Lithium metal battery and manufacturing method therefor
The lithium metal battery design with a ceramic coating layer on the separator and gel-type polymer electrolyte addresses dendrite growth and stability issues, enhancing lifespan and performance by minimizing side reactions and maintaining high ionic conductivity.
Patent Information
- Application Number
- PCT/KR2024/003331
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium metal batteries face issues with lithium dendrite growth due to side reactions with the electrolyte, leading to short circuits and reduced lifespan, and existing carbon-based anode materials have limited capacity and stability concerns.
A lithium metal battery design featuring a ceramic coating layer on one side of a porous substrate separator with a gel-type polymer electrolyte in its pores, which suppresses dendrite formation and enhances electrolyte wettability, improving the battery's lifespan and performance.
The solution effectively reduces dendrite growth and increases the battery's lifespan by minimizing side reactions and maintaining high ionic conductivity, while also improving heat resistance and reducing material costs.
Smart Images

Figure KR2024003331_03102024_PF_FP_ABST
Abstract
Description
Lithium metal battery and manufacturing method thereof
[0001] It relates to a lithium metal battery and a method for manufacturing the same.
[0002] Lithium metal batteries currently on the market primarily use carbon-based anode materials, such as graphite. Carbon-based anode materials exhibit no volume change during charge / discharge, enhancing the stability of lithium metal batteries. However, their low capacity necessitates the use of higher-capacity anode materials.
[0003] Lithium metal, which has a much larger theoretical electric capacity than carbon-based negative electrode materials, can be used as a negative electrode material.
[0004] When lithium metal is charged and discharged, dendrites are formed on the surface of the lithium metal due to a side reaction with the electrolyte, and the growth of the dendrites can cause a short circuit between the positive and negative electrodes, which can reduce the life characteristics of a lithium metal battery containing lithium metal.
[0005] One aspect is to provide a lithium metal battery with a new structure.
[0006] Another aspect is to provide a method for manufacturing the above-described lithium metal battery.
[0007] According to the implementation example
[0008] A lithium metal battery is provided, comprising: a negative electrode current collector; a positive electrode; and a separator disposed between the negative electrode current collector and the positive electrode, wherein the negative electrode current collector and the separator include a negative electrode active material layer disposed between the negative electrode current collector and the separator or wherein the negative electrode active material layer is absent; the separator includes a porous substrate; and a ceramic coating layer disposed on one surface of the porous substrate, wherein the ceramic coating layer is positioned to face the negative electrode current collector, and the other surface of the porous substrate is free of the ceramic coating layer, and wherein the pores of the porous substrate include a gel-type polymer electrolyte.
[0009] The above ceramic coating layer includes large-diameter inorganic particles and small-diameter inorganic particles. In addition, the mixing weight ratio of the large-diameter inorganic particles and the small-diameter inorganic particles in the ceramic coating layer is 9:1 to 1:1.
[0010] According to another embodiment, the method comprises the steps of: preparing a negative electrode current collector; forming a ceramic coating layer on one surface of a porous substrate to form a separator; preparing a positive electrode;
[0011] A step of arranging a separator on a negative electrode current collector, such that the ceramic coating layer faces the negative electrode current collector; a step of forming a battery structure by arranging a negative electrode current collector, a separator, and a positive electrode; a step of housing the battery structure in a battery case, and then injecting a composition for forming a gel-type polymer electrolyte into the battery structure; and
[0012] A method for manufacturing a lithium metal battery is provided, including a step of forming a gel-type polymer electrolyte by curing the composition for forming the gel-type polymer electrolyte.
[0013] According to one aspect, a lithium metal battery is provided in which dendrite formation is suppressed and electrolyte wettability is increased by using a separator having a ceramic coating layer only on the surface facing the negative electrode collector in the porous substrate and containing a gel-type polymer electrolyte in the pores of the porous substrate, thereby improving life characteristics.
[0014] Figure 1 is a cross-sectional view of a cathode according to an exemplary embodiment.
[0015] Figure 2 is a cross-sectional view of a cathode according to another exemplary embodiment.
[0016] Figure 3 is a schematic diagram of a lithium metal battery according to an embodiment.
[0017] Figure 4 is a schematic diagram of a lithium metal battery according to another embodiment.
[0018] Figure 5 is a schematic diagram of a lithium metal battery according to another embodiment.
[0019] <Explanation of key symbols in the drawing>
[0020] 1: Lithium metal battery 2, 20: Cathode
[0021] 3, 10: Anode 4: Separator
[0022] 5: Battery case 6: Cap assembly
[0023] 7: Battery structure 8: Electrode tab
[0024] The present inventive concept described below is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail. However, this is not intended to limit the present inventive concept to specific embodiments, but rather to encompass all modifications, equivalents, or alternatives within the technical scope of the present inventive concept.
[0025] The terminology used below is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. Hereinafter, the terms "comprises" or "has" and the like are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. The " / " used below may be interpreted as "and" or "or" depending on the context.
[0026] To clearly represent multiple layers and areas in a drawing, the thickness is enlarged or reduced.
[0027] . Similar parts are given the same drawing reference numerals throughout the specification. When a layer, film, region, plate, etc. is said to be "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. Terms such as first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only for the purpose of distinguishing one component from another. In this specification and the drawings, components having substantially the same functional configuration are referred to by the same reference numerals, and redundant descriptions are omitted.
[0028] In the present disclosure, the "particle diameter" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle diameter of a particle can be measured using a particle size analyzer (PSA). The "particle diameter" of a particle is, for example, the average particle diameter. The average particle diameter is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of a particle corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by, for example, laser diffraction. The average particle diameter and average major axis length of a particle can be measured using a scanning electron microscope. When the particle size is measured using a scanning electron microscope, it is determined as the average value of 30 or more randomly selected particles having a size of 1 μm or more, excluding fine particles.
[0029] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0030] In this disclosure, “alloy” means a mixture of two or more metals.
[0031] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.
[0032] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0033] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material.
[0034] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.
[0035] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.
[0036] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.
[0037] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.
[0038] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.
[0039]
[0040] Hereinafter, a lithium metal battery and a manufacturing method thereof according to embodiments will be described in more detail.
[0041] A non-cathode lithium metal battery is a battery that uses only a cathode current collector without a cathode active material layer. When charging, lithium ions transferred from the cathode are deposited on the surface of the cathode current collector, and when discharging, the lithium deposited on the cathode current collector is eluted again and inserted into the cathode, thereby operating the battery.
[0042] Non-cathode lithium metal batteries offer the advantage of maximizing energy density per volume / weight of the battery by omitting lithium metal as the anode active material. However, lithium metal precipitates during operation, and the uneven current concentration during oxidation / reduction causes lithium dendrites to grow. These dendrites not only cause lithium anode loss, reducing battery capacity and lifespan, but can also cause short-circuiting between the anode and cathode, posing safety concerns.
[0043] To solve the above-mentioned problems, a method has been proposed in which a protective film is introduced to minimize contact between lithium and the electrolyte and thereby reduce side reactions, or a method has been proposed in which a liquid electrolyte is introduced into a network of cross-linked polymers to minimize exposure of the electrolyte on the electrode surface and to create a uniform flow of lithium ions throughout the electrode, thereby suppressing lithium dendrite growth by using a gel polymer electrolyte.
[0044] Polyolefin membranes, used as porous substrates for lithium secondary battery separators, have limited porosity and tortuosity to prevent short circuits. Consequently, polyolefin membranes exhibit approximately 10 times lower ionic conductivity than bulk electrolytes. In contrast, gel-type polymer electrolytes offer improved safety compared to pure liquid electrolytes, but at the cost of increased resistance.
[0045] A lithium metal battery according to an embodiment of the present invention can solve the above-described problem by forming a ceramic coating layer only in a direction facing adjacent to a negative electrode current collector in a porous substrate and using a separator containing a gel-type polymer electrolyte in the pores of the porous substrate.
[0046] A lithium metal battery according to an embodiment of the present invention includes a negative electrode current collector; a positive electrode; and a separator disposed between the negative electrode current collector and the positive electrode.
[0047] It includes a negative electrode active material layer disposed between the negative electrode current collector and the separator, or the negative electrode active material layer is absent (free).
[0048] The above separator comprises a porous substrate; and a ceramic coating layer disposed on one surface of the porous substrate; wherein the ceramic coating layer is positioned to face the negative electrode current collector,
[0049] The other side of the above porous substrate is free of a ceramic coating layer,
[0050] The pores of the above porous substrate contain a gel-type polymer electrolyte.
