Fire and heat resistant material
A multi-layered material with a silica fabric and a fire-resistant layer of Na2B4O7·10H2O, PDMS, and ZnO addresses the limitations of existing materials by offering enhanced heat resistance and durability, effectively preventing ignition and fire spread.
Patent Information
- Application Number
- PCT/TR2023/050332
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-08
- Publication Date
- 2024-10-17
AI Technical Summary
Current fire and heat-resistant materials, such as Nomex and Kevlar, have limitations including short heat resistance duration, poor UV resistance, low flexibility, moisture sensitivity, and limited gas absorption efficiency, making them inadequate for long-term protection against high temperatures and environmental exposure.
A multi-layered material comprising a silica fabric with a fire and heat-resistant layer composed of Na2B4O7·10H2O, polidimethyl siloxane (PDMS), silicone, and ZnO, optionally with an aluminum or moisture barrier coating, which is mixed and heated to form a stable chemical bond, enhancing durability and resistance to temperatures up to 1100°C.
The solution provides a durable, long-lasting material resistant to high temperatures and environmental factors, effectively preventing ignition and fire spread, with improved flexibility and gas absorption compared to existing technologies.
Smart Images

Figure TR2023050332_17102024_PF_FP_ABST
Abstract
Description
[0001] FIRE AND HEAT RESISTANT MATERIAL
[0002] Technical Field
[0003] Invention is related with an insulation material which is fire and heat resistant.
[0004] State of the Art
[0005] It has long been desirable to provide methods of treating various useful materials to prevent them from being unduly flammable. This is desirable to prevent immediate ignition of materials upon the application of heat and to prevent the spread of fire if it does become started in the vicinity of the treated material. This sort of treatment is particularly important in materials utilized in structural elements of housing and business buildings and also in furniture. Another area in which flame retardant materials are particularly valuable is in the fighting of fires, such as forest and brush fires. Any and all methods which can possibly be utilized are desirable to stop the spread fires.
[0006] Wearable insulating materials like Nomex, has heat resistance of for only 30 seconds between 425°C - 625°C. Direct sunlight damages the material so it can only wearable during night. Nomex’ s lifetime is only 4 years and can reach the highest temperature in terms of the degree of feeling the heat in the human body, 70°C. One of the disadvantages of this technology is its low gas absorption efficiency: Due to the characteristic of the polymer in its chemical component, the saturation flow density of the product is high. The saturation flow density can typically be specified as 0.5 T'<.
[0007] Kevlar is another technology in state of the art, which is resistant to 550°C- 800°C for 10 seconds. It has a very poor UV resistance and therefore degrades when exposed to sunlight for long time. The structure of Kevlar consists of relatively rigid molecules, which tend to form mostly planar sheet-like structures, such as silk protein. For this reason, the elasticity coefficient is low, and it carries the risk of breakage. In addition to its low flexibility, Kevlar has some additional disadvantages that limit its efficiency. Kevlar fibers absorb moisture quickly, meaning they are more sensitive to their environment than other materials. Although Kevlar is strong and stretchy, its ability to cope with compression is quite poor and can be difficult to cut.
[0008] Boron, which is in IIIA group with the atomic number of 10, is only found in the nature as oxo compounds. Its chemical properties resemble to C and Si rather than same group elements. Although 230 different boron compounds are found in nature, some of them are commercially important. Most important ones are kernite, tincal, ulexite, colemanite, szaibelyite and probertite. In addition to natural ones, numerous boron containing compounds can be synthesized with various chemical methods. Elemental boron, refractory boron compounds (boron nitride (BN), boron carbide (BC)), borates (sodium borate, zinc borate (ZnB), calcium borate (CaB)), organo boron compounds (borate esters, boroxine), boron-phosphorus compounds, boron-halogen compounds, boron-sulfur compounds, boron-nitrogen compounds, and boranes can be synthesized. Boron compounds also find application area as a multifunctional flame-retardant additive in various polymeric materials due to their different modes of flame retardant action both in the condensed and gas phases depending upon the boron compound, polymer and other flame retardant additive types, and amounts. In the condensed phase, increased char formation, the stabilization of the char via physical and chemical routes, hindering the dripping, improvement the barrier effect of char via acting as sintering and fluxing agent are generally observed. Most of the inorganic boron compounds decompose endothermically (heat sink action) and liberates water (fuel dilution). These are the generally observed physical flame -retardant action of boron compounds in the gas phase. As well as the aforementioned flame -retardant actions, some organoboron compounds liberate free radicals acting as radical scavengers during the combustion (flame inhibition) and liberates noncombustible gases rather than water (fuel dilution). With the diversity of action modes, boron containing additives can function as flame retardant, smoke suppressant, afterglow suppressant, antitracking agent, anti-arching agent, and fluxing agent. Boron compounds are used solely or with other flame retardants with various polymers in commercial applications. Boron compounds are commercially used to impart flame retardancy in cellulose-based products (cotton, wood, and paper) and polyvinyl chloride (PVC).
