High hardness au-ni-pd-pt-based noble metal alloy

The Au-Ni-Pd-Pt alloy with added metal elements achieves high hardness through spinodal decomposition and ordering, overcoming the limitations of conventional strengthening methods and ensuring high wear resistance and biocompatibility for medical and electronic applications.

WO2024214666A1PCT designated stage expired Publication Date: 2024-10-17TANAKA KIKINZOKU KOGYO KK
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014224
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-08
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional noble metal alloys face limitations in achieving high hardness due to the limitations of existing strengthening mechanisms such as solid solution strengthening, precipitation hardening, and work hardening, which can lead to material embrittlement and insufficient hardness, particularly in applications requiring high wear resistance and biocompatibility.

Method used

A high hardness Au-Ni-Pd-Pt noble metal alloy is developed by utilizing spinodal decomposition and ordering phenomena, with the addition of metal element α, such as In, Sn, Mg, Al, or Ti, to enhance hardness without relying on work hardening, thereby creating a modulated or ordered structure that increases Vickers hardness to 500 Hv or more.

Benefits of technology

The alloy achieves unprecedented hardness without causing material embrittlement, effectively addressing the limitations of conventional strengthening methods by leveraging spinodal decomposition and ordering to provide high wear resistance and biocompatibility suitable for medical and electronic applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014224_17102024_PF_FP_ABST
    Figure JP2024014224_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is an Au-Ni-Pd-Pt-based noble metal alloy obtained by adding a metal element α to a base alloy comprising Au, Ni, Pd, and Pt. In the present invention, the metal element α is at least one metal element selected from In, Sn, Mg, Al, and Ti. In addition, the noble metal alloy according to the present invention includes: Au at 4 to 24 atom%; Ni at 5 to 60 atom% or less; Pd at 2.5 to 40 atom%; Pt at 10 to 60 atom%; metallic element α at 0.15 to 7.5 atom%; and unavoidable impurities. The noble metal alloy according to the present invention is configured to have a high hardness as a result of a modulated structure due to spinodal decomposition and / or a regular phase due to regulation, and is configured to have a Vickers hardness of 500 Hv or more. The noble metal alloy according to the present invention is a high-hardness noble metal alloy to which a strengthening mechanism different from conventional methods such as work hardening and precipitation hardening has been applied.
Need to check novelty before this filing date? Find Prior Art

Description

High hardness Au-Ni-Pd-Pt noble metal alloy

[0001] The present invention relates to a high-hardness precious metal alloy containing the precious metals Au, Pt, and Pd as essential constituent metals, specifically, a precious metal alloy in which a predetermined metal element α is added to an Au—Ni—Pd—Pt alloy as a base alloy, and in which high hardness is achieved by spinodal decomposition and / or ordering.

[0002] Precious metals such as platinum (Pt) and gold (Au) have excellent chemical stability and corrosion resistance, as well as excellent electrical properties such as conductivity. Therefore, precious metals and their alloys are utilized in various fields, including electrical and electronics and medical fields. Examples of applications of precious metal alloys in the electrical and electronic fields include probe pins incorporated in probe cards for testing semiconductor devices, and electrical contacts (sliding contacts and open / close contacts) for motor brushes, relays, switches, and the like. Their use in the medical field has recently attracted attention, and precious metal alloys are used as components of various medical devices. Examples of such medical devices include various types of medical devices such as embolization coils, embolization clips, guidewires, stents, and catheters. These medical devices are implanted into the human body and therefore require biocompatibility and chemical stability. Furthermore, medical devices also require X-ray visibility for use in X-ray surgery and diagnosis. Precious metal alloys also exhibit excellent biocompatibility and X-ray visibility.

[0003] Precious metal alloys used in the various applications described above are required to have improved mechanical properties, such as hardness and strength. For example, probe pins are required to have wear resistance because they are subjected to repeated long-term contact with mating materials. In particular, the development of probe pins with even higher hardness is required to keep up with the recent trend toward higher integration of various devices and higher performance motors. Furthermore, in the case of medical devices, devices that are implanted and moved within pulsating blood vessels, such as guide wires and embolization coils, require mechanical properties such as hardness and springiness to prevent malfunction.

[0004] Because precious metal alloys are metallic materials, their hardness can be improved by applying common strengthening mechanisms used in metallic materials. That is, the hardness of conventional precious metal alloys has been improved by combining the strengthening mechanisms of work hardening (dislocation hardening), solid solution hardening, and precipitation hardening (dispersion hardening). Examples of hardening improvements in precious metal alloys used as probe pins and contact materials include the Pt—Ni alloy described in Patent Document 1 and the Pt—W alloy described in Patent Document 2. These alloys achieve increased hardness through solid solution hardening achieved by alloying Pt with Ni, W, or other metals, as well as work hardening achieved by increasing the final work rate. Furthermore, Patent Document 3 (Ag—Pd—Cu-based alloy) and Patent Document 4 (Pt—Cr—Ni-based alloy) achieve high hardness by adjusting the work rate in addition to solid solution hardening and precipitation hardening achieved by additive elements.

[0005] Japanese Patent Publication No. 2005-233967 Japanese Patent No. 6997354 Japanese Patent Publication No. 2012-242184 Japanese Patent No. 6372952

[0006] As described above, various applications require precious metal alloys to have improved mechanical properties such as hardness. To meet this demand, it may be necessary to further strengthen the alloys using the various strengthening mechanisms described above. However, with regard to solid solution strengthening and precipitation strengthening, attempts have been made to optimize the selection and amount of additive elements and the manufacturing process, such as heat treatment, but there is a limit to the amount of hardening that can be achieved. For example, in the precious metal alloys of Patent Documents 3 and 4, the increase in hardness due to precipitation hardening is approximately 150 Hv, and sufficient hardness cannot be achieved by precipitation hardening alone. In these precious metal alloys, the hardness is actually compensated for by work hardening in addition to precipitation hardening.

[0007] Furthermore, there are concerns about the excessive application of work hardening. Work hardening is a useful strengthening method because it produces a large amount of hardening, but on the other hand, it can cause embrittlement in the material. Material embrittlement can lead to breakage during wire drawing, cracking and fracture during secondary processing (pressing, coiling, bending, etc.), and actual use. Electrical materials such as probe pins and medical devices such as guide wires and embolization coils are made by processing thin wires, so it is necessary to ensure workability in the processing of thin wires. Therefore, when considering issues of material embrittlement and workability, it must be said that there is a limit to the amount of hardening that can be achieved by work hardening.

[0008] The present invention was made in light of the above background, and provides a precious metal alloy containing the precious metals Au, Pd, and Pt as essential constituent elements, which has been strengthened by a strengthening mechanism different from that conventionally used. In particular, the present invention proposes a material strengthening mechanism based on a process mainly consisting of heat treatment, without relying on work hardening, which is a concern due to the risk of embrittlement.

