Precursor material and preparation method therefor, positive electrode material, positive electrode sheet, secondary battery, and electronic device
By using a precursor material with the chemical formula NixCoyMnzMa(OH)2, controlling the number of (101) crystal plane layers and crystal plane orientation, and combining with the co-precipitation reaction method, the DC internal resistance and structural stability of existing cathode materials at high temperatures have been solved. sexual issues, achieving battery performance with high capacity and good cycle performance.
Patent Information
- Application Number
- PCT/CN2023/089600
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-24
AI Technical Summary
It is difficult for existing precursor materials to produce cathode materials with high capacity and good cycle performance at the same time. Especially under high temperature conditions, they show increased DC internal resistance and structural instability, which cannot meet the needs of a new generation of electrochemical systems.
A precursor material with the chemical formula NixCoyMnzMa(OH)2 is used, in which the M element includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, and La. By controlling the number of (101) crystal plane layers in the range of 20-70, combined with the two-stage co-precipitation reaction method, the crystal growth rate and crystal plane orientation are controlled, the growth of (001) crystal planes is suppressed, and the lithium ion transmission efficiency is improved. and structural stability.
It significantly improves the capacity and dynamic performance of the battery, reduces the DC internal resistance, improves the high-temperature cycle performance, and ensures the structural stability and high-temperature capacity retention rate of the cathode material.
Smart Images

Figure CN2023089600_24102024_PF_FP_ABST
Abstract
Description
Precursor Material, Its Preparation Method, Cathode Material, Cathode Plate, Secondary Battery and Electrical Device Technical Field
[0001] This application relates to the technical field of secondary batteries, and particularly to a precursor material, its preparation method, a cathode material, a cathode plate, a secondary battery and an electrical device. Background Art
[0002] In recent years, secondary batteries have been widely used in energy storage power systems such as hydroelectric, thermal, wind and solar power stations, as well as in multiple fields such as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc.
[0003] The performance of the cathode material has a crucial impact on the performance of the secondary battery, and the performance of the cathode material is largely affected by the performance of the precursor material. The cathode materials synthesized from the existing precursor materials either have a relatively high capacity but poor cycling performance, or have a relatively high cycling performance but a low capacity, making it difficult for the cathode material to have good comprehensive electrochemical performance and unable to meet the application requirements of the new generation of electrochemical systems.
[0004] Summary of the Invention
[0005] This application is made in view of the above problems. This application provides a precursor material, aiming to increase the capacity of the battery and reduce the DC internal resistance of the battery, and can also improve the high-temperature cycling performance of the battery.
[0006] The first aspect of this application provides a precursor material, and the chemical formula of the precursor material is Ni ,
[0007] ,
[0008] , Co y Mn z M a (OH)2,
[0007] where M element includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, La, 0.55 ≤ x < 1.0, 0 ≤ y < 0.45, 0 ≤ z < 0.45, 0 < a ≤ 0.45, a + x + y + z = 1, and the number of crystal plane layers of the (101) crystal plane of the precursor material is 20 - 70.
[0008] The number of (101) crystal plane sheets of the precursor material is within a suitable range, so that the positive electrode material prepared therefrom has multiple lithium ion active crystal planes, which can expose a large number of lithium ion active sites, improve the gram capacity of the positive electrode material, and improve the capacity of the battery. In addition, the (101) crystal plane, as the dominant crystal plane for lithium ion transmission, can structurally shorten the transmission distance of lithium ions, reduce the DC internal resistance of the battery, and improve the kinetic performance of the battery. In addition, the number of (101) crystal plane sheets of the precursor material is within a suitable range, so that the positive electrode material prepared therefrom has excellent structural stability, and improves the high-temperature cycle performance of the battery.
[0009] In any embodiment, the chemical formula Ni x Co y Mn z M a (OH)2, 0.90≤x<1.0, 0≤y<0.10, 0≤z<0.10, 0 <a≤0.10,a+x+y+z=1。
[0010] In any embodiment, the number of (101) crystal plane layers of the precursor material is 25-55.
[0011] Controlling the number of crystal facet layers of the precursor material to 25-55 can further increase the capacity of the battery and reduce the DC internal resistance of the battery.
[0012] In any embodiment, the deformation stacking fault rate fD of the precursor material is less than or equal to 7.0%, and can be optionally less than or equal to 4.0%.
[0013] The precursor material has a small deformation stacking fault rate fD, which can greatly stabilize the coordinated atoms at the center of the tetrahedron, inhibit the formation of vacancies, is beneficial to the stability of the actual stoichiometric ratio and transition metal valence, promotes the orderliness and structural stability of the positive electrode material prepared from the precursor material, and is beneficial to improving the high-temperature cycle performance of the secondary battery.
[0014] In any embodiment, the grain size ratio of the (100) crystal plane to the (001) crystal plane of the precursor material is greater than or equal to 2.0, and can be optionally greater than or equal to 4.4.
[0015] Controlling the grain size ratio of the (100) crystal plane to the (001) crystal plane within a suitable range is beneficial to controlling the deformation stacking fault rate fD of the precursor material within a suitable range, improving the structural stability of the positive electrode material prepared therefrom, and is beneficial to improving the high-temperature cycle performance of the secondary battery.
[0016] In any embodiment, the pore volume of the precursor material is greater than or equal to 0.02 cm 3 / g, can be selected to be greater than or equal to 0.025cm 3 / g.
[0017] Adjust the pore volume of the precursor material to be greater than or equal to 0.02 cm 3 / g, which is beneficial for the precursor material to maintain appropriate looseness and rich porosity, thereby facilitating the diffusion of lithium ions and improving the capacity of the battery during the preparation of the positive electrode material.
[0018] In any embodiment, the Dv50 of the precursor material is 3 μm to 15 μm.
[0019] Controlling the Dv50 of the precursor material within a suitable range can shorten the transmission distance of lithium ions and reduce the DC internal resistance of the battery. At the same time, the precursor material has a suitable Dv50, so that the positive electrode material prepared therefrom has more lithium ion reaction active sites, thereby increasing the gram capacity of the positive electrode material and the capacity of the battery.
[0020] In any embodiment, the specific surface area of the precursor material is 4m 2 / g-20m 2 / g, optional 8m 2 / g-13m 2 / g.
[0021] The specific surface area of the precursor material is within a suitable range, and the positive electrode material prepared therefrom has a large number of active reaction sites for lithium ions, thereby improving the capacity of the battery.
[0022] In any embodiment, the diffraction peak intensity ratio of the (001) crystal plane to the (101) crystal plane of the precursor material is 0.60-1.25, and can be optionally 0.9-1.18.
[0023] By controlling the diffraction peak intensity ratio of the (001) crystal plane to the (101) crystal plane of the precursor material within an appropriate range, the precursor material has a good crystal plane orientation, the positive electrode material prepared therefrom has a high ionic order, and the battery has a high capacity and excellent cycle performance.
[0024] A second aspect of the present application provides a method for preparing a precursor material, the method comprising the following steps:
[0025] The precursor material is prepared by coprecipitation reaction, and the chemical formula of the precursor material is Ni x Co y Mn z M a (OH)2,
[0026] Among them, the M element includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, and La, 0.55 ≤ x < 1.0, 0 ≤ y < 0.45, 0 ≤ z < 0.45, 0 < a ≤ 0.45, a + x + y + z = 1, and the number of (101) crystal plane layers of the precursor material is 20 - 70.
[0027] By using the preparation method of the present application, a precursor material with the number of (101) crystal plane layers being 20 - 70 can be obtained, which can increase the capacity of the battery, reduce the DC internal resistance of the battery, and improve the high-temperature cycle performance of the battery.
[0028] In any implementation manner, the preparation method specifically includes step (1) and step (2):
[0029] Step (1): A mixed salt solution containing nickel salt, cobalt salt, and manganese salt, a precipitant solution, a complexing agent solution, and a surfactant are joined in a confluent manner and added to the reaction bottom liquid to conduct a first co-precipitation reaction. After reaching the first target particle size D V 50, the reaction is stopped to obtain a precursor mother liquid;
[0030] Step (2): A precipitant solution, a complexing agent solution, and an M salt solution are added in a parallel flow manner to the precursor mother liquid, and the second co-precipitation reaction is continued. After reaching the second target particle size D V 50, the reaction is ended to obtain the precursor material.
[0031] Using a two-stage co-precipitation reaction to prepare the precursor material is beneficial to regulating the crystal growth rate, can effectively control the crystal plane orientation of crystal growth, making the number of (101) crystal plane layers within a suitable range. In addition, a surfactant is added in step (1) to inhibit the growth of the (001) crystal plane, enabling the (101) crystal plane to grow orderly, exposing more advantageous surfaces for lithium ion transmission, reducing the DC internal resistance of the battery, and improving the rate performance and cycle performance of the battery; at the same time, the M element is added in step (2), which is beneficial to generating flaky primary particles, facilitating the growth of the (101) crystal plane, obtaining a precursor material with controllable number of (101) crystal plane layers, and thus obtaining a positive electrode material with controllable number of (101) crystal plane layers.
[0032] In any implementation manner, the mass percentage content of the surfactant added in step (1) is 0.1% - 5%, based on the total mass of the nickel salt, cobalt salt, and manganese salt in the mixed salt solution.
[0033] In any implementation manner, the hydrophilic-lipophilic balance value of the surfactant added in step (1) is greater than 10, and it can be selected from one or more of polyvinylpyrrolidone, triethanolamine oleate, polyoxyethylene oleyl ether, or polyoxyethylene lauryl ether.
[0034] Adding a surfactant with a hydrophilic-lipophilic balance greater than 10 in step (1) helps inhibit the growth of (001) crystal planes and promote the orderly growth of (101) crystal planes. Furthermore, controlling the mass percentage of the added surfactant can, to a certain extent, adjust the number of (101) crystal plane layers and the aspect ratio of the primary particles of the positive electrode material, thereby increasing the capacity of the secondary battery.
[0035] In any embodiment, the first target particle size D in step (1) V 50 is 3 μm-9.5 μm, and the second target particle size D in the step (2) V 50 is 3μm-15μm.
[0036] Controlling the first target particle size Dv50 value in step (1) within a suitable range is conducive to adjusting the second target particle size Dv50 within a suitable range, and then controlling the Dv50 of the precursor material within a suitable range, which is conducive to further improving the capacity of the battery and reducing the DC internal resistance.
[0037] In any embodiment, the reaction temperature of the first coprecipitation reaction in step (1) is 65-85°C, and the reaction temperature of the second coprecipitation reaction in step (2) is 65-85°C.
[0038] By controlling the appropriate reaction temperature of the first coprecipitation and the second coprecipitation, the first coprecipitation reaction and the second coprecipitation reaction are smoother and more efficient, and the structural properties of the subsequent precursor material and positive electrode material are better, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0039] In any embodiment, the pH value of the first coprecipitation reaction in step (1) is 8.5-11.5, and the pH value of the second coprecipitation reaction in step (2) is 8.5-11.5.
[0040] By controlling the appropriate pH values of the first coprecipitation and the second coprecipitation, the first coprecipitation reaction and the second coprecipitation reaction are smoother and more efficient, and the structural properties of the subsequent precursor material and positive electrode material are better, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0041] In any embodiment, the molar concentration of the complexing agent in the first coprecipitation reaction system in step (1) is 0.5-1 mol / L, and the molar concentration of the complexing agent in the second coprecipitation reaction system in step (2) is 0.5-1 mol / L.
