Wire rod, steel wire, and machine component

The wire rod with specific chemical composition and bainite structure addresses the low yield strength and high elongation issues in non-thermal bolts, achieving high strength and formability without the need for bluing, enhancing processing efficiency and reducing costs.

WO2024204819A1PCT designated stage expired Publication Date: 2024-10-03NIPPON STEEL CORPORATION

Patent Information

Application Number
PCT/JP2024/013327
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional non-thermal bolts face challenges with high dislocation density leading to low 0.2% yield strength and large permanent elongation, making them difficult to apply to high-strength bolts, and require a bluing process to maintain material properties, which is costly and inefficient.

Method used

A wire rod with a chemical composition of C: 0.08-0.80%, Si: 0.03-1.50%, Mn: 0.50-2.00%, and a bainite area ratio of 70% or more at 1/4D depth, achieving a 0.05% proof stress to tensile strength ratio of 0.72-0.40, and a standard deviation of Vickers hardness of 0.150 or less, allowing for high 0.2% proof stress without bluing treatment.

Benefits of technology

The solution provides mechanical parts with excellent strength and formability, achieving high 0.2% yield strength and suppressing permanent elongation, even without the bluing treatment, resulting in improved processing and reduced material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This wire rod has a predetermined chemical composition, in which: when the diameter of the wire rod is noted as D, the metal structure in a 1 / 4 D part, which is a part found in a cross section taken perpendicular to the length direction of the wire rod, at the depth of 1 / 4 D from the surface of the wire rod, includes bainite which accounts for an area ratio of 70% or more; the ratio of 0.05% yield strength to tensile strength (0.05% yield strength / tensile strength) is 0.72-0.40 × (C%) or more, where (C%) is the content of C in mass%; and a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the length direction of the wire rod by the average value of Vickers hardness is 0.150 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Wire rods, steel wires, and machine parts

[0001] The present disclosure relates to wire rods, steel wires, and machine parts.

[0002] High-strength materials are required for machine parts such as steel bolts and screws in order to reduce their weight and size. Conventionally, these machine parts have been manufactured by softening a steel wire rod for machine structures containing C, Mn, Cr, Mo, etc. through spheroidizing annealing, then forming it into a predetermined shape through cold heading or rolling, and then quenching and tempering it to impart strength.

[0003] Heat treatments such as spheroidizing annealing and quenching / tempering reduce manufacturing costs and CO 2 In order to increase the amount of discharged bolts, non-heat treated bolts are known, which are manufactured by omitting these heat treatments and instead increasing the strength of wire rod by adjusting the composition or by rapid cooling, and then by wiredrawing the wire rod to impart strength to the bolts. Various wire rods and steel wires for manufacturing machine parts such as non-heat treated bolts have been proposed (see, for example, Patent Documents 1 to 6).

[0004] Patent Document 1: JP 2-166229 A Patent Document 2: WO 2016 / 121820 Patent Document 3: WO 2017 / 122830 Patent Document 4: WO 2018 / 008698 Patent Document 5: JP 2021-183710 A Patent Document 6: JP 3-6325 A

[0005] Non-heat treated bolts are made by forming steel wire that has been strengthened by wire drawing. As the strength of the steel wire increases, the mold becomes more susceptible to damage and wear during forming, and the product is more susceptible to processing cracks, making it difficult to apply to high-strength bolts. Furthermore, conventional non-heat treated bolts have a high dislocation density, resulting in low 0.2% yield strength, which results in high permanent elongation. To address this issue, a bluing process is required after forming into mechanical parts such as bolts, in which the bolts are held at 300-400°C.

[0006] An object of the present disclosure is to provide a wire rod and steel wire for obtaining mechanical parts that are excellent in strength and formability, and that can achieve high 0.2% yield strength and suppressed permanent elongation even when a bluing treatment is omitted after molding into the mechanical parts, and to provide the mechanical parts.

[0007] The above-mentioned problems are solved by the following means. <1> In mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, A wire rod having a chemical composition consisting of Sb: 0 to 0.005%, and Ca: 0 to 0.0050%, with the balance consisting of Fe and impurity elements, wherein, when the diameter of the wire rod is D, a metal structure at a 1 / 4D portion that is 1 / 4D deep from the surface of the wire rod in a cross section perpendicular to the longitudinal direction of the wire rod contains bainite at an area ratio of 70% or more, wherein, when the content of C in mass % is (C%), the ratio of 0.05% proof stress to tensile strength (0.05% proof stress / tensile strength) is 0.72-0.40 × (C%) or more, and a value obtained by dividing the standard deviation of Vickers hardness in the cross section perpendicular to the longitudinal direction of the wire rod by the average value of the Vickers hardness is 0.150 or less.<2> In mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, a steel wire having a chemical composition consisting of Sb: 0 to 0.005%, and Ca: 0 to 0.0050%, with the balance consisting of Fe and impurity elements; where d is the diameter of the steel wire, a metal structure at a 1 / 4d portion that is 1 / 4d deep from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire contains bainite at an area ratio of 70% or more; where (C%) is the C content in mass %, the tensile strength is 610 + 900 × (C%) MPa or more, the reduction of area is 62 - 32 × (C%)% or more, the tensile strength (MPa) × reduction of area (%) is 52,000 or more, the ratio of 0.2% proof stress to tensile strength (0.2% proof stress / tensile strength) is 0.985 - 0.083 × (C%) or more; and a value obtained by dividing the standard deviation of Vickers hardness in the cross section perpendicular to the longitudinal direction of the steel wire by the average value of the Vickers hardness is 0.150 or less.<3> A mechanical part including a shaft portion, comprising, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, Ti: 0 to 0.050%, B: 0 to 0.0050%, Cr: 0 to 1.50%, Mo: 0 to 0.50%, Nb: 0 to 0.050%, V: 0 to 0.20%, Cu: 0 to 0.50%, Ni: 0 to 0.70%, Sn: 0 to 0.30%, a mechanical component having a chemical composition consisting of Sb: 0-0.005%, and Ca: 0-0.0050%, with the balance being Fe and impurity elements; wherein, when the diameter of the shaft portion is dm, a metal structure at a 1 / 4 dm portion located 1 / 4 dm deep from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft contains bainite in an area ratio of 70% or more; when the C content in mass % is (C%), the tensile strength of the shaft is 580 + 900 × (C%) MPa or more; a ratio of 0.2% proof stress to the tensile strength (0.2% proof stress / tensile strength) is 0.90 or more; and a value obtained by dividing the standard deviation of Vickers hardness in the cross section perpendicular to the longitudinal direction of the shaft by the average value of the Vickers hardness is 0.150 or less.

