Electrolyte for anode-free lithium metal battery and anode-free lithium metal battery comprising same

The introduction of a specific electrolyte with a metal salt in lithium metal batteries addresses dendrite formation and side reactions, improving energy density and lifespan by forming a lithium alloy that reduces reactivity and internal resistance.

WO2024205200A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG SDI CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003787
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-03
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium metal batteries with lithium metal thin films as negative electrodes suffer from dendrite formation and reduced lifespan due to side reactions with the electrolyte, leading to inadequate energy density and long-life characteristics.

Method used

An electrolyte containing a metal salt with a standard reduction potential lower than -1.68V, capable of forming an alloy with lithium and belonging to period 4 or higher of the periodic table, is introduced to suppress side reactions and reduce internal resistance by forming a lithium alloy with the metal cations, which precipitate on the negative electrode current collector.

Benefits of technology

The electrolyte effectively prevents dendrite formation and enhances the lifespan and charge/discharge efficiency of lithium metal batteries by reducing reactivity with the electrolyte and maintaining excellent electronic conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003787_03102024_PF_FP_ABST
    Figure KR2024003787_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an electrolyte for an anode-free lithium metal battery comprising: a lithium salt; a metal salt; and an organic solvent, wherein the metal salt is an ionic bonding compound of a metal cation and an anion, and the metal cation has a standard reduction potential lower than -1.68 V with respect to a standard hydrogen reduction electrode, is capable of forming an alloy with lithium (Li), and belongs to Period 4 or higher of the Periodic Table of Elements.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte for a non-anode lithium metal battery and a non-anode lithium metal battery containing the same

[0001] An electrolyte for a non-anode lithium metal battery and a non-anode lithium metal battery including the same are presented.

[0002] Lithium secondary batteries are high-performance secondary batteries with the highest energy density among the currently commercialized secondary batteries and can be used in various fields such as electric vehicles.

[0003] Lithium metal thin films can be used as anodes in lithium secondary batteries. These films are typically manufactured by rolling lithium into a plate shape. However, in lithium secondary batteries using these films as anodes, dendrites form and grow on the film, resulting in unsatisfactory energy density and long-life characteristics. This leaves significant room for improvement.

[0004] One aspect is to provide an electrolyte for anode-free lithium metal batteries that improves energy efficiency.

[0005] Another aspect is to provide a method for manufacturing the above-described non-anode lithium metal battery.

[0006] According to one aspect

[0007] Contains lithium salts; metal salts; and organic solvents,

[0008] The above metal salt contains metal cations and anions,

[0009] An electrolyte for a non-anode lithium metal battery is provided, wherein the metal cation has a standard reduction potential lower than -1.68 V with respect to a standard hydrogen reduction electrode, can form an alloy with lithium (Li), and belongs to period 4 or higher of the periodic table of elements.

[0010] Depending on other aspects

[0011] positive current collector;

[0012] A cathode containing a cathode active material layer;

[0013] negative current collector; and

[0014] An electrolyte according to claim 1; a non-anode lithium metal battery including the same is provided.

[0015] According to an embodiment, an electrolyte capable of suppressing side reactions and reducing internal resistance of lithium metal transition and a non-anode lithium metal battery including the same can be manufactured.

[0016] Figure 1 schematically illustrates the structure of a non-anode lithium metal battery according to an embodiment.

[0017] Figure 2 schematically illustrates the structure of a non-negative lithium metal battery after charging according to an embodiment.

[0018] Figure 3 is a cross-sectional view showing a cathode and electrolyte laminate according to an embodiment.

[0019] Hereinafter, an electrolyte for a non-anode lithium metal battery according to an exemplary embodiment and a non-anode lithium metal battery comprising the same will be examined in more detail. These examples are provided solely as examples to more specifically illustrate the present invention, and it will be apparent to those skilled in the art that the scope of the present invention is not limited by these examples.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, the present specification, including its definitions, shall prevail.

[0021] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, suitable methods and materials are described herein. The singular expression "singular" includes plural expression unless the context clearly indicates otherwise.

[0022] In this specification, the terms "include" or "have" are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials or combinations thereof.

[0023] The term "combination of these" in this specification means a mixture or combination of one or more of the described components.

[0024] As used herein, the term "and / or" is meant to include any and all combinations of one or more of the items described herein. As used herein, the term "or" means "and / or." The expressions "at least one," "one or more," or "one or more" preceding elements herein may supplement the entire list of elements and do not mean that they supplement individual elements described above.

[0025] In order to clearly represent various layers and regions in the drawings, the thicknesses are enlarged or reduced. The same drawing reference numerals are used for similar parts throughout the specification. When a layer, film, region, plate, etc. is referred to as being "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. The terms first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only to distinguish one component from another.

[0026] The electrolyte for the above-mentioned non-anode lithium metal battery comprises a lithium salt; a metal salt; and an organic solvent, wherein the metal salt comprises a metal cation and an anion, and the metal cation has a standard reduction potential lower than -1.68 V compared to a standard hydrogen reduction electrode, can form an alloy with lithium (Li), and belongs to a period 4 or higher of the periodic table of elements.

[0027] Lithium metal batteries that use a lithium metal film as an anode suffer from lithium loss due to the formation and growth of lithium dendrites on the upper portion of the lithium metal film during charge and discharge, which leads to the formation of a lithium dead volume as a result of the dendrite growth. As a result, the lifespan and capacity characteristics of the lithium metal battery may be reduced. In addition, since the lithium metal film has a plate-like shape, it can only expand upwards during charging. As a result, it is difficult to control the volume expansion of the lithium metal battery after charge and discharge to a desired level, and improvements in this area have been required. In addition, the energy density was improved by using only an anode current collector without a plate-like lithium anode film.

[0028] However, since lithium metal contained in the electrolyte is deposited on the anode current collector instead of the lithium anode thin film, side reactions occur between the lithium metal and the electrolyte, which accelerates the cycling of the lithium metal and the electrolyte, reducing the lifespan of the lithium metal battery. Therefore, a method to suppress side reactions between the lithium metal and the electrolyte was required.

[0029] To solve the above-described problems, the inventors of the present invention added a metal salt to the electrolyte, and the metal salt has a standard reduction potential lower than -1.68 V compared to a standard hydrogen reduction electrode, can form an alloy with lithium (Li), and contains a metal cation belonging to Period 4 or higher of the Periodic Table of Elements. In this case, when lithium ions contained in the electrolyte are deposited on the negative electrode current collector, the metal cations contained in the metal salt and the lithium ions form an alloy and are deposited, thereby suppressing side reactions between the lithium metal and the electrolyte.

[0030] In particular, since the metal cation belongs to the 4th period or higher of the periodic table of elements, not only is the reactivity of lithium and the metal cation alloy with the electrolyte effectively suppressed, but also excellent electronic conductivity is maintained, so that the problem of increased internal resistance in a non-anode lithium metal battery can be effectively prevented.