[0009] For cellulosic systems, endothermic release of water and melting to form a sodium borate or boric oxide coating from borate fire retardants (such as boric acid, borax pentahydrate and disodium octaborate tetrahydrate) are responsible for the fire retardancy. Chemically, borates can also react with the C6-hydroxyl group of cellulose to give a borate ester, blocking the release of flammable C-6 fragments. In addition, dehydration of alcohols is enhanced by boric acid, which accounts for the larger quantities of char produced when borate treated cellulose is burned. Boric oxide or any precursors such as boric acid, which can form boric oxide under fire conditions, is well known to reduce afterglow combustions. It is generally believed that boric oxide, a low melting glass, can cover the char and inhibit oxygen permeation, and thus prevent oxidation of the char. Another school of thought believes that effectiveness of boric oxide in afterglow suppression is related to its high ionization energy / or electron affinity. Active sites for oxygen adsorption on the char surface may be deactivated by boric oxide via electron transfer. Ammonium pentaborate, upon thermal decomposition, can evolve a large amount of water, ammonia, and boric oxide, which is a glass former. Ammonium pentaborate functions as both an inorganic blowing agent and a glass forming fire retardant.
[0010] Figure
[0011] Figure 1. Graphic of surface temperature and heat resistivity
[0012] Detailed Description of the Invention
[0013] The invention is a multi-layered material.
[0014] 1) +1100°C flame, steam and water resistant silica fabric
[0015] 2) Fire and heat resistant layer
[0016] Na2B40?.10H20, polidimethyl siloxane (PDMS), silicone and Ah (SO^. ZnO is optionally added.
[0017] 3) Fabric with aluminum or moisture barrier coating
[0018] 4) Fiber wool
[0019] 5) Primer
[0020] In a preffered embodiment, fire and heat resistant layer is as follows:
[0021] • ZnO: 10%
[0022] • Na2B407.10H20: 30%
[0023] • PDMS: 50%
[0024] • Ab (SO4)3): 10%
[0025] Preparation method of fire and heat resistant layer is as follows:
[0026] Mixing Step:
[0027] ZnO, Na2B40?.10H20, PDMS-Silicone and Ab (SO4)3are added together at 50°C and mixed for 5 minutes and then cool.
[0028] Heating Step:
[0029] Prepared mixture is heated to 100°C for 15 minutes. This step solidify and strengthen the material by allowing the mixture to reach a higher temperature and therefore achieve a more stable chemical bond. This heating process could also help to remove any remaining moisture from the material, which could compromise its properties and reduce its durability. Overall, this additional heating step likely serves to ensure that the multi-layered material is as strong and durable as possible, and that it can withstand the high temperatures and other environmental factors it is designed to resist.
[0030] Maintaining Step:
[0031] After the cooling process is finished, it is taken to rest for 24 hours. As a result, a mixture which is resistant to 1100°C heat is obtained.
Claims
CLAIMS1. Fire and heat resistant composition characterized in comprising Na2B40?.10H20, polydimethyl siloxane and ALISON2. Fire and heat resistant composition according to claim 1 characterized in further comprising ZnO.
3. Fire and heat resistant composition according to claim 2 characterized in comprising 30% Na2B40?.10H20, 50% polydimethyl siloxane, 10% A12(SO4)3 and 10% ZnO.
4. Wearable insulating multi-layer material characterized in comprising at least one layer of fire and heat resistant composition according to Claim 3.
5. Wearable insulating multi-layer material according to Claim 4 characterized in comprising layers of: i. flame, steam and water resistant fabric ii. Fire and heat resistant layer iii. Fabric with aluminum or moisture barrier coating iv. Fiber wool
Citation Information
Patent Citations
Multifunctional three-layer composite flame-retardant fabric
CN111452447A
Multilayer structured spun yarn, and heat-resistant fabric and heat-resistant protective garment using multilayer structured spun yarn
JP2016176149A
Knit fabrics and base layer garments made therefrom with improved thermal protective properties
US20090019624A1