[0051] When a ceramic coating layer is formed on both sides of the porous substrate constituting the separator, the separator has excellent ionic conductivity due to a compensatory effect of improved electrolyte wettability, but the volumetric energy density of the lithium metal battery may decrease as the cell thickness increases.
[0052] However, in a lithium metal battery according to one embodiment, a ceramic coating layer is formed only on one side of a porous substrate, thereby maximizing cell performance in a lithium metal battery by suppressing lithium dendrite formation through the rigidity of the ceramic coating layer without significantly increasing the resistance of the cell.
[0053] The ceramic coating layer has nanopores, which cause a capillary phenomenon and improve electrolyte wettability. Here, the nanopores have a size of 1 nm to 500 nm, 2 nm to 480 nm, 3 nm to 450 nm, 5 nm to 400 nm, 10 nm to 300 nm, 20 nm to 300 nm, 30 nm to 300 nm, 25 nm to 280 nm, 50 nm to 250 nm, or 50 nm to 150 nm. Alternatively, the nanopores have a size of, for example, 50 nm to 500 nm, 100 nm to 400 nm, or 150 nm to 300 nm.
[0054] In this specification, the size of a nanopore refers to the average diameter when the nanopore is spherical in shape, and the average major axis length when the nanopore is non-spherical. The size of the nanopore can be confirmed through scanning electron microscope image analysis. In this disclosure, the size refers to the average size.
[0055] Adopting a separator with a ceramic coating layer featuring the aforementioned nanopores can ensure heat resistance and improve heat shrinkage characteristics. Furthermore, by reducing the separator margin for safety during cell design, the material costs of lithium metal batteries can be reduced. Furthermore, by physically inhibiting dendrite growth on the cathode, lithium metal batteries can be manufactured with improved long-term lifespans at both room and high temperatures.
[0056] If the ceramic coating layer is formed on both sides of the porous substrate so that each ceramic coating layer faces the positive and negative electrodes, the overall resistance of the cell increases due to an increase in the additional resistance component, which may increase the overvoltage, resulting in a reduction in the long-term lifespan and a decrease in the volumetric energy density.
[0057] The thickness of the ceramic coating layer is 10 nm to 5,000 nm, 30 nm to 4,500 nm, 50 nm to 4,000 nm, 80 nm to 3,800 nm, 100 nm to 3,500 nm, 150 nm to 3,200 nm, 200 nm to 3,000 nm, 250 nm to 2,800 nm, 300 nm to 2,500 nm, or 500 nm to 2,000 nm. When the thickness of the ceramic coating layer is within the above range, a lithium metal battery having excellent electrolyte wettability and excellent dendrite growth suppression effect can be manufactured. In the present specification, thickness means an average thickness.
[0058] The ceramic coating layer includes inorganic particles and a binder.
[0059] According to an embodiment, any inorganic particle that can be used when forming a coating layer of a separation membrane can be used, and for example, any inorganic oxide of SiO2, Al2O3, Al(OH)3, AlO(OH), TiO2, BaTiO3, ZnO2, Mg(OH)2, AIN(Aluminum Nitride), SiC(Silicon Carbide), BoN(Boron Nitride) or a combination thereof can be used.
[0060] According to another implementation example, the inorganic particles include BaTiO3, BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb having a dielectric constant of 5 or more. 1-a La a Zr 1-b Ti b O3 (PLZT, where, 0 <a<1, 0<b<1임), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC or a combination thereof can be used.
[0061] In addition to the ceramic coating layer, the inorganic particles having lithium ion transfer capability, i.e. lithium phosphate (Li3PO4), lithium titanium phosphate (Li c Ti d (PO4)3, 0 <d<2, 0<d<3), 리튬알루미늄티타늄포스페이트 (Li a1 Al b1 Ti c1 (PO4)3, 0 <a1<2, 0<b1<1, 0<c1<3), 14Li2O-9Al2O3-38TiO2-39P2O5 등과 같은 (LiAlTiP) a2 O b2 Series Glass (0) <a2<4, 0<b2<13), 리튬란탄티타네이트 (Li a3 La b3 TiO3, 0 <a3<2, 0<b3<3), Li 3.25 Ge0.25 P 0.75 Lithium germanium thiophosphate (Li) such as S4 a4 Ge b4 P c2 S d , 0 <a4<4, 0<b4<1, 0<c2<1, 0<d<5), Li3N 등과 같은 리튬나이트라이드 (Li a5 N b5 , 0 <a5<4, 0<b5<2), Li3PO4-Li2S-SiS2 등과 같은 SiS2 계열 글래스 (Li a6 Si b6 S c3 , 0 <a6<3, 0<b6<2, 0<c3<4), LiI-Li2S-P2S5 등과 같은 P2S5 계열 글래스 (Li a7 P b7 S c4 , 0 <a7<3, 0<b7<3, 0<c4<7) 또는 이들의 혼합물 등이 더 함유될 수 있다.
[0062] The binder may include, for example, one or more selected from polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trichloroethylene copolymer, polyvinylidene fluoride-chlorotrifluoroethylene copolymer, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene vinyl acetate copolymer, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxyl methyl cellulose (CMC), acrylonitrile styrene butadiene copolymer, and polyimide.
[0063] A gel-type polymer electrolyte containing a liquid electrolyte and a cross-linked polymer may be contained in the pores of a porous substrate constituting the separator. In a separator having such a structure, the liquid electrolyte may be contained in a cross-linked polymer network having a cross-linked structure, thereby preventing leakage to the outside.
[0064] Referring to FIG. 1, a separator (30) including a porous substrate (31) and a ceramic coating layer (32) disposed on one surface of the porous substrate (31) is laminated on a negative electrode current collector (21).
[0065] The ceramic coating layer (32) is positioned so as to be in direct contact with the negative electrode current collector (21) as shown in Fig. 1. Here, the negative electrode (20) contains the negative electrode current collector (21), the negative electrode active material layer is absent, and the ceramic coating layer (32) is positioned adjacent to the negative electrode current collector (21).
[0066] As shown in Fig. 1, a ceramic coating layer (32) is not formed on the other side of the porous substrate (31), and a positive electrode (10) is disposed on the other side of the porous substrate (31). The positive electrode (10) contains a positive electrode active material layer (12) and a positive electrode current collector (11).
[0067] The ceramic coating layer (32) includes large-diameter inorganic particles and small-diameter inorganic particles. By using large-diameter inorganic particles and small-diameter inorganic particles together, a ceramic coating layer with excellent film strength is formed, thereby effectively suppressing the growth of lithium dendrites formed between the negative electrode current collector and the separator.
[0068] The mixing weight ratio of large-diameter inorganic particles and small-diameter inorganic particles in the ceramic coating layer is 9:1 to 1:1, 8:1 to 1:1, 7:1 to 1:1, 6:1 to 1:1, 5:1 to 1:1, 4:1 to 1:1, 3:1 to 1:1, or 2:1 to 1:1. When the mixing weight ratio of large-diameter inorganic particles and small-diameter inorganic particles is within the above range, a lithium metal battery in which dendrite growth is effectively suppressed in the negative electrode can be manufactured.
[0069] The average particle size of the small-diameter inorganic particles is 50 nm to 500 nm, 60 nm to 450 nm, 70 nm to 400 nm, 80 nm to 380 nm, 90 nm to 350 nm, or 100 nm to 300 nm.
[0070] The average particle size of the large-diameter inorganic particles is 0.6 um to 10 um, 0.7 um to 10 um, 0.8 um to 10 um, 0.9 um to 10 um, 1 um to 10 um, 1 um to 9.5 um, 1 um to 9 um, 1 um to 8.5 um, 1 um to 8 um, 1.1 um to 8 um, 1.5 um to 7.5 um, or 2 um to 7 um. When the average particle size of the large-diameter inorganic particles and the small-diameter inorganic particles is within the above range, dendrite growth can be effectively suppressed on the cathode.
[0071] The small-diameter inorganic particles and the large-diameter inorganic particles can each use two or more types of particles having the above-described average particle size range.
