Curable liquid silicone composition and cured product
The curable liquid silicone composition, activated by moisture and oxygen, addresses the limitations of existing technologies by enabling long-term storage and deep curing at room temperature, resulting in transparent and low-coloration products with enhanced visibility and energy efficiency.
Patent Information
- Application Number
- PCT/JP2024/010509
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-17
AI Technical Summary
Existing curable liquid silicone compositions face challenges with short shelf life and insufficient deep curability, particularly in UV shadow areas, limiting their applications due to reliance on heating, UV activation, or inadequate crosslinking reactions.
A curable liquid silicone composition utilizing a platinum-based catalyst mixture activated by moisture and/or oxygen, combined with a dehydrating agent and organic zirconium compound, which undergoes hydrosilylation addition reactions at room temperature, ensuring long-term storage stability and deep curing without heating, resulting in transparent and low-coloration products.
The composition achieves long-term storage stability and excellent deep curing properties, providing transparent and low-coloration silicone rubber or gel products, enhancing internal visibility and applicability in various parts and products while aligning with energy-saving and SDG goals.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Curable liquid silicone composition and cured product
[0001] The present invention relates to a curable liquid silicone composition (curable liquid silicone rubber composition or curable liquid silicone gel composition) that can be cured with a platinum-based catalyst mixture that is activated by moisture and / or oxygen to give a cured silicone rubber (silicone elastomer elastic material) or cured silicone gel that has excellent transparency, low coloration, and internal visibility, and to the cured product thereof.
[0002] In light of the demands for energy conservation and the SDGs (Sustainable Development Goals), there has been a growing demand in recent years for curable liquid silicone compositions that can be cured without heating. Furthermore, in order to simplify the use of curable liquid silicone compositions, and for the purposes of workability and preventing formulation errors during use, one-component curable liquid silicone compositions are preferred.
[0003] Among the curable liquid silicone compositions that are one-component and can be cured without heating through crosslinking reactions such as condensation reactions, UV radical reactions, and hydrosilylation addition reactions, some have extremely short shelf lives, and some can activate the catalyst with UV light. However, all of these reactions have insufficient deep curing ability or curing ability in the shadow areas of UV light, limiting the applications in which they can be used.
[0004] The following prior art is relevant to the present invention.
[0005] U.S. Patent No. 4,510,094 U.S. Patent No. 4,530,879 Japanese Patent No. 6,020,740 International Publication No. 2022 / 270366
[0006] The present invention has been made in view of the above circumstances, and has as its object the provision of a curable liquid silicone composition and a cured product thereof which have a one-component shelf life for long periods in a light-shielded sealed container under refrigeration to room temperature (-5 to 38°C), and which, upon contact with moisture and / or oxygen, particularly moisture (humidity) and / or oxygen in the atmosphere, can give a cured silicone rubber or cured silicone gel product that is cured to the interior and has excellent transparency, low coloration, and internal visibility, and which in particular allows easy observation of the interior of parts and gives a colorless, transparent cured product that is effective for verifying defects, etc. in sealing parts, and a cured product thereof.
[0007] As a result of extensive research by the present inventors to solve the above-mentioned problems, they have discovered that a curable liquid silicone composition containing an aerobic platinum-based catalyst mixture that is activated upon contact with moisture and / or oxygen, particularly atmospheric moisture (humidity) and / or oxygen, to act as a hydrosilylation addition reaction catalyst, a dehydrating agent such as at least one compound selected from silylketenes and α-silyl esters, and an organozirconium compound as a dehydration accelerator, has long-term storage stability as a one-component composition, and upon exposure to the atmosphere for a predetermined period of time, becomes a curable liquid silicone rubber composition or curable liquid silicone gel composition that exhibits good curability, including internally, and gives a transparent cured product that is excellent in transparency, low coloration, and internal visibility, and has led to the completion of the present invention.
[0008] The present invention cures a liquid silicone composition into silicone rubber or silicone gel using a curing (crosslinking) reaction system that employs a hydrosilylation addition reaction using an (aerobic) platinum-based catalyst mixture that is activated by moisture and / or oxygen. Of particular note, the curable liquid silicone composition of the present invention can be "stored as a single-part product in a sealed container in the dark" at temperatures ranging from refrigeration to room temperature (temperature range of -5 to 38°C), and in the absence of heat (i.e., at room temperature (23°C±15°C)), the catalytic function is activated upon "contact with air (atmospheric moisture (humidity) and / or oxygen)," causing the hydrosilylation addition reaction to proceed, resulting in curing not only on the surface exposed to air, but also in the interior (deep areas) and shadow areas.
[0009] Accordingly, the present invention provides the following curable liquid silicone composition and a cured product of the curable liquid silicone composition. [1] A curable liquid silicone composition comprising: (A) a diorganopolysiloxane having at least one alkenyl group per molecule; (B) an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule, in an amount such that there are 0.5 to 4 moles of silicon-bonded hydrogen atoms in component (B) per mole of alkenyl groups in component (A); (C) a platinum-based catalyst mixture activated by moisture and / or oxygen, in an amount such that the platinum atoms in component (C) are 0.1 to 1,000 ppm by mass relative to the combined mass of components (A) and (B); (D) a dehydrating agent, in an amount of 0.01 to 5 parts by mass per 100 parts by mass of components (A) and (B); and (E) an organozirconium compound, in an amount of 0.001 to 5 parts by mass per 100 parts by mass of components (A) and (B). [2] The curable liquid silicone composition according to [1], wherein the dehydrating agent of component (D) is at least one compound selected from silylketenes and α-silyl esters. [3] The curable liquid silicone composition according to [1] or [2], wherein component (C) is an aerobic platinum-based catalyst mixture consisting of a reaction mixture of a platinum-alkenyl group-containing organosiloxane complex and an organosilicon compound having at least one silicon-bonded hydrogen atom per molecule, in an amount such that there is a molar excess of silicon-bonded hydrogen atoms relative to the alkenyl groups in the platinum-alkenyl group-containing organosiloxane complex. [4] A cured product of the curable liquid silicone composition according to any of [1] to [3].
[0010] The curable liquid silicone composition of the present invention is one in which the curing reaction proceeds due to an aerobic platinum-based catalyst mixture that is activated upon contact with moisture and / or oxygen, particularly atmospheric moisture (humidity) and / or oxygen, and acts as a hydrosilylation addition reaction catalyst. The curable liquid silicone composition of the present invention, which contains the platinum-based catalyst mixture, a dehydrating agent such as at least one compound selected from silylketenes and α-silyl esters, and an organozirconium compound as a dehydration accelerator, has a sufficiently long shelf life as a one-part product when stored or transported at refrigerated to room temperature in a light-shielded sealed container. During use, the platinum-based catalyst mixture is activated upon contact with moisture and / or oxygen, particularly atmospheric moisture (humidity) and / or oxygen, without heating (i.e., at room temperature), causing the hydrosilylation addition reaction to proceed, resulting in a cured product that is minimally colored not only at the air interface but also in the interior / shadowed areas (excellent transparency, low coloration, and interior visibility). Therefore, the curable liquid silicone compositions of the present invention (curable liquid silicone rubber compositions and curable liquid silicone gel compositions) can contribute to energy conservation and the production of various parts and products in line with the SDGs.
