Hot-stamped object
The hot-stamped molded article with a tailored chemical composition and microstructure addresses the challenges of forming high-strength steel into complex shapes and enhances collision resistance, achieving both high tensile strength and improved formability for automotive applications.
Patent Information
- Application Number
- PCT/JP2024/014707
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
High-strength steel sheets with tensile strength of 780 MPa or more are difficult to form into complex shapes due to decreased ductility and increased residual stress, leading to springback and wall warpage, and existing hot stamping techniques do not adequately address the need for improved collision resistance.
A hot-stamped molded article with a specific chemical composition and microstructure, including a high martensite area ratio, controlled carbide distribution, and a decarburization index, which enhances collision resistance properties by reducing coarse carbides and retained austenite, and incorporating a surface coating for improved hydrogen embrittlement resistance.
The solution enables the formation of high-strength steel components with excellent collision resistance and improved formability, meeting stringent automotive safety standards while maintaining high tensile strength.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Hot stamped compact
[0001] This application claims priority to Japanese Patent Application No. 2023-065610, filed on April 13, 2023, the contents of which are incorporated herein by reference.
[0002] In the field of automotive steel sheets, in response to recent tightening of environmental regulations and collision safety standards, the application of steel sheets having high tensile strength (high-strength steel sheets) is expanding in order to improve both fuel economy and collision safety. However, as the strength of steel sheets increases, the press formability of the steel sheets decreases, making it difficult to manufacture products with complex shapes.
[0003] Specifically, as the strength of steel sheets increases, their ductility decreases, resulting in the problem of fracture at highly processed locations when they are processed into complex shapes. Furthermore, as the strength of steel sheets increases, residual stress after processing causes springback and wall warping, resulting in reduced dimensional accuracy. Therefore, it is not easy to press-form high-strength steel sheets, particularly those with a tensile strength of 780 MPa or more, into products with complex shapes. While roll forming, rather than press forming, makes it easier to process high-strength steel sheets, its application is limited to parts with a uniform cross section in the longitudinal direction.
[0004] Therefore, in recent years, hot stamping has been adopted as a technique for press-forming difficult-to-form materials such as high-strength steel sheets, as disclosed in, for example, Patent Documents 1 to 3. Hot stamping is a hot forming technique in which a material to be formed is heated and then formed.
[0005] In this technology, the material is heated before being formed. Therefore, the steel is soft during forming and has good formability. This allows even high-strength steel sheets to be formed into complex shapes with high precision. In addition, in hot stamping, the steel is quenched at the same time as it is formed using a press die, so the steel (steel member, hot-stamped body) after forming has sufficient strength.
[0006] For example, Patent Document 1 discloses that hot stamping can impart a tensile strength of 1400 MPa or more to a steel member obtained by forming a steel plate.
[0007] In recent years, countries around the world have been experiencing higher CO 2 Automobile companies have set reduction targets and are working to reduce fuel consumption while taking collision safety into consideration. Higher strength materials are required not only for gasoline-powered vehicles but also for electric vehicles, which are rapidly being developed, to protect not only passengers but also batteries from collisions and to offset the resulting weight increase. For example, steel members used in automobiles and the like are required to have higher strength and superior collision resistance properties than those described in the aforementioned Patent Document 1 and those generally used in steel members currently formed by hot stamping (hot-stamped bodies).
[0008] Regarding high-strength steel materials having a tensile strength of 1.5 GPa or more, for example, Patent Document 2 discloses a hot-press-formed press-formed product having excellent toughness and a tensile strength of 1.8 GPa or more. Patent Document 3 discloses a steel material having an extremely high tensile strength of 2.0 GPa or more and also having good toughness and ductility. Patent Document 4 discloses a steel material having a high tensile strength of 1.8 GPa or more and also having good toughness. Patent Document 5 discloses a steel material having an extremely high tensile strength of 2.0 GPa or more and also having good toughness.
[0009] However, as a result of investigations by the present inventors, it has been found that Patent Documents 2 to 5 may not provide sufficient crash resistance characteristics (resistance to bending cracks and crack propagation resistance during crash deformation) to meet the increasing demands of recent years.
[0010] Japanese Patent Publication No. 2002-102980 Japanese Patent Publication No. 2012-180594 Japanese Patent Publication No. 2012-1802 International Publication No. 2015 / 182596 International Publication No. 2015 / 182591
[0011] As described above, hot-stamped steel sheets having a tensile strength of 1.5 GPa (1500 MPa) or more have been disclosed in the past. However, in all cases, there is room for improvement in terms of impact resistance. Therefore, an object of the present invention is to provide a hot-stamped steel sheet having high strength and excellent impact resistance.
[0012] The present inventors conducted research into improving crash resistance, assuming a hot-stamped steel sheet with an increased C content to achieve high strength. As a result, they discovered the following: (i) When obtaining a hot-stamped steel sheet with high strength (e.g., a tensile strength of 1.5 GPa or more), a large amount of carbon (C) is added to ensure high strength, as disclosed in Patent Documents 2 and 3. In this case, undissolved carbides tend to remain in the hot-stamped steel sheet. If a large number of coarse carbides (iron-based carbides) with a circle-equivalent diameter of more than 0.5 μm are present in the microstructure of the hot-stamped steel sheet, these carbides can serve as crack initiation points during bending or as crack propagation initiation points. (ii) The fewer coarse carbides there are, the better the crash resistance (bendability and crack propagation resistance). Furthermore, even when coarse carbides are present, ensuring a certain average distance between the carbides improves crack propagation resistance. (iii) In the microstructure of a hot-stamped steel, when a large amount of ferrite or pearlite is present, the impact resistance properties (bendability and crack propagation resistance) are reduced, and when a large amount of retained austenite is present, the crack propagation resistance properties are reduced. Furthermore, when the prior austenite grain size becomes coarse, the impact resistance properties (bendability and crack propagation resistance properties) are reduced.
[0013] The present invention has been made in view of the above findings. The gist of the present invention is as follows. [1] A hot stamped steel according to one aspect of the present invention comprises, in mass%, C: 0.20 to 0.70%, Si: 0.010 to 2.000%, Mn: 0 to 2.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, O: 0.0200% or less, Al: 0.0010 to 0.5000%, and Mo: 0.0010 to 1.00%. 00%, B: 0.0005-0.0100%, Ti: 0.010-0.100%, Nb: 0-0.100%, Cr: 0-1.00%, Co: 0-3.00%, Ni: 0 ~3.00%, Cu: 0~1.00%, V: 0~1.000%, W: 0~1.00%, Ca: 0~1.0000%, Mg: 0~1.0000%, REM: 0~1.00 00%, Sb: 0 to 1.000%, Zr: 0 to 1.000%, As: 0 to 1.000%, one or more selected from Ta, Re, Os, Ir, Tc, Pb, Se, Bi, and Sn: 0 to 1.000% in total, and the balance: Fe and impurities, and when a range from a position of 1 / 8 to a position of 3 / 8 of the thickness from the surface in the thickness direction is defined as a 1 / 4 depth position, the microstructure at the 1 / 4 depth position contains, in area ratios, martensite: 80.0% or more and retained austenite: 0.0% or more and less than 5.0%, and in the microstructure at the 1 / 4 depth position, the number density of iron-based carbides having an equivalent circle diameter of more than 0.5 μm present in the martensite is 0.050 pieces / μm 2[2] The hot-stamped steel according to [1] may have a decarburization index Dc of 0.085 or more. [3] In the hot-stamped steel according to [1] or [2], when the range from the surface to 50 μm is defined as a surface layer portion, the microstructure of the surface layer portion may contain, in terms of area ratio, more than 5.0% ferrite. [4] The hot stamped steel according to any one of [1] to [3], wherein the chemical composition is, in mass%, C: more than 0.40% and 0.70% or less, Si: 0.010 to 2.000%, Mn: 0 to 1.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, O: 0.0200% or less, Al: 0.0010 to 0.5000%, Mo: 0.0010 to 1.0000%, B: 0.0005 to 0.0100%, Ti: 0.010 to 0.100%, Nb: 0 to 0.100%, [5] The hot-stamped steel according to any one of [1] to [4] may have a coating on its surface. [6] In the hot-stamped steel according to [5], the coating may be mainly composed of an Fe—Al alloy. [7] In the hot-stamped steel according to [5], the coating may be mainly composed of an Fe—Zn alloy.
[0014] According to the above-described aspects of the present invention, it is possible to provide a hot-stamped steel sheet having high strength and excellent crash resistance.
[0015] FIG. 1 is a diagram showing an example of an impact force-displacement curve obtained by an instrumented impact test.
[0016] <Hot-stamped body> A hot-stamped body according to one embodiment of the present invention (a hot-stamped body according to this embodiment) will be described. Hereinafter, the range from the surface in the thickness direction, from ⅛ to ⅜ of the thickness, will be referred to as the ¼ depth position, and the range from the surface to 50 μm will be referred to as the surface layer portion. However, the surface that serves as the reference for the surface layer portion and the ¼ depth position is the surface of the hot-stamped body, but when the hot-stamped body has a coating (has a base material and a coating), it means the surface of the base material excluding the coating.
[0017] The hot stamped steel according to the present embodiment has a predetermined chemical composition, and when the range from the surface to the thickness direction is defined as a 1 / 4 depth position, the microstructure at the 1 / 4 depth position contains, in area ratios, martensite: 80.0% or more and retained austenite: 0.0% or more and less than 5.0%, and in the microstructure at the 1 / 4 depth position, iron-based carbides having an equivalent circle diameter of more than 0.5 μm present in the martensite have a number density of 0.050 pieces / μm 2 The average distance between the iron-based carbide and the nearest other iron-based carbide is 3.0 μm or more, and the prior austenite grain size in the microstructure at the 1 / 4 depth position is 20.0 μm or less. The hot-stamped product according to this embodiment may have a coating on its surface. In this case, the hot-stamped product has a base material made of steel and a coating formed on the surface of the base material. In this case, the chemical composition and microstructure described above refer to the chemical composition and microstructure of the base material. Each of these will be described below.
[0018] [Chemical Composition] The chemical composition of the hot stamped steel according to this embodiment is, in mass %, C: 0.20 to 0.70%, Si: 0.010 to 2.000%, Mn: 0 to 2.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, O: 0.0200% or less, Al: 0.0010 to 0.5000%, Mo: 0.0010 to 1.0000%, B: 0.0005 to 0.0100%, Ti: 0.010 to 0.100%, Nb: 0 to 0.100%, Cr: 0 to 1. 00%, Co: 0-3.00%, Ni: 0-3.00%, Cu: 0-1.00%, V: 0-1.000%, W: 0-1.00%, Ca: 0-1.0000%, Mg: 0-1.0000%, REM: 0-1.0000%, Sb: 0-1.000%, Zr: 0-1.000%, As: 0-1.000%, one or more elements selected from Ta, Re, Os, Ir, Tc, Pb, Se, Bi, and Sn: 0-1.000% in total, and the balance: Fe and impurities. The reasons for limiting the content of each element are as follows. Hereinafter, the range indicated by "A to B" indicates a range (A or more and B or less) with A being the lower limit and B being the upper limit. However, values marked as "over" or "under" are not included in the lower or upper limit. For example, "over A to B" indicates that the value is over A and equal to or less than B.
[0019] C: 0.20 to 0.70% C is an element that improves the hardenability of steel and increases the strength of the hot-stamped body obtained after the steel sheet is subjected to quenching, such as hot stamping. If the C content is less than 0.20%, it becomes difficult to ensure sufficient strength in the hot-stamped body. Therefore, the C content is set to 0.20% or more. The C content is preferably set to 0.30% or more, and to obtain even higher tensile strength, the C content is more preferably 0.33% or more or more than 0.40%. More preferably, the C content is set to more than 0.44%. On the other hand, if the C content exceeds 0.70%, the number density and average distance of coarse iron-based carbides fall outside the specified range, resulting in a decrease in impact resistance properties (bendability and crack propagation resistance). Therefore, the C content is set to 0.70% or less. The C content is preferably set to 0.60% or less, and more preferably 0.55% or less. That is, the C content is 0.20 to 0.70%, for example, preferably 0.30 to 0.70%, more preferably more than 0.40 to 0.70%, still more preferably more than 0.44 to 0.70%, and may be 0.30 to 0.60%, 0.33 to 0.60%, more than 0.40 to 0.60%, more than 0.44 to 0.60%, or more than 0.44 to 0.55%.