[0072] According to one embodiment, the small-diameter inorganic particles may be a mixture of first small-diameter inorganic particles having an average particle diameter of 50 to 200 nm and second small-diameter inorganic particles having an average particle diameter of 250 to 400 nm. The average particle diameter of the first small-diameter inorganic particles may be, for example, 60 to 200 nm, 70 to 200 nm, 80 to 200 nm, or 100 to 200 nm.
[0073] The second small-diameter inorganic particles have a larger average particle size than the first small-diameter inorganic particles, for example, an average particle size of 280 to 400 nm, 290 to 350 nm, or 300 to 320 nm. The mixing weight ratio of the first small-diameter inorganic particles and the second small-diameter inorganic particles is 1:9 to 1:1, 1:7 to 1:1, 1:5 to 1:1, or 1:4 to 1:1. By using the first small-diameter inorganic particles and the second small-diameter inorganic particles having such a mixing weight ratio, the ceramic coating layer has a dense characteristic, thereby effectively suppressing dendrite growth on the negative electrode.
[0074] The first small-diameter inorganic particles and the second small-diameter inorganic particles may be inorganic particles having the same or different compositions. By using small-diameter inorganic particles with different average particle diameters and / or compositions together, a dense ceramic coating layer can be formed, which can effectively suppress lithium dendrite growth on the negative electrode.
[0075] According to another embodiment, the large-diameter inorganic particles may include first large-diameter alumina particles and second large-diameter alumina particles. The first large-diameter alumina particles and the second large-diameter alumina particles may have different compositions. The first large-diameter alumina particles and the second large-diameter alumina particles may have the same average particle diameter. For example, 1 to 5 um, 1 to 3 um, or 1 to 2 um. The mixing weight ratio of the first small-diameter inorganic particles and the second small-diameter inorganic particles is 1:9 to 1:1, 1:7 to 1:1, 1:5 to 1:1, or 1:4 to 1:1. By using the first small-diameter inorganic particles and the second small-diameter inorganic particles having such a mixing weight ratio, the ceramic coating layer has a dense characteristic, thereby effectively suppressing dendrite growth on the negative electrode.
[0076] The first and second large-diameter inorganic particles may have different average particle sizes. For example, the first large-diameter inorganic particles have an average particle size of 1 to 5 μm, and the second large-diameter inorganic particles have an average particle size of 5 to 10 μm.
[0077] The average particle size of the first large-diameter inorganic particles is, for example, 1 to 3 um, or 1 to 2 um, and the average particle size of the second large-diameter inorganic particles is, for example, 6 to 10 um, or 7 to 10 um.
[0078] The mixing weight ratio of the first small-diameter inorganic particles and the second small-diameter inorganic particles is 1:9 to 1:1, 1:7 to 1:1, 1:5 to 1:1, or 1:4 to 1:1. By using the first large-diameter inorganic particles and the second large-diameter inorganic particles having such a mixing weight ratio, dendrite growth on the cathode can be effectively suppressed.
[0079] The ceramic coating layer (32) further includes a binder.
[0080] Binders include, for example, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butylene rubber, acrylic polymers, fluoroelastomers, or combinations thereof.
[0081] The binder content in the ceramic coating layer is 3 to 20 parts by weight, 4 to 20 parts by weight, 5 to 20 parts by weight, or 5.5 to 10 parts by weight based on 100 parts by weight of the total weight of the large-diameter inorganic particles and the small-diameter inorganic particles. When the binder content is within the above range, the bonding strength of the ceramic coating layer to the porous substrate is excellent.
[0082] As shown in Fig. 1, there is no negative electrode active material layer between the negative electrode current collector (21) and the ceramic coating layer (32).
[0083] Although not shown in FIG. 1, a protective layer may be further included between the negative electrode current collector and the separator. When the negative electrode active material layer is disposed, the protective layer may be formed between the negative electrode active material layer and the separator.
[0084] The protective layer contains a polymer such as, for example, polyvinyl alcohol, polyimide, vinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride, carboxymethyl cellulose, styrene butylene rubber, or a polymer and an inorganic filler. The inorganic filler can be, for example, SiO2, Al2O3, Al(OH)3, AlO(OH), TiO2, BaTiO3, ZnO2, Mg(OH)2, AIN(Aluminum Nitride), SiC(Silicon Carbide), BoN(Boron Nitride), or a combination thereof. The thickness of the protective layer is, for example, 1 to 20 um, 1 to 15 um, or 1 to 10 um. In the present disclosure, the thickness represents an average thickness. Introducing an additional protective layer like this can minimize contact between lithium and the electrolyte, thereby reducing side reactions, and can suppress lithium dendrite growth by creating a uniform flow of lithium ions throughout the electrode.
[0085] A gel-type polymer electrolyte containing a liquid electrolyte and a cross-linked polymer can be contained in the pores of the porous substrate (31).
[0086] The above cross-linked polymer refers to a polymerization product of a cross-linked monomer obtained by a polymerization reaction (cross-linking reaction) of a composition for forming a gel-type polymer electrolyte, which comprises a cross-linking monomer, a lithium salt, an organic solvent, and an initiator. In the present disclosure, the polymerization product may contain both a cross-linked product and a cured product.
[0087] In one embodiment, the crosslinked polymer is a polymerization product of trimethylolpropane trimethacrylate (TMPTMA).
[0088] The pore diameter of the separator (30) is generally 0.01 to 10 μm, and the thickness can generally be 5 to 20 μm. As such a separator, for example, an olefin-based polymer such as polypropylene, polypropylene, or a sheet or non-woven fabric made of glass fiber or polyethylene, etc. can be used. When a solid polymer electrolyte is used as the electrolyte, the solid polymer electrolyte can also function as a separator.
[0089] Among the above separation membranes (30), specific examples of olefin-based polymers may include polyethylene, polypropylene, or a multilayer membrane of two or more layers thereof, and mixed multilayer membranes such as a polyethylene / polypropylene two-layer separation membrane, a polyethylene / polypropylene / polyethylene three-layer separation membrane, and a polypropylene / polyethylene / polypropylene three-layer separation membrane may be used.
[0090] The membrane may be a polymer membrane, including, for example, polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polyimide, polycarbonate, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenyleneoxide, cyclic olefin copolymer, polyphenylenesulfide, and polyethylenenaphthalene, or combinations thereof.
[0091] Crosslinking monomers include, for example, trimethylolpropane trimethacrylate (TMPTMA), diethylene glycol diacrylate (DEGDA), diethylene glycol dimethacrylate (DEGDMA), triethylene glycol diacrylate (TEGDA), triethylene glycol dimethacrylate (TEGDMA), tetraethylene glycol diacrylate (TTEGDA), glycidyl methacrylate, polyethylene glycol diacrylate (PEGDA), polyethylene glycol dimethacrylate (PEGDMA), polypropylene glycol diacrylate (PPGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), dianol diacrylate (DDA), dianol dimethacrylate (DDMA), ethoxylated trimethylolpropane triacrylate: ETPTA), acrylate-functionalized ethylene oxide, butanediol dimethacrylate, ethoxylated neopentyl glycol diacrylate (NPEOGDA), propoxylated neopentyl glycol diacrylate (NPPOGDA), trimethylol propane triacrylate (TMPTA), trimethylol propane trimethacrylate (TMPTMA), pentaerythritol triacrylate (PETA), ethoxylated propoxylated trimethylolpropane triacrylate (TMPEOTA) / (TMPPOTA), propoxylated glyceryl triacrylate, tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA), pentaerythritol tetraacrylate (PETTA), Dipentaerythritol pentaacrylate (DPEPA), ditrimethylol propane tetraacrylate (DTMPTTA);It may include at least one selected from the group consisting of diglycidyl ester, diallyl suberate, acrylamide and divinylbenzene.;
[0092] The crosslinking monomer is a material that is electrochemically stable at a voltage of about 4.3 V or higher, for example, in an operating environment of a positive electrode using a positive electrode active material having a nickel content of 90 mol% or higher. Examples of such crosslinking monomers include polyfunctional (3-substituted) methacrylates and trimethylol propane triacrylate.
[0093] The weight average molecular weight of the crosslinking monomer may be in the range of 200 to 2,000, 200 to 1,500, 200 to 1,000, 200 to 800, for example, 200 to 500. If the weight average molecular weight of the crosslinking monomer is less than 200, the density of crosslinking points within the molecular structure of the polymer after crosslinking may be too high, which may prevent free movement of the lithium salt, and if the weight average molecular weight of the crosslinking monomer is greater than 2,000, the density of crosslinking points within the molecular structure of the polymer after crosslinking may be too low, which may reduce the electrolyte blocking ability. In the present disclosure, the weight average molecular weight is determined using gel permeation chromatography.
