Light-emitting device, manufacturing method for light-emitting device, and display apparatus

By using the electronic functional layer of the second carbon quantum dot material and the optimized hole functional layer structure in the light-emitting device, the problem of insufficient photoelectric performance and service life of the light-emitting device is solved, and its photoelectric performance and service life are significantly improved.

WO2024213140A1PCT designated stage expired Publication Date: 2024-10-17TCL TECHNOLOGY GROUP CORPORATION

Patent Information

Application Number
PCT/CN2024/087596
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-12
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Light-emitting devices, especially quantum dot light-emitting diodes, suffer from insufficient optoelectronic performance and lifetime, mainly due to low hole injection levels and imbalanced electron-hole transport.

Method used

An electronic functional layer and a hole functional layer are introduced into the light-emitting device. The electronic functional layer material contains a second carbon quantum dot to improve the excess electron injection, and improves the hole injection level through the gradient energy level structure of the hole functional layer, combined with the first and properties of the second carbon quantum dot to optimize the electron-hole transport balance.

Benefits of technology

It effectively improves the photoelectric performance and service life of the light-emitting device, and extends the working life of the device by improving the electron-hole transport balance and reducing interface defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024087596_17102024_PF_FP_ABST
    Figure CN2024087596_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A light-emitting device (1), comprising: an anode (11) and a cathode (12), which are disposed opposite each other; a light-emitting layer (13), which is disposed between the anode (11) and the cathode (12); and an electron functional layer (15), which is disposed between the cathode (12) and the light-emitting layer (13), wherein the material of the electron functional layer (15) comprises second carbon quantum dots, so as to facilitate electron-hole transport balance, thereby increasing the photoelectric performance of the light-emitting device (1) and the device life thereof. Further provided are a manufacturing method for a light-emitting device (1), and a display apparatus.
Need to check novelty before this filing date? Find Prior Art

Description

Light-emitting device, method for manufacturing light-emitting device, and display device

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 13, 2023, with application number 202310395945.7 and application name “Light-emitting device, method for preparing light-emitting device and display device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of optoelectronic technology, and in particular to a light-emitting device, a method for preparing a light-emitting device, and a display device. Background Art

[0003] Optoelectronic devices refer to a class of devices made using the photoelectric effect of semiconductors, including but not limited to light-emitting devices, solar cells, or photodetectors. Taking light-emitting devices as an example, light-emitting devices include but are not limited to organic light-emitting diodes (OLEDs) and quantum dot light-emitting diodes (QLEDs). OLEDs / QLEDs have a "sandwich" structure, that is, they include an anode, a cathode, and a light-emitting layer, wherein the anode and the cathode are arranged opposite each other, and the light-emitting layer is arranged between the anode and the cathode. The light-emitting principle of OLEDs / QLEDs is: electrons are injected from the cathode of the device into the light-emitting region, and holes are injected from the anode of the device into the light-emitting region. The electrons and holes recombine in the light-emitting region to form excitons, and the recombined excitons release photons through radiative transitions, thereby emitting light. Technical issues

[0004] After years of development, light-emitting devices have made great progress in performance indicators and have shown great application development potential. However, there are still shortcomings. The photoelectric performance and service life of light-emitting devices need to be further improved, especially for quantum dot light-emitting diodes. Technical Solutions

[0005] The present application provides a light-emitting device, a method for preparing the light-emitting device, and a display device, thereby improving the photoelectric performance and device life of the light-emitting device.

[0006] In a first aspect, the present application provides a light-emitting device, comprising:

[0007] an anode and a cathode arranged opposite to each other;

[0008] a light-emitting layer, disposed between the anode and the cathode;

[0009] The electronic functional layer is arranged between the cathode and the light-emitting layer, and the material of the electronic functional layer includes second carbon quantum dots.

[0010] In a second aspect, the present application provides a method for preparing a light-emitting device, comprising the following steps:

[0011] providing a bottom electrode, and forming a light emitting layer on one side of the bottom electrode; and

[0012] forming a top electrode on a side of the light-emitting layer away from the bottom electrode;

[0013] Wherein, when the light-emitting device is of a positive structure, the bottom electrode is an anode and the top electrode is a cathode, and before the step of forming the light-emitting layer on one side of the bottom electrode, the method for preparing the light-emitting device further comprises the steps of: forming an electronic functional layer on a side of the light-emitting layer away from the bottom electrode; and forming the top electrode on a side of the electronic functional layer away from the light-emitting layer;

[0014] Alternatively, when the light-emitting device has an inverted structure, the bottom electrode is a cathode and the top electrode is an anode, and before the step of forming the light-emitting layer on one side of the bottom electrode, the method for preparing the light-emitting device further comprises the steps of: forming an electronic functional layer on one side of the bottom electrode; the light-emitting layer is formed on a side of the electronic functional layer away from the bottom electrode;

[0015] Wherein, the material of the electronic functional layer includes second carbon quantum dots.

[0016] In a third aspect, the present application provides a display device, the display device including a light-emitting device, the light-emitting device including:

[0017] an anode and a cathode arranged opposite to each other;

[0018] a light-emitting layer, disposed between the anode and the cathode;

[0019] The electronic functional layer is arranged between the cathode and the light-emitting layer, and the material of the electronic functional layer includes second carbon quantum dots. Beneficial effects

[0020] In the light-emitting device, the material of the electronic functional layer includes second carbon quantum dots, which have higher conduction bands and valence bands, can block electrons and easily conduct holes, effectively improving the problem of excessive electron injection, thereby promoting the electron-hole transfer balance of the light-emitting device; in addition, when the electronic functional layer containing the second carbon quantum dots is in contact with the cathode, due to the low number of oxygen functional groups located on the surface of the second carbon quantum dots, the chemical reaction between the cathode and the electronic functional layer can be weakened, thereby reducing the electron injection level, further promoting the electron-hole transfer balance of the light-emitting device, thereby further improving the photoelectric device and device life of the light-emitting device. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0022] FIG1 is a schematic structural diagram of a first light-emitting device provided in an embodiment of the present application.

[0023] FIG2 is a schematic structural diagram of a second light-emitting device provided in an embodiment of the present application.

[0024] Implementation Methods of the Application

[0025] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without making creative efforts are within the scope of protection of this application.

[0026] The present invention provides a quantum dot light-emitting layer, a method for preparing the same, and a quantum dot light-emitting diode device. Each of these embodiments is described in detail below. It should be noted that the order in which the following embodiments are described does not limit the preferred order of the embodiments. Furthermore, in the description of this application, the term "including" means "including but not limited to." The terms "first," "second," and "third," etc., are used merely as designations and do not impose numerical requirements or establish an order. Various embodiments of the present invention may be presented in the form of a range. It should be understood that describing a range in this format is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the invention. Therefore, the range description should be considered to specifically disclose all possible subranges and individual numbers within that range. For example, a range description of 1 to 6 should be considered to specifically disclose subranges such as 1 to 3, 1 to 4, 1 to 5, 2 to 4, 2 to 6, 3 to 6, etc., as well as individual numbers within that range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is indicated herein, it is intended to include any cited number (fractional or integer) within the indicated range.

[0027] In this application, the term "including" means "including but not limited to".

[0028] The term "and / or" is used to describe the association relationship of associated objects, indicating that three relationships may exist. For example, "A and / or B" can represent three situations: the first situation is that A exists alone; the second situation is that A and B exist at the same time; the third situation is that B exists alone, where A and B can be singular or plural respectively.

[0029] The term "at least one" means one or more, and "a plurality of" means two or more. The terms "at least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can be expressed as: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or plural, respectively.

[0030] The terms “layer A is formed on one side of layer B”, “layer A is formed on the side of layer B away from layer C” or similar descriptions may mean that layer A is directly formed on one side of layer B or on the side of layer B away from layer C, i.e., layer A is in direct contact with layer B, or that layer A is indirectly formed on one side of layer B or on the side of layer B away from layer C, i.e., another spacing structure layer may be formed between layer A and layer B. Similarly, “layer A is arranged on one side of layer B”, “layer A is arranged on the side of layer B away from layer C” may mean that layer A is in direct contact with layer B, or that another spacing structure layer is provided between layer A and layer B; “layer A is arranged between layer B and layer C” may mean that layer A is in direct contact with layer B and layer A is in direct contact with layer C, or that layer A is in direct contact with layer B and one or more spacing structure layers are provided between layer A and layer C, or that one or more spacing structure layers are provided between layer A and layer B and one or more spacing structure layers are provided between layer A and layer C, or that layer A and layer B are provided with one or more spacing structure layers and layer A is in direct contact with layer C.

[0031] In the present application, “gradually widens”, “gradually narrows”, “gradually increases”, “gradually decreases” or similar expressions should be understood in a broad sense, that is, they can be gradually changed in a step-like manner or in a continuous manner.

[0032] An embodiment of the present application provides a light-emitting device, as shown in Figures 1 and 2, the light-emitting device 1 includes an anode 11, a cathode 12, a light-emitting layer 13 and an electronic functional layer 15, wherein the anode 11 and the cathode 12 are arranged opposite to each other, the light-emitting layer 13 is arranged between the anode 11 and the cathode 12, the electronic functional layer 15 is arranged between the cathode 12 and the light-emitting layer 13, and the material of the electronic functional layer 15 includes second carbon quantum dots.

[0033] In the light-emitting device 1 of the embodiment of the present application, the material of the electronic functional layer 15 includes second carbon quantum dots, which have higher conduction bands and valence bands, can block electrons and easily conduct holes, effectively improving the problem of excessive electron injection, thereby promoting the electron-hole transfer balance of the light-emitting device 1; in addition, when the electronic functional layer containing the second carbon quantum dots is in contact with the cathode, since the number of oxygen functional groups located on the surface of the second carbon quantum dots is low, for example, much lower than the oxygen functional groups on the surface of metal oxides (such as ZnO) synthesized by a solution method, the chemical reaction between the cathode 12 and the electronic functional layer 15 can be weakened, thereby reducing the electron injection level, promoting the electron-hole transfer balance of the light-emitting device 1, and thus improving the photoelectric device and device life of the light-emitting device 1.

[0034] In the light-emitting device 1 of the embodiment of the present application, the electronic functional layer 15 can be a single-layer structure or a multi-layer structure. In order to further balance the promotion of electron-hole transport balance and the reduction of interface defects in the light-emitting device 1, in some embodiments of the present application, please continue to refer to Figure 2. The electronic functional layer 15 includes a first electronic functional sublayer 151 and a second electronic functional sublayer 152 arranged in a stacked manner. The first electronic functional sublayer 151 is closer to the light-emitting layer 13 than the second electronic functional sublayer 152. The material of the first electronic functional sublayer 151 includes the second carbon quantum dots and / or the first compound, and the material of the second electronic functional sublayer 152 includes the second carbon quantum dots and / or the second compound.

