Multi-component curable resin composition, dry film, cured product, and electronic component

By adding an epoxy compound with a weight average molecular weight of 700 or more to two-component curable resin compositions, the stability and sensitivity issues at high temperatures are addressed, resulting in stable and effective coating film properties.

WO2024204644A1PCT designated stage expired Publication Date: 2024-10-03TAIYO HOLDINGS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012888
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional two-component curable resin compositions face challenges in maintaining stability and sensitivity when prepared at high temperatures, particularly due to the reactivity of carboxyl group-containing resins and photopolymerization initiators, which can lead to unwanted reactions and affect the properties of the coating film.

Method used

Incorporating an epoxy compound with a weight average molecular weight of 700 or more into the composition liquid containing a carboxyl group-containing resin and at least one of a primary, secondary, or tertiary amine, including an oxime ester photopolymerization initiator, to delay reaction and maintain stability, even when prepared at elevated temperatures.

Benefits of technology

This approach ensures stable coating film characteristics and maintains quality stability during storage and usage, improving sensitivity and productivity by preventing premature reaction and ensuring consistent performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a multi-component curable resin composition that exhibits stable characteristics such as sensitivity after mixing, even after each composition component has been prepared at a high temperature (for example, 60°C). In this multi-component curable resin composition, a carboxyl group-including resin, at least one among a first amine, a second amine, and a third amine, and an epoxy compound that has a weight average molecular weight of 700 or greater are combined in the same composition component.
Need to check novelty before this filing date? Find Prior Art

Description

Multi-component curable resin composition, dry film, cured product, and electronic component

[0001] The present invention relates to a multi-component curable resin composition, a dry film, a cured product, and an electronic component.

[0002] In printed wiring boards, solder resist has traditionally been used as a protective material for wiring board circuits. Examples of compositions for such protective materials include curable resin compositions. These curable resin compositions contain, for example, an oxime ester-based photopolymerization initiator (i.e., a highly photosensitive compound) to form more precise patterns (specifically, to increase sensitivity during exposure). In recent years, two-component curable resin compositions have also been proposed from the standpoint of quality stability (e.g., Patent Documents 1 and 2).

[0003] However, the oxime ester photopolymerization initiators are highly reactive and therefore require careful handling, one of which is the production process of the composition.

[0004] To solve this problem of quality stability during storage, a two-part photocurable / thermosetting resin composition composed of a liquid composition containing a photopolymerization initiator having an oxime bond and a liquid composition containing a resin having a carboxyl group or a reactive diluent (the invention described in Patent Document 1) has been proposed. Also proposed is a two-part alkali-developable curable resin composition composed of a liquid composition containing a photopolymerization initiator having an oxime bond and a liquid composition containing an alkali-soluble resin (the invention described in Patent Document 2).

[0005] International Publication No. 2004 / 048434 Pamphlet Japanese Patent Application Laid-Open No. 2020-140161

[0006] In prior art such as the inventions described in Patent Documents 1 and 2, specifically, each composition liquid was prepared using a three-roll mill at a temperature of about 40°C. The ability to prepare each composition liquid using a separate device (e.g., a bead mill) instead of the conventional three-roll mill is advantageous in that it allows for a wider range of preparation methods to be selected. However, when a bead mill is used as a separate device, each composition liquid is prepared at a higher temperature (e.g., about 60°C) than the temperature in the three-roll mill, which increases the likelihood of changes in properties such as sensitivity when the composition liquids are mixed. In particular, from the viewpoint of productivity such as mixing and dispersion, some curable resin compositions contain a carboxyl group-containing resin and a photopolymerization initiator in the same composition liquid. This tendency is particularly pronounced when the photopolymerization initiator is an oxime ester-based photopolymerization initiator, leaving room for improvement.

[0007] An object of the present invention is to provide a multi-component curable resin composition that can exhibit stable properties such as sensitivity after mixing, even after each component liquid is prepared at a high temperature (for example, about 60°C).

[0008] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by further adding an epoxy compound having a weight-average molecular weight of 700 or more to a liquid composition containing a resin having a carboxyl group and at least one of a primary amine, a secondary amine, and a tertiary amine (for example, an oxime ester-based photopolymerization initiator), and have thus completed the present invention.

[0009] That is, the above-mentioned object can be achieved by a multi-component curable resin composition according to the present invention, which comprises: a carboxyl group-containing resin; at least one of a primary amine, a secondary amine, and a tertiary amine; and an epoxy compound having a weight-average molecular weight of 700 or more, wherein the carboxyl group-containing resin, the at least one of a primary amine, a secondary amine, and a tertiary amine, and the epoxy compound having a weight-average molecular weight of 700 or more are blended in the same composition liquid.

[0010] In a preferred embodiment of the multi-component curable resin composition according to the present invention, at least one of the primary amine, secondary amine and tertiary amine comprises an oxime ester photopolymerization initiator.

[0011] According to another preferred embodiment of the multi-component curable resin composition of the present invention, the composition further contains another photopolymerization initiator different from the oxime ester-based photopolymerization initiator.

[0012] In yet another preferred embodiment of the multi-component curable resin composition according to the present invention, the oxime ester photopolymerization initiator is blended in a larger amount than the other photopolymerization initiators.

[0013] According to yet another preferred embodiment of the multi-component curable resin composition of the present invention, the composition further comprises an epoxy compound having a weight-average molecular weight of less than 700, and the epoxy compound having a weight-average molecular weight of less than 700 is blended in a liquid composition different from the liquid composition containing at least one of the primary amine, secondary amine, and tertiary amine.

[0014] The present invention also relates to a dry film having a resin layer formed from the curable resin composition.

[0015] The present invention also relates to a cured product obtained by curing the multi-component curable resin composition or the resin layer of the dry film.

[0016] The present invention also relates to an electronic component having the cured product.

[0017] According to the multi-component curable resin composition of the present invention, even after each component liquid is prepared at a high temperature (for example, about 60° C.), stable properties such as sensitivity can be exhibited after mixing.