[0031] In addition, the metal cation has a standard reduction potential lower than -1.68 V compared to a standard hydrogen reduction electrode, so that side reactions between the metal salt and the positive and negative current collectors can be suppressed during the process of injecting electrolyte into a non-anode lithium metal battery.

[0032] In this specification, the term "non-anode battery" means a battery in which i) there is no lithium-removable negative active material, or ii) no negative active material layer is used during battery assembly. Here, "thickness of the negative electrode" means the total thickness of the negative electrode current collector and the negative active material layer.

[0033] According to one embodiment, an electrolyte for a non-anode lithium metal battery may include a metal salt and an organic solvent. For example, the metal salt may include a metal cation and an anion. For example, the metal salt may refer to a compound in which the metal cation and the anion are ionically bonded, or a state in which the metal cation and the anion are dissociated within the organic solvent.

[0034] According to one embodiment, the metal cation has a standard reduction potential lower than -1.68 V compared to a standard hydrogen reduction electrode, can form an alloy with lithium (Li), and can belong to period 4 or higher of the periodic table of elements.

[0035] For example, when the metal cation has a standard source potential lower than -1.68 eV with respect to a standard hydrogen reduction electrode, when an electrolyte including the metal cation is introduced into a non-anode lithium metal battery, an oxidation-reduction reaction that may occur between the metal cation and the current collector can be suppressed.

[0036] For example, when the metal cation can form an alloy with lithium and belongs to period 4 or higher of the periodic table of elements, when an electrolyte containing the metal cation is introduced into a non-anode lithium metal battery and charge / discharge is performed, when lithium metal is precipitated, a lithium alloy of lithium ions and metal cations is precipitated together with the lithium metal, so that the reactivity of the lithium metal may be reduced. Accordingly, the reactivity between the precipitated lithium metal and the electrolyte is suppressed from side reactions, and the life characteristics of the non-anode lithium metal battery may be improved.

[0037] In particular, when an electrolyte including the metal salt is introduced into a lithium metal battery including a lithium thin film, an oxidation-reduction reaction may occur between the lithium thin film and the metal included in the metal salt, so that the metal cations may be unevenly deposited on the lithium metal. In this case, since lithium is deposited only at a specific location during charge and discharge, lithium dendrites may be formed, which may reduce the lifespan of the lithium metal battery. Therefore, by introducing an electrolyte including the metal salt into a non-anode lithium metal battery that does not include a lithium thin film, side reactions between the lithium thin film and the metal salt can be effectively suppressed.

[0038] In one embodiment, the metal cation may comprise a monovalent, divalent, trivalent, tetravalent cation, or any combination thereof. For example, the metal cation may comprise a divalent cation.

[0039] According to one embodiment, the metal cation is Ca 2+ , Sr 2+ , Ba 2+ or any combination thereof.

[0040] According to one embodiment, the anion may include an imide anion, an amide anion, a triazole anion, an imidazole anion, a phosphate anion, a borate anion, a nitrate anion, or any combination thereof.

[0041] According to one embodiment, the anion may include an imide anion, an amide anion, a triazole anion, an imidazole anion, a nitrate anion, or any combination thereof. According to another embodiment, the anion may include a nitrate anion.

[0042] According to one embodiment, the anion is bis(trifluoromethanesulfonyl)amide (TFSI). - ), bis((perfluoroethyl)sulfonyl)amide (BETI) - ), fluorosulfonyl-(perfluoroethyl)sulfonylamide (FPFSI) -), tetrafluoro-(perfluoroethoxy)ethanesulfonate, bis(fluorosulfonyl)amide (FSI) - ), trifluoromethanesulfonate (OTf) - ), fluorosulfonyl-trifluorosulfonylamide (FTFSI) - ), perfluorobutylsulfonate, methanesulfonate, perfluorohexylsulfonate, tris(pentafluoroethyl)trifluorophosphate (FAP) - ), cyclo-hexafluoropropane-bis(sulfonyl)imide (HPSI) - ), sulfate (SO4) - ), cyclo-difluoromethane-bis(sulfonyl)imide (DMSI) - ), bis(fluoromalonato)borate (BFMB) - ), hexafluorophosphate (PF6) - ), tetrafluoroborate (BF4) - ), dicyanotriazolate (DCTA) - ), tetracyanoborate (Bison -), dicyano-trifluoromethyl-imidazole (dicyano-trifluoromethyl-imidazole, TDI) - ), difluoro-di-oxalatophosphate (DFOP) - ), dicyano-pentafluoroethyl-imidazole (PDI) - ), difluoro(oxalate)borate (DFOB) - ), Tetra(phosphorodifluoridate)borate, bis(oxalate)borate (BOB) - ), nitrate (NO3) - ), difluorophosphate, tetrafluoro-oxalatophosphate, trifluorotrisperfluoroethylphosphate, or any combination thereof.

[0043] According to one embodiment, the concentration of the metal salt in the electrolyte is 0.02 to 10.0 M, for example, 0.02 to 5.0 M, 0.02 to 4.0 M, 0.2 to 10.0 M, 1 to 5.0 M, 1 to 4.0 M, 2 to 10.0 M, 2 to 5.0 M, or 2 to 4.0 M. When the concentration of the metal salt is within the above range, lithium alloy formation can be promoted during charge and discharge. Accordingly, as the reactivity of the lithium metal layer described below is lowered, side reactions with the electrolyte are suppressed, and thus further improved life characteristics of a non-anode lithium metal battery can be obtained.

[0044] According to one embodiment, the organic solvent may include at least one selected from an ester solvent, a glyme solvent, a dioxolane solvent, an ether solvent, a fluorinated ether solvent, a sulfone solvent, a ketone solvent, a nitrile solvent, and a carbonate compound.

[0045] The above-mentioned glyme solvents are, for example, ethylene glycol dimethyl ether (1,2-dimethoxyethane), ethylene glycol diethyl ether (1,2-diethoxyethane), propylene glycol dimethyl ether, propylene glycol diethyl ether, butylene glycol dimethyl ether, butylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol diethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, tetrapropylene glycol dimethyl ether, dipropylene glycol diethyl ether, tripropylene glycol diethyl ether, tetrapropylene glycol diethyl ether, dibutylene glycol dimethyl ether, tributylene glycol dimethyl ether, tetrabutylene glycol dimethyl ether, dibutylene glycol diethyl ether, tributylene glycol diethyl ether and tetrabutylene glycol. It may contain one or more selected from diethyl ether.

[0046] The above ester solvent may include, for example, one or more selected from methyl propionate, ethyl propionate, ethyl butyrate, methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, gamma butyrolactone, decanolide, gamma valerolactone, mevalonolactone, and caprolactone.

[0047] The above ether solvent may include, for example, one or more selected from dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, and tetrahydrofuran.

[0048] The above ketone solvent may include cyclohexanone, and the above nitrile solvent may include at least one selected from acetonitrile (AN), succinonitrile (SN), and adiponitrile.

