Electrolytes, electrolyte materials, and manufacturing thereof
Patent Information
- Application Number
- PCT/US2024/022418
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-11-14
AI Technical Summary
Current sodium-ion conductors, such as sulfides and halides, face limitations in stability and conductivity, leading to poor performance and short cycle life in sodium secondary batteries, with sulfides having a narrow electrochemical window and halides exhibiting lower conductivity and thermal instability.
A new oxychloride-based sodium electrolyte with the formula NaAxMi.xOC14-x, where 0
The new electrolyte provides high ionic conductivity, thermal stability, and improved rate capability, preventing cathode-electrolyte interphase formation and maintaining performance over a wide temperature range, thus enhancing the durability and Coulombic efficiency of sodium secondary batteries.
Smart Images

Figure US2024022418_14112024_PF_FP_ABST
Abstract
Description
ELECTROLYTES, ELECTROLYTE MATERIALS, AND MANUFACTURING THEREOF BACKGROUND OF THE DISCLOSURE
[0001] Bateries comprise one or more of an electrochemical cell, such a cell generally comprises a cathode, an anode and an electrolyte. Sodium ion secondary bateries may use a sodium transition metal oxide or ferrocyanide positive electrode active material and a hard carbon-based, oxide-based, alloy-based, metal elemental, or nonmetal elemental negative electrode active material and may use different types of electrolytes such as an electrolyte in solid or liquid form and an organic or inorganic electrolyte, to ensure sodium ionic conductivity between the positive electrode and the negative electrode.SUMMARY OF THE DISCLOSURE
[0002] In certain aspects, the present disclosure relates to a compound having a chemical formula of NaAxMi.x0C14.x, where 0<x<l, wherein A may be an element with a 4+ oxidation state, wherein M may be an element with a 5+ oxidation state. In some embodiments, 0<x<l.
[0003] In some embodiments, the compound NaAxMi.xOC14-xmay have a chemical formula of NaAOCh. where x = 1. In some embodiments, the compound NaAxMi.xOC14-xmay have a chemical formula of NaMOCL, where x = 0.
[0004] In some embodiments, x may be from about 0 to about 0.9. In some embodiments, x may be from about 0 to about 0.8. In some embodiments, x may be from about 0 to about 0.7. In some embodiments, x may be from about 0. 1 to about 0.5. In some embodiments, x may be about 0.25.
[0005] In some embodiments, the element with the 4+ oxidation state may comprise Zr, Ti, Si, Ge, or Sn. In some embodiments, the element with the 5+ oxidation state may comprise Nb, Ta, Mo, V, Mn, or Sb.
[0006] In some embodiments, the compound may be a conductor based on a sodium cation. In some embodiments, the compound may be an electrolyte including a sodium cation.
[0007] In some embodiments, the compound may have an ionic conductivity of from about 10'11to about 10'6S / cm. In some embodiments, the compound may have an ionic conductivity of from about 10'10to about 10'5S / cm. In some embodiments, the compound may have an ionic conductivity of from about 10'8to about 10'4S / cm. In some embodiments, the compound may have an ionic conductivity of from about 10'7to about 10'4S / cm. In some embodiments, the compound may have an ionic conductivity of from about 10'6to about 10'3S / cm. In some embodiments, the compound may have an ionic conductivity of from about 10'5to about 10'2S / cm.
[0008] In some embodiments, the compound may be formed by a chemical reaction between a sodium-containing compound and a metal chloride, wherein the metal may be the element with 4+ oxidation state, the element with 5+ oxidation state, or combinations thereof.
[0009] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and an element with a 4+ oxidation state, wherein a molar ratio between the element with the 4+ oxidation state and the sodium cation may be up to 1 or less.
[0010] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and an element with a 5+ oxidation state, wherein a molar ratio between the element with the 5+ oxidation state and the sodium cation may be up to 1 or less.
[0011] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state wherein a molar ratio between the element with the 4+ oxidation and the sodium cation may be up to 1 or less or a molar ratio between the element with the 5+ oxidation state and the sodium cation may be up to 1 or less.
[0012] In some embodiments, a molar ratio between the chloride and the sodium cation may be from about 3 to about 4.
[0013] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation may be from about 3 to about 4.
[0014] In certain aspects, the present disclosure relates to a composition consisting essentially of sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation may be from about 3 to about 4.
[0015] In certain aspects, the present disclosure relates to a composition consisting of sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation may be from about 3 to about 4.
[0016] In some embodiments, a molar ratio between the element with the 4+ oxidation state and the sodium cation may be up to 1 or less. In some embodiments, a molar ratio between the element with the 5+ oxidation state and the sodium cation may be up to 1 or less.
[0017] In some embodiments, a molar ratio between the sodium cation and a molar combination of the element with the 4+ oxidation state and the element with the 5+ oxidation state may be 1.
[0018] In some embodiments, a molar ratio of the chloride to the element with a 4+ oxidation state to the element with a 5+ oxidation state may be 4-x : x : 1-x, where 0<x<l. In some embodiments, 0<x<l.
[0019] In some embodiments, the composition may have a chemical formula of NaAOCh. wherein x= 1 and wherein A may be the element with a 4+ oxidation state. In some embodiments, the composition may have a chemical formula of NaMOC’h. wherein x = 0 and wherein M may be the element with a 5+ oxidation state.
[0020] In some embodiments, x may be from about 0 to about 0.9. In some embodiments, x may be from about 0 to about 0.8. In some embodiments, x may be from about 0 to about 0.7. In some embodiments, x may be from about 0.1 to about 0.5. In some embodiments, x may be about 0.25. In some embodiments, the element with the 4+ oxidation state may comprise Zr, Ti, Si, Ge, or Sn. In some embodiments, the element with the 5+ oxidation state may comprise Nb, Ta, Mo, V, Mn, or Sb.
[0021] In some embodiments, the composition may be a conductor based on the sodium cation. In some embodiments, the composition may be an electrolyte including the sodium cation.
[0022] In some embodiments, the composition may have an ionic conductivity of from about 10"11to about 10'6S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'10to about 10'5S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'8to about 10'4S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'7to about 10'4S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'6to about 10'3S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'5to about 10'2S / cm.
[0023] In some embodiments, the composition may be formed by a chemical reaction between a sodium containing compound and a metal chloride, wherein the metal may be the element with 4+ oxidation state, the element with 5+ oxidation state, or a combination thereof.
[0024] In certain aspects, the present disclosure relates to a composition formed by a chemical reaction between a sodium containing compound and a metal chloride, wherein the metal may be an element with a 4+ oxidation state, a 5+ oxidation state, or a combination thereof.
[0025] In some embodiments, the composition may comprise sodium cation (Na+), oxygen (O), chloride (Cl), and the element with a 4+ oxidation state, wherein a molar ratio between the element with the 4+ oxidation state and the sodium cation may be up to 1 or less. In some embodiments, thecomposition may comprise sodium cation (Na+), oxygen (O), chloride (Cl), and the element with a 5+ oxidation state, wherein a molar ratio between the element with the 5+ oxidation state and the sodium cation may be up to 1 or less. In some embodiments, the composition may comprise sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from the element with a 4+ oxidation state and the element with a 5+ oxidation state wherein a molar ratio between the element with the 4+ oxidation and the sodium cation may be up to 1 or less or a molar ratio between the element with the 5+ oxidation state and the sodium cation may be up to 1 or less.
[0026] In some embodiments, a molar ratio between the chloride and the sodium cation may be from about 3 to about 4. In some embodiments, the composition may comprise sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation may be from about 3 to about 4. In some embodiments, the composition consists essentially of sodium cation (Na+), oxygen (O), chloride (Cl), and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation may be from about 3 to about 4. In some embodiments, the composition consists of sodium cation (Na+), oxygen (O), chloride (Cl), and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation may be from about 3 to about 4.
[0027] In some embodiments, a molar ratio between the element with the 4+ oxidation state and the sodium cation may be up to 1 or less. In some embodiments, a molar ratio between the element with the 5+ oxidation state and the sodium cation may be up to 1 or less.
[0028] In some embodiments, a molar ratio between the sodium cation and a molar combination of the element with the 4+ oxidation state and the element with the 5+ oxidation state may be 1.
[0029] In some embodiments, a molar ratio of the chloride to the element with a 4+ oxidation state to the element with a 5+ oxidation state may be 4-x : x : 1-x, where 0<x<l. In some embodiments, 0<x<l.
[0030] In some embodiments, the compound NaAxMi.xOC14-x may have a chemical formula of NaAOCh. wherein x = 1 and wherein A may be the element with a 4+ oxidation state. In some embodiments, the compound may have a chemical formula of NaMOC’h. where in x = 0 and wherein M may be the element with a 5+ oxidation state.
[0031] In some embodiments, x may be from about 0 to about 0.9. In some embodiments, x may be from about 0 to about 0.8. In some embodiments, x may be from about 0 to about 0.7.
[0032] In some embodiments, x may be from about 0. 1 to about 0.5. In some embodiments, x may be about 0.25. In some embodiments, x may be about 0.
[0033] In some embodiments, the element with the 4+ oxidation state may comprise Zr, Ti, Si, Ge, or Sn. In some embodiments, the element with the 5+ oxidation state may comprise Nb, Ta, Mo, V, Mn, or Sb.
[0034] In some embodiments, the composition may be a conductor based on sodium cation.
[0035] In some embodiments, the composition may be an electrolyte including sodium cation.
[0036] In some embodiments, the composition may have an ionic conductivity of from about 10"11to about 10'6S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'10to about 10'5S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'8to about 10'4S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'7to about 10'4S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'6to about 10'3S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'5to about 10'2S / cm.
[0037] In some embodiments, the sodium containing compound may be sodium hydroxide (NaOH), sodium chloride (NaCl), sodium oxide (Na2O), or combinations thereof. In some embodiments, sodium hydroxide (NaOH) is in solid form, powder form or pellet form.