[0018] The multi-component curable resin composition of the present invention contains a carboxyl group-containing resin, at least one of a primary amine, a secondary amine, and a tertiary amine, and an epoxy compound having a weight-average molecular weight of 700 or more. The carboxyl group-containing resin, at least one of a primary amine, a secondary amine, and a tertiary amine, and an epoxy compound having a weight-average molecular weight of 700 or more are blended in the same liquid composition. By further incorporating an epoxy compound having a weight-average molecular weight of 700 or more into a liquid composition containing a carboxyl group-containing resin and at least one of a primary amine, a secondary amine, and a tertiary amine, the quality stability of each liquid composition can be maintained even when the liquid compositions are blended with the carboxyl group-containing resin and at least one of a primary amine, a secondary amine, and a tertiary amine (e.g., an oxime ester photopolymerization initiator) in the same liquid composition and then prepared and stored at a high temperature (e.g., about 60°C). The reason for this is presumed to be as follows. That is, in the past, when a carboxyl group-containing resin and at least one of a primary amine, a secondary amine, and a tertiary amine were contained in the same liquid composition, there was a concern that they would react due to the high temperatures applied during the manufacturing process, such as kneading, and that this would affect the coating film properties when they were subsequently mixed. However, by further adding an epoxy compound having a weight-average molecular weight of 700 or more to the same liquid composition, stable coating film properties can be obtained, and it is thought that this has the effect of delaying the reaction. However, this is merely speculation and is not limited to this. The multi-component curable resin composition of the present invention is composed of at least two or more liquid compositions (preferably two liquid compositions), and each component of the multi-component curable resin composition is contained in one of at least two or more liquid compositions so as to satisfy the condition that the carboxyl group-containing resin, at least one of a primary amine, a secondary amine, and a tertiary amine, and an epoxy compound having a weight-average molecular weight of 700 or more are blended in the same liquid composition. Below, each component contained in the multi-component curable resin composition of the present invention will be described.

[0019] [Carboxyl Group-Containing Resin] The carboxyl group-containing resin contained in the curable resin composition of the present invention can be any known or commonly used resin compound containing a carboxyl group in the molecule. Furthermore, when preparing an alkali-developable resin composition, a carboxyl group-containing photosensitive resin having an ethylenically unsaturated double bond in the molecule is more preferred in terms of photocurability and development resistance. The unsaturated group is preferably derived from an acrylic acid or methacrylic acid derivative. When using only a carboxyl group-containing resin without an ethylenically unsaturated double bond, a photopolymerizable monomer (acrylate component) having two or more ethylenically unsaturated groups in the molecule, as described below, must be used in combination to make the composition photocurable. Specific examples of the carboxyl group-containing resin include the compounds listed below (either oligomers or polymers).

[0020] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, or isobutylene.

[0021] (2) Carboxyl group-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl group-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0022] (3) Carboxyl group-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with (meth)acrylates of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins, and biphenol type epoxy resins, or their partially acid anhydride-modified products, carboxyl group-containing dialcohol compounds, and diol compounds.

[0023] (4) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylate formed by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, or (meth)acrylic acid during the synthesis of the resin (2) or (3) above.

[0024] (5) A carboxyl group-containing photosensitive urethane resin that is (meth)acrylated at the terminal by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reaction product of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3) above.

[0025] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid, and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the hydroxyl groups present in the side chains.

[0026] (7) A carboxyl group-containing photosensitive resin obtained by reacting a polyfunctional epoxy resin in which the hydroxyl groups of a bifunctional (solid) epoxy resin are further epoxidized with epichlorohydrin with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.

[0027] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin, and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.

[0028] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl groups of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, or adipic acid.

[0029] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.

[0030] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.

[0031] (12) A carboxyl group-containing photosensitive resin obtained by adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to the resins (1) to (11) above.

[0032] Among these carboxyl group-containing resins, preferred are (X) carboxyl group-containing polyurethane resins, particularly those in which the isocyanate group-containing component (including diisocyanate) of the urethane resin is not directly bonded to a benzene ring, and (Y) when the polyfunctional epoxy resin used in the synthesis of the resin is a compound having a bisphenol A structure, a bisphenol F structure, a biphenol structure, a biphenyl novolac structure, or a bis-xylenol structure, particularly a biphenyl novolac structure, or a hydrogenated compound thereof, these are preferred in terms of low warpage and bending resistance. In another aspect, the above-mentioned (2), (3), (4), (5), and their modified products such as (12) have urethane bonds in the main chain and are therefore preferred in terms of warpage resistance. Furthermore, resins other than the above-mentioned (1), (2), and (8), i.e., resins (3), (4), (5), (6), (7), (9), (10), (11), and (12), have photosensitive groups in their molecules and are therefore highly photoreactive and therefore preferred. In this specification, (meth)acrylate is a general term that refers to acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.

[0033] The above-mentioned carboxyl group-containing resin has many free carboxyl groups in the side chains of the backbone polymer, which serve as crosslinking points during thermal curing. Furthermore, when formed into a photocurable resin composition, it can be developed with a dilute alkaline aqueous solution. Furthermore, the acid value of the carboxyl group-containing resin is preferably in the range of 10 to 200 mgKOH / g, more preferably 30 to 200 mgKOH / g, more preferably 40 to 200 mgKOH / g, and particularly preferably 45 to 120 mgKOH / g. By having an acid value of 30 mgKOH / g or more, the alkaline developability of the curable resin composition is improved. Furthermore, by having an acid value of less than 200 mgKOH / g, it is possible to easily draw a good resist pattern.

[0034] The weight-average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally in the range of 2,000 to 150,000, and preferably 5,000 to 100,000. A weight-average molecular weight of 2,000 or more can improve tack-free performance and resolution. A weight-average molecular weight of 150,000 or less can improve the developability and storage stability of the curable resin composition.

[0035] The amount of the carboxyl group-containing resin, calculated as solid content, of the total composition is preferably 10 to 60% by mass, more preferably 20 to 60% by mass, and even more preferably 30 to 60% by mass. An amount less than the above range is undesirable because the coating strength decreases. On the other hand, an amount greater than the above range is undesirable because the viscosity of the composition increases and the coatability and other properties decrease.

[0036] These carboxyl group-containing resins can be used alone or in combination of two or more.

[0037] [At least one of primary amine, secondary amine, and tertiary amine] (Oxime ester photopolymerization initiator) As at least one of primary amine, secondary amine, and tertiary amine, for example, an oxime ester photopolymerization initiator having a group represented by the following general formula (I) can be mentioned. (In the formula, R 1 represents a hydrogen atom, a phenyl group (which may be substituted with an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a halogen atom), an alkyl group having 1 to 20 carbon atoms (which may be substituted with one or more hydroxyl groups and which may have one or more oxygen atoms in the middle of the alkyl chain), a cycloalkyl group having 5 to 8 carbon atoms, an alkanoyl group having 2 to 20 carbon atoms, or a benzoyl group (which may be substituted with an alkyl group having 1 to 6 carbon atoms or a phenyl group), R 2represents a phenyl group (which may be substituted with an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a halogen atom), an alkyl group having 1 to 20 carbon atoms (which may be substituted with one or more hydroxyl groups and which may have one or more oxygen atoms in the middle of the alkyl chain), a cycloalkyl group having 5 to 8 carbon atoms, an alkanoyl group having 2 to 20 carbon atoms, or a benzoyl group (which may be substituted with an alkyl group having 1 to 6 carbon atoms or a phenyl group).