[0035] In order to further improve the comprehensive performance of the light-emitting device, in some embodiments of the present application, the first electronic functional sublayer 151 and the second electronic functional sublayer 152 are any of the following:

[0036] (a) The material of the first electronic functional layer 151 is a mixture of the second carbon quantum dots and the first compound, and the material of the second electronic functional layer 152 is the second compound;

[0037] (b) the material of the first electronic functional sublayer 151 is the second carbon quantum dots, and the material of the second electronic functional sublayer 152 is the second compound;

[0038] (c) The material of the first electronic functional sublayer 151 is the first compound; the material of the second electronic functional sublayer 152 is the second carbon quantum dots, or the material of the second electronic functional sublayer 152 is a mixture of the second carbon quantum dots and the second compound.

[0039] The first compound and the second compound are independently selected from an undoped or doped second metal oxide, the doped second metal oxide is selected from one or more of ZnO, TiO2, SnO2, BaO, Ta2O3, Al2O3 and ZrO2, the doped second metal oxide is selected from one or more of zinc magnesium oxide, zinc calcium oxide, zinc zirconium oxide, zinc gallium oxide, zinc aluminum oxide, zinc lithium oxide, zinc titanium oxide, yttrium zinc oxide, indium tin oxide and titanium lithium oxide, for example, Zn (1-x) Mg x O, Zn (1-x) Ca x O, Zn (1-x) Zr x O, Zn (1-x) Ga x O, Zn (1-x) Al x O, Zn (1-x) Li x O、Al (1-x) Zn x O, Zn (1-x) Ti x O, Zn (1-x) Y x O、In (1-x) Sn x O and Ti (1-x) Li x One or more of O, where 0<x≤0.5.

[0040] In order to further improve the comprehensive performance of the light-emitting device 1, in some embodiments of the present application, under the condition of case (a), the thickness of the first electronic functional sublayer 151 is 5 nm to 10 nm, for example, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or a value between any two of the aforementioned values, and the thickness of the second electronic functional sublayer 152 is 20 nm to 50 nm, for example, 20 nm, 30 nm, 40 nm, 50 nm, or a value between any two of the aforementioned values. Alternatively, under the condition of case (b), the thickness of the first electronic functional sublayer 151 is 5 nm to 10 nm, for example, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or a value between any two of the aforementioned values, and the thickness of the second electronic functional sublayer 152 is 20 nm to 50 nm, for example, 20 nm, 30 nm, 40 nm, 50 nm, or a value between any two of the aforementioned values. Alternatively, under the conditions of case (c), the thickness of the first electronic functional sublayer 151 is 20nm to 50nm, for example, 20nm, 30nm, 40nm, 50nm and a value between any two of the aforementioned values, and the thickness of the second electronic functional sublayer 151 is 5nm to 10nm, for example, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm and a value between any two of the aforementioned values.

[0041] In order to further improve the overall performance of the light-emitting device 1, in some embodiments of the present application, when the material of the first electronic functional layer sublayer 151 is a mixture of the second carbon quantum dots and the first compound, the mass ratio of the first compound to the second carbon quantum dots is 1:(0.01-1), for example, 1:0.01, 1:0.05, 1:0.1, 1:0.5, 1:1, and values ​​between any two of the foregoing values. Alternatively, when the material of the second electronic functional sublayer 152 is a mixture of the second carbon quantum dots and the second compound, the mass ratio of the second compound to the second carbon quantum dots is 1:(0.01-1), for example, 1:0.01, 1:0.05, 1:0.1, 1:0.5, 1:1, and values ​​between any two of the foregoing values.

[0042] In order to further promote the electron-hole transport balance of the light-emitting device 1 and further improve the comprehensive performance of the light-emitting device 1, in some embodiments of the present application, with continued reference to Figures 1 and 2, the light-emitting device 1 further includes a hole functional layer 14 disposed between the anode 11 and the light-emitting layer 13, and the material of the hole functional layer 14 includes first carbon quantum dots. The first carbon quantum dot layer closest to the light-emitting layer 13 in the hole functional layer 14 is a first sublayer, the average band gap of the first carbon quantum dots in the first sublayer is a first band gap, and the thickness of the first sublayer is the largest particle size of the first carbon quantum dots in the first sublayer; the first carbon quantum dot layer closest to the anode 11 in the hole functional layer 14 is a second sublayer, the average band gap of the first carbon quantum dots in the second sublayer is a second band gap, and the thickness of the second sublayer is the largest particle size of the first carbon quantum dots in the second sublayer; the first band gap is wider than the second band gap.

[0043] As used herein, "band gap," also known as energy band gap, refers to the energy difference between the lowest point of the conduction band of a carbon quantum dot and the highest point of its valence band. "Average band gap" refers to the average band gap of all first carbon quantum dots in the first or second sublayer. Those skilled in the art can determine the average band gap using statistical methods.

[0044] Taking QLED as an example, the low hole injection level caused by the high hole injection barrier is one of the main factors affecting the luminous efficiency and service life of QLED. The specific manifestations are: first, the hole injection of QLED is blocked, resulting in a high turn-on voltage of QLED, and holes are easily accumulated at the interface of adjacent film layers, leading to oxidation and denaturation of hole functional materials; second, the hole transport resistance is large, causing QLED to easily heat up during operation, and the thermal effect of the film layer will accelerate the aging of the functional materials of each layer, shortening the service life of QLED; third, the energy gap between the hole functional layer and the light-emitting layer is large. The level matching is not ideal, which makes it difficult to inject holes into the light-emitting layer, resulting in the number of electrons injected into the light-emitting layer being much higher than the number of holes injected into the light-emitting layer, causing an imbalance in the electron-hole transfer, and the excess electrons will make the quantum dots in the light-emitting layer negatively charged, which is prone to form Auger recombination, causing the QLED performance to drop sharply; fourth, excess electrons accumulate at the interface between the hole functional layer and the light-emitting layer, and the electrons will recombine with holes in the hole transport layer, causing the hole functional layer to emit light and heat, and will damage the hole functional material, thereby sharply reducing the service life and brightness of the QLED.

[0045] In the light-emitting device 1 of the present application, on the one hand, since the average band gap of the first carbon quantum dots in the second sublayer is narrow, it is closer to the work function of the anode material, making it easier for holes to be injected from the anode 11 to the hole functional layer 14, effectively improving the hole injection level of the light-emitting device 1; on the other hand, since the average band gap of the first carbon quantum dots in the first sublayer is wide, it can reduce the barrier for hole injection into the light-emitting layer 13, effectively improving the hole mobility, thereby improving the hole transport capacity of the hole functional layer 14, and further optimizing the photoelectric performance of the light-emitting device 1 and extending the service life of the light-emitting device 1. In addition, the first carbon quantum dots have the advantages of controllable particle size, controllable energy level, controllable conductivity, easy synthesis, easy dispersion in polar or non-polar solvents, and strong resistance to water and oxygen. The conductivity of the first carbon quantum dots can be no less than 10 -4 cm 2 / V·s, the conductivity of the first carbon quantum dots can be 1 to 3 orders of magnitude higher than that of many hole-forming organic materials, which can further improve the optoelectronic device and device life of the light-emitting device 1.

[0046] In order to further improve the hole injection level of the light-emitting device, in some embodiments of the present application, referring to FIG1 , the average band gap of the first carbon quantum dots in the hole functional layer 14 gradually widens in the direction from the anode 11 to the light-emitting layer 13, so that the hole functional layer has an energy level gradient. Furthermore, in at least one embodiment of the present application, the average particle size of the first carbon quantum dots in the hole functional layer 14 gradually decreases in the direction from the anode 11 to the light-emitting layer 13. It is understood that the hole functional layer may include the first carbon quantum dot sublayer X1 to the first carbon quantum dot sublayer X2. t , t is a positive integer greater than or equal to 2, and along the direction from the anode 11 to the light-emitting layer 13, the first carbon quantum dot sublayer X1 to the first carbon quantum dot sublayer X t The first carbon quantum dots in each first carbon quantum dot sub-layer have an average band gap, and the first carbon quantum dots in each first carbon quantum dot sub-layer have an average particle size. The average band gap of the first carbon quantum dots in the first carbon quantum dot sub-layer X1 is about 1 / 4 of the first carbon quantum dot sub-layer X2. t The average band gap of the first carbon quantum dots in the first carbon quantum dot layer becomes wider, and / or the average particle size of the first carbon quantum dot sub-layer X1 becomes larger than the average particle size of the first carbon quantum dot sub-layer X2. t The average particle size of the first carbon quantum dots decreases successively.

[0047] In some embodiments of the present application, the particle size distribution range of the first carbon quantum dots in the hole functional layer 14 is 1 nm to 50 nm.

[0048] In some embodiments of the present application, the first carbon quantum dots include carbon quantum dot material A and / or carbon quantum dot material B, and the average particle size of carbon quantum dot material A is greater than the average particle size of carbon quantum dot material B; the hole functional layer 14 includes a hole injection layer and / or a hole transport layer, and for the hole functional layer including the hole injection layer and the hole transport layer, the hole injection layer is closer to the anode 11 than the hole transport layer; wherein, the material of the hole injection layer includes carbon quantum dot material A, and / or the material of the hole transport layer includes carbon quantum dot material B. As an example, referring to Figure 1, the hole functional layer 14 includes a hole injection layer 141 and a hole transport layer 142. The hole injection layer 141 is closer to the anode 11 than the hole transport layer 142, and the hole transport layer 142 is closer to the light-emitting layer 13 than the hole injection layer 141. The thickness of the hole injection layer 141 can be, for example, 10nm to 100nm, and the thickness of the hole transport layer 142 can be, for example, 10nm to 100nm.

[0049] In some embodiments of the present application, the average particle size of the carbon quantum dot material A is 10 nm to 30 nm; and / or the average particle size of the carbon quantum dot material B is 1 nm to 10 nm.

