Foam sheet and adhesive tape
The foam sheet with tailored properties addresses the challenge of easy peeling and adhesive residue in adhesive tapes by combining specific tensile and breaking strengths with a structured layer configuration, ensuring clean removal and mechanical integrity for electronic devices.
Patent Information
- Application Number
- PCT/JP2024/013350
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional adhesive tapes with foam sheets as base materials face challenges in being easily peeled off without leaving adhesive residue, particularly in thin electronic devices like TVs, due to issues with tensile strength, breaking strength, and flexibility, which affects their usability and reliability.
A foam sheet with specific properties, including tensile strength of 1 to 9 MPa, breaking strength of 3.5 MPa or less, and a thickness of 0.05 to 0.9 mm, featuring a core layer with a high foaming ratio and closed cell ratio, and outer layers with lower expansion ratios, allowing for easy plane-direction tearing and clean peeling without adhesive residue.
The foam sheet enables easy peeling off without leaving adhesive residue, maintaining mechanical strength and flexibility, making it suitable for thin electronic devices and large displays, while ensuring excellent step followability and releasability.
Smart Images

Figure JP2024013350_03102024_PF_FP_ABST
Abstract
Description
Foam sheets, adhesive tapes
[0001] The present invention relates to a foam sheet and a pressure-sensitive adhesive tape using the foam sheet as a substrate.
[0002] In recent years, with the increasing size of displays used in information terminals such as smartphones, tablets, and personal computers, as well as televisions, and the rapid spread of OLEDs, it has become common for display panels used in these applications to be removed for repair and then reattached after the repair. Such display panels are generally fixed to the housing of the electronic device or the like with adhesive tape.
[0003] As a specific example of an adhesive tape, for example, Patent Document 1 discloses an adhesive sheet before photocuring formed from a resin composition containing a (meth)acrylic copolymer (A), a crosslinking agent (B), and a photopolymerization initiator (C), which has photocurability and satisfies predetermined requirements for shape retention, self-adhesiveness, and viscosity. Patent Document 1 also discloses that, although there has been a problem in that distortion due to unevenness such as steps on an adherend that cannot be absorbed by the adhesive tape is applied to a display panel, causing display unevenness on the display panel, the display unevenness can be improved by improving the flexibility of the adhesive sheet.
[0004] Furthermore, many pressure-sensitive adhesive tapes using a foam sheet as a substrate have also been proposed. For example, Patent Document 2 discloses a multilayer foam sheet including a substrate layer made of a foam layer and a surface layer made of a foam layer or a resin film laminated on at least one surface of the substrate layer, and a pressure-sensitive adhesive tape provided with an adhesive material on at least one surface of the multilayer foam sheet. Furthermore, Patent Document 3 discloses a multilayer foam sheet including a resin layer and foam layers on both sides of the resin layer, and a pressure-sensitive adhesive tape provided with an adhesive material on at least one surface of the multilayer foam sheet.
[0005] International Publication No. WO 2016 / 194957 International Publication No. WO 2022 / 080219 International Publication No. WO 2022 / 030649
[0006] With the increasing size of TVs and the widespread use of devices equipped with high-end OLED panels, there is an increasing demand for temporarily removing display panels, such as when recovering a healthy display panel from a faulty device and reusing it in another device, or when repairing such devices to make them usable again. Furthermore, in recent years, as televisions and other devices have become thinner from the standpoint of design and other factors, thinness is also being demanded of adhesive tapes used to secure display panels inside televisions and other devices. Therefore, adhesive tapes are required to be thin yet be easily peelable without leaving adhesive residue on the display panel. Therefore, the present inventors have considered a way to make adhesive tapes easily peelable, for example, by tearing the interior of the tape substrate in the planar direction, a so-called "middle tear," and then peeling off the remaining tape.
[0007] However, when attempting to perform center tearing using conventional adhesive tapes, because they were not designed to be peeled off by center tearing, it was not possible to easily peel them off without leaving any adhesive on the panel. Specifically, adhesive tapes using a foam with a low expansion ratio as the substrate of the adhesive tape have the problem that the substrate cannot be torn in the plane direction, and the necessary step-conforming ability (flexibility) is lost, making them unusable for panel fixing applications such as televisions. On the other hand, adhesive tapes using a foam with a high expansion ratio as the substrate of the adhesive tape can tear the substrate in the plane direction, but when the adhesive-attached foam remaining on the display panel is subsequently peeled off, the foam is pulled by the adhesive due to its low tensile strength, and the foam is torn or torn during peeling, making it difficult to peel off.
[0008] Therefore, an object of the present invention is to provide a foam sheet that is thin and can be easily peeled off without leaving any adhesive on the adherend.
[0009] As a result of extensive investigation, the present inventors have found that the above-mentioned problems can be solved by controlling both the tensile strength and the breaking strength in interlaminar strength measurement of a foam sheet to a certain level or less and controlling the overall thickness within a predetermined range. That is, the present invention provides the following [1] to
[13] .
[0010] [1] A foam sheet having a tensile strength of 1 to 9 MPa and a breaking strength of 3.5 MPa or less when measuring interlaminar strength, the foam sheet having a total thickness of 0.05 to 0.9 mm. [2] The foam sheet according to [1], wherein the 25% compressive strength of the foam sheet is 150 kPa or less. [3] The density of the foam sheet as a whole is 0.07 to 0.60 g / cm. 3 [4] The foam sheet according to any one of [1] to [3], comprising a core layer which is a foam, and outer layers which are provided on both sides of the core layer and which are foams having a lower expansion ratio than the core layer or which are non-foamed. [5] The foam sheet according to [4], wherein the expansion ratio of the core layer is 5 to 20 times. [6] The foam sheet according to [4] or [5], wherein the thickness ratio of the core layer to the outer layers (thickness of the core layer / average thickness of the outer layers) is 2 or more. [7] The foam sheet according to any one of [4] to [6], wherein the closed cell ratio of the core layer is 90% or more. [8] The foam sheet according to any one of [4] to [7], wherein the thickness of each of the outer layers is 5 μm or more. [9] The foam sheet according to any one of [4] to [8], wherein the average bubble diameter of the bubbles in the core layer is 20 to 500 μm.
[10] The foam sheet according to any one of [4] to [9], wherein the core layer is a crosslinked foam.
[11] The foam sheet according to
[10] , wherein the core layer has a gel fraction of 20 to 50 mass %.
[12] The foam sheet according to any one of [4] to
[11] , wherein the resin constituting the core layer is at least one selected from the group consisting of polyolefin resins, urethane resins, acrylic resins, and elastomer resins.
[13] A pressure-sensitive adhesive tape comprising the foam sheet according to any one of [1] to
[12] , and a pressure-sensitive adhesive provided on at least one surface of the foam sheet.
[0011] According to the present invention, it is possible to provide a foam sheet that has good conformability to unevenness, is thin, and can be easily peeled off without leaving any adhesive on the adherend.
[0012] It is a schematic diagram showing an example of the configuration of a foam sheet of the present invention.It is a schematic diagram showing an example of the configuration of a pressure-sensitive adhesive tape of the present invention.It is a schematic diagram showing a breaking strength measuring device.
[0013] [Foam Sheet] The foam sheet of the present invention has a tensile strength of 1 to 9 MPa, a breaking strength when measuring interlaminar strength (hereinafter simply referred to as "breaking strength") of 3.5 MPa or less, and an overall thickness of the foam sheet of 0.05 to 0.9 mm. Because the foam sheet of the present invention has the above-mentioned configuration, when used as a substrate for, for example, an adhesive tape, the adhesive tape can be easily peeled from the adherend by tearing the foam sheet in the planar direction with a cutter or the like and then peeling off the portion of the adhesive tape remaining on the adherend without leaving any adhesive on the adherend. The foam sheet will be described in more detail below.