[0038] Preferred examples of the oxime ester photopolymerization initiator having a group represented by general formula (I) above include 2-(acetyloxyiminomethyl)thioxanthen-9-one represented by general formula (II) below, a compound represented by general formula (III) below, and a compound represented by general formula (IV) below.

[0039] (In the formula, R 3 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyclopentyl group, a cyclohexyl group, a phenyl group, a benzyl group, a benzoyl group, an alkanoyl group having 2 to 12 carbon atoms, an alkoxycarbonyl group having 2 to 12 carbon atoms (when the alkyl group constituting the alkoxyl group has 2 or more carbon atoms, the alkyl group may be substituted with one or more hydroxyl groups and may have one or more oxygen atoms in the middle of the alkyl chain), or a phenoxycarbonyl group; R 4 , R 6 each independently represents a phenyl group (which may be substituted with an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a halogen atom), an alkyl group having 1 to 20 carbon atoms (which may be substituted with one or more hydroxyl groups and which may have one or more oxygen atoms in the middle of the alkyl chain), a cycloalkyl group having 5 to 8 carbon atoms, an alkanoyl group having 2 to 20 carbon atoms, or a benzoyl group (which may be substituted with an alkyl group having 1 to 6 carbon atoms or a phenyl group), 5represents a hydrogen atom, a phenyl group (which may be substituted with an alkyl group having 1 to 6 carbon atoms, a phenyl group, or a halogen atom), an alkyl group having 1 to 20 carbon atoms (which may be substituted with one or more hydroxyl groups and which may have one or more oxygen atoms in the middle of the alkyl chain), a cycloalkyl group having 5 to 8 carbon atoms, an alkanoyl group having 2 to 20 carbon atoms, or a benzoyl group (which may be substituted with an alkyl group having 1 to 6 carbon atoms or a phenyl group).

[0040] (In the formula, R 7 , R 8 and R 13 each independently represents an alkyl group having 1 to 12 carbon atoms; R 9 , R 10 , R 11 and R 12 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; M represents O, S, or NH; and p and q each independently represent an integer of 0 to 5.

[0041] The oxime ester photopolymerization initiator having a group represented by the general formula (II) is preferred because it has good initiator efficiency and is effective in improving sensitivity even in a small amount, and therefore produces little outgas during heat treatment after the formation of a resist film, and is effective in reducing warpage of the film.

[0042] Among the above oxime ester-based photopolymerization initiators, 2-(acetyloxyiminomethyl)thioxanthen-9-one represented by the above general formula (II), ethanone represented by the above general formula (III), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-,1-(O-acetyloxime), and the compound represented by the general formula (IV) are more preferred. Commercially available products include Irgacure OXE02 and Irgacure OXE04 manufactured by BASF Japan Ltd. The amount of the oxime ester-based photopolymerization initiator blended is preferably 0.01 to 30 parts by mass, and more preferably 0.5 to 20 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin, calculated as solid content. From the viewpoint of sensitivity and resolution, it is preferable that the oxime ester photopolymerization initiator be blended in an amount greater than other photopolymerization initiators different from the oxime ester photopolymerization initiator (specifically, the photopolymerization initiators containing a nucleophilic group and the photopolymerization initiators not containing a nucleophilic group, which will be described later). Specifically, the ratio of the oxime photopolymerization initiator to the other photopolymerization initiator is preferably 1:0.01 to 1:20, more preferably 1:0.02 to 1:10, even more preferably 1:0.02 to 1:1, and particularly preferably 1:0.02 to 1:0.7.

[0043] (Photopolymerization initiator containing a nucleophilic group) Examples of at least one of the primary amine, secondary amine, and tertiary amine include photopolymerization initiators containing a nucleophilic group different from the above-mentioned oxime ester-based photopolymerization initiators (for example, an α-aminoacetophenone-based photopolymerization initiator having a group represented by the following general formula (V)). (In the formula, R 14 and R 15 each independently represents an alkyl group or an arylalkyl group having 1 to 12 carbon atoms; R 16 and R 17 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a cyclic alkyl ether group formed by bonding two of these groups together.

[0044] Examples of α-aminoacetophenone-based photopolymerization initiators having a group represented by general formula (V) include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and N,N-dimethylaminoacetophenone. Commercially available products include Omnirad 369 and Omnirad 379 manufactured by IGM Resins. The amount of the α-aminoacetophenone-based photopolymerization initiator, calculated as solid content, is preferably 0.1 to 80 parts by mass, and preferably 2 to 50 parts by mass, per 100 parts by mass of the carboxyl group-containing resin. The photopolymerization initiators may be used alone or in combination of two or more.

[0045] The oxime ester photopolymerization initiator having a group represented by the general formula (V) is preferred because it has good initiator efficiency and is effective in improving sensitivity even in a small amount, and therefore produces little outgas during heat treatment after formation of a resist film, and is effective in reducing warpage of the film.

[0046] (Catalyst Containing a Nucleophilic Group) At least one of the primary amine, secondary amine, and tertiary amine may be, for example, a catalyst containing a nucleophilic group. Examples of the catalyst containing a nucleophilic group include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; and hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide. The catalyst is not limited to these, and may be a heat curing catalyst for epoxy resins or oxetane compounds, or any catalyst that promotes the reaction between at least one of an epoxy group and an oxetanyl group and a carboxyl group. These catalysts may be used alone or in combination of two or more. Also usable are S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine-isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine-isocyanuric acid adduct. These compounds, which also function as adhesion promoters, are preferably used in combination with the heat curing catalyst. These compounds may be used alone or in combination of two or more. Examples of commercially available products include CUA-4 (primary amine) manufactured by Kumiai Chemical Industry Co., Ltd., DMP-30 (tertiary amine) manufactured by ThreeBond Co., Ltd., and Melamine (primary amine) manufactured by Nissan Chemical Industries, Ltd.

[0047] The amount of the catalyst containing a nucleophilic functional group to be blended is sufficient in a normal quantitative ratio, and is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin, calculated as solid content.

