Multi-element positive electrode material and preparation method therefor, and lithium ion battery

By adding specific coatings to lithium-ion battery cathode materials and improving preparation methods, the deficiencies in low-temperature and cycle performance of lithium-ion batteries are solved, achieving higher capacity and more stable electrochemical performance.

WO2024216447A1PCT designated stage expired Publication Date: 2024-10-24BEIJING EASPRING MATERIAL TECH CO LTD +2
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/088747
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The capacity and cycle performance of existing lithium-ion batteries' cathode materials cannot meet actual needs, especially in low-temperature environments and electric vehicle applications. The micro-powder problem caused by high-temperature sintering affects the cycle and storage performance of the battery.

Method used

It uses a multi-element cathode material whose surface contains specific point-like or island-like coatings. The arithmetic mean roughness and coverage are measured by a three-dimensional scanning electron microscope, and are prepared by acid solution washing and high-temperature sintering methods to reduce the fine powder content and improve Particle size distribution and coating effect.

Benefits of technology

It significantly improves the capacity and cycle performance of lithium-ion batteries, avoids the problems of poor slurry dispersion and uneven coating caused by micro-powder, and enhances the structural stability and electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023088747_24102024_PF_FP_ABST
    Figure CN2023088747_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium ion batteries. Disclosed are a multi-element positive electrode material and a preparation method therefor, and a lithium ion battery. The surface of the multi-element positive electrode material comprises a dot-shaped coating and / or an island-shaped coating; the particle size D1 of the multi-element positive electrode material at which the cumulative distribution of particles is 1% is greater than or equal to 0.7 μm; the arithmetic average roughness Ra of the coatings of the multi-element positive electrode material measured by a three-dimensional scanning electron microscope meets the equation: 20 nm≤Ra≤200 nm; and the coverage rate Q of the dot-shaped coating and / or island-shaped coating of the multi-element positive electrode material meets the equation: 3%≤Q≤30%. The surface of the multi-element positive electrode material comprises the dot-shaped coating and / or the island-shaped coating, the coatings have specific arithmetic average roughness and coverage rate, and the multi-element positive electrode material has relatively large particle size distribution D1, thereby reducing the content of micro powder in the multi-element positive electrode material, such that a lithium ion battery comprising the positive electrode material has excellent capacity and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Multi-element positive electrode material and preparation method thereof, and lithium-ion battery Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a multi-element positive electrode material and a preparation method thereof, and a lithium ion battery. Background Art

[0002] In recent years, lithium-ion batteries have been widely used in portable electronic devices, electric vehicles, and energy storage systems due to their high energy density.

[0003] Although lithium-ion batteries are widely used, electric vehicles still cannot meet the needs of the majority of consumers compared to fuel vehicles. The main reasons are low mileage, poor low-temperature performance, and safety issues of electric vehicles.

[0004] Cathode materials are a major factor limiting the performance of lithium-ion batteries. While graphite anodes can achieve an energy density of 360 mAh / g, cathode materials, such as ternary 622 materials, have an energy density of only 180 mAh / g. Furthermore, cathode materials are the most expensive and heaviest component of lithium-ion batteries. Therefore, improving the energy density and cycling stability of cathode materials can effectively reduce the weight and price of electric vehicles.

[0005] Summary of the Invention

[0006] The purpose of the present invention is to overcome the problem that the capacity and cycle performance of lithium-ion battery positive electrode materials in the prior art cannot meet actual needs, and to provide a multi-element positive electrode material and its preparation method, and a lithium-ion battery. The surface of the multi-element positive electrode material includes a point-shaped coating and / or an island-shaped coating, and the coating has a specific arithmetic mean roughness and coverage, and the multi-element positive electrode material has a large particle size distribution D1, thereby reducing the content of fine powder in the multi-element positive electrode material, so that the lithium-ion battery containing the positive electrode material has excellent capacity and cycle performance.

[0007] In order to achieve the above-mentioned object, the present invention provides a multi-element positive electrode material in a first aspect, wherein the surface of the multi-element positive electrode material includes a dot-shaped coating and / or an island-shaped coating;

[0008] The cumulative distribution of particles of the multi-element positive electrode material is 1% of the particle size D1 ≥ 0.7 μm;

[0009] The arithmetic average roughness Ra of the coating of the multi-element positive electrode material measured by a three-dimensional scanning electron microscope satisfies: 20nm≤Ra≤200nm;

[0010] The coverage rate Q of the point-shaped coatings and / or island-shaped coatings of the multi-element positive electrode material satisfies: 3%≤Q≤30%.

[0011] A second aspect of the present invention provides a method for preparing a multi-element positive electrode material, the method comprising:

[0012] (1) mixing a multi-element positive electrode material precursor, a first lithium source, and an optional dopant, and subjecting the mixture to a first high-temperature sintering to obtain a multi-element positive electrode material process product 1;

[0013] (2) After the multi-element positive electrode material product 1 is coarsely crushed, it is washed with an acid solution, washed with water, and dried to obtain a multi-element positive electrode material product 2;

[0014] (3) mixing the multi-component positive electrode material process product 2, optionally a second lithium source, and a coating agent, performing a second high-temperature sintering, and screening to obtain the multi-component positive electrode material;

[0015] The conditions for the acid solution flushing include: the concentration of the acid solution is 0.01-0.05 g / mL, and the flushing time is 1-120 s;

[0016] The sintering temperature T2 of the second high temperature sintering is 200-1000°C;

[0017] The coating agent is added in an amount according to a stoichiometric ratio of 0<[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.03.

