose salt includes sodium carboxymethylcellulose.

8. The secondary battery according to any one of claims 1 to 7, wherein the content of the carboxymethyl cellulose salt in the positive electrode active material layer is 0.6% by weight or more and 2.0% by weight or less.

9. The secondary battery according to any one of claims 1 to 8, wherein the positive electrode active material particles are secondary particles formed by aggregating a plurality of primary particles, the median diameter of the primary particles is 1 μm or less, and the median diameter of the positive electrode active material particles which are the secondary particles is 4 μm or more and 20 μm or less.

10. The secondary battery according to claim 1, which is a lithium ion secondary battery.

11. A positive electrode for a secondary battery, comprising: a positive electrode active material layer, the positive electrode active material layer comprising a plurality of positive electrode active material particles, a positive electrode binder, a positive electrode conductor, and a carboxymethyl cellulose salt, the positive electrode active material particles comprising a phosphate compound having an olivine type crystal structure, the positive electrode binder comprising an acrylic acid ester polymer, the positive electrode conductor comprising carbon black, and a volume resistivity of the positive electrode active material layer being 10 Ω·cm or more and 100 Ω·cm or less.

Citation Information

Patent Citations

  • Electrode composition for nonaqueous electrolyte secondary battery, and electrode and battery using the same

    JP2012124181A

  • Method of producing composition containing plural positive electrode active materials, conductive assistant, binder and solvent

    JP2017054649A

  • Positive electrode for lithium ion secondary battery

    JP2021044236A

  • Positive electrode active material fine particles, positive electrode and secondary battery, and manufacturing method of positive electrode active material fine particles

    JP2023022752A

  • Positive electrode active material, positive electrode, nonaqueous electrolyte power storage element, power storage device, method for producing positive electrode active material, method for producing positive electrode, and method for producing nonaqueous electrolyte power storage element

    WO2022050101A1

Cited By

  • Electrode slurry for lithium iron phosphate battery, preparation method of electrode slurry, positive plate, negative plate and lithium ion battery

    CN119786786A