[0048] The amount of at least one compound selected from primary amines, secondary amines, and tertiary amines, calculated as solid content, is preferably 0.1 to 20 parts by mass, and more preferably 0.1 to 12 parts by mass, per 100 parts by mass of the carboxyl group-containing resin. When the amount of at least one compound selected from primary amines, secondary amines, and tertiary amines is 0.1 parts by mass or more, this is preferred because it improves photocurability on copper and also improves coating properties such as chemical resistance. On the other hand, when the amount is less than 20 parts by mass, this is preferred because it results in adequate light absorption at the surface of the solder resist coating film and tends to improve deep curing.

[0049] [Epoxy Compounds Having a Weight-Average Molecular Weight of 700 or More] Examples of epoxy compounds having a weight-average molecular weight of 700 or more include bisphenol A epoxy compounds, phenol novolac epoxy compounds, and hydrogenated bisphenol A epoxy compounds. The lower limit of the weight-average molecular weight of these epoxy compounds is 700 or more, preferably 800 or more, and more preferably 850 or more. The upper limit of the weight-average molecular weight of this epoxy compound is preferably 5,000 or less, more preferably 3,000 or less. These lower and upper limits can be combined arbitrarily. The weight-average molecular weight of this epoxy compound can be measured, for example, by gel permeation chromatography (GPC). Epoxy compounds having a weight-average molecular weight within the above range can be obtained using the common technical knowledge of those skilled in the art. The epoxy compounds having a weight-average molecular weight of 700 or more can be used alone or in combination of two or more. Commercially available products include N-870 manufactured by DIC Corporation, P201 manufactured by Nippon Kayaku Co., Ltd., and ST-5100 manufactured by Nippon Steel Chemical & Material Co., Ltd.

[0050] The content of the epoxy compound having a weight average molecular weight of 700 or more is preferably 1 to 100% by mass, more preferably 5 to 60% by mass, calculated as solid content, based on the total composition.

[0051] [Epoxy Compound with Weight-Average Molecular Weight Less than 700] The multi-component curable resin composition of the present invention may further contain an epoxy compound with a weight-average molecular weight less than 700. Examples of epoxy compounds with a weight-average molecular weight less than 700 include hydrogenated resin-type epoxy compounds, biphenyl-type epoxy compounds, and bisphenol A-type epoxy compounds. The lower limit of the weight-average molecular weight of these epoxy compounds is preferably 5 or more, and preferably 10 or more. The upper limit of the weight-average molecular weight of this epoxy compound is less than 700. These lower and upper limits can be combined as desired. The weight-average molecular weight of this epoxy compound can be obtained, for example, by the same measurement method as described above for epoxy compounds with a weight-average molecular weight of 700 or more. Epoxy compounds with a weight-average molecular weight within the above range can be obtained using the common technical knowledge of those skilled in the art. The epoxy compounds with a weight-average molecular weight less than 700 can be used alone or in combination of two or more. Commercially available products include YX-8034 and jER834 manufactured by Mitsubishi Chemical Corporation.

[0052] The content of the epoxy compound having a weight average molecular weight of less than 700 is preferably 1 to 100% by mass, more preferably 5 to 60% by mass, calculated as solid content, based on the total composition.

[0053] The epoxy compound having a weight-average molecular weight of less than 700 is preferably blended in a liquid composition different from the liquid composition containing at least one of the primary amine, secondary amine, and tertiary amine, since the reaction with the epoxy compound having a weight-average molecular weight of less than 700 may be accelerated.

[0054] [(Meth)acrylate Component] The photopolymerizable monomer ((meth)acrylate component) is photocured by irradiation with active energy rays, and makes or helps to make the multi-component curable resin composition of the present invention insoluble in an alkaline aqueous solution. Examples of such compounds include diacrylates of glycols such as ethylene glycol, methoxytetraethylene glycol, polyethylene glycol, and propylene glycol; polyhydric alcohols such as hexanediol, trimethylolpropane, pentaerythritol, dipentaerythritol, and tris-hydroxyethyl isocyanurate, or polyhydric acrylates such as their ethylene oxide adducts, propylene oxide adducts, and ε-caprolactone adducts; polyhydric acrylates such as phenoxy acrylate, bisphenol A diacrylate, and ethylene oxide adducts or propylene oxide adducts of these phenols; polyhydric acrylates of glycidyl ethers such as glycerin diglycidyl ether, glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and melamine acrylate, and at least one of the methacrylates corresponding to the above acrylates. In this specification, (meth)acrylate is a general term for acrylate, methacrylate and mixtures thereof, and the same applies to other similar expressions.

[0055] Further examples include epoxy acrylate resins obtained by reacting acrylic acid with a multifunctional epoxy resin such as a cresol novolac epoxy resin, and epoxy urethane acrylate compounds obtained by reacting the hydroxyl groups of the epoxy acrylate resin with a half-urethane compound of a hydroxy acrylate such as pentaerythritol triacrylate and a diisocyanate such as isophorone diisocyanate. Such epoxy acrylate resins can improve photocurability without reducing dryness to the touch.

[0056] The above compounds can be used alone or in combination of two or more. Commercially available products include DPCA-60 manufactured by Nippon Kayaku Co., Ltd. and DPHA manufactured by Kyoeisha Chemical Co., Ltd.

[0057] The blending amount of such a (meth)acrylate component is, in terms of solid content, 5 to 80 parts by mass, more preferably 10 to 40 parts by mass, relative to 100 parts by mass of the carboxyl group-containing resin. A blending amount of 5 parts by mass or more is preferred because it improves photocurability and facilitates pattern formation by alkaline development after irradiation with active energy rays. On the other hand, a blending amount of less than 80 parts by mass is preferred because it provides a coating film with a suitable surface hardness.

[0058] [Photopolymerization initiator not containing a nucleophilic group] The multi-component curable resin composition of the present invention may further contain a photopolymerization initiator not containing a nucleophilic group (nucleophilic functional group). As the photopolymerization initiator not containing a nucleophilic functional group, it is preferable to use one or more photopolymerization initiators selected from the group consisting of acylphosphine oxide photopolymerization initiators having a group represented by the following formula (VI): (In the formula, R 18 and R 19 each independently represents a linear or branched alkyl group having 1 to 10 carbon atoms, a cyclohexyl group, a cyclopentyl group, an aryl group, or an aryl group substituted with a halogen atom, an alkyl group, or an alkoxy group, provided that R 10 and R 11 may represent an R--C(.dbd.O)-- group, where R is a hydrocarbon group having 1 to 20 carbon atoms.

[0059] Examples of acylphosphine oxide photopolymerization initiators having a group represented by general formula (VI) include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. These compounds can be used alone or in combination of two or more. Commercially available products include Omnirad 819 and Omnirad 1173 manufactured by IGM Resins.

