Radiant catalytic ionization detoxification system and use thereof, and radiant catalytic ionization detoxification method
By designing the radiation catalytic ionization detoxification system and FeWO4-rGO composite material, the safety and efficiency problems of liquid material handling in the existing technology have been solved, and non-contact, efficient detoxification and sterilization effects have been achieved, which is suitable for large-scale liquid materials deal with.
Patent Information
- Application Number
- PCT/CN2023/095433
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2023-05-22
- Publication Date
- 2024-10-24
AI Technical Summary
Existing radiation catalytic ionization technology performs detoxification and sterilization under laboratory conditions, which poses food safety risks and lacks suitable large-scale liquid material processing equipment. The types of photocatalytic materials are limited and have different efficiencies, making it difficult to meet the needs under production conditions.
A radiation catalytic ionization detoxification system is designed, including a gas-liquid mixer and a reaction tube, using FeWO4-rGO composite material as a photocatalyst, through the gas-liquid mixing and circulation design of the reaction tube, combined with a radiation catalytic ionization box to provide activity Oxygen is used to achieve non-contact detoxification of liquid materials, and active oxygen is continuously replenished through the air supply pipe to improve detoxification efficiency.
It achieves non-contact detoxification treatment, avoids the contamination and quality degradation of liquids caused by photocatalytic materials, improves detoxification efficiency, is suitable for sterilization and detoxification of water and edible oil, and provides a safe and efficient solution.
Smart Images

Figure CN2023095433_24102024_PF_FP_ABST
Abstract
Description
Irradiation catalytic ionization detoxification system and its use and irradiation catalytic ionization detoxification method Technical Field
[0001] The invention belongs to the technical field of radiation catalytic ionization equipment, and particularly relates to a radiation catalytic ionization detoxification system and its application, and a radiation catalytic ionization detoxification method. Background Art
[0002] The active oxygen species after irradiation catalytic ionization is obtained through irradiation catalytic ionization technology. Radiant catalytic ionization (RCI) is an emerging sterilization and detoxification technology that can be used without restrictions in environments with humans, animals, and plants because it does not produce potentially hazardous byproducts such as ozone, formaldehyde, or carbon monoxide. The core of this technology is the photocatalytic effect, which is to generate electrons (e) by absorbing light energy through photocatalytic materials. – ) and holes (h + ) are converted into highly oxidizing reactive oxygen species (ROS), which participate in redox reactions of organic matter. Existing technologies for detoxification and sterilization use this technology only in laboratory conditions. During these experiments, the liquid must come into direct contact with the photocatalytic material, which poses certain food safety risks. Furthermore, there is currently no suitable equipment to complete the detoxification and sterilization of large quantities of liquid materials under production conditions.
[0003] Photocatalytic materials are crucial to radiation catalytic ionization technology. Different photocatalytic materials have different efficiencies in producing active oxygen. Currently, there are relatively few types of photocatalytic materials available, and the more common materials include TiO2, ZnO, etc.
[0004] Summary of the Invention
[0005] In response to the problems existing in the prior art, the present invention proposes a radiation catalytic ionization detoxification system, which includes a gas-liquid mixer for mixing air carrying active oxygen after radiation catalytic ionization with liquid materials to be detoxified and a reaction tube for circulating the mixed gas-liquid mixture.
[0006] Based on the above scheme, the reaction tube includes several U-shaped tubes and connecting tubes for connecting the U-shaped tubes; the end of the straight tube section of the U-shaped tube is detachably connected to an air supply tube for filling the U-shaped tube with air carrying active oxygen after irradiation catalytic ionization; and several air supply holes are provided on the wall of the air supply tube.
[0007] On the basis of the above solution, a plurality of fins are further provided on the air supply pipe.
[0008] Based on the above scheme, the air carrying active oxygen after radiation catalytic ionization is provided by an radiation catalytic ionization box; the radiation catalytic ionization box includes a box body, a plurality of mesh sheets arranged in the box body, and a lamp tube for providing an irradiation light source; the mesh sheets are attached with a photocatalytic material that generates active oxygen after light irradiation.
[0009] Based on the above solution, the box is also provided with a fixing frame for fixing the mesh and the lamp tube; the fixing frame is provided with fixing holes for fixing the lamp tube and fixing columns for fixing the mesh; the mesh is provided with mounting holes for the lamp tube to pass through and fixing holes for the fixing columns to pass through.
[0010] Based on the above solution, the photocatalytic material is a FeWO4-rGO composite material.
[0011] The present invention also provides a method for preparing a FeWO4-rGO composite material. Specifically, the method comprises the following steps:
[0012] (1) Preparation of FeWO4
[0013] First, 5 mmol of FeCl3·6H2O and 5 mmol of Na2WO4·2H2O were dissolved in 25 mL of distilled water, respectively. Then, ascorbic acid was added to the FeCl3 solution under continuous stirring to completely dissolve it. Next, the Na2WO4 solution was slowly added to the above mixture. After further stirring for 30 minutes, the mixture was added to a 100 mL autoclave (the autoclave only served as a reaction vessel) and maintained at 150-200°C for more than 9 hours. The autoclave was then naturally cooled to room temperature. The resulting precipitate was collected by centrifugation, washed several times with distilled water and anhydrous ethanol, and dried in air at 80°C for 6 hours.
