Composition for forming resist underlayer film

The composition for forming a resist underlayer film, featuring a compound with α,β-unsaturated carbonyl groups and a solvent, addresses defects in semiconductor manufacturing by creating patterns with low roughness and preventing intermixing, enhancing semiconductor manufacturing quality.

WO2024204780A1PCT designated stage expired Publication Date: 2024-10-03NISSAN CHEM CORP
View PDF 63 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013227
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In semiconductor manufacturing, defects in resist pattern formation due to influences from semiconductor substrates have become a major issue, especially as devices become more highly integrated, and existing methods struggle to form resist patterns with small roughness without intermixing with the resist film.

Method used

A composition for forming a resist underlayer film is developed, comprising a compound with a side chain or terminal having a linear α,β-unsaturated carbonyl group and a solvent, which includes a reaction product of compounds with epoxy groups, along with a crosslinking agent and curing catalyst, to create a film with low roughness and prevent intermixing.

Benefits of technology

The solution effectively forms resist patterns with small roughness and prevents intermixing with the resist film, improving the quality of semiconductor manufacturing by addressing defects and integration challenges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The composition for forming a resist underlayer film contains: a compound (A) containing a side chain or a terminal having a chain alpha, beta-unsaturated carbonyl group; and a solvent (B).
Need to check novelty before this filing date? Find Prior Art

Description

Composition for forming resist underlayer film

[0001] The present invention relates to a composition for forming a resist underlayer film, a resist underlayer film, a laminate, a method for producing a semiconductor element, and a method for forming a pattern.

[0002] In the manufacture of semiconductor devices, microfabrication by lithography using a resist composition has traditionally been performed. This microfabrication process involves forming a thin film of a photoresist composition on a semiconductor substrate, such as a silicon wafer, irradiating the substrate with actinic rays such as ultraviolet light through a mask pattern bearing a device pattern, developing the thin film, and etching the substrate using the resulting photoresist pattern as a protective film, thereby forming fine irregularities on the substrate surface corresponding to the photoresist pattern. In recent years, the integration density of semiconductor devices has increased, and in addition to the conventionally used i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), and ArF excimer laser (wavelength 193 nm), the practical use of EUV light (wavelength 13.5 nm) or EB (electron beam) is being considered for cutting-edge microfabrication. As a result, poor resist pattern formation due to influences from the semiconductor substrate, etc., has become a major problem. To address this issue, methods of providing a resist underlayer film between the resist and the semiconductor substrate have been widely investigated.

[0003] A resist underlayer film-forming composition has been proposed, which comprises a reaction product of a compound (A) represented by formula (1) (in formula (1), A represents an organic group containing an aliphatic ring, an aromatic ring, or a heterocycle) dissolved in a solvent, a compound (B) having two functional groups reactive with an epoxy group, and a compound (C) having one functional group reactive with an epoxy group (see Patent Document 1).

[0004] International Publication No. 2022 / 075339

[0005] Properties required for a resist underlayer film include, for example, not intermixing with a resist film formed on top (being insoluble in a resist solvent), the ability to form a resist pattern with minimal roughness, etc. The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a composition for forming a resist underlayer film that is capable of forming a resist pattern with minimal roughness, as well as methods for producing a resist underlayer film, a laminate, and a semiconductor device, and a pattern formation method that use the composition for forming a resist underlayer film.

[0006] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved, and have completed the present invention having the following gist.

[0007] That is, the present invention encompasses the following aspects. [1] A composition for forming a resist underlayer film, comprising a compound (A) having a side chain or terminal end containing a chain α,β-unsaturated carbonyl group, and a solvent (B). [2] The composition for forming a resist underlayer film according to [1], wherein the total number of chain α,β-unsaturated carbonyl groups in the compound (A) is 3 or more. [3] The composition for forming a resist underlayer film according to [1] or [2], wherein the compound (A) is a reaction product of a reactant containing a compound (A-1) having an epoxy group and a compound (A-2) having a chain α,β-unsaturated carbonyl group and capable of reacting with an epoxy group. [4] The composition for forming a resist underlayer film according to [3], wherein the reactant further contains a compound (A-3) having two or more groups capable of reacting with an epoxy group. [5] The composition for forming a resist underlayer film according to [4], wherein the compound (A-3) is a compound having two groups capable of reacting with an epoxy group. [6] The composition for forming a resist underlayer film according to any one of [1] to [5], wherein the compound (A) is represented by the following formula (1): (In formula (1), R 1 R each independently represents a chain carbon-carbon double bond or a chain carbon-carbon triple bond which may be substituted with a hydrocarbon group having 1 to 6 carbon atoms. 2each independently represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Each X independently represents -O- or -N(R)- (wherein R represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms). Each Q independently represents a single bond or a divalent organic group. [7] The composition for forming a resist underlayer film according to any one of [1] to [6], wherein the solvent (B) contains at least one selected from the group consisting of alkylene glycol monoalkyl ethers and monocarboxylic acid esters of alkylene glycol monoalkyl ethers. [8] The composition for forming a resist underlayer film according to any one of [1] to [7], further containing a crosslinking agent (C). [9] The composition for forming a resist underlayer film according to [8], wherein the crosslinking agent (C) is at least one selected from the group consisting of aminoplast crosslinking agents and phenoplast crosslinking agents.

[10] The composition for forming a resist underlayer film according to any one of [1] to [9], further containing a curing catalyst (D).

[11] A resist underlayer film that is a cured product of the composition for forming a resist underlayer film according to any one of [1] to

[10] .

[12] A laminate comprising: a semiconductor substrate; and the resist underlayer film according to

[11] .

[13] A method for manufacturing a semiconductor device, comprising: forming a resist underlayer film on a semiconductor substrate using the composition for forming a resist underlayer film according to any one of [1] to

[10] , and forming a resist film on the resist underlayer film.

[14] A pattern formation method, comprising: forming a resist underlayer film on a semiconductor substrate using the composition for forming a resist underlayer film according to any one of [1] to

[10] , forming a resist film on the resist underlayer film, irradiating the resist film with light or an electron beam and then developing the resist film to obtain a resist pattern, and etching the resist underlayer film using the resist pattern as a mask.

[0008] According to the present invention, it is possible to provide a composition for forming a resist underlayer film that can form a resist pattern with small roughness, as well as methods for producing a resist underlayer film, a laminate, and a semiconductor element, and a pattern formation method, all of which use the composition for forming a resist underlayer film.

[0009] (Composition for forming a resist underlayer film) The composition for forming a resist underlayer film of the present invention contains a compound (A) and a solvent (B). The composition for forming a resist underlayer film may also contain a crosslinking agent (C), a curing catalyst (D), and the like. The compound (A) contains a side chain or terminal having a chain-like α,β-unsaturated carbonyl group. When the compound (A) contains a side chain or terminal having a chain-like α,β-unsaturated carbonyl group, a resist pattern with low roughness can be formed on a resist underlayer film formed from the composition for forming a resist underlayer film containing the compound (A).

[0010] <Compound (A)> Compound (A) contains a side chain or terminal having a chain-like α,β-unsaturated carbonyl group.

[0011] The compound (A) may contain one, two or more, or three or more side chains or terminals having a chain-like α,β-unsaturated carbonyl group.

[0012] The compound (A) may be a low molecular weight compound or a high molecular weight compound (polymer).

[0013] Examples of the chain α,β-unsaturated carbonyl group located on a side chain or at a terminal include groups represented by the following formula (1A) or (1B). (In formulas (1A) and (1B), R 11 ~R 14 each independently represents a hydrogen atom, a halogen atom, or an organic group having 1 to 6 carbon atoms. * represents a bond.

