Duplex stainless steel material
The duplex stainless steel material with a tailored chemical composition and microstructure addresses the inadequate corrosion resistance in supercritical environments by enhancing both general and pitting corrosion resistance, ensuring effective performance in aggressive industrial conditions.
Patent Information
- Application Number
- PCT/JP2024/010074
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-17
AI Technical Summary
Current duplex stainless steel materials lack sufficient general and pitting corrosion resistance in supercritical corrosion environments, which are characterized by high temperatures, high pressures, and the presence of CO2, SOx, and O2, leading to aggressive corrosive conditions.
A duplex stainless steel material with a specific chemical composition, including C: 0.050% or less, Si: 1.00% or less, Mn: 0.40-3.00%, P: 0.050% or less, Cr: 20.00-24.50%, Cu: 0.10-3.00%, Ni: 2.00-10.00%, Mo: 0.80-5.00%, W: 0.01-1.50%, N: 0.001-0.350%, Co: 0.10-1.00%, Sn: 0.001-0.050%, and controlled microstructure, is developed to enhance corrosion resistance. The material has a microstructure consisting of ferrite and austenite with a reduced number density of coarse Mn and Ca sulfides, and specific inclusions are unevenly distributed to prevent selective pitting corrosion.
The proposed duplex stainless steel material demonstrates excellent general and pitting corrosion resistance in supercritical corrosion environments, with a corrosion rate of 0.100 mm/year or less and no pitting corrosion observed, thereby extending its lifespan and performance in harsh industrial conditions.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Duplex stainless steel material
[0001] The present disclosure relates to steel products, and more particularly to duplex stainless steel products.
[0002] Currently, carbon dioxide (CO 2 The rise in CO 2 Efforts to reduce CO emissions are underway. 2 Among efforts to curb CO2 emissions, CCUS is attracting particular attention.
[0003] CCUS is an abbreviation for Carbon dioxide Capture, Utilization and Storage. 2 It includes three technologies: CO capture, utilization, and storage. 2 CO2 emitted from industrial facilities such as power plants and factories is stored as a technology. 2 and CO2 2 Technology to inject and store gas has been attracting attention.
[0004] Such CO 2 The steel used in the storage technology is 2 High strength is required to press in the CO 2 is a corrosive substance that corrodes steel. 2 The steel used in CO storage technology 2 Excellent corrosion resistance is required in corrosive environments containing a large amount of zinc.
[0005] Duplex stainless steel materials having a two-phase structure of ferrite and austenite are known as steel materials with excellent corrosion resistance in corrosive environments. Duplex stainless steel materials are disclosed, for example, in Japanese Patent Laid-Open Nos. 5-132741 (Patent Document 1) and 9-195003 (Patent Document 2).
[0006] The duplex stainless steel material disclosed in Patent Document 1 has a chemical composition, in mass%, of C: 0.03% or less, Si: 1.0% or less, Mn: 1.5% or less, P: 0.040% or less, S: 0.008% or less, sol. Al: 0.040% or less, Ni: 5.0 to 9.0%, Cr: 23.0 to 27.0%, Mo: 2.0 to 4.0%, W: more than 1.5 to 5.0%, N: 0.24 to 0.32%, with the balance being Fe and unavoidable impurities, and PREW (= Cr + 3.3 (Mo + 0.5W) + 16N) is 40 or more.
[0007] The duplex stainless steel material disclosed in Patent Document 2 contains, by mass%, C: 0.12% or less, Si: 1% or less, Mn: 2% or less, Ni: 3 to 12%, Cr: 20 to 35%, Mo: 0.5 to 10%, W: over 3 to 8%, Co: 0.01 to 2%, Cu: 0.1 to 5%, N: 0.05 to 0.5%, and the balance being Fe and unavoidable impurities.
[0008] In the duplex stainless steel materials disclosed in Patent Documents 1 and 2, the corrosion resistance is improved by adjusting the chemical composition.
[0009] JP-A-5-132741 JP-A-9-195003
[0010] By the way, the carbon dioxide storage technology mentioned above involves storing CO in depleted oil wells. 2 In order to inject CO into the steel pipe 2 is compressed and pressurized to produce CO 2 On the other hand, CO recovered from industrial facilities such as power plants and factories is 2 SOx and O 2 Here, SOx is SO 2 SOx is a general term for sulfur oxides, such as sulfur dioxide, sulfur dioxide, and sulfur dioxide. SOx dissolves in water to form acidic compounds (sulfuric acid, sulfurous acid, etc.), which cause general corrosion on the surface of steel. 2 Therefore, SOx and O 2 Supercritical CO containing 2 In this specification, SOx and O 2 Supercritical CO containing 2 The corrosive environment formed by this is called a "supercritical corrosive environment."
[0011] In other words, steel materials used in supercritical corrosion environments are required to have better general corrosion resistance and pitting corrosion resistance than those in conventional corrosive environments. The duplex stainless steel materials disclosed in Patent Documents 1 and 2 are not intended for use in such supercritical corrosion environments.
[0012] An object of the present disclosure is to provide a duplex stainless steel material that has excellent general corrosion resistance and pitting corrosion resistance even in supercritical corrosion environments.
[0013] The duplex stainless steel material according to the present disclosure has, in mass %, C: 0.050% or less, Si: 1.00% or less, Mn: 0.40 to 3.00%, P: 0.050% or less, S: 0.0050% or less, Cr: 20.00 to 24.50%, Cu: 0.10 to 3.00%, Ni: 2.00 to 10.00%, Mo: 0.80 to 5.00%, W: 0.01 to 1.50%, N: 0.001 to 0.350%, Co: 0.10 to 1.00%, Sn: 0.001 to 0.050%, sol. Al: 0.050% or less, V: 0.01 to 0.50%, Ti: 0.001 to 0.050%, Ca: 0.0005 to 0.0100%, B: 0.0015 to 0.0050%, O: 0.010% or less, Mg: 0 to 0.010%, rare earth elements: 0 to 0.010%, Zr: 0 to 0.010%, Nb: 0 to 0.500%, Ta: 0 to 0.100%, As: 0 to 0.050%, Zn: 0 to 0.010%, Pb: 0 to 0.010%, Sb: 0 to 0.010%, and the balance being Fe and impurities, on the assumption that the content of each of the elements is within the above-mentioned range. Fn1 defined by formula (1) is 40.0 or more, and in the duplex stainless steel material, when particles having an equivalent circle diameter of 1.0 μm or more, a Mn content of 10 mass% or more, and an S content of 10 mass% or more are defined as coarse Mn sulfides, and particles having an equivalent circle diameter of 2.0 μm or more, a Ca content of 20 mass% or more, an S content of 10 mass% or more, and an Mn content of less than 10 mass% are defined as coarse Ca sulfides, the total number density of the coarse Mn sulfides and the coarse Ca sulfides is 0.50 particles / mm2 the microstructure of the duplex stainless steel material is composed of ferrite and austenite, and the total number density of the coarse Mn sulfides and the coarse Ca sulfides in the ferrite is NDA particles / mm 2 The total number density of the coarse Mn sulfides and the coarse Ca sulfides in the austenite is defined as NDG pieces / mm 2 When the formula (2) is defined as follows, the NDA and the NDG satisfy the formula (2): Fn1=Cr+3.3(Mo+0.5W)+16N+2Ni+Cu+2Co+10Sn (1) NDA / NDG<0.50 (2) Here, the element symbols in the formula (1) are substituted with the contents of the corresponding elements in mass%.
[0014] The duplex stainless steel material according to the present disclosure has excellent general corrosion resistance and pitting corrosion resistance even in supercritical corrosion environments.
[0015] The inventors have investigated the relationship between SOx and O 2 Supercritical CO containing 2 We investigated duplex stainless steel materials that have excellent resistance to general corrosion and pitting corrosion in the supercritical corrosion environment formed by the above.
[0016] The present inventors first investigated a steel material having excellent general corrosion resistance and excellent pitting corrosion resistance in a supercritical corrosion environment from the viewpoint of chemical composition, and as a result, the steel material contained, in mass%, 0.050% or less of C, 1.00% or less of Si, 0.40 to 3.00% of Mn, 0.050% or less of P, 0.0050% or less of S, 20.00 to 24.50% of Cr, 0.10 to 3.00% of Cu, 2.00 to 10.00% of Ni, 0.80 to 5.00% of Mo, 0.01 to 1.50% of W, 0.001 to 0.350% of N, 0.10 to 1.00% of Co, 0.001 to 0.050% of Sn, and sol. It was considered that a steel material having a chemical composition consisting of Al: 0.050% or less, V: 0.01 to 0.50%, Ti: 0.001 to 0.050%, Ca: 0.0005 to 0.0100%, B: 0.0015 to 0.0050%, O: 0.010% or less, Mg: 0 to 0.010%, rare earth elements: 0 to 0.010%, Zr: 0 to 0.010%, Nb: 0 to 0.500%, Ta: 0 to 0.100%, As: 0 to 0.050%, Zn: 0 to 0.010%, Pb: 0 to 0.010%, Sb: 0 to 0.010%, and the balance being Fe and impurities, could potentially provide excellent general corrosion resistance and excellent pitting corrosion resistance in a supercritical corrosion environment.
[0017] On the other hand, even duplex stainless steel materials having the above-mentioned chemical composition sometimes fail to provide sufficient general corrosion resistance in supercritical corrosion environments. Therefore, the present inventors further investigated means for improving general corrosion resistance in supercritical corrosion environments.
[0018] Specifically, the inventors focused on the effects of each element in the chemical composition. It has been known that, among the elements contained in the above-mentioned chemical composition, Cr, Mo, W, and N enhance general corrosion resistance in normal corrosive environments containing chlorides, such as seawater. Therefore, the inventors considered that these elements may also enhance general corrosion resistance in supercritical corrosion environments. The inventors further investigated elements other than Cr, Mo, W, and N that enhance general corrosion resistance in supercritical corrosion environments. As a result, it was revealed that, in supercritical corrosion environments, not only Cr, Mo, W, and N, but also Ni, Cu, Co, and Sn enhance the general corrosion resistance of duplex stainless steel materials.
