Composition for cavity formation
A cavity-forming composition with urethane-bonded polymers addresses the limitations of existing methods by forming cavities with high thermal stability and low residue, effectively reducing parasitic capacitance and enhancing semiconductor device integration.
Patent Information
- Application Number
- PCT/JP2024/014633
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
Current methods for reducing parasitic capacitance between conductive wiring patterns in semiconductor devices, such as plasma treatment, are limited by equipment costs and material restrictions, and existing thermally decomposable polymers do not adequately form cavities with minimal residue, affecting electrical characteristics.
A cavity-forming composition containing a polymer with urethane bonds, derived from a condensate of polyol and polyisocyanate, is used, which exhibits high thermal decomposition rates and minimal residue, allowing for effective cavity formation between conductive wiring patterns on semiconductor substrates through heating.
The composition forms cavities with high thermal stability and low residue, reducing parasitic capacitance and maintaining electrical integrity, and can be processed at lower costs compared to plasma treatments, enabling better integration of semiconductor devices.
Smart Images

Figure JP2024014633_17102024_PF_FP_ABST
Abstract
Description
Cavity forming composition
[0001] The present invention relates to a cavity-forming composition for forming cavities between conductive wiring patterns, and to a method for manufacturing a semiconductor device using the cavity-forming composition.
[0002] In recent years, semiconductor devices have tended to become more highly integrated, and as a result, the distance between wires has become smaller. As the distance between wires becomes smaller, the parasitic capacitance between wires increases. When the parasitic capacitance between wires increases, noise and delays occur in electrical signals.
[0003] Therefore, a method of providing gaps between wirings has been proposed as a method of reducing the parasitic capacitance between wirings (see Patent Document 1). In this proposed technology, in a method of manufacturing a semiconductor device, spaces are provided between the wirings by the following steps: selectively covering the surface of a predetermined first insulating film of a semiconductor substrate to form a plurality of wirings in the same layer; forming an organic resin film on the surface of the first insulating film selectively covered with the wirings; thinning the organic resin film to expose the surfaces of the wirings; depositing a sparse second insulating film over the entire surface; removing the organic resin film; and depositing a dense third insulating film. In the organic resin film removal step, O 2 In this process, O 2 By performing the plasma treatment, carbon in the second insulating film (organic SOG film) is removed and it changes into a sparse film, and as a result, O 2 The plasma passes through the second insulating film, and the organic resin film (resist film) can be removed (see paragraph
[0023] of Patent Document 1). 2 In order to reduce damage to the substrate caused by the plasma treatment, a process of removing the organic resin film by heat has also been investigated (see Patent Document 2).
[0004] Japanese Patent Application Laid-Open No. 09-172068 Japanese Patent Application Laid-Open No. 2021-114524
[0005] In the technique of Patent Document 1, an O 2 In the plasma treatment, the second insulating film is filled with O 2 Since the plasma must pass through, there are significant restrictions on the material of the second insulating film. 2A device for plasma processing is required.
[0006] On the other hand, if the organic resin film can be removed by heating as in the technique of Patent Document 2, the restrictions on the second insulating film are relatively small, and the heating device is O. 2 The cost can be kept relatively low compared to plasma treatment equipment. However, from the viewpoint of providing a cavity-forming composition that is suitable for forming cavities between conductive wiring patterns on a semiconductor substrate by heating and leaves little residue after thermal decomposition so as not to affect the electrical characteristics of the semiconductor device, the thermally decomposable polymer described in Patent Document 2 cannot be said to be sufficient, and there is room for further study.
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a cavity-forming composition suitable for forming cavities between conductive wiring patterns on a semiconductor substrate by heating, and a method for manufacturing a semiconductor element using the cavity-forming composition.
[0008] As a result of intensive research conducted by the inventors in order to solve the above-mentioned problems, they discovered that a cavity-forming composition containing a polymer having a urethane bond, which is a condensate of a polyol and a polyisocyanate, exhibits high thermal decomposition properties, leaves little residue, and can solve the above-mentioned problems, thereby completing the present invention.
