Resin-coated metal sheet and resin-coated metal sheet production method

The resin-coated metal plate with controlled surface roughness and peak heights addresses adhesion and appearance issues by using direct roll coating with a zinc-plated metal base, achieving strong bonding and bubble-free coatings.

WO2024204591A1PCT designated stage expired Publication Date: 2024-10-03TOYO KOHAN CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012750
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing resin-coated metal plates face issues with air bubbles entering between the metal plate and the coating layer, leading to poor appearance, and adhesion problems when chromate treatment is avoided, resulting in peeling of the metal plate and coating layer.

Method used

A resin-coated metal plate with a resin layer having a protruding mountain portion on its surface, characterized by a height Rpk of 0.46 μm or more, and a method involving direct roll coating with an aqueous dispersion at a solid content concentration of 15% by weight or more, using a metal base material with a zinc plating layer, to enhance adhesion and appearance.

Benefits of technology

The solution provides excellent adhesion to adhesive resin and improves the appearance of coated metal plates by controlling the surface roughness and protruding peak heights, preventing air bubbles and ensuring strong bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012750_03102024_PF_FP_ABST
    Figure JP2024012750_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a resin-coated metal sheet which comprises a metal base and a resin layer provided on the metal base, and in which a protruding peak height Rpk on the surface of the resin layer is at least 0.46 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Resin-coated metal sheet and method for manufacturing the same

[0001] The present invention relates to a resin-coated metal sheet and a method for producing a resin-coated metal sheet.

[0002] Coated metal sheets, which have a resin coating layer formed on a metal sheet, are widely used as building exterior components and automobile components, and are known, for example, as joint materials used in joints (see, for example, Patent Document 1).

[0003] Japanese Patent Application Laid-Open No. 2019-173544

[0004] The coated metal sheet disclosed in Patent Document 1 has a problem in that air bubbles may get trapped between the metal sheet and the coating layer, which may cause a poor appearance. Furthermore, the coated metal sheet disclosed in Patent Document 1 has a specification in which the coating layer is provided on a chromate treatment. On the other hand, there is a technology in which an adhesive layer is provided between the metal sheet and the coating layer without performing the chromate treatment in order to reduce the environmental impact, but there is room for improvement in adhesion, and there is a problem in that the metal sheet and the coating layer may peel off.

[0005] An object of the present invention is to provide a resin-coated metal sheet that has excellent adhesion to an adhesive resin used for bonding to the coating layer and also has a good appearance.

[0006] As a result of intensive research into achieving the above-mentioned object, the present inventors have found that the above-mentioned object can be achieved by a resin-coated metal plate having a metal substrate and a resin layer provided on the metal substrate, in which the protruding peak height Rpk on the surface of the resin layer is 0.46 μm or more, and have thus completed the present invention.

[0007] [1] That is, according to a first aspect of the present invention, there is provided a resin-coated metal sheet having a steel sheet, a metal substrate, and a resin layer provided on the metal substrate, wherein the protruding peak height Rpk on the surface of the resin layer is 0.46 μm or more.

[0008] [2] According to a second aspect of the present invention, there is provided the resin-coated metal sheet according to the first aspect, wherein a height Spk of a protruding peak on the surface of the resin layer is 0.6 μm or more.

[0009] [3] According to a third aspect of the present invention, there is provided the resin-coated metal sheet according to the first or second aspect, wherein the resin layer is made of a resin material containing an olefin-based and / or urethane-based resin.

[0010] [4] According to the fourth aspect of the present invention, the arithmetic mean height Sa of the resin layer 1 The resin-coated metal sheet according to any one of Aspects 1 to 3, wherein the thickness is 0.5 μm or more.

[0011] [5] According to a fifth aspect of the present invention, there is provided the resin-coated metal sheet according to any one of the first to fourth aspects, wherein a height Rpk of a protruding peak on the surface of the resin layer is 0.6 μm or more.

[0012] [6] According to a sixth aspect of the present invention, there is provided a resin-coated metal sheet according to any one of the first to fifth aspects, wherein the metal substrate comprises a metal base plate and a zinc-containing metal plating layer, and the resin layer is formed on the metal plating layer.

[0013] [7] According to the seventh aspect of the present invention, in the metal base sheet, an arithmetic mean height Sa of the surface on which the metal plating layer is formed is 2 7. The resin-coated metal sheet according to any one of Aspects 1 to 6, wherein the thickness is 0.5 μm or more.

[0014] [8] According to aspect 8 of the present invention, there is provided a method for producing a resin-coated metal sheet according to any one of aspects 1 to 7, comprising the steps of applying an aqueous dispersion containing a resin material at a solid content concentration of 15% by weight or more onto the metal substrate by a direct roll coating method, and drying the layer made of the aqueous dispersion to form the resin layer.

[0015] [9] According to a ninth aspect of the present invention, the solid content concentration of the aqueous dispersion is 15% by weight or more and less than 70% by weight, the metal substrate comprises a metal base plate and a zinc-containing metal plating layer, and the arithmetic mean height Sa of the surface of the metal base plate on which the metal plating layer is formed is 2 The method for producing a resin-coated metal sheet according to aspect 8 is provided, wherein the thickness is 0.75 μm or more.

[0016]

[10] According to a tenth aspect of the present invention, there is provided the method for producing a resin-coated metal sheet according to the eighth or ninth aspect, wherein the resin material contains an olefin-based and / or urethane-based resin.

[0017] According to the present invention, it is possible to provide a resin-coated metal sheet that has excellent adhesion to an adhesive resin and a good appearance.