[0049] The above fluorinated ether solvent may include, for example, at least one selected from 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, and 2,2,3,3,4,4,5,5-octafluoropentyl 1,1,2,2-tetrafluoroethyl ether.

[0050] The above dioxolane solvent may include, for example, at least one selected from 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, 2-methyl-1,3-dioxolane, 2-vinyl-1,3-dioxolane, 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, and 2-ethyl-2-methyl-1,3-dioxolane.

[0051] The above sulfone solvent may include, for example, one or more selected from dimethylsulfone, diethylsulfone, and ethylmethylsulfone.

[0052] The above carbonate solvent may include, for example, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, butylene carbonate, ethyl methyl carbonate, fluoroethylene carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, and the like.

[0053] According to one embodiment, the organic solvent may include at least one selected from a glyme solvent, a dioxolane solvent, a fluorinated ether solvent, a sulfone solvent, and a carbonate solvent.

[0054] According to one embodiment, the organic solvent may contain a fluorinated ether compound.

[0055] According to one embodiment, the content of the fluorinated ether compound may be 50% by volume or less, for example, 0.1 to 50% by volume, for example, 1 to 30% by volume, based on the total content of the organic solvent.

[0056] For example, fluorinated ether compounds have a high flash point of about 80℃ or higher, so they have excellent flame retardancy, and when used as an organic solvent for liquid electrolytes, they can produce anode-free lithium metal batteries with improved high-temperature stability. In addition, fluorinated ether solvents have a structure in which fluorine-substituted functional groups are bonded centered on a -CH2-O- moiety and have low polarity. Therefore, these fluorinated ether solvents have excellent miscibility with high-solubility ether solvents capable of solvating lithium ions, such as DME.

[0057] The above fluorine-substituted ether solvent may be a compound represented by the following chemical formula 1.

[0058] [Chemical Formula 1]

[0059] R-CH2-OC n F 2n H

[0060] In the above chemical formula 1, R is C m+1 H m F 2m or C m F 2m+1 , n is an integer from 2 to 5, and m is an integer from 1 to 5.

[0061] The fluorine-substituted ether solvent represented by the above chemical formula 1 is, for example, at least one selected from the group consisting of HCF2CF2CH2OCF2CF2H, HCF2CF2CH2OCF2CF2CF2H, HCF2CF2OCH2CF3, HCF2CF2OCH2CH2OCF2CF2H, HCF2CF2OCH2CH2OCF2CF2H, HCF2CF2OCH2CH2OCF2CF2H, HCF2CF2OCH2CH2CH2OCF2CF2H, HCF2CF2OCF2CF2CF2H, HCF2CF2OCH2CH2OCF2CF2CF2H, HCF2CF2OCH2CH2OCF2CF2CF2H, and HCF2CF2OCH2CH2CH2OCF2CF2CF2H.

[0062] The fluorine-substituted ether solvent represented by the above chemical formula 1 may be, for example, 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, or 2,2,3,3,4,4,5,5-octafluoropentyl 1,1,2,2-tetrafluoroethyl ether.

[0063] The above electrolyte may include a lithium salt.

[0064] For example, the lithium salt may be any lithium salt commonly used in the art for manufacturing electrolytes.

[0065] According to one embodiment, the lithium salt is LiSCN, LiN(CN)2, Li(CF3SO2)3C, Li(FSO2)2N(LiFSI), LiC4F9SO3, LiN(SO2CF2CF3)2, LiPF3(C2F5)3, LiCl, LiF, LiBr, LiI, LiB(C2O4)2, LiPF6, LiPF5(CF3), LiPF5(C2F5), LiPF5(C3F7), LiPF4(CF3)2, LiPF4(CF3)(C2F5), LiPF3(CF3)3, LiPF3(CF2CF3)3, LiPF4(C2O4)2, LiBF4, LiBF3(C2F5), lithium tetrafluoro(oxalate) phosphate, lithium difluoro(bisoxalato) phosphate lithium bis(oxalato)borate (LiBOB), lithium oxalyldifluoroborate (LIODFB), lithium difluoro(oxalato)borate (LiDFOB), lithium bis(trifluoro methanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI, LiN(SO2F)2), LiN(SO2C2F5)2, LiCF3SO3, LiAsF6, LiSbF6, LiClO4, or mixtures thereof.

[0066] According to one embodiment, the concentration of the lithium salt in the electrolyte is 0.1 to 10.0 M, for example, 0.1 to 5.0 M, 0.1 to 4.0 M, 1 to 10.0 M, 1 to 5.0 M, 1 to 4.0 M, 2 to 10.0 M, 2 to 5.0 M, or 2 to 4.0 M. When the concentration of the lithium salt is within the above range, further improved lithium secondary battery characteristics can be obtained.

[0067] According to one embodiment, the electrolyte may further include at least one selected from an ionic liquid and a polymer ionic liquid.

[0068] For example, the ionic liquid may be used without limitation as long as it is an ionic substance that is in a molten state at room temperature (25°C) and contains cations and anions.

[0069] The cation of the ionic liquid may include imidazolium, ammonium, pyrrolidinium, or piperidinium, and the anion of the ionic liquid may include bis(fluorosulfonyl)imide, bis(fluorosufonyl)amide, fluoroborate, or fluorophosphate.

[0070] The cation of the ionic liquid may include an alkylammonium such as triethylammonium, an imidazolium such as ethylmethylimidazolium or butylmethylimidazolium, a pyrrolidinium such as 1-methyl-1-propylpyrrolidinium, or a methylpropylpiperidinium.

[0071] The anion of the ionic liquid may include bis(trifluoromethylsulfonyl)imide (TFSI), bis(pentafluoroethylsufonyl)amide (BETI), tetrafluoroborate (BF4), or hexafluorophosphate (PF6).