[0009] In order to solve the above problems, the present inventors have focused on two phenomena, spinodal decomposition and ordering, as a strengthening method different from the commonly used methods described above.

[0010] Spinodal decomposition is a type of phase separation in a material structure. It is a phenomenon in which decomposition progresses due to a continuous increase in concentration fluctuations, rather than the nucleation and growth process used in precipitation hardening. The material structure produced by spinodal decomposition caused by this concentration fluctuation exhibits a very fine periodic structure of several nanometers to several tens of nanometers, called a modulated structure. In the modulated structure generated by spinodal decomposition, the concentration of solute atoms in the crystal periodically fluctuates as a function of location, and the lattice constant also changes periodically. This generates a periodic internal stress field on the slip plane, which interacts with dislocations. The strengthening mechanism by spinodal decomposition is similar to precipitation strengthening by nucleation and growth, but differs in that the lattice constant change caused by concentration modulation, rather than precipitates, acts as an obstacle to dislocation movement. Furthermore, because spinodal decomposition strengthening exhibits a high hardening amount due to the fine modulated structure described above, it is considered useful as a means of improving hardness without inducing material embrittlement such as work hardening.

[0011] On the other hand, ordering is a phenomenon in which an ordered phase having a predetermined structure is formed by ordering the arrangement of the constituent elements of an alloy. The ordered phase formed by ordering contributes to increasing the hardness of the alloy due to the following factors: (i) the Burgers vector of dislocations becomes larger, (ii) antiphase boundaries can occur within the ordered phase, and (iii) the volume change associated with ordering distorts the lattice inside and outside the ordered phase, thereby suppressing dislocation motion. Ordering may occur in conjunction with the spinodal decomposition described above, or it may occur alone.

[0012] Regarding spinodal decomposition and ordering, these phenomena and the material structure that manifests them are publicly known. It is also publicly known that there are precious metal alloys with compositions that can cause spinodal decomposition and ordering. Regarding spinodal decomposition, Pt—Au alloys are known as precious metal alloys that can cause spinodal decomposition. Figure 1 shows a Pt—Au system phase diagram. Thermodynamic calculations have revealed the composition and temperature range (chemical spinodal curve) of Pt—Au alloys that can cause spinodal decomposition.

[0013] On the other hand, regarding ordering of precious metal alloys, Pt-Ni based alloys are known as alloys that can exhibit ordering. It is known that ordering in Pt-Ni based alloys occurs through solution treatment and aging treatment, and that ordering and hardening occur through aging treatment in the order-disorder transformation region or air cooling from the single phase region. In the ordering of this Pt-Ni based alloy, L1 0 Type structure or L1 2 An ordered phase with a crystalline structure can be formed. Although not as well known as Pt—Ni alloys, Au—Pd alloys are also known to have the potential for ordering. If ordering occurs in Au—Pd alloys, it is predicted that an ordered phase similar to that in Pt—Ni alloys will be formed, resulting in hardening.

[0014] Although it is known that spinodal decomposition and ordering can contribute to an increase in the hardness of alloy materials, the extent of the increase in hardness due to these processes is not particularly large in known alloy systems. For example, in the case of the Pt—Au alloy described above, even if hardening occurs due to spinodal decomposition, the extent of the increase in hardness is at most about 160 Hv, making it difficult to stably achieve a hardness of 500 Hv or more for precious metal alloys. Furthermore, it is also difficult to achieve a hardness of 500 Hv or more for Pt—Ni alloys, which can exhibit ordering.

[0015] Furthermore, although the phenomena and mechanisms of spinodal decomposition and ordering are well known, there are few specific examples of their application, especially to precious metal alloys. Therefore, the present inventors have considered that there is much room for improvement in spinodal decomposition and ordering as a method for hardening and strengthening precious metal alloys, and have decided to conduct further research. As a result, they have come up with the following two approaches to improvement.

[0016] The first approach taken by the present inventors to increase the hardness of precious metal alloys is to diversify the composition of the precious metal alloy. The present inventors believed that there was a limit to optimizing the composition within the range of binary alloys (Pt—Au alloys, Pt—Ni alloys, Au—Pd alloys, etc.) in order to maximize the hardening ability of precious metal alloys due to spinodal decomposition and ordering, and therefore considered the application of ternary or higher alloys. As a result of extensive research, the present inventors discovered that, for quaternary alloys of Au, Ni, Pd, and Pt as the precious metal alloy, optimizing the composition and performing appropriate heat treatment can effectively increase hardness due to spinodal decomposition and / or ordering.

[0017] The second approach to increasing the hardness of precious metal alloys is to use the above-mentioned Au—Ni—Pd—Pt alloy as a base alloy and further add another metal element to this base alloy. In the present invention, this added element is referred to as metal element α. This metal element α does not change the material structure due to spinodal decomposition and / or ordering that occurs in the Au—Ni—Pd—Pt alloy, but rather imparts an additional hardness increase to the base alloy strengthened by spinodal decomposition and / or ordering. Although the mechanism of this additional hardness increase is not clear, the inventors suspect several factors, such as the effect of metal element α on the matrix.

[0018] Based on the above two approaches, the present inventors conducted detailed studies on the range of the metal element α to be added to the base alloy, Au—Ni—Pd—Pt alloy, and the composition range of the Au—Ni—Pd—Pt alloy in which high hardness due to spinodal decomposition and / or ordering is effective when the metal element α is added, and arrived at the present invention.

[0019] That is, the present invention provides an Au-Ni-Pd-Pt based noble metal alloy obtained by adding a metal element α to a base alloy consisting of Au, Ni, Pd, and Pt, wherein the metal element α is at least one of In, Sn, Mg, Al, and Ti, and the Au-Ni-Pd-Pt based noble metal alloy contains 4 atomic % to 24 atomic % of Au, 5 atomic % to 60 atomic % of Ni, 2.5 atomic % to 40 atomic % of Pd, 10 atomic % to 60 atomic % of Pt, 0.15 atomic % to 7.5 atomic % of the metal element α, and unavoidable impurities.

[0020] As described above, the precious metal alloy made of the Au-Ni-Pd-Pt alloy according to the present invention contains a modulated structure and / or an ordered phase due to spinodal decomposition.

[0021] The Au—Ni—Pd—Pt-based noble metal alloy according to the present invention is hardened by spinodal decomposition and / or ordering, and the hardened Au—Ni—Pd—Pt-based noble metal alloy has a Vickers hardness of 500 Hv or more.

[0022] As explained above, the precious metal alloy according to the present invention is strengthened by a modulated structure due to spinodal decomposition and / or an ordered phase due to ordering, instead of the solid solution strengthening, precipitation strengthening, and work hardening that have been widely used until now as material strengthening methods. According to the present invention, a precious metal alloy with high hardness can be obtained by a strengthening ability not previously available, without relying on work hardening (dislocation strengthening), which may embrittle the material.