[0050] In order to improve the energy level control capability of the hole functional layer, in some embodiments of the present application, the material of the hole functional layer 14 further comprises a third compound, and the third compound is selected from poly (3,4-ethylenedioxythiophene): poly (styrene sulfonic acid), copper phthalocyanine, titanium phthalocyanine, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanodimethyl-p-benzoquinone, 2,3,6,7,10,11-hexyano-1,4,5,8,9,12-hexaazatriphenylene, 3-hexyl substituted polythiophene, poly (9-vinyl carbazole), 4,4'-bis (9-carbazole) biphenyl, poly [bis (4-phenyl) (4 -butylphenyl) amine], 4,4'-cyclohexylbis[N,N-bis(4-methylphenyl) aniline], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl) diphenylamine)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl)) diphenylamine)], poly(N,N'-bis(4-butylphenyl)-N,N'-diphenyl-1,4-phenylenediamine-co-9,9-dioctylfluorene), 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)tris(1,2-diamino-1,4-phenylenediamine) Aniline, 4,4',4"-tris(carbazol-9-yl)triphenylamine, 4,4',4'-tris(2-naphthylphenylamino)triphenylamine, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine, N,N'-bis[4-(diphenylamino)phenyl]-N,N'-diphenylbenzidine, N,N'-bis(3-methylphenyl)-N,N'-diphenyl-9,9-spirobifluorene-2,7-diamine, N2,N7-diphenylamine -1-naphthyl-N2,N7-diphenyl-9,9'-spirobi[9H-fluorene]-2,7-diamine, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, doped or undoped nickel oxide, doped or undoped molybdenum oxide, doped or undoped tungsten oxide, doped or undoped vanadium oxide, doped or undoped P-type gallium nitride, doped or undoped chromium oxide, doped or undoped copper oxide, transition metal sulfide and transition metal selenide. One or more.Among them, transition metal sulfides include but are not limited to one or more of molybdenum sulfide, tungsten sulfide and copper sulfide; transition metal selenides include but are not limited to one or more of molybdenum selenide and tungsten selenide; an example of doped or undoped nickel oxide is NiO; an example of doped or undoped molybdenum oxide is MoO3; an example of doped or undoped tungsten oxide is WO3; an example of doped or undoped vanadium oxide is V2O5; an example of doped or undoped chromium oxide is CrO3; an example of doped or undoped copper oxide is CuO and one or more of Cu2O.

[0051] In order to further improve both the energy level control capability and the conductivity of the hole functional layer 14 , in some embodiments of the present application, when the material of the hole functional layer 14 further includes a third compound, in the hole functional layer 14 , the mass ratio of the third compound to the first carbon quantum dots is 1:(0.01~1).

[0052] As an example, referring to FIG1 , when the material of the hole injection layer 141 includes a carbon quantum dot material A, the material of the hole injection layer 141 also includes a first material. The selection range of the first material refers to the description of the third compound in the previous text. In the hole injection layer 141, the mass ratio of the first material to the carbon quantum dot material A is 1:(0.01-1), for example, it can be 1:(0.01-0.03), 1:(0.03-0.05), 1:(0.05-0.07), 1:(0.05-0.1), 1:(0.1-0.5), or 1:(0.1-1), examples are 1:0.01, 1:0.05, 1:0.1, 1:1 :0.5, or 1:1; and / or, when the material of the hole transport layer 142 includes B carbon quantum dot material, the material of the hole transport layer 142 also includes a second material, and the selection range of the second material refers to the description of the third compound in the above text, and the mass ratio of the second material to the B carbon quantum dot material is 1:(0.01~1), for example, it can be 1:(0.01~0.03), 1:(0.03~0.05), 1:(0.05~0.07), 1:(0.05~0.1), 1:(0.1~0.5), or 1:(0.1~1), examples are 1:0.01, 1:0.05, 1:0.1, 1:0.5, or 1:1.

[0053] In some embodiments of the present application, the hole injection layer 141 includes a first hole injection sublayer to an M-th hole injection sublayer arranged in a stacked manner, where M is a positive integer greater than or equal to 2, and the first hole injection sublayer to the M-th hole injection sublayer are arranged in sequence along the direction of the anode 11 toward the light-emitting layer 13. The average band gaps of the A carbon quantum dot materials contained in the first hole injection sublayer to the M-th hole injection sublayer are respectively the first band gap to the M-th band gap, and the first band gap to the M-th band gap become wider in sequence; and / or, the average particle sizes of the A carbon quantum dot materials contained in the first hole injection sublayer to the M-th hole injection sublayer are respectively the first average particle size to the M-th average particle size, and the first average particle size to the M-th average particle size become smaller in sequence.

[0054] As an example, as shown in Figure 2, the hole injection layer 141 includes a first hole injection sublayer 1411, a second hole injection sublayer 1412 and a third hole injection sublayer 1413 which are stacked in sequence. The first hole injection sublayer 1411 is closer to the anode 11 than the third hole injection sublayer 1413, and the third hole injection sublayer 1413 is closer to the light-emitting layer 13 than the first hole injection sublayer 1411. In the direction from the first hole injection sublayer 1411 to the third hole injection sublayer 1413, the average particle size of the A carbon quantum dot material in each layer gradually decreases. For example, the average particle size of the A carbon quantum dot material in the first hole injection sublayer 1411 is 30 nm, the average particle size of the A carbon quantum dot material in the second hole injection sublayer 1412 is 20 nm, and the average particle size of the A carbon quantum dot material in the third hole injection sublayer 1413 is 10 nm.

[0055] In some embodiments of the present application, the hole transport layer 142 includes a first hole transport sublayer to an Nth hole transport sublayer that are stacked, where N is a positive integer greater than or equal to 2. Along the direction from the anode 11 to the light-emitting layer 13, the first hole transport sublayer to the Nth hole transport sublayer are arranged in sequence, and the average band gaps of the B carbon quantum dot materials contained in the first hole transport sublayer to the Mth hole transport sublayer are respectively from band gap one to band gap N, and the band gaps from band gap one to band gap N become wider in sequence; and / or, the average particle sizes of the B carbon quantum dot materials contained in the first hole transport sublayer to the Nth hole transport sublayer are respectively from average particle size one to average particle size N, and the average particle size from average particle size one to average particle size N become smaller in sequence.

[0056] As an example, referring to Figure 2, the hole transport layer 142 includes a first hole transport sublayer 1421, a second hole transport sublayer 1422 and a third hole transport sublayer 1423 which are stacked in sequence. The first hole transport sublayer 1421 is closer to the anode 11 than the third hole transport sublayer 1423, and the third hole transport sublayer 1423 is closer to the light-emitting layer 13 than the first hole transport sublayer 1421. In the direction from the first hole transport sublayer 1421 to the third hole transport sublayer 1423, the average particle size of the B carbon quantum dot material in each layer gradually decreases. For example, the average particle size of the B carbon quantum dot material in the first hole transport sublayer 1421 is 10 nm, the average particle size of the B carbon quantum dot material in the second hole transport sublayer 1422 is 5 nm, and the average particle size of the B carbon quantum dot material in the third hole transport sublayer 1423 is 1 nm.

[0057] In the light-emitting device 1 of the embodiment of the present application, the materials of the anode 11 and the cathode 12 are independently selected from one or more of metals, carbon materials and first metal oxides, wherein the metals include but are not limited to one or more of Al, Ag, Cu, Mo, Au, Ba, Pt, Ca and Mg; the carbon materials include but are not limited to one or more of graphite, carbon nanotubes, graphene and carbon fibers; the first metal oxide may be doped or undoped, including but not limited to one or more of indium tin oxide (ITO), fluorine-doped tin oxide (FTO), antimony tin oxide (ATO), aluminum-doped zinc oxide (AZO), gallium-doped zinc oxide (GZO), indium-doped zinc oxide (IZO) and magnesium-doped zinc oxide (MZO). The anode 11 or cathode 12 may also be a composite electrode having a "sandwich" structure, wherein the upper and lower layers are made of doped or undoped transparent metal oxides, respectively, and the middle layer is made of a metal, such as one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2. The thickness of the middle layer does not exceed 35 nm. The thickness of the anode 11 may be, for example, 20 nm to 300 nm, and the thickness of the cathode 12 may be, for example, 20 nm to 300 nm.

[0058] The material of the light-emitting layer 13 can be selected from organic light-emitting materials or quantum dots. The corresponding light-emitting device 1 is an OLED or a QLED. The thickness of the light-emitting layer 13 can be, for example, 10 nm to 50 nm. The light-emitting layer 13 can have a single-layer structure or a multi-layer structure. For example, the light-emitting layer 13 can have two or more layers.

[0059] Organic light-emitting materials include, but are not limited to, one or more of 4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distyrene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delay materials, polymers containing covalent bonds of BN, hybrid localized charge transfer excited state materials, and exciplex light-emitting materials.

[0060] Quantum dots include but are not limited to one or more of red quantum dots, green quantum dots and blue quantum dots, and quantum dots include but are not limited to one or more of single-component quantum dots, core-shell structure quantum dots, inorganic perovskite quantum dots, organic perovskite quantum dots and organic-inorganic hybrid perovskite quantum dots. The average particle size of the quantum dots can be, for example, 5nm to 10nm, and the average particle size of the quantum dots is exemplified as 5nm, 6nm, 7nm, 8nm, 9nm, 10nm and values ​​between any two of the foregoing values.

[0061] For single-component quantum dots and core-shell quantum dots, the material of the single-component quantum dots, the material of the core of the core-shell quantum dots or the material of the shell of the core-shell quantum dots are, but are not limited to, at least one of a II-VI compound, a III-V compound, a IV-VI compound or a I-III-VI compound, wherein the II-VI compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, Zn One or more of STe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and a Group III-V compound selected from GaN, GaP, GaAs, GaSb, AlN, AlP, Al As, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, I nPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNA s, InAlNSb, InAlPAs and InAlPSb, the IV-VI group compound is selected from one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, and the I-III-VI group compound is selected from one or more of CuInS, CuInSe and AgInS. It should be noted that for the material of the aforementioned single-component quantum dot, or the material of the core of the core-shell structure quantum dot, or the material of the shell of the core-shell structure quantum dot, the chemical formula provided only indicates the elemental composition, and does not indicate the content of each element. For example: CdZnSe only indicates that it is composed of three elements: Cd, Zn and Se. If the content of each element is expressed, it corresponds to Cd x Zn 1-x Se,0 <x<1。

[0062] For inorganic perovskite quantum dots, the general structural formula of inorganic perovskite quantum dots is AMX3, where A is Cs + ion, M is a divalent metal cation, M includes but is not limited to Pb 2+ 、Sn 2+ 、Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ 、Mn 2+ 、Co 2+ 、Fe 2+ 、Ge 2+ 、Yb 2+ or Eu 2+ , X is a halogen anion, including but not limited to Cl - Br - or I - .

[0063] For organic perovskite quantum dots, the general structural formula of organic perovskite quantum dots is CMX3, wherein C is a formamidinium group, and M is a divalent metal cation, including but not limited to Pb 2+ 、Sn 2+ 、Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ 、Mn 2+ 、Co 2+ 、Fe 2+ 、Ge 2+ 、Yb 2+ or Eu 2+ , X is a halogen anion, including but not limited to Cl - Br - or I - .