[0042] By controlling the appropriate molar concentrations of the complexing agents of the first coprecipitation and the second coprecipitation, the first coprecipitation reaction and the second coprecipitation reaction are smoother and more efficient, and the structural properties of the subsequent precursor material and positive electrode material are better, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0043] In any embodiment, the molar concentration of the mixed salt solution added in step (1) is 1-5 mol / L; the molar concentration of the precipitant solution added in step (1) is 1-10 mol / L; the concentration of the precipitant solution added in step (2) is 1-10 mol / L; the molar concentration of the M salt solution added in step (2) is 0.5-1 mol / L.
[0044] By controlling the molar concentrations of the precipitants of the first coprecipitation and the second coprecipitation, and the molar concentrations of the mixed salt solution and the M salt solution within appropriate ranges, the first coprecipitation reaction and the second coprecipitation reaction are smoother and more efficient, and the structural properties of the precursor material and the positive electrode material obtained subsequently are better, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0045] The third aspect of the present application provides a use of a precursor material as described in the present application or a precursor material prepared by the preparation method as described in the present application for preparing a positive electrode material.
[0046] A fourth aspect of the present application provides a positive electrode material, which is prepared from the precursor material described in the present application or the precursor material prepared by the preparation method described in the present application.
[0047] The positive electrode material prepared using the precursor material of the first aspect or the precursor material obtained by the preparation method of the second aspect has a high gram capacity, can also reduce the DC internal resistance of the battery, and improve the high-temperature cycle performance of the battery.
[0048] In any embodiment, the positive electrode material satisfies formula (I) or formula (II), Li c1 Ni x1 Co y1 Mn z1 M1 a1 O 2-d1 , formula (Ⅰ); Li c2 Ni x2 Co y2 Mn z2 M1 a2 M2 e O 2-d2 , formula (II);
[0049] Wherein, M1 and M2 each independently include at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, and La, 0.5≤c1<1.2, 0.55≤x1<1.0, 0≤y1<0.45, 0≤z1<0.45, 0 <a1≤0.45,a1+x1+y1+z1=1,-0.1≤d1<0.1;0.5≤c2<1.2,0.55≤x2<1.0,0≤y2<0.45,0≤z2<0.45,0<a2≤0.45,0<a2≤0.45,0<e≤0.45,a2+x2+y2+z2+e=1,-0.1≤d2<0.1。
[0050] In any embodiment, the micro stress of the positive electrode material is less than or equal to 0.5%, and can be optionally less than or equal to 0.2%.
[0051] The micro-stress of the positive electrode material is within a smaller range, and the positive electrode material is not easily deformed during the charge and discharge process of the battery, which helps to improve the high-temperature cycle performance of the battery.
[0052] In any embodiment, the aspect ratio of the primary particles of the positive electrode material is 1.5-10, and can be optionally 2-5.
[0053] By controlling the aspect ratio of the primary particles of the positive electrode material within an appropriate range, the battery has high capacity, small DC internal resistance and excellent cycle capacity retention, which comprehensively improves the battery performance.
[0054] A fifth aspect of the present application provides a positive electrode plate, which includes the positive electrode material described in the present application.
[0055] A sixth aspect of the present application provides a secondary battery comprising the positive electrode sheet described in the present application.
[0056] A seventh aspect of the present application provides an electrical device comprising the secondary battery described in the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0058] FIG2 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG1 ;
[0059] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application;
[0060] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0061] FIG5 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG4 ;
[0062] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0063] Description of reference numerals:
[0064] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION
[0065] Below, the embodiments of the positive electrode material, preparation method thereof, secondary battery, battery module, battery pack and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0066] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0067] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0068] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0069] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0070] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0071] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0072] Ternary materials, known for their high theoretical specific capacity, have attracted significant attention in industries such as new energy vehicles and power tools. However, in actual production, researchers have discovered that existing ternary materials exhibit poor electrical conductivity, resulting in an increase in DC internal resistance during cycling, which deteriorates rate performance. Furthermore, during charge and discharge, ternary materials are susceptible to electrolyte corrosion, leading to structural collapse and impacting battery cycle performance. Therefore, there is a need to develop a positive electrode material that can reduce the DC internal resistance and improve the battery's cycle performance while meeting the demands of high-capacity batteries, in order to meet the application needs of next-generation electrochemical systems.
[0073] [Precursor materials]
[0074] Based on this, this application proposes a precursor material, the chemical formula of which is Ni x Co y Mn z M a (OH)2,
[0075] Among them, the M element contains at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, La, 0.55 ≤ x < 1.0, 0 ≤ y < 0.45, 0 ≤ z < 0.45, 0 < a ≤ 0.45, a + x + y + z = 1, and the number of (101) crystal plane layers of the precursor material is 20 - 70.
[0076] In some embodiments, M can be Zr, Ta or Sb.
[0077] In some embodiments, x can be 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.96, 1.0, or a value within the range formed by any two of the above.
[0078] In some embodiments, y can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.08, 0.1, 0.2, 0.3, 0.4, 0.45, or a value within the range formed by any two of the above.
[0079] In some embodiments, z can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.08, 0.1, 0.2, 0.3, 0.4, 0.45, or a value within the range formed by any two of the above.
[0080] In some embodiments, a can be 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.02, 0.03, 0.04, 0.05, 0.1, 0.2, 0.3, 0.4, 0.45, or a value within the range formed by any two of the above.
[0081] In some embodiments, the chemical formula Ni x Co y Mn z M a (OH)2, 0.90 ≤ x < 1.0, 0 ≤ y < 0.10, 0 ≤ z < 0.10, 0 < a ≤ 0.10, a + x + y + z = 1.
[0082] The number of (101) crystal plane layers of the precursor material can be calculated by methods and equipment known in the art. For example, by fitting through X-ray diffraction pattern (XRD) test. As an example, the following steps can be followed: set the XRD test conditions: use a Cu target, set the tube voltage (for example, 40V), set the tube current (for example, 40mA), set the scanning speed (for example, <2° / min), set the 2θ scanning range (for example, 15°-70°), set the step size (for example, 0.02°), set the emission slit (DS) (for example, 1mm), set the anti-scattering slit (SS) (for example, 8mm), and use a graphite monochromator. After fitting the XRD spectrum of the precursor material, the grain size D of the (101) crystal plane is calculated. 101 :D 101 =kλ / (B 101 *cosθ 101 ); among them, B 101 is the half-peak width of the diffraction peak of the (101) crystal plane of the precursor material, k is the coefficient (usually 0.89-0.90), θ 101 is the diffraction angle of the (101) crystal plane diffraction peak of the precursor material, and λ is the wavelength of the copper target; the corresponding value can be obtained by subsequent calculation. After fitting the XRD spectrum of the precursor material, the interplanar spacing d of the (101) crystal plane is calculated. 101 :d 101 =nλ / (2*sinθ 101 ), where θ 101 is the diffraction angle of the (101) crystal plane diffraction peak of the precursor material, and λ is the wavelength of the copper target; the corresponding value can be obtained by subsequent calculation. After summarizing the above parameters, the number of (101) crystal plane layers N is obtained. 101 =D 101 / d 101 .
[0083] The chemical formula of the precursor material can be determined by measuring methods and equipment known in the art. For example, it can be measured by an ion emission spectrometer (ICP-OES). As an example, the following steps can be followed: first, a certain mass (e.g., 1 g) of the precursor material is weighed in a beaker, and a certain volume (e.g., 25 mL) of an acid (e.g., HNO3) solution of a certain concentration (e.g., a concentration of 25% by volume) is added to the precursor material to dissolve the precursor material, and the precursor material is diluted with a certain volume (e.g., 475 mL) of deionized water, and then the diluted liquid is placed in an ion emission spectrometer (e.g., ICAP7400 from Thermo Fisher Scientific, USA) for target element analysis, and the chemical formula of the precursor material is obtained by calculation.
[0084] The number of (101) crystal plane sheets of the precursor material is within a suitable range, so that the positive electrode material prepared therefrom has multiple lithium ion active crystal planes, which can expose a large number of lithium ion active sites, increase the gram capacity of the positive electrode material, and improve the capacity of the battery; and the (101) crystal plane, as the dominant crystal plane for lithium ion transmission, can structurally shorten the transmission distance of lithium ions, reduce the DC internal resistance of the battery, and improve the kinetic performance of the battery. At the same time, the number of (101) crystal plane sheets of the precursor material is within a suitable range, which to a certain extent reduces the possibility of increased lithium ion diffusion obstacles caused by excessive thickness of the particles of the positive electrode material prepared therefrom; in addition, the number of (101) crystal plane sheets of the precursor material is within a suitable range, so that the positive electrode material prepared therefrom has excellent structural stability, and improves the high-temperature cycle performance of the battery.
[0085] In some embodiments, the number of (101) crystal plane layers of the precursor material is 25-55.
[0086] In some embodiments, the number of (101) crystal plane layers of the precursor material can be 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, or a value in the range formed by any two of the above points.
[0087] Controlling the number of (101) crystal plane layers of the precursor material within the range of 25-55 can further increase the capacity of the battery and reduce the DC internal resistance of the battery.
[0088] In some embodiments, the precursor material has a deformation stacking fault fD less than or equal to 7.0%.
[0089] In some embodiments, the deformation stacking fault rate fD of the precursor material can be 7.0%, 6.5%, 6%, 5.5%, 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, or a value in the range formed by any two of the above points.
[0090] The deformation stacking fault rate fD of the precursor material can be calculated by methods and equipment known in the art. For example, by fitting through X-ray diffraction pattern (XRD) test. As an example, the following steps can be followed: set the XRD test conditions: use a Cu target, set the tube voltage (for example, 40V), set the tube current (for example, 40mA), set the scanning speed (for example, <2° / min), set the 2θ scanning range (for example, 15°-70°), set the step size (for example, 0.02°), set the emission slit (DS) (for example, 1mm), set the anti-scattering slit (SS) (for example, 8mm), and use a graphite monochromator. After fitting the XRD spectrum of the precursor, the deformation stacking fault rate f is calculated. D :
[0091] Among them, B101 is the half-height width of the diffraction peak of the (101) crystal plane of the precursor material, B 102 is the half-height width of the diffraction peak of the (102) crystal plane of the precursor material, D 001 It is the grain size of the (001) crystal plane diffraction peak of the precursor material, and the corresponding value can be obtained by subsequent calculation.
[0092] The precursor material of the present application has a small deformation stacking fault rate fD, which can greatly stabilize the coordinated atoms at the center of the tetrahedron, inhibit the formation of vacancies, is beneficial to the stability of the actual stoichiometric ratio and transition metal valence, improves the orderliness and structural stability of the positive electrode material prepared from the precursor material, and is beneficial to improving the high-temperature cycle performance of the secondary battery.
[0093] In some embodiments, the precursor material has a deformation stacking fault fD less than or equal to 4.0%.
[0094] In some embodiments, the deformation stacking fault fD of the precursor material may be 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, or a value within a range formed by any two of the above points.
[0095] By controlling the deformation stacking fault rate fD of the precursor material to be less than or equal to 4.0%, the cycle capacity retention rate of the battery at high temperature can be further improved, thereby improving the high-temperature cycle performance of the battery.
[0096] In some embodiments, the precursor material has a grain size ratio of (100) crystal plane to (001) crystal plane greater than or equal to 2.0.
[0097] In some embodiments, the grain size ratio of the (100) crystal plane to the (001) crystal plane of the precursor material can be 2.0, 2.5, 3, 3.5, 4, 4.4, 5, 5.5, 6, 6.5, 7, 7.5, or a value in the range formed by any two of the above points.
