Electrophotographic photoreceptor

The use of compounds with specific electron transporting structures and polymerizable functional groups in the protective layer of electrophotographic photoreceptors addresses the challenges of electrical and mechanical properties, achieving improved residual potential, hardness, and solubility, resulting in efficient and effective photoreceptor performance.

WO2024204544A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP

Patent Information

Application Number
PCT/JP2024/012663
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Electrophotographic photoreceptors face challenges in achieving excellent electrical properties such as residual potential, hardness, and elastic deformation rate, while also requiring good solubility of compounds used in the protective layer, particularly those with electron transporting structures, which often have insufficient solubility and mechanical properties.

Method used

The use of specific compounds represented by formula (1) with electron transporting structures, satisfying molecular weight and solubility ratios, and containing polymerizable functional groups, which form a protective layer with improved charge mobility and mechanical strength, enhancing electron transport properties and solubility in organic solvents.

Benefits of technology

The proposed solution results in electrophotographic photoreceptors with enhanced electrical and mechanical properties, including improved residual potential, hardness, and elastic deformation rate, while ensuring excellent solubility of the protective layer compounds, leading to efficient manufacturing and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012663_03102024_PF_FP_ABST
    Figure JP2024012663_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an electrophotographic photoreceptor having at least a photosensitive layer and a protective layer in this order on a conductive support body, and provides an electrophotographic photoreceptor which has superior electrical characteristics such as a residual potential characteristic and mechanical characteristics such as hardness and elastic deformation rate, and for which an electron transporting compound that is used in the formation of the protective layer has superior solubility in organic solvents. The electrophotographic photoreceptor has at least a photosensitive layer and a protective layer in this order on a conductive support body, wherein the protective layer includes a compound represented by formula (1), and the compound represented by formula (1) satisfies expression (I) and expression (II-1). (I): METM≥700 (II-1): 0.32≤MX / METM≤0.60 (In expression (I) and expression (II-1), METM represents the molecular weight of the compound represented by formula (1). In expression (II-1), MX represents the molecular weight of a compound resulting from substituting a hydrogen atom at every bonding site of X in formula (1).)
Need to check novelty before this filing date? Find Prior Art

Description

Electrophotographic photoreceptor

[0001] The present invention relates to an electrophotographic photoreceptor for use in copiers, printers, etc., which has at least a photosensitive layer and a protective layer sequentially on a conductive support, and which has improved electrical properties such as residual potential characteristics, and improved mechanical properties such as hardness and elastic deformation rate.

[0002] In printers and copiers, when a charged organic photoconductor (OPC) drum is irradiated with light, the part is discharged, an electrostatic latent image is formed, and an image is obtained by attaching toner to the electrostatic latent image. In such devices that use electrophotography, the photoconductor is a key component.

[0003] Because this type of organic photoreceptor offers a wide range of material options and allows for easy control of photoreceptor properties, "function-separated photoreceptors," in which the functions of charge generation and transport are shared by separate compounds, have become mainstream. For example, known electrophotographic photoreceptors include a single-layer electrophotographic photoreceptor (hereinafter referred to as a "single-layer photoreceptor") that contains a charge-generating material (CGM) and a charge-transport material (CTM) in the same layer, and a multilayer electrophotographic photoreceptor (hereinafter referred to as a "multilayer photoreceptor") that consists of a charge-generating layer containing a charge-generating material (CGM) and a charge-transport layer containing a charge-transport material (CTM). Furthermore, photoreceptor charging methods include a negative charging method, in which the photoreceptor surface is negatively charged, and a positive charging method, in which the photoreceptor surface is positively charged. Currently available photoreceptor layer configuration and charging method combinations include a "negatively charged multilayer photoreceptor" and a "positively charged single-layer photoreceptor."

[0004] A "negatively charged laminated photoreceptor" generally has a structure in which an undercoat layer (UCL) made of a resin or the like is provided on a conductive substrate such as an aluminum tube, on which a charge generation layer (CGL) made of a charge generation material (CGM) and a resin or the like is provided, and on which a charge transport layer (CTL) made of a hole transport material (HTM) and a resin or the like is provided.

[0005] On the other hand, a "positively charged single-layer photoreceptor" generally has a configuration in which an undercoat layer (UCL) made of a resin or the like is provided on a conductive substrate such as an aluminum tube, and a single-layer photosensitive layer made of a charge generating material (CGM), a hole transporting material (HTM), an electron transporting material (ETM), and a resin or the like is provided thereon (see, for example, Patent Document 1).

[0006] In either case, the surface of the photoreceptor is first charged using corona discharge or contact, and then the photoreceptor is exposed to light to neutralize the surface charge, forming an electrostatic latent image due to the potential difference with the surrounding surface. Toner is then brought into contact with the photoreceptor surface to form a toner image corresponding to the electrostatic latent image, which is then transferred to paper or other media and heated to fuse and fix to create a print.

[0007] As described above, the basic structure of an electrophotographic photoreceptor is a photosensitive layer formed on a conductive support, but a protective layer may also be provided on the photosensitive layer for the purpose of improving abrasion resistance, etc.

[0008] As a technique for improving the mechanical strength or abrasion resistance of the photoreceptor surface, a photoreceptor has been disclosed in which a layer containing a compound having a chain-polymerizable functional group as a binder resin is formed on the outermost layer of the photoreceptor, and this is polymerized by applying energy such as heat, light, or radiation to form a cured resin layer (see, for example, Patent Documents 1 and 2). Such a protective layer is generally formed by dissolving a curable composition containing a compound having a chain-polymerizable functional group in an organic solvent to prepare a coating liquid for forming the protective layer, and then applying the coating liquid for forming the protective layer to the surface of the photoreceptor.

[0009] U.S. Patent No. 9,417,538 International Publication No. 2010 / 035683

[0010] It is known that a protective layer is provided to improve the abrasion resistance of a photoreceptor. Among these, protective layers using curable compounds (compounds having chain-polymerizable functional groups) have particularly excellent mechanical strength. Furthermore, from the viewpoint of improving the electrical properties of a photoreceptor, the protective layer is also required to have good electron transport properties. Furthermore, from the viewpoint of improving abrasion resistance, the protective layer is required to have high hardness and elastic deformation rate. That is, to improve the abrasion resistance and electrical properties of a photoreceptor, it is considered effective to use a compound having an electron transport structure as the curable compound forming the protective layer. However, it has been found that some compounds having an electron transport structure have insufficient solubility when preparing a coating solution for forming a protective layer. It has also been found that some photoreceptors having a protective layer formed thereon have insufficient residual potential, hardness, and elastic deformation rate.

[0011] An object of the present invention is to provide an electrophotographic photoreceptor having at least a photosensitive layer and a protective layer successively formed on a conductive support, which is excellent in electrical properties such as residual potential characteristics, and mechanical properties such as hardness and elastic deformation rate, and which also has excellent solubility in organic solvents of a compound used to form the protective layer.

[0012] The present inventors have found that when a compound represented by the following formula (1) and satisfying the following formulas (I) and (II-1), or a compound represented by the following formula (1) and satisfying the following formulas (I) to (III), is used as a compound for forming a protective layer, the solubility is improved and the residual potential, hardness, and elastic deformation rate are also improved. The present invention was achieved based on this finding and is summarized as follows.

[0013] [1] An electrophotographic photoreceptor having at least a photosensitive layer and a protective layer formed in this order on a conductive support, wherein the protective layer contains a compound represented by the following formula (1), and the compound represented by the formula (1) satisfies the following formulas (I) and (II-1):

[0014]

[0015] In formula (1), X represents an n-valent electron transport skeleton. A represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, a group represented by formula (2) below, or a group represented by formula (1B) below. n represents an integer of 1 or greater. When n is 1, A represents a group represented by formula (2) below or a group represented by formula (1B) below. When n is 2 or greater, multiple A's may be the same or different, and at least one A represents a group represented by formula (2) below or a group represented by formula (1B) below.

[0016]

[0017] In formula (2), * represents a bond to X. 1 and R 2each independently represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a group represented by the following formula (1B). 1 and L 2 each independently represents a direct bond, a divalent group, a group represented by the following formula (1A) or a group represented by the following formula (3A), Z represents a hydrogen atom, an alkyl group, an alkoxy group, an amide group, or a polymerizable functional group, provided that x1 + y1 = 3, where x1 is an integer of 0 to 2 and y1 is an integer of 1 to 3, x2 + y2 = 3, where x2 is an integer of 0 to 2 and y2 is an integer of 1 to 3, and when x1 is an integer of 2 or more, R 1 may be the same or different from each other, and when y1 is an integer of 2 or more, R 2 , x2, y2, L 1 , L 2 and Z may be the same or different from each other, and when x2 is an integer of 2 or more, R 2 may be the same or different from each other, and when y2 is an integer of 2 or more, L 2 and Z may be the same or different from each other.

[0018]

[0019] In formula (1B), * represents a bond to any atom in formula (1) or (2), and B 1 and B 2 R each independently represents a direct bond or a divalent group. 3represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a polymerizable functional group.

[0020]

[0021]

[0022] In formula (1A) and formula (3A), * represents a bond to any atom in formula (1) and formula (2). 1 and B 2 each independently represents a direct bond or a divalent group. In formula (3A), n is an integer of 1 or more.

[0023] M ETM ≧700 (I) 0.32≦M X / M ETM ≦0.60 (II-1) (In formula (I) and formula (II-1), M ETM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) have been replaced with hydrogen atoms.

[0024] [2] An electrophotographic photoreceptor having at least a photosensitive layer and a protective layer formed in this order on a conductive support, wherein the protective layer contains a polymer of a compound represented by the following formula (1), and the compound represented by the formula (1) satisfies the following formulas (I), (II-2), and (III):

[0025]

[0026] In formula (1), X represents an n-valent electron transport skeleton. A represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, a group represented by formula (2) below, or a group represented by formula (1B) below. n represents an integer of 1 or greater. When n is 1, A represents a group represented by formula (2) below or a group represented by formula (1B) below. When A represents a group represented by formula (2) below, at least one of Z's is a polymerizable functional group. When A represents a group represented by formula (1B) below, R 3 is a polymerizable functional group. When n is 2 or more, the multiple A's may be the same as or different from one another, and at least one A is a group represented by the following formula (2) or a group represented by the following formula (1B), and the structure contains at least one polymerizable functional group.

[0027]

[0028] In formula (2), * represents a bond to X. 1 and R 2L each independently represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a group represented by the following formula (1B): 1 and L 2 each independently represents a direct bond, a divalent group, a group represented by the following formula (1A) or a group represented by the following formula (3A), Z represents a hydrogen atom, an alkyl group, an alkoxy group, an amide group, or a polymerizable functional group, provided that x1 + y1 = 3, where x1 is an integer of 0 to 2 and y1 is an integer of 1 to 3, x2 + y2 = 3, where x2 is an integer of 0 to 2 and y2 is an integer of 1 to 3, and when x1 is an integer of 2 or more, R 1 may be the same or different from each other, and when y1 is an integer of 2 or more, R 2 , x2, y2, L 1 , L 2 and Z may be the same or different from each other, and when x2 is an integer of 2 or more, R 2 may be the same or different from each other, and when y2 is an integer of 2 or more, L 2 and Z may be the same or different from each other.

[0029]

[0030] In formula (1B), * represents a bond to any atom in formula (1) or (2), and B 1 and B 2 R each independently represents a direct bond or a divalent group. 3represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a polymerizable functional group.

[0031]

[0032]

[0033] In formula (1A) and formula (3A), * represents a bond to any atom in formula (1) and formula (2). 1 and B 2 each independently represents a direct bond or a divalent group. In formula (3A), n is an integer of 1 or more.

[0034] M ETM ≧700 (I) M X / M ETM >0.31 (II-2) A ETM ≧1.8 (III)

[0035] In formula (I) and formula (II-2), M ETM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms. ETM represents the number of polymerizable functional groups contained per 1000 of molecular weight of the compound represented by formula (1).

[0036] [3] The electrophotographic photoreceptor according to [1] or [2] above, wherein the compound represented by formula (1) further satisfies the following formula (IV):X ≧3.8 (IV) (In formula (IV), EA X represents the electron affinity (eV) of the compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms.

[0037] [4] The electrophotographic photoreceptor according to any one of [1] to [3] above, wherein in formula (1), X is represented by formulas (A-1) to (A-27) shown below.

[0038] [5] The electrophotographic photoreceptor according to any one of [1] to [4] above, wherein at least one of A in the formula (1) is represented by the formula (2).

[0039] [6] In the formula (2), L and L 2 [6] The electrophotographic photoreceptor according to any one of [1] to [5] above, wherein at least one of the following is a group represented by formula (1A) or a group represented by formula (3A).

[0040] [7] The electrophotographic photoreceptor according to any one of [1] to [6] above, wherein the compound represented by formula (1) has at least one polymerizable functional group in one molecule. [8] The electrophotographic photoreceptor according to any one of [1] to [7] above, wherein the polymerizable functional group is selected from the following formulae (M1) to (M7):

[0041]

[0042] In the above formulas (M1) to (M7), R 110 represents a hydrogen atom or an alkyl group which may have a substituent, and * represents the bonding position.

[0043] [9] In the formula (2), R 1 [9] The electrophotographic photoreceptor according to any one of [1] to [8] above, wherein is an alkyl group which may have a substituent.

[0044]

[10] The electrophotographic photoreceptor according to any one of [1] to [9], wherein the protective layer further contains a polymer of a polymerizable compound having no electron transport skeleton.

[11] The electrophotographic photoreceptor according to any one of [1] to

[10] , wherein the protective layer further contains an electron donating compound.

[0045]

[12] An electrophotographic photoreceptor cartridge having the electrophotographic photoreceptor according to any one of [1] to

[11] .

[13] An image forming apparatus having the electrophotographic photoreceptor according to any one of [1] to

[11] .

[0046] According to the present invention, it is possible to provide an electrophotographic photoreceptor having at least a photosensitive layer and a protective layer successively formed on a conductive support, which is excellent in electrical properties such as residual potential characteristics, and mechanical properties such as hardness and elastic deformation rate. Moreover, in the present invention, since the compound used to form the protective layer has excellent solubility in organic solvents such as alcohol-based solvents, in forming the protective layer, an electrophotographic photoreceptor having excellent electrical properties and mechanical properties can be efficiently produced with good workability due to its good solvent solubility.

[0047] 1 is a diagram illustrating an example of the configuration of an image forming apparatus that can be configured using an electrophotographic photosensitive member according to an embodiment of the present invention, and FIG. 2 is a graph illustrating a general relationship between the indentation depth of an indenter and a load curve when measuring the Martens hardness and elastic deformation rate of a photosensitive member.

[0048] The following describes in detail the mode for carrying out the present invention (hereinafter referred to as "embodiments of the invention"). Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the invention.

[0049] <<Photoreceptor of the Present Invention>> An electrophotographic photoreceptor according to one example of the embodiment of the present invention (hereinafter also referred to as "photoreceptor of the present invention") is an electrophotographic photoreceptor comprising at least a photosensitive layer and a protective layer, successively formed on a conductive support, and the protective layer contains Compound A or B of the present invention, which will be described below. When Compound A or B of the present invention has a polymerizable functional group in one molecule, it may be present in the form of a polymer in the protective layer after curing. For example, Compound A or B of the present invention may be polymerized with itself to form a polymer, or when the protective layer contains a curable compound, it may be polymerized with the curable compound to form a polymer.

