Lithium battery and manufacturing method therefor
The lithium battery design with an integrated current collector and separator structure, using a gel-type polymer electrolyte and lithium metal layer, addresses dendrite formation and capacity limitations, enhancing lifespan and thermal stability.
Patent Information
- Application Number
- PCT/KR2024/003725
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium metal batteries face challenges with dendrite formation and short circuits due to side reactions with the electrolyte, leading to reduced lifespan, and existing carbon-based anode materials have limited capacity.
A lithium battery design with an integrated negative electrode current collector and separator structure, utilizing a gel-type polymer electrolyte and a lithium metal layer, where the initial adhesion between the current collector and separator is optimized, and a protective layer may be included to prevent dendrite growth and improve thermal stability.
The design enhances the lifespan and high-rate characteristics of lithium batteries by minimizing interfacial resistance and preventing dendrite formation, while also improving thermal stability and safety.
Smart Images

Figure KR2024003725_03102024_PF_FP_ABST
Abstract
Description
Lithium battery and manufacturing method thereof
[0001] It relates to a lithium battery and a method for manufacturing the same.
[0002] Lithium batteries currently on the market primarily use carbon-based anode materials, such as graphite. Carbon-based anode materials exhibit no volume change during charge and discharge, contributing to the stability of lithium batteries. However, their low capacity necessitates the use of higher-capacity anode materials.
[0003] Lithium metal, which has a much larger theoretical electric capacity than carbon-based negative electrode materials, can be used as a negative electrode material.
[0004] When lithium metal is charged and discharged, dendrites are formed on the surface of the lithium metal due to a side reaction with the electrolyte, and the growth of the dendrites can cause a short circuit between the positive and negative electrodes, which can reduce the life characteristics of a lithium battery containing lithium metal.
[0005] One aspect is to provide a lithium metal battery with a new structure.
[0006] Another aspect is to provide a method for manufacturing the above-described lithium metal battery.
[0007] According to the implementation example
[0008] A lithium battery in which a negative electrode collector, a separator, and a positive electrode are sequentially arranged.
[0009] There is no negative active material layer or protective layer between the negative electrode current collector and the separator.
[0010] The above negative electrode collector and separator are an integrated structure,
[0011] A lithium battery is provided in which the initial adhesive strength of the interface between the negative electrode current collector and the separator of the above-mentioned integral structure is 0.15 gf / cm to 1.0 gf / cm.
[0012] A gel-type polymer electrolyte may be placed between the interface of the negative electrode collector and the separator.
[0013] According to one embodiment, a gel-like polymer electrolyte may be present in the pores of the separator.
[0014] The above separator is made of polyethylene, polypropylene, polyethylene terephthalate,
[0015] Polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, polyvinylidene fluoride, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride hexafluoropropylene copolymer, or a combination thereof.
[0016] The interface between the negative electrode collector and the separator of the integrated structure before and after charging and discharging of the above lithium battery
[0017] The adhesive strength is 0.15 to 1.0 gf / cm. The gel-like polymer electrolyte present at the interface between the negative electrode collector and the separator includes a liquid electrolyte containing an organic solvent and a lithium salt, and a cross-linked polymer. The gel-like polymer electrolyte may be present in the pores of the separator.
[0018] The thickness of the gel polymer electrolyte present at the interface between the negative electrode current collector and the separator is not particularly limited, but is 1 um or less, 0.001 to 1 um, 0.01 to 1 um, 0.1 to 1 um, 0.1 to 0.9 um, 0.1 to 0.8 um, 0.1 to 0.7 um, 0.1 to 0.5 um, 0.1 to 0.3 um, or 0.1 to 0.2 um.
[0019] The above crosslinked polymer is a polymerization product of a crosslinkable monomer, and the crosslinkable monomer is diethylene glycol diacrylate (DEGDA), diethylene glycol dimethacrylate (DEGDMA), triethylene glycol diacrylate (TEGDA), triethylene glycol dimethacrylate (TEGDMA), tetraethylene glycol diacrylate (TTEGDA), glycidyl methacrylate, polyethylene glycol diacrylate (PEGDA), polyethylene glycol dimethacrylate (PEGDMA), polypropylene glycol diacrylate (PPGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), dianol diacrylate (DDA), dianol dimethacrylate (DDMA), ethoxylated trimethylolpropane triacrylate (ETPTA), acrylate functionalized ethylene Acrylate-functionalized ethylene oxide, butanediol dimethacrylate, ethoxylated neopentyl glycol diacrylate (NPEOGDA), propoxylated neopentyl glycol diacrylate (NPEOGDA), trimethylol propane triacrylate (TMPTA), trimethylol propane trimethacrylate (TMPTMA), pentaerythritol triacrylate (PETA), ethoxylated propoxylated trimethylolpropane triacrylate (TMPEOTA) / (TMPPOTA), propoxylated glyceryl triacrylate, tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA), pentaerythritol tetraacrylate (PETTA), dipentaerythritol pentaacrylate (DPEPA), ditrimethylol propane tetraacrylate (DTMPTTA); diglycidyl ester, diallyl suberate;acrylamide, divinylbenzene or a combination thereof;
[0020] The above lithium battery further includes a liquid electrolyte, a solid electrolyte, or a combination thereof containing a lithium salt and an organic solvent, and the liquid electrolyte may be a positive electrode electrolyte.
[0021] A negative electrode active material layer is further included between the negative electrode current collector and the separator, and the thickness of the negative electrode active material layer is 0.1 ㎛ to 80 ㎛. The negative electrode active material layer includes a lithium metal foil, a lithium metal powder, a lithium alloy foil, a lithium alloy powder, or a combination thereof, and the lithium alloy contains lithium and a first metal.
[0022] The first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.
[0023] The above negative electrode active material layer includes a negative electrode active material, and the negative electrode active material may contain a carbon-based material; a mixture of a carbon-based material and at least one selected from a metal or a metalloid; a composite of a carbon-based material and at least one selected from a metal or a metalloid; or a combination thereof.
[0024] The above carbon-based material includes amorphous carbon, and the above carbon-based material includes carbon black, carbon nanotubes, carbon nanofibers, fullerenes, activated carbon, carbon fibers, or a combination thereof.
[0025] A lithium battery according to an embodiment may have a structure in which a negative electrode current collector / lithium metal layer / gel-type polymer electrolyte / separator are sequentially arranged before and after charge and discharge. The lithium metal layer is a deposited lithium layer.
[0026] According to another embodiment, when a lithium battery further includes a negative electrode active material layer, it may have a structure in which a negative electrode current collector / lithium metal layer / negative electrode active material layer / gel-type polymer electrolyte / separator are sequentially arranged before and after charge and discharge.
[0027] A protective layer may be further included between the negative electrode current collector and the separator. This protective layer may be formed between the negative electrode active material layer and the separator. When the lithium battery further includes a protective layer, it may have a structure in which the negative electrode current collector / lithium metal layer / protective layer / gel-type polymer electrolyte / separator are sequentially arranged before and after charge and discharge.
[0028] The positive electrode includes a positive electrode current collector and a positive electrode active material layer, and at least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one or both sides of the base film, and the base film includes a polymer, and the polymer includes polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof.
[0029] The above metal layer includes indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
[0030] Step of preparing a cathode current collector according to another aspect;
[0031] A step of manufacturing a negative electrode collector / separator structure by placing a separator on one side of a negative electrode collector;
[0032] A step of manufacturing an integrated negative electrode current collector / separator structure containing a gel-type polymer electrolyte by injecting a composition for forming a gel-type polymer electrolyte into a negative electrode current collector / separator structure and performing heat treatment; and
[0033] Steps to prepare the anode;
[0034] A step of forming a battery structure by placing a positive electrode on top of an integrated negative electrode collector / separator structure containing a gel-type polymer electrolyte; and
[0035] A method for manufacturing a lithium battery is provided, which includes a step of housing the above-described battery structure in a battery case.
[0036] The above heat treatment is performed at 40 to 120°C. And the composition for forming the gel-type polymer electrolyte includes a crosslinking monomer, a lithium salt, an organic solvent, and a polymerization initiator.
[0037] The above manufacturing method injects a liquid electrolyte containing a lithium salt and an organic solvent into the battery structure in the step of housing the battery case, and further includes at least one selected from a negative electrode active material layer and a protective layer between the negative electrode current collector and the separator.