[0038] The present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl), an element with a 4+ oxidation state, or an element with a 5+ oxidation state, wherein the composition may have an ionic conductivity of from about 10'11to about 10'6S / cm.
[0039] In some embodiments, the composition may have an ionic conductivity of from about 10"10to about 10'5S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'8to about 10'4S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'7to about 10'4S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'6to about 10'3S / cm. In some embodiments, the composition may have an ionic conductivity of from about 10'5to about 10'2S / cm.
[0040] In some embodiments, a molar ratio between the chloride and the sodium cation may be from about 3 to about 4.
[0041] In some embodiments, a molar ratio between the element with the 4+ oxidation state and the sodium cation may be up to 1 or less. In some embodiments, a molar ratio between the element with the 5+ oxidation state and the sodium cation may be up to 1 or less.
[0042] The present disclosure relates to an electrolyte comprising a compound discussed above or a composition discussed above.
[0043] In some embodiments, the electrolyte may further comprise a conductive material.In some embodiments, the conductive material may be selected from the group consisting of natural graphite, artificial graphite, Super-P, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, Denka black, vapor grown carbon fibers, carbon nanotubes and combinations thereof.
[0044] In some embodiments, the electrolyte may further comprise a binder resin. In some embodiments, the binder resin may be selected from the group consisting of polytetrafluoroethylene, polyvinylidene difluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride- co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan and carboxyl methyl cellulose, polyacrylic acid, polyacrylic acid salt derivatives, and combinations thereof.
[0045] The present disclosure relates to a battery comprising the electrolyte related to the present disclosure, a negative electrode material, and a positive electrode material.
[0046] In some embodiments, the battery may further comprise a catholyte. In some embodiments, the battery may further comprise an anolyte.
[0047] In some embodiments, the electrolyte may be in contact with the positive electrode material, a catholyte, or a combination thereof.
[0048] In some embodiments, the electrolyte may be a catholyte.
[0049] In some embodiments, the battery further may comprise an anolyte-side electrolyte different from the electrolyte and in contact with the negative electrode material or an anolyte, or a combination thereof.
[0050] In some embodiments, the anolyte-side electrolyte may comprise a closo-borate.
[0051] In some embodiments, the negative electrode material may comprise a metal anode material, a metal elemental anode material, a nonmetal elemental anode material, an alloy material, a transition metal oxide material, a carbon-based material, or combinations thereof.
[0052] In some embodiments, the negative material may comprise a binder resin, a conductive carbon additive material, a solid electrolyte, or combinations thereof.
[0053] In some embodiments, the positive material may be included in a positive active material layer.
[0054] In some embodiments, the positive electrode material may comprise sodium transition metal oxide active material as a positive electrode active material, and preferably the transition metal may comprise at least one of Cr, Mn, Fe, Ni, or V. In some embodiments, the positive electrode material may comprise sodium transition metal oxide, sodium transition metal polyanionic oxide, sodium ferrocyanide or combinations thereof as a positive electrode active material, and wherein the transition metal may comprise at least one of Cr, Mn, Fe, Ni, or V. In some embodiments, the positive electrode material may comprise a NasX lPCb); cathode (NVP). In some embodiments, the positive electrode material may comprise a NaCrCF cathode (NCO).
[0055] In some embodiments, the positive electrode material may comprise a binder resin, a conductive material, the electrolyte, or combinations thereof.
[0056] In some embodiments, the positive electrode active material layer may be formed from a dry mixing without a solvent using the positive electrode active material, the conductive material and the binder resin.
[0057] In some embodiments, the battery may further comprise a conductive material.In some embodiments, the conductive material may be selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powder, conductive whiskers, conductive metal oxide, activated carbon, polyphenylene derivatives, and combinations thereof.
[0058] In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, more preferably at least 95%, more preferably at least 100% for the first 50 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 40 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 30 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 20 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 10 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 5 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 3 cycles. In some embodiments,the batery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first cycle.
[0059] In some embodiments, the batery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of from about 0. 1 to about 30.0.BRIEF DESCRIPTION OF THE DRAWINGS
[0060] It is to be expressly understood that the drawings are for the purpose of illustration and description only and are not intended as a definition of the limits of the disclosure.
[0061] FIG. 1 shows an X-ray diffraction patern of the electrolyte NaNbOCb. in some embodiments.
[0062] FIG. 2 shows an X-ray diffraction patern of the electrolyte NaTaOC’b. in some embodiments.
[0063] FIG. 3 shows the ionic conductivity of the electrolytes NaMOCb, where M = Nb, Ta, in some embodiments.
[0064] FIG. 4 are Arrhenius plots of the conductivities of the electrolytes NaMOCb, where M = Nb, Ta, in some embodiments.
[0065] FIG. 5 shows the ionic conductivity of the electrolytes NaZro.25Tao.75OQ3.75 and NaZrOCb. where Zr (which has an oxidation state of 4+) has substituted for Ta (which has an oxidation state of 5+); the formulas NaZro.25Tao.75OCl3.75 and NaZrOCb correspond to 25% and 100% substitution (Zr for Ta), respectively, in some embodiments.
[0066] FIG. 6 shows the electronic conductivity of the electrolyte NaNbOCb, in some embodiments.
[0067] FIG. 7 shows the electronic conductivity of the electrolyte NaTaOCb, in some embodiments.
[0068] FIG. 8 shows the linear sweep voltammetry (LSV) scan (from open circuit voltage, or OCV, to 5V, and from OCV to 0V) of NaNbOCb, in some embodiments.
[0069] FIG. 9 shows the linear sweep voltammetry (LSV) scan (from open circuit voltage, or OCV, to 5V, and from OCV to 0V) of NaTaOCL, in some embodiments.
[0070] FIG. 10 shows the room temperature rate performance comparison between the electrolyte NaTaOC’h and a reference halide. These are incorporated in a sodium secondary battery comprising of Na-Sn 2: 1 alloy as the anode, a reference closo-borate electrolyte as the electrolyte, the catholyte, and a Nas ¥2(004)3 cathode (NVP), in some embodiments. One battery has a reference halide electrolyte as the catholyte, and another has NaTaOC’h as the catholyte, in some embodiments.
[0071] FIG. 11 shows the voltage profdes from cycling of a sodium secondary battery, comprising of Na-Sn 2: 1 alloy as the anode, a reference closo-borate as the electrolyte, NaTaOC’h as the catholyte, and an NVP cathode, in some embodiments.
[0072] FIG. 12 shows the capacity retention from cycling of a sodium secondary battery, the same as shown in FIG. 11, which comprises of Na-Sn 2: 1 alloy as the anode, a reference closo-borate as the electrolyte, NaTaOCU as the catholyte, and a NaCrO? cathode (NCO), in some embodiments.
[0073] FIG. 13 shows the X-ray diffraction pattern of NaNbOC’h after annealing, or heat treatment, at 300°C (over 24 hours), under an argon atmosphere, in some embodiments.
[0074] FIG. 14 shows the X-ray diffraction pattern of NaTaOC’h after annealing, or heat treatment, at 300°C (over 24 hours), under an argon atmosphere, in some embodiments.
[0075] FIG. 15 shows the ionic conductivity of NaNbOC’h after annealing or heat treatment to 300°C over 24 hours, in some embodiments.
[0076] FIG. 16 shows the ionic conductivity of and NaTaOCL after annealing or heat treatment to 300°C over 24 hours, in some embodiments.DETAILED DESCRIPTION OF THE DISCLOSURE
[0077] Hereinafter, the present disclosure will be described in detail. Prior to the description, it should be understood that the terms or words used in the specification and the appended claims should not be construed as limited to general and dictionary meanings, but rather interpreted based on the meanings and concepts corresponding to the technical aspects of the present disclosure on the basis of the principle that the inventor is allowed to define terms appropriately for the best explanation. Therefore, the embodiments described herein and the elements shown in the drawings is just a most preferred embodiment of the present disclosure, but not intended to fully describe the technical aspects of the present disclosure, so it should be understood that other equivalents and modifications could have been made thereto at the time the application was filed.Certain Definitions
[0078] The use of the terms "a" and "an" and "the" and similar referents in the context of describing the disclosure (especially in the context of the following claims) are to be construed to cover both the singular and the plural, unless otherwise indicated herein or clearly contradicted by context. The terms "comprising," "having," "including," and "containing" are to be construed as open-ended terms (i.e., meaning "including, but not limited to,") unless otherwise noted. Recitation of ranges of values herein are merely intended to serve as a shorthand method of referring individually to each separate value falling within the range, unless otherwise indicated herein, and each separate value is incorporated into the specification as if it were individually recited herein. All methods described herein can be performed in any suitable order unless otherwise indicated herein or otherwise clearly contradicted by context. The use of any and all examples, or exemplary language (e.g., "such as") provided herein, is intended merely to better illuminate the disclosure and does not pose a limitation on the scope of the disclosure unless otherwise claimed. No language in the specification should be construed as indicating any non-claimed element as essential to the practice of the disclosure.
[0079] The terms "about" and "essentially" are used herein in the sense of at, or nearly at, when given the manufacturing and material tolerances inherent in the stated circumstances and are used to prevent the unscrupulous infringer from unfairly taking advantage of the present disclosure where exact or absolute figures are stated as an aid to understanding the present disclosure.
[0080] "A and / or B" when used in this specification, specifies "either A or B or both".
[0081] Sodium all-solid-state batteries generally can comprise of a cathode, i.e. the positive electrode, for example a sodium transition metal oxide, an anode, i.e. the negative electrode, for example Na metal, Na alloys, or others, and a solid sodium-ion conducting solid electrolyte, which ensures Na ion transport between the two electrodes.
[0082] In certain aspects, the present disclosure recognizes that the solid electrolyte can be sulfide- based. Sulfides may have some limitations. For example, sulfides have a narrow electrochemical window or stability window. Going above / below this window during battery charging / discharging leads to oxidation / reduction, respectively, and thus, degradation of the electrolyte, which leads to poor battery performance, cycle life, and calendar life. Degradation can either occur spontaneously (a chemical reaction) or during cycling (an electrochemical reaction). A wider stability window enables the electrolyte to be compatible with the anode, cathode, or both.