[0009] That is, the present invention encompasses the following aspects. [1] A cavity-forming composition for forming cavities between conductive wiring patterns on a semiconductor substrate, the cavity-forming composition comprising a polymer and a solvent, wherein the polymer is a polymer having a urethane bond that is a reaction product of a reactant containing a polyol and a polyisocyanate. [2] The cavity-forming composition according to [1], wherein the polymer is a polymer having a urethane bond and a urea bond that is a second reaction product of a urethane prepolymer that is a first reaction product of a first reactant containing a polyol and a polyisocyanate, and a second reactant containing an amine compound. [3] The cavity-forming composition according to [1], wherein the polymer having a urethane bond includes an alicyclic hydrocarbon structural moiety. [4] The cavity-forming composition according to [2], wherein the polymer having a urethane bond and a urea bond includes an alicyclic hydrocarbon structural moiety. [5] A method for manufacturing a semiconductor element, comprising: a step (A) of applying the cavity-forming composition according to any one of [1] to [4] onto a semiconductor substrate on which a conductive wiring pattern has been formed; a step (B) of heating the semiconductor substrate after the step (A) to form a cavity-forming film between the conductive wiring patterns from the cavity-forming composition; a step (C) of forming an insulating layer on the conductive wiring pattern and on the cavity-forming film between the conductive wiring patterns after the step (B); and a step (D) of heating the semiconductor substrate after the step (C) to burn off the cavity-forming film. [6] A method for manufacturing a semiconductor element according to [5], wherein the cavity-forming film is also formed on the conductive wiring pattern during the step (B), and the method comprises a step (E) of removing the cavity-forming film on the conductive wiring pattern before the step (C). [7] The method for manufacturing a semiconductor element according to [5], further comprising a step (F) of removing a cavity-forming film formed from the cavity-forming composition and present on the conductive wiring pattern between the steps (A) and (B). [8] The method for manufacturing a semiconductor element according to any one of [5] to [7], wherein in the step (C), the insulating layer is formed by chemical vapor deposition.
[0010] According to the present invention, it is possible to provide a cavity-forming composition suitable for forming cavities between conductive wiring patterns on a semiconductor substrate by heating, and a method for manufacturing a semiconductor element using the cavity-forming composition.
[0011] 1 is a schematic cross-sectional view for explaining an example of a method for manufacturing a semiconductor element (part 1); 2 is a schematic cross-sectional view for explaining an example of a method for manufacturing a semiconductor element (part 2); 3 is a schematic cross-sectional view for explaining an example of a method for manufacturing a semiconductor element (part 3); 4 is a schematic cross-sectional view for explaining an example of a method for manufacturing a semiconductor element (part 5); and 6 is a schematic cross-sectional view for explaining an example of a method for manufacturing a semiconductor element (part 6).
[0012] (Cavity-forming composition) The cavity-forming composition of the present invention is a composition for forming cavities between conductive wiring patterns on a semiconductor substrate. The cavity-forming composition contains a polymer and a solvent. The polymer is a reaction product of a reactant containing a polyol and a polyisocyanate. More preferably, the polymer is a second reaction product of a urethane prepolymer, which is a first reaction product of a first reactant containing a polyol and a polyisocyanate, and a second reactant containing an amine compound.
[0013] <Polymer> The polymer according to the present invention is a polymer having a urethane bond, which is a reaction product of a reactant containing a polyol and a polyisocyanate. More preferably, the polymer according to the present invention is a polymer having a urethane bond and a urea bond, which is a second reaction product of a urethane prepolymer, which is a first reaction product of a first reactant containing a polyol and a polyisocyanate, and a second reactant containing an amine compound.
[0014] A preferred embodiment [1] of the polymer according to the present invention is, for example, a polymer having a urethane bond (urethane resin), which is a reaction product of a reaction product containing a polyol shown below and a polyisocyanate shown below.
[0015] <<Embodiment [1]>> A general reaction formula for obtaining a urethane resin by reacting a polyol with a polyisocyanate is shown below.
[0016]
[0017] <<Polyol>> A preferred embodiment of the polyol is a diol. Examples of the polyol according to the present invention include low molecular weight diols and polycarbonate polyols. The low molecular weight diol is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a diol containing an alicyclic hydrocarbon structural moiety. Also, it is preferable that the diol does not contain an aromatic hydrocarbon structural moiety. Examples of diols containing an alicyclic hydrocarbon structural moiety include cyclohexanediol and cyclohexanedimethanol.
[0018] Furthermore, instead of the diol containing the alicyclic hydrocarbon structural moiety, or together with the diol containing the alicyclic hydrocarbon structural moiety, a diol having a chain structure such as dimethylolbutanoic acid can also be used.