[0020] Si: 0.010 to 2.000% Si is an element that improves the hardenability of steel, suppresses the increase of coarse iron-based carbides, and ensures the number density and average distance of the coarse iron-based carbides, thereby effectively ensuring the impact resistance properties (bendability and crack propagation resistance) of the hot-stamped steel. To achieve the above effects, the Si content is set to 0.010% or more. The Si content is preferably set to 0.100% or more, and more preferably set to 0.200% or more. On the other hand, if the Si content in the steel exceeds 2.000%, the amount of retained austenite increases and the crack propagation resistance deteriorates. Therefore, the Si content is set to 2.000% or less. The Si content is preferably set to 1.500% or less, and more preferably set to 1.000% or less. That is, the Si content is 0.010 to 2.000%, for example, preferably 0.100 to 1.500%, and more preferably 0.200 to 1.000%.
[0021] Mn: 0 to 2.00%. Mn does not necessarily need to be present (it can be 0%), but it is a highly effective element for improving the hardenability of steel and ensuring strength after quenching. Mn also lowers the Ac3 (transformation point) and promotes lower quenching temperatures. Therefore, Mn may be added. To achieve the above effects, the Mn content is preferably 0.05% or more, more preferably 0.15% or more, and even more preferably 0.17% or more or 0.20% or more. On the other hand, if the Mn content exceeds 2.00%, the number density and average distance of coarse iron-based carbides increase, making it impossible to satisfy the number density and average distance of the coarse iron-based carbides, and the impact resistance properties (bendability and crack propagation resistance) after quenching deteriorate. Therefore, the Mn content is set to 2.00% or less. The Mn content is preferably 1.50% or less, more preferably 1.00% or less, and even more preferably 0.80% or less, or 0.60% or less. That is, the Mn content is 0 to 2.00%, for example, preferably 0.05 to 1.50% or 0 to 1.00%, more preferably 0.15 to 1.00%, and further preferably 0.17 to 0.80%, or 0.20 to 0.60%.
[0022] P: 0.100% or less P is an impurity element, and its segregation at grain boundaries reduces grain boundary strength and crack propagation resistance. Therefore, the P content is set to 0.100% or less. The P content is preferably 0.050% or less, 0.030% or less, or 0.020% or less. There is no need to specify a lower limit for the P content, and the lower limit is 0%. However, reducing the P content to less than 0.0001% significantly increases the cost of dephosphorization, which is economically undesirable. Therefore, the P content may be set to 0.0001% or more, 0.001% or more, 0.003% or more, or 0.005% or more. That is, the P content is 0 to 0.100%, for example, preferably 0.0001 to 0.100%.
[0023] S: 0.0100% or less S is an impurity element that forms inclusions in steel. These inclusions serve as fracture initiation points and crack propagation paths, so a high S content reduces impact resistance (bendability and crack propagation resistance). Therefore, the S content is set to 0.0100% or less. The S content is preferably 0.0080% or less, 0.0050% or less, 0.0030% or less, 0.0020% or less, or 0.0010% or less. There is no need to specify a lower limit for the S content, and the lower limit is 0%. However, reducing the S content to less than 0.0001% significantly increases the desulfurization cost, which is economically undesirable. Therefore, the S content may be set to 0.0001% or more, 0.0002% or more, or 0.0003% or more. That is, the S content is 0 to 0.0100%, and for example, preferably 0.0001 to 0.0100%.
[0024] N: 0.0100% or less N is an impurity element that forms nitrides in steel. Because these nitrides act as fracture initiation points and crack propagation paths, a high N content reduces impact resistance (bendability and crack propagation resistance). Therefore, the N content is set to 0.0100% or less. The N content is preferably set to 0.0080% or less, 0.0050% or less. There is no need to specify a lower limit for the N content, and the lower limit is 0%. However, reducing the N content to less than 0.0001% significantly increases the cost of denitrification, which is economically undesirable. Therefore, the N content may be set to 0.0001% or more, 0.0004% or more, or 0.0010% or more. That is, the N content is 0 to 0.0100%, for example, preferably 0.0001 to 0.0100%.
[0025] O: 0.0200% or less O is an impurity element that forms coarse oxides of Al, Ti, Mg, etc., which serve as fracture initiation sites. As the O content increases, the amount of coarse oxides of Al, Ti, Mg, etc. increases, resulting in a decrease in the impact resistance (bendability and crack propagation resistance) of the hot-stamped steel. Therefore, the O content is set to 0.0200% or less. The O content is preferably 0.0100% or less, more preferably 0.0050% or less, and even more preferably 0.0040% or less, 0.0030% or less, or 0.0020% or less. There is no need to specify a lower limit for the O content, and the lower limit is 0%. However, an O content of less than 0.0001% significantly increases deoxidation costs and is therefore economically undesirable. Therefore, the O content may be set to 0.0001% or more, 0.0005% or more, or 0.0010% or more. That is, the O content is 0 to 0.0200%, and for example, preferably 0.0001 to 0.0200%.
[0026] Al: 0.0010 to 0.5000% Al is an element that deoxidizes molten steel to improve its soundness (suppressing the occurrence of defects such as blowholes in the steel). If the Al content is less than 0.0010%, deoxidation is insufficient, resulting in an increase in blowholes and coarse oxides, and reduced impact resistance (bendability and crack propagation resistance). Therefore, the Al content is set to 0.0010% or more. The Al content is preferably 0.0050% or more, 0.0100% or more, 0.0150% or more, 0.0200% or more, or 0.0250% or more. On the other hand, if the Al content exceeds 0.5000%, coarse oxides increase in the steel, reducing the impact resistance (bendability and crack propagation resistance) of the hot-stamped steel. Therefore, the Al content is set to 0.5000% or less. The Al content is preferably 0.4000% or less, 0.3000% or less, 0.2000% or less, 0.1500% or less, 0.1000% or less, or 0.0750% or less. That is, the Al content is 0.0010 to 0.5000%, for example, preferably 0.0050 to 0.4000%, more preferably 0.0100 to 0.3500% or 0.0150 to 0.3000%, and even more preferably 0.0200 to 0.2000%, 0.0250 to 0.1500%, 0.0200 to 0.1000%, or 0.0200 to 0.0750%. In this embodiment, the Al content refers to the total Al content (Total-Al content).
[0027] Mo: 0.0010 to 1.0000% Mo is an element that dissolves in prior austenite grains during heating before hot stamping, thereby increasing the strength of the hot-stamped body. To ensure this effect, the Mo content is set to 0.0010% or more. The Mo content is preferably 0.0100% or more. On the other hand, if the Mo content exceeds 1.0000%, the amount of Mo-based inclusions increases. These inclusions act as crack initiation points and crack propagation paths, so a high Mo content reduces the impact resistance properties (bendability and crack propagation resistance) of the hot-stamped body. Therefore, the Mo content is set to 1.0000% or less. The Mo content is preferably 0.8000% or less or 0.6000% or less. That is, the Mo content is 0.0010 to 1.0000%, and for example, preferably 0.0100 to 0.8000%, or 0.0100 to 0.6000%.
[0028] B: 0.0005 to 0.0100% B is an element that improves the hardenability of steel. If the B content is less than 0.0005%, the hardenability decreases and martensite is reduced, making it impossible to obtain the desired strength. In addition, the impact resistance properties (bendability and crack propagation resistance) decrease. Therefore, the B content is set to 0.0005% or more. The B content is preferably 0.0010% or more, and more preferably 0.0015% or more. On the other hand, if the B content exceeds 0.0100%, the amount of coarse nitrides such as BN increases, and the impact resistance properties (bendability and crack propagation resistance) of the hot-stamped steel sheet decrease. Therefore, the B content is set to 0.0100% or less. The B content is preferably 0.0080% or less, 0.0060% or less, 0.0040% or less, or 0.0030% or less. That is, the B content is 0.0005 to 0.0100%, for example, preferably 0.0010 to 0.0080%, more preferably 0.0015 to 0.0060%, 0.0015 to 0.0040%, or 0.0015 to 0.0030%.
[0029] Ti: 0.010 to 0.100% Ti is an element that fixes nitrogen as TiN, improves hardenability through solute B, and increases the strength of hot-stamped steel through precipitation strengthening by forming fine carbides and carbonitrides. If the Ti content is less than 0.010%, these effects cannot be achieved. Therefore, the Ti content is set to 0.010% or more. The Ti content is preferably 0.020% or more or 0.030% or more. On the other hand, if the Ti content exceeds 0.100%, the amount of coarse TiN and nitrides and carbonitrides such as (Ti, Nb)(C, N) increases in the steel, degrading the impact resistance (bendability and crack propagation resistance) of the hot-stamped steel. Therefore, the Ti content is set to 0.100% or less. The Ti content is preferably 0.080% or less, 0.060% or less, 0.050% or less, or 0.040% or less. That is, the Ti content is 0.010 to 0.100%, for example, preferably 0.020 to 0.080%, more preferably 0.030 to 0.060%, 0.030 to 0.050%, or may be 0.010 to 0.040%, or 0.020 to 0.040%.
[0030] The chemical composition of the hot-stamped steel according to this embodiment may contain the above-mentioned elements (basic elements) with the balance being Fe and impurities. Alternatively, the hot-stamped steel may further contain one or more of the following elements (optional elements) in place of a portion of Fe:
[0031] Nb: 0 to 0.100% Nb is an element that forms carbides and carbonitrides in steel, thereby increasing the strength of hot-stamped steel through precipitation strengthening. Therefore, Nb may be added. To obtain the above effects, the Nb content is preferably 0.001% or more. The Nb content is more preferably 0.005% or more, 0.009% or more, or 0.015% or more. On the other hand, if the Nb content exceeds 0.100%, the amount of carbides and carbonitrides such as NbC and (Nb, Ti)(C, N) in the steel increases, resulting in a decrease in the toughness of the hot-stamped steel. Therefore, the Nb content is set to 0.100% or less. The Nb content is preferably 0.080% or less, 0.060% or less, or 0.050% or less. That is, the Nb content is 0 to 0.100%, preferably 0.001 to 0.100%, more preferably 0.005 to 0.080%, and further preferably 0.009 to 0.060%, or 0.015 to 0.050%.
[0032] Cr: 0 to 1.00% Cr is an element that dissolves in prior austenite grains during heating before hot stamping, thereby increasing the strength of the hot-stamped body. Therefore, Cr may be added. To obtain the above effect, the Cr content is preferably 0.01% or more. The Cr content is more preferably 0.10% or more or 0.20% or more. On the other hand, if the Cr content exceeds 1.00%, the hydrogen embrittlement resistance (hydrogen embrittlement resistance characteristics) of the hot-stamped body decreases. Therefore, the Cr content is set to 1.00% or less. The Cr content is preferably 0.70% or less, 0.65% or less, 0.60% or less, or 0.55% or less. That is, the Cr content is 0 to 1.00%, for example, preferably 0.01 to 1.00%, more preferably 0.10 to 0.70%, and further preferably 0.20 to 0.65%, 0.20 to 0.60%, or 0.20 to 0.55%.
[0033] Co: 0 to 3.00% Co is an element that increases the strength of the hot stamped body through solid solution strengthening. Therefore, it may be added. To obtain the above effect, the Co content is preferably 0.01% or more. More preferably, it is 0.10% or more, and even more preferably, it is 0.20% or more. On the other hand, even if a large amount of Co is added, the above effect saturates, so the Co content is set to 3.00% or less. Preferably, it is 2.50% or less. More preferably, it is 2.20% or less, 2.00% or less, 1.00% or less, 0.70% or less, 0.65% or less, 0.60% or less, or 0.55% or less. That is, the Co content is 0 to 3.00%, for example, preferably 0.01 to 2.50%, more preferably 0.01 to 2.20%, 0.01 to 2.00%, 0.10 to 2.20%, 0.10 to 2.00%, or 0.20 to 2.00%, and still more preferably 0.20 to 1.00%, 0.20 to 0.70%, 0.20 to 0.65%, 0.20 to 0.60%, or 0.20 to 0.55%.