[0018] A third aspect of the present invention provides a multi-element positive electrode material prepared by the above method.

[0019] A fourth aspect of the present invention provides a lithium-ion battery, comprising the above-mentioned multi-element positive electrode material.

[0020] Through the above technical solution, the multi-element positive electrode material and preparation method thereof, and the lithium-ion battery provided by the present invention achieve the following beneficial effects:

[0021] The surface of the multi-element positive electrode material provided by the present invention includes point-shaped coatings and / or island-shaped coatings, and the coatings have a specific arithmetic mean roughness and coverage, and the multi-element positive electrode material has a large particle size distribution D1, thereby reducing the content of fine powder in the multi-element positive electrode material, so that the lithium-ion battery containing the positive electrode material has excellent capacity and cycle performance.

[0022] In the method for preparing a multi-element positive electrode material provided by the present invention, the dissociation of the multi-element positive electrode material process product 1 obtained by the first high-temperature sintering is achieved by washing with an acid solution, which can achieve a good dissociation effect and does not produce fine powder, thereby avoiding the generation of a large amount of fine powder caused by the traditional strong dissociation method, and further avoiding the poor slurry dispersion, uneven coating and consumption of electrolyte caused by the presence of excessive fine powder, which leads to a decrease in the cycle performance and storage performance of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG1 is a SEM image of a multi-element cathode material process product 2 prepared in Example 1;

[0024] FIG2 is a SEM image of the multi-element cathode material prepared in Example 1; the box is marked with 1 μm 2 Calculate the coverage area.

[0025] FIG3 is a SEM image of a multi-element cathode material product 2 prepared in Comparative Example 1;

[0026] FIG4 is a SEM image of the multi-element cathode material prepared in Comparative Example 1;

[0027] FIG5 is a graph showing the cycle performance of the positive electrode materials prepared in Example 1 and Comparative Example 1 at a 1C rate, wherein the test temperature is 45° C. and the voltage range is 3-4.3V. DETAILED DESCRIPTION

[0028] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0029] A first aspect of the present invention provides a multi-element positive electrode material, characterized in that the surface of the multi-element positive electrode material includes a dot-shaped coating and / or an island-shaped coating;

[0030] The cumulative distribution of particles of the multi-element positive electrode material is 1% of the particle size D1 ≥ 0.7 μm;

[0031] The arithmetic average roughness Ra of the coating of the multi-element positive electrode material measured by a three-dimensional scanning electron microscope satisfies: 20nm≤Ra≤200nm;

[0032] The coverage rate Q of the point-shaped coatings and / or island-shaped coatings of the multi-element positive electrode material satisfies: 3%≤Q≤30%.

[0033] In the existing technology, the multi-element positive electrode materials are mostly hard blocks with serious adhesion between particles. After strong dissociation, they are easy to form micropowders, which remain on the surface of the multi-element positive electrode or are mixed in the multi-element positive electrode materials. During the battery manufacturing process, this will lead to poor slurry dispersion and uneven coating. In addition, the micropowders will consume more electrolyte, thereby affecting the cycle and storage performance of the lithium-ion battery.

[0034] In the present invention, the multi-element positive electrode material has a larger particle size distribution D1, indicating that there are fewer particles with small particle sizes in the multi-element positive electrode material and the content of fine powder in the multi-element positive electrode material is low, so that the lithium ion battery containing the positive electrode material has excellent capacity and cycle performance.

[0035] Furthermore, surface coating of positive electrode materials can significantly improve the structural stability of the materials. In the prior art, in order to improve the cycling and storage performance of lithium-ion batteries, most studies have focused on the influence of the type of coating elements on the materials. The inventors of the present invention have found through research that the coating amount and coating state of the coating on the surface of the multi-element positive electrode material also have a very important influence on the multi-element positive electrode material. Specifically: when the point-shaped coating and / or island-shaped coating contained on the surface of the multi-element positive electrode material has the arithmetic mean roughness and coverage specified in the present invention, the lithium-ion battery made from the multi-element positive electrode material has better electrical performance.

[0036] Furthermore, in the present invention, the multi-component positive electrode material has a low fine powder content, which can prevent the coating from being adsorbed by excessive fine powder, resulting in reduced effective coating and, consequently, reduced capacity of the lithium-ion battery containing the multi-component positive electrode material. Furthermore, in the present invention, the multi-component positive electrode material has a low fine powder content, which can reduce the amount of coating agent used while still ensuring that the lithium-ion battery made from the multi-component positive electrode material has excellent cycle performance and capacity.

[0037] In the present invention, the surface arithmetic average roughness of the coating of the multi-element positive electrode material is measured using a three-dimensional scanning electron microscope (3D-SEM) according to the method of JIS B 0601 (2001) to measure the arithmetic average roughness Ra of the particle surface. The coverage of the coating is calculated as 1 μm on the surface of a single particle under the electron microscope. 2 The total area of ​​the point-like and / or island-like coatings in the region divided by 1 μm 2 The area of ​​the region. The area marked by the box in Figure 2 is averaged over 300 different particles.

[0038] In a preferred embodiment of the present invention, the cumulative distribution of particles of the multi-element positive electrode material is such that 1% of the particle size satisfies 1 μm≤D1≤2 μm;

[0039] The arithmetic average roughness Ra of the coating of the multi-element positive electrode material measured by a three-dimensional scanning electron microscope satisfies 30nm≤Ra≤100nm;

[0040] The coverage rate Q of the point-shaped coatings and / or island-shaped coatings of the multi-element positive electrode material satisfies the following: 5%≤Q≤15%.