[0011] The present invention will be described in detail below.
[0012] [Curable Liquid Silicone Composition] The curable liquid silicone composition of the present invention (curable liquid silicone rubber composition or curable liquid silicone gel composition) is a composition containing components (A) to (E) described below, and, if necessary, other components.
[0013] [(A) Alkenyl Group-Containing Diorganopolysiloxane] The alkenyl group-containing diorganopolysiloxane of component (A) is a linear or branched diorganopolysiloxane having at least one, and preferably 1 to 20, alkenyl group per molecule. It functions as the main component (base polymer) of the curable liquid silicone composition of the present invention (hereinafter also referred to as the composition of the present invention). Typically, it is a linear diorganopolysiloxane whose main chain is basically composed of repeating diorganosiloxane units and whose molecular chain is terminally blocked with triorganosiloxy groups; however, it may also be a branched diorganopolysiloxane containing a branched structure as part of the siloxane structure that makes up the molecular chain.
[0014] The alkenyl-containing diorganopolysiloxane of component (A) contains at least one alkenyl group (usually 1 to 50), preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 or 2 alkenyl groups per molecule. Examples of alkenyl groups include vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, and cyclohexenyl, which typically have about 2 to 8 carbon atoms. The alkenyl group may be bonded to a silicon atom at a molecular chain terminal or to a silicon atom at a non-terminal (intermediate) location in the molecular chain. Preferably, the alkenyl group contains an alkenyl group bonded to a silicon atom at at least one or both of the molecular chain terminals. In this case, the alkenyl group may be present only at one or both of the molecular chain terminals, or at both of the molecular chain terminals and non-terminal (intermediate) locations in the molecular chain.
[0015] Examples of such alkenyl group-containing diorganopolysiloxanes include linear diorganopolysiloxanes represented by the following general formula (1). (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups that do not contain aliphatic unsaturated bonds. X is an alkenyl group, and at least one is contained in one molecule. n is an integer of 0 or greater, m is an integer of 0 or greater, and a is an integer of 0 to 3 for each silicon atom to which it is bonded, with at least one of a and m at both ends being an integer of 1 or greater.
[0016] In the formula, R 1 Examples of the unsubstituted or substituted monovalent hydrocarbon group not containing an aliphatic unsaturated bond include those having 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 6 carbon atoms. Specific examples include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenylyl; aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl; and groups in which some or all of the hydrogen atoms bonded to carbon atoms of these groups have been substituted with halogen atoms such as fluorine, chlorine or bromine, or with cyano groups, for example, chloromethyl group, 2-bromoethyl group, 3-chloropropyl group, 3,3,3-trifluoropropyl group, chlorophenyl group, fluorophenyl group, cyanoethyl group, 3,3,4,4,5,5,6,6,6-nonafluorohexyl group, and the like, preferably unsubstituted or substituted alkyl groups having 1 to 3 carbon atoms such as methyl group, ethyl group, propyl group, chloromethyl group, bromoethyl group, 3,3,3-trifluoropropyl group, cyanoethyl group, and the like, and unsubstituted or substituted phenyl groups such as phenyl group, chlorophenyl group, fluorophenyl group, and the like. R 1 As the alkyl group, a methyl group and a phenyl group are preferred.
[0017] In the formula, examples of the alkenyl group represented by X include those having about 2 to 8 carbon atoms, such as vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, and cyclohexenyl groups, and among these, lower alkenyl groups such as vinyl and allyl are preferred.
[0018] In the formula, n is an integer of 0 or greater, preferably an integer of 10 to 2,000, more preferably an integer of 50 to 1,200, and m is an integer of 0 or greater, preferably an integer of 0 to 40, more preferably an integer of 0 to 20. Furthermore, n and m are preferably integers that satisfy 10≦n+m≦2,000, more preferably 50≦n+m≦1,200, and 0≦m / (n+m)≦0.2. In this case, the units in parentheses enclosed by n and m may be arranged randomly. In the formula, a is an integer of 0 to 3, preferably an integer of 1 to 3, for each silicon atom to be bonded.
[0019] The alkenyl group-containing diorganopolysiloxane may be, for example, a diorganopolysiloxane having a monofunctional siloxy unit (X a R 1 (3-a) SiO 1 / 2 unit) and difunctional siloxane units ((X)(R 1 ) SiO 2 / 2 Units, (R 1 ) SiO 2 / 2 In addition to the trifunctional siloxane unit (i.e., (R 1 ) SiO 3 / 2 or (X) SiO 3 / 2 Examples of suitable branched chain diorganopolysiloxanes include those having a small amount of silsesquioxane units represented by the following formula (a) in the molecule, which may contain a cyclic structure, a ladder structure, and / or a cage structure in the molecule.
[0020] Furthermore, it is preferable that such alkenyl-containing diorganopolysiloxanes have a viscosity at 23°C of about 10 to 1,000,000 mPa·s, and particularly about 100 to 500,000 mPa·s.
[0021] In the present invention, the number of repeating diorganosiloxane units in a molecule (or degree of polymerization) can be determined as the polystyrene-equivalent number average molecular weight (or number average degree of polymerization) by gel permeation chromatography (GPC) analysis using toluene or the like as a developing solvent. Viscosity can be measured using a rotational viscometer (e.g., BL type, BH type, BS type, cone-plate type, rheometer, etc.) at 23°C.
[0022] The alkenyl group-containing diorganopolysiloxane of component (A) may be used alone or in combination of two or more. Furthermore, in order to avoid impairing the function of the platinum catalyst mixture of component (C), which will be described later, it is advisable to reduce the oxygen and water contents in the alkenyl group-containing diorganopolysiloxane of component (A) before blending it into the composition. This can be done, for example, by replacing the atmosphere with an inert gas such as nitrogen gas, by heating or reducing the pressure, or by a combination of these methods.
[0023] [(B) Organohydrogenpolysiloxane] The organohydrogenpolysiloxane of component (B) is an organohydrogenpolysiloxane with a linear, cyclic, branched, or three-dimensional network structure (resin structure) that contains at least two (typically 2 to 200), and preferably about 2 to 100, silicon-bonded hydrogen atoms (SiH groups) per molecule, and functions as a curing agent (crosslinking agent) for the curable liquid silicone composition of the present invention.