[0094] Based on the total weight of the crosslinking monomer and the electrolyte, the content of the crosslinking monomer is 1 to 20 parts by weight, 1 to 15 parts by weight, 2 to 10 parts by weight, or 3 to 7 parts by weight, and the content of the electrolyte is 80 to 99 parts by weight, 85 to 99 parts by weight, 90 to 98 parts by weight, or 93 to 97 parts by weight. If the content of the crosslinking monomer is less than the above range, the degree of crosslinking of the gel polymer during crosslinking is too low, making it difficult to sufficiently express the crosslinking characteristics, and the electrolyte moisture absorption capacity and mechanical properties may deteriorate. In addition, if the content of the crosslinking monomer exceeds 20 parts by weight, the internal resistance of the battery increases, and the capacity during high-rate charge / discharge of the lithium metal battery may decrease.
[0095] The composition for forming the above gel-type polymer electrolyte may further include a crosslinking agent, an initiator, etc. to assist in crosslinking of the crosslinkable monomer. The crosslinking agent, initiator, etc. are not particularly limited as long as they are commonly used in the relevant technical field.
[0096] The initiator can be, for example, benzoin ethyl ether.
[0097] The content of the crosslinking agent or initiator may be within a conventional range. For example, the content of the initiator may be used in a range of 0.1 to 5 parts by weight, or 0.2 to 3 parts by weight, per 100 parts by weight of the crosslinking monomer.
[0098] By using a gel-type polymer electrolyte according to an embodiment, the ionic conductivity can be maintained at a value close to that of a liquid electrolyte, and the gel-type polymer electrolyte inside the positive and negative electrodes can play a role in preventing leakage of the liquid electrolyte. The electrolyte can be trapped in the polymer matrix of the gel-type polymer electrolyte and maintained within the polymer matrix, thereby helping the smooth movement of lithium ions. In addition, the excellent electrochemical properties of the polymer can effectively suppress the electrolyte decomposition reaction within the range of -1 V to 5 V.
[0099] In a lithium metal battery according to an embodiment, a liquid electrolyte is impregnated with a gel-type polymer electrolyte within a polymer matrix, so that there is no leakage, and electrochemical side reactions and electrolyte decomposition reactions occurring at the positive and negative electrodes are suppressed, thereby ensuring stability and improving battery characteristics.
[0100] The liquid electrolyte contains a lithium salt and an organic solvent.
[0101] Organic solvents are non-aqueous solvents, and for example, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxy franc, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxy methane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl pyropionate, and ethyl propionate. Can be used. Carbonate solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, and diethyl carbonate can be used.
[0102] The above lithium salt can be any one that is commonly used in lithium secondary batteries, and as a material that is easily dissolved in the non-aqueous solvent, for example, one or more of the following materials can be used: LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2)3, LiC(FSO2)3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, and LiB(C2O4)2.
[0103] The concentration of the lithium salt may be, for example, 1 to 5 M, for example, 1 to 2.5 M, in the organic electrolyte. In the above range, a sufficient amount of lithium ions required for charging and discharging a lithium secondary battery can be generated.
[0104] When a gel-type polymer electrolyte exists in the pores of a porous substrate, the interfacial resistance between the positive electrode, negative electrode, and separator is minimized, and lithium movement becomes easier.
[0105] As shown in Fig. 2, a negative electrode active material layer (22) can be placed between the negative electrode current collector (21) and the ceramic coating layer (32).
[0106] According to one embodiment, the negative electrode active material layer can be arranged during the assembly of the lithium metal battery. According to another embodiment, the negative electrode active material layer can include the negative electrode active material layer by plating lithium metal after charging. The negative electrode active material layer can be a plated lithium layer. A battery in which the negative electrode active material layer arranged between the negative electrode current collector and the separator is free before charging is a lithium battery.
[0107] The above negative electrode active material layer (22) includes lithium metal or a lithium alloy.
[0108] The thickness of the negative electrode active material layer (22) may be 1 to 500 μm, 5 μm to 500 μm, or 10 μm to 500 μm. When the thickness of the negative electrode active material layer is within the above range, the cycle characteristics of the lithium metal battery are improved without reducing the energy density.
[0109] When the negative electrode active material layer is placed at the time of assembly, it may include only a carbon-based material, a carbon-based material, and at least one selected from metals and metalloids.
[0110] The carbon-based material includes amorphous carbon, and the average particle diameter of the amorphous carbon is 10 nm to 100 nm, and the carbon-based material includes carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, or a combination thereof.
[0111] The above negative active material layer includes a lithium metal foil, a lithium metal powder, a lithium alloy foil, a lithium alloy powder, or a combination thereof, wherein the lithium alloy contains lithium and a first metal.
[0112] The first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.
[0113] The negative electrode active material layer (22) may include, for example, lithium foil, lithium powder, or a combination thereof. The lithium foil may include, for example, lithium metal foil, lithium alloy foil, or a combination thereof. The lithium powder may include lithium metal powder, lithium alloy powder, or a combination thereof. A lithium alloy is an alloy of lithium and another metal that can be alloyed with lithium, such as a lithium-silver alloy, a lithium-zinc alloy, a lithium-magnesium alloy, or a lithium-tin alloy. The negative electrode active material layer including a lithium metal foil may be, for example, a lithium metal layer. The negative electrode active material layer including a lithium alloy foil may be, for example, a lithium alloy layer. The negative electrode active material layer including a lithium metal powder and / or a lithium alloy powder may be introduced by coating a slurry including lithium powder and a binder, etc., on a negative electrode current collector. The binder may be, for example, a fluorine-based binder such as polyvinylidene fluoride (PVDF). The negative electrode active material layer may not include a carbon-based negative electrode active material. Therefore, the negative electrode active material layer can be made of a metal-based negative electrode active material.
[0114] The negative electrode current collector is composed of a material that does not react with lithium, i.e., does not form an alloy or compound. The material constituting the negative electrode current collector includes, but is not limited to, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), and any material that is used as an electrode current collector in the relevant technical field may be used. The negative electrode current collector may be composed of one of the above-mentioned metals, or may be composed of an alloy or a coating material of two or more metals. The negative electrode current collector is, for example, in the form of a plate or foil.
[0115] The negative electrode active material layer may contain a negative electrode active material and a binder.
[0116] The negative active material has, for example, a particle form. The average particle diameter of the negative active material having a particle form is, for example, 10 nm to 4 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the negative active material has an average particle diameter in this range, reversible plating and / or dissolution of lithium can be facilitated during charge and discharge. The average particle diameter of the negative active material is, for example, a median diameter (D50) measured using a laser particle size distribution analyzer.
[0117] The negative electrode active material may include, for example, at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material. The carbon-based negative electrode active material may be, for example, amorphous carbon. Examples of the carbon-based negative electrode active material include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., and any material classified as amorphous carbon in the relevant technical field may be used. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon. The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium, and therefore is not a metal negative electrode active material in the present specification. The negative electrode active material layer includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the negative electrode active material layer may include a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture may be, for example, 10:1 to 1:2, 10:1 to 1:1, 7:1 to 1:1, 5:1 to 1:1, or 4:1 to 2:1 by weight.The negative electrode active material included in the negative electrode active material layer may include a mixture of first particles made of, for example, amorphous carbon and second particles made of a metal or a metalloid. The metal includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture. When the second particles have a content in this range, the cycle characteristics of, for example, a lithium metal battery are further improved.
[0118] The binder included in the negative electrode active material layer may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders. When the negative electrode active material layer does not include a binder, the negative electrode active material layer can be easily separated from the ceramic coating layer (21) or the negative electrode current collector (21). The content of the binder included in the negative electrode active material layer may be, for example, 1 to 20 wt% based on the total weight of the negative electrode active material layer.
[0119] The thickness of the negative electrode active material layer is, for example, 1 ㎛ to 500 ㎛, and the thickness of the negative electrode active material layer may be, for example, 1% to 50%, 1% to 30%, 1% to 10%, or 1% to 5% of the thickness of the positive electrode active material layer. If the thickness of the negative electrode active material layer is too thin, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium metal battery. If the thickness of the negative electrode active material layer increases excessively, the energy density of the lithium metal battery employing the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics.