[0008] According to the present disclosure, there are provided a wire rod and a steel wire for obtaining mechanical parts that are excellent in strength and formability, and that can achieve high 0.2% yield strength and suppressed permanent elongation even when a bluing treatment is omitted after molding into the mechanical parts, and the mechanical parts.

[0009] 1A and 1B are diagrams showing an example of an SEM photograph mainly showing a bainite structure, and another example of an SEM photograph mainly showing a bainite structure.

[0010] The wire rod according to the present disclosure will be described. In this disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. However, when the numerical values ​​before and after "to" are followed by "greater than" or "less than," the numerical range does not include the numerical values ​​as the lower or upper limit. The content of an element in a chemical composition may be expressed by adding "amount" to the element symbol (e.g., C content, Si content, etc.). Regarding the content of an element in a chemical composition, "%" means "mass %." When the content of an element in a chemical composition is described as "0 to," this means that the element may not be included. The term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. The "surface" of a wire rod means the "outer peripheral surface." The "central axis" of a wire rod means an imaginary line that passes through the center point of a cross section perpendicular to the longitudinal direction of the wire rod and extends in the longitudinal direction (axial direction). "1 / 4D" is synonymous with "D / 4".

[0011] The inventors of the present disclosure have studied the effects of the structure and mechanical properties of a wire rod on the characteristics of steel wire and mechanical parts after wiredrawing, and have found that by setting the components of the wire rod within a specific range, by making the structure of the wire rod mainly bainite with reduced area ratios of ferrite, pearlite, and martensite, by setting the ratio of the tensile strength and 0.05% yield strength of the wire rod, i.e., 0.05% yield strength / tensile strength (hereinafter referred to as the "0.05% yield strength ratio of the wire rod") within a specific range, and by reducing the standard deviation of the hardness of the wire rod, it is possible to obtain a steel wire with excellent strength and formability after wiredrawing, and to obtain a high 0.2% yield strength ratio (0.2% yield strength / tensile strength) and reduced permanent elongation of the bolt after processing into a non-heat treated bolt.

[0012] When the structure of the wire rod is mainly ferrite or pearlite, the 0.2% yield strength ratio of the bolt decreases. Untempered bolts have a high dislocation density because their strength is imparted by wire drawing. If they contain a large number of mobile dislocations, they undergo plastic deformation with small strains, lowering the elastic limit and resulting in lower yield strength. In order to increase the yield strength of steel with a high dislocation density, it is effective to use solute carbon and nitrogen contained in the steel to lock the dislocations and suppress their movement.

[0013] Conventional non-tempered bolts use a heat treatment called bluing, which involves holding the bolt at 300-400°C to fix carbon to dislocations, thereby suppressing dislocation movement and increasing the bolt's 0.2% yield strength. The inventors of the present disclosure discovered that by using a bainite-based wire structure and setting the wire's 0.05% yield strength ratio within a specific range, the 0.2% yield strength ratio of non-tempered bolts can be increased without bluing. Wire rods with a typical bainite structure have a high mobile dislocation density and a low elastic limit. When solute carbon fixes mobile dislocations, dislocation movement is suppressed, increasing the elastic limit. Because the commonly used 0.2% yield strength is affected by plastic deformation, this disclosure uses 0.05% yield strength, which represents a value closer to the elastic limit. Wire rods with a bainite structure that have a high 0.05% yield strength have a high amount of solute carbon fixed to dislocations. Because the wiredrawing process removes solute carbon from dislocation fixation, it is thought that steel wire drawn from bainite structure wire with a high 0.05% yield strength has a high solute carbon concentration. With a high amount of solute carbon, carbon can be fixed to mobile dislocations without heating to the bluing treatment temperature of 300 to 400°C, suppressing dislocation movement, and it is presumed that this increases the 0.2% yield strength ratio of the bolt.

[0014] If the martensite fraction of the wire is high, the wire may break during drawing, cracks may occur during forming, and the 0.2% proof stress ratio of the bolt may decrease. Even if the wire has a bainite-based structure, if the 0.05% proof stress ratio of the wire is low, the 0.2% proof stress ratio of the bolt may decrease. This is presumably because, in order to increase the 0.2% proof stress ratio of the bolt, a sufficient amount of solute carbon is required to pin mobile dislocations after drawing. However, when the 0.05% proof stress ratio of the wire is low, the 0.2% proof stress ratio of the bolt decreases due to a lack of solute carbon. Furthermore, a bainite-based structure reduces work hardening, which suppresses work hardening during high-strain processing, such as bolt head processing, thereby reducing the load on the mold. Furthermore, since the cementite in the bainite structure is fragmented and has high ductility, work cracking can be suppressed.

[0015] If the hardness of the wire rod varies widely, the 0.2% yield strength ratio of the bolt after forming decreases. Furthermore, processing cracks are more likely to occur during bolt forming. The reason for this is thought to be that the non-uniform deformation caused by wire drawing leads to non-uniform distribution of dislocations.

[0016] <Wire Rod> The wire rod according to the present disclosure was discovered based on the above findings. Hereinafter, the chemical composition, metal structure, mechanical properties, manufacturing method, etc. of the wire rod according to the present disclosure will be described.

[0017] [Chemical composition] The chemical composition of the wire rod according to the present disclosure contains, in mass %, as essential elements: C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, and N: 0.0010 to 0.0150%, O: 0.003% or less, with the balance consisting of Fe and impurity elements. The wire rod according to the present disclosure may contain other optional elements as necessary.

[0018] C: 0.08 to 0.80% C is contained to ensure the strength required for mechanical parts. If the C content is less than 0.08%, it is difficult to ensure the strength required for mechanical parts. On the other hand, if the C content exceeds 0.80%, ductility, toughness, and cold forgeability deteriorate. Therefore, the C content is set to 0.08 to 0.80%. The lower limit of the C content is 0.08%, preferably 0.15%, and more preferably 0.20%, and the upper limit of the C content is 0.80%, preferably 0.75%, and more preferably 0.70%. A preferred C content that achieves high strength, ductility, toughness, and cold workability is 0.15 to 0.75%, and more preferably 0.20 to 0.70%.