[0024] Examples of such organohydrogenpolysiloxanes include organohydrogenpolysiloxanes represented by the following average composition formula (2): b R 2 c SiO (4-b-c) / 2 (2) (wherein, R 2 are independently an unsubstituted or substituted monovalent hydrocarbon group containing no aliphatic unsaturated bonds, and b and c are numbers that satisfy 0.001≦b≦1.2, 0.8≦c≦2, and 0.8<b+c≦3, and preferably 0.05≦b≦1, 1.5≦c≦2, and 1.8≦b+c≦2.7.
[0025] In the formula, R 2The unsubstituted or substituted monovalent hydrocarbon group not containing an aliphatic unsaturated bond includes R 1 Examples include those having 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 7 carbon atoms, and particularly preferred are lower alkyl groups having 1 to 3 carbon atoms such as a methyl group, a phenyl group, and a 3,3,3-trifluoropropyl group.
[0026] Component (B) is preferably a compound that is liquid at room temperature (23°C ± 15°C, hereinafter the same) and has 2 to 300 silicon atoms per molecule, particularly 3 to 150, and especially about 3 to 100. The hydrogen atoms bonded to the silicon atoms may be located at either the terminals of the molecular chain, midway along the molecular chain (non-terminal), or both.
[0027] Examples of such organohydrogenpolysiloxanes include methylhydrogencyclosiloxane oligomers such as 1,1,3,3-tetramethyldisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, 1,3,5,7-tetramethyltetracyclosiloxane, and 1,3,5,7,9-pentamethylpentacyclosiloxane; tris(dimethylhydrogensiloxy)methylsilane; tris(dimethylhydrogensiloxy)phenylsilane; methylhydrogenpolysiloxanes terminated at both molecular chain terminals with trimethylsiloxy groups; dimethylsiloxane-methylhydrogensiloxane copolymers terminated at both molecular chain terminals with trimethylsiloxy groups; diphenylsiloxane-methylhydrogensiloxane copolymers terminated at both molecular chain terminals with trimethylsiloxy groups; and methylphenylsiloxane-methylhydrogensiloxanes terminated at both molecular chain terminals with trimethylsiloxy groups. copolymer, dimethylsiloxane-diphenylsiloxane-methylhydrogensiloxane copolymer terminated at both molecular chain ends with trimethylsiloxy groups, dimethylpolysiloxane terminated at both molecular chain ends with dimethylhydrogensiloxy groups, methylhydrogenpolysiloxane terminated at both molecular chain ends with dimethylhydrogensiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer terminated at both molecular chain ends with dimethylhydrogensiloxy groups, diphenylsiloxane-methylhydrogensiloxane copolymer terminated at both molecular chain ends with dimethylhydrogensiloxy groups, methylphenylsiloxane-methylhydrogensiloxane copolymer terminated at both molecular chain ends with dimethylhydrogensiloxy groups, dimethylsiloxane-diphenylsiloxane-methylhydrogensiloxane copolymer terminated at both molecular chain ends with dimethylhydrogensiloxy groups, 4 / 2Examples of suitable organosilicon compounds include silicone resins having a three-dimensional network structure consisting of units, which may optionally contain trimethylsiloxy units, dimethylsiloxane units, methylhydrogensiloxane units, hydrogensilsesquioxane units, and / or methylsilsesquioxane units, and compounds in which some or all of the methyl groups in the above-mentioned exemplary compounds have been substituted with other alkyl groups or phenyl groups. Note that component (B) and the organosilicon compound in component (C), which will be described later, may be the same.
[0028] The organohydrogenpolysiloxane used in the composition of the present invention can be obtained by known methods, for example, a compound represented by the following general formula: 2 SiHCl2 and R 2 2SiHCl (wherein R 2 is the same as above.) or by (co)hydrolytic condensation of the chlorosilane with a compound represented by the following general formula: R 2 3SiCl and R 2 2SiCl2 (wherein, R 2 are the same as above.) and at least one chlorosilane selected from the group consisting of chlorosilanes ...
[0029] From the viewpoint of providing a good silicone rubber or gel upon curing, the amount of organohydrogenpolysiloxane of component (B) blended is an amount such that the number of hydrogen atoms bonded to silicon atoms (i.e., SiH groups) in the organohydrogenpolysiloxane of component (B) is 0.5 to 4 moles, and preferably 0.8 to 2.5 moles, per mole of alkenyl groups in the alkenyl group-containing diorganopolysiloxane of component (A).
[0030] The organohydrogenpolysiloxane of component (B) may be used alone or in combination of two or more. Furthermore, in order not to impair the function of the aerobic platinum-based catalyst mixture of component (C), which will be described later, it is advisable to reduce the oxygen and water contents in the organohydrogenpolysiloxane of component (B) before blending it into the composition. This can be done, for example, by replacing the atmosphere with an inert gas such as nitrogen gas, by heating or reducing the pressure, or by a combination of these methods.
[0031] [(C) Platinum-Based Catalyst Mixture Activated by Moisture and / or Oxygen] The platinum-based catalyst mixture activated by moisture and / or oxygen, component (C), is activated upon contact with moisture and / or oxygen, particularly atmospheric moisture (humidity) and / or oxygen, and acts as a hydrosilylation addition reaction catalyst. This aerobic platinum-based catalyst mixture comprises a reaction mixture of a platinum-alkenyl group-containing organosiloxane complex and an organosilicon compound having at least one silicon-bonded hydrogen atom (SiH group) per molecule, in an amount such that the silicon-bonded hydrogen atom (SiH group) is in molar excess (a molar ratio of greater than 1) relative to the alkenyl groups in the platinum-alkenyl group-containing organosiloxane complex. Furthermore, this platinum-based catalyst mixture has also been confirmed to be activatable by ultraviolet light, and curing of the composition can be promoted by irradiating the composition with ultraviolet light. In the present invention, "aerobic" refers to a property (aerobic reaction type) in which, while catalytic activity as a hydrosilylation addition reaction catalyst is low in an oxygen-free, low-moisture, sealed state where contact with moisture (humidity) and oxygen is blocked, the catalyst is activated as a hydrosilylation addition reaction catalyst upon contact with moisture (humidity) and / or oxygen in the atmosphere. Furthermore, "sealed state (or under sealing)" refers to a state in which contact with the atmosphere is blocked (i.e., contact with moisture (humidity) and oxygen is blocked), and a sealed container refers to a container that achieves this sealed state.