[0098] The grain size ratio of the (100) crystal plane to the (001) crystal plane of the precursor material is calculated by methods and equipment known in the art. For example, the grain size ratio is calculated by X-ray diffraction (XRD) test fitting. As an example, the following steps can be followed: set the XRD test conditions: use a Cu target, set the tube voltage (for example, 40V), set the tube current (for example, 40mA), set the scanning speed (for example, <2° / min), set the 2θ scanning range (for example, 15°-70°), set the step size (for example, 0.02°), set the emission slit (DS) (for example, 1mm), set the anti-scattering slit (SS) (for example, 8mm), and use a graphite monochromator. After fitting the XRD spectrum of the precursor material, the grain size D of the (100) crystal plane is calculated. 100 :D 100 =kλ / (B100 *cosθ 100 ); among them, B 101 is the half-peak width of the diffraction peak of the (100) crystal plane of the precursor material, k is the coefficient (usually 0.89-0.90), θ 101 is the diffraction angle of the (100) crystal plane diffraction peak of the precursor material, and λ is the wavelength of the copper target; the corresponding value can be obtained by subsequent calculation. The grain size D of the (001) crystal plane is calculated by fitting the XRD spectrum of the precursor material. 001 :D 001 =kλ / (B 001 *cosθ 001 ); among them, B 001 is the half-peak width of the (001) diffraction peak of the precursor material, k is the coefficient (usually 0.89-0.90), θ 101 is the diffraction angle of the (001) crystal plane diffraction peak of the precursor material, and λ is the wavelength of the copper target; the corresponding value can be obtained by subsequent calculation. After summarizing the above parameters, the grain size ratio D of the (100) and (001) crystal planes is obtained. 100 / D 001 .
[0099] Controlling the grain size ratio of the (100) crystal plane to the (001) crystal plane within an appropriate range is beneficial to controlling the deformation stacking fault rate fD of the precursor material within an appropriate range, improving the structural stability of the positive electrode material prepared therefrom, and thus helping to improve the high-temperature cycle performance of the battery.
[0100] In some embodiments, the ratio of the grain size of the (100) crystal plane to the (001) crystal plane of the precursor material is greater than or equal to 4.4.
[0101] In some embodiments, the grain size ratio of the (100) crystal plane to the (001) crystal plane of the precursor material can be 4.4, 5, 5.5, 6, 6.5, 7, 7.5, 8 or a value in the range of any two of the above points.
[0102] Controlling the grain size ratio of the (100) crystal plane to the (001) crystal plane of the precursor material within an appropriate range can further improve the cycle capacity retention rate of the battery at high temperature and improve the high-temperature cycle performance of the battery.
[0103] In some embodiments, the pore volume of the precursor material is greater than or equal to 0.02 cm 3 / g.
[0104] As used herein, the term "pore volume" refers to the volume of pores per unit mass of a precursor material.
[0105] In some embodiments, the pore volume of the precursor material may be 0.02 cm3 / g, 0.024cm 3 / g, 0.025cm 3 / g, 0.026cm 3 / g, 0.028cm 3 / g, 0.030cm 3 / g, 0.032cm 3 / g, 0.034cm 3 / g, 0.036cm 3 / g, 0.038cm 3 / g, 0.040cm 3 / g, or a value in the range formed by any two of the above points.
[0106] The pore volume of the precursor material can be measured using methods and equipment known in the art. For example, the pore volume can be measured according to the method in GB / T 21650.2-2008, "Determination of Pore Size Distribution and Porosity of Solid Materials by Mercury Intrusion and Gas Adsorption - Part 2: Analysis of Mesopores and Macropores by Gas Adsorption." As an example, the following steps can be followed: a certain mass of sample is weighed, placed in a true density tester, the test system is sealed, and helium or nitrogen is introduced according to the program. The true volume is calculated by measuring the pressure of the gas in the sample chamber and the expansion chamber according to Bohr's law (PV = nRT).
[0107] Adjust the pore volume of the precursor material to be greater than or equal to 0.02 cm 3 / g, which is beneficial for the precursor material to maintain appropriate looseness and rich porosity, so that in the process of preparing the positive electrode material, it is beneficial for lithium ion diffusion and improves the capacity of the battery.
[0108] In some embodiments, the pore volume of the precursor material is greater than or equal to 0.025 cm 3 / g.
[0109] In some embodiments, the pore volume of the precursor material may be 0.025 cm 3 / g, 0.026cm 3 / g, 0.028cm 3 / g, 0.030cm 3 / g, 0.032cm 3 / g, 0.034cm 3 / g, 0.036cm 3 / g, 0.038cm 3 / g, 0.040cm 3 / g, or a value in the range formed by any two of the above points.
[0110] Control the pore volume of the precursor material to be greater than or equal to 0.025cm3 / g, which can further improve the capacity of the battery.
[0111] In some embodiments, the Dv50 of the precursor material is 3 μm to 15 μm.
[0112] As used herein, the term "Dv50" refers to the median particle size of a precursor material. Specifically, Dv50 represents a particle size at which the volume accumulation reaches 50% from the smallest particle size side in a volume-based particle size distribution of the precursor material.
[0113] In some embodiments, the Dv50 of the precursor material may be 3 μm, 5 μm, 7 μm, 9 μm, 10 μm, 12 μm, 14 μm, 15 μm, or a value within a range formed by any two of the above points.
[0114] The Dv50 of the precursor material can be measured by methods and equipment known in the art. For example, it can be measured with reference to the method specified in GB / T19077-2016. As an example, the following steps can be followed: weigh a certain mass (for example, 0.1g-0.13g) of the precursor material sample to be tested in a beaker, add a certain mass (for example, 5g) of anhydrous ethanol, put it in a stirrer and seal it with plastic wrap. After the sample is ultrasonically treated for a certain time (for example, 5min), it is transferred to a magnetic stirrer and stirred at a certain speed (for example, 500 rpm) for a certain time (for example, more than 20min). A laser particle size analyzer (for example, Malvern 3000 laser particle size analyzer from Malvern Instruments Ltd., UK) is used for testing. Among them, Dv50 is the particle size corresponding to the cumulative volume distribution percentage of the secondary particles of the precursor material reaching 50%.
[0115] Particles of different sizes have different areas and different numbers of reactive sites. Therefore, the size of the particle size will affect the speed of ion deintercalation and embedding, and affect the gram capacity of the material. Controlling the Dv50 of the precursor material within a suitable range so that the Dv50 of the positive electrode material prepared therefrom is within a suitable range can shorten the transmission distance of lithium ions, reduce the DC internal resistance of the battery, increase the gram capacity of the material, and increase the capacity of the battery.
[0116] In some embodiments, the specific surface area of the precursor material is 4 m 2 / g-20m 2 / g,.
[0117] As used herein, the term "specific surface area" refers to the total area per unit mass of a precursor material.
[0118] In some embodiments, the specific surface area of the precursor material can be 4m 2 / g、6m 2 / g、8m2 / g、10m 2 / g、12m 2 / g、14m 2 / g、16m 2 / g、18m 2 / g, 20m 2 / g, or a value within the range consisting of any two of the above points.
[0119] The specific surface area of the precursor material can be measured by methods and equipment known in the art. For example, the gas adsorption method can be used to test according to the GB / T19587-2017 test standard. As an example, the following steps can be followed: take the precursor material as a sample, immerse the sample tube in -196°C liquid nitrogen, and measure the adsorption amount of nitrogen on the solid surface at different pressures at a certain relative pressure (for example, 0.05-0.30 relative pressure). The sample monolayer adsorption amount is obtained based on the BET multilayer adsorption theory and its formula, thereby calculating the specific surface area of the precursor material.
[0120] The specific surface area of the precursor material is within a suitable range, and the positive electrode material prepared therefrom has a large number of active reaction sites for lithium ions, thereby improving the capacity of the battery.
[0121] In some embodiments, the specific surface area of the precursor material is 8 m 2 / g-13m 2 / g.
[0122] In some embodiments, the specific surface area of the precursor material can be 8m 2 / g、10m 2 / g、12m 2 / g、14m 2 / g、16m 2 / g、18m 2 / g, 20m 2 / g, or a value within the range consisting of any two of the above points.
[0123] The specific surface area of the precursor material is within an appropriate range, so that the positive electrode material prepared therefrom has more lithium ion active sites, thereby improving the capacity of the battery. At the same time, it can also reduce the possibility of excessive active sites and increase the side reaction between the positive electrode material and the electrolyte, thereby worsening the cyclability of the battery. It can take into account both the capacity and the cycle capacity retention rate of the battery at the same time, and comprehensively improve the performance of the battery.
[0124] In some embodiments, the ratio of the diffraction peak intensity of the (001) crystal plane to the (101) crystal plane of the precursor material is 0.60-1.25.
[0125] In some embodiments, the diffraction peak intensity ratio of the (001) crystal plane to the (101) crystal plane of the precursor material can be 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, 1.00, 1.05, 1.10, 1.15, 1.20, 1.25, or a value in the range of any two of the above points.
[0126] The diffraction peak intensity ratio of the (001) crystal plane and the (101) crystal plane of the precursor material can be measured by methods and equipment known in the art. For example, XRD can be used for measurement and calculation. As an example, the XRD spectrum of the tested sample is scanned at a slow speed (<2° / min), and the image is processed according to smoothing and filtering to obtain the diffraction peak integral area I of the (001) crystal plane and the (101) crystal plane. 001 , I 101 , through (I 001 / I 101 ) is used to calculate the diffraction peak intensity ratio of the (001) crystal plane and the (101) crystal plane of the precursor material.
[0127] By controlling the diffraction peak intensity ratio of the (001) crystal plane to the (101) crystal plane of the precursor material within an appropriate range, the precursor material has a good crystal plane orientation, the positive electrode material prepared therefrom has a high ionic order, and the battery has a high capacity and excellent cycle performance.
[0128] In some embodiments, the ratio of the diffraction peak intensity between the (001) crystal plane and the (101) crystal plane of the precursor material is 0.9-1.18.
[0129] In some embodiments, the diffraction peak intensity ratio of the (001) crystal plane to the (101) crystal plane of the precursor material can be 0.90, 0.95, 1.00, 1.05, 1.10, 1.15, 1.18, or a value in the range of any two of the above points.
[0130] By controlling the diffraction peak intensity ratio of the (001) crystal plane and the (101) crystal plane of the precursor material within an appropriate range, the precursor material has a good crystal plane orientation, and at the same time can reduce the phenomenon of lithium nickel mixing in the subsequent preparation process of the positive electrode material, which can take into account the high capacity and cycle capacity retention rate of the battery, and comprehensively improve the performance of the battery.
[0131] [Preparation method of precursor]
[0132] The present application provides a method for preparing a precursor material, the preparation method comprising the following steps:
[0133] The precursor material is prepared by coprecipitation reaction. The chemical formula of the precursor material is Ni xCo y Mn z M a (OH)2
[0134] Among them, the M element includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, La, 0.55 ≤ x < 1.0, 0 ≤ y < 0.45, 0 ≤ z < 0.45, 0 < a ≤ 0.45, a + x + y + z = 1, and the number of crystal plane layers of the (101) crystal plane of the precursor material is 20 - 70.
[0135] In this article, the term "coprecipitation reaction" refers to the precipitation reaction jointly carried out by a metal solution, a precipitant, and a complexing agent at a certain temperature.
[0136] In some embodiments, x can be 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.96, 1.0, or a value within the range formed by any two of the above.
[0137] In some embodiments, y can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.08, 0.1, 0.2, 0.3, 0.4, 0.45, or a value within the range formed by any two of the above.
[0138] In some embodiments, z can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.08, 0.1, 0.2, 0.3, 0.4, 0.45, or a value within the range formed by any two of the above.