[0014] R in formula (1A) and formula (1B) 11 ~R 14 Examples of the halogen atom in R in formula (1A) and formula (1B) include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 11 ~R 14 Examples of the organic group having 1 to 6 carbon atoms in the formula (R) include an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, and an alkoxycarbonylalkyl group having 3 to 6 carbon atoms (R a -C(=O)-R b - group: R arepresents an alkoxy group having 1 to 4 carbon atoms, and R b represents an alkylene group having 1 to 4 carbon atoms), an acylamino group having 2 to 6 carbon atoms (R a -C(=O)-N(H)- group: R a represents an alkyl group having 1 to 5 carbon atoms.

[0015] R in formula (1A) 11 and R 12 is preferably a hydrogen atom. 13 is preferably a hydrogen atom or a methyl group. 14 is preferably a hydrogen atom.

[0016] Compound (A) may have a ring structure. The ring structure in the present invention may be an aromatic ring or an aliphatic ring (non-aromatic ring). The ring structure in the present invention may be a hydrocarbon ring or a heterocyclic ring. Examples of aromatic rings include aromatic hydrocarbon rings and aromatic heterocyclic rings. The hydrocarbon ring is not particularly limited. The hydrocarbon ring may be a 5-membered ring, a 6-membered ring, or a 7-membered ring. The heterocyclic ring is not particularly limited. The heterocyclic ring may be a 5-membered ring, a 6-membered ring, or a 7-membered ring. In this specification, an oxirane ring is not included in the heterocyclic ring. Examples of heteroatoms contained in the heterocyclic ring include a nitrogen atom and an oxygen atom. Examples of heterocyclic rings include an isocyanuric acid structure and a triazine structure. Examples of aromatic hydrocarbon rings include a benzene ring and a naphthalene ring. Examples of aromatic heterocyclic rings include a triazine structure. The isocyanuric acid structure and the triazine structure are represented below. (In the formula, * represents a bond.)

[0017] From the viewpoint of suitably achieving the effects of the present invention, compound (A) is preferably a reaction product of a reactant (also referred to as a reactant, reaction raw material, or reactant) containing compound (A-1) and compound (A-2). Compound (A-1) is a compound having an epoxy group. Compound (A-2) is a compound having a chain α,β-unsaturated carbonyl group and capable of reacting with an epoxy group. Furthermore, the reactant may contain a compound other than compound (A-1) and compound (A-2). As such a compound, compound (A-3) having two or more groups capable of reacting with an epoxy group is preferred.

[0018] The reaction may be carried out in the presence of a catalyst, for example. Examples of the catalyst include quaternary phosphonium salts such as tetrabutylphosphonium bromide and ethyltriphenylphosphonium bromide, and quaternary ammonium salts such as benzyltriethylammonium chloride. The amount of catalyst used can be selected appropriately from the range of 0.1 to 10 mass% based on the total mass of the reaction raw materials used in the reaction. Optimal reaction temperature and time can be selected from the ranges of, for example, 80 to 160°C and 2 to 50 hours.

[0019] When the reactant does not contain the compound (A-3), the molar ratio of the compounds (A-1) and (A-2) during the reaction, (A-2) / (A-1), is preferably 3 or more, more preferably 3 or more and 3.5 or less.

[0020] When the reactant contains compound (A-3), the molar ratio of compounds (A-1), (A-2), and (A-3) during the reaction, (A-2) / [(A-1)+(A-3)], is preferably 0.5 or more and 2 or less. By reacting a mixture of compounds (A-1), (A-2), and (A-3) in a molar ratio of (A-2) / [(A-1)+(A-3)] in the range of 0.5 or more and 2 or less, an excessive increase in the weight-average molecular weight of the reaction product is suppressed, and a reaction product can be produced in which compound (A-2) is present at a certain proportion at each terminal of the reaction product molecule. The presence of compound (A-2) at the terminal improves solubility in the above-mentioned solvent.

[0021] <<Compound (A-1)>> The compound (A-1) has an epoxy group.

[0022] The number of epoxy groups that the compound (A-1) has is not particularly limited and may be, for example, 3 to 6, but from the viewpoint of suitably achieving the effects of the present invention, 3 or 4 is preferred.

[0023] The epoxy group in compound (A-1) may or may not be an alicyclic epoxy group. Examples of compound (A-1) include compounds having a total of three or more epoxy groups. Examples of such compounds include compounds represented by the following formula (A-1-1): (In formula (A-1-1), R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; X represents an n-valent group; and n represents an integer of 3 to 6.

[0024] X in formula (A-1-1) has, for example, a ring structure. When X in formula (A-1-1) has a ring structure, the number of ring structures that X has may be one or may be two or more, but preferably one.

[0025] R in formula (A-1-1) 2 is preferably a hydrogen atom or a methyl group, more preferably a hydrogen atom.

[0026] n is an integer of 3 to 6, with 3 or 4 being preferred.

[0027] Examples of the compound represented by formula (A-1-1) include the following compounds:

[0028] The molecular weight of the compound (A-1) is not particularly limited, but may be, for example, 300 to 800.

[0029] <<Compound (A-2)>> The compound (A-2) is a compound capable of reacting with an epoxy group and has a chain α,β-unsaturated carbonyl group.

[0030] The number of "groups reactive with epoxy groups" contained in the compound (A-2) may be one or two or more, but is preferably one. Examples of groups reactive with epoxy groups include a carboxy group, an amino group, a phenolic hydroxy group, and an acid dianhydride group.

[0031] The number of chain α,β-unsaturated carbonyl groups contained in compound (A-2) may be one or two or more, but is preferably one. From the viewpoint of more suitably achieving the effects of the present invention, the chain α,β-unsaturated carbonyl group contained in compound (A-2) is preferably a group represented by formula (1A) or a group represented by formula (1B).

[0032] The compound (A-2) may or may not have a ring structure, but preferably does not have a ring structure. Examples of the ring structure include an aliphatic ring and an aromatic ring.

[0033] Examples of the compound (A-2) include compounds represented by the following formulas (A-2-1) to (A-2-6). (In formulas (A-2-1) to (A-2-6), R 11 ~R 14 are R in formula (1A) and formula (1B), respectively. 11 ~R 14 X represents -O- or -N(R)- (wherein R represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms). Y 1 each independently represents an organic group having 1 to 10 carbon atoms. 2 each independently represents a single bond or an organic group having 1 to 6 carbon atoms.

[0034] Y 1 The organic group having 1 to 10 carbon atoms in the formula Y may or may not have a heteroatom. 1 The organic group having 1 to 10 carbon atoms in Y may or may not have an ester bond. 1In the above formula, examples of the organic group having 1 to 10 carbon atoms include alkylene groups having 1 to 10 carbon atoms. The alkylene group may be linear, branched, or cyclic, or may be a combination of two or more of these.

[0035] Y 2 The organic group having 1 to 6 carbon atoms in the formula Y may or may not have a heteroatom. 2 In the above formula, examples of the organic group having 1 to 6 carbon atoms include alkylene groups having 1 to 6 carbon atoms. The alkylene group may be linear, branched, or cyclic, or may be a combination of two or more of these.

[0036] Specific examples of the compound (A-2) include the following compounds:

[0037] Among these, acrylic acid and methacrylic acid are preferred as the compound (A-2) from the viewpoint of suitably achieving the effects of the present invention.