[0041] According to the present invention, the cumulative distribution of particles of the multi-element positive electrode material is 50% of the particle size D 502-8 μm, preferably 2.5-7 μm.

[0042] In the present invention, the particle size D1 of the multi-element positive electrode material with a cumulative distribution of 1% and the particle size D 50 Measured by laser particle size analyzer.

[0043] According to the present invention, the average primary particle size P of the multi-element positive electrode material measured by SEM is 50 0.8-6 μm, preferably 1-4 μm.

[0044] According to the present invention, the specific surface area S of the multi-element positive electrode material satisfies: 0.2m 2 / g≤S≤1.2m 2 / g, and / or, 1 / P 50 -0.1≤S≤1 / P 50 +0.2.

[0045] In the present invention, P 50 The unit is μm, S is m 2 / g is the unit, and the above relationship is only a numerical relationship.

[0046] In the present invention, the multi-element positive electrode material has a larger particle size distribution D1, a smaller specific surface area S, and the specific surface area increases with the average size of the primary particles P. 50 The specific surface area S decreases with the increase of the primary particle average size P 50 The size of the multi-element cathode material has a significant correlation, and the relationship between the macroscopic index and the microscopic particle size is established. In particular, when the specific surface area S of the multi-element cathode material satisfies 0.2m 2 / g≤S≤1.2m 2 / g and 1 / P 50 -0.1≤S≤1 / P 50 +0.2, indicating that the appropriate dissociation conditions and coating and sintering conditions were used in the preparation of the positive electrode material, indicating that the multi-element positive electrode material provided by the present invention does not have excessive dissociation to produce fine powder, nor does it have a large amount of adhesion caused by insufficient dissociation. If the particle size distribution D1 is too small (i.e., the content of fine powder is relatively high), the specific surface area S of the multi-element positive electrode material will be too large. If insufficient dissociation leads to more adhesion, the specific surface area S of the multi-element positive electrode material will be too small. Then the specific surface area S is proportional to the average size of the primary particles P. 50 No good arithmetic relationship can be established.

[0047] In the present invention, further, the surface coating condition also affects the specific surface area of ​​the material. If there is too much surface coating residue, the specific surface area is larger, and if there is too little surface coating residue, the specific surface area is smaller. Only when the surface coating residue is within an appropriate range, the above relationship is established and the electrochemical performance of the multi-element positive electrode material is better.

[0048] Furthermore, the specific surface area S of the multi-element positive electrode material satisfies: 0.3m 2 / g≤S≤1m 2 / g, and / or, 1 / P 50 -0.05≤S≤1 / P 50 +0.05.

[0049] In a preferred embodiment of the present invention, the specific surface area S of the multi-element positive electrode material satisfies: 0.2 m 2 / g≤S≤1.2m 2 / g, and 1 / P 50 -0.1≤S≤1 / P 50 +0.2;

[0050] Preferably, 0.3m 2 / g≤S≤1m 2 / g, and 1 / P 50 -0.05≤S≤1 / P 50 +0.05.

[0051] According to the present invention, the multi-element positive electrode material is a spherical and / or ellipsoidal particle.

[0052] According to the present invention, the matrix of the multi-element positive electrode material has a composition shown in Formula I, and the coating comprises a lithium oxygen compound containing the J element and / or an oxide containing the J element;

[0053] Li a Ni x Mn y Co z M b O2 Formula I;

[0054] Among them, 0.9≤a≤1.1, 0.5≤x<1, 0 <y<0.5,0<z<0.5,0≤b≤0.02;

[0055] The contents of the matrix and the coating are such that 0<[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.03 in the positive electrode material;

[0056] M and J are each independently selected from at least one of Ba, Ra, Zr, Fe, Ca, Zn, B, W, Nb, Cd, Pb, Si, Mo, Cu, V, Ta, Cr, La, Al, Ce, Er, Ho, Y, Mg, Sr and Ti.

[0057] In the present invention, the lithium oxygen compound containing the J element and / or the oxide containing the J element may further include at least one element selected from Ni, Co, Mn, and M derived from the matrix.

[0058] Furthermore, 1≤a≤1.06, 0.6≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0.001≤b≤0.01;

[0059] The contents of the matrix and the coating are such that 0.001≤[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.01 in the positive electrode material;

[0060] M and J are each independently selected from at least one of Ba, Zr, B, W, Nb, La, Al, Y, Mg, Sr and Ti.

[0061] A second aspect of the present invention provides a method for preparing a multi-element positive electrode material, the method comprising:

[0062] (1) mixing a multi-element positive electrode material precursor, a first lithium source, and an optional dopant, and subjecting the mixture to a first high-temperature sintering to obtain a multi-element positive electrode material process product 1;

[0063] (2) After the multi-element positive electrode material product 1 is coarsely crushed, it is washed with an acid solution, washed with water, and dried to obtain a multi-element positive electrode material product 2;

[0064] (3) mixing the multi-component positive electrode material process product 2, optionally a second lithium source, and a coating agent, performing a second high-temperature sintering, and screening to obtain the multi-component positive electrode material;

[0065] The conditions for the acid solution flushing include: the concentration of the acid solution is 0.01-0.05 g / mL, and the flushing time is 1-120 s;

[0066] The sintering temperature T2 of the second high temperature sintering is 200-1000°C;

[0067] The coating agent is added in an amount according to a stoichiometric ratio of 0<[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.03.