[0064] For organic-inorganic hybrid perovskite quantum dots, the general structural formula of organic-inorganic hybrid perovskite quantum dots is BMX3, wherein B is selected from organic amine cations, and the organic amine cations include but are not limited to CH3(CH2) n-2 NH 3+ (n≥2) or NH3(CH2) n NH3 2+ (n≥2), M is a divalent metal cation, including but not limited to Pb 2+ 、Sn 2+ 、Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ 、Mn 2+ 、Co 2+ 、Fe2+ 、Ge 2+ 、Yb 2+ or Eu 2+ , X is a halogen anion, including but not limited to Cl - Br - or I - .

[0065] It is understood that when the material of the light-emitting layer 13 includes quantum dots, the material of the light-emitting layer 13 also includes ligands connected to the surface of the quantum dots, and the ligands include but are not limited to at least one of amine ligands, carboxylic acid ligands, thiol ligands, (oxy)phosphine ligands, phospholipids, soft phospholipids or polyvinyl pyridine, and the amine ligands are, for example, selected from at least one of methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, nonylamine, decylamine, dodecylamine, hexadecylamine, octadecylamine, dimethylamine, diethylamine, dipropylamine, tributylamine, or trioctylamine. , the carboxylic acid ligand is, for example, selected from at least one of formic acid, acetic acid, propionic acid, butyric acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid or benzoic acid, the thiol ligand is, for example, selected from at least one of methyl mercaptan, ethyl mercaptan, propyl mercaptan, butyl mercaptan, pentyl mercaptan, hexyl mercaptan, octadecyl mercaptan, dodecanethiol, hexadecyl mercaptan, octadecyl mercaptan or benzyl mercaptan, and the (oxygen) phosphine ligand is selected from at least one of methyl phosphine, ethyl phosphine, propyl phosphine, butyl phosphine, pentyl phosphine, octyl phosphine, dioctyl phosphine, tributyl phosphine or trioctyl phosphine.

[0066] In some embodiments of the present application, when the material of the light-emitting layer 13 includes quantum dots, the average band gap of the first carbon quantum dots in the first sublayer is wider than the average band gap of the quantum dots to improve the recombination efficiency of hole-electron pairs in the light-emitting layer 13.

[0067] The present application also provides a method for preparing a light-emitting device, which can be used to prepare any of the light-emitting devices described above, comprising the following steps:

[0068] S1. providing a bottom electrode and forming a light-emitting layer on one side of the bottom electrode;

[0069] S2. Form a top electrode on a side of the light-emitting layer away from the bottom electrode.

[0070] When the light-emitting device has an upright structure, the bottom electrode is an anode and the top electrode is a cathode. Prior to the step of forming the light-emitting layer on one side of the bottom electrode and prior to step S2, the method for preparing the light-emitting device further comprises the steps of: forming an electronic functional layer on a side of the light-emitting layer remote from the bottom electrode; and forming the top electrode on a side of the electronic functional layer remote from the light-emitting layer. Alternatively, when the light-emitting device has an inverted structure, the bottom electrode is a cathode and the top electrode is an anode. Prior to the step of forming the light-emitting layer on one side of the bottom electrode, the method for preparing the light-emitting device further comprises the steps of: forming an electronic functional layer on one side of the bottom electrode; and forming the light-emitting layer on a side of the electronic functional layer remote from the bottom electrode. The material of the electronic functional layer comprises a second carbon quantum dot.

[0071] To further improve the overall performance of the light-emitting device, in some embodiments of the present application, when the light-emitting device has an upright structure, the method for preparing the light-emitting device further includes the steps of: forming a hole-functional layer on one side of the bottom electrode; and forming the light-emitting layer on the side of the hole-functional layer away from the bottom electrode; or, when the light-emitting device has an inverted structure, the method for preparing the light-emitting device further includes the steps of: forming a hole-functional layer on the side of the light-emitting layer away from the bottom electrode; and forming a top electrode on the side of the hole-functional layer away from the light-emitting layer. The structural composition of the hole-functional layer is as described above.

[0072] In some embodiments of the present application, when the light-emitting device is of an upright structure, the method for forming the hole functional layer includes the steps of: sequentially forming a first cured film layer to an Nth cured film layer on one side of the bottom electrode, where N is a positive integer greater than or equal to two; or, when the light-emitting device is of an inverted structure, the method for forming the hole functional layer includes the steps of: sequentially forming an Nth cured film layer to a first cured film layer on a side of the light-emitting layer away from the bottom electrode, where N is a positive integer greater than or equal to two; wherein each of the first to Nth cured film layers contains first carbon quantum dots.

[0073] In order to further improve the hole injection level of the light-emitting device, in some embodiments of the present application, the average band gap of the first carbon quantum dots in each cured film layer gradually widens along the direction from the first cured film layer to the Nth cured film layer; and / or, the average particle size of the first carbon quantum dots in each cured film layer gradually decreases along the direction from the first cured film layer to the Nth cured film layer, so that the hole functional layer has a gradient energy level structure.

[0074] In some embodiments of the present application, a method for preparing at least one of the first to Nth cured film layers includes the steps of depositing a third dispersion containing first carbon quantum dots, and then performing a third drying process on the deposited third dispersion to obtain a cured film layer. The third dispersion may be deposited using a solution method, including but not limited to at least one of spin coating, coating, printing, doctor blade coating, dip-pull, immersion, spraying, roller coating, or casting.

[0075] Specifically, the "third drying process" includes any process capable of increasing the energy of the deposited third dispersion and converting it into a solidified film layer, including but not limited to heat treatment or vacuum drying. In some embodiments of the present application, the third drying process is a heat treatment at a temperature of 80°C to 230°C; and / or the third drying process lasts for 5 to 60 minutes.

[0076] For the first carbon quantum dots having ligands attached to their surfaces, to further enhance the conductivity of the first carbon quantum dots, the third drying process is performed under an inert gas atmosphere for at least a portion of the entire process, thereby reducing at least a portion of the ligands on the surfaces of the first carbon quantum dots. The inert gas is selected from a class of gases that do not react with the first carbon quantum dots, including but not limited to at least one of nitrogen, helium, neon, argon, krypton, or xenon.

[0077] As an example, the third drying process includes the following steps:

[0078] Sa, performing a first heat treatment on the deposited third dispersion to obtain a cured film;

[0079] Sb. Under an inert atmosphere, the cured film is subjected to a second heat treatment.

[0080] Specifically, in step Sa, the temperature of the first heat treatment is 80°C to 230°C, the time of the first heat treatment can be 10 minutes to 30 minutes, and the first heat treatment can be performed in an atmospheric environment at room temperature and pressure, or in an inert atmosphere at room temperature and pressure.

[0081] In step Sb, the temperature of the second heat treatment is 80° C. to 230° C.; and the time of the second heat treatment is 10 min to 30 min.

[0082] In order to improve the energy level control capability of the hole functional layer and further enhance the hole injection level of the light-emitting device, in some embodiments of the present application, the third dispersion further comprises a third compound, as described above. In order to further enhance the overall performance of the light-emitting device, in some embodiments of the present application, the mass ratio of the third compound to the first carbon quantum dots in the third dispersion is 1:(0.01-1).

[0083] In order to improve the film-forming quality of the hole functional layer, in some embodiments of the present application, the concentration of the first carbon quantum dots in the third dispersion is 0.5 mg / mL to 10 mg / mL, for example, it can be 0.5 mg / mL to 1 mg / mL, 1 mg / mL to 2 mg / mL, 2 mg / mL to 3 mg / mL, 3 mg / mL to 4 mg / mL, 4 mg / mL to 5 mg / mL, 5 mg / mL to 6 mg / mL, 6 mg / mL to 7 mg / mL, 7 mg / mL to 8 mg / mL, 8 mg / mL to 9 mg / mL, or 9 mg / mL to 10 mg / mL, exemplified by 0.5 mg / mL, 1 mg / mL, 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, 9 mg / mL or 10 mg / mL.

[0084] To further improve the film-forming quality of the hole functional layer, in some embodiments of the present application, the third dispersion further comprises a crosslinking agent, wherein the third compound is an organic compound. During the formation of the cured film, the crosslinking agent undergoes a crosslinking reaction with the organic compound to form a crosslinked compound, so that the first carbon quantum dots can be uniformly attached to the crosslinked network structure, thereby achieving the purpose of uniform dispersion. It is understood that the crosslinking agent can be a photocrosslinking agent or a thermal crosslinking agent. For photocrosslinking agents, a light treatment step can be added before the third drying step to carry out the photocrosslinking reaction; for thermal crosslinking agents, the third drying step can be a heat treatment to carry out the crosslinking reaction during the third drying step.

[0085] In order to further improve the film formation quality, in some embodiments of the present application, in the third dispersion, the mass ratio of the third compound to the cross-linking agent is 1:(0.01~0.04), for example, it can be 1:(0.01~0.02), 1:(0.02~0.03), or 1:(0.02~0.04), with examples being 1:0.01, 1:0.02, 1:0.03, or 1:0.04.

[0086] In some embodiments of the present application, the crosslinking agent is selected from a thermal crosslinking agent, and the crosslinking reaction is carried out during the heat treatment process. The thermal crosslinking agent includes, but is not limited to, at least one of polyethylene glycol, polypropylene glycol, trimethylolpropane, or trimethylolethane. The crosslinking reaction temperature is, for example, 100°C to 230°C, and the crosslinking reaction time is, for example, 5 minutes to 30 minutes.

[0087] In order to further balance the promotion of the electron-hole transport balance of the light-emitting device and the reduction of interface defects, in some embodiments of the present application, when the light-emitting device is a positive structure, the step of forming an electronic functional layer on the side of the light-emitting layer away from the bottom electrode includes: forming a first electronic functional sublayer and a second electronic functional sublayer in sequence on the side of the light-emitting layer away from the bottom electrode; or, when the light-emitting device is an inverted structure, the step of forming an electronic functional layer on one side of the bottom electrode includes: forming a second electronic functional sublayer and a first electronic functional sublayer in sequence on one side of the bottom electrode. Wherein, the situation of the first electronic functional sublayer and the second electronic functional sublayer refers to the above description. It should be noted that the method for forming the first electronic functional sublayer and the second electronic functional sublayer includes but is not limited to a solution method.

[0088] In order to further improve the comprehensive performance of the light-emitting device, in some embodiments of the present application, when the material of the first electronic functional sublayer is a mixture of second carbon quantum dots and a first compound, the method for forming the first electronic functional sublayer includes the steps of: depositing a first dispersion containing the second carbon quantum dots and the first compound, and then performing a first drying process on the deposited first dispersion to obtain the first electronic functional sublayer; wherein, in the first dispersion, the mass ratio of the first compound to the second carbon quantum dots is 1:(0.01-1). Alternatively, when the material of the second electronic functional sublayer is a mixture of second carbon quantum dots and a second compound, the method for forming the second electronic functional sublayer includes the steps of: depositing a second dispersion containing the second carbon quantum dots and the second compound, and then performing a second drying process on the deposited second dispersion to obtain the second electronic functional sublayer; wherein, in the second dispersion, the mass ratio of the second compound to the second carbon quantum dots is 1:(0.01-1).