[0038] <<Compound (A-3)>> The compound (A-3) is a compound having two or more groups capable of reacting with an epoxy group. The compound (A-3) is, for example, a compound having two groups capable of reacting with an epoxy group.

[0039] Examples of groups capable of reacting with an epoxy group include a carboxy group, an amino group, a phenolic hydroxy group, and an acid dianhydride group.

[0040] When the group capable of reacting with an epoxy group is an acid dianhydride group, the carboxy group remaining after the reaction of the epoxy group with the acid dianhydride group may be present in compound (A) or may have reacted with at least one compound represented by the following formula (3d): (In formula (3d), R 1 represents a methyl group or an ethyl group.)

[0041] The compound (A-3) contains, for example, an aliphatic ring, an aromatic ring, a heterocyclic ring, a fluorine atom, an iodine atom, or a sulfur atom. The sulfur atom is preferably contained in the compound (A-3) as a sulfide bond, a disulfide bond, or a sulfonyl group.

[0042] Examples of the compound (A-3) include the following compounds:

[0043] The molecular weight of the compound (A-3) is not particularly limited, but may be, for example, 118 to 500. The molecular weight of 118 is the molecular weight of succinic acid.

[0044] The compound (A) is represented, for example, by the following formula (1). (In formula (1), R 1 R each independently represents a chain carbon-carbon double bond or a chain carbon-carbon triple bond which may be substituted with a hydrocarbon group having 1 to 6 carbon atoms. 2 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; each X independently represents -O- or -N(R)- (wherein R represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms); each Q independently represents a single bond or a divalent organic group.

[0045] R in formula (1) 1 Examples of the hydrocarbon group having 1 to 6 carbon atoms as an optional substituent in formula (1) include an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, and a phenyl group. 1 Examples of the group include the following groups: (* represents a bond.)

[0046] R in formula (1) 1 The —C(═O)— group is preferably a group represented by the above formula (1A) or a group represented by the above formula (1B).

[0047] R in formula (1) 2 is preferably a hydrogen atom or a methyl group, more preferably a hydrogen atom.

[0048] The divalent organic group for Q in formula (1) is, for example, represented by the following formula (2). In formula (2), A represents a residue obtained by removing hydrogen atoms bonded to oxygen atoms or nitrogen atoms of compound (A-3), and when compound (A-3) is an acid dianhydride, A represents a residue obtained by removing hydrogen atoms bonded to oxygen atoms from at least two carboxy groups of the corresponding tetracarboxylic acid. R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. T represents a residue obtained by removing a glycidyl group from a compound represented by formula (A-1-1). G represents a monovalent organic group. a* represents a bond on the X side in formula (1). b* represents a bond on the opposite side to X in formula (1). n is an integer of 1 or more.

[0049] In formula (2), G can further contain a partial structure of formula (2), so compound (A) is, for example, a hyperbranched polymer, a dendrimer, a linear polymer, a branched polymer, an oligomer thereof, or a low molecular weight compound.

[0050] The lower limit of the weight average molecular weight of the compound (A) is, for example, 500, 1,000, 2,000, or 3,000. The upper limit of the weight average molecular weight of the compound (A) is, for example, 30,000, 20,000, or 10,000.

[0051] The content of compound (A) in the composition for forming a resist underlayer film is not particularly limited, but from the viewpoint of suitably obtaining the effects of the present invention, it is preferably 40% by mass to 99% by mass, more preferably 45% by mass to 95% by mass, and particularly preferably 50% by mass to 90% by mass, based on the film-constituting components. In the present invention, the film-constituting components refer to components other than the solvent contained in the composition.

[0052] <Solvent (B)> The solvent (B) is not particularly limited and may be water or an organic solvent. Examples of the organic solvent include alkylene glycol monoalkyl ethers and monocarboxylic acid esters of alkylene glycol monoalkyl ethers.

[0053] Examples of the alkylene group of the alkylene glycol monoalkyl ether include alkylene groups having 2 to 4 carbon atoms. Examples of the alkyl group of the alkylene glycol monoalkyl ether include alkyl groups having 1 to 4 carbon atoms. Examples of the number of carbon atoms of the alkylene glycol monoalkyl ether include 3 to 8. Examples of the alkylene glycol monoalkyl ether include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether.

[0054] Examples of the alkylene group of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include alkylene groups having 2 to 4 carbon atoms. Examples of the alkyl group of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include alkyl groups having 1 to 4 carbon atoms. Examples of the monocarboxylic acid of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include saturated monocarboxylic acids having 2 to 4 carbon atoms. Examples of saturated monocarboxylic acids having 2 to 4 carbon atoms include acetic acid, propionic acid, and butyric acid. Examples of the number of carbon atoms of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include those having 5 to 10 carbon atoms. Examples of the monocarboxylic acid ester of alkylene glycol monoalkyl ether include methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, and propylene glycol propyl ether acetate.

[0055] Other organic solvents include, for example, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0056] Among these solvents (B), alkylene glycol monoalkyl ethers and monocarboxylic acid esters of alkylene glycol monoalkyl ethers are preferred.

[0057] These solvents (B) may be used alone or in combination of two or more.

[0058] The mass proportion of the organic solvent in the solvent (B) is not particularly limited, but is preferably 50 mass % to 100 mass %.

[0059] The content of the solvent (B) in the composition for forming a resist underlayer film is not particularly limited, but is preferably 50% by mass to 99.99% by mass, more preferably 75% by mass to 99.95% by mass, and particularly preferably 90% by mass to 99.9% by mass.

[0060] <Crosslinking Agent (C)> The crosslinking agent (C) is not particularly limited. The crosslinking agent (C) has a structure different from that of the compound (A).

[0061] The crosslinking agent (C) is preferably an aminoplast crosslinking agent or a phenoplast crosslinking agent. The aminoplast crosslinking agent is an addition condensation product of a compound having an amino group, such as melamine or guanamine, with formaldehyde. The phenoplast crosslinking agent is an addition condensation product of a compound having a phenolic hydroxy group with formaldehyde.

[0062] Examples of the crosslinking agent (C) include compounds having two or more of the following structures. (In the structure, R 101 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxyalkyl group having 2 to 6 carbon atoms. * represents a bond.) The bond is bonded to, for example, a nitrogen atom or a carbon atom constituting an aromatic hydrocarbon ring.

[0063] R 101 is preferably a hydrogen atom, a methyl group, an ethyl group or a group represented by the following structure. (In the structure, R 102 represents a hydrogen atom, a methyl group, or an ethyl group. * represents a bond.

[0064] The crosslinking agent (C) is preferably a melamine compound, a guanamine compound, a glycoluril compound, a urea compound, or a compound having a phenolic hydroxy group, which may be used alone or in combination of two or more.

[0065] Examples of the melamine compound include hexamethylol melamine, hexamethoxymethyl melamine, a compound in which 1 to 6 methylol groups of hexamethylol melamine have been methoxymethylated, or a mixture thereof, hexamethoxyethyl melamine, hexaacyloxymethyl melamine, a compound in which 1 to 6 methylol groups of hexamethylol melamine have been acyloxymethylated, or a mixture thereof.

[0066] Examples of the guanamine compound include tetramethylolguanamine, tetramethoxymethylguanamine, a compound in which one to four methylol groups of tetramethylolguanamine are methoxymethylated, or a mixture thereof; tetramethoxyethylguanamine, tetraacyloxyguanamine, a compound in which one to four methylol groups of tetramethylolguanamine are acyloxymethylated, or a mixture thereof; and the like.