[0018] Fig. 1 is a cross-sectional view showing the configuration of a resin-coated metal sheet according to an embodiment of the present invention. Fig. 2(a) is a diagram illustrating a method for applying an aqueous dispersion by a direct roll coating method according to an embodiment of the present invention, and Fig. 2(b) is a cross-sectional view showing the surface shape of a resin layer 20 formed by applying an aqueous dispersion having a solid content of 15% by weight or more by the direct roll coating method. Fig. 3 is a reference diagram showing a resin layer formed by applying an aqueous dispersion having a solid content of less than 15% by weight by the direct roll coating method.

[0019] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0020] 1 is a cross-sectional view showing the configuration of a resin-coated metal sheet 1 according to this embodiment. The resin-coated metal sheet 1 according to this embodiment includes a metal substrate 10 and a resin layer 20 provided on the metal substrate 10. The resin-coated metal sheet 1 according to this embodiment is used as a joint material, an automotive interior material, or the like, by forming a coating layer made of a resin material on the resin layer 20 using an adhesive resin.

[0021] <Metal Substrate 10> The metal substrate 10 in this embodiment is a plated plate including a metal original sheet 11 and a metal plating layer 12 containing zinc formed on the metal original sheet 11.

[0022] The metal base plate 11 is not particularly limited, but examples include iron- or aluminum-based metal base plates. Examples of iron-based metal base plates include carbon steel plates and stainless steel plates. Examples of carbon steel plates include low-carbon aluminum-killed steel (carbon content: 0.01 to 0.15 wt.%), ultra-low carbon steel (carbon content: less than 0.01 wt.%), and non-aging carbon steel obtained by adding Ti, Nb, or the like to ultra-low carbon steel. When using a steel plate as the metal base plate 11, it is preferable to use a hot-rolled plate of such steel that is pickled to remove surface scale (oxide film), cold-rolled, electrolytically cleaned, annealed, and temper-rolled. The annealing method may be either continuous annealing or box annealing, and is not particularly limited.

[0023] From the viewpoint of controlling the height of the protruding peaks of the resin layer 20 described later, the arithmetic mean height Sa of the surface of the metal original plate 11 on which the metal plating layer 12 is formed is set to 0.5 mm. 2 The arithmetic mean height Sa of the metal plate 11 is preferably 0.5 μm or more, and more preferably 0.75 μm or more. 2 An example of a method for making the surface roughness of the raw metal sheet 11 within the above range is to use a rolling roll having a predetermined surface roughness when rolling the steel into the raw metal sheet 11. The arithmetic mean roughness Ra of the rolling roll measured along the central axis of the rolling roll (a direction perpendicular to the rolling direction of the raw metal sheet 11) is preferably 0.8 μm or more, more preferably 2.5 μm or more, and even more preferably 3.2 μm or more. There is no particular upper limit to the arithmetic mean roughness Ra of the rolling roll, but the arithmetic mean height Sa of the raw metal sheet 11 is 2 If the arithmetic mean roughness Ra of the rolling roll is too large, there is a possibility that the thickness will be non-uniform when the metal plating layer 12 or the resin layer 20 is formed on the metal original sheet 11. Therefore, from the viewpoint of enhancing the uniform stability of the metal plating layer 12 and the resin layer 20, the arithmetic mean roughness Ra of the rolling roll is preferably 8.0 μm or less, and more preferably 6.0 μm or less. From the same viewpoint, the arithmetic mean height Sa of the metal original sheet 11 is 2 The upper limit of the arithmetic mean height Sa is preferably 2.0 μm or less. 2can be measured based on ISO 25178, and the arithmetic mean roughness Ra can be measured based on JIS B 0671:2002.

[0024] The thickness of the metal plate 11 in this embodiment is not particularly limited, but is preferably 0.04 to 2.0 mm, and more preferably 0.04 to 1.5 mm.

[0025] The metal plating layer 12 is a layer containing zinc provided on the original metal sheet 11. Examples of metal plating that constitutes the metal plating layer 12 include zinc-based platings such as zinc plating, zinc-cobalt-molybdenum alloy plating, zinc-nickel alloy plating, zinc-iron alloy plating, alloyed hot-dip galvanizing, and zinc-aluminum-magnesium alloy plating. Among these zinc-based platings, zinc-cobalt-molybdenum alloy plating or pure zinc plating (hereinafter also referred to as pure zinc plating) having a zinc weight percentage of 99.9 wt % or more is more preferred from the viewpoint of improving the corrosion resistance of the resin-coated metal sheet 1. The metal plating layer can be formed by electroplating the surface of the original metal sheet 11 using a plating bath of a predetermined composition.

[0026] For example, when the metal plating layer 12 is made of zinc-cobalt-molybdenum alloy plating, it can be formed by electroplating using a plating bath having a composition of 150 to 300 g / L of zinc sulfate, 5 to 60 g / L of cobalt sulfate, 0.01 to 0.5 g / L of ammonium molybdate, 5 to 60 g / L of ammonium sulfate, and 50 g / L or less of sodium sulfate. The electroplating conditions are preferably pH 2.5 to 4.0, bath temperature 30 to 60°C, and current density 5 to 50 A / dm 2 When the metal plating layer 12 is made of pure zinc plating, it can be formed by electroplating using a plating bath having a composition of 150 to 300 g / L of zinc sulfate and 10 to 100 g / L of sodium sulfate. The electroplating conditions are preferably pH 0.5 to 2.5, bath temperature 30 to 60°C, and current density 5 to 80 A / dm 2 is.

[0027] When the metal plating layer 12 is formed of a zinc-cobalt-molybdenum alloy plating, the content of zinc, cobalt, and molybdenum in the metal plating layer 12 is preferably 0.1 to 5 wt % cobalt, 0.001 to 1 wt % molybdenum, and the remainder zinc. The content of the metals in the metal plating layer 12 can be adjusted by adjusting the composition of the plating bath and the electroplating conditions to suitable ranges.