[0019] Si: 0.03 to 1.50% Si functions as a deoxidizing element and is effective in imparting the necessary strength to mechanical components. If the Si content is less than 0.03%, these effects are insufficient. If the Si content exceeds 1.50%, the ductility and toughness of the mechanical component deteriorate, and the deformation resistance of the steel wire increases, deteriorating cold forgeability. Therefore, the Si content is set to 0.03 to 1.50%. The Si content is preferably 0.05 to 1.00%, and more preferably 0.10 to 0.60%.

[0020] Mn: 0.50 to 2.00% Mn is an element necessary for imparting the necessary strength to mechanical components. If the Mn content is less than 0.50%, the effect is insufficient. If the Mn content exceeds 2.00%, the toughness of the mechanical components deteriorates, and the deformation resistance of the steel wire increases, deteriorating cold forgeability. Therefore, the Mn content is set to 0.50 to 2.00%. The preferred Mn content is 0.70 to 1.50%, and more preferably 0.90 to 1.20%.

[0021] P: 0.050% or less P is contained in the wire rod as an impurity. P segregates at the grain boundaries of mechanical components and deteriorates toughness, so it is desirable to reduce the P content. Therefore, the upper limit of the P content is set to 0.050%. A preferred upper limit of the P content is 0.020%, and a more preferred upper limit is 0.015% or less. Note that the lower limit of the P content is preferably 0% (i.e., no P is contained), but from the viewpoint of reducing the dephosphorization cost, it may be more than 0% (or 0.0001% or more).

[0022] S: 0.050% or less S is contained in the wire rod as sulfides such as MnS. If the S content exceeds 0.050%, the cold heading property of the steel wire is deteriorated and the toughness of the mechanical parts is deteriorated. Therefore, the upper limit of the S content is set to 0.050%. A preferable upper limit of the S content is 0.030%. A more preferable upper limit is 0.015%. Note that the lower limit of the S content may be more than 0% (or 0.001% or more) from the viewpoint of reducing desulfurization costs.

[0023] Al: 0.005 to 0.080% Al functions as a deoxidizing element, and also forms AlN to refine crystal grains and improve the toughness of mechanical components. It also has the effect of fixing solute N, suppressing dynamic strain aging, and reducing deformation resistance. If the Al content is less than 0.005%, these effects are insufficient. If the Al content exceeds 0.080%, the effects saturate and manufacturability may decrease. Therefore, the Al content is set to 0.005 to 0.080%. The preferred Al content is 0.010 to 0.065%, and more preferably 0.020 to 0.055%.

[0024] N: 0.0010 to 0.0150% N forms nitrides with Al, Ti, Nb, V, etc., which refines crystal grains and improves the toughness of machine parts. If the N content is less than 0.0010%, the amount of nitride precipitation is insufficient, and the effect cannot be obtained. If the N content exceeds 0.0150%, dynamic strain aging due to solute N increases the deformation resistance of the steel wire, degrading workability. Therefore, the N content is set to 0.0010 to 0.0150%. The N content is preferably 0.0020 to 0.0100%, and more preferably 0.0025 to 0.0060%.

[0025] O: 0.003% or less O is an impurity and is inevitably contained in steel. If the O content exceeds 0.003%, coarse oxides may form, which may reduce fatigue strength, so the O content is limited to 0.003% or less. The preferred upper limit of the O content is 0.002%.

[0026] Balance: Fe and impurity elements In the chemical composition of the wire rod according to the present disclosure, the balance is Fe and impurity elements (sometimes referred to as "impurities" as appropriate in the present disclosure). Here, impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally added. Furthermore, impurities also include components that are intentionally added but contained in amounts that do not affect the performance of a steel wire obtained by wiredrawing the wire rod according to the present disclosure.

[0027] Furthermore, the wire rod according to the present disclosure may contain, in mass %, one or more elements selected from the group consisting of the following groups A to D, in place of a portion of Fe. Note that the elements in the following groups A to D are optional elements, and these elements may not be included, i.e., may be 0%.

[0028] [Group A] One or two selected from the group consisting of Ti: 0.050% or less, and B: 0.0050% or less

[0029] Ti: 0.050% or less Ti functions as a deoxidizing element and is effective in facilitating the formation of bainite. If the Ti content exceeds 0.050%, these effects become saturated and coarse oxides or nitrides are formed, which may deteriorate the fatigue strength of mechanical parts. Therefore, if Ti is contained, the Ti content should be 0.002 to 0.050%. The preferred Ti content is 0.003 to 0.050%, and more preferably 0.007 to 0.040%.

[0030] B: 0.0050% or less B has the effect of facilitating the formation of bainite. If the B content exceeds 0.0050%, carbides are formed at grain boundaries, which may deteriorate wiredrawability. Therefore, when B is contained, the B content should be 0.0002 to 0.0050%. The preferred B content is 0.0003 to 0.0050%, and more preferably 0.0008 to 0.0030%.

[0031] [Group B] One or more selected from the group consisting of Cr: 1.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, and V: 0.20% or less.

[0032] Cr: 1.50% or less Cr is an element necessary for imparting the necessary strength to mechanical components. If the Cr content exceeds 1.50%, the martensite fraction of the wire rod increases, degrading wiredrawability and increasing the deformation resistance of the steel wire, degrading cold forgeability. Therefore, the Cr content is set to 1.50% or less. The preferred Cr content is 0.02 to 0.80%, and more preferably 0.10 to 0.50%.

[0033] Mo: 0.50% or less Mo has the effect of imparting the necessary strength to mechanical parts. If the Mo content exceeds 0.50%, the alloy cost increases, and the deformation resistance of the steel wire increases, deteriorating cold forgeability. Therefore, when Mo is contained, the Mo content should be 0.02 to 0.50%. The Mo content is preferably 0.03 to 0.35%, and more preferably 0.05 to 0.25%. The Mo content may be 0.15% or less.

[0034] Nb: 0.050% or less Nb has the effect of increasing the strength of machine parts by precipitating carbides and nitrides, the effect of improving toughness by refining crystal grains, and the effect of reducing solute N and reducing deformation resistance. If the Nb content exceeds 0.050%, the effect saturates and cold forgeability may deteriorate. Therefore, if Nb is contained, the Nb content should be 0.002 to 0.050%. A preferable Nb content is 0.001 to 0.040%. A more preferable Nb content is 0.005 to 0.030%.

[0035] V: 0.20% or less V has the effect of precipitating carbides and nitrides to increase the strength of mechanical parts. If the V content exceeds 0.20%, the alloy cost increases. Therefore, if V is contained, the V content should be 0.02 to 0.20%. The preferred V content range is 0.01 to 0.15%.

