High-strength steel for reducer gears of new energy vehicles and manufacturing method therefor
Patent Information
- Application Number
- PCT/CN2023/115132
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2023-08-28
- Publication Date
- 2024-11-14
AI Technical Summary
New energy vehicle reducer gears bear large external forces during high-speed operation and require steel with high strength, structural uniformity and low hardness to extend fatigue life. However, it is difficult to ensure fine austenite grains and tensile strength with existing technology.
It adopts low-carbon designed chemical composition, adds appropriate amounts of nickel and molybdenum elements, and uses continuous casting high-temperature forced cooling process and three-stage isothermal heat treatment to form steel with fine austenite grains and high tensile strength, ensuring that the hardness of the steel is within Below 160HBW and no crack defects on the surface.
It achieves the high tensile strength and low hardness of steel, ensures the long life and efficient operation of high-strength reducer gears for new energy vehicles, and fills the domestic technology gap.
Smart Images

Figure CN2023115132_14112024_PF_FP_ABST
Abstract
Description
A new energy vehicle high-strength reducer gear steel and its manufacturing method Technical Field
[0001] The present invention belongs to the technical field of special steel smelting, and specifically relates to a high-strength steel for reducer gears of new energy vehicles and a manufacturing method thereof. Background Art
[0002] New energy vehicle reducer gears operate at very high speeds during transmission, with some high-quality gears exceeding 10,000 rpm. These high-speed operations continuously subject the gears to significant external forces. These reducer gears must possess high strength, excellent structural uniformity, and precise assembly to ensure a long fatigue life. The corresponding steel must possess excellent banded structure, low hardness, a crack-free surface for easy cold forging, fine austenite grains, and high strength.
[0003] Patent No. CN112981271A discloses a method for manufacturing steel for electric vehicle reducer gears. This method belongs to the field of iron-based alloy technology, and particularly relates to gear steel. The elemental composition design involves the following: C: 0.20-0.35%, Si: 0.05-0.35%, Mn: 1.20-1.60%, Cr: 1.10-1.50%, Mo: 0.20-0.50%, S: ≤0.035%, P: ≤0.015%, Cu: ≤0.20%, Ni: ≤0.20%, Al: 0.010-0.080%, N: 0.0060-0.0260%, Al / N ratio: 1.5-3.9, with the balance being Fe and unavoidable impurities. The smelting process includes: pre-treated molten iron and selected scrap steel → primary smelting in an electric furnace → refining in a LF furnace → vacuum degassing in a VD furnace → continuous casting of billets → shot blasting of billets → heating in a walking beam furnace → high-pressure water descaling → continuous casting of billets → surface and internal ultrasonic testing of hot-rolled round steel → quality inspection → storage. The combined elemental composition and smelting process meet the high strength and fatigue life requirements of electric vehicle reducer steel, while also achieving significant advantages in hardenability and grain uniformity.
[0004] Summary of the Invention
[0005] The technical problem to be solved by the present invention is to provide a high-strength steel for reducer gears of new energy vehicles and a manufacturing method thereof in response to the above-mentioned existing technology, so as to ensure that the steel has fine austenite grains and high tensile strength.
[0006] The technical solution adopted by the present invention to solve the above-mentioned problem is: a high-strength steel for reducer gears of new energy vehicles, wherein the chemical composition of the gear steel is as follows by weight: C: 0.13-0.18%, Si: ≤0.15%, Mn: 1.10-1.35%, Cr: 1.20-1.45%, P: ≤0.012%, S: ≤0.003%, Ni: 0.15-0.35%, Mo: 0.05-0.20%, Al: 0.015-0.050%, Nb: 0.015-0.050%, N: 0.0085-0.0225%, B: 0.0015-0.0035%, and the balance is Fe and unavoidable impurities.
[0007] The steel has a banded structure of ≤1.5, a hardness of ≤160 HBW, an austenite grain size of ≥8, no crack defects on the surface of the steel, and a tensile strength of ≥1180 MPa after 870°C oil quenching + 200°C tempering.
[0008] The main functions and design basis of each chemical element in the steel of the present invention are:
[0009] C: Carbon is the most important element affecting steel's strength. The higher the carbon content, the higher the steel's tensile strength and hardness. To ensure a low hardness, the present invention adopts a low-carbon design, with a carbon content range of 0.13-0.18%.
[0010] Si: The steel of the present invention is used for cold forging. To prevent cold work hardening during the cold forging process, the silicon content in the steel needs to be strictly controlled. The silicon content of the present invention is selected within the range of Si≤0.15%.
[0011] Mn: Manganese is a carbide-forming element that enters cementite to replace some iron atoms. Manganese lowers the critical transition temperature in steel, refines pearlite, and indirectly increases pearlite strength. The Mn content in the present invention is preferably in the range of 1.10 to 1.35%.