[0089] Specifically, the first drying treatment and the second drying treatment are independently selected from heat treatment and / or vacuum drying. The concentration of the second carbon quantum dots in the first dispersion is 0.5 mg / mL to 10 mg / mL, and / or the concentration of the second carbon quantum dots in the first dispersion is 0.5 mg / mL to 10 mg / mL. In addition, the dispersants of the first dispersion and the second dispersion are, for example, selected from alcohol compounds, such as methanol, ethanol, or glycerol.

[0090] It should be noted that, in addition to the electron functional layer and the hole functional layer, the methods for forming the other functional layers in the light-emitting device are, but are not limited to, chemical and / or physical methods. Among them, chemical methods include, but are not limited to, one or more of chemical vapor deposition, continuous ion layer adsorption and reaction, anodic oxidation, electrolytic deposition, and co-precipitation. Physical methods include, but are not limited to, physical plating and solution methods. Physical plating methods include, but are not limited to, one or more of thermal evaporation, electron beam evaporation, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition, and pulsed laser deposition. Solution methods include, but are not limited to, spin coating, printing, inkjet printing, doctor blade coating, printing, dip-coating, immersion, spraying, roller coating, casting, slot coating, and strip coating. After the functional layers of the light-emitting device are prepared, a packaging process is required. The packaging process can be performed by conventional machine packaging or manual packaging. In the packaging process environment, the oxygen content and water content are both less than 0.1 ppm to ensure the stability of the light-emitting device.

[0091] The methods for forming the bottom electrode, the hole functional layer, the light-emitting layer or the top electrode include but are not limited to solution method and deposition method. The solution method includes but is not limited to spin coating, printing, inkjet printing, doctor blade coating, printing, dip-coating, immersion, spraying, roll coating, casting, slit coating and strip coating. The deposition method includes chemical method and physical method. The chemical method includes but is not limited to chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition and co-precipitation. The physical method includes but is not limited to thermal evaporation coating, electron beam evaporation coating, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition and pulsed laser deposition.

[0092] The present application also provides a display device, comprising any of the light-emitting devices described in the present application, or comprising a light-emitting device produced by any of the preparation methods described in the present application. The display device can be any electronic product with a display function, including but not limited to a smartphone, tablet computer, laptop computer, digital camera, digital video camera, smart wearable device, smart weighing electronic scale, vehicle-mounted display, television, or e-book reader. The smart wearable device can be, for example, a smart bracelet, smart watch, virtual reality (VR) helmet, etc.

[0093] The technical solutions and technical effects of the present application are described in detail below through specific embodiments, comparative examples and experimental examples. The following embodiments are only some embodiments of the present application and do not specifically limit the present application.

[0094] Example 1

[0095] This embodiment provides a light-emitting device and a preparation method thereof. The light-emitting device is a quantum dot light-emitting diode with an upright structure. As shown in FIG2 , from bottom to top, the light-emitting device 1 includes a substrate 10, an anode 11, a hole functional layer 14, a light-emitting layer 13, an electron functional layer 15 and a cathode 12 arranged in sequence.

[0096] The hole functional layer 14 includes a stacked hole injection layer 141 and a hole transport layer 142. The hole injection layer 141 is closer to the anode 11 than the hole transport layer 142, and the hole transport layer 142 is closer to the light-emitting layer 13 than the hole injection layer 141. The hole injection layer 141 is composed of a first hole injection sublayer 1411, a second hole injection sublayer 1412, and a third hole injection sublayer 1413 stacked in sequence. The first hole injection sublayer 1411 is closer to the anode 11 than the third hole injection sublayer 1413. The hole transport layer 142 is composed of a first hole transport sublayer 1421, a second hole transport sublayer 1422, and a third hole transport sublayer 1423 stacked in sequence. The first hole transport sublayer 1421 is closer to the anode 11 than the third hole transport sublayer 1423.

[0097] The electronic functional layer 15 includes a first electronic functional sublayer 151 and a second electronic functional sublayer 152 that are stacked. The first electronic functional sublayer 151 is closer to the light emitting layer 13 than the second electronic functional sublayer 152 .

[0098] The materials and thicknesses of the various layers in the light emitting device 1 are:

[0099] The substrate 10 is made of glass and has a thickness of 3 mm.

[0100] The material of the anode 11 is ITO with a thickness of 10 nm;

[0101] The cathode 12 is made of Al and has a thickness of 20 nm;

[0102] The material of the light-emitting layer 13 is a core-shell structure quantum dot of ZnCdSe (core) / ZnCdSe (inner shell) / ZnS (first intermediate shell) / ZnCdS (second intermediate shell) / ZnS (outer shell). 5 mmol of oleic acid ligands are connected to the surface of each 1 mg of quantum dots. The average particle size of the quantum dots is 7 nm, the emission wavelength is 471 nm and the half-peak width is 19 nm. The emission color is blue, and the thickness of the light-emitting layer 13 is 60 nm.

[0103] The materials and thicknesses of the various layers in the hole functional layer 14 are:

[0104] The material of the first hole injection sublayer 1411 includes PEDOT:PSS and Al carbon quantum dots with an average particle size of 30 nm, wherein the mass ratio of Al carbon quantum dots:PEDOT:PSS is 0.025:1, and the thickness of the first hole injection sublayer 1411 is 20 nm;

[0105] The material of the second hole injection sublayer 1412 includes PEDOT:PSS and A2 carbon quantum dots with an average particle size of 20 nm, the mass ratio of A2 carbon quantum dots:PEDOT:PSS is 0.025:1, and the thickness of the second hole injection sublayer 1412 is 20 nm;

[0106] The third hole injection layer 1413 includes PEDOT:PSS and A3 carbon quantum dots with an average particle size of 10 nm. The mass ratio of A3 carbon quantum dots to PEDOT:PSS is 0.025:1. The thickness of the third hole injection layer 1413 is 15 nm.

[0107] The material of the first hole transport sublayer 1421 includes TFB and B1 carbon quantum dots with an average particle size of 10 nm, the mass ratio of B1 carbon quantum dots to TFB is 1:1, and the thickness of the first hole transport sublayer 1421 is 15 nm;

[0108] The material of the second hole transport sublayer 1422 includes TFB and B2 carbon quantum dots with an average particle size of 5 nm, the mass ratio of B2 carbon quantum dots to TFB is 1:1, and the thickness of the second hole transport sublayer 1422 is 20 nm;

[0109] The material of the third hole transport sublayer 1423 includes TFB and B3 carbon quantum dots with an average particle size of 1 nm, the mass ratio of B3 carbon quantum dots to TFB is 1:1, and the thickness of the third hole transport sublayer 1423 is 20 nm;

[0110] The materials and thicknesses of the various layers in the electronic functional layer 15 are:

[0111] The material of the first electronic functional sublayer 151 is nano ZnO (average particle size is 5 nm), and the thickness of the first electronic functional sublayer 151 is 40 nm;

[0112] The material of the second electronic functional sublayer 152 is a mixture of nano ZnO (average particle size of 5 nm) and second carbon quantum dots (average particle size of 5 nm). The thickness of the second electronic functional sublayer 152 is 10 nm, and the mass ratio of nano ZnO (average particle size of 5 nm): second carbon quantum dots is 1:0.5.

[0113] The method for preparing the light-emitting device in this embodiment includes the following steps:

[0114] S1.1. Providing a substrate, vapor-depositing ITO on one side of the substrate to obtain an ITO layer, then ultrasonically cleaning the ITO-containing substrate with acetone for 15 minutes, ultrasonically cleaning with a detergent for 15 minutes, ultrasonically cleaning with deionized water for 15 minutes, and ultrasonically cleaning with isopropyl alcohol for 15 minutes, drying, and surface treating with UV-ozone for 20 minutes to obtain a substrate containing an anode;

[0115] S1.2. Dispersing Al carbon quantum dots having an average particle size of 30 nm in a PEDOT:PSS aqueous solution to obtain a first mixed solution, wherein the concentration of PEDOT:PSS in the first mixed solution is 20 mg / mL and the concentration of Al carbon quantum dots is 0.5 mg / mL. Then, under normal temperature and pressure, the first mixed solution is spin-coated on the side of the anode away from the substrate, followed by a constant temperature heat treatment at 120°C to cure the film, thereby obtaining a first hole injection sublayer.

[0116] S1.3. Dispersing A2 carbon quantum dots having an average particle size of 20 nm in a PEDOT:PSS aqueous solution to obtain a second mixed solution, wherein the concentration of PEDOT:PSS in the second mixed solution is 20 mg / mL and the concentration of the A2 carbon quantum dots is 0.5 mg / mL. Then, under normal temperature and pressure, the second mixed solution is spin-coated on a side of the first hole injection sublayer away from the anode, followed by a constant temperature heat treatment at 120° C. to cure the film, thereby obtaining a second hole injection sublayer.

[0117] S1.4. Dispersing A3 carbon quantum dots having an average particle size of 10 nm in a PEDOT:PSS aqueous solution to obtain a third mixed solution, wherein the concentration of PEDOT:PSS in the third mixed solution is 20 mg / mL and the concentration of the A3 carbon quantum dots is 0.5 mg / mL. Then, under normal temperature and pressure, spin-coating the third mixed solution on a side of the second hole injection sublayer away from the first hole injection sublayer, followed by heat treatment at 120° C. to cure the mixed solution into a film, thereby obtaining a third hole injection sublayer.

[0118] S1.5. Dispersing B1 carbon quantum dots with an average particle size of 10 nm in a TFB-chloroform solution to obtain a fourth mixed solution, wherein the concentration of TFB in the fourth mixed solution is 4 mg / mL and the concentration of the B1 carbon quantum dots is 4 mg / mL. Then, under a nitrogen environment at room temperature and pressure, the fourth mixed solution is spin-coated on the side of the third hole injection sublayer away from the second hole injection sublayer. The mixture is then heat-treated at 120°C to solidify the film, thereby obtaining a first hole transport sublayer.

[0119] S1.6. Dispersing B2 carbon quantum dots with an average particle size of 5 nm in a TFB-chloroform solution to obtain a fifth mixed solution, wherein the concentration of TFB in the fifth mixed solution is 4 mg / mL and the concentration of the B2 carbon quantum dots is 4 mg / mL. Then, under a nitrogen environment at room temperature and pressure, the fifth mixed solution is spin-coated on the side of the first hole transport sublayer away from the third hole injection sublayer. The mixture is then heat-treated at 120°C to cure the film, thereby obtaining a second hole transport sublayer.