[0036] [Group C] One or more selected from the group consisting of Cu: 0.50% or less, Ni: 0.70% or less, Sn: 0.30% or less, and Sb: 0.005% or less.

[0037] Cu: 0.50% or less Cu precipitates finely, imparting the necessary strength to mechanical components and improving corrosion resistance. If the Cu content exceeds 0.50%, hot ductility deteriorates and surface defects become more likely to occur. Therefore, if Cu is contained, the Cu content should be 0.02 to 0.50%. The preferred Cu content is 0.02 to 0.30%.

[0038] Ni: 0.70% or less Ni has the effect of improving corrosion resistance. If the Ni content exceeds 0.70%, the alloy cost increases. Therefore, if Ni is contained, the Ni content should be 0.02 to 0.70%. The Ni content is preferably 0.02 to 0.50%, and more preferably 0.05 to 0.30%.

[0039] Sn: 0.30% or less Sn has the effect of improving corrosion resistance. When Sn is contained, the Sn content is preferably 0.002% or more. However, if the Sn content exceeds 0.30%, the ductility decreases and the cold workability deteriorates, so the Sn content is limited to 0.30% or less. The preferred upper limit of the Sn content is 0.20%.

[0040] Sb: 0.005% or less Sb has the effect of improving corrosion resistance. When Sb is contained, the Sb content is preferably 0.001% or more. However, if the Sb content exceeds 0.005%, the ductility decreases and the cold workability deteriorates, so the Sb content is limited to 0.005% or less. The preferred upper limit of the Sb content is 0.004%, and the more preferred upper limit is 0.003%.

[0041] [Group D] Ca: 0.0050% or less Ca is contained as a deoxidizing element. Ca has the effect of refining oxides and improving fatigue strength. If the Ca content exceeds 0.0050%, ductility decreases and cold workability deteriorates, so the Ca content is limited to 0.0050% or less. The preferred upper limit of the Ca content is 0.0040%, and the more preferred upper limit is 0.0030%.

[0042] [Metal Structure of Wire Rod] Next, the metal structure of the wire rod according to the present disclosure will be described. In the metal structure of the wire rod according to the present disclosure, in a cross section (C cross section) perpendicular to the longitudinal direction of the wire rod, the area ratio of bainite at a depth of ¼D from the surface (outer peripheral surface) of the wire rod is 70% or more. If the bainite area ratio is less than 70%, the 0.2% proof stress ratio of the mechanical component decreases and workability deteriorates. The bainite area ratio is preferably 80% or more, and more preferably 90% or more.

[0043] (Method for Measuring the Metallic Structure of Wire Rod) The structure was observed by taking two samples from positions 50 mm apart in the axial direction of the wire rod, mirror-polishing a cross section (C section) perpendicular to the central axis of each wire rod sample, etching it with picral, and observing the 1 / 4D section. First, the C section of the wire rod to be measured was mirror-polished and then etched with picral (a solution of 5% picric acid and 95% ethanol) to reveal the structure. Next, a microstructure photograph of a 20 μm × 20 μm or larger area at each of four locations circumferentially spaced 90° apart in the 1 / 4D section was taken at 5000x magnification using a field emission scanning electron microscope (FE-SEM). Examples of bainite structures are shown in Figures 1A and 1B, respectively.

[0044] The metal structure may contain bainite, pearlite, martensite, and ferrite. Of these, martensite and ferrite do not contain carbides within the grains. The pearlite structure is a structure in which cementite and ferrite are alternately arranged in approximately parallel rows. Therefore, structures other than bainite (structures that do not contain carbides within the grains, pearlite structures) in the photographed structure are visually marked, and the area of ​​the region of the structure other than bainite is determined by image analysis (software name: Nireco's small general-purpose image processing analysis system LUZEX_AP). Note that this operation is performed by measuring and calculating two samples, averaging the results, and subtracting the area percentage of the structure other than bainite from the total area (100%) to determine the area percentage of bainite in this disclosure.

[0045] [Mechanical properties of wire rod] 0.05% yield strength / tensile strength: 0.72-0.40×(C%) or more In the wire rod according to the present disclosure, when the C content in mass % is (C%), the ratio of 0.05% yield strength to tensile strength (0.05% yield strength / tensile strength) is 0.72-0.40×(C%) or more. When the 0.05% yield strength / tensile strength is 0.72-0.40×(C%) or more, a high 0.2% yield strength ratio can be obtained after forming into a mechanical part without performing a bluing treatment. The 0.05% yield strength / tensile strength is preferably 0.78-0.40×(C%) or more.

[0046] Tensile tests of wire rods were performed using JIS Z2241:2011 No. 14A test pieces according to the test method of JIS Z2241:2011 to measure tensile strength (TS), 0.05% proof stress, and reduction of area. The 0.05% proof stress was determined by the offset method specified in JIS Z2241:2011 and was defined as the stress at which the plastic elongation reached 0.05% relative to the extensometer gauge length. Tensile test pieces were machined immediately after straightening the wire rod. Tensile tests were performed on three samples, and the average value was used.

[0047] (Vickers hardness of wire rod) The wire rod according to the present disclosure has a value obtained by dividing the standard deviation of the Vickers hardness in a cross section (C cross section) perpendicular to the longitudinal direction of the wire rod by the average value of the Vickers hardness of 0.150 or less. When this value is 0.150 or less, the 0.2% proof stress ratio of a mechanical part manufactured from the steel wire after wire drawing is high. In addition, the workability when forming into a mechanical part is improved. The value is preferably 0.100 or less, more preferably 0.050 or less.

[0048] The hardness test is carried out by mirror-polishing the C-section of the wire, and using a Vickers hardness tester, measurements are taken at four locations at a depth of 1.0 mm from the surface of the wire, rotated at 90° intervals in the circumferential direction of the wire, four locations at a depth of D / 4 (where D is the diameter of the wire), rotated at 90° intervals in the circumferential direction of the wire, and one location in the center, for a total of nine locations, and the average value and standard deviation are calculated. 1 , x 2 ,...x n When this is done, the average value X ave and standard deviation s were calculated using the following formula: ave = (1 / n) × Σx n s=((1 / n)×Σ(x n -X ave ) 2 ) (1/2) The test force for measuring Vickers hardness is 9.8 N, and the measurement is performed according to the method of JIS Z2244-1:2020.

[0049] (Diameter of Wire Rod) The wire diameter D of the wire rod according to the present disclosure is not particularly limited, but is preferably 3.0 to 25.0 mm, and more preferably 5.0 to 18.0 mm.