[0028] The thickness of the metal plating layer 12 is not particularly limited, but is preferably 0.3 to 8.0 μm. The thicker the metal plating layer 12, the smoother the surface roughness of the metal plating layer 12, which may affect the subsequent formation of the resin layer 20. In particular, in the case of zinc-based plating, crystals precipitate in a plate-like shape, which tends to smooth the surface roughness of the metal plating layer 12. Therefore, the thickness of the metal plating layer 12 is more preferably 0.3 to 5.0 μm from the viewpoint of controlling the surface roughness of the metal plating layer 12 and the height of the protruding peaks of the resin layer 20. The thickness of the metal plating layer 12 is even more preferably 0.6 to 5.0 μm from the viewpoint of corrosion resistance. The thickness of the metal plating layer 12 is particularly preferably 0.7 μm to 4.5 μm from the viewpoint of achieving both corrosion resistance and suppressing reduction in surface roughness due to metal plating.

[0029] In the present embodiment, the metal substrate 10 has the metal plating layer 12 formed on both sides of the original metal plate 11, but the configuration of the metal substrate 10 is not particularly limited thereto, and the metal plating layer 12 may be formed on only one side of the original metal plate 11. Alternatively, the metal substrate 10 may be composed of only the original metal plate 11 without having the metal plating layer 12.

[0030] <Resin layer 20> The resin layer 20 is a layer formed on the metal plating layer 12. The resin layer 20 is provided to improve adhesion between the metal substrate 10 and an adhesive resin used in combination with the resin-coated metal sheet 1 of this embodiment. In this embodiment, the resin layer 20 is formed on both sides of the metal substrate 10, but is not particularly limited thereto, and the resin layer 20 may be formed on only one side of the metal substrate 10.

[0031] Resins contained in the resin layer 20 include, but are not limited to, olefin-based resins and urethane-based resins. Examples of olefin-based resins include polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic ester copolymer, ethylene-acrylic acid copolymer, and ethylene-methacrylic acid copolymer, with ethylene-acrylic acid copolymer and ethylene-methacrylic acid copolymer being more preferred. Examples of urethane-based resins include reaction products of polyols such as polyacrylic polyols, polyester polyols, and polyether polyols with polyisocyanates such as aliphatic diisocyanates, aromatic diisocyanates, and aromatic aliphatic diisocyanates. The olefin-based resins and urethane-based resins may be used alone or in combination. As described below, the resin layer 20 is formed by applying an aqueous dispersion containing a resin material. However, it is preferable that the resin layer 20 substantially contains no components other than the resin material, except for unavoidable components derived from additives contained in the aqueous dispersion. The content of the resin contained in the resin layer 20 is preferably 90% by weight or more, and more preferably 99% by weight or more. In other words, the resin layer 20 is preferably composed essentially of the above-mentioned resin alone.

[0032] When an ethylene-acrylic acid copolymer or an ethylene-methacrylic acid copolymer is used as the resin contained in the resin layer 20, the weight average molecular weight is preferably 20,000 to 150,000, more preferably 30,000 to 100,000, and even more preferably 40,000 to 80,000.

[0033] Furthermore, the proportion of polar components in the surface free energy of the resin layer 20 is preferably 3% to 35%, more preferably 10% to 35%, and even more preferably 20% to 35%. The proportion of polar components in the surface free energy can be calculated from the surface free energy obtained by applying the contact angles of ion-exchanged water, ethylene glycol, and diiodomethane measured using a fully automatic contact angle meter (DM-701, manufactured by Kyowa Interface Science Co., Ltd.) to the Kitazaki-Hata theoretical formula. Specifically, after determining the surface free energies of the dispersion component, dipole component, and hydrogen bond component, the proportion of the polar component can be determined as the ratio of the sum of the surface free energy of the dipole component and the surface free energy of the hydrogen bond component to the total value of these. Methods for achieving the proportion of polar components in the surface free energy of the resin layer 20 surface within the above range include, but are not limited to, selecting the resin material constituting the resin layer 20. For example, when an ethylene-acrylic acid copolymer is used as the resin constituting the resin layer 20, the proportion of polar components in the surface free energy of the resin layer 20 surface can be controlled by adjusting the content of acrylic acid units in the ethylene-acrylic acid copolymer. Furthermore, when an ethylene-methacrylic acid copolymer is used as the resin constituting the resin layer 20, the proportion of polar components in the surface free energy of the surface of the resin layer 20 can be controlled by adjusting the content of methacrylic acid units in the ethylene-methacrylic acid copolymer.

[0034] The thickness of the resin layer 20 is not particularly limited, but is preferably 0.3 to 3.0 μm. From the viewpoint of facilitating the formation of convex shapes over the entire surface so that the protruding peak height Rpk (described below) on the surface of the resin layer 20 falls within a specific range, the thickness of the resin layer 20 is preferably 0.5 μm or more, and more preferably 0.6 μm or more. The upper limit of the thickness of the resin layer 20 is not particularly limited, but if the thickness is too large, the adhesive strength of the resin layer 20 to the adhesive resin may be weakened, so the upper limit is preferably 2.0 μm or less.