[0120] When the thickness of the negative electrode active material layer decreases, the charge capacity of the negative electrode active material layer also decreases, for example. The charge capacity of the negative electrode active material layer may be, for example, 0.1% to 50%, 1% to 30%, 1% to 10%, 1% to 5%, or 1% to 2% of the charge capacity. If the charge capacity of the negative electrode active material layer is too small, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium metal battery. If the charge capacity of the negative electrode active material layer increases excessively, the energy density of the lithium metal battery using the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics. The charge capacity of the positive electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer. When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values is the charge capacity of the positive electrode active material layer. The charge capacity of the negative electrode active material layer is also calculated in the same way. That is, the charge capacity of the negative electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode active material layer. When multiple types of negative electrode active materials are used, the charge capacity density × mass value is calculated for each negative electrode active material, and the sum of these values is the capacity of the negative electrode active material layer. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is the estimated capacity using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer and the negative electrode active material layer are directly measured by measuring the charge capacity using an all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer and the negative electrode active material layer may be the initial charge capacity measured at the first charge cycle.
[0121] [Lithium metal battery]
[0122] According to one embodiment, a lithium metal battery includes a positive electrode; a negative electrode; and a separator disposed between the positive electrode and the negative electrode. Such a lithium metal battery can simultaneously provide excellent life characteristics. The lithium metal battery may be, but is not limited to, a lithium primary battery, a lithium secondary battery, a lithium-sulfur battery, a lithium-air battery, etc., and any lithium metal battery used in the relevant technical field may be used.
[0123] Lithium metal batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.
[0124] (anode)
[0125] First, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon.
[0126] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c Dc (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G dO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤
[0127] 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used.
[0128] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0129] The cathode active material is, for example, Li a Ni x Co y M z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0 <y≤0.3, 0<z≤0.3, 및 x+y+z=1이고, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Mn z Al w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1), Li a Co x M y O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof), Li a Ni x Mn y M' z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), Li a M1 x M2 y PO 4-b X b (Here, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며, M1이 크롬(Cr), 망간(Mn), 철(Fe), 코발트(Co), 니켈(Ni), 구리(Cu), 지르코늄(Zr) 또는 이들의 조합이며, M2가 마그네슘(Mg), 칼슘(Ca), 스트론튬(Sr), 바륨(Ba), 티탄(Ti), 아연(Zn), 보론(B), 니오븀(Nb), 갈륨(Ga), 인듐(In), 몰리브덴(Mo), 텅스텐(W), 알루미늄(Al), 실리콘(Si), 크롬(Cr), 바나듐(V), 스칸듐(Sc), 이트륨(Y) 또는 이들의 조합이며, X가 O, F, S, P 또는 이들의 조합), Li a M3 z PO4 (0.90≤a≤1.1, 0.9≤z≤1.1, and M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof).
[0130] The conductive material may include, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used. Alternatively, the anode may not include a separate conductive material, for example.
[0131] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.
[0132] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.
[0133] The contents of the cathode active material, conductive agent, binder, and solvent used in the cathode are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium metal battery, one or more of the conductive agent, binder, and solvent may be omitted.
[0134] The binder content included in the positive electrode may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.
[0135] In one embodiment of the present invention, the positive electrode collector (11) may include, for example, a base film and a metal layer disposed on one or both sides of the base film.
[0136] The positive electrode collector uses a plate or foil made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The thickness of the positive electrode collector is, for example, 1 ㎛ to 100 ㎛, 1 ㎛ to 50 ㎛, 5 ㎛ to 25 ㎛, or 10 ㎛ to 20 ㎛.
[0137] The cathode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The base film may be, for example, an insulator. Since the base film includes an insulating thermoplastic polymer, when a short circuit occurs, the base film may soften or liquefy, thereby blocking battery operation and suppressing a sudden increase in current. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The metal layer can act as an electrochemical fuse and cut off in case of overcurrent to prevent short circuits. The limit current and maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer can be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or maximum current of the positive electrode current collector decreases, thereby improving the stability of the lithium battery in case of a short circuit. A lead tab can be added to the metal layer for external connection. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal layer melt, so that the metal layer can be electrically connected to the lead tab. To strengthen the welding between the metal layer and the lead tab, a metal chip can be added between the metal layer and the lead tab.The metal piece may be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the welding process of the lead tab. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to μm. Since the metal layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the electrode assembly. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure as the cathode current collector, the weight of the cathode can be reduced, and as a result, the energy density of the cathode and lithium metal battery can be improved.
[0138] (Separator)
[0139] Next, a separator to be inserted between the anode and cathode is prepared.
[0140] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion transport and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in nonwoven or woven form. For lithium-ion batteries, rollable separators, such as polyethylene or polypropylene, are used, while for lithium-ion polymer batteries, separators with excellent organic electrolyte absorption capacity are used.
[0141] The membrane is manufactured by the following exemplary method, but is not limited to this method and may be adjusted according to required conditions.
[0142] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast onto a support and dried, and then a separator film peeled from the support is laminated onto the electrode to form a separator.
[0143] The polymer used in membrane manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.
[0144] (cathode)
[0145] The cathode contains a cathode current collector.
[0146] In one embodiment of the present invention, although not shown in the drawings, the negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The polymer may be an insulating polymer. Since the base film includes an insulating thermoplastic polymer, when a short circuit occurs, the base film softens or liquefies, thereby blocking battery operation and suppressing a sudden increase in current. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may correspond to, for example, the first metal substrate. The metal layer may additionally include a coating layer including a second metal. The negative electrode current collector (21) may additionally include a metal piece and / or a lead tab. For more specific details on the base film, metal layer, metal piece (metal chip), and lead tab of the negative electrode current collector (21), refer to the positive electrode current collector. Since the negative electrode current collector (21) has this structure, the weight of the negative electrode can be reduced, and as a result, the energy density of the negative electrode and the lithium battery can be improved. A negative electrode active material layer can be formed on the negative electrode current collector. The negative electrode active material layer can be formed as a lithium deposition layer after charging. Alternatively, the negative electrode active material layer can be formed using a negative electrode active material during battery assembly.
[0147] The method of forming a negative electrode active material layer using a negative electrode active material can be manufactured in the same manner as described above, except that the negative electrode active material is used instead of the positive electrode active material when forming the positive electrode active material layer.
[0148] A lithium metal battery may further include, for example, a thin film comprising an element capable of forming an alloy with lithium on one surface of an anode current collector. The thin film is disposed between the anode current collector and the anode active material layer. The thin film includes, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium includes, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of one of these metals or an alloy of several types of metals. By disposing the thin film on one surface of the anode current collector, for example, the deposition shape of the first anode active material layer deposited between the thin film and the anode active material layer becomes flatter, and the cycle characteristics of the lithium metal battery may be further improved.
[0149] (Separator)
[0150] A separation membrane according to the embodiment is used.
[0151] Organic electrolytes are manufactured, for example, by dissolving lithium salts in organic solvents.
[0152] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0153] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.
[0154] A lithium metal battery according to one embodiment may further include a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof. The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.
[0155] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12(M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 A garnet-type solid electrolyte selected from (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10).
[0156] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1??x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x( "LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5(An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n (0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.
[0157] The polymer solid electrolyte may, for example, comprise a mixture of a lithium salt and a polymer, or a polymer having ion-conducting functional groups. The polymer solid electrolyte may, for example, be a polymer electrolyte that is solid at 25°C and 1 atm. The polymer solid electrolyte may, for example, not comprise a liquid.The polymer solid electrolyte comprises a polymer, and the polymer is, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), Polyacrylonitrile (PAN), polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-Diphenylanthracene-2-sulfonate (lithium 9,10-diphenylanthracene-2-sulfonate, DPASLi. +) or a combination thereof, but is not limited thereto, and any lithium salt that can be used in polymer electrolytes in the relevant technical field is possible. The lithium salt can be any lithium salt that can be used in the relevant technical field. The lithium salt is, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (x and y are each 1 to 20), LiCl, LiI or a mixture thereof, etc. The polymer included in the polymer solid electrolyte may be, for example, a compound including 10 or more, 20 or more, 50 or more or 100 or more repeating units. The weight average molecular weight of the polymer included in the polymer solid electrolyte may be, for example, 1000 Dalton or more, 10,000 Dalton or more, 100,000 Dalton or more or 1,000,000 Dalton or more.