[0050] [Wire Rod Manufacturing Method] An example of a wire rod manufacturing method according to the present disclosure will be described. A billet of steel consisting of predetermined components satisfying the aforementioned chemical composition is heated to 1100 to 1250°C, held in a furnace for 90 minutes or more, then hot rolled at an entry temperature of 750 to 800°C for finish rolling, and coiled into a ring shape at 780 to 820°C. After coiling, the billet is subjected to primary cooling to 750°C at an average cooling rate of 2 to 15°C / s. Then, secondary cooling is performed from 750°C to 500°C at an average cooling rate of 25°C / s or more. Next, tertiary cooling is performed from 500°C to 450°C at an average cooling rate of 20°C / s or less. The wire is then held at 420 to 440°C for 30 to 100 seconds (primary holding), heated from 490 to 550°C at an average heating rate of 10°C / s or more, held at 580 to 620°C for 60 to 200 seconds (secondary holding), and then water-cooled to obtain a wire.

[0051] If the heating temperature is less than 1100°C or the heating furnace time is less than 90 minutes, the solid solution of carbides becomes insufficient, resulting in a decrease in the 0.05% proof stress ratio of the wire rod. If the heating temperature exceeds 1250°C, the surface hardness of the wire rod decreases due to decarburization. If the entry temperature of finish rolling exceeds 800°C, γ grains (austenite grains) become coarse, the ductility of the wire rod decreases, and workability deteriorates. If the entry temperature is less than 750°C, the γ grain size becomes non-uniform, and the standard deviation of the hardness of the wire rod increases. If the coiling temperature exceeds 820°C, the γ grains become coarse, the ductility of the wire rod decreases, and workability deteriorates. If the coiling temperature is less than 780°C, the area ratio of bainite decreases, resulting in a decrease in the 0.05% proof stress ratio of the wire rod. If the primary average cooling rate up to 750°C after coiling is less than 2°C / s, the γ grains become coarse, the ductility of the wire rod decreases, and workability deteriorates. If the cooling rate exceeds 15°C / s, the recovery and recrystallization of γ grains are delayed, resulting in mixed grains. This results in nonuniform γ grain size, a large standard deviation in the hardness of the wire, and a deterioration in the 0.2% yield strength ratio and permanent elongation of mechanical parts. If the secondary average cooling rate from 750°C to 500°C is less than 25°C / s, the area ratio of ferrite and pearlite increases, resulting in a decrease in the 0.05% yield strength ratio of the wire. If the tertiary average cooling rate from 500°C to 450°C exceeds 20°C / s, the standard deviation in the hardness of the wire increases, resulting in a deterioration in the formability of the bolt after wiredrawing and a deterioration in the 0.2% yield strength ratio and permanent elongation of the bolt. If the primary holding time at 420-440°C is less than 30 seconds, the hardness variation of the wire increases, resulting in a deterioration in the 0.2% yield strength ratio and permanent elongation of mechanical parts. If the primary holding time exceeds 100 seconds, the 0.05% yield strength ratio of the wire decreases. If the average heating rate from 490°C to 550°C is less than 10°C / s, the 0.05% yield strength ratio of the wire rod will decrease, and the 0.2% yield strength ratio and permanent elongation of the mechanical parts will deteriorate. If the secondary holding temperature is less than 580°C, the 0.2% yield strength ratio and permanent elongation of the mechanical parts will deteriorate, and if it exceeds 620°C, the strength will decrease. If the secondary holding time is less than 60 seconds, the 0.05% yield strength ratio of the wire rod will decrease. If the secondary holding time exceeds 200 seconds, carbides will coarsen and the reduction in area of ​​the steel wire after wiredrawing will decrease.

[0052] The wire rod according to the present disclosure is drawn at an area reduction rate of 15 to 50% to form a steel wire, which is then cold-headed and rolled to form a mechanical part such as a bolt. If the drawing area reduction rate is less than 15%, the yield strength ratio of the mechanical part decreases and the permanent elongation increases. If the drawing area reduction rate is 50% or more, the workability of the mechanical part deteriorates. After the drawing, galvanization and baking treatment are performed as necessary.

[0053] Steel wires manufactured using the wire rod of the present disclosure have high strength and drawing capacity, and are excellent in terms of bolt strength and formability. Non-heat-treated bolts manufactured using such steel wires can achieve a high 0.2% yield strength ratio and excellent permanent elongation even when the bluing treatment after forming is omitted. The steel wires and mechanical components according to the present disclosure will be described below. The chemical compositions of the steel wires and mechanical components according to the present disclosure are the same as those of the wire rods described above, and will not be described below.

[0054] <Steel Wire> The steel wire according to the present disclosure is obtained by wiredrawing the above-mentioned wire rod, and plastic flow is observed in the surface layer of the longitudinal cross section of the steel wire. The metallographic structure and mechanical properties of the steel wire according to the present disclosure will be described.

[0055] [Metal Structure of Steel Wire] In the steel wire according to the present disclosure, when the diameter of the steel wire is d, the metal structure at a ¼ d portion, which is a depth of ¼ d from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire, contains bainite at an area ratio of 70% or more. If the bainite area ratio is less than 70%, the 0.2% proof stress ratio of the mechanical component decreases and workability deteriorates. The bainite area ratio is preferably 80% or more, and more preferably 90% or more. The metal structure of the steel wire can be measured in the same manner as the metal structure of the wire rod described above.

[0056] [Mechanical Properties of Steel Wire] Tensile strength: 610+900×(C%) MPa or more Reduction of area: 62−32×(C%)% or more Tensile strength (MPa)×reduction of area (%): 52,000 or more 0.2% yield strength ratio (0.2% yield strength / tensile strength): 0.985−0.083×(C%) or more In the steel wire according to the present disclosure, when the C content in mass% is (C%), the tensile strength is 610+900×(C%) MPa or more, the reduction of area is 62−32×(C%)% or more, the tensile strength (MPa)×reduction of area (%) is 52,000 or more, and the 0.2% yield strength ratio (0.2% yield strength / tensile strength) is 0.985−0.083×(C%) or more. When the tensile strength, reduction in area, and 0.2% yield strength ratio of the steel wire satisfy the above relationships, when a non-tempered mechanical part is manufactured from this steel wire, the cold workability is improved and sufficient strength for the mechanical part is obtained.

[0057] From the viewpoint of achieving both cold workability and tensile strength when made into a mechanical part, it is preferable that the tensile strength is 640 + 900 × (C%) MPa or more, the reduction in area is 66 - 32 × (C%)% or more, the tensile strength (MPa) × reduction in area (%) is 53,000 or more, and the 0.2% yield strength ratio is 0.990 - 0.083 × (C%) or more.