[0014] <Tensile Strength> If the tensile strength of the foam sheet is less than 1 MPa, the foam sheet will be pulled by the adhesive when peeled off, causing it to break, making it difficult to peel off the foam sheet cleanly. Furthermore, if the tensile strength exceeds 9 MPa, the breaking strength will be greater than a predetermined value, making it difficult to tear the foam sheet in the planar direction before peeling it off. Furthermore, flexibility may decrease, resulting in poor conformability to uneven surfaces. Taking these points into consideration, the tensile strength is preferably 1.2 to 8.5 MPa, and more preferably 1.3 to 5 MPa. The tensile strength can be measured by the method described in the examples.
[0015] <Thickness> If the total thickness of the foam sheet exceeds 0.9 mm, the foam sheet will be too thick and difficult to use inside thin electronic devices, etc. Furthermore, if the total thickness is less than 0.05 mm, sufficient gaps for cutting into the foam sheet with a cutter or the like will not be secured, making it impossible to tear in the surface direction and making it difficult to impart excellent releasability to the foam sheet. In light of the above, the total thickness is preferably 0.07 to 0.8 mm, and more preferably 0.12 to 0.5 mm.
[0016] <Breaking Strength> As described above, the foam sheet of the present invention has a breaking strength of 3.5 MPa or less. However, if the breaking strength exceeds 3.5 MPa, the foam sheet cannot be torn in the planar direction, making it difficult to impart excellent releasability to the foam sheet. From this perspective, the breaking strength is preferably 3.2 MPa or less, and more preferably 3 MPa or less. Furthermore, from the viewpoint of imparting a certain level of mechanical strength to the foam sheet and preventing a panel fixed by the tape from falling when used as a substrate for an adhesive tape, the breaking strength is preferably 0.1 MPa or more, more preferably 0.3 MPa or more, and even more preferably 0.5 MPa or more. The breaking strength can be measured at the time of measuring the interlaminar strength by the method described in the Examples.
[0017] <25% Compression Strength> The foam sheet of the present invention preferably has a 25% compression strength of 150 kPa or less, more preferably 100 kPa or less, and even more preferably 70 kPa or less. When the 25% compression strength is equal to or less than the above upper limit, the flexibility of the foam sheet is good and the conformability to unevenness is excellent. Furthermore, even when the foam sheet is sandwiched between components inside an electronic device such as a television, the load on the components is reduced, making it easier to prevent malfunctions of the electronic device. On the other hand, from the viewpoint of imparting a certain level of mechanical strength to the foam sheet, the 25% compression strength is preferably 10 kPa or more, more preferably 15 kPa or more, and even more preferably 20 kPa or more. The 25% compression strength can be measured by the method described in the examples.
[0018] <Density> The density of the entire foam sheet is 0.07 to 0.60 g / cm 3 is preferably 0.10 to 0.50 g / cm 3 More preferably, it is 0.20 to 0.45 g / cm 3 It is more preferable that the density of the entire foam sheet is equal to or greater than the lower limit, the foam sheet is provided with a certain tensile strength and is less likely to be torn by the adhesive during peeling. On the other hand, if the density of the entire foam sheet is equal to or less than the upper limit, the breaking strength of the foam sheet is kept below a certain level, making it easier to tear the core layer in the planar direction before peeling the foam sheet. In addition, it is easier to impart excellent conformability to the foam sheet. Note that the density referred to here means the apparent density, including the overall density. The apparent density can be measured together with the expansion ratio described below by the method described in the Examples.
[0019] <Configuration> The foam sheet of the present invention may be composed solely of a core layer made of a foam, or may have an outer layer on at least one side of the foam core layer. When an outer layer is provided, the foam sheet may be a multilayer body having an outer layer on only one side of the core layer, or a multilayer body having outer layers on both sides of the core layer. However, as shown in Figure 1, a multilayer body 1 is preferred, in which outer layers B and C are provided on both sides of the core layer A. Providing outer layers on both sides of the core layer facilitates increasing the tensile strength of the foam sheet. Therefore, when the foam sheet is used as a substrate for an adhesive tape, after the core layer is torn in the planar direction, the tape is prevented from breaking during peeling when the tape is peeled from the adherend, thereby achieving excellent peelability. Furthermore, excellent peelability can also be achieved by providing an adhesive on both sides of the foam sheet. Furthermore, although the outer layer is preferably laminated directly to the core layer, it may also be laminated via an adhesive layer or the like.
[0020] The outer layer may be a foamed layer made of a foamed material, or a non-foamed layer made of a non-foamed material. When the outer layer is a foamed layer, it is sufficient that the foamed layer has a lower expansion ratio than the foamed layer constituting the core layer. In the present invention, the outer layer is preferably a non-foamed material. The use of a non-foamed material improves the tensile strength of the foamed material sheet, prevents the foamed material sheet from breaking during peeling, and makes it easier to achieve excellent peelability.
[0021] [Core Layer (Foam)] The foam constituting the core layer will be described in more detail below.
[0022] <Expansion Ratio> The foam of the core layer preferably has an expansion ratio of 5 to 20 times, more preferably 5.2 to 15 times, and even more preferably 6 to 8.5 times. When the expansion ratio is equal to or greater than the lower limit, the breaking strength of the foam sheet is kept below a certain level, making it easier to tear the core layer in the plane direction before peeling the foam sheet. This also makes it easier to impart excellent conformability to the foam sheet. On the other hand, when the expansion ratio is equal to or less than the upper limit, the foam sheet is imparted with a certain level of tensile strength, making it less likely to be torn by the adhesive during peeling. Furthermore, when the foam sheet has an outer layer, the outer layer may be compressed and stretched during the manufacturing process due to the expansion of the foamable composition, which is the raw material for the core layer. However, when the expansion ratio is equal to or less than the upper limit, this stretching is suppressed, making it easier to maintain the tensile strength of the entire foam sheet at a certain level or higher.
[0023] <Average Cell Diameter> The core layer preferably has an average cell diameter of 20 to 500 μm, more preferably 30 to 300 μm, and even more preferably 35 to 200 μm. When the average cell diameter is equal to or greater than the lower limit, the foam sheet is more likely to be imparted with excellent releasability and step-following properties. Furthermore, the foam sheet is more likely to tear in the in-plane direction. On the other hand, when the average cell diameter is equal to or less than the upper limit, the foam sheet is imparted with a certain level of tensile strength, which makes it more likely to be imparted with excellent releasability. Furthermore, the foam sheet can be more easily thinned. The average cell diameter in the present invention is the maximum value among the average cell diameters in the MD (Machine Direction), TD (Transverse Direction), and ZD (perpendicular to both MD and TD) directions.
[0024] In the core layer, the average bubble diameter in the MD direction is preferably 15 to 450 μm, more preferably 25 to 250 μm, and even more preferably 30 to 150 μm. The average bubble diameter in the TD direction is preferably 20 to 500 μm, more preferably 30 to 300 μm, and even more preferably 35 to 200 μm. The average bubble diameter in the ZD direction is preferably 5 to 100 μm, more preferably 10 to 70 μm, and even more preferably 15 to 50 μm. The average bubble diameter can be measured by the method described in the Examples.
[0025] <Closed Cell Ratio> The core layer preferably has a closed cell ratio of 70% or more, more preferably 80% or more, and even more preferably 90% or more. The upper limit of the closed cell ratio is not particularly limited, and is 100%. A closed cell ratio equal to or greater than the lower limit makes it easier to impart excellent step-following properties. Furthermore, the increased shear strength of the core layer has the advantage of preventing problems such as the core layer tearing and the panel falling when incorporated into an electronic device such as a television. The closed cell ratio can be measured by the method described in the examples.