[0083] In certain aspects, the present disclosure recognizes that a class of sodium-ion conductor, halides, can be used. These have substantially higher oxidative stability than sulfides and have been demonstrated to be stable and compatible, both chemically and electrochemically, with certain transition metal oxide cathodes. With chloride-based sodium-ion conductors, it is possible to extend thecycle life of the solid-state batteries. However, chlorine-based halides have their own drawbacks. In general, they have lower conductivity than the sulfides, which lowers the rate capability of the battery, some halides are also not thermally stable, i.e. their desirable properties degrade with varying temperature, and in addition, they have stability and degradation issues at the anode or negative electrode side, where they have been shown to degrade and reduce even more readily and severely than sulfides. Thus, other classes of sodium-ion conductors have been used for their anode stability, such as the closo-borates. While closo-borate anolytes have helped to address electrolyte stability issues at the anode or negative electrode, a highly conductive and stable catholyte is still necessary to enable sodium all-solid-state battery operation.
[0084] In certain aspects, the present disclosure recognizes that an oxyhalide-based lithium-ion conductor, LiMOC’L. where M = Nb or Ta, may be utilized. Such electrolytes are found to have very high ionic conductivities of 9 mS / cm and 7 mS / cm at room temperature (for the Ta and Nb versions respectively). They can have high oxidation stability by being inert with the oxide cathode LiCoO? and can be used as catholytes in solid-state battery configurations (with a different electrolyte used on the anode side or anolyte). LiMOCU, having an order of magnitude increase in the conductivity of the lithium halide class of solid electrolytes, opens up another new material space for solid ion conductors.
[0085] In certain aspects, the present disclosure relates to a sodium secondary battery comprising a solid or liquid electrolyte material as an electrolyte . Specific examples of the sodium secondary battery include any type of primary battery, secondary battery, fuel cell, solar cell or capacitor such as a super capacitor. In particular, the secondary battery is, to be specific, a sodium ion secondary battery.
[0086] In certain aspects, the present disclosure relates to a sodium based conducting material such as solid-state sodium-ion conducting material. The present disclosure relates to high energy density sodium-based batteries. The present disclosure relates to application, for example, to solid-state batteries, batteries for electric vehicles, portable devices, and stationary energy storage devices.
[0087] In certain aspects, the present disclosure relates to a solid electrolyte that has good properties such as high conductivity, the ability to withstand a higher current density, and a high first cycle Coulombic efficiency.
[0088] In certain aspects, the present disclosure relates to an oxychloride-based sodium electrolyte, or sodium-ion conductor.
[0089] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and an element with a 4+ oxidation state, wherein a molar ratio between the element with the 4+ oxidation state and the sodium cation may be up to 1 or less.
[0090] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and an element with a 5+ oxidation state, wherein a molar ratio between the element with the 5+ oxidation state and the sodium cation may be up to 1 or less.
[0091] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state wherein a molar ratio between the sodium cation and the element with the 4+ oxidation may be up to 1 or less or a molar ratio between the sodium cation the element with the 5+ oxidation state and may be up to 1 or less.
[0092] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.
[0093] In certain aspects, the present disclosure relates to a composition consisting essentially of sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.
[0094] In certain aspects, the present disclosure relates to a composition consisting of sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.
[0095] In certain aspects, the present disclosure relates to a composition comprising sodium cation (Na+), oxygen (O), chlorine (Cl), an element with a 4+ oxidation state, or an element with a 5+ oxidation state, wherein the compound may have an ionic conductivity of from about 10'11to about 10'6S / cm.
[0096] In certain aspects, the present disclosure relates to a composition formed by a chemical reaction between a sodium containing compound and a metal chloride, wherein the metal may be an element with a 4+ oxidation state, a 5+ oxidation state, or a combination thereof.
[0097] In certain aspects, the present disclosure relates to a compound having a chemical formula of NaAxMi.xOCkx, where 0<x<l, wherein A may be an element with a 4+ oxidation state, wherein M may be an element with a 5+ oxidation state.
[0098] In certain aspects, the present disclosure relates to a new sodium-ion conducting electrolyte, NaAxMi.xOC x, where 0<x<l, A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinationsthereof. In the case of the end members, i.e. where only a 4+ element is present, i.e. x = 1, the formula is NaAOCh, and in the case where only a 5+ element is present, i.e. x=0, then the formula is NaMOC
[0099] In some embodiments, x can be more than about 0, such as 0.01. In some embodiments, x can be more than about 0.02, such as 0.01 or 0.03. In some embodiments, x can be more than about 0.05, such as 0.04 or 0.06. In some embodiments, x can be more than about 0.07, such as 0.06 or 0.08. In some embodiments, x can be more than about 0.1, such as 0.09 and 0.11. In some embodiments, x can be more than about 0.12, such as 0.11 and 0.13. In some embodiments, x can be more than about 0.15, such as 0.14 and 0.16. In some embodiments, x can be more than about 0.17, such as 0.16 and 0.18. In some embodiments, x can be more than about 0.2, such as 0.19 and 0.21. In some embodiments, x can be more than about 0.22, such as 0.21 and 0.23. In some embodiments, x can be more than about 0.25, such as 0.24 and 0.26. In some embodiments, x can be more than about 0.27, such as 0.26 and 0.28. In some embodiments, x can be more than about 0.3, such as 0.29 and 0.31. In some embodiments, x can be more than about 0.32, such as 0.31 and 0.33. In some embodiments, x can be more than about 0.35, such as 0.34 and 0.36. In some embodiments, x can be more than about 0.37, such as 0.36 and 0.38. In some embodiments, x can be more than about 0.4, such as 0.39 and 0.41. In some embodiments, x can be more than about 0.42, such as 0.41 and 0.43. In some embodiments, x can be more than about 0.45, such as 0.44 and 0.46. In some embodiments, x can be more than about 0.47, such as 0.46 and 0.48. In some embodiments, x can be more than about 0.5, such as 0.49 and 0.51. In some embodiments, x can be more than about 0.52, such as 0.51 and 0.53. In some embodiments, x can be more than about 0.55, such as 0.54 and 0.56. In some embodiments, x can be more than about 0.57, such as 0.56 and 0.58. In some embodiments, x can be more than about 0.6, such as 0.59 and 0.61. In some embodiments, x can be more than about 0.62, such as 0.61 and 0.63. In some embodiments, x can be more than about 0.65, such as 0.64 and 0.66. In some embodiments, x can be more than about 0.67, such as 0.66 and 0.68. In some embodiments, x can be more than about 0.7, such as 0.69 and 0.71. In some embodiments, x can be more than about 0.72, such as 0.71 and 0.73. In some embodiments, x can be more than about 0.75, such as 0.74 and 0.76. In some embodiments, x can be more than about 0.77, such as 0.76 and 0.78. In some embodiments, x can be more than about 0.8, such as 0.79 and 0.81. In some embodiments, x can be more than about 0.82, such as 0.81 and 0.83. In some embodiments, x can be more than about 0.85, such as 0.84 and 0.86. In some embodiments, x can be more than about 0.87, such as 0.86 and 0.88. In some embodiments, x can be more than about 0.9, such as 0.89 and 0.91. In some embodiments, x can be more than about 0.92, such as 0.91 and 0.93. In some embodiments, x can be more than about 0.95, such as 0.94 and 0.96. In some embodiments, x can be more than about 0.97, such as 0.96 and 0.98. In some embodiments, x can be more than about 0.99, such as 0.98.
[0100] In some embodiments, x can be less than about 0.01, such as 0. In some embodiments, x can be less than about 0.02, such as 0.01 or 0.03. In some embodiments, x can be less than about 0.05,such as 0.04 or 0.06. In some embodiments, x can be less than about 0.07, such as 0.06 or 0.08. In some embodiments, x can be less than about 0.1, such as 0.09 and 0.11. In some embodiments, x can be less than about 0.12, such as 0.11 and 0.13. In some embodiments, x can be less than about 0.15, such as 0.14 and 0.16. In some embodiments, x can be less than about 0.17, such as 0.16 and 0.18. In some embodiments, x can be less than about 0.2, such as 0.19 and 0.21. In some embodiments, x can be less than about 0.22, such as 0.21 and 0.23. In some embodiments, x can be less than about 0.25, such as 0.24 and 0.26. In some embodiments, x can be less than about 0.27, such as 0.26 and 0.28. In some embodiments, x can be less than about 0.3, such as 0.29 and 0.31. In some embodiments, x can be less than about 0.32, such as 0.31 and 0.33. In some embodiments, x can be less than about 0.35, such as 0.34 and 0.36. In some embodiments, x can be less than about 0.37, such as 0.36 and 0.38. In some embodiments, x can be less than about 0.4, such as 0.39 and 0.41. In some embodiments, x can be less than about 0.42, such as 0.41 and 0.43. In some embodiments, x can be less than about 0.45, such as 0.44 and 0.46. In some embodiments, x can be less than about 0.47, such as 0.46 and 0.48. In some embodiments, x can be less than about 0.5, such as 0.49 and 0.51. In some embodiments, x can be less than about 0.52, such as 0.51 and 0.53. In some embodiments, x can be less than about 0.55, such as 0.54 and 0.56. In some embodiments, x can be less than about 0.57, such as 0.56 and 0.58. In some embodiments, x can be less than about 0.6, such as 0.59 and 0.61. In some embodiments, x can be less than about 0.62, such as 0.61 and 0.63. In some embodiments, x can be less than about 0.65, such as 0.64 and 0.66. In some embodiments, x can be less than about 0.67, such as 0.66 and 0.68. In some embodiments, x can be less than about 0.7, such as 0.69 and 0.71. In some embodiments, x can be less than about 0.72, such as 0.71 and 0.73. In some embodiments, x can be less than about 0.75, such as 0.74 and 0.76. In some embodiments, x can be less than about 0.77, such as 0.76 and 0.78. In some embodiments, x can be less than about 0.8, such as 0.79 and 0.81. In some embodiments, x can be less than about 0.82, such as 0.81 and 0.83. In some embodiments, x can be less than about 0.85, such as 0.84 and 0.86. In some embodiments, x can be less than about 0.87, such as 0.86 and 0.88. In some embodiments, x can be less than about 0.9, such as 0.89 and 0.91. In some embodiments, x can be less than about 0.92, such as 0.91 and 0.93. In some embodiments, x can be less than about 0.95, such as 0.94 and 0.96. In some embodiments, x can be less than about 0.97, such as 0.96 and 0.98. In some embodiments, x can be less than about 0.99, such as 0.98.
