Composition, substrate laminate, and method for producing substrate laminate

The use of a composition with cationic functional groups and a crosslinking agent in the substrate laminate addresses thermal expansion mismatches, enhancing bonding strength and stability in semiconductor substrate stacks, thereby improving the reliability of hybrid bonding.

WO2024204624A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012850
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for stacking semiconductor substrates to achieve high integration face challenges in thermal expansion mismatch, leading to warping and peeling issues due to the use of adhesives, which can compromise bonding strength and reliability.

Method used

A composition comprising a compound with cationic functional groups, a crosslinking agent, and a polar solvent is used to form a layer with low thermal expansion and high bonding strength, enabling hybrid bonding of substrate stacks by reacting to form a rigid, thermoset film that reduces thermal expansion and enhances electrode bonding.

Benefits of technology

The solution provides a substrate laminate with improved thermal stability and strong bonding between electrodes, effectively addressing the issues of warping and peeling, while maintaining electrical conductivity and reliability over repeated thermal cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012850_03102024_PF_FP_ABST
    Figure JP2024012850_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This composition comprises: a compound (A) having a Si-O bond and a cationic functional group including at least one selected from among a primary nitrogen atom and a secondary nitrogen atom; a crosslinking agent (B) represented by formula (1); and a polar solvent (C), wherein the compound (A) has three Si-O bonds for one Si atom, and in formula (1) which is the crosslinking agent (B), R1 represents a linking group containing at least two aromatic rings or a linking group containing at least one aliphatic ring, each X independently represents a hydrogen atom or an alkyl group having 1-6 carbon atoms, 1 to 4 of X's are hydrogen atoms, and the weight-average molecular weight of X is 200 to 500.
Need to check novelty before this filing date? Find Prior Art

Description

Composition, substrate laminate, and method for manufacturing substrate laminate

[0001] SUMMARY The present disclosure relates to compositions, substrate laminates, and methods for making substrate laminates.

[0002] As electronic devices become smaller, lighter, and more powerful, there is a demand for higher integration of semiconductor chips and the like, in which electrodes are arranged on a substrate. However, it is difficult to fully meet the demand for higher integration simply by miniaturizing circuits. Therefore, in recent years, a method for achieving higher integration by stacking multiple semiconductor substrates to form a multilayer three-dimensional structure has been proposed. Proposed methods for stacking substrates (wafers), chips, and the like (hereinafter sometimes referred to as "substrates, etc.") include a method for directly bonding substrates together (fusion bonding) and a method for adhering substrates together using an adhesive. A method using an adhesive as a hybrid bond for bonding substrates together, where the metal and insulating film surfaces of the substrates are exposed, has also been proposed (see, for example, Patent Documents 1 to 3).

[0003] Patent Document 1: Japanese Patent Application Laid-Open No. 4-132258 Patent Document 2: Japanese Patent Application Laid-Open No. 2010-226060 Patent Document 3: Japanese Patent Application Laid-Open No. 2016-47895

[0004] While the method using an adhesive has the advantage of being able to bond substrates at a lower temperature than fusion bonding, it has the risk of warping or peeling due to strain at the bonding surface caused by the difference in thermal expansion coefficient between the adhesive and the substrate. One possible method for reducing the thermal expansion coefficient of the adhesive is to add inorganic fillers, but the addition of inorganic fillers may reduce the adhesive strength.

[0005] An object of one embodiment of the present disclosure is to provide a composition that has a low coefficient of thermal expansion and provides excellent bonding strength between opposing electrodes when hybrid bonding a substrate laminate.Another embodiment of the present disclosure is to provide a substrate laminate using the composition, and a method for manufacturing the substrate laminate.

[0006] Specific means for solving the above problems include the following aspects.

[0007] <1> A polymerizable composition comprising a compound (A) having a cationic functional group containing at least one selected from a primary nitrogen atom and a secondary nitrogen atom and an Si—O bond, a crosslinking agent (B) represented by the following formula (1), and a polar solvent (C), wherein the compound (A) has three Si—O bonds per one Si atom, and the crosslinking agent (B) represented by the following formula (1) is a compound (A) having a cationic functional group containing at least one selected from a primary nitrogen atom and a secondary nitrogen atom and an Si—O bond, and wherein the compound (A) has three Si—O bonds per one Si atom, and the crosslinking agent (B) is a compound represented by the following formula (1) represented by R 1 represents a linking group containing two or more aromatic rings or a linking group containing one or more aliphatic rings; each X independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and one or more and four or less Xs are hydrogen atoms; and the composition has a weight average molecular weight of 200 or more and 500 or less.

[0008]

[0009] In the formula (1), R 1 represents a linking group containing two or more aromatic rings, and X represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0010] <2> R in the formula (1) 1 is a linking group that is a condensed ring of two or more aromatic rings, or a linking group in which two or more aromatic rings are linked to each other via a bond selected from a single bond and an ether bond. <3> The composition according to <1> or <2>, which is used for connecting wiring in a laminate of two or more substrates having a substrate and wiring.

[0011] <4> A substrate laminate comprising: a first laminate including a first substrate, an electrode on the first substrate, and a layer containing the composition according to any one of <1> to <3>; and a second laminate including a second substrate, an electrode on the second substrate, and a layer made of an inorganic material or a resin, wherein a surface of the first laminate having the electrode faces a surface of the second laminate having the electrode, and the electrode of the first laminate and the electrode of the second laminate, and the layer containing the composition of the first laminate and the layer made of the inorganic material or the resin of the second laminate are directly bonded to each other.

[0012] <5> A method for producing a substrate laminate, comprising: step I of preparing a laminate including a substrate and an electrode; step II of applying the composition according to any one of <1> to <3> to the electrode side surface of the laminate to form a composition layer; step IV of preparing the laminate polished in step III and a laminate separately including an electrode and a layer made of an inorganic material or a resin on a substrate, and stacking the two laminates so that the electrodes on the electrode-containing sides of the prepared two laminates come into contact with each other; and step V of heating and bonding the stacked laminates prepared in step VI.

[0013] According to one embodiment of the present disclosure, it is possible to provide a composition that has a low thermal expansion coefficient and that provides excellent bonding strength between opposing electrodes when hybrid bonding a substrate laminate. According to another embodiment of the present disclosure, it is possible to provide a substrate laminate using the composition, and a method for manufacturing the substrate laminate.

[0014] 1 is a schematic process diagram showing an example of a process for producing a substrate laminate through steps I to V in a method for producing a substrate laminate according to the present disclosure, showing an example of a state in which electrodes of the laminates are brought into contact with each other and superimposed in step IV. FIG. 2 is a schematic process diagram showing an example of a process for producing a substrate laminate through steps I to V in a method for producing a substrate laminate according to the present disclosure, showing an example of a state in which the laminates are bonded together by heating in step V.

[0015] In this disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the upper and lower limits. In numerical ranges described in stages in this disclosure, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another staged numerical range. Furthermore, in numerical ranges described in this disclosure, the upper or lower limit value of that numerical range may be replaced with a value shown in the examples. In this disclosure, a "laminate" refers to a structure having electrodes on a substrate, and a "substrate laminate" refers to a structure in which two or more laminates each having a substrate and an electrode are stacked one on top of the other. In other words, a "substrate laminate" has a structure in which two laminates are bonded via a composition layer formed on the laminate. Components indicated with the same reference numeral in each drawing are the same components. The drawings are schematic, and the dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.

[0016] [Composition] The composition of the present disclosure includes a compound (A) having a cationic functional group containing at least one selected from a primary nitrogen atom and a secondary nitrogen atom and an Si—O bond, a crosslinking agent (B) represented by the following formula (1), and a polar solvent (C), wherein the compound (A) has three Si—O bonds per one Si atom, and the crosslinking agent (B) represented by the following formula (1) is a compound (A) having a cationic functional group containing at least one selected from a primary nitrogen atom and a secondary nitrogen atom and an Si—O bond, and the compound (A) has three Si—O bonds per one Si atom, and the crosslinking agent (B) represented by the following formula (1) is a polar solvent (C), wherein R 1 represents a linking group containing two or more aromatic rings or a linking group containing one or more aliphatic rings; each X independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and one to four of X are hydrogen atoms; and the composition has a weight average molecular weight of 200 or more and 500 or less.