[0050] The photoreceptor of the present invention may optionally have layers other than the photosensitive layer and the protective layer. The charging method of the photoreceptor of the present invention may be either a negative charging method in which the surface of the photoreceptor is negatively charged, or a positive charging method in which the surface of the photoreceptor is positively charged. Of these, the positive charging method is preferred, since it is considered that the effects of the present invention can be more effectively achieved with the positive charging method, which requires the protective layer to have electron transport properties.

[0051] In the photoreceptor of the present invention, the side opposite to the conductive support is the upper side or front side, and the conductive support side is the lower side or back side.

[0052] <Protective Layer> The protective layer of the photoreceptor of the present invention (sometimes referred to as "protective layer") contains a polymer of an electron transporting compound A (sometimes referred to as "compound A of the present invention") represented by the following formula (1) and satisfying the following formulas (I) and (II-1), or an electron transporting compound B (sometimes referred to as "compound B of the present invention") represented by the following formula (1) and satisfying the following formulas (I), (II-2), and (III). In this specification, "compounds A and B of the present invention" means compound A or B of the present invention, and "compound of the present invention" collectively means compounds A and B of the present invention.

[0053] In the present invention, the term "electron transporting compound" refers to a compound having electron transporting properties, in other words, a compound having an electron transporting skeleton.

[0054]

[0055] M ETM ≧700 (I) 0.32≦M X / M ETM ≦0.60 (II-1) (In formula (I) and formula (II-1), M ETM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) have been replaced with hydrogen atoms.

[0056] M ETM ≧700 (I) M X / M ETM>0.31 (II-2) A ETM ≧1.8 (III) (in formula (I) and formula (II-2), M ETM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms. ETM represents the number of polymerizable functional groups contained per 1,000 of molecular weight of the compound represented by formula (1).

[0057] The mechanism by which the photoreceptor of the present invention having a protective layer containing Compound A of the present invention exhibits excellent electrical properties is believed to be as follows. Compound A of the present invention has an electron-transporting structure. Therefore, by using Compound A of the present invention in forming the protective layer, charge injection from the photosensitive layer to the protective layer and charge mobility to the outermost surface are enhanced through the electron-transporting skeleton, resulting in an electrophotographic photoreceptor with excellent electrical properties, such as residual potential characteristics. Furthermore, when Compound A of the present invention has a polymerizable functional group, Compound A of the present invention is polymerized in the protective layer formation step described below to form a polymer, which can form a protective layer with excellent mechanical strength. In this case, the polymer may be a polymer formed by polymerizing Compound A itself, or, when a polymerizable compound without an electron-transporting skeleton is contained in the protective layer, it may be a copolymer formed by polymerizing Compound A of the present invention with the polymerizable compound. Furthermore, when Compound A of the present invention is equal to or less than the upper limit of Formula (II-1) below, the proportion of the mother skeleton, which is a hydrophobic π-conjugated skeleton, falls within a preferred range, resulting in increased solubility in alcohol-based solvents, improved coatability of the coating solution when forming the protective layer, and the formation of a uniform protective layer without unevenness. This is thought to improve the electron transport properties in the protective layer, resulting in improved electrical properties of the photoreceptor. Furthermore, when the ratio is equal to or greater than the lower limit of the following formula (II-1), the structure present in the protective layer that contributes to electron transport is high, and the electron transport properties are high, resulting in even better electrical properties. Furthermore, when compound A of the present invention satisfies formulas (I) and (II-1), the side chain moiety that contributes to solubility in alcohol-based solvents increases, resulting in even better solubility in alcohol-based solvents. Furthermore, when compound A of the present invention further satisfies formula (IV), electron injection from adjacent layers is good and the electron transport properties of the mother skeleton are excellent, resulting in even better electrical properties.

[0058] The mechanism by which the photoreceptor of the present invention having a protective layer containing a polymer of compound B of the present invention exhibits excellent electrical properties is believed to be as follows. Because compound B of the present invention has an electron-transporting structure, using compound B of the present invention in forming the protective layer enhances charge injection from the photosensitive layer to the protective layer and charge mobility to the outermost surface through the electron-transporting skeleton, resulting in an electrophotographic photoreceptor with excellent electrical properties such as residual potential characteristics. Furthermore, because compound B of the present invention has a polymerizable functional group, compound B of the present invention is polymerized during the protective layer formation process described below to form a polymer, which can form a protective layer with excellent mechanical strength. In this case, the polymer may be a polymer formed by polymerizing compounds of compound B of the present invention together, or, if the protective layer contains a polymerizable compound without an electron-transporting skeleton, it may be a copolymer formed by polymerizing compound B of the present invention with the polymerizable compound. Furthermore, when compound B of the present invention satisfies formula (I) and formula (II-2), the proportion of structures thought to contribute to electron transport in the protective layer increases, which is advantageous for electron transport. Furthermore, when formula (III) is satisfied, the protective layer contains a large number of polymerizable functional groups, which facilitates the formation of a dense network structure. As a result, the hardness and elastic deformation rate are improved. Furthermore, when the compound B of the present invention further satisfies formula (IV), electron injection from the adjacent layer is good and the electron transport property of the main skeleton is excellent, resulting in further improved electrical properties.

[0059] From the viewpoint of more effectively obtaining the effects of the compounds A and B of the present invention, the protective layer is preferably the outermost layer, i.e., the outermost layer located on the opposite side from the conductive support. However, the protective layer does not necessarily have to be the outermost layer to obtain the effects of the present invention. For example, in cases where some kind of segregation layer exists in the outermost layer of the photoreceptor, the protective layer can still obtain the effects even if it is not the outermost layer.

[0060] In the following, first, the compounds A and B of the present invention used in forming the protective layer of the present invention will be described, and then the composition containing the compounds A and B of the present invention (hereinafter also referred to as the "composition of the present invention" or "this composition") and the electrophotographic photoreceptor of the present invention will be described in sequence.

[0061] <<Compound A of the Present Invention>> Compound A of the present invention is preferably a compound represented by the following formula (1) and satisfying the following formulas (I) and (II-1).

[0062]

[0063] <X> In the above formula (1), X represents an electron-transporting skeleton having a valence of n. X is preferably a skeleton represented by any of the following formulas (A-1) to (A-27). When the electron-transporting skeleton is a skeleton represented by the following formula (A-10), (A-11), or (A-26), the electron-transporting property is excellent and the electrical properties (VL) are further improved, which is more preferable.

[0064]

[0065]

[0066]

[0067]

[0068]

[0069]

[0070]

[0071]

[0072]

[0073]

[0074]

[0075]

[0076]

[0077]

[0078]

[0079]

[0080]

[0081]

[0082]

[0083]

[0084]

[0085]

[0086]

[0087]

[0088]

[0089]

[0090]

[0091] In formulas (A-1) to (A-27), * represents a bond to A. A11 , R A21 , R A31 , R A41 , R A51 , R A61 , R A62 , R A71 , R A72 , R A81 , R A82 , R A91 , R A92 , R A101 , R A111 , R A121 , R A131 , R A141 , R A151 , R A161 , R A171 , R A181 , R A182 , R A191 , R A192 , R A201 , R A202 , R A211 , R A212 , R A221 , R A222 , R A231 , R A232 , R A241 , R A242 , R A251 , R A252 , R A261 , RA262 each independently represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted aralkyl group, an optionally substituted aromatic group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted acyl group, an optionally substituted ester group, a cyano group, a nitro group, an optionally substituted sulfone group, a hydroxy group, an optionally substituted aldehyde group, or a halogen atom.

[0092] In formulas (A-1) to (A-27), m11, m21, m31, m41, m51, m61, m62, m71, m72, m81, m82, m91, m92, m101, m111, m121, m131, m141, m151, m161, m171, m181, m182, m191, m192, m201, m202, m211, m212, m221, m222, m231, m232, m241, m242, m251, m252, m261, and m262 each independently represent an integer of 0 or more. When m11, m21, m31, m41, m51, m61, m62, m71, m72, m81, m82, m91, m92, m101, m111, m121, m131, m141, m151, m161, m171, m181, m182, m191, m192, m201, m202, m211, m212, m221, m222, m231, m232, m241, m242, m251, m252, m261, and m262 are each 2 or more, R A11 ~R A262 may be different from each other.

[0093] <n> In the above formula (1), n ​​represents an integer of 1 or more, and when n is 2 or more, a plurality of As may be the same or different from each other.

[0094] A in the above formula (1) is a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, a group represented by the following formula (2), or a group represented by the following formula (1B):

[0095] In the present invention, the phrase "optionally having a substituent" means that the group can have a substituent, and includes both the case where the group has a substituent and the case where the group does not have a substituent.

[0096] When n is 1, A is a group represented by the following formula (2) or a group represented by the following formula (1B). When A is a group represented by the following formula (2), at least one of Z is a polymerizable functional group. When A is a group represented by the following formula (1B), R 3 is a polymerizable functional group. When n is 2 or more, the multiple A's may be the same as or different from one another, and at least one A is a group represented by the following formula (2) or a group represented by the following formula (1B), and the structure contains at least one polymerizable functional group.

[0097] In particular, from the viewpoint of further improving the solubility in organic solvents, it is preferable that at least one of A is a group represented by the following formula (2).

[0098] (Group Represented by Formula (2)) The group represented by formula (2) is an example of A in the above formula (1).

[0099]

[0100] In formula (2), * represents a bond to X. 1 and R 2 each independently represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a group represented by the following formula (1B):

[0101] From the viewpoint of further improving the solubility in organic solvents, the group represented by formula (2) preferably has two branches and a polymerizable functional group in the side chain. 1 is an alkyl group which may have a substituent, the formula (2) is branched at the alkyl group, and the solubility in organic solvents is further improved, which is preferable.

[0102] In formula (2), L 1 and L 2 each independently represents a direct bond, a divalent group, a group represented by the following formula (1A) or a group represented by the following formula (3A). In particular, if the side chain having a urethane bond is branched, the solubility in organic solvents is further improved, so L 1 and L 2 At least one of the above is preferably a group represented by the following formula (1A) or a group represented by the following formula (3A).

[0103] In formula (2), Z represents a hydrogen atom, an alkyl group, an alkoxy group, an amide group, or a polymerizable functional group, provided that x1+y1=3, where x1 is an integer of 0 to 2 and y1 is an integer of 1 to 3, and x2+y2=3, where x2 is an integer of 0 to 2 and y2 is an integer of 1 to 3; and when x1 is an integer of 2 or more, R1 may be the same or different from each other, and when y1 is an integer of 2 or more, R 2 , x2, y2, L 1 , L 2 and Z may be the same or different from each other, and when x2 is an integer of 2 or more, R 2 may be the same or different from each other, and when y2 is an integer of 2 or more, L 2 and Z may be the same or different from each other.

[0104] (Group represented by formula (1B)) The group represented by formula (1B) is an example of A in the above formula (1), and is also an example of L in the above formula (2). 1 and L 2 This is also an example of...

[0105]

[0106] In formula (1B), * represents a bond to any atom in formula (1) or (2). 1 and B 2 R each independently represents a direct bond or a divalent group. 3 represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a polymerizable functional group.

[0107] (Group represented by formula (1A)) The group represented by formula (1A) is L in the above formula (2). 1 and L 2 This is an example.

[0108]

[0109] In formula (1A), * represents a bond to any atom in formula (1) and formula (2). 1 and B 2 each independently represents a direct bond or a divalent group. Examples of the divalent group include an alkylene group, a divalent group having a ketone group, a divalent group having an ether bond, a divalent group having an ester bond, or a group formed by linking these groups.

[0110] (Group represented by formula (3A)) The group represented by formula (3A) is L in the above formula (2). 1 and L 2 This is an example.

[0111]

[0112] In formula (3A), * represents a bond to any atom in formula (1) and formula (2), and n is an integer of 1 or more.

[0113] (Formula (I) and Formula (II-1)) Compound A of the present invention is preferably a compound that satisfies the following formula (I) and formula (II-1). ETM " represents the molecular weight of the compound represented by the formula (1). X " represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms.

[0114] M ETM ≧700 (I) 0.32≦M X / M ETM ≦0.60 (II-1)

[0115] As in formula (I), the molecular weight (M ETM From the viewpoint of film-forming property and charge transport property, it is preferable that the molecular weight (M ETM) is more preferably 750 or more, even more preferably 800 or more, even more preferably 900 or more, and particularly preferably 1000 or more. On the other hand, from the viewpoint of solubility, the molecular weight is preferably 2000 or less. Therefore, the molecular weight is preferably 1800 or less, even more preferably 1600 or less, even more preferably 1500 or less, and particularly preferably 1400 or less.

[0116] "M" in formula (II-1) X / M ETM " That is, the ratio of the molecular weight of a compound in which all bonding sites of X in Formula (1) are replaced with hydrogen atoms to the molecular weight of the compound represented by Formula (1) means the ratio of structures capable of participating in electron transfer in the compound. A ratio of 0.32 or more is preferable because the amount of structures present in the protective layer that contribute to electron transport increases, resulting in high electron transport properties and further improved electrical properties. From this perspective, the ratio is more preferably 0.33 or more, even more preferably 0.34 or more, even more preferably 0.35 or more, and particularly preferably 0.36 or more. On the other hand, a ratio of 0.60 or less is preferable because the proportion of the hydrophobic π-conjugated skeleton as the mother skeleton falls within a preferred range, resulting in high solubility in alcohol-based solvents and improved coatability of the coating solution when forming the protective layer. From this perspective, the ratio is more preferably 0.58 or less, even more preferably 0.56 or less, even more preferably 0.54 or less, and particularly preferably 0.53 or less.

[0117] The molecular weight (M X ) may be any molecular weight that satisfies the above formula (II-1). X ) is more preferably 250 or more, even more preferably 300 or more, even more preferably 350 or more, and particularly preferably 400 or more. On the other hand, it is preferably 800 or less, even more preferably 750 or less, even more preferably 700 or less, and particularly preferably 650 or less.

[0118] (Formula (IV)) It is particularly preferable that the compound A of the present invention is a compound further satisfying the following formula (IV): X represents the electron affinity (eV) of a compound in which all of the binding sites of X in the formula (1) are replaced with hydrogen atoms. As described in the Examples below, this parameter is determined by quantum scientific calculations.

[0119] EA X ≧3.8 (IV)

[0120] When the electron affinity (eV) of the compound in which all the bonding sites of X in the formula (1) are replaced with hydrogen atoms as in the formula (IV) is 3.8 or more, the electron injection property from the adjacent layer and the electron transport property in the protective layer become good, which is preferable. From this viewpoint, the electron affinity (EA X ) is more preferably 3.83 or more, even more preferably 3.85 or more, even more preferably 3.89 or more, and particularly preferably 3.94 or more. X From the viewpoint of electron trapping properties, it is preferable that the electron affinity is 6.0 or less. Therefore, the electron affinity is preferably 5.5 or less, more preferably 5.0 or less, even more preferably 4.7 or less, and particularly preferably 4.4 or less.

[0121] <Polymerizable Functional Group> Compound A of the present invention preferably has at least one polymerizable functional group per molecule. By having one or more polymerizable functional groups, crosslinkability is further enhanced, the hardness of the protective layer is increased, and mechanical strength can be further increased. Compound A of the present invention may have one or more polymerizable functional groups, but from the viewpoints of solubility in organic solvents and curability, it is preferable that there are two or more polymerizable functional groups, and more preferably four or more polymerizable functional groups. On the other hand, from the viewpoint of compound stability, the number of polymerizable functional groups contained in compound A of the present invention is preferably 12 or less, more preferably 10 or less, and more preferably 8 or less.