[0120] S1.7. Dispersing B3 carbon quantum dots with an average particle size of 1 nm in a TFB-chloroform solution to obtain a fifth mixed solution, wherein the concentration of TFB in the fifth mixed solution is 4 mg / mL and the concentration of the B3 carbon quantum dots is 4 mg / mL. Then, under a nitrogen environment at room temperature and pressure, the sixth mixed solution is spin-coated on the side of the second hole transport sublayer away from the first hole transport sublayer. The mixture is then heat-treated at 120°C to cure the film, thereby obtaining a third hole transport sublayer.

[0121] S1.8. Under a nitrogen environment at room temperature and pressure, spin-coat a 30 mg / mL ZnCdSe / ZnCdSe / ZnS / ZnCdS / ZnS quantum dot-n-octane solution on the side of the third hole transport sublayer away from the light-emitting layer, followed by heat treatment at 100°C to cure the film and obtain a light-emitting layer.

[0122] S1.9. Under a nitrogen atmosphere at room temperature and pressure, spin-coat a 30 mg / mL nano-ZnO-ethanol solution on the side of the light-emitting layer away from the third hole transport sublayer. Heat-treat the solution at 80°C to cure the film, thereby forming the first electronic functional sublayer.

[0123] S1.10. Dispersing the second carbon quantum dots in a nano-ZnO-ethanol solution to obtain a sixth mixed solution, wherein the concentration of the second carbon quantum dots is 10 mg / mL and the concentration of the nano-ZnO is 20 mg / mL. Then, under a nitrogen environment at room temperature and pressure, the sixth mixed solution is spin-coated on a side of the first electronic functional sublayer away from the light-emitting layer. The mixture is then heat-treated at 80°C to cure the mixture into a film, thereby obtaining a second electronic functional sublayer.

[0124] S1.11, vacuum degree not higher than 3×10 -4 Pa vacuum environment, Al was thermally evaporated on the side of the second electronic functional sublayer away from the first electronic functional sublayer at a rate of 1 angstrom / second for 800 seconds to obtain a cathode, which was then encapsulated with UV-curable adhesive to obtain a light-emitting device.

[0125] Example 2

[0126] This embodiment provides a light-emitting device and a preparation method thereof. Compared with the light-emitting device in Example 1, the light-emitting device in this embodiment is different only in that the material of the second electronic functional sublayer is replaced with "second carbon quantum dots (average particle size of 5 nm)".

[0127] Compared with the preparation method of the light-emitting device in Example 1, the difference of the preparation method of the light-emitting device in this embodiment is that: step S1.10 is replaced by "under a nitrogen environment at room temperature and normal pressure, spin-coat a second carbon quantum dot-ethanol solution with a concentration of 30 mg / mL on the side of the first electronic functional sublayer away from the light-emitting layer, and then place it at 80°C for constant temperature heat treatment to solidify into a film to obtain the second electronic functional sublayer."

[0128] Example 3

[0129] This embodiment provides a light-emitting device and a preparation method thereof. Compared with the light-emitting device in Example 1, the difference of the light-emitting device in this embodiment is only that: the material of the first electronic functional sublayer is replaced by "second carbon quantum dots (average particle size of 5 nm)", and the thickness of the first electronic functional sublayer is replaced by "10 nm", and the material of the second electronic functional sublayer is replaced by "nano ZnO (average particle size of 5 nm)", and the thickness of the second electronic functional sublayer is replaced by "40 nm".

[0130] Compared with the preparation method of the light-emitting device in Example 1, the difference of the preparation method of the light-emitting device in this embodiment is that: step S1.9 is replaced by "under a nitrogen environment at room temperature and pressure, spin-coating a second carbon quantum dot-ethanol solution with a concentration of 30 mg / mL on the side of the light-emitting layer away from the third hole transport sublayer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain a first electronic functional sublayer", and step S1.10 is replaced by "under a nitrogen environment at room temperature and pressure, spin-coating a nano ZnO-ethanol solution with a concentration of 30 mg / mL on the side of the first electronic functional sublayer away from the light-emitting layer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain a second electronic functional sublayer".

[0131] Example 4

[0132] This embodiment provides a light-emitting device and a preparation method thereof. Compared with the light-emitting device in Example 1, the difference of the light-emitting device in this embodiment is only that: the material of the first electronic functional sublayer is replaced by "a mixture of nano ZnO (average particle size of 5 nm) and second carbon quantum dots (average particle size of 5 nm)", and the thickness of the first electronic functional sublayer is replaced by "10 nm", and the material of the second electronic functional sublayer is replaced by "nano ZnO (average particle size of 5 nm)", and the thickness of the second electronic functional sublayer is replaced by "40 nm".

[0133] Compared with the preparation method of the light-emitting device in Example 1, the difference of the preparation method of the light-emitting device in this embodiment is that: step S1.9 is replaced by "dispersing the second carbon quantum dots in the nano-ZnO-ethanol solution to obtain a sixth mixed liquid, in which the concentration of the second carbon quantum dots is 10 mg / mL, and the concentration of nano-ZnO is 20 mg / mL, and then, under a nitrogen environment at room temperature and pressure, spin-coating the sixth mixed liquid on the side of the first electronic functional sublayer away from the light-emitting layer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain the first electronic functional sublayer", and step S1.10 is replaced by "under a nitrogen environment at room temperature and pressure, spin-coating a nano-ZnO-ethanol solution with a concentration of 30 mg / mL on the side of the first electronic functional sublayer away from the light-emitting layer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain the second electronic functional sublayer".

[0134] Example 5

[0135] This embodiment provides a light-emitting device and a preparation method thereof. Compared with the light-emitting device in Example 1, the light-emitting device in this embodiment is different only in that the material of the first electronic functional sublayer is replaced by "second carbon quantum dots (average particle size of 5 nm)".

[0136] Compared with the preparation method of the light-emitting device in Example 1, the difference of the preparation method of the light-emitting device in this embodiment is that: step S1.9 is replaced by "under a nitrogen environment at room temperature and normal pressure, spin-coating a second carbon quantum dot-ethanol solution with a concentration of 30 mg / mL on the side of the light-emitting layer away from the third hole transport sublayer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain the first electronic functional sublayer."

[0137] Example 6

[0138] This embodiment provides a light-emitting device and a preparation method thereof. Compared with the light-emitting device in Example 1, the difference of the light-emitting device in this embodiment is only that: the material of the first electronic functional sublayer is replaced by "a mixture of nano ZnO (average particle size of 5 nm) and second carbon quantum dots (average particle size of 5 nm)", and the material of the second electronic functional layer is replaced by "second carbon quantum dots (average particle size of 5 nm)".

[0139] Compared with the preparation method of the light-emitting device in Example 1, the difference of the preparation method of the light-emitting device in this embodiment is that: step S1.9 is replaced by "dispersing the second carbon quantum dots in the nano-ZnO-ethanol solution to obtain a sixth mixed liquid, in which the concentration of the second carbon quantum dots is 10 mg / mL, and the concentration of nano-ZnO is 20 mg / mL, and then, under a nitrogen environment at room temperature and pressure, spin-coating the sixth mixed liquid on the side of the first electronic functional sublayer away from the light-emitting layer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain the first electronic functional sublayer", and step S1.10 is replaced by "under a nitrogen environment at room temperature and pressure, spin-coating the second carbon quantum dot-ethanol solution with a concentration of 30 mg / mL on the side of the first electronic functional sublayer away from the light-emitting layer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain the second electronic functional sublayer".

[0140] Example 7

[0141] This embodiment provides a light-emitting device and a preparation method thereof. Compared with the light-emitting device in Example 1, the light-emitting device in this embodiment is different only in that: the electronic functional layer is a single-layer structure, the thickness of the electronic functional layer is 50 nm, and the material of the electronic functional layer is a second carbon quantum dot.

[0142] Compared with the preparation method of the light-emitting device in Example 1, the difference of the preparation method of the light-emitting device in this embodiment is that: step S1.9 is replaced by "under a nitrogen environment at room temperature and normal pressure, spin-coating a second carbon quantum dot-ethanol solution with a concentration of 30 mg / mL on the side of the light-emitting layer away from the third hole transport sublayer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain an electronic functional layer", and step S1.10 is omitted.

[0143] Example 8

[0144] This embodiment provides a light-emitting device and a preparation method thereof. Compared with the light-emitting device in Example 1, the light-emitting device in this embodiment is different only in that: the electronic functional layer is a single-layer structure, the thickness of the electronic functional layer is 50 nm, and the material of the electronic functional layer is a mixture of second carbon quantum dots and nano-ZnO.

[0145] Compared with the preparation method of the light-emitting device in Example 1, the difference of the preparation method of the light-emitting device in this embodiment is that: step S1.9 is replaced by "dispersing the second carbon quantum dots in the nano-ZnO-ethanol solution to obtain a sixth mixed liquid, in which the concentration of the second carbon quantum dots is 10 mg / mL, and the concentration of nano-ZnO is 20 mg / mL, and then under a nitrogen environment at room temperature and pressure, spin-coating the sixth mixed liquid on the side of the light-emitting layer away from the third hole transport sublayer, and then placing it at 80°C for constant temperature heat treatment to solidify into a film to obtain an electronic functional layer", and omitting step S1.10.

[0146] Example 9

[0147] This embodiment provides a light-emitting device and a method for preparing the same. Compared with the light-emitting device in Example 1, the light-emitting device in this embodiment differs only in that: (1) the hole injection layer is a single-layer structure, the material of the hole injection layer is PEDOT:PSS, and the thickness of the hole injection layer is 55 nm; (2) the hole transport layer is a single-layer structure, the material of the hole transport layer is TFB, and the thickness of the hole transport layer is 55 nm.

[0148] Compared with the preparation method of Example 1, the difference of the preparation method of this comparative example is that: step S1.2 is replaced by "under an atmospheric environment at room temperature and normal pressure, spin-coat a PEDOT:PSS aqueous solution (the concentration of PEDOT:PSS is 30 mg / mL) on the side of the anode away from the substrate, and then place it at 120°C for constant temperature heat treatment to solidify into a film to obtain a hole injection layer", and steps S1.3 and S1.4 are omitted, and step S1.5 is replaced by "under a nitrogen environment at room temperature and normal pressure, spin-coat a TFB-chloroform solution (the concentration of TFB is 4 mg / mL) on the side of the hole injection layer away from the anode, and then place it at 120°C for constant temperature heat treatment for 20 minutes to obtain a hole transport layer", and steps S1.6 and S1.7 are omitted.