[0038] According to one aspect, the thermal shrinkage function of the separator is reduced, and by using such a separator, a battery short circuit due to shrinkage at high temperatures can be prevented, thereby improving thermal stability and safety as well as providing a lithium battery with improved high-rate characteristics and life characteristics.
[0039] Figure 1 is a drawing for explaining the manufacturing process of an integrated negative electrode current collector / separator structure containing a gel-type polymer electrolyte according to an embodiment.
[0040] Figure 2 shows the results of a heat shrinkage test after storing the lithium batteries of Example 1 and Comparative Example 1 in a chamber at 140°C for 1 hour.
[0041] Figure 3 shows the results of a heat shrinkage test after storing the lithium batteries of Example 1 and Comparative Example 1 in a chamber at 150°C for 1 hour.
[0042] Figure 4 is a schematic diagram of a lithium battery according to an embodiment.
[0043] Figure 5 is a schematic diagram of a lithium battery according to another embodiment.
[0044] Figure 6 is a schematic diagram of a lithium battery according to another embodiment.
[0045] <Explanation of key symbols in the drawing>
[0046] 1 lithium battery 2, 20 cathode
[0047] 3, 10 anode 4 separator
[0048] 5 Battery case 6 Cap assembly
[0049] 7 Battery structure 8 Electrode tab
[0050] The present inventive concept described below is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail. However, this is not intended to limit the present inventive concept to specific embodiments, but rather to encompass all modifications, equivalents, or alternatives within the technical scope of the present inventive concept.
[0051] The terminology used below is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. Hereinafter, the terms "comprises" or "has" and the like are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. The " / " used below may be interpreted as "and" or "or" depending on the context.
[0052] In order to clearly express various layers and regions in the drawings, the thickness is shown enlarged or reduced. Similar parts are designated by the same drawing reference numerals throughout the specification. When a part such as a layer, film, region, or plate is said to be "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. Terms such as first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only for the purpose of distinguishing one component from another. In this specification and the drawings, components having substantially the same functional configuration are referred to by the same reference numerals, and redundant descriptions are omitted.
[0053] In the present disclosure, the "particle diameter" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle diameter of a particle can be measured using a particle size analyzer (PSA). The "particle diameter" of a particle is, for example, the average particle diameter. The average particle diameter is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of a particle corresponding to 50% of the cumulative volume, calculated from the side of particles having a small particle size in a size distribution of particles measured by, for example, laser diffraction. The average particle diameter and average major axis length of a particle can be measured using a scanning electron microscope. When the particle size is measured using a scanning electron microscope, it is determined as the average value of 30 or more randomly selected particles having a size of 1 μm or more, excluding fine particles.
[0054] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0055] In this disclosure, “alloy” means a mixture of two or more metals.
[0056] In the present disclosure, “positive electrode active material” means a positive electrode material capable of undergoing lithiation and delithiation, and “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0057] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material, and “delithiation” and “delithiating” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.
[0058] In the present disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery, and “discharging” and “discharging” mean a process of removing electrochemical energy from a battery.
[0059] In the present disclosure, “positive electrode” and “cathode” mean an electrode where electrochemical reduction and lithiation occur during a discharge process, and “negative electrode” and “anode” mean an electrode where electrochemical oxidation and delithiation occur during a discharge process.
[0060] In this disclosure, “thickness” means “average thickness.”
[0061] Hereinafter, lithium batteries and their manufacturing methods according to embodiments will be described in more detail.
[0062] Gel polymer electrolytes (GPEs) are semi-solid electrolytes composed of a liquid polymer electrolyte and a gel. They are typically manufactured as free-standing films or by injecting the GPE into the electrolyte solution and then curing it. Compared to pure lithium batteries, GPEs exhibit increased resistance, which can lead to a decrease in capacity, but they offer significantly improved stability. However, when applied to lithium metal batteries, gel polymer electrolytes can exhibit reduced high-rate performance due to their inherent resistance.
[0063] In order to solve the above-described problem, a lithium battery according to an embodiment of the present invention applies GPE to a separator to prevent high-temperature shrinkage of the separator, and improves high-rate characteristics by using a liquid electrolyte together.
[0064] According to an embodiment, a lithium battery having an integrated substrate / separator structure with a gel polymer electrolyte that improves thermal stability and reduces interfacial resistance by injecting a composition for forming a gel polymer electrolyte while a negative electrode current collector and a separator are attached and then curing the composition, and a method for manufacturing the same are provided.
[0065] According to an embodiment, a lithium battery comprises a negative electrode current collector, a separator, and a positive electrode sequentially arranged, and a negative electrode active material layer or a protective layer is absent (free) between the negative electrode current collector and the separator, the negative electrode current collector and the separator are an integrated structure, and the initial adhesive strength of the interface between the negative electrode current collector and the separator of the integrated structure is 0.15 gf / cm to 1.0 gf / cm.
[0066] A gel-type polymer electrolyte is placed between the negative electrode collector and the separator.
[0067] The above lithium battery is, for example, a lithium ion battery or a lithium metal battery.
[0068] In this specification, “initial adhesion of the interface between the negative electrode collector and the separator of the integrated structure” refers to the adhesion of the negative electrode collector and the separator before performing charge / discharge after assembling the lithium battery.
[0069] The initial interfacial adhesion was evaluated by fixing a tape (26 mm x 76 mm) on top of the cathode substrate-integrated separator and pulling the end of the tape in a T-shape using an Instron 3342 device at a speed of 20 mm / min to 80 mm / min, 40 mm / min to 70 mm / min, for example, about 60 mm / min, and a load of 0.1 kgf to 0.8 kgf, 0.2 kgf to 0.7 kgf, for example, 0.5 kgf, to measure the peel strength.
[0070] The initial adhesive strength of the interface between the negative electrode current collector and the separator of the integral structure is, for example, 0.18 gf / cm to 1.0 gf / cm, 0.2 gf / cm to 1.0 gf / cm, 0.2 gf / cm to 0.9 gf / cm, 0.25 gf / cm to 0.9 gf / cm, 0.33 gf / cm to 0.9 gf / cm, 0.35 gf / cm to 0.9 gf / cm, 0.36 gf / cm to 0.9 gf / cm, 0.38 gf / cm to 0.9 gf / cm, 0.38 gf / cm to 0.87 gf / cm, or 0.38 gf / cm to 0.85 gf / cm.
[0071] According to another implementation, the initial adhesive strength of the interface between the negative electrode collector and the separator of the integral structure is 0.33 gf / cm to 0.56 gf / cm.
[0072] The negative electrode current collector and the separator can be combined without a binder, and when the lithium battery is charged, lithium is uniformly deposited between the negative electrode current collector and the separator, thereby suppressing dendrite formation.
[0073] The above-mentioned integrated structure is an integrated negative electrode current collector / separator structure containing a gel-type polymer electrolyte, and the above-mentioned integrated structure is a product obtained by the steps of: preparing a negative electrode current collector; arranging a separator on one surface of the negative electrode current collector to manufacture the negative electrode current collector / separator structure; and injecting a composition for forming a gel-type polymer electrolyte into the negative electrode current collector / separator structure and heat-treating the same.
[0074] The lithium battery of the present invention can manufacture an anode current collector / separator structure having an integrated structure, in which a composition for forming a gel-type polymer electrolyte is partially introduced into a separator and a negative electrode current collector, which is a substrate, and the composition for forming a gel-type polymer electrolyte is gelated so that the substrate serves to hold the separator. In this way, when the negative electrode current collector, which is a substrate, holds the separator, thermal stability is improved, and shrinkage of the separator due to heat can be effectively prevented.
[0075] The substrate acts as a supporting membrane on which the separator is placed, and an example thereof may be a negative electrode current collector.
[0076] The membrane includes a porous substrate, and may contain polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, polyvinylidene fluoride, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride hexafluoropropylene copolymer, or a combination thereof.
[0077] The pores of the above separator, i.e., the pores of the porous substrate, contain a gel-type polymer electrolyte, and the gel-type polymer electrolyte can also be arranged at the interface between the negative electrode collector and the separator.
[0078] The above anode may contain a liquid electrolyte, an ionic liquid, or a combination thereof.
[0079] According to an embodiment, the adhesive strength of the interface between the negative electrode current collector and the separator of the integrated structure before and after charge and discharge of the lithium battery is 0.1 gf / cm to 0.3 gf / cm, 0.11 gf / cm to 0.29 gf / cm, 0.13 gf / cm to 0.29 gf / cm, 0.14 gf / cm to 0.29 gf / cm, 0.15 gf / cm to 0.29 gf / cm, or 0.17 gf / cm to 0.29 gf / cm.