[0058] The tensile strength, 0.2% proof stress ratio, and reduction in area of ​​the steel wire according to the present disclosure can be measured in accordance with the test method of JIS Z2241:2011 using a No. 14A test piece of JIS Z2241:2011, similar to the tensile test of the wire rod described above.

[0059] (Vickers hardness of steel wire) The steel wire according to the present disclosure has a value obtained by dividing the standard deviation of the Vickers hardness in a cross section (C cross section) perpendicular to the longitudinal direction of the steel wire by the average value of the Vickers hardness of 0.150 or less. If this value is 0.150 or less, the workability when forming into a mechanical part is improved, and the 0.2% proof stress ratio of the mechanical part is also high. The value is preferably 0.100 or less, more preferably 0.050 or less. The hardness test of the steel wire can be performed in the same manner as the hardness test of the wire rod described above, and the average value and standard deviation can be determined in the same manner.

[0060] (Diameter of Steel Wire) The wire diameter d of the steel wire according to the present disclosure is not particularly limited, but may be, for example, 2.0 to 23.0 mm, or 4.0 to 18.0 mm.

[0061] <Mechanical component> The mechanical component according to the present disclosure is obtained by cold heading and rolling the above-mentioned steel wire and processing it into the shape of a mechanical component such as a bolt. The mechanical component according to the present disclosure includes a shaft portion, and the shaft portion has the following metal structure and mechanical properties.

[0062] [Metal structure of shank portion] When the diameter of the shank portion is dm, the metal structure at a 1 / 4 dm depth from the surface of the shank portion in a cross section (C cross section) perpendicular to the longitudinal direction of the shank portion contains bainite at an area ratio of 70% or more. If the bainite area ratio is less than 70%, the 0.2% proof stress ratio of the mechanical component decreases and workability deteriorates. The bainite area ratio is preferably 80% or more, and more preferably 90% or more. The metal structure of the shank portion can be measured using the same method as the metal structure of the wire rod described above.

[0063] [Mechanical properties of the shaft portion] Tensile strength of the shaft portion: 580 + 900 × (C%) MPa or more In the mechanical component according to the present disclosure, the tensile strength of the shaft portion is 580 + 900 × (C%) MPa or more, where (C%) is the C content in mass %. By having such a tensile strength, the mechanical component exhibits high strength.

[0064] 0.2% Yield Strength / Tensile Strength: 0.90 or More The mechanical component according to the present disclosure has a ratio of 0.2% yield strength to the tensile strength of the shaft portion (0.2% yield strength / tensile strength) of 0.90 or more. The mechanical component according to the present disclosure can achieve a high 0.2% yield strength ratio of 0.90 or more even without being subjected to a bluing treatment. The 0.2% yield strength / tensile strength is preferably 0.92 or more.

[0065] The tensile test can be performed using a linear test piece with the shaft cut off, using a No. 14A test piece of JIS Z2241:2011, in the same manner as in the tensile test of the wire rod described above, in accordance with the test method of JIS Z2241:2011.

[0066] (Vickers hardness of shank portion) In the mechanical component according to the present disclosure, the value obtained by dividing the standard deviation of the Vickers hardness in a cross section (C cross section) perpendicular to the longitudinal direction of the shank portion by the average value of the Vickers hardness is 0.150 or less. When this value is 0.150 or less, the 0.2% proof stress ratio of the mechanical component manufactured from the steel wire through wire drawing is high. In addition, the processability when forming into the mechanical component is improved. The value is preferably 0.100 or less, more preferably 0.050 or less. The hardness test of the shank portion can be performed in the same manner as the hardness test of the wire rod described above, and the average value and standard deviation can be determined in the same manner.

[0067] (Diameter of Shank Portion) The diameter dm of the shaft portion of the mechanical component according to the present disclosure is not particularly limited, but may be, for example, 2.0 to 23.0 mm, or 4.0 to 18.0 mm.

[0068] (Permanent elongation) The mechanical component according to the present disclosure has a high 0.2% yield strength and suppresses permanent elongation. To achieve permanent elongation, the shaft portion of the mechanical component is machined into a coarse thread shape by rolling or machining. After threading, the mechanical component is attached to an adapter as specified in JIS B1051:2014 so that the length of the play thread portion is equal to the outer diameter of the thread. When the tensile strength of the mechanical part is 600 MPa or more but less than 700 MPa, it is 440 MPa, when it is 700 MPa or more but less than 800 MPa, it is 515 MPa, when it is 800 MPa or more but less than 900 MPa, it is 580 MPa, when it is 900 MPa or more but less than 1000 MPa, it is 650 MPa, when it is 1000 MPa or more but less than 1100 MPa, it is 830 MPa, when it is 1100 MPa or more but less than 1200 MPa, it is 910 MPa, when it is 1200 MPa or more but less than 1300 MPa, it is 970 MPa, when it is 1300 MPa or more but less than 1400 MPa, it is 1050 MPa A tensile stress of 1050 MPa is applied in the axial direction for 15 seconds. The difference (L1 - L0) between the total length L1 of the mechanical part after unloading and the total length L0 of the mechanical part before the test is defined as the permanent elongation. The total length L1 of the mechanical part after unloading and the total length L0 of the mechanical part before the test were measured using a micrometer.

[0069] The wire rod according to the present disclosure will be described in more detail below with reference to examples, although these examples do not limit the wire rod according to the present disclosure.

[0070] <Production and Evaluation of Wire Rod> Steels A to U having the chemical compositions shown in Table 1 were heated, hot rolled, cooled, and held under the conditions shown in Table 2 to produce wire rods. In Table 1, blanks mean that the element was not included, and the remainder is Fe and impurities. In each table, underlines mean that the element is outside the scope of the present disclosure.

[0071]

[0072]

[0073] The obtained wire rods were subjected to microstructural observation, tensile testing, and hardness measurement by the methods described above. Table 3 shows the microstructure and mechanical properties of the wire rods for each test number. In Table 3, F, P, and M in the remaining microstructure represent ferrite, pearlite, and martensite, respectively.