[0034] Ni: 0 to 3.00% Ni is a useful element for dissolving in austenite, improving the hardenability of steel, and increasing tensile strength. Therefore, it may be added. To obtain the above effects, the Ni content is preferably 0.001% or more. The Ni content is more preferably 0.01% or more, or 0.10% or more. On the other hand, if the Ni content exceeds 3.00%, the above effects saturate and alloy costs increase. Therefore, the Ni content is set to 3.00% or less. The Ni content is preferably 2.50% or less or 2.00% or less, more preferably 1.00% or less, 0.70% or less, 0.65% or less, 0.60% or less, or 0.55% or less. That is, the Ni content is 0 to 3.00%, for example, preferably 0.001 to 2.50% or 0.01 to 2.00%, more preferably 0.10 to 1.00%, and still more preferably 0.10 to 0.70%, 0.10 to 0.65%, 0.10 to 0.60%, or 0.10 to 0.55%.
[0035] Cu: 0 to 1.00% Cu is an element that dissolves in prior austenite grains during heating before hot stamping, thereby increasing the strength of the hot-stamped body. Therefore, Cu may be added. To obtain the above effect, the Cu content is preferably 0.01% or more. More preferably, it is 0.10% or more. On the other hand, even if a large amount is added, the above effect saturates, so the Cu content is set to 1.00% or less. The Cu content is preferably 0.80% or less, 0.60% or less, or 0.30% or less. That is, the Cu content is 0 to 1.00%, for example, preferably 0.01 to 0.80% or 0.01 to 0.60%, more preferably 0.10 to 0.80%, and even more preferably 0.10 to 0.60% or 0.10 to 0.30%.
[0036] V: 0 to 1.000% V is an element that forms carbonitrides in steel and has the effect of increasing the strength of hot-stamped steel through precipitation strengthening. Therefore, V may be added. To obtain this effect, the V content is preferably 0.010% or more. On the other hand, if the V content exceeds 1.000%, a large amount of carbonitrides is formed in the steel, reducing the hydrogen embrittlement resistance of the hot-stamped steel. Therefore, the V content is set to 1.000% or less. The V content is preferably 0.800% or less, 0.600% or less, or 0.300% or less. That is, the V content is 0 to 1.000%, for example, preferably 0.010 to 0.800%, more preferably 0.010 to 0.600%, and even more preferably 0.010 to 0.300%.
[0037] W: 0 to 1.00% W is an element that has the effect of increasing the strength of the hot-stamped body. Therefore, it may be contained. To obtain this effect, the W content is preferably 0.01% or more, and more preferably 0.10% or more. However, even if a large amount is added, the effect saturates, so the W content is set to 1.00% or less. The W content is preferably 0.80% or less, 0.60% or less, or 0.30% or less. That is, the W content is 0 to 1.00%, for example, preferably 0.01 to 0.80%, more preferably 0.01 to 0.60%, even more preferably 0.01 to 0.30%, or 0.10 to 0.30%.
[0038] Ca: 0 to 1.0000% Ca is an element that suppresses the generation of coarse oxides that serve as starting points for fracture. Therefore, it may be contained. To obtain the above effect, the Ca content is preferably 0.0001% or more, and more preferably 0.0010% or more. On the other hand, even if a large amount is added, the above effect saturates, so the Ca content is set to 1.0000% or less. The Ca content is preferably 0.4000% or less, 0.1000% or less, 0.0700% or less, 0.0200% or less, or 0.0100% or less. That is, the Ca content is 0 to 1.0000%, for example, preferably 0.0001 to 0.4000%, 0.0001 to 0.1000%, or 0.0001 to 0.0700%, more preferably 0.0010 to 0.1000%, and still more preferably 0.0010 to 0.0700%, 0.0010 to 0.0200%, or 0.0010 to 0.0100%.
[0039] Mg: 0 to 1.0000% Mg is an element that forms fine oxides and sulfides in molten steel and suppresses the formation of coarse MnS. Furthermore, Mg has the effect of dispersing a large number of fine oxides and refining the metal structure. Therefore, Mg may be added. To obtain the above effect, the Mg content is preferably 0.0001% or more. On the other hand, if the Mg content exceeds 1.0000%, the oxides in the steel increase, adversely affecting the toughness of the hot-stamped steel. Therefore, the Mg content is set to 1.0000% or less. The Mg content is preferably 0.4000% or less, 0.1000% or less, 0.0700% or less, 0.0200% or less, or 0.0100% or less. That is, the Mg content is 0 to 1.0000%, for example, preferably 0.0001 to 0.4000%, more preferably 0.0001 to 0.1000%, and still more preferably 0.0001 to 0.0700%, 0.0001 to 0.0200%, 0.0001 to 0.0100%, 0.0010 to 0.1000%, 0.0010 to 0.0700%, 0.0010 to 0.0200%, or 0.0010 to 0.0100%.
[0040] REM: 0 to 1.0000% REM is an element that suppresses the generation of coarse oxides that serve as starting points for fracture. Therefore, it may be contained. To obtain the above effect, the REM content is preferably 0.0001% or more, and more preferably 0.0010% or more. On the other hand, even if a large amount is contained, the above effect saturates, so the REM content is set to 1.0000% or less. The REM content is preferably 0.4000% or less, 0.1000% or less, 0.0700% or less, 0.0200% or less, or 0.0100% or less. That is, the REM content is 0 to 1.0000%, for example, preferably 0.0001 to 1.0000%, 0.0001 to 0.4000%, or 0.0001 to 0.1000%, more preferably 0.0010 to 0.1000%, and even more preferably 0.0010 to 0.0700%, 0.0010 to 0.0200%, or 0.0010 to 0.0100%. In this embodiment, REM refers to a total of 17 elements consisting of Sc, Y, and lanthanoids, and the REM content refers to the total content of these elements.
[0041] Sb: 0 to 1.000% Sb is an element that improves the deformability of the hot-stamped steel by suppressing the generation of oxides that serve as fracture initiation sites. Therefore, Sb may be added. To obtain the above-mentioned effects, the Sb content is preferably 0.001% or more, more preferably 0.002% or more, and even more preferably 0.010% or more. However, since the above-mentioned effects saturate even when a large amount of Sb is added, the Sb content is set to 1.000% or less. The Sb content is preferably 0.400% or less, 0.100% or less, 0.050% or less, or 0.020% or less. That is, the Sb content is 0 to 1.000%, for example, preferably 0.001 to 1.000%, 0.001 to 0.400%, 0.001 to 0.100%, 0.001 to 0.050%, or 0.001 to 0.020%, more preferably 0.002 to 0.400%, 0.002 to 0.100%, or 0.010 to 0.050%, and still more preferably 0.001 to 0.020%, 0.002 to 0.020%, or 0.010 to 0.020%.
[0042] Zr: 0 to 1.000% Zr is an element that contributes to inclusion control, particularly to finely dispersing inclusions, and improves the toughness of hot-stamped steel sheets. Therefore, it may be added. To obtain the above effects, the Zr content is preferably 0.001% or more, and more preferably 0.010% or more. On the other hand, if a large amount of Zr is added, deterioration of surface properties may become apparent. Therefore, the Zr content is set to 1.000% or less. The Zr content is preferably 0.400% or less, 0.200% or less, or 0.100% or less. That is, the Zr content is 0 to 1.000%, for example, preferably 0.001 to 1.000%, 0.001 to 0.400%, 0.001 to 0.200%, or 0.001 to 0.100%, more preferably 0.010 to 0.200%, and even more preferably 0.010 to 0.100%.
[0043] As: 0 to 1.000% As is an element that contributes to improving hydrogen embrittlement resistance by reducing the austenite single-phase temperature and thereby refining prior austenite grains. Therefore, it may be contained. To obtain the above effect, the As content is preferably 0.001% or more, and more preferably 0.005% or more. However, since the above effect saturates even when a large amount of As is contained, the As content is set to 1.000% or less. The As content is preferably 0.400% or less, 0.200% or less, or 0.100% or less. That is, the As content is 0 to 1.000%, for example, preferably 0.001 to 1.000%, 0.001 to 0.400%, or 0.005 to 0.400%, more preferably 0.001 to 0.200% or 0.005 to 0.400%, and still more preferably 0.001 to 0.100% or 0.005 to 0.100%.
[0044] One or more elements selected from Ta, Re, Os, Ir, Tc, Pb, Se, Bi, and Sn: 0 to 1.000% in total. Ta, Re, Os, Ir, Tc, Pb, Se, Bi, and Sn are elements that improve hydrogen embrittlement resistance. Therefore, they may be contained. To obtain the above effects, the total content is preferably 0.010% or more. On the other hand, if the total content of these elements exceeds 1.000%, the effect saturates and costs increase. Therefore, if these elements are contained, the total content is 1.000% or less. Preferably, the total content is 0.800% or less, more preferably 0.500% or less, 0.400% or less, 0.200% or less, or 0.100% or less. That is, the total content of one or more elements selected from Ta, Re, Os, Ir, Tc, Pb, Se, Bi, and Sn is 0 to 1.000%, for example, preferably 0.010 to 0.800%, more preferably 0.010 to 0.500%, and even more preferably 0.010 to 0.400%, 0.010 to 0.200%, or 0.010 to 0.100%.
[0045] As described above, the chemical composition of the hot-stamped steel according to this embodiment contains the basic elements with the balance being Fe and impurities, or contains the basic elements and one or more optional elements with the balance being Fe and impurities. Examples of impurities include elements that are mixed in from steel raw materials or scrap and / or during the steelmaking process and are permissible within a range that does not impair the properties of the hot-stamped steel according to this embodiment.
[0046] The chemical composition of the hot-stamped body described above can be measured by a general analytical method after removing the decarburized layer (described below) by mechanical grinding or the like. For example, measurement can be performed using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Elements that are difficult to measure using ICP-AES can be measured by other methods. For example, C and S can be measured using combustion-infrared absorption, N can be measured using inert gas fusion-thermal conductivity, and O can be measured using inert gas fusion-non-dispersive infrared absorption. Tc can be measured using ICP-MS (Inductively Coupled Plasma-Mass Spectrometry). If the hot-stamped body has a coating on its surface, the coating and decarburized layer can be removed by mechanical grinding before analyzing the chemical composition of the base material.
[0047] [Microstructure] <The microstructure at the 1 / 4 depth position includes, in area fraction, 80.0% or more of martensite and 0.0% or more but less than 5.0% of retained austenite> When the area fraction of martensite is below a predetermined amount and a large amount of ferrite, pearlite, or bainite is present, the impact resistance properties (bendability and crack propagation resistance) are reduced. Tensile strength is also reduced. Therefore, the area fraction of martensite is set to 80.0% or more (including 100.0%). In this embodiment, martensite includes so-called fresh martensite and tempered martensite (including self-tempered martensite). To further improve the impact resistance properties (bendability and crack propagation resistance), the area fraction of martensite is preferably 85.0% or more, more preferably 90.0% or more, and even more preferably 95.0% or more. That is, the martensite area is 80.0% or more (up to 100.0%), for example, preferably 85.0 to 100.0%, more preferably 90.0 to 100.0%, and even more preferably 95.0 to 100.0%. Furthermore, retained austenite transforms into hard martensite due to stress-induced transformation during collision deformation. Therefore, a high area fraction of retained austenite reduces crack propagation resistance. In the hot-stamped steel according to this embodiment, the area fraction of retained austenite is less than 5.0% (including 0.0%). To further improve crack propagation resistance, the area fraction of retained austenite is preferably less than 4.0%, more preferably less than 2.0%. That is, the area fraction of retained austenite is 0.0% or more and less than 5.0%, preferably 0.0% or more and less than 4.0%, and more preferably 0.0% or more and less than 2.0%.
[0048] The remainder of the microstructure other than martensite and retained austenite is ferrite, pearlite, and bainite. The area ratio of these components should be 20.0% or less in total (including 0.0%) to ensure 80.0% or more of martensite. The area ratio is preferably less than 20.0%, more preferably 15.0% or less, and even more preferably 10.0% or less or 5.0% or less.