[0080] According to another embodiment, the interfacial adhesive strength of the negative electrode collector and the separator of the integrated structure before and after charge and discharge of the lithium battery is 0.17 gf / cm to 0.29 gf / cm. Here, the charge and discharge conditions of the lithium battery are 0.1C charge / 0.1C discharge. In this way, since the negative electrode collector and the separator have excellent interfacial adhesive properties even after charge and discharge, a lithium battery with improved cycle life and high-rate characteristics can be manufactured.
[0081] The porous substrate constituting the separator contains a gel-like polymer electrolyte containing a liquid electrolyte and a cross-linked polymer within the pores. The gel-like polymer electrolyte may reside at the interface between the negative electrode collector and the separator. In a separator having this structure, the liquid electrolyte is contained within a cross-linked polymer network with a cross-linked structure, preventing leakage to the outside.
[0082] The gel polymer electrolyte comprises a crosslinked polymer and a liquid electrolyte, and the weight ratio of the liquid electrolyte and the crosslinked polymer is 99:1 to 90:10.
[0083] The content of the crosslinked polymer is 1 to 10 parts by weight, 1 to 8 parts by weight, 1 to 5 parts by weight, 2 to 5 parts by weight, or 3 to 5 parts by weight based on 100 parts by weight of the gel-type polymer electrolyte. When the content of the liquid electrolyte and the crosslinked polymer is within the above range, the high-temperature shrinkage characteristics of the separator can be effectively controlled.
[0084] An anode active material layer may further be included between the anode current collector and the separator. The anode active material layer may be, for example, a lithium metal thin film.
[0085] A lithium battery according to an embodiment may further include a liquid electrolyte, a solid electrolyte, or a combination thereof containing an organic solvent and a lithium salt. The liquid electrolyte may be a positive electrode electrolyte.
[0086] A protective layer may be further introduced between the negative electrode current collector and the separator. It is also possible to introduce a protective layer further between the negative electrode active material layer and the separator.
[0087] The protective layer contains a polymer such as polyvinyl alcohol, polyimide, vinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride, carboxymethyl cellulose, styrene butylene rubber, or a polymer and an inorganic filler. Inorganic fillers include, for example, SiO2, Al2O3, Al(OH)3, AlO(OH), TiO2, BaTiO3, ZnO2, Mg(OH)2, Aluminum Nitride (AlN), Silicon Carbide (SiC), Boron Nitride (BoN), or a combination thereof. Introducing an additional protective layer in this way can minimize contact between lithium and the electrolyte, thereby reducing side reactions, and can suppress lithium dendrite growth by creating a uniform flow of lithium ions throughout the electrode.
[0088] The lithium battery according to one embodiment may further include a solid electrolyte, a semi-solid gel electrolyte, or a combination thereof in addition to a gel polymer electrolyte.
[0089] The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.
[0090] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0 <a<2) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.
[0091] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1-x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x ("LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n(0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.
[0092] The above sulfide-based solid electrolyte is, for example, Li2S-P2S5, Li2S-P2S5-LiX, X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n , m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x (0 <x<2), Li 7-x PS 6-x Br x (0 <x<2), 및 Li 7-x PS 6-x I x (0 <x<2) 중에서 선택된 하나 이상을 들 수 있다.
[0093] According to another embodiment, a ceramic coating layer can be formed on both sides of the porous substrate constituting the separator.
[0094] Forming a ceramic coating layer can improve cell performance in lithium batteries by suppressing lithium dendrite formation through the rigidity of the ceramic coating layer without significantly increasing cell resistance. Furthermore, employing a separator with the aforementioned ceramic coating layer ensures heat resistance, improving heat shrinkage characteristics and reducing the separator margin for safety during cell design, thereby reducing the material cost of lithium batteries. Furthermore, by physically inhibiting dendrite growth on the anode, long-term lifespan at both room and high temperatures can be improved.
[0095] The ceramic coating layer includes inorganic particles and a binder.
[0096] Any inorganic particle that can be used when forming a coating layer of a separation membrane can be used, and for example, any one of the inorganic oxides of SiO2, Al2O3, Al(OH)3, AlO(OH), TiO2, BaTiO3, ZnO2, Mg(OH)2, AIN(Aluminum Nitride), SiC(Silicon Carbide), BoN(Boron Nitride), or a combination thereof can be used.
[0097] Inorganic particles include BaTiO3, BaTiO3, Pb(Zr,Ti)O3 (PZT), and Pb with a dielectric constant of 5 or higher. 1-a La a Zr 1-b Ti b O3 (PLZT, where, 0 <a<1, 0<b<1임), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC or a combination thereof can be used.
[0098] In addition to the ceramic coating layer, the inorganic particles having lithium ion transfer capability, i.e. lithium phosphate (Li3PO4), lithium titanium phosphate (Li c Ti d (PO4)3, 0 <d<2, 0<d<3), 리튬알루미늄티타늄포스페이트 (Li a1 Al b1 Ti c1 (PO4)3, 0 <a1<2, 0<b1<1, 0<c1<3), 14Li2O-9Al2O3-38TiO2-39P2O5 등과 같은 (LiAlTiP) a2 O b2 Series Glass (0) <a2<4, 0<b2<13), 리튬란탄티타네이트 (Li a3 La b3 TiO3, 0 <a3<2, 0<b3<3), Li 3.25 Ge 0.25 P 0.75 Lithium germanium thiophosphate (Li) such as S4 a4 Ge b4 P c2 S d , 0 <a4<4, 0<b4<1, 0<c2<1, 0<d<5), Li3N 등과 같은 리튬나이트라이드 (Li a5 N b5 , 0 <a5<4, 0<b5<2), Li3PO4-Li2S-SiS2 등과 같은 SiS2 계열 글래스 (Li a6 Si b6 S c3 , 0 <a6<3, 0<b6<2, 0<c4<4), LiI-Li2S-P2S5 등과 같은 P2S5 계열 글래스 (Li a7 P b7 S c5 , 0 <a7<3, 0<b7<3, 0<c5<7) 또는 이들의 혼합물 등이 더 함유될 수 있다
[0099] Referring to Fig. 1, a structure is obtained by stacking a separator (21) on a negative electrode current collector (11), a composition for forming a gel-type polymer electrolyte is injected therein, and the composition is cured by heat treatment, so that a gel-type polymer electrolyte (31) is arranged at the interface between the negative electrode current collector (11) and the separator (21) and in the pores of the separator. Here, the negative electrode active material layer is absent. The separator (21) is a porous substrate having a coating layer formed on the surface thereof.
[0100] There is no negative active material layer between the negative current collector (11) and the separator (21). In addition, GPE exists at the interface between the negative current collector (11) and the separator (21) through curing or crosslinking of the composition for forming a gel-type polymer electrolyte, thereby exhibiting low interfacial resistance characteristics.
[0101] A gel polymer electrolyte containing a liquid electrolyte and a crosslinked polymer is contained in the pores of a porous substrate, wherein the crosslinked polymer is a polymerization product of a crosslinking monomer. The presence of the gel polymer electrolyte in the pores of the porous substrate minimizes the interfacial resistance between the positive electrode, negative electrode, and separator, and facilitates lithium movement.
[0102] The pore diameter of the separator (21) is generally 0.01 to 10 μm, and the thickness can generally be 5 to 20 μm. As such a separator, for example, an olefin-based polymer such as polypropylene; a sheet or non-woven fabric made of glass fiber or polyethylene; or the like can be used. When a solid polymer electrolyte is used as the electrolyte, the solid polymer electrolyte can also function as a separator.
[0103] The crosslinking monomer is a material that is electrochemically stable at a voltage of about 4.3 V or higher, for example, in an operating environment of a positive electrode using a positive electrode active material having a nickel content of 90 mol% or higher. Examples of such crosslinking monomers include polyfunctional (3-substituted) methacrylates and trimethylol propane triacrylate.
