Anode composition for lithium ion secondary battery, anode slurry, anode, and lithium ion secondary battery

The use of a water-based binder with (meth)acrylamide and a nonionic vinyl dispersant in the negative electrode composition of lithium-ion batteries addresses volume expansion issues, improving the batteries' performance and lifespan by maintaining conductivity and stability.

WO2024205294A1PCT designated stage expired Publication Date: 2024-10-03LG ENERGY SOLUTION LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004014
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-28
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face issues with volume expansion of silicon-based negative electrode active materials during charging and discharging, leading to conductive path blockage and deterioration of battery characteristics, which conventional binder polymers and conductive materials like carbon black and single-walled carbon nanotubes (SWCNTs) fail to adequately address.

Method used

A negative electrode composition using a water-based binder with a specific content of (meth)acrylamide and a nonionic vinyl-based dispersant to control the dispersibility of SWCNTs, preventing volume expansion and improving phase stability and mechanical properties.

Benefits of technology

The solution enhances the performance and lifespan of lithium-ion secondary batteries by maintaining conductivity and stability, ensuring safety and long-term functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present application relates to an anode composition, comprising an anode active material, a conductive material, and an aqueous binder, for a lithium ion secondary battery, wherein the conductive material comprises a pre-dispersion containing a specific type of dispersant, and the aqueous binder comprises a specific content of (meth)acrylamide (AM). Additionally, the present application relates to an anode slurry comprising the anode composition for a lithium ion secondary battery, an anode for a lithium ion secondary battery, and a lithium ion secondary battery. The anode composition for a lithium ion secondary battery can contribute to the improvement in phase stability and the suppression of volume expansion due to battery charging and discharging.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode composition for lithium-ion secondary batteries, negative electrode slurry, negative electrode, and lithium-ion secondary battery

[0001] The present application relates to a negative electrode composition for a lithium ion secondary battery, a negative electrode slurry, a negative electrode, and a lithium ion secondary battery.

[0002] This application claims the benefit of the filing dates of Korean Patent Application No. 10-2023-0042670, filed with the Korean Intellectual Property Office on March 31, 2023, and Korean Patent Application No. 10-2024-0042404, filed with the Korean Intellectual Property Office on March 28, 2024, the entire contents of which are incorporated herein by reference.

[0003] Due to the rapid increase in fossil fuel use, there is a growing demand for alternative or clean energy sources, and the most actively researched field within this area is power generation and storage using electrochemical reactions.

[0004] Currently, a representative example of an electrochemical device that utilizes this type of electrochemical energy is a secondary battery, and its application area is gradually expanding.

[0005] Meanwhile, with technological development and increasing demand for mobile devices, the demand for secondary batteries is rapidly increasing. Consequently, lithium-ion secondary batteries, which feature high energy density and voltage, long cycle life, and low self-discharge rates, are being commercialized and widely used. Accordingly, active research is being conducted to develop electrodes with high energy density per unit volume for high-capacity lithium-ion secondary batteries.

[0006] In general, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. In particular, the negative electrode includes a negative electrode active material, and silicon particles having a large charge and discharge capacity can be used as the negative electrode active material.

[0007] In particular, in response to the recent demand for secondary batteries with high-energy electrodes, Si / C, SiOx (x=0), and SiOx (0) with a capacity more than 10 times greater than that of graphite-based materials have been used as negative electrode active materials. <x<2) 등과 같은 실리콘계 화합물을 함께 사용하여 용량을 늘리는 방법에 대한 연구가 활발하게 진행되고 있다. 다만, 실리콘계 화합물의 경우, 기존의 흑연계 소재 대비, 충전, 방전의 반복 과정에서 수소 가스의 발생으로 부피가 팽창하여 도전 경로를 차단하고, 이로써 전지 특성을 저하시키는 문제점이 있다.

[0008] To address the volume expansion caused by the repeated charging and discharging processes described above, research on binder composition has been conducted, resulting in research into binder polymers with high stress resistance. However, these binder polymers alone have limitations in preventing the increase in electrode thickness due to shrinkage and expansion of the negative electrode active material and the resulting performance degradation of lithium-ion secondary batteries.

[0009] Additionally, to ensure the conductivity of the cathode, the secondary battery additionally includes a conductive material. While carbon black and the like have been primarily used in the past, single-walled carbon nanotubes (SWCNTs) with a thin and long shape are now being used to enhance the capacity of the secondary battery.

[0010] However, when using single-walled carbon nanotubes as a conductive material, they must be used in the form of a dispersion of single-walled carbon nanotubes in order to uniformly distribute the single-walled carbon nanotubes within the active material layer. However, as the degree of dispersion of the dispersion increases, the density difference between the conductive material containing the dispersion and the active material becomes more severe, and this causes the conductive material to migrate from the current collector to the upper layer, which causes a problem in that the phase stability and conductivity of the negative electrode composition deteriorate.

[0011] Accordingly, various methods are being discussed in terms of changing the components of the negative electrode composition in order to improve battery characteristics while controlling the dispersion of the SWCNTs.

[0012] The inventors of the present invention have discovered that by using single-walled carbon nanotubes (SWCNTs) as the conductive material, adopting a nonionic vinyl compound as a dispersant to control compatibility and dispersibility with the conductive material, and adopting an aqueous binder containing a specific content of (meth)acrylamide to further improve dispersibility, problems such as volume expansion of the negative electrode and cycle performance can ultimately be solved.

[0013] The present invention provides an anode composition for a lithium ion secondary battery in which the dispersibility of single-walled carbon nanotubes is controlled and the volume expansion problem of the anode is improved in the future by using a specific type of dispersant and a specific content of (meth)acrylamide-containing aqueous binder, and an anode slurry, a cathode, and a lithium ion secondary battery including the same are also provided.

[0014] One embodiment of the present specification provides an anode composition for a lithium ion secondary battery, comprising: a cathode active material; a conductive material; and an aqueous binder, wherein the conductive material comprises a pre-dispersion solution containing single-walled carbon nanotubes (SWCNTs) and a dispersant, the aqueous binder comprises 30 wt% or more and 80 wt% or less of (meth)acrylamide (AM) based on 100 wt% of the total aqueous binder, and the dispersant comprises a nonionic vinyl compound.