[0026] <Degree of Crosslinking> The core layer is preferably a crosslinked foam. Specifically, the degree of crosslinking (gel fraction) of the core layer is preferably 20 to 50% by mass, more preferably 30 to 45% by mass. By setting the degree of crosslinking of the core layer within the above range, it becomes easier to improve the mechanical strength, flexibility, impact absorption, etc. of the foam sheet. It also becomes possible to perform appropriate foaming in the core layer. The method for measuring the degree of crosslinking is as follows. A test piece of approximately 100 mg is taken from the core layer, and the weight A (mg) of the test piece is precisely weighed. Next, this test piece is immersed in 30 cm of xylene at 120°C. 3 After immersion for 24 hours, the insoluble matter on the mesh was filtered through a 200-mesh wire netting, vacuum-dried, and the weight B (mg) of the insoluble matter was precisely weighed. The degree of crosslinking (mass%) was calculated from the obtained value using the following formula: Degree of crosslinking (mass%) = 100 × (B / A).
[0027] The thickness of the core layer is preferably 0.03 to 0.7 mm, more preferably 0.05 to 0.5 mm, and even more preferably 0.08 to 0.3 mm. When the thickness of the core layer is equal to or greater than the above-mentioned lower limit, a sufficient gap is secured for cutting into the core layer with a cutter or the like, allowing the foam sheet to be torn in the plane direction, making it easier to impart excellent releasability to the foam sheet. When the thickness of the core layer is equal to or less than the above-mentioned upper limit, the overall thickness of the foam sheet can be made thin, making it easier to use inside thin electronic devices, etc.
[0028] <Resin> The resin constituting the core layer of the present invention is preferably at least one selected from the group consisting of polyolefin-based resins, urethane-based resins, acrylic-based resins, and elastomer-based resins.
[0029] (Polyolefin Resin) Examples of polyolefin resins include polyethylene resins, polypropylene resins, and ethylene-vinyl acetate copolymers, among which polyethylene resins are preferred. Examples of polyethylene resins include polyethylene resins polymerized with a polymerization catalyst such as a Ziegler-Natta compound, a metallocene compound, or a chromium oxide compound, among which polyethylene resins polymerized with a polymerization catalyst such as a metallocene compound are preferred.
[0030] Furthermore, linear low-density polyethylene is preferred as the polyethylene resin. The use of linear low-density polyethylene imparts high flexibility to the foam sheet and enables the foam sheet to be made thinner. Furthermore, the linear low-density polyethylene is more preferably a linear low-density polyethylene obtained by copolymerizing ethylene (for example, 75% by mass or more, preferably 90% by mass or more, based on the total amount of monomers) with a small amount of an α-olefin as needed. Specific examples of the α-olefin include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene, and among these, α-olefins having 4 to 10 carbon atoms are preferred. The density of the polyethylene resin, for example, the linear low-density polyethylene described above, is 0.870 to 0.910 g / cm 3 is preferably 0.875 to 0.907 g / cm 3 More preferably, 0.880 to 0.905 g / cm 3 As the polyethylene resin, a plurality of polyethylene resins may be used, and a polyethylene resin having a density outside the above range may be added.
[0031] (Metallocene Compound) Examples of metallocene compounds include compounds such as bis(cyclopentadienyl) metal complexes having a structure in which a transition metal is sandwiched between π-electron unsaturated compounds. More specifically, examples include compounds in which one or more cyclopentadienyl rings or analogs thereof are present as ligands on a tetravalent transition metal such as titanium, zirconium, nickel, palladium, hafnium, or platinum. Such metallocene compounds have uniform active site properties, with each active site having the same activity. Polymers synthesized using metallocene compounds have high uniformity in molecular weight, molecular weight distribution, composition, composition distribution, etc., so when a sheet containing a polymer synthesized using a metallocene compound is crosslinked, the crosslinking proceeds uniformly. A uniformly crosslinked sheet is foamed uniformly, making it easier to stabilize its physical properties. Furthermore, since it can be stretched uniformly, the thickness of the foam sheet can be made uniform.
[0032] Examples of the ligand include a cyclopentadienyl ring and an indenyl ring. These cyclic compounds may be substituted with a hydrocarbon group, a substituted hydrocarbon group, or a hydrocarbon-substituted metalloid group. Examples of hydrocarbon groups include a methyl group, an ethyl group, various propyl groups, various butyl groups, various amyl groups, various hexyl groups, 2-ethylhexyl groups, various heptyl groups, various octyl groups, various nonyl groups, various decyl groups, various cetyl groups, and a phenyl group. The term "various" refers to various isomers including n-, sec-, tert-, and iso-. Alternatively, a cyclic compound polymerized as an oligomer may be used as the ligand. In addition to π-electron unsaturated compounds, monovalent anionic ligands such as chlorine and bromine, or divalent anionic chelating ligands, hydrocarbons, alkoxides, arylamides, aryloxides, amides, arylamides, phosphides, arylphosphides, and the like may also be used.
[0033] Examples of metallocene compounds containing a tetravalent transition metal or ligand include cyclopentadienyltitanium tris(dimethylamide), methylcyclopentadienyltitanium tris(dimethylamide), bis(cyclopentadienyl)titanium dichloride, and dimethylsilyltetramethylcyclopentadienyl-t-butylamido zirconium dichloride. When combined with a specific cocatalyst (promoter), metallocene compounds function as catalysts during the polymerization of various olefins. Specific cocatalysts include methylaluminoxane (MAO) and boron-based compounds. The ratio of the cocatalyst to the metallocene compound is preferably 100,000 to 1,000,000 moles, more preferably 50 to 5,000 moles. When the linear low-density polyethylene described above is used as the polyolefin resin, the linear low-density polyethylene may be used alone or in combination with other polyolefin resins other than linear low-density polyethylene. For example, the linear low-density polyethylene may be used in combination with a polyolefin resin other than polyethylene resin, as described below. When other polyolefin resins are used in combination, the ratio of the other polyolefin resins to the linear low-density polyethylene (100% by mass) is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.
[0034] Examples of the ethylene-vinyl acetate copolymer used as the polyolefin resin include an ethylene-vinyl acetate copolymer containing 50% by mass or more of ethylene. Examples of the polypropylene resin include homopolypropylene and a propylene-α-olefin copolymer containing, for example, preferably 70% by mass or more, more preferably 90% by mass or more of propylene. These may be used alone or in combination of two or more. Specific examples of the α-olefin constituting the propylene-α-olefin copolymer include ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene. Of these, α-olefins having 6 to 12 carbon atoms are preferred.
[0035] Furthermore, when a polyolefin resin is used as the resin, the polyolefin resin may be used alone, or may contain a resin other than the polyolefin resin. The proportion of the polyolefin resin to the total amount of resin is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. As the resin other than the polyolefin resin to be used in combination as the polyolefin resin, a resin other than the polyolefin resin may be used from among the above-mentioned resins, but preferably an elastomer resin is used.
[0036] (Urethane-based resin) As the urethane-based resin, a reaction product of polyol and polyisocyanate can be suitably used. There is no particular limitation on the polyol, and it can be appropriately selected depending on the purpose, and examples thereof include polyester polyol, polyether polyol, polycarbonate polyol, etc. These may be used alone or in combination of two or more.
[0037] Examples of polyester polyols include polyesters obtained by esterification reaction of low-molecular-weight polyols with polycarboxylic acids, polyesters obtained by ring-opening polymerization reaction of cyclic ester compounds such as ε-caprolactone, copolymer polyesters thereof, etc. Examples of low-molecular-weight polyols that can be used in producing polyester polyols include aliphatic alkylene glycols having a weight-average molecular weight of approximately 50 to 300, such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, neopentyl glycol, and 1,3-butanediol, as well as cyclohexanedimethanol.