[0032] In the platinum catalyst mixture of component (C), the platinum-alkenyl group-containing organosiloxane complex is preferably a complex of platinum, platinum chloride, chloroplatinic acid or a chloroplatinate salt with a vinyl group-containing siloxane (for example, an organodisiloxane compound having two alkenyl groups per molecule, such as 1,3-divinyl-1,1,3,3-tetramethyldisiloxane). For example, in the case of a complex of chloroplatinic acid (HPtCl) and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, three molecules of the bidentate ligand 1,3-divinyl-1,1,3,3-tetramethyldisiloxane are coordinated to one molecule of chloroplatinic acid.
[0033] The platinum-alkenyl group-containing organosiloxane complex is preferably used by dissolving it in a solvent such as toluene, a lower alcohol, a higher alcohol, a silicone-based solvent, etc. In this case, the platinum atom content (concentration) in the solution is preferably 0.05 to 5 mass %.
[0034] In the platinum catalyst mixture of component (C), the organosilicon compound having at least one silicon-bonded hydrogen atom (SiH group) per molecule can be an organohydrogensilane, an organohydrogensiloxane oligomer, or the like, having at least one SiH group per molecule (e.g., 1 to 10, preferably 1 to 5). From the standpoints of ease of handling and safety, however, organohydrogensiloxane oligomers are more preferred. The molecular structure of this organohydrogensiloxane oligomer may be linear or cyclic, and the number of silicon atoms per molecule is preferably 2 to 40, more preferably 2 to 10, and even more preferably 2 to 5.
[0035] Examples of the organohydrogensilane and organohydrogensiloxane oligomer used in the present invention include trialkoxy(hydrogen)silane, alkyldialkoxy(hydrogen)silane, dialkylalkoxy(hydrogen)silane, 1,1,1,3,3-pentamethyldisiloxane, 1,1,3,3-tetramethyldisiloxane, 1,1,1,3,5,5,5-heptamethyltrisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, 1,1,1,3,5,7,7,7-octamethyltetrasiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, and 1,3,5,7,9-pentamethylcyclopentasiloxane. These compounds may be used alone or in combination of two or more.
[0036] The platinum catalyst mixture of component (C) is a reaction mixture in which the alkenyl groups in the platinum-alkenyl group-containing organosiloxane complex react with SiH groups derived from the organosilicon compound, which is added during preparation of the mixture in a molar excess relative to the alkenyl groups (i.e., more than 1 mole, preferably about 1.1 to 30 moles, more preferably about 1.5 to 25 moles, and even more preferably about 5 to 25 moles per mole of alkenyl groups), in a moisture- and oxygen-free atmosphere (for example, an oxygen-free, sealed environment with low moisture content that is isolated from contact with moisture (humidity) and oxygen), resulting in all of the alkenyl groups being converted to alkylene groups by a hydrosilylation addition reaction (the alkenyl groups have essentially disappeared), and in which excess SiH groups derived from the organosilicon compound remain in the mixture.
[0037] The platinum catalyst mixture of component (C) is prepared by mixing the platinum-alkenyl group-containing organosiloxane complex and the organosilicon compound having at least one silicon-bonded hydrogen atom (SiH group) per molecule in a proportion such that the SiH groups of the organosilicon compound are in molar excess relative to the alkenyl groups in the platinum-alkenyl group-containing organosiloxane complex in a moisture- and oxygen-free atmosphere to obtain a reaction mixture.
[0038] Here, the blending ratio in which the SiH groups of the organosilicon compound having at least one hydrogen atom bonded to a silicon atom (SiH group) per molecule are in excess molar amount relative to the alkenyl groups in the platinum-alkenyl group-containing organosiloxane complex means that the blending amounts of the platinum-alkenyl group-containing organosiloxane complex and the organosilicon compound are such that the SiH groups in the organosilicon compound are greater than 1 mole, preferably 1.1 to 30 moles, more preferably 1.5 to 25 moles, and even more preferably about 5 to 25 moles, per mole of alkenyl groups in the complex.
[0039] The mixing method is not particularly limited as long as it is a method that uniformly mixes the platinum-alkenyl group-containing organosiloxane complex and the organosilicon compound having at least one hydrogen atom bonded to a silicon atom (SiH group) per molecule. However, it is preferred to use, for example, a glass reactor such as a glass flask or a stainless steel reactor.
[0040] The mixing atmosphere is preferably moisture- and oxygen-free, and is preferably an inert gas atmosphere such as nitrogen or a reduced pressure (vacuum). The temperature during mixing does not need to be elevated, and room temperature is sufficient. The mixing time (i.e., reaction time) may be any time required to uniformly mix the platinum-alkenyl group-containing organosiloxane complex and the organosilicon compound having at least one silicon-bonded hydrogen atom (SiH group) per molecule, and is preferably, for example, 0.5 to 100 hours, and particularly preferably 1 to 24 hours.
[0041] Furthermore, in the platinum-based catalyst mixture of component (C), when the organosilicon compound having at least one hydrogen atom bonded to a silicon atom (SiH group) per molecule is an organohydrogensiloxane oligomer having at least two hydrogen atoms (hereinafter sometimes referred to as adjacent SiH groups) bonded to adjacent silicon atoms (hereinafter sometimes referred to as adjacent silicon atoms) via ether oxygen atoms that form a siloxane bond (Si—O—Si) per molecule (for example, when the organosilicon compound is 1,1,3,3-tetramethyldisiloxane, 1,1,1,3,5,7,7,7-octamethyltetrasiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5,7,9-pentamethylcyclopentasiloxane, etc.), In this case, the reaction mixture is preferably prepared by uniformly mixing the organohydrogensiloxane oligomer having at least two vicinal SiH groups and the platinum-alkenyl group-containing organosiloxane complex in a moisture- and oxygen-free atmosphere, and then contacting the resulting mixture with moisture and / or oxygen by means of mixing in the air, or by mixing the organohydrogensiloxane oligomer having at least two vicinal SiH groups and the platinum-alkenyl group-containing organosiloxane complex in a blending ratio such that the SiH groups in the organohydrogensiloxane oligomer having at least two vicinal SiH groups are in molar excess relative to the alkenyl groups in the platinum-alkenyl group-containing organosiloxane complex, while still in contact with moisture and / or oxygen. As a result, a curable liquid silicone composition containing this mixture as a hydrosilylation addition reaction catalyst can exhibit improved long-term one-part storage stability in a sealed state, without losing its curability when exposed to atmospheric moisture (humidity) and / or oxygen, provided that the system (composition) is substantially free of moisture and oxygen during storage.