[0049] The area ratio of each structure (each phase) in the microstructure can be determined by the following method. A sample is cut out from an arbitrary position 50 mm or more away from the end of the hot-stamped body (if a sample cannot be taken from this position, a position avoiding the end), in a cross section parallel to the rolling direction and thickness direction (thickness direction of the base steel sheet), so that the metal structure can be observed at a 1 / 4 depth position (in the thickness direction, in the range from 1 / 8 of the thickness from the surface to 3 / 8 of the thickness from the surface). The size of the sample depends on the measuring device, but it should be large enough to allow observation of about 10 mm in the rolling direction.
[0050] The structure of the sample was identified using the following method. A cross section (observation surface) parallel to the rolling and thickness directions was polished with #600 to #1500 silicon carbide paper, and then polished to a mirror finish using a liquid in which diamond powder with a particle size of 1 to 6 μm was dispersed, either in a diluted solution such as alcohol or pure. Next, the sample was polished for 8 minutes at room temperature using colloidal silica with a particle size of 0.25 μm and no alkaline solution, to remove strain introduced into the surface layer. At any longitudinal position on the sample cross section, a length of 200 μm in the rolling direction, centered at 1 / 4 of the thickness from the surface, was measured using electron backscatter diffraction at 0.1 μm measurement intervals over a range from 1 / 8 of the thickness to 3 / 8 of the thickness from the surface, to obtain crystal orientation information. For the measurement, an EBSD analyzer consisting of a thermal field emission scanning electron microscope (JSM-7001F manufactured by JEOL) and an EBSD detector (Hikari detector manufactured by AMETEK) is used. At this time, the degree of vacuum inside the EBSD analyzer is 9.6 × 10 -5The pressure was set to 0.02 Pa or less, the acceleration voltage was 20 kV, the working distance (WD) was 15 mm, and the probe current level was 18. When collecting the EBSD pattern, the camera settings in the "OIM Data Collection" function of the software attached to the EBSD analyzer were set to EXPOSURE TIME 3.65 and Gain 0.39. When detecting the bands of the EBSD pattern, the Max Peak Count of the Hough transformation was set to 9 and the Min Peak Count to 5. For the analysis, the database Iron (Alpha) for bcc crystal structures and the database Iron (Gamma) for fcc crystal structures were selected. If the crystal structure of the tissue to be analyzed is a bct structure, it is analyzed as a bcc structure. The obtained crystal orientation information is used with the "Phase Map" function of the software "OIM Analysis (registered trademark)" attached to the EBSD analyzer to determine that the crystal structure is fcc as retained austenite. The area fraction of this retained austenite is calculated to obtain the area fraction of retained austenite. Next, regions with a bcc crystal structure are determined to be bainite, ferrite, pearlite, or martensite (fresh martensite and tempered martensite). For these regions, the "Grain Orientation Spread MAP" function of the above-mentioned "OIM Analysis (registered trademark)" is used to extract regions with a "Grain Orientation Spread" of 1° or less as ferrite under the condition that boundaries with a crystal orientation difference of 15° or more are considered to be grain boundaries (15° grain boundaries). The area fraction of the extracted ferrite is calculated to obtain the area fraction of ferrite. Next, the "Highlight" function installed in the above-mentioned "OIM Analysis (registered trademark)" is used to separate the ferrite region (the region where the "Grain Orientation Spread" is 1° or less) from the remaining region (the region where the "Grain Orientation Spread" is more than 1°).Next, for the ferrite region (the region where the "Grain Orientation Spread" is 1° or less), the "Grain Average IQ MAP" function installed in the above-mentioned "OIM Analysis (registered trademark)" is used to determine the maximum value Iα of the "Grain Average IQ" of the ferrite region under the condition that the 15° grain boundary is regarded as the crystal grain boundary. Next, for the remaining region (the region where "Grain Orientation Spread" exceeds 1°), the "Grain Average IQ MAP" function installed in the above-mentioned "OIM Analysis (registered trademark)" is used to extract the region where Iα / 2 exceeds "bainite and pearlite" and the region where Iα / 2 or less is "martensite (fresh martensite and tempered martensite)" under the condition that the 15° grain boundary is regarded as a crystal grain boundary. By calculating the area ratio of the extracted "bainite and pearlite" and the area ratio of the extracted "martensite (fresh martensite and tempered martensite)", the area ratios of "bainite and pearlite" and "martensite (fresh martensite and tempered martensite)" are obtained. The area fractions of each structure are obtained using the "Phase MAP," "Grain Orientation Spread MAP," and "Grain Average IQ MAP" functions included in the aforementioned "OIM Analysis (registered trademark)." Here, if the ferrite area fraction is 0%, a separate sample is taken from the hot-stamped body being measured, heated to a temperature of Ac3-70°C, held at that temperature range for 10 minutes, and then quenched from that temperature range to room temperature at an average cooling rate of 100°C / s or more to generate ferrite. The ferrite Iα of that sample is determined using the procedure described above. The determined ferrite Iα is then used to determine the area fractions of bainite, pearlite, and martensite of the hot-stamped body being measured using the procedure described above. To observe the same region as the EBSD measurement region using an SEM, a Vickers indentation is stamped near the observation position. Thereafter, the surface contamination is removed by polishing in the area including the Vickers indentation, and the area is then etched with nital.Next, the same field of view as the EBSD observation surface is observed using a thermal field emission scanning electron microscope (FE-SEM: JSM-7001F manufactured by JEOL) at an acceleration voltage of 15 kV and a secondary electron image at a magnification of 3000. Through the observation, the position of the structure corresponding to the position determined to be martensite in the above-mentioned EBSD structure identification is identified.
[0051] Here, when the rolling direction of the hot-stamped body is unclear, the rolling direction is first determined by the following method before cutting out a sample so that a cross section parallel to the rolling direction and thickness direction can be observed. A test piece is taken from any position at least 50 mm away from the end of the hot-stamped body so that a cross section parallel to the thickness direction can be observed. The cross section of the taken sample is mirror-polished and then observed using an optical microscope at magnifications of 100x, 200x, 500x, and 1000x. Depending on the size of the inclusion, an appropriate magnification at which the dimensions of the inclusion can be measured is selected. The observation range is 500 μm or more in width and across the entire thickness, and areas with dark brightness are determined to be inclusions. During observation, multiple fields of view may be observed so that at least two or more inclusions can be observed. Next, using the cross section initially observed by the above method as a reference, a plane parallel to a plane rotated in 5° increments in the range of 0 to 180° around the thickness direction is observed by the above method. For each inclusion in each cross section obtained, the maximum length is calculated as the inclusion's length, and the length of the inclusion in the direction perpendicular to the direction of the maximum length is calculated as the inclusion's thickness. The average aspect ratio (length / thickness) of multiple inclusions is calculated for each cross section, and the cross section with the largest average aspect ratio is identified. The direction parallel to the longitudinal direction of the inclusion in that cross section is determined to be the rolling direction.
[0052] <In the microstructure at a 1 / 4 depth position, the number density of iron-based carbides having a circle equivalent diameter of more than 0.5 μm present in martensite is 0.050 pieces / μm 2If a large number of coarse carbides (iron-based carbides) having an equivalent circle diameter of more than 0.5 μm are present in martensite, they can become crack initiation points during bending or act as crack propagation initiation points. Therefore, in the hot-stamped steel according to this embodiment, the number density of such coarse iron-based carbides is reduced. Specifically, the number density of iron-based carbides having an equivalent circle diameter of more than 0.5 μm (iron-based carbides having an equivalent circle diameter of more than 0.5 μm) present in martensite is set to 0.050 pieces / μm or less. 2 If the number density of iron-based carbides having a circle equivalent diameter of more than 0.5 μm in martensite is 0.050 pieces / μm, the impact resistance (bendability and crack propagation resistance) will be significantly reduced. 2 From the viewpoint of further improving the impact resistance characteristics (bending property and crack propagation resistance), the number density is set to less than 0.030 particles / μm 2 Preferably, less than 0.020 pieces / μm 2 More preferably, less than 0.010 particles / μm 2 The fewer the coarse iron-based carbides, the more the impact resistance properties (bendability and crack propagation resistance properties) are improved, so there is no lower limit for the number density, but it is preferable that the number density is 0 particles / μm 2 It is not easy to achieve this, so the lower limit is set to 0.0001 particles / μm. 2 The number density is more preferably 0.001 particles / μm 2 More preferably, 0.002 pieces / μm 2 Above, 0.003 pieces / μm 2 Above, 0.005 pieces / μm 2 That is, the number density of iron-based carbides having a circle equivalent diameter of more than 0.5 μm present in martensite is, for example, 0.0001 pieces / μm 2 0.050 pieces / μm or more 2 It may be less than 0.001 particles / μm 2 0.050 pieces / μm or more 2 It may be less than 0.001 particles / μm 2 0.030 pieces / μm or more 2 It may be less than 0.002 particles / μm 2 0.030 pieces / μm or more 2 Less than 0.003 particles / μm 20.020 pieces / μm or more 2 Less than 0.005 pieces / μm 2 0.010 pieces / μm or more 2 It may be less than.
[0053] <In the microstructure at the ¼ depth position, the average distance between iron-based carbides present in martensite and having an equivalent circle diameter of more than 0.5 μm and the nearest iron-based carbide present in other martensite and having an equivalent circle diameter of more than 0.5 μm is 3.0 μm or more.> Even when the above-described coarse iron-based carbides are present, crack propagation resistance is improved by ensuring an average carbide-to-carbide distance between the coarse iron-based carbides of at least a certain amount. Therefore, in the hot-stamped steel according to this embodiment, the average distance between iron-based carbides present in martensite and having an equivalent circle diameter of more than 0.5 μm and the nearest iron-based carbide present in other martensite and having an equivalent circle diameter of more than 0.5 μm is set to 3.0 μm or more. That is, in the hot-stamped steel according to this embodiment, the crack propagation resistance is improved by reducing the presence of closely spaced coarse iron-based carbides. The average distance is preferably 5.0 μm or more, more preferably 8.0 μm or more. The upper limit of the average distance is not limited, but the average distance may be 30.0 μm or less. The average distance is preferably 20.0 μm or less or 15.0 μm or less. That is, the average distance is 3.0 μm or more, but may be, for example, 3.0 to 30.0 μm, 5.0 to 30.0 μm, 5.0 to 20.0 μm, 5.0 to 15.0 μm, or 8.0 to 30.0 μm.
[0054] The identification of iron-based carbides, the measurement of the circle-equivalent diameter of iron-based carbides, the number density of iron-based carbides with a circle-equivalent diameter of more than 0.5 μm, and the average distance between an iron-based carbide with a circle-equivalent diameter of more than 0.5 μm and the nearest other iron-based carbide with a circle-equivalent diameter of more than 0.5 μm can be performed by the following method. The iron-based carbides are identified by performing metallographic identification using the FE-SEM described above, and then observing the same sample with the indentation under a scanning transmission electron microscope (STEM: JEM-2100 manufactured by JEOL). Precipitates are extracted by the extraction replica method within a range of 200 μm in length in the rolling direction and extending from a position 1 / 8 to a position 3 / 8 of the thickness from the surface, with the center being a position 1 / 4 of the thickness from the surface, in the thickness direction, of the field of view in which the metallographic structure is observed. To extract precipitates, carbon is vapor-deposited on the surface of the specimen observed with the FE-SEM as described above, followed by immersion in a stripping solution to dissolve only the base material. The floating replica film is then washed and collected on a grid. The extracted precipitates are observed at 5000x magnification using a scanning transmission electron microscope (STEM) in the area identified as martensite in the metallographic structure (excluding the grid area), and point analysis is performed using energy dispersive X-ray spectroscopy (EDX: JEOL JED-2300T) attached to the microscope. Point analysis is performed at the center of gravity of the observed precipitates (the center of gravity determined from the observed image (planar shape)). Quantitative analysis of precipitates using EDX is performed for all alloy elements listed above except for Fe, C, N, B, O, P, and S. Precipitates containing 70% or more iron (Fe) by mass are determined to be iron-based carbides. Observation of precipitates by STEM is performed at an acceleration voltage of 200 kV, and point analysis of precipitates by EDX is performed at an irradiation current of 2.56 nA, with measurement for 60 seconds at each point. 2 This is done for at least 5 visual fields per visual field. The circle equivalent diameter of precipitates that are determined to be iron-based carbides is obtained. In this case, the maximum length of the iron-based carbides is taken as the major axis and the minimum length as the minor axis, and the major axis x minor axis of the iron-based carbides is calculated. 0.5The value calculated as above is defined as the circle equivalent diameter. Here, the maximum length refers to the maximum length among the intervals between parallel lines that contact the outer periphery of the iron-based carbide when sandwiched between two parallel lines. The minimum length refers to the minimum length among the intervals between parallel lines that contact the outer periphery of the iron-based carbide when sandwiched between the two parallel lines. Carbides with a circle equivalent diameter of more than 0.5 μm are extracted from the iron-based carbide, and the number density in each visual field is calculated by dividing the number by the area in each visual field. The average value of the number densities is defined as the number density of iron-based carbides with a circle equivalent diameter of more than 0.5 μm in the hot-stamped steel according to this embodiment. In addition, the distance between iron-based carbides with a circle equivalent diameter of more than 0.5 μm is measured, and the distance between the closest carbides is determined in each visual field. Specifically, iron-based carbides with a circle equivalent diameter of more than 0.5 μm are extracted, and their centroid coordinates are calculated. Next, one iron-based carbide is arbitrarily selected, and particles are searched for radially from the centroid coordinates of that iron-based carbide. In this case, the step angle for the radial search is set to 1 degree or less. For all carbides detected from the step angle, the shortest distance between the outer peripheries (edges) of the carbides is found and used as the measurement value. This process is performed for all detected carbides to find the distance between the closest carbides. Using the above method, the average value of the distances between the closest carbides measured in each field of view is used as the average distance between the closest other iron-based carbides.