[0104] The above cross-linked polymer is a polymerization product of a cross-linking monomer. Here, the polymerization product of a cross-linking monomer means a product obtained by polymerization and / or cross-linking reaction of a cross-linking monomer. Crosslinking monomers are compounds having at least three crosslinkable functional groups, for example, diethylene glycol diacrylate (DEGDA), diethylene glycol dimethacrylate (DEGDMA), triethylene glycol diacrylate (TEGDA), triethylene glycol dimethacrylate (TEGDMA), tetraethylene glycol diacrylate (TTEGDA), glycidyl methacrylate, polyethylene glycol diacrylate (PEGDA), polyethylene glycol dimethacrylate (PEGDMA), polypropylene glycol diacrylate (PPGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), dianol diacrylate (DDA), dianol dimethacrylate (DDMA), ethoxylated trimethylolpropane triacrylate (ETPTA), acrylate functionalized ethylene Acrylate-functionalized ethylene oxide, butanediol dimethacrylate, ethoxylated neopentyl glycol diacrylate (NPEOGDA), propoxylated neopentyl glycol diacrylate (NPEOGDA), trimethylol propane triacrylate (TMPTA), trimethylol propane trimethacrylate (TMPTMA), pentaerythritol triacrylate (PETA), ethoxylated propoxylated trimethylolpropane triacrylate (TMPEOTA) / (TMPPOTA), propoxylated glyceryl triacrylate, tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA), pentaerythritol tetraacrylate (PETTA),Dipentaerythritol pentaacrylate (DPEPA), ditrimethylol propane tetraacrylate (DTMPTTA); diglycidyl ester, diallyl suberate; acrylamide, divinylbenzene, or a combination thereof.
[0105] The above crosslinking monomer may have a weight average molecular weight in the range of 200 to 2,000, and may be in the range of 200 to 1,000, for example, in the range of 200 to 500. If the weight average molecular weight is less than 200, the density of crosslinking points within the molecular structure of the polymer after crosslinking may be too high, preventing free movement of the lithium salt. On the other hand, if the weight average molecular weight is greater than 2,000, the density of crosslinking points within the molecular structure of the polymer after crosslinking may be too low, reducing the electrolyte blocking ability.
[0106] Based on the total weight of the crosslinking monomer and the liquid electrolyte, the content of the crosslinking monomer is 1 to 10 parts by weight, and the content of the liquid electrolyte is 90 to 99 parts by weight. If the content of the crosslinking monomer is less than 1 part by weight, the degree of crosslinking during crosslinking is too low, so that the crosslinking characteristics cannot be sufficiently expressed, and the electrolyte moisture absorption capacity and mechanical characteristics may be poor, and if it exceeds 10 parts by weight, the internal resistance within the electrode plate increases, which may act as a cause of capacity reduction during high-rate charge / discharge.
[0107] The composition for forming the above gel-type polymer electrolyte may further include a crosslinking agent, a photoinitiator, etc. to assist in crosslinking of the crosslinkable monomer. The crosslinking agent, initiator, etc. are not particularly limited as long as they are commonly used in the relevant technical field.
[0108] The initiator can be, for example, benzoin ethyl ether.
[0109] The content of the crosslinking agent, initiator, etc. may be within a conventional range. For example, the content of the initiator may be used in a range of 0.1 to 5 parts by weight, or 0.2 to 3 parts by weight, based on 100 parts by weight of the crosslinking monomer. Using the gel polymer electrolyte formed in this way, the ionic conductivity can be maintained at a value close to that of the liquid electrolyte, and the gel polymer electrolyte inside the positive and negative electrodes can play a role in preventing leakage of the liquid electrolyte. The electrolyte can be trapped in the polymer matrix of the gel polymer electrolyte and maintained within the polymer matrix, thereby helping the smooth movement of lithium ions. In addition, the excellent electrochemical properties of the polymer can suppress the electrolyte decomposition reaction within the range of -1 V to 5 V.
[0110] Among the above separation membranes (21), specific examples of olefin-based polymers may include polyethylene, polypropylene, or a multilayer membrane of two or more layers thereof, and mixed multilayer membranes such as a polyethylene / polypropylene two-layer separation membrane, a polyethylene / polypropylene / polyethylene three-layer separation membrane, and a polypropylene / polyethylene / polypropylene three-layer separation membrane may be used.
[0111] A coating layer may be disposed on at least one surface of the porous substrate.
[0112] A positive electrode is placed. The positive electrode (10) contains a positive electrode active material layer (12) and a positive electrode current collector (11).
[0113] The ceramic coating layer contains inorganic particles. By containing these inorganic particles, a ceramic coating layer with excellent film strength can be formed, effectively suppressing the growth of lithium dendrites formed between the negative electrode current collector and the separator.
[0114] The inorganic particles may contain small-diameter inorganic particles, large-diameter inorganic particles, or a combination thereof. The average particle diameter of the small-diameter inorganic particles is 50 nm to 500 nm, 70 nm to 400 nm, 80 nm to 450 nm, or 100 nm to 300 nm, and the average particle diameter of the large-diameter inorganic particles is 1 um to 10 um, 2 to 9 um, 4 um to 8 um, or 5 to 7 um. When the average particle diameters of the large-diameter inorganic particles and the small-diameter inorganic particles are within the above ranges, dendrite growth can be effectively suppressed.
[0115] The ceramic coating layer further includes a binder, and the binder includes polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butylene rubber, acrylic polymer, fluoroelastomer, or a combination thereof. The content of the binder is 5 to 20 parts by weight based on 100 parts by weight of the total weight of the large-diameter inorganic particles and the small-diameter inorganic particles. When the content of the binder is within the above range, the bonding strength of the ceramic coating layer to the porous substrate is excellent.
[0116] The liquid electrolyte contains a lithium salt and an organic solvent.
[0117] In a lithium battery according to an embodiment, a liquid electrolyte is imbibed in a polymer matrix as a gel-type polymer electrolyte, so that there is no leakage, and electrochemical side reactions and electrolyte decomposition reactions occurring at the positive and negative electrodes are suppressed, thereby ensuring stability and improving battery characteristics.
[0118] As the above non-aqueous solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxy franc, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolan, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxy methane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl pyrropionate, ethyl propionate, etc. can be used. Carbonate solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, and diethyl carbonate can be used.
[0119] The above lithium salt can be any one that is commonly used in lithium secondary batteries, and as a material that is easily dissolved in the non-aqueous solvent, for example, one or more of the following materials can be used: LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2)3, LiC(FSO2)3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, and LiB(C2O4)2.
[0120] The concentration of the lithium salt may be, for example, 1 to 5 M, for example, 1 to 2.5 M, in the organic electrolyte. In the above range, a sufficient amount of lithium ions required for charging and discharging a lithium secondary battery can be generated.
[0121] A layer of negative active material can be placed between the negative current collector and the separator.
[0122] According to one embodiment, the negative electrode active material layer may be disposed during the assembly of the lithium battery. According to another embodiment, the negative electrode active material layer may include a negative electrode active material layer by plating lithium metal after charging. The negative electrode active material layer may be a plated lithium layer.
[0123] The above negative electrode active material layer (22) includes lithium metal or a lithium alloy.
[0124] The thickness of the negative electrode active material layer may be 1 to 500 μm, 5 to 500 μm, 10 μm to 30 μm, or 10 μm to 25 μm. When the thickness of the negative electrode active material layer is within the above range, the cycle characteristics of the lithium battery are improved without reducing the energy density.
[0125] When the negative electrode active material layer is placed at the time of assembly, it may include only a carbon-based material, a carbon-based material, and at least one selected from metals and metalloids.
[0126] The carbon-based material includes amorphous carbon, and the average particle diameter of the amorphous carbon is 10 nm to 100 nm, and the carbon-based material includes carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, or a combination thereof.
[0127] The above negative active material layer includes a lithium metal foil, a lithium metal powder, a lithium alloy foil, a lithium alloy powder, or a combination thereof, wherein the lithium alloy contains lithium and a first metal.
[0128] The first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof.
[0129] The negative electrode active material layer (22) may include, for example, lithium foil, lithium powder, or a combination thereof. The lithium foil may include, for example, lithium metal foil, lithium alloy foil, or a combination thereof. The lithium powder may include lithium metal powder, lithium alloy powder, or a combination thereof. A lithium alloy is an alloy of lithium and another metal that can be alloyed with lithium, such as a lithium-silver alloy, a lithium-zinc alloy, a lithium-magnesium alloy, or a lithium-tin alloy. The negative electrode active material layer including a lithium metal foil may be, for example, a lithium metal layer. The negative electrode active material layer including a lithium alloy foil may be, for example, a lithium alloy layer. The negative electrode active material layer including a lithium metal powder and / or a lithium alloy powder may be introduced by coating a slurry including lithium powder and a binder, etc., on a negative electrode current collector. The binder may be, for example, a fluorine-based binder such as polyvinylidene fluoride (PVDF). The negative electrode active material layer may not include a carbon-based negative electrode active material. Therefore, the negative electrode active material layer can be made of a metal-based negative electrode active material.
