Negative electrode sheet and preparation method therefor, battery cell, battery and electric device

By forming an organic-inorganic composite layer on the negative electrode sheet of the battery, the problems of short cycle life and lithium dendrite formation of lithium metal batteries are solved, and battery performance with high energy density and long cycle life is achieved.

WO2024217008A1PCT designated stage expired Publication Date: 2024-10-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/137467
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2023-12-08
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Traditional batteries using carbon-based materials as negative electrodes have shortcomings in energy density and cycle life. Although lithium metal batteries have high energy density, they have short cycle life and are prone to the formation of lithium dendrites, leading to the risk of short circuits.

Method used

The negative electrode sheet is used, including a negative electrode matrix and an organic-inorganic composite layer. The composite layer is composed of polymer and lithium inorganic components (such as LiI, LiF, Li2S, Li3N). It is formed through in-situ reaction to enhance the peeling strength and the negative electrode matrix. Elastic modulus, regulates lithium metal deposition behavior and reduces lithium dendrite formation.

Benefits of technology

It improves the Coulombic efficiency, energy density and cycle life of the battery, reduces the probability of lithium dendrites penetrating the isolation film, and improves the reliability and cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023137467_24102024_PF_FP_ABST
    Figure CN2023137467_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present application are a negative electrode sheet and a preparation method therefor, a battery cell, a battery and an electric device. The negative electrode sheet comprises a negative electrode matrix and an organic-inorganic composite layer, which is located on at least one surface of the negative electrode matrix. The negative electrode matrix comprises a first matrix layer close to the organic-inorganic composite layer, wherein the first matrix layer comprises a first metal material, the first metal material comprising one or more of lithium elementary substance and a lithium alloy. The organic-inorganic composite layer comprises a polymer and a first inorganic component, wherein the first inorganic component comprises one or more of LiI, LiF, Li2S, Li3N and Li3P. The peel strength between the organic-inorganic composite layer and the negative electrode matrix is greater than or equal to 500 N / m.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode sheet, preparation method thereof, battery cell, battery and electrical device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310423012.4 filed on April 19, 2023, entitled “Negative electrode sheet, preparation method thereof, battery cell, battery and electrical device,” the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to a negative electrode plate, a preparation method thereof, a battery cell, a battery and an electrical device. Background Art

[0004] In recent years, batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as in smart phones, tablet computers, smart wearables, power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. With the application and promotion of batteries, the energy density of traditional batteries with carbon-based materials as negative electrodes can no longer meet the demand, so a battery system with higher energy density is needed. Batteries with materials such as lithium metal as negative electrodes have high energy density, but the cycle life of the battery is short. The above statements are only used to provide background technical information related to this application and do not necessarily constitute prior art.

[0005] Summary of the Invention

[0006] The present application provides a negative electrode plate, a preparation method thereof, a battery cell, a battery and an electrical device, which can enable the battery to have a long cycle life.

[0007] In a first aspect, the present application provides a negative electrode plate, comprising a negative electrode substrate and an organic-inorganic composite layer located on at least one surface of the negative electrode substrate; the negative electrode substrate comprises a first substrate layer close to the organic-inorganic composite layer, the first substrate layer comprises a first metal material, the first metal material comprises one or more of lithium element and lithium alloy; the organic-inorganic composite layer comprises a polymer and a first inorganic component, the first inorganic component comprises one or more of LiI, LiF, Li2S, Li3N, and Li3P; the peel strength between the organic-inorganic composite layer and the negative electrode substrate is greater than or equal to 500 N / m.

[0008] The organic-inorganic composite layer of the negative electrode provided in the embodiment of the present application is dense and uniform, has a uniform ion field, and has the function of regulating the deposition behavior of lithium metal. It can be tightly combined with the negative electrode matrix, and can also have good elasticity, a suitable electrolyte swelling rate, a high ionic conductivity, and a high elastic modulus. Therefore, the negative electrode provided in the embodiment of the present application can reduce side reactions, reduce the consumption of electrolyte and the first metal material, reduce the capacity loss of the battery, and can also reduce the volume expansion of the negative electrode side during the charging process, so that the battery has high coulombic efficiency, high energy density, and long cycle life; in addition, it can also reduce the formation of lithium dendrites, reduce the probability of lithium dendrites penetrating the isolation membrane, reduce the probability of battery short circuit, and improve the reliability of the battery.

[0009] In any embodiment, the peel strength between the organic-inorganic composite layer and the negative electrode substrate is 600 N / m-3200 N / m, and optionally 800 N / m-2800 N / m. This can effectively reduce the volume expansion of the negative electrode during charging and reduce the probability of the organic-inorganic composite layer peeling from the negative electrode substrate surface, thereby ensuring the long-term function of the organic-inorganic composite layer and extending the cycle life of the battery.

[0010] In any embodiment, the elastic modulus of the organic-inorganic composite layer is 0.1 MPa-70 MPa, and can be optionally 19 MPa-53 MPa. When the elastic modulus of the organic-inorganic composite layer is within the above range, the probability of lithium dendrites penetrating the separator can be reduced, the probability of battery short circuit can be reduced, and the reliability of the battery can be improved.

[0011] In any embodiment, the elastic deformation of the organic-inorganic composite layer is 7%-700%, and optionally 9%-310%. When the elastic deformation of the organic-inorganic composite layer is within the above range, it is beneficial to accommodate the volume expansion of the negative electrode during charging, reduce the probability of fracture or cracking of the organic-inorganic composite layer, thereby ensuring the long-term function of the organic-inorganic composite layer and extending the cycle life of the battery.