[0068] In the prior art, during the preparation of multi-element positive electrode materials, due to the high primary sintering temperature, hard blocks are easily formed after sintering, and the particles are severely adhered to each other, requiring a stronger dissociation method for dissociation, which easily forms fine powder.

[0069] In the present invention, in the method for preparing the multi-element positive electrode material, the dissociation of the multi-element positive electrode material process product 1 obtained by the first high-temperature sintering is achieved by washing with an acid solution, which can achieve a good dissociation effect and does not produce fine powder, thereby avoiding the generation of a large amount of fine powder caused by the traditional strong dissociation method, and further avoiding the poor slurry dispersion, uneven coating and consumption of electrolyte caused by the presence of excessive fine powder, which leads to a decrease in the cycle performance and storage performance of the lithium-ion battery.

[0070] Furthermore, the acid solution rinse will corrode the surface of the multi-element positive electrode material process product 1, thereby increasing the roughness of the surface of the obtained multi-element positive electrode material process product 2. At the same time, there are no attached particles on the surface of the multi-element positive electrode material process product 2, so that after it is mixed with the coating agent and subjected to a second high-temperature sintering, the coating can be more tightly combined with the surface of the obtained multi-element positive electrode material, and during the cycle of the lithium-ion battery, the coating is not easy to fall off from the surface of the positive electrode material, thereby better achieving the coating effect. In particular, controlling the acid solution rinse conditions to meet the above range can separate the particles of the obtained multi-element positive electrode material from each other and not produce fine powder. Specifically, when the acid solution concentration is too low or the rinse time is too short, the separation effect cannot be achieved; when the acid solution concentration is too high or the rinse time is too long, the structure of the surface of the multi-element positive electrode material will be destroyed, ultimately resulting in reduced performance of the lithium-ion battery containing the multi-element positive electrode material.

[0071] Furthermore, in the present invention, by washing the multi-element positive electrode material process product 1 with an acid solution, the multi-element positive electrode material has a low micropowder content, which can ensure that the lithium-ion battery containing the multi-element positive electrode material provided by the present invention has excellent cycle performance and high capacity while reducing the amount of coating agent added.

[0072] In the present invention, the multi-element cathode material product 2 is a spherical and / or ellipsoidal particle with good independence.

[0073] Furthermore, the acid solution rinse removes residual lithium carbonate and lithium hydroxide from the surface of the multi-element cathode material product 1, resulting in a reduction in residual lithium on the surface of the resulting multi-element cathode material. This also makes the surface layer susceptible to lithium deficiency. Therefore, the addition of a second lithium source during the second high-temperature sintering process ensures that the lithium-ion battery containing the resulting multi-element cathode material has a high capacity. Furthermore, the second lithium source acts as a solubility aid. Adding the second lithium source during the second high-temperature sintering process can lower the second high-temperature sintering temperature and reduce energy consumption.

[0074] According to the present invention, the multi-element cathode material precursor is a nickel-cobalt-manganese ternary cathode material precursor.

[0075] In the present invention, the multi-element cathode material precursor can be purchased commercially or prepared in-house.

[0076] According to the present invention, the first lithium source and the second lithium source are each independently selected from one of lithium carbonate, lithium hydroxide, lithium oxide and lithium acetate.

[0077] According to the present invention, the dopant and the coating agent are each independently selected from one of carbonates, hydroxides, oxides and acetates that can provide at least one element among Ba, Ra, Zr, Fe, Ca, Zn, B, W, Nb, Cd, Pb, Si, Mo, Cu, V, Ta, Cr, La, Al, Ce, Er, Ho, Y, Mg, Sr and Ti.

[0078] According to the present invention, the acid solution is selected from at least one of sulfuric acid, carbonic acid, acetic acid and oxalic acid.

[0079] According to the present invention, the total amount of the first lithium source and the second lithium source added is added according to the stoichiometric ratio of 0.9≤[n(Li1)+n(Li2)] / [n(Ni)+n(Co)+n(Mn)]≤1.1.

[0080] Furthermore, the total amount of the first lithium source and the second lithium source is added according to a stoichiometric ratio of 1≤[n(Li1)+n(Li2)] / [n(Ni)+n(Co)+n(Mn)]≤1.06.

[0081] In the present invention, there is no particular limitation on the amount of each of the first lithium source and the second lithium source added, as long as the total amount of the first lithium source and the second lithium source added meets the above range.

[0082] In a specific embodiment of the present invention, the amount of the first lithium source added is according to a chemical ratio of 0.9≤[n(Li1)] / [n(Ni)+n(Co)+n(Mn)]≤1.05, and the amount of the second lithium source added is according to a chemical ratio of 0≤[n(Li2)] / [n(Ni)+n(Co)+n(Mn)]≤0.05.

[0083] In a preferred embodiment of the present invention, the amount of the first lithium source added is according to a chemical ratio of 0.99≤[n(Li1)] / [n(Ni)+n(Co)+n(Mn)]≤1.05, and the amount of the second lithium source added is according to a chemical ratio of 0.01≤[n(Li2)] / [n(Ni)+n(Co)+n(Mn)]≤0.01.

[0084] According to the present invention, the dopant is added in an amount according to a stoichiometric ratio of 0≤[n(M)] / [n(Ni)+n(Co)+n(Mn)]≤0.02, preferably 0≤[n(M)] / [n(Ni)+n(Co)+n(Mn)]≤0.01.

[0085] According to the present invention, the coating agent is added in an amount according to a stoichiometric ratio of 0<[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.03.