[0019] <<Polyisocyanate>> A preferred embodiment of the polyisocyanate is a diisocyanate. The polyisocyanate according to the present invention is not particularly limited and can be appropriately selected depending on the purpose. For example, a polyisocyanate containing an alicyclic hydrocarbon structural moiety such as isophorone diisocyanate, or a polyisocyanate having a chain structure such as hexamethylene diisocyanate can be used. Of these, it is preferable to use isophorone diisocyanate.
[0020] The polymer having a urethane bond preferably contains an alicyclic hydrocarbon structural moiety.
[0021] A preferred embodiment [2] of the polymer according to the present invention is, for example, a polymer having a urethane bond and a urea bond (urethane urea resin), which is a second reaction product of a urethane prepolymer having isocyanate groups at both ends, which is a first reaction product of a first reactant containing the above-mentioned polyol and the above-mentioned polyisocyanate, and a second reactant containing an amine compound.
[0022] <<Embodiment [2]>> The polymer of embodiment [2] is obtained by reacting, for example, the urethane prepolymer shown below with an amine compound to obtain a urethane urea resin.
[0023]
[0024] <<Amine Compound>> The amine compound is not particularly limited and can be appropriately selected depending on the purpose. For example, a monoamine such as diethanolamine or a diamine such as ethylenediamine or 2-(2-aminoethylamino)ethanol can be used. Among these, it is preferable to use a polyamine. A preferred embodiment of the polyamine is a diamine.
[0025] In the present invention, it is preferable to use a diamine and a monoamine in combination as the amine compound, which is the second reactant used in producing the urethane urea resin reaction product. In this case, the diamine can be used for chain extension, and the monoamine can be used for end-capping. A preferred embodiment of the diamine used in the present invention is a diamine having a secondary amino group and a primary amino group. The diamine preferably has a hydroxyl group, and more preferably has a primary hydroxyl group. For example, a preferred example is a diamine with a hydroxyl group introduced at the terminal, such as 2-(2-aminoethylamino)ethanol. Furthermore, the monoamine used in the present invention preferably has a hydroxyl group, and more preferably has a primary hydroxyl group.
[0026] The polymer having a urethane bond and a urea bond preferably contains an alicyclic hydrocarbon structural moiety.
[0027] As a more specific example of the above embodiment [1], the following embodiment [3] will be mentioned. The following describes embodiment [3].
[0028] <<Embodiment [3]>> The urethane resin according to the present invention can be obtained by using, for example, 1,4-cyclohexanedimethanol represented by the following formula (a) and dimethylolbutanoic acid represented by the following formula (b) as the polyol component, and isophorone diisocyanate represented by the following formula (c) as the polyisocyanate component, and reacting these respective monomers.
[0029]
[0030] As a more specific example of the above embodiment [2], the following embodiment [4] will be described below.
[0031] <<Embodiment [4]>> The urethane urea resin according to the present invention is a reaction product obtained, for example, from the polyol and polyisocyanate described in embodiment [3] above, and can be obtained by reacting a urethane prepolymer having isocyanate groups at both ends with an amine compound. In embodiment [4], for example, 2-(2-aminoethylamino)ethanol represented by formula (d) below and diethanolamine represented by formula (e) below are used as the amine compounds. This allows, for example, the urethane prepolymer represented by formula (I) below, obtained using the polyol and polyisocyanate described in embodiment [3] above, to react with the amine compounds represented by formulas (d) and (e) below to produce the urethane urea resin according to the present invention, which has a skeletal structure represented by formula (II) below.
[0032]
[0033] In formula (I), X1 is a group represented by the following formula (x) (X1 in formula (II) also has the same meaning):
[0034]
[0035] In formula (x), * represents a bond.
[0036]
[0037]
[0038] The weight average molecular weight of the polymer of the present invention is preferably from 1,000 to 10,000, more preferably from 3,000 to 7,000. The acid value is preferably from 1 to 10 mgKOH / g, and the hydroxyl value is preferably from 100 to 300 mgKOH / g.
[0039] The cavity-forming composition is suitably used in the manufacture of a semiconductor device, which includes the following steps (A) to (D): step (A): applying the cavity-forming composition onto a semiconductor substrate on which a conductive wiring pattern has been formed; step (B): heating the semiconductor substrate after step (A) to form a cavity-forming film formed from the cavity-forming composition between the conductive wiring patterns; step (C): forming an insulating layer on the conductive wiring pattern and the cavity-forming film between the conductive wiring patterns after step (B); and step (D): heating the semiconductor substrate after step (C) to burn off the cavity-forming film.