[0055] <Prior austenite grain size is 20.0 μm or less in the microstructure at the ¼ depth> Coarsening of prior austenite grains reduces crash resistance (bendability and crack propagation resistance). Therefore, in the hot-stamped steel according to this embodiment, the prior austenite grain size is set to 20.0 μm or less. From the viewpoint of further improving crash resistance (bendability and crack propagation resistance), the prior austenite grain size is preferably 15.0 μm or less, and more preferably 13.0 μm or less, 12.0 μm or less, 11.0 μm or less, or 10.0 μm or less. On the other hand, there is no particular restriction on the lower limit of the prior austenite grain size. However, in order to improve the hardenability of the hot-stamped steel in the hot stamping process and obtain a predetermined martensite fraction, the prior austenite grain size is preferably 2.0 μm or more, and more preferably 3.0 μm or more. That is, the prior austenite grain size is 20.0 μm or less, but may be, for example, 2.0 to 20.0 μm, 2.0 to 15.0 μm, 3.0 to 15.0 μm, 3.0 to 13.0 μm, 3.0 to 12.0 μm, 3.0 to 11.0 μm, or 3.0 to 10.0 μm.
[0056] The prior austenite grain size (prior γ grain size) can be determined using the following method. A sample is cut from any position at least 50 mm away from the end of the hot-stamped body (or from a position avoiding the end if a sample cannot be taken from this position) so that a cross section parallel to the rolling direction and thickness direction can be observed. The size of the sample depends on the measurement device, but it should be large enough to allow observation of approximately 10 mm in the rolling direction. The cross section to be observed of the sample is polished using #600 to #1500 silicon carbide paper, and then polished to a mirror finish using a diluted solution such as alcohol or a liquid prepared by dispersing diamond powder with a particle size of 1 to 6 μm in pure water. The observation surface is then polished by electrolytic polishing. At any position in the longitudinal direction of the sample cross section, a 200 μm long area is measured at 0.1 μm intervals over a range from 1 / 8 to 3 / 8 of the thickness from the surface, with the center being located at 1 / 4 of the thickness from the surface, to obtain crystal orientation information. For the measurement, an EBSD analyzer consisting of a thermal field emission scanning electron microscope and an EBSD detector may be used, and the EBSD analyzer may be configured with a JEOL JSM-7001F and an AMETEK Hikari detector. At this time, the degree of vacuum in the EBSD analyzer is 9.6 × 10 -5The pressure was set to 0.02 Pa or less, the acceleration voltage was 20 kV, the working distance (WD) was 15 mm, and the probe current level was 18. When collecting the EBSD pattern, the camera settings in the "OIM Data Collection" function of the software attached to the EBSD analyzer were set to EXPOSURE TIME 3.65 and Gain 0.39. When detecting the bands of the EBSD pattern, the Max Peak Count of the Hough transformation was set to 9 and the Min Peak Count to 5. For the analysis, the database Iron (Alpha) for bcc crystal structures and the database Iron (Gamma) for fcc crystal structures were selected. If the crystal structure of the tissue to be analyzed is a bct structure, it is analyzed as a bcc structure. Using the obtained crystal orientation information, the crystal orientation of the prior austenite grains is calculated from the crystal orientation relationship between the prior austenite grains and the crystal grains with a BCC structure after transformation, and this is used to calculate the average crystal grain size of the prior austenite grains. The crystal orientation of the prior austenite grains is calculated using the following method. First, a crystal orientation map of the prior austenite grains is created using the method described in Nippon Steel & Sumitomo Metal Technical Report No. 404 (2016) pp. 24-30. Analysis is performed under the following conditions: the orientation relationship between ferrite (BCC structure) and austenite (FCC structure) has a tolerance angle of within 3 degrees based on the K-S relationship, and when reconstructing the austenite structure, the tolerance error for the orientation difference between austenite grains that are determined to be common austenite is within 5 degrees, and the austenite structure before phase transformation is reconstructed. The grain boundaries of the reconstructed austenite are determined to have a misorientation between adjacent crystal grains of 15 degrees or more. Furthermore, prior austenite grains not entirely included in the photographed field of view, such as at the edge of the photographed field of view, are analyzed using the "Area Fraction" of the "Grain Size (diameter)" chart in the above-mentioned "OIM Analysis (registered trademark)" to obtain the average grain size of the prior austenite grains.
[0057] <Preferably, the decarburization index Dc is 0.085 or greater.> In addition to the above-described microstructure control, the presence of a decarburized layer within a certain range from the surface of the hot-stamped steel sheet enables further improvement in impact resistance (bendability and crack propagation resistance). Conventionally, evaluation criteria for the decarburized layer include the thickness of the decarburized layer and the hardness distribution within the decarburized layer. However, the inventors' studies have found that, although these criteria correlate with impact resistance (bendability and crack propagation resistance), merely controlling these criteria does not necessarily improve impact resistance (bendability and crack propagation resistance). For example, the inventors' studies have found that, even when the decarburized layer thickness (decarburization depth) is the same, if the hardness distribution in the surface layer region is steep (the degree of change in hardness is large), the improvement in bendability is smaller than when the hardness distribution is gradual, and the correlation with the decarburized layer thickness (decarburization depth) is weaker. Therefore, the hot-stamped steel sheet according to this embodiment uses the decarburization index as a new index and controls it to improve impact resistance compared to conventional steel sheets. This index takes into account not only the thickness of the decarburized layer (decarburization depth) but also the hardness information of the surface layer region, and therefore has a high correlation with crashworthiness. Specifically, the decarburization index Dc is set to 0.085 or more. This decarburization index quantifies the amount of carbon loss from the surface of the hot-stamped steel sheet to a position 200 μm away. From the viewpoint of ensuring bendability, the decarburization index Dc is preferably 0.100 or more, more preferably 0.120 or more, 0.130 or more, 0.140 or more, or 0.150 or more. Due to the calculation method of the decarburization index Dc, the upper limit is 1.000. From the viewpoint of ensuring tensile strength, the decarburization index Dc is preferably 0.800 or less. The decarburization index Dc is more preferably 0.500 or less, and even more preferably 0.200 or less. That is, Dc is 0.085 or more, and may be 0.085 or more and 0.800 or less, 0.085 or more and 0.800 or less, 0.100 or more and 0.800 or less, 0.085 or more and 0.500 or less, 0.085 or more and 0.200 or less, 0.100 or more and 0.500 or less, 0.120 or more and 0.500 or less, 0.130 or more and 0.500 or less, 0.140 or more and 0.200 or less, 0.150 or more and 0.500 or less, or 0.150 or more and 0.200 or less.
[0058] The decarburization index Dc can be determined by the following method. A glow discharge optical emission spectrometry (GD-OES) is used to measure the element concentration distribution in the thickness direction of the hot-stamped steel. The measurement range is from the surface of the hot-stamped steel to a position 200 μm from the surface (a position 200 μm deep), and the measurement interval is 0.02 μm or less. Measurements are performed for all elements contained in the hot-stamped steel.
[0059] When the hot-stamped body has a coating on its surface, the surface referred to here is the interface between the coating and the base material. When the surface has a coating or the like, the coating or the like is partially or completely removed by mechanical polishing or chemical polishing so that measurements can be made up to a depth of 200 μm from the surface of the base material (the interface between the base material and the coating or the like) before the GD-OES measurement. In the GD-OES measurement, the region where the Fe concentration (Fe content) is 90 mass% or more is considered to be the base material, and the measurement point where the Fe concentration first reaches 90 mass% or more from the surface is considered to be the surface of the base material. Next, the average value of the measured values (1,000 or more) of the C concentration (C content) from a position 180 μm (180 μm depth position) to a position 200 μm depth from the surface of the hot-stamped body is calculated, and this average value is considered to be the C concentration in the portion not affected by decarburization. However, if measurements can be made down to a depth at which it can be determined that the C content has reached the same level as the average C content of the base material (a portion not affected by decarburization), the measurement range may be extended to a depth of 200 μm toward the surface (but measurements must be made at least 50 μm from the surface). In this case, if, among the measured C concentrations in the region from the deepest part analyzed to a region 20 μm from the deepest part toward the surface, the absolute value of the difference between the average C concentration in the region 20 μm from the deepest part toward the surface and the maximum C concentration measured in the region 20 μm from the deepest part toward the surface is 0.05 mass% or less, and the absolute value of the difference between the average C concentration in the region 20 μm from the deepest part toward the surface and the minimum C concentration measured in the region 20 μm from the deepest part toward the surface is 0.05 mass% or less, the average C concentration in the region 20 μm from the deepest part toward the surface may be used as the C concentration in a portion not affected by decarburization. When the deepest part is 120 μm, "the measured value of the C concentration in the region from the deepest part to 20 μm toward the surface" means the C concentration included in the position from 100 μm to 120 μm.
[0060] In the region from the surface of the hot-stamped body to the C concentration at a position where no decarburization has occurred, the decrease in C concentration per unit depth (the value obtained by subtracting the C concentration at each measurement point from the C concentration at a position where no decarburization has occurred) is calculated, and the integral of the product of the decrease in C concentration by unit depth is determined to be the area of the C-deficient region (area A). Here, unit depth refers to the measurement interval of GD-OES. Next, the product of the C concentration at a position where no decarburization has occurred and 200 (μm) is defined as the reference area (area B), and the value (area A / area B) obtained by dividing the C-deficient area (area A) by the reference area (area B) is defined as the decarburization index Dc.
[0061] Furthermore, in this embodiment, the decarburization depth is defined as the distance from the surface to the position where, as a result of GDS analysis, it is first determined that the C content is equivalent to the average C content of the base material (the C concentration at a position determined to be unaffected by decarburization) (however, a range of 50 μm or more from the surface is analyzed). In the hot-stamped steel according to this embodiment, from the viewpoint of productivity, the decarburization depth is preferably 180 μm or less. More preferably, it is 150 μm or less. Alternatively, it may be a thickness less than ⅛ of the thickness of the flat portion of the steel. The decarburization depth is preferably 10 μm or more.
[0062] <Preferably, the microstructure of the surface layer portion contains more than 5.0% ferrite in terms of area ratio> By including a certain amount or more of a structure softer than the interior of the surface layer portion of the molded body and appropriately controlling the structure of the surface layer portion, it is possible to further improve the impact resistance characteristics (bendability and crack propagation resistance). Therefore, it is preferable that the area ratio of ferrite in the microstructure of the surface layer portion is more than 5.0%. The area ratio of ferrite is preferably 10.0% or more, more preferably 20.0% or more. In the microstructure of the surface layer portion, the remainder other than ferrite is more than 5.0% in total of martensite (fresh martensite, tempered martensite) and / or bainite, and less than 5.0% of retained austenite and pearlite.