[0017]

[0018] <Compound (A)> Compound (A) in the present disclosure is a compound having a cationic functional group containing at least one selected from a primary nitrogen atom and a secondary nitrogen atom and an Si—O bond, and has three Si—O bonds per molecule. The cationic functional group containing at least one of a primary nitrogen atom and a secondary nitrogen atom contained in compound (A) reacts with crosslinker (B) to form a cured product. The three Si—O bonds contained in compound (A) per molecule contribute to improving the bonding strength with the substrate. In the composition, one type of compound (A) may be used alone, or two or more types may be used in combination.

[0019] The cationic functional group is not particularly limited as long as it can bear a positive charge and contains at least one of a primary nitrogen atom and a secondary nitrogen atom. Compound (A) may also contain a tertiary nitrogen atom in addition to the primary and secondary nitrogen atoms.

[0020] In the present disclosure, a "primary nitrogen atom" refers to a nitrogen atom that is bonded to only two hydrogen atoms and one atom other than a hydrogen atom (e.g., a primary amino group (-NH 2 "Secondary nitrogen atom" refers to a nitrogen atom bonded to only one hydrogen atom and two atoms other than hydrogen atoms (i.e., a nitrogen atom contained in a functional group represented by formula (a) below), or a nitrogen atom (cation) bonded to only two hydrogen atoms and two atoms other than hydrogen atoms. "Tertiary nitrogen atom" refers to a nitrogen atom bonded to only three atoms other than hydrogen atoms (i.e., a nitrogen atom that is a functional group represented by formula (b) below), or a nitrogen atom (cation) bonded to only one hydrogen atom and three atoms other than hydrogen atoms.

[0021]

[0022] In formula (a) and formula (b), * indicates the bonding position to an atom other than a hydrogen atom. The functional group represented by formula (a) is a secondary amino group (-NHR a group; where R aThe functional group represented by the formula (b) (i.e., a tertiary nitrogen atom) may be a functional group constituting a part of a tertiary amino group (—NR b R c group; where R b and R c and each independently represent an alkyl group).

[0023] From the viewpoint of reducing the water absorption rate of the cured product and reducing the amount of outgassing, compound (A) preferably has three Si-O bonds per Si atom, and has two alkyl groups bonded to the oxygen atoms constituting each Si-O bond, and more preferably has an alkyl group bonded to each of the two oxygen atoms bonded to one silicon atom constituting the Si-O bond. The two alkyl groups each independently preferably have 1 to 5 carbon atoms, more preferably 1 or 2, and even more preferably 2.

[0024] The weight average molecular weight of the compound (A) is not particularly limited and may be, for example, 130 or more and 10,000 or less, 130 or more and 5,000 or less, or 130 or more and 2,000 or less.

[0025] In the present disclosure, the weight-average molecular weight of a compound refers to a polyethylene glycol-equivalent weight-average molecular weight measured by gel permeation chromatography (GPC). Specifically, the weight-average molecular weight is calculated using an aqueous solution of sodium nitrate with a concentration of 0.1 mol / L as a developing solvent, a Shodex DET RI-101 analyzer, and two analytical columns (TSKgel G6000PWXL-CP and TSKgel G3000PWXL-CP, manufactured by Tosoh Corporation) to detect the refractive index at a flow rate of 1.0 mL / min, and analysis software (Empower3, manufactured by Waters) using polyethylene glycol / polyethylene oxide as standards.

[0026] Specific examples of compound (A) include compounds having three Si—O bonds and an amino group. Examples of compounds having three Si—O bonds and an amino group include 3-aminoalkylalkoxysilane and N-(2-aminoalkyl)-3-aminoalkyltrimethoxysilane. The alkyl group in the 3-aminoalkylalkoxysilane includes alkyl groups having 2 to 6 carbon atoms, and among these, from the viewpoint of reactivity, ethyl and propyl groups are preferred, with propyl being more preferred. Furthermore, examples of the alkoxy group in the alkoxysilane include alkoxy groups having 1 to 5 carbon atoms, with methoxy and ethoxy groups being preferred, and ethoxy groups being more preferred from the viewpoint of reactivity.

[0027] Specific examples of compound (A) include N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, and hydrolysates thereof. Among these, 3-aminopropyltriethoxymethylsilane, 3-aminopropyltriethoxysilane, etc. are preferred as compound (A), and 3-aminopropyltriethoxymethylsilane is more preferred.

[0028] Since compound (A) has a cationic functional group containing at least one of a primary nitrogen atom and a secondary nitrogen atom, it can strongly bond substrates to each other by electrostatic interaction with functional groups such as hydroxyl groups, epoxy groups, carboxy groups, amino groups, and mercapto groups that may be present on the surface of the substrate, or by forming a covalent bond with the functional group. Furthermore, since compound (A) has a cationic functional group containing at least one of a primary nitrogen atom and a secondary nitrogen atom, it has excellent solubility in polar solvents. Therefore, it has a high affinity with substrates with hydrophilic surfaces such as silicon, and can form a smooth film.

[0029] As the compound (A), a compound having an amino group as a cationic functional group is preferred from the viewpoint of heat resistance, and further, a compound having a primary amino group is preferred from the viewpoint of forming a thermally crosslinked structure such as an amide, an amide-imide, or an imide to further improve heat resistance.

[0030] The ratio of the total number of primary and secondary nitrogen atoms to the number of silicon atoms in compound (A) (total number of primary and secondary nitrogen atoms / number of silicon atoms) is not particularly limited, but is preferably 0.2 or more and 5 or less from the viewpoint of forming a smooth thin film.

[0031] In the compound (A), it is preferable that the molar ratio of the Si element in the molecule to the non-crosslinkable group such as a methyl group bonded to the Si element (non-crosslinkable group / Si element) is less than 2 (satisfying the relationship non-crosslinkable group / Si element<2). By satisfying this condition, it is thought that the crosslinking density of the formed film (crosslinking between Si-O-Si bonds and amide bonds, imide bonds, etc.) can be improved, and the amount of thermal expansion of the obtained cured film can be reduced. The molar ratio of the Si element in the molecule to the non-crosslinkable group such as a methyl group bonded to the Si element (non-crosslinkable group / Si element) can be 1 or less, for example, it can be 0.

[0032] As mentioned above, compound (A) has a cationic functional group containing at least one of a primary nitrogen atom and a secondary nitrogen atom.Here, when compound (A) contains a primary nitrogen atom, the proportion of primary nitrogen atoms in the total nitrogen atoms in compound (A) is preferably 20 mol% or more, more preferably 25 mol% or more, and even more preferably 30 mol% or more.When the proportion of primary nitrogen atoms in the total nitrogen atoms in compound (A) is 20 mol% or more, bonding with functional groups that may be present on the surface of the substrate is formed densely, and the substrates can be bonded more strongly.

[0033] When compound (A) contains a secondary nitrogen atom, the proportion of the secondary nitrogen atoms in all nitrogen atoms in compound (A) is preferably 5 mol % or more and 50 mol % or less, and more preferably 5 mol % or more and 30 mol % or less.

[0034] Compound (A) may contain a tertiary nitrogen atom in addition to a primary nitrogen atom and a secondary nitrogen atom. When compound (A) contains a tertiary nitrogen atom, the proportion of tertiary nitrogen atoms in all nitrogen atoms in compound (A) is preferably 20 mol % or more and 50 mol % or less, and more preferably 25 mol % or more and 45 mol % or less.

[0035] The content of compound (A) in the composition is not particularly limited, as long as the proportion of the primary and secondary nitrogen atoms contained in compound (A) to the total of the primary and secondary nitrogen atoms contained in compound (A) and the primary nitrogen atoms contained in compound (C) is 3 mol % to 95 mol %. From the viewpoint of the balance between the thermal expansion coefficient and the bonding strength, the proportion is preferably 5 mol % to 75 mol %, and more preferably 10 mol % to 50 mol %.

[0036] Since the compound (A) has an uncrosslinked cationic functional group, when the compound (A) is contained as a component of the bonding portion between the substrates without containing the crosslinking agent (B) described below, the crosslinking density is low and the heat resistance is insufficient. On the other hand, in the composition layer formed by the composition of the present disclosure, the cationic functional group of the compound (A) reacts with the carboxyl group or the like of the crosslinking agent (B) to form a covalent bond, thereby increasing the crosslinking density and resulting in a cured product with high heat resistance.