[0040] In step (C), when an insulating layer is formed, if the cavity-forming film softens and deforms when heat is applied to the cavity-forming film, it is difficult to form a uniform insulating layer. However, the cavity-forming film formed using the cavity-forming composition of the present invention is less likely to soften, and therefore a uniform insulating layer can be formed. Furthermore, when the cavity-forming film is heated to burn off in step (D), the polymer contained in the cavity-forming composition of the present invention exhibits a high decomposition rate, so that the cavity-forming film can be burned off without leaving any residue of the cavity-forming film. Therefore, the cavity-forming composition of the present invention is suitable for forming cavities between conductive wiring patterns on a semiconductor substrate by heating.
[0041] In a preferred embodiment of the cavity-forming composition of the present invention, the cavity-forming film formed from the cavity-forming composition has a sufficiently high glass transition temperature, for example, 86°C or higher. The higher the glass transition temperature, the more uniform the insulating layer formed. The glass transition temperature is more preferably 90°C or higher, even more preferably 93°C or higher, and particularly preferably 100°C or higher. There is no particular upper limit to the glass transition temperature, but for example, the glass transition temperature may be 130°C or lower or 120°C or lower. The glass transition temperature can be measured, for example, by the following method. The cavity-forming composition is applied by spin coating to form a coating film on a silicon substrate at a predetermined bake temperature (e.g., 205°C or 215°C). The coating film has a thickness of 40 nm to 50 nm. The coating film is then scraped off, and the resulting powder is subjected to differential scanning calorimetry (DSC). Differential scanning calorimetry (DSC) is used for the measurement. First, the temperature is raised to 140°C to erase the thermal history, and then the temperature is lowered to 0°C at a rate of 20°C / min. Measurement is then performed again at a rate of 20°C / min. The temperature is taken as the inflection point in the transition region that appears in a stepped manner on the thermogram. For results in which no inflection point is observed, the glass transition temperature is considered to be 100°C or higher. The apparatus used is a Q2000 manufactured by TA Instruments, and the sample weight is approximately 5 mg. The baking temperature may be, for example, the heating temperature in step (B) above.
[0042] In a preferred embodiment of the cavity-forming composition of the present invention, a cavity-forming film formed from the cavity-forming composition has a decomposition rate of 95% or more when heated at 400°C for 30 minutes in a nitrogen atmosphere. The higher the decomposition rate, the lower the dielectric constant of the formed cavity (e.g., the cavity formed in step (D) above). The decomposition rate is preferably 96% or more, more preferably 97% or more, even more preferably 98% or more, and particularly preferably 99% or more. The decomposition rate can be measured, for example, by the following method. The cavity-forming composition is applied by spin coating to form a coating film on a silicon substrate at a predetermined bake temperature (e.g., 205°C or 215°C). The coating film has a thickness of 40 nm to 50 nm. The bake temperature may be, for example, the heating temperature in step (B) above. The thickness of the coating film is measured using a VM-3210 (manufactured by SCREEN Semiconductor Solutions Co., Ltd.). The silicon substrate coated with the cavity-forming composition is then heated for 30 minutes in a nitrogen atmosphere on a plate preheated to 400°C. Finally, the thickness of the resulting coating film on the substrate is measured again using RE-3100 and RE-3500 (manufactured by SCREEN Semiconductor Solutions Co., Ltd.). The thermal decomposition rate of the coating film is calculated from the obtained results using the following formula 1: (Decomposition rate [%]) = 100 × (1 - T 1 / T 0 ) Formula 1 T 0 = coating thickness before baking 1 = Thickness of coating film after baking
[0043] The content of the polymer in the cavity-forming composition is not particularly limited, but is preferably 50% by mass to 100% by mass, more preferably 80% by mass to 100% by mass, and particularly preferably 95% by mass to 100% by mass, based on the non-volatile content (i.e., components excluding the solvent) in the cavity-forming composition.