[0015] In another embodiment, a negative electrode slurry is provided, which includes the negative electrode composition for a lithium ion secondary battery and a solvent.

[0016] In another embodiment, an electrode is provided, comprising: a current collector layer; and a negative electrode active material layer provided on one or both sides of the current collector layer, wherein the negative electrode active material layer includes the negative electrode slurry or a dried product thereof.

[0017] Finally, a lithium ion secondary battery is provided, comprising a first electrode; a second electrode; a separator interposed between the first electrode and the second electrode; and an electrolyte, wherein one of the first electrode and the second electrode is the negative electrode.

[0018] According to one embodiment of the present invention, a negative electrode composition for a lithium ion secondary battery controls the dispersibility of single-walled carbon nanotubes in a conductive material, improves compatibility and / or phase stability between a conductive material and an aqueous binder by using an aqueous binder containing (meth)acrylamide having high strength characteristics, and prevents volume expansion of a negative electrode active material, thereby enabling the provision of a lithium ion secondary battery with high performance and long life characteristics in the future.

[0019] Furthermore, since the negative electrode slurry, negative electrode, and lithium ion secondary battery according to one embodiment of the present invention include the negative electrode composition for a lithium ion secondary battery, the above-described effects are exhibited as is, and thus the safety and stability of the lithium ion secondary battery can be secured.

[0020] Before explaining the present invention, some terms are first defined.

[0021] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless specifically stated otherwise.

[0022] In this specification, 'p to q' means a range of 'p or more and q or less'.

[0023] In this specification, when x parts by weight is based on 100 parts by weight, it can be used interchangeably with wt%.

[0024] In this specification, the meaning of a polymer including a monomer as a repeating unit means that the monomer participates in a polymerization reaction and is included as a repeating unit in the polymer.

[0025] In this specification, when it is said that a polymer includes a monomer, this is interpreted as the same as saying that the polymer includes a monomer as a monomer unit.

[0026] In this specification, the term 'polymer' is understood to be used in a broad sense including copolymers unless 'homopolymer' is specified.

[0027] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are polystyrene-equivalent molecular weights measured by gel permeation chromatography (GPC) using monodisperse polystyrene polymers (standard samples) of various degrees of polymerization commercially available for molecular weight measurement as standard materials.

[0028] In this specification, molecular weight means weight average molecular weight unless otherwise specified.

[0029] Hereinafter, the present invention will be described in detail with reference to the drawings so that those skilled in the art can easily practice it. However, the present invention can be implemented in various different forms and is not limited to the following description.

[0030] <Cathode composition for lithium-ion secondary batteries>

[0031] One embodiment of the present specification provides an anode composition for a lithium ion secondary battery, comprising: a cathode active material; a conductive material; and an aqueous binder, wherein the conductive material comprises a pre-dispersion solution containing single-walled carbon nanotubes (SWCNTs) and a dispersant, the aqueous binder comprises 30 wt% or more and 80 wt% or less of (meth)acrylamide (AM) based on 100 wt% of the total aqueous binder, and the dispersant comprises a nonionic vinyl compound.

[0032] According to one embodiment of the present invention, a negative electrode composition for a lithium ion secondary battery controls the dispersibility of single-walled carbon nanotubes in a conductive material, improves compatibility and / or phase stability between a conductive material and an aqueous binder by using an aqueous binder containing (meth)acrylamide having high strength characteristics, and prevents volume expansion of a negative electrode active material, thereby enabling the provision of a lithium ion secondary battery with high performance and long life characteristics in the future.

[0033] The negative electrode composition for a lithium ion secondary battery according to the above embodiment can improve phase stability, improve mechanical properties, and further improve cycle and / or life performance in terms of future batteries by satisfying the above content range of (meth)acrylamide, which is the first repeating unit.

[0034] In this specification, the term “(meth)acrylamide” may include methacrylamide or acrylamide.

[0035] In the present specification, the aqueous binder may further include (meth)acrylic acid (AA) in addition to (meth)acrylamide.

[0036] In the present specification, the aqueous binder may additionally include (meth)acrylonitrile in addition to (meth)acrylamide and (meth)acrylic acid.

[0037] In this specification, the aqueous binder means a binder based on water as a solvent or electrolyte.

[0038] In this specification, unless otherwise specified, the aqueous binder means a copolymer containing two or more repeating units.

[0039] In this specification, the copolymer is a concept encompassing alternating copolymers, random copolymers, block copolymers, and graft copolymers, unless otherwise specified.

[0040] According to one embodiment of the present specification, the pre-dispersed liquid may include single-walled carbon nanotubes having a length of more than 0 μm and less than 0.2 μm in an amount of more than 0 part by weight and less than 1 part by weight, based on 100 parts by weight of the total single-walled carbon nanotubes, and single-walled carbon nanotubes having a length of more than 10 μm and less than 100 μm in an amount of more than 15 parts by weight.

[0041] The negative electrode composition for a lithium ion secondary battery of the above embodiment can control dispersibility and efficiently improve conductivity. Specifically, when the single-walled carbon nanotubes having a length of more than 0㎛ and less than 0.2㎛ are 1 part by weight or less based on 100 parts by weight of the total single-walled carbon nanotubes, damage to the single-walled carbon nanotubes due to excessive linear dispersion can be suppressed, and deterioration of the connection performance of the conductive network can be prevented, and as long as the single-walled carbon nanotubes having a length of more than 10㎛ and less than 100㎛ are satisfactorily 15 parts by weight or more based on 100 parts by weight of the total single-walled carbon nanotubes, the lifespan can be improved due to excellent connection of the conductive network due to volume expansion of the electrode during charge and discharge.

[0042] In the present specification, the pre-dispersed liquid can be manufactured by adding single-walled carbon nanotubes and a dispersant (additionally, a dispersion medium, a viscosity modifier, etc.), mixing them, and milling the mixture.

[0043] In this specification, the pre-dispersion liquid is prepared by a method of preparing a single-wall carbon nanotube and then using a high-pressure homogenizer or the like to produce the pre-dispersion liquid.