[0019] Therefore, the inventors further investigated the relationship between the contents of Cr, Mo, W, N, Ni, Cu, Co, and Sn in duplex stainless steel materials and general corrosion resistance in supercritical corrosion environments. As a result, it was found that for duplex stainless steel materials having the above chemical composition, if Fn1, defined by formula (1), is 40.0 or more, general corrosion resistance in supercritical corrosion environments can be improved. Fn1 = Cr + 3.3(Mo + 0.5W) + 16N + 2Ni + Cu + 2Co + 10Sn (1) Here, the element symbols in formula (1) are substituted with the contents of the corresponding elements in mass%.
[0020] On the other hand, even in duplex stainless steel materials having the above-mentioned chemical composition and satisfying Fn1 of 40.0 or more, there are cases in which excellent pitting corrosion resistance is not sufficiently obtained in supercritical corrosion environments. Therefore, the present inventors further investigated means for improving pitting corrosion resistance in supercritical corrosion environments.
[0021] As mentioned above, the supercritical corrosion environment includes high-temperature and high-pressure supercritical CO 2 Not only gas, but also SOx gas and O 2 SOx gas and O gas in supercritical corrosive environments are also included. 2 Gases dissolve easily in water, making the environment more acidic. Therefore, in such supercritical corrosion environments, if inclusions exist on the surface of duplex stainless steel, they tend to dissolve. When the inclusions dissolve, pits form on the surface. Furthermore, pits formed by the dissolution of large inclusions tend to become the starting point for pitting corrosion in supercritical corrosion environments.
[0022] Further investigations by the present inventors revealed that in a supercritical corrosion environment, not all of the coarse inclusions (oxides, sulfides, nitrides, etc.) present in the surface layer of a duplex stainless steel material become the initiation points of pitting corrosion, but rather coarse Mn sulfides and coarse Ca sulfides dissolve to form pits on the steel surface. In other words, if the number density of coarse Mn sulfides and coarse Ca sulfides can be reduced, it may be possible to improve the pitting corrosion resistance of a duplex stainless steel material having the above-mentioned chemical composition.
[0023] Specifically, the inventors focused on Mn sulfides having an equivalent circle diameter of 1.0 μm or more and Ca sulfides having an equivalent circle diameter of 2.0 μm or more. Hereinafter, in this specification, particles having a Mn content of 10 mass% or more and an S content of 10 mass% or more will also be referred to as Mn sulfides. Similarly, in this specification, particles having a Ca content of 20 mass% or more, an S content of 10 mass% or more, and an Mn content of less than 10 mass% will also be referred to as Ca sulfides. Furthermore, in this specification, Mn sulfides having an equivalent circle diameter of 1.0 μm or more will also be referred to as "coarse Mn sulfides." Similarly, in this specification, Ca sulfides having an equivalent circle diameter of 2.0 μm or more will also be referred to as "coarse Ca sulfides." In this specification, coarse Mn sulfides and coarse Ca sulfides will also be collectively referred to as "specific inclusions."
[0024] The present inventors considered that if the formation of large coarse Mn sulfides as well as large coarse Ca sulfides could be suppressed, the pitting corrosion resistance of duplex stainless steel materials having the above-mentioned chemical composition could be improved. Specifically, when the total number density of specific inclusions (coarse Mn sulfides and coarse Ca sulfides) is 0.50 pieces / mm 2 It was thought that if the chemical composition of the duplex stainless steel material described above is as follows, excellent pitting corrosion resistance can be obtained.
[0025] On the other hand, the above-mentioned chemical composition is satisfied, Fn1 is 40.0 or less, and the total number density of specific inclusions is 0.50 pieces / mm 2 Even when the pitting corrosion resistance is less than 100%, there are cases where excellent pitting corrosion resistance is not obtained. Therefore, the present inventors conducted a detailed investigation into cases where excellent pitting corrosion resistance is not obtained and studied means for improving pitting corrosion resistance. As a result, it was found that when excellent pitting corrosion resistance is not obtained, pitting corrosion is likely to occur in the ferrite of the microstructure of the duplex stainless steel material.
[0026] Here, a duplex stainless steel material having the above-described chemical composition has a microstructure consisting of ferrite and austenite. In this specification, "consisting of ferrite and austenite" means that phases other than ferrite and austenite are negligibly small. Furthermore, austenite has superior corrosion resistance to ferrite. Therefore, in a duplex stainless steel material having the above-described chemical composition, there is a concern that pitting corrosion may occur selectively in the ferrite. Therefore, the present inventors believed that if specific inclusions in a duplex stainless steel material could be concentrated in the austenite, it might be possible to suppress the occurrence of selective pitting corrosion in the ferrite.
[0027] As a result of detailed studies by the present inventors based on the above findings, it was found that the above chemical composition is satisfied, Fn1 is set to 40.0 or less, and the total number density of specific inclusions is set to 0.50 pieces / mm 2 After reducing the total number density NDA (number / mm 2 ) and the total number density NDG (number / mm 2 It has been revealed that if NDA / NDG<0.50 (2) satisfies the formula (2), excellent general corrosion resistance and pitting corrosion resistance can be obtained even in a supercritical corrosion environment.
[0028] Fn2 is defined as NDA / NDG. Fn2 is an index showing the extent to which specific inclusions (coarse Mn sulfides and coarse Ca sulfides) are present in ferrite. If Fn2 is less than 0.50, the number density of specific inclusions in ferrite can be sufficiently reduced. As a result, the occurrence of selective pitting corrosion in ferrite can be suppressed, provided that the other configurations of this embodiment are satisfied. On the other hand, if Fn2 is 0.50 or more, the ferrite contains a large number of specific inclusions, which may result in selective pitting corrosion.
[0029] Therefore, the duplex stainless steel material according to this embodiment has the above-mentioned chemical composition, Fn1 is 40.0 or more, and the total number density of specific inclusions is 0.50 pieces / mm 2or less, and Fn2 is set to be less than 0.50. As a result, the duplex stainless steel material according to this embodiment has excellent general corrosion resistance and pitting corrosion resistance even in a supercritical corrosion environment.
[0030] The duplex stainless steel material according to this embodiment, which was completed based on the above findings, has the following features.
[0031] [1] A duplex stainless steel material comprising, in mass%, C: 0.050% or less, Si: 1.00% or less, Mn: 0.40 to 3.00%, P: 0.050% or less, S: 0.0050% or less, Cr: 20.00 to 24.50%, Cu: 0.10 to 3.00%, Ni: 2.00 to 10.00%, Mo: 0.80 to 5.00%, W: 0.01 to 1.50%, N: 0.001 to 0.350%, Co: 0.10 to 1.00%, Sn: 0.001 to 0.050%, sol. Al: 0.050% or less, V: 0.01 to 0.50%, Ti: 0.001 to 0.050%, Ca: 0.0005 to 0.0100%, B: 0.0015 to 0.0050%, O: 0.010% or less, Mg: 0 to 0.010%, rare earth elements: 0 to 0.010%, Zr: 0 to 0.010%, Nb: 0 to 0.500%, Ta: 0 to 0.100%, As: 0 to 0.050%, Zn: 0 to 0.010%, Pb: 0 to 0.010%, Sb: 0 to 0.010%, and the balance being Fe and impurities, on the assumption that the content of each of the elements is within the above-mentioned range. Fn1 defined by formula (1) is 40.0 or more, and in the duplex stainless steel material, when particles having an equivalent circle diameter of 1.0 μm or more, a Mn content of 10 mass% or more, and an S content of 10 mass% or more are defined as coarse Mn sulfides, and particles having an equivalent circle diameter of 2.0 μm or more, a Ca content of 20 mass% or more, an S content of 10 mass% or more, and an Mn content of less than 10 mass% are defined as coarse Ca sulfides, the total number density of the coarse Mn sulfides and the coarse Ca sulfides is 0.50 particles / mm 2the microstructure of the duplex stainless steel material is composed of ferrite and austenite, and the total number density of the coarse Mn sulfides and the coarse Ca sulfides in the ferrite is NDA particles / mm 2 The total number density of the coarse Mn sulfides and the coarse Ca sulfides in the austenite is defined as NDG pieces / mm 2 A duplex stainless steel material, wherein the NDA and the NDG satisfy the following formula (2): Fn1=Cr+3.3(Mo+0.5W)+16N+2Ni+Cu+2Co+10Sn (1) NDA / NDG<0.50 (2) where the element symbols in formula (1) are substituted with the contents of the corresponding elements in mass%.
[0032] [2] The duplex stainless steel material according to [1], containing one or more elements selected from the group consisting of Mg: 0.001 to 0.010%, rare earth elements: 0.001 to 0.010%, Zr: 0.001 to 0.010%, Nb: 0.001 to 0.500%, Ta: 0.001 to 0.100%, As: 0.001 to 0.050%, Zn: 0.001 to 0.010%, Pb: 0.001 to 0.010%, and Sb: 0.001 to 0.010%.
[0033] [3] The duplex stainless steel material according to [1] or [2], wherein the duplex stainless steel material is a steel pipe.
[0034] The shape of the duplex stainless steel material according to this embodiment is not particularly limited. The duplex stainless steel material according to this embodiment may be a steel pipe, a round bar (solid material), or a steel plate. The round bar refers to a steel bar having a circular cross section perpendicular to the axial direction. The steel pipe may be a seamless steel pipe or a welded steel pipe.
[0035] The duplex stainless steel material according to this embodiment will be described in detail below.
[0036] [Chemical Composition] The chemical composition of the duplex stainless steel material according to this embodiment contains the following elements: "%" relating to elements means mass % unless otherwise specified.