[0023] 1 is a diagram showing a Pt—Au system phase diagram and a spinodal curve in a Pt—Au alloy; 2 is a diagram showing XRD results of a solution-treated material and an aged material of the precious metal alloy (Au12.5-Ni30.625-Pd25-Pt30.625-Sn1.25) of Example B-5; 3 is a STEM-EDS mapping image showing a modulated structure of the precious metal alloy (Au12.5-Ni30.625-Pd25-Pt30.625-Sn1.25) of Example B-5; 4 is a diagram showing an ordered phase (L1 2 Electron diffraction pattern showing the structure.

[0024] The following describes embodiments of the present invention. As described above, the precious metal alloy according to the present invention is an Au—Ni—Pd—Pt-based alloy in which a predetermined metal element α is added to an Au—Ni—Pd—Pt alloy as a base alloy. The precious metal alloy according to the present invention includes, as its hardening factor, at least one of a modulated structure due to spinodal decomposition and an ordered phase due to ordering. In the following description, in order to disclose (A) the configuration of the precious metal alloy according to the present invention, the following items will be explained: (A-1) the strengthening mechanisms applied in the present invention (spinodal decomposition and ordering), (A-2) the constituent metals and their composition ranges of the precious metal alloy according to the present invention, (A-3) the material structure of the precious metal alloy according to the present invention, and (A-4) the hardness of the precious metal alloy according to the present invention. Furthermore, (B) the manufacturing method (heat treatment process) of the precious metal alloy according to the present invention will also be described.

[0025] (A) Structure of the Precious Metal Alloy According to the Present Invention (A-1) Strengthening Mechanism of the Precious Metal Alloy According to the Present Invention (1) Spinodal Decomposition As already mentioned, the structure formed by spinodal decomposition is called a modulated structure. In a modulated structure, periodic concentration fluctuations occur, which contribute to high hardness by forming an internal stress field around it. The resistance force (critical shear stress) to dislocation motion in this periodic internal stress field is expressed by the following formula, and the lattice strain (ε), elastic modulus (Y), and concentration modulation amplitude (A) are thought to be the governing factors (for detailed references, see, for example, "Introduction to Dislocation Theory" by Masaharu Kato (published in August 1999, published by Shokabo)).

[0026]

[0027] In a study based on the above formula (1), it is believed that, as a rough trend, the elastic modulus is proportional to the Young's modulus of each constituent metal, and the lattice strain ε is proportional to the lattice constant difference between the constituent metals. Furthermore, it is believed that the concentration modulation amplitude A in formula (3) exhibits a larger value as the mixing enthalpy between the metal elements increases. The lattice constants of Au, Ni, Pd, and Pt constituting the Au-Ni-Pd-Pt alloy, which is the base alloy of the present invention, are known to have the values ​​shown in Table 1 below. Furthermore, the mixing enthalpy values ​​are known to have the values ​​shown in Table 2 below (Reference: Akira Takeuchi, Akihisa Inoue, "Classification of Bulk Metallic Glasses by Atomic Size Difference, Heat of Mixing and Period of Constituent Elements and Its Application to Characterization of the Main Alloying Element", Materials Transactions, Vol. 46 (2005), pp. 2817-2829).

[0028]

[0029]

[0030] Referring to Table 2, the mixing enthalpy is positive in the combinations of Au—Pt, Au—Ni, and Pt—Pd. Although Au—Pt and Au—Ni alloys form a single phase at high temperatures, their binary phase diagrams reveal that they are characterized by very high values ​​of mixing enthalpy. The occurrence of spinodal decomposition and significant hardening due to modulated structure in the precious metal alloy according to the present invention can be estimated by taking into account the lattice constants in Table 1 and the mixing enthalpies in Table 2, based on the binary phase diagrams of the respective constituent metals, and by considering Equation 3. This point will be explained in more detail later.

[0031] (2) Ordering (Ordered Phase) As described above, the ordered phase generated by ordering contributes to increasing the hardness of the alloy through the Burgers vector of dislocations, the generation of antiphase boundaries within the ordered phase, and lattice strain due to volume changes associated with ordering. The precious metal alloy according to the present invention includes both metal combinations that constitute Pt—Ni-based alloys and Au—Pd-based alloys, which are known as metal combinations that cause ordering.

[0032] The precious metal alloy according to the present invention can also achieve high hardness due to the ordered phase formed by the manifestation of ordering, similar to Pt—Ni-based alloys and Au—Pd-based alloys. The structure of the ordered phase in the present invention is not necessarily completely clear, but it is believed to be a phase having the same or similar crystal structure as the ordered phase that can be formed in Pt—Ni-based alloys or Au—Pd-based alloys. That is, it is a phase consisting of Pt and Ni or a phase consisting of Au and Pd, and has an fcc structure and / or an fct structure. The ordered phase in the present invention is preferably a phase having an L1 0 Type structure (PtNi, AuPd) or L1 2 Mold structure (Pt 3 Ni, Ni 3 Pt, Au 3 Pd, Pd 3 Au) or a phase with a similar crystal structure.

[0033] (A-2) Constituent Metals and Composition Ranges of the Precious Metal Alloy of the Present Invention The precious metal alloy of the present invention is formed by adding a metal element α to an Au—Ni—Pd—Pt alloy of a predetermined composition as the base alloy. The constituent metals and composition ranges of the base alloy, as well as the range and addition concentration of the element that constitutes the metal element α, are described below. (1) Constituent Metals of the Base Alloy (Au—Ni—Pd—Pt Alloy) The base alloy that forms the basis of the present invention is an Au—Ni—Pd—Pt quaternary alloy. The base alloy exhibits at least one of spinodal decomposition and ordering, which are the strengthening mechanisms applied in the present invention, thereby ensuring the basic material structure and strength. In other words, the base alloy itself exhibits high hardness, with a hardness equal to or greater than that of precious metal alloys that utilize conventional strengthening mechanisms (solid solution strengthening, precipitation strengthening, work hardening).

[0034] The base alloy is composed of metal elements (Au, Ni, Pd, and Pt) that effectively induce spinodal decomposition and / or ordering. Regarding the occurrence of spinodal decomposition, referring to the binary phase diagram for each constituent metal of the base alloy, Au—Ni, Au—Pt, and Pt—Pd alloys exhibit two-phase separation. Furthermore, Table 2 above reveals that there are many element combinations in which the enthalpy of mixing between the Au, Ni, Pd, and Pt metal elements is positive. From these findings, it is believed that Au—Ni—Pd—Pt alloys have a high enthalpy of mixing and a strong tendency toward phase separation at low temperatures. Therefore, Au—Ni—Pd—Pt quaternary alloys are likely to exhibit spinodal decomposition, and the resulting concentration amplitude (A) is also likely to be large. Furthermore, since Pt and Ni have relatively high Young's moduli, they are also believed to have high elastic moduli (Y). Furthermore, Ni has a large difference in lattice constant from Au, Pt, and Pd, and is therefore thought to have a large lattice strain (ε). Considering these and equation 3, the constituent metals of the base alloy in the present invention are thought to be a suitable combination for achieving spinodal decomposition and high hardness due to spinodal decomposition.