[0044] In this specification, "100 parts by weight of the entire single-walled carbon nanotube" refers to the solid content, i.e., the solid component of the pre-dispersed liquid. The solid content and the weight parts by weight of each component based on the solid content can be measured using general analytical methods used in the art, such as liquid chromatography or gas chromatography.

[0045] In the present specification, the milling can be manufactured by a milling method using a ball mill, a bead mill, a disc mill, a basket mill, or a high pressure homogenizer, and preferably, a high pressure homogenizer can be used that can effectively achieve dispersion without causing damage to the single-wall carbon nanotubes.

[0046] In the present specification, milling by a high-pressure homogenizer can be achieved by, for example, pressurizing the mixture with a plunger pump of the high-pressure homogenizer and pushing it through a gap of a homogenization valve, thereby applying forces such as cavitation, shear, impact, and explosion when the mixture passes through the gap.

[0047] In this specification, the particle size of single-walled carbon nanotubes (SWCNTs) can be measured using a particle size analyzer (Malvensa) utilizing the laser diffraction method. The laser diffraction method can generally measure a wide range of particle sizes (especially length) from submicron to several millimeters, and can obtain analysis results with high reproducibility and high resolution.

[0048] In one embodiment of the present specification, the negative electrode active material may include at least one selected from the group consisting of a silicon-based active material and a carbon-based active material.

[0049] In another embodiment of the present specification, the negative active material may be a silicon-based active material.

[0050] The negative electrode composition for a lithium ion secondary battery according to the above embodiment can have a capacity that is at least 10 times higher than that of the carbon-based active material by including a silicon-based active material as the negative electrode active material. Accordingly, when a silicon-based active material is applied to the negative electrode, an electrode having a high level of energy density can be realized with a thinner thickness than when a carbon-based active material is included alone.

[0051] In another embodiment of the present specification, the negative active material may include a silicon-based active material and a carbon-based active material.

[0052] In another embodiment of the present specification, when the negative electrode active material includes a silicon-based active material and a carbon-based active material, the weight ratio between the silicon-based active material and the carbon-based active material may be within a range of 2:98 to 30:70.

[0053] The negative electrode active material according to the above embodiment has a carbon-based active material as its main component, and thus has a small volume expansion of the active material during charging and discharging, resulting in less swelling, and can additionally provide the effect of excellent conductive connectivity of the negative electrode.

[0054] In one embodiment of the present specification, the silicon-based active material is SiOx (x=0), SiOx (0 <x<2), SiC 및 Si 합금 중 1 이상을 포함할 수 있다.

[0055] In this specification, the case of SiO2 in which x is 2 in the above SiOx is not included, and this SiO2 does not react with lithium ions and thus cannot store lithium. Therefore, it is preferable that x is within the range of the above embodiment.

[0056] In this specification, the silicon-based active material may be Si / C or Si composed of a complex of Si and C.

[0057] In this specification, two or more types of the above silicon-based active materials can be mixed and used.

[0058] In one embodiment of the present specification, the negative electrode active material may be at least 60 parts by weight based on 100 parts by weight of the negative electrode composition for the lithium ion secondary battery.

[0059] In one embodiment of the present specification, the negative electrode active material may be included in an amount of 60 parts by weight or more, preferably 65 parts by weight or more, and more preferably 70 parts by weight or more, based on 100 parts by weight of the negative electrode composition for a lithium ion secondary battery, and may be included in an amount of 95 parts by weight or less, preferably 90 parts by weight or less.

[0060] In the present specification, the silicon-based active material may exist in, for example, a crystalline or amorphous form. Specifically, the silicon particles of the silicon-based active material may preferably be spherical particles, but are not limited thereto.

[0061] In one embodiment of the present specification, when the negative active material is composed solely of a silicon-based active material, the silicon-based active material is SiOx (x=0) and SiOx (0 <x<2)로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 70 중량부 이상 포함할 수 있다.

[0062] In another embodiment, the silicon-based active material may contain 70 parts by weight or more, preferably 80 parts by weight or more, more preferably 90 parts by weight or more of the SiOx (x=0) based on 100 parts by weight of the silicon-based active material, or may contain 100 parts by weight or less, preferably 99 parts by weight or less, more preferably 95 parts by weight or less.

[0063] In another embodiment of the present invention, when the silicon-based active material includes SiOx (x=0), the average particle diameter (D) of SiOx (x=0) 50) can be 3㎛ to 10㎛.

[0064] When the above range is satisfied, the structural stability of the active material during charging and discharging can be ensured, the problem of the level of volume expansion / contraction increasing as the particle size becomes excessively large can be prevented, and the problem of initial efficiency decreasing as the particle size becomes excessively small can be prevented.

[0065] The particle size of the above negative active material can be controlled by methods such as a ball mill, a jet mill, or airflow classification, but is not limited thereto.

[0066] In this specification, "D n " means particle size distribution, and means particle size at the n% point of the cumulative particle number distribution according to particle size. That is, D 50 is the particle size (average particle size) at the 50% point of the cumulative particle number distribution according to particle size, and D 90 is the particle size at the 90% point of the cumulative distribution of particle numbers according to particle size, and D 10 is the particle size at the 10% point of the cumulative particle number distribution according to particle size. Meanwhile, the particle size distribution can be measured using the laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and the difference in diffraction pattern according to particle size is measured when the particles pass through the laser beam, thereby calculating the particle size distribution.

[0067] In one embodiment of the present specification, the carbon-based active material may include at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, and soft carbon.

[0068] In one embodiment of the present specification, the conductive material may be present in an amount of 0.03 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the cathode composition.

[0069] In another embodiment of the present specification, the conductive material may be included in an amount of 0.03 parts by weight or more and 40 parts by weight or less, preferably 0.05 parts by weight or more and 30 parts by weight or less, and more preferably 0.5 parts by weight or more and 25 parts by weight or less, based on 100 parts by weight of the negative electrode composition.

[0070] In this specification, the conductive material and the aqueous binder included in the negative electrode composition for the lithium ion secondary battery may mean a negative electrode conductive material and a negative electrode aqueous binder, respectively.