[0074]

[0075] <Production of Steel Wire> Steel wires were obtained by wiredrawing the wire rods shown in Table 3 at the area reduction rates shown in Table 4. Using the obtained steel wires, microstructure observation, hardness measurement, and tensile tests in air at room temperature were performed by the methods described above to measure the tensile strength (TS) and reduction of area (RA). Steel wires in which TS × RA was 52,000 or more, TS was 610 + 900 × (C%) MPa or more, RA was 62 - 32 × (C%)% or more, 0.2% proof stress ratio was 0.985 - 0.083 × (C%) or more, and the value obtained by dividing the standard deviation of Vickers hardness by the average value of Vickers hardness was 0.150 or less were judged to have good strength, formability, and proof stress.

[0076]

[0077] <Bolt Manufacturing> The steel wires listed in Table 4 were cold-headed and rolled to form bolts. Test Nos. 1 and 13 had threads of M5 and shank lengths of 100 mm, Test Nos. 10 and 17 had threads of M6 and shank lengths of 100 mm, and Test Nos. 2 to 9, 11, 12, 14 to 16, 18 to 20, and 22 to 25 had threads of M8 and shank lengths of 100 mm. These bolts were then electrogalvanized and baked at 200°C for 120 minutes to obtain bolts. Test No. 21 cracked during bolt processing, making it impossible to form the bolt into a bolt shape. JIS Z2241:2011 Type 14A test pieces were machined from the shanks of the resulting bolts, and measurements were performed according to the test method of JIS Z2241:2011. The diameter of the parallel portion of the tensile test specimen was 4 mm for the bolt with thread M5, 5 mm for the bolt with thread M6, and 7 mm for the bolt with thread M8. Tensile test specimens were collected and subjected to microstructure observation, hardness measurement, and tensile testing using the methods described above to measure tensile strength (TS) and 0.2% yield strength. The 0.2% yield strength ratio of the bolt was calculated by dividing the 0.2% yield strength by the tensile strength. The bolts obtained were also measured for permanent elongation using the method described above. Table 5 shows the TS, 0.2% yield strength ratio, and permanent elongation of each bolt. A test specimen was judged to be good if the TS was 580 + 900 × (C%) MPa or more, the 0.2% yield strength ratio (bolt yield strength ratio) was 0.90 or more, the value obtained by dividing the standard deviation of the Vickers hardness by the average Vickers hardness was 0.150 or less, and the permanent elongation was 1 μm or less.

[0078]

[0079] From the above results, the wire rods and steel wires of test numbers 1 to 19 that satisfy the requirements of the present disclosure have excellent formability during bolt processing, and a high 0.2% yield strength ratio was obtained even without performing a bluing treatment after bolt processing.

[0080] (Additional Notes) The present disclosure includes the following aspects. <1> A wire rod having a chemical composition, in mass %, of C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, with the balance being Fe and impurity elements, wherein, when the diameter of the wire rod is D, a metal structure at a ¼D portion that is a depth of ¼D from the surface of the wire rod in a cross section perpendicular to the longitudinal direction of the wire rod contains bainite in an area ratio of 70% or more, A wire rod in which, when the C content in mass % is (C%), the ratio of 0.05% proof stress to tensile strength (0.05% proof stress / tensile strength) is 0.72-0.40×(C%) or more, and a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the longitudinal direction of the wire rod by the average value of the Vickers hardness is 0.150 or less.<2> The chemical composition contains, in mass%, C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, and further contains one or more elements selected from the group consisting of the following A to D groups, with the balance consisting of Fe and impurity elements: [Group A] One or two elements selected from the group consisting of Ti: 0.050% or less, and B: 0.0050% or less [Group B] Cr: 1.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, and V [Group C] One or more selected from the group consisting of Cu: 0.50% or less, Ni: 0.70% or less, Sn: 0.30% or less, and Sb: 0.005% or less [Group D] Ca: 0.0050% or less When the diameter of the wire is D, a metal structure at a 1 / 4D portion that is 1 / 4D deep from the surface of the wire in a cross section perpendicular to the longitudinal direction of the wire contains bainite at an area ratio of 70% or more, when the content of C in mass% is (C%), the ratio of 0.05% proof stress to tensile strength (0.05% proof stress / tensile strength) is 0.72-0.40 × (C%) or more, and a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the longitudinal direction of the wire by the average value of the Vickers hardness is 0.150 or less. <3> The wire rod according to <2>, having a chemical composition including, by mass%, the Group A. <4> The wire rod according to <2> or <3>, having a chemical composition including, by mass%, the Group B. <5> The wire rod according to any one of <2> to <4>, having a chemical composition including, by mass%, the Group C. <6> The wire rod according to any one of <2> to <5>, having a chemical composition including, by mass%, the Group D.

[0081] <7> A steel wire having a chemical composition, in mass%, of C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, with the balance being Fe and impurity elements, wherein, when a diameter of a steel wire is d, a metal structure at a ¼ d part that is a depth of ¼ d from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire contains bainite in an area ratio of 70% or more, A steel wire having a tensile strength of 610+900×(C%) MPa or more, a reduction in area of ​​62−32×(C%)% or more, a tensile strength (MPa)×reduction in area (%) of 52,000 or more, a ratio of 0.2% yield strength to tensile strength (0.2% yield strength / tensile strength) of 0.985−0.083×(C%) or more, and a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the longitudinal direction of the steel wire by the average value of the Vickers hardness of 0.150 or less.<8> A steel having a chemical composition, in mass%, of C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, and further containing one or more elements selected from the group consisting of the following A to D groups, with the balance consisting of Fe and impurity elements: [Group A] One or two elements selected from the group consisting of Ti: 0.050% or less, and B: 0.0050% or less [Group B] Cr: 1.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, and V [Group C] One or more selected from the group consisting of Cu: 0.50% or less, Ni: 0.70% or less, Sn: 0.30% or less, and Sb: 0.005% or less [Group D] Ca: 0.0050% or less When the diameter of the steel wire is d, a metal structure at a 1 / 4d portion that is 1 / 4d deep from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire contains bainite in an area ratio of 70% or more, A steel wire having a tensile strength of 610 + 900 × (C%) MPa or more, an area reduction of 62 - 32 × (C%)% or more, a tensile strength (MPa) × area reduction of 62,000 or more, a tensile strength (MPa) × area reduction of 52,000 or more, a ratio of 0.2% proof stress to tensile strength (0.2% proof stress / tensile strength) of 0.985 - 0.083 × (C%) or more, and a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the longitudinal direction of the steel wire by the average value of the Vickers hardness of 0.150 or less, where the C content in mass % is (C%). <9> The steel wire according to <8>, having a chemical composition including Group A by mass. <10> The steel wire according to <8> or <9>, having a chemical composition including Group B by mass. <11> The steel wire according to any one of <8> to <10>, having a chemical composition including Group C by mass. <12> The steel wire according to any one of <8> to <11>, having a chemical composition including, by mass%, the D group.