[0130] The negative electrode current collector is composed of a material that does not react with lithium, i.e., does not form an alloy or compound. The material constituting the negative electrode current collector includes, but is not limited to, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), and any material that is used as an electrode current collector in the relevant technical field may be used. The negative electrode current collector may be composed of one of the above-mentioned metals, or may be composed of an alloy or a coating material of two or more metals. The negative electrode current collector is, for example, in the form of a plate or foil.
[0131] In one embodiment of the present invention, the negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof.
[0132] The metal layer can act as an electrochemical fuse and cut off in the event of an overcurrent, thereby preventing a short circuit. The limit current and maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer can be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or maximum current of the negative electrode current collector decreases, thereby improving the stability of the lithium battery in the event of a short circuit. A lead tab can be added to the metal layer for external connection. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal layer melts, thereby electrically connecting the metal layer to the lead tab. To strengthen the welding between the metal layer and the lead tab, a metal piece can be added between the metal layer and the lead tab. The metal piece can be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, an aluminum foil, a copper foil, a SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate by welding the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced.The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the welding process of the lead tab. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to μm. Since the metal layer has a thickness within this range, conductivity can be maintained while ensuring the stability of the electrode assembly. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure as the negative electrode collector, the weight of the electrode can be reduced, and as a result, the energy density can be improved.
[0133] In one embodiment of the present invention, the positive electrode current collector may include, for example, a base film and a metal layer disposed on one or both surfaces of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may be liquefied when a short circuit occurs, thereby suppressing a sudden increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may additionally include a metal piece and / or a lead tab. For more specific details regarding the base film, metal layer, metal piece, and lead tab of the positive electrode current collector, refer to the negative electrode current collector described above. By having this structure, the positive electrode current collector can reduce the weight of the electrode, thereby improving energy density.
[0134] The positive electrode current collector (11) may additionally include a metal piece and / or a lead tab. For more specific details regarding the base film, metal layer, metal piece, and lead tab of the positive electrode current collector (11), refer to the negative electrode current collector (21) described above. By having such a structure, the positive electrode current collector (11) can reduce the weight of the electrode and consequently improve the energy density.
[0135] The negative electrode active material layer may contain a negative electrode active material and a binder.
[0136] The negative active material has, for example, a particle form. The average particle diameter of the negative active material having a particle form is, for example, 10 nm to 4 ㎛, 10 nm to 1 ㎛, 10 nm to 500 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the negative active material has an average particle diameter in this range, reversible plating and / or dissolution of lithium can be facilitated during charge and discharge. The average particle diameter of the negative active material is, for example, a median diameter (D50) measured using a laser particle size distribution analyzer.
[0137] The negative electrode active material may include, for example, at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material. The carbon-based negative electrode active material may be, for example, amorphous carbon. Examples of the carbon-based negative electrode active material include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., and any material classified as amorphous carbon in the relevant technical field may be used. Amorphous carbon is carbon that has no crystallinity or very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon. The metal or metalloid negative electrode active material includes, but is not limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the relevant technical field may be used. For example, nickel (Ni) does not form an alloy with lithium, and therefore is not a metal negative electrode active material in the present specification. The negative electrode active material layer includes a type of negative electrode active material among these negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the negative electrode active material layer may include a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture may be, for example, 10:1 to 1:2, 10:1 to 1:1, 7:1 to 1:1, 5:1 to 1:1, or 4:1 to 2:1 by weight.The negative electrode active material included in the negative electrode active material layer may include a mixture of first particles made of, for example, amorphous carbon and second particles made of a metal or a metalloid. The metal includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt% based on the total weight of the mixture. When the second particles have a content in this range, the cycle characteristics of, for example, a lithium battery are further improved.
[0138] The binder included in the negative electrode active material layer may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders. When the negative electrode active material layer does not include a binder, the negative electrode active material layer can be easily separated from the ceramic coating layer (21) or the negative electrode current collector (21). The content of the binder included in the negative electrode active material layer may be, for example, 1 to 20 wt% based on the total weight of the negative electrode active material layer.
[0139] The thickness of the negative electrode active material layer may be, for example, 1 ㎛ to 20 ㎛, 1 ㎛ to 15 ㎛, or 2 ㎛ to 10 ㎛, or 3 ㎛ to 7 ㎛. The thickness of the negative electrode active material layer may be, for example, 1% to 50%, 1% to 30%, 1% to 10%, or 1% to 5% of the thickness of the positive electrode active material layer. If the thickness of the negative electrode active material layer is too thin, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium battery. If the thickness of the negative electrode active material layer is excessively increased, the energy density of the lithium battery employing the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics.
[0140] If the thickness of the negative electrode active material layer decreases, for example, the charge capacity of the negative electrode active material layer also decreases. The charge capacity of the negative electrode active material layer may be, for example, 0.1% to 50%, 1% to 30%, 1% to 10%, 1% to 5%, or 1% to 2% of the charge capacity. If the charge capacity of the negative electrode active material layer is too small, lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the lithium battery. If the charge capacity of the negative electrode active material layer increases excessively, the energy density of the lithium battery using the negative electrode (20) may decrease, and it may be difficult to improve the cycle characteristics. The charge capacity of the positive electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer. When multiple types of positive electrode active materials are used, the charge capacity density × mass value is calculated for each positive electrode active material, and the sum of these values is the charge capacity of the positive electrode active material layer. The charge capacity of the negative electrode active material layer is calculated in the same way. That is, the charge capacity of the negative electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode active material layer. When multiple types of negative electrode active materials are used, the charge capacity density × mass value is calculated for each negative electrode active material, and the sum of these values is the capacity of the negative electrode active material layer. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is the capacity estimated using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer and the negative electrode active material layer are directly measured by measuring the charge capacity using an all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer and the negative electrode active material layer may be the initial charge capacity measured at the first charge cycle.
[0141] [Lithium battery]
[0142] According to one embodiment, a lithium battery includes a positive electrode; a negative electrode; and a separator disposed between the positive electrode and the negative electrode. Such a lithium battery can simultaneously provide excellent life characteristics. The lithium battery may be, but is not limited to, a lithium primary battery, a lithium secondary battery, a lithium-sulfur battery, a lithium-air battery, etc., and any lithium battery used in the relevant technical field may be used.
[0143] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.
[0144] (anode)
[0145] First, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly coated and dried on an aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon. Alternatively, the positive electrode active material composition is cast on a separate support, and then the film obtained by peeling from the support is laminated on the aluminum current collector to produce a positive electrode plate having a positive electrode active material layer formed thereon.
[0146] The cathode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c(In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G dO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤
[0147] 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) A compound represented by any one of the chemical formulas Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used.
[0148] In the chemical formula representing the above-described compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-described compound, or it is also possible to use a mixture of the above-described compound and the compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes a coating element compound of, for example, an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since the specific coating method is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0149] The cathode active material is, for example, Li a Ni x Co y M z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0 <y≤0.3, 0<z≤0.3, 및 x+y+z=1이고, M은 망간(Mn), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1), LiNi x Co y Mn z Al w O2(0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1), Li a Co x M y O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof), Li a Ni x Mn y M' z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M'는 코발트(Co), 니오븀(Nb), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al), 보론(B) 또는 이들의 조합이고, A는 F, S, Cl, Br 또는 이들의 조합), Li a M1 x M2 y PO 4-b X b (Here, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며, M1이 크롬(Cr), 망간(Mn), 철(Fe), 코발트(Co), 니켈(Ni), 구리(Cu), 지르코늄(Zr) 또는 이들의 조합이며, M2가 마그네슘(Mg), 칼슘(Ca), 스트론튬(Sr), 바륨(Ba), 티탄(Ti), 아연(Zn), 보론(B), 니오븀(Nb), 갈륨(Ga), 인듐(In), 몰리브덴(Mo), 텅스텐(W), 알루미늄(Al), 실리콘(Si), 크롬(Cr), 바나듐(V), 스칸듐(Sc), 이트륨(Y) 또는 이들의 조합이며, X가 O, F, S, P 또는 이들의 조합), Li a M3 z PO4 (0.90≤a≤1.1, 0.9≤z≤1.1, and M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof).
[0150] The conductive material may include, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any conductive material used in the relevant technical field may be used. Alternatively, the anode may not include a separate conductive material, for example.
[0151] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymer, etc. are used, and as the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.
[0152] It is also possible to form pores inside the electrode plate by further adding a plasticizer or a pore forming agent to the positive electrode active material composition.