[0063] The microstructure of the surface layer can be observed in the same manner as at the 1 / 4 depth position, and the area ratio of each can be measured. However, the measurement position is not the 1 / 4 depth position, but the range from the surface to 50 μm in the thickness direction.
[0064] [Coating] The hot-stamped steel according to this embodiment may have a coating on part or all of its surface. The coating may be a coating primarily composed of an Fe—Al alloy (Fe—Al coating) or a coating primarily composed of an Fe—Zn alloy (Fe—Zn coating). The coating is also referred to as a film, alloyed plating layer, or intermetallic compound layer. A coating primarily composed of an Fe—Al alloy is a coating containing a total of 70 mass% or more of Fe and Al, and a coating primarily composed of an Fe—Zn alloy is a coating containing a total of 70 mass% or more of Fe and Zn. The coating primarily composed of an Fe—Al alloy may further contain, in addition to Fe and Al, Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Zn, Co, In, Bi, Zr, Se, As, and REM, with the remainder being impurities. The coating primarily made of an Fe-Zn alloy may contain, in addition to Fe and Zn, Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Al, Co, In, Bi, Zr, Se, As, and REM, with the remainder being impurities. The presence of the coating provides corrosion resistance, thereby improving hydrogen embrittlement resistance in automotive applications. The thickness of the coating is preferably 10 to 100 μm.
[0065] For example, such a coating can be formed by hot stamping or other heat treatment on a steel sheet having an Al-based coating (Al-based coating) if the coating is primarily made of an Fe—Al alloy. Alternatively, a coating can be formed by hot stamping or other heat treatment on a steel sheet having a Zn-based coating (Zn-based coating) if the coating is primarily made of an Fe—Zn alloy. An Al-based coating is a coating containing 70% by mass or more of Al, and a Zn-based coating is a coating containing 70% by mass or more of Zn. The Al-based coating may contain Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Zn, Co, In, Bi, Zr, Se, As, and REM, with the remainder being impurities. The Zn-based coating may further contain, in addition to Zn, Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Al, Co, In, Bi, Zr, Se, As, and REM, with the remainder being impurities.
[0066] The chemical composition and thickness of the coating can be determined by line analysis (qualitative and quantitative analyses described below) using a cross-section field emission electron microanalyzer (FE-EPMA). Specifically, a sample is cut from any position 50 mm or more away from the end of the hot-stamped compact (if a sample cannot be taken from this position, a position avoiding the end) so that a cross section parallel to the rolling direction and thickness direction can be observed. The size of the sample depends on the measurement device, but it should be large enough to allow observation of approximately 10 mm in the rolling direction. Next, the cross section parallel to the rolling direction and thickness direction (observation surface) is polished with #600 to #1500 silicon carbide paper, and then polished to a mirror finish using a diluted solution such as alcohol or a pure dispersion of diamond powder with a particle size of 1 to 6 μm. Line analysis of the sample is performed using the FE-EPMA. The observation range using the FE-EPMA (JXA-8530F manufactured by JEOL) is set at 500x magnification, and the content of each element is quantitatively analyzed by line analysis. FE-EPMA uses an acceleration voltage of 15 kV and a beam diameter of 100 nm to perform line analysis (qualitative analysis) across the entire wavelength range using a high-speed scanning method to detect the contained elements. Next, under the same conditions of acceleration voltage and beam diameter, an irradiation time per point of 1000 ms, and a measurement pitch of 60 nm, line analysis (quantitative analysis) is performed using the ZAF method for the elements Fe, Al, Zn, and Si, as well as other elements detected by the above-mentioned qualitative analysis, over a length of 200 μm from the surface of the coating in the depth direction of the plate thickness, to determine the quantitative value of each element. The region where the Fe concentration is 90% by mass or more is defined as the base material, and the region where the Fe concentration is less than 90% by mass is defined as the coating. The depth direction distance from the surface of the coating to the position where the Fe concentration first reaches 90% by mass or more is measured, and this is defined as the coating thickness. The above-mentioned coating thickness measurement is performed five times per field of view, with measurement points spaced at a distance of 10 μm or more between each measurement point. This is performed for any 10 fields of view. The average value of the coating thickness obtained from the above-mentioned 50 measurements is taken as the coating thickness. The chemical composition of the coating is determined in the process of measuring the coating thickness described above.Specifically, in the quantitative analysis for measuring the thickness of the coating described above, the average values of the analyzed elements Fe, Al, Zn, and Si, as well as the other elements detected in the qualitative analysis described above, are calculated for the range from the "surface of the coating" to the "position where the Fe concentration first becomes less than 90 mass %," to determine the chemical composition of the coating. This measurement is performed five times per field of view, with the measurement points spaced at a distance of 10 μm or more. This is performed for any 10 fields of view. The average value of a total of 50 measurements of the chemical composition of the coating obtained per measurement is calculated, and this is used as the chemical composition of the coating.
[0067] [Characteristics] (Tensile strength) In the hot stamped steel according to this embodiment, the tensile strength is preferably 1500 MPa or more in consideration of contributing to weight reduction of automobile bodies. The tensile strength is preferably 1800 MPa or more, more preferably 2000 MPa or more, and even more preferably 2200 MPa or more. In order to ensure hydrogen embrittlement resistance, the tensile strength may be 3000 MPa or less.
[0068] Tensile strength was measured by taking a sub-size plate test piece (parallel length: 32 mm, parallel width: 6.25 mm) conforming to ASTM A370:2022 from a flat portion of the hot-stamped body (for example, in the case of a hat-shaped member, the top plate portion or other flat portion) with the material thickness intact (without removing the coating if present), so that the tensile direction was parallel to the rolling direction, and performing a tensile test conforming to JIS Z 2241:2022 with a gauge length of 25 mm and a crosshead displacement rate of 1.0 mm / min at 20°C. The tensile strength was calculated as the maximum test force divided by the cross-sectional area obtained by multiplying the material thickness (thickness excluding the measured coating thickness if present) by the parallel width of 6.25 mm.
[0069] (Impact Resistance Characteristics) As described above, the hot-stamped steel according to this embodiment has excellent impact resistance characteristics (bendability and crack propagation resistance) due to the controlled chemical composition and microstructure. As described below, a bending test is performed to measure bendability. A sample having a width of 30 mm in the direction perpendicular to the rolling direction and a length of 60 mm in the rolling direction is taken from a flat portion of the hot-stamped steel (for example, in the case of a hat-shaped member, the top plate portion or other flat portion) with the thickness of the hot-stamped steel intact (without removing the coating, if present), in accordance with VDA standard VDA238-100:2017, with the bend ridgeline oriented perpendicular to the rolling direction. The product of the maximum bend angle and tensile strength obtained by the bending test is preferably 80,000 (MPa·degrees) or more. It is more preferably 90,000 (MPa·degrees) or more. It is even more preferably 100,000 (MPa·degrees) or more. The crack propagation resistance is determined by tests in accordance with JIS Z 2242: 2018 and JIS B 7755: 2011. A test piece (having a shape conforming to JIS Z 2242: 2018, including the notch shape described below, except for the thickness) measuring 10 mm wide and 55 mm long is taken from a flat portion of the hot-stamped body (for example, in the case of a hat-shaped member, the top plate portion or other flat portion) using the original thickness of the hot-stamped body (without removing the coating, if any), with the rolling direction being the longitudinal direction of the test piece, and a 2 mm deep V-notch (notch angle: 45°, notch bottom radius: 0.25 mm, notch bottom width: 8 mm, notch position (center): 27.5 mm from the longitudinal end of the test piece) is formed in this test piece, and three pieces are stacked and fixed with screws to perform an instrumented impact test. However, if the plate thickness is 2.00 mm or less, the test is performed with three plates stacked, but if the plate thickness is over 2.00 mm, the test is performed with a single plate without stacking. The instrumented impact test is performed at 20°C, and the time from the start to the end of the test and the impact force are measured. Next, the displacement is calculated from the product of the test speed and the measured time of the instrumented impact test. Since the fracture surface length of the Charpy test specimen is 8 mm, the average value of the impact force measured in the area where the displacement is 8 mm or more is taken as the background. After subtracting the background from the impact force at all measurement points, an impact force-displacement curve is created. Figure 1 shows an example of an impact force-displacement curve obtained by instrumented impact testing.Since the impact force obtained in the instrumented Charpy test contains noise due to natural vibration, a smoothing process is performed by performing a 30-point moving average. The area under the obtained impact force-displacement curve from 0 mm to 8 mm of displacement was calculated, and the obtained value was defined as the total impact energy. Next, the impact force at which a sudden drop in the impact force-displacement curve begins (the time of crack initiation in Figure 1) is found, and the corresponding displacement (displacement at crack initiation) is determined. The area under this curve from 0 mm of displacement to the time of crack initiation is calculated as the crack initiation energy. The value obtained by subtracting the crack initiation energy from the total impact energy is defined as the crack propagation energy. The ratio of the crack propagation energy to the total impact energy (crack propagation energy / (crack initiation energy + crack propagation energy)) is used as an index of crack propagation resistance. A sudden drop in the impact force-displacement curve refers to a case where the impact force reduction per unit displacement is accompanied by an impact force reduction of 50% or more of the maximum impact force measured. For crack propagation resistance, it is preferable that the ratio of crack propagation energy / (crack initiation energy + crack propagation energy) is 0.10 or greater. It is more preferably 0.20 or more, and even more preferably 0.30 or more.
[0070] (Thickness) In the hot stamped steel, the thickness of the flat portion (the thickness of the steel sheet (excluding the coating) serving as the base material) is preferably 0.8 to 3.0 mm from the viewpoint of hardenability. The thickness may be 1.2 to 3.0 mm, 1.4 to 3.0 mm, or 1.5 to 3.0 mm.
[0071] <Manufacturing Method> The hot stamped product according to this embodiment can be manufactured by a manufacturing method including the following steps. (I) a preliminary heat treatment step in which a steel sheet having a predetermined chemical composition is heated to a temperature range of more than 950°C and not more than 1200°C at an average heating rate of 2°C / s or more, the steel sheet is held in the temperature range for 1 second or more and not more than 1200 seconds, and after holding, the steel sheet is cooled so that the average cooling rate from the temperature range to a cooling stop temperature of 100°C or less is less than 15°C / s and the average cooling rate between 700°C and 500°C is less than 10°C / s; and (II) a hot stamping step in which the steel sheet after the preliminary heat treatment step is heated to a temperature range of Ac3 to 1100°C at an average heating rate of 2°C / s or more and less than 50°C / s, the steel sheet is held in this temperature range for 10 seconds or more and not more than 600 seconds, and after holding, forming is started in a temperature range of 650°C or more, and hot stamp forming (simultaneous cooling in a mold) is performed so that the average cooling rate to 250°C is 10°C / s or more. Furthermore, when forming a coating on the surface of a hot-stamped product, a coating step for forming a coating may be included between the preliminary heat treatment step and the hot stamping step. Preferred conditions for each step are explained below. Well-known conditions can be applied to conditions not explained. Here, Ac3 can be calculated using the content of each element using the following formula: Ac3 (°C) = 910 - 203 × C 0.5 + 66 × Si − 25 × Mn + 700 × P − 11 × Cr + 109 × Al + 400 × Ti − 15.2 × Ni + 104 × V + 31.5 × Mo (1) The element symbols in the above formula (1) indicate the content of each element in mass%, and 0 is substituted when the element is not contained.