[0072] For example, the ionic liquids include [emim]Cl / AlCl3 (emim = ethyl methyl imidazolium), [bmpyr]NTf2 (bppyr = butyl methyl pyridinium), [bpy]Br / AlCl3 (bpy = 4, 4'-bipyridine), [choline]Cl / CrCl3·6H2O, [Hpy(CH2)3pyH][NTf2]2(NTf = trifluoromethanesulfonimide), [emim]OTf / [hmim]I(hmim = hexyl methyl imidazolium), [choline]Cl / HOCH2CH2OH, [Et2MeN(CH2CH2OMe)]BF4(Et = ethyl, Me = methyl, Pr = propyl, Bu = butyl, Ph = phenyl, Oct = octyl, Hex = hexyl), [Bu3PCH2CH2C8F 17 ]OTf (OTf = trifluoromethane sulfonate), [bmim]PF6 (bmim = butyl methyl imidazolium), [bmim]BF4, [omim]PF6 (omim = octyl methyl imidazolium), [Oct3PC 18 H 37]I, [NC(CH2)3mim]NTf2(mim = methyl imidazolium), [Pr4N][B(CN)4], [bmim]NTf2, [bmim]Cl, [bmim][Me(OCH2CH2)2OSO3], [PhCH2mim]OTf, [Me3NCH(Me)CH(OH)Ph] NTf2, [pmim][(HO)2PO2] (pmim = propyl methyl imidazolium), [b(6-Me)quin]NTf2(bquin = butyl quinoline, [bmim][Cu2Cl3], [C 18 H 37 OCH2mim]BF4(mim = methyl imidazolium) 14 H 29 mim]Br(mim = methyl imidazolium), [Me2N(C 12 H 25 )2]NO3, [emim]BF4, [mm(3-NO2)im][dinitrotriazolate], [MeN(CH2CH2OH)3], [MeOSO3], [Hex3PC 14 H 29 ]NTf2, [emim][EtOSO3], [choline][ibuprofenate], [emim]NTf2, [emim][(EtO)2PO2], [emim]Cl / CrCl2, [Hex3PC 14 H 29 ]N(CN)2, or any combination of these may be included.

[0073] The above polymeric ionic liquid may include an ionic compound in the form of a polymer composed of an organic cation containing an imidazolium group and an organic or inorganic anion.

[0074] For example, the organic cation of the polymeric ionic liquid may include poly(1-vinyl-3-alkylimidazolium), poly(1-allyl-3-alkylimidazolium), poly(1-(meth)acryloyloxy-3-alkylimidazolium). The organic anion of the polymeric ionic liquid may include CH3COO. - , CF3COO - , CH3SO3 - , CF3SO3 - , (CF3SO2)2N - , (CF3SO2)3C - , (CF3CF2SO2)2N - , C4F9SO3 - , C3F7COO - , (CF3SO2)(CF3CO)N - may include.

[0075] For example, the polymeric ionic liquid may comprise poly(1-vinyl-3-alkylimidazolium), poly(1-allyl-3-alkylimidazolium), poly(1-(meth)acryloyloxy-3-alkylimidazolium), or any combination thereof.

[0076] According to one embodiment, the viscosity of the electrolyte may be 5 cP or less at 25°C. For example, when the electrolyte satisfies the viscosity range described above, ions within the electrolyte may move freely and have excellent ionic conductivity. For example, the ionic conductivity of the electrolyte may be 1.0 mS / cm to 5.0 mS / cm at 25°C.

[0077] According to another embodiment, the electrolyte may further include at least one selected from gamma-butyrolactone, succinonitrile, adiponitrile, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, 4-methyldioxolane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, dioxane, sulfolane, dichloroethane, chlorobenzene, and nitrobenzene, in addition to the organic solvent described above.

[0078] According to one embodiment, the electrolyte may be in a liquid, gel, or semi-solid form. When the electrolyte is in a liquid, gel, or semi-solid form, the disadvantages of conventional lithium metal batteries can be overcome because at least one selected from lithium metal and lithium alloys can be freely expanded during charging and discharging, compared to when the electrolyte is in a completely solid form.

[0079]

[0080] [Non-cathode lithium metal battery (100)]

[0081] Referring to FIGS. 1 and 2, a non-anode lithium metal battery according to an embodiment will be described in detail. FIG. 2 shows a state in which a metal layer is deposited as the non-anode lithium metal battery of FIG. 1 is charged.

[0082] A non-anode lithium metal battery according to an embodiment includes, as shown in FIG. 1, an anode current collector (110) without a plate-shaped lithium metal thin film, an electrolyte (120) disposed on the anode current collector (110), and a cathode (150) disposed on the electrolyte (120).

[0083] According to one embodiment, a non-anode lithium metal battery (100) may further include a metal layer (125) disposed between an anode current collector (110) and an electrolyte (120), as shown in FIG. 2. For example, the metal layer (125) may include a lithium alloy generated by a reaction between lithium ions included in an electrolyte and metal cations included in a metal salt during a process of charging the non-anode lithium metal battery (100). For example, the metal layer (125) may be dissociated into lithium ions and metal cations during a discharge process, so that the thickness of the metal layer (125) may be reduced. For example, when the non-anode lithium metal battery (100) is completely discharged, the non-anode lithium metal battery (100) may not include the metal layer (125).

[0084]

[0085] [Cathode current collector (110)]

[0086] According to one embodiment, the negative electrode current collector (110) may include indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

[0087] According to one embodiment, the negative electrode current collector (110) may include copper (Cu).

[0088] According to one embodiment, the plate-shaped lithium metal thin film may be absent (free) on the negative electrode current collector (110) before performing charge / discharge. For example, when the plate-shaped lithium metal thin film is disposed on the negative electrode current collector (110) before performing charge / discharge, in the process of disposing the electrolyte on the negative electrode current collector (110), the metal cations included in the electrolyte may react with the lithium metal thin film, causing the metal cations to be precipitated as metal. In this case, the precipitated metal may be non-uniformly deposited on the lithium metal thin film, causing the lithium metal thin film to have an uneven surface state. Accordingly, since lithium deposition proceeds only at a specific location in the lithium metal battery charge / discharge cycle, dendrites may be formed on the surface of the lithium metal thin film, which may deteriorate the life characteristics of the lithium metal battery. Accordingly, in the case of a non-anode lithium metal battery in which the plate-shaped lithium metal thin film is absent (free) on the negative electrode current collector (110) before performing charge / discharge, the formation of dendrites may be prevented, thereby further improving the life characteristics.

[0089] For example, the negative electrode current collector may be a mesh-type current collector. Using a mesh-type current collector as the negative electrode current collector allows the electrolyte to be effectively supported on the negative electrode current collector. Therefore, the use of a nonwoven fabric within the electrolyte described above may be unnecessary.

[0090]

[0091] [Electrolyte (120)]

[0092] For example, the electrolyte (120) may include a lithium salt as described above; a metal salt; and an organic solvent.

[0093] According to another embodiment, the electrolyte (120) may further include a nonwoven fabric. The nonwoven fabric may serve to support at least one selected from lithium metal and lithium alloys precipitated during the charging process. For example, the nonwoven fabric may be omitted. For example, if the negative electrode current collector is of the mesh type, the nonwoven fabric may not be used.

[0094] The above nonwoven fabric may have a porosity of 10 to 90%, for example, 10 to 80%, for example, 10 to 50 vol%, for example, 25 to 50 vol%, and an average pore size of 0.1 to 10 µm, for example, 0.01 to 8 µm, for example, 0.1 to 1.0 µm. The average pore size represents the diameter when the pore shape is spherical, and represents the major axis length when the pore shape is non-spherical.

[0095] According to one embodiment, the nonwoven fabric may include one or more nonwoven fabrics selected from cellulose, polyester (e.g., polyethylene terephthalate (PET), polyetherimide, polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyamide, polyacetal, polycarbonate, polyimide, polyetherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, nylon, and polyparaphenylenebenzobisoxazole.