[0122] The polymerizable functional group is not particularly limited as long as it is a functional group having polymerizability, and examples thereof include polymerizable functional groups represented by the following formulae (M1) to (M7).

[0123]

[0124] In the above formulas (M1) to (M7), R 110 represents a hydrogen atom or an alkyl group which may have a substituent, and * represents the bonding position.

[0125] R in the above formulas (M1) to (M7) 110 is preferably a hydrogen atom or an alkyl group having no substituent, more preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and particularly preferably a hydrogen atom or a methyl group. When compound A of the present invention has two or more polymerizable functional groups, they do not all need to be the same and may be different, but from the viewpoint of curability, they are preferably the same.

[0126] <<Compound B of the Present Invention>> Compound B of the present invention is preferably a compound represented by the above formula (1) and satisfying the following formulas (I) and (II-2).

[0127] Since the formula (1) of the compound B of the present invention is the same as the formula (1) of the compound A of the present invention, the explanation of the formula (1) of the compound A of the present invention will be used to explain the formula (1) of the compound B of the present invention.

[0128] (Formula (I), Formula (II-2) and Formula (III)) Compound B of the present invention is preferably a compound satisfying the following formulas (I) to (III). In formula (I) and formula (II-2), M ETM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms. ETM represents the number of polymerizable functional groups contained per 1000 of molecular weight of the compound represented by formula (1).

[0129] M ETM ≧700 (I) M X / M ETM >0.31 (II-2) A ETM≧1.8 (III)

[0130] As in formula (I), the molecular weight (M ETM If the molecular weight (M) of the compound represented by the formula (1) is 700 or more, the amorphous property is improved and crystallization is easily suppressed, so that the film-forming property is improved and the film becomes uniform, resulting in good charge transport properties, which is preferable. ETM ) is more preferably 750 or more, even more preferably 800 or more, even more preferably 900 or more, and particularly preferably 1000 or more. On the other hand, from the viewpoint of solubility, the molecular weight is preferably 2000 or less. Therefore, the molecular weight is preferably 1800 or less, even more preferably 1600 or less, even more preferably 1500 or less, and particularly preferably 1400 or less.

[0131] "M" in formula (II-2) X / M ETM " That is, the ratio of the molecular weight of a compound in which all of the bonding sites of X in Formula (1) are replaced with hydrogen atoms to the molecular weight of the compound represented by Formula (1) means the ratio of structures capable of participating in electron transfer in the compound. If the ratio is greater than 0.31, the amount of structures present in the protective layer that contribute to electron transport increases, and the electron transport ability is high, resulting in better electrical properties, which is preferable. From this perspective, the ratio is more preferably 0.32 or more, more preferably 0.33 or more, even more preferably 0.34 or more, even more preferably 0.35 or more, and particularly preferably 0.36 or more. On the other hand, if the ratio is 0.60 or less, the proportion of the mother skeleton, which is a hydrophobic π-conjugated skeleton, falls within a preferred range, resulting in higher solubility in alcohol-based solvents and better coatability of the coating solution when forming the protective layer, which is preferable. From this viewpoint, the ratio is more preferably 0.58 or less, even more preferably 0.56 or less, even more preferably 0.54 or less, and particularly preferably 0.53 or less.

[0132] The molecular weight (MX ) may be any molecular weight that satisfies the above formula (II-2). X ) is more preferably 250 or more, even more preferably 300 or more, even more preferably 350 or more, and particularly preferably 400 or more. On the other hand, it is preferably 800 or less, even more preferably 750 or less, even more preferably 700 or less, and particularly preferably 650 or less.

[0133] As shown in formula (III), the number of polymerizable functional groups (A ETM If the number of polymerizable functional groups (A) is 1.8 or more, the number of polymerizable functional groups present in the protective layer is large, and a dense network structure is easily formed, resulting in good hardness and elastic deformation rate. ETM On the other hand, the number of polymerizable functional groups (A) contained per 1000 molecular weight of the compound represented by formula (1) is more preferably 1.9 or more, even more preferably 2.2 or more, still more preferably 2.5 or more, and particularly preferably 2.8 or more. ETM If the number of polymerizable functional groups (A) is too large, the electron transport property may decrease and the residual potential may deteriorate. ETM ) is preferably 7.0 or less, more preferably 6.0 or less, even more preferably 5.0 or less, and particularly preferably 4.0 or less.

[0134] (Formula (IV)) Like Compound A of the present invention, Compound B of the present invention is particularly preferably a compound which further satisfies the above formula (IV).

[0135] <Polymerizable Functional Group> Compound B of the present invention preferably has at least one polymerizable functional group per molecule. By having one or more polymerizable functional groups, crosslinkability is further enhanced, the hardness of the protective layer is increased, and mechanical strength can be further increased. Compound B of the present invention may have one or more polymerizable functional groups, but from the viewpoints of solubility in organic solvents and curability, it is preferable that there are two or more polymerizable functional groups, and more preferably four or more polymerizable functional groups. On the other hand, from the viewpoint of compound stability, the number of polymerizable functional groups contained in compound B of the present invention is preferably 12 or less, more preferably 10 or less, and more preferably 8 or less.

[0136] The polymerizable functional group that Compound B of the present invention can have is the same as the polymerizable functional group that Compound A of the present invention can have, and therefore the description of the polymerizable functional group in Compound A of the present invention will be used as the description of the polymerizable functional group in Compound B of the present invention.

[0137] <Specific Examples> Specific examples of the compounds A and B of the present invention include the following: However, the compounds A and B of the present invention are not limited to the following compounds.

[0138]

[0139]

[0140]

[0141]

[0142]

[0143]

[0144]

[0145]

[0146]

[0147]

[0148]

[0149]

[0150]

[0151]

[0152] <Method for Producing Compounds A and B of the Present Invention> Compounds A and B of the present invention can be produced, for example, according to the method described in the Examples below.

[0153] <Solubility of Compounds A and B of the Present Invention> Compounds A and B of the present invention have excellent solubility in organic solvents, particularly alcoholic solvents and mixed solvents containing alcoholic solvents, and are preferably soluble in a mixed solvent of toluene and 2-propanol (toluene 30% by mass, 2-propanol 70% by mass) at a concentration of 3% by mass or more, particularly 6% by mass or more.

[0154] <<Present Composition>> The composition of the present invention (hereinafter also referred to as "the present composition") contains the above-described present compound, and is used as a curable composition for preparing a coating liquid for forming a protective layer of the electrophotographic photoreceptor of the present invention, as described below.

[0155] The composition contains an electron transporting compound containing at least the compound of the present invention, and optionally contains a polymerizable compound not having an electron transporting skeleton, an electron donating compound, a polymerization initiator, inorganic particles, and other materials. In the present invention, the term "composition" refers to a composition consisting solely of solid components, excluding solvents. Therefore, the content of each component, such as the compound of the present invention, in 100 parts by mass of the composition described below corresponds to the content of each component in 100 parts by mass of the total protective layer formed using the composition. The total mass of the protective layer refers to the total mass of the protective layer after curing, which is the same as the total mass of the solids in the coating solution for forming the protective layer described below.

[0156] <Electron Transporting Compound> The electron transporting compound contained in the present composition includes at least the compound of the present invention, and may contain an electron transporting compound other than the compound of the present invention as necessary. The present composition may contain only one type of the compound of the present invention, or may contain two or more types of the compound of the present invention.

[0157] Examples of electron transporting compounds other than the compound of the present invention include the compounds shown below.

[0158]

[0159]

[0160] As for the electron transporting compounds other than the compound of the present invention, only one kind may be contained in the composition, or two or more kinds may be contained.

[0161] From the viewpoint of electron transporting properties, the content of the electron transporting compound in the composition is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more, relative to 100 parts by mass of the total mass of the composition. On the other hand, from the viewpoint of the hardness and elastic deformation rate of the protective layer, the content is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less. Note that when the composition contains an electron transporting compound other than the compound of the present invention, from the viewpoint of effectively obtaining the excellent solvent solubility, electrical properties, and mechanical properties due to the compound of the present invention, the content of the compound of the present invention is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 60 parts by mass or more, relative to 100 parts by mass of the total mass of the electron transporting compounds in the composition.

[0162] <Polymerizable Compound Not Having an Electron Transporting Skeleton> The present composition may contain a polymerizable compound not having an electron transporting skeleton. When the present composition contains a polymerizable compound not having an electron transporting skeleton, the present protective layer, described below, contains a polymer of a polymerizable compound not having an electron transporting skeleton. The compound of the present invention has one or more polymerizable functional groups, and therefore can also serve as a curable compound. Therefore, even if the present composition does not contain a polymerizable compound not having an electron transporting skeleton, a protective layer can be formed with good curability by the method described below. However, by using a polymerizable compound not having an electron transporting skeleton in addition to the compound of the present invention, the mechanical strength of the formed protective layer can be further improved.

[0163] The polymerizable compound without an electron transport backbone may be any compound having a chain-polymerizable functional group. Among them, a monomer, oligomer, or polymer having a radically polymerizable functional group is preferred. Among them, a curable compound having crosslinking properties, particularly a photocurable compound, is preferred. For example, a curable compound having two or more radically polymerizable functional groups can be used. A compound having one radically polymerizable functional group can also be used in combination.

[0164] The radically polymerizable functional group may be either an acryloyl group (including an acryloyloxy group) or a methacryloyl group (including a methacryloyloxy group), or both of these groups.

[0165] Examples of preferred compounds as curable compounds having a radical polymerizable functional group are listed below. Examples of monomers having an acryloyl group or a methacryloyl group include trimethylolpropane triacrylate (TMPTA), trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, glycerol triacrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexaacrylate, dimethylolpropane tetraacrylate, pentaerythritol ethoxy tetraacrylate, EO-modified phosphate triacrylate, 2,2,5,5-tetrahydroxymethylcyclopentanone tetraacrylate, 2-hydroxy-3-acryloyloxypropyl methacrylate, polyethylene glycol diacrylate, and the like. acrylate, polypropylene glycol diacrylate, polytetramethylene glycol diacrylate, EO-modified bisphenol A diacrylate, PO-modified bisphenol A diacrylate, 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene, tricyclodecane dimethanol diacrylate, decanediol diacrylate, hexanediol diacrylate, ethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, EO-modified bisphenol A dimethacrylate, PO-modified bisphenol A dimethacrylate, tricyclodecane dimethanol dimethacrylate, decanediol dimethacrylate, hexanediol dimethacrylate, and the like.

[0166] Examples of oligomers and polymers having an acryloyl group or a methacryloyl group include urethane acrylate, ester acrylate, acrylic acrylate, epoxy acrylate, etc. Among these, urethane acrylate and ester acrylate are preferred, and ester acrylate is more preferred.

[0167] The above compounds can be used alone or in combination of two or more.

[0168] A preferred example of a polymerizable compound that does not have an electron transport skeleton is a polyfunctional acrylate compound that does not have an aromatic ring such as a benzene ring, as shown in the following structure. The inclusion of such a polyfunctional acrylate compound not only enhances crosslinking, increases the hardness of the protective layer, and increases the mechanical strength, but also disperses the compound of the present invention and inhibits crystallization. Crystallization is undesirable for a photoreceptor because it generates leakage current.

[0169]

[0170] When the present composition contains such a polymerizable compound having no electron transport skeleton, the content ratio (mass ratio) of the polymerizable compound to the electron transport compound in the present composition is preferably 1.5 or less, more preferably 1.0 or less, and even more preferably 0.75 or less, from the viewpoint of electron transportability. On the other hand, from the viewpoint of the hardness and elastic deformation rate of the protective layer, this content ratio (mass ratio) is preferably 0.2 or more, more preferably 0.3 or more, and even more preferably 0.4 or more. The content ratio of the polymerizable compound having no electron transport skeleton in the present composition corresponds to the content ratio of the polymer in the present protective layer described below.

[0171] <Electron-donating compound> The present composition may further contain an electron-donating compound. When the present composition contains an electron-donating compound, the present protective layer described below contains the electron-donating compound.

[0172] In the present invention, the term "electron donor compound" refers to a compound capable of donating electrons to the protective layer. In other words, the term "electron donor compound" refers to a compound capable of reducing the energy barrier during electron transfer in a target compound (electron transport compound) in the protective layer by any mechanism, thereby injecting electrons into the target compound. The mechanism may be, for example, a mechanism in which the electron donor compound directly transfers electrons to the target compound, a mechanism in which the electron donor compound transfers electrons by forming a hydrogen bond with the target compound, or a mechanism in which the electron donor compound forms a hydrogen bond with the target compound to reduce the energy barrier during electron transfer, thereby injecting electrons transferred from the photosensitive layer into the target compound present in the protective layer.

[0173] Currently known electron donating compounds include compounds having structures such as triphenylmethane, acridine, amine, amidine, aniline, pyridine, xanthene, benzimidazole, guanidine, and phosphazene. Compounds that will be recognized to have such effects in the future are also included.

[0174] As described above, examples of the electron donating compound include compounds having a structure such as triphenylmethane, acridine, amine, amidine, aniline, pyridine, xanthene, benzimidazole, guanidine, and phosphazene. Among them, compounds having a benzimidazole structure or a guanidine structure are preferred from the viewpoint of stability. As the guanidine structure, either a chain guanidine structure or a cyclic guanidine structure can be used, but from the viewpoint of stability, a cyclic guanidine structure is preferred.

[0175] The electron donor compound is preferably a compound having one or more heteroatoms in the molecule, and more preferably a compound having one or more nitrogen atoms (N atoms) in the molecule. From the viewpoint of stability, the number of heteroatoms in one molecule of the electron donor compound is preferably one or more, more preferably two or more, and even more preferably three or more. From the viewpoint of electron donating ability, the number of nitrogen atoms (N atoms) in one molecule of the electron donor compound is preferably one or more, more preferably two or more, and even more preferably three or more. From the viewpoint of stability, the electron donor compound is preferably a compound having one or more cyclic structures.

[0176] The electron donor compound is preferably an electron donor compound represented by the following formula (4) or (5). These electron donor compounds are activated, for example, when heated to room temperature or higher, and are able to donate electrons to the protective layer. Specifically, the electron donor compound represented by the following formula (4) is activated when heated to about 80°C or higher, and is able to donate electrons to the protective layer. The electron donor compound represented by the following formula (5) is activated when heated to room temperature or higher, and is able to donate electrons to the protective layer. Therefore, for example, when forming the protective layer, these compounds are activated by the temperature increase associated with ultraviolet irradiation, and are able to donate electrons to the protective layer.

[0177]

[0178] In formula (4), E 1 ~E 4 are each independently preferably a hydrogen atom, a halogen atom, an optionally substituted alkyl group, an optionally substituted thioalkyl group, an optionally substituted thioaryl group, an optionally substituted arylsulfonyl group, an optionally substituted amino group, an optionally substituted alkylamino group, an optionally substituted arylamino group, an optionally substituted hydroxy group, an optionally substituted alkoxy group, an optionally substituted acylamino group, an optionally substituted acyloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted carboxy group, an optionally substituted carboxamido group, an optionally substituted carboalkoxy group, an optionally substituted acyl group, an optionally substituted sulfonyl group, an optionally substituted cyano group, an optionally substituted nitro group, or a derivative of any of these groups. 1 ~E 4 may be bonded to each other to form a ring.