[0139] In some embodiments, a can be 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.02, 0.03, 0.04, 0.05, 0.1, 0.2, 0.3, 0.4, 0.45, or a value within the range formed by any two of the above.
[0140] In some embodiments, the chemical formula Ni x Co y Mn z M a (OH)2, 0.90 ≤ x < 1.0, 0 ≤ y < 0.10, 0 ≤ z < 0.10, 0 < a ≤ 0.10, a + x + y + z = 1.
[0141] By adopting the preparation method of the present application, a precursor material with 20-70 (101) crystal plane layers can be obtained, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0142] In some embodiments, the preparation method specifically includes steps (1) and (2):
[0143] Step (1): Add the mixed salt solution containing nickel salt, cobalt salt, manganese salt, precipitant solution, complexing agent solution and surfactant into the reaction base liquid to perform the first coprecipitation reaction to achieve the first target particle size D V After 50, the reaction was stopped to obtain the precursor mother solution;
[0144] Step (2): Add the precipitant solution, the complexing agent solution and the M salt solution to the precursor mother solution in parallel, and continue the second coprecipitation reaction to achieve the second target particle size D V After 50, the reaction was terminated to obtain the precursor material.
[0145] In some embodiments, the nickel salt includes one or more of nickel sulfate, nickel hydrochloride, nickel nitrate, and nickel acetate.
[0146] In some embodiments, the cobalt salt includes one or more of cobalt sulfate, cobalt oxalate, cobalt nitrate, and cobalt acetate.
[0147] In some embodiments, the manganese salt includes one or more of manganese sulfate, manganese hydrochloride, manganese nitrate, and manganese acetate.
[0148] In some embodiments, the M salt comprises a zirconium salt, a tantalum salt, or an antimony salt, and may be an antimony salt.
[0149] In some embodiments, the zirconium salt includes one or more of zirconium sulfate, zirconium hydrochloride, zirconium nitrate, zirconium oxalate, zirconium acetate, and sodium zirconate.
[0150] In some embodiments, the tantalum salt includes one or more of tantalum sulfate, tantalum hydrochloride, tantalum nitrate, tantalum acetate, tantalum oxalate, and sodium tantalate.
[0151] In some embodiments, the antimony salt includes one or more of antimony sulfate, antimony hydrochloride, antimony nitrate, antimony acetate, antimony oxalate, and sodium antimonate.
[0152] In some embodiments, the precipitant includes one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, and ammonium bicarbonate, and sodium hydroxide can be selected.
[0153] In some embodiments, the complexing agent includes one or more of ammonia water, lactic acid, and polyvinyl pyrrolidone, and ammonia water can be selected.
[0154] The use of a two-stage coprecipitation reaction to prepare a precursor material is conducive to regulating the growth rate of the crystal and can effectively control the crystal plane orientation of the crystal growth, so that the number of (101) crystal plane layers is within an appropriate range. In addition, a surfactant is added in step (1) to inhibit the growth of the (001) crystal plane, so that the (101) crystal plane grows in an orderly manner, exposing more advantageous surfaces for lithium ion transmission, reducing the DC internal resistance of the battery, and improving the battery's rate performance and cycle performance; at the same time, the addition of the M element in step (2) is conducive to the generation of thin-sheet primary particles, which is conducive to the growth of the (101) crystal plane, and obtaining a precursor material with a controllable number of (101) crystal plane layers, thereby obtaining a positive electrode material with a controllable number of (101) crystal plane layers. In addition, the added M element can generate Li with excellent lithium ion conductivity in the subsequent process of preparing the positive electrode material. p M q O m , which is beneficial to increasing the lithium ion transmission speed of the positive electrode material and improving the battery's rate performance.
[0155] In some embodiments, the mass percentage of the surfactant added in step (1) is 0.1%-5%, based on the total mass of the nickel salt, cobalt salt and manganese salt in the mixed salt solution.
[0156] In some embodiments, based on the total mass of nickel salt, cobalt salt and manganese salt in the mixed salt solution, the mass percentage of the surfactant added in step (1) can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a value in the range formed by any two of the above points.
[0157] In some embodiments, the surfactant added in step (1) has a hydrophilic-lipophilic balance value greater than 10, and can be selected from one or more of polyvinyl pyrrolidone, triethanolamine oleate, polyoxyethylene oleyl ether, or polyoxyethylene lauryl ether.
[0158] In some embodiments, the surfactant comprises one or more of vinyl pyrrolidone, polyoxyethylene oxypropylene oleate, polyoxypropylene lanolin alcohol ether, triethanolamine oleate, polyoxyethylene oleyl alcohol ether, polyoxyethylene cholesterol ether, polyoxyethylene castor oil, or polyoxyethylene lauryl ether. In some embodiments, the surfactant comprises vinyl pyrrolidone.
[0159] As used herein, the term "hydrophile-lipophile balance" refers to a quantity that characterizes the size and degree of balance between the hydrophilic and lipophilic groups in a surfactant molecule. Specifically, hydrophile-lipophile balance = hydrophilicity of the hydrophilic group / lipophilicity of the lipophilic group. A larger hydrophile-lipophile balance value represents a stronger hydrophilicity, and a smaller hydrophile-lipophile balance value represents a stronger lipophilicity.
[0160] Adding a surfactant having a hydrophilic-lipophilic balance value greater than 10 in step (1) is beneficial for inhibiting the growth of the (001) crystal plane and promoting the orderly growth of the (101) crystal plane. At the same time, controlling the mass percentage of the added surfactant can, to a certain extent, adjust the number of (101) crystal plane layers of the precursor material and the aspect ratio of the primary particles of the positive electrode material within an appropriate range, so that the precursor material and the positive electrode material have excellent structural properties.
[0161] In some embodiments, the first target particle size D in step (1) is V 50 is 3 μm-9.5 μm, the second target particle size D in step (2) V 50 is 3μm-15μm.
[0162] In some embodiments, the first target particle size Dv50 in step (1) can be 3 μm, 5 μm, 7 μm, 9 μm, 9.5 μm, or a value within a range formed by any two of the above points. The second target particle size Dv50 in step (2) can be 3 μm, 5 μm, 7 μm, 9 μm, 10 μm, 12 μm, 14 μm, 15 μm, or a value within a range formed by any two of the above points.
[0163] Controlling the first target particle size Dv50 value in step (1) within a suitable range is conducive to adjusting the second target particle size Dv50 within a suitable range, and further controlling the Dv50 of the precursor material within a suitable range is conducive to further improving the capacity of the battery and reducing the DC internal resistance.
[0164] In some embodiments, the reaction temperature of the first coprecipitation reaction in step (1) is 65-85°C, and the reaction temperature of the second coprecipitation reaction in step (2) is 65-85°C.
[0165] In some embodiments, the reaction temperature of the first coprecipitation reaction in step (1) can be 65°C, 70°C, 75°C, 80°C, 85°C, or a value within a range formed by any two of the above points. The reaction temperature of the second coprecipitation reaction in step (2) can be 65°C, 70°C, 75°C, 80°C, 85°C, or a value within a range formed by any two of the above points.
[0166] By controlling the appropriate reaction temperature of the first coprecipitation and the second coprecipitation, the first coprecipitation reaction and the second coprecipitation reaction are smoother and more efficient, and the structural properties of the subsequent precursor material and positive electrode material are better, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0167] In some embodiments, the pH value of the first coprecipitation reaction in step (1) is 8.5-11.5, and the pH value of the second coprecipitation reaction in step (2) is 8.5-11.5.
[0168] In some embodiments, the pH value of the first coprecipitation reaction in step (1) can be 8.5, 9, 9.5, 10, 10.5, 11, 11.5, or a value within a range formed by any two of the above points. The pH value of the second coprecipitation reaction in step (2) can be 8.5, 9, 9.5, 10, 10.5, 11, 11.5, or a value within a range formed by any two of the above points.
[0169] By controlling the appropriate pH values of the first coprecipitation and the second coprecipitation, the first coprecipitation reaction and the second coprecipitation reaction are smoother and more efficient, and the structural properties of the subsequent precursor material and positive electrode material are better, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0170] In some embodiments, the molar concentration of the complexing agent in the first coprecipitation reaction system in step (1) is 0.5-1 mol / L, and the molar concentration of the complexing agent in the second coprecipitation reaction system in step (2) is 0.5-1 mol / L.
[0171] In some embodiments, the molar concentration of the complexing agent in the first coprecipitation reaction system in step (1) is 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, or 1.0 mol / L, or a value within the range formed by any two of the above. The molar concentration of the complexing agent in the second coprecipitation reaction system in step (2) is 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, or 1.0 mol / L, or a value within the range formed by any two of the above.
[0172] By controlling the appropriate molar concentrations of the complexing agents of the first coprecipitation and the second coprecipitation, the first coprecipitation reaction and the second coprecipitation reaction are smoother and more efficient, and the structural properties of the subsequent precursor material and positive electrode material are better, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0173] In some embodiments, the molar concentration of the mixed salt solution added in step (1) is 1-5 mol / L; the molar concentration of the precipitant solution added in step (1) is 1-10 mol / L; the concentration of the precipitant solution added in step (2) is 1-10 mol / L; the molar concentration of the M salt solution added in step (2) is 0.5-1 mol / L.
[0174] In some embodiments, the molar concentration of the mixed salt solution added in step (1) can be 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, or a value within the range formed by any two of the above points.
[0175] In some embodiments, the molar concentration of the precipitant solution added in step (1) can be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, or a value within the range of any two of the above points.
[0176] In some embodiments, the concentration of the precipitant solution added in step (2) can be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, or a value within the range of any two of the above points.
[0177] In some embodiments, the molar concentration of the M salt solution added in step (2) can be 0.5 mol / L, 0.55 mol / L, 0.6 mol / L, 0.65 mol / L, 0.7 mol / L, 0.75 mol / L, 0.8 mol / L, 0.85 mol / L, 0.9 mol / L, 1.0 mol / L, or a value in the range formed by any two of the above points.
[0178] By controlling the molar concentration of the precipitant in the first coprecipitation and the second coprecipitation, and the molar concentration of the mixed salt solution and the M salt solution within an appropriate range, the first coprecipitation reaction and the second coprecipitation reaction are smoother and more efficient, and the structural properties of the precursor material and the positive electrode material obtained subsequently are better, thereby increasing the capacity of the battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0179] In some embodiments, step (1) specifically includes:
[0180] Prepare a mixed salt solution containing nickel salt, cobalt salt and manganese salt with a molar concentration of 1-5 mol / L, a precipitant solution with a molar concentration of 1-10 mol / L, a complexing agent solution with a molar concentration of 1-5 mol / L and an M salt solution with a molar concentration of 0.5-1 mol / L;
[0181] Add pure water, complexing agent solution and precipitant solution into the reaction kettle as the reaction bottom liquid, control the pH value of the reaction bottom liquid to be 8.5-11.5, and the molar concentration of the complexing agent to be 0.5-1 mol / L;
[0182] A mixed salt solution, a precipitant solution, a complexing agent solution, and a surfactant with a mass percentage of 0.1%-5% based on the total mass of the manganese salt, cobalt salt, and nickel salt in the mixed salt solution are combined and added to the reaction base liquid. The pH value and the molar concentration of the complexing agent are controlled to remain unchanged. The reaction temperature is controlled to be 65-85°C and the rotation speed is controlled to be 200-800 rpm, optionally 300-400 rpm. A first coprecipitation reaction is carried out. After reaching a first target particle size Dv50 of 3 μm-9.5 μm, the reaction is stopped to obtain a precursor mother solution.
