All-solid-state secondary battery
The integration of a carbon-based material matrix and protective layer in all-solid-state secondary batteries addresses safety concerns and lifespan issues by preventing side reactions and lithium dendrite growth, ensuring improved safety and performance.
Patent Information
- Application Number
- PCT/KR2024/003359
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-05
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
All-solid-state secondary batteries with liquid electrolytes face safety risks due to flammable solvents, and sulfide-based solid electrolytes react with negative electrode current collectors, leading to reduced lifespan and potential short circuits caused by lithium dendrite growth and uneven precipitation.
Incorporating a carbon-based material matrix with a metal-based negative electrode active material and a protective layer between the negative electrode current collector and active material layer, which includes a carbon-based nanostructure, to prevent agglomeration and ensure uniform thickness, thereby reducing the risk of short circuits and improving cycle characteristics.
The solution enhances the safety and lifespan of all-solid-state secondary batteries by preventing side reactions and lithium dendrite growth, while maintaining high energy density and rate characteristics.
Smart Images

Figure KR2024003359_03102024_PF_FP_ABST
Abstract
Description
All-solid-state secondary batteries
[0001] It's about all-solid-state secondary batteries.
[0002] Recently, there has been active development of batteries that offer increased energy density and safety. Lithium batteries are used in information technology, communication devices, and automobiles. Because automobiles are life-threatening, safety is paramount.
[0003] Lithium batteries containing liquid electrolytes contain flammable organic solvents. Lithium batteries containing liquid electrolytes have a high risk of overheating and fire in the event of a short circuit.
[0004] Solid electrolytes offer reduced risk of overheating and fire during short circuits compared to liquid electrolytes. Lithium batteries containing solid electrolytes can offer improved safety compared to those containing liquid electrolytes.
[0005] Sulfide-based solid electrolytes are prone to reacting with the negative electrode collector, causing side reactions. For example, if the sulfide-based solid electrolyte comes into contact with the negative electrode collector during charge / discharge, side reactions between the sulfide-based solid electrolyte and the negative electrode collector can shorten the life of the lithium battery. Therefore, a method for preventing contact between the sulfide-based solid electrolyte and the negative electrode collector is required.
[0006] The negative electrode active material layer, which is wet-positioned between the solid electrolyte layer and the negative electrode current collector, is difficult to form with a uniform thickness. The thickness variation of the negative electrode active material layer may cause non-uniform lithium deposition and growth of lithium dendrites between the negative electrode active material layer and the negative electrode current collector. Such non-uniform lithium deposition and / or growth of lithium dendrites may cause a short circuit in the lithium battery. A method for reducing the thickness variation of the negative electrode active material layer is required.
[0007] The negative electrode active material layer, which is wet-positioned between a solid electrolyte layer and a negative electrode current collector, is prone to forming agglomerates of the negative electrode active material within the negative electrode active material layer during the drying process. The agglomerated negative electrode active material may cause an uneven current density within the negative electrode active material layer. The uneven current density may cause uneven lithium deposition and / or growth of lithium dendrites between the negative electrode material layer and the negative electrode current collector. Such uneven lithium deposition and / or growth of lithium dendrites may cause a short circuit in a lithium battery. A method for suppressing agglomeration of the negative electrode active material within the negative electrode active material layer is required.
[0008] One aspect is to provide a new structure of all-solid-state secondary battery.
[0009] According to one side example
[0010] It comprises an anode layer; a cathode layer; and a solid electrolyte layer disposed between the anode layer and the cathode layer,
[0011] The above positive electrode layer includes a positive electrode current collector; and a positive electrode active material layer, and the solid electrolyte layer includes a sulfide-based solid electrolyte.
[0012] The negative electrode layer includes a negative electrode current collector; a first negative electrode active material layer; and a first protective layer disposed between the negative electrode current collector and the first negative electrode active material layer.
[0013] The first negative electrode active material layer includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix,
[0014] wherein the above carbon-based material matrix comprises a first carbon-based nanostructure, and the first protective layer comprises a second carbon-based nanostructure,
[0015] An all-solid-state secondary battery is provided, wherein the specific heat capacity of the negative electrode collector is 450 J / Kg·K or more.
[0016] According to another example
[0017] It comprises an anode layer; a cathode layer; and a solid electrolyte layer disposed between the anode layer and the cathode layer,
[0018] The above positive electrode layer includes a positive electrode current collector; and a positive electrode active material layer, and the solid electrolyte layer includes a sulfide-based solid electrolyte.
[0019] The negative electrode layer includes a negative electrode current collector; a first negative electrode active material layer; and a first protective layer disposed between the negative electrode current collector and the first negative electrode active material layer.
[0020] The first negative electrode active material layer includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix,
[0021] An all-solid-state secondary battery is provided, wherein the carbon-based material matrix includes a first carbon-based nanostructure, and the first protective layer includes a second carbon-based nanostructure.
[0022] According to one aspect, by using an all-solid-state secondary battery having a novel structure, it is possible to provide an all-solid-state secondary battery in which short circuit is suppressed and cycle characteristics are improved by improving the uniformity of the thickness of the negative electrode active material layer and suppressing aggregation of the negative electrode active material.
[0023] Figure 1 is a cross-sectional view of an all-solid-state secondary battery according to an exemplary embodiment.
[0024] Figure 2 is a cross-sectional view of a bi-cell all-solid-state secondary battery according to an exemplary embodiment.
[0025] Figure 3 is a cross-sectional view of an all-solid-state secondary battery according to an exemplary embodiment.
[0026] Figure 4 is a cross-sectional view of an all-solid-state secondary battery according to an exemplary embodiment.
[0027] Figure 5 is a cross-sectional view of a bi-cell all-solid-state secondary battery according to an exemplary embodiment.
[0028] Various embodiments are illustrated in the accompanying drawings. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. Like reference numerals in the drawings indicate like elements.
[0029] When a component is referred to as being "on" another component, it can be understood that it is either directly on top of the other component or that other components may be intervening between them. Conversely, when a component is referred to as being "directly on" another component, no intervening components are present.
[0030] Although the terms "first," "second," "third," etc. may be used herein to describe various components, elements, regions, layers, and / or zones, these components, elements, regions, layers, and / or zones should not be limited by these terms. These terms are used only to distinguish one component, element, region, layer, or zone from another component, element, region, layer, or zone. Thus, a first component, element, region, layer, or zone described below may be referred to as a second component, element, region, layer, or zone without departing from the teachings of this specification.
[0031] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms including "at least one," unless the content clearly dictates otherwise. "At least one" should not be construed as limiting to the singular. As used herein, the term "and / or" includes any and all combinations of one or more of the listed items. The terms "comprises" and / or "comprising" as used in the detailed description specify the presence of stated features, regions, integers, steps, operations, components, and / or ingredients, but do not preclude the presence or addition of one or more other features, regions, integers, steps, operations, components, ingredients, and / or groups thereof.
[0032] Spatially relative terms such as "below," "under," "bottom," "above," "above," and "top" may be used herein to readily describe the relationship of one component or feature to another. It will be understood that spatially relative terms are intended to encompass different orientations of the device when in use or operation in addition to the orientations depicted in the drawings. For example, if the device in the drawings were turned over, a component described as "below" or "below" another component or feature would then be oriented "above" the other component or feature. Thus, the exemplary term "below" can encompass both the above and below orientations. The device can be arranged in other orientations (rotated 90 degrees or otherwise rotated), and the spatially relative terms used herein can be interpreted accordingly.
[0033] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. Furthermore, it will be understood that terms defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning within the context of the relevant art and the present disclosure, and not in an idealized or overly formal sense.
[0034] Exemplary embodiments are described herein with reference to cross-sectional drawings that are schematic representations of idealized embodiments. As such, variations from the shapes depicted are to be expected, for example, as a result of manufacturing techniques and / or tolerances. Therefore, the embodiments described herein should not be construed as limited to the specific shapes of regions as depicted herein, but should encompass variations in shapes resulting from, for example, manufacturing. For example, regions depicted or described as flat may typically have rough and / or non-linear features. Moreover, angles depicted as sharp may be rounded. Therefore, the regions depicted in the drawings are schematic in nature, and their shapes are not intended to depict the precise shapes of the regions, nor are they intended to limit the scope of the claims.
[0035] "Group" means a group in the periodic table of elements according to the International Union of Pure and Applied Chemistry ("IUPAC") Group 1-18 classification system.
[0036] In the present disclosure, “specific heat” can be measured, for example, using a Differential Scanning Calorimeter (DSC).
[0037] In the present disclosure, “aspect ratio” can be measured, for example, from scanning electron microscope (SEM), transmission electron microscope (TEM) or atomic force microscope (AFM) images.
[0038] In the present disclosure, the “nanostructure,” “length,” “width,” “thickness,” “diameter,” and / or “aligned angle” of the first carbon-based nanostructure, the second carbon-based nanostructure, and the third carbon-based nanostructure can be measured, for example, from scanning electron microscope (SEM), transmission electron microscope (TEM), or atomic force microscope (AFM) images.
[0039] In the present disclosure, the “thickness” and / or “diameter” of the core and shell of the negative electrode active material can be measured from, for example, scanning electron microscope (SEM), transmission electron microscope (TEM) or atomic force microscope (AFM) images.
[0040] In the present disclosure, "porosity", "specific area", "pore size" and "pore volume" can be measured, for example, by a gas adsorption method. The gas used in the gas adsorption method can be, for example, nitrogen.
[0041] In this disclosure, "particle diameter" refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle diameter can be measured using a particle size analyzer (PSA). The "particle diameter" is, for example, the average particle diameter. The "average particle diameter" is, for example, D50, the median particle diameter.
[0042] D50 is the size of the particle corresponding to 50% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.
[0043] D90 is the size of the particle corresponding to 90% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.
[0044] D10 is the size of the particle corresponding to 10% of the cumulative volume, calculated from the particle side with a small particle size in the particle size distribution measured by laser diffraction.
[0045] Alternatively, in the present disclosure, the “particle size” is measured manually or by software from a scanning electron microscope and / or transmission electron microscope image of a cross-section of an all-solid-state secondary battery, and is an arithmetic average of the particle sizes of a plurality of particles shown in the image.
[0046] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0047] In this disclosure, “alloy” means a mixture of two or more metals.
[0048] In the present disclosure, “electrode active material” means an electrode material capable of undergoing lithiation and delithiation.
[0049] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.
[0050] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0051] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to an electrode active material.
[0052] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from an electrode active material.
[0053] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.
[0054] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.
[0055] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.
[0056] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.
[0057] While specific implementations have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently anticipated or unforeseen may occur to the applicant or those skilled in the art. Accordingly, the appended claims, as filed and as amended, are intended to encompass all such alternatives, modifications, variations, improvements, and substantial equivalents.
[0058]
[0059] Hereinafter, an all-solid-state secondary battery according to exemplary implementation examples will be described in more detail.
[0060] [All-solid-state secondary battery]
[0061] According to one embodiment, an all-solid-state secondary battery comprises: a positive electrode layer; a negative electrode layer; and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer comprises a positive electrode current collector; and a positive electrode active material layer, wherein the solid electrolyte layer comprises a sulfide-based solid electrolyte, the negative electrode layer comprises a negative electrode current collector; a first negative electrode active material layer; and a first protective layer disposed between the negative electrode current collector and the first negative electrode active material layer, wherein the first negative electrode active material layer comprises a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix, wherein the carbon-based material matrix comprises a first carbon-based nanostructure, and the first protective layer comprises a second carbon-based nanostructure, wherein the negative electrode current collector has a specific heat capacity of 450 J / Kg·K or more.
[0062] By including a carbon-based nanostructure that is dry-formed as the first negative electrode active material layer, defects such as uneven thickness of the negative electrode active material layer and agglomeration of the negative electrode active material that occur in the wet negative electrode active material layer can be prevented. By including the first negative electrode active material layer in the all-solid-state secondary battery, uneven lithium precipitation and / or growth of lithium dendrites during the charge and discharge process are suppressed. As a result, short-circuiting of the all-solid-state secondary battery is suppressed and life characteristics are improved. By including the first protective layer in the all-solid-state secondary battery, side reactions due to contact between the sulfide-based solid electrolyte and the negative electrode current collector are suppressed. As a result, the reversibility of the electrode reaction is improved, and the life characteristics of the all-solid-state secondary battery are improved.
[0063] Since the specific heat of the negative electrode collector is 450 J / Kg·K or higher, local temperature changes in the negative electrode layer due to heat generated during charging and discharging of the all-solid-state secondary battery can be mitigated. Accordingly, deterioration of the all-solid-state secondary battery due to local temperature changes can be effectively prevented.
[0064]
[0065] Referring to FIGS. 1 to 5, an all-solid-state secondary battery (1) includes a positive electrode layer (10); a negative electrode layer (20); and a solid electrolyte layer (30) disposed between the positive electrode layer (10) and the negative electrode layer (20), wherein the positive electrode layer (10) includes a positive electrode current collector (11); and a positive electrode active material layer (12), the solid electrolyte layer (30) includes a sulfide-based solid electrolyte, and the negative electrode layer (20) includes a negative electrode current collector (21); a first negative electrode active material layer (22); And a first protective layer (23) disposed between a negative electrode current collector (21) and a first negative electrode active material layer (22), wherein the first negative electrode active material layer (22) includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix, wherein the carbon-based material matrix includes a first carbon-based nanostructure, and the first protective layer (23) includes a second carbon-based nanostructure, and the specific heat capacity of the negative electrode current collector (21) is 450 J / Kg·K or more.
[0066] [Cathode layer]
[0067] [Cathode layer: carbon-based material matrix]
[0068] Referring to FIGS. 1 to 5, the negative electrode layer (20) includes a negative electrode current collector (21); a first negative electrode active material layer (22); and a first protective layer (23, 23a, 23b) disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22). The first negative electrode active material layer (22) includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix.
[0069] The first negative electrode active material layer (22) includes a carbon-based material matrix. The carbon-based material matrix includes a first carbon-based nanostructure. The carbon-based nanostructure is a structure having nano-sized dimensions and made of a carbon-based material. The carbon-based nanostructure may include, for example, a one-dimensional carbon-based nanostructure, a two-dimensional carbon-based nanostructure, a three-dimensional carbon-based nanostructure, or a combination thereof. The one-dimensional carbon-based nanostructure may include, for example, carbon nanorods, nanofibers, carbon nanotubes, or a combination thereof. The two-dimensional carbon-based nanostructure may include, for example, carbon nanosheets, carbon nanobelts, carbon nanoflakes, graphene, graphene oxide (GO), reduced graphene oxide (rGO), or a combination thereof. The three-dimensional carbon-based nanostructure may be a structure in which a plurality of one-dimensional carbon-based nanostructures and / or two-dimensional carbon-based nanostructures are connected or stacked. The first carbon-based nanostructure may include, for example, a two-dimensional carbon-based nanostructure. The first carbon-based nanostructure may include, for example, graphene, graphene oxide (GO), reduced graphene oxide (rGO), or a combination thereof.
[0070] The carbon-based material matrix may include, for example, a first carbon-based nanostructure arranged in a certain direction. The first carbon-based nanostructure may include, for example, graphene. The carbon-based material matrix may include graphene arranged in a certain direction. The carbon-based material matrix may include, for example, a first carbon-based nanostructure aligned in a direction parallel to a surface of the negative electrode current collector (21). The carbon-based material matrix may include, for example, graphene. The carbon-based material matrix may include graphene aligned in a direction parallel to a surface of the negative electrode current collector (21). The graphene may be aligned, for example, at an angle of -30° to 30°, -20° to 20°, -10° to 10°, or -5° to 5° with respect to the surface of the negative electrode current collector (21). By aligning the first carbon-based nanostructures in the carbon-based material matrix in a direction parallel to the surface of the negative electrode current collector (21), the growth of lithium dendrites through the first negative electrode active material layer (22) can be more effectively suppressed. In addition, the first carbon-based nanostructures in the carbon-based material matrix can have a structure in which they are stacked along the thickness direction of the first negative electrode active material layer (22). A plurality of first carbon-based nanostructures can be stacked along the thickness direction of the first negative electrode active material layer (22) in the carbon-based material matrix. The carbon-based material matrix can include, for example, a plurality of first carbon-based nanostructure layers stacked along the thickness direction of the first negative electrode active material layer (22). By stacking the first carbon-based nanostructures in the carbon-based material matrix along the thickness direction of the first negative electrode active material layer (22), the structural density and structural stability of the first negative electrode active material layer (22) can be further improved.
[0071] The carbon-based material matrix may include, for example, first carbon-based nanostructures that are irregularly arranged and non-aligned. The first carbon-based nanostructure may include, for example, graphene, and the carbon-based material matrix may include graphene that is irregularly arranged and non-aligned. The carbon-based material matrix may include, for example, first carbon-based nanostructures that are irregularly and / or randomly arranged with respect to the surface of the negative electrode current collector (21). The carbon-based material matrix may include, for example, graphene, and the carbon-based material matrix may include graphene that is irregularly and / or randomly arranged with respect to the surface of the negative electrode current collector (21). By the first carbon-based nanostructures in the carbon-based material matrix being irregularly and / or randomly arranged with respect to the surface of the negative electrode current collector (21), the lithium ion transport path and / or electron transport path through the first negative electrode active material layer (22) may be diversified. Therefore, the internal resistance of an all-solid-state secondary battery including a carbon-based material matrix may be further reduced.