[0014] Among them: Fe 3+ : The molar ratio of ascorbic acid is: 5:0.2-5:1;
[0015] (2) Preparation of FeWO4-rGO composite materials
[0016] First, 2g of FeWO4 was added to 300mL of ethanol and ultrasonically treated (ultrasonic conditions 300W) for 30min. After adding 2mL of APTES to the FeWO4 suspension, the mixture was heated at 70°C for 4h. Subsequently, the powder was collected, washed several times with ethanol, and then dried at 80°C overnight. After that, 1g of APTES-modified FeWO4 was added to 60mL of distilled water and ultrasonically treated (ultrasonic conditions 300W) for 15min, and then 0.05g of rGO was added. After stirring for 60min, the resulting suspension was transferred to an autoclave and kept at 180°C for 12h. The resulting product was collected, washed with water, and dried at 80°C overnight to obtain FeWO4-rGO.
[0017] The above-mentioned irradiation catalytic ionization detoxification system can be used for water sterilization or edible oil aflatoxin removal.
[0018] The present invention also provides a radiation catalytic ionization detoxification method, which uses the above-mentioned system and includes the steps of obtaining active oxygen by radiation catalytic ionization, mixing the air carrying the active oxygen after radiation catalytic ionization with the liquid material to be detoxified, and detoxifying the bacteria or aflatoxins in the liquid material with the active oxygen.
[0019] The detoxification system of the present invention can be used for sterilizing water or removing aflatoxin from edible oil. The irradiation catalytic ionization box in the system can provide the system with air containing active oxygen. The use of a mesh with a photocatalytic material attached to the box not only increases the content of the photocatalytic material in the unit space, but also increases the area of illumination because the photocatalytic material is evenly attached to the surface of the mesh. The system uses a U-shaped tube as a reaction tube, and the length of the reaction tube can be freely designed according to the actual detoxification requirements. The installation is convenient and quick. For the detoxification efficiency of the system, the system of the present invention uses an air supply tube to continuously replenish new air carrying active oxygen after irradiation catalytic ionization. At the same time, the photocatalytic material used in the present invention, the FeWO4-rGO composite material, has a simple preparation method. Ascorbic acid can be used not only as a reducing agent but also as a structure-directing agent to synthesize FeWO4 products. Surface charge modification provides a reasonable method for constructing FeWO4-rGO nanocomposite photocatalysts with sufficient interface contact through electrostatic self-assembly. The FeWO4-rGO composite material prepared by the method of the present invention has strong photocatalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] FIG1 is a schematic diagram showing the principle of the system described in Example 1;
[0021] FIG2 is a schematic structural diagram of an irradiation catalytic ionization box in a detoxification system according to the present invention;
[0022] FIG3 is a schematic structural diagram of a mesh in a detoxification system according to the present invention;
[0023] FIG4 is a schematic structural diagram of a reaction tube in a detoxification system according to the present invention;
[0024] FIG5 is a schematic diagram of the structure of the air supply pipe in the detoxification system of the present invention and a partially enlarged schematic diagram;
[0025] FIG6 is a schematic structural diagram of a fixed frame in the detoxification system of the present invention;
[0026] Figure 7 shows the XRD patterns of the samples in Example 2, including (a) snowflake-shaped FeWO4, (b) FeWO4-rGO-U, and (c) FeWO4-rGO;
[0027] Figure 8 shows the Raman spectra of the samples in Example 2, including (a) GO, (b) FeWO4, and (c) FeWO4-rGO.
[0028] Figure 9 shows the UV-vis diffuse reflectance spectra of the samples in Example 2, including (a) FeWO4, (b) FeWO4-rGO-U, and (c) FeWO4-rGO;
[0029] Figure 10 shows the N2 adsorption and desorption isotherms of the samples in Example 2; (a) snowflake FeWO4, (b) FeWO4-rGO-U, and (c) FeWO4-rGO;
[0030] Figure 11 shows the SEM and TEM images of the samples in Example 2; (a, b) SEM images of snowflake-shaped FeWO4 and (c) FeWO4-rGO composite. (d) (e) HRTEM and (f) corresponding SAED images of the FeWO4-rGO composite.
[0031] FIG12 is a schematic reaction mechanism diagram of the photocatalytic redox reaction on the FeWO4-rGO composite photocatalyst under visible light irradiation;
[0032] Figure 13 is the SEM images of FeWO4 generated under different temperature conditions; (a) 120℃, (b) 150℃, (c, d) 200℃;
[0033] Figure 14 shows the SEM images and XRD patterns of FeWO4 produced under different reaction conditions; (a) 0h, (b) 2h, (c) 6h, (d) 9h and (e) 12h. (f) XRD patterns of the prepared samples after hydrothermal treatment at 180℃ for different reaction times.