[0067] Examples of glycoluril compounds include tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, compounds in which one to four methylol groups of tetramethylol glycoluril are methoxymethylated or mixtures thereof, and compounds in which one to four methylol groups of tetramethylol glycoluril are acyloxymethylated or mixtures thereof.

[0068] The glycoluril compound may be, for example, a glycoluril derivative represented by the following formula (1E). (In formula (1E), four R 1 each independently represents a methyl group or an ethyl group, R 2 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group.

[0069] Examples of the glycoluril derivative represented by the formula (1E) include compounds represented by the following formulas (1E-1) to (1E-6).

[0070] The glycoluril derivative represented by formula (1E) can be obtained, for example, by reacting a glycoluril derivative represented by the following formula (2E) with at least one compound represented by the following formula (3d).

[0071] (In formula (2E), R 2 and R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group; R 4 each independently represents an alkyl group having 1 to 4 carbon atoms.

[0072] (In formula (3d), R 1 represents a methyl group or an ethyl group.

[0073] Examples of glycoluril derivatives represented by formula (2E) include compounds represented by formulas (2E-1) to (2E-4) below. Furthermore, examples of compounds represented by formula (3d) include compounds represented by formulas (3d-1) and (3d-2) below.

[0074] Examples of the urea compound include tetramethylol urea, tetramethoxymethyl urea, tetramethylol urea compounds in which one to four methylol groups are methoxymethylated, or mixtures thereof, and tetramethoxyethyl urea.

[0075] Examples of the compound having a phenolic hydroxy group include compounds represented by the following formula (G-1) or (G-2). (In formula (G-1) and formula (G-2), Q 1 represents a single bond or a monovalent organic group. 1 and R 4 R represents an alkyl group having 2 to 10 carbon atoms, or an alkyl group having 2 to 10 carbon atoms and an alkoxy group having 1 to 10 carbon atoms. 2 and R 5 R represents a hydrogen atom or a methyl group. 3 and R 6 n represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. 1 is 1≦n 1 an integer ≦3, n 2 is 2≦n 2 n is an integer ≦5 3 is 0≦n 3 an integer ≦3, n 4 is 0≦n 4 an integer ≦3, 3≦(n 1 +n 2 +n 3 +n 4 ) represents an integer ≦6. 5 is 1≦n5 an integer ≦3, n 6 is 1≦n 6 n is an integer ≦4 7 is 0≦n 7 an integer ≦3, n 8 is 0≦n 8 an integer ≦3, 2≦(n 5 +n 6 +n 7 +n 8 ) represents an integer of ≦5. m1 represents an integer of 2 to 10.

[0076] Examples of compounds having a phenolic hydroxy group include compounds represented by the following formula (G-3) or formula (G-4): The compound represented by formula (G-1) or formula (G-2) may be obtained by reacting a compound represented by the following formula (G-3) or formula (G-4) with a hydroxyl group-containing ether compound or an alcohol having 2 to 10 carbon atoms. (In formula (G-3) and formula (G-4), Q 2 represents a single bond or a divalent organic group. 8 , R 9 , R 11 and R 12 R represents a hydrogen atom or a methyl group. 7 and R 10 n represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. 9 is 1≦n 9 an integer ≦3, n 10 is 2≦n 10 n is an integer ≦5 11 is 0≦n 11 an integer ≦3, n 12 is 0≦n 12 an integer ≦3, 3≦(n 9 +n 10 +n 11 +n 12 ) represents an integer ≦6. 13 is 1≦n 13 an integer ≦3, n 14 is 1≦n 14 n is an integer ≦4 15 is 0≦n 15 an integer ≦3, n 16 is 0≦n 16an integer ≦3, 2≦(n 13 +n 14 +n 15 +n 16 ) represents an integer of ≦5. m2 represents an integer of 2 to 10. 2 In the above, the m2-valent organic group includes, for example, an m2-valent organic group having 1 to 4 carbon atoms.

[0077] Examples of the compound represented by formula (G-1) or formula (G-2) include the following compounds:

[0078] Examples of the compound represented by formula (G-3) or formula (G-4) include the following compounds: The above compound is available as a product of Asahi Organic Chemicals Co., Ltd. and Honshu Chemical Industry Co., Ltd. An example of the product is TMOM-BP, a product name of Asahi Organic Chemicals Co., Ltd.

[0079] Among these, glycoluril compounds are preferred, specifically tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, tetramethylol glycoluril compounds in which one to four methylol groups have been methoxymethylated or mixtures thereof, and tetramethylol glycoluril compounds in which one to four methylol groups have been acyloxymethylated or mixtures thereof, with tetramethoxymethyl glycoluril being more preferred.

[0080] The molecular weight of the crosslinking agent (C) is not particularly limited, but is preferably 500 or less.

[0081] The content of the crosslinking agent (C) in the composition for forming a resist underlayer film is not particularly limited, but is, for example, 1% by mass to 70% by mass, and preferably 5% by mass to 60% by mass, relative to the compound (A).

[0082] <Curing Catalyst (D)> The curing catalyst (D) contained as an optional component in the composition for forming a resist underlayer film may be either a thermal acid generator or a photoacid generator, but it is preferable to use a thermal acid generator. Examples of the thermal acid generator include sulfonic acid compounds and carboxylic acid compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium-p-toluenesulfonate (pyridinium-p-toluenesulfonic acid), pyridinium phenolsulfonic acid, pyridinium-p-hydroxybenzenesulfonic acid (pyridinium p-phenolsulfonate salt), pyridinium-trifluoromethanesulfonic acid, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, hydroxybenzoic acid, N-methylmorpholine-p-toluenesulfonic acid, N-methylmorpholine-p-hydroxybenzenesulfonic acid, and N-methylmorpholine-5-sulfosalicylic acid.

[0083] Examples of the photoacid generator include an onium salt compound, a sulfonimide compound, and a disulfonyldiazomethane compound.

[0084] Examples of the onium salt compound include iodonium salt compounds such as diphenyliodonium hexafluorophosphate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nonafluoro-normal butanesulfonate, diphenyliodonium perfluoro-normal octanesulfonate, diphenyliodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium camphorsulfonate, and bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate; and sulfonium salt compounds such as triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoro-normal butanesulfonate, triphenylsulfonium camphorsulfonate, and triphenylsulfonium trifluoromethanesulfonate.

[0085] Examples of the sulfonimide compound include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoronormalbutanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, and N-(trifluoromethanesulfonyloxy)naphthalimide.

[0086] Examples of the disulfonyldiazomethane compound include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, and methylsulfonyl-p-toluenesulfonyldiazomethane.

[0087] The curing catalyst (D) may be used alone or in combination of two or more.

[0088] When the curing catalyst (D) is used, the content of the curing catalyst (D) relative to the crosslinking agent (C) is, for example, 0.1% by mass to 50% by mass, and preferably 1% by mass to 30% by mass.

[0089] <Other Components> A surfactant may be further added to the composition for forming a resist underlayer film in order to prevent pinholes, striations, and the like from occurring and to further improve the coatability against surface irregularities.

[0090] Examples of surfactants include linear or branched alkylbenzenesulfonic acids (e.g., dodecylbenzenesulfonic acid, etc.), polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether, polyoxyethylene-polyoxypropylene block copolymers, sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate, and polyoxyethylene sorbitan monolaurate. nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; fluorine-based surfactants such as Eftop EF301, EF303, and EF352 (trade names, manufactured by Tochem Products Co., Ltd.), Megafac F171, F173, and R-30 (trade names, manufactured by DIC Corporation), Fluorad FC430 and FC431 (trade names, manufactured by Sumitomo 3M Limited), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (trade names, manufactured by AGC Inc.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The amount of these surfactants to be added is usually 2.0 mass % or less, and preferably 1.0 mass % or less, based on the total solid content of the composition for forming a resist underlayer film. These surfactants may be added alone or in combination of two or more.