[0072] The carbon-based material matrix may include, for example, crystalline carbon, amorphous carbon, or a combination thereof. The carbon-based material matrix includes a first carbon-based nanostructure, and the first carbon-based nanostructure may include, for example, crystalline carbon nanostructures, amorphous carbon nanostructures, or a combination thereof. A carbon-based material matrix composed of crystalline carbon nanostructures may have high crystallinity. A carbon-based material matrix composed of amorphous carbon nanostructures may have low crystallinity. The carbon-based material matrix may have high crystallinity by including, for example, the first carbon-based nanostructures aligned in a certain direction. As the content of the first carbon-based nanostructures aligned in a certain direction increases in the carbon-based material matrix, the crystallinity of the first negative electrode active material layer (22) may increase. The carbon-based material matrix may have low crystallinity, for example, by including the first carbon-based nanostructures that are randomly arranged. As the content of the first carbon-based nanostructures that are randomly arranged within the carbon-based material matrix increases, the crystallinity of the first negative electrode active material layer (22) may decrease. The crystallinity of the carbon-based material matrix may be determined, for example, by a Raman spectrum, an XRD spectrum, a high-resolution transmission electron microscope, or the like.
[0073] The carbon-based material matrix comprises a first carbon-based nanostructure, and the first carbon-based nanostructure can be doped with, for example, a dopant. The dopant can comprise an n-type dopant, a p-type dopant, or a combination thereof. An n-type dopant is a dopant that introduces electrons into the carbon-based material by having more electrons than carbon, for example. A p-type dopant is a dopant that introduces holes into the carbon-based material by having fewer electrons than carbon. The first carbon-based nanostructure can comprise, for example, dopant-doped graphene. The doped graphene can comprise, for example, an n-type dopant, a p-type dopant, or a combination thereof. The dopant can comprise, for example, nitrogen (N), phosphorus (P), boron (B), sulfur (S), fluorine (F), chlorine (Cl), bromine (Br), germanium (Ge), gallium (Ga), or a combination thereof. Nitrogen (N) and phosphorus (P) are, for example, n-type dopants. Gallium (Ga) is, for example, a p-type dopant. The content of the dopant included in the doped first carbon-based nanostructure may be, for example, 3 at% or less, 2 at% or less, 1 at% or less, or 0.5 at% or less. By doping the first carbon-based nanostructure with the dopant, the conductivity of the first carbon-based nanostructure may be further increased. By including the doped first carbon-based nanostructure in the carbon-based material matrix, the internal resistance of the first negative electrode active material layer (22) may be reduced, and the interfacial resistance between the first negative electrode active material layer (22) and the solid electrolyte layer (30) may be further reduced. As a result, the internal resistance of the all-solid-state secondary battery may be reduced, and the high-rate characteristics may be further improved.
[0074] The carbon-based material matrix may not include a binder. By not including a binder in the carbon-based material matrix, the internal resistance of the first negative electrode active material layer (22) may be reduced and the ionic conductivity and / or electronic conductivity may be improved. Consequently, the cycle characteristics, such as the high-rate characteristics of the all-solid-state secondary battery, may be improved.
[0075] The carbon-based material matrix may further include, for example, pores arranged within the carbon-based material matrix. The carbon-based material matrix may include a plurality of first carbon-based nanostructures, and pores defined by the plurality of first carbon-based nanostructures may be formed within the carbon-based material matrix by the plurality of first carbon-based nanostructures being randomly arranged. The carbon-based material matrix may have a low porosity by including, for example, the first carbon-based nanostructures aligned in a certain direction. As the content of the first carbon-based nanostructures aligned in a certain direction within the carbon-based material matrix increases, the content of pores included in the carbon-based material matrix may decrease. Accordingly, the first negative electrode active material layer (22) may have a reduced porosity. The porosity of the carbon-based material matrix may increase by including, for example, the first carbon-based nanostructures that are randomly arranged. As the content of the first carbon-based nanostructures randomly arranged within the carbon-based material matrix increases, the content of pores contained in the carbon-based material matrix may increase. Accordingly, the first negative electrode active material layer (22) may have an increased porosity. The porosity of the carbon-based material matrix can be measured, for example, by a gas adsorption method.
[0076] The carbon-based material matrix may be, for example, a lithium host. The carbon-based material matrix may be, for example, an electrochemically inert lithium host. An electrochemically inert lithium host is a lithium host that does not react with lithium to form a compound and acts as a conductor for electron transfer and / or a receptor for accepting precipitated lithium. By the carbon-based material matrix acting as an electrochemically inert lithium host, the deterioration of the all-solid-state secondary battery (1) due to volume change and / or physical property change of the first negative electrode active material layer (22) during charge and discharge can be more effectively prevented. Therefore, by the carbon-based material matrix acting as an electrochemically inert lithium host, electron transfer and / or lithium precipitation in the first negative electrode active material layer (22) can be performed more effectively. Alternatively, the carbon-based material matrix may be, for example, an electrochemically active lithium host. An electrochemically active lithium host is a lithium host that reacts with lithium to form a compound. Since the carbon-based material matrix acts as an electrochemically active lithium host, non-uniform lithium precipitation in the first negative electrode active material layer (22) can be more effectively prevented, thereby further improving the cycle characteristics of the all-solid-state secondary battery (1). Therefore, since the carbon-based material matrix acts as an electrochemically active lithium host, uniform lithium precipitation can be performed in the first negative electrode active material layer (22). Since the carbon-based material matrix further includes pores, lithium metal can be precipitated within the pores.
[0077] [Cathode layer: Cathode active material]
[0078] Referring to FIGS. 1 to 5, the negative electrode layer (20, 20a, 20b) includes a negative electrode current collector (21, 21a, 21b); and a first negative electrode active material layer (22, 22a, 22b) disposed on the negative electrode current collector. The first negative electrode active material layer (22) includes a metal-based negative electrode active material disposed within a carbon-based material matrix.
[0079] A metal-based negative electrode active material is a negative electrode active material that forms an alloy or compound with lithium. The metal-based negative electrode active material includes, but is not limited to, one or more alloy-forming elements selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal-based negative electrode active material that forms an alloy or compound with lithium in the art may be used. For example, nickel (Ni) does not form an alloy with lithium and is therefore not a metal-based negative electrode active material. The metal-based negative electrode active material may not include, for example, a metal oxide. The metal-based negative electrode active material includes, for example, a metal that forms an alloy or compound with lithium, and may not include an oxide of such a metal. The metal-based negative electrode active material includes, for example, silver (Ag), but may not include an oxide of silver (Ag) (e.g., Ag2O).
[0080] The metal-based negative electrode active material may be, for example, a composite negative electrode active material having a core / shell structure. The metal-based negative electrode active material may include, for example, a core; and a shell disposed along a surface of the core. The shell may cover part or all of the surface of the core. The core may include, for example, a metal that forms an alloy or compound with lithium. The metal that forms an alloy or compound with lithium may include, for example, one or more alloy-forming elements selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The shell may include, for example, a carbon-based material. The shell may include, for example, a third carbon-based nanostructure. The third carbon-based nanostructure may be, for example, the same carbon-based nanostructure as the first carbon-based nanostructure. The third carbon-based nanostructure may include, for example, graphene, graphene oxide, reduced graphene oxide, or a combination thereof. The third carbon-based material nanostructure may be distinguished from the first carbon-based nanostructure included in the carbon-based material matrix in one or more of the following properties: composition, thickness, location, crystallinity, etc. The third carbon-based nanostructure may constitute, for example, a shell of a metal-based negative electrode material and may be distinguished from the carbon-based material matrix. The metal-based negative electrode material may have a structure of a shell including, for example, a metal core including lithium and an alloy or compound; and a third carbon-based nanostructure disposed on the core. The metal-based negative electrode material may have a structure of a metal core including, for example, lithium and an alloy or compound; and a shell including graphene disposed on the core. The shell may include, for example, amorphous carbon.By including amorphous carbon in the shell, ion transfer and / or electron transfer between the core and the carbon-based material matrix can be more easily performed. The shell can be, for example, an amorphous carbon coating layer disposed on the core. The metal-based negative electrode active material can have a structure of, for example, a metal core including lithium and an alloy or compound; and an amorphous carbon-containing shell disposed on the core. The metal-based negative electrode active material can have a structure of, for example, a metal core including lithium and an alloy or compound; and an amorphous carbon coating layer disposed on the core.
[0081] The metal-based negative electrode active material has, for example, a particle form. The particle size of the metal-based negative electrode active material having a particle form is, for example, 2 μm or less, 1.5 μm or less, 1 μm or less, 0.5 μm or less, or 100 nm or less. The particle size of the negative electrode active material having a particle form is, for example, 1 nm to 2 μm, 1 nm to 1.5 μm, 5 nm to 1 μm, 10 nm to 500 nm, 10 nm to 400 nm, 10 nm to 200 nm, or 10 nm to 100 nm. When the metal-based negative electrode active material has a particle size in this range, reversible absorption and / or desorption of lithium may be facilitated during charge and discharge. The metal-based negative electrode active material may be a reduction product of a metal-based negative electrode active material precursor. The metal-based negative electrode active material may be a reduction product of a metal ion. Since the metal-based negative electrode active material is a reduction product of metal ions, it can be uniformly dispersed and distributed within the carbon-based material matrix without agglomerating with each other. The particle size of the metal-based negative electrode active material is, for example, an arithmetic mean value of particle sizes of the metal-based negative electrode active material obtained by analyzing an electron microscope image of a cross-section of the first negative electrode active material layer (22) by software or by manual means. The metal-based negative electrode active material particles may include a core; and a shell arranged along the surface of the core. The particle size of the core is, for example, 1 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 400 nm, 10 nm to 300 nm, 10 nm to 200 nm, or 10 nm to 100 nm. The thickness of the shell is, for example, 100 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The thickness of the shell is, for example, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, 1 nm to 20 nm, or 1 nm to 10 nm.The cycle characteristics of an all-solid-state secondary battery (1) including metal-based negative electrode active material particles can be further improved by having the core and shell each having a particle size and thickness within this range.
[0082] The content of the metal-based negative electrode active material may be 10 parts by weight or less, 5 parts by weight or less, 3 parts by weight or less, or 2 parts by weight or less, based on 100 parts by weight of the carbon-based material matrix. The content of the metal-based negative electrode active material may be 0.1 to 10 parts by weight, 0.5 to 5 parts by weight, 0.5 to 3 parts by weight, or 0.5 to 2 parts by weight, based on 100 parts by weight of the carbon-based material matrix. When the metal-based negative electrode active material has a content within this range, the cycle characteristics of the all-solid-state secondary battery (1) may be further improved. Compared to a conventional first negative electrode active material layer (11) including a simple blend of a metal-based negative electrode active material and a carbon-based material, the first negative electrode active material layer (22) employed in the all-solid-state secondary battery (1) of FIGS. 1 to 5 may have a reduced content of the metal-based negative electrode active material. By including a metal-based negative electrode active material dispersed and arranged in a carbon-based material matrix by a dry method as the first negative electrode active material layer (22), an all-solid-state secondary battery (1) having excellent cycle characteristics at a relatively low content of metal-based negative electrode active material can be provided.
[0083] The carbon-based material matrix may further include a carbon-based negative electrode active material disposed within the carbon-based material matrix. The carbon-based negative electrode active material is, for example, amorphous carbon. Amorphous carbon includes, but is not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), etc., and any material classified as amorphous carbon in the art may be included. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon. The carbon-based negative electrode active material may be omitted.
[0084] [Cathode layer: first cathode active material layer]
[0085] The thickness of the first negative electrode active material layer (22) is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode active material layer (12). The thickness of the first negative electrode active material layer (22) is, for example, 20 μm or less, 10 μm or less, 7 μm or less, or 5 μm or less. The thickness of the first negative electrode active material layer (22) is, for example, 1 μm to 20 μm, 2 μm to 10 μm, 2 μm to 7 μm, or 2 μm to 5 μm. If the thickness of the first negative electrode active material layer (22) is too thin, lithium dendrites formed between the first negative electrode active material layer (22) and the negative electrode current collector (21) collapse the first negative electrode active material layer (22), making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). If the thickness of the first negative electrode active material layer (22) is excessively increased, the energy density of the all-solid-state secondary battery (1) decreases and the internal resistance of the all-solid-state secondary battery (1) due to the first negative electrode active material layer (22) increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1).
[0086] When the thickness of the first negative electrode active material layer (22) decreases, the charge capacity of the first negative electrode active material layer (22) also decreases, for example. The charge capacity of the first negative electrode active material layer (22) is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, 5% or less, or 2% or less than the charge capacity of the positive electrode active material layer (12). The charge capacity of the first negative electrode active material layer (22) is, for example, 0.1% to 50%, 0.1% to 40%, 0.1% to 30%, 0.1% to 20%, 0.1% to 10%, 0.1% to 5%, or 0.1% to 2% than the charge capacity of the positive electrode active material layer (12). If the charge capacity of the first negative electrode active material layer (22) is too small, the thickness of the first negative electrode active material layer (22) becomes very thin, so that lithium dendrites formed between the first negative electrode active material layer (22) and the negative electrode current collector (21) during repeated charge and discharge processes collapse the first negative electrode active material layer (22), making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). If the charge capacity of the first negative electrode active material layer (22) increases excessively, the energy density of the all-solid-state secondary battery (1) decreases and the internal resistance of the all-solid-state secondary battery (1) due to the first negative electrode active material layer (22) increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery (1). The ratio (C1 / C2) of the charge capacity (C1) of the first negative electrode active material layer (22) and the charge capacity (C2) of the positive electrode active material layer (12) is, for example, 0.001 to 0.45, 0.001 to 0.4, 0.001 to 0.3, 0.001 to 0.3, 0.001 to 0.2, 0.001 to 0.1, 0.001 to 0.05, or 0.001 to 0.02. The charge capacity of the positive electrode active material layer (12) is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer (12). When several types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values is the charge capacity of the positive electrode active material layer (12).The charge capacity of the first negative electrode active material layer (22) is also calculated in the same way. That is, the charge capacity of the first negative electrode active material layer (22) is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the first negative electrode active material layer (22). When multiple types of negative electrode active materials are used, the charge capacity density × mass value is calculated for each negative electrode active material, and the sum of these values is the capacity of the first negative electrode active material layer (22). Here, the charge capacity densities of the positive electrode active material and the negative electrode active material are capacities measured using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacities of the positive electrode active material layer (12) and the first negative electrode active material layer (22) are directly measured by measuring the charge capacity using the all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer (12) and the first negative electrode active material layer (22) may be the initial charge capacity measured at the time of the first charge cycle.
[0087] The first negative electrode active material layer (22) may be free of a binder. Since the first negative electrode active material layer (22) is formed by a dry method, the first negative electrode active material layer (22) may not include a binder. Since the first negative electrode active material layer (22) does not include a binder, the electronic conductivity and / or ionic conductivity of the first negative electrode active material layer (22) may be improved, and the internal resistance may be reduced. Accordingly, the cycle characteristics, such as the high rate characteristics, of the all-solid-state secondary battery (1) including the first negative electrode active material layer (22) may be improved. The first negative electrode active material layer may be manufactured by a dry method, such as CVD or PVD. The dry method used to manufacture the first negative electrode active material layer is not particularly limited, and any dry method used without a binder in the relevant technical field may be used.
[0088] The thickness of the first negative electrode active material layer (22, 22a, 22b) may be greater than the thickness of the first protective layer (23, 23a, 23b). The thickness of the first negative electrode active material layer (22, 22a, 22b) may be 150% or more, 200% or more, 300% or more, or 500% or more of the thickness of the first protective layer (23, 23a, 23b). Since the first negative electrode active material layer (22) has a thickness within this range, the thickness of the first protective layer (23, 23a, 23b) is relatively reduced, and thus the energy density of the all-solid-state secondary battery can be further improved.
[0089] In the Raman spectrum for the cathode layer (20), 1350 cm is derived from amorphous carbon. -1 Nearby D-band peak intensity (I D ) and 1580 cm derived from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G ) can be, for example, 20 or less, 15 or less, 10 or less, 6 or less, 4 or less, 3 or less, 1 or less, 0.8 or less, or 1.5 or less.
[0090] In the Raman spectrum for the cathode layer (20), 1350 cm is derived from amorphous carbon. -1 Nearby D-band peak intensity (I D ) and 1580 cm derived from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G ) can be, for example, greater than 0, greater than or equal to 0.01, greater than or equal to 0.05, greater than or equal to 0.1, greater than or equal to 0.3, greater than or equal to 0.5, greater than or equal to 1.0, or greater than or equal to 1.5.