[0183] In some embodiments, step (2) specifically includes:
[0184] Add the precipitant solution, complexing agent solution and M salt solution to the precursor mother liquor in parallel, control the reaction temperature to 65-85℃, pH value to 8.5-11.5, and the molar concentration of the complexing agent to 0.5-1 mol / L, and continue the second coprecipitation reaction to achieve the second target particle size D V After 50 is 3μm-15μm, the reaction is terminated to obtain the precursor material.
[0185] The present application provides a use of a precursor material of the present application or a precursor material prepared by the preparation method of the present application for preparing a positive electrode material.
[0186] [Cathode material]
[0187] The present application provides a positive electrode material, which is prepared from the precursor material of the present application or the precursor material prepared by the preparation method of the present application.
[0188] The positive electrode material has a high gram capacity, increases the capacity of the battery, reduces the direct current internal resistance of the battery, and improves the high-temperature cycle performance of the battery.
[0189] In some embodiments, the positive electrode material satisfies formula (I) or formula (II), Li c1 Ni x1 Co y1 Mn z1 M1 a1 O 2-d1 , formula (Ⅰ); Li c2 Ni x2 Co y2 Mn z2 M1 a2 M2 e O 2-d2 , formula (II);
[0190] Wherein, M1 and M2 each independently include at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, and La, 0.5≤c1<1.2, 0.55≤x1<1.0, 0≤y1<0.45, 0≤z1<0.45, 0 <a1≤0.45,a1+x1+y1+z1=1,-0.1≤d1<0.1;0.5≤c2<1.2,0.55≤x2<1.0,0≤y2<0.45,0≤z2<0.45,0<a2≤0.45,0<a2≤0.45,0<e≤0.45,a2+x2+y2+z2+e=1,-0.1≤d2<0.1。
[0191] In some embodiments, M1 and M2 comprise the same elements.
[0192] In some embodiments, M1 and M2 comprise different elements.
[0193] In some embodiments, c1 may be 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, or a value within a range formed by any two of the above values.
[0194] In some embodiments, x1 may be 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.96, 1.0, or a value within a range formed by any two of the foregoing values.
[0195] In some embodiments, y1 can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.08, 0.1, 0.2, 0.3, 0.4, 0.45, or a value in the range formed by any two of the above points.
[0196] In some embodiments, z1 can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.08, 0.1, 0.2, 0.3, 0.4, 0.45, or a value in the range formed by any two of the above points.
[0197] In some embodiments, a1 can be 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.02, 0.03, 0.04, 0.05, 0.1, 0.2, 0.3, 0.4, 0.45, or a value in the range formed by any two of the above points.
[0198] In some embodiments, d1 may be -0.1, -0.05, 0, 0.05, 0.1, or a value within a range formed by any two of the above points.
[0199] The chemical formula of the positive electrode material can be confirmed by measuring by methods and equipment known in the art. For example, it can be measured by an ion emission spectrometer (ICP-OES). As an example, the following steps can be followed: first, a certain mass (e.g., 1 g) of positive electrode material is weighed in a beaker, and a certain volume (e.g., 25 mL) of a certain concentration (e.g., a concentration of 25% by volume) of an acid (e.g., HNO3) solution is added to the positive electrode material to dissolve the positive electrode material, and diluted with a certain volume (e.g., 475 mL) of deionized water. The diluted liquid is then placed in an ion emission spectrometer (e.g., ICAP7400, Thermo Fisher Scientific, USA) for target element analysis, and the chemical formula of the positive electrode material is obtained by calculation.
[0200] In some embodiments, the positive electrode material satisfies formula (II), Li c2 Ni x2 Co y2 Mn z2 M1 a2 M2 e O 2-d2 , formula (II);
[0201] Wherein, M1 and M2 each independently include at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, and La, 0.5≤c2<1.2, 0.55≤x2<1.0, 0≤y2<0.45, 0≤z2<0.45, 0 <a2≤0.45,0<a2≤0.45,0<e≤0.45,a2+x2+y2+z2+e=1,-0.1≤d2<0.1。
[0202] In some embodiments, c2 may be 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, or a value within a range formed by any two of the foregoing values.
[0203] In some embodiments, x2 may be 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.96, 1.0, or a value within a range formed by any two of the foregoing values.
[0204] In some embodiments, y2 can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.08, 0.1, 0.2, 0.3, 0.4, 0.45, or a value in the range formed by any two of the above points.
[0205] In some embodiments, z2 can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.08, 0.1, 0.2, 0.3, 0.4, 0.45, or a value in a range formed by any two of the above points.
[0206] In some embodiments, a2 can be 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.02, 0.03, 0.04, 0.05, 0.1, 0.2, 0.3, 0.4, 0.45, or a value in the range formed by any two of the above points.
[0207] In some embodiments, d2 may be -0.1, -0.05, 0, 0.05, 0.1, or a value within a range formed by any two of the above points.
[0208] In some embodiments, e can be 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.02, 0.03, 0.04, 0.05, 0.1, 0.2, 0.3, 0.4, 0.45, or a value in the range formed by any two of the above points.
[0209] The positive electrode material contains M2 elements, which can promote the radial distribution of the particles of the positive electrode material. The positive electrode material has a good lithium ion transmission channel, which is beneficial to the lithium ion transmission during the charging and discharging process, increases the capacity of the battery, reduces the DC internal resistance of the battery, and improves the high-temperature cycle performance of the battery.
[0210] In some embodiments, the microstress of the positive electrode material is less than or equal to 0.5%.
[0211] In this article, the term “micro stress” refers to the micro strain that exists and balances itself inside the cathode material in the absence of external force or torque.
[0212] In some embodiments, the microstress of the positive electrode material can be 0.5%, 0.45%, 0.4%, 0.35%, 0.3%, 0.25%, 0.2%, 0.18%, 0.16%, 0.14%, 0.12%, 0.1%, or a value in the range formed by any two of the above points.
[0213] The micro stress of the positive electrode material can be calculated by methods and equipment known in the art. For example, by fitting through X-ray diffraction pattern (XRD) test. As an example, the following steps can be followed: set XRD test conditions: use Cu target, set tube voltage (for example, 40V), set tube current (for example, 40mA), set scanning speed (for example, <2° / min), set 2θ scanning range (for example, 15°-70°), set step size (for example, 0.02°), set emission slit (DS) (for example, 1mm), set anti-scattering slit (SS) (for example, 8mm), and use graphite monochromator. After fitting the XRD spectrum, the micro stress is obtained: MS=(B hkl *Cosθ hkl ) / (4sinθ hkl ), where θ hkl is the diffraction angle of the positive electrode material (hkl) crystal plane in the XRD diffraction pattern, B hkl is the half-height width of the crystal plane of the positive electrode material (hkl) in the XRD diffraction pattern.
[0214] The micro-stress of the positive electrode material is within a smaller range, and the positive electrode material is not easily deformed during the charge and discharge process of the battery, which helps to improve the high-temperature cycle performance of the battery.
[0215] In some embodiments, the micro stress of the positive electrode material is less than or equal to 0.2%.
[0216] In some embodiments, the micro stress of the positive electrode material may be 0.2%, 0.18%, 0.16%, 0.14%, 0.12%, 0.1%, or a value within a range formed by any two of the above values.
[0217] Controlling the micro stress of the positive electrode material to be less than or equal to 0.2% can further improve the cycle capacity retention rate of the battery at high temperature and improve the high temperature cycle performance of the battery.
[0218] In some embodiments, the aspect ratio of primary particles of the positive electrode material is 1.5-10.
[0219] In some embodiments, the term "primary particles" refers to particles of the positive electrode material before agglomeration.
[0220] In some embodiments, the aspect ratio of the primary particles of the positive electrode material can be 1.5, 1.8, 2.0, 2.3, 2.5, 2.8, 3.0, 3.5, 4, 4.5, 5, 6, 7, 8, 9, 10, or a value in the range formed by any two of the above points.
[0221] The aspect ratio of the primary particles of the positive electrode material can be measured by methods and equipment known in the art. For example, static image processing technology can be used for measurement. As an example, the following steps can be followed: using a scanning electron microscope photograph of the primary particles of the static positive electrode material, the long diameter RL and wide diameter RS data of the primary particles are obtained through intelligent recognition by software, and then the aspect ratio = RL / RS is calculated. Among them, the wide diameter refers to the shortest distance passing through the center point of the projected image of the primary particle and intersecting with the edge of the projected image. The long diameter refers to the longest distance passing through the center point of the projected image of the primary particle and intersecting with the edge of the projected image.
[0222] When the aspect ratio of the primary particles of the positive electrode material is within an appropriate range, the transmission distance of lithium ions can be shortened, and a large number of active sites of lithium ions can be exposed, thereby increasing the gram capacity of the material. At the same time, when the aspect ratio of the primary particles is within an appropriate range, it can also reduce the contact area between the material and the electrolyte, reduce the possibility of side reactions between the material and the electrolyte, and improve the high-temperature cycle performance of the battery.
[0223] When the aspect ratio of the primary particles of the positive electrode material is within a suitable range, the battery has high capacity and low DC internal resistance, and the battery has excellent high-temperature cycle performance.
[0224] In some embodiments, the primary particles of the positive electrode material have an aspect ratio of 2-5.
[0225] In some embodiments, the aspect ratio of the primary particles of the positive electrode material can be 2.0, 2.3, 2.5, 2.8, 3.0, 3.5, 4, 4.5, 5, or a value in the range formed by any two of the above points.
[0226] When the aspect ratio of the primary particles of the positive electrode material is within an appropriate range, the battery capacity, DC internal resistance and cycle capacity retention can be taken into account, thereby comprehensively improving the battery performance.
[0227] [Method for preparing positive electrode material]
[0228] In some embodiments, the preparation method of the positive electrode material is as follows:
[0229] The lithium source, the precursor material of the present application, and the compound containing the M2 element are calcined to obtain a positive electrode material, wherein the molar ratio of the lithium element to the nickel element, the cobalt element, and the manganese element in the precursor material is controlled to be 0.9-1.1.
[0230] In some embodiments, the calcination temperature is 700-900°C.
[0231] In some embodiments, the calcination temperature may be 700° C., 800° C., 900° C., or a value within a range consisting of any two of the above values.
[0232] In some embodiments, the calcination time is 10-20 hours.
[0233] In some embodiments, the calcination time may be 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, or a value in a range formed by any two of the above points.
[0234] In some embodiments, the M2 element is the same as the M element in the precursor material.
[0235] In some embodiments, the M2 element is different from the M element in the precursor material.
[0236] In some embodiments, the compound containing the M2 element includes one or more of a salt containing the M2 element and an oxide containing the M2 element.
[0237] Adding compounds containing M2 elements during the calcination process of preparing positive electrode materials is beneficial to the radial distribution of positive electrode material particles. The positive electrode material has a good lithium ion transmission channel, which is beneficial to the lithium ion transmission during the charge and discharge process, increases the capacity of the battery, reduces the DC internal resistance of the battery, and improves the high-temperature cycle performance of the battery.
[0238] [Positive electrode]
[0239] The present application provides a positive electrode plate, which includes the positive electrode material of the present application.
[0240] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer formed on at least a portion of the surface of the positive electrode current collector, and the positive electrode material layer includes the positive electrode material in some embodiments.
[0241] The positive electrode material layer may further include a conductive agent to improve the conductivity of the positive electrode. The conductive agent may be selected from one or more of Super P, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphite, graphene, and carbon nanofibers.
[0242] The positive electrode material layer may further include a binder to firmly bond the positive electrode material and optional conductive agent to the positive electrode current collector. The binder may be at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), polyvinyl alcohol (PVA), ethylene-vinyl acetate copolymer (EVA), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), sodium alginate (SA), polymethacrylic acid (PMA), and carboxymethyl chitosan (CMCS).