[0044] <Solvent> The solvent used in the cavity-forming composition is not particularly limited as long as it can uniformly dissolve the solid components contained therein at room temperature, but organic solvents generally used in chemical solutions for semiconductor lithography processes are preferred. Specifically, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, cyclohexane, cyclohexane-1, cyclohexane-2, cyclohexane-3, cyclohexane-4, cyclohexane-5, cyclohexane-6, cyclohexane-7, cyclohexane-8, cyclohexane-9, cyclohexane-10, cyclohexane-11, cyclohexane-12, cyclohexane-13, cyclohexane-14, cyclohexane-15, cyclohexane-16, cyclohexane-17, cyclohexane-18, cyclohexane-19, cyclohexane-20, cyclohexane-21, cyclohexane-22, cyclohexane-23, cyclohexane-24, cyclohexane-25, cyclohexane-26, cyclohexane-27, cyclohexane-28, cyclohexane-29, cyclohexane-30, cyclohexane-31, cyclohexane-32, cyclohexane-33, cyclohexane-34, cyclohexane-35, cyclohexane-36, cyclohexane-37, cyclohexane-38, cyclohexane-49, cyclohexane-49, cyclohexane-49, cyclohexane-49, cyclohexane-49, cyclohexane-51, cyclohexane-52, cyclohexane-53, cyclohexane-16, cyclohexane-18, cyclohexane- Examples of suitable solvents include heptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. These solvents may be used alone or in combination of two or more.
[0045] Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate, and cyclohexanone are preferred, with propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate being particularly preferred.
[0046] <Other Components> A surfactant may be further added to the cavity-forming composition to prevent pinholes, striations, etc., and further improve application properties for surface unevenness. Examples of surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl aryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether; polyoxyethylene-polyoxypropylene block copolymers; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; polyoxyethylene sorbitan monolaurate; and polyoxyethylene sorbitan monopalmitate. nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; fluorine-based surfactants such as Eftop EF301, EF303, and EF352 (trade names, manufactured by Tochem Products Co., Ltd.), Megafac F171, F173, R-30, and R-40 (trade names, manufactured by DIC Corporation), Fluorad FC430 and FC431 (trade names, manufactured by Sumitomo 3M Limited), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (trade names, manufactured by Asahi Glass Co., Ltd.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The amount of these surfactants to be added is usually 2.0% by mass or less, and preferably 1.0% by mass or less, based on the total solid content of the protective film-forming composition. These surfactants may be added alone or in combination of two or more.
[0047] The nonvolatile content of the cavity-forming composition, that is, the components excluding the solvent, is, for example, 0.01% by mass to 10% by mass.
[0048] (Method for manufacturing a semiconductor element) The method for manufacturing a semiconductor element of the present invention includes the following steps (A) to (D). Step (A): a step of applying the cavity-forming composition of the present invention onto a semiconductor substrate on which a conductive wiring pattern has been formed. Step (B): a step of heating the semiconductor substrate after step (A) to form a cavity-forming film formed from the cavity-forming composition between the conductive wiring patterns. Step (C): a step of forming an insulating layer on the conductive wiring pattern and the cavity-forming curable material between the conductive wiring patterns after step (B). Step (D): a step of heating the semiconductor substrate after step (C) to burn off the cavity-forming film.
[0049] <Step (A)> Step (A) is a step in which the cavity-forming composition of the present invention is applied onto a semiconductor substrate on which a conductive wiring pattern has been formed.
[0050] Examples of semiconductor substrates include silicon wafers, germanium wafers, and wafers of compound semiconductors such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.
[0051] The material, size, and shape of the conductive wiring pattern are not particularly limited, and examples of the material for the conductive wiring pattern include copper, cobalt, ruthenium, molybdenum, chromium, tungsten, manganese, rhodium, nickel, palladium, platinum, silver, gold, and aluminum.
[0052] An insulating layer may be formed on the conductive wiring pattern. Examples of materials for the insulating layer include silicon dioxide, silicon oxycarbide, silicon oxynitride, silicon nitride, silicon carbon nitride (SiCN), aluminum nitride, aluminum oxynitride, and aluminum oxide. Examples of methods for forming the insulating layer include vapor deposition.
[0053] The line width of each wire in the conductive wiring pattern is not particularly limited, but may be, for example, 3 nm to 50 nm. The width of the space between each wire in the conductive wiring pattern is not particularly limited, but may be, for example, 3 nm to 50 nm.
[0054] The method for forming the conductive wiring pattern is not particularly limited, and for example, a conventionally known lithography process can be used.
[0055] The cavity-forming composition is applied onto the semiconductor substrate by a suitable application method such as using a spinner or a coater.
[0056] <Step (B)> Step (B) is a step in which, after step (A), the semiconductor substrate is heated to form a cavity-forming film made of a cavity-forming composition between the conductive wiring patterns.