[0153] The contents of the cathode active material, conductive agent, binder, and solvent used in the cathode are at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the conductive agent, binder, and solvent may be omitted.
[0154] The binder content included in the positive electrode may be 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content included in the positive electrode may be 80 wt% to 99 wt%, 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.
[0155] The positive electrode current collector is, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may be omitted. The thickness of the positive electrode current collector is, for example, 1 ㎛ to 100 ㎛, 1 ㎛ to 50 ㎛, 5 ㎛ to 25 ㎛, or 10 ㎛ to 20 ㎛.
[0156] The positive electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. By having such a structure, the positive electrode current collector can reduce the weight of the electrode and consequently improve the energy density of the lithium battery.
[0157] (Separator)
[0158] Next, a separator to be inserted between the anode and cathode is prepared.
[0159] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion transport and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in nonwoven or woven form. For lithium-ion batteries, rollable separators, such as polyethylene or polypropylene, are used, while for lithium-ion polymer batteries, separators with excellent organic electrolyte absorption capacity are used.
[0160] The membrane is manufactured by the following exemplary method, but is not limited to this method and may be adjusted according to required conditions.
[0161] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast onto a support and dried, and then a separator film peeled from the support is laminated onto the electrode to form a separator.
[0162] The polymer used in membrane manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.
[0163] (cathode)
[0164] The cathode contains a cathode current collector.
[0165] In one embodiment of the present invention, the negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film can be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse, which may be cut in the event of an overcurrent to prevent a short circuit. The limit current and maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer may be plated or deposited on the base film. As the thickness of the metal layer decreases, the limit current and / or maximum current of the negative electrode current collector (521b, 522b) decrease, thereby improving the stability of the lithium battery in the event of a short circuit. A lead tab may be added on the metal layer for external connection. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. During welding, the base film and / or the metal layer may be melted, electrically connecting the metal layer to the lead tab. In order to strengthen the welding of the metal layer and the lead tab, a metal piece may be added between the metal layer and the lead tab. The metal piece may be a thin piece of the same material as the metal of the metal layer.The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, an aluminum foil, a copper foil, a SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate by welding the lead tab. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film may be, for example, 100°C to 300°C, 100°C to 250°C, or 100°C to 200°C. Since the base film has a melting point within this range, the base film can be melted and easily bonded to the lead tab during the welding process. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to ㎛. Since the metal layer has a thickness within this range, the stability of the electrode assembly can be secured while maintaining conductivity. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure, the negative electrode current collector (521b, 522b) can reduce the weight of the electrode and consequently improve the energy density.
[0166] A negative electrode active material layer may be formed on the negative electrode current collector. The negative electrode active material layer may be formed as a lithium deposition layer after charging. Alternatively, the negative electrode active material layer may be formed using a negative electrode active material during battery assembly.
[0167] The method of forming a negative electrode active material layer using a negative electrode active material can be manufactured in the same manner as described above, except that the negative electrode active material is used instead of the positive electrode active material when forming the positive electrode active material layer.
[0168] A lithium battery may further include, for example, a thin film comprising an element capable of forming an alloy with lithium on one surface of an anode current collector. The thin film is disposed between the anode current collector and the anode active material layer. The thin film includes, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium includes, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., and any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of one of these metals or an alloy of several types of metals. By disposing the thin film on one surface of the anode current collector, for example, the deposition shape of the first anode active material layer deposited between the thin film and the anode active material layer becomes flatter, and the cycle characteristics of the lithium battery may be further improved.
[0169] (Separator)
[0170] A separation membrane according to the embodiment is used.
[0171] Organic electrolytes are manufactured, for example, by dissolving lithium salts in organic solvents.
[0172] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0173] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a mixture thereof. The concentration of the lithium salt is, for example, 0.1 M to 5.0 M.
[0174] A lithium battery according to an embodiment may further include a solid electrolyte. The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.
[0175] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), Li3PO4, Li x Ti y(PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 A garnet-type solid electrolyte selected from (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10).
[0176] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1??x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x( "LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5( An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n(0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.
[0177] (lithium battery)
[0178] Referring to FIG. 4, a lithium battery (1) according to an embodiment includes a positive electrode (3), a negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0179] Referring to FIG. 5, a lithium battery (1) according to an embodiment includes a positive electrode (3), a negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.
[0180] Referring to FIG. 6, a lithium battery (1) according to an embodiment includes a positive electrode (3), a negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2) to form a battery structure. The battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, and may be, for example, a cylindrical shape, a thin film shape, etc.
[0181] In the lithium batteries of FIGS. 4 to 6, the gel-type polymer electrolyte is not shown, but exists between the separator (4) and the positive electrode (3).
[0182] A pouch-type lithium battery corresponds to the lithium batteries of FIGS. 5 and 6, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0183] The lithium battery of the present disclosure has excellent discharge capacity and lifespan characteristics, as well as high energy density, and is therefore used in, for example, electric vehicles (EVs). For example, it is used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). It is also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.
[0184] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0185] [Method for manufacturing lithium batteries]
[0186] According to one embodiment, a lithium battery can be manufactured through the steps of: preparing a negative electrode current collector; arranging a separator on one surface of the negative electrode current collector to manufacture a negative electrode current collector / separator structure; injecting a composition for forming a gel-type polymer electrolyte into the negative electrode current collector / separator structure and heat-treating the composition to manufacture a gel-type polymer electrolyte-containing integral negative electrode current collector / separator structure; preparing a positive electrode; arranging a positive electrode on top of the gel-type polymer electrolyte-containing integral negative electrode current collector / separator structure to form a battery structure; and housing the battery structure in a battery case.
[0187] The composition for forming the above gel-type polymer electrolyte comprises a crosslinking monomer, a lithium salt, an organic solvent, and an initiator.
[0188] The step of injecting the composition for forming a gel-type polymer electrolyte into the battery structure may be performed as an impregnation step under vacuum so that the composition can sufficiently penetrate into the pores of the porous substrate.
[0189] Methods for forming a gel-type polymer electrolyte include curing using heat, UV, or high-energy radiation (electron beam, γ-ray). The curing reaction using heat can be carried out at a temperature of 40°C to 120°C, 45°C to 100°C, for example, 50°C to 90°C for 30 to 180 minutes.
[0190] The above heat treatment varies depending on the type of crosslinking monomer, but is performed at, for example, 40°C to 120°C. When the heat treatment is performed within the above-described range, a lithium battery having an excellent function of suppressing high-temperature shrinkage of the separator can be manufactured.
[0191] In the step of housing the battery case in the above battery structure, a liquid electrolyte containing a lithium salt and an organic solvent can be injected. In addition, a step of further including at least one selected from a negative electrode active material layer and a protective layer between the negative electrode current collector and the separator can be performed.
[0192] A lithium battery according to an embodiment is, for example, a lithium ion battery or a lithium metal battery.
[0193] A lithium battery according to an embodiment of the present invention can have a structure in which the cathode / separator / negative electrode are separated after repeated charging and discharging after battery assembly, so that the separator and negative electrode are separated, and the cathode and separator remain integral.
[0194] The present invention is explained in more detail through the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0195] Example 1: 3% content of cross-linked polymer in gel polymer electrolyte (GPE)
[0196] A cross-section of a 20㎛ thick polyethylene single-layer substrate film used as a porous substrate
[0197] A negative electrode collector / separator structure was prepared by laminating a separator on a copper foil with a thickness of 10 μm, which is a negative electrode collector.
[0198] A composition for forming a gel-type polymer electrolyte was injected into the above structure, and the structure was heat-treated at about 70°C for about 120 minutes to undergo a thermal curing process, thereby manufacturing a negative electrode current collector / separator structure having an integrated structure containing a gel-type polymer electrolyte (GPE).
[0199] A lithium metal battery was manufactured by stacking a positive electrode on top of the above structure, placing it in a battery case, and supplying a liquid electrolyte.
[0200] In the gel-type polymer electrolyte, the content of the crosslinking polymer is 3 wt% based on the total content of the liquid electrolyte and the crosslinking polymer. The composition for forming the gel-type polymer electrolyte was prepared by mixing trimethylolpropane triacrylate (TMPTA) as a crosslinking monomer, a mixed solvent (weight ratio 1:1:0.5) of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in which 1.3 M LiPF6 was dissolved as a liquid electrolyte, and benzoin ethyl ether (Sigma-Aldrich, 240.30 g / mol) as an initiator. The composition for forming the gel-type polymer electrolyte includes 97 parts by weight of the crosslinking monomer and the liquid electrolyte based on 100 parts by weight of the total weight of the composition, and the initiator was used in an amount of 3 parts by weight based on 100 parts by weight of the crosslinking monomer.