[0071] In this specification, the negative electrode conductive material has a completely separate composition from the positive electrode conductive material applied to the positive electrode. That is, in the case of the negative electrode conductive material according to the present application, it serves to secure the contact between silicon-based active materials that greatly expand the volume of the negative electrode due to charging and discharging, and the positive electrode conductive material serves to provide some conductivity while acting as a buffer when rolled, and is completely different in composition and role from the negative electrode conductive material of the present invention.

[0072] In addition, the negative electrode conductive material according to the present application may have a composition completely different from that of a conductive material applied to a graphite-based active material (i.e., a carbon-based active material containing only graphite) when the negative electrode active material includes a silicon-based active material. That is, the conductive material used in the negative electrode having the graphite-based active material simply has smaller particles than the active material, and thus has the characteristics of improving output characteristics and imparting some conductivity, and is completely different in composition and role from the negative electrode conductive material applied together with a silicon-based active material as in the present invention.

[0073] In this specification, the use of a carbon-based active material as an active material means that it is processed into a dot or spherical shape and used as a material that stores or releases lithium.

[0074] That is, in one embodiment of the present application, the carbon-based active material, artificial graphite or natural graphite, is in a dot-like shape and has a BET specific surface area of ​​0.1 m2 / g or more than 4.5 m 2 / g or less can be satisfied. In addition, the plate-shaped graphite, which is a planar conductive material, has a BET surface area of ​​5 m in the form of a planar surface. 2 / g can be more than that.

[0075] In one embodiment of the present invention, the nonionic vinyl compound may be at least one selected from the group consisting of polyvinyl pyrrolidone (PVP) and polyvinyl butyral (PVB). Preferably, the dispersant may be polyvinyl pyrrolidone (PVP).

[0076] When the above dispersant is used in a negative electrode composition for a lithium ion secondary battery, the phase stability is improved during the manufacture of a negative electrode slurry in the future, and accordingly, the life performance of a negative electrode including the negative electrode slurry can be improved.

[0077] In particular, among nonionic vinyl compounds, PVP has excellent solubility in water and excellent mutual bonding with SWCNTs, and is insensitive to interaction with single-walled carbon nanotubes (SWCNTs) in response to pH changes depending on changes in the composition of the slurry according to the type and content of the aqueous binder and conductive agent, so it has excellent phase stability.

[0078] In another embodiment of the present invention, the dispersant may further include an elastomer such as hydrogenated nitrile butadiene rubber (H-NBR).

[0079] In another embodiment of the present invention, the dispersant may be present in an amount of 0.5 parts by weight or more and 5 parts by weight or less, based on 100 parts by weight of the cathode composition.

[0080] In another embodiment of the present invention, the dispersant is used for the purpose of dispersing the SWCNT conductive material, and the upper limit is not particularly limited, and it can be used to the extent that it does not affect the physical properties of the binder, and suitably, 20 parts by weight or less, or 10 parts by weight or less, based on 100 parts by weight of the binder. The lower limit of the dispersant is 20 parts by weight or more, suitably 50 parts by weight or more, 100 parts by weight or more, or 150 parts by weight or more, based on 100 parts by weight of the SWCNT. If the dispersant is less than 20 parts by weight based on 100 parts by weight of the SWCNT, it is difficult to effectively disperse the SWCNT, and the dispersion stability after dispersion may deteriorate.

[0081] In one embodiment of the present invention, the aqueous binder may be a copolymer comprising (meth)acrylamide (AM) as a first repeating unit and (meth)acrylic acid (AA) as a second repeating unit.

[0082] When the above copolymer is included as an aqueous binder, the solubility in a solvent (a solvent used in preparing a slurry) can be further improved.

[0083] In another embodiment of the present invention, when the aqueous binder is a copolymer composed of two types of repeating units of (meth)acrylamide (AM) and (meth)acrylic acid (AA), the weight ratio of AM:AA may be 30 to 80:20 to 70.

[0084] When the above weight ratio is satisfied, the aqueous binder can secure improved mechanical properties and cycle characteristics, and its dispersibility with single-walled carbon nanotubes (SWCNTs) can be controlled. In addition, when the above weight ratio is satisfied, the aqueous binder can further improve its solubility in a solvent (a solvent used in preparing a slurry, such as water).

[0085] In one embodiment of the present invention, the aqueous binder may be a copolymer further comprising (meth)acrylonitrile (AN) as a third repeating unit. In other words, the aqueous binder may be a copolymer comprising a first repeating unit derived from (meth)acrylamide (AM), a second repeating unit derived from (meth)acrylic acid (AA), and a third repeating unit derived from (meth)acrylonitrile (AN).

[0086] According to the above embodiment, the solubility and / or dispersibility in a solvent (a solvent used in preparing a slurry) can be further improved, and the adhesive properties can be further improved.

[0087] In another embodiment of the present invention, when the aqueous binder is a terpolymer including three types of repeating units of (meth)acrylamide (AM), (meth)acrylic acid (AA), and (meth)acrylonitrile (AN), the weight ratio of AM: AA: AN may be 30 to 80: 10 to 40: 10 to 30.

[0088] Aqueous binders satisfying the above weight ratios can secure improved mechanical properties and cycle characteristics, and their dispersibility with single-walled carbon nanotubes (SWCNTs) can be controlled, thereby enhancing network connectivity. Furthermore, aqueous binders satisfying the above weight ratios can further enhance their solubility in solvents (e.g., water, a solvent used in slurry preparation). Furthermore, when the above weight ratios are satisfied, their binding properties can be enhanced.

[0089] In this specification, a polymerization initiator is used for the production of the aqueous binder (copolymer), and ammonium persulfate can be used as an example of the polymerization initiator, but is not limited thereto.

[0090] In this specification, for the production of the above-mentioned aqueous binder, after the copolymer is produced, it can be neutralized with a certain concentration of acid or base as needed.

[0091] In one embodiment of the present specification, the aqueous binder may be in an amount of 2 parts by weight or more and 30 parts by weight or less based on 100 parts by weight of the negative electrode composition.

[0092] In another embodiment of the present specification, the aqueous binder may comprise 30 parts by weight or less, preferably 25 parts by weight or less, more preferably 20 parts by weight or less, or 2 parts by weight or more, 5 parts by weight or more, or 10 parts by weight or more, based on 100 parts by weight of the negative electrode composition.