[0035] As for whether ordering can occur, as mentioned above, Pt and Ni, and Au and Pd are combinations of metals that can contribute to the generation of an ordered phase through ordering. The specific effects of each metal constituting the base alloy are explained as follows.

[0036] Au Au is an essential element for causing spinodal decomposition in the alloy system of the present invention. Spinodal decomposition does not occur if the Au concentration is too low or too high, and there is a concentration range of Au necessary for its occurrence. If the Au concentration is outside the optimal range, normal nucleation and growth tend to occur, making it impossible to obtain a suitable increase in hardness. In addition, Au is a metal that can form an ordered phase with Pd, and also has the effect of contributing to the increase in hardness due to ordering.

[0037] Ni Ni acts as a strengthening factor when the base alloy exhibits spinodal decomposition. Ni has a higher Young's modulus than Au, Pt, and Pd. Furthermore, as can be seen from Table 1 above, Ni has a large difference in lattice constant with each of the metals Au, Pt, and Pd, which increases the lattice strain ε. Therefore, from the above equation 3, Ni has the effect of increasing the strengthening ability due to spinodal decomposition. Furthermore, Ni is a metal that can form an ordered phase with Pt, and also has the effect of contributing to an increase in hardness due to ordering.

[0038] In addition, Ni is an element of the same group as Pt and Pd and has a similar electronic structure, so it can be used to form alloys without impairing the corrosion resistance and oxidation resistance of precious metals to the greatest extent possible, which also has the secondary effect of reducing the price of the entire precious metal alloy.

[0039] Pd Pd expands the solid solubility limits of the elements constituting the base alloy, broadening the concentration range in which the base alloy exhibits spinodal decomposition and promoting spinodal decomposition. As a result, Pd has the effect of improving the hardening amount due to spinodal decomposition. Furthermore, Au is a metal that can form an ordered phase with Pd, and also contributes to increasing hardness through ordering. However, if excessive Pd is added, the spinodal decomposition temperature drops excessively, which tends to inhibit spinodal decomposition. Furthermore, excessive Pd addition also tends to suppress ordering, resulting in a decrease in the total hardening amount of the alloy system. Therefore, in order to optimize the hardening amount of a precious metal alloy, the optimal concentration range for Pd also exists.

[0040] Pt Pt is also an essential element for spinodal decomposition in the alloy system of the present invention. Spinodal decomposition does not occur if the Pt concentration is too low or too high, and there is a Pt concentration range required for this to occur. Pt also forms an ordered phase with Ni, which can contribute to increased hardness. Furthermore, the Young's modulus of Pt is relatively high at 169.9 GPa. As can be seen from the above-mentioned equation 3, Pt is expected to be a metal that increases the hardening amount of the alloy when spinodal decomposition occurs.

[0041] (2) Metal Element Constituting Metal Element α The present invention relates to a precious metal alloy obtained by adding a metal element α to the Au—Ni—Pd—Pt alloy having the above-described configuration as the base alloy. The metal element α acts to increase the hardness of the precious metal alloy after aging heat treatment without changing the material structure of the base alloy. In other words, the base alloy has a material structure including a modulated structure due to spinodal decomposition and / or an ordered phase due to ordering, but the metal element α is not an additive element that affects these. While the reason why the addition of the metal element α increases the hardness of the precious metal alloy is unclear, the inventors believe that one of the factors is an increase in the strength of the alloy matrix due to increased lattice strain.

[0042] The metal element α is In, Sn, Mg, Al, or Ti. According to the inventors' investigations, these metal elements are found to increase the hardness of the Au—Ni—Pd—Pt alloy. At least one metal selected from the above group of metal elements is added as the metal element α.

[0043] (3) Composition of the Precious Metal Alloy of the Present Invention The composition ranges of the constituent metals of the precious metal alloy of the present invention are as follows: Au is 4 atomic % to 24 atomic %; Ni is 5 atomic % to 60 atomic %; Pd is 2.5 atomic % to 40 atomic %; and Pt is 10 atomic % to 60 atomic %. These composition ranges are concentration ranges specified to induce spinodal decomposition and ordering, which are effective in increasing hardness.

[0044] Furthermore, the above-mentioned composition ranges of Au, Ni, Pd, and Pt are concentration ranges in which an increase in hardness due to the addition of the metal element α is expected. That is, from the viewpoint of the possibility of occurrence of spinodal decomposition and / or ordering, it is possible to set a composition range that is expanded from the above range. However, in such expanded composition ranges, an increase in hardness due to the addition of the metal element α may not be observed. The composition ranges of Au, Ni, Pd, and Pt of the present invention are ranges in which a clear increase in hardness due to both spinodal decomposition and / or ordering and the effect of adding the metal element α is expected.

[0045] The composition range of at least one of the metal element α, In, Sn, Mg, Al, and Ti, is 0.15 atomic % to 7.5 atomic %. Addition of less than 0.15 atomic % is unlikely to contribute to increasing the hardness of the base alloy. Addition of more than 7.5 atomic % of the metal element α does not significantly increase the hardness, but tends to decrease ductility.

[0046] Spinodal decomposition and ordering occur during the solution treatment and aging heat treatment processes in which a solid solution alloy having the above composition range is rapidly cooled. The precious metal alloy of the present invention has a wide range of complete solid solution at high temperatures, while having a solubility gap at low temperatures. Therefore, it is believed that a precious metal alloy in which a metal element α is added to a base alloy having the above composition range forms a supersaturated solid solution by performing a solution treatment at high temperatures and then rapidly cooling, and spinodal decomposition and ordering can occur by subsequent aging heat treatment. Regarding the thermodynamic behavior (transformation point, phase equilibrium, solid solubility limit, melting point, etc.) of the precious metal alloy of the present invention, the CALPHAD method (Calculation of Phase Diagrams) can also be effectively used. For calculations using the CALPHAD method, it is preferable to use commercially available thermodynamic calculation software (for example, Thermo-Calc (Itochu Techno-Solutions Corporation)) and a precious metal alloy database (for example, TCNOB1 (Itochu Techno-Solutions Corporation)).

[0047] The precious metal alloy according to the present invention is a precious metal alloy containing Au, Ni, Pd, Pt, the metal element α, and inevitable impurities within the above-mentioned composition ranges. Preferably, the precious metal alloy is composed of Au, Ni, Pd, Pt, the metal element α, and inevitable impurities within the above-mentioned composition ranges. The inevitable impurities are unavoidable components that are present due to impurities in the raw materials or the manufacturing process. Specific examples of inevitable impurities include Ag, Rh, Ir, Ru, Fe, Sc, Y, Zn, Re, Mo, Cr, Nb, Ta, V, W, Co, Si, Cu, Th, H, and rare earth elements. These inevitable impurities are introduced from the raw materials and the equipment used during melt casting. The content of these inevitable impurities is preferably within a range that does not impair the properties of the precious metal alloy according to the present invention, and is preferably 0.1 atomic % or less per element, preferably 0.5 atomic % or less in total, and particularly preferably 0.1 atomic % or less in total. In addition, when the above-mentioned inevitable impurities are contained in a precious metal alloy, it is difficult to clearly distinguish whether they are components that are inevitably contained or components that are intentionally added. In the present invention, as long as the components do not change the properties of the precious metal alloy, they are considered to be inevitable impurities regardless of the intention of their inclusion.