[0101] For example, x can be from about 0 to about 1. For example, x can be from about 0.05 to about 0.95 For example, x can be from about 0.1 to about 0.9. For example, x can be from about 0.15 to about 0.85. For example, x can be from about 0.2 to about 0.8. For example, x can be from about 0.25 to about 0.75. For example, x can be from about 0.3 to about 0.7. For example, x can be from about 0.35 to about 0.65. For example, x can be from about 0.4 to about 0.6. For example, x can be from about 0.45 to about 0.55.
[0102] For example, x can be from about 0 to about 1. For example, x can be from about 0.05 to about 1. For example, x can be from about 0.1 to about 1. For example, x can be from about 0.15 to about 1. For example, x can be from about 0.2 to about 1. For example, x can be from about 0.25 to about 1. For example, x can be from about 0 to about 1. For example, x can be from about 0.3 to about 1. For example, x can be from about 0.35 to about 1. For example, x can be from about 0.4 to about 1. For example, x can be from about 0.45 to about 1. For example, x can be from about 0.5 to about 1. For example, x can be from about 0.55 to about 1. For example, x can be from about 0.6 to about 1. For example, x can be from about 0.65 to about 1. For example, x can be from about 0.7 to about 1. For example, x can be from about 0.75 to about 1. For example, x can be from about 0.8 to about 1. For example, x can be from about 0.85 to about 1. For example, x can be from about 0.9 to about 1. For example, x can be from about 0.95 to about 1.
[0103] For example, x can be from about 0 to about 0.95. For example, x can be from about 0 to about 0.9. For example, x can be from about 0 to about 0.85. For example, x can be from about 0 to about 0.8. For example, x can be from about 0 to about 0.75. For example, x can be from about 0 to about 0.7. For example, x can be from about 0 to about 0.65. For example, x can be from about 0 to about 0.6. For example, x can be from about 0 to about 0.55. For example, x can be from about 0 to about 0.5. For example, x can be from about 0 to about 0.45. For example, x can be from about 0 to about 0.4. For example, x can be from about 0 to about 0.35. For example, x can be from about 0 to about 0.3. For example, x can be from about 0 to about 0.25. For example, x can be from about 0 to about 0.2. For example, x can be from about 0 to about 0.15. For example, x can be from about 0 to about 0.2. For example, x can be from about 0 to about 0.15. For example, x can be from about 0 to about 0.2. For example, x can be from about 0 to about 0.1. For example, x can be from about 0 to about 0.05. For example, x can be from about 0 to about 0.05.
[0104] For example, x can be from about 0 to about 0.5. For example, x can be from about 0.1 to about 0.6. For example, x can be from about 0.2 to about 0.7. For example, x can be from about 0.3 to about 0.8. For example, x can be from about 0.4 to about 0.9. For example, x can be from about 0.5 to about 1. For example, x can be from about 0 to about 0.3. For example, x can be from about 0.1 to about0.4. For example, x can be from about 0.2 to about 0.5. For example, x can be from about 0.3 to about0.6. For example, x can be from about 0.4 to about 0.7. For example, x can be from about 0.5 to about0.8. For example, x can be from about 0.6 to about 0.9. For example, x can be from about 0.7 to about1. For example, x may be from about 0 to about 0.9. For example, x may be from about 0 to about 0.8. For example, x may be from about 0 to about 0.7. For example, x may be from about 0.1 to about 0.5. For example, x may be from about 0.2 to about 0.4. For example, x may be from about 0.2 to about 0.3. For example, x may be about 0.25. For example, x may be about 0.05. For example, x may be about 0.1. For example, x may be about 0.15. For example, x may be about 0.2. For example, x may be about0.25. For example, x may be about 0.3. For example, x may be about 0.35. For example, x may be about 0.4. For example, x may be about 0.45. For example, x may be about 0.5. For example, x may be about 0.55. For example, x may be about 0.6. For example, x may be about 0.65. For example, x may be about 0.7. For example, x may be about 0.75. For example, x may be about 0.8. For example, x may be about 0.85. For example, x may be about 0.9. For example, x may be about 0.95. For example, x may be about 1.
[0105] The present disclosure relates to a solid electrolyte that has good properties such as high conductivity, is thermally stable, is stable with the cathode, and has high Coulombic efficiency in a sodium battery application. It will be readily appreciated that these and other objects and advantages of the present disclosure may be realized by means or methods described in the appended claims and a combination thereof.
[0106] Hereinafter, the compound, composition, composite material, electrode, battery, and technical effects of the present disclosure will be described in detail.
[0107] The present disclosure relates to a sodium containing material that provides an ionic transport pathway between the negative electrode and the positive electrode. This electrolyte has the formula NaAxMi.x0C14-x, where 0<x<l, A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, or Sn. For example, the combinations may include one or more element from Nb, Ta, Mo, V, Mn, or Sb. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, Sn, Nb, Ta, Mo, V, Mn, or Sb.
[0108] A first aspect of the present disclosure relates to a sodium electrolyte that provides an ionic transport pathway between the negative electrode and the positive electrode. This electrolyte has the formula NaAxMi.xOC14-x, where 0<x<l, A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, or Sn. For example, the combinations may include one or more element from Nb, Ta, Mo, V, Mn, or Sb. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, Sn, Nb, Ta, Mo, V, Mn, or Sb.
[0109] In some embodiments, the electrolyte may contain other materials, such as conductive carbon additives or binders in a composite with electrode materials.
[0110] A second aspect of the present disclosure relates to a sodium secondary battery in the first aspect wherein the electrolyte contains NaAxMi.xOC14-x, where 0<x<l, wherein A is an element with a4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, or Sn. For example, the combinations may include one or more element from Nb, Ta, Mo, V, Mn, or Sb. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, Sn, Nb, Ta, Mo, V, Mn, or Sb.[oni] A third aspect of the present disclosure relates to a sodium secondary battery in the second aspect wherein the electrolyte in contact with the anode, or anolyte, is another material, and the electrolyte in contact with the cathode, or catholyte, NaAxMi.xOC14-x, where 0<x<l, wherein A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, or Sn. For example, the combinations may include one or more element from Nb, Ta, Mo, V, Mn, or Sb. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, Sn, Nb, Ta, Mo, V, Mn, or Sb.
[0112] The anolyte and catholyte may also contain other materials such as conductive carbon additives or binders in a composite with the respective anode and cathode materials.
[0113] A fourth aspect of the present disclosure relates to the sodium secondary battery in any of the second to third aspects wherein the negative electrode comprises an anode material that is metallic, elemental, an alloy, carbon-based, or a transition metal oxide-based host.
[0114] A fifth aspect of the present disclosure relates to the sodium secondary battery in any one of the second to fourth aspects wherein the negative electrode material layer further comprises at least one of a binder resin, a conductive carbon additive material, or another anolyte.
[0115] A sixth aspect of the present disclosure relates to the sodium secondary battery in any one of the second to fifth aspects wherein the positive electrode comprises a positive electrode active material layer, the positive electrode active material layer comprises a sodium transition metal oxide, sodium transition metal polyanionic oxide or sodium ferrocyanide as a positive electrode active material, and the transition metal comprises at least one of Cr, Mn, Fe, Ni, or V.
[0116] A seventh aspect of the present disclosure relates to the sodium secondary battery in any one of the second to sixth aspects wherein the positive electrode active material layer further comprises at least one of a binder resin, a conductive material, and / or the solid electrolyte NaAxMi.x0C14-x, where 0<x<l, wherein A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, or Sn. For example,the combinations may include one or more element from Nb, Ta, Mo, V, Mn, or Sb. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, Sn, Nb, Ta, Mo, V, Mn, or Sb.
[0117] An eighth aspect of the present disclosure relates to the sodium secondary battery in any one of the second to seventh aspects wherein the positive electrode active material layer is obtained using the positive electrode active material, the conductive material, the binder resin, and the electrolyte NaAxMi.xOC x (where 0<x<l, A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof) by a manufacturing method according to a dry mixing process without a solvent. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, or Sn. For example, the combinations may include one or more element from Nb, Ta, Mo, V, Mn, or Sb. For example, the combinations may include one or more element from Zr, Ti, Si, Ge, Sn, Nb, Ta, Mo, V, Mn, or Sb.
[0118] A ninth aspect of the present disclosure relates to the sodium secondary battery in any one of the second to eighth aspects wherein the battery has a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0.1 to about 30.0.
[0119] For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 35.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 34.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 33.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 33.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 32.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 32.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 31.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 31.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 30.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 29.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 29.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 28.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 28.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 27.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 27.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 26.5. Forexample, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 26.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 25.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 25.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 24.5.
[0120] For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 20. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 5 to about 25. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 10 to about 30. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 15 to about 35. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 10. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 5 to about 15. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 10 to about 20. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 15 to about 25. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 20 to about 30. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 25 to about 35.Electrolytes and Related Compounds and Compositions
[0121] According to one aspect of the present disclosure, provided in certain embodiments herein are electrolytes comprising the compound or the composition disclosed herein.
[0122] The electrolyte according to the present disclosure may be in solid form and has a high conductivity and high stability, enabling its use in a sodium secondary battery. Its high conductivity leads to high rate capability in a solid state battery application, improving the performance of the battery.