[0096]

[0097]

[0098] [Metal layer]

[0099] Referring to FIG. 2, the non-anode lithium metal battery (100) may further include a metal layer (125) disposed between the negative electrode current collector (110) and the electrolyte (120). For example, the metal layer (125) may include a lithium alloy. For example, the lithium alloy has lower reactivity with the electrolyte (120) than lithium metal, so that side reactions between the metal layer (125) and the electrolyte (120) may be suppressed. In addition, the lithium alloy has excellent electrical conductivity, so that the internal resistance of the non-anode lithium metal battery (100) including the lithium alloy may be reduced. Accordingly, the non-anode lithium metal battery (100) including the metal layer (125) may have improved not only life characteristics but also charge / discharge efficiency.

[0100] According to one embodiment, the lithium alloy may be a reaction product of lithium ions and metal cations contained in the electrolyte. For example, the metal layer (125) is free during the process of manufacturing the non-anode lithium metal battery (100), but when the non-anode lithium metal battery (100) is charged, the lithium ions contained in the electrolyte (120) and the metal cations described above react and are deposited on the negative electrode current collector (110), thereby forming the metal layer (125).

[0101] According to one embodiment, the metal layer (125) may further include lithium metal in addition to the lithium alloy. For example, the lithium metal is free during the process of manufacturing the non-anode lithium metal battery (100), but may be generated as lithium ions included in the electrolyte (120) are deposited on the negative electrode current collector (110) as the non-anode lithium metal battery (100) is charged. In this case, the metal layer (125) may include a lithium alloy and a lithium metal. For example, the lithium alloy included in the metal layer (125) may weaken the reactivity of the lithium metal, thereby effectively preventing a side reaction between the metal layer (125) and the electrolyte (120). In addition, the metal layer (125) has excellent electrical conductivity, so that the internal resistance of the non-anode lithium metal battery (100) may be reduced compared to when the non-anode lithium metal battery (100) includes a coating layer. Accordingly, the non-anode lithium metal battery (100) including the metal layer (125) can have improved charge / discharge efficiency as well as life characteristics.

[0102] The lithium alloy may include an alloy of lithium (Li) and a metal belonging to period 4 or higher of the periodic table of elements, and having a standard reduction potential lower than -1.68 V with respect to a standard hydrogen reduction electrode. The lithium alloy may include an alloy of lithium and Ca, Sr, or Ba. For example, the lithium alloy may include a lithium-calcium alloy, a lithium-strontium alloy, a lithium-barium alloy, or a combination thereof.

[0103] According to one embodiment, the metal layer may further include lithium metal.

[0104] Fig. 3 is a cross-sectional view showing a negative electrode and electrolyte laminate according to an embodiment. Referring to Fig. 3, when the metal layer (125) is uniformly divided into three parts in the thickness direction and sequentially defined as a first region (125A), a second region (125B), and a third region (125C) from a region near to a region far from the negative electrode current collector, the weight ratio of the metal element derived from the metal cation to the carbon element in the first region may be 0.75 to 5. For example, the weight ratio of the metal element derived from the metal cation to the carbon element in the first region may be 0.75 to 3, 0.75 to 2.9, 0.75 to 2.8, or 0.75 to 2.5.

[0105]

[0106] [anode]

[0107] As shown in Fig. 1, a positive electrode active material layer (130) is disposed on a positive electrode current collector (140) to form a positive electrode (150). More specifically, a positive electrode active material layer (130) may be disposed on an electrolyte (120), and a positive electrode current collector (140) may be disposed on the positive electrode active material layer (130).

[0108]

[0109] [Anode: Anode current collector]

[0110] Referring to FIGS. 1 and 2, the positive electrode (150) includes a positive electrode current collector (140). For example, the positive electrode (150) can be prepared by forming the positive electrode active material layer (130) on the positive electrode current collector (140).

[0111] For example, the positive electrode current collector (140) may include indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

[0112] According to one embodiment, the positive electrode current collector (140) may include aluminum (Al). For example, when the positive electrode current collector (140) includes aluminum (Al), even if the above-described metal salt is introduced into the electrolyte, the metal cation included in the metal salt has a standard reduction potential lower than -1.68 V with respect to a standard hydrogen reduction electrode, so that an oxidation-reduction reaction between the metal cation and the positive electrode current collector can be prevented. Accordingly, the side reaction resulting from introducing the metal salt into the electrolyte is effectively suppressed, and only the reactivity of the metal layer (125) to be described later, which is deposited during charge and discharge, is reduced, so that the life characteristics of the non-anode lithium metal battery can be further improved.

[0113]

[0114] [Anode: Anode active material layer]

[0115] The above positive electrode active material layer (130) may include a positive electrode active material, a conductive material, and a binder.

[0116] For example, the cathode active material may be at least one of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof, and a specific example thereof is Li a A 1-b B 1 b D 1 2 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B 1 b O 2-c D 1 c(In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B 1 b O 4-c D 1 c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B 1 c D 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 α(In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:

[0117] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; B 1 is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, Ga, Si, W, Mo, Cu, Zn, Ti, boron (B), rare earth elements or a combination thereof; D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F 1 is F, S, P, Cl, Br or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I is Cr, V, Fe, Sc, Y or a combination thereof; J may be V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0118] For example, the positive electrode active material may include a lithium transition metal oxide containing nickel and another transition metal. In the lithium transition metal oxide containing nickel and another transition metal, the content of nickel may be 60 mol% or more, for example, 75 mol% or more, for example, 80 mol% or more, for example, 85 mol% or more, for example, 90 mol% or more, based on the total mole number of transition metals.

[0119] For example, the lithium transition metal oxide may be a compound represented by the following chemical formula 1:

[0120] <Chemical Formula 1>

[0121] Li a Ni x Co y M z O 2-b A b

[0122] In chemical formula 1, 1.0≤a≤1.2, 0≤b≤0.2, 0.6≤x<1, 0≤y≤0.3, 0 <z≤0.3, x+y+z=1, M은 망간(Mn), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al) 및 보론(B)으로 이루어진 군으로부터 선택된 하나 이상이고,

[0123] A is F, S, Cl, Br or a combination thereof.

[0124] For example, in chemical formula 1, 0.7≤x<1, 0 <y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.2, 0<z≤0.2; 0.83≤x<0.97, 0<y≤0.15, 0<z≤0.15; 또는 0.85≤x<0.95, 0<y≤0.1, 0<z≤0.1일 수 있다.

[0125] For example, the lithium transition metal oxide may be at least one of the compounds represented by the following chemical formulae 2 and 3:

[0126] <Chemical Formula 2>

[0127] LiNi x Co y Mn z O2

[0128] In chemical formula 2, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이고,

[0129] <Chemical Formula 3>

[0130] LiNi x Co y Al z O2

[0131] In chemical formula 3, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.8≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.82≤x≤0.95, 0<y≤0.15, 0<z≤0.15이다. 예를 들어, 0.85≤x≤0.95, 0<y≤0.1, 0<z≤0.1이다.