[0201] The above anode was manufactured according to the following method.
[0202] Li 1.04 Ni 0.88 Co 0.1 Al 0.02 O2 powder and carbon conductive material (Super-P; Timcal Ltd.) were uniformly mixed at a weight ratio of 90:5, and then a PVDF (polyvinylidene fluoride) binder solution was added to prepare a positive electrode active material slurry with a weight ratio of active material:carbon conductive material:binder = 90:5:5.
[0203] The manufactured slurry was coated on a 15 ㎛ thick aluminum substrate using a doctor blade, dried under reduced pressure at 120°C, and rolled using a roll press to form a sheet to manufacture a positive electrode.
[0204] In the above lithium battery, the pores of the separator contain a gel-type polymer electrolyte, and the negative electrode current collector / separator has an integrated structure.
[0205] Example 2
[0206] A lithium battery was manufactured in the same manner as in Example 1, except that the content of the crosslinking monomer in the composition for forming a gel-type polymer electrolyte was changed to 5 parts by weight based on 100 parts by weight of the composition so that the content of the crosslinking polymer in the gel-type polymer electrolyte was 5 wt% based on the total content of the gel-type polymer electrolyte.
[0207] Example 3
[0208] A lithium battery was manufactured in the same manner as in Example 1, except that the content of the crosslinking monomer in the composition for forming a gel-type polymer electrolyte was changed to 10 parts by weight based on 100 parts by weight of the composition so that the content of the crosslinking polymer in the gel-type polymer electrolyte was 10% by weight based on the total content of the gel-type polymer electrolyte.
[0209] Example 4
[0210] A lithium battery was manufactured in the same manner as in Example 1, except that the content of the crosslinking monomer in the composition for forming a gel-type polymer electrolyte was changed to 8 parts by weight based on 100 parts by weight of the composition so that the content of the crosslinking polymer in the gel-type polymer electrolyte was 8 wt% based on the total content of the gel-type polymer electrolyte.
[0211] Example 5
[0212] A lithium battery was manufactured in the same manner as in Example 1, except that polyethylene glycol dimethacrylate was used instead of trimethylolpropane triacrylate as a crosslinking monomer in the manufacture of a gel-type polymer electrolyte.
[0213] Comparative Example 1
[0214] A cross-section of a 5.5㎛ thick polyethylene single-layer substrate film used as a porous substrate
[0215] The composition for forming a gel-type polymer electrolyte manufactured in Example 1 was injected and heat-treated at 70°C for 120 minutes to manufacture a gel-type polymer electrolyte on one side of a separator. A copper foil with a thickness of 10 μm, which serves as a negative electrode current collector, was laminated on the other side of the separator.
[0216] Next, a positive electrode was laminated on top of the gel-type polymer electrolyte to manufacture a laminate. This laminate was placed in a battery case and a liquid electrolyte was supplied to manufacture a lithium battery.
[0217] The positive electrode was the same as that of Example 1, and the liquid electrolyte of Example 1 was used as the liquid electrolyte.
[0218] In the above lithium battery, the negative electrode current collector and separator have a separate structure. The content of the cross-linked polymer in the gel-type polymer electrolyte is 3 wt% based on the total weight of the gel-type polymer electrolyte.
[0219] Comparative Example 2
[0220] A lithium battery was manufactured in the same manner as in Comparative Example 1, except that the content of the crosslinked polymer in the gel-type polymer electrolyte was changed to 3 wt% based on the total weight of the gel-type polymer electrolyte.
[0221] Comparative Example 3
[0222] A lithium battery was manufactured in the same manner as in Comparative Example 1, except that the content of the crosslinked polymer in the gel-type polymer electrolyte was changed to 5 wt% based on the total weight of the gel-type polymer electrolyte.
[0223] Comparative Example 4
[0224] A lithium battery was manufactured in the same manner as in Comparative Example 1, except that the content of the crosslinked polymer in the gel-type polymer electrolyte was changed to 10 wt% based on the total weight of the gel-type polymer electrolyte.
[0225] Evaluation Example 1: Membrane heat shrinkage experiment
[0226] The integrated negative electrode collector / separator structure manufactured in Example 1 and the separate negative electrode collector / separator structure manufactured in Comparative Example 1 were stored in a chamber at 140°C or 150°C for 1 hour, and then the degree of shrinkage was measured, and the results are shown in FIGS. 2 and 3.
[0227] Figure 2 shows the results of a heat shrinkage test after storage at 140°C for 1 hour, and Figure 3 shows the results of a heat shrinkage test after storage in a chamber at 150°C for 1 hour.
[0228] With reference to this, when the integrated negative electrode collector / separator structure of Example 1 was cured with a gel polymer electrolyte (GPE) as an integrated separator / substrate (negative electrode collector), the heat shrinkage prevention effect was greater than that of Comparative Example 1 when the separator was immersed in GPE and cured, and then placed together with the negative electrode collector as a substrate and a heat export test was performed, so that the stability was improved.
[0229] Evaluation Example 2: Initial interfacial adhesion
[0230] The initial interfacial adhesion between the negative electrode current collector and the separator in the lithium batteries of Examples 1 to 5 and Comparative Examples 1 to 4 was evaluated. The results are shown in Table 3.
[0231] The initial interfacial adhesion was evaluated by fixing a tape (26 mm x 76 mm) on top of the cathode substrate-integrated separator and measuring the peel strength by pulling the end of the tape and cathode substrate in a T shape at a speed of 60 mm / min and a load of 0.5 kgf using Instron 3342 equipment.
[0232] Initial interfacial adhesion (gf / cm) Example 10.33 Example 20.33 Example 30.38 Example 40.43 Example 50.56 Comparative Example 10.10 Comparative Example 20.09 Comparative Example 30.12 Comparative Example 40.14
[0233] Referring to Table 1, it was found that the initial interfacial adhesion between the negative electrode collector and the separator in the structures of Examples 1 to 5 was significantly improved compared to the structures of Comparative Examples 1 to 4.
[0234] Evaluation Example 3: Interfacial adhesive strength before and after charging and discharging
[0235] Lithium batteries manufactured according to Examples 1 to 5 and Comparative Examples 1 to 4 were charged and discharged under the following conditions.
[0236] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) during discharge (formation cycle).
[0237] The lithium battery, which had undergone a Mars cycle, was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle). These cycles are 100 th The cycle was repeated under the same conditions.
[0238] In every charge / discharge cycle, a 10-minute pause was provided after each charge / discharge cycle.
[0239] After performing charge and discharge, the interfacial adhesive strength of the negative electrode collector and the separator in the lithium batteries manufactured according to Example 1-5 and Comparative Example 1-4 was evaluated according to the same method as described in Evaluation Example 2, and the evaluation results are shown in Table 2 below.
[0240] Interfacial adhesive strength (gf / cm) before and after charging and discharging Example 10.11 Example 20.13 Example 30.17 Example 40.21 Example 50.29 Comparative Example 1 N / A Comparative Example 20.02 Comparative Example 30.05 Comparative Example 40.08
[0241] Referring to Table 2, the adhesive strength of the negative electrode collector and separator manufactured by Examples 1 to 5 was improved compared to Comparative Examples 1 to 4 even after charge and discharge.
[0242] Evaluation Example 3: Lifespan at room temperature (25℃)
[0243] The charge / discharge characteristics of the lithium batteries of Example 1-5 and Comparative Example 1-4 were evaluated under the following conditions.
[0244] The battery was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.2 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.2 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) during discharge (formation cycle).
[0245] The lithium battery, which had undergone a Mars cycle, was charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) (1 st cycle). These cycles are 100 th The cycle was repeated under the same conditions.
[0246] In all charge / discharge cycles, a 10-minute pause was observed after each charge / discharge cycle. Some of the results of the room-temperature charge / discharge experiments are shown in Table 3.
[0247] The capacity retention rate is defined by the following equation 1.