[0179] In the above formula (4), h is an integer of 0 or more, and from the viewpoint of stability, it is preferably 2 or less, more preferably 1 or less, and even more preferably 0.

[0180] In the above formula (5), g1 is an integer of 1 or more, and from the viewpoint of electrical properties, it is preferably 4 or less, more preferably 3 or less, and even more preferably 2 or less.

[0181] In the above formula (5), Ar is preferably represented by the following formula (6).

[0182]

[0183] In formula (6), * represents G in formula (5). 21 It represents a bond with 22 is preferably an alkyl group which may have a substituent, an alkoxy group which may have a substituent, or a halogen atom.

[0184] In formula (6), g2 is an integer of 0 or more, and from the viewpoint of stability, it is preferably 2 or less, more preferably 1 or less, and most preferably 0.

[0185] G in formula (5) 21 is preferably a hydrocarbon group which may have a substituent. The number of carbon atoms in the hydrocarbon group is preferably 1 or more, more preferably 3 or more, and is preferably 12 or less, more preferably 10 or less. When g1 is 1, the hydrocarbon group is preferably an alkyl group, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a hexyl group, an octyl group, or a decyl group. When g1 is 2, the hydrocarbon group is preferably an alkylene group, such as a methylene group or an ethylene group.

[0186] From the viewpoint of electrical properties, the content of the electron donor compound in the composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 part by mass or more, per 100 parts by mass of the total composition, while from the viewpoint of electrical properties, the content is preferably 25 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 5.0 parts by mass or less, per 100 parts by mass of the total composition.

[0187] Specific examples of the electron donating compound are shown below, but the present invention is not limited to these.

[0188]

[0189] The composition may contain only one of these electron donating compounds, or may contain two or more of them.

[0190] <Polymerization initiator> Examples of the polymerization initiator include a thermal polymerization initiator, a photopolymerization initiator, etc. Examples of the thermal polymerization initiator include a peroxide compound such as 2,5-dimethylhexane-2,5-dihydroperoxide, and an azo compound such as 2,2′-azobis(isobutyronitrile).

[0191] Photopolymerization initiators can be classified into direct cleavage type and hydrogen abstraction type based on the radical generation mechanism. Direct cleavage type photopolymerization initiators generate radicals by cleaving some of the covalent bonds within the molecule when they absorb light energy. On the other hand, hydrogen abstraction type photopolymerization initiators generate radicals when the molecule becomes excited by absorbing light energy and abstracts hydrogen from the hydrogen donor.

[0192] Examples of the direct cleavage type photopolymerization initiator include acetophenone or ketal compounds such as acetophenone, 2-benzoyl-2-propanol, 1-benzoylcyclohexanol, 2,2-diethoxyacetophenone, benzyl dimethyl ketal, and 2-methyl-4'-(methylthio)-2-morpholinopropiophenone; benzoin ether compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isobutyl ether, benzoin isopropyl ether, and O-tosylbenzoin; and acylphosphine oxide compounds such as diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and lithium phenyl(2,4,6-trimethylbenzoyl)phosphonate.

[0193] Examples of hydrogen abstraction photopolymerization initiators include benzophenone-based compounds such as benzophenone, 4-benzoylbenzoic acid, 2-benzoylbenzoic acid, methyl 2-benzoylbenzoate, methyl benzoylformate, benzyl, p-anisil, 2-benzoylnaphthalene, 4,4'-bis(dimethylamino)benzophenone, 4,4'-dichlorobenzophenone, and 1,4-dibenzoylbenzene, and anthraquinone- or thioxanthone-based compounds such as 2-ethylanthraquinone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone. Examples of other photopolymerization initiators include camphorquinone, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, acridine-based compounds, triazine-based compounds, and imidazole-based compounds.

[0194] In order to efficiently absorb light energy and generate radicals, the photopolymerization initiator preferably has an absorption wavelength in the wavelength region of the light source used for light irradiation. Among these, it is preferable to contain an acylphosphine oxide compound, which has an absorption wavelength on the relatively long wavelength side. Furthermore, from the viewpoint of supplementing curability, it is even more preferable to use an acylphosphine oxide compound and a hydrogen abstraction initiator in combination. In this case, the content ratio of the hydrogen abstraction initiator to the acylphosphine oxide compound is not particularly limited. From the viewpoint of supplementing surface curability, it is preferably 0.1 parts by mass or more per part by mass of the acylphosphine oxide compound, and from the viewpoint of maintaining internal curability, it is preferably 5 parts by mass or less.

[0195] Furthermore, a compound having a photopolymerization promoting effect can be used alone or in combination with the above photopolymerization initiator. Examples of compounds having a photopolymerization promoting effect include triethanolamine, methyldiethanolamine, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, (2-dimethylamino)ethyl benzoate, and 4,4'-dimethylaminobenzophenone.

[0196] The polymerization initiator may be used alone or in combination of two or more. The content of the polymerization initiator is 0.5 to 40 parts by mass, preferably 1 to 20 parts by mass, per 100 parts by mass of the total radically polymerizable ingredients. The total radically polymerizable ingredients include the compound of the present invention and the polymerizable compound not having an electron transport skeleton.

[0197] <Inorganic Particles> The composition of the present invention may contain inorganic particles from the viewpoint of improving the strong exposure characteristics and mechanical strength of the protective layer to be formed, or from the viewpoint of imparting charge transport ability. However, inorganic particles are not an essential component of the composition of the present invention. In the present invention, by using the compound of the present invention, a protective layer having excellent mechanical strength can be formed without the need for inorganic particles.

[0198] Examples of the inorganic particles include metal powder, metal oxide, metal fluoride, potassium titanate, boron nitride, etc. Generally, any inorganic particles that can be used for electrophotographic photoreceptors can be used. Only one type of inorganic particles may be used, or multiple types of particles may be mixed and used.

[0199] <Other Materials> The present composition may contain other materials in addition to those described above, as necessary. Examples of other materials include stabilizers (heat stabilizers, UV absorbers, light stabilizers, antioxidants, etc.), dispersants, antistatic agents, colorants, lubricants, etc. These may be used alone or in any combination and ratio.

[0200] <Method of Forming the Present Protective Layer> The present protective layer is preferably formed from the present composition described above. The method of forming the present protective layer using the present composition will be described below.

[0201] (Coating liquid for forming protective layer) The protective layer can be formed by applying the above-mentioned composition, i.e., a curable composition containing an electron transporting compound including the compound of the present invention, and optionally containing a polymerizable compound not having an electron transporting skeleton, an electron donating compound, a polymerization initiator, inorganic particles, and other materials, to the photosensitive layer, and curing the coating liquid obtained by dissolving the composition in a solvent or dispersing the composition in a dispersion medium (hereinafter also referred to as the "coating liquid for forming the protective layer").

[0202] The content of the electron transport compound including the compound of the present invention in the coating liquid for forming a protective layer is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the solvent, from the viewpoints of film uniformity and solubility of the protective layer. The content of the curable compound in the coating liquid for forming a protective layer, i.e., the total content of the compound of the present invention and the polymerizable compound not having an electron transport skeleton, is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the solvent, from the viewpoint of residual potential. On the other hand, from the viewpoints of hardness and elastic deformation rate of the protective layer, it is preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, and even more preferably 1.5 parts by mass or more.

[0203] The content of other components in the present protective layer-forming coating liquid, i.e., components other than the electron transporting compound and curable compound contained in the present composition, is the same as the content of each component in the present composition described above.

[0204] The solvent used in the protective layer-forming coating liquid may be, for example, an organic solvent. Examples of the organic solvent include alcohols such as methanol, ethanol, propanol, and 2-methoxyethanol; ethers such as tetrahydrofuran, 1,4-dioxane, and dimethoxyethane; esters such as methyl formate and ethyl acetate; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; aromatic hydrocarbons such as benzene, toluene, xylene, and anisole; chlorinated hydrocarbons such as dichloromethane, chloroform, 1,2-dichloroethane, 1,1,2-trichloroethane, 1,1,1-trichloroethane, tetrachloroethane, 1,2-dichloropropane, and trichloroethylene; nitrogen-containing compounds such as n-butylamine, isopropanolamine, diethylamine, triethanolamine, ethylenediamine, and triethylenediamine; and aprotic polar solvents such as acetonitrile, N-methylpyrrolidone, N,N-dimethylformamide, and dimethyl sulfoxide. Mixed solvents of these solvents may also be used in any combination and in any ratio. Among these, from the viewpoints of solubility and coatability, alcohols, ethers, aromatic hydrocarbons, and aprotic polar solvents are preferred, alcohols, ethers, and aromatic hydrocarbons are more preferred, alcohols and ethers are even more preferred, and alcohols are most preferred.

[0205] Furthermore, even if an organic solvent does not dissolve the electron transport compound used in the protective layer of the photoreceptor of the present invention by itself, it can be used if it can dissolve the compound by, for example, mixing it with the above-mentioned organic solvent. Generally, using a mixed solvent can reduce coating unevenness. When using a dip coating method as the coating method described below, it is preferable to select a solvent that does not dissolve the lower layer. From this viewpoint, it is particularly preferable to add an alcohol.

[0206] The ratio of the amount of the solvent to the amount of solids used in the coating solution for forming the protective layer varies depending on the coating method for the coating solution for forming the protective layer, and may be appropriately changed so as to form a uniform coating film in the coating method to be used.

[0207] (Coating Method of the Protective Layer-Forming Coating Liquid) The coating method of the protective layer-forming coating liquid for forming the protective layer is not particularly limited, and examples thereof include spray coating, spiral coating, ring coating, and dip coating.

[0208] After forming the coating film by the above coating method, the coating film is dried. In this case, the drying temperature and time are not important as long as necessary and sufficient drying is obtained. However, if the protective layer is coated by only air drying after coating the photosensitive layer, it is preferable to carry out sufficient drying by the method described below in the method for forming the photosensitive layer.

[0209] (Method for Curing the Protective Layer) The protective layer can be formed by applying the protective layer-forming coating liquid and then curing it by applying external energy. Examples of the external energy used in this process include heat, light, and radiation.

[0210] Examples of methods for applying heat energy include heating methods using gases such as air and nitrogen, steam, various heat media, infrared rays, and electromagnetic waves. Heating can be carried out from the coated surface side or the support side. The heating temperature is preferably 100°C or higher and 170°C or lower.

[0211] As the light energy, UV irradiation light sources that emit light mainly in the ultraviolet (UV) range, such as high-pressure mercury lamps, metal halide lamps, electrodeless lamp bulbs, light-emitting diodes, etc. It is also possible to select a visible light source in accordance with the absorption wavelength of the polymerizable compound and photopolymerization initiator.

[0212] From the viewpoint of curing, the light irradiation amount is 10 J / cm 2 More than 15 J / cm is preferable. 2 More preferably, 20 J / cm or more 2 More preferably, the electric field strength is 400 J / cm or more. 2 Preferably, 200 J / cm or less 2 More preferably, 150 J / cm or less 2 The following are more preferred: On the other hand, examples of radiation energy include those using electron beams (EB).

[0213] Among these energies, light energy is preferred from the viewpoints of ease of reaction rate control, simplicity of the device, and long pod life.

[0214] After the protective layer is cured, a heating step may be performed from the viewpoints of relieving residual stress, relieving residual radicals, and improving electrical properties. The heating temperature is preferably 60° C. or higher, more preferably 100° C. or higher, and is preferably 200° C. or lower, more preferably 150° C. or lower.

[0215] (Layer Thickness) From the viewpoint of abrasion resistance, the thickness of the protective layer is preferably 0.5 μm or more, more preferably 1 μm or more. On the other hand, from the viewpoint of electrical properties, it is preferably 5 μm or less, more preferably 4 μm or less. From the same viewpoint, the thickness of the protective layer is preferably 1 / 50 or more of the thickness of the photosensitive layer, more preferably 1 / 40 or more, and even more preferably 1 / 30 or more. On the other hand, it is preferably 1 / 5 or less, more preferably 1 / 10 or less, and even more preferably 1 / 20 or less.

[0216] <Present Photosensitive Layer> The photosensitive layer in the photoreceptor of the present invention (hereinafter also referred to as "present photosensitive layer") may be a layer containing at least a charge generating material (CGM) and a charge transport material.

[0217] The photosensitive layer may be a single-layer type photosensitive layer containing both a charge generating material and a charge transporting material in the same layer, or may be a multi-layer type photosensitive layer separated into a charge generating layer and a charge transporting layer.

[0218] <Single-Layer Photosensitive Layer> When the photosensitive layer is a single-layer photosensitive layer, it is preferable that at least a charge generating material (CGM), a hole transporting material (HTM), an electron transporting material (ETM), and a binder resin are contained in the same layer.

[0219] (Charge-Generating Material) As the charge-generating material (CGM) used in the present photosensitive layer, for example, various photoconductive materials such as inorganic photoconductive materials and organic pigments can be used. Among them, organic pigments are particularly preferred, and phthalocyanine pigments and azo pigments are more preferred.

[0220] In particular, when a phthalocyanine pigment is used as the charge generating material, specific examples include metal-free phthalocyanine, phthalocyanines coordinated with metals such as copper, indium, gallium, tin, titanium, zinc, vanadium, silicon, and germanium, or oxides, halides, etc. Among these, particularly highly sensitive X-type and τ-type metal-free phthalocyanine, A-type, B-type, D-type titanyl phthalocyanine, vanadyl phthalocyanine, chloroindium phthalocyanine, chlorogallium phthalocyanine, and hydroxygallium phthalocyanine are preferred.

[0221] When an azo pigment is used, various known bisazo pigments and trisazo pigments are preferably used.

[0222] The charge generation material may be used singly or in any combination and ratio of two or more. When two or more charge generation materials are used in combination, the charge generation materials may be mixed after the respective charge generation materials are mixed, or may be mixed during the production or processing steps of the charge generation materials, such as synthesis, pigmentation, or crystallization.

[0223] From the viewpoint of electrical properties, it is desirable that the particle diameter of the charge generating substance is small. Specifically, the particle diameter of the charge generating substance is preferably 1 μm or less, more preferably 0.5 μm or less, with the lower limit being 0.01 μm or more. Here, the particle diameter of the charge generating substance means the particle diameter in a state in which it is contained in the photosensitive layer.

[0224] Furthermore, the amount of the charge generating substance in the single-layer photosensitive layer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, from the viewpoint of sensitivity, and is preferably 50% by mass or less, more preferably 20% by mass or less, from the viewpoint of sensitivity and chargeability.

[0225] (Charge transport material) Charge transport materials are classified into hole transport materials having mainly hole transport ability and electron transport materials having mainly electron transport ability. However, when the present photosensitive layer is a single-layer type photosensitive layer, it is preferable that at least a hole transport material and an electron transport material are contained in the same layer.

[0226] (Hole Transporting Material) The hole transporting material (HTM) can be selected from known materials and used. Examples thereof include electron donating materials such as heterocyclic compounds such as carbazole derivatives, indole derivatives, imidazole derivatives, oxazole derivatives, pyrazole derivatives, thiadiazole derivatives, and benzofuran derivatives, aniline derivatives, hydrazone derivatives, arylamine derivatives, stilbene derivatives, butadiene derivatives, and enamine derivatives, as well as compounds in which a plurality of these compounds are bonded, and polymers having a group consisting of these compounds in the main chain or side chain.