[0037] C: 0.050% or less Carbon (C) is unavoidably contained. That is, the lower limit of the C content is greater than 0%. C forms Cr carbides at grain boundaries, increasing the corrosion susceptibility at the grain boundaries. Therefore, if the C content is too high, the corrosion resistance of the steel material will decrease even if the contents of other elements are within the ranges of this embodiment. Therefore, the C content is 0.050% or less. A preferred upper limit of the C content is 0.048%, more preferably 0.045%. The C content is preferably as low as possible. However, an extreme reduction in the C content significantly increases manufacturing costs. Therefore, considering industrial production, a preferred lower limit of the C content is 0.001%, more preferably 0.003%, and even more preferably 0.005%.
[0038] Si: 1.00% or less Silicon (Si) is unavoidably contained. That is, the lower limit of the Si content is more than 0%. Si deoxidizes steel. On the other hand, if the Si content is too high, the toughness of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Si content is 1.00% or less. A preferred upper limit of the Si content is 0.90%, more preferably 0.80%, and even more preferably 0.70%. To more effectively obtain the above effects, a preferred lower limit of the Si content is 0.01%, more preferably 0.05%, even more preferably 0.10%, and even more preferably 0.20%.
[0039] Mn: 0.40 to 3.00% Manganese (Mn) deoxidizes and desulfurizes steel. Mn also improves the hot workability of steel. If the Mn content is too low, the above effects cannot be fully achieved even if the contents of other elements are within the ranges of this embodiment. On the other hand, Mn combines with sulfur (S) to form Mn sulfides. Therefore, if the Mn content is too high, even if the contents of other elements are within the ranges of this embodiment, a large number of coarse Mn sulfides are formed, reducing the pitting corrosion resistance of the steel in a supercritical corrosion environment. Therefore, the Mn content is 0.40 to 3.00%. A preferred lower limit of the Mn content is 0.50%, more preferably 0.60%. A preferred upper limit of the Mn content is 2.90%, more preferably 2.70%.
[0040] P: 0.050% or less Phosphorus (P) is unavoidably contained. That is, the lower limit of the P content is greater than 0%. P segregates at grain boundaries. Therefore, if the P content is too high, the corrosion resistance of the steel material will decrease even if the contents of other elements are within the ranges of this embodiment. Therefore, the P content is 0.050% or less. A preferred upper limit of the P content is 0.045%, more preferably 0.040%, and even more preferably 0.030%. The P content should be as low as possible. However, an extreme reduction in the P content significantly increases manufacturing costs. Therefore, considering industrial production, a preferred lower limit of the P content is 0.001%, more preferably 0.003%.
[0041] S: 0.0050% or less Sulfur (S) is unavoidably contained. That is, the lower limit of the S content is greater than 0%. S segregates at grain boundaries. Therefore, if the S content is too high, the corrosion resistance of the steel material will decrease even if the contents of other elements are within the ranges of this embodiment. Therefore, the S content is 0.0050% or less. A preferred upper limit of the S content is 0.0040%, more preferably 0.0030%, and even more preferably 0.0020%. The S content should be as low as possible. However, an extreme reduction in the S content significantly increases manufacturing costs. Therefore, considering industrial production, a preferred lower limit of the S content is 0.0001%, more preferably 0.0003%, and even more preferably 0.0005%.
[0042] Cr: 20.00 to 24.50% Chromium (Cr) forms a passive film as an oxide on the surface of a steel material, improving the general corrosion resistance and pitting corrosion resistance of the steel material in a supercritical corrosion environment. If the Cr content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Cr content is too high, the hot workability of the steel material will deteriorate even if the contents of other elements are within the ranges of this embodiment. Therefore, the Cr content is 20.00 to 24.50%. A preferred lower limit of the Cr content is 20.20%, more preferably 20.50%, and even more preferably 21.00%. A preferred upper limit of the Cr content is 24.30%, more preferably 24.00%, and even more preferably 23.80%.
[0043] Cu: 0.10 to 3.00% Copper (Cu) improves the general corrosion resistance of steel materials in supercritical corrosion environments. If the Cu content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Cu content is too high, the hot workability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Cu content is 0.10 to 3.00%. A preferred lower limit of the Cu content is 0.15%, more preferably 0.20%, and even more preferably 0.25%. A preferred upper limit of the Cu content is 2.90%, more preferably 2.75%, and even more preferably 2.50%.
[0044] Ni: 2.00 to 10.00% Nickel (Ni) stabilizes austenite in steel. Ni also enhances the general corrosion resistance of steel in supercritical corrosion environments. If the Ni content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ni content is too high, the volume fraction of austenite becomes too high, even if the contents of other elements are within the ranges of this embodiment, and the yield strength of the steel decreases. Therefore, the Ni content is 2.00 to 10.00%. A preferred lower limit of the Ni content is 2.50%, more preferably 3.00%, even more preferably 3.50%, and even more preferably 4.00%. A preferred upper limit of the Ni content is 9.80%, more preferably 9.60%, even more preferably 9.30%, and even more preferably 9.00%.
[0045] Mo: 0.80 to 5.00% Molybdenum (Mo) improves the general corrosion resistance of steel materials in supercritical corrosion environments. If the Mo content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mo content is too high, the hot workability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Mo content is 0.80 to 5.00%. A preferred lower limit of the Mo content is 0.85%, more preferably 1.00%, and even more preferably 1.50%. A preferred upper limit of the Mo content is 4.80%, more preferably 4.50%, and even more preferably 4.30%.
[0046] W: 0.01 to 1.50% Tungsten (W) improves the general corrosion resistance of steel in supercritical corrosion environments. If the W content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the W content is too high, the toughness of the steel decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the W content is 0.01 to 1.50%. The preferred lower limit of the W content is 0.05%, more preferably 0.07%, even more preferably 0.10%, and even more preferably 0.15%. The preferred upper limit of the W content is 1.45%, even more preferably 1.35%, and even more preferably 1.25%.
[0047] N: 0.001 to 0.350% Nitrogen (N) stabilizes austenite in steel. N also enhances the general corrosion resistance of steel in supercritical corrosion environments. If the N content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the N content is too high, the hot workability of the steel deteriorates even if the contents of other elements are within the ranges of this embodiment. Therefore, the N content is 0.001 to 0.350%. A preferred lower limit of the N content is 0.003%, more preferably 0.005%, and even more preferably 0.010%. A preferred upper limit of the N content is 0.345%, and even more preferably 0.340%.
[0048] Co: 0.10 to 1.00% Cobalt (Co) forms a coating on the surface of a steel material, improving the general corrosion resistance and pitting corrosion resistance of the steel material in a supercritical corrosion environment. If the Co content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Co content is too high, the manufacturing cost will increase dramatically even if the contents of other elements are within the ranges of this embodiment. Therefore, the Co content is 0.10 to 1.00%. The preferred lower limit of the Co content is 0.11%, more preferably 0.12%, and even more preferably 0.15%. The preferred upper limit of the Co content is 0.95%, more preferably 0.90%, and even more preferably 0.80%.
[0049] Sn: 0.001 to 0.050% Tin (Sn) improves the general corrosion resistance and pitting corrosion resistance of steel materials in supercritical corrosion environments. If the Sn content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Sn content is too high, the hot workability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Sn content is 0.001 to 0.050%. A preferred lower limit of the Sn content is 0.002%, more preferably 0.003%, and even more preferably 0.005%. A preferred upper limit of the Sn content is 0.045%, more preferably 0.040%, and even more preferably 0.035%.
[0050] Sol. Al: 0.050% or less Aluminum (Al) is inevitably contained. That is, the lower limit of the Al content is more than 0%. Al deoxidizes steel. On the other hand, if the Al content is too high, coarse oxide-based inclusions are formed, reducing the toughness of the steel material, even if the contents of other elements are within the ranges of this embodiment. Therefore, the Al content is 0.050% or less. A preferred lower limit of the Al content is 0.001%, more preferably 0.005%, and even more preferably 0.010%. A preferred upper limit of the Al content is 0.045%, and even more preferably 0.040%. Note that the Al content referred to in this specification means the content of "acid-soluble Al," that is, sol. Al.
[0051] V: 0.01 to 0.50% Vanadium (V) increases the strength of steel. If the V content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the V content is too high, the strength of the steel becomes too high, and the toughness of the steel decreases, even if the contents of other elements are within the ranges of this embodiment. Therefore, the V content is 0.01 to 0.50%. A preferred lower limit of the V content is 0.02%, more preferably 0.03%, even more preferably 0.05%, and even more preferably 0.10%. A preferred upper limit of the V content is 0.45%, more preferably 0.40%, and even more preferably 0.30%.
[0052] Ti: 0.001 to 0.050% Titanium (Ti) forms carbonitrides and increases the strength of the steel material. If the Ti content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ti content is too high, the strength of the steel material becomes too high, and the toughness of the steel material decreases, even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ti content is 0.001 to 0.050%. A preferred lower limit of the Ti content is 0.002%, more preferably 0.003%, and even more preferably 0.005%. A preferred upper limit of the Ti content is 0.045%, more preferably 0.040%, even more preferably 0.030%, even more preferably 0.025%, and even more preferably 0.020%.
[0053] Ca: 0.0005 to 0.0100% Calcium (Ca) combines with S in the steel to form Ca sulfides and suppress the formation of coarse Mn sulfides. As a result, the number density of coarse Mn sulfides in the steel is reduced, and the pitting corrosion resistance of the steel in a supercritical corrosion environment is improved. If the Ca content is too low, the above effect cannot be sufficiently achieved even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ca content is too high, a large number of coarse Ca sulfides are formed, and the pitting corrosion resistance of the steel in a supercritical corrosion environment is reduced, even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ca content is 0.0005 to 0.0100%. The preferred lower limit of the Ca content is 0.0006%, more preferably 0.0007%, and even more preferably 0.0008%. The upper limit of the Ca content is preferably 0.0090%, more preferably 0.0080%, further preferably 0.0060%, and still further preferably 0.0050%.
[0054] B: 0.0015 to 0.0050% Boron (B) suppresses the segregation of S to grain boundaries in steel and improves the hot workability of the steel. If the B content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the B content is too high, boron nitride (BN) is formed, reducing the toughness of the steel, even if the contents of other elements are within the ranges of this embodiment. Therefore, the B content is 0.0015 to 0.0050%. The preferred lower limit of the B content is 0.0018%, more preferably 0.0020%, and even more preferably 0.0025%. The preferred upper limit of the B content is 0.0045%, more preferably 0.0040%, and even more preferably 0.0035%.