[0072] <Preliminary Heat Treatment Step> In the preliminary heat treatment step, a steel sheet (including those having a coating on the surface) having a predetermined chemical composition is heated to a preliminary heat treatment temperature in a temperature range of more than 950°C and less than 1200°C so that the average heating rate is 2°C / s or more, and the steel sheet is held at this temperature range for 1 second to 1200 seconds. After the holding, the steel sheet is cooled so that the average cooling rate from this temperature range (specifically, the temperature at the end of the holding step) to a cooling stop temperature of 100°C or less is less than 15°C / s, and the average cooling rate between 700°C and 500°C is less than 10°C / s. In this step, iron-based carbides that were once dissolved are re-precipitated during cooling and grow by Ostwald ripening, thereby increasing the distance between the iron-based carbides. Although some of the iron-based carbides generated in the preliminary heat treatment step may not be completely dissolved and remain in the subsequent hot stamping step, the average distance between the carbides is ensured to be greater than or equal to a predetermined value, thereby improving crack propagation resistance. The preliminary heat treatment is performed before the hot stamping process, but differs from the annealing performed on cold-rolled steel sheets in the following respects. Annealing performed on ordinary cold-rolled steel sheets is based on the idea of homogenizing the metal structure of the base material, heating at a low temperature within a range that does not coarsen the prior austenite grain size, suppressing coarsening of iron-based carbides, and finely dispersing them to ensure stretch flangeability, elongation, etc. In contrast, the preliminary heat treatment in this embodiment is different in that it is based on the idea of remelting the iron-based carbides formed in the cold-rolling annealing stage by high-temperature heating, and coarsening the iron-based carbides by Ostwald ripening during the cooling process, thereby controlling the distance between carbides and controlling the crack propagation resistance after hot stamping.
[0073] If the average heating rate to the pre-heat treatment temperature is less than 2°C / s, prior austenite grains will coarsen, resulting in a deterioration in impact resistance properties (bendability and crack propagation resistance). While there is no upper limit to the average heating rate, productivity in terms of fuel consumption will decrease, so the average heating rate is preferably 50°C / s or less, more preferably 10°C / s or less. Furthermore, if the pre-heat treatment temperature (holding temperature range) is 950°C or less, the iron-based carbides in the steel sheet will remain undissolved, and the number density of iron-based carbides with a circle equivalent diameter of more than 0.5 μm and the average distance between iron-based carbides will not fall within the desired range after the hot stamping process. In this case, the impact resistance properties (bendability and crack propagation resistance) will decrease. On the other hand, if the pre-heat treatment temperature is more than 1200°C, prior austenite grains will coarsen. In this case, the impact resistance properties (bendability and crack propagation resistance) will decrease. If the holding time in the above temperature range is less than 1 second, the iron-based carbides in the steel sheet will remain undissolved, and the number density and average distance of iron-based carbides having a circle-equivalent diameter of more than 0.5 μm will not fall within the desired range after the hot stamping process. On the other hand, if the holding time exceeds 1,200 seconds, the prior austenite grains will become coarse. In this case, the impact resistance properties (bendability and crack propagation resistance) will be reduced.
[0074] If the average cooling rate from the holding temperature to the cooling stop temperature of 100°C or less is 15°C / s or more, Ostwald ripening of iron-based carbides formed during cooling is insufficient, and the average distance of iron-based carbides having a circle-equivalent diameter of more than 0.5 μm after the hot stamping process does not fall within the desired range. There is no particular lower limit for the average cooling rate from the holding temperature to the cooling stop temperature of 100°C or less, but from the viewpoint of productivity, the average cooling rate to 100°C or less is preferably 2°C / s or more, and more preferably 5°C / s or more. Ostwald ripening is particularly affected by the temperature range of 700 to 500°C. Therefore, even if the average cooling rate from the holding temperature to the cooling stop temperature of 100°C or less is less than 15°C / s, if the average cooling rate from 700 to 500°C is 10°C / s or more, Ostwald ripening of iron-based carbides formed during cooling is insufficient, and the average distance of iron-based carbides having a circle-equivalent diameter of more than 0.5 μm after the hot stamping process does not fall within the desired range. Therefore, both cooling rates must be satisfied. While the lower limit of the average cooling rate from 700 to 500°C is not particularly specified, from the viewpoint of productivity, the average cooling rate from 700 to 500°C is preferably 1°C / s or higher, and more preferably 4°C / s or higher. Furthermore, if hot stamping is performed without cooling to 100°C or lower, untransformed austenite with concentrated carbon remains. This untransformed austenite may decompose into iron-based carbides during heating in the hot stamping process, resulting in an excessive number density of iron-based carbides with a circle-equivalent diameter of more than 0.5 μm. Therefore, cooling is performed to 100°C or lower under the above conditions.
[0075] Since the chemical composition does not change during the preliminary heat treatment process and the subsequent hot stamping process, the chemical composition of the steel sheet subjected to the preliminary heat treatment process may be the same as that of the hot-stamped steel sheet to be finally obtained. The steel sheet may be either a hot-rolled steel sheet or a cold-rolled steel sheet, and is not limited thereto. The manufacturing method is also not limited, but it may be manufactured under the conditions described below, for example. The microstructure of the steel sheet subjected to the preliminary heat treatment process is not limited, but from the viewpoint of workability, it is preferably a structure consisting of ferrite and pearlite. The remaining structure may include bainite or retained austenite.
[0076] <Coating Step> When a coating is formed on the surface, a coating step may be included after the preliminary heat treatment step and before the hot stamping step. In the coating step, a coating is formed on the surface of the steel sheet to produce a coated steel sheet. The coating method is not particularly limited, and methods such as hot-dip galvanization, electroplating, vacuum deposition, cladding, and thermal spraying are possible. Hot-dip galvanization is the most widely used method industrially. Examples of coating methods include Al-based coatings containing Al and Zn-based coatings containing Zn. When an Al-based coating is applied, this coating becomes an Fe-Al-based coating in the subsequent hot stamping step. Furthermore, when a Zn-based coating is applied, this coating becomes an Fe-Zn-based coating in the subsequent hot stamping step.
[0077] When an Al-based coating is formed by hot-dip plating, the plating bath often contains Fe as an impurity in addition to Al. Furthermore, as long as the plating bath contains 70 mass% or more of Al, the plating bath may contain Si, Mg, Ca, Sr, Ni, Cu, Mo, Mn, Cr, C, Nb, Ti, B, V, Sn, W, Sb, Zn, Co, In, Bi, Zr, Se, As, or misch metal in addition to the elements described above. When hot-dip plating is performed, the steel sheet after the preliminary heat treatment step may be heated to a temperature close to the plating bath temperature (e.g., 650 to 750°C for Al-based plating, 400 to 500°C for Zn-based plating).
[0078] There are no particular limitations on the pre-treatment or post-treatment for coating, and possible treatments include pre-coating, solvent application, alloying treatment, etc. As the alloying treatment, for example, heat treatment at 450 to 600°C can be performed for Zn-based plating, and heat treatment at 650 to 750°C can be performed for Al-based plating.
[0079] <Hot Stamping Process> In the hot stamping process, the steel sheet after the preliminary heat treatment process or the coating process is heated to a hot stamp heating temperature in a temperature range of Ac3 (°C) or higher and 1100°C or lower at an average heating rate of 2°C / s or higher and less than 50°C / s, and is held in this temperature range for 10 seconds or higher and 600 seconds or lower. After holding, forming begins in a temperature range of 650°C or higher, and hot stamping (simultaneous cooling in a mold) is performed so that the average cooling rate to 250°C is 10°C / s or higher. In this process, the prior austenite grain size and the area ratio of each phase in the microstructure are mainly controlled.
[0080] If the average heating rate up to the hot stamp heating temperature is less than 2°C / s, the prior austenite grains coarsen. On the other hand, if the average heating rate is 50°C / s or more, the amount of undissolved iron-based carbides with a circle-equivalent diameter of more than 0.5 μm increases, and the number density and average distance between iron-based carbides with a circle-equivalent diameter of more than 0.5 μm cannot be within the specified range. Furthermore, if the hot stamp heating temperature (and the subsequent holding temperature range) is less than Ac3 (°C), the ferrite area ratio increases in the microstructure at the 1 / 4 depth position of the hot stamped body, and the specified martensite area ratio cannot be obtained. Furthermore, the amount of undissolved iron-based carbides increases, and the number density of iron-based carbides with a circle-equivalent diameter of more than 0.5 μm and the average distance between iron-based carbides with a circle-equivalent diameter of more than 0.5 μm do not fall within the desired range. If the heating temperature exceeds 1100°C, the prior austenite grains coarsen, and the impact resistance properties (bendability and crack propagation resistance) deteriorate. Furthermore, from the viewpoint of suppressing deterioration in impact resistance properties (bendability and crack propagation resistance), the heating temperature is preferably 1000°C or lower, and more preferably 950°C or lower. Furthermore, if the holding time is less than 10 seconds, excessive undissolved iron-based carbides having a circle equivalent diameter of more than 0.5 μm are generated, and the number density and average distance of iron-based carbides having a circle equivalent diameter of more than 0.5 μm cannot be set within the predetermined range. On the other hand, if the holding time is more than 600 seconds, prior austenite grains become coarse.
[0081] If the hot stamping start temperature is less than 650°C, ferrite increases, and the hot stamped steel sheet cannot achieve a predetermined martensite area ratio. If the average cooling rate to 250°C is less than 10°C / s, at least one of ferrite, pearlite, and bainite increases during cooling, and the hot stamped steel sheet cannot achieve a predetermined martensite area ratio.
[0082] [Preferred Manufacturing Method of Steel Sheet to be Subjected to Preliminary Heat Treatment Step] The steel sheet to be subject to the preliminary heat treatment step is obtained under manufacturing conditions that include, for example, the following "heating step," "hot rolling step," and "coiling step," and further include, as necessary, a "cold rolling step" and / or an "annealing step." Furthermore, when a coated hot stamped steel sheet is to be obtained, a "coating formation step" may be further carried out to form a coating on the steel sheet to be subject to the preliminary heat treatment step.
[0083] "Heating step" In the heating step, a steel material such as a slab having a predetermined chemical composition is heated before being subjected to hot rolling. The heating temperature is preferably 1100°C or higher, and the holding time in this temperature range is preferably 20 minutes or longer. After this holding time, hot rolling is performed.
[0084] In view of the rolling load in the hot rolling process, the heating temperature is preferably 1100°C or higher and the holding time is preferably 20 minutes or longer. More preferably, the heating temperature is 1200°C or higher and the holding time is 25 minutes or longer. The heating temperature is preferably 1350°C or lower and the holding time is preferably 120 minutes or shorter.
[0085] "Hot Rolling Step" The hot rolling step usually includes rough rolling, finish rolling, and coiling. Of these, in terms of plate shape, the finish rolling is preferably carried out in a temperature range where the finish rolling temperature (completion temperature) is 800°C or higher, more preferably 830°C or higher. The finish rolling temperature is preferably 1050°C or lower.
[0086] After finish rolling, the steel sheet is wound into a coil, thereby obtaining a hot-rolled steel sheet. The coiling temperature is preferably 750°C or less in order to promote scale removal in the subsequent pickling step. In addition, the coiling temperature is preferably 600°C or more in terms of the rolling load in the cold rolling step.
[0087] [Cold Rolling Step] The steel sheet subjected to the preliminary heat treatment step may be a hot-rolled steel sheet after the hot rolling step, or may be a cold-rolled steel sheet obtained by cold-rolling a hot-rolled steel sheet. When a cold-rolled steel sheet is obtained, the cold rolling may be cold-rolling performed at a normal cumulative reduction, for example, a cumulative reduction of 30 to 90%. When cold-rolling is performed, the hot-rolled steel sheet may be subjected to a reheating treatment (hot-rolled sheet annealing) for the purpose of softening before cold rolling.