[0038] Examples of polycarboxylic acids include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and dodecanedicarboxylic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and naphthalenedicarboxylic acid; and anhydrides or esters thereof.
[0039] Examples of polyether polyols include those obtained by addition polymerization of alkylene oxides using one or more compounds having two or more active hydrogen atoms as an initiator.
[0040] As the polycarbonate polyol, for example, a product obtained by reacting a carbonate ester and / or phosgene with a low molecular weight polyol described below can be used.
[0041] Examples of carbonate esters include methyl carbonate, dimethyl carbonate, ethyl carbonate, diethyl carbonate, cyclocarbonate, and diphenyl carbonate.
[0042] Examples of low molecular weight polyols that can be used to produce polycarbonate polyols and that can react with carbonate esters and / or phosgene include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,5-hexanediol, 1,6-hexanediol, 2,5-hexanediol, 1 ,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, 1,4-cyclohexanedimethanol, hydroquinone, resorcinol, bisphenol A, bisphenol F, 4,4'-biphenol, and the like.
[0043] The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include alicyclic polyisocyanates, aliphatic polyisocyanates, aromatic polyisocyanates, etc., and examples thereof include alicyclic polyisocyanates, etc. These may be used alone or in combination of two or more.
[0044] Examples of alicyclic polyisocyanates include isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 4,4'-dicyclohexylmethane diisocyanate, 2,4-methylcyclohexane diisocyanate, 2,6-methylcyclohexane diisocyanate, cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, bis(2-isocyanatoethyl)-4-cyclohexylene-1,2-dicarboxylate, 2,5-norbornane diisocyanate, 2,6-norbornane diisocyanate, dimer acid diisocyanate, bicycloheptane triisocyanate, etc. These may be used alone or in combination of two or more.
[0045] (Acrylic Resin) As the acrylic resin, a polymer containing a (meth)acrylate monomer unit and optionally further containing other monomer units can be used. In the present invention, the phrase "containing a monomer unit" means that "a polymer obtained using the monomer contains a repeating unit derived from the monomer." In the present invention, "(meth)acrylate" means acrylate and / or methacrylate.
[0046] Here, the (meth)acrylate monomer unit is a repeating unit derived from a (meth)acrylate monomer. The (meth)acrylate monomer is not particularly limited, but examples thereof include (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, n-heptyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-dodecyl (meth)acrylate; and (meth)acrylic acid alkoxyalkyl ester monomers such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, and ethoxymethyl (meth)acrylate. The (meth)acrylate monomers may be used alone or in combination of two or more. In the present invention, the term "(meth)acrylic" means acrylic and / or methacrylic. The other monomer units are not particularly limited, and examples thereof include a repeating unit derived from an unsaturated carboxylic acid monomer, a repeating unit derived from a vinyl cyanide monomer, and a repeating unit derived from an alkenyl aromatic monomer.
[0047] (Elastomeric Resin) Examples of elastomeric resins include acrylonitrile butadiene rubber, ethylene-propylene-diene rubber (EPDM), ethylene-propylene rubber (EPM), natural rubber, polybutadiene rubber, polyisoprene rubber, styrene rubber, silicone rubber, and acrylic rubber. Styrene rubber may be a random copolymer or a hydrogenated product thereof, as long as it is a polymer of styrene and a conjugated diene compound. Specific examples include styrene-butadiene copolymer (SBR) and its hydrogenated product (HSBR). Examples of elastomeric resins include thermoplastic elastomers. Examples of thermoplastic elastomers include olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, vinyl chloride-based thermoplastic elastomers, polyurethane-based thermoplastic elastomer resins, polyester-based thermoplastic elastomers, and polyamide-based thermoplastic elastomers. The elastomer may be one of the above components, or two or more of them may be used in combination. A thermoplastic elastomer is preferred. Furthermore, silicone rubber, olefin-based thermoplastic elastomers, and styrene-based thermoplastic elastomers are more preferred from the viewpoint of easily adjusting the tensile storage modulus, rate of change in tensile storage modulus, sheet recovery rate, etc., within the above ranges. Furthermore, the above rubbers and elastomers may be mixed together, or thermoplastic resins with good compatibility may be mixed and used, as described below.
[0048] Examples of olefin-based thermoplastic elastomers include blend-type, dynamically crosslinked, and polymerized types. More specifically, examples include thermoplastic elastomers that use a thermoplastic crystalline polyolefin such as polypropylene or polyethylene for the hard segment and fully vulcanized or partially vulcanized rubber for the soft segment. Examples of the thermoplastic crystalline polyolefin include a homopolymer of an α-olefin having 1 to 4 carbon atoms or a copolymer of two or more α-olefins, with polyethylene or polypropylene being preferred. Examples of soft segment components include butyl rubber, halobutyl rubber, EPDM, EPM, acrylonitrile / butadiene rubber, NBR, and natural rubber, with EPDM being preferred. The olefin-based thermoplastic elastomer used in the present invention is preferably an olefin-based thermoplastic elastomer that can be produced by dynamic crosslinking and in which EPDM forms fine island phases within a polypropylene phase. When such an olefin-based thermoplastic elastomer is used, the sheet recovery rate and the rate of change in tensile storage modulus can be adjusted within the above-mentioned ranges, regardless of whether the resin foam sheet is crosslinked or not, although the reason is unclear. Examples of commercially available products of such thermoplastic elastomers include "Prime TPO" manufactured by Prime Polymer Co., Ltd. and "EXCELINK 4700P" manufactured by JSR Corporation.
[0049] Further, the olefin-based thermoplastic elastomer may be a block copolymer type. Examples of the block copolymer type include those having a crystalline block and a soft segment block, and more specifically, a crystalline olefin block-ethylene-butylene copolymer-crystalline olefin block copolymer (CEBC). In the CEBC, the crystalline olefin block is preferably a crystalline ethylene block, and examples of commercially available CEBCs include "DYNARON 6200P" manufactured by JSR Corporation.
[0050] Examples of the styrene-based thermoplastic elastomer include block copolymers having a styrene polymer or copolymer block and a conjugated diene compound polymer or copolymer block. Examples of the conjugated diene compound include isoprene and butadiene. The styrene-based thermoplastic elastomer used in the present invention may or may not be hydrogenated. When hydrogenation is performed, the hydrogenation can be performed by a known method.
[0051] The styrene-based thermoplastic elastomer is usually a block copolymer, and examples thereof include styrene-isoprene block copolymer, styrene-isoprene-styrene block copolymer, styrene-butadiene block copolymer, styrene-butadiene-styrene block copolymer, styrene-ethylene / butylene-styrene block copolymer (SEBS), styrene-ethylene / propylene-styrene block copolymer (SEPS), styrene-ethylene / butylene block copolymer (SEB), styrene-ethylene / propylene block copolymer (SEP), styrene-ethylene / butylene-crystalline olefin block copolymer (SEBC), etc. As the above-mentioned styrene-based thermoplastic elastomer, a block copolymer is preferred, and among these, SEBS and SEBC are more preferred.
[0052] Commercially available styrene-based thermoplastic elastomers include those manufactured by JSR Corporation, such as trade names "DYNARON 8600P" (styrene content: 15% by mass), "DYNARON 4600P" (styrene content: 20% by mass), and "DYNARON 1321P" (styrene content: 10% by mass).