[0123] Additionally, the electrolyte is thermally stable up to about 80°C, retaining its conductivity and electrochemical properties over a wide temperature range.
[0124] Additionally, the electrolyte is thermally stable up to about 50°C, retaining its conductivity and electrochemical properties over a wide temperature range. Additionally, the electrolyte is thermally stable up to 60°C, retaining its conductivity and electrochemical properties over a wide temperature range. Additionally, the electrolyte is thermally stable up to 70°C, retaining its conductivity and electrochemical properties over a wide temperature range. Additionally, the electrolyte is thermallystable up to 90°C, retaining its conductivity and electrochemical properties over a wide temperature range. Additionally, the electrolyte is thermally stable up to about 100°C, retaining its conductivity and electrochemical properties over a wide temperature range. Additionally, the electrolyte is thermally stable up to about 110°C, retaining its conductivity and electrochemical properties over a wide temperature range. Additionally, the electrolyte is thermally stable up to about 120°C, retaining its conductivity and electrochemical properties over a wide temperature range . Additionally, the electrolyte is thermally stable up to about 130°C, retaining its conductivity and electrochemical properties over a wide temperature range. Additionally, the electrolyte is thermally stable up to about 140°C, retaining its conductivity and electrochemical properties over a wide temperature range. Additionally, the electrolyte is thermally stable up to about 150°C, retaining its conductivity and electrochemical properties over a wide temperature range.
[0125] In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'11to about 101S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 1011to about 10'2S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-10to about 10'2S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'9to about 10'3S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'8to about 10'4S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'7to about 10'5S / cm.
[0126] In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'12to about 10'3S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'12to about 10'4S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 1011to about 10'6S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-10to about 10'5S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'9to about 10'4S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or acomposition comprised in the electrolyte may have an ionic conductivity of from about IO-8to about 10'3S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'7to about 10'2S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'6to about 10'1S / cm.
[0127] In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about 10'11to about IO-8S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO10to about IO-7S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-9to about IO-6S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-8to about IO-5S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-7to about IO-4S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-6to about IO-3S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-5to about IO-2S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-4to about 10'1S / cm.
[0128] In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO10to about IO-5S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-8to about IO-4S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-7to about IO-4S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-6to about IO-3S / cm. In some embodiments, the electrolyte, a compound comprised in the electrolyte, or a composition comprised in the electrolyte may have an ionic conductivity of from about IO-5to about IO-2S / cm.
[0129] Additionally, due to its stability on the cathode side, a cathode -electrolyte interphase (CEI) layer may not be substantially formed or may not be formed on the positive electrode interface, thereby preventing the loss of active material.
[0130] Additionally, the electrolyte is relatively easily synthesized via a one-step process, so it is more readily scalable than other electrolyte classes and reduces the complexity of both material synthesis and in turn, battery fabrication.
[0131] With these features, the electrolyte according to the present disclosure has good suitable properties toward sodium secondary batteries with high energy density, durability, and high Coulombic efficiency.
[0132] In some embodiments, the sodium electrolyte according to the present disclosure is a sodium electrolyte that has the formula NaAxMi.x0C14-x, where 0<x<l, wherein A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof. This electrolyte can transport Na+ions between the anode, or negative electrolyte, and the cathode, a positive electrolyte, in a sodium secondary battery.
[0133] When the sodium electrolytes are sulfide- (S) based or halide- (Cl, Br) based, these electrolytes are found to readily react, both chemically and electrochemically, with a variety of anode materials, resulting in electrolyte degradation, the formation of a solid-electrolyte interphase (SEI); such degradation is practically detrimental to the performance of a sodium secondary battery, especially if the SEI is relatively more electronically conductive, which leads to continuous SEI formation and continuous electrolyte degradation. However, Cl-based electrolytes have been shown to be stable with the cathode and no discernable degradation to a cathode -electrolyte interphase (CEI) occurs with the proper selection of cathodes. However, halide-based sodium-conducting electrolytes typically have lower ionic conductivities, namely I0'4S / cm or lower. The electrolyte according to the present disclosure, which has higher conductivity of a few times or more than an order of magnitude, drastically improves the rate capability and the performance of the battery.
[0134] Lithium oxychloride, LiMOCL, where M = Nb and Ta may be possible.
[0135] However, the sodium analogues according to this present disclosure (NaAxMi.x0C14-x, where 0<x<l, A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof) has not been used before in this application or setting, namely battery applications. In such batteries, a higher rate capability has been observed with this new electrolyte.
[0136] Hereinafter, the configuration and effect of the present disclosure will be described in detail.
[0137] In the present disclosure, the electrolyte has the formula NaAxMi.x0C14-x, where 0<x<l, A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof. For example, the combinations may include one or more elements from Zr, Ti, Si, Ge, or Sn. For example, the combinations may include one or more elements from Nb, Ta, Mo, V, Mn, or Sb. For example, the combinations may include one or more elements from Zr, Ti, Si, Ge, Sn, Nb, Ta, Mo, V, Mn, or Sb. All of the compounds in this range demonstrated similar properties, notably high ionic conductivity and cathode stability.
[0138] In some embodiments of the present disclosure, NaAxMi.xOC14-x(where 0<x<l, A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof) is used as the catholyte, or the electrolyte that is in direct contact with the cathode material, in a sodium secondary battery. It may be used in a composite with the cathode material. The electrolyte in contact with the anode, or anolyte, is another material, and can be a closo-borate (but not limited to this class). The anolyte and catholyte may also contain other materials such as conductive carbon additives or binders in a composite with the respective electrode materials. The cathode, or the positive electrode active material layer comprises a sodium transition metal oxide or sodium ferrocyanide as a positive electrode active material, and the transition metal comprises at least one of Cr, Mn, Fe, Ni, or V, and it too can further comprise at least one of a binder resin, a conductive material, or the solid electrolyte NaAxMi.x0C14.x(where 0<x<l, A is an element with a 4+ oxidation state such as Zr, Ti, Si, Ge, or Sn, and M is an element with a 5+ oxidation state such as Nb, Ta, Mo, V, Mn, or Sb, or combinations thereof). The negative electrode capacity to positive electrode capacity (N / P) ratio can be a range discussed in the present disclosure and can be, for example, from 0. 1 to 30.0.
[0139] In some embodiments of the present disclosure, the structural and electrochemical property of the electrolyte during operation should be retained and uncontaminated.
[0140] In some embodiments of the present disclosure, the electrolyte may be manufactured, for example, by the following method.
[0141] In some embodiments of the present disclosure, the electrolyte may be obtained by mixing powders of NaOH and / or ACI4 (where A = Zr, Ti, Si, Ge, or Sn) and / or MCI5 (where M = Nb, Ta, Mo, V, Mn, or Sb,) or combinations thereof, in the desired molar ratio followed by transferring to a ball miller and grinded by milling media to induce the reaction to form NaAxMi.x0C14-x. Once the millingis complete NaAxMi.x0C14-xpowder can be extracted and used in a solid-state sodium secondary battery.
[0142] In some electrolyte embodiments, the electrolyte further may comprise a negative electrode material. In some electrolyte embodiments, the negative electrode material may be a metal anode material, a metal elemental anode material, a nonmetal elemental anode material, an alloy material, or a transition metal oxide material. In some electrolyte embodiments, the negative electrode material may be a Na-Sn alloy. In some electrolyte embodiments, the negative electrode material may be a Na-Sn (2: 1) alloy.
[0143] In some electrolyte embodiments, the electrolyte may further comprise a conductive material. In some electrolyte embodiments, the conductive material may be selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powder, conductive whiskers, conductive metal oxide, activated carbon, polyphenylene derivatives, and combinations thereof. In some electrolyte embodiments, the conductive material may be selected from the group consisting of natural graphite, artificial graphite, Super-P, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, Denka black, vapor grown carbon fibers, and combinations thereof.
[0144] In some electrolyte embodiments, the electrolyte may further comprise a binder resin. In some electrolyte embodiments, the binder resin may be selected from the group consisting of polytetrafluoroethylene, polyvinylidene difluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, poly butylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan and carboxyl methyl cellulose, polyacrylic acid, polyacrylic acid salt derivatives, and combinations thereof.Battery
[0145] The present disclosure relates to a battery comprising the electrolyte related to the present disclosure, a negative electrode material, and a positive electrode material.
[0146] According to one aspect of the present disclosure, provided in certain embodiments herein are batteries that may comprise: a) a negative electrode, b) a positive electrode, c) the electrolyte disclosed herein and / or d) one or more other electrolyte different from the electrolyte disclosed herein.
[0147] In some embodiments, the battery may further comprise a catholyte.
[0148] In some embodiments, the battery may further comprise an anolyte.
[0149] In some embodiments, the electrolyte may be in contact with the positive electrode material, a catholyte, or a combination thereof.
[0150] In some embodiments, the electrolyte may be a catholyte.
[0151] In some embodiments, the battery further may comprise an anolyte-side electrolyte different from the electrolyte and in contact with the negative electrode material or an anolyte, or a combination thereof.
[0152] In some battery embodiments, the positive electrode may comprise sodium transition metal oxide active material as a positive electrode active material, and preferably the transition metal comprises at least one of Cr, Mn, Fe, Ni, or V. In some battery embodiments, the positive electrode comprises NasX fPCh); (NVP). In some battery embodiments, the positive electrode comprises NaCrO? cathode (NCO).
[0153] In some battery embodiments, the negative electrode material may be a metal anode material, a nonmetal elemental anode material, an alloy material, or a transition metal oxide material. In some battery embodiments, the negative electrode material may be a Na-Sn alloy. In some battery embodiments, the negative electrode material is a Na-Sn (2: 1) alloy.
[0154] In some battery embodiments, the negative electrode and / or the positive electrode may further comprise a conductive material. In some battery embodiments, the conductive material may be selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powder, conductive whiskers, conductive metal oxide, activated carbon, polyphenylene derivatives, and combinations thereof. In some battery embodiments, the conductive material may be selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, denka black, vapor grown carbon fiber, and combinations thereof.