[0132] For example, lithium transition metal oxide is LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.88 Co 0.08 Mn 0.04 O2, LiNi 0.8 Co 0.15 Mn 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.88 Co 0.1 Mn 0.02 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.2 O2 or LiNi 0.88 Co 0.1 Al 0.02 It could be O2.

[0133] For example, the above cathode active material may be used as one having a coating layer on the surface of the lithium transition metal oxide, or may be used by mixing the lithium transition metal oxide and a lithium transition metal oxide having a coating layer.

[0134] For example, the coating layer may include a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element.

[0135] For example, the compound forming the coating layer may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or mixtures thereof. The coating layer forming process may use any coating method as long as it can coat the lithium transition metal oxide with the coating elements by a method (e.g., spray coating, dipping, etc.) that does not adversely affect the properties of the positive electrode active material. Since this is well understood by those working in the relevant field, a detailed description thereof will be omitted.

[0136] Carbon black, graphite particles, etc. may be used as the above-mentioned conductive material, but are not limited thereto, and any conductive material that can be used in the relevant technical field may be used.

[0137] As the above binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene and mixtures thereof, or styrene butadiene rubber polymers may be used, but are not limited thereto, and any binder that can be used in the relevant technical field may be used.

[0138]

[0139] [Separator]

[0140] According to an embodiment, a non-anode lithium metal battery may further include a separator (not shown).

[0141] Specific examples of the above separator include polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof, and mixed multilayer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and a polypropylene / polyethylene / polypropylene three-layer separator may be used.

[0142]

[0143] [Method for manufacturing a non-cathode lithium metal battery]

[0144] According to one embodiment, a non-anode lithium metal battery (100) may be prepared by preparing a negative electrode current collector (110). Thereafter, a positive electrode (150) including a positive electrode active material layer (130) and a positive electrode current collector (140) may be prepared. Thereafter, the negative electrode current collector (110) and the positive electrode (150) may be sequentially stacked to prepare an electrode structure. In this case, the positive electrode (150) may be placed on the negative electrode current collector (110) such that the positive electrode active material layer (130) adjacent to the negative electrode current collector (110) is placed. Thereafter, the above-described electrolyte (120) may be injected into the electrode structure, thereby manufacturing a non-anode lithium metal battery. In this case, the electrolyte (120) may be injected between the negative electrode collector (110) and the positive electrode (150). Accordingly, a negative electrode current collector (110), an electrolyte (120), a positive electrode active material layer (130), and a positive electrode current collector (140) can be sequentially stacked.

[0145] According to another embodiment, a separator (not shown) can be prepared. The separator can be laminated between the negative electrode current collector (110) and the positive electrode (150).

[0146] The anode (150) can be prepared according to the following method.

[0147] According to one embodiment, a positive electrode active material composition comprising a positive electrode active material, a conductive agent, a binder, and a solvent may be prepared. The positive electrode active material composition may be coated on a positive electrode current collector (140) to prepare a positive electrode (150).

[0148] According to another embodiment, the positive electrode active material composition may be cast on a separate support, and then a film peeled from the support may be laminated onto a positive electrode current collector (140) to manufacture a positive electrode (150). For example, the positive electrode (150) is not limited to the forms listed above and may have forms other than the above.

[0149] Reference may be made to the above-described description of the positive electrode active material, conductive agent, and binder included in the positive electrode active material composition. The solvent included in the positive electrode active material composition may be, but is not limited to, N-methylpyrrolidone, acetone, or water, and any solvent that can be used in the relevant technical field may be used.

[0150] The contents of the positive electrode active material, conductive agent, binder, and solvent included in the above positive electrode active material composition are at levels typically used in lithium metal batteries. Depending on the intended use and configuration of the lithium metal battery, one or more of the conductive agent, binder, and solvent may be omitted.

[0151]

[0152] According to one embodiment, the battery case including the non-anode lithium metal battery may be cylindrical, square, thin-film, etc. For example, the lithium metal battery may be a large-scale thin-film battery. The lithium metal battery may be a lithium ion battery.

[0153] According to one implementation example, examples of the non-anode lithium metal battery include a lithium-air battery, a lithium-sulfur battery, etc.

[0154] According to one embodiment, a non-cathode lithium metal battery can be used in electric vehicles (EVs) due to its excellent cycle life and high-rate characteristics. For example, it can be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). Furthermore, it can be used in applications requiring large amounts of power storage, such as electric bicycles and power tools.

[0155] When stacking multiple anode-less lithium metal batteries (100) according to an embodiment, a gel-like electrolyte may be placed between the cathode and the liquid-impermeable ion-conductive composite membrane. The gel-like electrolyte may include, for example, a VDF-HFP copolymer, a lithium salt, and an organic solvent.

[0156]

[0157] Hereinafter, the following examples will be used to explain in more detail, but the present invention is not limited to the following examples.

[0158] Example 1: Non-anode lithium metal battery

[0159] A copper foil, which serves as a negative current collector, was prepared. Separately, the positive electrode was manufactured according to the following method.

[0160] LiNi x Co y Al 1-x-y O2, a conductive agent (Super-P; Timcal Ltd.), polyvinylidene fluoride (PVdF) and N-methylpyrrolidone were mixed to obtain a composition for forming a positive electrode active material layer. LiNi in the composition for forming a positive electrode active material layer x Co y Al 1-x-y The mixing weight ratio of O2, the challenge agent, and polyvinylidene fluoride (PVDF) was 97:1.5:1.5.

[0161] The composition for forming the above positive electrode active material was coated on top of aluminum foil (thickness: about 15 μm), dried at 25°C, and the dried resultant was dried in a vacuum at about 110°C to manufacture a positive electrode.

[0162] The positive electrode was placed on the negative electrode current collector so that the positive electrode active material layer was adjacent to the negative electrode current collector, and the positive electrode was combined to prepare an electrode structure.

[0163] Afterwards, an electrolyte was injected between the negative electrode current collector and the positive electrode to manufacture a non-anode lithium battery.

[0164] The electrolyte was prepared by mixing lithium hexafluorophosphate (LiPF6) and Ca(TFSI)2 with fluoroethylene carbonate and diethyl carbonate in a volume ratio of 1:2. The concentrations of lithium hexafluorophosphate (LiPF6) and Ca(TFSI)2 in the electrolyte were 1.2 M and 0.1 M, respectively.

[0165]

[0166] Example 2: Non-anode lithium metal battery

[0167] A non-anode lithium metal battery was manufactured using the same method as Example 1, except that Sr(TFSI)2 was used instead of Ca(TFSI)2 as the metal salt.

[0168]

[0169] Example 3: Non-anode lithium metal battery

[0170] A non-anode lithium metal battery was manufactured in the same manner as Example 1, except that Ba(TFSI)2 was used instead of Ca(TFSI)2 as the metal salt.