[0034] FIG15 is a schematic diagram of the L-ascorbic acid oxidation process;
[0035] FIG16 is a schematic diagram showing the formation of FeWO4 having a snowflake-like structure;
[0036] Figure 17 is a SEM image of FeWO4 generated under different ascorbic acid dosage conditions, in which: Fe 3+ : The molar ratio of ascorbic acid is different, including (a, b) 5:0.2, (c, d) 5:0.3 and (e, f) 5:1;
[0037] Figure 18 is the SEM images of FeWO4 prepared from different raw materials, where (a, b) Fe(NO3)3 is used instead of FeCl3; (c, d) 5mmol FeCl3·6H2O, 5mmol Na2WO4·2H2O, 0.5mmol ascorbic acid and 0.1mmol hexadecyltrimethylammonium bromide. DETAILED DESCRIPTION
[0038] Unless otherwise specified, the terms used in the present invention generally have the meanings commonly understood by those skilled in the art.
[0039] The present invention will be further described in detail below with reference to specific examples and data. The following examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention in any way.
[0040] Example 1
[0041] As shown in Figure 1, this patent provides a radiation catalytic ionization detoxification system, which includes a gas-liquid mixer 1 for mixing air carrying active oxygen after radiation catalytic ionization with liquid materials to be detoxified and a reaction tube 4 for circulating the mixed gas-liquid mixture.
[0042] The active oxygen species after irradiation catalytic ionization is obtained through irradiation catalytic ionization technology. Radiant catalytic ionization (RCI) is an emerging sterilization and detoxification technology that can be used without restrictions in environments with humans, animals, and plants because it does not produce potentially hazardous byproducts such as ozone, formaldehyde, or carbon monoxide. The core of this technology is the photocatalytic effect, which is to generate electrons (e) by absorbing light energy through photocatalytic materials. – ) and holes (h + ) are converted into highly oxidizing reactive oxygen species (ROS), which participate in the redox reactions of organic matter. A wide range of photocatalytic materials are currently available, including g-C3N4 and / or FeWO4-rGO composites, as well as TiO2, Bi2WO6, upconversion nanoparticles@TiO2, and Ag-AgCl / α-Fe2O3.
[0043] The gas-liquid mixer 1 is a device for fully mixing gas and liquid. During the mixing process, the gas in the liquid is broken into small bubbles or micron or nanometer-type bubbles, thereby increasing the contact area between the gas and the liquid, and effectively improving the redox reaction between the active oxygen in the gas and the object to be treated in the liquid.
[0044] The liquid material to be detoxified can be edible oil contaminated with aflatoxin (it can also be zearalenone, vomitoxin, etc.), beverages, soy milk, milk, etc., or it can be sewage to be sterilized.
[0045] The detoxification system of the present invention uses a method of performing detoxification without contact between the photocatalytic material and the liquid to be treated. First, it can avoid secondary contamination of the liquid by the photocatalytic material. Second, it can avoid the risk of quality reduction caused by direct exposure of the liquid to light (for example, light can change the acid value, peroxide value, unsaturated fatty acids, etc. of peanut oil).
[0046] As the active oxygen-carrying air and the liquid material to be detoxified circulate within the reaction tube 4, the active oxygen continuously undergoes a redox reaction. However, as the active oxygen in the air is continuously consumed, the oxidizing power of the gas gradually decreases. To address this issue, it is necessary to continuously inject air carrying active oxygen ionized by irradiation catalytically into the gas-liquid mixture as it circulates within the reaction tube 4, thereby achieving rapid treatment. If the amount of active oxygen in the active oxygen-containing air injected into the liquid material is sufficient, there is no need to add new active oxygen to the reaction tube 4. However, if the amount of active oxygen-containing air injected into the liquid material is insufficient to treat the liquid material to be detoxified, based on the above-described technical solution, it is necessary to continuously inject air carrying active oxygen ionized by irradiation catalytically into the gas-liquid mixture as it circulates within the reaction tube 4.
[0047] As a specific embodiment, the present invention provides a specific implementation case of a reaction tube 4, as shown in Figure 4, the reaction tube 4 includes several U-shaped tubes 4-1 and connecting tubes 4-2 for connecting the U-shaped tubes 4-1; the connecting tubes 4-2 can be connected between the U-shaped tubes 4-1 by threaded connection. This method can freely design the length of the reaction tube according to the actual detoxification requirements, and the installation is convenient and quick.
[0048] During the circulation of the mixed material in the reaction tube 4, the active oxygen in the air is continuously consumed, and the oxidizing ability of the gas gradually decreases. Therefore, in order to improve the detoxification efficiency, it is necessary to maintain the content of active oxygen in the mixed material. To this end, it is necessary to continuously replenish new air carrying active oxygen after catalytic ionization by radiation. As a specific embodiment, as shown in Figure 4, the present invention designs the end of the straight tube section of the U-shaped tube 4-1 into an open structure that can be opened or closed at any time. When it is necessary to replenish active oxygen gas, the opening is opened, and the air supply pipe 4-3 is inserted into the straight tube section from the opening. The air supply pipe 4-3 is used to fill the U-shaped tube 4-1 with air carrying active oxygen after catalytic ionization by radiation; the air supply pipe 4-3 is detachably connected to the end of the straight tube section of the U-shaped tube 4-1; when air supply is not needed, the end of the straight tube section of the U-shaped tube 4-1 is sealed with an end plug (not shown in the figure). A plurality of air supply holes 4-31 are provided on the wall of the air supply pipe 4-3.