[0155] In some battery embodiments, the negative electrode and / or the positive electrode may further comprise a binder resin. In some battery embodiments, the binder resin is selected from the group consisting of polytetrafluoroethylene, polyvinylidene difluoride, polyvinylidene fluoride-co- hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan and carboxyl methyl cellulose, polyacrylic acid, polyacrylic acid salt derivatives, and combinations thereof.
[0156] In some batery embodiments, the batery may further comprise a catholyte. In some batery embodiments, the catholyte comprises a reference closo-borate. In some batery embodiments, the catholyte comprises a reference halide. In some batery embodiments, the catholyte comprises the electrolyte in some embodiments.
[0157] In some embodiments, the batery may further comprise a catholyte. In some embodiments, the batery may further comprise an anolyte. In some embodiments, the electrolyte may be in contact with the positive electrode material, a catholyte, or a combination thereof.
[0158] In some embodiments, the electrolyte may be a catholyte.
[0159] In some embodiments, the batery further may comprise an anolyte-side electrolyte different from the electrolyte and in contact with the negative electrode material or an anolyte, or a combination thereof.
[0160] In some embodiments, the anolyte-side electrolyte may comprise a closo-borate.
[0161] In some embodiments, the negative electrode material may comprise a metal anode material, a metal elemental anode material, a nonmetal elemental anode material, an alloy material, a transition metal oxide material, a carbon-based material, or combinations thereof.
[0162] In some embodiments, the negative material may comprise a binder resin, a conductive carbon additive material, a solid electrolyte, or combinations thereof.
[0163] In some embodiments, the positive material may be included in a positive active material layer.
[0164] In some embodiments, the positive electrode material may comprise sodium transition metal oxide active material as a positive electrode active material, and preferably the transition metal may comprise at least one of Cr, Mn, Fe, Ni, or V.
[0165] In some embodiments, the positive electrode material may comprise sodium transition metal oxide, sodium transition metal polyanionic oxide, sodium ferrocyanide or combinations thereof as a positive electrode active material, and wherein the transition metal may comprise at least one of Cr, Mn, Fe, Ni, or V.
[0166] In some embodiments, the positive electrode material may comprise a NasX fPChh cathode (NVP). In some embodiments, the positive electrode material may comprise a NaCrO? cathode (NCO).
[0167] In some embodiments, the positive electrode material may comprise a binder resin, a conductive material, the electrolyte, or combinations thereof. In some embodiments, the positiveelectrode active material layer may be formed from a dry mixing without a solvent using the positive electrode active material, the conductive material and the binder resin.
[0168] In some embodiments, the battery may further comprise a conductive material.In some embodiments, the conductive material may be selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powder, conductive whiskers, conductive metal oxide, activated carbon, polyphenylene derivatives, and combinations thereof.
[0169] In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, more preferably at least 95%, more preferably at least 100% for the first 50 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, more preferably at least 95%, more preferably at least 100% for the first 45 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 40 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 35 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 30 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 25 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 20 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 15 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 10 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 5 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 3 cycles. In some embodiments, the battery may have a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first cycle.
[0170] In some embodiments, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of from about 0. 1 to about 30.0.
[0171] For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 35.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 34.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 33.5. For example, the battery may have a negative electrode capacity to positive electrode capacity(N / P) ratio of about 0 to about 33.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 32.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 32.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 31.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 31.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 30.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 29.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 29.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 28.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 28.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 27.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 27.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 26.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 26.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 25.5. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 25.0. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 24.5.
[0172] For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 20. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 5 to about 25. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 10 to about 30. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 15 to about 35. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 0 to about 10. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 5 to about 15. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 10 to about 20. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 15 to about 25. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 20 to about 30. For example, the battery may have a negative electrode capacity to positive electrode capacity (N / P) ratio of about 25 to about 35 ANON-LIMITING EMBODIMENTS
[0173] The present disclosure is also described and demonstrated by way of the following nonlimiting embodiments. However, the use of these and other embodiments anywhere in the specification is illustrative only and in no way limits the scope and meaning of the disclosure or of any exemplified term. Likewise, the disclosure is not limited to any particular preferred embodiment or aspect described herein. Indeed, suitable modifications and variations may be apparent to those skilled in the art upon reading this specification, and such variations can be made without departing from the disclosure in spirit or in scope.1. A compound having a chemical formula ofNaAxMi.xOC14-x, where 0<x<l, wherein A is an element with a 4+ oxidation state, wherein M is an element with a 5+ oxidation state.2. The compound of Embodiment 1, wherein 0<x<l.3. The compound of Embodiment 1, wherein the compound has a chemical formula of NaAOCL, where x = 1.4. The compound of Embodiment 1, wherein the compound has a chemical formula of NaMOCL, where x = 0.5. The compound of Embodiment 1 or Embodiment 2, wherein x is from about 0 to about 0.9.6. The compound of Embodiment 1 or Embodiment 2, wherein x is from about 0 to about 0.8.7. The compound of Embodiment 1 or Embodiment 2, wherein x is from about 0 to about 0.7.8. The compound of Embodiment 1 or Embodiment 2, wherein x is from about 0. 1 to about 0.5.9. The compound of Embodiment 1 or Embodiment 2, wherein x is about 0.25.10. The compound of Embodiment 1-9, wherein the element with the 4+ oxidation state comprises Zr, Ti, Si, Ge, or Sn.11. The compound of Embodiment 1-10, wherein the element with the 5+ oxidation state comprises Nb, Ta, Mo, V, Mn, or Sb.12. The compound of Embodiment 1-11, wherein the compound is a conductor based on a sodium cation.13. The compound of Embodiment 1-12, wherein the compound is an electrolyte including a sodium cation.14. The compound of Embodiment 1-13, wherein the compound has an ionic conductivity of from about 1011to about 10'6S / cm.15. The compound of Embodiment 1-13, wherein the compound has an ionic conductivity of from about IO-10to about 10'5S / cm.16. The compound of Embodiment 1-13, wherein the compound has an ionic conductivity of from about 10'8to about 10'4S / cm.17. The compound of Embodiment 1-13, wherein the compound has an ionic conductivity of from about 10'7to about 10'4S / cm.18. The compound of Embodiment 1-13, wherein the compound has an ionic conductivity of from about 10'6to about 10'3S / cm.19. The compound of Embodiment 1-13, wherein the compound has an ionic conductivity of from about 10'5to about 10'2S / cm.20. The compound of Embodiment 1-19, wherein the compound is formed by a chemical reaction between a sodium-containing compound and a metal chloride, wherein the metal is the element with 4+ oxidation state, the element with 5+ oxidation state, or a combination thereof.21. A composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and an element with a 4+ oxidation state, wherein a molar ratio between the element with the 4+ oxidation state and the sodium cation is up to 1 or less.22. A composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and an element with a 5+ oxidation state, wherein a molar ratio between the element with the 5+ oxidation state and the sodium cation is up to 1 or less.23. A composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state wherein a molar ratio between the element with the 4+ oxidation and the sodium cation is up to 1 or less or a molar ratio between the element with the 5+ oxidation state and the sodium cation is up to 1 or less.24. The composition of Embodiment 21-23, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.25. A composition comprising sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.26. A composition consisting essentially of sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.27. A composition consisting of sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.28. The composition of Embodiment 25-27, wherein a molar ratio between the element with the 4+ oxidation state and the sodium cation is up to 1 or less.29. The composition of Embodiment 25-28, wherein a molar ratio between the element with the 5+ oxidation state and the sodium cation is up to 1 or less.30. The composition of Embodiment 23-29, wherein a molar ratio between the sodium cation and a molar combination of the element with the 4+ oxidation state and the element with the 5+ oxidation state is 1.31. The composition of Embodiment 23-30, wherein a molar ratio of the chloride to the element with a 4+ oxidation state to the element with a 5+ oxidation state is 4-x : x : 1-x, where 0<x<l.32. The composition of Embodiment 31, wherein 0<x<l.33. The composition of Embodiment 21 and 23-31, wherein the composition has a chemical formula of NaAOCE, wherein A is the element with a 4+ oxidation state.34. The composition of Embodiment 22-31, wherein the composition has a chemical formula of NaMOC , wherein M is the element with a 5+ oxidation state.35. The composition of Embodiment 31-32, wherein x is from about 0 to about 0.9.36. The composition of Embodiment 31-32, wherein x is from about 0 to about 0.8.37. The composition of Embodiment 31-32, wherein x is from about 0 to about 0.7.38. The composition of Embodiment 31-32, wherein x is from about 0.1 to about 0.5.39. The composition of Embodiment 31-32, wherein x is about 0.25.40. The composition of Embodiment 21 and 23-39, wherein the element with the 4+ oxidation state comprises Zr, Ti, Si, Ge, or Sn.41. The composition of Embodiment 22-39, wherein the element with the 5+ oxidation state comprises Nb, Ta, Mo, V, Mn, or Sb.42. The composition of Embodiment 21-41, wherein the composition is a conductor based on the sodium cation.43. The composition of Embodiment 21-42, wherein the composition is an electrolyte including the sodium cation.44. The composition of Embodiment 21-43, wherein the composition has an ionic conductivity of from about 1011to about 10'6S / cm.45. The composition of Embodiment 21-43, wherein the composition has an ionic conductivity of from about IO-10to about 10'5S / cm.46. The composition of Embodiment 21-43, wherein the composition has an ionic conductivity of