[0057] The semiconductor substrate is heated using a heating means such as a hot plate. When the cavity-forming composition contains an acid catalyst that crosslinks the polymer, a crosslinked structure of the polymer is formed by heating the semiconductor substrate in step (B). As a result, a cavity-forming film is obtained from the cavity-forming composition containing the crosslinked polymer. The heating temperature can be appropriately selected depending on the type of polymer and the type of acid catalyst optionally contained in the cavity-forming composition, but is preferably 200 to 260°C. The heating time is not particularly limited, but is preferably 30 seconds to 2 minutes.
[0058] <Step (C)> Step (C) is a step that follows step (B) and involves forming an insulating layer on the conductive wiring patterns and the cavity-forming film between the conductive wiring patterns.
[0059] The material of the insulating layer is not particularly limited and may be an organic material or an inorganic material. When the insulating layer is made of an inorganic material, examples of the material include silicon dioxide, silicon oxycarbide, silicon oxynitride, silicon nitride, silicon carbon nitride (SiCN), aluminum nitride, aluminum oxynitride, aluminum oxide, tantalum oxide, titanium oxide, yttrium oxide, lanthanum oxide, hafnium oxide, zirconium oxide, and mixtures thereof.
[0060] The thickness of the insulating layer is not particularly limited, but may be, for example, 0.2 nm to 10 nm.
[0061] The method for forming the insulating layer is not particularly limited, but chemical vapor deposition (CVD) is preferred. That is, in step (C), the insulating layer is preferably formed by chemical vapor deposition.
[0062] <Step (D)> In step (D), which is performed after step (C), the semiconductor substrate is heated to burn off the cavity-forming film.
[0063] When the cavity-forming film is heated, the cavity-forming film is thermally decomposed and burned away due to the thermal decomposition of the polymer.
[0064] The heating temperature is not particularly limited as long as it is a temperature at which the cavity-forming film disappears, and can be appropriately selected depending on the type of polymer, etc., but is preferably 300 to 500° C. The heating time is not particularly limited, but is preferably 30 to 90 minutes.
[0065] The amount of the cavity-forming film that is burned away (decomposition rate) is preferably 100%, but does not have to be 100% and may be 99.9% or less. The decomposition rate is preferably 90% or more, more preferably 95% or more, more preferably 96% or more, more preferably 97% or more, even more preferably 98% or more, and particularly preferably 99% or more.
[0066] <Step (E)> In step (B), the cavity-forming film may also be formed on the conductive wiring pattern. In that case, the method for manufacturing a semiconductor device preferably includes step (E) of removing the cavity-forming film on the conductive wiring pattern before step (C).
[0067] The cavity-forming film on the conductive wiring pattern can be removed by, for example, etching the cavity-forming film, which may be wet etching or dry etching.
[0068] <Step (F)> Between steps (A) and (B), step (F) may be included in which the cavity-forming composition present on the conductive wiring pattern is removed.
[0069] The cavity-forming composition on the conductive wiring pattern can be removed, for example, by etching the cavity-forming composition. The etching may be wet etching or dry etching.
[0070] An example of a method for manufacturing a semiconductor device will be described below with reference to FIGS. 1A to 1F. First, as shown in FIG. 1A, a semiconductor substrate 1 having a conductive wiring pattern 2 formed thereon is prepared. Next, in step (A), a cavity-forming composition is applied to the semiconductor substrate 1 having the conductive wiring pattern 2 formed thereon. As a result, a cavity-forming composition 3A is disposed on the conductive wiring pattern 2 and in the gaps between the conductive wiring patterns 2 (FIG. 1B). Next, in step (B), the semiconductor substrate 1 is heated. As a result, a cavity-forming film 3B made of the cavity-forming composition is formed on the conductive wiring pattern 2 and in the gaps between the conductive wiring patterns 2 (FIG. 1C). Next, in step (E), the cavity-forming film 3B on the conductive wiring pattern 2 is removed (FIG. 1D). Next, in step (C), an insulating layer 4 is formed on the cavity-forming film 3B in the gaps between the conductive wiring patterns 2 (FIG. 1E). Subsequently, in step (D), the semiconductor substrate 1 is heated to burn off the cavity-forming film 3B between the conductive wiring patterns 2, thereby forming cavities 3C between the conductive wiring patterns 2. As a result, cavities are formed between the conductive wiring patterns of the semiconductor substrate.
[0071] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples.