[0158] A gel electrolyte is, for example, a polymer gel electrolyte. A gel electrolyte can have a gel state without containing a polymer, for example.
[0159] A polymer gel electrolyte may include, for example, a liquid electrolyte and a polymer, or an organic solvent and a polymer having an ion-conducting functional group. The polymer gel electrolyte may be, for example, a polymer electrolyte that is in a gel state at 25°C and 1 atm. The polymer gel electrolyte may, for example, have a gel state without containing a liquid. The liquid electrolyte used in the polymer gel electrolyte may be, for example, an ionic liquid, a mixture of a lithium salt and an organic solvent; a mixture of a lithium salt and an organic solvent; a mixture of an ionic liquid and an organic solvent; or a mixture of a lithium salt, an ionic liquid, and an organic solvent. The polymer used in the polymer gel electrolyte may be selected from among the polymers used in solid polymer electrolytes. The organic solvent may be selected from among the organic solvents used in liquid electrolytes. The lithium salt may be selected from among the lithium salts used in solid polymer electrolytes. An ionic liquid refers to a salt that has a melting point below room temperature, is composed solely of ions, and is liquid at room temperature or a molten salt at room temperature. The ionic liquid may include, for example, one or more cations selected from among a) ammonium compounds, pyrrolidinium compounds, pyridinium compounds, pyrimidinium compounds, imidazolium compounds, piperidinium compounds, pyrazolium compounds, oxazolium compounds, pyridazinium compounds, phosphonium compounds, sulfonium compounds, triazolium compounds, and mixtures thereof, and b) one or more anions selected from among BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-. A polymer solid electrolyte can form a polymer gel electrolyte, for example, by being impregnated into a liquid electrolyte in a secondary battery. The polymer gel electrolyte may further include inorganic particles. The polymer included in the polymer gel electrolyte may be, for example, a compound containing 10 or more, 20 or more, 50 or more, or 100 or more repeating units.The weight average molecular weight of the polymer included in the polymer gel electrolyte may be, for example, 500 Dalton or more, 1000 Dalton or more, 10,000 Dalton or more, 100,000 Dalton or more, or 1,000,000 Dalton or more.
[0160] (lithium metal battery)
[0161] Referring to FIG. 3, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2) according to one embodiment, and a separator (4).
[0162] The negative electrode (2) may contain only a negative electrode current collector or may include a negative electrode current collector and a negative electrode active material layer. In addition, the separator (4) includes a separator according to one embodiment, and the separator includes a porous substrate and a ceramic coating layer disposed on one surface of the porous substrate, wherein the ceramic coating layer is positioned to face the negative electrode current collector, and the pores of the porous substrate include a gel-type polymer electrolyte.
[0163] A positive electrode (3), a negative electrode (2), and a separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing a lithium metal battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0164] Referring to FIG. 3, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium metal battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.
[0165] Referring to FIG. 4, a lithium metal battery (1) according to one embodiment includes a positive electrode (3), a negative electrode (2) according to one embodiment, and a separator (4).
[0166] The negative electrode (2) may contain only a negative electrode current collector or may include a negative electrode current collector and a negative electrode active material layer. In addition, the separator (4) includes a separator according to one embodiment, and the separator includes a porous substrate and a ceramic coating layer disposed on one surface of the porous substrate, wherein the ceramic coating layer is positioned to face the negative electrode current collector, and the pores of the porous substrate include a gel-type polymer electrolyte.
[0167] A separator (4) is placed between the positive electrode (3) and the negative electrode (2) to form a battery structure. The battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium metal battery (1). The battery case (5) is square, but is not necessarily limited to this shape, and may have, for example, a cylindrical shape, a thin film shape, etc.
[0168] A pouch-type lithium metal battery corresponds to the lithium metal batteries of FIGS. 4 and 5, each of which uses a pouch as a battery case. The pouch-type lithium metal battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium metal battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium metal battery.
[0169] The lithium metal battery of the present disclosure has excellent discharge capacity and cycle life characteristics, as well as high energy density, and is therefore used in, for example, electric vehicles (EVs). For example, it is used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). It is also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.
[0170] Lithium metal batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0171] [Method for manufacturing lithium metal batteries]
[0172] According to one embodiment, a lithium metal battery can be manufactured by including the steps of: preparing a negative electrode current collector; forming a ceramic coating layer on one surface of a porous substrate to form a separator; preparing a positive electrode; arranging a separator on the negative electrode current collector such that the ceramic coating layer faces the negative electrode current collector; arranging the negative electrode current collector, the separator, and the positive electrode to form a battery structure; housing the battery structure in a battery case, and then injecting a composition for forming a gel-type polymer electrolyte into the battery structure; and curing the composition for forming a gel-type polymer electrolyte to form a gel-type polymer electrolyte.
[0173] The above ceramic coating layer can be formed using a composition for forming a ceramic coating layer. The composition for forming a ceramic coating layer can be obtained by mixing small-diameter inorganic particles, large-diameter inorganic particles, and a solvent to obtain an inorganic dispersion, and adding a binder thereto.
[0174] In the composition for forming a ceramic coating layer, the content of solids is 20 to 30 parts by weight, and the content of the remainder is 70 to 80 parts by weight.
[0175] The organic solvent is volatilized through drying after coating the coating composition, and is no longer present in the coating layer of the final separator. Examples of organic solvents that can be used include, but are not limited to, N-methylpyrrolidone, acetone, or water, and any solvent that can be used in the relevant technical field may be used. For example, acetone may be used as the organic solvent.
[0176] The step of injecting the composition for forming a gel-type polymer electrolyte into the battery structure may be performed as an impregnation step under vacuum so that the composition can sufficiently penetrate into the pores of the porous substrate.
[0177] Methods for forming a gel-type polymer electrolyte include curing using heat, UV, or high-energy radiation (electron beam, γ-ray). The curing reaction using heat can be carried out at a temperature of 40°C to 120°C, for example, 50°C to 90°C, for 30 to 120 minutes.
[0178] The above heat treatment varies depending on the type of crosslinking monomer, but is performed at, for example, 40 to 120°C. When the heat treatment is performed within the above range, a separator containing a gel-type polymer electrolyte in the pores of a porous substrate is used, thereby suppressing dendrite formation and increasing electrolyte wettability, thereby providing a lithium metal battery with improved life characteristics.
[0179]
[0180] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0181] Example 1
[0182] Alumina having an average particle size of approximately 200 nm as small-diameter inorganic particles and alumina having an average particle size of approximately 1 μm as large-diameter inorganic particles were mixed in a weight ratio of 2:8 (1:4), and water was added to the mixture to obtain an aqueous dispersion of inorganic particles. The total content of alumina having an average particle size of approximately 200 nm and alumina having an average particle size of approximately 1 μm in the inorganic particle dispersion is 30 parts by weight.
[0183] A composition for forming a ceramic coating layer was formed by adding carboxymethylcellulose (CMC), a binder, to an aqueous dispersion of inorganic particles. Here, the content of CMC was 5 parts by weight and the total weight of the inorganic particles was 95 parts by weight.
[0184] The ceramic coating layer composition manufactured above is used as a porous substrate with a thickness of 5.5㎛.
[0185] A separator having a ceramic coating layer (coating thickness: 2 μm) was manufactured by coating a cross-section of a polyethylene single-layer substrate film using a gravure coating method and then drying it for 10 seconds under conditions of a drying temperature of 70°C and a wind speed of 15 m / sec. The total thickness of the separator having a ceramic coating layer is 7.5 μm.
[0186] A copper foil having a thickness of 10 μm, which is a negative current collector, was laminated on the ceramic coating layer of the separator, a positive electrode was laminated on the other side of the separator, and this was placed in a battery case. Then, a composition for forming a gel polymer electrolyte was injected therein and heat-treated at 70°C for 120 minutes to manufacture a lithium metal battery in which a gel polymer electrolyte was formed in the pores of the separator.
[0187] The composition for forming the above gel-type polymer electrolyte was prepared by mixing trimethylolpropane trimethacrylate (TMPTMA) as a crosslinking monomer, a mixed solvent (weight ratio 1:1:0.5) of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in which 1.3 M LiPF6 was dissolved as an electrolyte, and benzoin ethyl ether (Sigma-Aldrich, 240.30 g / mol) as an initiator. The composition for forming the above gel-type polymer electrolyte contained 5 parts by weight of the crosslinking monomer and 95 parts by weight of the electrolyte based on 100 parts by weight of the total weight of the composition, and the initiator was used in an amount of 5 parts by weight based on 100 parts by weight of the crosslinking monomer.