[0049] In order to improve the mixing degree between the newly added gas and the liquid, a plurality of fins 4-32 are provided on the gas supply pipe 4-3 as shown in Figure 5. The provision of the plurality of fins 4-32 can not only break up the newly added gas into small bubbles, but also effectively improve the mixing degree of the gas and the liquid.
[0050] For the detoxification system of the present invention, the amount of active oxygen carried in the air is crucial to the detoxification effect. In order to increase the concentration of active oxygen carried in the air, the present invention provides a specific implementation case, as shown in Figure 2, the air carrying active oxygen after irradiation catalytic ionization is provided by an irradiation catalytic ionization box 2; the irradiation catalytic ionization box 2 includes a box body 2-1, a plurality of mesh sheets 2-2 arranged in the box body 2-1 and a lamp tube 2-3 for providing an irradiation light source; the mesh sheets 2-2 are attached with a photocatalytic material that generates active oxygen after light irradiation.
[0051] The irradiation catalytic ionization box 2 of the present invention is provided with several mesh sheets 2-2 with attached photocatalytic materials. Under the illumination of the lamp tube 2-3, more active oxygen can be stimulated. The box body 2-1 is open at both ends, with one end for air intake and the other end for air exhaust. The active oxygen is driven from the box body 2 into the gas-liquid mixer 1 by a fan (not shown in the figure) to mix with the liquid material to be treated. Specifically, the mesh sheets 2-2 can be made of a light-transmitting material, and the surface of the mesh sheets 2-2 is attached with a photocatalytic material. Compared with existing catalytic ionization equipment, the irradiation catalytic ionization box 2 of the present invention uses mesh sheets 2-2 with attached photocatalytic materials, rather than setting the photocatalytic materials on a flat plate. This not only increases the content of photocatalytic materials per unit space, but also increases the area of illumination because the photocatalytic materials are evenly attached to the surface of the mesh sheets. At the same time, the mesh structure of the mesh sheets 2-2 not only meets the needs of gas circulation, but also facilitates the circulation of air through the mesh sheets and removes the active oxygen generated by the irradiation of the photocatalytic materials on the mesh sheets. It also carries more photocatalytic materials, thereby providing sufficient active oxygen for the system. As a specific implementation example, the mesh 2-2 is made of a light-transmitting acrylic plate, PC or PVC hard plate provided with air holes, on which a photocatalytic material is attached.
[0052] As a specific application solution, as shown in FIG2 , a fixing frame 2-4 for fixing the mesh 2-2 and the light tube 2-3 is further provided in the box 2-1; fixing holes 2-41 for fixing the light tube 2-3 and fixing posts 2-42 for fixing the mesh 2-2 are provided on the fixing frame 2-4; and as shown in FIG3 , a mounting hole 2-21 for the light tube 2-3 to pass through and a fixing hole 2-22 for the fixing post 2-42 to pass through are provided on the mesh 2-2. In this way, the mesh 2-2, the light tube 2-3 and the fixing frame 2-4 can be assembled in advance outside the box 2-1, and after assembly, they can be inserted into the box 2-1, and the fixing frame 2-4 can be fixed in the box 2-1 (the four legs of the fixing frame 2-4 are fixed to the inner wall of the box 2-1). FIG3 only shows one implementation method of the position and number of the mounting hole 2-21 and the fixing hole 2-22. When in use, the position and number of the mounting hole 2-21 and the fixing hole 2-22 can be freely set as needed.
[0053] The structure of the fixing frame 2-4 is shown in Figure 6. Since the box 2-1 is ventilated when in use, in order to increase the stability of the mesh 2-2 and the lamp tube 2-3, as shown in Figure 2, a fixing frame is added on the other side of the mesh (the left side in the figure). The fixing column is replaced by a round hole in the middle of this fixing frame. The round hole is used for inserting the fixing column 2-42, which will not be repeated here.
[0054] The specific type of lamp 2-3 is not particularly limited, as long as it can irradiate the catalytic semiconductor material to produce active oxygen, such as an ordinary fluorescent lamp or a lamp that produces light of a special wavelength, such as a 300-watt xenon lamp and an optical cutoff filter used in Example 3.
[0055] During use, the lamps 2-3 in the irradiation catalytic ionization chamber 2 are turned on for irradiation catalysis. A pump is used to pump the material to be treated in the liquid tank 3 into the gas-liquid mixer 1. At the same time, a fan is used to inject the active oxygen generated by the irradiation catalytic ionization chamber 2 into the gas-liquid mixer 1 to mix with the liquid material. The mixed material is then pumped into the reaction tube 4 for detoxification. In the reaction tube 4, the oxidizing capacity of the gas gradually decreases. Therefore, to improve the detoxification efficiency, the gas supply pipe 4-3 is used to supply gas to the reaction tube 4.