[0248] <Formula 1>
[0249] Capacity retention rate [%] = [100 th Discharge capacity in cycles / 1 st Discharge capacity in cycle] × 100
[0250] Capacity retention rate [%] Capacity retention rate [%] Example 181.2 Comparative example 162.4 Example 282.3 Comparative example 268.3 Example 373.5 Comparative example 3 < 10 Example 459.8 Comparative example 4 < 10 Example 570.2
[0251] As shown in Table 3, the lithium batteries of Examples 1 to 5 showed improved capacity retention characteristics compared to Comparative Examples 1 to 4. This result is because the negative electrode current collector, separator, and gel polymer electrolyte have an integrated structure, which improves the thermal stability of the separator and reduces the interfacial resistance.
[0252] Evaluation Example 4: High-rate characteristics
[0253] The first and second charge / discharge and cycle charge / discharge were performed at 25°C for lithium batteries manufactured according to Examples 1 to 4 and Comparative Examples 1 and 2.
[0254] The batteries manufactured according to Examples 1 to 4 and Comparative Example 1 were each CC charged at 0.1 C to 4.7 V and then discharged at a constant current of 0.1 C to 2.5 V.
[0255] From the second charge, after charging at 4.6 V CC / CV 0.5 C, the battery was charged to 0.05 C current, and then discharged at 2.5 V 0.2 C / 1 C / 2 C. The cycle evaluation was performed by charging at 4.6 V CC 1 C and then discharging at 2.5 V 1 C 50 times.
[0256] The above-described cycle was performed 50 times.
[0257] The high-rate characteristic is expressed by Equation 2 below.
[0258] [Formula 2]
[0259] High-rate characteristics = {(2C discharge capacity) / (0.2C discharge capacity)} × 100
[0260] The high-rate characteristics obtained as a result of the charge-discharge characteristic evaluation for the lithium battery manufactured according to the above Example 1-4 and Comparative Example 1-2 are shown in Table 4 below.
[0261] Distinction ratio characteristics (2C / 0.2C) (%) Example 10.65 Example 20.62 Example 30.21 Example 40.11 Comparative example 10.43 Comparative example 20.42
[0262] From Table 4 above, the high-rate characteristics of the lithium battery manufactured according to Example 1-4 show improved results compared to the lithium battery of Comparative Example 1-2.
[0263] While exemplary embodiments have been described in detail with reference to the attached drawings, the present invention is not limited to these examples. It is self-evident that those skilled in the art to which the present invention pertains can devise various modifications or variations within the scope of the technical concepts described in the patent claims, and these also naturally fall within the technical scope of the present invention.
Claims
1. A lithium battery in which a negative electrode collector, a separator, and a positive electrode are sequentially arranged. There is no negative active material layer or protective layer between the negative electrode current collector and the separator. The above negative electrode collector and separator are an integrated structure, A lithium battery having an initial adhesive strength at the interface between the negative electrode current collector and the separator of the above-mentioned integrated structure of 0.15 gf / cm to 1.0 gf / cm.
2. In the first paragraph, the separator is a lithium battery made of polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, polyvinylidene fluoride, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride hexafluoropropylene copolymer, or a combination thereof.
3. A lithium battery in accordance with paragraph 1, wherein the adhesive strength of the interface between the negative electrode current collector and the separator of the integrated structure before and after charging and discharging of the lithium battery is 0.1 to 0.3 gf / cm.
4. A lithium battery in which a gel-type polymer electrolyte is disposed at the interface between the negative electrode current collector and the separator in the first paragraph.
5. A lithium battery in accordance with claim 1, wherein a gel-type polymer electrolyte exists in the pores of the separator.
6. In the fourth paragraph, the gel-type polymer electrolyte is a lithium battery comprising a liquid electrolyte containing an organic solvent and a lithium salt and a crosslinked polymer.
7. A lithium battery in accordance with claim 6, wherein the weight ratio of the liquid electrolyte and the crosslinked polymer is 99:1 to 90:
10.
8. In the 6th paragraph, the crosslinked polymer is a polymerization product of a crosslinkable monomer, The above crosslinking monomers are diethylene glycol diacrylate (DEGDA), diethylene glycol dimethacrylate (DEGDMA), triethylene glycol diacrylate (TEGDA), triethylene glycol dimethacrylate (TEGDMA), tetraethylene glycol diacrylate (TTEGDA), glycidyl methacrylate, polyethylene glycol diacrylate (PEGDA), polyethylene glycol dimethacrylate (PEGDMA), polypropylene glycol diacrylate (PPGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA), dianol diacrylate (DDA), dianol dimethacrylate (DDMA), trimethylolpropane triacrylate (TMPTA), ethoxylated trimethylolpropane triacrylate (ETPTA), Acrylate-functionalized ethylene oxide, butanediol dimethacrylate, ethoxylated neopentyl glycol diacrylate (NPEOGDA), propoxylated neopentyl glycol diacrylate (NPEOGDA), trimethylol propane triacrylate (TMPTA), trimethylol propane trimethacrylate (TMPTMA), pentaerythritol triacrylate (PETA), ethoxylated propoxylated trimethylolpropane triacrylate (TMPEOTA) / (TMPPOTA), propoxylated glyceryl triacrylate, tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA), pentaerythritol tetraacrylate (PETTA), Dipentaerythritol pentaacrylate (DPEPA), ditrimethylol propane tetraacrylate (DTMPTTA);Diglycidyl ester, diallyl suberate; acrylamide, divinylbenzene or a combination thereof, lithium battery.; 9. In the first paragraph, the lithium battery further includes a liquid electrolyte, a solid electrolyte, a semi-solid gel electrolyte, or a combination thereof containing a lithium salt and an organic solvent, The above liquid electrolyte is a positive electrode electrolyte, a lithium battery.
10. In the first paragraph, a negative electrode active material layer is further included between the negative electrode current collector and the separator, A lithium battery, wherein the thickness of the negative electrode active material layer is 1 ㎛ to 500 ㎛.
11. A lithium battery in accordance with claim 10, wherein the negative electrode active material layer comprises lithium metal foil, lithium metal powder, lithium alloy foil, lithium alloy powder, or a combination thereof, wherein the lithium alloy contains lithium and a first metal.
12. In the 11th paragraph, the first metal is indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), silver (Ag), zinc (Zn), nickel, iron, cobalt, chromium, cesium, sodium, potassium, calcium, yttrium, bismuth, tantalum, hafnium, barium, vanadium, strontium, lanthanum, or a combination thereof, a lithium battery.
13. A lithium battery according to claim 1, wherein the integrated structure is a gel-type polymer electrolyte-containing integrated negative electrode collector / separator structure.
14. In the first paragraph, the integral structure, A lithium battery, comprising: a step of preparing a negative current collector; a step of arranging a separator on one side of the negative current collector to manufacture a negative current collector / separator structure; and a product obtained by injecting a gel-type polymer electrolyte forming composition containing a crosslinking monomer, a lithium salt, an organic solvent, and a polymerization initiator into the negative current collector / separator structure and performing a heat treatment.
15. A lithium battery further comprising a protective layer between the negative electrode current collector and the separator in the first paragraph.
16. In the first paragraph, the positive electrode includes a positive electrode current collector and a positive electrode active material layer, At least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film contains a polymer, The above polymer includes polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, A lithium battery, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
17. Step of preparing the negative electrode collector; A step of manufacturing a negative electrode collector / separator structure by placing a separator on one side of a negative electrode collector; A step of manufacturing an integrated negative electrode current collector / separator structure containing a gel-type polymer electrolyte by injecting a composition for forming a gel-type polymer electrolyte into a negative electrode current collector / separator structure and performing heat treatment; and Steps to prepare the anode; A step of forming a battery structure by placing a positive electrode on top of an integrated negative electrode collector / separator structure containing a gel-type polymer electrolyte; and A method for manufacturing a lithium battery, including a step of housing the above battery structure in a battery case.
18. A method for manufacturing a lithium battery according to claim 17, wherein the heat treatment is performed at 40°C to 120°C.
19. A method for manufacturing a lithium battery according to claim 17, wherein the composition for forming the gel-type polymer electrolyte comprises a crosslinking monomer, a lithium salt, an organic solvent, and an initiator.
20. In the 17th paragraph, in the step of housing the battery case in the battery structure, a liquid electrolyte containing a lithium salt and an organic solvent is injected, A method for manufacturing a lithium battery further comprising at least one selected from a negative electrode active material layer and a protective layer between the negative electrode current collector and the separator.
Citation Information
Patent Citations
Lithium secondary battery
KR100670483B1
Producing method of lithium polymer secondary battery
KR1020010092192A
Nonvolatile memory apparatus and memory system using the same
KR1020210000057A
Water cooled air conditoner
KR102076274B1
Current collector for positive electrodes
KR102424631B1