[0053] Among the resins mentioned above, the resin constituting the foam sheet of the present invention is preferably at least one selected from the group consisting of polyolefin-based resins, urethane-based resins, and elastomer-based resins, more preferably polyolefin-based resins, even more preferably ethylene-based resins, and particularly preferably ethylene-based resins polymerized with metallocene compounds. Using a polyolefin-based resin in the core layer reduces the generation of resin debris when the foam sheet is torn in the planar direction, making it easier to prevent malfunctions in electronic devices caused by the inclusion of foreign matter due to the debris. Furthermore, the use of these specific types of resins also makes it easier to peel the foam sheet cleanly. Furthermore, it also makes it easier to improve unevenness conformability.
[0054] <Foaming Agent> The foam sheet of the present invention is preferably a foam obtained by foaming a foamable composition containing the above-mentioned resin and a foaming agent. The foam obtained by foaming is composed of a resin alone or a resin blended with additives as needed as a matrix resin, and has a large number of cells formed therein. Examples of the foaming agent include thermally decomposing foaming agents, and organic and inorganic foaming agents can be used as thermally decomposing foaming agents. Thermally decomposing foaming agents usually have a decomposition temperature higher than the melting temperature of the resin, and it is sufficient to use one with a decomposition temperature of, for example, 140 to 270°C. Specific organic blowing agents include azo compounds such as azodicarbonamide, azodicarboxylic acid metal salts (e.g., barium azodicarboxylate), and azobisisobutyronitrile; nitroso compounds such as N,N'-dinitrosopentamethylenetetramine; hydrazine derivatives such as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), and toluenesulfonylhydrazide; and semicarbazide compounds such as toluenesulfonylsemicarbazide. Inorganic blowing agents include ammonium carbonate, sodium carbonate, ammonium bicarbonate, sodium bicarbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate. Among these, azo compounds are preferred, and azodicarbonamide is particularly preferred, from the viewpoints of obtaining fine bubbles, economy, and safety. These thermally decomposable blowing agents can be used alone or in combination of two or more. The amount of the thermally decomposable foaming agent in the foamable composition is preferably 0.5 to 20 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, per 100 parts by mass of the resin.
[0055] When using a polyolefin resin, an acrylic resin, or an elastomer resin as the resin, it is preferable to use the above-mentioned thermal decomposition foaming agent as the foaming agent.However, foaming agents other than thermal decomposition foaming agents may also be used as the foaming agent.For example, when using a urethane resin, it is preferable to use water, an organic halogen compound, etc. as the foaming agent.The organic halogen compound may include an organic chlorine compound, an organic fluorine compound, etc., and is preferably an organic fluorine compound.The organic fluorine compound may include hydrofluorocarbons (HFCs), hydrofluoroolefins (HFOs), etc., which may further contain chlorine atoms.
[0056] A physical foaming agent may also be used as the foaming agent. A high-pressure inert gas is preferably used as the physical foaming agent. The inert gas is not particularly limited as long as it is inert to the resin composition and can be impregnated, and examples thereof include carbon dioxide, butane gas, nitrogen gas, and air. These gases may be used in combination. Of these, carbon dioxide and butane gas are preferred from the viewpoint of easily increasing the expansion ratio of the foam. The inert gas used for impregnation is preferably in a supercritical or subcritical state.
[0057] <Other Additives> The foam sheet or foamable composition may contain additives commonly used in foams, such as antioxidants, heat stabilizers, colorants, flame retardants, antistatic agents, fillers, and decomposition temperature regulators, as needed. Among these, antioxidants and decomposition temperature regulators are preferably used. Specific examples of decomposition temperature regulators include zinc oxide, zinc stearate, and urea. The content of the decomposition temperature regulator is preferably 0.01 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the resin.
[0058] [Outer Layer] When the outer layer is a non-foamed material, the outer layer may be a non-foamed resin layer, or may be a layer other than a resin, such as paper. The resin constituting the outer layer is not particularly limited as long as it can prevent the foam sheet from breaking when peeled off, but examples of resins that can be used include polyolefin resins, polyester resins such as polyethylene terephthalate, styrene acrylate resins, elastomer resins, and acrylic resins.
[0059] Among the above, polyolefin-based resins and polyester-based resins are preferred, with polyolefin-based resins being more preferred. The polyolefin-based resins are as described above for the foam, with polyethylene-based resins being more preferred. The polyolefin-based resins used in the core layer and the outer layer may be the same or different, but it is preferable to use the same. Using the same resins facilitates increasing the adhesive strength between the core layer and the outer layer and prevents interfacial delamination. When a foam sheet is produced by the first production method described below, the resin constituting the outer layer is preferably a polyolefin-based resin, more preferably a polyethylene-based resin. When a foam sheet is produced by the second production method, the resin used in the outer layer is preferably a polyolefin-based resin or a polyester-based resin, with polyethylene-based resins, polypropylene-based resins, and polyethylene terephthalate being more preferred. When a foam sheet is produced by the second production method, the resin layer used in the outer layer may be an oriented film or a non-oriented film. For example, when a propylene-based resin is used, it is preferable to use an OPP film.
[0060] When the outer layer is a foam, the foam constituting the outer layer only needs to have an expansion ratio lower than that of the foam constituting the core layer. Specifically, the expansion ratio is preferably greater than 1 and less than 5, more preferably 1.1 to 4, and even more preferably 1.1 to 2. When the outer layer is a foam, the resin constituting the outer layer is the same as the resin constituting the core layer described above, and a description thereof will be omitted. The closed cell ratio and degree of crosslinking may also be the same as those of the core layer described above. The resin for the outer layer may also contain additives as appropriate. The additives used may be the same as those used in the core layer.
[0061] (Thickness of Outer Layer) The thickness of the outer layer provided in the foam sheet of the present invention is preferably 5 μm or more, more preferably 6 μm or more, and even more preferably 10 μm or more. The thickness of the outer layer is preferably 300 μm or less, more preferably 100 μm or less, and even more preferably 40 μm or less. When the thickness of the outer layer is equal to or greater than the above-mentioned lower limit, the outer layer imparts tensile strength to the foam sheet, preventing the foam sheet from tearing during peeling from the adherend, and making it easier to impart excellent releasability to the foam sheet. When the thickness of the outer layer is equal to or less than the above-mentioned upper limit, the overall thickness of the foam sheet can be reduced, making it easier to use in thin electronic devices. Note that when the foam sheet is configured to have outer layers on both sides of the core layer, the thickness of the outer layer refers to the thickness of each outer layer. For example, when the thickness of each outer layer is 5 μm or more, it means that both outer layers are 5 μm or more. In addition, when the foam sheet has an outer layer on both sides of the core layer, it is preferable that both outer layers have the thickness within the above range. When the foam sheet has an outer layer on both sides of the core layer, the thicknesses of the outer layers may be the same or different, but are preferably the same.
[0062] When the foam sheet of the present invention is a multilayer body having outer layers, from the viewpoint of achieving excellent step-conforming ability and peelability of the foam sheet, the ratio of the thickness of the core layer to the thickness of the outer layer (thickness of core layer / thickness of each outer layer) is preferably 2.0 or more, more preferably 3.0 or more, even more preferably 5.0 or more, even more preferably 8.0 or more, and is preferably 50 or less, more preferably 30 or less, and even more preferably 20 or less. In the case of a multilayer body having outer layers on both sides of the core layer, the thickness of the outer layer when determining the above thickness ratio is the average value of the thicknesses of the outer layers on both sides.
[0063] <Method for Producing Foam Sheet> Hereinafter, methods for producing a foam sheet when the foam sheet is a multilayer body having a core layer and an outer layer will be described as production methods 1 and 2. (First Production Method) The foam sheet of the present invention is not particularly limited, but can be produced, for example, by a method (hereinafter also referred to as the "first production method") in which an outer layer is laminated on one or both sides of a layer made of a foamable composition to obtain a laminate sheet, and then the laminate sheet is foamed.