[0086] In the present invention, when the amount of coating agent added is controlled to meet the above-mentioned range, it can be ensured that the prepared multi-element positive electrode material has an appropriate content of coating, and further ensure that the prepared multi-element positive electrode material has a stable structure and does not have too much coating remaining on the surface. Specifically, when the amount of coating agent added is too high, too much coating remains on the surface of the material, affecting the transmission of lithium ions, resulting in poor capacity and rate performance of the lithium-ion battery containing the multi-element positive electrode material; and when the amount of coating agent added is too low, the coating effect cannot be exerted. During the cycle, the electrolyte easily destroys the surface structure of the multi-element positive electrode material, resulting in a decrease in the performance of the lithium-ion battery containing the multi-element positive electrode material.

[0087] According to the present invention, the coating agent is added in an amount according to a stoichiometric ratio of 0.001≤[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.01.

[0088] According to the present invention, the conditions for the first high-temperature sintering include: a sintering temperature T1 of 700-1200° C., a sintering time of 10-30 hours, and a sintering atmosphere of oxygen and / or air.

[0089] Furthermore, the conditions for the first high-temperature sintering include: a sintering temperature T1 of 700-1050° C., a sintering time of 15-25 hours, and a sintering atmosphere of oxygen and / or air.

[0090] According to the present invention, the conditions for the acid solution flushing include: the concentration of the acid solution is 0.02-0.04 g / mL, and the flushing time is 5-60 s.

[0091] In the present invention, the coarse crushing can be carried out by conventional methods well known to those skilled in the art, the purpose of which is to decompose large blocks into small blocks, with weaker dissociation strength and less generation of fine powder, such as roller dissociation with a wider gap.

[0092] In the present invention, the purpose of washing the product after washing with the acid solution with water is to remove the residual acid solution.

[0093] According to the present invention, the sintering temperature of the second high-temperature sintering is 300-900°C.

[0094] According to the present invention, the sintering time of the second high-temperature sintering is 5-20 hours, preferably 6-15 hours.

[0095] According to the present invention, the second high-temperature sintering is performed in air and / or oxygen.

[0096] According to the present invention, the sintering temperature T2 of the second high temperature sintering is 200-1000°C, and the sintering temperature T2 is equal to the melting point T m The following relationship is satisfied:

[0097] 100×lnT m -200≤T2≤100×lnT m +100.

[0098] In the present invention, the inventors have found that adjusting the sintering temperature of the second high-temperature sintering according to the type of the coating agent can better achieve the coating effect of the coating agent on the positive electrode material. Specifically, when the melting point of the coating agent and the sintering temperature of the second high-temperature sintering are controlled to satisfy the above-mentioned relationship, a better coating effect can be obtained.

[0099] Furthermore, the sintering temperature T2 of the second high temperature sintering is 300-900°C, and the sintering temperature T2 is equal to the melting point T m Satisfies the following relationship: 100×lnT m -100≤T2≤100×lnT m +50.

[0100] A third aspect of the present invention provides a multi-element positive electrode material prepared by the above preparation method.

[0101] A fourth aspect of the present invention provides a lithium-ion battery, comprising the above-mentioned multi-element positive electrode material.

[0102] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all raw materials are commercially available.

[0103] Unless otherwise specified, the room temperature in the present invention refers to 25±2°C.

[0104] In the following examples and comparative examples, the relevant parameters were obtained by testing using the following methods:

[0105] (1) Particle size test: laser particle size analyzer.

[0106] (2) Morphology and surface roughness test: Scanning electron microscope ERA-9200 model from ELIONIX, Japan.

[0107] (3) Specific surface area test: Micromeritics Tristar 3020 specific surface area meter.

[0108] (4) Electrochemical performance test:

[0109] In the following examples and comparative examples, the electrochemical performance of the multi-element positive electrode materials was tested using 2025 button cells.

[0110] The preparation process of 2025 button battery is as follows:

[0111] Pole sheet preparation: The multi-element positive electrode material, acetylene black and polyvinylidene fluoride (PVDF) were mixed with an appropriate amount of N-methylpyrrolidone (NMP) in a mass ratio of 95:3:2 to form a uniform slurry. The slurry was coated on aluminum foil and dried at 120°C for 12 hours. It was then stamped with a pressure of 100 MPa to form a positive electrode sheet with a diameter of 12 mm and a thickness of 120 μm. The loading amount of the multi-element positive electrode material was 15 mg / cm 2 .

[0112] Battery Assembly: In an argon-filled glove box with water and oxygen contents less than 5 ppm, the positive electrode, separator, negative electrode, and electrolyte were assembled into 2025-type button cells and allowed to rest for 6 hours. The negative electrode used a 17 mm diameter, 1 mm thick lithium metal sheet; the separator used a 25 μm thick polyethylene porous membrane (Celgard 2325); and the electrolyte was a mixture of equal parts ethylene carbonate (EC) and diethyl carbonate (DEC) containing 1 mol / L LiPF6.

[0113] Electrochemical performance test:

[0114] In the following examples and comparative examples, the electrochemical performance of 2025 button batteries was tested using a Shenzhen Xinweier battery testing system, and the charge and discharge current density at 0.1C was 200 mA / g.

[0115] The charge and discharge voltage range was controlled at 3.0-4.3V. At room temperature, the button battery was charged and discharged at 0.1C to evaluate the initial charge and discharge specific capacity and initial charge and discharge efficiency of the multi-electrode positive electrode material.