[0227] Among these, carbazole derivatives, arylamine derivatives, stilbene derivatives, butadiene derivatives, enamine derivatives, and compounds in which a plurality of these compounds are combined are preferred, and arylamine derivatives and enamine derivatives are more preferred.

[0228] The hole transporting substance may be used alone or in any combination of two or more kinds in any ratio.

[0229] The amount of the hole transport substance in the single-layer photosensitive layer is preferably 20% by mass or more, more preferably 30% by mass or more, based on 100% by mass of the entire photosensitive layer, from the viewpoint of hole transportability, and is preferably 55% by mass or less, more preferably 45% by mass or less, from the viewpoint of solubility.

[0230] (Electron Transporting Material) The electron transporting material (ETM) can be selected from known materials. Examples include electron-withdrawing substances such as aromatic nitro compounds such as 2,4,7-trinitrofluorenone, cyano compounds such as tetracyanoquinodimethane, and quinone compounds such as diphenoquinone, as well as known cyclic ketone compounds and perylene pigments (perylene derivatives). Among these, from the viewpoint of electrical properties, quinone compounds and perylene pigments (perylene derivatives) are preferred, and quinone compounds are more preferred. Among the quinone compounds, from the viewpoint of electrical properties, diphenoquinone or dinaphthylquinone is preferred. Of these, dinaphthylquinone is more preferred.

[0231] The electron transport material may be used alone or in any combination of two or more kinds in any ratio.

[0232] Preferred examples of the structure of the electron transport material are shown below.

[0233]

[0234] Among the above electron transport materials, ET-2 and ET-5 are preferred, with ET-2 being more preferred, in terms of electrical properties.

[0235] The amount of the electron transport material in the single-layer photosensitive layer is preferably 15% by mass or more, more preferably 25% by mass or more, based on 100% by mass of the entire photosensitive layer, from the viewpoint of electron transportability, and is preferably 40% by mass or less, more preferably 30% by mass or less, from the viewpoint of solubility.

[0236] (Binder Resin) Examples of binder resins used in the present photosensitive layer include vinyl polymers or copolymers thereof such as polymethyl methacrylate, polystyrene, and polyvinyl chloride; vinyl alcohol resins; polyvinyl butyral resins; polyvinyl formal resins; partially modified polyvinyl acetal resins; polyarylate resins; polyamide resins; polyurethane resins; polycarbonate resins; polyester resins; polyester carbonate resins; polyimide resins; phenoxy resins; epoxy resins; silicone resins; and partially crosslinked cured products thereof. The above resins may also be modified with a silicon reagent or the like. These may also be used alone or in any ratio and combination of two or more.

[0237] The binder resin used in the present photosensitive layer preferably contains one or more polymers obtained by interfacial polymerization.

[0238] The binder resin obtained by the interfacial polymerization is preferably a polycarbonate resin or a polyester resin, more preferably a polycarbonate resin or a polyarylate resin, and particularly preferably a polymer made from an aromatic diol.

[0239] (Other Substances) In addition to the materials described above, the photosensitive layer may contain additives such as well-known antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, and visible light shielding agents in order to improve film-forming properties, flexibility, coating properties, contamination resistance, gas resistance, light resistance, and the like. The photosensitive layer may also contain various additives, such as sensitizers, dyes, pigments (excluding the charge-generating materials, hole-transporting materials, and electron-transporting materials described above), and surfactants, as needed. Examples of surfactants include silicone oils and fluorine-based compounds. In the present invention, these may be used alone or in any combination of two or more types in any ratio.

[0240] Furthermore, for the purpose of reducing frictional resistance on the surface of the photosensitive layer, the photosensitive layer may contain a fluorine-based resin, a silicone resin, or the like, or may contain particles made of these resins or particles of an inorganic compound such as aluminum oxide.

[0241] (Layer Thickness) When the present photosensitive layer is a single-layer type photosensitive layer, the thickness of the present photosensitive layer is preferably 20 μm or more, more preferably 25 μm or more, from the viewpoint of dielectric breakdown resistance, and is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of electrical properties.

[0242] <Laminated Photosensitive Layer> When the photoreceptor of the present invention has a laminated photosensitive layer, for example, it may have a structure in which a charge transport layer (CTL) containing a charge transport material is laminated on a charge generation layer (CGL) containing a charge generation material (CGM). In this case, it is also possible to provide layers other than the charge generation layer (CGL) and the charge transport layer (CTL).

[0243] (Charge Generation Layer (CGL)) The charge generation layer (CGL) usually contains a charge generation material (CGM) and a binder resin. The charge generation material (CGM) and the binder resin are the same as those described in the single-layer type photosensitive layer above.

[0244] In addition to the charge generating material and the binder resin, the charge generating layer may contain other components as needed, such as known additives such as antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, visible light shielding agents, and fillers, for the purpose of improving film-forming properties, flexibility, coatability, stain resistance, gas resistance, light resistance, etc.

[0245] In the charge generation layer, if the ratio of the charge generation material is too high, the stability of the coating liquid may be reduced due to aggregation of the charge generation material, while if the ratio of the charge generation material is too low, the sensitivity of the photoreceptor may be reduced, so the compounding ratio (mass) of the charge generation material is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, relative to 100 parts by mass of the binder resin. On the other hand, the compounding ratio (mass) of the charge generation material is preferably 1000 parts by mass or less, more preferably 500 parts by mass or less, relative to 100 parts by mass of the binder resin, and from the viewpoint of film strength, a ratio of 300 parts by mass or less is even more preferable, and a ratio of 200 parts by mass or less is particularly preferable.

[0246] The thickness of the charge generating layer is preferably 0.1 μm or more, more preferably 0.15 μm or more, and is preferably 10 μm or less, more preferably 0.6 μm or less.

[0247] (Charge Transport Layer (CTL)) The charge transport layer (CTL) usually contains a charge transport material and a binder resin. The charge transport material and the binder resin are the same as those described in the single-layer type photosensitive layer above.

[0248] In the charge transport layer (CTL), the blending ratio of the hole transport material (HTM) to the binder resin is preferably 20 parts by mass or more per 100 parts by mass of the binder resin, more preferably 30 parts by mass or more from the viewpoint of reducing residual potential, and even more preferably 40 parts by mass or more from the viewpoints of stability and charge mobility during repeated use. On the other hand, from the viewpoint of thermal stability of the photosensitive layer, the blending ratio of the hole transport material (HTM) to 100 parts by mass of the binder resin is preferably 200 parts by mass or less, and from the viewpoint of compatibility between the hole transport material (HTM) and the binder resin, more preferably 150 parts by mass or less, and particularly preferably 120 parts by mass or less from the viewpoint of glass transition temperature.

[0249] In the charge transport layer (CTL), the blending ratio of the electron transport material (ETM) to the binder resin is preferably 20 parts by mass or more per 100 parts by mass of the binder resin, more preferably 30 parts by mass or more from the viewpoint of reducing residual potential, and even more preferably 40 parts by mass or more from the viewpoints of stability and charge mobility during repeated use. On the other hand, from the viewpoint of thermal stability of the photosensitive layer, the blending ratio of the electron transport material (ETM) to 100 parts by mass of the binder resin is preferably 200 parts by mass or less, and from the viewpoint of compatibility between the electron transport material (ETM) and the binder resin, more preferably 150 parts by mass or less, and particularly preferably 120 parts by mass or less from the viewpoint of glass transition temperature.

[0250] The charge transport layer may contain other components as needed in addition to the electron transport material (ETM), hole transport material (HTM), and binder resin. For example, known additives such as antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, visible light shielding agents, and fillers may be added to improve film-forming properties, flexibility, coating properties, contamination resistance, gas resistance, light resistance, etc.

[0251] The thickness of the charge transport layer is not particularly limited, but from the viewpoints of electrical properties, image stability, and high resolution, it is preferably from 5 μm to 50 μm, more preferably from 10 μm to 40 μm, and even more preferably from 15 μm to 35 μm.

[0252] <Method of Forming the Present Photosensitive Layer> In both the multilayer type and the single-layer type, the above-mentioned layers can be formed as follows. A coating liquid obtained by dissolving or dispersing a substance to be contained in a solvent can be applied to a conductive support by a known method such as dip coating, spray coating, nozzle coating, bar coating, roll coating, or blade coating, and the layers can be formed by repeating the steps of coating and drying sequentially for each layer. However, the formation method is not limited to this.

[0253] The solvent or dispersion medium used to prepare the coating liquid is not particularly limited. Specific examples include alcohols, ethers, aromatic hydrocarbons, chlorinated hydrocarbons, etc. These may be used alone or in any combination of two or more of them.

[0254] The amount of solvent or dispersion medium used is not particularly limited. It is preferable to appropriately adjust the solids concentration, viscosity, and other physical properties of the coating solution so that they fall within the desired range, taking into account the purpose of each layer and the properties of the selected solvent or dispersion medium. The coating film is preferably dried by heating, usually at a temperature of 30°C or higher and 200°C or lower, for 1 minute to 2 hours, either stationary or under airflow. The heating temperature may be constant, or the temperature may be varied during drying.

[0255] <Conductive Support> The conductive support of the photoreceptor of the present invention (hereinafter also referred to as the "conductive support") is not particularly limited as long as it supports the layers formed thereon and exhibits conductivity. Examples of the conductive support include metal materials such as aluminum, aluminum alloys, stainless steel, copper, and nickel, resin materials imparted with conductivity by the coexistence of metals, carbon, and conductive powders such as tin oxide, and resins, glass, and paper on whose surfaces conductive materials such as aluminum, nickel, and ITO (indium oxide tin oxide alloy) are vapor-deposited or coated. The conductive support may be in the form of a drum, cylinder, sheet, belt, or the like. The conductive support may also be a metal conductive support coated with a conductive material having an appropriate resistance value for controlling conductivity, surface properties, and the like or for covering defects.

[0256] When a metal material such as an aluminum alloy is used as the conductive support, the metal material may be anodized before use. The average thickness of the anodized film is preferably 20 μm or less, and more preferably 7 μm or less. When an anodized film is applied to the metal material, it is preferable to perform a sealing treatment. The sealing treatment can be performed by a known method.

[0257] The surface of the conductive support may be smooth, or may be roughened by using a special cutting method or by polishing, or by mixing particles of an appropriate particle size into the material constituting the support.

[0258] <Present Undercoat Layer> The photoreceptor of the present invention may have an undercoat layer (also referred to as "present undercoat layer") between the present conductive support and the present photosensitive layer in order to improve adhesion, blocking properties, etc.

[0259] The undercoat layer may be made of, for example, a resin, a resin in which organic pigments or particles of metal oxides are dispersed, etc. The undercoat layer may also contain a known antioxidant, etc.

[0260] Examples of organic pigments used in the undercoat layer include phthalocyanine pigments, azo pigments, perylene pigments, etc. Among them, phthalocyanine pigments and azo pigments, specifically, the phthalocyanine pigments and azo pigments used as the charge generating material described above, can be mentioned.

[0261] Examples of metal oxide particles used in the present undercoat layer include metal oxide particles containing one type of metal element such as titanium oxide, aluminum oxide, silicon oxide, zirconium oxide, zinc oxide, and iron oxide, and metal oxide particles containing multiple metal elements such as calcium titanate, strontium titanate, and barium titanate. The undercoat layer may contain only one type of particle, or multiple types of particles may be mixed in any ratio and combination.

[0262] Among the above metal oxide particles, titanium oxide and aluminum oxide are preferred, with titanium oxide being particularly preferred.

[0263] The particle size of the metal oxide particles used in the present undercoat layer is not particularly limited. From the viewpoint of the properties of the undercoat layer and the stability of the dispersion liquid for forming the undercoat layer, the average primary particle size is preferably 10 nm or more, and is preferably 100 nm or less, more preferably 50 nm or less.

[0264] The binder resin used in the undercoat layer can be selected from, for example, polyvinyl acetal resins such as polyvinyl butyral resins; and insulating resins such as polyarylate resins, polycarbonate resins, polyester resins, phenoxy resins, acrylic resins, methacrylic resins, polyamide resins, polyurethane resins, epoxy resins, silicone resins, polyvinyl alcohol resins, and styrene-alkyd resins. However, the binder resin is not limited to these polymers. These binder resins may be used alone or in combination with two or more types, or may be used in a cured form with a curing agent. Among these, polyvinyl acetal resins, alcohol-soluble copolymer polyamides, modified polyamides, and the like are preferred because of their good dispersibility and coatability. Of these, alcohol-soluble copolymer polyamides are particularly preferred.

[0265] The mixing ratio of the particles to the binder resin can be selected arbitrarily, but it is preferable to use the particles in the range of 10% by mass to 500% by mass in terms of the stability and coatability of the dispersion.

[0266] The thickness of the undercoat layer can be selected arbitrarily, but is preferably 0.1 μm or more, more preferably 20 μm or less, in view of the characteristics of the electrophotographic photoreceptor and the coatability of the dispersion.

[0267] <Other Layers> The photoreceptor of the present invention may have other layers as needed in addition to the conductive substrate, photosensitive layer, protective layer and undercoat layer described above.

[0268] <Physical Properties of the Photoreceptor of the Present Invention> The photoreceptor of the present invention may have the following physical properties.

[0269] (Martens Hardness) In order to provide the photoreceptor of the present invention with sufficient wear resistance for practical use, the Martens hardness is set to 175 N / mm 2 More preferably, it is 200 N / mm 2 Above all, 220N / mm 2 In the present invention, the Martens hardness of the photoreceptor means the Martens hardness measured from the surface side of the photoreceptor. The Martens hardness can be measured by the method described in the examples below.

[0270] (Elastic Deformation Rate) From the viewpoint of providing the photoreceptor of the present invention with sufficient wear resistance for practical use, the elastic deformation rate varies depending on the composition of the protective layer, but is preferably 25% or more, more preferably 30% or more, and even more preferably 40% or more. In the present invention, the elastic deformation rate of the photoreceptor means the elastic deformation rate measured from the surface side of the photoreceptor. The elastic deformation rate can be measured by the method described in the Examples below.

[0271] (Residual Potential) In order to provide the photoreceptor of the present invention with a practically sufficient residual potential, the residual potential varies depending on the component composition of the protective layer, but is preferably 250 V or less, more preferably 200 V or less, even more preferably 150 V or less, and even more preferably 100 V or less. In the present invention, the residual potential of the photoreceptor means the potential after the photoreceptor has been charged and irradiated with exposure light. The residual potential can be measured by the method described in the Examples below.

[0272] <<Image Forming Apparatus of the Present Invention>> An image forming apparatus (hereinafter also referred to as "image forming apparatus of the present invention") can be configured using the photoreceptor of the present invention. However, the image forming apparatus of the present invention described below is one example of an image forming apparatus that can be configured using the electrophotographic photoreceptor of the present invention.

[0273] As shown in FIG. 1, the image forming apparatus of the present invention is configured to include a photoreceptor 1 of the present invention, a charging device 2, an exposure device 3, and a developing device 4, and may further include a transfer device 5, a cleaning device 6, and a fixing device 7 as required.

[0274] There are no particular limitations on the present invention photoreceptor 1 as long as it is the above-described present invention photoreceptor. Figure 1 shows an example of a drum-shaped photoreceptor in which the above-described photosensitive layer is formed on the surface of a cylindrical conductive support. A charging device 2, an exposure device 3, a developing device 4, a transfer device 5, and a cleaning device 6 are arranged along the outer periphery of this present invention photoreceptor 1.