[0243] The positive electrode current collector can be a conductive carbon sheet, metal foil, carbon-coated metal foil, porous metal plate, or a composite current collector. The conductive carbon material of the conductive carbon sheet can be selected from one or more of Super P, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphite, graphene, and carbon nanofibers. The metal material of the metal foil, carbon-coated metal foil, and porous metal plate can each be independently selected from at least one of copper, aluminum, nickel, and stainless steel. The composite current collector can be a composite of metal foil and a polymer-based film.
[0244] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0245] [Negative electrode]
[0246] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. The negative electrode film layer includes a negative electrode active material.
[0247] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0248] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0249] In some embodiments, the negative electrode active material may be a negative electrode material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode materials for batteries may also be used. These negative electrode materials may be used alone or in combination of two or more.
[0250] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0251] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0252] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0253] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode film layer, such as the negative electrode material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0254] [Electrolytes]
[0255] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0256] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0257] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0258] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0259] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0260] [Isolation film]
[0261] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0262] In some embodiments, the material of the separator can be selected from at least one of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester, and natural fibers. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0263] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0264] [Secondary battery]
[0265] The present application provides a secondary battery, including the positive electrode plate of the present application.
[0266] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0267] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0268] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 is an example of a secondary battery 5 having a square structure, and FIG2 is an exploded view of the secondary battery 5 .
[0269] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The non-Newtonian fluid electrolyte composition is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0270] [Battery Module]
[0271] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0272] Figure 3 shows an example battery module 3. Referring to Figure 3 , within a battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.
[0273] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0274] [Battery Pack]
[0275] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0276] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0277] [Electrical devices]
[0278] The present application provides an electrical device, including the secondary battery of the present application.
[0279] In some embodiments, the electric device includes at least one of the secondary battery of any embodiment, the battery module of any embodiment, or the battery pack of any embodiment.
[0280] Secondary batteries, battery modules, or battery packs can be used as power sources or energy storage units for electrical devices. Electrical devices may include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, and energy storage systems.
[0281] As an electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0282] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.
[0283] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0284] Example
[0285] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0286] 1. Preparation method
[0287] Example 1
[0288] 1) Preparation of precursor materials
[0289] Solution preparation: nickel sulfate, cobalt sulfate, and manganese sulfate were prepared at a molar ratio of Ni:Co:Mn = 96:3:1 to form a mixed salt solution with a concentration of 1.5 mol / L. Antimony sulfate was used to prepare an antimony salt solution with a concentration of 0.75 mol / L. 5 mol / L NaOH solution was used as an alkaline solution precipitant, and 2 mol / L ammonia water was used as a complexing agent.
[0290] Preparation of reaction base solution: Add 10 L of deionized water to a 20 L controlled crystallization reactor, add a certain amount of concentrated ammonia water to make the ammonia concentration in the reactor 0.65 mol / L, and add a certain amount of NaOH solution to make the pH in the reactor 11 to obtain the reaction base solution;
[0291] First coprecipitation reaction: Under a nitrogen atmosphere, the reaction base liquid was heated to 75°C. At a stirring speed of 350 rpm, a mixed salt solution, alkali solution, ammonia solution, and a surfactant polyvinylpyrrolidone (PVP) were added to the reaction base liquid in parallel, wherein the mass fraction of PVP was 0.5%, based on the total mass of nickel sulfate, cobalt sulfate, and manganese sulfate. By adjusting the flow rate of the mixed salt solution, alkali solution, and ammonia solution, the pH of the reaction solution was 11 and the ammonia concentration was 0.65 mol / L. After the reaction reached the first target particle size Dv50 (9.5 μm), the pumping was stopped to obtain a precursor mother solution;
[0292] Second coprecipitation reaction: Under the reaction conditions of reaction temperature of 75°C and stirring speed of 350 rpm, antimony salt solution, alkali solution and ammonia solution were continuously added to control the pH of the reaction solution to 11 and the ammonia concentration to 0.65 mol / L. Feeding was stopped after the reaction reached the second target particle size Dv50 (10.5 μm);
[0293] Post-treatment: The reaction solution was allowed to stand for 24 hours to obtain an aged slurry containing the precursor material, and the slurry was washed and dried to obtain the precursor material.
[0294] 2) Preparation of positive electrode materials
[0295] LiOH·H2O is uniformly mixed with the above-mentioned precursor material and Sb2O3 in a molar ratio of 1.05:1:0.0024, and then sintered at 800°C for 15 hours in a box furnace under a pure oxygen atmosphere. The ternary positive electrode material can be obtained by crushing and sieving.
[0296] 3) Preparation of positive electrode sheet
[0297] The positive electrode material, conductive carbon black and binder PVDF prepared above were dispersed in solvent N-methylpyrrolidone (NMP) in a weight ratio of 90:5:5 and mixed evenly to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet was obtained.
[0298] 4) Preparation of negative electrode sheet
[0299] The negative electrode active material artificial graphite, hard carbon, conductive agent acetylene black, binder SBR, and thickener carbon methyl cellulose sodium (CMC) are fully stirred and mixed in a deionized water solvent system according to a weight ratio of 90:5:2:2:1, and then coated on a copper foil, dried, and cold pressed to obtain a negative electrode sheet.
[0300] 5) Electrolyte
[0301] Ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC) are mixed in a volume ratio of 1:1:1 to obtain a solvent, and then lithium salt LiPF6 is dissolved in the above solvent to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0302] 6) Isolation film
[0303] Polypropylene film is used as the isolation film.
[0304] 7) Preparation of full battery
[0305] The positive electrode sheet, separator, and negative electrode sheet of Example 1 were stacked in order, with the separator positioned between the positive and negative electrode sheets to provide isolation. The cells were then wound to obtain a bare cell. The tabs were welded to the bare cell and placed in an aluminum shell. The cells were then baked at 80°C to remove moisture. The electrolyte was then injected and sealed to obtain an uncharged battery. The uncharged battery then underwent a series of steps, including resting, hot and cold pressing, formation, shaping, and capacity testing, to obtain the lithium-ion battery product of Example 1.
[0306] Example 2-28
[0307] The preparation method of the battery of Example 2-28 is similar to that of the battery of Example 1, but the preparation parameters of the precursor material are adjusted. The specific parameters are shown in Tables 1 and 2.
[0308] Comparative Example 1-2
[0309] The preparation method of the battery of Comparative Example 1-2 is similar to that of the battery of Example 1, but the preparation parameters of the precursor material are adjusted. The specific parameters are shown in Table 1 and Table 2.
[0310] Comparative Example 3
[0311] The battery of Comparative Example 3 was prepared in a similar manner to that of Example 1, but the preparation of the precursor material was adjusted as follows:
[0312] Solution preparation: nickel sulfate, cobalt sulfate, and manganese sulfate were prepared at a molar ratio of Ni:Co:Mn = 96:2:2 to form a 1.5 mol / L mixed salt solution. 5 mol / L NaOH solution was used as the alkali solution, and 2 mol / L ammonia water was used as the complexing agent.
[0313] Preparation of reaction base solution: Add 10 L of deionized water to a 20 L controlled crystallization reactor, add a certain amount of concentrated ammonia water to make the ammonia concentration in the reactor 0.65 mol / L, and add a certain amount of NaOH solution to make the pH in the reactor 11 to obtain the reaction base solution;
[0314] Coprecipitation reaction: Under a nitrogen atmosphere, the reaction base liquid was heated to 75°C. At a stirring speed of 350 rpm, a mixed salt solution, alkali solution, ammonia solution, and a surfactant polyvinylpyrrolidone (PVP) were added to the reaction base liquid in parallel. The flow rates of the mixed salt solution, alkali solution, and ammonia solution were adjusted to adjust the pH of the reaction solution to 11 and the ammonia concentration to 0.65 mol / L. The reaction was continued until the target particle size Dv50 (10.5 μm) was reached, and then the pumping was stopped.
[0315] Post-treatment: The reaction solution was allowed to stand for 24 hours to obtain an aged slurry containing the precursor material, and the slurry was washed and dried to obtain the precursor material.
[0316] Comparative Example 4
[0317] The battery of Comparative Example 4 was prepared in a similar manner to that of Example 1, but the preparation of the precursor material was adjusted as follows:
[0318] Nickel sulfate, cobalt sulfate, and manganese sulfate were prepared into a mixed salt solution with a concentration of 1.5 mol / L according to the molar ratio of Ni:Co:Mn=96:3:1. Sodium tungstate was used to prepare an antimony salt solution with a concentration of 0.75 mol / L. 5 mol / L NaOH solution was used as an alkali solution, and 2 mol / L ammonia water was used as a complexing agent.
[0319] 10 L of deionized water was added to a 20 L controlled crystallization reactor, a certain amount of concentrated ammonia water was added to make the ammonia concentration in the reactor 0.65 mol / L, and a certain amount of NaOH solution was added to make the pH in the reactor 11 to obtain a reaction bottom solution;
[0320] Under a nitrogen atmosphere, the reaction base liquid was heated to 75° C., and a mixed salt solution, alkali solution, and ammonia solution were added to the reaction base liquid at a stirring speed of 350 rpm. The flow rates of the mixed salt solution, alkali solution, and ammonia solution were adjusted so that the pH of the reaction solution was 11 and the ammonia concentration was 0.65 mol / L. After the reaction reached the first target particle size Dv50 (9.5 μm), the pumping was stopped to obtain a precursor mother solution.
[0321] Under the reaction conditions of a reaction temperature of 75°C and a stirring speed of 350 rpm, antimony salt solution, alkali solution, and ammonia solution were continuously added to control the pH of the reaction solution to 11 and the ammonia concentration to 0.65 mol / L. The feeding was stopped after the reaction reached the second target particle size Dv50 (10.5 μm);
[0322] Post-treatment: The reaction solution was allowed to stand for 24 hours to obtain an aged slurry containing the precursor material, which was then washed and dried to obtain the precursor material.
[0323] 2. Performance Testing
[0324] 1. Precursor material performance test
[0325] 1) Chemical formula
[0326] An ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometer) was used, using a Thermo Fisher Scientific ICAP7400. First, 1 gram of sample was weighed into a beaker. 25 ml of a 25% by volume HNO3 solution was added to dissolve the sample. The solution was then diluted with 475 ml of deionized water. The diluted solution was then placed into the instrument for target elemental analysis, which resulted in the chemical formula of the precursor material.
[0327] 2)(101)Number of crystal facet layers N 101
[0328] X-ray diffraction (XRD) test conditions: Cu target, tube voltage 40 V, tube current 40 mA, scanning speed <2° / min, 2θ scanning range 15°-70°, step size 0.02°, emission slit (DS) 1 mm, anti-scatter slit (SS) 8 mm, graphite monochromator;
[0329] The grain size D of the (101) crystal plane was calculated by fitting the XRD spectrum of the precursor material. 101 :D 101 =kλ / (B 101 *cosθ 101 ); among them, B 101 is the half-peak width of the diffraction peak of the (101) crystal plane of the precursor material, k is the coefficient (usually 0.89-0.90), θ101 is the diffraction angle of the (101) crystal plane diffraction peak of the precursor material, and λ is the wavelength of the copper target; the corresponding value can be obtained by subsequent calculation.
[0330] The interplanar spacing d of the (101) crystal plane was calculated by fitting the XRD spectrum of the precursor material. 101 :d 101 =nλ / (2*sinθ 101 ), where θ 101 is the diffraction angle of the (101) crystal plane diffraction peak of the precursor material, and λ is the wavelength of the copper target; the corresponding value can be obtained by subsequent calculation.