[0055] O: 0.010% or less Oxygen (O) is unavoidably contained. That is, the lower limit of the O content is greater than 0%. O forms oxides and reduces the toughness of the steel material. Therefore, if the O content is too high, the corrosion resistance of the steel material will decrease even if the contents of other elements are within the ranges of this embodiment. Therefore, the O content is 0.010% or less. A preferred upper limit of the O content is 0.009%, more preferably 0.008%, and even more preferably 0.007%. The O content is preferably as low as possible. However, an extreme reduction in the O content significantly increases manufacturing costs. Therefore, considering industrial production, a preferred lower limit of the O content is 0.001%, more preferably 0.003%.
[0056] The balance of the chemical composition of the duplex stainless steel material according to this embodiment is composed of Fe and impurities. Here, the impurities in the chemical composition refer to substances that are mixed in from raw materials such as ore or scrap or the manufacturing environment during industrial production of the duplex stainless steel material, and are acceptable within a range that does not adversely affect the duplex stainless steel material according to this embodiment.
[0057] [Optional Elements] The chemical composition of the duplex stainless steel material according to this embodiment may further contain one or more elements selected from the group consisting of Mg and rare earth elements in place of a portion of Fe. All of these elements are optional elements and improve the hot workability of the steel material.
[0058] Mg: 0 to 0.010% Magnesium (Mg) is an optional element and does not necessarily need to be contained. That is, the Mg content may be 0%. When contained, Mg neutralizes S in the steel material by fixing it as sulfide, thereby improving the hot workability of the steel material. Even if even a small amount of Mg is contained, the above effects can be obtained to some extent. However, if the Mg content is too high, even if the contents of other elements are within the ranges of this embodiment, oxides in the steel material will coarsen, reducing the toughness of the steel material. Therefore, the Mg content is 0 to 0.010%. The preferred lower limit of the Mg content is more than 0%, more preferably 0.001%, even more preferably 0.002%, and even more preferably 0.003%. The preferred upper limit of the Mg content is 0.009%, even more preferably 0.008%.
[0059] Rare Earth Elements: 0 to 0.010% Rare earth elements (REM) are optional elements and do not necessarily need to be contained. That is, the REM content may be 0%. When contained, REM neutralizes S in the steel material by fixing it as sulfides, improving the hot workability of the steel material. Even if even a small amount of REM is contained, the above effects can be achieved to some extent. However, if the REM content is too high, even if the contents of other elements are within the ranges of this embodiment, oxides in the steel material will coarsen, reducing the toughness of the steel material. Therefore, the REM content is 0 to 0.010%. The preferred lower limit of the REM content is more than 0%, more preferably 0.001%, even more preferably 0.002%, and even more preferably 0.003%. The preferred upper limit of the REM content is 0.009%, even more preferably 0.008%.
[0060] In this specification, REM refers to one or more elements selected from the group consisting of scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanoids lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. In addition, in this specification, the REM content refers to the total content of these elements.
[0061] The chemical composition of the duplex stainless steel material according to this embodiment may further contain one or more elements selected from the group consisting of Zr, Nb, and Ta in place of a portion of Fe. All of these elements are optional elements and increase the strength of the steel material.
[0062] Zr: 0 to 0.010% Zirconium (Zr) is an optional element and does not necessarily need to be contained. That is, the Zr content may be 0%. When contained, Zr forms carbonitrides and increases the strength of the steel material. Even if even a small amount of Zr is contained, the above effect can be obtained to some extent. However, if the Zr content is too high, even if the contents of other elements are within the ranges of this embodiment, the strength of the steel material will be too high and the toughness of the steel material will decrease. Therefore, the Zr content is 0 to 0.010%. The preferred lower limit of the Zr content is more than 0%, more preferably 0.001%, even more preferably 0.002%, and even more preferably 0.003%. The preferred upper limit of the Zr content is 0.009%, even more preferably 0.008%.
[0063] Nb: 0 to 0.500% Niobium (Nb) is an optional element and does not necessarily need to be contained. That is, the Nb content may be 0%. When contained, Nb forms carbonitrides and increases the strength of the steel material. Even if even a small amount of Nb is contained, the above effect can be obtained to some extent. However, if the Nb content is too high, even if the contents of other elements are within the ranges of this embodiment, the strength of the steel material will be too high and the toughness of the steel material will decrease. Therefore, the Nb content is 0 to 0.500%. The preferred lower limit of the Nb content is more than 0%, more preferably 0.001%, even more preferably 0.005%, even more preferably 0.010%, and even more preferably 0.050%. The preferred upper limit of the Nb content is 0.400%, even more preferably 0.300%, and even more preferably 0.200%.
[0064] Ta: 0 to 0.100% Tantalum (Ta) is an optional element and does not necessarily need to be contained. That is, the Ta content may be 0%. When contained, Ta forms carbonitrides and increases the strength of the steel material. Even if even a small amount of Ta is contained, the above effect can be obtained to some extent. However, if the Ta content is too high, even if the contents of other elements are within the ranges of this embodiment, the strength of the steel material will be too high and the toughness of the steel material will decrease. Therefore, the Ta content is 0 to 0.100%. The preferred lower limit of the Ta content is more than 0%, more preferably 0.001%, even more preferably 0.002%, even more preferably 0.003%, and even more preferably 0.005%. The preferred upper limit of the Ta content is 0.095%, even more preferably 0.090%, and even more preferably 0.080%.
[0065] The chemical composition of the duplex stainless steel material according to this embodiment may further contain one or more elements selected from the group consisting of As, Zn, Pb, and Sb in place of a portion of Fe. All of these elements are optional elements and enhance the corrosion resistance of the steel material.
[0066] As: 0 to 0.050% Arsenic (As) is an optional element and does not necessarily need to be contained. That is, the As content may be 0%. When contained, As improves the general corrosion resistance of steel in supercritical corrosion environments. Even if even a small amount of As is contained, the above effect can be obtained to some extent. However, if the As content is too high, even if the contents of other elements are within the ranges of this embodiment, the general corrosion resistance and pitting corrosion resistance of the steel in supercritical corrosion environments may actually decrease. Therefore, the As content is 0 to 0.050%. The preferred lower limit of the As content is more than 0%, more preferably 0.001%, and even more preferably 0.002%. The preferred upper limit of the As content is 0.045%, more preferably 0.040%, and even more preferably 0.035%.
[0067] Zn: 0 to 0.010% Zinc (Zn) is an optional element and does not necessarily need to be contained. That is, the Zn content may be 0%. When contained, Zn improves the general corrosion resistance of the steel material in a supercritical corrosion environment. Even if even a small amount of Zn is contained, the above effect can be obtained to some extent. However, if the Zn content is too high, even if the contents of other elements are within the ranges of this embodiment, the general corrosion resistance and pitting corrosion resistance of the steel material in a supercritical corrosion environment may actually decrease. Therefore, the Zn content is 0 to 0.010%. The preferred lower limit of the Zn content is more than 0%, more preferably 0.001%, even more preferably 0.002%, and even more preferably 0.003%. The preferred upper limit of the Zn content is 0.009%, even more preferably 0.008%, and even more preferably 0.007%.
[0068] Pb: 0 to 0.010% Lead (Pb) is an optional element and does not necessarily need to be contained. That is, the Pb content may be 0%. When contained, Pb improves the general corrosion resistance of steel in supercritical corrosion environments. Even if even a small amount of Pb is contained, the above effect can be obtained to some extent. However, if the Pb content is too high, numerous defects will occur on the surface of the steel after hot working, even if the contents of other elements are within the ranges of this embodiment. Therefore, the Pb content is 0 to 0.010%. The preferred lower limit of the Pb content is more than 0%, more preferably 0.001%, even more preferably 0.002%, and even more preferably 0.003%. The preferred upper limit of the Pb content is 0.009%, even more preferably 0.008%, and even more preferably 0.007%.
[0069] Sb: 0 to 0.010% Antimony (Sb) is an optional element and does not necessarily need to be contained. That is, the Sb content may be 0%. When contained, Sb improves the general corrosion resistance of steel in supercritical corrosion environments. Even if even a small amount of Sb is contained, the above effect can be obtained to some extent. However, if the Sb content is too high, even if the contents of other elements are within the ranges of this embodiment, the manufacturing cost will increase dramatically. Therefore, the Sb content is 0 to 0.010%. The preferred lower limit of the Sb content is more than 0%, more preferably 0.001%, even more preferably 0.002%, and even more preferably 0.003%. The preferred upper limit of the Sb content is 0.009%, even more preferably 0.008%.
[0070] [Fn1] The duplex stainless steel material according to this embodiment has an Fn1 defined by formula (1) of 40.0 or more, provided that the content of each element in the chemical composition is within the above-mentioned range: Fn1 = Cr + 3.3(Mo + 0.5W) + 16N + 2Ni + Cu + 2Co + 10Sn (1) where the element symbols in formula (1) are substituted with the content of the corresponding element in mass%.
[0071] Fn1 is an index of the general corrosion resistance of a duplex stainless steel material in a supercritical corrosion environment. 2 The gas contains SOx gas and O 2 In a supercritical corrosion environment containing gas, among the elements of the above-mentioned chemical composition, not only Cr, Mo, W, and N but also Ni, Cu, Co, and Sn contribute to improving general corrosion resistance. In other words, Fn1 is a parameter formula established in consideration of the contribution of each element to general corrosion resistance in a supercritical corrosion environment for a duplex stainless steel material having the above-mentioned chemical composition. In a duplex stainless steel material having the above-mentioned chemical composition, if Fn1 is 40.0 or more, general corrosion resistance in a supercritical corrosion environment is significantly improved. Therefore, in this embodiment, Fn1 is 40.0 or more.