[0035] The resin layer 20 of the resin-coated metal sheet 1 in this embodiment has a surface protruding peak height Rpk of 0.46 μm or more, preferably 0.60 μm or more, as measured according to JIS B 0671:2002. The upper limit of the protruding peak height Rpk is not particularly limited, but is preferably 2.0 μm or less, and from the viewpoint of stable ease of manufacture, 1.5 μm or less is more preferable. The protruding peak height Rpk is one of the parameters for evaluating the roughness curve specified in JIS B 0671-1 and represents the height of protruding peaks on the roughness curve. More specifically, Rpk is the average height of protruding peaks above the core, calculated after dividing the surface shape into three stages: peaks, cores, and valleys based on the roughness curve. The larger the protruding peak height Rpk of the resin layer 20, the higher the average height of the protrusions on the surface of the resin layer 20. By setting Rpk to 0.46 μm or more, it is possible to ensure that protruding convex portions corresponding to the protruding peaks are sufficiently formed. It is presumed that by setting the protruding peak height Rpk within this range, when a coating layer is applied to the resin layer 20 using an adhesive resin, the adhesive resin flows along the protruding portions, wets, and spreads, thereby improving adhesion. By setting the protruding peak height Rpk of the resin layer 20 within the above range, the resin-coated metal sheet 1 can have excellent adhesion to the adhesive resin.

[0036] In the past, when a metal substrate having a zinc-containing metal plating layer formed on a metal original sheet was used, and a chromium-free resin layer was used for environmental reasons, it was sometimes difficult to improve adhesion to the adhesive resin even when a resin layer was formed on the metal substrate. According to the resin-coated metal sheet 1 of the present embodiment, by controlling the protruding peak height Rpk on the surface of the resin layer 20, it is possible to improve adhesion of the resin layer 20 to the adhesive resin even when a metal substrate 10 having a zinc-containing metal plating layer 12 formed thereon is used.

[0037] The height Rpk of the protruding peaks on the surface of the resin layer 20 can be measured at any point on the surface of the resin layer 20. However, in order to take into account the influence of the protruding peaks formed on the resin layer 20 due to the streak shape (rolling streaks) formed on the surface of the metal original plate 11 by rolling the metal original plate 11, and to evaluate a more average roughness including the rolling streaks, it is more preferable that the height Rpk of the protruding peaks on a line along the width direction of the resin-coated metal plate 1 (the direction perpendicular to the direction in which the metal original plate 11 was rolled on the surface of the resin layer) be within the above range.

[0038] In this embodiment, the resin layer 20 of the resin-coated metal sheet 1 preferably has a surface protruding peak height Spk of 0.60 μm or more, more preferably 0.70 μm or more, and even more preferably 0.80 μm or more, as measured according to ISO 25178. While the protruding peak height Rpk is a value calculated from the line roughness load curve, the protruding peak height Spk is a value calculated from the surface roughness load curve, and represents the average height of the protruding peaks on the resin layer surface from a more global perspective. The larger the protruding peak height Spk, the higher the protruding peaks present throughout the entire resin layer 20. By having the protruding peak height Spk within the above range, when the resin layer 20 is coated with a coating resin using an adhesive resin, air bubbles generated between the resin layer 20 and the adhesive resin can escape through the gaps between the protruding peaks. More specifically, when the adhesive resin and the coating layer are simultaneously and continuously poured onto the resin layer 20 and adhered to each other, air bubbles can escape through gaps in the protrusions present on the entire surface, thereby improving the appearance of the coated metal sheet manufactured using the resin-coated metal sheet 1.

[0039] In the resin-coated metal sheet 1 of this embodiment, adhesion can be further improved by setting the protruding peak height Rpk of the resin layer 20 to 0.6 μm or more and the protruding peak height Spk to 0.6 μm or more. The reason for this is not clear, but it is thought that by setting the protruding peak height Rpk and the protruding peak height Spk in the above ranges, the adhesive resin can be made to wet and spread more uniformly and air bubbles can be made to escape more easily, thereby reducing unevenness in the thickness of the adhesive resin and suppressing the formation of air bubbles.

[0040] The arithmetic mean height Sa of the surface of the resin layer 20 measured based on ISO 25178 1 is preferably 0.5 μm or more, and more preferably 0.6 μm or more, from the viewpoint of improving adhesion with the adhesive resin, in a state in which a convex shape for setting the protruding peak height Rpk within a specific range is formed on the entire surface of the resin layer 20. 1 The upper limit of is not particularly limited, but if it is too large, the thickness of the resin layer 20 may become non-uniform, so it is preferably 2.0 μm or less.

[0041] In addition, as a general concept of surface roughness and adhesion strength, it is known that the greater the arithmetic mean height of the surface of a material, the greater the resin adhesion strength to that material. Meanwhile, the present inventors, while diligently studying ways to improve the adhesion strength between a metal substrate coated with a resin layer and an adhesive resin, noticed that the strength of adhesion of the adhesive resin to the resin layer does not depend on the arithmetic mean height of the resin layer, and found that the adhesion strength can be improved by controlling the surface shape of the resin layer 20 and setting the protruding peak height Rpk within a specific range.

[0042] As described above, the resin-coated metal sheet 1 in this embodiment has excellent adhesion to the adhesive resin because the protruding peak height Rpk on the surface of the resin layer 20 is within the above range. Examples of such adhesive resins include olefin-based resins such as polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic ester copolymer, ethylene-acrylic acid copolymer, and ethylene-methacrylic acid copolymer, as well as urethane-based resins.

[0043] The resin-coated metal sheet 1 in this embodiment can be produced by the following method: applying an aqueous dispersion containing a resin material at a solid content concentration of 15% by weight or more onto the metal substrate 10 by a direct roll coating method, and drying the layer made of the aqueous dispersion to form the resin layer 20.