[0091] In the Raman spectrum for the cathode layer (20), 1350 cm is derived from amorphous carbon. -1 Nearby D-band peak intensity (I D) and 1580 cm derived from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G ) can be, for example, from 0 to 20, from 0 to 15, from 0 to 10, from 0.01 to 10, from 0.01 to 6, from 0.1 to 4, from 0.5 to 3, from 1.0 to 3, or from 1.5 to 3. In the Raman spectrum for the cathode layer (20), 1350 cm derived from amorphous carbon -1 Nearby D-band peak intensity (I D ) and 1580 cm derived from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G ) can be, for example, 1 to 10, 1 to 6, 1 to 4, 1.5 to 4. 2 to 4 or 1.5 to 4. In the Raman spectrum for the cathode layer (20), 1350 cm derived from amorphous carbon -1 Nearby D-band peak intensity (I D ) and 1580 cm derived from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G) can be, for example, 1 to 10, 1 to 6, 2 to 6, 3 to 6, or 3.5 to 6. The Raman spectrum is for the first negative electrode active material layer (22) and the first protective layer (22) of the negative electrode layer (20). Since the negative electrode layer (20) has a peak intensity ratio in this range, the deterioration of the negative electrode current collector (21) due to the solid electrolyte can be more effectively prevented. If the intensity ratio of the negative electrode layer (20) increases excessively, it may be difficult to effectively prevent the deterioration of the negative electrode current collector (21) due to the solid electrolyte. The negative electrode layer (20) including the nickel negative electrode current collector (21) may have a relatively lower intensity ratio as described above compared to the negative electrode layer (20) including the copper negative electrode current collector (21).
[0092] The porosity obtained using the nitrogen gas adsorption method (multi-point BET) for the cathode layer (20) may be, for example, 30% or less, 25% or less, 20% or less, 15% or less, 10% or less, 5% or less, 3% or less, 2% or less, 1% or less, 0.8% or less, or 0.5% or less.
[0093] The porosity obtained using the nitrogen gas adsorption method (multi-point BET) for the cathode layer (20) may be, for example, more than 0%, 0.1% or more, 0.5% or more, or 1% or more.
[0094] The porosity obtained using the nitrogen gas adsorption method (multi-point BET) for the cathode layer (20) may be, for example, more than 0 to 30%, more than 0 to 25%, more than 0 to 20%, 0.1 to 15%, 0.1 to 10%, 1 to 10%, or 2 to 8%. The porosity obtained using the nitrogen gas adsorption method (multi-point BET) for the cathode layer (20) may be, for example, 1 to 25%, 2 to 15%, 5 to 15%, or 8 to 15%. The porosity obtained using the nitrogen gas adsorption method (multi-point BET) for the cathode layer (20) may be, for example, 1 to 25%, 5 to 25%, or 5 to 25%. Since the negative electrode layer (20) has a porosity within this range, deterioration of the negative electrode current collector (21) caused by the solid electrolyte can be more effectively prevented. If the porosity of the negative electrode layer (20) increases excessively, it may be difficult to effectively prevent deterioration of the negative electrode current collector (21) caused by the solid electrolyte.
[0095] [Cathode layer: first protective layer]
[0096] Referring to FIGS. 1 to 5, the negative electrode layer (20) includes a negative electrode current collector (21); a first negative electrode active material layer (22); and a first protective layer (23, 23a, 23b) disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22).
[0097] The first protective layer (23, 23a, 23b) is, for example, a conductive coating layer including a carbon-based material. Since the first protective layer (23, 23a, 23b) is a conductive coating layer, an increase in the internal resistance of the all-solid-state secondary battery can be suppressed despite the addition of the first protective layer (23, 23a, 23b). The first protective layer (23a, 23a, 23b) includes, for example, a second carbon-based nanostructure. The carbon-based nanostructure is a structure having nano-sized dimensions and made of a carbon-based material. The carbon-based nanostructure may include, for example, a one-dimensional carbon-based nanostructure, a two-dimensional carbon-based nanostructure, a three-dimensional carbon-based nanostructure, or a combination thereof. The second carbon-based nanostructure may include, for example, a two-dimensional carbon-based nanostructure. The second carbon-based nanostructure may include, for example, graphene, graphene oxide (GO), reduced graphene oxide (rGO), or a combination thereof. The second carbon-based nanostructure may be selected from the first carbon-based nanostructures described above. The second carbon-based nanostructure may be doped with a dopant. The second carbon-based nanostructure doped with a dopant may be selected from the first carbon-based nanostructure doped with a dopant.
[0098] The first protective layer (23, 23a, 23b) may include, for example, a second carbon-based nanostructure arranged in a certain direction with respect to the surface of the negative electrode current collector (21). The second carbon-based nanostructure may include, for example, graphene. The first protective layer (23, 23a, 23b) may include graphene arranged in a certain direction with respect to the surface of the negative electrode current collector (21).
[0099] The first protective layer (23, 23a, 23b) may include, for example, a second carbon-based nanostructure aligned in a direction parallel to the surface of the negative electrode collector (21). The second carbon-based nanostructure may be aligned in a direction parallel to the surface of the negative electrode collector (21). The first protective layer (23, 23a, 23b) may include, for example, graphene. The first protective layer (23, 23a, 23b) may include graphene aligned in a direction parallel to the surface of the negative electrode collector (21). The graphene may be aligned at an angle of, for example, -30° to 30°, -20° to 20°, -10° to 10°, or -5° to 5° with respect to the surface of the negative electrode collector (21). By aligning the second carbon-based nanostructure in the first protective layer (23, 23a, 23b) in a direction parallel to the surface of the negative electrode collector (21), contact between the solid electrolyte and the negative electrode collector (21) can be more effectively suppressed.
[0100] The first protective layer (23, 23a, 23b) may include, for example, second carbon-based nanostructures aligned in a direction protruding from the surface of the negative electrode collector (21). The second carbon-based nanostructures may be aligned in a direction protruding from the surface of the negative electrode collector (21). The first protective layer (23, 23a, 23b) may include, for example, graphene. The first protective layer (23, 23a, 23b) may include graphene aligned in a direction protruding from the surface of the negative electrode collector (21). The second carbon-based nanostructures may be aligned at, for example, an angle of 45° to 135°, 50° to 130°, 60° to 120°, 70° to 110°, or 80° to 100° with respect to the surface of the negative electrode collector (21). The second carbon-based nanostructures may be aligned, for example, perpendicular to the surface of the negative electrode collector (21). By aligning the second carbon-based nanostructures in the first protective layer (23, 23a, 23b) in a direction protruding from the surface of the negative electrode collector (21), electron transfer between the first negative electrode active material layer (22) and the negative electrode collector (21) can be performed more easily. As a result, an increase in the internal resistance of the all-solid-state secondary battery (1) can be more effectively suppressed.
[0101] The first protective layer (23, 23a, 23b) may have a structure in which the second carbon-based nanostructures are laminated along the thickness direction of the first protective layer (23, 23a, 23b). A plurality of second carbon-based nanostructures may be laminated along the thickness direction of the first protective layer (23, 23a, 23b) within the first protective layer (23, 23a, 23b). The first protective layer (23, 23a, 23b) may include, for example, a plurality of second carbon-based nanostructure layers laminated along the thickness direction of the first protective layer (23, 23a, 23b). By laminating the second carbon-based nanostructures along the thickness direction of the negative electrode current collector (21) within the first protective layer (23, 23a, 23b), the structural density and structural stability of the first protective layer (23, 23a, 23b) can be further improved. The second carbon-based structures can be laminated within the first protective layer (23, 23a, 23b) in, for example, 2000 layers or less, 1500 layers or less, 1000 layers or less, 500 layers or less, 100 layers or less, 70 layers or less, 50 layers or less, or 30 layers or less. The second carbon-based structures can be laminated within the first protective layer (23, 23a, 23b) in, for example, 1 to 100 layers, 5 to 70 layers, 10 to 50 layers, or 20 to 30 layers. The second carbon-based structure can be laminated within the first protective layer (23, 23a, 23b) in, for example, 1 to 2000 layers, 10 to 1000 layers, 100 to 1000 layers, 100 to 500 layers, or 100 to 300 layers. The second carbon-based structure can be laminated within the first protective layer (23, 23a, 23b) in, for example, 1 to 2000 layers, 10 to 2000 layers, 100 to 2000 layers, 500 to 2000 layers, or 1000 to 2000 layers. By having the second carbon-based structure having a number of layers within this range, the structural stability of the first protective layer (23, 23a, 23b) can be further improved.
[0102] The first protective layer (23, 23a, 23b) may be directly disposed on one surface of the negative electrode current collector (21). The first protective layer (23, 23a, 23b) may be inert to a solid electrolyte, particularly a sulfide-based solid electrolyte. By directly disposing the first protective layer (23, 23a, 23b) on one surface of the negative electrode current collector (21), contact between the negative electrode current collector (21) and the sulfide-based solid electrolyte is blocked, thereby more effectively preventing deterioration of the negative electrode current collector (21), such as corrosion of the negative electrode current collector (21).
[0103] The first protective layer (23, 23a, 23b) may be disposed, for example, on one surface of the negative electrode current collector (21) facing the solid electrolyte layer. The first protective layer (23, 23a, 23b) may also be disposed on the other surface of the negative electrode current collector (21) opposing the one surface of the negative electrode current collector (21), and may also be disposed on a side surface of the negative electrode current collector (21) between the one surface and the other surface. By covering part or all of the negative electrode current collector (21) with the first protective layer (23, 23a, 23b), deterioration caused by the sulfide-based solid electrolyte can be more effectively prevented. Therefore, the life characteristics of the all-solid-state secondary battery (1) including the first protective layer (23, 23a, 23b) can be improved.
[0104] The thickness of the first protective layer (23, 23a, 23b) may be, for example, 5 μm or less, 3 μm or less, 2 μm or less, 1.5 μm or less, 1 μm or less, 500 nm or less, 300 nm or less, or 100 nm or less. The thickness of the first protective layer (23, 23a, 23b) may be, for example, equal to or greater than the thickness of a graphene monolayer, 1 nm or more, 10 nm or more, 20 nm or more, 50 nm, or 100 nm or more. The thickness of the first protective layer (23, 23a, 23b) may be, for example, equal to or greater than the thickness of a graphene monolayer, 10 nm to 1.5 μm, 50 nm to 1 μm, 100 nm to 900 nm, 200 nm to 800 nm, or 300 nm to 700 nm. The thickness of the first protective layer (23, 23a, 23b) may be, for example, the thickness of a graphene single layer to 2 ㎛, 1 nm to 1.5 ㎛, 5 nm to 1 ㎛, 10 nm to 500 nm, 20 nm to 300 nm, or 20 nm to 100 nm. If the first protective layer (23, 23a, 23b) is too thick, the internal resistance of the all-solid-state secondary battery may increase and the energy density may decrease. If the thickness of the first protective layer (23, 23a, 23b) is too thin, it may be difficult to effectively block side reactions between the negative electrode current collector (21) and the solid electrolyte.
[0105] The first protective layer (23, 23a, 23b) may be free of a binder. Since the first protective layer (23, 23a, 23b) is formed by a dry method, the first protective layer (23, 23a, 23b) may not include a binder. Since the first protective layer (23, 23a, 23b) does not include a binder, the electronic conductivity of the first protective layer (23, 23a, 23b) may be improved and the internal resistance may be reduced. Accordingly, the cycle characteristics, such as the high rate characteristics, of the all-solid-state secondary battery (1) including the first protective layer (23, 23a, 23b) may be improved. The first protective layer (23, 23a, 23b) may be manufactured by a dry method, such as CVD or PVD. The dry method used to manufacture the first protective layer (23, 23a, 23b) is not particularly limited, and any dry method that can be used without a binder in the relevant technical field may be used. The first protective layer (23, 23a, 23b) may be formed of, for example, a second carbon-based nanostructure and may not include a binder. The first protective layer (23, 23a, 23b) may be formed of, for example, graphene and may not include a binder.
[0106] By arranging the first protective layer (23, 23a, 23b), the interfacial resistance between the negative electrode current collector (21) and the first negative electrode active material layer (22) can be reduced. Accordingly, by reducing the internal resistance of the all-solid-state secondary battery (1) including the negative electrode layer (20), the cycle characteristics of the all-solid-state secondary battery (1) can be further improved.
[0107] In addition, by arranging the first protective layer (23, 23a, 23b), heat dissipation of the negative electrode collector (21) can be more effectively performed. Since the first protective layer (23, 23a, 23b) includes a carbon-based material, the carbon-based material acts as a heat sink, thereby more effectively transferring heat generated in the negative electrode collector (21) to the outside of the all-solid-state secondary battery (1) during charge and discharge of the all-solid-state secondary battery (1). Therefore, local thermal runaway occurring during the charge and discharge process of the all-solid-state secondary battery (1) can be more effectively prevented.
[0108] [Cathode layer: negative electrode collector]
[0109] The specific heat capacity of the negative electrode current collector (21) is, for example, 450 J / Kg·K or more, 460 J / Kg·K or more, 480 J / Kg·K or more, or 490 J / Kg·K or more. The specific heat capacity of the negative electrode current collector (21) is, for example, 450 to 700 J / Kg·K, 460 to 650 J / Kg·K, 480 to 600 J / Kg·K, or 490 to 550 J / Kg·K. Since the negative electrode current collector has such a high specific heat, it can effectively alleviate local temperature changes within the negative electrode layer. Therefore, deterioration of the all-solid-state secondary battery (1) due to local temperature changes can be effectively prevented. The negative electrode current collector (21) is composed of, for example, a material that does not react with lithium, i.e., does not form an alloy or a compound. The material constituting the negative electrode current collector (21) is not necessarily limited to, for example, stainless steel (SUS), titanium (Ti), iron (Fe), and nickel (Ni), and any material that is used as an electrode current collector in the relevant technical field and has a specific heat of 450 J / Kg·K or higher is possible. The material constituting the negative electrode current collector (21) is particularly stainless steel (SUS). Stainless steel includes, for example, SUS316, SUS301, SUS304, SUS430, and the like, but is not limited to, these.
[0110] The negative electrode collector (21) may be composed of one of the above-described metals, or may be composed of an alloy or a coating material of two or more metals. The negative electrode collector (21) is, for example, in the form of a plate or foil.
[0111] The negative electrode current collector (21) may further include, for example, a thin film including an element capable of forming an alloy with lithium on the negative electrode current collector (21). The thin film is disposed between the negative electrode current collector (21) and the first negative electrode active material layer (22). The thin film includes, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium includes, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of one of these metals or an alloy of several types of metals. By disposing the thin film on the negative electrode current collector (21), for example, the deposition shape of the second negative electrode active material layer deposited between the thin film (24) and the first negative electrode active material layer (22) becomes flatter, and the cycle characteristics of the all-solid-state secondary battery (1) can be further improved. The thin film may be disposed, for example, between the first protective layer (23) and the first negative electrode active material layer (22), or between the first protective layer (23) and the negative electrode current collector (21).
[0112] The thickness of the thin film is, for example, 1 nm to 800 nm, 10 nm to 500 nm, or 50 nm to 100 nm. If the thickness of the thin film is less than 1 nm, it may be difficult for the thin film to function. If the thickness of the thin film is excessively thick, the content of lithium precipitated from the negative electrode layer (20) may decrease due to the thin film itself irreversibly absorbing lithium. As a result, the actual energy density of the all-solid-state secondary battery (1) may decrease, and the cycle characteristics of the all-solid-state secondary battery (1) may deteriorate. The thin film may be disposed on the negative electrode current collector (21) by, for example, a vacuum deposition method, a sputtering method, a plating method, or the like, but is not necessarily limited to these methods, and any method capable of forming a thin film in the relevant technical field may be used.
[0113] [Cathode layer: second cathode active material layer]
[0114] Although not shown in the drawing, the all-solid-state secondary battery (1) further includes a second negative electrode active material layer disposed, for example, between the solid electrolyte layer (30) and the negative electrode current collector (21) by charging. The second negative electrode active material layer may be disposed, for example, between the first negative electrode active material layer (22) and the first protective layer (23, 23a, 23b) and between the first negative electrode active material layer (22) and the solid electrolyte layer (30). The all-solid-state secondary battery (1) further includes a second negative electrode active material layer disposed, for example, between the first negative electrode active material layer (22) and the first protective layer (23, 23a, 23b). The all-solid-state secondary battery (1) further includes a second negative electrode active material layer disposed, for example, between the first negative electrode active material layer (22) and the solid electrolyte layer (30). The second negative electrode active material layer is deposited between the first negative electrode active material layer (22) and the first protective layer (23, 23a, 23b), for example, during the charging process of an all-solid-state secondary battery (1).
[0115] The second negative electrode active material layer is a metal layer containing lithium or a lithium alloy. The metal layer contains lithium or a lithium alloy. Therefore, since the second negative electrode active material layer is a metal layer containing lithium, it functions as, for example, a lithium reservoir. The lithium alloy includes, but is not limited to, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, etc., and any lithium alloy used in the art can be used. The second negative electrode active material layer can be made of one of these alloys or lithium, or made of several types of alloys. The second negative electrode active material layer is, for example, a plated layer.