[0056] Example 2
[0057] Based on the detoxification system in Example 1, this example provides a photocatalytic material that can be used in the system - FeWO4-rGO composite material, the FeWO4-rGO composite material is prepared by the following method:
[0058] (1) Preparation of FeWO4
[0059] First, 5 mmol of FeCl3·6H2O and 5 mmol of Na2WO4·2H2O were dissolved in 25 mL of distilled water, respectively. Then, 0.5 mmol of ascorbic acid was added to the FeCl3 solution under continuous stirring to completely dissolve it. Next, the Na2WO4 solution was slowly added to the above mixture. After further stirring for 30 minutes, the mixture was added to a 100 mL autoclave (the autoclave in this example was only used as a reaction vessel) and kept at 180°C for 12 hours. The autoclave was then cooled naturally to room temperature. The resulting precipitate was collected by centrifugation, washed several times with distilled water and anhydrous ethanol, and dried in air at 80°C for 6 hours.
[0060] (2) Preparation of FeWO4-rGO composite materials
[0061] First, 2g of FeWO4 was added to 300mL of ethanol and ultrasonically treated (ultrasonic conditions 300W) for 30min. After adding 2mL of APTES to the FeWO4 suspension, the mixture was heated at 70°C for 4h. Subsequently, the powder was collected, washed several times with ethanol, and then dried at 80°C overnight. After that, 1g of APTES-modified FeWO4 was added to 60mL of distilled water and ultrasonically treated (ultrasonic conditions 300W) for 15min, and then 0.05g of rGO was added. After stirring for 60min, the resulting suspension was transferred to an autoclave and kept at 180°C for 12h. The resulting product was collected, washed with water, and dried at 80°C overnight to obtain FeWO4-rGO.
[0062] Example 3
[0063] In order to compare the superiority of the charge modification method, the snowflake-shaped FeWO4 prepared in step (1), FeWO4-rGO-U (FeWO4-rGO-U is a mixture of FeWO4 and rGO directly ground and mixed) and FeWO4-rGO prepared by the above method were tested.
[0064] (1) XRD test
[0065] The results are shown in Figure 7. All product diffraction peaks can be attributed to the standard card of FeWO4 (JCPDS No. 46-1446). In addition, no diffraction peaks of rGO were observed.
[0066] (2) Raman spectroscopy test
[0067] The results are shown in Figure 8. Raman analysis further confirmed that the composite contained rGO. As shown in Figure 8 (a), the rGO -1 Two main peaks were observed near 93, 132, 215, 179, 349, 683 and 875 cm-1, which should be attributed to the G band and D band of GO. -1 The peak at 1598 cm corresponds to the Raman spectrum of FeWO4. For the FeWO4-rGO composite, in addition to the peaks attributed to FeWO4, the G band and D band of rGO are located at 1598 cm and 1345 cm, respectively. -1 This clearly indicates the presence of rGO in the prepared rGO-FeWO4 composites.
[0068] (3) UV-vis diffuse reflection
[0069] The results are shown in Figure 9. The optical properties of the material can be characterized by UV-vis DRS spectroscopy, and the snowflake-shaped FeWO4 shows strong absorption in the visible light region. By adding rGO, enhanced absorption of visible light in the region between 500 and 800 nm can be clearly observed. The expansion of the light absorption range can achieve more efficient utilization of the solar spectrum and enhanced photocatalytic activity. In addition, the background absorption of the FeWO4-rGO composite in the visible light region is significantly enhanced.
[0070] (4) N2 adsorption and desorption
[0071] The N2 adsorption-desorption isotherms of the prepared products are shown in Figure 10. The specific surface areas of FeWO4-rGO, FeWO4-rGO-U and pure snowflake-like FeWO4 are 49.18, 47.03 and 45.80 cm 3 g -1 , there is no significant difference in the values.
[0072] (5) SEM and TEM testing
[0073] The results are shown in Figure 11. The morphology and structure of the snowflake-shaped FeWO4 and FeWO4-rGO composites were investigated using SEM and TEM. As shown in Figure 11(a), FeWO4 is composed of uniform snowflake-shaped crystallites with a diameter of approximately 1 μm. High-magnification SEM reveals that each snowflake-shaped FeWO4 with approximately six-fold symmetry is composed of nanorods assembled in a specific direction (Figure 11(b)). As for the FeWO4-rGO composite (Figure 11(cd)), FeWO4 is wrapped by rGO nanosheets, which means that there is potential for sufficient contact and effective interfacial interaction between FeWO4 and rGO. The TEM of the FeWO4-rGO composite is shown in Figure 11(d). The FeWO4 assemblies are deposited on the surface of the rGO sheets. The sample shows some wrinkles at the edges of both the rGO sheets and the interlayer sheets, providing more active sites for adsorption. Figure 11(e) shows well-defined lattice fringes with a spacing of 0.22 nm, which corresponds to the (020) planes of FeWO4. Furthermore, selected area electron diffraction (SAED) showed well-defined rings, which confirmed the polycrystalline nature of the sample.