[0171]

[0172] Comparative Example 1: Non-anode lithium metal battery

[0173] A non-anode lithium metal battery was manufactured using the same method as Example 1, except that Mg(TFSI)2 was used instead of Ca(TFSI)2 as the metal salt.

[0174]

[0175] Comparative Example 2: Non-cathode lithium metal battery

[0176] A non-anode lithium metal battery was manufactured in the same manner as Example 1, except that LiNO3 was used instead of Ca(TFSI)2 as the metal salt.

[0177]

[0178] Comparative Example 3: Electrolyte containing a heterometal salt additive having a standard reduction potential higher than -1.68 V (vs. standard hydrogen reduction electrode)

[0179] A non-anode lithium metal battery was manufactured using the same method as Example 1, except that Sn(TFSI)2 was used instead of Ca(TFSI)2 as the metal salt.

[0180] The above anode is LiNi x Co y Al 1-x-y O2, a conductive agent (Super-P; Timcal Ltd.), polyvinylidene fluoride (PVdF) and N-methylpyrrolidone were mixed to obtain a cathode composition. LiNi in the cathode composition x Co y Al 1-x-y The mixing weight ratio of O2, the challenge agent, and PVDF was 97:1.5:1.5. Then, the positive electrode composition was coated on top of aluminum foil (thickness: approximately 15 μm), dried at 25°C, and the dried resultant was dried in a vacuum at approximately 110°C to produce a positive electrode.

[0181]

[0182] Evaluation Example 1: Initial Capacity Comparison

[0183] In order to compare the resistance characteristics of the non-anode lithium metal batteries manufactured according to Examples 1 to 3 and Comparative Examples 1 to 3, the discharge capacities of the first cycle were compared.

[0184] Each lithium metal battery was charged at a constant current of 0.1 C at 45°C until the voltage reached 4.30 V (vs. Li), and then cut-off at a current of 0.05 C while maintaining 4.30 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.1 C until the voltage reached 3.6 V (vs. Li) (Mars stage, 1 st cycle). In the next cycle, the battery was charged at a constant current of 0.2C rate until the voltage reached 4.30 V (vs. Li), and then cut off at a current of 0.05C rate while maintaining 4.30 V in constant voltage mode. Then, the battery was discharged at a constant current of 0.2C rate until the voltage reached 3.6 V (vs. Li) during discharge (Mars stage, 2 nd Cycle). This charging and discharging process was performed to complete the Mars process.

[0185] After the Mars process, the battery was charged at a constant current rate of 0.33 C until the voltage reached 4.30 V (vs. Li), and then cut off at a current rate of 0.05 C while maintaining 4.30 V in constant voltage mode. Subsequently, the battery was discharged at a constant current rate of 1.0 C until the voltage reached 3.6 V (vs. Li), and the resistance characteristics of each example and comparative example were compared by comparing the 1.0 C rate discharge capacity. The results are shown in Table 1 below.

[0186] Discharge capacity (mAh) Example 1 10.3890 Example 2 10.5307 Example 3 10.4405 Comparative Example 1 10.3645 Comparative Example 2 10.3441 Comparative Example 3 10.2426

[0187]

[0188] Referring to Table 1, it was found that the discharge capacity of Examples 1 to 3 increased compared to Comparative Examples 1 to 3.

[0189]

[0190] Evaluation Example 2: Charge / Discharge Characteristics

[0191] In order to compare the life characteristics of the non-anode lithium metal batteries manufactured according to Examples 1 to 3 and Comparative Examples 1 to 3, the discharge capacity of the first cycle was compared.

[0192] Each of the non-anode lithium metal batteries according to Examples 1 to 3 and Comparative Examples 1 to 3 was charged at a constant current of 0.1 C at 45°C until the voltage reached 4.30 V (vs. Li), and then cut-off was made at a current of 0.05 C while maintaining 4.30 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.1 C until the voltage reached 3.6 V (vs. Li) (Mars Stage, 1 st cycle). In the next cycle, the battery was charged at a constant current of 0.2C rate until the voltage reached 4.30 V (vs. Li), and then cut off at a current of 0.05C rate while maintaining 4.30 V in constant voltage mode. Then, the battery was discharged at a constant current of 0.2C rate until the voltage reached 3.6 V (vs. Li) during discharge (Mars stage, 2 nd Cycle). This charging and discharging process was performed to complete the Mars process.

[0193] After the Mars process, the battery was charged at a constant current rate of 0.33C until the voltage reached 4.30 V (vs. Li), and then cut off at a current rate of 0.05C while maintaining 4.30 V in constant voltage mode. Subsequently, the battery was discharged at a constant current rate of 1.0C until the voltage reached 3.6 V (vs. Li), and continuous charge / discharge was performed under the same conditions to observe the capacity change and compare the life characteristics.

[0194] In all the above charge / discharge cycles, a 10-minute pause was allowed after each charge / discharge cycle. The results are shown in Table 2 below. Here, 50 th The capacity retention rate in the cycle is defined by Equation 2 below.

[0195] [Formula 2]

[0196] Capacity retention rate (%) = [ x 100]

[0197] Composition capacity retention rate (%) Example 195.0 Example 294.7 Example 394.4 Comparative example 178.7 Comparative example 280.0 Comparative example 327.3

[0198] Referring to Table 2 above, it was found that the non-anode lithium metal batteries according to Examples 1 to 3 had improved capacity retention rates compared to the non-anode lithium metal batteries according to Comparative Examples 1 to 3.

[0199]

[0200] Evaluation Example 3: Evaluation of lithium alloy content in metal layer

[0201] After the anode-free lithium metal battery manufactured according to Examples 1 to 3 was charged in the first chemistry stage, the element distribution of the cross-section of the lithium metal deposited on the anode current collector was analyzed through scanning electron microscope EDS analysis.

[0202] Referring to Figure 3, when lithium metal is uniformly divided into three parts in the thickness direction and sequentially defined as first to third regions from the region near to the region far from the negative electrode current collector, the element distribution ratio for the first region is analyzed, and the ratio of the heterogeneous metal and carbon atoms is as follows. The heterogeneous metal is derived from the metal cation included in the electrolyte.

[0203] Sectional EDS heterometal / carbon element ratio (wt / wt) Example 1 (Ca) Ca / C = 0.775 Example 2 (Sr) Sr / C = 1.78 Example 3 (Ba) Ba / C = 2.86

[0204] While the above has been described with reference to drawings and examples, these are merely exemplary, and those skilled in the art will appreciate that various modifications and equivalent implementations are possible. Accordingly, the scope of protection of the present invention should be defined by the appended claims.