[0048] (A-3) Material Structure of the Precious Metal Alloy According to the Present Invention The precious metal alloy according to the present invention has increased hardness due to spinodal decomposition and / or ordering. Therefore, the material structure of the precious metal alloy according to the present invention may include a finely modulated structure due to spinodal decomposition and / or an ordered phase due to ordering. A modulated structure is a material structure whose composition fluctuates with a modulation period at the nano-level. These material structures can be confirmed by X-ray diffraction (XRD), transmission electron microscopy (TEM), TEM electron diffraction patterns, scanning transmission electron microscopy (STEM), and STEM-EDS mapping images.

[0049] In an X-ray diffraction pattern obtained by X-ray diffraction (XRD) or an electron beam diffraction pattern obtained by TEM, a broad peak called a sideband peak (satellite peak) is observed on at least one side (preferably both sides) of the main peak. The presence or absence of this sideband peak can determine whether or not a spinodal decomposition structure is present. Since the crystal structure of the matrix of the precious metal alloy according to the present invention is a face-centered cubic (fcc) structure, Miller index planes {111}, {200}, {220}, {311}, etc. appear as main peaks. In a spinodal decomposition structure, sideband peaks appear on both sides or one side of at least one of the main peaks. Note that if a sideband peak appears only on one side of the main peak, it is thought that it is difficult to separate it from the main peak.

[0050] The presence of an ordered phase in an X-ray diffraction pattern or an electron diffraction pattern can be confirmed by observing ordered reflection peaks. For example, in the observation of ordered reflection peaks in an X-ray diffraction pattern, in the case of θ-2θ measurement using CuKα rays as an X-ray source, ordered reflection peaks appear around 2θ=30° to 35°.

[0051] The modulated structure in the precious metal alloy according to the present invention tends to be composed of two regions: a region where the Au concentration and Pd concentration are relatively high (a region where the Pt concentration and Ni concentration are relatively low) and a region where the Au concentration and Pd concentration are relatively low (a region where the Pt concentration and Ni concentration are relatively high). 0 Type structure or L1 2 It contains at least one of ordered phases of type structure, particularly L1 2 They tend to contain ordered phases of the type structure.

[0052] (A-4) Hardness of the Precious Metal Alloy According to the Present Invention The precious metal alloy according to the present invention has the composition range described above and is hardened by spinodal decomposition and / or ordering. The precious metal alloy according to the present invention can stably exhibit a Vickers hardness of 500 Hv or more. The addition of the metal element α is expected to further increase hardness, and can achieve a high hardness of 550 Hv or more or 600 Hv or more. The precious metal alloy according to the present invention can be made into a high-hardness precious metal alloy having the above-mentioned Vickers hardness by heat treatment alone, without utilizing work hardening at all, i.e., without causing material embrittlement due to dislocation strain.

[0053] The upper limit of the hardness of the precious metal alloy according to the present invention should not be particularly limited, but it is preferable that the upper limit is 850 Hv or less. If the hardness exceeds 850 Hv, there is a risk of breakage or chipping during use. The Vickers hardness described above is a value at room temperature. The Vickers hardness can be measured using a known Vickers hardness tester. The measurement load is preferably 0.05 kgf or more and 0.5 kgf or less, and more preferably 0.2 kgf.

[0054] The shape and form of the precious metal alloy according to the present invention are not particularly limited. For the above-mentioned medical instruments, probe pins, etc., the present invention can generally be used as a bulk (lump) alloy that has been appropriately processed. The present invention can also be formed in the form of a layer or film on an appropriate base material or substrate.

[0055] (B) Manufacturing Method of Precious Metal Alloy According to the Present Invention Next, a method for manufacturing a precious metal alloy according to the present invention will be described. As described above, the precious metal alloy according to the present invention can be provided in various shapes and forms. In the following description, a method for manufacturing a bulk precious metal alloy, which is a frequently applied form, will be described in detail, and a method for manufacturing a layered or film-shaped precious metal alloy will also be mentioned.

[0056] In the present invention, high hardness is achieved by selecting the constituent metals (Au, Ni, Pd, Pt, and metallic element α) of the precious metal alloy, optimizing their composition ranges, and then subjecting them to spinodal decomposition and / or ordering. The precious metal alloy of the present invention is produced by producing an alloy ingot having the above-described composition range, and then performing an appropriate heat treatment process. The appropriate heat treatment process is a heat treatment process that combines a solution treatment and an aging heat treatment, through which spinodal decomposition and / or ordering progress, resulting in high hardness. The method for producing such a precious metal alloy of the present invention is a method for hardening the material by heat treatment without relying on work hardening.

[0057] The method for producing a precious metal alloy according to the present invention will be described below with reference to each heat treatment step. Processing methods that can be performed during or after the production of the precious metal alloy according to the present invention will also be described. In the present invention, the temperatures, such as the heating temperature, in the various heat treatments described below refer to the temperature of the precious metal alloy being treated, unless otherwise specified.

[0058] (B-1) Preparation Step (Preparation of Precious Metal Alloy) First, an unheated precious metal alloy ingot is prepared as a precursor for the precious metal alloy of the present invention. The precursor precious metal alloy ingot can be produced by a conventional melt casting method. The above-mentioned metal raw materials, Au, Ni, Pd, Pt, and metal element α, are adjusted to the above composition by appropriate weighing or the like, and then melted and cast to produce an alloy ingot. At this time, a base alloy such as an Au—Ni—Pd—Pt alloy, or a binary alloy such as an Au—Pd alloy or a Pt—Ni alloy may be appropriately combined and melted as a master alloy. Melt casting of the precious metal alloy can be performed by known means such as arc melting, high-frequency melting, vacuum melting, or continuous casting.

[0059] The precious metal alloy may be prepared by a method other than melt casting, such as powder metallurgy. In powder metallurgy, a precious metal alloy powder prepared to the above composition (e.g., a precious metal alloy powder produced by atomization) is sintered to obtain an alloy ingot to be heat-treated. Alternatively, a near-net-shape ingot may be produced by a known additive manufacturing method using the precious metal alloy powder prepared to the above composition. Furthermore, a precious metal alloy layer of the above composition may be formed on any base material by a known alloy formation method, such as sputtering or thermal spraying.