[0037] <Crosslinking Agent (B)> The crosslinking agent (B) in the present disclosure has a structure represented by the following formula (1), in which R 1 represents a linking group containing two or more aromatic rings or a linking group containing one or more aliphatic rings, each X independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and one to four of X are hydrogen atoms, and the compound has a weight average molecular weight of 200 to 500.

[0038]

[0039] That is, the crosslinking agent (B) is R 1 or a structure in which four -C(=O)OX groups are bonded to a linking group containing two or more aromatic rings represented by R 1The compound has a structure in which four —C(═O)OX groups are bonded to a linking group containing one or more aliphatic rings represented by the following formula:

[0040] R in formula (1) 1 represents a linking group containing two or more aromatic rings, and by containing two or more aromatic rings, the main skeleton has a ring structure and is rigid, and in addition, the two or more aromatic rings form a relatively short molecular chain, which shortens the distance between the crosslinking points formed at both ends of the crosslinking agent (B), and is thought to suppress the thermal expansion of the cured film obtained by curing the composition. 1 has a structure in which two or more aromatic rings are linked by a single bond, an ether bond, a carbonyl bond, an alkylene group (including acetylene) having 1 to 2 carbon atoms which may be substituted with a hetero atom, a bond via a sulfur atom, or the like, or the two or more aromatic rings can have a structure in which the two or more aromatic rings are condensed rings. 1 Examples of such a compound include the following structures: In the following structures, * indicates the bonding site with the -C(=O)OX group.

[0041]

[0042] The linking group R in formula (1) containing one or more aliphatic rings 1 Examples of such a compound include the following structures: In the following structures, * indicates the bonding site with the -C(=O)OX group.

[0043]

[0044] In particular, from the viewpoint of suppressing the thermal expansion of the cured film, it is believed that the short distance between the two aromatic rings shortens the distance between the imide bonds present at both ends, improves the crosslink density, and suppresses the thermal expansion of the cured film. From this viewpoint, it is preferable that R 1 is preferably a linking group which is a condensed ring of two or more aromatic rings, or a linking group in which two or more aromatic rings are linked to each other via a structure selected from a single bond and an ether bond.

[0045] The two or more aromatic rings in the crosslinking agent (B) are not particularly limited as long as they are ring structures exhibiting aromaticity, and examples thereof include benzene-based aromatic rings such as benzene rings, aromatic heterocycles such as pyridine rings and thiophene rings, and non-benzene-based aromatic rings such as indene rings and azulene rings. Furthermore, the two or more aromatic rings may be condensed with each other to form a naphthalene ring, an anthracene ring, or a perylene ring. The one or more aliphatic rings in the crosslinking agent (B) are not particularly limited as long as they are aliphatic rings, and examples thereof include a cyclohexane ring, a cyclobutane ring, and a cyclopentane ring.

[0046] The ring structure that compound (B) has in the molecule is R 1 However, when two or more aromatic rings are bonded via a linking group, a benzene ring is preferred, and a naphthalene ring formed by condensing two or more aromatic rings is preferred. From the viewpoint of further improving the heat resistance of the cured product, R 1 is preferably an embodiment in which two benzene rings are bonded together via the above-mentioned linking group, or a naphthalene ring.

[0047] As shown in formula (1), the crosslinking agent (B) has R 1 In formula (1), X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Of the four Xs, it is preferable that one to four are hydrogen atoms. That is, it is preferable that one to four of the -C(=O)OX groups are -C(=O)OH groups (hereinafter also referred to as "-COOH groups"). When the crosslinking agent (B) has one to four -COOH groups in the molecule, the solubility of the crosslinking agent (B) in the composition is further improved. In the composition, one type of crosslinking agent (B) may be used alone, or two or more types may be used in combination.

[0048] In the crosslinking agent (B), X in the -C(=O)OX group is a hydrogen atom or an alkyl group having from 1 to 6 carbon atoms, and among these, X is preferably a hydrogen atom, a methyl group, an ethyl group, or a propyl group. Note that X in the -C(=O)OX group may be the same or different.

[0049] When the crosslinking agent (B) has one to four -COOH groups in the molecule, the crosslinking agent (B) can react efficiently with the above-mentioned compound (A). In particular, the crosslinking agent (B) is preferably a compound having two to four -COOH groups in the molecule, where X is a hydrogen atom, and more preferably a compound having two or three -COOH groups in the molecule. When the crosslinking agent (B) has two to four -COOH groups in the molecule, the solubility in the composition is further improved. In other words, the crosslinking agent (B) can be said to have the structure of the following compound in which the carboxylic acid in formula (1) is half-esterified. The following example is R 1 The examples shown are those in which two aromatic rings are bonded by an ether group, those in which two aromatic rings are bonded by a single bond, and those in which two aromatic rings are condensed into a naphthalene ring.

[0050]

[0051] The crosslinking agent (B) which is the half-esterified compound can be produced, for example, by mixing a carboxylic acid anhydride, which is an anhydride of a carboxylic acid compound such as those shown below, with an alcohol solvent and ring-opening the carboxylic acid anhydride.

[0052]

[0053] The following example is 1 is bonded via a substituent containing one or more alicyclic hydrocarbon groups.

[0054]

[0055] The crosslinking agent (B) which is the half-esterified compound can be produced, for example, by mixing a carboxylic acid anhydride, which is an anhydride of a carboxylic acid compound such as those shown below, with an alcohol solvent and ring-opening the carboxylic acid anhydride.

[0056]

[0057] The weight average molecular weight of the crosslinking agent (B) is not particularly limited. For example, the weight average molecular weight of the crosslinking agent (B) is 200 or more and 500 or less, or may be 200 or more and 450 or less, or may be 250 or more and 450 or less. When the weight average molecular weight of the crosslinking agent (B) is within the above range, the crosslinking density in the cured film of the composition is improved, and the thermal expansion coefficient of the cured film is further reduced. The weight average molecular weight of the crosslinking agent (B) can be measured by GPC method in the same way as the method for the compound (A) described above.

[0058] <Content ratio of compound (A) and crosslinking agent (B) during composition preparation> That is, the composition of the present disclosure contains the compound (A) and crosslinking agent (B) in the polar solvent (C) described below. By introducing the compound (A) into both ends of the crosslinking agent (B), the composition can obtain a rigid cured product with a high crosslink density. The content ratio (charge ratio) of the compound (A) to the crosslinking agent (B) in the composition is preferably a molar ratio of compound (A):crosslinking agent (B) of 2:0.9 to 1.1, more preferably a molar ratio of 2:1, from the viewpoint of minimizing the amount of unreacted crosslinking agent (B) remaining. It is believed that the compound (A) and crosslinking agent (B) exist in the polar solvent (C) as a mixture in which the amino group of the compound (A) and the carboxyl group of the crosslinking agent (B) form a salt. As will be described later, the composition of the present disclosure is considered to contain, as a structural unit, a reaction product of the compound (A) and the crosslinking agent (B) as exemplified below, when a composition layer is formed and then heat-cured. This reaction product forms a cured film having a low coefficient of thermal expansion, and therefore the composition is useful for various applications such as adhesives.

[0059]

[0060]

[0061] <Polar Solvent (C)> The composition of the present disclosure contains a polar solvent (C). In the present disclosure, "polar solvent" refers to a solvent having a relative dielectric constant of 5 or more at room temperature (25°C). When the composition contains the polar solvent (C), the solubility of each component in the composition is improved. The polar solvent may be used alone or in combination of two or more.

[0062] Specific examples of the polar solvent (C) include protic solvents such as water and heavy water; alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutyl alcohol, isopentyl alcohol, cyclohexanol, ethylene glycol, propylene glycol, 2-methoxyethanol, 2-ethoxyethanol, benzyl alcohol, diethylene glycol, triethylene glycol, and glycerin; ethers such as tetrahydrofuran and dimethoxyethane; aldehydes and ketones such as furfural, acetone, ethyl methyl ketone, and cyclohexanone; acid derivatives such as ethyl acetate, butyl acetate, ethylene carbonate, propylene carbonate, formaldehyde, N-methylformamide, N,N-dimethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and hexamethylphosphoric acid amide; nitriles such as acetonitrile and propionitrile; and nitro compounds such as nitromethane and nitrobenzene; and sulfur compounds such as dimethyl sulfoxide. The polar solvent (C) preferably contains a protic solvent, more preferably contains water, and further preferably contains ultrapure water as the water.