[0042] When the organosilicon compound having at least one silicon-bonded hydrogen atom (SiH group) per molecule is an organohydrogensiloxane oligomer having at least two hydrogen atoms (adjacent SiH groups) per molecule, each bonded to adjacent silicon atoms via an ether oxygen atom forming a siloxane bond (Si—O—Si), the preparation method preferably includes a step of further mixing the reaction mixture obtained by mixing in the moisture- and oxygen-free atmosphere while contacting it with moisture and / or oxygen. This step involves contacting the reaction mixture with moisture and / or oxygen by means of mixing in air, for example. The mixing time in air is preferably 0.5 to 100 hours, particularly 1 to 12 hours. The platinum-based catalyst mixture is then placed in a sealed container.
[0043] Furthermore, when the organosilicon compound having at least one silicon-bonded hydrogen atom (SiH group) per molecule is an organohydrogensiloxane oligomer having at least two hydrogen atoms (adjacent SiH groups) per molecule, each hydrogen atom being bonded to adjacent silicon atoms via an ether oxygen atom forming a siloxane bond (Si—O—Si), another preparation method involves mixing a platinum-alkenyl group-containing organosiloxane complex with the organohydrogensiloxane oligomer in contact with moisture and / or oxygen at the aforementioned blending ratio such that the SiH groups in the organohydrogensiloxane oligomer are in molar excess relative to the alkenyl groups in the platinum-alkenyl group-containing organosiloxane complex. This preparation method involves contacting the components with moisture and / or oxygen by means such as mixing in air, with the mixing time in air being preferably 0.5 to 100 hours, more preferably 1 to 12 hours. Thereafter, the platinum-based catalyst mixture is placed in a sealed container.
[0044] Component (C) may be used alone or in combination with two or more. The amount of the platinum catalyst mixture in component (C) is 0.1 to 1,000 ppm, preferably 0.5 to 200 ppm, of platinum atoms contained in component (C) relative to the total mass of components (A) and (B). If the amount of component (C) is less than the above range, the curable liquid silicone composition will not cure sufficiently due to catalyst inhibition factors, while if the amount is greater than the above range, the shelf life will be poor. Note that, because the amount of component (C) is a so-called catalytic amount, any excess molar amount of SiH groups remaining in component (C) is negligibly small and does not substantially affect the molar ratio of SiH groups in component (B) to alkenyl groups in component (A).
[0045] [(D) Dehydrating Agent] The dehydrating agent (D) is incorporated to remove water from the curable liquid silicone composition of the present invention, and by incorporating the dehydrating agent (D), it becomes possible to obtain even better storage stability.
[0046] As mentioned above, the platinum catalyst mixture of component (C), which is one of the core technologies of the present invention, has the property that its catalytic activity is kept low in an oxygen-free, low-moisture environment where it is isolated from contact with moisture (humidity) and oxygen, but that its catalytic function as a hydrosilylation addition reaction catalyst is activated upon contact with moisture and / or oxygen from the outside air (atmosphere) (aerobic reaction type). For this reason, it has been confirmed that reducing the amount of moisture in each component and in the mixed composition improves the one-component shelf life of the curable liquid silicone composition, and introducing a mechanism (dehydration using a dehydrating agent (D)) that consumes moisture from each component in the composition and trace amounts of moisture that enter from outside the container within the composition when stored in a sealed container is useful in ensuring one-component shelf life.
[0047] As the dehydrating agent for component (D), either an inorganic or organic compound will do, provided it does not impair the functions of components (A), (B), and (C). However, depending on the dehydrating agent, compounds produced as by-products in the dehydration reaction may cause foaming. Furthermore, many dehydrating agents may also cause decomposition of the organohydrogenpolysiloxane of component (B) or the organosilicon compound containing at least one silicon-bonded hydrogen atom (SiH group) per molecule contained in component (C), or may reduce the catalytic activity of the platinum-based catalyst mixture of component (C).
[0048] Therefore, silyl ketenes (including silyl ketene acetals), silyl enol esters, and α-silyl esters are suitable as dehydrating agents for component (D), as they enable efficient in-situ dehydration. These compounds have a structure in which the by-products produced during dehydration do not impair the functions of components (A), (B), and (C). Furthermore, they dissolve in the curable liquid silicone composition, allowing for the formation of a stable curable liquid silicone composition. Among these, silyl ketenes (including silyl ketene acetals) and α-silyl esters undergo dehydration reactions under non-basic conditions, and therefore do not decompose the organohydrogenpolysiloxane of component (B) or the organosilicon compound containing at least one silicon-bonded hydrogen atom (SiH group) per molecule contained in component (C), or do not reduce the catalytic activity of the platinum-based catalyst mixture of component (C).
[0049] Examples of silyl ketenes (containing silyl ketene acetals) include 1-methoxy-2-methyl-1-(trimethylsiloxy)propene, dimethyl ketene trimethylsilyl acetal, and tert-butoxy-1-(trimethylsiloxy)propene.
[0050] Examples of α-silyl esters include ethyl 2-(trimethoxysilyl)propionate (ECMS) and octyl 2-(methyldimethoxysilyl)propionate (OCMS-2).
[0051] The dehydrating agent of component (D) may be added to each component in advance, during the preparation of the composition, or after the composition has been prepared. The amount added is 0.01 to 5 parts by mass per 100 parts by mass of the combined total of components (A) and (B), and is preferably 0.01 to 5% by mass, particularly 0.1 to 2% by mass, of the total composition. If the amount of component (D) added is too small, the dehydrating effect may be insufficient, while if the amount of component (D) added is too large, this may adversely affect the changes in the physical properties of the cured product during heat resistance.
[0052] [(E) Organic Zirconium Compound] Component (E) is an organic zirconium compound that functions as a catalyst (i.e., a dehydration promoter) for promoting the reaction between the dehydrating agent (D) and water. Specific examples of the organic zirconium compound for component (E) include zirconium alkoxyester compounds such as tetraethoxyzirconium, tetra-normal-propoxyzirconium, tetraisopropoxyzirconium (also known as tetra(isopropyl)zirconate), tetra-normal-butoxyzirconium (also known as tetra(normal-butyl)zirconate), and tetra(2-ethylhexyloxy)zirconium; and zirconium chelate compounds such as zirconium diisopropoxybis(ethylacetoacetate) and zirconium tetraacetylacetonate.
[0053] The amount of component (E) added is 0.001 to 5 parts by mass per 100 parts by mass of the combined total of components (A) and (B), and is preferably 0.001 to 5% by mass, and particularly preferably 0.01 to 1% by mass, of the entire composition. If the amount of component (E) added is too small, water removal (dehydration) within the composition may be insufficient, while if the amount of component (E) added is too large, it may cause deterioration of the organohydrogenpolysiloxane (crosslinking agent) of component (B).