[0275] Examples of the charging device 2 include a non-contact corona charging device such as a corotron or scorotron, or a contact-type charging device (direct-type charging device) that charges the photosensitive member by bringing a charging member to which a voltage is applied into contact with the surface of the photosensitive member. Examples of contact charging devices include a charging roller and a charging brush. Note that FIG. 1 shows a roller-type charging device (charging roller) as an example of the charging device 2.

[0276] The type of exposure device 3 is not particularly limited as long as it can expose the photoreceptor 1 of the present invention to light and form an electrostatic latent image on the photosensitive surface of the photoreceptor 1 of the present invention. Also, exposure may be performed by an internal photoreceptor exposure method. Any light may be used for exposure.

[0277] The type of toner T is arbitrary, and in addition to powder toner, polymerized toner produced by a suspension polymerization method or an emulsion polymerization method can be used.

[0278] The developing device 4 may have any configuration. The developing device 4 shown in Fig. 1 has a configuration in which the toner T is formed into a thin layer by a regulating member (developing blade) 45, frictionally charged to a predetermined polarity, and carried and transported by a developing roller 44 to contact the surface of the photoreceptor 1. However, this configuration is not limited to this. The transfer device 5 is not particularly limited in type, and any device using an electrostatic transfer method such as corona transfer, roller transfer, or belt transfer, a pressure transfer method, or an adhesive transfer method may be used.

[0279] There are no particular limitations on the cleaning device 6. Any cleaning device can be used, such as a brush cleaner, a magnetic roller cleaner, or a blade cleaner. If there is little or almost no toner remaining on the photoreceptor surface, the cleaning device 6 may be omitted. The fixing device 7 may also have any configuration. In addition to the configuration described above, the image forming apparatus may also be configured to be capable of performing, for example, a static elimination process.

[0280] Furthermore, the image forming apparatus may be further modified and configured, for example, to be capable of performing processes such as a pre-exposure process and an auxiliary charging process, or to be configured to perform offset printing, or even to be configured as a full-color tandem system using multiple types of toner.

[0281] <<Cartridge of the Present Invention>> The photoreceptor 1 of the present invention can be combined with one or more of a charging device 2, an exposure device 3, a developing device 4, a transfer device 5, a cleaning device 6, and a fixing device 7 to form an integrated cartridge (referred to as the "cartridge of the present invention"). However, the cartridge of the present invention described below is one example of an electrophotographic cartridge that can be constructed using the electrophotographic photoreceptor of the present invention.

[0282] The cartridge of the present invention can be configured to be detachable from the main body of an electrophotographic apparatus such as a copying machine, a laser beam printer, etc. In this case, for example, when the photoreceptor 1 of the present invention or other members deteriorate, the electrophotographic photoreceptor cartridge can be removed from the main body of the image forming apparatus and a new electrophotographic photoreceptor cartridge can be mounted in the main body of the image forming apparatus, thereby facilitating maintenance and management of the image forming apparatus.

[0283] <<Explanation of Terms>> In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it means "X or more and Y or less," and also includes the meaning of "preferably greater than X" or "preferably smaller than Y." Furthermore, when written as "X or more" or "X≦" (X is any number), it also includes the meaning of "preferably greater than X" unless otherwise specified, and when written as "Y or less" or "≦Y" (Y is any number), it also includes the meaning of "preferably smaller than Y" unless otherwise specified.

[0284] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples. However, the following examples are provided to explain the present invention in detail, and the present invention is not limited to the examples shown below, and can be practiced by modifying it as desired, as long as it does not deviate from the gist of the present invention. Furthermore, in the following examples and comparative examples, "parts" refers to "parts by mass" unless otherwise specified.

[0285] As used herein, DMF means N,N-dimethylformamide, NMP means N-methyl-2-pyrrolidone, Et means ethyl group, Ac means acetyl group, and MEHQ means 4-methoxyphenol.

[0286] [Synthesis of Compounds] The synthesis methods of the following compounds 1 to 12 will be described.

[0287] <Synthesis of Compound 1> The synthesis scheme of Compound 1 is shown below.

[0288]

[0289] The synthesis procedure for Compound 1 is shown below.

[0290] (Synthesis of Intermediate 1-1) Under a nitrogen atmosphere, 100 mL of 1,4-dioxane was added to a mixture of succinic anhydride (11.0 g, 109.5 mmol) and 4-DMAP (4-dimethylaminopyridine, 0.26 g, 2.19 mmol) to prepare a solution. To this solution, a solution of glycerol dimethacrylate (25 g, 109.5 mmol) and MEHQ (27 mg, 0.22 mmol) dissolved in 50 mL of 1,4-dioxane was added dropwise, and the mixture was stirred at 80°C for 9 hours. After cooling to room temperature, the mixture was poured into 200 mL of water and extracted with dichloromethane. The organic layer was washed with water and then dried over magnesium sulfate. The solid was filtered, and the solvent from the filtrate was distilled off under reduced pressure. The residue was dried to obtain Intermediate 1-1 (yield: 30 g, 83% by mass).

[0291] (Synthesis of Intermediate 1-2) Under a nitrogen atmosphere, 100 mL of anhydrous dichloromethane and 1 mL of anhydrous dimethylformamide were added to Intermediate 1-1 (21.6 g, 65.8 mmol), and the mixture was ice-cooled. Oxalyl chloride (11.2 mL, 131.6 mmol) was added dropwise, and the mixture was stirred under ice-cooling for 2 hours and then at room temperature for 12 hours. The solvent was distilled off under reduced pressure, and the residue was dried to obtain Intermediate 1-2 (yield: 21.5 g, 94% by mass).

[0292] (Synthesis of Intermediate 1-3) Under a nitrogen atmosphere, 60 mL of N,N-dimethylformamide was added to naphthalene-1,4,5,8-tetracarboxylic dianhydride (7.18 g, 26.8 mmol) to prepare a solution. A solution of L-(+)-leucinol (4.71 g, 40.2 mmol) and 2-ethylhexylamine (5.19 g, 40.2 mmol) dissolved in 40 mL of N,N-dimethylformamide was added dropwise to this solution, followed by stirring at 120°C for 8 hours. After cooling to room temperature, the solution was poured into 200 mL of ice water, and 1N hydrochloric acid was added to acidify the reaction solution. Extraction was performed with dichloromethane, and the organic layer was washed with water and dried over magnesium sulfate. The resulting solid was filtered. The solvent in the filtrate was distilled off under reduced pressure, and the residue was dried to obtain Intermediate 1-3 (yield: 10.7 g, 84% by mass).

[0293] (Synthesis of Compound 1) Under a nitrogen atmosphere, 150 mL of anhydrous dichloromethane and triethylamine (11.7 mL, 84.4 mmol) were added to intermediate 1-3 (10.1 g, 21.1 mmol) and 4-methoxyphenol (0.01 g), and the mixture was ice-cooled. Intermediate 1-2 (14.6 g, 42.2 mmol) dissolved in 50 mL of anhydrous dichloromethane was added dropwise, and the mixture was stirred under ice-cooling for 1 hour and then at room temperature for 12 hours. The reaction solution was poured into 100 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered, and the solvent in the filtrate was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 1 (yield: 5.3 g, 32% by mass).

[0294] <Synthesis of Compound 2> The synthesis scheme of Compound 2 is shown below.

[0295]

[0296] The synthesis procedure for compound 2 is shown below.

[0297] (Synthesis of Intermediate 2-1) Under a nitrogen atmosphere, 3,4,9,10-perylenetetracarboxylic dianhydride (11.4 g, 29.0 mmol), zinc acetate (5.32 g, 29.0 mmol), 50 g of imidazole, and L-(+)-leucinol (8.5 g, 72.5 mmol) were mixed and stirred at 160°C for 7 hours. After cooling to room temperature, the mixture was dissolved in dichloromethane, and the solution was poured into 200 mL of ice water. 1N hydrochloric acid was added to make the reaction solution acidic. Extraction was performed with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered, and the solvent in the filtrate was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain Intermediate 2-1 (yield: 12.0 g, 70% by mass).

[0298] (Synthesis of Compound 2) Under a nitrogen atmosphere, 150 mL of anhydrous dichloromethane and triethylamine (29.5 mL, 213 mmol) were added to intermediate 2-1 (21.0 g, 35.5 mmol) and 4-methoxyphenol (0.05 g), and the mixture was ice-cooled. Intermediate 1-2 (36.9 g, 107 mmol) dissolved in 50 mL of anhydrous dichloromethane was added dropwise, and the mixture was stirred under ice-cooling for 1 hour and then at room temperature for 2 hours. The reaction solution was poured into 100 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered, and the solvent in the filtrate was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 1 (yield: 32.5 g, 76% by mass).

[0299] <Synthesis of Compound 3> The synthesis scheme of Compound 3 is shown below.

[0300]

[0301] The synthesis procedure for compound 3 is shown below.

[0302] (Synthesis of Intermediate 3-1) Under a nitrogen atmosphere, 100 mL of dehydrated dichloromethane was added to [2-(2-methoxyethoxy)ethoxy]acetic acid (6.3 g, 35.3 mmol) and the mixture was ice-cooled. 0.5 mL of N,N-dimethylformamide was added to this solution, and then oxalyl chloride (6.1 mL, 70.7 mmol) was added dropwise. The mixture was stirred under ice-cooling for 1 hour and then at room temperature for 12 hours. The solvent was distilled off under reduced pressure, and the residue was dried to obtain Intermediate 4-1 (yield 6.9 g, 99% by mass).

[0303] (Synthesis of Compound 3) Under a nitrogen atmosphere, 200 mL of anhydrous dichloromethane and triethylamine (19.5 mL, 141 mmol) were added to intermediate 2-1 (13.9 g, 23.5 mmol) and 4-methoxyphenol (0.04 g), and the mixture was ice-cooled. Intermediate 3-1 (12.2 g, 35.3 mmol) and intermediate 1-2 (6.94 g, 35.3 mmol) dissolved in 80 mL of anhydrous dichloromethane were added dropwise, and the mixture was stirred under ice-cooling for 1 hour and then at room temperature for 12 hours. The solvent of the reaction solution was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain compound 3 (yield 22 g, 88% by mass, molar ratio of compound 3-a to compound 3-b:3-b=2:1).

[0304] <Synthesis of Compound 4> The synthesis scheme of Compound 4 is shown below.

[0305]

[0306] The synthesis procedure for compound 4 is shown below.

[0307] (Synthesis of Intermediate 4-1) Under a nitrogen atmosphere, 5,6,12,13-Tetrachloroperilo[3,4-cd:9,10-c'd']dipyran-1,3,8,10-tetrone (13.0 g, 24.5 mmol) and L-(+)-leucinol (7.2 g, 61.3 mmol) were added to 200 mL of toluene and stirred at 110°C for 9 hours. After cooling to room temperature, the solution was poured into 200 mL of ice water, and 1N hydrochloric acid was added to make the reaction solution acidic. Extraction was performed with toluene and tetrahydrofuran, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was dried to obtain Intermediate 4-1 (yield: 11.8 g, 66% by mass).

[0308] (Synthesis of Compound 4) Under a nitrogen atmosphere, 100 mL of anhydrous dichloromethane and triethylamine (6.6 mL, 47.8 mmol) were added to intermediate 4-1 (5.8 g, 7.96 mmol) and 4-methoxyphenol (0.05 g), and the mixture was ice-cooled. Intermediate 1-2 (8.3 g, 23.9 mmol) dissolved in 70 mL of anhydrous dichloromethane was added dropwise, and the mixture was stirred under ice-cooling for 1 hour and then at room temperature for 12 hours. The reaction solution was poured into 200 mL of ice water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered, and the solvent in the filtrate was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 4 (yield 5.7 g, 53% by mass).

[0309] <Synthesis of Compound 5> The synthesis scheme of Compound 5 is shown below.

[0310]

[0311] The synthesis procedure for compound 5 is shown below.

[0312] (Synthesis of Compound 5) Under a nitrogen atmosphere, 70 mL of dehydrated dichloromethane was added to intermediate 4-1 (5.1 g, 6.93 mmol), and 2-(acryloyloxy)ethyl isocyanate (2.5 g, 17.3 mmol) was added dropwise. 0.1 mL of dibutyltin dilaurate was added, and the mixture was stirred at room temperature for 12 hours. The reaction solution was poured into 200 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered, and the solvent in the filtrate was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 5 (yield 2.3 g, 33% by mass).

[0313] <Synthesis of Compound 6> The synthesis scheme of Compound 6 is shown below.

[0314]

[0315] The synthesis procedure for compound 6 is shown below.

[0316] (Synthesis of Intermediate 6-1) Under a nitrogen atmosphere, 250 mL of acetic acid was added to a mixture of benzene-1,2,4,5-tetracarboxylic anhydride (19.3 g, 88.4 mmol) and L-leucine (23.2 g, 176.9 mmol), and the mixture was stirred at room temperature for 12 hours and then at 130°C for 12 hours. After cooling to room temperature, the mixture was poured into 400 mL of ice water, and the solid was filtered and washed with water. After drying, Intermediate 6-1 (yield: 38.7 g, 98%) was obtained.

[0317] (Synthesis of Intermediate 6-2) Under a nitrogen atmosphere, 200 mL of anhydrous dichloromethane and 1 mL of anhydrous dimethylformamide were added to Intermediate 6-1 (23.0 g, 51.8 mmol), and the mixture was ice-cooled. Oxalyl chloride (26.6 mL, 310.5 mmol) was added dropwise, and the mixture was stirred under ice-cooling for 2 hours and then at room temperature for 12 hours. The solvent was distilled off under reduced pressure, and the solid was filtered and washed with hexane. After drying, Intermediate 6-2 (yield: 23.5 g, 94% by mass) was obtained.

[0318] (Synthesis of Compound 6) Under a nitrogen atmosphere, 4-methoxyphenol (0.01 g) was added to N-(2-hydroxyethyl)acrylamide (17.9 g, 51.7 mmol), and then 200 mL of dehydrated dichloromethane and triethylamine (43 mL, 310.2 mmol) were added and the mixture was ice-cooled. Intermediate 6-2 (23.5 g, 48.8 mmol) dissolved in 100 mL of dehydrated dichloromethane was added dropwise, and the mixture was stirred under ice-cooling for 2 hours and then at room temperature for 2 hours. The solvent was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain Compound 6 (yield 14.2 g, 46% by mass).

[0319] <Synthesis of Compound 7> The synthesis scheme of Compound 7 is shown below.

[0320]

[0321] The synthesis procedure for compound 7 is shown below.

[0322] (Synthesis of Intermediate 7-1) Under a nitrogen atmosphere, 3,4,9,10-perylenetetracarboxylic dianhydride (7.6 g, 19.4 mmol), 2-amino-1,3-propanediol (3.5 g, 38.7 mmol), and 200 mL of NMP were mixed and stirred at 150°C for 8 hours. After cooling to room temperature, the solution was poured into 400 mL of ice water, and 1 N hydrochloric acid was added to make the reaction solution acidic. The resulting solid was filtered, and the filtered product was washed with water. The filtered product was dried to obtain Intermediate 7-1 (yield: 10.0 g, 96% by mass).