from about 10'8to about 10'4S / cm.47. The composition of Embodiment 21-43, wherein the composition has an ionic conductivity of from about 10'7to about 10'4S / cm.48. The composition of Embodiment 21-43, wherein the composition has an ionic conductivity of from about 10'6to about 10'3S / cm.49. The composition of Embodiment 21-43, wherein the composition has an ionic conductivity of from about 10'5to about 10'2S / cm.50. The composition of Embodiment 21-49, wherein the composition is formed by a chemical reaction between a sodium containing compound and a metal chloride, wherein the metal is the element with 4+ oxidation state, the element with 5+ oxidation state, or a combination thereof.51. A composition formed by a chemical reaction between a sodium containing compound and a metal chloride, wherein the metal is an element with a 4+ oxidation state, a 5+ oxidation state, or a combination thereof.52. The composition of Embodiment 51, wherein the composition comprises sodium cation (Na+), oxygen (O), chloride (Cl), and the element with a 4+ oxidation state, wherein a molar ratio between the element with the 4+ oxidation state and the sodium cation is up to 1 or less.53. The composition of Embodiment 51, wherein the composition comprises sodium cation (Na+), oxygen (O), chloride (Cl), and the element with a 5+ oxidation state, wherein a molar ratio between the element with the 5+ oxidation state and the sodium cation is up to 1 or less.54. The composition of Embodiment 51, wherein the composition comprises sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from the element with a 4+ oxidation state and the element with a 5+ oxidation state wherein a molar ratio between the element with the 4+ oxidation and the sodium cation is up to 1 or less or a molar ratio between the element with the 5+ oxidation state and the sodium cation is up to 1 or less.55. The composition of Embodiment 51-54, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.56. The composition of Embodiment 51, wherein the composition comprises sodium cation (Na+), oxygen (O), chloride (Cl) and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.57. The composition of Embodiment 51, wherein the composition consists essentially of sodium cation (Na+), oxygen (O), chloride (Cl), and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.58. The composition of Embodiment 51, wherein the composition consists of sodium cation (Na+), oxygen (O), chloride (Cl), and at least one element selected from an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.59. The composition of Embodiment 56-58, wherein a molar ratio between the element with the 4+ oxidation state and the sodium cation is up to 1 or less.60. The composition of Embodiment 56-59, wherein a molar ratio between the element with the 5+ oxidation state and the sodium cation is up to 1 or less.61. The composition of Embodiment 56-60, wherein a molar ratio between the sodium cation and a molar combination of the element with the 4+ oxidation state and the element with the 5+ oxidation state is 1.62. The composition of Embodiment 56-61, wherein a molar ratio of the chloride to the element with a 4+ oxidation state to the element with a 5+ oxidation state is 4-x : x : 1-x, where 0<x<l.63. The composition of Embodiment 62, wherein 0<x<l.64. The composition of Embodiment 51-63, wherein the compound has a chemical formula of NaAOCh, wherein A is the element with a 4+ oxidation state.65. The composition of Embodiment 51-64, wherein the compound has a chemical formula of NaMOCU, wherein M is the element with a 5+ oxidation state.66. The composition of Embodiment 62-63, wherein x is from about 0 to about 0.9.67. The composition of Embodiment 62-63, wherein x is from about 0 to about 0.8.68. The composition of Embodiment 62-63, wherein x is from about 0 to about 0.7.69. The composition of Embodiment 62-63, wherein x is from about 0.1 to about 0.5.70. The composition of Embodiment 62-63, wherein x is about 0.25.71. The composition of Embodiment 62-63, wherein x is about 0.72. The composition of Embodiment 51-71, wherein the element with the 4+ oxidation state comprises Zr, Ti, Si, Ge, or Sn.73. The composition of Embodiment 51-72, wherein the element with the 5+ oxidation state comprises Nb, Ta, Mo, V, Mn, or Sb.74. The composition of Embodiment 51-73, wherein the composition is a conductor based on sodium cation.75. The composition of Embodiment 51-74, wherein the composition is an electrolyte including sodium cation.76. The composition of Embodiment 51-75, wherein the composition has an ionic conductivity of from about 1011to about 10'6S / cm.77. The composition of Embodiment 51-75, wherein the composition has an ionic conductivity of from about IO-10to about 10'5S / cm.78. The composition of Embodiment 51-75, wherein the composition has an ionic conductivity of from about 10'8to about 10'4S / cm.79. The composition of Embodiment 51-75, wherein the composition has an ionic conductivity of from about 10'7to about 10'4S / cm.80. The composition of Embodiment 51-75, wherein the composition has an ionic conductivity of from about 10'6to about 10'3S / cm.81. The composition of Embodiment 51-75, wherein the composition has an ionic conductivity of from about 10'5to about 10'2S / cm.82. The composition of Embodiment 51-81, wherein the sodium containing compound is sodium hydroxide (NaOH), sodium chloride (NaCl), sodium oxide (Na2O), or combinations thereof.83. The composition of Embodiment 82, wherein the sodium hydroxide (NaOH) is in solid form, powder form or pellet form.84. A composition comprising sodium cation (Na+), oxygen (O), chloride (Cl), and at least one of an element with a 4+ oxidation state and an element with a 5+ oxidation state, wherein the composition has an ionic conductivity of from about 1011to about 10'6S / cm.85. The composition of Embodiment 84, wherein the composition has an ionic conductivity of from about IO-10to about 10'5S / cm.86. The composition of Embodiment 84, wherein the composition has an ionic conductivity of from about 10'8to about 10'4S / cm.87. The composition of Embodiment 84, wherein the composition has an ionic conductivity of from about 10'7to about 10'4S / cm.88. The composition of Embodiment 84, wherein the composition has an ionic conductivity of from about 10'6to about 10'3S / cm.89. The composition of Embodiment 84, wherein the composition has an ionic conductivity of from about 10'5to about 10'2S / cm.90. The composition of Embodiment 84, wherein a molar ratio between the chloride and the sodium cation is from about 3 to about 4.91. The composition of Embodiment 90, wherein a molar ratio between the element with the 4+ oxidation state and the sodium cation is up to 1 or less.92. The composition of Embodiment 90, wherein a molar ratio between the element with the 5+ oxidation state and the sodium cation is up to 1 or less.93. A electrolyte comprising the compound of Embodiment 1-20 or the composition of Embodiment 21-92.94. The electrolyte of Embodiment 93, further comprising a conductive material.95. The electrolyte of Embodiment 94, wherein the conductive material is selected from the group consisting of natural graphite, artificial graphite, Super-P, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, Denka black, vapor grown carbon fibers, carbon nanotubes and combinations thereof.96. The electrolyte of Embodiment 93-95, further comprising a binder resin.97. The electrolyte of Embodiment 96, wherein the binder resin is selected from the group consisting of polytetrafluoroethylene, polyvinylidene difluoride, polyvinylidene fluoride-co- hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan and carboxyl methyl cellulose, polyacrylic acid, polyacrylic acid salt derivatives, and combinations thereof.98. A battery comprising the electrolyte of Embodiment 93-97, a negative electrode material, and a positive electrode material.99. The battery of Embodiment 98, further comprising a catholyte.100. The battery of Embodiment 98-99, further comprising an anolyte.101. The batery of Embodiment 98-100, wherein the electrolyte is in contact with the positive electrode material, a catholyte, or a combination thereof.102. The batery of Embodiment 98-100, wherein the electrolyte is a catholyte.103. The batery of Embodiment 98-102, wherein the batery further comprises an anolyteside electrolyte different from the electrolyte and in contact with the negative electrode material or an anolyte, or a combination thereof.104. The batery of embodiment 103, wherein the anolyte-side electrolyte comprises a closo- borate.105. The batery of Embodiment 98-104, wherein the negative electrode material comprises a metal anode material, a metal elemental anode material, a nonmetal elemental anode material, an alloy material, a transition metal oxide material, a carbon-based material, or combinations thereof106. The batery of Embodiment 98-105, wherein the negative material comprises a binder resin, a conductive carbon additive material, a solid electrolyte, or combinations thereof.107. The batery of Embodiment 98-106, wherein the positive material is included in a positive active material layer.108. The batery of Embodiment 98-107, wherein the positive electrode material comprises sodium transition metal oxide active material as a positive electrode active material, and preferably the transition metal comprises at least one of Cr, Mn, Fe, Ni, or V.109. The batery of Embodiment 98-107, wherein the positive electrode material comprises sodium transition metal oxide, sodium transition metal polyanionic oxide, sodium ferrocyanide or combinations thereof as a positive electrode active material, and wherein the transition metal comprises at least one of Cr, Mn, Fe, Ni, or V.110. The batery of Embodiment 98-109, wherein the positive electrode material comprises a Na3V2(PO4)3 cathode (NVP).111. The batery of Embodiment 98-108, wherein the positive electrode material comprises a NaCrCE cathode (NCO).112. The batery of Embodiment 98-111, wherein the positive electrode material comprises a binder resin, a conductive material, the electrolyte, or combinations thereof.113. The batery of Embodiment 107-112, wherein the positive electrode active material layer is formed from a dry mixing without a solvent using the positive electrode active material, the conductive material and the binder resin.114. The batery of Embodiment 98-111, further comprising a conductive material.115. The batery of Embodiment 114, wherein the conductive material is selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powder, conductive whiskers, conductive metal oxide, activated carbon, polyphenylene derivatives, and combinations thereof.116. The batery of Embodiment 98-115, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, more preferably at least 95%, more preferably at least 100% for the first 50 cycles.117. The batery of Embodiment 98-115, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 40 cycles.118. The batery of Embodiment 98-115, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 30 cycles.119. The batery of Embodiment 98-115, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 20 cycles.120. The batery of Embodiment 98-115, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 10 cycles.121. The batery of Embodiment 98-115, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 5 cycles.122. The batery of Embodiment 98-115, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 3 cycles.123. The batery of Embodiment 98-115, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first cycle.124. The batery of Embodiment 98-123, wherein the batery has a negative electrode capacity to positive electrode capacity (N / P) ratio of from about 0.1 to about 30.0.NON-LIMITING EXAMPLES
[0174] The present disclosure is also described and demonstrated by way of the following nonlimiting examples. However, the use of these and other examples anywhere in the specification is illustrative only and in no way limits the scope and meaning of the disclosure or of any exemplified term. Likewise, the disclosure is not limited to any particular embodiment or aspect described herein. Indeed, suitable modifications and variations may be apparent to those skilled in the art upon reading this specification, and such variations can be made without departing from the disclosure in spirit or in scope.Example 1 - Crystallinitv / Amorphousness
[0175] To demonstrate the crystallinity / amorphousness of the disclosed electrolyte compound and composition, various precursor compounds and electrolyte compounds were analyzed using X-ray powder diffraction (XRD).