[0054] The organic zirconium compound may be used as is, or may be diluted with a solvent as necessary from the viewpoint of workability, etc. In this case, examples of the solvent include lower alcohols such as toluene, isopropanol (IPA), and normal butanol, higher alcohols, and silicone-based solvents. In this case, the content of the organic zirconium compound in the solution is preferably 1% by mass or more.
[0055] Examples of catalysts with similar functions as dehydration accelerators include titanate esters (tetra(isopropyl)titanate (TPT), tetrabutyl titanate (TBT), tetra(2-ethylhexyl)titanate (TOT), etc.) and titanium chelate compounds (titanium diisopropoxybis(ethylacetoacetate), titanium tetraacetylacetonate, etc.), but these cause coloration or yellowing of the cured product and are therefore not applicable to the object of the present invention of obtaining a colorless and transparent cured product that allows easy observation of the inside of the cured product and is effective for verifying defects in sealing parts, etc. Further, examples of dehydration accelerators include tin compounds (dibutyldimethoxytin, dibutyltin dilaurate, etc.), but their use is not preferred due to environmental impact concerns.
[0056] [Other Components] In addition to the components (A) through (E) described above, the curable liquid silicone composition of the present invention can contain various optional components, as described below, as needed, provided that the object of the present invention is not impaired.
[0057] [(F) Hydrosilylation Addition Reaction Inhibitor] It is also useful to further incorporate, as an optional component, a hydrosilylation addition reaction inhibitor (component (F)) into the curable liquid silicone composition of the present invention, if necessary, for the purpose of improving the storage stability of the one-component composition.
[0058] As described above, the platinum catalyst mixture of component (C) of the composition of the present invention has the property that its catalytic function is activated by contact with moisture and / or oxygen. Therefore, moisture in each component, moisture mixed in during the composition preparation process or the container filling process, and oxygen and moisture entering from outside the sealed container may cause a portion of the platinum catalyst mixture of component (C) to be activated as a hydrosilylation addition reaction catalyst. This partially activated catalyst may significantly reduce the one-component shelf life of the composition. However, the supplemental incorporation of a hydrosilylation addition reaction inhibitor, component (F), can suppress such a decrease in one-component shelf life.
[0059] Examples of hydrosilylation addition reaction inhibitors include acetylene alcohols such as 1-ethynylcyclohexanol and 3-methyltridec-1-yn-3-ol (EMDC), silanes of acetylene alcohols such as dimethylbis(1,1-dimethyl-2-propynyloxy)silane (PLR-22) and 3-(trimethylsilyloxy)-3-methyl-1-butyne (PLR-31), siloxane-modified products, tri(isopropyl)phosphite, tris(di-tert-butylphenyl)phosphite, triphenylphosphite, tris(2-ethylhexyl)phosphite, and the like. Examples of suitable compounds include compounds selected from the group consisting of phosphorous acid compounds (particularly phosphite esters) such as tri(isopropyl)phosphite and tris(di-tert-butylphenyl)phosphite, ethylenediamines such as tetramethylethylenediamine, benzotriazoles such as 5-methyl-1H-benzotriazole, and mixtures thereof. In particular, phosphorous acid compounds, and particularly the phosphorous acid esters tri(isopropyl)phosphite and tris(di-tert-butylphenyl)phosphite are preferred, as they provide a curable liquid silicone composition that has good one-component storage stability when shielded from light and sealed.
[0060] The amount of the hydrosilylation addition reaction inhibitor (component (F)) may be any amount that does not affect the curability of the composition of the present invention, depending on the performance of the respective hydrosilylation addition reaction inhibitor. Preferably, however, the amount added is within a range that does not impair the curability of the composition through the hydrosilylation addition reaction promoted by the platinum-based catalyst mixture (component (C)) activated by exposure to the atmosphere (moisture and / or oxygen). In the case of a phosphorous acid compound such as a phosphite ester, the amount added may be small, less than 1 mole, particularly about 0 to 0.75 moles, per mole of platinum atoms contained in the composition. When incorporated, an amount of 0.1 mole or more per mole of platinum atoms contained in the composition is preferred. Addition of too much component (F) may deactivate the platinum-based catalyst mixture (component (C)) activated by moisture and / or oxygen during use, or, in the case of component (G) described below, the platinum-based catalyst (component (G)) activated by ultraviolet light during use, thereby potentially reducing the curability when exposed to the atmosphere.
[0061] [(G) Platinum-Based Catalyst Activated by Ultraviolet Light] As mentioned above, the platinum-based catalyst mixture of component (C) is catalytically activated by ultraviolet light in addition to oxygen / air. However, if it is necessary to impart even more pronounced curing acceleration by ultraviolet light, it is possible to add an ultraviolet-activated platinum-based catalyst. The platinum-based catalyst is activated by light with a wavelength of 200 to 500 nm, preferably ultraviolet light with a wavelength of 200 to 410 nm. In other words, the platinum-based catalyst is inactive in the dark and, upon exposure to light with a wavelength of 200 to 500 nm, preferably ultraviolet light with a wavelength of 200 to 410 nm, it is converted into a platinum-based catalyst (hydrosilylation addition reaction catalyst) that is active at room temperature and is capable of promoting the hydrosilylation addition reaction between alkenyl groups in component (A) and silicon-bonded hydrogen atoms in component (B).
[0062] Examples of the platinum catalyst activated by ultraviolet light, component (G), include platinum acetylacetonato complexes and platinum cyclopentadienyl complexes, as disclosed in U.S. Pat. Nos. 4,510,094 and 4,530,879. Specific examples of component (G) include complexes of (η5-cyclopentadienyl)trialiphatic platinum compounds. Of these, cyclopentadienyltrimethylplatinum complexes and methylcyclopentadienyltrimethylplatinum complexes are preferred. Also included are complexes of bis(β-diketonato)platinum compounds. Of these, bis(acetylacetonato)platinum complexes are preferred.
[0063] The platinum-based catalyst activated by ultraviolet light is preferably used by dissolving it in a solvent such as toluene, a lower alcohol, a higher alcohol, a silicone-based solvent, etc. In this case, the content (content concentration) of the platinum-based catalyst activated by ultraviolet light in the solution is preferably 0.05 to 5 mass %.
[0064] The amount of platinum catalyst in component (G) is preferably 0.1 to 1,000 ppm, more preferably 0.1 to 500 ppm, and even more preferably 0.1 to 50 ppm, of platinum atoms contained in component (G) relative to the total mass of components (A) and (B). In particular, in the low-coloration composition of the present invention, ultraviolet light can easily penetrate deep into the composition, resulting in good ultraviolet curability.