[0116] The thickness of the second negative electrode active material layer is not particularly limited, but is, for example, 1 ㎛ to 200 ㎛, 1 ㎛ to 150 ㎛, 1 ㎛ to 100 ㎛, or 1 ㎛ to 50 ㎛. If the thickness of the second negative electrode active material layer is too thin, it is difficult for the second negative electrode active material layer to perform the role of a lithium reservoir. If the thickness of the second negative electrode active material layer is too thick, the mass and volume of the all-solid-state secondary battery (1) may increase, and the cycle characteristics may rather deteriorate. The second negative electrode active material layer may be, for example, a metal foil having a thickness within this range.
[0117] In the all-solid-state secondary battery (1), the second negative electrode active material layer is disposed, for example, between the negative electrode collector (21) and the solid electrolyte layer (30) before assembling the all-solid-state secondary battery (1), or is deposited between the negative electrode collector (21) and the solid electrolyte layer (30) by charging after assembling the all-solid-state secondary battery (1). In the all-solid-state secondary battery (1) in which the second negative electrode active material layer (23) is disposed between the negative electrode collector (21) and the solid electrolyte layer (30) before assembling the all-solid-state secondary battery (1), the second negative electrode active material layer is a metal layer containing lithium and thus functions as a lithium reservoir. For example, a lithium foil is disposed between the negative electrode collector (21) and the solid electrolyte layer (30) before assembling the all-solid-state secondary battery (1). As a result, the cycle characteristics of the all-solid-state secondary battery (1) including the second negative electrode active material layer are further improved. In an all-solid-state secondary battery (10) in which a second negative electrode active material layer is precipitated by charging, the energy density of the all-solid-state secondary battery (1) increases because the second negative electrode active material layer is not included when assembling the all-solid-state secondary battery (1). For example, when charging the all-solid-state secondary battery (1), the charging is performed in excess of the charging capacity of the first negative electrode active material layer (22). That is, the first negative electrode active material layer (22) is overcharged. At the beginning of charging, lithium is absorbed into the first negative electrode active material layer (22). The negative electrode active material included in the first negative electrode active material layer (22) forms an alloy or compound with lithium ions that have moved from the positive electrode layer (10). When charging exceeds the capacity of the first negative electrode active material layer (22), for example, lithium is deposited on the front and / or back surface of the first negative electrode active material layer (22), that is, between the first negative electrode active material layer (22) and the first protective layer (23, 23a, 23b) and / or between the first negative electrode active material layer (22) and the solid electrolyte layer (30), and a metal layer corresponding to the second negative electrode active material layer is formed by the deposited lithium. The second negative electrode active material layer is a metal layer mainly composed of lithium (i.e., metallic lithium). This result is obtained, for example, by the negative electrode active material included in the first negative electrode active material layer (22) including a material that forms an alloy or compound with lithium.During discharge, lithium in the first negative electrode active material layer (22) and the second negative electrode active material layer, i.e., the metal layer, is ionized and moves toward the positive electrode layer (10). Therefore, it is possible to use lithium as the negative electrode active material in the all-solid-state secondary battery (1). In addition, when the first negative electrode active material layer (22) is disposed between the solid electrolyte layer (30) and the second negative electrode active material layer, since the first negative electrode active material layer (22) covers the second negative electrode active material layer, it acts as a protective layer for the second negative electrode active material layer, i.e., the metal layer, and at the same time, it plays a role in suppressing the precipitation and growth of lithium dendrites. Therefore, short-circuiting and capacity reduction of the all-solid-state secondary battery (1) are suppressed, and as a result, the cycle characteristics of the all-solid-state secondary battery (1) are improved. In addition, when the second negative electrode active material layer is disposed by charging after assembling the all-solid-state secondary battery (1), the region between the negative electrode current collector (21) and the solid electrolyte layer (30) is a Li-free region that does not contain lithium (Li), for example, in the initial state or post-discharge state of the all-solid-state secondary battery.
[0118]
[0119] [Solid electrolyte layer]
[0120] [Solid electrolyte layer: sulfide-based solid electrolyte]
[0121] Referring to FIGS. 1 to 5, a solid electrolyte layer (30) is disposed between the anode layer (10) and the cathode layer (20). The solid electrolyte layer (30) includes a sulfide-based solid electrolyte.
[0122] The sulfide-based solid electrolyte included in the solid electrolyte layer (30) is, for example, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n, m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li3PS4, Li7P3S 11 , Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , at least one selected from 0≤x≤2. The sulfide-based solid electrolyte is manufactured by treating starting materials such as Li2S and P2S5 by a melting rapid cooling method or a mechanical milling method. In addition, heat treatment may be performed after the treatment. The solid electrolyte may be amorphous, crystalline, or a mixture thereof. In addition, the solid electrolyte may be, for example, one containing sulfur (S), phosphorus (P), and lithium (Li) as constituent elements among the above-described sulfide-based solid electrolyte materials. For example, the solid electrolyte may be a material containing Li2S-P2S5. When using a sulfide-based solid electrolyte material containing Li2S-P2S5 to form the solid electrolyte, the mixing molar ratio of Li2S and P2S5 is, for example, in the range of Li2S: P2S5= 50:50 to 90:10. The sulfide-based solid electrolyte may include, for example, an argyrodite type solid electrolyte represented by the following chemical formula A:
[0123] <Chemical Formula A>
[0124] Li + 12-n-x A n+ X 2- 6-x Y - x
[0125] In the above formula, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta, X is S, Se or Te, Y is Cl, Br, I, F, CN, OCN, SCN or N3, and 1(n(5, 0(x(2). The sulfide-based solid electrolyte is, for example, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , 0≤x≤2. The sulfide-based solid electrolyte may be, for example, an argyrodite-type compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I. The density of the argyrodite-type solid electrolyte may be 1.5 to 2.0 g / cc. Since the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and penetration of the solid electrolyte layer by Li can be effectively suppressed.
[0126] The elastic modulus of the sulfide-based solid electrolyte may be, for example, 40 GPa or less. The elastic modulus of the sulfide-based solid electrolyte may be, for example, 5 GPa to 40 GPa, 10 GPa to 40 GPa, or 15 GPa to 30 GPa.
[0127] The average particle size of the sulfide-based solid electrolyte particles included in the solid electrolyte layer (30) may be, for example, 1 um to 50 um, 3 um to 30 um, or 3 um to 20 um. When the sulfide-based solid electrolyte particles have an average particle size within this range, the cycle characteristics of the all-solid-state secondary battery can be further improved.
[0128] [Solid electrolyte layer: binder]
[0129] The solid electrolyte layer (30) may further include, for example, a binder. The binder included in the solid electrolyte layer (30) may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used in the relevant technical field may be used. The binder of the solid electrolyte layer (30) may be selected from among the binders included in the positive electrode active material layer (12). The binder may be omitted.
[0130] The binder included in the solid electrolyte layer may include, for example, a conductive binder and / or a non-conductive binder. The conductive binder may be, for example, an ion-conductive binder and / or an electron-conductive binder. A binder having both ion-conductive and electron-conductive properties may be classified as either an ion-conductive binder or an electron-conductive binder. The conductive binder refers to the first protective layer (23, 23a, 23b) described above.
[0131] The binder included in the solid electrolyte layer (30) may include, for example, a first binder. The first binder is, for example, a dry binder. A dry binder is, for example, a binder that is not impregnated, dissolved, or dispersed in a solvent. A dry binder is, for example, a binder that does not include or come into contact with a solvent.
[0132] The first binder is, for example, a fibrillated binder. The fibrillated binder can support a plurality of sulfide-based solid electrolyte particles and inorganic particles included in the solid electrolyte layer and serve as a fibrous matrix that binds them to each other. The fibrillated binder can be confirmed to have a fibrous form, for example, as shown in a scanning electron microscope image of a cross-section of an electrode. The fibrillated binder can have an aspect ratio of, for example, 10 or more, 20 or more, 50 or more, or 100 or more. The first binder is not necessarily limited to, but may include, for example, polytetrafluoroethylene (PTFE), a polyvinylidene fluoride-hexapropylene (PVDF-HFP) copolymer, and any fibrillated binder used in the manufacture of a dry composition. The first binder may particularly include a fluorinated binder. The fluorinated binder is, for example, polytetrafluoroethylene (PTFE).
[0133] The binder included in the solid electrolyte layer (30) may further include, for example, a second binder. The second binder is, for example, a dry binder. The description of the dry binder is the same as that of the first binder.
[0134] The second binder is, for example, a non-fibrillated binder. The non-fibrillated binder supports the sulfide-based solid electrolyte particles and inorganic particles included in the solid electrolyte layer and can serve as a binding site to bind them together. The non-fibrillated binder can be confirmed, for example, in a scanning electron microscope image of a cross-section of an electrode, to be arranged in a particle-like form rather than in a fibrous form. The non-fibrillated binder can have, for example, an aspect ratio of 5 or less, 3 or less, or 2 or less. The second binder may be, but is not limited to, any binder used in the manufacture of a dry electrode, such as, but not limited to, polyvinylidene fluoride (PVDF), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, cellulose, polyvinylpyrrolidone, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or copolymers thereof. The second binder may include, in particular, a fluorinated binder. The fluorinated binder is, for example, polyvinylidene fluoride (PVDF).
[0135] The content of the binder included in the solid electrolyte layer (30) is, for example, 1 wt% to 10 wt%, 1 wt% to 5 wt%, or 1 wt% to 3 wt% based on the total weight of the solid electrolyte layer. By including a binder in this content range in the solid electrolyte layer, the binding force of the solid electrolyte layer is improved, and the all-solid-state secondary battery can maintain a high energy density.
[0136] The solid electrolyte layer (30) is, for example, a self-standing film. The solid electrolyte layer can maintain a film form, for example, without a support. Therefore, the solid electrolyte layer can be prepared as a separate self-standing film and then placed between the anode layer and the cathode layer. The solid electrolyte layer can be free of, for example, a residual processing solvent. For example, since the solid electrolyte layer is manufactured by a dry process, it does not contain an intentionally added processing solvent. For example, it does not contain a residual processing solvent. Although a trace amount of unintended solvent may remain in the solid electrolyte layer, such solvent is not an intentionally added processing solvent. Therefore, the solid electrolyte layer is distinguished from a wet solid electrolyte layer manufactured by mixing sulfide-based solid electrolyte particles with a processing solvent and then drying to remove some or all of the processing solvent.
[0137]
[0138] [Anode layer]
[0139] [Anode layer: cathode active material]
[0140] Referring to FIGS. 1 to 5, the positive electrode active material layer (12) includes, for example, a positive electrode active material and a solid electrolyte. The solid electrolyte included in the positive electrode active material layer (12) may be selected from among the solid electrolytes included in the solid electrolyte layer (30). For details on the solid electrolyte, refer to the section on the solid electrolyte layer (30). The solid electrolyte may be omitted.
[0141] The cathode active material included in the cathode active material layer (12) is a cathode active material capable of reversibly absorbing and desorbing lithium ions. The cathode active material includes, for example, an oxide-based cathode active material, a sulfide-based cathode active material, or a combination thereof.
[0142] The oxide-based cathode active material includes, for example, a lithium transition metal oxide, a metal oxide, or a combination thereof. The lithium transition metal oxide includes, for example, lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt mangense oxide, lithium manganate, lithium iron phosphate, or a combination thereof. The lithium oxide includes, for example, iron oxide, vanadium oxide, or a combination thereof.
[0143] Sulfide-based cathode active materials include, for example, nickel sulfide, copper sulfide, Li2S, Li2S-containing complexes, or combinations thereof.
[0144] The oxide-based cathode active material may be, for example, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof. The oxide-based cathode active material may be, for example, Li. a A 1-b B' b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B' b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B' b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Lia Ni 1-b-c Co b B' c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B' c O 2-α F' α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B' c O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Mn b B' c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B' c O 2-α F' α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B' c O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d Ge O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); LiV2O5; LiI'O2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Fe2(PO4)3(0 ≤ f ≤ 2); may include a compound represented by any one of the chemical formulas of LiFePO4.
[0145] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B' is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F' is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I' is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0146] The oxide-based cathode active material may include, for example, a lithium transition metal oxide represented by the following chemical formulas 1 to 8:
[0147] <Chemical Formula 1>
[0148] Li a Ni x Co y M z O2-b A b
[0149] In the above chemical formula 1,
[0150] 1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0≤y≤0.3, 0 <z≤0.3, 및 x+y+z=1이고,
[0151] M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof,
[0152] A is F, S, Cl, Br or a combination thereof,
[0153] <Chemical Formula 2>
[0154] LiNi x Co y Mn z O2
[0155] <Chemical Formula 3>
[0156] LiNi x Co y Al z O2
[0157] In the above chemical formulas 2 and 3, 0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1이며,
[0158] <Chemical Formula 4>
[0159] LiNi x Co y Mn z Al w O2
[0160] In the above chemical formula 4, 0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1이며,
[0161] <Chemical Formula 5>
[0162] Li a Co x M y O 2-b Ab
[0163] In the above chemical formula 5,
[0164] 1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1,
[0165] M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof,
[0166] A is F, S, Cl, Br or a combination thereof,
[0167] <Chemical Formula 6>
[0168] Li a Ni x Mn y M' z O 2-b A b
[0169] In the above chemical formula 6,
[0170] 1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고,
[0171] M' is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof,
[0172] A is F, S, Cl, Br or a combination thereof,
[0173] <Chemical Formula 7>
[0174] Li a M1 x M2 y PO 4-b X b
[0175] In the above chemical formula 7, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며,
[0176] M1 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr) or a combination thereof,
[0177] M2 is magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y) or a combination thereof, and X is O, F, S, P or a combination thereof.
[0178] <Chemical Formula 8>
[0179] Li a M3 z PO4
[0180] In the above chemical formula 8, 0.90≤a≤1.1, 0.9≤z≤1.1,
[0181] M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.
[0182] The oxide-based cathode active material may be covered by a covering layer. The covering layer may be any material known as a covering layer for cathode active materials of all-solid-state secondary batteries. Examples of the covering layer include Li2O-ZrO2 (LZO).
[0183] The sulfide-based cathode active material may include, for example, a Li2S-containing composite. The Li2S-containing composite includes, for example, a composite of Li2S and carbon, a composite of Li2S and carbon and a solid electrolyte, a composite of Li2S and a solid electrolyte, a composite of Li2S and a metal carbide, a composite of Li2S and carbon and a metal carbide, a composite of Li2S and a metal nitride, a composite of Li2S and carbon and a metal nitride, a composite of Li2S and a metal, a composite of Li2S and a metal and carbon, or a combination thereof.
[0184] The Li2S and carbon complex comprises carbon. The carbon may be any material containing carbon atoms that is used as a conductive material in the art. The carbon may be, for example, crystalline carbon, amorphous carbon, or a combination thereof. The carbon may be, for example, a sintered product of a carbon precursor. The carbon may be, for example, a carbon nanostructure. The carbon nanostructure may be, for example, a one-dimensional carbon nanostructure, a two-dimensional carbon nanostructure, a three-dimensional carbon nanostructure, or a combination thereof. The carbon nanostructure may be, for example, a carbon nanotube, a carbon nanofiber, a carbon nanobelt, a carbon nanorod, graphene, graphene oxide (GO), reduced graphene oxide (rGO), graphene balls (GB), or a combination thereof. The carbon may be, for example, porous carbon or non-porous carbon. The porous carbon may include, for example, periodic and regular two-dimensional or three-dimensional pores. The porous carbon may be, for example, carbon black such as Ketjen black, acetylene black, Denka black, thermal black, channel black, etc.; graphite, activated carbon, or a combination thereof. The form of the carbon may be, for example, particle form, sheet form, flake form, etc., but is not limited thereto, and any method used as carbon in the art may be used. The method for preparing the composite of Li2S and carbon may be, for example, a dry method, a wet method, or a combination thereof, but is not limited thereto, and the method for preparing the composite of Li2S and carbon in the art may be, for example, milling, heat treatment, deposition, etc., but is not necessarily limited thereto, and any method used in the art may be used.
[0185] The composite of Li2S, carbon, and a solid electrolyte comprises carbon and a solid electrolyte. Carbon refers to the composite of Li2S and carbon described above. The solid electrolyte can be any material used as an ion-conducting material in the relevant technical field, for example. The solid electrolyte is, for example, an inorganic solid electrolyte. The solid electrolyte is, for example, a crystalline solid electrolyte, an amorphous solid electrolyte, or a combination thereof. The solid electrolyte is, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a lithium salt compound, or a combination thereof. The sulfide-based solid electrolyte comprises, for example, Li, S, and P, and may optionally further comprise a halogen element. The sulfide-based solid electrolyte can be selected from among the sulfide-based solid electrolytes used in the solid electrolyte layer. The sulfide-based solid electrolyte has, for example, a density of 1×10 at room temperature. -5 It can have an ionic conductivity of S / cm or more. Sulfide-based solid electrolytes include, for example, Li3PO4-Li2SO4, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z. m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x, may include one or more selected from 0≤x≤2. The oxide-based solid electrolyte includes, for example, Li, O, and a transition metal element, and may optionally further include other elements. The oxide-based solid electrolyte may include, for example, 1×10 at room temperature. -5 It may be a solid electrolyte having an ionic conductivity of S / cm or more. The oxide-based solid electrolyte may be selected from oxide-based solid electrolytes used in the solid electrolyte layer. The lithium salt compound is, for example, an inorganic compound. The solid electrolyte includes, for example, a lithium salt compound, and the lithium salt compound does not include, for example, a sulfur (S) atom. The lithium salt compound may be, for example, a binary compound composed of lithium and one element selected from Groups 13 to 17 of the Periodic Table of Elements. The binary compound may include, for example, one or more selected from LiF, LiCl, LiBr, LiI, LiH, Li2S, Li2O, Li2Se, Li2Te, Li3N, Li3P, Li3As, Li3Sb, LiI3, and LiB3. The lithium salt compound may be, for example, a ternary compound composed of lithium and two elements selected from Groups 13 to 17 of the Periodic Table of Elements. The ternary compound includes, for example, one or more selected from Li3OCl, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiNO3, Li2CO3, LiBH4, Li2SO4, Li3BO3, Li3PO4, Li4NCl, Li5NCl2 and Li3BN2. The lithium salt compound is particularly one or more lithium halide compounds selected from LiF, LiCl, LiBr and LiI. The solid electrolyte may be, for example, a mixture of a sulfide-based solid electrolyte and a lithium salt compound. For example, it may be a mixture of Li3PO4-Li2SO4 and a binary lithium salt compound or a mixture of Li3PO4-Li2SO4 and a ternary lithium salt compound.