[0063] The content of the polar solvent (C) in the composition is not particularly limited, and may be, for example, 1.0 mass% or more and 99.99896 mass% or less, or 40 mass% or more and 99.99896 mass% or less, relative to the entire composition.

[0064] In the production of the substrate laminate of the present disclosure described below, the boiling point of the polar solvent (C) is preferably 150°C or lower, more preferably 120°C or lower, from the viewpoint of volatilizing the polar solvent (C) by heating when forming the composition layer and reducing the amount of residual solvent in the composition layer.

[0065] Although the mechanism of action of the composition of the present disclosure is unclear, it is believed that a cationic functional group containing at least one selected from a primary nitrogen atom and a secondary nitrogen atom having three SiO bonds at its terminal reacts with a -C(=O)OX group, preferably a -COOH group, at the terminal of the crosslinking agent (B), resulting in a reaction product having three SiO bonds per Si atom, which increases the crosslink density after curing. Furthermore, since the main skeleton of the main chain of the crosslinking agent (B) that forms the imide bond is formed of a relatively short molecular chain having a ring structure, the distance between the crosslinking points is shortened, and therefore, the composition of the present disclosure forms a rigid thermosetting film by removing the polar solvent (C) through heating. Therefore, the combined functions of these two functions allow the composition to form a rigid thermosetting film, even when used, for example, to bond substrate laminates. Therefore, even when a thermal cycle test in which heating and cooling are repeated after bonding the substrate laminates is performed, it is believed that disconnection of wiring between substrates due to thermal expansion and thermal contraction is also suppressed.

[0066] <Production of Composition> The composition of the present disclosure can be produced by a known method. For example, the composition may be produced by a production method including: step a) mixing 3-aminopropyltriethoxysilane (hereinafter also referred to as "3APTES"), which is the compound (A), with water to obtain solution A containing a hydrolyzate of 3APTES; step b) adding ethanol to oxydiphthalic acid (hereinafter also referred to as "ODPA"), which is a precursor of crosslinking agent (B), and heating and refluxing to prepare solution B in which an ODPA half ester is dissolved; and step c) combining solution A, solution B, 1-propanol, which is the polar solvent (C), and water. By performing step c, the composition of the present disclosure containing compound (A), crosslinking agent (B), and polar solvent (C) can be obtained. Note that the method for producing the composition is not limited to the above. The production of the composition will be described in detail in the Examples.

[0067] <Other Components> The composition of the present disclosure may contain known additives, such as an acid having a carboxy group and a weight average molecular weight of 46 to 195, a base having a nitrogen atom and no ring structure and a weight average molecular weight of 17 to 120, and a solvent other than the polar solvent (C).

[0068] The composition may contain a solvent other than the polar solvent (C). Examples of the solvent other than the polar solvent include normal hexane.

[0069] The composition may also contain benzotriazole or a derivative thereof, for example to inhibit copper corrosion.

[0070] The pH of the composition is not particularly limited, but is preferably 2.0 or more and 12.0 or less. When the pH of the composition is 2.0 or more and 12.0 or less, damage to the substrate by the composition is suppressed. The composition preferably has a sodium and potassium content of 10 mass ppb or less on an elemental basis. When the sodium or potassium content is 10 mass ppb or less on an elemental basis, it is possible to suppress the occurrence of problems in the electrical characteristics of the semiconductor device, such as transistor malfunction.

[0071] When the composition contains components other than the compound (A), the crosslinking agent (B), and the polar solvent (C), the total content of the compound (A) and the crosslinking agent (B) is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more of the total mass of nonvolatile components in the composition. In the present disclosure, "nonvolatile components" refers to components other than components (such as solvents) that are removed when the composition becomes a cured product.

[0072] (Use of Composition) The use of the composition of the present disclosure is not particularly limited. Since the composition contains many crosslinking points and has a rigid main skeleton, when a cured product is formed using the composition, a cured product that is less likely to undergo thermal expansion is obtained. From this perspective, the composition of the present disclosure can be suitably used for wiring bonding in a laminate of two or more layers having a substrate and wiring.

[0073] The composition of the present disclosure has a low coefficient of thermal expansion, and when hybrid bonding substrate laminates, it forms a cured product with excellent bonding strength between opposing electrodes. Therefore, the use of the composition of the present disclosure is not limited to bonding wiring, and it can be used for bonding various components, including the manufacture of semiconductor devices. Examples of uses of the composition of the present disclosure include bonding two or more hard components together, such as forming a composition layer on or between substrates to bond them to other components, filling voids such as "cracks" formed in components, and forming an adhesive layer while filling gaps on a substrate.

[0074] [Substrate Laminate] The substrate laminate of the present disclosure is a substrate laminate obtained using the composition of the present disclosure. The substrate laminate of the present disclosure includes a first substrate, a first laminate including an electrode on the first substrate, and a layer (composition layer) containing the composition of the present disclosure; and a second substrate, a second laminate including an electrode on the second substrate, and a layer made of an inorganic material or a resin, wherein the side of the first laminate having the electrode faces the side of the second laminate having the electrode, and the electrode of the first laminate and the electrode of the second laminate, and the composition layer of the first laminate and the layer made of the inorganic material or a resin of the second laminate are directly bonded. The substrate laminate of the present disclosure can be obtained, for example, by the manufacturing method of the substrate laminate of the present disclosure described below.

[0075] [Method for Manufacturing Substrate Laminate] A method for manufacturing a substrate laminate according to the present disclosure (hereinafter sometimes simply referred to as the "manufacturing method of the present disclosure") includes the steps of: Step I of preparing a laminate including a substrate and an electrode; Step II of applying the composition of the present disclosure to the electrode side of the laminate to form a composition layer; Step IV of preparing the laminate polished in Step III and a separate laminate including an electrode and a layer made of an inorganic material or a resin on a substrate, and stacking the two laminates so that the electrodes of the two laminates are in contact with each other; and Step V of heating and bonding the stacked laminates prepared in Step VI. The method for manufacturing a substrate laminate according to the present disclosure may be a method of bonding the electrode sides of the laminate prepared in Step I with another separately prepared laminate to obtain a substrate laminate, or may be a method of bonding the electrode sides of two or more laminates prepared in Step I to obtain a substrate laminate. The composition of the present disclosure is suitable for bonding laminates having electrodes on the substrates, but it goes without saying that it can also be used to bond substrates that do not have electrodes.

[0076] (Step I) Step I is a step of preparing a laminate including a substrate and an electrode.

[0077] (Step II) Step II is a step of applying the composition of the present disclosure to the electrode side surface of the laminate prepared in Step I to form a composition layer. There are no particular limitations on the method of applying the composition of the present disclosure to the electrode side of the substrate. The composition of the present disclosure contains a polar solvent and can be adjusted to an appropriate viscosity, so the composition can be applied by a coating method. Note that in Steps I and II, the procedure for producing a pair of substrates is not particularly limited, and the order in which the electrode and composition layer are formed on the substrate is arbitrary.

[0078] The heating temperature of the composition for forming a film applied to the surface of a substrate is preferably 100°C to 450°C, more preferably 150°C to 450°C, and even more preferably 180°C to 400°C. The aforementioned temperature refers to the surface temperature of the composition layer applied to the surface. By heating the composition layer, the solvent in the composition layer is removed. Furthermore, the components in the composition layer react to obtain a cured product, and a cured film of the composition containing the cured product is formed.

[0079] The pressure when heating the semi-composition layer is not particularly limited, and is preferably an absolute pressure above atmospheric pressure of 17 Pa or less. The absolute pressure is more preferably 1,000 Pa or more but not more than atmospheric pressure, even more preferably 5,000 Pa or more but not more than atmospheric pressure, and particularly preferably 10,000 Pa or more but not more than atmospheric pressure.