[0060] (B-2) Solution Treatment: The precious metal alloy prepared as described above is subjected to solution treatment to form a supersaturated solid solution. Solution treatment is a process in which a precious metal alloy is heated to a high temperature to form a single-phase or similar solid solution structure, followed by rapid cooling to form a supersaturated solid solution. The heating temperature for solution treatment is preferably at or above (Tm - 500°C) but below Tm, where Tm is the melting point (solidus) of the precious metal alloy (°C). Temperatures below (Tm - 500°C) result in low solid solubility of each element and are insufficient to form a supersaturated solid solution. Temperatures above Tm are undesirable because melting of the material begins near the grain boundaries. The holding time during heating is preferably between 0.0001 and 168 hours. Heating for less than 0.0001 hours results in insufficient formation of a supersaturated solid solution, and heating for more than 168 hours does not significantly affect the formation of a supersaturated solid solution, making this undesirable from the standpoint of productivity. In the present invention, the melting point means the solidus temperature.

[0061] Furthermore, cooling from the solution treatment temperature requires rapid cooling, i.e., rapid cooling, so as not to cause excessive grain boundary reactions in the high-temperature range. If grain boundary reactions occur in the high-temperature range, the grain boundaries are strengthened, improving ductility, but the hardness after aging heat treatment may be insufficient. Specifically, a cooling rate of 10°C / s or higher is preferred, and 50°C / s or higher is more preferred. On the other hand, a slow cooling rate is preferred from the viewpoint of preventing quench cracking, dimensional change, deformation, etc. Therefore, from the viewpoint of improving the hardness of the precious metal alloy, the cooling rate referred to as rapid cooling is not necessary in the low-temperature range where grain boundary reactions do not occur and spinodal decomposition and / or ordering do not proceed excessively. For example, rapid cooling is not required for the cooling rate in the temperature range below 300°C. Therefore, in order to suppress or reduce the occurrence of quench cracking, etc., rapid cooling to 200°C may be performed, followed by air cooling in the temperature range below 200°C. The end point of cooling in the solution treatment is preferably room temperature.

[0062] (B-3) Aging Heat Treatment Spinodal decomposition and ordering in the precious metal alloy according to the present invention proceed by subjecting the supersaturated solid solution formed above to aging heat treatment in a temperature range lower than the spinodal decomposition temperature and the order-disorder transformation temperature.

[0063] The conditions for aging heat treatment of a supersaturated solid solution are that the heating temperature be 300°C or higher and 700°C or lower. If the temperature is lower than 300°C, transformation does not proceed easily. If the temperature exceeds 700°C, material softening due to grain boundary reaction is significant. The heating temperature is more preferably 350°C or higher and 650°C or lower. The heating time for the aging heat treatment is preferably 0.001 hours or higher and 168 hours or lower. If the heating time is less than 0.001 hours, transformation will be insufficient and hardness will vary, while treatment for 168 hours or longer will result in poor productivity and high manufacturing costs. There are no particular restrictions on the cooling method after the aging heat treatment.

[0064] (B-4) Other Heat Treatment Steps The precious metal alloy according to the present invention is manufactured by undergoing the above-described solution treatment and aging heat treatment, but other heat treatment steps may be included in the manufacturing process. Examples of such other heat treatment steps include homogenization treatment, two-phase treatment, intermediate annealing, etc. However, these other heat treatment steps do not affect the progress of spinodal decomposition or ordering. Therefore, these heat treatment steps are optional steps.

[0065] Homogenization is a heat treatment performed on precious metal alloys prepared by melt casting to form a metal structure with a uniform distribution of element concentrations in the precious metal alloy. The homogenization is a heat treatment in which the precious metal alloy is heated at a high temperature below its melting point for a long period of time (preferably 0.1 to 72 hours).

[0066] The dual-phase treatment is a heat treatment for forming a two-phase structure, which has the best workability among the alloys of the present invention, and is carried out to facilitate warm working and cold working. The heating temperature for the dual-phase treatment is 700°C or higher and 900°C or lower, more preferably 750°C or higher and 850°C or lower. The heating time is 0.1 hours or higher and 10 hours or lower, more preferably 0.2 hours or higher and 2 hours or lower.

[0067] Intermediate annealing is a heat treatment performed during processing of precious metal alloy ingots, etc., in which strain accumulates during warm working or cold working, as described below. Intermediate annealing is a treatment for reducing the material strength and restoring workability. The heating temperature for intermediate annealing is 700°C or higher and 900°C or lower, more preferably 750°C or higher and 850°C or lower. The heating time is 0.1 hours or higher and 10 hours or lower, more preferably 0.2 hours or higher and 2 hours or lower.

[0068] (B-5) Processing Process of the Precious Metal Alloy According to the Present Invention The precious metal alloy according to the present invention can be processed into various shapes depending on the application by undergoing at least one processing step before aging treatment. Examples of this processing step include hot working, warm working, cold working, skin-pass, straightening, coiling, bending, etc. Hot working can destroy the solidification structure in the prepared precious metal alloy ingot and eliminate defects such as voids. Warm working and cold working not only change the overall shape of the alloy, but also have the significance of controlling the shape of the crystal grains. When warm working or cold working is performed multiple times, the intermediate annealing described above may be performed between processing passes.

[0069] In particular, warm working, cold working, skin pass, straightening, coiling, and bending after solution treatment are useful as processing steps for the precious metal alloy according to the present invention. This is because the ductility of the precious metal alloy after solution treatment is improved. Furthermore, the precious metal alloy after solution treatment (before aging) can be processed into a final shape or a shape close to the final shape corresponding to its intended use by the above-mentioned processing methods.

[0070] However, the precious metal alloy according to the present invention may be processed after aging (after hardening). Even a precious metal alloy that has been highly hardened after aging can still be processed. Furthermore, the precious metal alloy after aging can also be processed for final adjustment, such as grinding / polishing, cutting, electric discharge machining, pressing, bending, and straightening. Furthermore, since the spinodal decomposition and ordering that occur in the precious metal alloy according to the present invention are reversible, solution treatment and aging treatment may be repeated. Processing may also be performed between multiple combinations of solution treatment and aging treatment.

[0071] (B-6) Other Manufacturing Methods of the Present Invention in the Present Invention In the manufacturing methods described above, the precious metal alloy of the present invention is obtained by subjecting an alloy ingot that has been subjected to a melting and casting process to a solution treatment and an aging treatment. In the present invention, although the solution treatment is an important heat treatment step, there are cases in which a precious metal alloy in a structural state equivalent to that of a solid solution obtained by a solution treatment can be prepared without performing the solution treatment step. In such cases, the precious metal alloy of the present invention can be manufactured by subjecting the precious metal alloy to an aging treatment.