[0091] The solid content of the composition for forming a resist underlayer film of the present invention, that is, the content of components excluding the solvent, is, for example, 0.01% by mass to 10% by mass.

[0092] (Resist Underlayer Film) The resist underlayer of the present invention is a cured product of the composition for forming a resist underlayer film described above. The resist underlayer film can be produced, for example, by applying the composition for forming a resist underlayer film described above onto a semiconductor substrate and baking it.

[0093] Examples of semiconductor substrates onto which the resist underlayer film-forming composition can be applied include silicon wafers, germanium wafers, and wafers of compound semiconductors such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.

[0094] When a semiconductor substrate having an inorganic film formed on its surface is used, the inorganic film can be formed by, for example, ALD (atomic layer deposition), CVD (chemical vapor deposition), reactive sputtering, ion plating, vacuum deposition, or spin coating (spin-on glass: SOG). Examples of the inorganic film include a polysilicon film, a silicon oxide film, a silicon nitride film, a BPSG (Boro-Phospho Silicate Glass) film, a titanium nitride film, a titanium nitride oxide film, a tungsten film, a gallium nitride film, and a gallium arsenide film.

[0095] The resist underlayer film-forming composition of the present invention is applied to such a semiconductor substrate by a suitable application method such as a spinner or coater. The composition is then baked using a heating means such as a hot plate to form a resist underlayer film. The baking conditions are appropriately selected from a baking temperature of 100°C to 400°C and a baking time of 0.3 to 60 minutes. A baking temperature of 120°C to 350°C and a baking time of 0.5 to 30 minutes are preferred, and a baking temperature of 150°C to 300°C and a baking time of 0.8 to 10 minutes are more preferred.

[0096] The thickness of the resist underlayer film may be, for example, 0.001 μm (1 nm) to 10 μm, 0.002 μm (2 nm) to 1 μm, 0.005 μm (5 nm) to 0.5 μm (500 nm), 0.001 μm (1 nm) to 0.05 μm (50 nm), 0.002 μm (2 nm) to 0.05 μm (50 nm), 0.003 μm (3 nm) to 0.05 μm (50 nm), 0.004 μm (4 nm) to 0.05 μm (50 nm), 0.005 μm (5 nm) to 0.05 μm (5 0 nm), 0.003 μm (3 nm) to 0.03 μm (30 nm), 0.003 μm (3 nm) to 0.02 μm (20 nm), 0.005 μm (5 nm) to 0.02 μm (20 nm), 0.005 μm (5 nm) to 0.02 μm (20 nm), 0.003 μm (3 nm) to 0.01 μm (10 nm), 0.005 μm (5 nm) to 0.01 μm (10 nm), 0.003 μm (3 nm) to 0.006 μm (6 nm), or 0.005 μm (5 nm).

[0097] The method for measuring the film thickness of the resist underlayer film in this specification is as follows: Name of measuring device: Ellipso film thickness measuring device RE-3100 (SCREEN Corporation) SWE (single wavelength ellipsometer) mode Arithmetic mean of 8 points (for example, measuring 8 points at 1 cm intervals in the X direction of the wafer)

[0098] (Laminate) The laminate of the present invention includes a semiconductor substrate and the resist underlayer film of the present invention. Examples of the semiconductor substrate include the semiconductor substrates described above. The resist underlayer film is disposed on the semiconductor substrate, for example.

[0099] (Method for manufacturing a semiconductor element, method for forming a pattern) The method for manufacturing a semiconductor element of the present invention includes at least the following steps: forming a resist underlayer film on a semiconductor substrate using the composition for forming a resist underlayer film of the present invention, and forming a resist film on the resist underlayer film.

[0100] The pattern forming method of the present invention includes at least the following steps: forming a resist underlayer film on a semiconductor substrate using the composition for forming a resist underlayer film of the present invention, forming a resist film on the resist underlayer film, irradiating the resist film with light or an electron beam and then developing the resist film to obtain a resist pattern, and etching the resist underlayer film using the resist pattern as a mask.

[0101] Typically, a resist layer is formed on the resist underlayer film. The film thickness of the resist layer is, for example, 3,000 nm or less, 2,000 nm or less, 1,800 nm or less, 1,500 nm or less, or 1,000 nm or less. The lower limit is 100 nm, 80 nm, 50 nm, 30 nm, 20 nm, or 10 nm.

[0102] The resist film formed on the resist underlayer film by a known method (e.g., coating and baking a resist composition) is not particularly limited as long as it is responsive to light or electron beam (EB) irradiation. Both negative and positive photoresists can be used. In this specification, resists responsive to EB are also referred to as photoresists. Examples of photoresists include positive photoresists composed of a novolak resin and a 1,2-naphthoquinone diazide sulfonic acid ester; chemically amplified photoresists composed of a binder having a group that decomposes in the presence of an acid to increase the alkaline dissolution rate and a photoacid generator; chemically amplified photoresists composed of a low-molecular-weight compound that decomposes in the presence of an acid to increase the alkaline dissolution rate of the photoresist, an alkali-soluble binder, and a photoacid generator; chemically amplified photoresists composed of a binder having a group that decomposes in the presence of an acid to increase the alkaline dissolution rate, a low-molecular-weight compound that decomposes in the presence of an acid to increase the alkaline dissolution rate of the photoresist, and a photoacid generator; and resists containing metal elements. Examples of such photoresists include V146G (trade name) manufactured by JSR Corporation, APEX-E (trade name) manufactured by Shipley Co., Ltd., PAR710 (trade name) manufactured by Sumitomo Chemical Co., Ltd., and AR2772 and SEPR430 (trade names) manufactured by Shin-Etsu Chemical Co., Ltd. Further examples include fluorine-containing polymer photoresists such as those described in Proc. SPIE, Vol. 3999, 330-334 (2000), Proc. SPIE, Vol. 3999, 357-364 (2000), and Proc. SPIE, Vol. 3999, 365-374 (2000).

[0103] Also, WO2019 / 188595, WO2019 / 187881, WO2019 / 187803, WO2019 / 167737, WO2019 / 167725, WO2019 / 187445, WO2019 / 167419, WO2019 / 123842, WO2019 / 054282, WO2019 / 058945, WO2019 / 058890, WO2019 / 039290, WO2019 / 044259, WO2019 / 044231, WO2019 / 026549, WO2018 / 193954, WO201 9 / 172054, WO2019 / 021975, WO2018 / 230334, WO2018 / 194123, JP 2018-180525, WO2018 / 190088, JP 2018-070596, JP 2018-028090, JP 2016-153409, JP 2016-130240, JP 2016-108325, JP 2016-047920, JP 2016-035570, JP 2016-035567, JP 2016-035565, JP 2019-101417, JP 2019-117373, JP 2019-052294, JP 2019-008280, JP 2019-008279, JP 2019-003176, JP 2019-003175, JP 2018-197853, JP 2019-191298, JP 2019-061217, JP 2018-045152, JP 2018-022039, JP 2016-090441, JP 2015-10878, JP 2012-168279, JP 2012-022261, JP 2012-022258, JP 2011-043749, JP 2010-18 1857, JP 2010-128369, WO2018 / 031896, JP 2019-113855, WO2017 / 156388, WO2017 / 066319, JP 2018-41099, WO2016 / 065120, WO2015 / 026482, JP 2016-29498, JP 2011-253185, etc., radiation-sensitive resin compositions, so-called resist compositions such as high-resolution patterning compositions based on organometallic solutions, and metal-containing resist compositions can be used, but are not limited to these.