[0149] Comparative Example

[0150] This comparative example provides a light-emitting device and a preparation method thereof. Compared with the light-emitting device of Example 1, the light-emitting device of this comparative example is different in that: (1) the hole injection layer is a single-layer structure, the material of the hole injection layer is PEDOT:PSS, and the thickness of the hole injection layer is 55 nm; (2) the hole transport layer is a single-layer structure, the material of the hole transport layer is TFB, and the thickness of the hole transport layer is 55 nm; (3) the electronic functional layer is a single-layer structure, the material of the electronic functional layer is nano-ZnO (average particle size of 5 nm), and the thickness of the electronic functional layer is 50 nm.

[0151] Compared with the preparation method of Example 1, the difference of the preparation method of this comparative example is that: step S1.2 is replaced by "under an atmospheric environment at room temperature and pressure, spin-coating a PEDOT:PSS aqueous solution (PEDOT:PSS concentration is 30 mg / mL) on the side of the anode away from the substrate, and then placing it at a constant temperature heat treatment of 120 ° C to solidify it into a film to obtain a hole injection layer", and steps S1.3 and S1.4 are omitted, and step S1.5 is replaced by "under a nitrogen environment at room temperature and pressure, spin-coating a PEDOT:PSS aqueous solution (PEDOT:PSS concentration is 30 mg / mL) on the side of the anode away from the substrate, and then placing it at a constant temperature heat treatment of 120 ° C to solidify it into a film to obtain a hole injection layer". The side of the injection layer away from the anode is spin-coated with a TFB-chloroform solution (the concentration of TFB is 4 mg / mL), and then heat-treated at 120°C for 20 minutes to obtain a hole transport layer", and steps S1.6 and S1.7 are omitted, and step S1.9 is replaced by "under a nitrogen environment at room temperature and pressure, spin-coat a nano-ZnO-ethanol solution with a concentration of 30 mg / mL on the side of the light-emitting layer away from the hole transport layer, and then heat-treated at 80°C to solidify into a film to obtain an electronic functional layer".

[0152] Experimental example

[0153] The performance of the light-emitting devices of Examples 1 to 8 and the comparative example was tested. The voltage, current, brightness, luminescence spectrum and other parameters of each optoelectronic module were obtained by detecting and obtaining key parameters such as external quantum efficiency and power efficiency, and the service life of each of the above-mentioned light-emitting devices was tested using a FPD optical property measurement device (including an Ocean Optics USB2000, a LabView-controlled QE-PRO spectrometer, a Keithley 2400, a high-precision digital source meter Keithley 6485, an optical fiber with an inner diameter of 50 μm, a device test probe and a fixture, various related connecting wires and data cards, an efficiency test cassette and a data acquisition system). Then, key parameters such as the external quantum efficiency and power efficiency were calculated, and the service life of each of the above-mentioned light-emitting devices was tested using a life test equipment.

[0154] The current efficiency test method is: set the luminous area to 2mm×2mm=4mm 2 , intermittently collect the brightness value of the photoelectric device with a driving voltage range of 0V to 8V. The initial voltage value of the brightness is 3V, and the data is collected every 0.2V. The brightness value collected each time is divided by the corresponding current density to obtain the current efficiency of the photoelectric device under the collection conditions, and the maximum current efficiency (CE max ,cd / A).

[0155] The service life test method is as follows: under the drive of constant current (1mA), a 128-channel QLED life test system is used to analyze the electroluminescence lifetime of each light-emitting device, record the time required for each light-emitting device to decay from maximum brightness to 95% (T95, h), and calculate the time required for the brightness of each light-emitting device to decay from 100% to 95% at a brightness of 1000nit (T95@1000nit, h).

[0156] The performance test data of each light emitting device are detailed in Table 1 below:

[0157] Table 1 Performance test results of the light emitting devices of Examples 1 to 8 and the comparative example

[0158] As shown in Table 1, compared with the comprehensive performance of the light-emitting devices in the comparative example, the comprehensive performance of the light-emitting devices in Examples 1 to 9 is better, specifically, the brightness and current efficiency are higher, and the device life is longer. Taking the light-emitting devices in Example 4 and the comparative example as an example, the L max is the L of the light emitting device in the comparative example max 2 times, and the CE of the light-emitting device in Example 4 max is the CE of the light-emitting device in the comparative example max The T95@1000nit of the light-emitting device in Example 4 is 3 times that of the light-emitting device, and the T95@1000nit of the light-emitting device in Example 4 is 12.5 times that of the light-emitting device in the comparative example. It can be seen that: in the light-emitting device, the material of the electronic functional layer includes the second carbon quantum dots, which is beneficial to improving the photoelectric performance and device life of the light-emitting device; further, the material of the hole functional layer includes the first carbon quantum dots, and compared with the average band gap of the first carbon quantum dots in a layer of the hole functional layer close to the anode, the average band gap of the first carbon quantum dots in a layer of the hole functional layer close to the light-emitting layer is wider, which can further improve the photoelectric performance and device life of the light-emitting device.

[0159] From the comprehensive performance of the light-emitting devices in Examples 1 to 8, it can be seen that compared with the electronic functional layer having a single-layer structure and the material of the electronic functional layer containing second carbon quantum dots, the electronic functional layer has a double-layer structure, and the material of one layer in the double-layer structure contains second carbon quantum dots, and the material of the other layer does not contain second carbon quantum dots, which is beneficial to further improve the photoelectric performance and device life of the light-emitting device.

[0160] The above is a detailed introduction to a method for preparing a photoelectric device, a photoelectric device, and an electronic device containing a photoelectric device provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A light emitting device, wherein: include: An anode and a cathode arranged opposite to each other; A light-emitting layer is disposed between the anode and the cathode; The electronic functional layer is disposed between the cathode and the light-emitting layer, and the material of the electronic functional layer includes second carbon quantum dots.

2. The light emitting device according to claim 1, wherein: The electronic functional layer comprises a first electronic functional sublayer and a second electronic functional sublayer which are stacked, the first electronic functional sublayer is closer to the light-emitting layer than the second electronic functional sublayer, the material of the first electronic functional sublayer comprises the second carbon quantum dots and / or the first compound, and the material of the second electronic functional sublayer comprises the second carbon quantum dots and / or the second compound; wherein the first compound and the second compound are independently selected from one or more of zinc oxide, titanium oxide, tin oxide, barium oxide, tantalum oxide, aluminum oxide, zirconium oxide, magnesium zinc oxide, calcium zinc oxide, zirconium zinc oxide, gallium zinc oxide, aluminum zinc oxide, lithium zinc oxide, titanium zinc oxide, yttrium zinc oxide, indium tin oxide and lithium titanium oxide; And / or, the total thickness of the electronic functional layer is 25 nm to 60 nm.

3. The light emitting device according to claim 2, wherein: The average particle size of the first compound is 2 nm to 30 nm, and / or the average particle size of the second compound is 2 nm to 30 nm.

4. The light emitting device according to claim 2 or 3, wherein: The first electronic functional sublayer and the second electronic functional sublayer are any of the following: (a) the material of the first electronic functional sublayer is a mixture of the second carbon quantum dots and the first compound, and the material of the second electronic functional sublayer is the second compound; (b) the material of the first electronic functional sublayer is the second carbon quantum dots, and the material of the second electronic functional sublayer is the second compound; (c) The material of the first electronic functional sublayer is the first compound; the material of the second electronic functional sublayer is the second carbon quantum dots, or the material of the second electronic functional sublayer is a mixture of the second carbon quantum dots and the second compound.

5. The light emitting device according to claim 4, wherein: For case (a), the thickness of the first electronic functional sublayer is 5 nm to 10 nm, and the thickness of the second electronic functional sublayer is 20 nm to 50 nm.

6. The light emitting device according to claim 4, wherein: For case (b), the thickness of the first electronic functional sublayer is 5 nm to 10 nm, and the thickness of the second electronic functional sublayer is 20 nm to 50 nm.

7. The light emitting device according to claim 4, wherein: For case (c), the thickness of the first electronic functional sublayer is 20 nm to 50 nm, and the thickness of the second electronic functional sublayer is 5 nm to 10 nm.

8. The light emitting device according to any one of claims 2 to 7, wherein: When the material of the first electronic functional sublayer is a mixture of the second carbon quantum dots and the first compound, the mass ratio of the first compound to the second carbon quantum dots is 1:(0.01-1); Alternatively, when the material of the second electronic functional sublayer is a mixture of the second carbon quantum dots and the second compound, the mass ratio of the second compound to the second carbon quantum dots is 1:(0.01-1).

9. The light emitting device according to any one of claims 1 to 8, wherein: The light emitting device further comprises a hole functional layer disposed between the anode and the light emitting layer, wherein the material of the hole functional layer comprises a first carbon quantum dot; The first carbon quantum dot layer closest to the light-emitting layer in the hole functional layer is the first sublayer, the average band gap of the first carbon quantum dots in the first sublayer is the first band gap, and the thickness of the first sublayer is the largest particle size of the first carbon quantum dots in the first sublayer; the first carbon quantum dot layer closest to the anode in the hole functional layer is the second sublayer, the average band gap of the first carbon quantum dots in the second sublayer is the second band gap, the thickness of the second sublayer is the largest particle size of the first carbon quantum dots in the second sublayer; the first band gap is wider than the second band gap.

10. The light emitting device according to claim 9, wherein: Along the direction from the anode to the light-emitting layer, the average band gap of the first carbon quantum dots in the hole functional layer gradually widens; and / or Along the direction from the anode to the light-emitting layer, the average particle size of the first carbon quantum dots in the hole functional layer gradually decreases; and / or The particle size distribution range of the first carbon quantum dots in the hole functional layer is 1 nm to 50 nm, and / or the average particle size of the second carbon quantum dots is 1 nm to 50 nm; and / or The material of the hole functional layer further comprises a third compound, and the third compound is selected from poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid), copper phthalocyanine, titanium phthalocyanine, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanodimethyl-p-benzoquinone, 2,3,6,7,10,11-hexycyano-1,4,5,8,9,12-hexaazatriphenylene, 3-hexyl substituted polythiophene, poly(9-vinylcarbazole), 4,4'-bis(9-carbazole)biphenyl, poly[bis(4-phenyl)(4-butylphenyl)amine], 4,4'-cyclohexylbis[N ,N-di(4-methylphenyl)aniline], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)], poly(N,N'-di(4-butylphenyl)-N,N'-diphenyl-1,4-phenylenediamine-co-9,9-dioctylfluorene), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, 4,4',4"-tri( carbazole-9-yl) triphenylamine, 4,4',4'-tri(2-naphthylphenylamino)triphenylamine, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-di(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine, N,N'-bis[4-(diphenylamino)phenyl]-N,N'-diphenylbenzidine, N,N'-bis(3-methylphenyl)-N,N'-diphenyl-9,9-spirobifluorene-2,7-diamine, N2,N7-di-1-naphthyl-N One or more of 2,N7-diphenyl-9,9'-spirobi[9H-fluorene]-2,7-diamine, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, doped or undoped nickel oxide, doped or undoped molybdenum oxide, doped or undoped tungsten oxide, doped or undoped vanadium oxide, doped or undoped P-type gallium nitride, doped or undoped chromium oxide, doped or undoped copper oxide, transition metal sulfide and transition metal selenide.