[0072] Examples of processes for obtaining a solid solution state precious metal alloy without solution treatment include a liquid quenching method applied to molten precious metal alloys, and a rapid heating and quenching process or rapid solidification process using a laser or the like applied to bulk metals. Furthermore, various film formation processes, such as welding, sputtering, plating, and thermal spraying, can also produce precious metal alloys that approximate a supersaturated solid solution state. Precious metal alloys produced by these processes can be made into the precious metal alloy of the present invention by aging treatment. These processes are useful for producing near-net-shape precious metal alloys and layered or film-like precious metal alloys for high-hardness coatings, etc. The preferred conditions for aging treatment without solution treatment are the same as those described above.

[0073] Examples that are specific embodiments of the present invention will be described below. In these examples, multiple Au—Ni—Pd—Pt-based precious metal alloys were manufactured while varying the composition of Au, Ni, Pd, Pt, and the metal element α, and their hardness was measured. In these examples, In, Sn, Mg, Al, and Ti were added as the metal element α.

[0074] [Production of precious metal alloy] As raw materials, high-purity ingots of Au, Ni, Pd, Pt, and metal elements α (In, Sn, Mg, Al, Ti) were weighed and mixed to obtain a predetermined composition, and then melt-cast into alloy ingots by arc melting in an inert gas atmosphere. Test pieces (5 mm × 5 mm × 3 mm) were then cut out from the alloy ingots.

[0075] [Heat Treatment Step (Solution Treatment)] The prepared test specimens were subjected to solution treatment and aging heat treatment. In the solution treatment, the test specimens were heated and held at a temperature of 1050°C to 1250°C for 16 hours, and then water-cooled to room temperature.

[0076] [Heat Treatment Step (Aging Heat Treatment)] The heating temperature in the aging heat treatment was set at temperatures from 450°C to 600°C in 25°C intervals, and the test pieces after the solution treatment were heated and held at each aging heat treatment temperature for 1 hour, and then water-cooled to room temperature. After the aging heat treatment, the test pieces were embedded in resin and roughly polished (#500, #800, #1200) and mirror-polished with a 1 μm and 1 / 4 μm diamond suspension to remove residual stress in the surface due to the oxide layer and thermal strain and to prepare samples for hardness measurement. Samples of various compositions were prepared in this manner.

[0077] In this embodiment, as an example, an Au-Ni-Pd-Pt based noble metal alloy consisting of Au, Ni, Pd, Pt, and a metal element α (In, Sn, Mg, Al, Ti) was produced.

[0078] As a reference example, an Au—Ni—Pd—Pt alloy was produced that had a composition similar to that of the precious metal alloys of each example, but to which the metal element α had not been added. Furthermore, as a comparative example, an Au—Ni—Pd—Pt alloy outside the composition range of the present invention, and an Au—Pt alloy and a Pt—Ni alloy, which are precious metal alloys capable of exhibiting spinodal decomposition or ordering, were produced as conventional examples. These reference examples, comparative examples, and conventional examples were also subjected to the same solution treatment and aging heat treatment as above, and samples were produced in the same manner as in the above embodiment.

[0079] [Hardness Measurement] Hardness measurements were performed on each of the precious metal alloy samples produced above. Hardness measurements were performed using a measuring device (HM-210 manufactured by Mitutoyo Corporation) at room temperature with a test load of 0.2 kgf. The measurement results are shown in Table 1. Hardness measurements were performed at 15 random locations on each sample, and the average value was used as the hardness value. Measurement locations on each sample were selected from multiple crystal grains, and measurements were taken at the non-grain boundary portions of each crystal grain, preferably near the center of the crystal grain. The hardness measurement results shown below (Tables 3 and 4) list the aging heat treatment temperature and hardness at which the highest hardness was obtained among multiple aging heat treatment temperatures set in the range of 450°C to 600°C. However, the precious metal alloys of the examples exhibited a minimum hardness of 520 Hv or more.

[0080] [Examination of Material Structure by XRD Analysis] Furthermore, XRD analysis was performed on each precious metal alloy to (a) confirm spinodal decomposition and (b) confirm the formation of an ordered phase. The analysis conditions, such as sample size, for each examination item by XRD were as follows. XRD analysis was performed on the precious metal alloy after solution treatment (solution material) and the precious metal alloy after aging heat treatment (aged material), and the results were compared to confirm the occurrence of spinodal decomposition and ordering due to aging heat treatment.

[0081] [Common conditions] Sample size: φ22 mm x 2 mmt XRD device: Rigaku SmartLab Target: Cu anode Optical system / detector: Concentrated optical system / semiconductor detector (HyPix-3000) Current / voltage: 40 kV / 30 mA Length limiting slit: 10 mm

[0082] (a) Confirmation of spinodal decomposition (sideband peak) 2θ scanning range: 20° to 130° 2θ step size (°): 0.0012 2θ scanning rate (° / min): 6

[0083] (b) Confirmation of ordered phase (ordered peak) 2θ scanning range: 20° to 38° 2θ step size (°): 0.0132 2θ scanning rate (° / min): 1.3

[0084] In examining spinodal decomposition by XRD, the XRD diffraction profile obtained under the above conditions was judged based on whether or not one or more side band peaks appeared on either or both sides (approximately ±0.5 to 3° in 2θ angle) of the main peak for the Miller indices {111}, {200}, {220}, and {311} planes. When one or more side band peaks appeared, it was deemed that spinodal decomposition had occurred, and when no side band peaks appeared, it was deemed that spinodal decomposition had not occurred, and evaluation was performed.

[0085] In addition, the examination of the ordered phase by XRD was judged based on the presence or absence of an ordered reflection peak occurring in the vicinity of 2θ=30° to 35°. Specifically, when the ordered peak intensity was higher than the background in that region, it was evaluated as having an ordered phase, and when the peak intensity was at or below the same level as the background, it was evaluated as not having an ordered phase.

[0086] As an example of the results of the XRD analysis performed in this embodiment, the XRD diffraction pattern of the example alloy B-5 (Au12.5-Ni30.625-Pd25-Pt30.625-Sn1.25) is shown in Figure 2. Figure 2(a) shows an XRD diffraction profile for confirming spinodal decomposition, and Figure 2(b) shows an XRD diffraction profile for confirming the ordered phase. Referring to Figure 2(a), in this precious metal alloy, clear peaks that can be identified as sideband peaks were confirmed on both sides of the peak corresponding to the {111} plane near 2θ = 40° to 41° and the peak corresponding to the {200} plane near 2θ = 46.5° to 47.5°. In addition, broad peaks that can be visually recognized as sideband peaks were confirmed on both sides or one side of the peaks corresponding to other crystal planes. From this, it is estimated that spinodal decomposition occurs in this precious metal alloy. 2(b), a peak (order peak) clearly higher than the background is observed in the region around 2θ=30° to 35°, which suggests that ordering also occurs in this noble metal alloy.