[0331] After summarizing the above parameters, we can get the number of (101) crystal plane layers N 101 =D 101 / d 101
[0332] 3) Grain size ratio of (100) crystal plane to (001) crystal plane
[0333] X-ray diffraction (XRD) test conditions: Cu target, tube voltage 40 V, tube current 40 mA, scanning speed <2° / min, 2θ scanning range 15°-70°, step size 0.02°, emission slit (DS) 1 mm, anti-scatter slit (SS) 8 mm, graphite monochromator;
[0334] The grain size D of the (100) crystal plane was calculated by fitting the XRD spectrum of the precursor material. 100 :D 100 =kλ / (B 100 *cosθ 100 ); among them, B 101 is the half-peak width of the diffraction peak of the (100) crystal plane of the precursor material, k is the coefficient (usually 0.89-0.90), θ 101 is the diffraction angle of the (100) crystal plane diffraction peak of the precursor material, and λ is the wavelength of the copper target; the corresponding value can be obtained by subsequent calculation.
[0335] The grain size D of the (001) crystal plane was calculated by fitting the XRD spectrum of the precursor material. 001 :D 001 =kλ / (B 001 *cosθ 001 ); among them, B 001 is the half-peak width of the (001) diffraction peak of the precursor material, k is the coefficient (usually 0.89-0.90), θ 101 is the diffraction angle of the (001) crystal plane diffraction peak of the precursor material, and λ is the wavelength of the copper target; the corresponding value can be obtained by subsequent calculation.
[0336] After summarizing the above parameters, the grain size ratio D of (100) and (001) crystal planes is obtained. 100 / D 001 .
[0337] 4) Pore volume
[0338] According to the method in GB / T 21650.2-2008, "Determination of Pore Size Distribution and Porosity of Solid Materials by Mercury Intrusion and Gas Adsorption - Part 2: Analysis of Mesopores and Macropores by Gas Adsorption," a certain mass of sample is weighed and placed in a true density tester. The test system is sealed and helium or nitrogen is introduced as programmed. The true volume is calculated by measuring the pressure of the gas in the sample chamber and expansion chamber according to Bohr's law (PV = nRT).
[0339] 5) Deformation stacking fault rate f D
[0340] X-ray diffraction (XRD) test conditions: Cu target, tube voltage 40 V, tube current 40 mA, scanning speed <2° / min, 2θ scanning range 15°-70°, step size 0.02°, emission slit (DS) 1 mm, anti-scatter slit (SS) 8 mm, graphite monochromator;
[0341] The deformation stacking fault rate f is calculated by fitting the XRD spectrum of the precursor material. D :
[0342] Among them, B 101 is the half-height width of the diffraction peak of the (101) crystal plane of the precursor material, B 102 is the half-height width of the diffraction peak of the (102) crystal plane of the precursor material, D 001 It is the grain size of the (001) crystal plane diffraction peak of the precursor material, and the corresponding value can be obtained by subsequent calculation.
[0343] 6)Dv50
[0344] According to the particle size distribution laser diffraction method specified in GB / T 19077-2016, 0.1g-0.13g of the composite cathode material sample to be tested was weighed into a 50mL beaker, 5g of anhydrous ethanol was added, a stirring bar approximately 2.5mm in diameter was placed, and the sample was sealed with plastic wrap. After ultrasonic treatment for 5 minutes, the sample was transferred to a magnetic stirrer and stirred at 500 rpm for at least 20 minutes. Two samples were taken from each batch for testing. Testing was performed using a Malvern 3000 laser particle size analyzer from Malvern Instruments Ltd., UK. Dv50 is the particle size corresponding to the 50% cumulative volume distribution percentage of the composite cathode secondary particles.
[0345] 7) Specific surface area
[0346] The specific surface area is tested by gas adsorption method according to the GB / T19587-2017 test standard, as follows:
[0347] The precursor was taken as a sample, and the sample tube was immersed in liquid nitrogen at -196°C. The adsorption amount of nitrogen on the solid surface at different pressures was measured at a relative pressure of 0.05-0.30. The monolayer adsorption amount of the sample was obtained based on the BET multilayer adsorption theory and its formula, thereby calculating the specific surface area of the precursor material.
[0348] 8) The diffraction peak intensity ratio of (001) crystal plane to (101) crystal plane
[0349] The XRD spectrum of the tested sample was scanned at a slow speed (<2° / min), and the image was processed by smoothing and filtering to obtain the diffraction peak integral area I of the (001) crystal plane and the (101) crystal plane. 001 , I 101 , through (I 001 / I 101 ) is used to calculate the diffraction peak intensity ratio of the (001) crystal plane to the (101) crystal plane.
[0350] 2. Cathode materials
[0351] 1) Confirmation of the chemical formula of the positive electrode material
[0352] An ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometer) was used, using an ICAP7400 from Thermo Fisher Scientific (USA). First, 1g of sample was weighed into a beaker. 25ml of a 25% by volume HNO3 solution was added to dissolve the sample. The solution was then diluted with 475ml of deionized water. The diluted solution was then placed into the instrument for target element analysis, which resulted in the chemical formula of the cathode material.
[0353] 2) Micro stress
[0354] X-ray diffraction (XRD) test conditions: Cu target, tube voltage 40 V, tube current 40 mA, scanning speed <2° / min, 2θ scanning range 15°-70°, step size 0.02°, emission slit (DS) 1 mm, anti-scatter slit (SS) 8 mm, graphite monochromator;
[0355] After fitting the XRD spectrum, the micro stress is obtained: MS = (B hkl *Cosθ hkl ) / (4sinθ hkl ), where θ hkl is the diffraction angle of the positive electrode material (hkl) crystal plane in the XRD diffraction pattern, B hklis the half-height width of the crystal plane of the positive electrode material (hkl) in the XRD diffraction pattern.
[0356] 3) Aspect ratio of primary particles
[0357] Static image processing technology: Using static scanning electron microscope photos of primary particles, the software intelligently identifies the long diameter RL and wide diameter RS data of the primary particles, and then calculates the aspect ratio = RL / RS.
[0358] 2. Battery performance test
[0359] 1) Fully charged initial gram capacity test
[0360] Under a constant temperature environment of 25℃, let it stand for 5 minutes, discharge at 1 / 3C to 2.8V, let it stand for 5 minutes, charge at 1 / 3C to 4.25V, then charge at constant voltage at 4.25V to a current ≤0.05C, let it stand for 5 minutes, and then discharge at 1 / 3C to 2.8V. The discharge capacity at this time is the initial gram capacity, recorded as D0.
[0361] 2) 45℃ cycle capacity retention test
[0362] At 45°C, charge at a constant current of 1C to 4.25V, then charge at a constant voltage of 4.25V until the current drops to 0.05C, and then discharge at a constant current of 1C to 2.8V. This is the first-cycle discharge capacity (Cd1). Repeat this charge and discharge cycle for the 300th cycle, and the discharge capacity after n cycles is recorded as Cdn. Capacity retention = discharge capacity after n cycles (Cdn) / first-cycle discharge capacity (Cd1).
[0363] 3) DC internal resistance
[0364] In a constant temperature environment of 25℃, let it stand for 5 minutes, discharge at 1 / 3C to 2.8V, let it stand for 5 minutes, charge at 1 / 3C to 4.25V, then charge at constant voltage at 4.25V to a current ≤0.05C, let it stand for 5 minutes, and then discharge at 1 / 3C to 2.8V. The discharge capacity at this time is recorded as D0.
[0365] In a constant temperature environment of 25℃, let it stand for 30 minutes, charge to 4.25V at a current of 1 / 3D0, then charge at a constant voltage at 4.25V to a current ≤0.05D0, let it stand for 30 minutes, then discharge to the capacity position of 0.5D0 at a current of 1 / 3D0, and let it stand for 10 minutes.
[0366] Place the battery in a constant temperature environment at -25℃ for 120min, discharge it at a current of 0.36D0 for 10s, and record the voltage change ΔU at this time. Calculate the DC internal resistance R at 50% SOC at -25℃ according to Ohm's formula.50% = ΔU / (0.36D0)
[0367] III. Analysis of Test Results of Each Embodiment and Comparative Example
[0368] Prepare the batteries of each embodiment and comparative example respectively according to the above method, and measure various performance parameters. The results are shown in Table 3 below.
[0369] Table 3 Test Results of Secondary Battery Performance
[0370] According to the results in the above table, Embodiments 1-28 disclose the precursor materials of the present application. The precursor materials have the following general formula: Ni x Co y Mn z M a (OH)2, wherein the M element includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, La, 0.55 ≤ x < 1.0, 0 ≤ y < 0.45, 0 ≤ z < 0.45, 0 < a ≤ 0.45, a + x + y + z = 1, and the number of (101) crystal plane layers of the precursor material is 20-70.
[0371] It can be seen from the comparison between Embodiments 1-28 and Comparative Examples 1-4 that when the precursor material contains elements such as Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce or La, and the number of (101) crystal plane layers of the precursor material is controlled to be 20-70, the capacity of the battery can be effectively improved, the DC internal resistance of the battery can be reduced, the cycle capacity retention rate of the battery at high temperature can be improved, and the high-temperature cycle performance of the battery can be improved.
[0372] It can be seen from the comparison between Embodiments 1, 3-4 and Embodiments 2, 5 that controlling the number of (101) crystal plane layers to be 25-55 can further improve the capacity of the battery and reduce the DC internal resistance of the battery.
[0373] From the comparison of Example 7-8 with Example 6, it can be seen that controlling the deformation stacking fault rate fD of the precursor material to be less than or equal to 7.0% is beneficial to improving the cycle capacity retention rate of the battery at high temperature and improving the high temperature cycle performance of the battery. From the comparison of Example 8 with Example 6-7, it can be seen that controlling the deformation stacking fault rate fD of the precursor material to be less than or equal to 4% can further improve the cycle capacity retention rate of the battery at high temperature and improve the high temperature cycle performance of the battery. From the comparison of Example 19 and 21 with Example 20, it can be seen that controlling the deformation stacking fault rate fD of the precursor material to be less than or equal to 7.0% is beneficial to improving the cycle capacity retention rate of the battery at high temperature and improving the high temperature cycle performance of the battery. From the comparison of Example 21 with Examples 19 and 20, it can be seen that controlling the deformation stacking fault rate fD of the precursor material to be less than or equal to 4% can further improve the cycle capacity retention rate of the battery at high temperature and improve the high temperature cycle performance of the battery.
[0374] Comparing Examples 7-8 with Example 6, it can be seen that controlling the grain size ratio of the (100) crystal plane to the (001) crystal plane of the precursor material to be greater than or equal to 2.0 is beneficial to improving the cycle capacity retention rate of the battery at high temperature and improving the high-temperature cycle performance of the battery. Comparing Example 8 with Examples 6-7, it can be seen that controlling the grain size ratio of the (100) crystal plane to the (001) crystal plane of the precursor material to be greater than or equal to 4.4 can further improve the cycle capacity retention rate of the battery at high temperature and improve the high-temperature cycle performance of the battery.
[0375] From the comparison between Examples 10-11 and Example 9, it can be seen that the pore volume of the precursor material is controlled to be greater than or equal to 0.02 cm 3 / g, which can effectively improve the capacity of the battery. From the comparison between Example 11 and Examples 9-10, it can be seen that the pore volume of the precursor material is controlled to be greater than or equal to 0.025cm 3 / g, which can further improve the capacity of the battery.
[0376] From the comparison between Examples 12-13 and Example 14, it can be seen that adjusting the Dv50 value of the precursor material to 3-15 μm can increase the capacity of the battery and reduce the DC internal resistance of the battery.