11. The light emitting device according to claim 10, wherein: When the material of the hole functional layer further includes a third compound, in the hole functional layer, the mass ratio of the third compound to the first carbon quantum dots is 1:(0.01-1).

12. The light emitting device according to any one of claims 1 to 11, wherein: The material of the light-emitting layer comprises one or more of an organic light-emitting material and quantum dots, wherein the organic light-emitting material is selected from one or more of 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing BN covalent bonds, hybrid localized charge transfer excited state materials and exciplex light-emitting materials; and / or The quantum dots are selected from one or more of single component quantum dots, core-shell structure quantum dots, inorganic perovskite quantum dots, organic perovskite quantum dots and organic-inorganic hybrid perovskite quantum dots; and / or The material of the single-component quantum dot, the material of the core of the core-shell structure quantum dot and the material of the shell of the core-shell structure quantum dot are independently selected from at least one of II-VI group compounds, III-V group compounds, IV-VI group compounds or I-III-VI group compounds, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe , HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the III-V group compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, one or more of GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, the IV-VI group compound is selected from one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, the I-III-VI group compound is selected from one or more of CuInS, CuInSe and AgInS; and / or The general structural formula of the inorganic perovskite quantum dot is AMX3, wherein A is Cs + ion, M is a divalent metal cation, M is selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ and Eu 2+ One or more of, X is a halogen anion; and / or The general structural formula of the organic perovskite quantum dots is CMX3, where C is a carboxamidine group; and / or The general structural formula of the organic-inorganic hybrid perovskite quantum dots is BMX3, where B is selected from organic amine cations; and / or The materials of the anode and the cathode are independently selected from one or more of metals, carbon materials and first metal oxides, the metals are selected from one or more of Al, Ag, Cu, Mo, Au, Ba, Pt, Ca and Mg, the carbon materials are selected from one or more of graphite, carbon nanotubes, graphene and carbon fibers, and the second metal oxides are selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide.

13. A method for preparing a light emitting device, wherein: The steps include: providing a bottom electrode, and forming a light emitting layer on one side of the bottom electrode; and forming a top electrode on a side of the light emitting layer away from the bottom electrode; Wherein, when the light-emitting device is of a positive structure, the bottom electrode is an anode and the top electrode is a cathode, before the step of forming a light-emitting layer on one side of the bottom electrode, the method for preparing the light-emitting device further comprises the steps of: forming an electronic functional layer on a side of the light-emitting layer away from the bottom electrode; the top electrode is formed on a side of the electronic functional layer away from the light-emitting layer; Alternatively, when the light-emitting device is an inverted structure, the bottom electrode is a cathode and the top electrode is an anode, before the step of forming a light-emitting layer on one side of the bottom electrode, the method for preparing the light-emitting device further comprises the steps of: forming an electronic functional layer on one side of the bottom electrode; the light-emitting layer is formed on a side of the electronic functional layer away from the bottom electrode; Wherein, the material of the electronic functional layer includes second carbon quantum dots.

14. The method for preparing a light emitting device according to claim 13, wherein: When the light emitting device is of a positive structure, the step of forming the electronic functional layer on the side of the light emitting layer away from the bottom electrode comprises: sequentially forming the first electronic functional sublayer and the second electronic functional sublayer on the side of the light emitting layer away from the bottom electrode; Alternatively, when the light emitting device is an inverted structure, the step of forming the electronic functional layer on one side of the bottom electrode comprises: sequentially forming the second electronic functional sublayer and the first electronic functional sublayer on one side of the bottom electrode; The material of the first electronic functional sublayer comprises the second carbon quantum dots and / or the first compound, and the material of the second electronic functional sublayer comprises the second carbon quantum dots and / or the second compound; the first compound and the second compound are independently selected from one or more of zinc oxide, titanium oxide, tin oxide, barium oxide, tantalum oxide, aluminum oxide, zirconium oxide, magnesium zinc oxide, calcium zinc oxide, zirconium oxide, gallium zinc oxide, aluminum zinc oxide, lithium zinc oxide, titanium zinc oxide, yttrium zinc oxide, indium tin oxide and lithium titanium oxide.

15. The method for preparing a light emitting device according to claim 14, wherein: When the material of the first electronic functional sublayer is a mixture of the second carbon quantum dots and the first compound, the method for forming the first electronic functional sublayer comprises the steps of: depositing a first dispersion containing the second carbon quantum dots and the first compound, and then performing a first drying treatment on the deposited first dispersion to obtain the first electronic functional sublayer; wherein, in the first dispersion, the mass ratio of the first compound to the second carbon quantum dots is 1:(0.01-1); Alternatively, when the material of the second electronic functional sublayer is a mixture of the second carbon quantum dots and the second compound, the method for forming the second electronic functional sublayer comprises the steps of: depositing a mixture containing the second carbon quantum dots and the second compound; A second dispersion of the second compound is prepared, and then the deposited second dispersion is subjected to a second drying process to obtain a second electronic functional sublayer; wherein, in the second dispersion, the mass ratio of the second compound to the second carbon quantum dots is 1:(0.01-1).

16. The method for preparing a light emitting device according to any one of claims 13 to 15, wherein: When the light-emitting device is of an upright structure, before the step of forming the light-emitting layer on one side of the bottom electrode, the method for preparing the light-emitting device further comprises the step of: forming a hole functional layer on one side of the bottom electrode; or, when the light-emitting device is of an inverted structure, before the step of forming the top electrode on the side of the light-emitting layer away from the bottom electrode, the method for preparing the light-emitting device further comprises the step of: forming a hole functional layer on the side of the light-emitting layer away from the bottom electrode; the top electrode is formed on the side of the hole functional layer away from the light-emitting layer; Among them, the first carbon quantum dot layer closest to the light-emitting layer in the hole functional layer is the first sublayer, the average band gap of the first carbon quantum dots in the first sublayer is the first band gap, and the thickness of the first sublayer is the largest particle size of the first carbon quantum dots in the first sublayer; the first carbon quantum dot layer closest to the anode in the hole functional layer is the second sublayer, the average band gap of the first carbon quantum dots in the second sublayer is the second band gap, and the thickness of the second sublayer is the largest particle size of the second carbon quantum dots in the second sublayer; the first band gap is wider than the second band gap.

17. The method for preparing a light emitting device according to claim 16, wherein: Along the direction from the anode to the light-emitting layer, the average band gap of the first carbon quantum dots in the hole functional layer gradually widens; and / or Along the direction from the anode to the light-emitting layer, the average particle size of the first carbon quantum dots in the hole functional layer gradually decreases; and / or The particle size distribution range of the first carbon quantum dots in the hole functional layer is 1 nm to 50 nm, and / or the average particle size of the second carbon quantum dots is 1 nm to 50 nm; and / or The material of the hole functional layer further comprises a third compound, and the third compound is selected from poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid), copper phthalocyanine, titanium phthalocyanine, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanodimethyl-p-benzoquinone, 2,3,6,7,10,11-hexycyano-1,4,5,8,9,12-hexaazatriphenylene, 3-hexyl substituted polythiophene, poly(9-vinylcarbazole), 4,4'-bis(9-carbazole)biphenyl, poly[bis(4-phenyl)(4-butylphenyl)amine], 4,4'-cyclohexylbis[N ,N-di(4-methylphenyl)aniline], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)], poly(N,N'-di(4-butylphenyl)-N,N'-diphenyl-1,4-phenylenediamine-co-9,9-dioctylfluorene), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, 4,4',4"-tri( carbazole-9-yl) triphenylamine, 4,4',4'-tri(2-naphthylphenylamino)triphenylamine, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-di(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine, N,N'-bis[4-(diphenylamino)phenyl]-N,N'-diphenylbenzidine, N,N'-bis(3-methylphenyl)-N,N'-diphenyl-9,9-spirobifluorene-2,7-diamine, N2,N7-di-1-naphthyl-N One or more of 2,N7-diphenyl-9,9'-spirobi[9H-fluorene]-2,7-diamine, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, doped or undoped nickel oxide, doped or undoped molybdenum oxide, doped or undoped tungsten oxide, doped or undoped vanadium oxide, doped or undoped P-type gallium nitride, doped or undoped chromium oxide, doped or undoped copper oxide, transition metal sulfide and transition metal selenide.

18. The method for preparing a light emitting device according to claim 17, wherein: When the material of the hole functional layer further includes a third compound, in the hole functional layer, the mass ratio of the third compound to the first carbon quantum dots is 1:(0.01-1).

19. A display device, wherein: The display device includes a light emitting device, and the light emitting device includes: An anode and a cathode arranged opposite to each other; A light-emitting layer is disposed between the anode and the cathode; The electronic functional layer is disposed between the cathode and the light-emitting layer, and the material of the electronic functional layer includes second carbon quantum dots.

20. The display device according to claim 19, wherein: The electronic functional layer comprises a first electronic functional sublayer and a second electronic functional sublayer which are stacked, the first electronic functional sublayer is closer to the light-emitting layer than the second electronic functional sublayer, the material of the first electronic functional sublayer comprises the second carbon quantum dots and / or the first compound, and the material of the second electronic functional sublayer comprises the second carbon quantum dots and / or the second compound; wherein the first compound and the second compound are independently selected from one or more of zinc oxide, titanium oxide, tin oxide, barium oxide, tantalum oxide, aluminum oxide, zirconium oxide, magnesium zinc oxide, calcium zinc oxide, zirconium zinc oxide, gallium zinc oxide, aluminum zinc oxide, lithium zinc oxide, titanium zinc oxide, yttrium zinc oxide, indium tin oxide and lithium titanium oxide; And / or, the total thickness of the electronic functional layer is 25 nm to 60 nm.

Citation Information

Patent Citations

  • Quantum dot light-emitting diode and preparation method thereof

    CN111490169A

  • Quantum dot light-emitting diode and preparation method thereof

    CN111490170A

  • Electroluminescent device and display device

    CN111883678A

  • Quantum dot light-emitting diode and preparation method thereof

    CN113130824A

  • Quantum dots based light emitting device and method of manufacturing the same

    KR1020180035278A

Cited By

  • Compact and ordered cadmium selenide quantum well film and method for preparing electroluminescent diode

    CN119486549A