[0044] The aqueous dispersion used in the production of the resin-coated metal sheet 1 is an aqueous dispersion obtained by dispersing the above-mentioned olefin-based resin and / or urethane-based resin in a medium such as water. The solids concentration of the aqueous dispersion is 15% by weight or more. By setting the solids concentration to 15% or more, when the aqueous dispersion that has contacted the surface of the metal substrate 11 is extruded from the roll together with the metal substrate 11 by the direct roll coating method, the aqueous dispersion can be pulled by the roll and lifted up against the metal substrate 10. As a result, in addition to the surface irregularities resulting from the surface morphology of the metal substrate 10, it is possible to form unique convex portions on the surface of the resin layer 20, thereby controlling the Rpk and Spk of the resin layer 20 within the above ranges. According to the present invention, by forming the resin layer 20 by direct roll coating using an aqueous dispersion containing a resin at a solids concentration of 15% by weight or more, the protruding peak heights Rpk and Spk of the surface of the resin layer 20 can be controlled within the above ranges.

[0045] The solid content concentration of the aqueous dispersion is determined by the arithmetic mean height Sa of the surface of the metal substrate 11 on which the metal plating layer 12 is formed. 2 For example, it is preferable to adjust the arithmetic mean height Sa of the metal plate 11 in accordance with 2When the arithmetic mean height Sa of the metal base plate 11 is 0.75 to 2.0 μm, the solids concentration of the aqueous dispersion is preferably 15% by weight or more, more preferably 20% by weight or more, from the viewpoint of facilitating the formation of unique convex portions of the resin layer 20 or facilitating the height of the convex portions. In this case, the upper limit of the solids concentration of the aqueous dispersion is not particularly limited, but is preferably less than 70% by weight, more preferably 65% ​​by weight or less, and even more preferably 55% by weight or less, from the viewpoint of facilitating the suppression of deterioration or solidification of the aqueous dispersion in continuous production and stably forming the surface shape of the resin layer 20. 2 is 0.65 μm or more and less than 0.75 μm, that is, the arithmetic mean height Sa of the metal substrate 2 When the arithmetic mean height Sa of the metal original plate 11 is relatively small, it is preferable to set the solid content concentration of the aqueous dispersion to 20% by weight or more and less than 70% by weight in order to easily form the convex portions unique to the resin layer 20 or to easily make the convex portions high. 2 When the arithmetic mean height Sa of the metal original plate 11 is 0.65 μm or more and less than 0.75 μm, the lower limit of the solid content concentration of the aqueous dispersion is more preferably 25 wt % or more, and even more preferably 30 wt % or more. 2 is set to any of the above ranges, and the arithmetic mean height Sa 2 From the viewpoint of improving adhesion strength, it is preferable to form the resin layer 20 by a direct roll coating method using an aqueous dispersion having a solid content according to the above. Furthermore, by using such a manufacturing method, it is possible to control the Rpk and Spk of the surface of the resin layer 20 and also to control the arithmetic mean height Sa of the surface of the resin layer 20. 1 can also be in a preferred range.

[0046] The method for producing such an aqueous dispersion is not particularly limited, but examples include a method in which the above-mentioned olefin-based resin and / or urethane-based resin is produced by a known emulsion polymerization method, solution polymerization method, or the like, and the polymer solution is vigorously stirred to prepare the dispersion.

[0047] The minimum film forming temperature (MFT) of the aqueous dispersion is preferably 0 to 200° C., and more preferably 5 to 150° C. The minimum film forming temperature of the aqueous dispersion can be adjusted by selecting the type of resin material contained in the aqueous dispersion.

[0048] The pH of the aqueous dispersion is preferably 3 to 11, and more preferably 4 to 10.

[0049] The viscosity at 25°C of the aqueous dispersion used to form the resin layer 20 is not particularly limited as long as the solids concentration of the aqueous dispersion is within the above range, but is preferably 10 to 150 mPa·s, and more preferably 20 to 100 mPa·s. Note that the viscosity of many aqueous dispersions changes significantly depending on the external force applied, and the viscosity and solids concentration of the aqueous dispersion are not necessarily proportional.

[0050] The aqueous dispersion used to form the resin layer 20 may contain, in addition to the above-mentioned resin, a surfactant, an emulsifying aid, colloidal silica, etc. as necessary. On the other hand, in order to form protruding resin peaks on the surface by lifting with rolls as described above, it is preferable that the aqueous dispersion does not contain metal oxides, and it is also preferable that the resin layer 20 does not contain metal oxides.

[0051] The layer made of the aqueous dispersion is preferably dried at a temperature of 50° C. to 200° C. for a drying time of 1 to 60 seconds.

[0052] <Method for manufacturing resin-coated metal sheet 1> In this embodiment, the resin-coated metal sheet 1 can be manufactured by a process of applying an aqueous dispersion containing a resin material at a solid content concentration of 15% by weight or more onto a metal substrate 10 by a direct roll coating method, and a process of drying the layer made of the aqueous dispersion to form a resin layer 20. As the aqueous dispersion, those described above can be used.

[0053] Fig. 2(a) is a diagram illustrating a method for applying an aqueous dispersion by direct roll coating in this embodiment, and Fig. 2(b) is a cross-sectional view showing the surface shape of a resin layer 20 formed by applying an aqueous dispersion having a solid content concentration of 15% by weight or more by direct roll coating. Fig. 3 is a reference diagram showing a resin layer formed by applying an aqueous dispersion having a solid content concentration of less than 15% by weight by direct roll coating.