[0080] The composition layer can be heated by a conventional method using a furnace or a hot plate. Examples of furnaces that can be used include SPX-1120 manufactured by APEX Corporation and VF-1000LP manufactured by Koyo Thermo Systems Co., Ltd. The composition layer can be heated in air or in an inert gas atmosphere (nitrogen gas, argon gas, helium gas, etc.).

[0081] The heating time for the composition layer to form a film on the surface of the substrate is not particularly limited, and is, for example, 3 hours or less, preferably 1 hour or less. The lower limit of the heating time is not particularly limited, and can be, for example, 5 minutes.

[0082] For the purpose of shortening the heating time, the composition layer for forming the film applied to the surface of the substrate may be irradiated with ultraviolet (UV) rays. Preferred examples of ultraviolet rays include ultraviolet light with a wavelength of 170 nm to 230 nm, excimer light with a wavelength of 222 nm, and excimer light with a wavelength of 172 nm. It is also preferred to irradiate with ultraviolet rays in an inert gas atmosphere.

[0083] Whether or not the composition layer has cured can be confirmed, for example, by measuring the peak intensity of specific bonds and structures by FT-IR (Fourier transform infrared spectroscopy). Examples of specific bonds and structures include bonds and structures generated by a crosslinking reaction. For example, when an amide bond, an imide bond, or the like is formed, it can be determined that the composition layer for forming a film has cured, and this can be confirmed by measuring the peak intensity derived from these bonds, structures, and the like by FT-IR. An amide bond has a peak intensity of about 1650 cm -1 and approximately 1520 cm -1 The imide bond can be confirmed by the presence of a vibration peak at approximately 1770 cm -1 and approximately 1720 cm -1 This can be confirmed by the presence of a vibration peak.

[0084] The surface of the cured composition layer may be planarized, as will be described in detail in the subsequent step III.

[0085] From the viewpoint of increasing the bonding strength between the substrate and other components, such as other substrates, the composition layer formed on the substrate preferably has a functional group capable of forming a chemical bond on the surface of the composition layer opposite the substrate. Examples of such functional groups include amino groups, epoxy groups, vinyl groups, and silanol groups (Si—OH groups). From the viewpoint of heat resistance, silanol groups are preferred. These functional groups may be formed by surface treatment after the formation of the composition layer, or by treatment with a silane coupling agent. Alternatively, compounds containing these functional groups may be mixed into a composition for forming a semiconductor film. Whether or not the surface of the composition layer contains silanol groups can be evaluated by surface analysis of the bonding layer using time-of-flight secondary ion mass spectrometry (TOF-SIMS). Specifically, whether or not the surface of the bonding layer contains silanol groups can be evaluated using a TOF-SIMS PHI nanoTOFII (ULVAC-PHI, Inc.) based on the presence or absence of a peak at a mass-to-charge ratio (m / Z) of 45.

[0086] When an electrode is provided on the surface of the substrate on the side facing the composition layer, from the viewpoint of improving bonding strength and suppressing variations in the thickness of the composition layer, the thickness of the composition layer is preferably 0.001 μm to 8.0 μm, more preferably 0.03 μm to 6.0 μm, and even more preferably 0.05 μm to 5.0 μm. A composition layer thickness of 0.001 μm or more can increase the bonding strength when bonding the substrate to another member via the composition layer. A bonding layer thickness of 8.0 μm or less can suppress variations in the thickness of the composition layer when the composition layer is formed on a large-area substrate.

[0087] When no electrode is provided on the surface of the substrate on the side of the composition layer, from the viewpoint of improving the bonding strength and suppressing variations in the thickness of the composition layer, the thickness of the composition layer is preferably 0.001 μm or more and less than 1.0 μm, more preferably 0.01 μm to 0.8 μm, and even more preferably 0.03 μm to 0.6 μm.

[0088] (Step III) Step III is a step of polishing the side of the laminate obtained in Step II that has the composition layer. That is, in Step III, a film made of the composition is formed on the electrode by applying the composition to the substrate, and therefore the composition layer (composition film) on the electrode is removed. This removes the composition applied to the electrode surface, exposing the electrode. Also, when the laminate obtained in Step II is superimposed on a separately prepared substrate comprising an electrode and a layer made of an inorganic material or resin, it is preferable to polish and remove the layer made of an inorganic material or resin on the electrode from the separately prepared substrate comprising an electrode and a layer made of an inorganic material or resin. Examples of methods for removing the composition layer applied to the electrode surface include flycutting, chemical mechanical polishing (CMP), plasma dry etching, and the like. One removal method may be used alone, or two or more methods may be used in combination. For example, a surface planer (DFS8910 (manufactured by Disco Corporation)) or the like may be used in the flycutting method. When CMP is used, the slurry may be, for example, a slurry containing silica or alumina, which is generally used for polishing resins, or a slurry containing hydrogen peroxide and silica, which is used for polishing metals.When plasma dry etching is used, fluorocarbon plasma, oxygen plasma, etc. may be used.

[0089] When the composition layer on the electrode surface is removed to expose the electrode, a reduction treatment of the oxide on the electrode surface may be performed, if necessary. Examples of reduction treatment methods include heating the substrate at 100°C to 300°C in an acid atmosphere such as formic acid, or heating the substrate in a hydrogen atmosphere. For example, when step III is performed by CMP, the electrode and the composition layer are reduced in thickness by CMP polishing, but the electrode containing copper, which is softer than the composition layer, is polished more, and a step may occur after polishing (see FIG. 1(A)). However, in the manufacturing method of the present disclosure, even if a step occurs, the step is eliminated by the subsequent steps IV and V, as described below, and suitable conduction between the electrodes can be achieved.

[0090] (Step IV) Step IV involves preparing the laminate polished in Step III and a separately prepared laminate, and stacking the two laminates so that the electrodes of the two laminates are in contact with each other. One of the two laminates is a laminate having an electrode and a composition layer on a substrate, while the other may be a separately prepared laminate or a laminate having an electrode and a composition layer on a substrate. Figure 1(A) is a schematic cross-sectional view showing the state of the two laminates stacked after Step IV. The laminate has an electrode 14 and a composition layer 16 on a substrate 12. Due to the polishing in Step III, the electrode 14 is slightly thinner than the composition layer 16, resulting in a small gap between the stacked electrodes 14.

[0091] (Step V) Step V is a step of heating and bonding the stacked laminates prepared in step VI. In step V, the electrode surfaces of a pair of laminates are brought into contact with each other and temporarily fixed, and the temporarily fixed pair of laminates are heated to harden the composition and bond the laminates to each other. The heating temperature can be appropriately selected depending on the structure of the substrate and the formulation of the composition. The heating temperature can be, for example, 100°C to 400°C, preferably 150°C to 350°C, and more preferably 150°C to 250°C.

[0092] An example of a method for manufacturing a substrate laminate according to the present disclosure will be described in detail with reference to Figure 1. Figure 1(A) is a schematic cross-sectional view showing an embodiment in which a composition layer 16 is formed on a substrate 12 on which an electrode 14 is arranged, and the electrode 14 sides of a pair of substrates 12 on which the composition layer 16 is formed are temporarily bonded. (Step III) In Figure 1(A), the thickness of the composition layer 16 is slightly greater than the thickness of the electrode 14. Note that Figure 1(A) shows an enlarged view of the step between the electrode 14 and the composition layer 16.

[0093] 1(B) is a schematic cross-sectional view showing a substrate laminate 20 obtained by heating a pair of temporarily bonded substrates to harden the composition layer 16 and then permanently bonding the pair of substrates. (Step V) FIG. 1(B) shows an example of the substrate laminate 20 after heating. Heating promotes hardening of the composition layer 16, removing the polar solvent (C), and increasing the density of the crosslinked structure, causing slight thermal shrinkage in the composition layer 16, resulting in a thickness of the composition layer 16 that is slightly thinner than before heating. Meanwhile, the copper electrode 14 expands slightly due to the heat, reducing the step between the electrode 14 and the composition layer 16. The pair of substrates are bonded by the composition layer, and the electrodes 14 are brought into close contact with each other, enabling electrical conduction between the electrodes 14 of the substrate laminate 20.