[0082] <13> A machine part including a shank, having a chemical composition, in mass%, of C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, with the balance being Fe and impurity elements, wherein, when the diameter of the shank is dm, a metallographic structure at a ¼ dm portion located at a depth of ¼ dm from the surface of the shank in a cross section perpendicular to the longitudinal direction of the shank contains bainite in an area ratio of 70% or more, and when the content of C in mass% is (C%), the tensile strength of the shank is 580 + 900 × (C%) MPa or more, a ratio of 0.2% yield strength to the tensile strength (0.2% yield strength / tensile strength) of 0.90 or more, and a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the longitudinal direction of the shaft portion by the average value of the Vickers hardness is 0.150 or less.<14> A machine part including a shaft portion, having a chemical composition, in mass%, of C: 0.08 to 0.80%, Si: 0.03 to 1.50%, Mn: 0.50 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005 to 0.080%, N: 0.0010 to 0.0150%, O: 0.003% or less, and further containing one or more elements selected from the group consisting of the following A to D groups, with the balance consisting of Fe and impurity elements: [Group A] one or two elements selected from the group consisting of Ti: 0.050% or less, and B: 0.0050% or less [Group B] Cr: 1.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, and V: 0.20% or less [Group C] One or more selected from the group consisting of Cu: 0.50% or less, Ni: 0.70% or less, Sn: 0.30% or less, and Sb: 0.005% or less [Group D] Ca: 0.0050% or less When the diameter of the shaft portion is dm, a metal structure at a 1 / 4 dm portion located 1 / 4 dm deep from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft portion contains bainite at an area ratio of 70% or more, When the content of C in mass% is (C%), the tensile strength of the shaft portion is 580 + 900 × (C%) MPa or more, The ratio of 0.2% proof stress to the tensile strength (0.2% proof stress / tensile strength) is 0.90 or more, A mechanical component in which a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the longitudinal direction of the shaft portion by the average value of the Vickers hardness is 0.150 or less. <15> The mechanical component according to <14>, having a chemical composition including Group A by mass%. <16> The mechanical component according to <14> or <15>, having a chemical composition including Group B by mass%. <17> The mechanical component according to any one of <14> to <16>, having a chemical composition including Group C by mass%. <18> The mechanical component according to any one of <14> to <17>, having a chemical composition including Group D by mass%.

[0083] The disclosure of Japanese Patent Application No. 2023-059430, filed on March 31, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated herein by reference.

Claims

1. In mass%, C: 0.08-0.80%, Si: 0.03-1.50%, Mn: 0.50-2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005-0.080%, N: 0.0010-0.0150%, O: 0.003% or less, Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, Sn: 0-0.30%, A wire having a chemical composition consisting of Sb: 0-0.005%, and Ca: 0-0.0050%, with the balance consisting of Fe and impurity elements; when the diameter of the wire is D, a metal structure at a 1 / 4D portion that is 1 / 4D deep from the surface of the wire in a cross section perpendicular to the longitudinal direction of the wire contains bainite at an area ratio of 70% or more; when the C content in mass % is (C%), a ratio of 0.05% proof stress to tensile strength (0.05% proof stress / tensile strength) is 0.72-0.40×(C%) or more; and a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the longitudinal direction of the wire by the average value of the Vickers hardness is 0.150 or less.

2. In mass%, C: 0.08-0.80%, Si: 0.03-1.50%, Mn: 0.50-2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005-0.080%, N: 0.0010-0.0150%, O: 0.003% or less, Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, Sn: 0-0.30%, a steel wire having a chemical composition consisting of Sb: 0-0.005% and Ca: 0-0.0050%, with the balance consisting of Fe and impurity elements; when a diameter of the steel wire is d, a metal structure at a 1 / 4d part that is 1 / 4d deep from the surface of the steel wire in a cross section perpendicular to the longitudinal direction of the steel wire contains bainite at an area ratio of 70% or more; when a C content in mass % is (C%), the tensile strength is 610+900×(C%) MPa or more, the reduction in area is 62-32×(C%)% or more, the tensile strength (MPa)×reduction in area (%) is 52,000 or more, the ratio of 0.2% proof stress to tensile strength (0.2% proof stress / tensile strength) is 0.985-0.083×(C%) or more; and a value obtained by dividing the standard deviation of Vickers hardness in a cross section perpendicular to the longitudinal direction of the steel wire by the average value of the Vickers hardness is 0.150 or less.

3. A machine part including a shaft, having the following mass percentages: C: 0.08-0.80%, Si: 0.03-1.50%, Mn: 0.50-2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.005-0.080%, N: 0.0010-0.0150%, O: 0.003% or less, Ti: 0-0.050%, B: 0-0.0050%, Cr: 0-1.50%, Mo: 0-0.50%, Nb: 0-0.050%, V: 0-0.20%, Cu: 0-0.50%, Ni: 0-0.70%, Sn: 0-0.30%, a metal structure at a 1 / 4 dm portion at a depth of 1 / 4 dm from the surface of the shaft portion in a cross section perpendicular to the longitudinal direction of the shaft portion contains bainite at an area ratio of 70% or more, and a tensile strength of the shaft portion is 580 + 900 × (C%) MPa or more, and a ratio of 0.2% proof stress to the tensile strength (0.2% proof stress / tensile strength) is 0.90 or more, and a value obtained by dividing the standard deviation of Vickers hardness in the cross section perpendicular to the longitudinal direction of the shaft portion by the average value of the Vickers hardness is 0.150 or less.

Citation Information

Patent Citations

  • Non-refined steel material for weld bolt and method for producing the same

    JP2015190002A

  • Steel wire, wire for non-heat-treated mechanical components, and non-heat-treated mechanical component

    JP2021183710A

  • Wire material for non-refined machine component; steel wire for non-refined machine component; non-refined machine component; and method for manufacturing wire material for non-refined machine component, steel wire for non-refined machine component, and non-refined machine component

    WO2013031640A1

  • Rod material for non-tempered machine component, steel rod for non-tempered machine component, and non-tempered machine component

    WO2016121820A1

  • Steel wire for non-thermal-refined machine component, and non-thermal-refined machine component

    WO2017122830A1

Cited By

  • Wire rods, steel wires, and machine parts

    JP7953244B2

  • JPWO2025258647A1

  • Wire rod, steel wire, and machine component

    WO2025258647A1