[0104] Examples of the resist composition include the following compositions.

[0105] An actinic ray-sensitive or radiation-sensitive resin composition comprising: Resin A having a repeating unit having an acid-decomposable group in which a polar group is protected with a protecting group that is cleaved by the action of an acid; and a compound represented by the following general formula (121):

[0106] In the general formula (121), m represents an integer of 1 to 6. 1 and R 2 each independently represents a fluorine atom or a perfluoroalkyl group. 1 is -O-, -S-, -COO-, -SO 2 - or -SO 3 - represents. 2 represents an alkylene group which may have a substituent or a single bond. 1 represents a cyclic organic group which may have a substituent. + represents a cation.

[0107] A metal-containing film-forming composition for extreme ultraviolet or electron beam lithography, comprising a compound having a metal-oxygen covalent bond and a solvent, wherein the metal element constituting the compound belongs to Periods 3 to 7 of Groups 3 to 15 of the periodic table.

[0108] A radiation-sensitive resin composition comprising: a polymer having a first structural unit represented by the following formula (31) and a second structural unit represented by the following formula (32) containing an acid-dissociable group; and an acid generator.

[0109] In formula (31), Ar is a group obtained by removing (n+1) hydrogen atoms from an arene having 6 to 20 carbon atoms. 1 is a hydroxy group, a sulfanyl group, or a monovalent organic group having 1 to 20 carbon atoms. n is an integer of 0 to 11. When n is 2 or more, multiple R 1 are the same or different. 2 is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group. 3 is a monovalent group having 1 to 20 carbon atoms containing the above acid-dissociable group. Z is a single bond, an oxygen atom, or a sulfur atom. R 4is a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group.

[0110] A resist composition comprising: a resin (A1) containing a structural unit having a cyclic carbonate structure, a structural unit represented by the following formula, and a structural unit having an acid labile group; and an acid generator.

[0111] [In the formula, R 2 represents an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, a hydrogen atom or a halogen atom; X 1 represents a single bond, —CO—O—*, or —CO—NR 4 -*, * represents a bond to -Ar, R 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and Ar represents an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have one or more groups selected from the group consisting of a hydroxy group and a carboxyl group.]

[0112] Examples of the resist film include the following.

[0113] A resist film comprising a base resin comprising a repeating unit represented by the following formula (a1) and / or a repeating unit represented by the following formula (a2), and a repeating unit that generates an acid bonded to a polymer main chain upon exposure:

[0114] (In formula (a1) and formula (a2), R A are each independently a hydrogen atom or a methyl group. 1 and R 2 are each independently a tertiary alkyl group having 4 to 6 carbon atoms. 3 are each independently a fluorine atom or a methyl group, and m is an integer of 0 to 4. 1 X is a single bond, a phenylene group, or a naphthylene group, or a linking group having 1 to 12 carbon atoms and containing at least one selected from an ester bond, a lactone ring, a phenylene group, and a naphthylene group. 2 is a single bond, an ester bond, or an amide bond.

[0115] Examples of resist materials include the following:

[0116] A resist material comprising a polymer having a repeating unit represented by the following formula (b1) or (b2):

[0117] (In formula (b1) and formula (b2), R A is a hydrogen atom or a methyl group. 1 is a single bond or an ester group. 2 is a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms or an arylene group having 6 to 10 carbon atoms, and some of the methylene groups constituting the alkylene group may be substituted with an ether group, an ester group or a lactone ring-containing group; and X 2 At least one hydrogen atom contained in X is substituted with a bromine atom. 3 Rf is a single bond, an ether group, an ester group, or a linear, branched, or cyclic alkylene group having 1 to 12 carbon atoms, and some of the methylene groups constituting the alkylene group may be substituted with an ether group or an ester group. 1 ~Rf 4 are each independently a hydrogen atom, a fluorine atom, or a trifluoromethyl group, but at least one is a fluorine atom or a trifluoromethyl group. 1 and Rf 2 may combine to form a carbonyl group. 1 ~R 5 are each independently a linear, branched, or cyclic alkyl group having 1 to 12 carbon atoms, a linear, branched, or cyclic alkenyl group having 2 to 12 carbon atoms, an alkynyl group having 2 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or an aryloxyalkyl group having 7 to 12 carbon atoms, in which some or all of the hydrogen atoms may be substituted with a hydroxy group, a carboxy group, a halogen atom, an oxo group, a cyano group, an amide group, a nitro group, a sultone group, a sulfone group, or a sulfonium salt-containing group, and in which some of the methylene groups constituting these groups may be substituted with an ether group, an ester group, a carbonyl group, a carbonate group, or a sulfonate ester group. 1 and R 2may be bonded to form a ring together with the sulfur atom to which they are attached.

[0118] A resist material comprising a base resin containing a polymer containing a repeating unit represented by the following formula (a):

[0119] (In formula (a), R A is a hydrogen atom or a methyl group. 1 is a hydrogen atom or an acid labile group. 2 is a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, or a halogen atom other than bromine. 1 X is a single bond, a phenylene group, or a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms which may contain an ester group or a lactone ring. 2 is -O-, -O-CH 2 - or -NH-. m is an integer of 1 to 4. u is an integer of 0 to 3. However, m+u is an integer of 1 to 4.

[0120] A resist composition that generates an acid upon exposure, and whose solubility in a developer changes due to the action of the acid, comprising: a base component (A) whose solubility in a developer changes due to the action of the acid; and a fluorine additive component (F) that exhibits decomposition in an alkaline developer, wherein the fluorine additive component (F) comprises a fluororesin component (F1) that has a structural unit (f1) that includes a base dissociable group, and a structural unit (f2) that includes a group represented by the following general formula (f2-r-1):

[0121] [In formula (f2-r-1), Rf 21 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a hydroxy group, a hydroxyalkyl group, or a cyano group. n" is an integer of 0 to 2. * is a bond.

[0122] The structural unit (f1) includes a structural unit represented by the following general formula (f1-1) or a structural unit represented by the following general formula (f1-2).

[0123] [In formulas (f1-1) and (f1-2), each R is independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. X is a divalent linking group that does not have an acid-dissociable site. A aryl represents a divalent aromatic cyclic group which may have a substituent. 01 is a single bond or a divalent linking group. 2 are each independently an organic group having a fluorine atom.

[0124] Coatings, coating solutions, and coating compositions include, for example:

[0125] A coating comprising a metal oxo-hydroxo network having organic ligands with metal carbon and / or metal carboxylate bonds.

[0126] Inorganic oxo / hydroxo-based compositions.

[0127] a coating solution comprising an organic solvent; a first organometallic composition having the formula R z SnO (2-(z/2)-(x/2)) (OH) x (where 0<z≦2 and 0<(z+x)≦4), formula R′ n SnX 4-n wherein n=1 or 2, or mixtures thereof, where R and R′ are independently hydrocarbyl groups having 1 to 31 carbon atoms, and X is a ligand having a hydrolyzable bond to Sn, or a combination thereof; and a hydrolyzable metal compound having the formula MX′ v wherein M is a metal selected from groups 2 to 16 of the periodic table of the elements, v is a number from 2 to 6, and X' is a ligand having a hydrolyzable M-X bond or a combination thereof.