[0065] In addition to the optional components (F) hydrosilylation addition reaction inhibitor and (G) ultraviolet-activated platinum catalyst, the curable liquid silicone composition of the present invention may also contain, as necessary, other optional components such as inorganic fillers, adhesion promoters, pigment pastes, and reinforcing silicone resins.
[0066] The curable liquid silicone composition of the present invention can be prepared by mixing the above components (A) to (E) and, if necessary, other components in a conventional manner, but it is preferable to add (A) the alkenyl group-containing diorganopolysiloxane, (B) the organohydrogenpolysiloxane, (D) the dehydrating agent, (E) the organozirconium compound, and (C) the platinum catalyst mixture activated by moisture and / or oxygen in this order while mixing. When (F) the hydrosilylation addition reaction inhibitor is added, it is preferably added after (E) the organozirconium compound. When (G) the platinum catalyst activated by ultraviolet light is added, it is preferably added after (C) the platinum catalyst mixture activated by moisture and / or oxygen.
[0067] The curable liquid silicone composition of the present invention can achieve better one-component shelf life by using a highly airtight container that can block or reduce the intrusion of oxygen and moisture, particularly atmospheric moisture (humidity) and oxygen, and storing the composition in a light-shielded sealed container. This makes it possible to distribute and sell the composition as a one-component curable liquid silicone composition. Furthermore, when the curable liquid silicone composition of the present invention is opened in a sealed container and exposed to the atmosphere at room temperature, and exposed to atmospheric moisture (humidity) and / or oxygen, it rapidly cures not only on the surface exposed to air but also in the interior / shadow areas, giving a silicone rubber or silicone gel cured product with little coloration.
[0068] [Method for curing curable liquid silicone composition] The curable liquid silicone composition of the present invention is usually cured by a step of exposing it to the atmosphere at room temperature for a predetermined period of time. However, it is also possible to cure it by a step of irradiating the curable liquid silicone composition with ultraviolet light at room temperature, followed by a step of exposing it to the atmosphere at room temperature for a predetermined period of time.
[0069] [Ultraviolet Light Irradiation Step] The ultraviolet light irradiation step can be carried out to promote curing of the composition, and involves irradiating the curable liquid silicone composition of the present invention with ultraviolet light at room temperature (23°C ± 15°C), preferably with light of 200 to 500 nm at room temperature. By irradiating with ultraviolet light, the platinum-based catalyst mixture of component (C) and the platinum-based catalyst of component (G) in the ultraviolet-irradiated section are activated and act as a hydrosilylation addition reaction catalyst, promoting the hydrosilylation addition reaction and curing the ultraviolet-irradiated section. There are no particular restrictions on the lamp used to irradiate ultraviolet light, as long as it can supply ultraviolet light with a wavelength of 200 to 500 nm. Examples include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, xenon lamps, metal halide lamps, and ultraviolet LED lamps. The amount of ultraviolet light irradiation varies depending on the type and amount of the photoactive platinum complex (the platinum-based catalyst mixture of component (C) and the platinum-based catalyst of component (G)) used, but it is sufficient as long as it is an amount sufficient to activate the photoactive platinum complex, and is generally 10 to 1,000 mW / cm. 2 , especially 20 to 400 mW / cm 2 It is preferable to irradiate the ultraviolet light having the above intensity for 0.1 seconds to 5 minutes, and particularly for 0.5 seconds to 1 minute.
[0070] [Step of Exposing to the Atmosphere] The step of exposing to the atmosphere involves exposing the curable liquid silicone composition of the present invention to the atmosphere at room temperature for a predetermined time (usually 0.5 hours or more, preferably 1 to 48 hours, and more preferably 2 to 24 hours) by exposing the curable liquid silicone composition of the present invention to the atmosphere at room temperature (23°C±15°C) for a predetermined time (usually 0.5 hours or more, preferably 1 to 48 hours, and more preferably 2 to 24 hours), which activates the platinum catalyst mixture of component (C) and causes it to act as a hydrosilylation addition reaction catalyst, further promoting the hydrosilylation addition reaction and thereby curing particularly areas that are shaded by ultraviolet irradiation or that are not reached by ultraviolet light.
[0071] The silicone rubbers and silicone gels that are cured products of the curable liquid silicone composition of the present invention obtained in this manner have excellent low colorability (transparency), heat resistance, and electrical insulation properties, and are applicable to automotive parts, aircraft, home appliances, and the like.
[0072] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The viscosity is measured at 23°C using a rotational viscometer, and the degree of polymerization is the number-average degree of polymerization in terms of polystyrene measured by GPC analysis using toluene as the developing solvent. Me represents a methyl group, and Vi represents a vinyl group. "Room temperature" means 23°C.
[0073] Examples 1 to 4, Comparative Examples 1 to 5 Curable liquid silicone compositions were prepared as follows. (Preparation of Curable Liquid Silicone Composition) Each composition was prepared by uniformly mixing the components in the amounts shown in Table 2 below in a brown glass bottle under a nitrogen atmosphere at room temperature (23°C), and then sealing the bottle in a light-shielded condition. The molar ratio of SiH groups in component (B) to vinyl groups in component (A) was approximately 1.0. The components were added in the following order while mixing: (A) alkenyl group-containing diorganopolysiloxane, (B) organohydrogenpolysiloxane, (D) dehydrating agent, (E) dehydration accelerator, (F) hydrosilylation addition reaction inhibitor, (C) platinum-based catalyst mixture activated by moisture and / or oxygen, and (G) platinum-based catalyst activated by ultraviolet light. If a component was not added, that component was skipped and the addition of the subsequent components was continued. To ensure reproducible preparation of the composition, (A) the alkenyl group-containing diorganopolysiloxane and (B) the organohydrogenpolysiloxane were each previously dehydrated by degassing under reduced pressure in a glass flask at 120° C. The mixing and container-filling steps for the composition were carried out under a nitrogen atmosphere.
[0074] The components are as follows: (A) Alkenyl group-containing diorganopolysiloxane: A vinyl group-containing branched diorganopolysiloxane having a viscosity of 800 mPa·s at 23° C. and represented by the following average formula:
[0075] (B) Organohydrogenpolysiloxane: A linear organohydrogenpolysiloxane represented by the following average formula:
[0076] (C) Aerobic Platinum-Based Catalyst Mixture: An aerobic platinum-based catalyst mixture prepared as follows was used. Under a nitrogen atmosphere at room temperature (23°C), 8.0 g of a toluene solution of a platinum-alkenyl group-containing organosiloxane complex (platinum atom content: 0.5% by mass) and 2.0 g of 1,1,3,3-tetramethyldisiloxane were mixed uniformly and reacted in a 25 g glass bottle over a period of 12 hours, and the mixture was then mixed uniformly in air at room temperature (23°C) while being in contact with the air for 2 hours, after which the bottle was sealed to prepare an aerobic platinum-based catalyst mixture.