[0094] The size of the electrodes 14 hardly changes even when the substrate laminate obtained after bonding is heated. In the composition layer 16 using the composition of the present disclosure, the cured product undergoes little thermal expansion or thermal contraction when the substrate laminate obtained after bonding is heated, so that voids are unlikely to occur between a pair of electrodes 14, and stable conduction can be maintained.

[0095] <Substrate> The material of the substrate is not particularly limited, and may be any material that is commonly used. Examples of the substrate material include inorganic materials, organic materials, and composites thereof. Specific examples of inorganic materials include semiconductors such as Si, InP, GaN, GaAs, InGaAs, InGaAlAs, SiGe, and SiC; boron silicate glass (Pyrex (registered trademark)); quartz glass (SiO 2 ), sapphire (Al 2 O 3 ), ZrO 2 , Si 3 N 4 , AlN, MgAl 2 O 4 Oxides, carbides or nitrides of BaTiO 3 , LiNbO 3 , SrTiO 3 , LiTaO 3Examples of the organic material include: piezoelectric or dielectric materials such as titanium, titanium dioxide, titanium carbide ...

[0096] The substrate may have a multilayer structure. Examples of multilayer substrate structures include a structure in which an inorganic layer such as silicon oxide, silicon nitride, or SiCN (silicon carbonitride) is formed on the surface of a silicon substrate or the like; a structure in which an organic layer such as polyimide resin, polybenzoxazole resin, imide-crosslinked siloxane resin, epoxy resin, epoxy-modified siloxane, parylene resin, cyclotene (Dow, Chem), or phenolic resin is formed on the surface of a silicon substrate or the like; and a structure in which a composite of an inorganic material and an organic material is formed on a silicon substrate. Alternatively, the substrate may be a low-k film formed by a CVD method, a sol-gel method, or an organic polymer coating method. Films formed by a CVD method include Black Diamond (Applied Materials), films formed by a sol-gel method include organic crosslinked siloxanes such as ethylene-crosslinked siloxanes and ethane-crosslinked siloxanes, and films formed by an organic polymer coating method include resins such as SiLK (trade name: Dow Chemical), Aurora, and fluorinated polyimide. Furthermore, photosensitive resins such as photosensitive polyimide, photosensitive benzocyclobutene, and photosensitive cyclotene (benzocyclobutene) may also be used.

[0097] The main applications of each material applied to the substrate are as follows: Substrates using Si are used for semiconductor memory, LSI stacking, CMOS image sensors, MEMS sealing, optical devices, LEDs, etc. SiO 2Substrates using InGaAlAs, InGaAs, and InP are used for optical devices, etc. Substrates using InGaAlAs, GaAs, and GaN are used for LEDs, etc.

[0098] The laminate prepared in step I may have an electrode on at least one surface of the substrate, or may have electrodes on both surfaces of the substrate. As described above, the composition of the present disclosure is suitable for bonding laminates having electrodes on the substrates, but it goes without saying that it can also be used suitably for bonding substrates having no electrodes.

[0099] The surface of the substrate (at least the surface in contact with another laminate) preferably has at least one group selected from the group consisting of a hydroxyl group, an epoxy group, a carboxyl group, an amino group, and a mercapto group, which can further increase the bonding strength with the layer of the cured product of the composition.

[0100] A surface having hydroxyl groups can be obtained by subjecting the surface of the substrate to surface treatment such as plasma treatment, chemical treatment, or ozone treatment.

[0101] A surface having an epoxy group, a carboxy group, an amino group, or a mercapto group can be obtained by subjecting the surface of the substrate to a surface treatment using a silane coupling agent having an epoxy group, a carboxy group, an amino group, or a mercapto group.

[0102] At least one selected from the group consisting of a hydroxyl group, an epoxy group, a carboxy group, an amino group, and a mercapto group is preferably in a state of being bonded to an element contained in the substrate, more preferably in a state of being bonded to at least one element selected from the group consisting of Si, Al, Ti, Zr, Hf, Fe, Ni, Cu, Ag, Au, Ga, Ge, Sn, Pd, As, Pt, Mg, In, Ta, and Nb, and even more preferably in the form of a silanol group containing a hydroxyl group (Si—OH group).

[0103] The thickness of the substrate is preferably 0.5 μm to 1 mm, more preferably 1 μm to 900 μm, and even more preferably 2 μm to 900 μm. When there are multiple substrates, the above thickness is the thickness of each substrate, and they may be the same or different.

[0104] The shape of the substrate is not particularly limited. For example, when the substrate is a silicon substrate, it may be a silicon substrate on which an interlayer insulating layer (low-k film) is formed. The substrate may have fine grooves (recesses), fine through-holes, etc. formed therein.

[0105] The laminate used in the production method of the present disclosure may further include a substrate that is not in contact with the composition layer. Preferred materials and other aspects of the substrate that is not in contact with the composition layer are the same as those of the substrate described above.

[0106] <Electrode> Examples of materials for the electrode include copper, solder, tin, gold, silver, aluminum, cobalt, ruthenium, etc. When forming an electrode on a substrate, examples of methods for forming the electrode include electrolytic plating, electroless plating, sputtering, and an inkjet method.

[0107] <Composition Layer> The composition layer is a layer obtained from the composition of the present disclosure, and contains the compound (A), crosslinking agent (B), and polar solvent (C) described above, and is a layer that is cured by heating. The composition that forms the composition layer is the composition of the present disclosure described above. Preferred physical properties of the composition layer will be described below.

[0108] <Coefficient of Linear Thermal Expansion in the Thickness Direction> The composition layer in the substrate laminate formed from the composition of the present disclosure preferably has a coefficient of linear thermal expansion in the thickness direction (hereinafter also referred to as CTE) of -10 ppm / K or more and 100 ppm / K or less. The CTE of the composition layer can be measured by the following method. A composition containing a polar solvent (C) is formed into a film on a Si substrate and cured at 200°C for 1 hour to produce a composition layer. Then, using an ellipsometer with a stage heating mechanism (manufactured by Nippon Semilab Co., Ltd.), the sample composition layer is heated from 30°C to 350°C under a nitrogen atmosphere, and the sample is then allowed to cool naturally to room temperature (25°C). Thereafter, the sample is again heated from 30°C to 350°C under a nitrogen atmosphere, and the film thickness expansion amount of the composition layer is measured. The CTE is calculated from the film thickness expansion amount using the following formula. CTE = [(film thickness at 150°C) - (film thickness at 30°C)] / (film thickness at 30°C) / 120K The CTE of the composition layer is preferably -10 ppm / K or more and 100 ppm / K or less, more preferably 60 ppm / K or less, and even more preferably 30 ppm / K or less. The composition layer formed from the composition of the present disclosure preferably satisfies the above physical properties.

[0109] In the method for manufacturing a substrate laminate according to the present disclosure, in step III, the surface energy of the interface of the joint in the substrate laminate during temporary bonding before the actual bonding by heating is 0.05 J / m 2 It is preferable that the surface energy of the interface of the bonded portion in the substrate laminate after the main bonding treatment by heating in step III is 1 J / m or more. 2 It is preferable that the concentration exceeds 2.5 (J / m 2 ) or more is more preferable.

[0110] The surface energy (bonding strength) of the interface between the electrode and composition layers in the substrate laminate can be determined by a blade insertion test according to the method described in non-patent document M. P. Maszara, G. Goetz, A. Cavigila, and J. B. Mckitterick, Journal of Applied Physics, 64 (1988) 4943-4950. A blade with a thickness of 0.1 mm to 0.3 mm is inserted into the interface between the electrodes and composition layers in a substrate laminate before or after heat treatment, and the distance from the blade edge to the laminate peeled off is measured using an infrared light source and an infrared camera. Thereafter, the surface energy can be determined based on the following formula: γ=3×10 9 ×t b 2 ×E 2 ×t 6 / (32 x L 4 ×E×t 3 ) where γ is the surface energy (J / m 2 ), t b represents the blade thickness (m), E represents the Young's modulus (GPa) of the substrate such as a silicon substrate included in the laminate, t represents the thickness (m) of the substrate in the laminate, and L represents the distance (m) from the blade tip to peel the laminate.