[0072] The preferred lower limit of Fn1 is 40.5, more preferably 41.0, even more preferably 41.5, and even more preferably 42.0. The upper limit of Fn1 is not particularly limited, but is substantially 74.6. The upper limit of Fn1 may be 70.0, 68.0, or 65.0. Fn1 is calculated by rounding the obtained value to one decimal place.
[0073] [Total Number Density of Specific Inclusions] The duplex stainless steel material according to this embodiment has the above-described chemical composition, Fn1 is 40.0 or more, and further has a total number density of specific inclusions of 0.50 pieces / mm 2 In this specification, the term "specific inclusions" refers collectively to particles (coarse Mn sulfides) having an equivalent circle diameter of 1.0 μm or more and containing, among predetermined elements identified by a method described below, 10% by mass or more of Mn and 10% by mass or more of S, and particles (coarse Ca sulfides) having an equivalent circle diameter of 2.0 μm or more and containing, among predetermined elements identified by a method described below, 20% by mass or more of Ca, 10% by mass or more of S, and less than 10% by mass of Mn.
[0074] In this specification, a unit area (1 mm 2 The sum of the number densities of the coarse Mn sulfides and the coarse Ca sulfides per sintered body was calculated as the total number density of the specific inclusions (numbers / mm 2 Hereinafter, the total number density of specific inclusions will also be referred to as the total number density ND (Number Density) of specific inclusions.
[0075] As described above, in a supercritical corrosion environment, inclusions in the surface layer of a steel material are likely to dissolve, and specific inclusions (coarse Mn sulfides and coarse Ca sulfides) are likely to become the starting points of pitting corrosion. Therefore, in this embodiment, the total number density ND of the specific inclusions is set to 0.50 pieces / mm 2 As a result, provided that the other configurations of this embodiment are satisfied, the duplex stainless steel material has excellent general corrosion resistance and pitting corrosion resistance even in a supercritical corrosion environment.
[0076] The preferred upper limit of the total number density ND of the specific inclusions is 0.49 pieces / mm 2 and more preferably 0.48 pieces / mm 2and more preferably 0.45 pieces / mm 2 The lower limit of the total number density ND of the specific inclusions is not particularly limited, and is 0.00 pieces / mm 2 In the duplex stainless steel material according to this embodiment, the lower limit of the total number density ND of the specific inclusions may be, for example, 0.01 pieces / mm 2 0.05 pieces / mm 2 0.10 pieces / mm 2 0.15 pieces / mm 2 The method for determining the total number density ND of the specific inclusions will be described later.
[0077] [Microstructure] The microstructure of the duplex stainless steel material according to this embodiment is composed of ferrite and austenite. In this specification, "composed of ferrite and austenite" means that phases other than ferrite and austenite are present in negligible amounts. For example, the volume fraction of precipitates and inclusions in the microstructure of the duplex stainless steel material according to this embodiment is negligibly low compared to the volume fraction of ferrite and austenite. In other words, the microstructure of the duplex stainless steel material according to this embodiment may contain minute amounts of precipitates, inclusions, etc. in addition to ferrite and austenite.
[0078] In the microstructure of the duplex stainless steel material according to this embodiment, the volume fractions of ferrite and austenite are not particularly limited. However, in the microstructure of the duplex stainless steel material according to this embodiment having the above-mentioned chemical composition, the volume fraction of ferrite may be, for example, 35 to 65%. In this case, the volume fraction of austenite is 35 to 65%. Note that a method for determining the volume fractions of ferrite and austenite in the microstructure will be described later.
[0079] [Fn2] The duplex stainless steel material according to this embodiment has the above-described chemical composition, Fn1 is 40.0 or more, and the total number density ND of specific inclusions is 0.50 pieces / mm 2 or less, and has a microstructure consisting of ferrite and austenite, and further, the total number density NDA (number / mm 2) and the total number density NDG (number / mm 2 ) satisfy the following formula (2): NDA / NDG<0.50 (2)
[0080] Fn2 (=NDA / NDG) is an index showing the extent to which specific inclusions (coarse Mn sulfides and coarse Ca sulfides) are present in ferrite. Compared to ferrite and austenite, austenite has superior corrosion resistance to ferrite. Therefore, in duplex stainless steel materials having the above-mentioned chemical composition, there is a concern that pitting corrosion may occur selectively in ferrite.
[0081] On the other hand, if Fn2 is less than 0.50, the number density of specific inclusions in ferrite can be sufficiently reduced. As a result, the occurrence of selective pitting corrosion in ferrite can be suppressed, provided that the other configurations of this embodiment are satisfied. Therefore, in this embodiment, Fn2 is reduced to less than 0.50. As a result, provided that the other configurations of this embodiment are satisfied, the duplex stainless steel material has excellent general corrosion resistance and pitting corrosion resistance even in a supercritical corrosion environment.
[0082] As described above, the duplex stainless steel material according to this embodiment has a microstructure in which the volume fraction of ferrite and austenite is, for example, 35 to 65%. In this case, if Fn2 is less than 0.50, the number of specific inclusions in ferrite is smaller than the number of specific inclusions in austenite. Therefore, the pitting corrosion resistance of ferrite can be stably improved.
[0083] The upper limit of Fn2 is preferably 0.49, more preferably 0.48, and even more preferably 0.47. The lower limit of Fn2 is not particularly limited and may be 0.00. In the duplex stainless steel material according to this embodiment, the lower limit of Fn2 may be 0.01, 0.05, 0.10, or 0.15.
[0084] In this embodiment, the total number density ND (number / mm 2), the volume fractions (%) of ferrite and austenite in the microstructure, and Fn2 can be determined by the following method. Specifically, a test piece for microstructure observation is prepared from the duplex stainless steel material according to this embodiment, and the volume fractions (%) of ferrite and austenite, and the number densities of coarse Mn sulfides and coarse Ca sulfides are determined. More specifically, when the steel material is a steel plate, a test piece having an observation surface including the rolling direction and the plate thickness direction is prepared from the center of the plate thickness. When the steel material is a steel pipe, a test piece having an observation surface including the pipe axial direction and the pipe radial direction (wall thickness direction) is prepared from the center of the wall thickness. When the steel material is a round bar, a test piece having an observation surface including the axial and radial directions is prepared from the R / 2 position on a cross section perpendicular to the axial direction of the round bar. Note that, in this specification, the R / 2 position on the round bar refers to the center position of the radius R on a cross section perpendicular to the axial direction of the round bar.
[0085] The observation surface of the prepared test piece is mirror-polished. The mirror-polished observation surface is etched in a mixture of aqua regia and glycerin to reveal the structure. The observation surface with the revealed structure is observed in 10 fields of view using an optical microscope. The area of each field of view is, for example, 2000 μm. 2 (Magnification: 500x). In each field of view, ferrite and austenite are identified from the contrast. The area fraction of the identified ferrite is measured using a point counting method in accordance with JIS G0555 (2020). In this embodiment, the arithmetic average value of the obtained ferrite area fractions in 10 fields of view is defined as the ferrite volume fraction (%). The ferrite volume fraction (%) is calculated by rounding the obtained value to the nearest tenth. The austenite volume fraction (%) is calculated by subtracting the obtained ferrite volume fraction (%) from 100.
[0086] Furthermore, particles in each field of view are identified based on their contrast. Element concentration analysis (EDS analysis) is then performed on each identified particle. In the EDS analysis, an acceleration voltage of 20 kV is used, and target elements are quantified as N, O, Mg, Al, Si, P, S, Ca, Ti, Cr, Mn, Fe, Cu, Zr, and Nb. Based on the EDS analysis results for each particle, particles with an Mn content of 10% by mass or more and an S content of 10% by mass or more are identified as "Mn sulfides," assuming that the total content of N, O, Mg, Al, Si, P, S, Ca, Ti, Cr, Mn, Fe, Cu, Zr, and Nb is 100% by mass. Similarly, based on the results of EDS analysis of each particle, particles having a Ca content of 20% by mass or more, an S content of 10% by mass or more, and an Mn content of less than 10% by mass, where the total content of N, O, Mg, Al, Si, P, S, Ca, Ti, Cr, Mn, Fe, Cu, Zr, and Nb is taken as 100% by mass, are identified as "Ca sulfides."
[0087] Among the Mn sulfides in each field of view, those with an equivalent circle diameter of 1.0 μm or more are specified as "coarse Mn sulfides." In other words, in this specification, "coarse Mn sulfides" refers to particles with an equivalent circle diameter of 1.0 μm or more, and where the total content of N, O, Mg, Al, Si, P, S, Ca, Ti, Cr, Mn, Fe, Cu, Zr, and Nb is defined as 100 mass%, the Mn content is 10 mass% or more, and the S content is 10 mass% or more. Similarly, among the Ca sulfides in each field of view, those with an equivalent circle diameter of 2.0 μm or more are specified as "coarse Ca sulfides." In other words, in this specification, "coarse Ca sulfides" means particles having an equivalent circle diameter of 2.0 μm or more, and when the total content of N, O, Mg, Al, Si, P, S, Ca, Ti, Cr, Mn, Fe, Cu, Zr, and Nb is defined as 100 mass%, the Ca content is 20 mass% or more, the S content is 10 mass% or more, and the Mn content is less than 10 mass%.
[0088] The coarse Mn sulfides and coarse Ca sulfides identified by the above method are counted in each visual field as "specific inclusions." Furthermore, the specific inclusions contained in ferrite in each visual field are counted. Similarly, the specific inclusions contained in austenite in each visual field are counted. As described above, ferrite and austenite can be identified from the contrast in each visual field.
[0089] Based on the total number of specific inclusions counted in 10 visual fields and the total area of the 10 visual fields, the total number density ND (numbers / mm 2 Based on the total number of specific inclusions in the ferrite counted in 10 fields of view and the total area of the ferrite in 10 fields of view, the total number density NDA (number / mm 2 Based on the total number of specific inclusions in the austenite counted in 10 visual fields and the total area of the austenite in 10 visual fields, the total number density NDG (number / mm 2 Using the obtained total number density NDA of the specific inclusions in ferrite and the total number density NDG of the specific inclusions in austenite, Fn2 (=NDA / NDG) is calculated.