[0188] The above anode was manufactured according to the following method.
[0189] Li 1.04 Ni 0.8 Co 0.1 Al 0.1O2 powder and carbon conductive material (Super-P; Timcal Ltd.) were uniformly mixed at a weight ratio of 90:5, and then a PVDF (polyvinylidene fluoride) binder solution was added to prepare a slurry for forming a positive electrode active material layer so that the weight ratio of active material:carbon conductive material:binder = 90:5:5.
[0190] The manufactured slurry for forming a positive electrode active material layer was coated on an aluminum substrate having a thickness of 15 ㎛ using a doctor blade, and the coated slurry was dried under reduced pressure at 120°C, then rolled using a roll press to form a sheet to manufacture a positive electrode.
[0191] The above lithium metal battery includes a negative electrode current collector / separator (ceramic coating layer / porous substrate) / positive electrode, and the pores of the separator contain a gel-type polymer electrolyte.
[0192] Example 2
[0193] A lithium metal battery was manufactured in the same manner as in Example 1, except that the mixing weight ratio of alumina having an average particle diameter of about 200 nm and large-diameter inorganic particles having an average particle diameter of about 1 um was changed from a 1:4 weight ratio to 1:1 when forming a ceramic coating layer.
[0194] Example 3
[0195] A lithium metal battery was manufactured in the same manner as in Example 1, except that the mixing weight ratio of alumina having an average particle diameter of about 200 nm and large-diameter inorganic particles having an average particle diameter of about 1 um was changed from a weight ratio of 1:4 to 1:8 when forming a ceramic coating layer.
[0196] Example 4
[0197] A lithium metal battery was manufactured in the same manner as in Example 1, except that when forming a ceramic coating layer, alumina having an average particle size of about 200 nm and silica having an average particle size of about 300 nm at a weight ratio of 1:1 were used as small-diameter inorganic particles, and alumina having an average particle size of about 1 um and silica having an average particle size of about 1 um at a weight ratio of 1:1 were used as large-diameter inorganic particles. In Example 4, the mixing weight ratio of the small-diameter inorganic particles and the large-diameter inorganic particles was 2:8.
[0198] Example 5
[0199] A lithium metal battery was manufactured in the same manner as in Example 4, except that the mixing weight ratio of small-diameter inorganic particles and large-diameter inorganic particles was changed from 2:8 to 1:1.
[0200] Example 6
[0201] A lithium metal battery was manufactured in the same manner as in Example 1, except that ethoxylated trimethylolpropane triacrylate (ETPTA) was used instead of trimethylolpropane trimethacrylate as a crosslinking monomer when manufacturing a composition for forming a gel-type polymer electrolyte.
[0202] Comparative Example 1
[0203] A cross-section of a 5.5㎛ thick polyethylene single-layer substrate film used as a porous substrate
[0204] A copper foil with a thickness of 10 μm, which is a negative current collector, was laminated, a positive electrode was laminated on the other side of a separator, and this was placed in a battery case. Then, the composition for forming a gel-type polymer electrolyte of Example 1 was injected into this and heat-treated at 70°C for 120 minutes to manufacture a lithium metal battery.
[0205] The positive electrode was the same as that used in Example 1.
[0206] The above lithium metal battery includes a negative electrode current collector / separator (ceramic coating layer / porous substrate) / positive electrode, and an electrolyte is contained in the pores of the separator.
[0207] Comparative Example 2
[0208] A lithium metal battery was manufactured in the same manner as in Example 1, except that the ceramic coating layer of the separator was placed on the positive electrode and a copper foil as a negative electrode collector was laminated on the other side of the separator.
[0209] Comparative Example 3
[0210] A lithium metal battery was manufactured in the same manner as in Example 1, except that a ceramic coating layer was formed on both sides of the porous substrate of the separator.
[0211] Evaluation Example 1: Lifespan at room temperature (25℃)
[0212] The charge / discharge characteristics of the lithium metal batteries of Examples 1 to 5 and Comparative Examples 1 to 3 were evaluated under the following conditions.
[0213] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.6 V (vs. Li) (formation cycle).
[0214] The lithium metal battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 3.6 V (vs. Li) (1 st cycle). These cycles are 200 th The cycle was repeated under the same conditions.
[0215] In all charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 1 below. The capacity retention rate is defined by Equation 1 below.
[0216] <Formula 1>
[0217] Capacity retention rate [%] = [200 th Discharge capacity in cycles / 1 st Discharge capacity in cycle] × 100
[0218] Capacity retention rate [%] Example 173 Example 268 Example 370 Example 467 Example 565 Comparative Example 158 Comparative Example 256 Comparative Example 360
[0219] As shown in Table 1, the capacity retention rate of the lithium metal battery of Comparative Example 1 was lowered due to lithium and electrolyte side reactions resulting from dendrite growth, and the capacity retention rate of the lithium metal battery of Comparative Example 2 was deteriorated due to positive electrode interfacial side reactions and negative electrode dendrite formation. In addition, the capacity retention rate of the lithium battery of Comparative Example 3 was reduced due to the continuous occurrence of side reactions caused by overvoltage.
[0220] In contrast, the lithium metal batteries of Examples 1 to 5 had improved capacity retention rates, unlike the lithium metal batteries of Comparative Examples 1 to 3. This improved capacity retention rate is because the ceramic coating layer was positioned facing the negative electrode current collector, thereby physically suppressing dendrite growth, thereby improving long-term life characteristics.
[0221] In contrast, according to Comparative Example 2, when a ceramic coating layer was formed on both sides of the porous substrate and the ceramic coating layer came into contact with the anode, it had a rather unfavorable effect on the crosslinking of the gel-type polymer electrolyte. This is because a side reaction due to moisture exists at the anode interface due to the hygroscopicity of the inorganic particles of the ceramic coating layer, which deteriorates the long-term life characteristics. In addition, when the ceramic coating layer according to Comparative Example 3 was applied to both sides of the separator, the overvoltage increased due to an increase in the overall resistance of the cell, the long-term life deteriorated, and the volumetric energy density decreased.
[0222] Evaluation Example 2: High Temperature (45℃) Lifespan
[0223] The charge / discharge characteristics of the lithium metal batteries of Examples 1 to 6 and Comparative Examples 1 to 3 were evaluated under the following conditions.
[0224] The battery was charged at a constant current of 0.1 C rate at 45°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.6 V (vs. Li) during discharge (formation cycle).
[0225] The lithium metal battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 45°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 3.6 V (vs. Li) (1 st cycle). These cycles are 160 th The cycle was repeated under the same conditions.
[0226] In all charge / discharge cycles, a 10-minute pause was observed after each charge / discharge cycle. Some of the results of the high-temperature charge / discharge experiments are shown in Table 2.
[0227] Capacity retention rate [%] Example 182 Example 275 Example 376 Example 475 Example 573 Comparative Example 170 Comparative Example 268 Comparative Example 371
[0228] As shown in Table 2, it was confirmed that the lithium metal batteries of Examples 1 to 5 had improved high-temperature lifespan compared to the lithium metal batteries of Comparative Examples 1 to 3.
[0229] In addition, the lithium metal battery of Example 6, although not shown in Table 2, exhibited high-temperature life characteristics equivalent to those of the lithium metal battery of Example 1.
[0230] Evaluation Example 3: Initial Capacity
[0231] Charging and discharging were performed on the lithium metal batteries of Examples 1 to 5 and Comparative Example 3 under the following conditions.
[0232] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) (formation cycle).
[0233] The lithium metal battery that had undergone the Mars cycle was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle).
[0234] The initial capacities were investigated and are shown in Table 3 below.
[0235] Classification Initial capacity (mAh / g) Example 1 196.9 Example 2 195.8 Example 3 196.0 Example 4 195.5 Example 5 195.1 Comparative example 3 189.2
[0236] As shown in Table 3, the lithium metal batteries of Examples 1 to 5 had improved initial capacities due to reduced interfacial resistance compared to Comparative Example 3. Among them, the lithium metal batteries of Examples 1 and 2, which used alumina in forming the ceramic coating layer, had relatively reduced resistance and better initial capacities compared to the lithium metal batteries of Examples 4 and 5, which used silica as an inorganic particle in forming the ceramic coating layer.