[0128] an organic solvent and a solution of the formula RSnO (3/2-x/2) (OH) xand a first organometallic compound of the formula: wherein 0<x<3, wherein the solution contains from about 0.0025M to about 1.5M tin, and R is an alkyl or cycloalkyl group having from 3 to 31 carbon atoms, the alkyl or cycloalkyl group being bonded to the tin at a secondary or tertiary carbon atom.

[0129] An aqueous inorganic patterning precursor solution comprising a mixture of water, metal suboxide cations, polyatomic inorganic anions, and radiation-sensitive ligands comprising peroxide groups.

[0130] Irradiation with light or electron beams is carried out, for example, through a mask (reticle) for forming a predetermined pattern. For example, i-line, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet), or EB (electron beam) can be used. The composition for forming a resist underlayer film of the present invention is preferably applied for EB (electron beam) or EUV (extreme ultraviolet: 13.5 nm) irradiation, more preferably for EUV (extreme ultraviolet) exposure. The irradiation energy of the electron beam and the exposure dose of light are not particularly limited.

[0131] After irradiation with light or electron beams and before development, baking (PEB: Post Exposure Bake) may be performed. The baking temperature is not particularly limited, but is preferably 60° C. to 150° C., more preferably 70° C. to 120° C., and particularly preferably 75° C. to 110° C. The baking time is not particularly limited, but is preferably 1 second to 10 minutes, more preferably 10 seconds to 5 minutes, and particularly preferably 30 seconds to 3 minutes.

[0132] For example, an alkaline developer is used for development. The development temperature can be, for example, 5°C to 50°C. The development time can be, for example, 10 seconds to 300 seconds. Examples of alkaline developers that can be used include aqueous solutions of alkalis such as inorganic alkalis (e.g., sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and aqueous ammonia); primary amines (e.g., ethylamine and n-propylamine); secondary amines (e.g., diethylamine and di-n-butylamine); tertiary amines (e.g., triethylamine and methyldiethylamine); alcohol amines (e.g., dimethylethanolamine and triethanolamine); quaternary ammonium salts (e.g., tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline); and cyclic amines (e.g., pyrrole and piperidine). Furthermore, the aqueous solutions of the alkalis can be used by adding an appropriate amount of alcohols (e.g., isopropyl alcohol) or a nonionic surfactant. Among these, preferred developers are aqueous solutions of quaternary ammonium salts, more preferably aqueous solutions of tetramethylammonium hydroxide and choline. Furthermore, surfactants and the like can also be added to these developers. Alternatively, development may be carried out with an organic solvent such as butyl acetate instead of an alkaline developer, and the portions of the photoresist where the alkaline dissolution rate is not improved may be developed.

[0133] Next, the resist underlayer film is etched using the formed resist pattern as a mask. The etching may be dry etching or wet etching, but dry etching is preferred. If the inorganic film is formed on the surface of the semiconductor substrate used, the surface of the inorganic film is exposed. If the inorganic film is not formed on the surface of the semiconductor substrate used, the surface of the semiconductor substrate is exposed. Thereafter, the semiconductor substrate is processed by a known method (e.g., dry etching), thereby manufacturing a semiconductor device.

[0134] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples.

[0135] The weight-average molecular weights of the polymers shown in the following Synthesis Examples 1 to 4 and Comparative Synthesis Example 1 are the results of measurement by gel permeation chromatography (hereinafter abbreviated as GPC). A GPC device manufactured by Tosoh Corporation was used for the measurement, and the measurement conditions were as follows: GPC column: Shodex GF-710HQ, Shodex GF-510HQ, Shodex GF-310HQ (registered trademark) (Showa Denko K.K.) Column temperature: 40°C Flow rate: 0.6 ml / min Eluent: N,N-dimethylformamide (DMF) Standard sample: polystyrene (Tosoh Corporation)

[0136] Synthesis Example 1 10.00 g of triglycidyl isocyanuric acid (Nissan Chemical Industries, Ltd.), 9.41 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.), 0.36 g of dibutylhydroxytoluene (Tokyo Chemical Industry Co., Ltd.), and 0.56 g of tetrabutylphosphonium bromide (ACROSS) were added to 30.50 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. After purging the reaction vessel with nitrogen, the reaction was carried out at 90°C for 24 hours to obtain a product solution. The product solution did not become cloudy even when cooled to room temperature, and had good solubility in propylene glycol monomethyl ether. GPC analysis revealed that the product in the obtained solution had a weight average molecular weight of 600 in terms of standard polystyrene. The reaction product obtained in this synthesis example has a structure represented by the following formulas (1a) and (1b).

[0137]

[0138] Synthesis Example 2 3.00 g of triglycidyl isocyanuric acid (Nissan Chemical Industries, Ltd.), 7.09 g of acrylic acid (Tokyo Chemical Industry Co., Ltd.), 0.11 g of dibutylhydroxytoluene (Tokyo Chemical Industry Co., Ltd.), and 0.12 g of tetrabutylphosphonium bromide (ACROSS) were added to 15.47 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. After purging the reaction vessel with nitrogen, the reaction was carried out at 90°C for 24 hours to obtain a product solution. The product solution did not become cloudy even when cooled to room temperature, and had good solubility in propylene glycol monomethyl ether. GPC analysis showed that the product in the obtained solution had a weight average molecular weight of 600 in terms of standard polystyrene. The reaction products obtained in this synthesis example have structures represented by the following formulas (1a) and (2b).

[0139]

[0140] Synthesis Example 3 10.00 g of triglycidyl isocyanuric acid (manufactured by Nissan Chemical Industries, Ltd.), 5.57 g of 3,3'-dithiodipropionic acid (manufactured by Sakai Chemical Industry Co., Ltd., trade name: DTDPA), 3.99 g of methacrylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.36 g of dibutylhydroxytoluene (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.56 g of tetrabutylphosphonium bromide (manufactured by ACROSS) were added to 24.74 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. The atmosphere in the reaction vessel was replaced with nitrogen, and the reaction was carried out at 90°C for 24 hours to obtain a polymer solution. The polymer solution did not become cloudy even when cooled to room temperature, and the solubility in propylene glycol monomethyl ether was good. GPC analysis revealed that the polymer in the obtained solution had a weight average molecular weight of 6,000 in terms of standard polystyrene. The polymers obtained in this synthesis example have structures represented by the following formulas (1a), (2a), and (1b).

[0141]

[0142] Synthesis Example 4 10.00 g of triglycidyl isocyanuric acid (Nissan Chemical Industries, Ltd.), 4.73 g of phthalic acid (Tokyo Chemical Industry Co., Ltd.), 4.29 g of methacrylic acid (Tokyo Chemical Industry Co., Ltd.), 0.39 g of dibutylhydroxytoluene (Tokyo Chemical Industry Co., Ltd.), and 0.60 g of tetrabutylphosphonium bromide (ACROSS) were added to 23.59 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. After replacing the atmosphere in the reaction vessel with nitrogen, the reaction was carried out at 90°C for 24 hours to obtain a polymer solution. The polymer solution did not become cloudy even when cooled to room temperature, and had good solubility in propylene glycol monomethyl ether. GPC analysis revealed that the polymer in the obtained solution had a weight average molecular weight of 6000 in terms of standard polystyrene. The polymer obtained in this synthesis example has a structure represented by the following formulas (1a), (3a), and (1b).