[0116] Cycling performance test: Control the charge and discharge voltage range to 3.0-4.3V. At a constant temperature of 45°C, the button battery is charged and discharged twice at 0.1C, and then charged and discharged 80 times at 1C to evaluate the high-temperature capacity retention rate of the multi-electrode positive electrode material.

[0117] Rate performance test: Control the charge and discharge voltage range to 3.0-4.3V. At room temperature, the button cell was cycled twice at 0.1C, and then once at 0.2C, 0.33C, 0.5C, and 1C. The rate performance of the multi-element cathode material was evaluated by the ratio of the 0.1C initial discharge capacity to the 1C discharge capacity. The 0.1C initial discharge capacity refers to the discharge capacity of the button cell after the first cycle, and the 1C discharge capacity refers to the discharge capacity of the button cell after the sixth cycle.

[0118] Example 1

[0119] This embodiment is intended to illustrate the positive electrode material prepared by the method of the present invention.

[0120] (1) Ni-Co-Mn hydroxide precursor Ni 0.8 Co 0.1 Mn 0.1 (OH)2, lithium hydroxide, and aluminum oxide are uniformly mixed in a ratio of n(Li):n(Al):[n(Ni)+n(Co)+n(Mn)]=1.04:0.001:1, sintered at 890°C for 20 hours in an oxygen atmosphere, and naturally cooled to room temperature to obtain a multi-element positive electrode material process product 1.

[0121] (2) After the multi-element cathode material product 1 was coarsely crushed, it was rinsed with 0.03 g / mL sulfuric acid for 30 seconds, and then rinsed with deionized water to remove the residual sulfuric acid. After drying, the multi-element cathode material product 2 was obtained: Li 1.04 Ni 0.8 Co 0.1 Mn 0.1 Al 0.001 O2.

[0122] (3) The multi-element positive electrode material process product 2, lithium hydroxide, magnesium oxide, and tungsten oxide are uniformly mixed in a ratio of n(Li):n(Mg):n(W):[n(Ni)+n(Co)+n(Mn)]=0.01:0.005:0.002:1, sintered at 700°C for 12h in an oxygen atmosphere, naturally cooled to room temperature, and sieved to obtain the multi-element positive electrode material.

[0123] Examples 2-7

[0124] The method of Example 1 was followed, except that the formula and process parameters used were different, as shown in Table 1. The rest were the same as in Example 1, to prepare a multi-element positive electrode material.

[0125] Table 1

[0126] Table 1 (continued)

[0127] Comparative Example 1

[0128] (1) Ni-Co-Mn hydroxide precursor Ni 0.8 Co 0.1 Mn 0.1 (OH)2, lithium hydroxide, and aluminum oxide are uniformly mixed in a ratio of n(Li):n(Al):[n(Ni)+n(Co)+n(Mn)]=1.04:0.001:1, sintered at 890°C for 20 hours in an oxygen atmosphere, and naturally cooled to room temperature to obtain a multi-element positive electrode material process product 1.

[0129] (2) After the multi-element cathode material product 1 is coarsely crushed, it is dissociated with a pair of rollers with a narrow gap to a target particle size of 6.2 μm to obtain the multi-element cathode material product 2: Li 1.04 Ni 0.8 Co 0.1 Mn 0.1 Al 0.001 O2.

[0130] (3) The multi-element positive electrode material process product 2, lithium hydroxide, magnesium oxide, and tungsten oxide are uniformly mixed in a ratio of n(Li):n(Mg):n(W):[n(Ni)+n(Co)+n(Mn)]=0.01:0.005:0.002:1, sintered at 700°C for 12h in an oxygen atmosphere, naturally cooled to room temperature, and sieved to obtain the multi-element positive electrode material.

[0131] Comparative Example 2

[0132] The method of Example 1 is followed, except that in step (3), the multi-element positive electrode material process product 2 and lithium hydroxide are uniformly mixed in a ratio of n(Li):[n(Ni)+n(Co)+n(Mn)]=0.01:1; the rest is the same as in Example 1, to obtain a multi-element positive electrode material: Li 1.05 Ni 0.8 Co 0.1 Mn 0.1 Al 0.001 O2. Characteristic parameter test data are shown in Table 2.

[0133] Comparative Example 3

[0134] The method of Example 1 was followed, except that in step (3), the ternary material product 2, lithium hydroxide, magnesium oxide, and tungsten oxide were uniformly mixed in a ratio of n(Li):n(Mg):n(W):[n(Ni)+n(Co)+n(Mn)]=0.01:0.03:0.03:1, and sintered at 400°C for 12 hours in an oxygen atmosphere. The remaining steps were the same as in Example 1, yielding a multi-element positive electrode material. The characteristic parameter test data are shown in Table 2.

[0135] Comparative Example 4

[0136] The method of Example 1 was followed, except that in step (3), sintering was performed at 1100° C. in an oxygen atmosphere; the remaining steps were the same as in Example 1, to obtain a multi-element positive electrode material. The characteristic parameter test data are shown in Table 2.

[0137] Comparative Example 5

[0138] The method of Example 1 was followed, except that in step (2), 0.1 g / mL sulfuric acid was used for rinsing for 180 seconds. The remaining steps were the same as in Example 1, to obtain a multi-element positive electrode material. The characteristic parameter test data are shown in Table 2.