[0060] The acylphosphine oxide initiator having a group represented by the above general formula (VI) has the best light transmittance in terms of photobleaching performance, and is effective in flame retardancy.

[0061] The amount of the photopolymerization initiator not containing a nucleophilic functional group as described above is suitably in the range of 0.1 to 80 parts by mass, preferably 2 to 50 parts by mass, per 100 parts by mass of the carboxyl group-containing resin, calculated as solid content. When the amount of the photopolymerization initiator not containing a nucleophilic functional group is 0.1 parts by mass or more, sufficient photocurability on copper is achieved, and coating film properties such as chemical resistance are improved, which is preferable. On the other hand, when the amount is less than 80 parts by mass, the photopolymerization initiator not containing a nucleophilic functional group exhibits adequate light absorption on the surface of the solder resist coating film, which tends to improve deep curing, which is preferable.

[0062] [Flame Retardant] The multi-component curable resin composition of the present invention may further contain a flame retardant. The flame retardant may be blended for the purpose of imparting flame retardancy to the cured product obtained after curing of the curable composition. The flame retardant is preferably one that can enhance the flame retardancy of the cured product without impairing the coatability, resolution, or warpage of the cured product. In particular, the flame retardant used in the present invention has the advantage of being able to improve warpage after exposure, tackiness, transparency, and storage stability in a well-balanced manner. Note that the flame retardant does not include compounds that are at least one of the above primary amines, secondary amines, and tertiary amines.

[0063] [Other Components] In the multi-component curable resin composition of the present invention, it is of course possible to blend further additives as other components as necessary within the scope of the object of the present invention. Examples of such components include colorants, solvents, thermal polymerization inhibitors, ultraviolet absorbers, silane coupling agents, plasticizers, flame retardants, antistatic agents, antioxidants, antibacterial and antifungal agents, leveling agents, thickeners, adhesion-imparting agents, thixotropy-imparting agents, photoinitiator assistants, sensitizers, photobase generators, thermoplastic resins, elastomers, organic fillers such as urethane beads, inorganic fillers, release agents, surface treatment agents, dispersants, dispersion assistants, surface modifiers, stabilizers, fluorescent materials, cellulose resins, etc.

[0064] [Method of producing and using the multi-component curable resin composition of the present invention] The multi-component curable resin composition of the present invention can be prepared by mixing and dispersing predetermined amounts of each liquid component containing one of the components at a high temperature (for example, about 60°C) using, for example, a bead mill, and then mixing these liquid components at the time of use.

[0065] The curable resin composition of the present invention can be used in the form of a liquid or in the form of a dry film.

[0066] [Dry Film] The dry film of the present invention can be produced by applying the curable resin composition of the present invention onto a first film and drying it to form a resin layer as a dry coating film. If necessary, a second film can be laminated onto the resin layer.

[0067] The first film serves to support the resin layer of the dry film and is the film onto which the curable resin composition is applied when forming the resin layer. Examples of the first film include polyester films such as polyethylene terephthalate and polyethylene naphthalate, thermoplastic resin films such as polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, and polystyrene films, as well as surface-treated paper. Among these, polyester films are preferred from the viewpoints of heat resistance, mechanical strength, and ease of handling. The thickness of the first film is not particularly limited, but is selected appropriately depending on the application within the range of approximately 10 to 150 μm. The surface of the first film on which the resin layer is to be formed may be subjected to a release treatment. Furthermore, sputtering or copper foil may be formed on the surface of the first film on which the resin layer is to be formed.

[0068] The second film is provided on the side of the resin layer opposite the first film for the purposes of preventing dust and other particles from adhering to the surface of the resin layer of the dry film and improving handleability. Examples of the second film that can be used include films made of thermoplastic resins such as those exemplified for the first film, and surface-treated paper. Among these, polyester film, polyethylene film, and polypropylene film are preferred. The thickness of the second film is not particularly limited, but is selected appropriately depending on the application within the range of approximately 10 to 150 μm. The surface of the second film on which the resin layer is provided may be subjected to a release treatment.

[0069] [Cured Product] The cured product of the present invention is obtained by curing the curable resin composition of the present invention or the resin layer of the dry film of the present invention.

[0070] To form a cured product using the multi-component curable resin composition of the present invention, the individual component liquids are first mixed. There are no particular limitations on the number of component liquids, as long as they are two or more components, but two components are preferred. Mixing is preferably performed using a stirring blade such as a dissolver. Next, the mixed composition is applied to a substrate, and the resulting resin layer is exposed (irradiated with light) after evaporating and drying the solvent, thereby curing the exposed areas (irradiated areas). Specifically, a resist pattern is formed by selectively exposing the composition to active energy rays through a patterned photomask using a contact or non-contact method, or by directly exposing the pattern using a laser direct exposure machine, and developing the unexposed areas with an alkaline aqueous solution (e.g., a 0.3 to 3 wt% sodium carbonate aqueous solution). Further, by heating to a temperature of approximately 100 to 220°C for thermal curing (post-cure), a cured coating (cured product) with excellent properties such as heat resistance, chemical resistance, moisture absorption resistance, adhesion, and electrical properties can be formed.

[0071] In the case of a dry film, either the first film or the second film is peeled from the dry film, heat-laminated onto a circuit board on which a circuit pattern has been formed, and then thermally cured. Thermal curing may be performed in an oven or by hot plate pressing. Copper foil or a circuit board can also be laminated simultaneously when laminating or hot plate pressing the dry film of the present invention onto a circuit board. A printed wiring board can be manufactured by forming a pattern or via hole by laser irradiation or drilling at a position corresponding to a predetermined position on the circuit board, thereby exposing the circuit wiring. At this time, if there is any residual component (smear) on the circuit wiring in the pattern or via hole that has not been completely removed, a desmear treatment is performed. The remaining first or second film can be peeled off either after lamination, heat curing, laser processing, or desmear treatment.

[0072] [Formation of a Film Using a Curable Resin Composition and a Cured Product] A cured film and a cured product can be formed using the multi-component curable resin composition of the present invention as follows. First, to form a cured film using the multi-component curable resin composition of the present invention, the respective composition liquids are mixed. There are no particular restrictions on the number of composition liquids as long as they are two or more liquids, but two liquids are preferred. Mixing is preferably performed using a stirring blade such as a dissolver. Next, the multi-component curable resin composition is applied to a substrate, and the resulting resin layer is exposed (irradiated with light) after evaporating and drying the solvent, thereby curing the exposed areas (irradiated areas). Specifically, the composition is selectively exposed to active energy rays through a patterned photomask using a contact or non-contact method, or the pattern is directly exposed using a laser direct exposure machine. The unexposed areas are then developed with an alkaline aqueous solution (e.g., a 0.3 to 3% by weight sodium carbonate aqueous solution) to form a resist pattern. Further, by heating to a temperature of approximately 100 to 220°C for thermal curing (post-curing), a cured product such as a cured coating having excellent properties such as heat resistance, chemical resistance, moisture absorption resistance, adhesion, and electrical properties can be formed.