[0054] The process of applying an aqueous dispersion containing a resin material by a direct roll coating method will be described. In the direct roll coating method, as shown in FIG. 2(a), the roll is rotated so that the rotation direction of the roll and the direction of travel of the metal substrate 10 are the same (so that the direction of travel of the portion of the roll that contacts the metal substrate 10 is the same as the direction of travel of the metal substrate 10), and the aqueous dispersion is applied. In this embodiment, by setting the solids concentration of the aqueous dispersion containing the resin material to 15% by weight or more, a portion of the aqueous dispersion extruded onto the metal substrate 10 is lifted from the metal substrate 10 toward the roll as the roll rotates. As a result, as shown in FIG. 2(b), protrusions can be formed on the surface of the resin layer 20 formed from the aqueous dispersion, and the protrusion peak heights Rpk and Spk on the surface of the resin layer 20 can be controlled within a predetermined range. On the other hand, in reverse roll coating, in which the rotation direction of the roll is opposite to the direction of travel of the metal substrate 10, the aqueous dispersion is applied to the metal substrate 10 by the roll, making it difficult to form protrusions.

[0055] On the other hand, when the solid content concentration of the aqueous dispersion is less than 15% by weight, even when the direct roll coating method is used, the aqueous dispersion is not lifted up by the roll, and therefore a resin layer having a smooth surface is formed as shown in FIG. 3 .

[0056] As described above, the metal substrate 10 is rolled using a rolling roll having an arithmetic mean roughness Ra of 0.8 μm or more, and has an arithmetic mean height Sa 2 It is preferable to use a metal plate 11 having a length of 0.5 m or more, which is plated with a zinc-based metal to form a metal plating layer 12.

[0057] The resin-coated metal sheet 1 obtained in this manner has appropriately controlled protruding peak heights Rpk and Spk of the resin layer 20, has excellent adhesion to the adhesive resin, and can provide a good appearance to joint materials, automotive interior materials, and other products made from coated metal sheets manufactured using the resin-coated metal sheet 1.

[0058] EXAMPLES The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0059] <Weight-Average Molecular Weight of Resin> The weight-average molecular weight of the resin was measured by high-temperature GPC-IR using an aqueous dispersion containing the resin material used in the examples.

[0060] <Protruding peak height and arithmetic mean height of resin layer, and arithmetic mean height of metal original sheet> Using a laser microscope (Olympus Corporation, 3D measuring laser microscope LEXT OLS5000), an analysis image with a field of view of 645 μm × 645 μm was obtained under the condition of a 20x objective lens (lens name: MPLAPON20XLEXT). Next, the obtained analysis image was subjected to automatic correction processes of noise removal and tilt correction using an analysis application. After that, analysis was performed by clicking the icons for line roughness measurement and surface roughness measurement, and the protruding peak heights Rpk, Spk and arithmetic mean height Sa of the resin layer 20 of the resin-coated metal sheet 1 were calculated. 1 The protruding peak height Rpk was determined in the width direction of the resin-coated metal sheet 1, i.e., on the surface of the resin-coated metal sheet 1, for a cross section along the direction (TD) perpendicular to the rolling direction (RD) of the original metal sheet 11. The arithmetic mean height Sa of the original metal sheet 11 2 was also measured in the same manner.

[0061] <Proportion of Polar Component in Surface Free Energy of Resin Layer Surface> Using a fully automatic contact angle meter (DM-701 manufactured by Kyowa Interface Science Co., Ltd.), the contact angles of ion-exchanged water, ethylene glycol, and diiodomethane on the surface of the resin layer 20 of the resin layer-coated metal sheet 1 were each measured. The measured contact angle values ​​were applied to the Kitazaki-Hata theoretical formula to determine the surface free energies of the dispersion component, dipole component, and hydrogen bond component. The proportion of the polar component was determined as the ratio of the sum of the surface free energy of the dipole component and the surface free energy of the hydrogen bond component to the total value of these.

[0062] <Peel Strength from Adhesive Resin> To evaluate adhesion to adhesive resin, a T-peel test (hereinafter also referred to as a peel test) was performed in accordance with JIS K 6854-3 to measure the peel strength of the resin-coated metal sheet 1. Specifically, two resin-coated metal sheets 1, each 25 mm wide and 80 mm long, were arranged facing each other, and nine particles of an olefin-based adhesive resin (product name: Mersen, manufactured by Tosoh Corporation) were sandwiched between the two resin-coated metal sheets 1. The resin-coated metal sheet 1 and the olefin-based adhesive resin were thermocompression-bonded at a temperature of 150°C, a pressure of 0.5 MPa, and a time of 2 minutes to obtain a laminate. The resulting laminate was subjected to a peel test using a tensile tester (product name "AGX-V," manufactured by Shimadzu Corporation) at a peel rate of 200 mm / min, and the maximum peel strength (unit: N / 25 mm) was measured.

[0063] <Appearance (presence or absence of bubbles), wetting and spreading of adhesive resin> The prepared resin-coated metal sheet 1 was heated on a hot plate set at 130°C, and one grain of olefin-based adhesive resin (product name Mersen, manufactured by Tosoh Corporation) was placed on the resin layer 20 of the resin-coated metal sheet 1. A 3.5 g, 9 cm 2A Teflon plate (Teflon is a registered trademark) was placed on top of the Teflon plate, and a 150 g weight was placed on top of the Teflon plate and maintained for 2 minutes. After 2 minutes, the Teflon plate and weight were removed, and the test was allowed to air-cool. The presence of air bubbles between the adhesive resin and the resin layer 20 was visually confirmed. The absence of air bubbles indicates that the coated metal sheets manufactured using the resin-coated metal sheet 1, as well as joint materials and automotive interior materials made from the coated metal sheets, have excellent appearance. To confirm the difference in wetting and spreading properties, the test was conducted using the same procedure as above, except that the hot plate temperature was changed to 100°C and 110°C. After air-cooling, the circularity c (c = b / a), which is the ratio of the major axis length a to the minor axis length b of the adhesive resin that had spread on the resin layer, was determined. A higher circularity c indicates more uniform spreading of the adhesive resin.