[0143]

[0144] Synthesis Example 5 10.00 g of triglycidyl isocyanuric acid (Nissan Chemical Industries, Ltd.), 11.62 g of sorbic acid (Tokyo Chemical Industry Co., Ltd.), 0.36 g of dibutylhydroxytoluene (Tokyo Chemical Industry Co., Ltd.), and 0.68 g of tetrabutylphosphonium bromide (ACROSS) were added to 30.50 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. After purging the reaction vessel with nitrogen, the reaction was carried out at 90°C for 24 hours to obtain a product solution. The product solution did not become cloudy even when cooled to room temperature, and had good solubility in propylene glycol monomethyl ether. GPC analysis showed that the product in the obtained solution had a weight average molecular weight of 800 in terms of standard polystyrene. The reaction products obtained in this synthesis example have structures represented by the following formulas (1a) and (3b).

[0145]

[0146] Comparative Synthesis Example 1 5.00 g of triglycidyl isocyanuric acid (Nissan Chemical Industries, Ltd.), 4.01 g of butanoic acid (Tokyo Chemical Industry Co., Ltd.), and 0.20 g of tetrabutylphosphonium bromide (ACROSS) were added to 12.12 g of propylene glycol monomethyl ether in a reaction vessel and dissolved. After replacing the atmosphere in the reaction vessel with nitrogen, the reaction was carried out at 90°C for 24 hours to obtain a product solution. The product solution did not become cloudy even when cooled to room temperature, and had good solubility in propylene glycol monomethyl ether. GPC analysis showed that the product in the obtained solution had a weight-average molecular weight of 600 in terms of standard polystyrene. The reaction products obtained in this synthesis example have structures represented by the following formulas (1a) and (3b).

[0147]

[0148] Examples and Comparative Examples The compounds or polymers obtained in Synthesis Examples 1 to 5 and Comparative Synthesis Example 1 above were mixed with a crosslinking agent, a curing catalyst, and a solvent in the proportions shown in Table 1, and the mixture was filtered through a 0.1 μm fluororesin filter to prepare solutions of compositions for forming resist underlayer films. The amounts of each component added are shown in parts by mass, and the solvents are shown in composition ratios. The abbreviations in Table 1 are as follows: PL-LI: tetramethoxymethylglycoluril Py-PSA: pyridinium-p-hydroxybenzenesulfonic acid PGMEA: propylene glycol monomethyl ether acetate PGME: propylene glycol monomethyl ether

[0149]

[0150] (Elution test into photoresist solvent) Each of the resist underlayer film-forming compositions of Examples 1 to 5 and Comparative Example 1 was applied onto a silicon wafer using a spinner. The silicon wafer was baked on a hot plate at 205°C for 60 seconds to obtain a resist underlayer film with a film thickness of 5 nm. These resist underlayer films were immersed in a mixed solution of propylene glycol monomethyl ether acetate / propylene glycol monomethyl ether = 70 / 30 (mass ratio), which is a solvent used in photoresists, and the results are shown in Table 2, with a film thickness change of 5 Å or less being rated as "good" and a film thickness change of more than 5 Å being rated as "poor."

[0151]

[0152] (Resist Patterning Evaluation) [Resist Pattern Formation Test Using Electron Beam Lithography Apparatus] Each of the resist underlayer film-forming compositions of Examples 1 to 4 and Comparative Example 1 was applied to a silicon wafer using a spinner. The silicon wafer was baked on a hot plate at 205°C for 60 seconds to obtain a 5 nm-thick resist underlayer film. An EUV positive resist solution was spin-coated onto the resist underlayer film and heated at 130°C for 60 seconds to form an EUV resist film. The resist film was exposed under specified conditions using an electron beam lithography apparatus (ELS-G130). After exposure, the resist was baked at 90°C for 60 seconds (PEB), cooled to room temperature on a cooling plate, and developed with an alkaline developer (2.38% TMAH), forming a 30 nm line-and-space pattern / 60 nm pitch resist pattern. A scanning electron microscope (CG4100, manufactured by Hitachi High-Technologies Corporation) was used to measure the resist pattern. A scanning electron microscope (CG4100, manufactured by Hitachi High-Technologies Corporation) was used to measure the length of the resist pattern. In forming the above resist patterns, LWR (Line Width Roughness) at a CD size of 30 nm was compared. The results are shown in Table 3.

[0153]

[0154] All of Examples 1 to 4 showed better LWR than Comparative Example 1. From the above results, it is clear that the use of compound (A) makes it possible to form a resist pattern with good LWR.

Claims

1. A composition for forming a resist underlayer film, comprising a compound (A) having a side chain or terminal having a linear α,β-unsaturated carbonyl group, and a solvent (B).

2. The composition for forming a resist underlayer film according to claim 1, wherein the compound (A) has a total of 3 or more chain-like α,β-unsaturated carbonyl groups.

3. The composition for forming a resist underlayer film according to claim 1, wherein the compound (A) is a reaction product of a reactant containing a compound (A-1) having an epoxy group and a compound (A-2) having a linear α,β-unsaturated carbonyl group and capable of reacting with the epoxy group.

4. The composition for forming a resist underlayer film according to claim 3, wherein the reactant further comprises a compound (A-3) having two or more groups capable of reacting with an epoxy group.

5. The composition for forming a resist underlayer film according to claim 4, wherein the compound (A-3) is a compound having two groups capable of reacting with an epoxy group.

6. The composition for forming a resist underlayer film according to claim 1, wherein the compound (A) is represented by the following formula (1): (In formula (1), R 1 R each independently represents a chain carbon-carbon double bond or a chain carbon-carbon triple bond which may be substituted with a hydrocarbon group having 1 to 6 carbon atoms. 2 Each X independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Each X independently represents -O- or -N(R)- (R represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms). Each Q independently represents a single bond or a divalent organic group.

7. The composition for forming a resist underlayer film according to claim 1, wherein the solvent (B) comprises at least one selected from the group consisting of alkylene glycol monoalkyl ethers and monocarboxylic acid esters of alkylene glycol monoalkyl ethers.

8. The composition for forming a resist underlayer film according to claim 1, further comprising a crosslinking agent (C).

9. The composition for forming a resist underlayer film according to claim 8, wherein the crosslinking agent (C) is at least one selected from the group consisting of aminoplast crosslinking agents and phenoplast crosslinking agents.

10. The composition for forming a resist underlayer film according to claim 1, further comprising a curing catalyst (D).

11. A resist underlayer film which is a cured product of the composition for forming a resist underlayer film according to any one of claims 1 to 10.

12. A laminate comprising: a semiconductor substrate; and the resist underlayer film according to claim 11.

13. A method for manufacturing a semiconductor device, comprising: a step of forming a resist underlayer film on a semiconductor substrate using a composition for forming a resist underlayer film according to any one of claims 1 to 10; and a step of forming a resist film on the resist underlayer film.

14. A pattern formation method comprising the steps of: forming a resist underlayer film on a semiconductor substrate using a composition for forming a resist underlayer film according to any one of claims 1 to 10; forming a resist film on the resist underlayer film; irradiating the resist film with light or an electron beam and then developing the resist film to obtain a resist pattern; and etching the resist underlayer film using the resist pattern as a mask.

Citation Information

Patent Citations

  • Positive resist composition and resist pattern forming method

    JP2010128369A

  • Positive resist composition, resist pattern forming method, and polymer compound

    JP2010181857A

  • Positive resist composition, resist pattern forming method and polymeric compound

    JP2011043749A

  • Patterned inorganic layers, radiation based patterning compositions and corresponding methods

    JP2011253185A

  • Positive resist composition and resist pattern formation method

    JP2012022258A