[0012] Cr: Chromium can increase the hardenability and strength of steel, but the hardness of the steel will also increase. The Cr content in the present invention is selected within the range of 1.20-1.45%.
[0013] P: This invention belongs to cold forging steel. Phosphorus can significantly reduce the tensile strength of steel, especially at low temperatures. The phosphorus content of this invention is selected within the range of P≤0.012%.
[0014] Sulfur (S) exists in the steel of this invention in the form of iron sulfide (FeS). FeS forms a low-melting-point (985°C) compound with Fe. Premature melting of the FeS compound during continuous casting, straightening, and rolling can cause surface cracking in the steel. The S content in this invention is preferably ≤ 0.003%.
[0015] Ni: Nickel can increase the tensile strength of steel. However, nickel is a precious metal. The Ni content in the present invention is selected within the range of 0.15-0.35%.
[0016] Mo: Molybdenum can effectively increase the tensile strength of steel. However, molybdenum is a precious metal. The Mo content of the present invention is selected within the range of 0.05-0.20%.
[0017] Al, N, Nb: Aluminum combines with oxygen in steel to deoxidize it. Aluminum combines with nitrogen to form AlN, which refines the steel's grain size. Niobium combines with nitrogen to form NbN, which also refines the steel's grain size. The Al content in the present invention is preferably within the range of 0.015-0.050%, the N content within the range of 0.0085-0.0225%, and the Nb content within the range of 0.015-0.050%.
[0018] Boron (B) is used in the present invention to increase the hardenability of steel and improve its tensile strength, thereby saving other more precious metals. The content of B in the present invention is preferably in the range of 0.0015-0.0035%.
[0019] The above-mentioned high-strength steel for reducer gears of new energy vehicles and its manufacturing method include the following process steps:
[0020] Molten steel, smelted using a primary refining-vacuum degassing process, is hoisted onto the continuous casting platform for casting. The continuous casting mold uses a forced cooling method to form a high-strength chill layer over 10mm thick on the surface of the ingot. This chill layer is composed of fine equiaxed crystal bands with different orientations. The high-strength fine equiaxed crystal bands ensure that the ingot will not develop surface cracks during the subsequent straightening process. To prevent excessive stress on the surface of the ingot during cooling, the ingot is delivered hot, with a temperature of ≥600°C.
[0021] The continuous casting billet with no surface crack defects and low stress is hot fed into the heating furnace and heated to 1180-1280℃. The heated continuous casting billet needs to undergo three stages of rolling deformation: rough rolling, intermediate rolling and finishing rolling. The temperature of the rolling deformation process in these three stages should be carried out at a relatively high plastic temperature. The method for determining the high plastic temperature is: the continuous casting billet is heated to different temperatures (the heating temperature range is 750-1100℃), and then the continuous casting billet is forged with the same force. The high plastic temperature is when the continuous casting billet can achieve large deformation after forging. The low stress on the rolled material surface ensures that the surface of the billet will not crack during the heating process; the rolling deformation at a high plastic temperature ensures that no crack defects will be generated on the material surface during the rolling process.
[0022] The rolled steel is sent to an isothermal furnace for isothermal heat treatment. The isothermal heat treatment is divided into three stages. The first stage is isothermal normalizing treatment. The purpose of this stage is to fully precipitate all the NbC and AlN particles that have not yet been completely precipitated in the rolled material in the shortest possible time. The method for determining the optimal normalizing holding temperature is to use a scanning electron microscope to observe the precipitation rate of NbC and AlN particles in the high-temperature rolled material at different temperatures in the range of 850-950℃. When the NbC and AlN particles have the highest precipitation rate, this temperature is the best. The steel is subjected to the optimal normalizing temperature. The second stage is rapid cooling, with a temperature drop rate of ≥10°C / s, to a temperature 20°C below the Ar1 temperature (705°C in this invention). This stage aims to reduce the precipitation of banded proeutectoid ferrite before the eutectoid transformation. The third stage is isothermal annealing, which aims to maintain the temperature 20°C below the Ar1 temperature for a period of time to allow the austenite structure to completely transform into fine and evenly distributed ferrite and pearlite, thereby reducing the banding of the steel. Finally, the steel is air-cooled to reduce its hardness to below 160 HBW.