[0064] Example 1 A cold-rolled sheet (thickness: 0.16 mm) of low-carbon aluminum-killed steel was prepared as the original metal sheet 11. This original metal sheet 11 was obtained by rolling the low-carbon aluminum-killed steel sheet using a rolling roll having an arithmetic mean roughness Ra of 2.5 to 5.5 μm. The original metal sheet 11 had an arithmetic mean height Sa 2 Next, the metal base plate 11 was subjected to alkaline electrolytic degreasing and pickling by immersion in sulfuric acid, and then subjected to a bath temperature of 40° C. and a current density of 15 A / dm 2 By carrying out plating under the above conditions, a metal substrate 10 was obtained in which a 1.5 μm thick metal plating layer 12 made of zinc-cobalt-molybdenum alloy plating was formed on both sides of the metal original sheet 11. The composition of the metal plating layer was measured by fluorescent X-ray analysis and found to be Co: 0.16 wt %, Mo: 0.02 wt %, and the balance Zn.

[0065] Next, an aqueous dispersion (solids concentration 20 wt %, viscosity 70 mPa·s, pH 9.3, MFT 12°C) containing an olefin-based resin (ethylene-acrylic acid copolymer) was applied onto the metal plating layer 12 of the metal substrate 10 by direct roll coating to form a layer made of the aqueous dispersion. The coating was then dried at a temperature of 150°C for 10 seconds to form a resin layer 20 containing the olefin-based resin. The thickness of the resin layer 20 was 0.6 μm. The resin layer 20 was formed on both sides of the metal substrate 10. In this manner, a resin-coated metal sheet 1 was obtained in which the resin layer 20 was formed on both sides of the metal substrate 10. The resulting resin-coated metal sheet 1 was evaluated for the height and arithmetic mean height of the protruding peaks of the resin layer, the proportion of polar components in the surface free energy of the resin layer surface, the peel strength against the adhesive resin, appearance (presence or absence of bubbles), and the wetting and spreading properties of the adhesive resin. The results are shown in Tables 1 to 3. The weight average molecular weight of the ethylene-acrylic acid copolymer measured by high temperature GPC-IR was 49,900.

[0066] Example 2 A resin-coated metal sheet 1 was obtained in the same manner as in Example 1, except that an aqueous dispersion containing an olefin-based resin (ethylene-methacrylic acid copolymer) (solids concentration 44.5 wt %, viscosity 40 mPa·s, pH 4.8, MFT 100°C) was used instead of the aqueous dispersion containing an olefin-based resin (ethylene-acrylic acid copolymer). The height and arithmetic mean height of the protruding peaks of the resin layer were measured, and the peel strength against the adhesive resin, appearance (presence or absence of bubbles), and wettability and spreadability of the adhesive resin were evaluated. The results are shown in Tables 1 to 3. The weight-average molecular weight of the ethylene-methacrylic acid copolymer measured by high-temperature GPC-IR was 69,300. The thickness of the resin layer 20 was 0.6 μm.

[0067] Comparative Example 1: The metal original plate 11 is rolled using a rolling roll having an arithmetic mean roughness Ra of 0.01 to 0.5 μm, and has an arithmetic mean height Sa 2 Resin-coated metal sheet 1 was obtained in the same manner as in Example 1, except that a resin layer 20 having a thickness of 0.3 μm was used. The height of the protruding peaks and the arithmetic mean height of the resin layer were measured, and the appearance (presence or absence of bubbles) was evaluated. The results are shown in Table 1. The thickness of resin layer 20 was 0.6 μm.

[0068] Comparative Example 2: The metal original plate 11 is rolled using a rolling roll having an arithmetic mean roughness Ra of 0.8 to 2.3 μm, and has an arithmetic mean height Sa 2 Resin-coated metal sheet 1 was obtained in the same manner as in Example 1, except that a resin layer 20 having a thickness of 0.73 μm was used. The height of the protruding peaks and the arithmetic mean height of the resin layer were measured, and the peel strength to the adhesive resin and the appearance (presence or absence of bubbles) were evaluated. The results are shown in Table 1. The thickness of resin layer 20 was 0.6 μm.

[0069]

[0070]

[0071]

[0072] As shown in Table 1, the resin-coated metal sheets 1 of Examples 1 and 2 had a protruding peak height Rpk of 0.46 μm or more, high peel strength against the adhesive resin, and excellent adhesion to the adhesive resin. Furthermore, the adhesive resin that wetted and spread on the resin layer 20 did not contain any air bubbles, and it was shown that a joint material with excellent appearance could be obtained.

[0073] On the other hand, the resin-coated metal sheets of Comparative Examples 1 and 2 had a protruding peak height Rpk of less than 0.46 μm, low peel strength against the adhesive resin, and poor adhesion to the adhesive resin. Furthermore, the resin-coated metal sheet of Comparative Example 1 had air bubbles mixed in the adhesive resin that had spread wet on the resin layer, resulting in a poor appearance when used as a joint material.

[0074] Furthermore, as can be seen from the comparison between Examples 1 and 2 and Comparative Examples 1 and 2, the arithmetic mean height Sa of the resin layer 20 1 This indicates that simply increasing the arithmetic mean height of the resin layer 20 does not improve adhesion to the adhesive resin, and that it is only by controlling the protruding peak height Rpk of the resin layer 20 to 0.46 μm or more that adhesion to the adhesive resin can be improved.