[0074] As shown in Figure 12, under visible light irradiation, electrons in the valence band (VB) are excited to the conduction band (CB), leaving holes in the VB and generating electron-hole pairs in FeWO4. Then, the photogenerated electrons (e-) are transferred from the FeWO4 microstructure to the rGO sheet and further react with O2 to produce highly active free radicals (O2·-). The holes in the VB of FeWO4 react with water to form active OH·. These free radicals can attack fungal toxins and eliminate them through photocatalytic redox reactions. On the other hand, compared with FeWO4-GO-U composites, surface charge modification provides a reasonable method for constructing FeWO4-rGO nanocomposite photocatalysts with sufficient interfacial contacts through electrostatic self-assembly. All of the above factors help to improve the separation efficiency of electron-hole pairs, thereby significantly improving the photoactivity of FeWO4-rGO composites.
[0075] Morphological changes of FeWO4 generated under different temperature conditions
[0076] First, 5 mmol of FeCl₃·6H₂O and 5 mmol of Na₂WO₄·2H₂O were dissolved in 25 mL of distilled water, respectively. Then, 0.5 mmol of ascorbic acid was added to the FeCl₃ solution under continuous stirring to completely dissolve it. Next, the Na₂WO₄ solution was slowly added to the mixture. After further stirring for 30 minutes, the mixture was placed in a 100 mL autoclave and maintained at a constant temperature for 12 hours. The autoclave was then cooled naturally to room temperature. The resulting precipitate was collected by centrifugation, washed several times with distilled water and anhydrous ethanol, and dried in air at 80°C for 6 hours.
[0077] The results are shown in Figure 13, which shows the effect of temperature on the morphology of the FeWO4 sample. Irregular shapes were observed at 120°C (Figure 13(a)). After the temperature was increased to 150°C, although the morphology of the product was similar to that of the sample hydrothermally treated at 120°C, the average size of the product was smaller. When the temperature was increased to 180°C (Figure 11(a) and (b)), the prepared sample consisted of snowflakes with perfect uniformity. When the temperature was 200°C, although the sample maintained a snowflake-like structure, the surface of the nanorods became smoother (Figure 13(c) and (d)). This result also shows that the final morphology depends on the formation temperature of the FeWO4 crystals.
[0078] Morphological changes of FeWO4 generated under different time conditions
[0079] First, 5 mmol of FeCl₃·6H₂O and 5 mmol of Na₂WO₄·2H₂O were dissolved in 25 mL of distilled water, respectively. Then, 0.5 mmol of ascorbic acid was added to the FeCl₃ solution under continuous stirring to completely dissolve it. Next, the Na₂WO₄ solution was slowly added to the mixture. After further stirring for 30 minutes, the mixture was placed in a 100 mL autoclave and maintained at 180°C for a specified period of time. The autoclave was then naturally cooled to room temperature. The resulting precipitate was collected by centrifugation, washed several times with distilled water and anhydrous ethanol, and dried in air at 80°C for 6 hours.
[0080] To understand the growth mechanism of snowflake-shaped FeWO₄, SEM images of materials prepared at different hydrothermal times are shown in Figure 14. When the reaction time is less than 2 h, the product consists of large, oval particles (Figures 14(a) and (b)). Figure 14(c) shows an image of a sample after 6 h of reaction, indicating the formation of plate-like aggregates. These aggregates are formed by numerous nanoparticles and nanorods. As the process continues, snowflake-like FeWO₄ structures emerge after 9 h, exhibiting hexagonal symmetry (Figure 14(d)). It should be noted that the nanorods extend outward from the center of the aggregates in a self-assembled manner. As the reaction continues, the irregular particles disappear, and longer nanorods form, indicating that the longer nanorods grow at the expense of smaller particles. After 12 h, the nanoparticles on the surface of the FeWO₄ snowflakes grow along their axes, forming nanorods (Figure 14(e)). These images clearly demonstrate the shape evolution of the obtained products, from aggregates constructed from nanoparticles to snowflake-like structures. Figure 14(f) shows the XRD patterns of FeWO₄ samples prepared at different hydrothermal times. The crystalline phase increases with the increase of hydrothermal time. All XRD patterns can be easily identified as FeWO4.