[0237] In the lithium metal battery of Comparative Example 3, a ceramic coating layer was applied to both sides of the porous substrate, and as shown in Table 3, the resistance was the highest and the initial capacity was the smallest.
[0238] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.
Claims
1. Containing a negative electrode current collector; a positive electrode; and a separator disposed between the negative electrode current collector and the positive electrode, It includes a negative electrode active material layer disposed between the negative electrode current collector and the separator, or the negative electrode active material layer is absent (free). The above separator comprises a porous substrate; and a ceramic coating layer disposed on one surface of the porous substrate; The above ceramic coating layer is positioned so as to face the negative electrode collector, A lithium metal battery comprising a gel-type polymer electrolyte in the pores of the above porous substrate.
2. In paragraph 1, A lithium metal battery, wherein the ceramic coating layer comprises large-diameter inorganic particles and small-diameter inorganic particles.
3. In paragraph 1, A lithium metal battery having a mixing weight ratio of large-diameter inorganic particles and small-diameter inorganic particles in the above ceramic coating layer of 9:1 to 1:
1.
4. In paragraph 2, The above large-diameter and small-diameter inorganic particles are SiO2, Al2O3, Al(OH)3, AlO(OH), TiO2, BaTiO3, ZrO2, ZnO2, Mg(OH)2, AIN(Aluminum Nitride), SiC(Silicon Carbide), BoN(Boron Nitride), BaTiO3, BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb, respectively. 1-a La a Zr 1-b Ti b O3 (PLZT, where, 0 <a<1, 0<b<1임), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC, lithium phosphate (Li3PO4), lithium titanium phosphate (Li c Ti d (PO4)3, 0 <d<2, 0<d<3), 리튬알루미늄티타늄포스페이트 (Li a1 Al b1 Ti c1 (PO4)3, 0 <a1<2, 0<b1<1, 0<c1<3), 14Li2O-9Al2O3-38TiO2-39P2O5, (LiAlTiP) a2 O b2 Series Glass (0) <a2<4, 0<b2<13), 리튬란탄티타네이트 (Li a3 La b3 TiO3, 0 <a3<2, 0<b3<3), Li 3.25 Ge 0.25 P 0.75 S4, Li a4 Ge b4 P c2 S d , 0 <a4<4, 0<b4<1, 0<c2<1, 0<d<5), Li3N , 리튬나이트라이드 (Li a5 N b5 , 0 <a5<4, 0<b5<2), Li3PO4-Li2S-SiS2, Li a6 You b6 With c3 , 0 <a6<3, 0<b6<2, 0<c3<4, LiI-Li2S-P2S5, Li a7 P b7 With c4 , 0 <a7<3, 0<b7<3, 0<c4<7 또는 그 조합인 리튬금속전지.
5. In paragraph 2, The average particle diameter of the above small-diameter inorganic particles is 50 nm to 500 nm, A lithium metal battery wherein the average particle diameter of the above large-diameter inorganic particles is 0.6 um to 10 um.
6. In paragraph 1, The above gel-type polymer electrolyte is a lithium metal battery including a liquid electrolyte containing an organic solvent and a lithium salt and a crosslinked polymer.
7. In paragraph 6, The above cross-linked polymer is a polymerization product of a cross-linkable monomer, The above crosslinking monomers are trimethylolpropane trimethacrylate (TMPTMA), diethylene glycol diacrylate (DEGDA), diethylene glycol dimethacrylate (DEGDMA), triethylene glycol diacrylate (TEGDA), triethylene glycol dimethacrylate (TEGDMA), tetraethylene glycol diacrylate (TTEGDA), glycidyl methacrylate, polyethylene glycol diacrylate (PEGDA), polyethylene glycol dimethacrylate (PEGDMA), polypropylene glycol diacrylate (PPGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), dianol diacrylate (DDA), dianol dimethacrylate (DDMA), ethoxylated trimethylolpropane triacrylate ( ETPTA), acrylate-functionalized ethylene oxide, butanediol dimethacrylate, ethoxylated neopentyl glycol diacrylate (NPEOGDA), propoxylated neopentyl glycol diacrylate (NPPOGDA), trimethylol propane triacrylate (TMPTA), trimethylol propane trimethacrylate (TMPTMA), pentaerythritol triacrylate (PETA), ethoxylated propoxylated trimethylolpropane triacrylate (TMPEOTA) / (TMPPOTA), propoxylated glyceryl triacrylate, tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA), pentaerythritol tetraacrylate (PETTA), Dipentaerythritol pentaacrylate (DPEPA), ditrimethylol propane tetraacrylate (DTMPTTA);Diglycidyl ester, diallyl suberate; acrylamide, divinylbenzene or a combination thereof, lithium metal battery.; 8. In paragraph 6, A lithium metal battery, wherein the content of the crosslinked polymer in the gel-type polymer electrolyte is 1 to 20 parts by weight based on 100 parts by weight of the gel-type polymer electrolyte.
9. In the first paragraph, the thickness of the ceramic coating layer is 10 nm to 5,000 nm, The above ceramic coating layer further includes a binder, A lithium metal battery comprising the binder selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butylene rubber, acrylic polymer, fluororubber, or a combination thereof.
10. In paragraph 1, Further comprising a negative electrode active material layer between the negative electrode current collector and the ceramic coating layer, A lithium metal battery, wherein the thickness of the negative electrode active material layer is 1 ㎛ to 500 ㎛.
11. In paragraph 10, The above negative active material layer includes lithium metal foil, lithium metal powder, lithium alloy foil, lithium alloy powder, or a combination thereof, The above lithium alloy contains lithium and a first metal, A lithium metal battery wherein the first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.
12. In Article 10 The above negative electrode active material layer includes a negative electrode active material, A lithium metal battery, wherein the negative active material comprises a carbon-based compound; a mixture of a carbon-based compound and at least one selected from among metals and metalloids; a composite of a carbon-based compound and at least one selected from among metals and metalloids; or a combination thereof.
13. In paragraph 12, The above carbon compound contains amorphous carbon, A lithium metal battery comprising the carbon-based compound selected from the group consisting of carbon black, carbon nanotubes, carbon nanofibers, fullerenes, activated carbon, carbon fibers, or a combination thereof.
14. In paragraph 1, The above porous substrate is a lithium metal battery comprising polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polyimide, polycarbonate, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene oxide, cyclic olefin copolymer, polyphenylene sulfide, polyethylenenaphthalene, or a combination thereof.
15. In the first paragraph, the lithium metal battery further includes an electrolyte, A lithium metal battery, wherein the electrolyte comprises a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof.
16. In the 15th paragraph, the solid electrolyte includes an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof, A lithium metal battery, wherein the polymer solid electrolyte comprises a polymer gel electrolyte.
17. In paragraph 1, The above positive electrode includes a positive electrode current collector and a positive electrode active material layer, At least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A lithium metal battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
18. Step of preparing the negative electrode collector; A step of forming a separator by forming a ceramic coating layer on one side of a porous substrate; Steps to prepare the anode; A step of placing a separator on a negative electrode collector, such that the ceramic coating layer faces the negative electrode collector; A step of forming a battery structure by arranging a negative electrode collector, a separator, and a positive electrode; A step of housing the above battery structure in a battery case, and then injecting a composition for forming a gel-type polymer electrolyte into the battery structure; and A method for manufacturing a lithium metal battery, comprising the step of forming a gel-type polymer electrolyte by curing the composition for forming the gel-type polymer electrolyte; 19. In paragraph 18, The step of forming a gel-type polymer electrolyte by curing the composition for forming the gel-type polymer electrolyte is performed by heat-treating the battery structure, A method for manufacturing a lithium metal battery, wherein the above heat treatment is performed at 40°C to 120°C.
20. In paragraph 18, A method for manufacturing a lithium metal battery, wherein the composition for forming the gel-type polymer electrolyte comprises a crosslinking monomer, a lithium salt, an organic solvent, and an initiator.
Citation Information
Patent Citations
Gel-formable electrolyte composition and lithiumsecondary batteries manufactured using the same andPreparation process thereof
KR1020040099606A
Separator for secondary battery and secondary battery comprising same
KR1020150015918A
Ceramic coating on battery separators
KR1020150094723A
Composite lithium battery separator and preparation method therefor