[0093] In another embodiment of the present specification, the weight average molecular weight of the binder may be 100,000 g / mol or more and 1,500,000 g / mol or less.

[0094] The negative electrode composition according to the above embodiment has excellent mechanical strength and enhanced intermolecular interaction, thereby achieving excellent negative electrode bonding properties, as the weight average molecular weight of the binder satisfies the above range. Furthermore, when the above range is satisfied, the viscosity of the aqueous binder can be controlled within an appropriate range, resulting in excellent coatability when manufacturing a negative electrode using the binder.

[0095] <Method for producing a negative electrode composition for a lithium-ion secondary battery>

[0096] One embodiment of the present invention provides a method for producing an anode composition for a lithium ion secondary battery, comprising the steps of: preparing a pre-dispersion solution by dispersing single-walled carbon nanotubes (SWCNTs) as a conductive material and a dispersant; mixing an aqueous binder containing 30 wt% or more and 80 wt% or less of (meth)acrylamide (AM) based on 100 wt% of the total aqueous binder; and adding and mixing an anode active material, wherein the dispersant contains a nonionic vinyl compound.

[0097] In this specification, the pre-dispersion liquid is prepared by a method of preparing single-wall carbon nanotubes and a dispersant, and then using a high-pressure homogenizer or the like to prepare the pre-dispersion liquid.

[0098] The specific details of each component in the method for manufacturing the negative electrode composition for the lithium ion secondary battery are as described above.

[0099] According to the method for manufacturing a negative electrode composition for a lithium ion secondary battery according to the above-described embodiment, the dispersibility of the conductive material is controlled, and the shape of the structure of the single-walled carbon nanotube formed according to the dispersion is easily maintained, thereby improving the phase stability and improving the life characteristics of the battery in the future.

[0100] <Cathode slurry>

[0101] In one embodiment of the present invention, a negative electrode slurry comprising the negative electrode composition for a lithium ion secondary battery and a solvent is provided.

[0102] In one embodiment of the present invention, the solvent may be water, but is not limited thereto.

[0103] In this specification, the solvent may be a solvent that can be combined with the cathode composition.

[0104] In some cases, the average particle diameter (D) of the silicon-based active material 50 ) In addition to appropriately controlling the specific surface area of ​​the particles, by appropriately controlling the viscosity of the negative electrode slurry within an appropriate range, the dispersion of components (e.g., conductive agent, binder, silicon-based active material, etc.) within the slurry can be improved. Accordingly, the contact area between the components is improved, so that the conductive network can be sustained, the capacity retention rate can be increased, and the uneven phenomenon of current density during charge / discharge can be prevented.

[0105] <Cathode>

[0106] Another embodiment of the present invention provides a negative electrode comprising a current collector layer; and a negative electrode active material layer provided on one or both sides of the current collector layer, wherein the negative electrode active material layer includes the negative electrode slurry or a dried product thereof.

[0107] In this specification, unless otherwise specified, the current collector layer of the negative electrode may be referred to as a negative electrode current collector layer.

[0108] In one embodiment of the present application, the solid content of the cathode slurry can satisfy 3 wt% or more and 50 wt% or less.

[0109] In another embodiment, the solid content of the cathode slurry can satisfy a range of 3 wt% or more and 50 wt% or less, preferably 5% or more and 45% or less, and more preferably 7 wt% or more and 40 wt% or less.

[0110] The solid content of the above cathode slurry may mean the content of the cathode composition included in the cathode slurry, and may mean the content of the cathode composition based on 100 parts by weight of the cathode slurry.

[0111] When the solid content of the above negative electrode slurry satisfies the above range, the viscosity is appropriate when forming the negative electrode active material layer, thereby minimizing particle agglomeration of the negative electrode composition, and thus has the characteristic of efficiently forming the negative electrode active material layer.

[0112] In one embodiment of the present application, the slurry solvent can be used without limitation as long as it can dissolve the negative electrode composition, and specifically, water or NMP can be used.

[0113] In one embodiment of the present application, the negative electrode current collector layer generally has a thickness of 1 μm to 100 μm. The negative electrode current collector layer is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the bonding strength of the negative electrode active material can be strengthened by forming fine unevenness on the surface, and can be used in various forms such as a film, sheet, foil, net, porous body, foam, non-woven fabric, etc.

[0114] In one embodiment of the present application, a negative electrode for a lithium ion secondary battery is provided, wherein the thickness of the negative electrode current collector layer is 1 μm or more and 100 μm or less, and the thickness of the negative electrode active material layer is 20 μm or more and 500 μm or less.

[0115] However, the thickness can be varied depending on the type and purpose of the cathode used and is not limited thereto.

[0116] In one embodiment of the present application, the porosity of the negative electrode active material layer can satisfy a range of 10% or more and 60% or less.

[0117] In another embodiment, the porosity of the negative electrode active material layer can satisfy a range of 10% or more and 60% or less, preferably 20% or more and 50% or less, and more preferably 30% or more and 45% or less.

[0118] The above porosity varies depending on the composition and content of the silicon-based active material; conductive material; and binder included in the negative electrode active material layer, and in particular, the silicon-based active material and conductive material according to the present application are included in a specific composition and content portion to satisfy the above range, and thus the negative electrode is characterized by having an appropriate range of electrical conductivity and resistance.

[0119] Lithium-ion secondary battery

[0120] In one embodiment of the present invention, a lithium ion secondary battery is provided, comprising: a first electrode; a second electrode; a separator interposed between the first electrode and the second electrode; and an electrolyte, wherein one of the first electrode and the second electrode is the negative electrode.

[0121] In this specification, the first electrode may be an anode and the second electrode may be a cathode, or vice versa.

[0122] A secondary battery according to one embodiment of the present specification may particularly include the anode for a lithium-ion secondary battery described above. Specifically, the secondary battery may include a cathode, a cathode, a separator interposed between the cathode and the anode, and an electrolyte, wherein the cathode is identical to the anode described above. Since the anode has been described above, a detailed description thereof will be omitted.

[0123] The above positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and including the positive electrode active material.