[0139] Test Case

[0140] (1) Morphology test

[0141] The present invention tests the scanning electron microscope images of the positive electrode materials prepared in the above embodiments and comparative examples and calculates the average primary particle size P of the multi-element positive electrode material. 50 , arithmetic mean roughness Ra, and coverage Q, as shown in Figures 1-4 and Table 2. Figure 1 shows that the surface of the multi-component positive electrode material product 2 obtained in Example 1 is free of attachment and exhibits good particle independence. Figure 2 shows that the surface of the multi-component positive electrode material exhibits dot- and island-shaped coatings. The surface of the multi-component positive electrode material product 2 obtained in Comparative Example 1 exhibits a high level of fine powder and debris, with worn edges and corners. In addition to the coating, the surface of the multi-component positive electrode material also exhibits a high level of fine powder.

[0142] (2) Physical property testing

[0143] The present invention tested the D1, D2 and D3 of the multi-element positive electrode materials prepared in the above examples and comparative examples. 50 、P 50 , S, Ra, Q, the specific test results are shown in Table 2.

[0144] Table 2

[0145] Table 2 (continued)

[0146] As can be seen from Table 2, compared with Example 1, Example 2 has a low sulfuric acid concentration and a short rinsing time, and the obtained S is smaller, indicating that the dissociation is insufficient and the particles are adhered; Example 3 has a high sulfuric acid concentration and a long rinsing time, and the obtained S is larger, and D 50 and P 50 is smaller, indicating that the surface of the positive electrode material is partially corroded by sulfuric acid.

[0147] Compared with Example 1, Example 4 has a larger coating amount, more residual coating agent on the surface, and larger S, Ra, and Q; Example 5 has a high second high-temperature sintering temperature, more coating agent is incorporated into the outer layer of the positive electrode material, less residue on the surface, and smaller S, Ra, and Q.

[0148] Examples 6 and 7 illustrate that different compositions and coating agents are also applicable.

[0149] Compared with Example 1, Comparative Example 1 uses a pair of rollers to dissociate to the target particle size, and the dissociation produces more fine powder, smaller D1, larger S, rougher surface and larger Ra, which is consistent with the conclusions of Figures 3 and 4.

[0150] In Comparative Example 2, no coating was performed, and the particles were slightly adhered after the second high-temperature sintering, so S was relatively small. In Comparative Example 3, the coating amount was too large, and the second high-temperature sintering temperature was low, so more coating agent remained on the surface, S was very large, and the surface roughness Ra and surface coverage Q were both large. In Comparative Example 4, the second high-temperature sintering temperature was high, the coating agent was incorporated into the outer layer of the positive electrode material, and the particles were adhered, resulting in a very small S.

[0151] Comparative Example 5: The acid solution concentration is high, and the washing time is long, resulting in severe surface corrosion. 50 and P 50 A is smaller, S is larger.

[0152] Table 3

[0153] It can be seen from Table 3 that compared with Example 1, Example 2 has a smaller S, particles adhere, a slightly lower material capacity, and slightly poorer rate and cycle performance; Example 3 has a larger S, the surface is partially corroded, and the material cycle performance is poor.

[0154] Compared with Example 1, Example 4 has a larger coating amount, resulting in more residual coating agent on the surface, which hinders lithium ion conduction, reduces material capacity, has poor rate capability, and slightly poor cycling performance. Example 5 has a high second high-temperature sintering temperature, resulting in less residual coating agent on the surface and poor cycling performance. Example 8 does not contain a second lithium source, resulting in lithium deficiency on the surface and lower capacity.

[0155] Compared with Example 1, Comparative Example 1 has more micropowder, consumes more electrolyte, and the electrolyte is insufficient, which is manifested as a decrease in material capacity. In addition, the micropowder will cause the battery electrode to be unstable, resulting in poor cycle performance.

[0156] Comparative Example 2 was not coated, and during the battery charging and discharging process, the surface was prone to structural changes, resulting in poor cycle performance; Comparative Example 3 had more surface residues, which hindered lithium ion transmission and resulted in poor material rate performance; Comparative Example 4 had a high second high-temperature sintering temperature, resulting in less coating agent residue and particle adhesion, resulting in poor material cycle stability.

[0157] In Comparative Example 5, the acid solution had a high solubility, a long flushing time, severe material corrosion, and poor cycle stability.

[0158] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.

Claims

1. A multi-element positive electrode material, characterized in that: The surface of the multi-element positive electrode material includes dot-shaped coatings and / or island-shaped coatings; The cumulative distribution of particles of the multi-element positive electrode material is 1% of the particle size D1 ≥ 0.7 μm; The arithmetic average roughness Ra of the coating of the multi-element positive electrode material measured by a three-dimensional scanning electron microscope satisfies: 20nm≤Ra≤200nm; The coverage rate Q of the point-shaped coatings and / or island-shaped coatings of the multi-element positive electrode material satisfies: 3%≤Q≤30%.

2. The multi-element positive electrode material according to claim 1, wherein: The cumulative distribution of particles of the multi-element positive electrode material is such that 1% of the particle size satisfies 1 μm≤D1≤2 μm; The arithmetic average roughness Ra of the coating of the multi-element positive electrode material measured by a three-dimensional scanning electron microscope satisfies 30nm≤Ra≤100nm; The coverage rate Q of the point-shaped coatings and / or island-shaped coatings of the multi-element positive electrode material satisfies: 5%≤Q≤15%.