[0073] Here, the multi-component curable resin composition of the present invention can be adjusted to a viscosity suitable for the coating method using an organic solvent, and applied to a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating. After that, the organic solvent contained in the composition can be evaporated and dried (pre-dried) at a temperature of about 60 to 100°C, thereby forming a tack-free resin layer.

[0074] Examples of substrates include printed wiring boards and flexible printed wiring boards on which circuits have been formed in advance using copper or the like, as well as copper-clad laminates for high-frequency circuits made from materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven cloth epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, fluororesin / polyethylene / polyphenylene ether, polyphenylene oxide / cyanate, and the like, including copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, PET films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc.

[0075] The volatilization drying or thermal curing can be carried out using, for example, a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method in which hot air in a dryer equipped with a heat source of an air heating type using steam is brought into countercurrent contact with the substrate, or a method in which hot air is blown onto the substrate from a nozzle).

[0076] The exposure device used for actinic energy ray irradiation may be a device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. Furthermore, a direct imaging device (for example, a laser direct imaging device that draws an image directly with a laser based on CAD data from a computer) may also be used. The lamp or laser light source of the direct imaging device may have a maximum wavelength in the range of 350 to 410 nm. The exposure dose for image formation varies depending on factors such as the film thickness, but is generally 20 to 2,000 mJ / cm. 2 , preferably 20 to 1,500 mJ / cm 2 The range may be:

[0077] The developing method may be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution may be an aqueous alkali solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, or an amine.

[0078] The multi-component curable resin composition of the present invention is preferably used to form a cured film on a printed wiring board, more preferably to form a permanent coating, and even more preferably to form a solder resist, an interlayer insulating layer, or a coverlay. It is particularly suitable for use in flexible printed wiring boards that require properties such as bending resistance.

[0079] [Method for Identifying Photopolymerization Initiator in Cured Product] The photopolymerization initiator component in the cured product can be identified and quantified, for example, by the following method. Examples of methods for identification include using a known Fourier transform infrared spectrometer (FT-IR) and a visible-ultraviolet spectrophotometer. A preferred method involves measuring the infrared absorption spectrum of the cured product using a Fourier transform infrared spectrophotometer (FT-IR) to identify the photopolymerization initiator component in the cured product. Examples of methods for identification and quantification include using a known visible-ultraviolet spectrophotometer and a Fourier transform infrared spectrophotometer (FT-IR). A preferred method involves obtaining a UV spectrum using a visible-ultraviolet spectrophotometer to identify and quantitate the photopolymerization initiator component in the cured product. For example, oxime ester photopolymerization initiators have strong absorption in the range of 320 nm to 350 nm, and can be quantified in this region.

[0080] [Electronic Components] The present invention also provides electronic components having the above-described cured product. By using the multi-component curable resin composition of the present invention, electronic components with high quality, durability, and reliability can be provided. In the present invention, the term "electronic components" refers to components used in electronic circuits, and includes active components such as printed wiring boards, transistors, light-emitting diodes, and laser diodes, as well as passive components such as resistors, capacitors, inductors, and connectors.

[0081] EXAMPLES The present invention will be specifically explained below by showing examples and comparative examples, but it goes without saying that the present invention is not limited to the following examples.

[0082] (Synthesis Example) (Synthesis of Carboxyl Group-Containing Resin A) In the above general formula (1), X is CH 2 380 parts of bisphenol F epoxy resin (epoxy equivalent: 950 g / eq, softening point: 85°C) having an average degree of polymerization (n) of 6.2 and 925 parts of epichlorohydrin were dissolved in 462.5 parts of dimethyl sulfoxide, and then 60.9 parts of 98.5% NaOH was added over 100 minutes at 70°C with stirring. After the addition, the reaction was continued for an additional 3 hours at 70°C. After completion of the reaction, 250 parts of water was added and the mixture was washed with water. After oil-water separation, most of the dimethyl sulfoxide and excess unreacted epichlorohydrin were recovered from the oil layer by distillation under reduced pressure, and the remaining reaction product containing by-product salt and dimethyl sulfoxide was dissolved in 750 parts of methyl isobutyl ketone. 10 parts of 30% NaOH was added and the mixture was reacted at 70°C for 1 hour. After completion of the reaction, the mixture was washed twice with 200 parts of water. After oil-water separation, methyl isobutyl ketone was recovered by distillation from the oil layer to obtain epoxy resin (a) with an epoxy equivalent of 310 g / eq and a softening point of 69°C. Based on the epoxy equivalent, the obtained epoxy resin (a) was found to have approximately 5 of the 6.2 alcoholic hydroxyl groups in the starting bisphenol F epoxy resin epoxidized. 310 parts of this epoxy resin (a) and 282 parts of carbitol acetate were charged into a flask, heated to 90°C, and stirred to dissolve. The resulting solution was cooled to 60°C, and then 72 parts (1 mol) of acrylic acid, 0.5 parts of methylhydroquinone, and 2 parts of triphenylphosphine were added. The mixture was heated to 100°C and reacted for approximately 60 hours to obtain a reaction product with an acid value of 0.2 mgKOH / g. 140 parts (0.92 mol) of tetrahydrophthalic anhydride was added to the mixture, heated to 90°C, and reacted to obtain a resin solution of carboxyl group-containing resin A. The resulting resin solution had a solid content of 65.0%, and the acid value (mgKOH / g) of the solid content was 100. The weight average molecular weight (Mw) was 15,000.

[0083] Examples 1 to 7 and Comparative Examples 1 and 2 Various components shown in Table 1 below were blended in the ratios (unit: parts by mass) shown in Table 1, and mixed and dispersed using a bead mill (temperature of first composition liquid and second composition liquid = approximately 60°C; rotation speed 700 to 1400 rpm, 3 to 12 minutes, discharge amount 5% to 40%, bead diameter 0.1 mm to 1.0 mm) to prepare first composition liquid and second composition liquid constituting a two-component curable resin composition.