[0111] (Examples of Laminate Structure of Substrate Laminate) Examples of laminate structures for various uses of the substrate laminate obtained by the method for producing a substrate laminate of the present disclosure are shown below. Note that the bonding layer in the laminate structures exemplified below is used to mean a layer in a bonded state containing at least one material selected from the group consisting of inorganic materials and resins, in addition to a composition layer formed from the composition of the present disclosure. For MEMS packaging: Si / bonding layer / Si, SiO 2 / Joining layer / Si, SiO 2 / Joining layer / SiO 2 , Cu / bonding layer / Cu, for microchannel; PDMS / bonding layer / PDMS, PDMS / bonding layer / SiO 2 , for CMOS image sensors; SiO 2 / Joining layer / SiO 2 , Si / bonding layer / Si, SiO 2 / Bonding layer / Si, for through silicon via (TSV); SiO2 (with Cu electrode) / bonding layer / SiO 2 (with Cu electrode), Si (with Cu electrode) / bonding layer / Si (with Cu electrode), for optical devices: (InGaAlAs, InGaAs, InP, GaAs) / bonding layer / Si, for LEDs: (InGaAlAs, GaAs, GaN) / bonding layer / Si, (InGaAlAs, GaAs, GaN) / bonding layer / SiO 2 , (InGaAlAs, GaAs, GaN) / bonding layer / (Au, Ag, Al), (InGaAlAs, GaAs, GaN) / bonding layer / sapphire.

[0112] According to the method for producing a substrate laminate of the present disclosure, by using the composition of the present disclosure, opposing electrodes in the laminate are firmly bonded to each other via a cured product having a low thermal expansion coefficient and a rigidity. Furthermore, since the cured composition layer has a low thermal expansion coefficient and rigid physical properties, stable bonding can be achieved over a long period of time even under conditions in which the substrate laminate is repeatedly exposed to heat. Therefore, the substrate laminate obtained by the production method of the present disclosure can be used, for example, in various applications requiring thermal stability over a long period of time.

[0113] The present disclosure will be specifically described below using examples, but the present disclosure is not limited to these examples. In the following, ultrapure water (Milli-Q water manufactured by Millipore, resistivity 18 MΩ cm (25°C) or less) was used as "water." Each evaluation was performed using the following method.

[0114] <Coefficient of Linear Thermal Expansion in the Thickness Direction: CTE> The CTE of the composition layer was measured by the following method. A composition was formed on a Si substrate and cured at 200°C for 1 hour to produce a composition layer. Then, using an ellipsometer with a stage heating mechanism (manufactured by Nippon Semilab Co., Ltd.), the composition layer sample was heated from 30°C to 350°C under a nitrogen atmosphere, and the sample was allowed to cool naturally to room temperature (25°C). Thereafter, the sample was heated again from 30°C to 350°C under a nitrogen atmosphere, and the film thickness expansion of the composition layer was measured. The CTE was calculated from the film thickness expansion using the following formula: CTE = [(film thickness at 150°C) - (film thickness at 30°C)] / (film thickness at 30°C) / 120K

[0115] <Bonding strength between electrodes> In the manufacturing method of the substrate laminate, the surface energy of the joint interface of a set of laminates at the time of temporary bonding before the actual bonding by heating, and the surface energy of the joint interface of a set of laminates after the actual bonding process by heating were measured and used as a guide for the bonding strength.

[0116] The surface energy (bonding strength) of the interface at the joint between the electrodes of the laminate was determined by a blade insertion test according to the method described in non-patent document M. P. Maszara, G. Goetz, A. Cavigila, and J. B. Mckitterick, Journal of Applied Physics, 64 (1988) 4943-4950. A blade with a thickness of 0.1 mm to 0.3 mm was inserted into the interface at the joint between a pair of laminates before or after heat treatment, and the distance from the blade edge to the laminate peeled off was measured using an infrared light source and an infrared camera. The surface energy was then determined based on the following formula: γ = 3 × 10 9 ×t b 2 ×E 2 ×t 6 / (32 x L 4 ×E×t 3 ) where γ is the surface energy (J / m 2 ), t b represents the blade thickness (m), E represents the Young's modulus (GPa) of the substrate such as a silicon substrate included in the laminate, t represents the thickness (m) of the substrate in the laminate, and L represents the distance (m) from the blade tip to peel the laminate.

[0117] <Initial Conductivity of Bonding Layer> The conductivity of the bonding layer was evaluated by resistance value. A probe for measuring electrical characteristics was brought into contact with the external terminal of the bottom chip, and the resistance value of the daisy chain was measured using the two-terminal method. The resistance measurement device used was a digital ultra-high resistance / microcurrent meter 5451A manufactured by Agency. When the resistance value was less than 10 Ω per Cu-Cu bonding part, it was evaluated as a level that was not problematic for practical use (Rank A), and when the resistance value was 10 Ω or more per Cu-Cu bonding part, it was evaluated as a level that was problematic for practical use (Rank B). Measurements were performed at four locations on one substrate laminate, and the arithmetic average value was used for evaluation.

[0118] Example 1 Preparation of Solution Containing Composition 1 A solution containing Composition 1 was prepared. Details are as follows. 50% by mass of 3-aminopropyltriethoxysilane (3APTES: (3-Aminopropyl)triethoxysilane) as compound (A) and 50% by mass of water were blended to obtain Solution A containing a hydrolyzate of 3APTES. Solution B was obtained containing 70% by mass of oxydiphthalic acid half ester (ODPA: structure below) and 30% by mass of ethanol. 24 g of the obtained Solution A, 15.6 g of Solution B, 20 g of 1-propanol, and 40.4 g of water were blended to prepare a solution containing Composition 1.

[0119]

[0120] Ethyl oxydiphthalate half ester was produced by adding ODPA to ethanol, refluxing the mixture in an oil bath heated to 90°C for 5 hours, and completely dissolving the raw material powder. Proton NMR confirmed that an ester group was formed in the produced eheODPA.

[0121] <Formation of Composition Layer> Using the above composition 1, a solution was prepared with its concentration adjusted to give a film thickness shown in Table 1. The solution was spin-coated onto a silicon substrate, dried at 150°C for 1 minute, and then heated at 200°C for 1 hour in a nitrogen atmosphere to form a composition layer containing an imide-crosslinked siloxane (structure shown below).

[0122]

[0123] Example 2 Preparation of Solution Containing Composition 2 A solution containing Composition 2 was prepared. Details are as follows. 50% by mass of 3-aminopropyltriethoxysilane (3APTES: (3-Aminopropyl)triethoxysilane) as compound (A) and 50% by mass of water were blended to obtain Solution A containing a hydrolyzate of 3APTES. Solution B was obtained containing 70% by mass of biphenyl phthalate half ester (BPDA: structure below) and 30% by mass of ethanol. 24 g of the obtained Solution A, 15 g of Solution B, 20 g of 1-propanol, and 41 g of water were blended to prepare a solution containing Composition 2.

[0124]

[0125] Ethyl biphenylphthalate half ester was produced by adding BPDA to ethanol, refluxing the mixture in an oil bath heated to 90°C for 16 hours, and completely dissolving the raw material powder. Proton NMR confirmed that an ester group was formed in the produced eheBPDA.

[0126] <Formation of Composition Layer> Using the above composition 2, a solution was prepared with its concentration adjusted to give a film thickness shown in Table 1. The solution was spin-coated onto a silicon substrate, dried at 150°C for 1 minute, and then heated at 200°C for 1 hour in a nitrogen atmosphere to form a composition layer containing an imide-crosslinked siloxane (structure shown below).

[0127]

[0128] Example 3 Preparation of a Solution Containing Composition 3 A solution containing Composition 3 was prepared. Details are as follows. 50% by mass of 3-aminopropyltriethoxysilane (3APTES; (3-Aminopropyl)triethoxylsilane) was blended with 50% by mass of water as compound (A) to obtain Solution A containing a hydrolyzate of 3APTES. Naphthalene tetracarboxylic acid half ester (NTCDA: structure shown below) was added to ethanol (70% by mass of NTCDA, 30% by mass of ethanol) and refluxed for 15 hours in an oil bath heated to 90°C, but the raw material powder could not be completely dissolved. Therefore, the suspension containing the raw material powder was recovered by vacuum filtration and further dried under reduced pressure at room temperature to obtain a white powder B. Proton NMR confirmed that ester groups were formed in the produced eheNTCDA. 24 g of the obtained solution A, 7.3 g of powder B, 20 g of 1-propanol, and 48.7 g of water were blended together to prepare a solution containing composition 3.