[0176] FIG. 1 shows an X-ray diffraction pattern of the electrolytes NaNbOCL, in some embodiments. This shows that processing the precursors yields a new compound. Referring to Fig. 1, This compound has a very low degree of crystallinity, or is amorphous.
[0177] FIG. 2 shows an X-ray diffraction pattern of the electrolytes NaTaOCL, in some embodiments. This shows that processing the precursors yields a new compound. This compound has a very low degree of crystallinity, or is amorphous.
[0178] FIG. 13 shows the X-ray diffraction pattern of NaNbOCL after annealing, or heat treatment, at 300°C (over 24 hours), under an argon atmosphere, in some embodiments. The material has undergone crystallization and is no longer amorphous.
[0179] FIG. 14 shows the X-ray diffraction pattern of NaTaOCL after annealing, or heat treatment, at 300°C (over 24 hours), under an argon atmosphere, in some embodiments. The material has undergone crystallization and is no longer amorphous.Example 2 -Conductivity
[0180] To demonstrate the conductivity of the disclosed electrolyte compound and composition, various example electrolyte compounds / compositions were evaluated.
[0181] FIG. 3 shows the ionic conductivity of the electrolytes NaMOCL, where M = Nb, Ta, in some embodiments. These electrolytes exhibit a conductivity higher than that of the previously-reportedchlorine-based sodium ion conductors. The conductivity values are suitable for use in sodium secondary batteries.
[0182] FIG. 4 are Arrhenius plots of the conductivities of the electrolytes NaNbOC’L and NaTaOCL (electrolytes NaMOC’L. where M = Nb, Ta), in some embodiments. The conductivity exhibits Arrhenius behavior as the temperature increases to 80°C, and upon cooling back down to ambient conditions or 20°C, the ionic conductivity values of the compounds are still maintained. This shows that NaNbOC’L. and NaTaOCL are thermally stable over a typical temperature range for battery operation.
[0183] FIG. 5 shows the ionic conductivity of the electrolytes NaZro.25Tao.75OQ3.75 and NaZrOCL. where Zr (which has an oxidation state of 4+) has substituted for Ta (which has an oxidation state of 5+); the formulas NaZro 25Tao75OQ375 and NaZrOCT correspond to 25% and 100% substitution (Zr for Ta), respectively, in some embodiments. This demonstrates another kind of elemental substitution, and Na ionic conductivity is exhibited for NaZro 25Tao 750C1375 and NaZrOCT; their conductivity values are suitable for use in sodium secondary batteries.
[0184] FIG. 6 shows the electronic conductivity of the electrolyte NaNbOC’L. in some embodiments. The low electronic conductivity (IO-9S / cm range) means that this material is primarily an ionic conductor, and thus a sodium ion conductor, suitable for use in secondary batteries.
[0185] FIG. 7 shows the electronic conductivity of the electrolyte NaTaOCL, in some embodiments. The low electronic conductivity (IO-9S / cm range) means that this material is primarily an ionic conductor, and thus a sodium ion conductor, suitable for use in secondary batteries.
[0186] FIG. 8 shows the linear sweep voltammetry (LSV) scan (from open circuit voltage, OCV, to 5V, and from OCV to 0V) of NaNbOC’L. in some embodiments. The cell configuration is Na-Sn 2: 1, a reference closo-borate, NaNbOC’L. and NaNbOC’L: acetylene black in a (70:30 ratio). The stability window of NaNbOCT is determined to be -3.0-4. IV vs Na / Na+.
[0187] FIG. 9 shows the linear sweep voltammetry (LSV) scan (from OCV to 5V, and from OCV to 0V) of NaTaOCL, in some embodiments. The cell configuration is Na-Sn 2: 1, a reference closo- borate, NaTaOCL, and NaTaOCL: acetylene black in a (70:30 ratio). The stability window ofNaTaOCL is determined to be ~2.6-4.4V vs Na / Na+.
[0188] FIG. 15 shows the ionic conductivity of NaNbOCL after annealing or heat treatment to 300°C over 24 hours, in some embodiments. A significant drop (3x) in the ionic conductivity is observed along with the transition from amorphous to crystalline.
[0189] FIG. 16 shows the ionic conductivity of and NaTaOC after annealing or heat treatment to 300°C over 24 hours, in some embodiments. A significant drop (3 Ox) in the ionic conductivity is observed along with the transition from amorphous to crystalline, in some embodiments.Example 3 - Rate Performance
[0190] To demonstrate the rate performance of the disclosed battery, an example battery using the disclosed compound / composition was evaluated against a reference battery using a known, electrolyte compound / composition .
[0191] FIG. 10 shows the room temperature rate performance comparison between the electrolyte NaTaOCk and a reference halide. These are incorporated in a sodium secondary battery comprising of Na-Sn 2: 1 alloy as the anode, a reference closo-borate electrolyte as the electrolyte, the catholyte, and a Nas ¥2(004)3 cathode (NVP), in some embodiments. One battery has a reference halide electrolyte as the catholyte, and another has NaTaOCk as the catholyte, in some embodiments. The battery containing NaTaOCk has superior utilization and rate performance.
[0192] FIG. 11 shows the voltage profdes from cycling of a sodium secondary battery, comprising of Na-Sn 2: 1 alloy as the anode, a reference closo-borate as the electrolyte, NaTaOCk as the catholyte, and an NVP cathode, in some embodiments. The first 50 cycles are shown, and this demonstrates that NaTaOC is suitable as a catholyte in a sodium secondary battery.Example 4 - Cycling Performance
[0193] To demonstrate the cycling performance of the disclosed battery, an example battery was evaluated.
[0194] FIG. 12 shows the capacity retention from cycling of a sodium secondary battery, the same as shown in FIG. 11, which comprises of Na-Sn 2: 1 alloy as the anode, a reference closo-borate as the electrolyte, NaTaOC as the catholyte, and a NaCrO2 cathode (NCO), in some embodiments. The first 50 cycles are shown (both the voltage vs. specific capacity, and specific capacity vs. cycle number). The first 50 cycles are shown, and this demonstrates that NaTaOC is suitable as a catholyte in a sodium secondary battery.
Claims
ClaimsWhat is claimed is:
1. A compound having a chemical formula ofNaAxMi.xOC14-x, where 0<x<l, wherein A is an element with a 4+ oxidation state, wherein M is an element with a 5+ oxidation state.
2. The compound of Claim 1, wherein 0<x<l.
3. The compound of Claim 1, wherein the compound has a chemical formula of NaAOCT. where x = 1.
4. The compound of Claim 1, wherein the compound has a chemical formula of NaMOC’h. where x = 0.
5. The compound of Claim 1 or Claim 2, wherein x is from about 0 to about 0.9.
6. The compound of Claim 1 or Claim 2, wherein x is from about 0 to about 0.8.
7. The compound of Claim 1 or Claim 2, wherein x is from about 0 to about 0.7.
8. The compound of Claim 1 or Claim 2, wherein x is from about 0. 1 to about 0.5.
9. The compound of Claim 1 or Claim 2, wherein x is about 0.25.
10. The compound of Claim 1-9, wherein the element with the 4+ oxidation state comprises Zr, Ti, Si, Ge, or Sn.
11. The compound of Claim 1-10, wherein the element with the 5+ oxidation state comprises Nb, Ta, Mo, V, Mn, or Sb.
12. The compound of Claim 1, wherein the compound is a conductor based on a sodium cation.
13. The compound of Claim 1, wherein the compound is an electrolyte including a sodium cation.
14. The compound of Claim 1, wherein the compound has an ionic conductivity of from about 1011to about 10'6S / cm.
15. The compound of Claim 1, wherein the compound has an ionic conductivity of from about 10'10to about 10'5S / cm.
16. The compound of Claim 1, wherein the compound has an ionic conductivity of from about 10'8to about 10'4S / cm.
17. The compound of Claim 1, wherein the compound has an ionic conductivity of from about 10'7to about 10'4S / cm.
18. The compound of Claim 1, wherein the compound has an ionic conductivity of from about 10'6to about 10'3S / cm.
19. The compound of Claim 1, wherein the compound has an ionic conductivity of from about 10'5to about 10'2S / cm.
20. The compound of Claim 1, wherein the compound is formed by a chemical reaction between a sodium-containing compound and a metal chloride, wherein the metal is the element with 4+ oxidation state, the element with 5+ oxidation state, or a combination thereof.
21. A electrolyte comprising the compound of Claim 1.
22. The electrolyte of Claim 21, further comprising a conductive material selected from the group consisting of natural graphite, artificial graphite, Super-P, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, Denka black, vapor grown carbon fibers, carbon nanotubes and combinations thereof.
23. The electrolyte of Claim 22, further comprising a binder resin selected from the group consisting of polytetrafluoroethylene, polyvinylidene difluoride, polyvinylidene fluoride-co- hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan and carboxyl methyl cellulose, polyacrylic acid, polyacrylic acid salt derivatives, and combinations thereof.
24. A battery comprising the electrolyte of Claim 21, a negative electrode material, and a positive electrode material.
25. The battery of Claim 24, further comprising a catholyte.
26. The battery of Claim 24, further comprising an anolyte.
27. The battery of Claim 24, wherein the battery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 50 cycles.
28. The batery of Claim 24, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first 10 cycles.
29. The batery of Claim 24, wherein the batery has a Coulombic efficiency of at least 60%, preferably at least 90%, and more preferably at least 95% for the first cycle.
30. The batery of Claim 24, wherein the batery has a negative electrode capacity to positive electrode capacity (N / P) ratio of from about 0. 1 to about 30.0.
Citation Information
Patent Citations
Ionic conductor materials
CA1182860A
Solid electrolyte material and battery using the same
US20210242494A1