[0084] Carboxyl group-containing resin A: Carboxyl group-containing resin A obtained in the above "Synthesis of carboxyl group-containing resin A" N-870: N-870 (bisphenol A type epoxy compound) manufactured by DIC Corporation [equivalent weight 200; weight average molecular weight 1,000 to 2,000] P201: P201 (phenol novolac type epoxy compound) manufactured by Nippon Kayaku Co., Ltd. [equivalent weight 200; weight average molecular weight 1,000 to 2,000] ST-5100: Nippon Steel Chemical & Material Co., Ltd. (hydrogenated bisphenol A type epoxy compound) [equivalent weight 450; weight average molecular weight 900] 834: jER834 (bisphenol A type epoxy compound) manufactured by Mitsubishi Chemical Corporation [equivalent weight 250; weight average molecular weight 500] DPCA-60: KAYARAD DPCA-60 (caprolactone-modified acrylate) manufactured by Nippon Kayaku Co., Ltd. OXE02: Irgacure OXE02 (oxime ester photopolymerization initiator) manufactured by BASF Japan Ltd.; Ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) OXE04: Irgacure OXE04 (oxime ester photopolymerization initiator) manufactured by BASF Japan Ltd. 369: Omnirad 369 (α-aminoalkylphenone, photopolymerization initiator) manufactured by IGM Resins; 2-benzyl-2-(dimethylamino)-4′-morpholinobutyrophenone 379: IGM Omnirad 379EG (α-aminoalkylphenone, photoinitiator) from Resins;2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one CUA-4 (primary amine): CUA-4 (trimethylene-bis(4-aminobenzoate)) manufactured by Kumiai Chemical Industry Co., Ltd. 2E4MZ (secondary amine): 2E4MZ (2-ethyl-4-methylimidazole) manufactured by Shikoku Chemical Industry Co., Ltd. DMP-30 (tertiary amine): DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol) manufactured by ThreeBond Co., Ltd. Melamine: melamine (primary amine) manufactured by Nissan Chemical Industries, Ltd. TPO: 2,4,6-trimethylbenzoyl-diphenyl phosphine oxide 819: Omnirad 819 (bisacylphosphine oxide initiator) manufactured by IGM Resins; Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide 1173: Omnirad 1173 (photopolymerization initiator, α-hydroxyacetophenone) manufactured by IGM Resins; 2-hydroxy-2-methyl-1-phenylpropanone; YX-8034: (biphenyl-type epoxy compound) manufactured by Mitsubishi Chemical Corporation [equivalent weight 270; weight average molecular weight 540]; DPHA: dipentaerythritol hexaacrylate; 2MZ-A (primary amine): 2MZ-A (2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine) manufactured by Shikoku Chemicals Corporation;

[0085] (Preparation of Coating Film) The first and second liquid compositions of Examples 1 to 7 and Comparative Examples 1 and 2 were thoroughly mixed (at 800 rpm and room temperature for 15 minutes) using a dissolver in a ratio of base agent to curing agent of 1:1, and then applied to a glass substrate with an applicator so that the film would have a dried thickness of 10 μm. The mixture was then dried in a hot air circulation drying oven at 80° C. for 30 minutes to prepare an initial coating film (not left standing at 50° C.). In addition, the first and second liquid compositions were separately prepared and left standing in a thermostatic chamber at 50° C. for 7 days, and then mixed and dried in the same manner as above to prepare a coating film.

[0086] (Sensitivity of Curable Resin Composition After Mixing) The first composition liquid and the second composition liquid prepared by mixing and dispersing in a bead mill as described above were thoroughly mixed in a 1:1 ratio using a dissolver (rotational speed: 800 rpm, room temperature for 15 minutes), and then coated onto the entire surface of an etched-out substrate so that the film thickness after drying would be 30 μm. The mixture was then dried at 80° C. for 30 minutes. A step tablet (Kodak No. 2) was attached to each coating film, and the resulting mixture was exposed to 500 mJ / cm 2 using a metal halide lamp exposure machine (HMW-680-GW20, manufactured by Oak Manufacturing Co., Ltd.). 2 and developed with a 1.0 mass % aqueous sodium carbonate solution at a spray pressure of 0.2 MPa at 30°C for 1 minute, and then the sensitivity was determined from the remaining step number and gloss step number obtained from a step tablet (Kodak No. 2) (hereinafter referred to as sensitivity 1). Meanwhile, various components shown in Table 1 were blended in the ratios (unit: parts by mass) shown in Table 1 and kneaded using a three-roll mill to prepare a first composition liquid and a second composition liquid constituting a two-component curable resin composition. The prepared first composition liquid and second composition liquid were thoroughly mixed in a 1:1 ratio using a dissolver (rotation speed 800 rpm, room temperature for 15 minutes), and then coated entirely on an etched-out substrate so that the film thickness after drying would be 30 μm, and dried at 80°C for 30 minutes. A step tablet (Kodak No. 2) was closely attached to each coating film, and the resulting mixture was exposed to 500 mJ / cm using a metal halide lamp exposure machine (HMW-680-GW20 manufactured by Oak Manufacturing Co., Ltd.). 2 and developed with a 1.0% by mass aqueous solution of sodium carbonate at a spray pressure of 0.2 MPa at 30°C for 1 minute, and then the sensitivity was determined from the residual step number and gloss step number obtained from a step tablet (Kodak No. 2) (hereinafter referred to as sensitivity 2). Sensitivity 1 and sensitivity 2 were compared and evaluated according to the following criteria: ◯: No change in sensitivity (the variation between sensitivity 1 and sensitivity 2 was ±1 step or less for both residual sensitivity and gloss sensitivity) ×: Sensitivity decreased (the variation between sensitivity 1 and sensitivity 2 was ±2 steps or more for both residual sensitivity and gloss sensitivity)

[0087] <Resolution of Curable Resin Composition After Mixing> The first and second liquid compositions were thoroughly mixed using a dissolver (rotation speed: 800 rpm, 15 minutes), to obtain a two-component curable resin composition. The mixed curable resin composition was then applied to the entire surface of a copper substrate by screen printing so that the dried coating thickness was 30 μm. The substrate was then dried at 80° C. for 30 minutes, and exposed to an optimal exposure dose using a negative film with an L / S of 100 μm / 50 μm and a metal halide lamp exposure machine (HMW-680-GW20, manufactured by Oak Manufacturing Co., Ltd.). After development, the remaining lines and shapes of 70 μm to 100 μm were confirmed, and the results were evaluated according to the following criteria. The optimum exposure dose was determined by exposing the surface of the dried coating film through a step tablet (Kodak No. 2) using an exposure machine equipped with a metal halide lamp as a light source, and developing with a 1.0 mass % aqueous sodium carbonate solution at a spray pressure of 0.2 MPa at 30°C for 1 minute, resulting in a remaining step tablet pattern of 6 to 7 steps. ⊚: 70 μm lines remain, and the shape is good. ○: 100 μm lines remain, and the shape is good. ×: No 100 μm lines remain.