[0186] The complex of Li2S and a solid electrolyte includes a solid electrolyte. The solid electrolyte refers to the solid electrolyte used in the complex of Li2S and carbon and a solid electrolyte described above. The complex of Li2S and a solid electrolyte includes, for example, a complex of Li2S and one or more lithium salts selected from LiF, LiCl, LiBr, LiI, LiH, Li2S, Li2O, Li2Se, Li2Te, Li3N, Li3P, Li3As, Li3Sb, LiI3, and LiB3.
[0187] The composite of Li2S and metal carbide includes metal carbide. The metal carbide is, for example, a two-dimensional metal carbide. The two-dimensional metal carbide is, for example, MXene. The two-dimensional metal carbide is, for example, M n+1 C n T x (M is a transition metal, T is a terminal group, T is O, OH and / or F, n=1, 2, or 3, and x is the number of terminal groups) is expressed as 2D metal carbides, for example, Ti2CT x , (Ti 0.5 , Nb 0.5 )2CT x , Nb2CT x , V2CT x , Ti3C2T x , (V 0.5 , Cr 0.5 )3C2T x , Ti3CNT x , Ta4C3T x , Nb4C3T x or a combination thereof. The surface of the two-dimensional metal carbide is terminated with O, OH and / or F.
[0188] The complex of Li2S, carbon, and metal carbide includes carbon and metal carbide. Carbon refers to the complex of Li2S and carbon described above. Metal carbide refers to the complex of Li2S and metal carbide described above.
[0189] The complex of Li2S and metal nitride includes a metal nitride. The metal nitride is, for example, a two-dimensional metal nitride. The two-dimensional metal nitride is, for example, M n+1 N n T x (M is a transition metal, T is a terminal group, T is O, OH and / or F, n=1, 2, or 3, and x is the number of terminal groups) is expressed as The surface of the two-dimensional metal nitride is terminated with O, OH and / or F.
[0190] A complex of Li2S, carbon, and a metal nitride includes carbon and a metal nitride. Carbon refers to the complex of Li2S and carbon described above. Metal carbide refers to the complex of Li2S and a metal nitride described above.
[0191] The shape of the positive electrode active material is, for example, a particle shape such as a sphere or an ellipse. The particle size of the positive electrode active material is not particularly limited and is within a range applicable to positive electrode active materials of a conventional all-solid-state secondary battery. The content of the positive electrode active material of the positive electrode layer (10) is also not particularly limited and is within a range applicable to positive electrode layers of a conventional all-solid-state secondary battery. The content of the positive electrode active material included in the positive electrode active material layer (12) may be, for example, 10 wt% to 99 wt%, 10 wt% to 90 wt%, 10 wt% to 80 wt%, 10 wt% to 70 wt%, or 10 wt% to 50 wt% of the total weight of the positive electrode active material layer (12).
[0192] [Anode layer: solid electrolyte]
[0193] The cathode active material layer (12) may further include, for example, a solid electrolyte. The cathode active material layer (12) may include an oxide-based solid electrolyte or a sulfide-based solid electrolyte.
[0194] The solid electrolyte included in the cathode active material layer (12) may be a sulfide-based solid electrolyte. For details on the sulfide-based solid electrolyte, refer to the section on the solid electrolyte layer (30).
[0195] The solid electrolyte included in the cathode active material layer (12) may be an oxide-based solid electrolyte. The oxide-based solid electrolyte may be, for example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12A garnet-type solid electrolyte selected from (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10).
[0196] The solid electrolyte included in the positive electrode active material layer (12) may have a smaller particle size than the solid electrolyte included in the solid electrolyte layer (30). For example, the particle size of the solid electrolyte included in the positive electrode active material layer (12) may be 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the particle size of the solid electrolyte included in the solid electrolyte layer (30). The particle size of the solid electrolyte is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of particles corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by, for example, laser diffraction.
[0197] [Anode layer: binder]
[0198] The cathode active material layer (12) may include a binder. The binder may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used in the relevant technical field may be used.
[0199] [Anode layer: conductive material]
[0200] The cathode active material layer (12) may include a conductive material. The conductive material may include, but is not limited to, graphite, carbon black, acetylene black, Ketjen black, carbon fiber, metal powder, etc., and any conductive material used in the relevant technical field may be used.
[0201] [Anode layer: Other additives]
[0202] The cathode active material layer (12) may further include additives such as fillers, coating agents, dispersants, and ion conductive aids in addition to the cathode active material, solid electrolyte, binder, and conductive agent described above.
[0203] As fillers, coating agents, dispersants, ion conductivity aids, etc. that the positive electrode active material layer (12) may include, known materials generally used in electrodes of all-solid-state secondary batteries may be used.
[0204] [Anode layer: Anode current collector]
[0205] The positive electrode collector (11) uses a plate or foil made of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel (SUS), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode collector (11) may be omitted. The thickness of the positive electrode collector (11) is, for example, 1 µm to 100 µm, 1 µm to 50 µm, 5 µm to 25 µm, or 10 µm to 20 µm.
[0206] The cathode current collector (11) is not shown in the drawing, but may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may melt when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. In particular, the metal layer may include, for example, aluminum (Al), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni) or an alloy thereof. The metal layer may act as an electrochemical fuse and may be cut off in the event of an overcurrent to prevent a short circuit. The limit current and the maximum current may be controlled by adjusting the thickness of the metal layer. The metal layer may be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or the maximum current of the positive electrode current collector (11) decrease, thereby improving the stability of the lithium battery in the event of a short circuit. A lead tab may be added on the metal layer for connection to the outside. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. When welding, the base film and / or the metal layer may be melted, so that the metal layer may be electrically connected to the lead tab.In order to make the welding between the metal layer and the lead tab more robust, a metal chip may be added between the metal layer and the lead tab. The metal chip may be a thin piece of the same material as the metal of the metal layer. The metal chip may be, for example, a metal foil, a metal mesh, etc. The metal chip may be, for example, copper foil, nickel foil, etc. By placing the metal chip on the metal layer and then welding it with the lead tab, the lead tab may be welded to the metal chip / metal layer laminate or the metal chip / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal chip may melt, so that the metal layer or the metal layer / metal chip laminate may be electrically connected to the lead tab. The metal chip and / or the lead tab may be added to a portion of the metal layer. The thickness of the base film may be, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. By having a thickness of the base film in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film can be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. By having a melting point in this range, the base film can be melted during the process of welding the lead tab and easily bonded to the lead tab. A surface treatment, such as corona treatment, can be performed on the base film to improve the adhesion between the base film and the metal layer. The thickness of the metal layer can be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to μm. By having a thickness of the metal layer in this range, conductivity can be maintained while ensuring the stability of the electrode assembly. The thickness of the metal piece can be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. By having the metal piece in this range of thickness, the connection between the metal layer and the lead tab can be performed more easily.By having this structure, the positive electrode collector (11) can reduce the weight of the positive electrode and consequently improve the energy density of the all-solid-state secondary battery.
[0207]
[0208] [Anode layer: inert member]
[0209] Referring to FIGS. 3 to 5, the positive electrode (10) includes a positive electrode current collector (11), a positive electrode active material layer (12) disposed on one side of the positive electrode current collector, and further includes an inactive member (40, 40a, 40b) disposed on one side of the positive electrode layer (10).
[0210] By including the inert member (40), cracking of the solid electrolyte layer (30) is prevented during the manufacture and / or charging and discharging of the all-solid-state secondary battery (1), and as a result, the cycle characteristics of the all-solid-state secondary battery (2) are improved. In the all-solid-state secondary battery (1) that does not include the inert member (40), when the manufacture and / or charging and discharging of the all-solid-state secondary battery (1) is performed, uneven pressure is applied to the solid electrolyte layer (30) in contact with the positive electrode (10), which increases the possibility of cracking in the solid electrolyte layer (30) and causing a short circuit due to the growth of lithium metal through the crack.
[0211] An inert member (40) is disposed along the side surface of the positive electrode layer (10) to surround the positive electrode layer. The inert member (40) surrounds, for example, part or all of the side surface of the positive electrode (10) and is in contact with the solid electrolyte layer (30). By the inert member (40) surrounding the side surface of the positive electrode (10) and being in contact with the solid electrolyte layer (30), cracks in the solid electrolyte layer (30) that occur due to a pressure difference during the pressing process in the solid electrolyte layer (30) that is not in contact with the positive electrode (20) can be effectively suppressed. The inert member (40) surrounds the side surface of the positive electrode (10) and is separated from the negative electrode (20), more specifically, the first negative electrode active material layer (22). The inert member (40) surrounds the side surface of the positive electrode (10), is in contact with the solid electrolyte layer (30), and is separated from the negative electrode (20). Accordingly, the possibility of a short circuit occurring due to physical contact between the positive electrode (10) and the first negative electrode active material layer (22) or due to overcharging of lithium, etc., is suppressed. Referring to FIG. 3, an inert member (40) is disposed on one side of the positive electrode active material layer (12) and simultaneously on one side of the positive electrode current collector (11), thereby more effectively suppressing the possibility of a short circuit occurring due to contact between the positive electrode current collector (11) and the negative electrode (20). Alternatively, referring to FIG. 4, the inert member (40) is disposed on one side of the positive electrode active material layer (12) and between the solid electrolyte layer (40) and the positive electrode current collector (11) facing the solid electrolyte layer (40). The inert member (40) is not disposed on one side of the positive electrode current collector (11). By placing an inert member (40) between the positive electrode collector (11) and the solid electrolyte layer (30), a short circuit caused by contact between the positive electrode collector (11) and the negative electrode (20) can be effectively prevented.
[0212] Although not shown in the drawing, some or all of the inert members (40, 40a, 40b) may be arranged spaced apart from the side surface of the positive electrode layer (10). By arranging some or all of the inert members (40, 40a, 40b) spaced apart from the side surface of the positive electrode layer (10), the manufacturing process of the all-solid-state secondary battery (1) may be facilitated and the manufacturing speed of the all-solid-state secondary battery (1) may be increased. By arranging some or all of the inert members (40, 40a, 40b) spaced apart from the side surface of the positive electrode layer (10), the volume change in the side surface direction of the positive electrode layer (10) during charge and discharge may be more effectively accommodated, thereby further improving the life characteristics of the all-solid-state secondary battery (1). The distance between the side of the inert member (40, 40a, 40b) and the anode layer (10) is independently, for example, 0.1 µm to 10 mm, 1 µm to 1 mm, 1 µm to 500 µm, 1 µm to 100 µm, 1 µm to 50 µm or 1 µm to 10 µm.
[0213] The inert member (40) may further include a position determining unit (not shown) configured to determine the position of the inert member (40) on the solid electrolyte layer (30). Since the inert member (40) includes the position determining unit, the position at which the inert member (40) is placed on the solid electrolyte layer (30) can be easily determined. As a result, the manufacturing speed of the all-solid-state secondary battery (1) can be increased and the ease of manufacturing can be improved.
[0214] Referring to FIGS. 3 and 4, the inert member (40) extends from one side of the positive electrode (30) to the end of the solid electrolyte layer (30). By extending the inert member (40) to the end of the solid electrolyte layer (30), cracks occurring at the end of the solid electrolyte layer (30) can be suppressed. The end of the solid electrolyte layer (30) is the outermost part that is in contact with the side of the solid electrolyte layer (30). The inert member (40) extends to the outermost part that is in contact with the side of the solid electrolyte layer (30). The inert member (40) is separated from the negative electrode layer (20), more specifically, from the first negative electrode active material layer (22). The inert member (40) extends to the end of the solid electrolyte layer (30), but does not contact the negative electrode layer (20). The inert member (40) fills a space extending from, for example, one side of the anode layer (30) to the end of the solid electrolyte layer (30).
[0215] The inert member (40) may be, for example, a gasket. By using a gasket as the inert member (40), cracks in the solid electrolyte layer (30) caused by a pressure difference during the pressing process can be effectively suppressed.
[0216] The inert member (40) has, for example, a single-layer structure. Alternatively, although not shown in the drawing, the inert member (40) may have a multi-layer structure. In the inert member (40) having a multi-layer structure, each layer may have a different composition. The inert member having a multi-layer structure may have, for example, a two-layer structure, a three-layer structure, a four-layer structure, or a five-layer structure. The inert member (40) having a multi-layer structure may include, for example, one or more adhesive layers and one or more support layers. The adhesive layer effectively prevents, for example, a separation between the positive electrode layer (10) and the solid electrolyte layer (30) due to a change in the volume of the positive electrode layer (10) that occurs during the charge / discharge process of the all-solid-state secondary battery (10), and improves the film strength of the inert member (40) by providing a bonding force between the support layer and other layers. The support layer provides support to the inert member (40), prevents unevenness of pressure applied to the solid electrolyte layer (30) during the pressurization process or the charge / discharge process, and prevents deformation of the all-solid-state secondary battery (1) being manufactured.
[0217] Referring to FIG. 5, the all-solid-state secondary battery (1) includes a positive electrode (10), a negative electrode (20), and a solid electrolyte layer (30, 30a, 30b) disposed therebetween, and the positive electrode layer (10) includes a positive electrode current collector (11) and a first positive electrode active material layer (12a) and a second positive electrode active material layer (12b) disposed on both sides of the positive electrode current collector (11), and the solid electrolyte layer (30) includes a first solid electrolyte layer (30a) in contact with the first positive electrode active material layer (12a) and a second solid electrolyte layer (30b) in contact with the second positive electrode active material layer (12b), and the negative electrode layer (20) includes a first negative electrode layer (20a) in contact with the first solid electrolyte layer (30a) and a second negative electrode layer (20b) in contact with the second solid electrolyte layer (30b), respectively, and an inert A member (40) is arranged to surround the side surface of the positive electrode layer (10) between the first solid electrolyte layer (30a) and the second solid electrolyte layer (30b) which face each other. The inert member (40) includes, for example, a first inert member (50a) which contacts the first solid electrolyte layer (30a) and a second inert member (40b) which contacts the second solid electrolyte layer (30b). Therefore, the all-solid-state secondary battery (1) has a bi-cell structure. Since the all-solid-state secondary battery (1) has such a bi-cell structure, the solid electrolyte layer (30) and the negative electrode layer (20) are arranged symmetrically to face each other with the positive electrode layer (10) as the center, so that structural deformation due to pressure applied during the manufacture of the all-solid-state secondary battery (1) is more effectively suppressed. Accordingly, cracking of the solid electrolyte layer (30) is suppressed during the manufacturing process and / or the charging / discharging process of the all-solid-state secondary battery (1), thereby preventing short circuit of the all-solid-state secondary battery (1), and consequently further improving the cycle characteristics of the all-solid-state secondary battery (1). In addition, since only one positive electrode collector (11) is used for a plurality of positive electrode active material layers (12a, 12b), the energy density of the all-solid-state secondary battery (1) is increased.
[0218] Referring to FIGS. 3 to 5, the inert member (40) is, for example, a flame-retardant inert member. The flame-retardant inert member provides flame retardancy, thereby preventing thermal runaway and ignition of the all-solid-state secondary battery (1). Consequently, the safety of the all-solid-state secondary battery (1) is further improved. The flame-retardant inert member absorbs residual moisture within the all-solid-state secondary battery (1), thereby preventing deterioration of the all-solid-state secondary battery (1), thereby improving the lifespan characteristics of the all-solid-state secondary battery (1).