[0090] The volume fractions of ferrite and austenite are calculated by rounding off the obtained values to the nearest tenth. 2 ), the total number density NDA of specific inclusions in ferrite (number / mm 2 ), the total number density NDG of specific inclusions in austenite (number / mm 2 ), and Fn2 are calculated by rounding the obtained numerical values to two decimal places.
[0091] [General corrosion resistance and pitting corrosion resistance] The duplex stainless steel material according to this embodiment has the above-described chemical composition, Fn1 is 40.0 or more, and the total number density ND of specific inclusions is 0.50 pieces / mm 2or less, has a microstructure consisting of ferrite and austenite, and Fn2 is less than 0.50. As a result, the duplex stainless steel material according to this embodiment has excellent general corrosion resistance and pitting corrosion resistance even in a supercritical corrosion environment. In this embodiment, excellent general corrosion resistance and pitting corrosion resistance in a supercritical corrosion environment are evaluated by the following method.
[0092] Specifically, test pieces for corrosion testing are prepared from the duplex stainless steel material according to this embodiment. When the steel material is a steel pipe, the test piece is prepared from the center position of the wall thickness. In this case, the longitudinal direction of the test piece is parallel to the axial direction of the steel pipe. When the steel material is a round bar, the test piece is prepared from the R / 2 position. In this case, the longitudinal direction of the test piece is parallel to the axial direction of the round bar. When the steel material is a steel plate, the test piece is prepared from the center position of the plate thickness. In this case, the longitudinal direction of the test piece is parallel to the rolling direction of the steel plate. The test piece is, for example, 30 mm long, 20 mm wide, and 2 mm thick.
[0093] The test specimen was placed in an autoclave and 0.01% by volume of SO 2 gas and 0.05% by volume O 2 A 5.0 mass % sodium chloride aqueous solution saturated with CO2 gas is poured into the autoclave so that the test piece is immersed in the solution. 2 The gas is charged under pressure and the corrosion test is started. The test time for the corrosion test is 96 hours, and the temperature inside the autoclave is maintained at 100°C during the test.
[0094] The mass, density, and surface area of the test specimen after 96 hours are determined, and the corrosion rate (mm / year) of the test specimen is calculated. In this embodiment, the corrosion rate is calculated by rounding the obtained value to the fourth decimal place. Furthermore, the surface of the test specimen after 96 hours is observed with a magnifying glass at 10x magnification to confirm the presence or absence of pitting corrosion. If pitting corrosion is suspected based on the observation with the magnifying glass, the surface is further observed with an optical microscope at 100x magnification to confirm the presence or absence of pitting corrosion. In this embodiment, if the corrosion rate obtained as a result of the corrosion test under the above conditions is 0.100 mm / year or less, the test specimen is evaluated as having excellent general corrosion resistance even in a supercritical corrosion environment. In this embodiment, if no pitting corrosion is observed as a result of the corrosion test under the above conditions, the test specimen is evaluated as having excellent pitting corrosion resistance even in a supercritical corrosion environment.
[0095] [Yield Strength] The yield strength of the duplex stainless steel material according to this embodiment is not particularly limited. The yield strength of the duplex stainless steel material according to this embodiment is, for example, 413 to 1035 MPa. In this embodiment, the lower limit of the yield strength of the duplex stainless steel material may be 427 MPa, 441 MPa, or 448 MPa. In this embodiment, the upper limit of the yield strength of the duplex stainless steel material may be 1020 MPa, 1007 MPa, or 1000 MPa.
[0096] The yield strength of the duplex stainless steel material according to this embodiment can be determined by the following method. Specifically, a tensile test is performed according to ASTM E8 / E8M (2022). A test specimen is prepared from the steel material according to this embodiment. When the steel material is a steel plate, a round bar-shaped tensile test specimen is prepared from the center of the plate thickness. In this case, the longitudinal direction of the tensile test specimen is parallel to the rolling direction of the steel plate. When the steel material is a steel pipe, a round bar-shaped tensile test specimen or an arc-shaped tensile test specimen is prepared from the center of the wall thickness. In this case, the longitudinal direction of the tensile test specimen is parallel to the axial direction of the steel pipe. When the steel material is a round bar, a round bar-shaped tensile test specimen is prepared from the R / 2 position. In this case, the longitudinal direction of the tensile test specimen is parallel to the axial direction of the round bar.
[0097] The size of the round bar-shaped tensile test specimen is, for example, 6.35 mm in parallel diameter and 25.4 mm in gauge length. The size of the arc-shaped tensile test specimen is, for example, the total thickness, 25.4 mm in width, and 50.8 mm in gauge length. Using the prepared test specimen, a tensile test is performed at room temperature (25°C) in air in accordance with ASTM E8 / E8M (2022). In this embodiment, the 0.2% offset proof stress obtained from the tensile test is defined as the yield strength (MPa). In this embodiment, the yield strength (MPa) is determined by rounding the obtained value to one decimal place.
[0098] [Shape of duplex stainless steel material] As described above, the shape of the duplex stainless steel material according to this embodiment is not particularly limited. The duplex stainless steel material according to this embodiment may be, for example, a steel pipe, a steel plate, a round bar, or a wire rod. Preferably, the duplex stainless steel material according to this embodiment is a seamless steel pipe. When the duplex stainless steel material according to this embodiment is a seamless steel pipe, it has excellent general corrosion resistance and pitting corrosion resistance in a supercritical corrosion environment, even if the wall thickness is 5 mm or more.
[0099] [Manufacturing Method] An example of a method for manufacturing a duplex stainless steel material according to this embodiment having the above-described configuration will be described. Note that the method for manufacturing a duplex stainless steel material according to this embodiment is not limited to the manufacturing method described below. The example of a method for manufacturing a duplex stainless steel material according to this embodiment includes a steelmaking process, a hot working process, and a solution treatment process. Each manufacturing process will be described in detail below.
[0100] [Steelmaking Process] The steelmaking process according to this embodiment includes a process of producing molten steel (refining process) and a process of producing a material by casting using the molten steel (material production process). Each process will be described below.
[0101] [Refining process] In the refining process, first, molten steel containing Cr is placed in a ladle, and the molten steel in the ladle is subjected to decarburization treatment under atmospheric pressure. This process is called the rough decarburization refining process. Slag is generated by the decarburization treatment in the rough decarburization refining process. Slag generated by the decarburization treatment floats on the surface of the molten steel after the rough decarburization refining process. In the rough decarburization refining process, Cr in the molten steel is oxidized to Cr 2 O 3 is produced. 2 O 3 Therefore, a deoxidizer is added to the ladle to remove Cr from the slag. 2 O 3 The slag is reduced and the Cr is recovered in the molten steel. This process is called the Cr reduction process. The rough decarburization refining process and the Cr reduction process are carried out by, for example, an electric furnace process, a converter process, or an AOD (Argon Oxygen Decarburization) process. After the Cr reduction process, the slag is removed from the molten steel. This process is called the slag removal process.
[0102] In the case of Cr-containing steel, the C activity is reduced by Cr, which inhibits the decarburization reaction. Therefore, the molten steel after the slag removal process is subjected to a final decarburization process. This process is called the final decarburization refining process. In the final decarburization refining process, the decarburization process is carried out under reduced pressure. If the decarburization process is carried out under reduced pressure, the partial pressure of CO gas in the atmosphere (P CO ) is lowered, and oxidation of Cr in the molten steel is suppressed. Therefore, if decarburization is performed under reduced pressure, the C concentration in the molten steel can be further reduced while suppressing oxidation of Cr. After the final decarburization refining process, a deoxidizer is added to the molten steel to reduce the Cr in the slag. 2 O 3 This process is called the Cr reduction process. The final decarburization refining process and the Cr reduction process after the final decarburization refining process may be performed by, for example, the VOD (Vacuum Oxygen Decarburization) method or the RH (Ruhrstahl-Heraeus) method.
[0103] After the Cr reduction treatment process, the molten steel in the ladle is subjected to final composition adjustment and temperature adjustment before the material production process. This process is called the composition adjustment process. The composition adjustment process is carried out, for example, by LT (Ladle Treatment). In the latter half of the composition adjustment process, Ca is added to the molten steel. Here, the time from the addition of Ca until the Ca is uniformly dispersed in the molten steel is defined as the "uniform mixing time τ." The uniform mixing time τ can be calculated using the following formula (A): τ = 800 × ε -0.4 (A) where ε is the stirring power density of molten steel at LT and is defined by equation (B): ε = 28.5 (Q / W) × T × log (1 + H / 1.48) (B) where Q is the top-blown gas flow rate (Nm 3 / min). W is the mass of molten steel (t). T is the temperature of molten steel (K). H is the depth of the molten steel in the ladle (steel bath depth) (m).
[0104] In the composition adjustment step, the temperature of the molten steel in the ladle is maintained at 1500 to 1700°C. Furthermore, the holding time after the uniform mixing time τ has elapsed since Ca was added to the molten steel is defined as "holding time t" (seconds). In this embodiment, the holding time t after the uniform mixing time τ has elapsed is preferably 60 seconds or more.
[0105] If the holding time t is too short, Ca may not be able to sufficiently modify the Mn sulfides in the molten steel. In this case, a large number of coarse Mn sulfides remain in the steel. As a result, the number density of specific inclusions in the produced duplex stainless steel becomes too high. Therefore, in the refining process according to this embodiment, it is preferable to set the holding time t after the uniform mixing time τ has elapsed to 60 seconds or more.
[0106] As described above, in the refining step of this embodiment, the retention time t after the uniform mixing time τ in the component adjusting step is set to 60 seconds or more. Note that, in the component adjusting step of this embodiment, the upper limit of the retention time t after the uniform mixing time τ has elapsed is not particularly limited, but is, for example, 3600 seconds.