[0072] The weight-average molecular weights of the polymers shown in the following examples were measured by gel permeation chromatography (hereinafter abbreviated as GPC). A GPC device manufactured by Tosoh Corporation was used for the measurement, and the measurement conditions were as follows: Column temperature: 40°C, Flow rate: 0.35 ml / min, Eluent: tetrahydrofuran (THF), Standard sample: polystyrene (Tosoh Corporation).
[0073] The compounds used in the examples are shown below.
[0074]
[0075]
[0076] Synthesis Example 1 Urethane urea resin (A-1) solution A reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping device, and nitrogen inlet tube was charged with 100.0 parts of 1,4-cyclohexanedimethanol represented by the above formula (a) and 4.7 parts of dimethylolbutanoic acid represented by the above formula (b) as polyol components, 214.5 parts of isophorone diisocyanate represented by the above formula (c) as polyisocyanate component, and 106.4 parts of propylene glycol monomethyl ether acetate as solvent, and the mixture was reacted at 80°C for 8 hours with stirring under a nitrogen atmosphere. After completion of the reaction, 106.4 parts of propylene glycol monomethyl ether acetate was added to obtain a solution of a urethane prepolymer having an isocyanate group at its terminal and a solids content of 60%. Next, while maintaining the resulting urethane prepolymer solution at 70 ° C., 10.4 parts of 2-(2-aminoethylamino)ethanol represented by the above formula (d) as a diamine component, 28.3 parts of diethanolamine represented by the above formula (e) as a monoamine component, and a solution containing 107.4 parts of propylene glycol monomethyl ether and 37.7 parts of propylene glycol monomethyl ether acetate as a solvent were added dropwise over 2 hours. After completion of the dropwise addition, the reaction was continued for another 8 hours at 70 ° C. to obtain a solution (A-1) containing a urethane urea resin with a hydroxyl value of 100.0 mg KOH / g, an acid value of 5.0 mg KOH / g, and a solids content of 50%. GPC analysis of the resulting polymer revealed that the weight average molecular weight (standard polystyrene equivalent) Mw was 5160.
[0077] (Example 1) 41.19 g of propylene glycol monomethyl ether (PGME) and 61.79 g of propylene glycol monomethyl ether acetate (PGMEA) were added to 20.00 g of the solution containing the polymer obtained in Synthesis Example 1 (solid content concentration: 10.2 mass%) to prepare a 1.66 mass% solution, which was then filtered through a polyethylene microfilter with a pore size of 0.05 μm to prepare a cavity-forming composition. The prepared solution was designated as an example as shown in Table 1 below.
[0078]
[0079] (Formation of Coating Film) The cavity-forming composition prepared in Example 1 was applied to a silicon substrate by spin coating and baked at a baking temperature of 215° C. for 60 seconds to form a coating film with a thickness of 43 nm.
[0080] (Glass Transition Temperature Measurement Test) The cavity-forming composition prepared in Example 1 was applied by spin coating to form a coating film on a silicon substrate at a predetermined bake temperature (215°C). The coating film had a thickness of approximately 43 nm. The coating film was then scraped off, and differential scanning calorimetry was performed on the resulting powder. The obtained glass transition temperature results are shown in Table 2. Details of the glass transition temperature measurement conditions are as follows. Differential scanning calorimetry (DSC) was used for the measurement. First, the temperature was raised to 140°C to erase the thermal history, and then the temperature was lowered to 0°C at a rate of 20°C / min. Measurement was then performed again at a rate of 20°C / min. The temperature was taken as the inflection point of the transition region, which appeared in a stepped manner on the thermogram. For results in which no inflection point was observed, the glass transition temperature was deemed to be 100°C or higher. A TA Instruments Q2000 was used, and the sample weight was approximately 5 mg.