[0219] The flame-retardant inert member includes, for example, a matrix and a filler. The matrix includes, for example, a substrate and a reinforcing material. The matrix includes, for example, a fibrous substrate and a fibrous reinforcing material. Since the matrix includes the substrate, the matrix can have elasticity. Therefore, the matrix can effectively accommodate a change in volume during charging and discharging of the all-solid-state secondary battery (1) and can be arranged at various positions. The substrate included in the matrix includes, for example, a first fibrous material. Since the substrate includes the first fibrous material, the volume change of the positive electrode layer (30) occurring during the charging and discharging process of the all-solid-state secondary battery (1) can be effectively accommodated and deformation of the first inert member (40) caused by the change in volume of the positive electrode layer (30) can be effectively suppressed. The first fibrous material is, for example, a material having an aspect ratio of 5 or more, 20 or more, or 50 or more. The first fibrous material is, for example, a material having an aspect ratio of 5 to 1000, 20 to 1000, or 50 to 1000. The first fibrous material is, for example, an insulating material. Since the first fibrous material is an insulating material, a short circuit between the positive electrode layer (30) and the negative electrode layer (20) caused by lithium dendrites, etc., generated during the charge and discharge process of the all-solid-state secondary battery (1) can be effectively prevented. The first fibrous material includes, for example, at least one selected from pulp fibers, insulating polymer fibers, and ion-conductive polymer fibers. The strength of the matrix is improved by the inclusion of a reinforcing material in the matrix. Therefore, the matrix can prevent excessive volume change during charge and discharge of the all-solid-state secondary battery (1) and deformation of the all-solid-state secondary battery. The reinforcing material included in the matrix includes, for example, a second fibrous material. Since the reinforcing material includes the second fibrous material, the strength of the matrix can be increased more uniformly. The second fibrous material is, for example, a material having an aspect ratio of 3 or more, 5 or more, or 10 or more.The first fibrous material is, for example, a material having an aspect ratio of 3 to 100, 5 to 100, or 10 to 100. The second fibrous material is, for example, a flame-retardant material. Since the second fibrous material is a flame-retardant material, ignition due to thermal runaway occurring during the charge / discharge process of the all-solid-state secondary battery (1) or due to external impact can be effectively suppressed. The second fibrous material is, for example, glass fiber, metal oxide fiber, ceramic fiber, etc.
[0220] The flame-retardant inert member includes a filler in addition to a matrix. The filler may be disposed within the matrix, on the surface of the matrix, or on both the interior and the surface. The filler is, for example, an inorganic material. The filler included in the flame-retardant inert member is, for example, a moisture getter, a flame retardant, or a lithium immobilizer. The moisture getter removes moisture remaining in the all-solid-state secondary battery (1) by adsorbing moisture, for example, at a temperature below 100°C, thereby preventing deterioration of the all-solid-state secondary battery (1). In addition, when the temperature of the all-solid-state secondary battery (1) increases to 150°C or higher due to thermal runaway occurring during the charge / discharge process of the all-solid-state secondary battery (1) or an external impact, the moisture getter releases the adsorbed moisture, thereby effectively suppressing ignition of the all-solid-state secondary battery (1). The moisture getter is, for example, a metal hydroxide having moisture adsorption properties. The metal hydroxide included in the filler is, for example, Mg(OH)2, Fe(OH)3, Sb(OH)3, Sn(OH)4, TI(OH)3, Zr(OH)4, Al(OH)3, or a combination thereof. The flame retardant includes, for example, at least one selected from zinc borate, calcium molybdate zinc complex, MoO3, (NH4)2Mo2O7, Sb2O3, and Sb3O5. The lithium fixing agent may be, for example, a compound that reacts with liquid lithium to fixate lithium at a lithium melting temperature of 180°C or higher. The lithium fixing agent may react with liquid lithium to change lithium into another insoluble compound, for example. The lithium fixing agent is, for example, a metal oxide that is reactive with liquid lithium. The metal oxide included in the filler is, for example, TiO2, ZrO2, HfO2, ThO2, or a combination thereof. Metal oxides react with liquid lithium, for example, to produce Li2O and the metal.For example, the reaction formula is 4Li + MO2-> M + 2Li2O. Liquid lithium is fixed by reacting with a metal oxide to produce lithium oxide. Leakage of molten liquid lithium to the cathode at high temperatures can be suppressed. Therefore, the safety of all-solid-state secondary batteries can be improved.
[0221] The content of the filler included in the flame-retardant inert member is, for example, 1 to 80 parts by weight, 5 to 80 parts by weight, 10 to 80 parts by weight, 20 to 80 parts by weight, 30 to 80 parts by weight, 40 to 80 parts by weight, 50 to 80 parts by weight, 60 to 80 parts by weight, or 65 to 80 parts by weight, based on 100 parts by weight of the flame-retardant inert member (4).
[0222] The flame-retardant inert member may further comprise, for example, a binder. The binder may comprise, for example, a curable polymer or a non-curable polymer. A curable polymer is a polymer that cures by heat and / or pressure. A curable polymer is, for example, a solid at room temperature. The flame-retardant inert member may comprise, for example, a thermo-pressure curable film and / or a cured product thereof. An example of a thermo-pressure curable polymer is TSA-66 from Toray.
[0223] The flame-retardant inert member may additionally include other materials in addition to the above-described substrate, reinforcing material, filler, and binder. The flame-retardant inert member may further include one or more selected from among paper, an insulating polymer, an ion-conducting polymer, an insulating inorganic material, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte. The insulating polymer may be, for example, an olefin-based polymer such as polypropylene (PP) or polyethylene (PE).
[0224] The density of the substrate or reinforcing material included in the flame-retardant inert material may be, for example, 10% to 300%, 10% to 150%, 10% to 140%, 10% to 130%, or 10% to 120% of the density of the positive electrode active material included in the lithium host layer (22).
[0225] The inert member (40) is a member that does not contain an electrochemically active material, for example, an electrode active material. The electrode active material is a material that absorbs / releases lithium. The inert member (40) is a member made of a material other than the electrode active material and used in the relevant technical field.
[0226]
[0227] [Manufacturing of all-solid-state secondary batteries]
[0228] (Cathode layer manufacturing)
[0229] A method for manufacturing a negative electrode layer includes, for example, a step of providing a negative electrode current collector; and a step of sequentially providing a first protective layer and a first negative electrode active material layer, wherein the first negative electrode active material layer includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix, the carbon-based material matrix includes a first carbon-based nanostructure, and the first protective layer includes a second carbon-based nanostructure.
[0230] A negative electrode current collector is provided. For specific details on the negative electrode current collector, refer to the negative electrode current collector section described above.
[0231] The step of sequentially providing a first protective layer and a first negative electrode active material layer includes, for example, a step of providing a negative electrode active material precursor on a negative electrode current collector; and a step of supplying a reaction gas including a carbon source gas to the negative electrode current collector on which the negative electrode active material precursor has been provided and performing a heat treatment. In the heat treatment step, a negative electrode active material is formed from the negative electrode active material precursor, a second carbon-based nanostructure grows between the negative electrode current collector and the negative electrode active material through a gas phase reaction to form a first protective layer, and a first carbon-based nanostructure grows on the negative electrode active material through a gas phase reaction to form a first negative electrode active material layer.
[0232] The step of providing a negative electrode active material precursor on the negative electrode current collector includes, for example, providing a precursor compound including a metal that forms an alloy or compound with lithium on the negative electrode current collector. The negative electrode active material precursor may be provided in a dry or wet manner. For example, a solution in which the negative electrode active material precursor is dissolved may be coated on the negative electrode current collector and then dried to place the negative electrode active material precursor on the negative electrode current collector. The metal that forms an alloy or compound with lithium includes gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), zinc (Zn), or a combination thereof. Precursor compounds containing a metal that forms an alloy or compound with lithium include, but are not limited to, nitrates of metals that form an alloy or compound with lithium, halogen salts of metals that form an alloy or compound with lithium, phosphates of metals that form an alloy or compound with lithium, sulfates of metals that form an alloy or compound with lithium, etc., and any compound that can be used as a precursor compound in the relevant technical field is possible. Precursor compounds containing silver (Ag) include, but are not limited to, silver nitrate (AgNO3), silver acetate (CH3COOAg), and diamine silver chloride (Ag(NH3)2Cl). Solvents that dissolve the precursor compounds include, but are not limited to, water, alcohol, etc. Alcohols include, but are not limited to, methanol, ethanol, etc.
[0233] Next, a reaction gas containing a carbon source gas is supplied to the negative electrode current collector provided with the negative electrode active material precursor and heat-treated. The carbon source gas may further include one or more inert gases selected from the group consisting of nitrogen, helium, and argon, for example.
[0234] The carbon source gas is a compound represented by the following chemical formula 9, a compound represented by the following chemical formula 10, a compound represented by the following chemical formula 11, or a mixed gas of two or more selected from a compound represented by the following chemical formula 9, a compound represented by the following chemical formula 10, and a compound represented by the following chemical formula 11.
[0235] <Chemical Formula 9>
[0236] C n H 2n+2
[0237] In the above chemical formula 9, n is 1 to 20;
[0238] <Chemical Formula 10>
[0239] C n H 2n
[0240] In the above chemical formula 10, n is 2 to 6,
[0241] <Chemical Formula 11>
[0242] C n H n
[0243] In the above chemical formula 11, n is 2 to 6.
[0244] The compound represented by chemical formula 9, the compound represented by chemical formula 10, and the compound represented by chemical formula 11 are at least one selected from the group consisting of, for example, methane, acetylene, ethylene, and propylene.
[0245] After the step of supplying a reaction gas containing a carbon source gas to the negative electrode current collector provided with the negative electrode active material precursor and performing a heat treatment, a cooling step using one or more inert gases selected from the group consisting of nitrogen, helium, and argon may be further performed. The cooling step refers to a step of adjusting the temperature to room temperature (20-25°C).
[0246] In the method for manufacturing a cathode layer, the process of growing carbon nanostructures according to a gas phase reaction to form a first protective layer and a first cathode active material layer can be performed under various conditions.
[0247] According to the first condition, for example, methane is first supplied to a reactor in which a negative electrode current collector provided with a negative electrode active material precursor is placed, and the temperature is increased to a heat treatment temperature (T). The heating time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 500 to 1100°C. The heat treatment is performed for the reaction time at the heat treatment temperature (T). The reaction time is, for example, 10 minutes to 8 hours. The heat-treated resultant is cooled to room temperature to manufacture a negative electrode layer. The time for the cooling process from the heat treatment temperature (T) to room temperature is, for example, 10 minutes to 5 hours.
[0248] According to the second condition, for example, hydrogen is first supplied to a reactor in which a negative electrode current collector provided with a negative electrode active material precursor is placed, and the temperature is increased to a heat treatment temperature (T). The heating time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 500 to 1100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), methane gas is supplied, and heat treatment is performed for the remaining reaction time. The reaction time is, for example, 10 minutes to 8 hours. The heat-treated resultant is cooled to room temperature to manufacture a negative electrode layer. Nitrogen is supplied during the cooling process. The time taken for the cooling process from the heat treatment temperature (T) to room temperature is, for example, 10 minutes to 5 hours.
[0249] According to the third condition, for example, hydrogen is first supplied to a reactor in which a negative electrode current collector provided with a negative electrode active material precursor is placed, and the temperature is increased to a heat treatment temperature (T). The heating time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 500 to 1100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), a mixed gas of methane and hydrogen is supplied, and heat treatment is performed for the remaining reaction time. The reaction time is, for example, 10 minutes to 8 hours. The heat-treated resultant is cooled to room temperature to manufacture a composite. Nitrogen is supplied during the cooling process. The time taken for the cooling process from the heat treatment temperature (T) to room temperature is, for example, 10 minutes to 5 hours.
[0250] The carbon source gas is, for example, methane; acetylene; a mixture containing methane and an inert gas; or a mixture containing acetylene and an inert gas.
[0251] The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas may not contain an inert gas such as nitrogen. The carbon source gas is, for example, a mixture of acetylene and nitrogen. In the mixture of acetylene and nitrogen, the molar ratio of acetylene to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas may not contain an inert gas such as nitrogen.
[0252] The heat treatment pressure can be selected by considering the heat treatment temperature, the composition of the gas mixture, and the required thickness of the cathode layer. The heat treatment pressure can be controlled by adjusting the amount of the incoming and outgoing gas mixtures. The heat treatment pressure can be, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more.
[0253] The heat treatment time is not particularly limited and can be appropriately adjusted depending on the heat treatment temperature, the pressure during the heat treatment, the composition of the gas mixture, and the required thickness of the cathode layer. For example, the reaction time at the heat treatment temperature is, for example, 10 minutes to 100 hours, 30 minutes to 90 hours, or 50 minutes to 40 hours. As the heat treatment time increases, the content of the growing carbon nanostructures increases, and thus the electrochemical properties of the manufactured cathode layer can be improved. However, this trend may not necessarily be directly proportional to time. For example, after a certain period of time, the growth of the carbon nanostructures may no longer occur or the growth rate may decrease.
[0254] (Manufacturing of solid electrolyte layer)
[0255] The solid electrolyte layer can be manufactured by a dry or wet method.
[0256] A method for manufacturing a solid electrolyte layer according to a dry process includes the steps of preparing a dry mixture by dry mixing a sulfide-based solid electrolyte and a binder; the step of preparing a solid electrolyte layer by molding the dry mixture; and the step of arranging the solid electrolyte layer between an anode layer and a cathode layer, wherein the average particle diameter of the inorganic particles is 50 nm to 5 ㎛ or less.
[0257] First, a sulfide-based solid electrolyte and a binder are mixed to prepare a dry mixture. Dry mixing refers to mixing without a process solvent. A dry mixture refers to a mixture to which a process solvent is not intentionally added. A process solvent is, for example, a solvent used in the preparation of an electrode slurry. The binder is, for example, a dry binder. A dry binder refers to a binder that does not contain a process solvent. The process solvent is, for example, water, NMP, etc., but is not limited thereto, and is not limited to any process solvent used in the preparation of an electrode slurry. Dry mixing can be performed using a stirrer at a temperature of, for example, 25 to 85°C or 65 to 85°C. Dry mixing can be performed using a stirrer at a rotation speed of, for example, 10 to 10,000 rpm or 100 to 10,000 rpm. Dry mixing can be performed using a stirrer for, for example, 1 to 200 minutes. Dry mixing can be performed one or more times, for example. A dry mixture comprising a fibrillated dry binder can be obtained by dry mixing. The agitator is, for example, a mixer or a kneader. The agitator includes, for example, a chamber; one or more rotating shafts disposed inside the chamber and rotating; and blades rotatably coupled to the rotating shaft and disposed in the longitudinal direction of the rotating shaft. The blades can be, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersing blade, and a screw blade. By including the blades, an electrode active material, a dry conductive material, and a dry binder can be effectively mixed without a solvent to produce a dough-like mixture.
[0258] Next, a solid electrolyte layer can be prepared by molding a dry mixture. The prepared dry mixture can be extruded into a sheet form, for example, by feeding it into an extrusion device. The pressure during extrusion is, for example, 4 MPa to 100 MPa, or 10 MPa to 90 MPa. The obtained mixture can be in a sheet form. That is, the obtained mixture in a sheet form can be a solid electrolyte layer. The extrusion device can be, for example, a roller or an extruder. The type and content of the sulfide-based solid electrolyte and the binder refer to the solid electrolyte layer section described above. The binder can be omitted. For example, since the sulfide-based solid electrolyte particles are partially sintered by pressurization, the binder can be omitted.
[0259] A method for manufacturing a solid electrolyte layer according to a wet process includes the steps of preparing a slurry by mixing a sulfide-based solid electrolyte, a binder, and a solvent; the step of forming and drying the slurry to prepare a solid electrolyte layer; and the step of arranging the solid electrolyte layer between an anode layer and a cathode layer.
[0260] First, a slurry is prepared by mixing a sulfide-based solid electrolyte, a binder, and a solvent. The sulfide-based solid electrolyte and binder refer to the solid electrolyte layer section described above. The binder may be the same as or different from the binder used in the dry method. The binder used in the solid electrolyte layer is not limited to, but is not limited to, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., and any binder used in the art may be used. The solvent is not particularly limited and any solvent that does not react with the sulfide-based solid electrolyte and can dissolve the binder may be used. The solvent may be, for example, octyl acetate.
[0261] Next, the slurry is molded and dried to prepare a solid electrolyte layer. The slurry can be applied to a substrate, dried, and then separated from the substrate to prepare a solid electrolyte layer. The application method and drying conditions can be performed within the range of methods and / or conditions commonly used in the art.
[0262] Next, a solid electrolyte layer is placed between the anode layer and the cathode layer. The solid electrolyte layer can be placed on the anode layer and / or the cathode layer after preparing a separate solid electrolyte layer as described above, or can be placed by applying and drying a slurry on the anode layer and / or the cathode layer.
[0263] (Anode layer manufacturing)
[0264] The anode layer can be manufactured by wet or dry process.
[0265] The positive electrode layer can be manufactured, for example, by a wet process. A positive electrode slurry is prepared by mixing a positive electrode active material, a sulfide-based solid electrolyte, a conductive agent, a binder, and a solvent. The positive electrode slurry is coated on a positive electrode current collector and then dried to prepare a positive electrode layer. The solvent used in the manufacture of the positive electrode slurry is not particularly limited, and any solvent used in positive electrode slurry in the art can be used. The solvent used in the positive electrode slurry is, for example, para-xylene. The types and contents of the positive electrode collector, positive electrode active material, conductive agent, and binder refer to the positive electrode layer section described above.