[0205]

[0206] [Explanation of symbols]

[0207] 100: Non-cathode lithium metal battery

[0208] 110: Cathode electrode assembly 120: Electrolyte

[0209] 130: Cathode active material layer 140: Cathode current collector

[0210] 150: Anode 125: Metal layer

Claims

1. Contains lithium salt; metal salt; and organic solvent, The above metal salt is an ionic compound of metal cations and anions, An electrolyte for a non-anode lithium metal battery, wherein the metal cation has a standard reduction potential lower than -1.68 V with respect to a standard hydrogen reduction electrode, can form an alloy with lithium (Li), and belongs to period 4 or higher of the periodic table of elements.

2. In paragraph 1, The electrolyte comprises the above metal cations including monovalent, divalent, trivalent, tetravalent cations or any combination thereof.

3. In paragraph 1, The above metal cation is Ca 2+ , Sr 2+ , Ba 2+ or any combination thereof, including electrolytes.

4. In paragraph 1, The above anion is an electrolyte including an imide anion, an amide anion, a triazole anion, an imidazole anion, a phosphate anion, a borate anion, a nitrate anion, or any combination thereof.

5. In paragraph 1, The above anion is bis(trifluoromethanesulfonyl)amide (TFSI). - ), bis((perfluoroethyl)sulfonyl)amide (BETI) - ), fluorosulfonyl-(perfluoroethyl)sulfonylamide (FPFSI) - ), tetrafluoro-(perfluoroethoxy)ethanesulfonate, bis(fluorosulfonyl)amide (FSI) - ), trifluoromethanesulfonate (OTf) - ), fluorosulfonyl-trifluorosulfonylamide (FTFSI) - ), perfluorobutylsulfonate, methanesulfonate, perfluorohexylsulfonate, tris(pentafluoroethyl)trifluorophosphate (FAP) - ), cyclo-hexafluoropropane-bis(sulfonyl)imide (HPSI) - ), sulfate (SO4) - ), cyclo-difluoromethane-bis(sulfonyl)imide (DMSI) - ), bis(fluoromalonato)borate (BFMB) - ), hexafluorophosphate (PF6) - ), tetrafluoroborate (BF4) - ), dicyanotriazolate (DCTA) - ), tetracyanoborate (Bison - ), dicyano-trifluoromethyl-imidazole (dicyano-trifluoromethyl-imidazole, TDI) - ), difluoro-di-oxalatophosphate (DFOP) - ), dicyano-pentafluoroethyl-imidazole (PDI) - ), difluoro(oxalate)borate (DFOB) - ), Tetra(phosphorodifluoridate)borate, bis(oxalate)borate (BOB) - ), nitrate (NO3) - ), difluorophosphate, tetrafluoro-oxalatophosphate, trifluorotrisperfluoroethylphosphate, or any combination thereof.

6. In the first paragraph, the concentration of the metal salt is 0.02 to 5.0 M, the electrolyte 7. In paragraph 1, An electrolyte wherein the organic solvent comprises at least one selected from among a glyme solvent, a dioxolane solvent, a fluorinated ether solvent, a sulfone solvent, and a carbonate solvent.

8. In paragraph 7, The above glyme solvents are ethylene glycol dimethyl ether (1,2-dimethoxyethane), ethylene glycol diethyl ether (1,2-diethoxyethane), propylene glycol dimethyl ether, propylene glycol diethyl ether, butylene glycol dimethyl ether, butylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol diethyl ether, tetraethylene glycol diethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol dimethyl ether, tetrapropylene glycol dimethyl ether, dipropylene glycol diethyl ether, tripropylene glycol diethyl ether, tetrapropylene glycol diethyl ether, dibutylene glycol dimethyl ether, tributylene glycol dimethyl ether, tetrabutylene glycol dimethyl ether, dibutylene glycol diethyl ether, tributylene glycol diethyl ether and tetrabutylene glycol Containing at least one selected from the group consisting of diethyl ether, The above fluorinated ether solvent comprises at least one selected from 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, and 2,2,3,3,4,4,5,5-octafluoropentyl 1,1,2,2-tetrafluoroethyl ether, The above dioxolane solvent includes at least one selected from 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, 2-methyl-1,3-dioxolane, 2-vinyl-1,3-dioxolane, 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, and 2-ethyl-2-methyl-1,3-dioxolane, The above sulfone solvent includes at least one selected from dimethyl sulfone, diethyl sulfone, and ethyl methyl sulfone, An electrolyte wherein the carbonate solvent comprises at least one selected from ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, butylene carbonate, ethyl methyl carbonate, fluoroethylene carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, and dibutyl carbonate.

9. In paragraph 7, The above organic solvent includes a fluorinated ether compound, An electrolyte in which the content of the above fluorinated ether compound is 50% by volume or less based on the total content of the organic solvent.

10. In paragraph 1, The above lithium salts are LiSCN, LiN(CN)2, Li(CF3SO2)3C, Li(FSO2)2N(LiFSI), LiC4F9SO3, LiN(SO2CF2CF3)2, LiPF3(C2F5)3, LiCl, LiF, LiBr, LiI, LiB(C2O4)2, LiPF6, LiPF5(CF3), LiPF5(C2F5), LiPF5(C3F7), LiPF4(CF3)2, LiPF4(CF3)(C2F5), LiPF3(CF3)3, LiPF3(CF2CF3)3, LiPF4(C2O4)2, LiBF4, LiBF3(C2F5), lithium bis(oxalato)borate (LiBOB), lithium oxalyldifluoroborate (LIODFB), lithium An electrolyte comprising lithium difluoro(oxalato)borate (LiDFOB), lithium bis(trifluoro methanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI, LiN(SO2F)2), LiN(SO2C2F5)2, LiCF3SO3, LiAsF6, LiSbF6, LiClO4, or any combination thereof.

11. In paragraph 1, The electrolyte is an electrolyte having a liquid or gel form.

12. Bipolar collector; A cathode containing a cathode active material layer; negative current collector; and A non-anode lithium metal battery comprising an electrolyte according to claim 1.

13. In paragraph 12, Further comprising a metal layer disposed between the negative electrode current collector and the electrolyte, A non-cathode lithium metal battery, wherein the metal layer comprises a lithium alloy.

14. In paragraph 13, The above lithium alloy is a non-anode lithium metal battery in which lithium ions and metal cations contained in the electrolyte are reaction products.

15. In paragraph 13, When the metal layer is uniformly divided into three parts in the thickness direction and the regions from the region close to the negative electrode collector to the region far from the negative electrode collector are sequentially defined as the first region to the third region, A non-anode lithium metal battery, wherein the weight ratio of the metal element derived from the metal cation to the carbon element in the first region is 0.75 to 5.

Citation Information

Patent Citations

  • Electrolyte for secondary battery, method of preparing thereof, and secondary battery including the electrolyte

    KR1020170009653A

  • Side view extended thermography

    KR1020210054372A

  • Electrolyte, anode-free rechargeable battery, method of forming anode-free rechargeable battery, battery, and method of forming battery

    US20210020986A1

  • KR20220139062A

  • KR20230032500A