3. The multi-element positive electrode material according to claim 1 or 2, wherein: The cumulative distribution of the particles of the multi-element positive electrode material is 50% of the particle size D 50 2-8 μm, preferably 2.5-7 μm; Preferably, the average primary particle size P of the multi-element positive electrode material measured by SEM is 50 0.8-6 μm, preferably 1-4 μm; Preferably, the specific surface area S of the multi-element positive electrode material satisfies: 0.2≤S≤1.2m 2 / g, and / or, 1 / P 50 -0.1≤S≤1 / P 50 +0.2; Preferably, the multi-element positive electrode material is spherical and / or ellipsoidal particles.

4. The multi-element positive electrode material according to any one of claims 1 to 3, wherein: The matrix of the positive electrode material has a composition shown in Formula I, and the coating includes a lithium oxygen compound containing the J element and / or an oxide containing the J element; Li a Ni x Mn y Co z M b O2 Formula I; Among them, 0.9≤a≤1.1, 0.5≤x<1, 0 <y<0.5,0<z<0.5,0≤b≤0.02; The contents of the matrix and the coating are such that 0<[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.03 in the positive electrode material; M and J are each independently selected from at least one of Ba, Ra, Zr, Fe, Ca, Zn, B, W, Nb, Cd, Pb, Si, Mo, Cu, V, Ta, Cr, La, Al, Ce, Er, Ho, Y, Mg, Sr and Ti.

5. A method for preparing a multi-element positive electrode material, characterized in that: The method comprises: (1) mixing a multi-element positive electrode material precursor, a first lithium source and an optional dopant, and subjecting the mixture to a first high-temperature sintering to obtain a multi-element positive electrode material process product 1; (2) After the multi-element positive electrode material process product 1 is coarsely crushed, it is washed with an acid solution, washed with water, and dried in sequence to obtain a multi-element positive electrode material process product 2; (3) Mixing the multi-component positive electrode material process product 2, optionally a second lithium source and a coating agent, sintering at a second high temperature, and sieving to obtain the multi-component positive electrode material; The conditions for washing with the acid solution include: the concentration of the acid solution is 0.01-0.05 g / mL, and the washing time is 1-120 s; The sintering temperature T2 of the second high temperature sintering is 200-1000°C; The coating agent is added in an amount according to a stoichiometric ratio of 0<[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.

03.

6. The method according to claim 5, wherein: The multi-element positive electrode material precursor is a nickel-cobalt-manganese ternary positive electrode material precursor; Preferably, the first lithium source and the second lithium source are each independently selected from one of lithium carbonate, lithium hydroxide, lithium oxide and lithium acetate; Preferably, the dopant and the coating agent are each independently selected from one of carbonates, hydroxides, oxides and acetates capable of providing at least one element of Ba, Ra, Zr, Fe, Ca, Zn, B, W, Nb, Cd, Pb, Si, Mo, Cu, V, Ta, Cr, La, Al, Ce, Er, Ho, Y, Mg, Sr and Ti; Preferably, the acid solution is selected from at least one of sulfuric acid, carbonic acid, acetic acid and oxalic acid.

7. The method according to claim 6, wherein: The total amount of the first lithium source and the second lithium source added is added according to the stoichiometric ratio of 0.9≤[n(Li1)+n(Li2)] / [n(Ni)+n(Co)+n(Mn)]≤1.1, preferably 1≤[n(Li1)+n(Li2)] / [n(Ni)+n(Co)+n(Mn)]≤1.06; Preferably, the dopant is added in an amount according to a stoichiometric ratio of 0.0001≤[n(M)] / [n(Ni)+n(Co)+n(Mn)]≤0.02, preferably 0.001≤[n(M)] / [n(Ni)+n(Co)+n(Mn)]≤0.01; Preferably, the coating agent is added in an amount according to a stoichiometric ratio of 0.001≤[n(J)] / [n(Ni)+n(Co)+n(Mn)]≤0.

01.

8. The method according to any one of claims 5 to 7, wherein: The conditions of the first high temperature sintering include: sintering temperature T1 is 700-1200° C., sintering time is 10-30 hours, and sintering atmosphere is oxygen and / or air; Preferably, the conditions for washing with the acid solution include: the concentration of the acid solution is 0.02-0.04 g / mL, and the washing time is 5-60 s; Preferably, the sintering temperature T2 of the second high temperature sintering is 300-900°C; Preferably, the sintering time of the second high temperature sintering is 5-20h, preferably 6-15h; Preferably, the second high temperature sintering is performed in air and / or oxygen.

9. The method according to any one of claims 5 to 8, wherein: The sintering temperature T2 of the second high temperature sintering is 200-1000°C, and the sintering temperature T2 is equal to the melting point T m Satisfies the following relationship: 100×lnT m -200≤T2≤100×lnT m +100; Preferably, the sintering temperature T2 of the second high temperature sintering is 300-900°C, and the sintering temperature T2 is 100°C to the melting point T2 of the coating agent. m Satisfies the following relationship: 100×lnT m -100≤T2≤100×lnT m +50.

10. A multi-element positive electrode material prepared by the method according to any one of claims 5 to 9.

11. A lithium ion battery, characterized in that: The lithium-ion battery comprises the multi-element positive electrode material according to any one of claims 1 to 4 and 10.

Citation Information

Patent Citations

  • Multi-element composite positive pole material for lithium secondary battery and preparation thereof

    CN101478044A

  • Ternary positive pole material with surface layer coated with lithium tungstate and doped with W and preparation method

    CN109742336A

  • Positive electrode material and preparation method thereof

    CN112968150A

  • Bimetallic element co-doped positive electrode material and preparation method thereof

    CN113839013A

  • Positive electrode material and preparation method and application thereof

    CN115347168A