[0088] <Electroless Gold Plating Resistance of Curable Resin Composition After Mixing> The first and second liquid compositions were thoroughly mixed using a dissolver (rotation speed: 800 rpm, 15 minutes), and then a mixed curable resin composition was obtained. The mixed curable resin composition was then screen-printed onto a copper substrate to form a 30 μm thick coating film after curing, dried at 80°C for 30 minutes, and exposed to an optimal exposure dose using a negative film with an L / S of 100 μm / 50 μm and a metal halide lamp exposure machine, followed by development. The optimal exposure dose was determined by exposing the surface of the dried coating film through a step tablet (Kodak No. 2) using an exposure machine (Oak Manufacturing Co., Ltd. HMW-680-GW20) equipped with a metal halide lamp as a light source, and developing with a 1.0% by mass aqueous sodium carbonate solution at a spray pressure of 0.2 MPa at 30°C for 1 minute, resulting in a remaining step tablet pattern of 6 to 7 steps. The test substrates were then heat-treated at 150°C for 60 minutes in a hot air circulation oven to obtain evaluation substrates with cured coatings. Using commercially available electroless nickel plating baths and electroless gold plating baths, the evaluation substrates were plated with nickel 3 μm and gold 0.03 μm thick. The resist layer was then evaluated for peeling and penetration by tape peeling, and the resist layer was then evaluated for peeling by tape peeling. The evaluation criteria were as follows: ∘: No peeling was observed. ×: Peeling was observed after plating.

[0089] <Solder heat resistance of curable resin composition after mixing> After thoroughly mixing the first composition liquid and the second composition liquid using a dissolver (rotation speed 800 rpm, 15 minutes), a two-component curable resin composition was obtained. Thereafter, the mixed curable resin composition was screen-printed onto a copper solid substrate so that the coating film after curing was 30 μm, dried at 80 ° C. for 30 minutes, exposed to an optimal exposure amount using a negative film with an L / S = 100 μm / 50 μm and a metal halide lamp exposure machine, and developed. The optimal exposure amount was determined by exposing the surface of the dried coating film through a step tablet (Kodak No. 2) using an exposure machine (Oak Manufacturing Co., Ltd. HMW-680-GW20) equipped with a metal halide lamp as a light source, and developing with a 1.0 mass% aqueous sodium carbonate solution at a spray pressure of 0.2 MPa at 30 ° C. for 1 minute, resulting in a remaining step tablet pattern of 6 to 7 steps. The boards were then heat treated at 150°C for 60 minutes in a hot air circulation drying oven to obtain evaluation boards with a cured coating. The evaluation boards coated with rosin-based flux were immersed in a solder bath pre-set to 260°C, and the flux was washed off with denatured alcohol. The resist layer was then visually evaluated for swelling and peeling. The evaluation criteria were as follows: ○: No peeling was observed after a single 10-second immersion. ×: The resist layer swelled and peeled after a single 10-second immersion.

[0090] <Productivity> The various components shown in Table 1 above were blended in the ratios (unit: parts by mass) shown in Table 1, and mixed and dispersed using a bead mill (temperature of first composition liquid and second composition liquid = approximately 60°C; rotation speed 700 to 1400 rpm, 3 to 12 minutes, discharge rate 5% to 40%, bead diameter 0.1 mm to 1.0 mm) to prepare a first composition liquid and a second composition liquid that constitute a two-component curable resin composition, and the mixing and dispersion time for each was measured and evaluated as follows: ○: Both the first composition liquid and the second composition liquid were mixed and dispersed within 15 minutes. △: Either the first composition liquid or the second composition liquid was mixed and dispersed within more than 15 minutes but within 30 minutes. ×: Both the first composition liquid and the second composition liquid were mixed and dispersed in more than 30 minutes.

[0091] <Results> The results of the sensitivity, resolution, resistance to electroless gold plating, solder heat resistance, and productivity are shown in Table 2 below.

[0092] As is clear from the above results, the two-component curable resin compositions of Examples 1 to 7 were good in all of the sensitivity, resolution, electroless gold plating resistance, and solder heat resistance of the curable resin compositions after mixing. On the other hand, the two-component curable resin compositions of Comparative Examples 1 and 2 were poor in all of the sensitivity, resolution, and electroless gold plating resistance of the curable resin compositions after mixing. Furthermore, as is clear from the productivity results, when a photopolymerization initiator was also blended in the same composition liquid as the carboxyl group-containing resin, the mixing and dispersion time was shortened and productivity was better.

Claims

1. A multi-component curable resin composition comprising: a carboxyl group-containing resin; at least one of a primary amine, a secondary amine and a tertiary amine; and an epoxy compound having a weight average molecular weight of 700 or more, wherein the carboxyl group-containing resin, the at least one of a primary amine, a secondary amine and a tertiary amine, and the epoxy compound having a weight average molecular weight of 700 or more are blended in a single composition liquid.

2. The multi-component curable resin composition according to claim 1, wherein at least one of the primary amine, secondary amine and tertiary amine comprises an oxime ester-based photopolymerization initiator.

3. The multi-component curable resin composition according to claim 2, further comprising another photopolymerization initiator different from the oxime ester-based photopolymerization initiator.

4. The multi-component curable resin composition according to claim 3, wherein the oxime ester photopolymerization initiator is blended in a larger amount than the other photopolymerization initiators.

5. The multi-component curable resin composition according to claim 1, further comprising an epoxy compound having a weight average molecular weight of less than 700, wherein the epoxy compound having a weight average molecular weight of less than 700 is blended in a composition liquid different from a composition liquid containing at least one of the primary amine, secondary amine and tertiary amine.

6. A dry film comprising a resin layer formed from the curable resin composition according to claim 1.

7. A cured product obtained by curing the multi-component curable resin composition according to any one of claims 1 to 5 or the resin layer of the dry film according to claim 6.

8. An electronic part comprising the cured product according to claim 7.

Citation Information

Patent Citations

  • Curable composition, and coated wiring board production process

    JP2016060869A

  • Black photosensitive resin composition, dry film, solder resist and printed wiring board

    JP2022154993A

  • Photo- and thermo-setting resin composition and printed wiring boards made by using the same

    WO2004048434A1