[0087] TEM / STEM analysis was performed on this B-5 precious metal alloy. An atomic resolution electron microscope (JEOL Ltd. JEM-ARM300F GRAND ARM) was used as the TEM / STEM analysis device (accelerating voltage 300 kV). Before the TEM / STEM analysis, the heat treatment process (solution treatment and aging heat treatment) and the post-heat treatment resin-filled polishing were performed in the same manner as above, and then a sample for TEM / STEM analysis was prepared using a focused ion beam (FIB).

[0088] FIG. 3 shows the results of mapping measurements of each constituent element (Au, Ni, Pd, Pt, Sn) by STEM-EDS (Pt, Au, Pd, Sn: L line, Ni: K line). From FIG. 3, it can be seen that the material structure of the precious metal alloy of this embodiment has a modulated structure having two regions: a region where the Au concentration and Pd concentration are relatively high and a region where the Au concentration and Pd concentration are relatively low, and these regions are alternately connected. Since this modulated structure does not have a clear interface, it is presumed to be due to spinodal decomposition. Furthermore, when looking at the distribution of Sn, no precipitates were observed, and it appears to be preferentially dissolved in the region where the Au concentration and Pd concentration are relatively high. From the above results, it can be said that Sn does not have a significant effect on the material structure (modulated structure, ordering) of the precious metal alloy.

[0089] 4 shows an electron beam diffraction pattern obtained by TEM analysis (<001> zone axis incidence condition) of the alloy B-5 of the example. From FIG. 4, in addition to the basic reflection due to the fcc structure, diffraction spots due to the ordered phase were confirmed in the precious metal alloy B-5 of this embodiment. The diffraction spots of the ordered phase were found to be L1 based on the appearance position, intensity, and interplanar spacing. 2 The structure was envisaged.

[0090] The hardness measurement results of the precious metal alloys of the examples, reference examples, comparative examples, and conventional examples produced in this embodiment are shown in Tables 3 and 4. These tables also show the presence or absence of modulated structures (sideband peaks) and ordered phases (order peaks) determined by XRD analysis. In these tables, in this embodiment, to confirm the effect of adding the metal element α, the precious metal alloys are grouped by the composition of the base alloy (the concentration of each element of Au, Ni, Pd, and Pt) being close to each other, and the alloy groups in each group are numbered with an alphabet (A to I) and a number.

[0091]

[0092]

[0093] From Tables 3 and 4, it can be seen that spinodal decomposition occurred in all of the precious metal alloys (alloys belonging to groups A to I) of the Examples and Reference Examples, in which the composition range of the Au—Ni—Pd—Pt-based alloy was set within the range of the present invention. Furthermore, with regard to ordering, the formation of an ordered phase was confirmed, with some exceptions. As with the results for alloy B-5, the ordered phase exhibited L1 2 The structural phases have been identified. The precious metal alloys of these Examples and Reference Examples all exhibit hardness exceeding 500 Hv. The hardness of these precious metal alloys is higher than that of the Au—Pt alloy (Alloy X-1) and the Pt—Ni alloy (Alloy Y-1), in which spinodal decomposition and / or ordering may occur. It is believed that the multi-element structure of the alloys effectively exerts the effect of increasing hardness due to spinodal decomposition and / or ordering.

[0094] When comparing the hardness of the examples and the reference examples for each group of precious metal alloys in Groups A to I, it is confirmed that the examples in which metal element α is added to the Au—Ni—Pd—Pt alloy exhibit a clear increase in hardness compared to the reference examples in which metal element α is not added. The increase in hardness due to metal element α depends on the alloy composition, but is at least 15 Hv or more, and in some compositions, an increase in hardness of 100 Hv or more is observed. This comparison confirms that the base alloy, the Au—Ni—Pd—Pt alloy, is a precious metal alloy with high hardness itself, but that the addition of metal element α enables a further increase in hardness.

[0095] Furthermore, even in the case of Au—Ni—Pd—Pt alloys such as alloys S-1 and S-2, which are comparative examples, depending on the composition range of Au, Ni, Pd, and Pt, neither spinodal decomposition nor ordering may occur. These precious metal alloys exhibit hardness of less than 500 Hv, which shows that setting the composition range of the base alloy is fundamentally important.

[0096] The comparative alloys S-3 and S-4 are precious metal alloys whose alloy compositions (Au concentrations) are outside the range of the present invention, and are used to confirm the effect of increasing hardness with or without the addition of metal element α. These precious metal alloys all undergo spinodal decomposition and ordering, exhibiting hardnesses of 500 Hv or more. However, in comparison with these, the increase in hardness due to the addition of metal element α is less than 10 Hv (6 Hv), indicating that the addition of metal element α has almost no effect. This confirms that, although spinodal decomposition and / or ordering may occur even outside the composition range of the present invention, it is preferable to apply the limited composition range of the present invention in order to maximize the hardness increase due to the effect of adding metal element α.

[0097] As described above, the present invention provides a noble metal alloy having a novel structure and composition range that can exhibit high hardness due to spinodal decomposition and / or ordering. According to the present invention, a high-hardness alloy material can be obtained without relying on work hardening (dislocation strengthening). Therefore, high hardness can be achieved without concern about embrittlement associated with work hardening.

[0098] The precious metal alloy according to the present invention is expected to be applicable to a variety of applications requiring high hardness and high wear resistance, such as electrical and electronic materials such as probe pins and electrical contacts, medical instruments, and high-hardness coating members. The precious metal alloy according to the present invention can be produced by subjecting a precious metal alloy obtained by melt casting and solution treatment, additive manufacturing technology, rapid solidification technology, or coating technology such as sputtering, thermal spraying, or plating, and can be applied to the various applications described above.

Claims

1. An Au-Ni-Pd-Pt based precious metal alloy obtained by adding a metal element α to a base alloy consisting of Au, Ni, Pd and Pt, wherein the metal element α is at least one of the metal elements In, Sn, Mg, Al and Ti, and the Au-Ni-Pd-Pt based precious metal alloy contains 4 atomic % to 24 atomic % Au, 5 atomic % to 60 atomic % Ni, 2.5 atomic % to 40 atomic % Pd, 10 atomic % to 60 atomic % Pt, 0.15 atomic % to 7.5 atomic % of the metal element α, and unavoidable impurities.

2. The Au-Ni-Pd-Pt based precious metal alloy according to claim 1, which contains a modulated structure due to spinodal decomposition in its material structure.

3. A Au-Ni-Pd-Pt based precious metal alloy according to claim 1 or 2, which contains an ordered phase in its material structure.

4. The Au-Ni-Pd-Pt based precious metal alloy according to claim 1, which has a Vickers hardness of 500 Hv or more.

Citation Information

Patent Citations

  • Material for probe pin

    JP2005233967A

  • Probe pin materiel, probe pin and manufacturing method thereof

    JP2012242184A

  • Probe pin material composed of a Pt-based alloy, method for manufacturing a probe pin

    JP6372952B2

  • Medical Pt alloy wire and medical Pt alloy coil

    JP6997354B1

  • Precious metal high-entropy alloy electric contact material and preparation method thereof

    CN115418545A