[0064] More specifically, the manufacturing method 1 includes the following steps I to II: (I) a step of obtaining a laminate sheet having a layer made of a foamable composition and an outer layer formed on one or both sides of the layer; and (II) a step of obtaining a foam sheet by foaming the layer made of the foamable composition of the laminate sheet.
[0065] Each step is described below. (Step (I)) The method for obtaining the laminate sheet in step (I) is not particularly limited, but co-extrusion molding is preferred. Specifically, when outer layers are formed on both sides of a layer made of a foamable resin composition, the resin for forming the outer layers and other additives blended as needed are fed to a first and a third extruder, respectively, and melt-kneaded to obtain a resin composition for forming the outer layers. The resin for forming the core layer, a foaming agent such as a thermally decomposable foaming agent, and other additives blended as needed are fed to a second extruder and melt-kneaded to obtain a foamable composition for forming the core layer. The compositions fed from the first to third extruders are then merged, with the composition fed from the second extruder forming the middle layer, and the resulting mixture is extruded into a sheet using a T-die or the like to obtain a three-layer laminate sheet. However, in a method for obtaining a three-layer laminate sheet, if the composition of both outer layers is the same, two extruders (first and third extruders) may not be used, but one extruder may be used, and the resin compositions of both outer layers may be supplied from that one extruder.
[0066] When an outer layer is formed on one side of a layer made of a foamable composition, the resin for forming the outer layer and other additives as needed are fed to a first extruder and melt-kneaded to obtain a resin composition for forming the outer layer. The resin for forming the core layer, a foaming agent such as a thermally decomposable foaming agent, and other additives as needed are fed to a second extruder and melt-kneaded to obtain a foamable resin composition for forming the core layer. The resin composition fed from the first extruder is then merged with the composition fed from the second extruder and extruded into a sheet using a T-die or the like to obtain a two-layer multilayer laminate sheet. In co-extrusion molding, either a feedblock method or a multi-manifold method may be used, but the feedblock method is preferred.
[0067] In the above method, it is preferable to further crosslink the laminate sheet after step (I). Although a crosslinking method may involve blending an organic peroxide in advance and heating the laminate sheet obtained in step (I) to crosslink it, it is preferable to crosslink the laminate sheet by irradiating it with ionizing radiation. Examples of ionizing radiation include electron beams and β-rays, with electron beams being preferred. The dose of ionizing radiation is preferably 1 to 10 Mrad, more preferably 1.5 to 5 Mrad. Crosslinking is preferably carried out before step (II).
[0068] (Step (II)) In step (II), the laminate sheet obtained in step (I) is foamed to foam the layer comprising the foamable composition. The layer comprising the foamable composition may be treated so as to foam the foaming agent. When the foaming agent is a thermally decomposable foaming agent, the foaming is achieved by heating the laminate sheet. The heating temperature may be equal to or higher than the temperature at which the thermally decomposable foaming agent decomposes, for example, about 150 to 320°C. The method for heating the laminate sheet is not particularly limited, and examples include a method in which the laminate sheet is heated with hot air, infrared radiation, a salt bath, or an oil bath, and these may be used in combination. The laminate sheet may also be appropriately stretched during or after foaming. Note that the above description has been given of an example in which the outer layer is a resin film (non-foamed material). However, when the outer layer is a foamed material, a foaming agent such as a thermally decomposable foaming agent may be blended as an additive in the resin composition for forming the outer layer, and foamed in step (II).
[0069] (Second Manufacturing Method) The foam sheet of the present invention can also be manufactured by another method. Specifically, a foam layer constituting the core layer is manufactured in advance, and a resin film or foam layer constituting the outer layer is superimposed on one or both sides of the foam layer and bonded to the foam layer (also referred to as a "second manufacturing method").
[0070] In the second production method, a foam may be obtained by melt-kneading a resin for forming the core layer, a thermally decomposable foaming agent, and additives blended as necessary to obtain a foamable composition for forming the core layer, and then molding the foamable composition into a sheet (foamable composition sheet). The method for melt-kneading the foamable composition and molding it into a sheet is not particularly limited, but it is preferably carried out using an extruder.
[0071] The obtained foamable composition sheet is preferably further crosslinked before foaming, as described below. Although a crosslinking method may involve blending an organic peroxide in advance and heating the foamable composition sheet to crosslink it, it is preferred to crosslink the foamable composition sheet by irradiating it with ionizing radiation. The type and dose of ionizing radiation are as described in the first production method above.
[0072] Next, the foamable composition sheet may be foamed. The layer made of the foamable composition may be treated so that the foaming agent foams. When the foaming agent is a thermally decomposable foaming agent, the laminate sheet is heated to foam. The heating temperature and heating method are as described in the first production method. The foamable composition sheet may be appropriately stretched during or after foaming.
[0073] Thereafter, a separately prepared resin film or foam for forming the outer layer is superimposed on one or both sides of the foam layer constituting the base layer and bonded to obtain a multilayer body. Specifically, the layers may be thermocompression bonded by heating and pressurizing using a press or the like. Alternatively, the foam layer and the surface layer may be bonded together by applying a pressure-sensitive adhesive, adhesive, or the like to the bonding surface between them, or by applying a double-sided adhesive tape. The foam for forming the outer layer may be produced by the same method as the foam for forming the core layer, or by a different method.
[0074] [Adhesive Tape] The present invention also provides an adhesive tape using the foam sheet as a substrate. The adhesive tape, for example, comprises an adhesive material provided on at least one side of the foam sheet. The adhesive tape can be adhered to other components via the adhesive material. The adhesive tape may comprise a foam sheet having an adhesive material provided on both sides or one side. The adhesive tape is preferably used to secure panels in thin electronic devices such as televisions and smartphones. Furthermore, when the foam sheet is a multilayer body, the adhesive material is preferably provided on an outer layer constituting the multilayer body. For example, when a multilayer body having an outer layer on only one side of the foam sheet is used as the substrate, the adhesive tape preferably comprises a multilayer body 2 in which a foam sheet A, an outer layer B, and an adhesive material X are laminated in this order, as shown in Figure 2. This configuration improves the tensile strength of the entire adhesive tape due to the outer layer, making the foam sheet less likely to be damaged during peeling, and facilitating peeling without leaving any adhesive on the adherend. When outer layers are provided on both sides of the foam sheet, the adhesive may be provided on only one side of the foam sheet or on both sides, but it is preferable that the adhesive be provided on both sides.
[0075] The adhesive material may comprise at least a pressure-sensitive adhesive layer. It may be a single pressure-sensitive adhesive layer laminated on the surface of a foam sheet, or a double-sided pressure-sensitive adhesive sheet attached to the surface of a foam sheet. However, a single pressure-sensitive adhesive layer is preferred. The double-sided pressure-sensitive adhesive sheet comprises a substrate and pressure-sensitive adhesive layers provided on both sides of the substrate. The double-sided pressure-sensitive adhesive sheet is used to adhere one pressure-sensitive adhesive layer to the foam sheet and the other pressure-sensitive adhesive layer to another component. The pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is not particularly limited, and examples include acrylic pressure-sensitive adhesives, urethane pressure-sensitive adhesives, and rubber pressure-sensitive adhesives. A release sheet such as release paper may be further laminated on the adhesive material. The thickness of the adhesive material is preferably 5 to 200 μm, more preferably 7 to 150 μm, and even more preferably 10 to 100 μm.