[0023] This invention targets high-strength steel for gear reducers in new energy vehicles. Its composition is designed to be low-carbon, with appropriate amounts of nickel and molybdenum, and trace amounts of aluminum, nitrogen, and niobium. Subsequent heat treatment allows AlN and NbN to fully precipitate, ensuring the steel possesses fine austenite grains and high tensile strength. The continuous casting process utilizes a strong cooling process within the crystallizer, which forms a high-strength chill layer exceeding 10 mm on the surface of the ingot. The ingot is then hot-rolled to reduce surface stress. The ingot undergoes rough, intermediate, and finish rolling at high plastic temperatures, ensuring the steel is free of surface cracks. After rolling, the steel undergoes a three-stage isothermal heat treatment to: ① fully and efficiently precipitate NbC and AlN particles at the fastest rate; ② reduce the precipitation of banded proeutectoid ferrite before the eutectoid transformation; and ③ transform the austenite structure into fine and evenly distributed ferrite and pearlite, thereby reducing the steel's banding and lowering its hardness to below 160 HBW. The resulting high-strength steel for reducer gears in new energy vehicles is characterized by: banding ≤ 1.5, hardness ≤ 160 HBW, austenite grain size ≥ 8, no surface cracks, and a tensile strength ≥ 1180 MPa after oil quenching at 870°C and tempering at 200°C.
[0024] Compared with the prior art, the advantages of the present invention are:
[0025] The present invention is aimed at the steel used for high-strength reducer gears of new energy vehicles. It adopts a low-carbon design in terms of composition, adds appropriate amounts of nickel and molybdenum elements, and adds trace amounts of aluminum, nitrogen, and niobium elements. Through the subsequent heat treatment process, AlN and NbN are fully precipitated to ensure that the steel has fine austenite grains and high tensile strength. In the continuous casting process, a strong cooling process is immediately adopted after the high-temperature ingot is discharged from the crystallizer, so as to form a high-strength chill layer of more than 10mm on the surface of the ingot; the continuous casting ingot adopts a hot delivery process to reduce the stress on the surface of the ingot; the continuous casting ingot is subjected to rough rolling, intermediate rolling and finish rolling at a high plastic temperature to ensure that the surface of the produced steel is free of crack defects. After rolling, the steel is subjected to three stages of isothermal heat treatment. The functions of each stage are: ① NbC and AlN particles are fully precipitated at the fastest rate; ② a fine and evenly distributed ferrite structure is formed to reduce the ferrite banding structure; ③ the hardness of the steel is reduced to below 160HBW. Through reasonable steelmaking, rolling and isothermal heat treatment processes, a high-strength steel for reducer gears of new energy vehicles was successfully manufactured, filling the domestic gap. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] FIG1 is a longitudinal banded structure (×100) of Example 1 of the present invention, and the banded structure grade is 0.5.
[0027] FIG2 is a longitudinal banded structure (×100 times) of Example 2 of the present invention, and the banded structure grade is 0.5. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be described in more detail with reference to the preferred embodiments of the present invention. However, these embodiments are merely descriptions of preferred implementations of the present invention and do not limit the scope of the present invention in any way.
[0029] Example 1 and Example 2:
[0030] The two embodiments involve a method for manufacturing high-strength steel for reducer gears in new energy vehicles: primary refining in a 100-ton electric furnace → refining in a 100-ton refining furnace → vacuum degassing in a VD furnace → continuous casting of square billets (300mm x 340mm) → hot transport of the billets → heating of the billets → rough rolling → intermediate rolling → finishing rolling → isothermal heat treatment in an isothermal furnace. Two batches of high-strength steel for reducer gears in new energy vehicles were produced.
[0031] The molten steel smelted by the electric furnace-refining-vacuum degassing process is hoisted to the continuous casting platform for casting. After the billet comes out of the crystallizer, it is forced cooled. The thickness of the surface chill layer is 15 mm (Example 1) and 17 mm (Example 2); the hot delivery temperature of the continuous casting billet is 633°C (Example 1) and 626°C (Example 2).
[0032] The hot cast slab is sent to a heating furnace and heated to 1180-1280°C. The heated slab is then rolled into a Φ52 mm (Example 1) or Φ95 mm (Example 2) through three stages of rough rolling, intermediate rolling, and finishing rolling. The rough rolling temperature is 1050°C, the intermediate rolling temperature is 1000°C, and the finishing rolling temperature is 975°C.
[0033] The rolled steel was fed into an isothermal furnace for isothermal heat treatment. In the first stage, the steel was subjected to isothermal normalizing treatment, with an isothermal temperature of 925°C and an isothermal time of 52 min (Example 1) and 95 min (Example 2). In the second stage, the steel was cooled by strong wind with a temperature drop rate of 12°C / s (Example 1) and 11°C / s (Example 2), rapidly cooled to 685°C, kept warm for 208 min (Example 1) and 380 min (Example 2), and finally air-cooled after being taken out of the furnace.
[0034] The chemical compositions of the steels prepared in Examples 1 and 2 are shown in Table 1;
[0035] Table 1 (wt%)
[0036] The steels obtained in Examples 1 and 2 had no crack defects on their surfaces. The banded structure grade, hardness, and austenite grain size grade of the steels were specifically shown in Table 2.