[0088] [Annealing Process] The cold-rolled steel sheet after cold rolling may be annealed for the purpose of homogenizing the steel structure. Examples of annealing conditions include heating to a temperature range of 750 to 900°C (annealing temperature), holding at this temperature range for 10 to 600 seconds, and then cooling to 500°C or less at an average cooling rate of 5°C / s or more. From the viewpoint of promoting recrystallization of the steel structure and homogenizing the steel structure, the annealing temperature is preferably 750°C or higher and the holding time in this temperature range is preferably 10 seconds or more. Furthermore, from the viewpoint of productivity, the annealing temperature is preferably 900°C or lower and the holding time in this temperature range is preferably 600 seconds or less. On the other hand, when the decarburization index Dc of the hot-stamped steel sheet is to be 0.085 or higher, it is preferable to decarburize the surface region of the steel sheet (a certain range from the surface) by controlling the annealing atmosphere in the annealing process. The annealing atmosphere contains 2 to 20% by volume of hydrogen and the remainder is impurities such as nitrogen and oxygen, and has a dew point of -10°C or higher and 20°C or lower. 2It is preferable to use an atmosphere containing O. In order to increase the oxygen potential in the atmosphere and promote decarburization, thereby increasing the decarburization index, the hydrogen concentration is preferably 2 vol% or more and the dew point is -10°C or more, preferably 3 vol% or more and 0°C or more, and more preferably 4 vol% or more and 5°C or more. On the other hand, in order to suppress condensation on the equipment and not hinder productivity, the hydrogen concentration is preferably 20 vol% or less and the dew point is 20°C or less, preferably 15 vol% or less and 15°C or less, and more preferably 10 vol% or less and 10°C or less. In addition, in order to promote the decarburization reaction and increase the decarburization index, the annealing temperature is preferably 780°C or more, more preferably 790°C or more. In addition, from the viewpoint of productivity, the annealing temperature is preferably 890°C or less, more preferably 880°C or less. In order to promote the decarburization reaction and increase the decarburization index, the holding time in this temperature range is preferably 20 seconds or more, more preferably 60 seconds or more. From the viewpoint of productivity, the holding time in this temperature range is preferably 590 seconds or less. Furthermore, when the ferrite area ratio in the surface layer portion of the hot-stamped steel is to exceed 5.0%, in addition to the above annealing conditions, it is preferable to control the annealing temperature to 820°C or higher and the holding time in this temperature range to 90 seconds or longer.
[0089] Slabs (steel types 1 to 61) having the chemical compositions shown in Tables 1-1 to 1-4 were prepared. (The "total of Ta, etc." column in the tables indicates the total content of one or more elements selected from Ta, Re, Os, Ir, Tc, Pb, Se, Bi, and Sn.) These slabs were subjected to a heating process, a hot rolling process, a cold rolling process, and an annealing process under the conditions shown in Tables 2-1 to 2-4, to obtain steel sheets of Test Nos. 1 to 113. In the tables, "-" indicates that the process was not performed. The average cooling rates in the annealing process in Tables 2-1 to 2-4 are the average cooling rates after holding to a cooling stop temperature of 500°C or less.
[0090] The obtained steel sheets were subjected to a preliminary heat treatment step and a hot stamping step under the conditions shown in Tables 2-5 to 2-12 to obtain hot-stamped steel sheets. In the hot stamping step, the steel sheets were formed into a hat shape using a die. Some of the steel sheets were also subjected to a coating step before the hot stamping step. In the coating step, hot-dip Zn plating or hot-dip Al plating was performed to form a plating layer on the surface.
[0091]
[0092]
[0093]
[0094]
[0095]
[0096]
[0097]
[0098]
[0099]
[0100]
[0101]
[0102]
[0103]
[0104]
[0105]
[0106]
[0107] The microstructures of the obtained hot-stamped steels at the 1 / 4 depth and in the surface layer were observed as described above, and the area ratios of each structure were determined. Although not shown in the table, the components other than the ferrite in the surface layer were a total of more than 5.0% martensite and / or bainite, and less than 5.0% retained austenite and / or pearlite. Furthermore, in the microstructure at the 1 / 4 depth, the number density of iron-based carbides with a circle-equivalent diameter of more than 0.5 μm present in the martensite and the average distance between the nearest iron-based carbides with a circle-equivalent diameter of more than 0.5 μm were determined. The decarburization index and decarburization depth were also determined. The results are shown in Tables 3-1 to 3-4. For the examples subjected to hot-dip Zn plating or hot-dip Al plating, a coating mainly composed of an Fe—Zn alloy or a coating mainly composed of an Fe—Al alloy was formed to a thickness of 30 μm.
[0108]
[0109]
[0110]
[0111]
[0112] Samples were taken from the top plate of the resulting hat-shaped hot-stamped body, and their tensile strength was measured as follows. Additionally, bendability and crack propagation resistance were evaluated as impact resistance. The results are shown in Tables 3-5 to 3-8.
[0113] [Tensile Strength] Subsize plate test pieces (parallel length: 32 mm, parallel width: 6.25 mm) conforming to ASTM A370:2022 were taken from the top plate portion of the hot-stamped body with the material thickness intact (without removing the coating, if present), so that the tensile direction was parallel to the rolling direction. Tensile strength was measured by performing a tensile test conforming to JIS Z 2241:2022 at 20°C with a gauge length of 25.0 mm and a crosshead displacement rate of 1.0 mm / min. The tensile strength was calculated as the maximum test force divided by the cross-sectional area obtained by multiplying the material thickness (excluding the thickness of the coating, if present) by the parallel width of 6.25 mm. A tensile strength of 1500 MPa or more was considered to be high strength.
[0114] [Bendability] A sample 30 mm wide (in the direction perpendicular to the rolling direction) and 60 mm long (in the rolling direction) was taken from the top plate portion of the hot-stamped body, retaining the material thickness of the hot-stamped body (without removing the coating, if any). A bending test was performed on this sample so that the direction of the bending ridge was perpendicular to the rolling direction. The bending test was performed in accordance with VDA standard VDA238-100:2017, and the maximum bending angle was determined. A product of tensile strength and maximum bending angle of 80,000 (MPa degrees) or more was determined to have excellent bendability. A product of tensile strength and maximum bending angle of 90,000 (MPa degrees) or more was determined to have even better bendability, and a product of 100,000 (MPa degrees) or more was determined to have even better bendability.
[0115] [Crack Propagation Resistance] The crack propagation resistance was determined by tests in accordance with JIS Z 2242:2018 and JIS B 7755:2011. Specifically, a test piece measuring 10 mm wide and 55 mm long was taken from the top plate portion of the hot-stamped body, using the original thickness of the hot-stamped body (without removing the coating, if any), with the rolling direction aligned with the longitudinal direction of the test piece. A 2 mm-deep V-notch (notch angle: 45°, notch bottom radius: 0.25 mm, notch bottom width: 8 mm, notch position (center): 27.5 mm from the longitudinal end of the test piece) was then formed in this test piece. Three sheets were then stacked and secured with screws, and an instrumented impact test was performed. Here, when the plate thickness was 2.00 mm or less, the test was performed using a three-sheet stack, but when the plate thickness was more than 2.00 mm, the test was performed using a single sheet without stacking. The instrumented impact test was conducted at 20°C, and the time from the start to the end of the test and the impact force were measured. The displacement was calculated from the product of the test speed and the measured time. Because the fracture surface length of the Charpy test specimen was 8 mm, the average value of the impact forces measured in the region where the displacement was 8 mm or more was used as the background. After subtracting the background from the impact forces at all measurement points, an impact force-displacement curve was created. Because the impact force obtained in the instrumented Charpy test contains noise due to natural vibration, a smoothing process was performed by performing a 30-point moving average. Figure 1 shows an example (schematic diagram) of an impact force-displacement curve. For the obtained impact force-displacement curve, the area under the curve from 0 mm to 8 mm displacement was calculated, and the obtained value was used as the total impact energy. Next, using the procedure described above, the impact force at which the impact force-displacement curve began to drop sharply was found, and the corresponding displacement (displacement at crack initiation) was determined. The area under the curve from 0 mm displacement to the displacement at crack initiation was calculated and used as the crack initiation energy. The crack propagation energy was determined by subtracting the crack initiation energy from the total impact energy. The ratio of the crack propagation energy to the total impact energy was used as an index of crack propagation resistance. If the ratio of the crack propagation energy to the total impact energy (crack propagation energy / total impact energy) was 0.10 or more, the crack propagation resistance was determined to be excellent.If the ratio of crack propagation energy to total impact energy was 0.20 or more, it was judged that the crack propagation resistance was better, and if it was 0.30 or more, it was judged that the crack propagation resistance was even better.
[0116]
[0117]
[0118]
[0119]
[0120] As can be seen from the results in Tables 1-1 to 3-8, in the hot stamped steel sheets having a tensile strength of 1500 MPa or more, excellent crash resistance was obtained in examples (invention examples) in which the chemical composition, the area fraction of the microstructure at the 1 / 4 depth position, the number density and average distance of iron-based carbides present in martensite and having an equivalent circle diameter of more than 0.5 μm, and the prior austenite grain size were within the ranges of the present invention.
[0121] In the comparative examples, the tensile strength was less than 1500 MPa, or even if the tensile strength was 1500 MPa or more, one or more of the chemical composition, the area fraction of the microstructure at the 1 / 4 depth position, the number density and average distance of iron-based carbides having a circle equivalent diameter of more than 0.5 μm present in martensite, and the prior austenite grain size were outside the range of the present invention. As a result, sufficient crash resistance properties were not obtained.
[0122] According to the present invention, it is possible to provide a hot-stamped product having high strength and excellent crash resistance, and therefore has high industrial applicability.
Claims
1. By mass, C: 0.20-0.70%, Si: 0.010-2.000%, Mn: 0-2.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, O: 0.0200% or less, Al: 0.0010-0.5000%, Mo: 0.0010-1.0000%, B: 0.0005-0.0100%, Ti: 0.010-0.100%, Nb: 0-0.100%, Cr: 0-1.00%, Co: 0-3.00%, Ni: 0-3.00%, Cu: 0-1.00%, V: 0-1.000%, the chemical composition consisting of W: 0-1.00%, Ca: 0-1.0000%, Mg: 0-1.0000%, REM: 0-1.0000%, Sb: 0-1.000%, Zr: 0-1.000%, As: 0-1.000%, one or more selected from Ta, Re, Os, Ir, Tc, Pb, Se, Bi, and Sn: 0-1.000% in total, and the balance: Fe and impurities, and when the range from the surface to the thickness direction is defined as the 1 / 4 depth position, the microstructure at the 1 / 4 depth position comprises, in area ratios, martensite: 80.0% or more, and retained austenite: 0.0% or more and less than 5.0%, In the microstructure at the 1 / 4 depth position, the number density of iron-based carbides having a circle equivalent diameter of more than 0.5 μm present in the martensite is 0.050 pieces / μm 2 the average distance between the iron-based carbide and the nearest other iron-based carbide is 3.0 μm or more; and in the microstructure at the ¼ depth position, a prior austenite grain size is 20.0 μm or less.
2. The hot stamped steel according to claim 1, characterized in that the decarburization index Dc is 0.085 or more.
3. The hot stamped product according to claim 1 or 2, characterized in that, when the range from the surface to 50 μm is defined as a surface layer portion, the microstructure of the surface layer portion contains, in terms of area ratio, ferrite: more than 5.0%.
4. The chemical composition is, in mass%, C: over 0.40% and 0.70% or less, Si: 0.010 to 2.000%, Mn: 0 to 1.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, O: 0.0200% or less, Al: 0.0010 to 0.5000%, Mo: 0.0010 to 1.0000%, B: 0.0005 to 0.0100%, Ti: 0.010 to 0.100%, Nb: 0 to 0.100%, Cr: 0 to 1.00%, Co: 0 to 3.00%, Ni: 0 to 3.00%, Cu: 0 to 1.00%, 3. The hot stamped body according to claim 1 or 2, characterized in that it consists of V: 0 to 1.000%, W: 0 to 1.00%, Ca: 0 to 1.0000%, Mg: 0 to 1.0000%, REM: 0 to 1.0000%, Sb: 0 to 1.000%, Zr: 0 to 1.000%, As: 0 to 1.000%, one or more elements selected from Ta, Re, Os, Ir, Tc, Pb, Se, Bi, and Sn: 0 to 1.000% in total, and the balance: Fe and impurities.
5. The hot stamped product according to claim 1 or 2, characterized in that the surface thereof is coated.
6. The hot stamped product according to claim 5, characterized in that the coating is mainly composed of an Fe-Al alloy.
7. The hot stamped product according to claim 5, characterized in that the coating is mainly composed of an Fe-Zn alloy.
Citation Information
Patent Citations
Manufacturing method for collision reinforcing material for vehicle and collision reinforcing material
JP2002102980A
Steel, and method for manufacturing the same, and steel sheet for quenching treatment
JP2012001802A
Hot-press molded steel sheet member, steel sheet for hot-pressed steel sheet member, and method for producing them
JP2012180594A
Information processing device, information processing method, information processing program, and computer-readable recording medium having information processing program recorded thereon
JP2023065610A
Heat-treated steel material and method for producing same
WO2015182591A1
Cited By
Steel member and steel sheet
WO2026225233A1
Post-treatment solution and method for manufacturing steel sheet using same
WO2026230717A1