[0107] [Material Production Process] The molten steel produced by the above-described refining process is used to produce a material. The material is a slab or an ingot. Specifically, the slab is produced by continuous casting using the molten steel. The slab may be a slab, a bloom, or a billet. Alternatively, the molten steel may be made into an ingot by ingot-making. The slab or ingot may be further subjected to blooming or the like to produce a billet.
[0108] In a duplex stainless steel material having the above-described chemical composition, austenite is generated during solidification of molten steel, and the temperature range in which the generated austenite grows is 1350 to 1100°C. Therefore, in this embodiment, the cooling rate between 1350 and 1100°C is controlled to cause specific inclusions to be unevenly distributed in the austenite. Specifically, if the cooling rate of the material between 1350 and 1100°C is slower than usual, austenite nucleates and grows preferentially near the inclusions, making it easier for the austenite to incorporate the inclusions.
[0109] On the other hand, if the cooling rate of the material at 1350 to 1100°C is too fast, the material will be supercooled, and the generation and growth of austenite will tend to occur randomly. As a result, in the manufactured duplex stainless steel material, specific inclusions will be less likely to be unevenly distributed in the austenite, and Fn2 may be 0.50 or more. On the other hand, if the cooling rate of the material at a temperature of 1350 to 1100°C is too slow, the austenite will tend to coarsen. As a result, the manufactured duplex stainless steel material may not achieve the desired mechanical properties.
[0110] Therefore, in the material production process according to this embodiment, the cooling rate when the material temperature is 1350 to 1100°C is preferably 8.0 to 25.0°C / min. The method for controlling the cooling rate when the material temperature is 1350 to 1100°C is not particularly limited, and any well-known method may be used. For example, when producing a material by continuous casting, the cooling rate can be controlled by adjusting the amount of cooling water (specific water amount) used to cool the slab. Furthermore, when producing a material by ingot casting, the cooling rate can be controlled by the material of the mold or the water cooling of the mold.
[0111] Here, measuring the internal temperature of the material is difficult in actual operation. Furthermore, in this embodiment, since the material is cooled in a steady state, the cooling rate based on the surface temperature of the material is equivalent to the cooling rate inside the material. More specifically, it was confirmed that, for the material of this embodiment, the cooling rate when the internal temperature of the material is 1350 to 1100°C is equivalent to the cooling rate when the surface temperature of the material is 1200 to 950°C. Therefore, in the material manufacturing process of this embodiment, if the internal temperature of the material cannot be controlled, it is preferable to set the cooling rate when the surface temperature of the material is 1200 to 950°C to 8.0 to 25.0°C / min. The surface temperature of the material can be measured using a non-contact infrared thermometer. The material is manufactured through the above process.
[0112] [Hot Working Step] In the hot working step according to this embodiment, the raw material prepared in the steelmaking step is hot worked to produce an intermediate steel material. In this specification, the intermediate steel material refers to a plate-shaped steel material if the final product is a steel plate, a mother pipe if the final product is a steel pipe, a steel material with a circular cross section if the final product is a round bar, or a wire-shaped steel material if the final product is a wire rod. The hot working may be hot forging, hot extrusion, or hot rolling. The hot working method is not particularly limited and may be a well-known method.
[0113] When the intermediate steel material is a mother pipe (seamless steel pipe), the hot working step may involve, for example, the Eugène-Séjournet method or the Erhardt push bench method (i.e., hot extrusion), or piercing-rolling by the Mannesmann method (i.e., hot rolling). The hot working may be carried out only once or multiple times. For example, the above-mentioned piercing-rolling may be carried out on the raw material, and then the above-mentioned hot extrusion may be carried out. For example, the above-mentioned piercing-rolling may be carried out on the raw material, and then the above-mentioned elongation rolling may be carried out. That is, in the hot working step, hot working is carried out by a well-known method to produce a mother pipe. The heating temperature of the raw material during hot working is, for example, 1000 to 1280°C.
[0114] When the steel material is round steel or steel plate, the intermediate steel material may be produced as follows. When the steel material is round steel, the material is first heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1000 to 1280°C. The material extracted from the heating furnace is hot worked to produce an intermediate steel material having a circular cross section perpendicular to the axial direction. The hot working is, for example, blooming using a blooming mill or hot rolling using a continuous rolling mill. The continuous rolling mill has horizontal stands each having a pair of grooved rolls arranged side by side in the vertical direction, and vertical stands each having a pair of grooved rolls arranged side by side in the horizontal direction, arranged alternately.
[0115] When the steel material is a steel plate, the material is first heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1000 to 1280°C. The material extracted from the heating furnace is hot-rolled using a blooming mill and a continuous rolling mill to produce an intermediate steel material in the shape of a steel plate.
[0116] [Solution Treatment Step] In the solution treatment step, the intermediate steel material is subjected to solution treatment. The solution treatment method is not particularly limited and may be a well-known method. For example, the intermediate steel material is charged into a heat treatment furnace, held at a desired temperature, and then rapidly cooled. Note that when the intermediate steel material is charged into a heat treatment furnace, held at a desired temperature, and then rapidly cooled to perform solution treatment, the solution treatment temperature refers to the temperature (°C) of the heat treatment furnace for performing the solution treatment. In this case, the solution treatment time refers to the time during which the intermediate steel material is held at the solution treatment temperature.
[0117] Preferably, the solution treatment temperature in the solution treatment step of this embodiment is set to 900 to 1200°C. If the solution treatment temperature is too low, precipitates (for example, σ phase, which is an intermetallic compound) may remain in the intermediate steel material after the solution treatment. In this case, the corrosion resistance of the manufactured duplex stainless steel material will decrease.
[0118] When the intermediate steel material is charged into a heat treatment furnace, held at a desired temperature, and then rapidly cooled to perform solution treatment, the solution treatment time is not particularly limited and may be performed under well-known conditions. The solution treatment time is, for example, 5 to 180 minutes. The rapid cooling method is, for example, water cooling.
[0119] [Other steps] If necessary, the duplex stainless steel material that has undergone solution treatment may be subjected to pickling treatment. In this case, the pickling treatment may be performed by a well-known method, and is not particularly limited. The duplex stainless steel material that has undergone solution treatment may also be subjected to cold working. When cold working is performed, the strength of the duplex stainless steel material can be increased. Even when cold working is performed, the duplex stainless steel material has the above-mentioned chemical composition, Fn1 is 40.0 or more, and the total number density ND of specific inclusions is 0.50 pieces / mm 2 A duplex stainless steel material having a microstructure consisting of ferrite and austenite and an Fn2 of less than 0.50 has excellent general corrosion resistance and pitting corrosion resistance even in a supercritical corrosion environment.
[0120] The duplex stainless steel material according to this embodiment can be manufactured by the above steps. Note that the above-described method for manufacturing a duplex stainless steel material is one example, and the duplex stainless steel material according to this embodiment may be manufactured by other methods. The duplex stainless steel material according to this embodiment will be described in more detail below using examples. Note that the examples described below are examples of conditions adopted to confirm the feasibility and effects of the duplex stainless steel material according to this embodiment. In other words, the duplex stainless steel material according to this embodiment is not limited to the examples described below.
[0121] Duplex stainless steel materials (seamless steel pipes) having the chemical compositions shown in Tables 1-1 to 1-3 were produced by the following method. Note that a "-" in the "Chemical Composition" column in Tables 1-1 to 1-3 means that the corresponding element content is 0% in the numerical values rounded to the smallest digit described in the embodiments. Specifically, the Mg content, REM content, Zr content, Nb content, Ta content, As content, Zn content, Pb content, and Sb content of Test No. 1 were 0% when rounded to the fourth decimal place.
[0122]
[0123]
[0124]
[0125] The molten steel for each test number was produced as follows. Molten steel containing Cr was placed in a ladle, and a well-known rough decarburization refining process and a Cr reduction treatment process were carried out by the AOD method. After the Cr reduction treatment process, a slag removal process was carried out to remove slag from the molten steel. Furthermore, a well-known finish decarburization refining process and a Cr reduction treatment process were carried out by the VOD method.
[0126] After the Cr reduction treatment process using the VOD method, the molten steel in the ladle was subjected to final composition adjustment using LT, and the temperature of the molten steel was adjusted before the material production process. The molten steel temperature was 1500 to 1700°C in all cases. Furthermore, Ca was added to the molten steel. After the Ca addition, the holding time t (seconds) after the uniform mixing time τ had elapsed was adjusted as shown in Table 2. Molten steel with each test number was produced using the above processes.
[0127]
[0128] The produced molten steel was used to produce billets by continuous casting. When producing the billets, the cooling rate at a billet temperature of 1350 to 1100°C was adjusted as shown in Table 2, "Cooling rate from 1350 to 1100°C (°C / min)." The cooling rate was adjusted by adjusting the specific water amount. Since it was difficult to measure the internal temperature of the billet, in this example, the cooling rate at a billet surface temperature of 1200 to 950°C was measured and considered to be the cooling rate at a billet internal temperature of 1350 to 1100°C. The surface temperature of the billet was also measured using an infrared radiation thermometer.
[0129] The produced billets were heated to 1250°C and then hot-rolled by the Mannesmann process to produce mother pipes (seamless steel pipes) with an outer diameter of 244.48 mm and a wall thickness of 13.84 mm. Furthermore, the mother pipes were subjected to solution treatment. The solution treatment temperature was 1080°C, and the solution treatment time was 15 minutes. After the solution treatment time had elapsed, the mother pipes were water-cooled. The water-cooled seamless steel pipes of test numbers 21 to 27 were further subjected to cold working. In this example, cold drawing was performed as the cold working. Through the above steps, the steel materials (seamless steel pipes) of each test number were produced.
[0130] [Evaluation Tests] A microstructure observation test, a tensile test, and a corrosion test were carried out on the steel materials of each test number. Note that the steel material of test number 41 was not subjected to any evaluation tests because defects occurred during the manufacturing process.