[0081] Based on the above analysis, the shape evolution process of the snowflake-like microstructure is shown in Figures 15 and 16. In this process, the oxygen-containing groups (such as -OH and C=O) in DHA and DGA strongly tend to react with Fe 2+ The cations coordinate and form a complex. Therefore, the free Fe 2+ The concentration of cations decreases. The slow formation rate of FeWO4 will lead to the separation of nucleation and growth steps. Then WO4 2-The FeWO4 cores react with the complex to form FeWO4 cores. DHA and DGA in the reaction system are absorbed by the FeWO4 core surface. Simultaneously, due to the reduction in the core surface energy and the hydrogen interactions between DHA and DGA, the FeWO4 cores tend to aggregate. Furthermore, due to the high intrinsic anisotropy of FeWO4, the nanoparticles prefer to grow into nanorods through directional attachment. With increasing hydrothermal treatment time, a snowflake-like microstructure forms. We can conclude that the formation of the hierarchical snowflake-like microstructure is the result of ascorbic acid-induced reduction, formation, and aggregation of nanoparticles, followed by nanorod growth and subsequent self-assembly. According to previously reported literature, FeWO4, after APTES modification, possesses amine functional groups. Under the action of electrostatic attraction, FeWO4 is anchored to the negatively charged surface of rGO nanosheets.
[0082] Effect of different amounts of ascorbic acid on product morphology
[0083] First, 5 mmol of FeCl₃·6H₂O and 5 mmol of Na₂WO₄·2H₂O were dissolved in 25 mL of distilled water. Then, a certain amount of ascorbic acid was added to the FeCl₃ solution under continuous stirring to completely dissolve it. Next, the Na₂WO₄ solution was slowly added to the mixture. After further stirring for 30 minutes, the mixture was placed in a 100 mL autoclave and maintained at 180°C for 12 hours. The autoclave was then cooled naturally to room temperature. The resulting precipitate was collected by centrifugation, washed several times with distilled water and anhydrous ethanol, and dried in air at 80°C for 6 hours.
[0084] The effect of varying amounts of ascorbic acid on the product morphology was investigated, and the results are shown in Figure 17. Figure 17 shows SEM images of samples prepared with varying amounts of ascorbic acid (0.2 to 1 mmol) in the reaction system. When 0.2 mmol of ascorbic acid was added, disordered tiny particles were the primary product (Figure 17(a)(b)). Increasing the amount of ascorbic acid to 0.3 mmol resulted in the formation of some particle aggregates (Figure 17(c)(d)). Further increasing the amount of ascorbic acid to 0.5 mmol resulted in the preparation of samples composed of perfectly uniform and monodisperse snowflakes (Figure 17(a)(b)). When the ascorbic acid dosage reached 1 mmol, the product exhibited a spherical shape composed of nanorods (Figure 17(e)(f)). Therefore, the successful preparation of the novel FeWO4 nanostructures demonstrates that, in this system, ascorbic acid can act not only as a reducing agent but also as a structure-directing agent for the synthesis of FeWO4 products.
[0085] Effects of different raw materials on FeWO4
[0086] While keeping step (1) in Example 2 unchanged, A only replaced FeCl3·6H2O with an equal mole of Fe(NO3)3·9H2O, and B only added 0.1 mmol of hexadecyltrimethylammonium bromide while adding ascorbic acid.
[0087] The results are shown in Figure 18. The morphology and size of the FeWO4 product depend on the iron precursor salt used. The anion of the iron precursor salt determines the final structure of FeWO4. Under similar conditions, using only Fe(NO3)3 instead of FeCl3 does not result in a uniform snowflake-like structure assembled by nanorods. The corresponding SEMs are shown in Figure 18 (a) and (b). In addition to the iron precursor salt, we found that the presence of CTAB also affects the morphology of the final product, as shown in Figure 18 (c) and (d). In the presence of CTAB, the final product can also be composed of nanorods, but the snowflake-like organized structure does not exist at all. Therefore, CTAB can also provide additional control over the product morphology.
[0088] Aflatoxin (AFB1) degradation test, the steps are as follows:
[0089] 500 mg of the flower-shaped FeWO4-rGO composite material prepared in Example 2 was coated on a glass substrate and then added to 100 mL of corn oil containing AFB1 (concentration 16.8 ppb) with magnetic stirring at 500 rpm. The suspension was then stirred in the dark for 30 minutes to reach adsorption-desorption equilibrium. A 300-watt xenon lamp was used to irradiate the suspension. 5 mL of corn oil was collected at 0 min, 15 min, 30 min, 45 min, 60 min, and 75 min irradiation times. Liquid chromatography was used to test the concentration of AFB1 in peanut oil, and the results are shown in Table 1. The control group consisted of snowflake-shaped FeWO4 and FeWO4-rGO-U prepared in the comparative example.
[0090] Table 1
[0091] It can be seen from Table 1 that compared with snowflake-like FeWO4 and FeWO4-rGO-U, flower-like FeWO4-rGO has excellent photocatalytic degradation performance for corn oil AFB1.
[0092] Application Example 2
[0093] The Escherichia coli suspension was mixed with the prepared material, and an optical cutoff filter (λ>420nm) was used to irradiate with a 300-watt xenon lamp for antibacterial performance evaluation. The bacterial suspension with different irradiation time intervals (0min, 5min, 10min, 15min, 20min, 25min) was spread on LB agar plates, cultured in a 37°C incubator for 4h, and the colony growth was observed. At the same time, the bacterial suspension was diluted, and the plate count was performed to determine the number of surviving bacteria and calculate the bactericidal efficiency. Bactericidal efficiency (%) = (N0-N t ) / N0×100%
[0094] Note: N0 and N in the formula t The number of colonies counted on the control group and sample plates respectively
[0095] The test results are shown in Table 2.