[0323] (Synthesis of Compound 7) Under a nitrogen atmosphere, 200 mL of anhydrous dichloromethane and triethylamine (30.9 mL, 223 mmol) were added to intermediate 7-1 (10.0 g, 18.6 mmol) and 4-methoxyphenol (0.05 g), and the mixture was ice-cooled. Intermediate 1-2 (38.6 g, 111 mmol) dissolved in 100 mL of anhydrous dichloromethane was added dropwise, and the mixture was stirred under ice-cooling for 1 hour and then at room temperature for 12 hours. The reaction solution was poured into 200 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered, and the solvent in the filtrate was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 7 (yield 6.80 g, 21% by mass).

[0324] <Synthesis of Compound 8> The synthesis scheme of Compound 8 is shown below.

[0325]

[0326] The synthesis procedure for compound 8 is shown below.

[0327] (Synthesis of Intermediate 8-1)

[0328] Under a nitrogen atmosphere, 100 mL of dichloromethane was added to mono(2-acryloyloxyethyl) succinate (11.7 g, 54.1 mmol) to prepare a solution, which was then ice-cooled. Oxalyl chloride (6.0 mL, 70.3 mmol) was added dropwise to this solution, and the mixture was stirred under ice-cooling for 1 hour and then at room temperature for 12 hours. The solvent was distilled off under reduced pressure, yielding Intermediate 8-1 (yield: 12 g, 94% by mass).

[0329] (Synthesis of Intermediate 8-2) Under a nitrogen atmosphere, 300 mL of ethanol was added to 3-methoxyacetophenone (16 g, 106.5 mmol) and the mixture was ice-cooled. Sodium borohydride (6.0 g, 159.8 mmol) was added in several portions, and the mixture was stirred under ice-cooling for 1 hour and then at room temperature for 2 hours. The reaction solution was poured into 300 mL of water, and the organic layer was extracted with ethyl acetate and washed with brine. After drying over magnesium sulfate, the solvent was distilled off under reduced pressure to obtain Intermediate 8-2 (yield: 15.1 g, 94% by mass).

[0330] (Synthesis of Intermediate 8-3) Under a nitrogen atmosphere, 300 mL of acetic acid was added to a mixture of 1-naphthol (32.5 g, 225.4 mmol) and Intermediate 8-2 (22.9 g, 150.2 mmol), and 8.0 mL of sulfuric acid was added dropwise. After stirring at room temperature for 40 minutes, the mixture was poured into 300 mL of water, and the organic layer was extracted with dichloromethane and washed with water. After drying over magnesium sulfate, the solvent was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain Intermediate 8-3 (yield 17 g, 41% by mass).

[0331] (Synthesis of Intermediate 8-4) Under a nitrogen atmosphere, 500 mL of chloroform was added to Intermediate 8-3 (17 g, 61.1 mmol), and chloranil (15 g, 61.1 mmol) was added. After stirring at room temperature for 24 hours, the mixture was filtered with dichloromethane. The solvent in the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel chromatography to obtain Intermediate 8-4 (yield 15 g, 89% by mass).

[0332] (Synthesis of Intermediate 8-5) Under a nitrogen atmosphere, 200 mL of dichloromethane was added to intermediate 8-4 (14 g, 25.3 mmol) and the mixture was cooled to -70°C. 130 mL of a 1 mol / L solution of boron tribromide in dichloromethane was added dropwise, and the mixture was warmed to room temperature and stirred for 12 hours. The mixture was cooled to 0°C, and 150 mL of water was added dropwise. After warming to room temperature, the organic layer was extracted with dichloromethane and washed with water. After drying over magnesium sulfate, the mixture was dissolved in 200 mL of chloroform, and chloranil (5.1 g, 20.7 mmol) was added and stirred at room temperature for 2.5 hours. The mixture was filtered with dichloromethane. The solvent in the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel chromatography to obtain intermediate 8-5 (yield 9.6 g, 72% by mass).

[0333] (Synthesis of Compound 8) Under a nitrogen atmosphere, 100 mL of dichloromethane was added to a mixture of intermediate 8-5 (7.6 g, 14.5 mmol) and 0.05 g of 4-methoxyphenol to prepare a solution, which was then ice-cooled. Triethylamine (8.0 mL, 58.0 mmol) was added to this solution, and then intermediate 8-1 (7.5 g, 31.9 mmol) was added dropwise. The mixture was stirred under ice-cooling for 1 hour and then at room temperature for 12 hours. The reaction solution was poured into 200 mL of water, extracted with dichloromethane, and the organic layer was washed with water. After drying over magnesium sulfate, the solvent was distilled off under reduced pressure, and the residue was subjected to silica gel chromatography to obtain compound 8 (yield 4.4 g, 33% by mass).

[0334] <Synthesis of Compound 9> The synthesis scheme of Compound 9 is shown below.

[0335]

[0336] The synthesis procedure for compound 9 is shown below.

[0337] (Synthesis of Compound 9) Under a nitrogen atmosphere, 200 mL of dichloromethane was added to a mixture of intermediate 8-5 (5.5 g, 10.5 mmol) obtained by the above procedure and 0.05 g of MEHQ to prepare a solution, which was then ice-cooled. Triethylamine (7.3 mL, 52.4 mmol) was added to this solution, and then intermediate 1-2 (10.9 g, 31.5 mmol) was added dropwise. The mixture was stirred under ice-cooling for 1 hour and then at room temperature for 2 hours. The reaction solution was poured into 100 mL of water, extracted with dichloromethane, and the organic layer was washed with water. After drying over magnesium sulfate, the solvent was distilled off under reduced pressure, and the residue was subjected to silica gel chromatography to obtain compound 9 (yield 4.8 g, 40% by mass).

[0338] <Synthesis of Compound 10> The synthesis scheme of Compound 10 is shown below.

[0339]

[0340] The synthesis procedure for compound 10 is shown below.

[0341] (Synthesis of Intermediate 10-1) Under a nitrogen atmosphere, 150 mL of N,N-dimethylformamide was added to naphthalene-1,4,5,8-tetracarboxylic dianhydride (4.5 g, 16.9 mmol) and L-(+)-leucinol (4.4 mL, 33.7 mmol) to prepare a solution, which was then stirred at 150°C for 6 hours. After cooling to room temperature, the solution was poured into 200 mL of ice water, and 1N hydrochloric acid was added to make the solution acidic. The solution was extracted with ethyl acetate, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered. The solvent in the filtrate was distilled off under reduced pressure, and the residue was dried to obtain Intermediate 10-1 (yield: 7.8 g, 99% by mass).

[0342] (Synthesis of Compound 10) Under a nitrogen atmosphere, 50 mL of anhydrous dichloromethane and triethylamine (5.1 mL, 36.8 mmol) were added to intermediate 10-1 (4.3 g, 9.21 mmol) and the mixture was ice-cooled. Intermediate 8-1 (4.8 g, 20.3 mmol) dissolved in 50 mL of anhydrous dichloromethane was added dropwise, and the mixture was stirred under ice-cooling for 1 hour and then at room temperature for 1 hour. The reaction solution was poured into 100 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The resulting solid was filtered, and the solvent in the filtrate was distilled off under reduced pressure. The residue was subjected to silica gel column chromatography to obtain compound 10 (yield 3.5 g, 45% by mass).

[0343] <Synthesis of Compound 11> The synthesis scheme of Compound 11 is shown below.

[0344]

[0345] The synthesis procedure for compound 11 is shown below.

[0346] (Synthesis of Compound 11) Under a nitrogen atmosphere, 200 mL of anhydrous dichloromethane and triethylamine (29 mL, 208.2 mmol) were added to a mixture of N-(2-hydroxyethyl)acrylamide (5.99 g, 52.0 mmol), 2-acetamidoethanol (5.37 g, 52.0 mmol), and 4-methoxyphenol (0.03 g), and the mixture was ice-cooled. A solution of intermediate 6-2 (16.7 g, 34.7 mmol) obtained in the above procedure dissolved in 100 mL of anhydrous dichloromethane was added dropwise, and the mixture was stirred under ice-cooling for 2 hours and then at room temperature for 2 hours. After distilling off the solvent under reduced pressure, the residue was subjected to silica gel column chromatography to obtain Compound 11 (yield 3.4 g, 16% by mass; molar ratio of Compound 11-a, Compound 11-b, and Compound 11-c: 11-a:11-b:11-c = 2:1:1).

[0347] <Synthesis of Compound 12> Compound 12 was synthesized according to the method described in Non-Patent Document 1 below. Non-Patent Document 1: Organic Letters, 2010, Vol. 12, No. 10, pp. 2382-2385

[0348]

[0349]

[0350] In Table 1, if each of Compounds 1 to 12 has a group represented by the above formula, it is marked with "◯", and if it does not have a group represented by the above formula, it is marked with "×". ETM " represents the molecular weight of the compound represented by the formula (1), and "M X " represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms, and "EA X " represents the electron affinity (eV) of a compound in which all the bonding sites of X in the formula (1) are replaced with hydrogen atoms, and "A ETM " represents the number of polymerizable functional groups contained per 1000 of molecular weight of the compound represented by formula (1).

[0351] The "electron affinity of a compound" is a value calculated using the software "Spartan'18 Parallel Suite" (Wavefunction, Inc.). The method for calculating the electron affinity of a compound will be described below. First, the density functional (DFT) method (functional "B3LYP", basis function "6-31G" is used. * "). Then, based on the optimized shape, "Energy at Ground State in Gas with Density Functional B3LYP 6-31G * " method to measure the lowest unoccupied molecular orbital (LUMO) level (E LUMO / eV) was calculated. The total charge was set to "Neutral (0)" and the unpaired electrons were set to "0". Next, the obtained E LUMO From electron affinity "EA X " was calculated. EA X (eV)=-0.8059×E LUMO +1.1451

[0352] [Evaluation of Solubility in Organic Solvents] Compounds 1 to 12 were each added to a mixed solvent of toluene / 2-propanol = 3 / 7 (mass ratio) at room temperature (25°C) so as to give a concentration of 6% by mass, and the mixture was stirred for 10 minutes with a rotor without heating or cooling. Thereafter, the state of dissolution was visually observed, and the solubility was evaluated according to the following criteria. If any undissolved compound was observed, the compound was heated in a water bath at a constant temperature (40°C) for 10 minutes, and then the state of dissolution was visually observed again, and the solubility was evaluated according to the following criteria. "◎" or "◯" was determined to indicate excellent solubility in organic solvents. The evaluation results are shown in Table 2.

[0353] ◎: Completely dissolved at room temperature. ◯: A small amount of undissolved material was observed at room temperature, but completely dissolved when heated at 40°C for less than 10 minutes. △: Some undissolved material was observed at room temperature, but completely dissolved when heated at 40°C for 10 minutes or more. ×: Some undissolved material was observed even when heated at 40°C for 10 minutes or more.

[0354] [Preparation of Electrophotographic Photoreceptor] <Preparation of Coating Solution P1 for Forming Undercoat Layer> 20 parts of D-type titanyl phthalocyanine, which exhibits a clear peak at a diffraction angle 2θ = 27.3° ± 0.2° in powder X-ray diffraction using CuKα radiation, and 280 parts of 1,2-dimethoxyethane were mixed and milled for 2 hours in a sand grind mill to perform a fine particle dispersion treatment. 400 parts of a 1,2-dimethoxyethane solution containing 2.5 mass % of polyvinyl butyral (manufactured by Denki Kagaku Kogyo Co., Ltd., trade name "Denka Butyral" #6000C) and 170 parts of 1,2-dimethoxyethane were further added and mixed to prepare Coating Solution P1 for forming an undercoat layer with a solids concentration of 3.4 mass %.

[0355] <Preparation of Coating Solution Q1 for Forming Single-Layer Photosensitive Layer> 2.6 parts of D-type titanyl phthalocyanine, which exhibits a clear peak at a diffraction angle 2θ=27.3°±0.2° in powder X-ray diffraction using CuKα radiation, 11.3 parts of a perylene pigment having the following structure, 0.5 parts of a polyvinyl butyral resin, 90 parts of the following hole transport material (HTM48, molecular weight 748), 70 parts of the following electron transport material (ET-2, molecular weight 424.2), 100 parts of a polycarbonate resin having a biphenyl structure, 0.05 parts of silicone oil (manufactured by Shin-Etsu Silicones Co., Ltd.: trade name KF-96) as a leveling agent, and 793.35 parts of a mixed solvent of tetrahydrofuran (hereinafter occasionally abbreviated as THF) and toluene (hereinafter occasionally abbreviated as TL) (THF 90% by mass, TL 10% by mass) were mixed to prepare a single-layer photosensitive layer-forming coating solution Q1 having a solids concentration of 25% by mass.

[0356]

[0357] <Preparation of Protective Layer-Forming Coating Liquids S1 to S12> The curable compound (polymerizable compound not having an electron transport skeleton) shown in Table 2, the electron donor compound shown in Table 2, and the electron transport compound shown in Table 2 were used in the blending amounts shown in Table 2 to obtain protective layer-forming coating liquids S1 to S12 (solid content concentration: approximately 8.0% by mass), each having a solvent composition of toluene / 2-propanol = 3 / 7 (mass ratio). The symbols for the curable compound and electron donor compound in Table 2 indicate the following: Curable compound: A-DPH (dipentaerythritol polyacrylate, product name "NK Ester A-DPH", manufactured by Shin-Nakamura Chemical Co., Ltd.) Curable compound: M9050 (polyester acrylate, product name "Aronix M-9050", manufactured by Toagosei Co., Ltd.)

[0358] Electron donor compound: N-DMBI (N,N-dimethylbenzylamine, manufactured by Tokyo Chemical Industry Co., Ltd.)

[0359] [Examples 1 to 5, Comparative Examples 1 to 7] In Examples 1 to 5 and Comparative Examples 1 to 7, single-layer photoreceptors A1 to A12 were prepared and evaluated as shown in Table 2. <Preparation of Single-Layer Photoreceptors A1 to A12> Single-layer photoreceptors were prepared according to the following procedure. An aluminum cylinder with a 30 mm diameter and a length of 244 mm, the surface of which had been machined, was dip-coated with Coating Solution P1 for forming an undercoat layer, to form an undercoat layer with a film thickness of 0.3 μm after drying. Coating Solution Q1 for forming a single-layer photosensitive layer was dip-coated onto the undercoat layer and dried at 100°C for 24 minutes, to form a single-layer photosensitive layer with a film thickness of 32 μm after drying. Coating Solutions S1 to S14 for forming a protective layer were each ring-coated onto the single-layer photosensitive layer, and immediately after coating, the photoreceptor was rotated at 60 rpm under a nitrogen atmosphere, and 365 nm LED light was applied at 0.9 W / cm. 2 Photoreceptor 2 was irradiated for 30 seconds, photoreceptors 1, 4, and 7 for 60 seconds, and photoreceptors 3, 5, 6, and 8 to 12 for 2 minutes at an intensity of 1.5 to 2.0 μm, and a protective layer was formed so that the film thickness after curing would be 1.5 to 2.0 μm, thereby producing photoreceptors A1 to A12, respectively.

[0360] [Measurement of Martens Hardness and Elastic Deformation Rate] The obtained photoreceptors A1 to A12 were measured from the surface side of the photoreceptor using a microhardness tester (Fischer: FISCHERSCOPE HM2000) under the following measurement conditions in an environment of a temperature of 25°C and a relative humidity of 50%.