[0124] In the above positive electrode, the positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 µm to 500 µm, and fine unevenness may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0125] The above positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound having the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4(0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein, M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3 Lithium manganese composite oxide represented by O2 (wherein, M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≤c3≤0.1) or Li2Mn3MO8 (wherein, M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); LiMn2O4, etc., in which a part of Li in the chemical formula is replaced with an alkaline earth metal ion, but is not limited thereto. The positive electrode may be Li-metal.

[0126] The above-described positive electrode active material layer may include a positive electrode conductive material and a positive electrode binder together with the positive electrode active material described above.

[0127] At this time, the positive electrode conductive material is used to provide conductivity to the positive electrode, and in the battery to be constructed, it can be used without special restrictions as long as it does not cause a chemical change and has electronic conductivity. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used.

[0128] In addition, the positive electrode binder plays a role of improving the adhesion between positive electrode active material particles and the adhesiveness between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof.

[0129] The separator is used to separate the negative electrode and the positive electrode and to provide a passage for lithium ions. Any separator commonly used in secondary batteries can be used without any particular restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.

[0130] Examples of the above electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium-ion secondary batteries.

[0131] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0132] As the above non-aqueous organic solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidone (NMP), propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolan, formamide, dimethylformamide, dioxolan, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxy methane, dioxolan derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl pyropionate, ethyl propionate, etc. can be used. Can be.

[0133] In particular, among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants and thus can be preferably used because they easily dissociate lithium salts. In addition, when low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate are mixed and used in an appropriate ratio with these cyclic carbonates, an electrolyte with high electrical conductivity can be produced, so that they can be used even more preferably.

[0134] The metal salt may be a lithium salt, and the lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte, for example, the anion of the lithium salt is F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 -, CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.

[0135] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as, for example, a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, a cyclic ether, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery.

[0136] One embodiment of the present invention provides a battery module including the secondary battery as a unit cell and a battery pack including the same. The battery module and battery pack include the secondary battery having high capacity, high rate characteristics, and cycle characteristics, and thus can be used as a power source for medium- to large-sized devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0137] <Method for manufacturing lithium-ion secondary batteries>

[0138] In another embodiment of the present invention, a method for manufacturing a lithium ion secondary battery includes the steps of: preparing an anode slurry by mixing the anode composition for a lithium ion secondary battery with a solvent; applying the anode slurry to one or both sides of a current collector layer; and drying the current collector layer to which the anode slurry is applied, wherein the anode composition for a lithium ion secondary battery, the anode slurry, the solvent, the current collector layer, and the application method are as described above.

[0139] In this specification, the drying uses a known method such as air drying.

[0140] In this specification, the steps such as rolling applied after the steps included in the method for manufacturing the lithium ion secondary battery are as known in the art.

[0141] Hereinafter, preferred embodiments are presented to help understand the present invention, but the above embodiments are only illustrative of the present disclosure, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of ​​the present disclosure, and it is natural that such changes and modifications fall within the scope of the appended patent claims.

[0142] <Synthesis Example: Synthesis of an Aqueous Binder>

[0143] Synthesis Example 1

[0144] Acrylamide (AM) and acrylic acid (AA) were mixed in a weight ratio of 40:60 in a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe, and then a polymerization initiator (ammonium persulfate) was added and reacted at 75°C for 8 hours to prepare a polymer aqueous solution.

[0145] Then, a 0.1 molar concentration aqueous solution of NaOH was added dropwise to the polymer aqueous solution to neutralize it, and then an aqueous binder 1 was prepared.

[0146] Synthesis Example 2

[0147] Aqueous binder 2 was prepared in the same manner as in Synthesis Example 1, except that acrylamide (AM: Acryl amide) and acrylic acid (AA: acrylic acid) were mixed in a weight ratio of 70:30.

[0148] Synthesis Example 3

[0149] Aqueous binder 3 was prepared in the same manner as in Synthesis Example 1, except that acrylamide (AM), acrylic acid (AA), and acrylonitrile (AN) were mixed in a weight ratio of 55:30:15.

[0150] Synthesis Example 4

[0151] Aqueous binder 4 was prepared in the same manner as in Synthesis Example 1, except that acrylamide (AM: Acryl amide) and acrylic acid (AA: acrylic acid) were mixed in a weight ratio of 80:20.

[0152] Comparative Synthesis Example 1

[0153] Comparative binder 1 was prepared in the same manner as in Synthesis Example 1, except that acrylamide (AM: Acryl amide) and acrylic acid (AA: acrylic acid) were mixed in a weight ratio of 5:95.

[0154] Comparative Synthesis Example 2

[0155] Comparative binder 2 was prepared in the same manner as in Synthesis Example 1, except that acrylamide (AM: Acryl amide) and acrylic acid (AA: acrylic acid) were mixed in a weight ratio of 85:10.

[0156] Comparative Synthesis Example 3

[0157] Comparative binder 3 was prepared in the same manner as in Synthesis Example 1, except that acrylamide (AM), acrylic acid (AA), and acrylonitrile (AN) were mixed in a weight ratio of 25:60:15.

[0158] Comparative Synthesis Example 4

[0159] Comparative binder 4 was prepared in the same manner as in Synthesis Example 1, except that styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) were mixed in a 2:1 ratio.

[0160] <Manufacturing Examples 1 to 3: Preparation of pre-dispersed solution>

[0161] Single-walled carbon nanotubes (SWCNT) (OCSiAl, Tuball) were used as a conductive agent, polyvinylpyrrolidone (PVP) (Zhangzhou huafu chemical, K15), a nonionic vinyl compound, was added as a dispersant, and tannic acid (Sigma-Aldrich) was added as a viscosity modifier. Then, SWCNT: PVP: Tannic Acid were mixed at a weight ratio of 1:1:0.4, and then primary dispersion was performed using a high-shear force in-line mixer (primary mixing).

[0162] Then, a pre-dispersed solution having a solid content of 1 wt% and a specific particle size was prepared by repeatedly circulating the solution while controlling the pressure five times using a high-pressure homogenizer (Micronox, model number: PICOMAX) (secondary mixing). The particle size of the single-walled carbon nanotubes was measured using a Malvern particle size distribution meter. The results are shown in Table 1 below.