[0077]
[0078] (D) Dehydrating agent: ethyl 2-(trimethoxysilyl)propionate (ECMS)
[0079] (E) Dehydration accelerator: (E-1) tetra(isopropyl)zirconate (75% by mass IPA solution) (E-2) tetra(normal butyl)zirconate (87% by mass normal butanol solution) (E-3) tetra(isopropyl)titanate (TPT / 100% by mass) (E-4) tetra(2-ethylhexyl)titanate (TOT / 100% by mass)
[0080] (F) Hydrosilylation addition reaction inhibitor: Tris(di-tert-butylphenyl)phosphite (0.31% by mass toluene solution) represented by the following formula:
[0081] (G) Platinum catalyst activated by ultraviolet light: Toluene solution of methylcyclopentadienyltrimethylplatinum complex (platinum content 0.5% by mass)
[0082] The prepared curable liquid silicone compositions were evaluated for the appearance of the cured product (colorability, internal visibility), one-component storage stability under light-shielded and sealed conditions, curability after UV irradiation after storage, and aerobic curability after storage, as described below.
[0083] [Appearance of Cured Product] The appearance of the cured product was evaluated visually, and included colorability and internal visibility. Colorability was evaluated by visually checking the color tone, including the degree of transparency (transparent, translucent) of the cured product. Internal visibility was evaluated by placing a printed material under a 20 mm thick cured gel product cured in a glass petri dish, and visually checking the characters (8 pt Mincho font) on the printed material. If the characters were readable, the evaluation was good; if the characters were illegible but visible, the evaluation was fair; and if the characters were not visible, the evaluation was poor.
[0084] [Single-component storage stability (light-shielding and sealed)] To determine the single-component storage stability, fill a brown glass bottle with a curable liquid silicone composition under a nitrogen atmosphere, seal it, and then leave the brown glass bottle in the air / room temperature, and observe the thickening and gelling behavior of the curable liquid silicone composition.At this time, when tilting the brown glass bottle, observe the degree to which the composition in the brown glass bottle flows along with the tilt (fluidity), and judge the state in which the fluidity becomes worse than that immediately after sealing as the curable liquid silicone composition has thickened or gelled.In addition, at this time, leave the brown glass bottle with the sealed curable liquid silicone composition in the air / room temperature, and then observe for 5 minutes, and then observe every day to confirm the time (minutes, days) until the curable liquid silicone composition thickens or gels.
[0085] For evaluation of post-UV curability and aerobic curability, a curable liquid silicone composition that had been stored in a sealed brown glass bottle for one day was used, as described above.
[0086] [Curing property after ultraviolet irradiation] The curing property after ultraviolet irradiation was measured by casting 50 g of each composition prepared in the examples and comparative examples into a black plastic petri dish having a diameter of 60 mm and a depth of 30 mm, and irradiating the composition with a UV-LED lamp having a wavelength of 365 nm at 23°C at an irradiation intensity of 100 mW / cm. 2 and a dose of 3,000 mJ / cm 2After irradiating with UV light so that the composition was cured, the composition was left to stand in the air at 23°C, and the cured product was removed from the plastic petri dish and the state of cure (deep curing) was confirmed. Observation was performed 10 minutes, 30 minutes, 1 hour, 6 hours, and 24 hours after UV irradiation. A sample with no cured or gelled areas on the surface or inside was considered uncured, a sample with cured or gelled areas only on the surface was considered to be surface-only cured, a sample with no deformation due to its own weight when tilted was considered to have stopped flowing, and a sample with uniform overall curing was considered to be gel-cured.
[0087] [Aerobic Curability] Aerobic curability (shadow curability (unirradiated with UV)) was determined by placing an aluminum plate (25 mm × 50 mm) with 1 mm spacers on both ends in an aluminum Petri dish with a diameter of 60 mm and a depth of 1 mm, and then casting 25 g of each composition prepared in the Examples and Comparative Examples into multiple samples. The compositions were allowed to stand in the air at 23°C to cure, and the cured state of the backside of the aluminum plate was visually confirmed 10 minutes, 30 minutes, 1 hour, 6 hours, and 24 hours after irradiation with UV light. A sample with no hardened or gelled areas on the surface or inside was judged to be uncured; a sample with no deformation due to its own weight when tilted was judged to have stopped flowing; and a sample with uniform curing throughout was judged to be gel-cured.
[0088]
[0089] The above results confirmed that the curable liquid silicone composition of the present invention has excellent one-component storage stability in a light-shielded, airtight container, and that the platinum-based catalyst mixture is activated after standing in the atmosphere, allowing the hydrosilylation addition reaction to proceed even in shaded areas, resulting in a rubbery or gel-like cured product that is transparent, has low coloration, and is easy to see inside.Furthermore, because of its high transparency, it also has excellent deep-section curing properties when cured with ultraviolet light, and it has been confirmed that there is a possibility of shortening the process time when sealing parts.
Claims
1. A curable liquid silicone composition comprising: (A) a diorganopolysiloxane having at least one alkenyl group per molecule; (B) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms per molecule, in an amount such that there are 0.5 to 4 moles of hydrogen atoms bonded to silicon atoms in component (B) per mole of alkenyl groups in component (A); (C) a platinum-based catalyst mixture activated by moisture and / or oxygen, in an amount such that the platinum atoms in component (C) are 0.1 to 1,000 ppm by mass relative to the combined mass of components (A) and (B); (D) a dehydrating agent, in an amount of 0.01 to 5 parts by mass per 100 parts by mass of components (A) and (B); and (E) an organozirconium compound, in an amount of 0.001 to 5 parts by mass per 100 parts by mass of components (A) and (B).
2. The curable liquid silicone composition according to claim 1, wherein the dehydrating agent of component (D) is at least one compound selected from the group consisting of silyl ketenes and α-silyl esters.
3. The curable liquid silicone composition according to claim 1, wherein component (C) is an aerobic platinum-based catalyst mixture consisting of a reaction mixture of a platinum-alkenyl group-containing organosiloxane complex and an organosilicon compound having at least one hydrogen atom bonded to a silicon atom per molecule in such an amount that there is a molar excess of hydrogen atoms bonded to silicon atoms relative to the alkenyl groups in the platinum-alkenyl group-containing organosiloxane complex.
4. A cured product of the curable liquid silicone composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Curable composition
JP2001254025A
Curable resin composition
WO2014021419A1
Curing catalyst, curable resin composition, and cured object obtained therefrom
WO2016027471A1
Platinum catalyst mixture, curable liquid silicone composition and method for curing curable liquid silicone composition, and method for preparing platinum catalyst mixture