[0377] From the comparison between Examples 10-12 and Example 9, it can be seen that the specific surface area of the precursor material is controlled to be 4m 2 / g-20m 2 / g, which can effectively improve the capacity of the battery. By comparing Example 11 with 9-10 and 12, it can be seen that the specific surface area of the precursor material is controlled to be 8m 2 / g-13m 2 / g, it can take into account both the battery capacity and cycle capacity retention rate, and comprehensively improve the battery performance. From the comparison between Example 13 and 12 / 14, it can be seen that the specific surface area of the precursor material is controlled to be 8m 2 / g-13m2 / g can take into account both the capacity and the cycle capacity retention rate of the battery, comprehensively improving the performance of the battery.
[0378] As can be seen from Example 1 and Examples 15 - 18, when the ratio of the diffraction peak intensities of the (001) crystal plane to the (101) crystal plane of the precursor material is controlled to be 0.6 - 1.25, the battery has a high capacity and excellent cycling performance. By comparing Example 1, Examples 16 - 17 with Examples 15 and 18, it can be seen that when the ratio of the diffraction peak intensities of the (001) crystal plane to the (101) crystal plane of the precursor material is controlled to be 0.9 - 1.18, it can take into account both the high capacity and the cycle capacity retention rate of the battery, comprehensively improving the performance of the battery.
[0379] The chemical formula of the positive electrode material in Examples 1 - 28 of this application is Li c1 Ni x1 Co y1 Mn z1 M1 a1 O 2-b1 , M includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, La, 0.5 ≤ c1 < 1.2, 0.55 ≤ x1 < 1.0, 0 ≤ y1 < 0.45, 0 ≤ z1 < 0.45, 0 < a1 ≤ 0.45, a1 + x1 + y1 + z1 = 1, -0.1 ≤ d1 < 0.1. From the comparison between Examples 1 - 28 and Comparative Examples 1 - 4, it can be seen that the positive electrode material of this application can increase the capacity of the battery, reduce the DC internal resistance of the battery, and improve the high-temperature cycling performance of the battery.
[0380] As can be seen from the comparison between Examples 7 - 8 and Example 6, controlling the micro stress of the positive electrode material to be less than or equal to 0.5% is beneficial to improving the cycle capacity retention rate of the battery at high temperature and improving the high-temperature cycling performance of the battery. From the comparison between Examples 19 and 21 and Example 20, it can be seen that controlling the micro stress of the positive electrode material to be less than or equal to 0.5% is beneficial to improving the cycle capacity retention rate of the battery at high temperature and improving the high-temperature cycling performance of the battery. From the comparison between Example 21 and Examples 19 and 20, it can be seen that controlling the micro stress of the positive electrode material to be less than or equal to 0.2% can further improve the cycle capacity retention rate of the battery at high temperature and improve the high-temperature cycling performance of the battery.
[0381] As can be seen from Examples 1 - 28, when the aspect ratio of the primary particles of the positive electrode material is controlled to be 1.5 - 10, the battery has a high capacity, a small DC internal resistance, and an excellent cycle capacity retention rate, comprehensively improving the performance of the battery. By comparing Example 1, Examples 24 - 25 with Examples 22 - 23, it can be seen that when the aspect ratio of the primary particles of the positive electrode material is controlled to be 2 - 5, it can take into account the capacity, DC internal resistance, and cycle capacity retention of the battery, comprehensively improving the performance of the battery.
[0382] In Comparative Example 3, during the preparation of the precursor material, no doping with Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, or La was performed, and the number of (101) crystal plane layers of the generated precursor material could not be made 20 to 70. From Comparative Example 3 and Examples 1-28, it can be seen that the addition of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, or La during the preparation of the precursor material is beneficial to increasing the capacity of the secondary battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0383] In Comparative Example 4, no surfactant was added during the preparation of the precursor material, and the number of (101) crystal plane layers in the generated precursor material could not be increased to 20-70. From Comparative Example 4 and Examples 1-28, it can be seen that adding a surfactant during the preparation of the precursor material is beneficial to increasing the capacity of the secondary battery, reducing the DC internal resistance of the battery, and improving the high-temperature cycle performance of the battery.
[0384] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A precursor material, characterized in that: The chemical formula of the precursor material is Ni x Co y Mn z M a (OH)2, Among them, the M element contains at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, and La, 0.55 ≤ x < 1.0, 0 ≤ y < 0.45, 0 ≤ z < 0.45, 0 < a ≤ 0.45, a + x + y + z = 1, and the number of (101) crystal plane layers of the precursor material is 20 - 70.
2. The precursor material according to claim 1, characterized in that The chemical formula Ni x Co y Mn z M a (OH)2, 0.90≤x<1.0, 0≤y<0.10, 0≤z<0.10, 0 <a≤0.10,a+x+y+z=1。 3. The precursor material according to claim 1, characterized in that The number of (101) crystal plane layers of the precursor material is 25 - 55.
4. The precursor material according to any one of claims 1 to 3, characterized in that The deformation stacking fault rate fD of the precursor material is less than or equal to 7.0%, and can be optionally less than or equal to 4.0%.
5. The precursor material according to any one of claims 1 to 4, characterized in that The grain size ratio of the (100) crystal plane to the (001) crystal plane of the precursor material is greater than or equal to 2.0, and can be optionally greater than or equal to 4.
4.
6. The precursor material according to any one of claims 1 to 5, characterized in that The pore volume of the precursor material is greater than or equal to 0.02 cm 3 / g, can be selected to be greater than or equal to 0.025cm 3 / g.
7. The precursor material according to any one of claims 1 to 6, characterized in that The Dv50 of the precursor material is 3 μm - 15 μm.
8. The precursor material according to any one of claims 1 to 7, characterized in that The specific surface area of the precursor material is 4m 2 / g-20m 2 / g, optional 8m 2 / g-13m 2 / g.
9. The precursor material according to any one of claims 1 to 8, characterized in that The diffraction peak intensity ratio of the (001) crystal plane to the (101) crystal plane of the precursor material is 0.60 - 1.25, and can be optionally 0.9 - 1.
18.
10. A method for preparing a precursor material, characterized in that: The preparation method includes the following steps: The precursor material is prepared by coprecipitation reaction, wherein the chemical formula of the precursor material is Ni x Co y Mn z M a (OH)2, Among them, M contains at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, and La, 0.55 ≤ x < 1.0, 0 ≤ y < 0.45, 0 ≤ z < 0.45, 0 < a ≤ 0.45, a + x + y + z = 1, and the number of (101) crystal plane layers of the precursor material is 20 - 70.
11. The preparation method according to claim 10, characterized in that: The preparation method specifically includes step (1) and step (2): Step (1): adding a mixed salt solution containing nickel salt, cobalt salt, manganese salt, precipitant solution, complexing agent solution and surfactant to the reaction base solution to perform a first coprecipitation reaction to achieve a first target particle size D V After 50, the reaction was stopped to obtain the precursor mother solution; Step (2): Add the precipitant solution, the complexing agent solution and the M salt solution to the precursor mother solution in parallel, and continue the second coprecipitation reaction to achieve the second target particle size D V After 50, the reaction is terminated to obtain the precursor material.
12. The preparation method according to claim 11, characterized in that: The mass percentage content of the surfactant input in step (1) is 0.1% - 5%, based on the total mass of nickel salt, cobalt salt, and manganese salt in the mixed salt solution.
13. The preparation method according to claim 11 or 12, characterized in that: The hydrophilic-lipophilic balance value of the surfactant input in step (1) is greater than 10, and can be optionally one or more of polyvinylpyrrolidone, triethanolamine oleate, polyoxyethylene oleyl ether, or polyoxyethylene lauryl ether.
14. The preparation method according to any one of claims 11 to 13, characterized in that: The first target particle size D in step (1) V 50 is 3 μm-9.5 μm, and the second target particle size D in the step (2) is V 50 is 3μm-15μm.
15. The preparation method according to any one of claims 11 to 14, characterized in that: The reaction temperature of the first co-precipitation reaction in step (1) is 65 - 85 °C, and the reaction temperature of the second co-precipitation reaction in step (2) is 65 - 85 °C.
16. The preparation method according to any one of claims 11 to 15, characterized in that: The pH value of the first co-precipitation reaction in step (1) is 8.5 - 11.5, and the pH value of the second co-precipitation reaction in step (2) is 8.5 - 11.
5.
17. The preparation method according to any one of claims 11 to 16, characterized in that: The molar concentration of the complexing agent in the first co-precipitation reaction system in step (1) is 0.5 - 1 mol / L, and the molar concentration of the complexing agent in the second co-precipitation reaction system in step (2) is 0.5 - 1 mol / L.
18. The preparation method according to any one of claims 11 to 17, characterized in that: The molar concentration of the mixed salt solution input in step (1) is 1 - 5 mol / L; the molar concentration of the precipitant solution input in step (1) is 1 - 10 mol / L; the concentration of the precipitant solution input in step (2) is 1 - 10 mol / L; the molar concentration of the M salt solution input in step (2) is 0.5 - 1 mol / L.
19. Use of the precursor material according to any one of claims 1 to 9 or the precursor material prepared by the preparation method according to any one of claims 10 to 18 for preparing a positive electrode material.
20. A positive electrode material, characterized in that: The positive electrode material is prepared from the precursor material described in any one of claims 1 to 9 or the precursor material prepared by the preparation method described in any one of claims 10 to 18.
21. The positive electrode material according to claim 20, characterized in that The positive electrode material satisfies formula (I) or formula (II), Li c1 Ni x1 Co y1 Mn z1 M1 a1 O 2-d1 , formula (Ⅰ); Li c2 Ni x2 Co y2 Mn z2 M1 a2 M2 e O 2-d2 , formula (II); Wherein, M1 and M2 each independently include at least one of Zr, Y, Al, Ti, W, Sr, Ta, Mo, Sb, Nb, Na, K, Ca, Ce, and La, 0.5≤c1<1.2, 0.55≤x1<1.0, 0≤y1<0.45, 0≤z1<0.45, 0 <a1≤0.45,a1+x1+y1+z1=1,-0.1≤d1<0.1;0.5≤c2<1.2,0.55≤x2<1.0,0≤y2<0.45,0≤z2<0.45,0<a2≤0.45,0<a2≤0.45,0<e≤0.45,a2+x2+y2+z2+e=1,-0.1≤d2<0.1。 22. The positive electrode material according to claim 20 or 21, characterized in that: The micro stress of the positive electrode material is less than or equal to 0.5%, and can be optionally less than or equal to 0.2%.
23. The positive electrode material according to any one of claims 21 to 22, characterized in that The primary particle aspect ratio of the positive electrode material is 1.5-10, and can be optionally 2-5.
24. A positive electrode plate, characterized in that: The positive electrode sheet comprises the positive electrode material according to any one of claims 20 to 23.
25. A secondary battery, characterized in that: Including the positive electrode sheet as described in claim 24.
26. An electrical device, characterized in that: Includes the secondary battery as claimed in claim 25.
Citation Information
Patent Citations
Crystal face induced high-nickel ternary precursor, preparation method thereof and positive electrode material
CN113023791A
Precursor, preparation method, positive electrode material comprising precursor, positive electrode and battery
CN114275825A
Ternary positive electrode material precursor and preparation method and application thereof
CN115140783A
High-nickel type nickel cobalt lithium manganate precursor and preparation method thereof
CN115403074A
Ternary precursor and preparation method thereof, ternary positive electrode material and electric device
CN115838189A
Cited By
Nanometer flaky ternary precursor as well as preparation method and application thereof
CN120440983A