[0163] The single-walled carbon nanotubes (SWCNTs) and dispersant were mixed in the ratios shown in Table 1 below (based on weight ratio (wt%) relative to 100 wt% of the cathode composition).

[0164] <Examples and Comparative Examples: Manufacturing of Cathode>

[0165] As described in Table 1 below, a solvent (water) was added to each cathode composition and stirred while taking into account the coating property and solid content to prepare a cathode slurry.

[0166] ClassificationCathode active material compositionConductorBinder (weight ratio)SWCNT (weight ratio) and particle size distribution (length)Dispersant (weight ratio)Example 1Pure Si(SiOx (x=0))(100)SWCNT (0.5)PVP(0.5)Aqueous binder 1(10)SWCNT content with a length of more than 0㎛ and less than 0.2㎛ (0.2 parts by weight based on 100 parts by weight of the total SWCNT) and SWCNT content with a length of more than 10㎛ and less than 100㎛ (42 parts by weight based on 100 parts by weight of the total SWCNT)Example 2Pure Si(100)SWCNT (0.5)PVP(0.75)Aqueous binder 2(10)Same dispersion particle size as in Example 1Example 3Artificial graphite + SiOx(0 < x < 2)(92:8) Weight ratio)(100)SWCNT (0.5)PVP(0.75)Aqueous binder 2(10)Same dispersion particle size as Example 1 Example 4 Artificial graphite + SiC(90:10)(100)SWCNT (0.5)PVP(0.35)Aqueous binder 2(10)Same dispersion particle size as Example 1 Example 5 Pure Si(100)SWCNT (0.5)PVP(0.5)Aqueous binder 3(10)Same dispersion particle size as Example 1 Example 6 Artificial graphite + SiOx(0 < x < 2)(92:8)(100)SWCNT (0.5)PVP(0.35)Aqueous binder 4(10)Same dispersion particle size as Example 1 Comparative example 1 Pure Si(100)SWCNT (0.5) Cellulose (0.5) Comparative binder 1 (10) Same dispersion particle size as Example 1 Comparative example 2 Pure Si (100) SWCNT (0.5) Cellulose dispersant (0.75) Comparative binder 4 (10) Same dispersion particle size as Example 1 Comparative example 3 Synthetic graphite + SiO x (0 < x < 2) (92:8) (100) SWCNT (0.5) Cellulose (0.5) Comparative binder 1 (10) Same dispersion particle size as Example 1 Comparative example 4 Synthetic graphite + SiC (90:10) (100) SWCNT (0.5) Cellulose (0.5) Comparative binder 1 (10) Same dispersion particle size as Example 1 Comparative example 5 Pure Si (100) SWCNT (0.5)PVP(0.75) Comparative binder 2 (10) Same dispersion particle size as Example 1 Comparative example 6 Artificial graphite + SiOx (0 < x < 2) (92:8) (100) SWCNT (0.5) Cellulose (0.7) Comparative binder 3 (10) Same dispersion particle size as Example 1 Comparative example 7 Pure Si (100) SWCNT (0.5) PVP (0.75) Comparative binder 4 (10) Same dispersion particle size as Example 1 Comparative example 8 Artificial graphite + SiC (90:10) (100) SWCNT (0.5) Cellulose (0.5) Aqueous binder 1 (10) Same dispersion particle size as Example 1 Reference example 1 Pure Si (100) SWCNT (0.5) PVP (0.5) Aqueous binder 1(10) Content of SWCNTs with a length exceeding 0㎛ and less than 0.2㎛ (15 parts by weight based on 100 parts by weight of total SWCNTs) and content of SWCNTs with a length exceeding 10㎛ and less than 100㎛ (8 parts by weight based on 100 parts by weight of total SWCNTs) Reference Example 2 Artificial graphite + SiC(90:10)(100)SWCNT (0.5)PVP(0.5)Water-based binder 2(10) Content of SWCNTs with a length exceeding 0㎛ and less than 0.2㎛ (0 parts by weight based on 100 parts by weight of total SWCNTs) and content of SWCNTs with a length exceeding 10㎛ and less than 100㎛ (7 parts by weight based on 100 parts by weight of total SWCNTs).

[0167] <Experimental Example: Battery Characteristics Experiment>

[0168] The negative electrode slurry described in Table 1 above was coated on a copper foil having a thickness of 15 μm, dried, and a negative electrode active material layer having a thickness of 48 μm was formed on one side of the copper foil, and then punched into a circle having a diameter of 14 Φ (mm) to manufacture a negative electrode for testing.

[0169] A 0.3 mm thick metallic lithium foil was used as the anode, a 0.1 mm thick porous polyethylene sheet was used as the separator, and a 7:3 volume ratio mixed solvent of fluoroethylene carbonate (FEC) and diethyl carbonate (DEC) was used as the electrolyte, and a 8:2 volume ratio of LiPF6 and LiTFSI (lithium bis(trisfluoromethanesulfonyl)imide) was used as the lithium salt, dissolved at a concentration of approximately 1 mol / L.

[0170] The above cathode, anode, separator, and electrolyte were sealed in a stainless steel container to manufacture a coin cell for evaluation with a thickness of 2 mm and a diameter of 32 mm.

[0171] No. Experimental Example 1: Initial Efficiency (%) Experimental Example 2: Capacity Retention Rate (%) Example 191.583 Example 291.887 Example 390.781 Example 493.185 Example 591.785 Example 693.86 Comparative Example 191.065 Comparative Example 290.266 Comparative Example 390.251 Comparative Example 493.056 Comparative Example 591.568 Comparative Example 693.771 Comparative Example 791.467 Comparative Example 893.274 Reference Example 191.876 Reference Example 293.071

[0172] - Initial efficiency (%): The coin cell was charged at a constant current of 0.05 C until the voltage became 0.01 V, and discharged at a constant current of 0.05 C until the voltage became 1.5 V, and the discharge capacity and initial efficiency were obtained, respectively, and expressed as a value of (discharge capacity / charge capacity) x 100 (%).

[0173] - Capacity retention rate (%): The coin cell was charged at a constant current of 0.05C until the voltage became 0.01V, discharged at a constant current of 0.05C until the voltage became 1.5V, and then the cycle characteristics were tested at a constant current of 0.2C in the same voltage range as above to perform a capacity retention rate test, and calculated based on 30 cycles.