[0096] Table 2
[0097] It can be seen from Table 2 that compared with snowflake-shaped FeWO4 and FeWO4-rGO-U, the snowflake-shaped FeWO4-rGO prepared in the present application has excellent photocatalytic killing performance against Escherichia coli.
[0098] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any other manner. Any person skilled in the art may utilize the above-disclosed technical content to modify or modify the present invention into equivalent embodiments. However, any simple modifications, equivalent variations, and modifications to the above embodiments that do not depart from the technical content of the present invention and are based on the technical essence of the present invention remain within the scope of protection of the present invention.
Claims
1. A radiation catalytic ionization detoxification system, characterized in that: The invention comprises a gas-liquid mixer (1) for mixing air carrying active oxygen after ionization by radiation catalysis with liquid material to be detoxified, and a reaction tube (4) for circulating the mixed gas-liquid mixture.
2. The radiation catalytic ionization detoxification system according to claim 1, characterized in that: The reaction tube (1) comprises a plurality of U-shaped tubes (4-1) and connecting tubes (4-2) for connecting the U-shaped tubes (4-1); the end of the straight tube section of the U-shaped tube (4-1) is detachably connected to an air supply tube (4-3) for filling the U-shaped tube (4-1) with air carrying active oxygen after ionization by radiation catalysis; and a plurality of air supply holes (4-31) are arranged on the wall of the air supply tube (4-3).
3. The radiation catalytic ionization detoxification system according to claim 2, characterized in that: The air supply pipe (4-3) is also provided with a plurality of fins (4-32).
4. The radiation catalytic ionization detoxification system according to claim 1, characterized in that: The air carrying active oxygen after irradiation catalytic ionization is provided by an irradiation catalytic ionization box (2); the irradiation catalytic ionization box (2) comprises a box body (2-1), a plurality of mesh sheets (2-2) arranged in the box body (2-1), and a lamp tube (2-3) for providing an irradiation light source; a photocatalytic material that generates active oxygen after light irradiation is attached to the mesh sheets (2-2).
5. The radiation catalytic ionization detoxification system according to claim 4, characterized in that: A fixing frame (2-4) for fixing the mesh (2-2) and the light tube (2-3) is also provided in the box body (2-1); a fixing hole (2-41) for fixing the light tube (2-3) and a fixing column (2-42) for fixing the mesh (2-2) are provided on the fixing frame (2-4); and a mounting hole (2-21) for the light tube (2-3) to pass through and a fixing hole (2-22) for the fixing column (2-42) to pass through are provided on the mesh (2-2).
6. The radiation catalytic ionization detoxification system according to claim 4, characterized in that: The photocatalytic material is a FeWO4-rGO composite material.
7. The radiation catalytic ionization detoxification system according to claim 6, characterized in that: The FeWO4-rGO composite material is prepared by the following method: FeWO4 was added to ethanol and ultrasonicated; after APTES was added to the FeWO4 suspension, the mixture was heated at 70 °C for 4 h; Subsequently, the powder was collected, washed with ethanol, and dried; Afterwards, APTES-modified FeWO4 was added to distilled water and ultrasonicated, and then rGO was added; after stirring for 60 min, the resulting suspension was kept at 180 °C for 12 h; finally, the resulting product was collected, washed with water and dried at 80 °C to obtain FeWO4-rGO.
8. The radiation catalytic ionization detoxification system according to claim 8, characterized in that: The FeWO4 is prepared by the following method: First, FeCl3·6H2O and Na2WO4·2H2O are dissolved in distilled water respectively; then, ascorbic acid is added to the FeCl3 solution under continuous stirring to completely dissolve; then, the Na2WO4 solution is slowly added to the above mixture; after further stirring, the mixture is kept at high temperature for a period of time; then naturally cooled to room temperature; the resulting precipitate is collected by centrifugation, washed and dried.
9. Use of the irradiation catalytic ionization detoxification system according to any one of claims 1 to 8 in water sterilization or edible oil aflatoxin removal.
10. A radiation catalytic ionization detoxification method, characterized in that: The system according to any one of claims 1 to 8 comprises the steps of obtaining active oxygen by radiation catalytic ionization, mixing air carrying active oxygen after radiation catalytic ionization with liquid material to be detoxified, and detoxifying bacteria or aflatoxins in the liquid material by using active oxygen.
Citation Information
Patent Citations
Surface self-cleaning carbon nitride Fenton-photocatalytic nanofiltration membrane and preparation method thereof
CN109569311A
Advanced oxidation treatment device rich in high-performance filler
CN111606409A
Visible-light-induced photocatalyst for treating hexavalent chromium wastewater and synthesis method thereof
CN112517068A
Degree of depth water treatment facilities
CN207210021U
Little electrolysis sewage treatment pond of iron carbon
CN208603779U