[0075] The resin-coated metal sheet 1 of Example 2 had superior peel strength compared to Example 1. This is thought to be because, as shown in Table 2, Example 2 had a higher roundness ratio compared to Example 1, which allowed the adhesive to wet and spread more uniformly.

[0076] <Reference Experimental Example 1> A cold-rolled sheet (thickness: 0.16 mm) of low-carbon aluminum-killed steel was prepared as the metal base sheet 11 by cold rolling, annealing, and then temper rolling with a roll having an arithmetic mean roughness Ra of 2.5 to 5.5 μm. The sheet was then plated in a pure zinc plating bath at a bath temperature of 50°C and a current density of 30 A / dm 2 A resin-coated metal sheet 1 was obtained by the direct roll coating method in the same manner as in Example 1, except that zinc plating was performed under the conditions of (a) to (c) above, and a zinc plating layer made of pure zinc was formed as the metal plating layer 12. The protruding peak height Rpk of the obtained resin-coated metal sheet 1 was measured in the same manner as in Example 1.

[0077] <Reference Experimental Example 2> A resin-coated metal sheet 1 was obtained in the same manner as in Reference Experimental Example 2, except that an aqueous dispersion containing an olefin-based resin (ethylene-methacrylic acid copolymer) (solid content concentration 44.5 wt%, viscosity 40 mPa s, pH 4.8, MFT 100°C) was used instead of the aqueous dispersion containing an olefin-based resin (ethylene-acrylic acid copolymer), and the protruding peak height Rpk was measured.

[0078] Comparative Example 1: A resin-coated metal sheet was obtained in the same manner as in Reference Experimental Example 1, except that the aqueous dispersion was applied using a bar coater instead of the direct roll coating method, and the protruding peak height Rpk was measured. The coating conditions using the bar coater were a wireless bar coater (Select-Roller / A-Bar, manufactured by OSG System Products Co., Ltd.) with a wireless bar number 0 (OSP-00) and a target film thickness of 1 μm.

[0079] <Reference Comparative Example 2> A resin-coated metal sheet was obtained in the same manner as in Reference Experimental Example 2, except that the aqueous dispersion was applied using a bar coater instead of the direct roll coating method, and the protruding peak height Rpk was measured. The measurement results of Rpk for Reference Experimental Examples 1 and 2 and Reference Comparative Examples 1 and 2, with Reference Comparative Example 1 as the standard, are shown in Table 4.

[0080]

[0081] It was confirmed that Rpk was significantly higher in Reference Experimental Examples 1 and 2, in which the aqueous dispersion was applied by a bar coater, than in Reference Comparative Examples 1 and 2, in which the aqueous dispersion was applied by the direct roll coating method. In contrast to coating with a bar coater, in which the liquid is not lifted up during coating, in the direct roll coating method, the aqueous dispersion is lifted up as shown in Figure 2(a) when the metal substrate 11 is sent out from the roll, which is thought to have enabled the protruding peak height Rpk to be increased.

[0082] DESCRIPTION OF SYMBOLS 1... Resin-coated metal sheet 10... Metal substrate 11... Metal original sheet 12... Metal plating layer 20... Resin layer

Claims

1. A resin-coated metal sheet comprising a metal substrate and a resin layer provided on the metal substrate, wherein the height Rpk of a protruding peak on the surface of the resin layer is 0.46 μm or more.

2. A resin-coated metal sheet according to claim 1, wherein the height Spk of the protruding peaks on the surface of the resin layer is 0.6 μm or more.

3. A resin-coated metal sheet according to claim 1 or 2, wherein the resin layer is made of a resin material containing an olefin-based and / or urethane-based resin.

4. The resin-coated metal sheet according to any one of claims 1 to 3, wherein the arithmetic mean height Sa of the resin layer 1 A resin-coated metal sheet having a thickness of 0.5 μm or more.

5. A resin-coated metal sheet according to any one of claims 1 to 4, wherein the height Rpk of the protruding peaks on the surface of the resin layer is 0.6 μm or more.

6. A resin-coated metal sheet according to any one of claims 1 to 5, wherein the metal substrate comprises an original metal sheet and a zinc-containing metal plating layer, and the resin layer is formed on the metal plating layer.

7. The resin-coated metal sheet according to claim 6, wherein the arithmetic mean height Sa of the surface of the original metal sheet on which the metal plating layer is formed is 2 A resin-coated metal sheet having a thickness of 0.5 μm or more.

8. A method for producing a resin-coated metal sheet according to any one of claims 1 to 7, comprising the steps of applying an aqueous dispersion containing a resin material at a solid content concentration of 15% by weight or more onto the metal substrate by a direct roll coating method, and drying a layer made of the aqueous dispersion to form the resin layer.

9. A method for producing a resin-coated metal sheet according to claim 8, wherein the solid content concentration of the aqueous dispersion is 15% by weight or more and less than 70% by weight, the metal substrate comprises a metal original sheet and a zinc-containing metal plating layer, and the arithmetic mean height Sa of the surface of the metal original sheet on which the metal plating layer is formed is 2 A method for producing a resin-coated metal sheet, wherein the thickness is 0.75 μm or more.

10. A method for producing a resin-coated metal sheet according to claim 8 or 9, wherein the resin material contains an olefin-based and / or urethane-based resin.

Citation Information

Patent Citations

  • Coating metal plate, joiner having the same, and bond breaker tape

    JP2019173544A

  • Developing method and developer carrier

    JP2007033667A

  • Resin-coated metal plate excellent in conductivity, and its manufacturing method

    JP2008273190A

  • Slide member

    JP2020097948A

  • Surface-treated copper foil, copper-clad laminate, and printed wiring board

    JP2021095595A