[0081] (Test on Decomposition Performance of Composition by Baking) The cavity-forming composition prepared in Example 1 was spin-coated to form a coating film on a silicon substrate at a predetermined bake temperature (215°C). The coating film had a thickness of approximately 43 nm. The thermal decomposition rate was measured using the resulting coating film. The results of the decomposition rate are shown in Table 2. The detailed conditions for measuring the thermal decomposition rate are as follows. First, the thickness of the coating film was measured using a VM-3210 (manufactured by SCREEN Semiconductor Solutions Co., Ltd.). Then, the silicon substrate coated with the cavity-forming composition was heated for 30 minutes on a plate preheated to 400°C under a nitrogen atmosphere. Finally, the thickness of the coating film on the resulting substrate was measured again using an RE-3100 and an RE-3500 (manufactured by SCREEN Semiconductor Solutions Co., Ltd.). The thermal decomposition rate of the coating film was calculated from the obtained results using the following equation 1. As a result of the investigation, the decomposition rates were as shown in Table 2. (Decomposition rate [%]) = 100 x (1-T 1 / T 0) Formula 1 T 0 = coating thickness before baking 1 = Thickness of coating film after baking
[0082] (Evaluation Test for Fillability) A processed silicon substrate (after silicon oxide film deposition: 20 nm trench (L(line) / S(space))) was prepared by depositing a silicon oxide film of about 20 nm by a CVD method on a silicon substrate having a 60 nm trench (L(line) / S(space)) formed thereon. The cavity-forming composition prepared in Example 1 was applied by spin coating onto the processed silicon substrate having a silicon oxide film formed on the surface of the trench (20 nm trench (L(line) / S(space)) after silicon oxide film deposition), and baked at 215°C for 60 seconds to form a coating film with a thickness of 43 nm. The fillability was confirmed using a cross-sectional SEM (S-4800, manufactured by Hitachi High-Technologies Corporation). A case in which the composition was filled into the 20 nm trench (L(line) / S(space)) substrate, which is the gap between the silicon oxide film, without generating voids (air gaps, etc.), was judged to have no voids.
[0083]
[0084] The decomposition rate is preferably 95% or more, and in Example 1, the decomposition rate was 99.7%.
[0085] The cavity-forming composition according to the present invention has a high glass transition temperature when formed into a coating film, and also exhibits good thermal decomposition properties at high temperatures, providing a film that is excellent in composition removal performance by baking.
[0086] REFERENCE SIGNS LIST 1 Semiconductor substrate 2 Conductive wiring pattern 3A Cavity-forming composition 3B Cavity-forming film 3C Cavity 4 Insulating layer
Claims
1. A cavity-forming composition for forming a cavity between conductive wiring patterns on a semiconductor substrate, the cavity-forming composition comprising a polymer and a solvent, the polymer being a polymer having a urethane bond that is a reaction product of a reactant containing a polyol and a polyisocyanate.
2. The cavity-forming composition according to claim 1, wherein the polymer is a polymer having urethane bonds and urea bonds, which is a second reaction product of a urethane prepolymer, which is a first reaction product of a first reactant containing a polyol and a polyisocyanate, and a second reactant containing an amine compound.
3. The cavity-forming composition according to claim 1, wherein the polymer having a urethane bond contains an alicyclic hydrocarbon structural portion.
4. The cavity-forming composition according to claim 2, wherein the polymer having a urethane bond and a urea bond contains a structural portion of an alicyclic hydrocarbon.
5. A method for manufacturing a semiconductor element, comprising: a step (A) of applying the cavity-forming composition according to any one of claims 1 to 4 onto a semiconductor substrate having a conductive wiring pattern formed thereon; a step (B) of heating the semiconductor substrate after the step (A) to form a cavity-forming film between the conductive wiring patterns, the cavity-forming film being formed from the cavity-forming composition; a step (C) of forming an insulating layer on the conductive wiring pattern and on the cavity-forming film between the conductive wiring patterns after the step (B); and a step (D) of heating the semiconductor substrate after the step (C) to burn off the cavity-forming film.
6. The method for manufacturing a semiconductor element according to claim 5, further comprising: during step (B), the cavity-forming film is also formed on the conductive wiring pattern; and prior to step (C), a step (E) is included in which the cavity-forming film on the conductive wiring pattern is removed.
7. The method for producing a semiconductor element according to claim 5, comprising a step (F) between the steps (A) and (B) of removing a cavity-forming film formed from the cavity-forming composition and present on the conductive wiring pattern.
8. The method for producing a semiconductor device according to claim 5, wherein in step (C), the insulating layer is formed by chemical vapor deposition.
Citation Information
Patent Citations
Porous silicon oxide coating film
JP2001287909A
Thermally decomposable organic polymer for forming cavity among multilayer wirings
JP2003342375A
Thermally decomposable filling composition, semiconductor device comprising cavity formed by using the composition, and method of manufacturing semiconductor device by using the composition
JP2015111610A
Semiconductor device manufacturing method and semiconductor device manufacturing system
JP2021108353A
Self-aligned airgap interconnect structures and methods of fabrication
US20120261788A1
Cited By
Method for manufacturing optical element having air gap
WO2026220921A1