[0076] [Uses] The uses of the foam sheet and the pressure-sensitive adhesive tape comprising the foam sheet are not particularly limited. For example, they are preferably used inside electronic devices, and can be used, for example, as a panel fixing material. Examples of electronic devices include televisions, notebook personal computers, mobile phones, smartphones, tablets, portable electronic devices such as portable music players, cameras, displays, game consoles, electronic organizers, and personal computers. As described above, the foam sheet of the present invention and the pressure-sensitive adhesive tape comprising the foam sheet have excellent release properties and also good step-conforming properties. Therefore, the pressure-sensitive adhesive tape comprising the foam sheet is preferably used for displays, particularly large displays, and specifically, displays of 20 inches or larger. The display may be a liquid crystal display or an organic electroluminescence (EL) display. When the pressure-sensitive adhesive tape comprising the foam sheet is used for a display, the pressure-sensitive adhesive tape comprising the foam sheet is used on the back surface or frame of the display, preferably the frame. Furthermore, as described above, the adhesive tape of the present invention has excellent step-conforming properties, so when the adhesive tape of the present invention is used in a display, the adhesive tape of the present invention can conform to the steps of the display housing, and as a result, the area of the gap between the adhesive tape and the housing can be reduced.
[0077] Furthermore, since the adhesive tape including the foam sheet can be torn in the planar direction and then peeled off, when used for the above-mentioned purposes, for example, when it is necessary to peel it off from components inside an electronic device during repair, it can be peeled off without relying on the peeling technique of the worker, without placing stress on the components inside the electronic device, and without leaving any adhesive on the components, thereby facilitating the reuse of components such as displays.
[0078] The present invention will be explained in more detail by way of examples, but the present invention is not limited to these examples in any way.
[0079] [Measurement Methods] The methods for measuring and evaluating each physical property are as follows.
[0080] <Thickness of Core Layer and Outer Layer> A cross section of the foam sheet was photographed using a digital microscope (manufactured by Keyence Corporation, product name VHX-900), and the thickness of each of the core layer and outer layer was measured from the photographed image.
[0081] <Total Thickness (Thickness of Foam Sheet)> The total thickness of the core layer and the outer layer was defined as the thickness of the foam sheet.
[0082] <Apparent density and expansion ratio> The apparent density was measured in accordance with JIS K7222. 3 The reciprocal of this was taken as the expansion ratio (times).
[0083] <Gel Fraction> A test piece of about 100 mg was taken from the foam constituting the core layer, and the mass A (mg) of the test piece was precisely weighed. Next, this test piece was immersed in 30 cm of xylene at 120°C. 3 After immersion in the solution for 24 hours, the insoluble matter on the screen was filtered through a 200-mesh wire netting, vacuum-dried, and the mass B (mg) of the insoluble matter was precisely weighed. From the obtained value, the gel fraction (mass%) was calculated using the following formula. The test pieces were collected evenly along the thickness direction of the foam constituting the core layer. Gel fraction (mass%) = 100 × (B / A)
[0084] <Average Cell Diameter> The foam constituting the core layer was cut into 50 mm squares, immersed in liquid nitrogen for 1 minute, and then cut in the thickness direction along each of the MD and TD. A 200x magnified photograph was taken using a digital microscope (Keyence Corporation, product name VHX-900). For the foam in the photographed image, the cell diameters in MD and ZD, and the cell diameters in TD and ZD were measured for all bubbles present in a 2 mm-long cut surface in each of the MD and TD, and this operation was repeated five times. The average values of the cell diameters of all bubbles in MD and TD were taken as the average cell diameters in MD and TD, and the average value of the cell diameters of all ZDs measured by the above operation was taken as the average cell diameter in ZD.
[0085] <Closed Cell Ratio> The closed cell ratio was measured according to the method of ASTM D2856 (1998). Specifically, the measurement was carried out as follows. First, a flat square test piece with a side length of 5 cm was cut out from the foam constituting the core layer. Then, the thickness of the test piece was measured to determine the apparent volume V of the test piece. 1 Calculate the weight of the test piece W 1 Next, the volume V occupied by the bubbles was measured. 2 was calculated based on the following formula: The density of the matrix resin constituting the test piece was ρ (g / cm 3 The volume occupied by the bubbles V 2 =V 1 -W 1 Next, the test piece was submerged in distilled water at 23°C to a depth of 100 mm from the water surface, and a pressure of 15 kPa was applied to the test piece for 3 minutes. After that, the pressure was released in the water, and the test piece was left to stand for 1 minute. Then, the test piece was taken out of the water, and the water adhering to the surface of the test piece was removed, and the weight W of the test piece was measured. 2 The open cell rate F and closed cell rate F were measured based on the following formula: 2 The open cell ratio F 1 (%) = 100 × (W 2 -W 1 ) / V 2 Closed bubble rate F 2 (%) = 100 - F 1
[0086] <25% Compression Strength> Measurement was carried out at a measurement temperature of 23°C according to a method in accordance with JIS K 6767.
[0087] <Tensile strength> The foam sheets produced in each of the Examples and Comparative Examples were cut into a dumbbell No. 1 shape as specified in JIS K6251 4.1. These were used as samples and subjected to measurements of tensile strength in the MD direction at a measurement temperature of 23°C and a speed of 500 mm / min using a tensile tester (product name: Tensilon RTF235, manufactured by A&D Co., Ltd.).
[0088] <Breaking Strength> FIG. 3 shows a schematic diagram of a test apparatus for evaluating breaking strength as interlaminar strength. A primer ("PPX Primer" manufactured by Cemedine Co., Ltd.) was applied to a 25 mm square area of the foam sheet 11 obtained in each Example and Comparative Example, and then a 5 mm diameter portion of adhesive 12 ("PPX" manufactured by Cemedine Co., Ltd.) was dripped onto the center of the applied area. Immediately thereafter, a 25 mm square aluminum jig 13 was placed on the adhesive dripped area, and the foam sheet and jig 13 were pressure-bonded together. The foam sheet was then cut to the size of the jig 13. Primer was applied to the side of the cut foam sheet not attached to the jig 13, and a 5 mm diameter portion of adhesive 12 was dripped onto the center of the applied area. Immediately thereafter, a 10 mm square aluminum jig 14 was placed on the adhesive dripped area, and the foam sheet and jig 14 were pressure-bonded together. After wiping off any adhesive that had protruded around the periphery of the jig 14, an incision 15 was made in the foam sheet along the size of the jig 14. This was left at room temperature for 30 minutes to cure the adhesive, and a sample for breaking strength measurement was prepared. Next, a 1 kN load cell was installed in a testing machine ("Tensilon Universal Material Testing Machine" manufactured by A&D Co., Ltd.) equipped with a thermostatic chamber so that testing could be performed in the thermostatic chamber. The sample for breaking strength measurement was then attached to the testing machine so that the sheet surface of the foam sheet was perpendicular to the tensile direction. The temperature of the thermostatic chamber was set to 23°C, and the sample for breaking strength measurement was left until the temperature of the sample for breaking strength measurement reached 23°C. One side of the jig was then pulled vertically upward at a speed of 100 mm / min, peeling only a 1 cm square area of the foam sheet. The breaking strength at this time was measured and recorded as the first measurement result. The same procedure was repeated three times, and the average value was recorded as the breaking strength at 23°C.
[0089] <Tearability> After applying a pressure-sensitive adhesive to the foam sheet produced in each Example and Comparative Example, the foam sheet was sandwiched between SUS plates, and the blade of a cutter (manufactured by OLFA, product name "Bending Blade Cutter Knife") was inserted into the side of the foam sheet in the MD direction, and the cutter was slid in the MD direction to cut (tear) the foam sheet. The tearability was evaluated based on the progress of the cutter. The evaluation criteria are as follows: (Evaluation Criteria) A: Excellent (the cutter progressed to the end without generating resin debris, and the foam sheet was torn in half). B: Good (the cutter progressed to the end, and the foam sheet was torn in half, but resin debris was generated). C: The cutter did not progress to the end, and the foam sheet could not be torn in half.