[0174] As shown in Table 2 above, Examples 1 to 6 used an aqueous binder containing (meth)acrylamide in an amount of 30 wt% or more and 80 wt% or less based on the total aqueous binder, and used a nonionic vinyl compound (PVP) as a dispersant. As a result, the initial efficiency was all 90% or more, and at the same time, the capacity retention rate was all 80% or more.

[0175] In contrast, Comparative Example 5 achieved a high initial efficiency of 91.5% by using a binder with a (meth)acrylamide content outside the range of the present invention (i.e., 30 wt% to 80 wt% based on 100 wt% of the total aqueous binder), even though a nonionic vinyl compound was used as a dispersant, but the capacity retention rate was 68%.

[0176] In addition, Comparative Example 7 achieved a high initial efficiency of 91.4%, but showed a capacity retention rate of 67%, because it used a binder that was a mixture of styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) that did not contain (meth)acrylamide, even though a nonionic vinyl compound was used as a dispersant.

[0177] In addition, Comparative Example 8 achieved a high initial efficiency of 93.2%, but showed a capacity retention rate of 74% because it did not use a nonionic vinyl compound as a dispersant even though it used an aqueous binder having a (meth)acrylamide content satisfying the range of the present invention.

[0178] In addition, in comparison, 1 to 4 and 6 not only used binders having a (meth)acrylamide content exceeding 30 wt% to 80 wt% based on 100 wt% of the total aqueous binder, but also used a cellulose dispersant and not a nonionic vinyl dispersant, all of which achieved initial efficiencies higher than 90%, but exhibited capacity retention rates of 65%, 66%, 51%, 56%, or 71%, respectively.

[0179] Therefore, considering Comparative Examples 5 and 7, it can be seen that when the (meth)acrylamide content of the aqueous binder is outside the range of 30 wt% to 80 wt%, the effect on the capacity retention rate is as great as that of not including (meth)acrylamide.

[0180] In addition, when comparing Comparative Examples 5 and 8, it can be seen that the (meth)acrylamide content factor has a greater effect on the improvement of capacity retention than the dispersant factor, and from Comparative Examples 1 to 4 and 6, it can be seen that when the above two factors are not satisfied, the deterioration of capacity retention is aggravated.

[0181] Comparing Reference Examples 1 and 2 with Examples 1 and 4, it can be seen that there is a difference in capacity retention depending on whether the particle size distribution range of the single-walled carbon nanotube according to the present invention is satisfied.

Claims

1. A negative electrode composition for a lithium ion secondary battery comprising a negative electrode active material; a conductive material; and an aqueous binder, The above-mentioned conductive agent comprises a pre-dispersed liquid containing single-walled carbon nanotubes (SWCNTs) and a dispersant, The above aqueous binder contains (meth)acrylamide (AM) in an amount of 30 wt% to 80 wt% based on 100 wt% of the total aqueous binder, A negative electrode composition for a lithium ion secondary battery, wherein the dispersant comprises a nonionic vinyl compound.

2. In claim 1, A negative electrode composition for a lithium ion secondary battery, wherein the negative electrode active material comprises at least one selected from the group consisting of silicon-based active materials and carbon-based active materials.

3. In claim 2, The above silicon-based active material is SiOx (x=0), SiOx (0 <x<2), SiC 및 Si 합금 중 1 이상을 포함하는 것인 리튬이온 이차전지용 음극 조성물.

4. In claim 2, When the above negative active material is composed solely of a silicon-based active material, the silicon-based active material is composed of SiOx (x=0) and SiOx (0 <x<2)로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 70 중량부 이상 포함하는 것인 리튬이온 이차전지용 음극 조성물.

5. In claim 2, A negative electrode composition for a lithium ion secondary battery, wherein the carbon-based active material comprises at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, and soft carbon.

6. In claim 2, A negative electrode composition for a lithium ion secondary battery, wherein when the negative electrode active material includes a silicon-based active material and a carbon-based active material, the weight ratio between the silicon-based active material and the carbon-based active material is within a range of 2:98 to 30:

70.

7. In claim 1, A negative electrode composition for a lithium ion secondary battery, wherein the nonionic vinyl compound comprises at least one selected from the group consisting of polyvinyl pyrrolidone (PVP) and polyvinyl butyral (PVB).

8. In claim 1, A negative electrode composition for a lithium ion secondary battery, wherein the above aqueous binder is a copolymer comprising (meth)acrylamide (AM) as a first repeating unit and (meth)acrylic acid (AA) as a second repeating unit.

9. In claim 8, A negative electrode composition for a lithium ion secondary battery, wherein the above aqueous binder is a copolymer further comprising (meth)acrylonitrile (AN) as a third repeating unit.

10. A negative electrode slurry comprising a negative electrode composition for a lithium ion secondary battery according to any one of claims 1 to 9 and a solvent.

11. A negative electrode comprising a current collector layer; and a negative electrode active material layer provided on one or both sides of the current collector layer, wherein the negative electrode active material layer comprises a negative electrode slurry according to claim 10 or a dried product thereof.

12. First electrode; Second electrode; A separator interposed between the first electrode and the second electrode; and A lithium ion secondary battery containing an electrolyte, A lithium ion secondary battery, wherein either one of the first electrode and the second electrode is a negative electrode according to claim 11.

Citation Information

Patent Citations

  • Negative electrode composition for lithium ion secondary battery, negative electrode slurry, negative electrode and lithium ion secondary battery

    KR1020240147950A

  • Binder for secondary battery comprising copolymer of vinyl acetate or vinyl alcohol

    KR1020090019630A

  • Slurry composition for negative electrode for lithium-ion secondary battery, negative electrode for lithium-ion secondary battery, and lithium-ion secondary battery

    KR1020150132156A

  • Binder composition for non-aqueous secondary cell electrode, slurry composition for non-aqueous secondary cell electrode, non-aqueous secondary cell electrode, and non-aqueous secondary cell

    KR1020180063077A

  • Photocatalyst composition and method for preparing the same

    KR1020220099768A