[0131] [Microstructure Observation Test] A microstructure observation test was carried out on the steel material of each test number except for test number 41 to identify the microstructure, and the total number density ND (number / mm 2 ), and Fn2 were determined. Specifically, a test piece for microstructure observation was prepared by the above-mentioned method, and the microstructure was identified. Furthermore, the total number density ND of the specific inclusions was determined by the above-mentioned method. Furthermore, Fn2 was determined by the above-mentioned method. The area of each field of view was 2000 μm 2 (magnification: 500x).
[0132] All of the steel materials with test numbers except for test number 41 had a microstructure consisting of ferrite and austenite. Furthermore, the volume fraction of ferrite was 35 to 65%. In addition, the total number density ND (numbers / mm 2 ) in Table 2, 2 The total number density NDA (number / mm) of specific inclusions in the ferrite of the steel material of each test number obtained is also shown. 2 ) and the total number density NDG (number / mm 2 ) and Fn2 (= NDA / NDG) was calculated. The obtained Fn2 is shown in Table 2. As mentioned above, the microstructure observation test was not performed for test number 41, and therefore "-" (no evaluation) is shown in Table 2.
[0133] [Tensile Test] Tensile tests were conducted on the steel materials of each test number except for test number 41 in accordance with ASTM E8 / E8M (2022) to determine the yield strength. Specifically, arc-shaped tensile test specimens were prepared for the tensile test using the method described above. The arc-shaped tensile test specimens had the same thickness as the wall thickness of the seamless steel pipe, a width of 25.4 mm, and a gauge length of 50.8 mm. Using the tensile test specimens of each test number, tensile tests were conducted at room temperature (25°C) in air to determine the 0.2% offset yield strength (MPa). The determined 0.2% offset yield strength was defined as the yield strength (MPa). The obtained yield strengths for each test number are shown in the "YS (MPa)" column of Table 2. Note that the yield strengths of all the steel materials of each test number except for test number 41 were in the range of 413 to 1035 MPa. As mentioned above, the tensile test was not performed for test number 41, and therefore the mark "-" (no evaluation) is shown in Table 2.
[0134] [Corrosion Test] A corrosion test was conducted on the steel materials of each test number except for test number 41 to evaluate their general corrosion resistance and pitting corrosion resistance in a supercritical corrosion environment. Specifically, test specimens for the corrosion test were prepared using the method described above. A corrosion test was conducted on the prepared test specimens under the conditions described above to determine the corrosion rate (mm / year). Furthermore, the presence or absence of pitting corrosion was confirmed for the test specimens after the corrosion test using the method described above. The obtained corrosion rates (mm / year) are shown in Table 2. Furthermore, test numbers in which pitting corrosion was not confirmed are indicated with "E (Excellent)" in the "Pitting Corrosion" column of Table 2. Furthermore, test numbers in which pitting corrosion was confirmed are indicated with "NA (Not Acceptable)" in the "Pitting Corrosion" column of Table 2. As described above, a corrosion test was not conducted on test number 41, and therefore "-" (no evaluation) is indicated in Table 2.
[0135] [Evaluation Results] Referring to Tables 1-1, 1-2, 1-3, and 2, the duplex stainless steel materials of test numbers 1 to 27 had appropriate chemical compositions, Fn1 of 40.0 or more, and the manufacturing method also satisfied the conditions of the above-mentioned preferred manufacturing method. Furthermore, these steel materials had a microstructure consisting of ferrite and austenite, and the total number density ND of specific inclusions was 0.50 pieces / mm 2or less, and Fn2 was less than 0.50. As a result, the corrosion rate of these steel materials was 0.100 mm / year or less, and no pitting corrosion was observed. In other words, these steel materials had excellent general corrosion resistance and pitting corrosion resistance even in a supercritical corrosion environment.
[0136] On the other hand, the Cr content of the steel material of test number 28 was too low. As a result, the corrosion rate of this steel material exceeded 0.100 mm / year. In other words, this steel material did not have excellent general corrosion resistance in a supercritical corrosion environment.
[0137] The steel material of test number 29 had an excessively low Cu content. As a result, the corrosion rate of this steel material exceeded 0.100 mm / year. In other words, this steel material did not have excellent general corrosion resistance in a supercritical corrosion environment.
[0138] The steel material of test number 30 had an excessively low W content. As a result, the corrosion rate of this steel material exceeded 0.100 mm / year. In other words, this steel material did not have excellent general corrosion resistance in a supercritical corrosion environment.
[0139] The steel material of test number 31 had an excessively low Co content. As a result, pitting corrosion was confirmed in the corrosion test. In other words, this steel material did not have excellent pitting corrosion resistance in a supercritical corrosion environment.
[0140] The steel material of test number 32 had an excessively low Sn content. As a result, pitting corrosion was confirmed in the corrosion test. In other words, this steel material did not have excellent pitting corrosion resistance in a supercritical corrosion environment.
[0141] The steel material of test number 33 had an excessively high Al content. Furthermore, this steel material had a total number density ND of specific inclusions of 0.50 pieces / mm 2 As a result, pitting corrosion was confirmed in the corrosion test of this steel material. In other words, this steel material did not have excellent pitting corrosion resistance in a supercritical corrosion environment.
[0142] The steel material of test number 34 had a too low Ca content. Furthermore, this steel material had a total number density ND of specific inclusions of 0.50 pieces / mm 2As a result, pitting corrosion was confirmed in the corrosion test of this steel material. In other words, this steel material did not have excellent pitting corrosion resistance in a supercritical corrosion environment.
[0143] The steel materials of test numbers 35 to 37 had too low Fn1. As a result, the corrosion rates of these steel materials exceeded 0.100 mm / year. In other words, these steel materials did not have excellent general corrosion resistance in a supercritical corrosion environment.
[0144] For the steel materials of test numbers 38 to 40, the holding time t after the uniform mixing time τ had elapsed after adding Ca was too short. Furthermore, for these steel materials, the total number density ND of specific inclusions was 0.50 pieces / mm 2 As a result, pitting corrosion was confirmed in these steel materials in corrosion tests. In other words, these steel materials did not have excellent pitting corrosion resistance in supercritical corrosion environments.
[0145] As described above, the steel material of test number 41 had defects that occurred during the manufacturing process.
[0146] The steel material of test number 42 had an excessively fast cooling rate between 1350 and 1100°C. Furthermore, this steel material had an Fn2 of 0.50 or more. As a result, pitting corrosion was confirmed in the corrosion test for this steel material. In other words, this steel material did not have excellent pitting corrosion resistance in a supercritical corrosion environment.
[0147] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments within the scope of the present disclosure.
Claims
1. A duplex stainless steel material having, by mass%, the following: C: 0.050% or less, Si: 1.00% or less, Mn: 0.40 to 3.00%, P: 0.050% or less, S: 0.0050% or less, Cr: 20.00 to 24.50%, Cu: 0.10 to 3.00%, Ni: 2.00 to 10.00%, Mo: 0.80 to 5.00%, W: 0.01 to 1.50%, N: 0.001 to 0.350%, Co: 0.10 to 1.00%, Sn: 0.001 to 0.050%, sol. Al: 0.050% or less, V: 0.01 to 0.50%, Ti: 0.001 to 0.050%, Ca: 0.0005 to 0.0100%, B: 0.0015 to 0.0050%, O: 0.010% or less, Mg: 0 to 0.010%, rare earth elements: 0 to 0.010%, Zr: 0 to 0.010%, Nb: 0 to 0.500%, Ta: 0 to 0.100%, As: 0 to 0.050%, Zn: 0 to 0.010%, Pb: 0 to 0.010%, Sb: 0 to 0.010%, and the balance being Fe and impurities, with the assumption that the contents of each of the elements are within the above-mentioned ranges. Fn1 defined by formula (1) is 40.0 or more, and in the duplex stainless steel material, when particles having an equivalent circle diameter of 1.0 μm or more, a Mn content of 10 mass% or more, and a S content of 10 mass% or more are defined as coarse Mn sulfides, and particles having an equivalent circle diameter of 2.0 μm or more, a Ca content of 20 mass% or more, a S content of 10 mass% or more, and a Mn content of less than 10 mass% are defined as coarse Ca sulfides, the total number density of the coarse Mn sulfides and the coarse Ca sulfides is 0.50 particles / mm 2 the microstructure of the duplex stainless steel material is composed of ferrite and austenite, and the total number density of the coarse Mn sulfides and the coarse Ca sulfides in the ferrite is NDA number / mm 2 The total number density of the coarse Mn sulfides and the coarse Ca sulfides in the austenite is defined as NDG pieces / mm 2A duplex stainless steel material, wherein the NDA and the NDG satisfy formula (2): Fn1 = Cr + 3.3 (Mo + 0.5W) + 16N + 2Ni + Cu + 2Co + 10Sn (1) NDA / NDG < 0.50 (2) where the element symbols in formula (1) are substituted with the contents of the corresponding elements in mass%.
2. The duplex stainless steel material according to claim 1, containing one or more elements selected from the group consisting of Mg: 0.001-0.010%, rare earth elements: 0.001-0.010%, Zr: 0.001-0.010%, Nb: 0.001-0.500%, Ta: 0.001-0.100%, As: 0.001-0.050%, Zn: 0.001-0.010%, Pb: 0.001-0.010%, and Sb: 0.001-0.010%.
3. A duplex stainless steel material according to claim 1 or 2, which is a steel pipe.
Citation Information
Patent Citations
Two-phase stainless steel material, two-phase stainless steel pipe and surface treatment method for two-phase stainless steel material
JP2016216816A
Ferrite-austenite two-phase system stainless steel material and method for manufacturing them, and corrosion-resistant member
JP2022155339A
Ferrite-austenite two-phase system stainless steel material and method for manufacturing the same, and corrosion-resistant member
JP2022155343A
Duplex stainless steel material
WO2023058630A1
Duplex stainless steel material
WO2023058631A1
Cited By
Duplex stainless steel seamless pipe
JP7769284B1
Stainless steel material
JP7883192B1
Duplex seamless stainless steel pipe
WO2025215951A1
Duplex stainless steel material
WO2026083491A1
Stainless steel material
WO2026083702A1