[0090] <Evaluation of Adhesive Residue Upon Peeling> After evaluating the tearability as described above, the split foam sheet was peeled off from the SUS plate as the adherend, and the SUS plate was observed after peeling to evaluate the adhesive residue upon peeling based on the amount of adhesive remaining. The evaluation criteria are as follows. (Evaluation Criteria) A: The adhesive layer was not broken at the interface between the adhesive layer and the adherend, and the split foam sheet was able to be peeled cleanly from the adherend all the way to the end. B: The adhesive layer was broken several times at the interface between the adhesive layer and the adherend, and although part of the adhesive layer remained on the adherend, the split foam sheet was able to be peeled all the way to the end. C: The adhesive layer was broken at the interface between the adhesive layer and the adherend, and the split foam sheet was torn or torn and could not be peeled all the way to the end.
[0091] <Overall Evaluation> The physical properties of the foam sheet were evaluated comprehensively based on the following evaluation criteria. (Evaluation Criteria) A: The evaluation result was not "C" in either the evaluation of tearability or the evaluation of adhesive residue upon peeling. B: The evaluation result was "C" in at least one of the evaluation of tearability or the evaluation of adhesive residue upon peeling.
[0092] Example 1: A metallocene-catalyzed linear low-density polyethylene resin (metallocene LLDPE, manufactured by Japan Polyethylene Corporation, trade name "Kernel KF283") was prepared as the resin for forming the core layer, which was a foam. Azodicarbonamide was prepared as the thermal decomposition type blowing agent. Furthermore, zinc oxide (manufactured by Sakai Chemical Industry Co., Ltd., trade name "OW-212F") was prepared as the decomposition temperature regulator. 2,6-di-t-butyl-p-cresol, a phenolic antioxidant, was prepared as the antioxidant. 100 parts by mass of the linear low-density polyethylene resin (metallocene LLDPE), 4.5 parts by mass of the thermal decomposition type blowing agent, 1 part by mass of the decomposition temperature regulator, and 0.5 parts by mass of the antioxidant were fed into a second extruder and melt-kneaded at 130°C to produce a foamable resin composition for the core layer. The resin, decomposition temperature regulator, and antioxidant for the outer layer were the same as those for the core layer. 100 parts by weight of linear low-density polyethylene resin (metallocene LLDPE), 1 part by weight of decomposition temperature regulator, and 0.5 parts by weight of antioxidant were fed into the first and third extruders and melt-kneaded at 130°C to prepare a resin composition for the outer layer. The foamable resin composition was co-extruded from the second extruder to a thickness of 330 μm, and the resin composition was co-extruded from the first and third extruders to a thickness of 220 μm each, to obtain an unfoamed laminate sheet comprising a layer made of the foamable resin composition for the core layer and layers made of the resin composition for the outer layer laminated on both sides of the core layer. The laminate sheet was then irradiated with an electron beam at an acceleration voltage of 550 kV at 4.0 Mrad to crosslink the laminate sheet. Thereafter, the crosslinked laminate sheet was continuously fed into a foaming furnace maintained at 250°C by hot air and an infrared heater, where it was heated and foamed, and stretched to a target thickness in a stretching step, thereby obtaining a foam sheet of Example 1 consisting of a non-foamed material (outer layer) / foamed material (core layer) / non-foamed material (outer layer).
[0093] Examples 2 and 3, Comparative Example 2 Foam sheets were obtained in the same manner as in Example 1, except that the content of the foaming agent in the foamable resin composition was changed as shown in Table 1.
[0094] [Examples 4 and 5] Foam sheets were obtained in the same manner as in Example 1, except that the thicknesses of the foamable resin composition co-extruded from the second extruder and the resin compositions co-extruded from the first and third extruders, and the content of the foaming agent in the foamable resin composition were changed as shown in Table 1.
[0095] [Example 6] A foam sheet was obtained in the same manner as in Example 1, except that the resin for forming the core layer was changed to a styrene-based thermoplastic elastomer (Hybler 7311F manufactured by Kuraray Co., Ltd.) and the content of the foaming agent in the foamable resin composition was changed as shown in Table 2.
[0096] [Example 7] A foam sheet was obtained in the same manner as in Example 1, except that a urethane resin foam (trade name "Poron" manufactured by Inoac Corporation) and a non-foamed material (outer layer) were bonded together using an adhesive. In Example 7, the gel fraction of the core layer was not measured.
[0097] [Comparative Example 1] A foam sheet was obtained in the same manner as in Example 1, except that the thicknesses of the foamable resin composition co-extruded from the second extruder and the resin compositions co-extruded from the first and third extruders, and the content of the foaming agent in the foamable resin composition were changed as shown in Table 2.
[0098] [Comparative Example 3] A core layer was obtained in the same manner as in Example 1, except that no raw materials were supplied to the first and third extruders, no resin composition was laminated on the layer made of the foamable resin composition for the core layer, and the thickness of the foamable resin composition co-extruded from the second extruder was changed as shown in Table 2.
[0099]
[0100]
[0101] As is clear from the above examples, the foam sheets satisfying the requirements of the present invention could be torn in the plane direction and, upon peeling, no adhesive remained on the adherend, thereby demonstrating excellent releasability. In contrast, the foam sheets produced in Comparative Examples 1 and 3 had low tensile strength, so the foam sheets were torn during peeling, leaving adhesive on the adherend. Furthermore, the foam sheet produced in Comparative Example 2 had high breaking strength, so it did not tear in the plane direction and was unable to demonstrate excellent releasability.
[0102] REFERENCE SIGNS LIST 1 Multilayer body 2 Adhesive sheet A Core layer (foam) B, C Outer layer X Adhesive material 11 Foam sheet 12 Adhesive 13 Jig 14 Jig 15 Notch
Claims
1. A foam sheet having a tensile strength of 1 to 9 MPa and a breaking strength of 3.5 MPa or less when measuring interlaminar strength, wherein the foam sheet has a total thickness of 0.05 to 0.9 mm.
2. The foam sheet according to claim 1, wherein the foam sheet has a 25% compressive strength of 150 kPa or less.
3. The density of the entire foam sheet is 0.07 to 0.60 g / cm 3 The foam sheet according to claim 1 , 4. The foam sheet according to claim 1, comprising a core layer which is a foam, and outer layers which are provided on both sides of the core layer and which are either foams having a lower expansion ratio than the core layer or non-foamed.
5. The foam sheet according to claim 4, wherein the expansion ratio of the core layer is 5 to 20 times.
6. The foam sheet according to claim 4, wherein a thickness ratio of the core layer to the outer layer (thickness of the core layer / average thickness of the outer layer) is 2 or more.
7. The foam sheet according to claim 4, wherein the core layer has a closed cell ratio of 90% or more.
8. The foam sheet according to claim 4, wherein each of the outer layers has a thickness of 5 μm or more.
9. The foam sheet according to claim 4, wherein the average bubble diameter of the bubbles in the core layer is 20 to 500 μm.
10. The foam sheet of claim 4, wherein the core layer is a crosslinked foam.
11. The foam sheet according to claim 10, wherein the core layer has a gel fraction of 20 to 50 mass %.
12. The foam sheet according to claim 4, wherein the resin constituting the core layer is at least one selected from the group consisting of polyolefin-based resins, urethane-based resins, acrylic-based resins, and elastomer-based resins.
13. An adhesive tape comprising the foam sheet according to any one of claims 1 to 12 and an adhesive material provided on at least one surface of the foam sheet.
Citation Information
Patent Citations
Photocurable adhesive sheet, adhesive sheet and image display device
WO2016194957A1
Multilayer foam sheet
WO2022030649A1
Multilayer foam sheet and adhesive tape
WO2022080219A1