[0037] Table 2
[0038] The steels prepared in Examples 1 and 2 were oil quenched at 870°C and tempered at 200°C. The tensile strength of the steels is shown in Table 3.
[0039] Table 3
[0040] Although the preferred embodiments of the present invention have been described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are intended to be included within the scope of protection of the present invention.
Claims
1. A high-strength steel for reducer gears of new energy vehicles, characterized in that The chemical composition of the steel is C: 0.13-0.18%, Si: ≤0.15%, Mn: 1.10-1.35%, Cr: 1.20-1.45%, P: ≤0.012%, S: ≤0.003%, Ni: 0.15-0.35%, Mo: 0.05-0.20%, Al: 0.015-0.050%, Nb: 0.015-0.050%, N: 0.0085-0.0225%, B: 0.0015-0.0035%, and the balance is Fe and unavoidable impurities.
2. The high-strength reducer gear steel for new energy vehicles according to claim 1 is characterized in that The banded structure of the gear steel is ≤ grade 1.5, the hardness of the steel is ≤160HBW, the austenite grain size of the steel is ≥grade 8, there is no crack defect on the surface of the steel, and the tensile strength of the steel after 870°C oil quenching + 200°C tempering is ≥1180MPa.
3. A method for manufacturing high-strength reducer gear steel for new energy vehicles as claimed in claim 1, characterized in that The main steps of the method are: 1) The molten steel smelted by the primary refining-refining-vacuum degassing process is hoisted to the continuous casting platform for casting; 2) The continuous casting billet with no surface crack defects and low stress is hot sent to the heating furnace and heated to 1180-1280℃. The heated continuous casting billet needs to undergo three stages of rolling deformation: rough rolling, intermediate rolling and finish rolling. 3) The rolled steel is sent to an isothermal furnace for isothermal heat treatment. The isothermal heat treatment is divided into three stages. The first stage is isothermal normalizing treatment. The purpose of this stage is to fully precipitate all NbC and AlN particles that have not yet been completely precipitated in the rolled material in the shortest time; the second stage is rapid cooling. The purpose of this stage is to reduce the precipitation of strip-shaped pro-eutectoid ferrite in the steel before the eutectoid phase transformation; the third stage is isothermal annealing treatment. The purpose of this stage is to keep the temperature below Ar1 temperature at 20°C for a period of time to allow the austenite structure to be completely transformed into fine and evenly distributed ferrite and pearlite structure, thereby reducing the banding of the steel. Finally, the steel is air-cooled to reduce the hardness of the steel to below 160HBW.
4. According to claim 3, a method for manufacturing high-strength reducer gear steel for new energy vehicles, characterized in that The continuous casting crystallizer is cooled by strong cooling, so that a high-strength chill layer with a thickness of more than 10 mm is formed on the surface of the ingot. The chill layer is composed of fine equiaxed crystal bands with different orientations. The high-strength fine equiaxed crystal bands ensure that the continuous casting ingot will not produce surface crack defects during the subsequent straightening process.
5. According to claim 4, a method for manufacturing high-strength reducer gear steel for new energy vehicles is characterized in that In order to prevent excessive stress on the surface of the continuous casting billet during the cooling process, the continuous casting billet adopts a hot delivery process with a hot delivery temperature ≥ 600℃.
6. The method for manufacturing high-strength reducer gear steel for new energy vehicles according to claim 3, characterized in that The temperatures of the three-stage rolling deformation process are all carried out at a relatively high plastic temperature. The method for determining the high plastic temperature is: the continuous casting billet is heated to different temperatures, and then the continuous casting billet is forged with the same force. The high plastic temperature is when the continuous casting billet can achieve large deformation after forging.
7. The method for manufacturing high-strength reducer gear steel for new energy vehicles according to claim 6, characterized in that The continuous casting slab is heated to a temperature of 750-1100°C.
8. The method for manufacturing high-strength reducer gear steel for new energy vehicles according to claim 3, characterized in that The method for determining the optimal normalizing holding temperature during isothermal normalizing treatment is to use a scanning electron microscope to observe the precipitation rate of NbC and AlN particles inside the high-temperature rolled material at different temperatures in the range of 850-950°C. When the NbC and AlN particles have the highest precipitation rate, this temperature is the optimal normalizing temperature.
9. The method for manufacturing high-strength reducer gear steel for new energy vehicles according to claim 3, characterized in that The temperature drop rate of the steel in the rapid cooling stage is ≥10℃ / s, and the steel is rapidly cooled to 20℃ below the Ar1 temperature, and the Ar1 temperature is 705℃.