[0266] The positive electrode layer can be manufactured, for example, by a dry method. First, a positive electrode active material, a sulfide-based solid electrolyte, a conductive agent, and a binder are dry-mixed to prepare a dry mixture. Next, the dry mixture is molded to prepare a positive electrode active material layer. Subsequently, the prepared positive electrode active material layer is placed on one or both sides of a positive electrode current collector and pressed to prepare a positive electrode layer. The binder is, for example, a dry binder. The specific manufacturing conditions and methods in the step of preparing the dry mixture and the step of molding the dry mixture are substantially the same as the method for manufacturing the solid electrolyte layer described above. The types and contents of the positive electrode collector, positive electrode active material, conductive agent, and binder refer to the above-described positive electrode layer section.
[0267] (Manufacturing of all-solid-state secondary batteries)
[0268] All-solid-state secondary batteries can be manufactured, for example, as follows.
[0269] First, an electrode assembly is provided, which includes an anode layer; a cathode layer; and a solid electrolyte layer disposed between the anode layer and the cathode layer.
[0270] A solid electrolyte layer is placed on the negative electrode layer so that the negative electrode active material layer is in contact with the solid electrolyte layer, thereby preparing a negative electrode layer / solid electrolyte layer laminate. Next, the solid electrolyte layer is placed on one or both sides of the positive electrode layer so that it faces the positive electrode active material layer, thereby preparing a negative electrode layer / solid electrolyte layer / positive electrode layer laminate. A gasket, which is an inert member that surrounds the side surface of the positive electrode layer, is placed around the positive electrode layer. The prepared negative electrode layer / solid electrolyte layer / positive electrode layer laminate is 50 to 100 o The solid electrolyte layer is partially sintered at a pressure of 300 to 600 MPa at C for 10 to 60 minutes (plate press). This pressurization process improves battery characteristics by providing the pressed laminate as an electrode assembly. The electrode assembly is sealed with a sealant to complete the all-solid-state secondary battery.
[0271]
[0272] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0273] Example 1: Methane 950-1100℃, horizontally aligned graphene layer (first protective layer) / Ag embedded horizontally aligned graphene layer (first negative electrode active material layer), mono-cell all-solid-state secondary battery
[0274] (Manufacturing of solid electrolyte layer, dry)
[0275] Li6PS5Cl sulfide solid electrolyte in the form of argyrodite crystals (D 50 = 10 (m, crystalline), 1 part by weight of polytetrafluoroethylene (PTFE) first binder and 1 part by weight of polyvinylidene fluoride (PVDF) second binder were added to 98 parts by weight of the solid electrolyte in a grinder mixer and mixed to prepare a mixture. The prepared mixture was added to a mortar heated to 80°C and stirred to prepare a dough. The prepared dough was passed through a roller to form a sheet to prepare a solid electrolyte membrane of a certain thickness. A solid electrolyte layer was manufactured by the above process. The elastic modulus of the sulfide-based solid electrolyte layer was about 15 GPa to 30 GPa.
[0276] (Cathode layer manufacturing)
[0277] A negative electrode was prepared by sequentially depositing a carbon layer as a first protective layer and a carbon layer containing a negative electrode active material as a first negative electrode active material layer on one side of a 20 ㎛ thick stainless steel (SUS304) thin film.
[0278] The first protective layer and the first negative electrode active material layer were formed by the following method.
[0279] A composition containing Ag precursor compound was prepared by dissolving AgNO3 as an Ag precursor compound in methanol as an organic solvent.
[0280] A composition containing a Ag precursor compound was coated on a stainless steel (SUS304) thin film, and then the organic solvent was removed to prepare a stainless steel (SUS304) thin film coated with a Ag precursor compound.
[0281] After placing a stainless steel (SUS304) thin film coated with a Ag precursor compound in a chamber, the temperature was raised to 1000°C while supplying a mixture of methane gas as a hydrocarbon gas and argon gas as an inert gas, thereby growing horizontally aligned graphene on the stainless steel (SUS304) thin film.
[0282] When the temperature inside the chamber is above 400°C, Ag ions are reduced to Ag particles, and graphene is horizontally arranged on a stainless steel (SUS304) current collector, and a carbon layer is formed by direct growth and lamination. A carbon layer is formed between the stainless steel (SUS304) current collector and the Ag particles.
[0283] At a chamber temperature of 1000°C, graphene was grown from Ag particles, forming a carbon-based material matrix containing graphene arranged horizontally on a carbon layer. Ag particles were dispersed and embedded within the carbon-based material matrix. A shell containing amorphous carbon was formed along the surface of the Ag particles. The particle size of the Ag core particles was approximately 50 nm. The thickness of the shell was approximately 10 nm.
[0284] The thickness of the carbon layer, which is the first protective layer, was approximately 500 nm. The thickness of the Ag-containing carbon layer, which is the first negative electrode active material layer, was approximately 3 μm.
[0285] Transmission electron microscopy (TEM) and high-resolution scanning electron microscopy (HR-SEM) measurements of the cross-section of the manufactured negative electrode confirmed that the first protective layer included graphene that was arranged and laminated in a direction parallel to the surface of the stainless steel (SUS304) current collector. In addition, it was confirmed that the first negative electrode active material layer included graphene and a silver core that were arranged in a direction parallel to the surface of the stainless steel (SUS304) current collector. In addition, the presence of a shell including amorphous carbon arranged on the silver core was confirmed. The initial charge capacity of the negative electrode layer (i.e., the first negative electrode active material layer) was measured using the half-cell described above.
[0286] (Anode layer manufacturing)
[0287] LiNi coated with Li2O-ZrO2 (LZO) as a cathode active material 0.8 Co 0.15 Mn 0.05 O2(NCM) was prepared. The LZO-coated cathode active material was manufactured according to the method disclosed in Korean Patent Publication No. 10-2016-0064942. Li6PS5Cl, an argyrodite-type crystal (D50 = 0.5 μm, crystalline), was prepared as a solid electrolyte. Polytetrafluoroethylene (PTFE) binder was prepared as a binder. Carbon nanofibers (CNF) were prepared as a conductive agent. These materials were mixed with a xylene solvent at a weight ratio of cathode active material: solid electrolyte: conductive agent: binder = 84: 11.5: 3: 1.5, and the slurry was molded into a sheet shape, and then vacuum-dried at 40°C for 8 hours to manufacture a cathode sheet. The manufactured cathode sheet was placed on the carbon layer of a cathode current collector composed of aluminum foil coated with a carbon layer on one side, and 85 oThe positive electrode layer was manufactured by heated roll pressing of C. The total thickness of the positive electrode layer was about 120 ㎛. The thickness of each of the positive electrode active material layers was about 95 ㎛, and the thickness of the carbon-coated aluminum foil was about 25 ㎛. The initial charge capacity of the positive electrode layer (i.e., the positive electrode active material layer) was measured using the half-cell described above. The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer and the initial charge capacity (A) of the positive electrode active material layer was less than 0.45. The initial charge capacity of the positive electrode active material layer was measured at the first open circuit voltage (1 st 4.2 V vs. Li / Li from open circuit voltage) + was determined by the charge up to . The initial charge capacity of the first negative active material layer was determined by the second open circuit voltage (2 nd 0.01 V vs. Li / Li from open circuit voltage) + It was determined by the charging up to . In addition, in Examples 2 to 5, the ratio (B / A) was less than 0.45, respectively.
[0288] (inert absence)
[0289] A flame-retardant inert member was manufactured by forming a slurry containing pulp fiber (cellulose fiber), glass fiber, aluminum hydroxide (Al(OH)3), an acrylic binder, and a solvent into a gasket shape and then removing the solvent.
[0290] The weight ratio of pulp fiber (cellulose fiber), glass fiber (glass fiber), aluminum hydroxide (Al(OH)3), and acrylic binder was 20:8:70:2. The thickness of the inert material was approximately 120 ㎛. The manufactured flame-retardant material was used after being left at room temperature for one week.
[0291] Before applying the inert material to the all-solid-state secondary battery, moisture, etc. of the inert material was removed by vacuum heat treatment at 80°C for 5 hours.
[0292] (Manufacturing of all-solid-state secondary batteries)
[0293] Referring to Fig. 3, a solid electrolyte layer was placed on the cathode layer such that the first cathode active material layer was in contact with the solid electrolyte layer. A flame-retardant inert material was placed on the solid electrolyte layer by heat and pressure to prepare a cathode layer / solid electrolyte layer / inert material laminate.
[0294] An anode layer / solid electrolyte layer / anode layer electrode assembly was prepared by arranging the inert member on one side of the anode layer so as to face the cathode active material layer. The inert member was arranged to surround the side of the anode layer and contact the solid electrolyte layer. The inert member was used as a gasket. The anode layer was arranged at the center of the solid electrolyte layer, and the gasket was arranged to surround the anode layer and extend to the end of the solid electrolyte layer. The area of the anode layer was approximately 90% of the area of the solid electrolyte layer, and the gasket was arranged over the entire area of the remaining 10% of the solid electrolyte layer where the anode layer was not arranged.
[0295] The prepared cathode layer / solid electrolyte layer / anode layer electrode assembly is 85 o The electrode assembly was plate-pressed at 500 MPa for 30 minutes at C. This pressurization process sintered the solid electrolyte layer, thereby improving battery characteristics. The thickness of the sintered solid electrolyte layer was approximately 45 μm. The sintered electrode assembly was placed in a pouch and sealed to prepare a sealed electrode assembly. Parts of the positive and negative current collectors were protruded outside the sealed electrode assembly to be used as positive and negative electrode terminals.
[0296] An electrode assembly was placed between two press plates (not shown) and the two press plates were fastened with screws to apply a constant pressure to both sides of the electrode assembly, thereby manufacturing an all-solid-state secondary battery.
[0297] Example 2: Methane 750-950℃, horizontally aligned graphene layer (first protective layer) / Ag embedded irregularly aligned graphene layer (first negative electrode active material layer), mono-cell all-solid-state secondary battery
[0298] A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the deposition temperature was changed to 850°C.
[0299] A negative electrode was prepared by sequentially depositing a carbon layer as a first protective layer and a carbon layer containing a negative electrode active material as a first negative electrode active material layer on one side of a 20 ㎛ thick stainless steel (SUS304) thin film.
[0300] The first protective layer has a structure in which graphene is laminated in multiple layers horizontally arranged on the surface of a stainless steel (SUS304) thin film.
[0301] The first negative electrode active material layer has a structure in which a carbon-based material matrix composed of irregularly arranged flake-shaped graphene is arranged, and Ag particles, which are negative electrode active materials, are dispersed and embedded within the carbon-based material matrix.
[0302] A shell containing amorphous carbon was coated on the surface of the Ag particles.
[0303] The thickness of the carbon layer, which is the first protective layer, was approximately 500 nm. The thickness of the Ag-containing carbon layer, which is the first negative electrode active material layer, was approximately 3 μm.
[0304] Transmission electron microscopy (TEM) and high-resolution scanning electron microscopy (HR-SEM) measurements of the cross-section of the manufactured negative electrode confirmed that the first protective layer included graphene arranged and laminated in a direction parallel to the surface of the stainless steel (SUS304) current collector. In addition, the first negative active material layer was confirmed to include irregularly arranged graphene and a silver core. In addition, the presence of a shell comprising amorphous carbon arranged on the silver core was confirmed.
[0305] Example 3: Acetylene 700-900℃, protruding array graphene layer (first protective layer) / Ag embedded irregular array graphene layer (first negative electrode active material layer), mono-cell all-solid-state secondary battery
[0306] A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the deposition temperature was changed to 800°C and the hydrocarbon gas was changed to acetylene.
[0307] A negative electrode was prepared by sequentially depositing a carbon layer as a first protective layer and a carbon layer containing a negative electrode active material as a first negative electrode active material layer on one side of a 20 ㎛ thick stainless steel (SUS304) thin film.
[0308] The first protective layer has a structure in which graphene is laminated in multiple layers in a direction protruding from the surface of a stainless steel (SUS304) thin film.
[0309] The first negative electrode active material layer has a structure in which a carbon-based material matrix composed of irregularly arranged flake-shaped graphene is arranged, and Ag particles, which are negative electrode active materials, are dispersed and embedded within the carbon-based material matrix.
[0310] A shell containing amorphous carbon was coated on the surface of the Ag particle core. The first negative electrode active material layer contained pores within the carbon-based material matrix by irregularly arranged graphene.
[0311] The thickness of the carbon layer, which is the first protective layer, was approximately 500 nm. The thickness of the Ag-containing carbon layer, which is the first negative electrode active material layer, was approximately 3 μm.
[0312] Transmission electron microscopy (TEM) and high-resolution scanning electron microscopy (HR-SEM) measurements of the cross-section of the manufactured negative electrode confirmed that the first protective layer included graphene arranged and laminated in a direction protruding from the surface of a stainless steel (SUS304) current collector. In addition, it was confirmed that the first negative active material layer included irregularly arranged graphene and a silver core. In addition, the presence of a shell including amorphous carbon arranged on the silver core was confirmed.
[0313] Example 4: Acetylene 500-700℃, protruding array graphene layer (first protective layer) / Ag embedded irregular array graphene layer (first negative electrode active material layer), mono-cell all-solid-state secondary battery
[0314] A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the heat treatment temperature was changed to 600°C and the hydrocarbon gas was changed to acetylene.
[0315] A negative electrode current collector was prepared by sequentially coating a carbon layer as a first protective layer and a carbon layer containing a negative electrode active material as a first negative electrode active material layer by deposition on one side of a 20 ㎛ thick stainless steel (SUS304) thin film.
[0316] The first protective layer has a structure in which graphene is laminated in multiple layers in a direction protruding from the surface of a stainless steel (SUS304) thin film.
[0317] The first negative electrode active material layer has a structure in which a carbon-based material matrix composed of irregularly arranged flake-shaped graphene is arranged, and Ag particles, which are negative electrode active materials, are dispersed and embedded within the carbon-based material matrix.
[0318] A shell containing amorphous carbon was coated on the surface of the Ag particle core. The first negative electrode active material layer contained pores within the carbon-based material matrix by irregularly arranged graphene.
[0319] The porosity of the first negative electrode active material layer of Example 4 was higher than that of the first negative electrode active material layer of Example 3.
[0320] The thickness of the carbon layer, which is the first protective layer, was approximately 500 nm. The thickness of the Ag-containing carbon layer, which is the first negative electrode active material layer, was approximately 3 μm.
[0321] Transmission electron microscopy (TEM) and high-resolution scanning electron microscopy (HR-SEM) measurements of the cross-section of the manufactured negative electrode confirmed that the first protective layer included graphene arranged and laminated in a direction protruding from the surface of a stainless steel (SUS304) current collector. In addition, it was confirmed that the first negative active material layer included irregularly arranged graphene and a silver core. In addition, the presence of a shell including amorphous carbon arranged on the silver core was confirmed.
[0322] Example 5: Bi-cell all-solid-state secondary battery
[0323] (Manufacture of solid electrolyte layer, cathode layer and inert member)
[0324] It was manufactured in the same manner as Example 1.
[0325] (Anode layer manufacturing)
[0326] LiNi coated with Li2O-ZrO2 (LZO) as a cathode active material 0.8 Co 0.15 Mn 0.05O2(NCM) was prepared. The LZO-coated cathode active material was manufactured according to the method disclosed in Korean Patent Publication No. 10-2016-0064942. Li6PS5Cl, an argyrodite-type crystal (D50 = 0.5 μm, crystalline), was prepared as a solid electrolyte. Polytetrafluoroethylene (PTFE) binder was prepared as a binder. Carbon nanofibers (CNF) were prepared as a conductive agent. These materials were mixed with xylene solvent in a weight ratio of cathode active material: solid electrolyte: conductive agent: binder = 84: 11.5: 3: 1.5, and the slurry was molded into a sheet shape, and then vacuum-dried at 40°C for 8 hours to manufacture a cathode sheet. The manufactured cathode sheets were placed on both sides of a cathode current collector composed of aluminum foil coated with a carbon layer on both sides, and 85 o The positive electrode layer was manufactured by heated roll pressing of C. The total thickness of the positive electrode layer was approximately 220 μm. The thickness of each positive electrode active material layer was approximately 96 μm, and the thickness of the carbon-coated aluminum foil was approximately 28 μm.
[0327] (Manufacturing of all-solid-state secondary batteries)
[0328] Referring to Fig. 4, a solid electrolyte layer was placed on the cathode layer such that the first cathode active material layer was in contact with the solid electrolyte layer. A flame-retardant inert material was placed on the solid electrolyte layer by heat and pressure to prepare two cathode layer / solid electrolyte layer / inert material laminates.
[0329] An electrode assembly (anode layer / solid electrolyte layer / anode layer / solid electrolyte layer / anode layer) was prepared by arranging the inert member on both sides of the anode layer so as to face the anode active material layer. The inert member was arranged to surround the side surfaces of the anode layer and contact the solid electrolyte layer. The inert member was used as a gasket. The anode layer was arranged at the center of the solid electrolyte layer, and the gasket was arranged to surround the anode layer and extend to the end of the solid electrolyte layer. The area of the anode layer was approximately 90% of the area of the solid electrolyte layer, and the gasket was arranged over the entire area of the remaining 10% of the solid electrolyte layer where the anode layer was not arranged.
[0330] Using the electrode assembly prepared above, an all-solid-state secondary battery was manufactured in the same manner as in Example 1.