[0361] <Conditions for measuring Martens hardness and elastic deformation rate> Indenter: Vickers square pyramidal diamond indenter with a facing angle of 136° Maximum indentation load: 0.2 mN Loading time: 10 seconds Unloading time: 10 seconds

[0362] The Martens hardness is calculated by the following formula: Martens hardness (N / mm 2 ) = Maximum indentation load / Indentation area at maximum indentation load

[0363] The elastic deformation rate is a value defined by the following formula, and is the ratio of the work performed by the membrane due to its elasticity when unloading to the total work required for pressing: Elastic deformation rate (%) = (We / Wt) x 100 In the above formula, the total work Wt (nJ) represents the area surrounded by A-B-D-A in Figure 2, and the elastic deformation work We (nJ) represents the area surrounded by C-B-D-C. The larger the elastic deformation rate, the less likely deformation in response to load will remain, and an elastic deformation rate of 100 means that no deformation will remain.

[0364] In the present invention, the Martens hardness (described as "hardness" in Table 2) is 200 N / mm 2 The test result was judged as "pass" when the test result was above 30%, and the test result was judged as "pass" when the elastic deformation rate was 30% or more.

[0365] [Measurement of Residual Potential] The obtained photoreceptors A1 to A12 were mounted on an electrophotographic property evaluation device manufactured in accordance with the measurement standards of the Electrophotographic Society (described in "Continued Fundamentals and Applications of Electrophotographic Technology," edited by the Electrophotographic Society, Corona Publishing, pp. 404-405), and the electrical properties were measured in the following manner through a cycle of charging, exposure, potential measurement, and de-electrification. First, the grid voltage was adjusted so that the initial surface potential (V0) of the photoreceptor was +700 V. Next, the exposure light was applied at a voltage of 1.3 μJ / cm 2 The sample was irradiated with light, and the residual potential (VL) was measured 60 milliseconds after irradiation. The exposure light used was a halogen lamp light converted to monochromatic light of 780 nm using an interference filter. The measurement was performed at a temperature of 25°C and a relative humidity of 50% (N / N environment). The smaller the absolute value of the residual potential (V), the better the result, since it means that charges have been transported sufficiently and the potential has decreased. In the present invention, a residual potential of 180 V or less was considered to be "pass."

[0366]

[0367] It was confirmed from Table 2 that Compounds 1 to 5 have excellent solubility in organic solvents. Furthermore, Table 2 also shows that the photoreceptors of Examples 1 to 5, which used Compounds 1 to 5, were superior in electrical properties such as residual potential characteristics and mechanical properties such as hardness and elastic deformation rate compared to the photoreceptors of Comparative Examples 1 to 7, which used Compounds 6 to 12.

[0368] All of the compounds of these examples were Compound A, which satisfied the formula (I) and formula (II-1). ETM ≧700 (I) 32≦M X / M ETM ≦0.60 (II-1) (In formula (I) and formula (II-1), M ETM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) have been replaced with hydrogen atoms.

[0369] If the compound forming the protective layer has an electron transport structure, charge injection from the photosensitive layer to the protective layer and charge mobility to the outermost surface are enhanced through the electron transport skeleton, thereby enabling the production of an electrophotographic photoreceptor with excellent electrical properties, such as residual potential characteristics. Furthermore, if the compound has a polymerizable functional group, the compound can be polymerized during the protective layer formation process to form a polymer, thereby forming a protective layer with excellent mechanical strength. Furthermore, if the compound is at or below the upper limit of formula (II-1), the proportion of the hydrophobic π-conjugated skeleton as the mother skeleton falls within a preferred range, resulting in increased solubility in alcohol-based solvents, improved coatability of the coating solution when forming the protective layer, and the formation of a uniform, even protective layer. This is believed to improve the electron transport properties in the protective layer and result in improved electrical properties for the photoreceptor. Furthermore, if the ratio is at or above the lower limit of formula (II-1), the protective layer will have a high level of structures contributing to electron transport, and the high electron transport properties will result in even better electrical properties. Furthermore, when the compound satisfies formula (I) and formula (II-1), the amount of side chain moiety that contributes to solubility in alcohol-based solvents increases, and it is believed that the solubility in alcohol-based solvents becomes even more excellent.

[0370] All of the compounds in the above examples were also compounds B satisfying formula (I), formula (II-2) and formula (III). ETM ≧700 (I) M X / M ETM >0.31 (II-2) A ETM ≧1.8 (III) (in formula (I) and formula (II-2), METM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms. ETM represents the number of polymerizable functional groups contained per 1,000 of molecular weight of the compound represented by formula (1).

[0371] If the compound forming the protective layer has an electron transport structure, using compound B in forming the protective layer is believed to enhance charge injection from the photosensitive layer to the protective layer and charge mobility to the outermost surface through the electron transport skeleton, thereby enabling the production of an electrophotographic photoreceptor with excellent electrical properties such as residual potential characteristics. Furthermore, if compound B has a polymerizable functional group, it can be polymerized during the protective layer formation process to form a polymer, thereby forming a protective layer with excellent mechanical strength. Furthermore, if compound B satisfies formula (I) and formula (II-2), the proportion of structures present in the protective layer that are thought to contribute to electron transport will be increased, which is believed to be advantageous for electron transport. Furthermore, if formula (III) is satisfied, the protective layer will have a large number of polymerizable functional groups, which will facilitate the formation of a dense network structure, resulting in even better hardness and elastic deformation ratio.

[0372] If the above compounds A and B further satisfy the following formula (IV), it is believed that the electron injection from the adjacent layer is good and the electron transport property of the main skeleton is excellent, resulting in further improved electrical properties. X ≧3.8 (IV) (In formula (IV), EA X represents the electron affinity (eV) of the compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms.

[0373] REFERENCE SIGNS LIST 1 Photoconductor (electrophotographic photoconductor) 2 Charging device (charging roller; charging section) 3 Exposure device (exposure section) 4 Developing device (developing section) 5 Transfer device 6 Cleaning device 7 Fixing device 41 Developer tank 42 Agitator 43 Supply roller 44 Developing roller 45 Regulating member 71 Upper fixing member (pressure roller) 72 Lower fixing member (fixing roller) 73 Heating device T Toner P Recording paper (paper, medium)

Claims

1. An electrophotographic photoreceptor having at least a photosensitive layer and a protective layer in this order on a conductive support, wherein the protective layer contains a compound represented by the following formula (1), and the compound represented by the formula (1) satisfies the following formulas (I) and (II-1): (In formula (1), X represents an n-valent electron transporting skeleton. A represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, a group represented by formula (2) below, or a group represented by formula (1B) below. n represents an integer of 1 or more. When n is 1, A is a group represented by formula (2) below or a group represented by formula (1B) below. When n is 2 or more, a plurality of A's may be the same or different from each other, and at least one A is a group represented by formula (2) below or a group represented by formula (1B) below. (In formula (2), * represents a bond to X. 1 and R 2each independently represents a hydrogen atom, an alkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, a heteroaryloxy group which may have a substituent, an alkoxycarbonyl group which may have a substituent, a dialkylamino group which may have a substituent, a diarylamino group which may have a substituent, an arylalkylamino group which may have a substituent, an acyl group which may have a substituent, a haloalkyl group which may have a substituent, an alkylthio group which may have a substituent, an arylthio group which may have a substituent, a silyl group which may have a substituent, a siloxy group which may have a substituent, an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, or a group represented by the following formula (1B). 1 and L 2 each independently represents a direct bond, a divalent group, a group represented by the following formula (1A) or a group represented by the following formula (3A). Z represents a hydrogen atom, an alkyl group, an alkoxy group, an amide group, or a polymerizable functional group. However, when x1+y1=3, x1 is an integer of 0 to 2 and y1 is an integer of 1 to 3, and when x2+y2=3, x2 is an integer of 0 to 2 and y2 is an integer of 1 to 3, and when x1 is an integer of 2 or more, R 1 may be the same or different, and when y1 is an integer of 2 or more, R 2 , x2, y2, L 1 , L 2 and Z may be the same or different from each other, and when x2 is an integer of 2 or more, R 2 may be the same or different, and when y2 is an integer of 2 or more, L 2 and Z may be the same or different from each other. (In formula (1B), * represents a bond to any atom in formula (1) or (2), and B 1 and B 2 R each independently represents a direct bond or a divalent group. 3represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a polymerizable functional group. In formula (1A) and formula (3A), * represents a bond to any atom in formula (1) and formula (2). In formula (1A), B 1 and B 2 Each independently represents a direct bond or a divalent group. In formula (3A), n is an integer of 1 or more. ETM ≧700 (I) 0.32≦M X / M ETM ≦0.60 (II-1) (In formula (I) and formula (II-1), M ETM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms.

2. An electrophotographic photoreceptor having at least a photosensitive layer and a protective layer in this order on a conductive support, wherein the protective layer contains a polymer of a compound represented by the following formula (1), and the compound represented by the formula (1) satisfies the following formulas (I), (II-2) and (III). (In formula (1), X represents an n-valent electron transporting skeleton. A represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, a group represented by formula (2) below, or a group represented by formula (1B) below. n represents an integer of 1 or more. When n is 1, A is a group represented by formula (2) below or a group represented by formula (1B) below. When A is a group represented by formula (2) below, at least one of Z is a polymerizable functional group. When A is a group represented by formula (1B) below, R 3 is a polymerizable functional group. When n is 2 or more, the multiple A's may be the same as or different from each other, and at least one A is a group represented by the following formula (2) or a group represented by the following formula (1B), and contains at least one polymerizable functional group in the structure. In formula (2), * represents a bond to X. 1 and R 2each independently represents a hydrogen atom, an alkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, a heteroaryloxy group which may have a substituent, an alkoxycarbonyl group which may have a substituent, a dialkylamino group which may have a substituent, a diarylamino group which may have a substituent, an arylalkylamino group which may have a substituent, an acyl group which may have a substituent, a haloalkyl group which may have a substituent, an alkylthio group which may have a substituent, an arylthio group which may have a substituent, a silyl group which may have a substituent, a siloxy group which may have a substituent, an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, or a group represented by the following formula (1B). 1 and L 2 each independently represents a direct bond, a divalent group, a group represented by the following formula (1A) or a group represented by the following formula (3A). Z represents a hydrogen atom, an alkyl group, an alkoxy group, an amide group, or a polymerizable functional group. However, when x1+y1=3, x1 is an integer of 0 to 2 and y1 is an integer of 1 to 3, and when x2+y2=3, x2 is an integer of 0 to 2 and y2 is an integer of 1 to 3, and when x1 is an integer of 2 or more, R 1 may be the same or different, and when y1 is an integer of 2 or more, R 2 , x2, y2, L 1 , L 2 and Z may be the same or different from each other, and when x2 is an integer of 2 or more, R 2 may be the same or different, and when y2 is an integer of 2 or more, L 2 and Z may be the same or different from each other. (In formula (1B), * represents a bond to any atom in formula (1) or (2), and B 1 and B 2 R each independently represents a direct bond or a divalent group. 3represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a polymerizable functional group. In formula (1A) and formula (3A), * represents a bond to any atom in formula (1) and formula (2). In formula (1A), B 1 and B 2 Each independently represents a direct bond or a divalent group. In formula (3A), n is an integer of 1 or more. ETM ≧700 (I) M X / M ETM >0.31 (II-2) A ETM ≧1.8 (III) (In formula (I) and formula (II-2), M ETM represents the molecular weight of the compound represented by formula (1). X represents the molecular weight of a compound in which all of the bonding sites of X in the formula (1) are replaced with hydrogen atoms. ETM represents the number of polymerizable functional groups contained per 1,000 molecular weight of the compound represented by formula (1).

3. The electrophotographic photoreceptor according to claim 1 or 2, wherein the compound represented by formula (1) further satisfies the following formula (IV): X ≧3.8 (IV) (In formula (IV), EA X represents the electron affinity (eV) of the compound in which all the bonding sites of X in the formula (1) are replaced with hydrogen atoms.

4. The electrophotographic photoreceptor according to claim 1, wherein in formula (1), X is represented by any one of the following formulas (A-1) to (A-27): (In formulas (A-1) to (A-27), * represents a bond to A, and R A11 , R A21 , R A31 , R A41 , R A51 , R A61 , R A62 , R A71 , R A72 , R A81 , R A82 , R A91 , R A92 , R A101 , R A111 , R A121 , R A131 , R A141 , R A151 , R A161 , R A171 , R A181 , R A182 , R A191 , R A192 , R A201 , R A202 , R A211 , R A212 , R A221 , R A222 , R A231 , R A232 , R A241 , R A242 , R A251 , RA252 , R A261 , R A262 each independently represents a hydrogen atom, an alkyl group which may have a substituent, an aralkyl group which may have a substituent, an aromatic group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, an acyl group which may have a substituent, an ester group which may have a substituent, a cyano group, a nitro group, a sulfone group which may have a substituent, a hydroxy group, an aldehyde group which may have a substituent, or a halogen atom. m11, m21, m31, m41, m51, m61, m62, m71, m72, m81, m82, m91, m92, m101, m111, m121, m131, m141, m151, m161, m171, m181, m182, m191, m192, m201, m202, m211, m212, m221, m222, m231, m232, m241, m242, m251, m252, m261, and m262 each independently represent an integer of 0 or more. When m11, m21, m31, m41, m51, m61, m62, m71, m72, m81, m82, m91, m92, m101, m111, m121, m131, m141, m151, m161, m171, m181, m182, m191, m192, m201, m202, m211, m212, m221, m222, m231, m232, m241, m242, m251, m252, m261, and m262 are each 2 or more, R A11 ~R A262 may be different from each other.) 5. The electrophotographic photoreceptor according to claim 1 or 2, wherein at least one A in said formula (1) is represented by said formula (2).

6. In the formula (2), L and L 2 3. The electrophotographic photoreceptor according to claim 1, wherein at least one of the following is a group represented by formula (1A) or a group represented by formula (3A).

7. The electrophotographic photoreceptor according to claim 1, wherein the compound represented by formula (1) has at least one polymerizable functional group in one molecule.

8. The electrophotographic photoreceptor according to claim 2 or 7, wherein the polymerizable functional group is selected from the groups represented by the following formulae (M1) to (M7). (In formulas (M1) to (M7), R 110 represents a hydrogen atom or an alkyl group which may have a substituent, and * represents the bonding position.

9. In the formula (2), R 1 3. The electrophotographic photoreceptor according to claim 1, wherein R is an alkyl group which may have a substituent.

10. The electrophotographic photoreceptor according to claim 1 or 2, wherein the protective layer further contains a polymer of a polymerizable compound having no electron transporting skeleton.

11. The electrophotographic photoreceptor according to claim 1 or 2, wherein the protective layer further contains an electron donating compound.

12. An electrophotographic photoreceptor cartridge comprising the electrophotographic photoreceptor according to claim 1 or 2.

13. An image forming apparatus comprising the electrophotographic photoreceptor according to claim 1 or 2.

Citation Information

Patent Citations

  • Electrophotographic photoreceptor, processing cartridge comprising it and electrophotographic apparatus

    JP2004126136A

  • Electrophotographic photosensitive member, process cartridge, electrophotographic apparatus, and imide compound

    JP2014224987A

  • Electron transport material and electronic material using the electron transport material

    JP2016095453A

  • Compound, photosensitive fluorescent resin composition containing the same, color conversion film, backlight unit and display device produced from the compound

    JP2022540305A

  • Stable solvent-free charge transfer liquid

    WO2020202177A1

Cited By

  • Compound, composition and electrophotographic photoreceptor

    JP2024146327A

  • Compounds, compositions, and electrophotographic photoreceptors

    JP7955792B2