[0129]

[0130] <Formation of Composition Layer> A solution was prepared using Composition 3, with its concentration adjusted to give a film thickness shown in Table 1. The solution was spin-coated onto a silicon substrate, dried at 150°C for 1 minute, and then heated at 200°C for 1 hour in a nitrogen atmosphere to form a composition layer containing an imide-crosslinked siloxane (structure shown below).

[0131]

[0132] Example 4 Preparation of a Solution Containing Composition 4 50% by mass of 3-aminopropyltriethoxysilane (3APTES: (3-Aminopropyl)triethoxysilane) as compound (A) and 50% by mass of water were blended to obtain a solution A containing a hydrolyzate of 3APTES. A solution B containing 70% by mass of cyclohexanetetracarboxylic acid half ester (HPMDA: structure shown below) and 30% by mass of ethanol was obtained.

[0133]

[0134] 28 g of the obtained solution A, 15 g of solution B, 20 g of 1-propanol, and 37 g of water were mixed together to prepare a solution containing composition 4.

[0135] <Formation of Composition Layer> A solution was prepared using Composition 4, with its concentration adjusted to give a film thickness shown in Table 1. The solution was spin-coated onto a silicon substrate, dried at 150°C for 1 minute, and then heated at 200°C for 1 hour in a nitrogen atmosphere to form a composition layer containing an imide-crosslinked siloxane (structure shown below).

[0136]

[0137] <Measurement of Surface Energy> The surface energy (bonding strength) at the bonding interface of the laminate was measured by a blade insertion test according to the method described in non-patent document M. P. Maszara, G. Goetz, A. Cavigila, and J. B. Mckitterick, Journal of Applied Physics, 64 (1988) 4943-4950. Specifically, a 0.25 mm thick blade was inserted between the substrates, and the distance from the blade tip to the separation of the substrates was measured using an infrared light source and an infrared camera. Thereafter, the surface energy was measured based on the following formula:

[0138]

[0139] In the formula, γ is the surface energy (J / m 2 ), tb is the blade thickness (m), E is the Young's modulus (GPa) of the silicon substrates included in the first substrate and the second substrate, t is the thickness (m) of the first substrate and the second substrate, and L is the peeling distance (m) between the substrates from the blade tip. The results are shown in Table 1.

[0140] <Evaluation> The CTE and initial conductivity between electrodes of the compositions of Examples 1 to 4 were measured by the methods already described. The results are shown in Table 1. The bonding strength of the substrate laminates obtained using the compositions of Examples 1 to 4 was measured by the methods already described. The results are shown in Table 1 below.

[0141] Comparative Example 1 Preparation of Solution Containing Comparative Composition 5 A solution containing Comparative Composition 5 was prepared. Details are as follows. 50% by mass of 3-aminopropyldiethoxymethylsilane (3APDES: (3-Aminopropyl)diethoxymethylsilane) as compound (A) and 50% by mass of water were blended to obtain Solution A containing a hydrolyzate of 3APTES. Solution B containing 70% by mass of oxydiphthalic acid half ester (ODPA: structure below) and 30% by mass of ethanol was obtained. 24 g of the obtained Solution A, 18.0 g of Solution B, 20 g of 1-propanol, and 38.0 g of water were blended to prepare a solution containing Comparative Composition 5.

[0142] <Formation of Composition Layer> Using the above-mentioned Comparative Composition 5, a solution was prepared by adjusting the concentration so as to obtain a film thickness shown in Table 1. The solution was spin-coated on a silicon substrate, dried at 150°C for 1 minute, and then heated at 200°C for 1 hour in a nitrogen atmosphere to form a composition layer containing a compound having the following structure.

[0143]

[0144] Comparative Example 2 Preparation of Solution Containing Comparative Composition 6 A solution containing Comparative Composition 6 was prepared. Details are as follows. 50% by mass of 3-aminopropyltriethoxysilane (3APTES) and 50% by mass of water were blended to obtain Solution A containing a hydrolyzate of 3APTES. Solution B was obtained to contain 70% by mass of bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)1,4-phenylene (TAHQ: structure below) and 30% by mass of ethanol. 24 g of the obtained Solution A, 18.0 g of Solution B, 20 g of 1-propanol, and 40.4 g of water were blended to prepare a solution containing Comparative Composition 6, but a uniform composition was not obtained.

[0145]

[0146] For Comparative Example 1, a composition layer was formed on a substrate in the same manner as in Example 1, and evaluation was performed in the same manner. Note that for Comparative Example 2, a uniform composition could not be obtained as described above, and a composition layer could not be formed on the substrate, so evaluation results for CTE and initial conductivity could not be obtained. The evaluation results are shown in Table 1 below. Note that in Table 1, "-" indicates that a composition layer could not be formed and evaluation was not possible.

[0147]

[0148] The results in Table 1 show that the compositions of Examples 1 to 4 provide a composition layer that has a low coefficient of linear thermal expansion and is a dense cured product. All of the substrate laminates obtained using the compositions of Examples 1 to 4 exhibited good initial conductivity that poses no practical problems. Therefore, it is presumed that the bonding strength of the joints is good. On the other hand, Comparative Example 1, which used a compound having only two Si—O bonds per Si atom, produced a composition layer with a high coefficient of linear thermal expansion and poor initial conductivity at the electrode joints. Comparative Example 2 contains a compound having three Si—O bonds per Si atom, but was unable to produce a uniform composition layer on the substrate, and therefore, no evaluation results could be obtained. [Explanation of Symbols]

[0149] 12 Substrate, 14 Electrode, 16 Composition layer, 20 Substrate laminate

[0150] The disclosure of Japanese Patent Application No. 2023-059237, filed on March 31, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. A compound (A) having a cationic functional group containing at least one selected from a primary nitrogen atom and a secondary nitrogen atom and a Si-O bond, a crosslinking agent (B) represented by the following formula (1), and a polar solvent (C), wherein the compound (A) has three Si-O bonds per one Si atom, and the crosslinking agent (B) represented by the following formula (1) is R 1 represents a linking group containing two or more aromatic rings, or a linking group containing one or more aliphatic rings; each X independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and one or more and four or less X's are hydrogen atoms; and the weight average molecular weight is 200 or more and 500 or less.

2. R in the above formula (1) 1 is a linking group which is a condensed ring of two or more aromatic rings, or a linking group in which two or more aromatic rings are linked to each other via a bond selected from a single bond and an ether bond.

3. The composition according to claim 1, which is used for bonding wiring in a laminate of two or more substrates having a substrate and wiring.

4. A substrate laminate comprising a first substrate, an electrode on the first substrate, and a first laminate comprising a layer containing the composition according to claim 1; and a second substrate, an electrode on the second substrate, and a layer made of an inorganic material or a resin, wherein a surface of the first laminate having an electrode faces a surface of the second laminate having an electrode, and the electrode of the first laminate and the electrode of the second laminate, and the layer containing the composition of the first laminate and the layer made of the inorganic material or resin of the second laminate are directly bonded to each other.

5. A method for producing a substrate laminate, comprising: step I of preparing a laminate comprising a substrate and an electrode; step II of applying the composition according to claim 1 to the electrode side of the laminate to form a composition layer; step III of polishing the surface of the laminate obtained in step II on the side having the composition layer; step IV of preparing the laminate polished in step III and a separate laminate comprising an electrode and a layer made of an inorganic material or resin on a substrate, and stacking the electrodes on the electrode sides of the two laminates prepared in contact with each other; and step V of heating and bonding the stacked laminates prepared in step VI.

Citation Information

Patent Citations

  • Resin composition for semiconductor protection

    JP1994025415A

  • Resin composition, cured film, semiconductor device and method for manufacturing semiconductor device

    JP2019031597A

  • Ink-jet ink

    WO2008123190A1

  • Composition, multilayer body and method for producing multilayer body

    WO2022054839A1

  • Resin composition, method for producing semiconductor device, cured object, semiconductor device, and method for synthesizing polyimide precursor