[0331] Comparative Example 1: Anode current collector without coating layer
[0332] An anode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that a 20 ㎛ thick stainless steel (SUS304) thin film was used as the anode collector.
[0333] Comparative Example 2: Carbon layer (first protective layer) only (first negative electrode active material layer omitted) negative electrode current collector
[0334] An anode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that only a carbon layer as the first protective layer was introduced on one side of a 20 ㎛ thick stainless steel (SUS304) thin film without introducing an Ag precursor compound.
[0335] Comparative Example 3: Graphene wet coating (first protective layer) + Ag-carbon wet coating (first negative electrode active material layer) negative electrode current collector
[0336] An anode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the first protective layer and the first negative electrode active material layer were each introduced by wet method on one side of a 20 ㎛ thick stainless steel (SUS304) thin film.
[0337] The cathode layer was manufactured by the following method.
[0338] (Cathode layer manufacturing)
[0339] A negative electrode current collector was prepared by wet-coating a carbon layer and a first negative electrode active material layer on one side of a 20 ㎛ thick stainless steel (SUS304) thin film.
[0340] The carbon layer was prepared by coating a graphene dispersion on a Cu foil and then drying it. The graphene dispersion was prepared by dispersing graphene oxide and a polyvinylidene fluoride (PVDF) binder in N-methylpyrrolidone.
[0341] Carbon black (CB) particles with a primary particle diameter of approximately 30 nm and silver (Ag) particles with an average particle diameter (D50) of approximately 60 nm were prepared as negative electrode active materials.
[0342] 4 g of a mixed powder containing carbon black (CB) and silver (Ag) particles in a weight ratio of 3:1 was placed in a container, and 4 g of an NMP solution containing 7 wt% PVDF binder (Kureha #9300) was added thereto to prepare a mixed solution. Subsequently, a slurry was prepared by stirring the mixed solution while adding NMP little by little to the mixed solution. The prepared slurry was applied onto the carbon layer of the prepared negative electrode collector using a bar coater and dried in the air at 80°C for 10 minutes. The laminate thus obtained was vacuum-dried at 40°C for 10 hours. The dried laminate was cold roll pressed to flatten the surface of the first negative electrode active material layer of the laminate. The negative electrode layer was manufactured through the above process.
[0343] The thickness of the first negative electrode active material layer included in the negative electrode layer was approximately 10 μm. The thickness of the carbon layer, which is the first protective layer, was approximately 1 μm.
[0344] Reference Example 1: Excluding inert elements (free)
[0345] An all-solid-state secondary battery was manufactured in the same manner as Example 1, except that no inert material was placed around the positive electrode active material layer.
[0346]
[0347] Evaluation Example 1: Evaluation of crystallinity and porosity
[0348] The crystallinity of the cathode layers manufactured in Examples 1 to 4 was evaluated using XRD, Raman, and transmission electron microscopy.
[0349] In the Raman spectrum of the cathode layer, 1350 cm is derived from amorphous carbon. -1 Nearby D-band peak intensity (I D ) and 1580 cm derived from crystalline carbon -1 Nearby G-band peak intensity (I G ) relative peak intensity ratio (I D / I G ) was used to determine the relative crystallinity of the cathode layer. The peak intensity ratio (I D / I G ) is higher, the lower the crystallinity, and the peak intensity ratio (I D / I G ) is lower, the higher the crystallinity. The measurement results are shown in Table 1 below.
[0350] Additionally, the relative crystallinity was determined from the intensity and / or half width of the peaks in the XRD spectrum for the cathode layer and the high-resolution TEM image and diffraction pattern thereof for the cathode layer.
[0351] The porosity of the cathode layers manufactured in Examples 1 to 4 was measured using a gas adsorption method (multi-point BET). The measurement results are shown in Table 1 below.
[0352] The crystallinity and porosity are for the first negative electrode active material layer and the first protective layer of the negative electrode layer.
[0353] The crystallinity of the cathode layer manufactured in Example 1 was relatively the highest, and the crystallinity of the cathode layer manufactured in Example 4 was relatively the lowest.
[0354] The relative order of crystallinity of the negative electrode layer in the all-solid-state secondary batteries of Examples 1 to 4 was Example 1 > Example 2 > Example 3 > Example 4.
[0355] The porosity of the cathode layer manufactured in Example 1 was relatively the lowest, and the porosity of the cathode layer manufactured in Example 4 was relatively the highest.
[0356] The relative order of the porosity of the negative electrode layer in the all-solid-state secondary batteries of Examples 1 to 4 was Example 4 > Example 3 > Example 2 > Example 1.
[0357] Raman peak intensity ratio (I D / I G )Porosity [%] Example 1 (1000℃, methane) First protective layer: Horizontally arranged graphene First negative electrode active material layer: Graphene horizontally arranged + Ag particle embedded Less than 1.5 Less than 2 Example 2 (850℃, methane) First protective layer: Horizontally arranged graphene First negative electrode active material layer: Graphene irregularly arranged + Ag particle embedded 2.35 Example 3 (800℃, acetylene) First protective layer: Protrudingly arranged graphene First negative electrode active material layer: Graphene irregularly arranged + Ag particle embedded 3.312 Example 4 (600℃, acetylene) First protective layer: Protrudingly arranged graphene First negative electrode active material layer: Graphene irregularly arranged + Ag particle embedded 4.823 Comparative example 2 (SUS / dry graphene layer structure) First protective layer: Graphene horizontally arranged First negative electrode active material layer: Free Less than 1.51.0 less than
[0358]
[0359] Evaluation Example 2: Charge / Discharge Test
[0360] The charge / discharge characteristics of the all-solid-state secondary batteries manufactured in Examples 1 to 5, Comparative Examples 1 to 3, and Reference Example 1 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid-state secondary batteries in a constant temperature bath at 45°C.
[0361] The first cycle involved charging at a constant current of 0.1 C until the battery voltage reached 4.2 V, and then constant voltage charging at 4.2 V with a 0.05 C cut-off condition was performed once the voltage reached 4.2 V. Subsequently, discharging was performed at a constant current of 0.1 C until the battery voltage reached 2.6 V.
[0362] After the second cycle, charge and discharge were performed for up to 800 cycles under the same conditions as the first cycle. This indicates that the lifespan characteristics improve as the number of cycles at which short circuits occur increases. The measurement results are shown in Table 2.
[0363] Short circuit occurrence time [times] Example 1 (1000℃, methane), SUS current collector 1st protective layer: horizontally arranged graphene 1st negative electrode active material layer: horizontally arranged graphene + embedded Ag particles 800 Example 2 (850℃, methane), SUS current collector 1st protective layer: horizontally arranged graphene 1st negative electrode active material layer: irregularly arranged graphene + embedded Ag particles 720 Example 3 (800℃, acetylene), SUS current collector 1st protective layer: protruding arranged graphene 1st negative electrode active material layer: irregularly arranged graphene + embedded Ag particles 600 Example 4 (600℃, acetylene), SUS current collector 1st protective layer: protruding arranged graphene 1st negative electrode active material layer: irregularly arranged graphene + embedded Ag particles 480 Comparative example 1 (SUS foil only) 1st protective layer: absent (free) 1st negative electrode active material layer: absent (free) 18 Comparative example 2 (SUS / dry graphene layer structure) 1st protective layer: horizontal arrangement of graphene 1st negative electrode active material layer: free 200 Comparative example 3 (SUS / wet graphene layer / Ag+C blend layer structure) 1st protective layer: wet graphene layer 1st negative electrode active material layer: Ag+C blend layer 160
[0364] As shown in Table 2, the all-solid-state secondary batteries of Examples 1 to 4 provided improved life characteristics compared to the all-solid-state secondary batteries of Comparative Examples 1 to 3.
[0365] It was determined that the solid-state secondary battery of Example 4 had relatively lower crystallinity of the first protective layer and the first negative electrode active material layer compared to the solid-state secondary batteries of Examples 1 to 3, and thus the deterioration of the negative electrode current collector due to the solid electrolyte relatively increased.
[0366] The all-solid-state secondary battery of Comparative Example 1 had significantly poorer life characteristics than the all-solid-state secondary batteries of Examples 1 to 4 due to the absence of both the first protective layer and the first negative electrode active material layer. This was judged to be because the absence of the first protective layer and the first negative electrode active material layer in the all-solid-state secondary battery of Comparative Example 1 increased side reactions between the negative electrode current collector and the solid electrolyte.
[0367] The all-solid-state secondary battery of Comparative Example 2 had relatively poor life characteristics compared to the all-solid-state secondary batteries of Examples 1 to 4 due to not including the first negative electrode active material layer. It was determined that this was because the all-solid-state secondary battery of Comparative Example 2 did not effectively suppress the generation and growth of lithium dendrites due to the absence of the first negative electrode active material layer, thereby deteriorating the all-solid-state secondary battery.
[0368] The all-solid-state secondary battery of Comparative Example 3 had relatively poor life characteristics compared to the all-solid-state secondary batteries of Examples 1 to 4 due to the inclusion of a wet graphene layer and a wet first active material layer. This was determined to be because the wet graphene layer and the wet first negative electrode active material layer in the all-solid-state secondary battery of Comparative Example 3 did not effectively prevent side reactions between the solid electrolyte and the negative electrode current collector compared to the first protective layer and the first negative electrode active material layer in Examples 1 to 4.
[0369] Although not shown in Table 1, the all-solid-state secondary battery of Example 5 had relatively improved life characteristics compared to the all-solid-state secondary battery of Example 1 due to improved structural stability.
[0370] Although not shown in Table 1, the all-solid-state secondary battery of Reference Example 1 had poor life characteristics compared to the all-solid-state secondary batteries of Examples 1 to 4 due to the absence of an inert gasket.
[0371] After the first cycle of charging was completed in the all-solid-state secondary batteries of Examples 1 to 4, SEM images of the cross-sections of these batteries were measured to confirm that a lithium metal precipitation layer corresponding to the second negative electrode active material layer was formed between the solid electrolyte layer and the negative electrode current collector.
[0372] The relative size of the volume density of the first protective layer (carbon layer) in the all-solid-state secondary batteries of Examples 1 to 4 was Example 1 ≒ Example 2 > Example 3 ≒ Example 4. The volume density of the dry first protective layer of Examples 1 to 4 was higher than the volume density of the wet first protective layer of Comparative Example 3.
[0373] As described above, the all-solid-state secondary battery related to the present embodiment can be applied to various portable devices, vehicles, etc.
[0374] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.
[0375] [Explanation of symbols]
[0376] 1 All-solid-state secondary battery 10 Cathode layer
[0377] 11. Cathode current collector 12. Cathode active material layer
[0378] 20 Cathode layer 21 Cathode current collector
[0379] 22 First negative electrode active material layer 23 First protective layer
[0380] 30 solid electrolyte layer 40 inert member
[0381] According to one aspect, by using an all-solid-state secondary battery having a novel structure, it is possible to provide an all-solid-state secondary battery in which short circuit is suppressed and cycle characteristics are improved by improving the uniformity of the thickness of the negative electrode active material layer and suppressing aggregation of the negative electrode active material.
Claims
1. It comprises an anode layer; a cathode layer; and a solid electrolyte layer between the anode layer and the cathode layer, The above positive electrode layer includes a positive electrode current collector; and a positive electrode active material layer, and the solid electrolyte layer includes a sulfide-based solid electrolyte. The negative electrode layer includes a negative electrode current collector; a first negative electrode active material layer; and a first protective layer between the negative electrode current collector and the first negative electrode active material layer. The first negative electrode active material layer includes a carbon-based material matrix and a metal-based negative electrode active material within the carbon-based material matrix, wherein the above carbon-based material matrix comprises a first carbon-based nanostructure, and the first protective layer comprises a second carbon-based nanostructure, An all-solid-state secondary battery having a specific heat capacity of the above-mentioned negative electrode collector of about 450 J / Kg·K or more.
2. In the first paragraph, the first carbon-based nanostructure includes a two-dimensional carbon-based nanostructure, An all-solid-state secondary battery, wherein the two-dimensional carbon nanostructure comprises graphene, graphene oxide, reduced graphene oxide, or a combination thereof.
3. An all-solid-state secondary battery comprising a first carbon-based nanostructure in which the carbon-based material matrix is arranged in a certain direction in the first paragraph.
4. An all-solid-state secondary battery comprising a first carbon-based nanostructure in which the carbon-based material matrix is irregularly arranged in the first paragraph.
5. An all-solid-state secondary battery according to claim 1, wherein the carbon-based material matrix comprises crystalline carbon, amorphous carbon, or a combination thereof.
6. An all-solid-state secondary battery according to claim 1, wherein the carbon-based material matrix further includes pores, and the carbon-based material matrix is a lithium host.
7. In the first paragraph, the metal-based negative electrode active material a core; and a shell on the surface of the core, An all-solid-state secondary battery, wherein the core comprises a metal that forms an alloy or compound with lithium, and the shell comprises a carbon-based material.
8. An all-solid-state secondary battery in accordance with claim 7, wherein the metal forming an alloy or compound with lithium includes an alloy-forming element selected from gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), zinc (Zn), or a combination thereof.
9. An all-solid-state secondary battery according to claim 7, wherein the shell comprises a third carbon-based nanostructure, or the shell comprises amorphous carbon.
10. An all-solid-state secondary battery in accordance with claim 7, wherein the metal-based negative electrode active material has a particle form, the particle diameter of the core is about 10 nm to about 500 nm, and the thickness of the shell is about 50 nm or less.
11. An all-solid-state secondary battery in the first paragraph, wherein the content of the metal-based negative electrode active material is 10 parts by weight or less of the metal-based negative electrode active material per 100 parts by weight of the carbon-based material matrix.
12. In the first paragraph, the thickness of the first negative electrode active material layer is about 20 ㎛ or less, and the first negative electrode active material layer is free of a binder, The ratio (C1 / C2) of the charge capacity (C1) of the first negative electrode active material layer and the charge capacity (C2) of the positive electrode active material layer is 0.001 to 0.45, The thickness of the first negative electrode active material layer is greater than the thickness of the first protective layer, In the Raman spectrum for the above cathode layer, 1350 cm is derived from amorphous carbon. -1 Nearby D-band peak intensity (I D ) and 1580 cm derived from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G ) is 0.01 to 5, all-solid-state secondary battery.
13. In the first paragraph, the second carbon nanostructure comprises a two-dimensional carbon nanostructure, An all-solid-state secondary battery, wherein the two-dimensional carbon nanostructure comprises graphene, graphene oxide, reduced graphene oxide, or a combination thereof.
14. In the 13th paragraph, the first protective layer includes a second carbon-based nanostructure arranged in a certain direction with respect to the surface of the negative electrode current collector, The second carbon nanostructure is aligned in a direction parallel to the surface of the negative electrode collector or in a direction protruding from the surface of the negative electrode collector, An all-solid-state secondary battery, wherein the second carbon-based nanostructure is laminated along the thickness direction of the first protective layer, and the second carbon-based nanostructure is laminated in 100 layers or less.
15. In the first paragraph, the first protective layer is directly disposed on the negative electrode current collector, and the first protective layer is inert to the sulfide-based solid electrolyte. An all-solid-state secondary battery, wherein the thickness of the first protective layer is about 2 ㎛ or less, and the first protective layer is free of a binder.
16. In the first paragraph, a second negative electrode active material layer is further included between the solid electrolyte layer and the negative electrode current collector, The second negative electrode active material layer is at least one of between the first negative electrode active material layer and the first protective layer and between the first negative electrode active material layer and the solid electrolyte layer, An all-solid-state secondary battery, wherein the second negative electrode active material layer is a metal layer containing lithium or a lithium alloy.
17. An all-solid-state secondary battery in the first paragraph, wherein the negative electrode collector comprises stainless steel (SUS), titanium (Ti), iron (Fe), nickel (Ni), chromium (Cr) or an alloy thereof.
18. In the first paragraph, the positive electrode collector includes a base film and a metal layer on at least one surface of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, An all-solid-state secondary battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
19. In the first paragraph, an inactive member is further included arranged on one side of the anode layer, The above inert member is arranged to surround the anode layer along the side of the anode layer, An all-solid-state secondary battery, wherein the inert member includes a position determining unit configured to determine the position of the inert member on the solid electrolyte layer.
20. In the first paragraph, the positive electrode active material layer includes a positive electrode active material, The above cathode active material includes an oxide-based cathode active material, a sulfide-based cathode active material, or a combination thereof, The above oxide-based cathode active material includes a lithium transition metal oxide, a metal oxide, or a combination thereof, and the lithium transition metal oxide includes lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt mangense oxide, lithium manganate, lithium iron phosphate, or a combination thereof, and the lithium oxide includes iron oxide, vanadium oxide, or a combination thereof. An all-solid-state secondary battery, wherein the sulfide-based cathode active material comprises nickel sulfide, copper sulfide, Li2S, a Li2S-containing complex, or a combination thereof.
Citation Information
Patent Citations
Cathode for lithium ion secondary battery, and lithium ion secondary battery
KR1020160064942A
Negative electrode mixture and all-solid battery
JP2017027886A
solid-state batteries
JP2023015339A
Display appratus
KR1020230171512A
Seat belt retractor
KR102725507B1