[0012] In any embodiment, the organic-inorganic composite layer has an electrolyte swelling rate of 9%-60% at 25°C, and can optionally be 11%-38%. When the electrolyte swelling rate of the organic-inorganic composite layer is within the above range, it can promote efficient ion transfer within the organic-inorganic composite layer and at the interface with the negative electrode substrate, which is beneficial to improving the cycle performance and kinetic performance of the battery.

[0013] In any embodiment, the ionic conductivity of the organic-inorganic composite layer at 25° C. is 0.001 mS / cm-5 mS / cm, and can optionally be 0.03 mS / cm-3.4 mS / cm. When the ionic conductivity of the organic-inorganic composite layer is within the above range, it facilitates efficient ion transfer within the organic-inorganic composite layer and at the interface with the negative electrode substrate, thereby improving the cycling performance and kinetic performance of the battery.

[0014] In any embodiment, the thickness of the organic-inorganic composite layer is 0.005 μm-10 μm, and can be optionally 0.02 μm-5 μm. When the thickness of the organic-inorganic composite layer is within the above range, side reactions can be reduced, the consumption of the electrolyte and the first metal material can be reduced, and the capacity loss of the battery can be reduced, so that the battery has high coulombic efficiency, high energy density and long cycle life. It can also regulate the effect of lithium metal deposition behavior, reduce lithium dendrite formation, reduce the probability of lithium dendrites penetrating the isolation membrane, reduce the probability of battery short circuit, and improve battery reliability. In addition, it can also make the negative electrode sheet have higher ionic conductivity and lower interface impedance, which is beneficial to improving the cycle performance and kinetic performance of the battery.

[0015] In any embodiment, the organic-inorganic composite layer includes a first surface proximal to the negative electrode substrate and a second surface distal to the negative electrode substrate. The mass content of the first inorganic component at the first surface is denoted as W1, and the mass content of the first inorganic component at the second surface is denoted as W2. Thus, W1>W2. This can enhance the regulatory effect of the organic-inorganic composite layer on lithium metal deposition behavior and further reduce lithium dendrite formation.

[0016] In any embodiment, based on the total weight of the organic-inorganic composite layer, the content of the polymer in the organic-inorganic composite layer is denoted as a, and the content of the first inorganic component is denoted as b, then a:b is 1:5-5:1, optionally 1:3-3:1. When the weight ratio of the polymer to the first inorganic component is within the above range, the organic-inorganic composite layer can have a high elastic modulus, high elastic deformation, and high ionic conductivity. It can also reduce the volume expansion of the negative electrode during charging, reduce the formation of lithium dendrites, and improve the cycle performance of the battery.

[0017] In any embodiment, based on the total weight of the organic-inorganic composite layer, the content of the polymer in the organic-inorganic composite layer is denoted as a, and a is 8 wt % to 80 wt %, and can be optionally 14 wt % to 71 wt %.

[0018] In any embodiment, based on the total weight of the organic-inorganic composite layer, the content of the first inorganic component in the organic-inorganic composite layer is denoted as b, and b is 8 wt %-80 wt %, and can be optionally 14 wt %-71 wt %.

[0019] In any embodiment, the organic-inorganic composite layer further includes a second inorganic component.

[0020] In any embodiment, the second inorganic component includes one or more of a lithium salt and a solid electrolyte, thereby adjusting the elastic modulus and / or ionic conductivity of the organic-inorganic composite layer, thereby improving the cycle performance and / or kinetic performance of the battery.

[0021] In any embodiment, based on the total weight of the organic-inorganic composite layer, the total content of the second inorganic component in the organic-inorganic composite layer is denoted as c, where c is greater than 0 and less than or equal to 55 wt %, and can optionally be 5 wt % to 50 wt %. When the total content of the second inorganic component is within the above range, one or more of the elastic modulus, ionic conductivity, electrolyte swelling, and elastic deformation of the organic-inorganic composite layer can be adjusted, thereby improving the cycling performance and / or kinetic performance of the battery.

[0022] In any embodiment, the lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), lithium tetrafluorooxalatophosphate, lithium difluorophosphate, and lithium trifluoromethanesulfonate.

[0023] In any embodiment, the solid electrolyte includes one or more of an oxide-type inorganic solid electrolyte, a sulfide-type inorganic solid electrolyte and a halide-type inorganic solid electrolyte. Optionally, the oxide-type inorganic solid electrolyte includes one or more of a NASICON-type solid electrolyte, a garnet-type solid electrolyte, a perovskite-type solid electrolyte and a LISICON-type solid electrolyte. Optionally, the sulfide-type inorganic solid electrolyte includes one or more of a sulfide-type crystalline solid electrolyte and a sulfide glass-type solid electrolyte.

[0024] In any embodiment, the organic-inorganic composite layer further includes a third inorganic component.

[0025] In any embodiment, the third inorganic component includes one or more of a film-forming additive and an inorganic filler. This can improve the quality of the negative electrode film and adjust one or more of the elastic modulus, ionic conductivity, electrolyte swelling, and elastic deformation of the organic-inorganic composite layer, thereby improving the cycling performance and / or kinetic performance of the battery.

[0026] In any embodiment, based on the total weight of the organic-inorganic composite layer, the total content of the third inorganic component in the organic-inorganic composite layer is denoted as d, and d is greater than 0 and less than or equal to 20 wt %.

[0027] In any embodiment, the film-forming additive includes one or more of fluoroethylene carbonate, vinylene carbonate, ethylene carbonate, vinyl sulfate, propylene sulfite, vinyl sulfite, diethyl sulfite, dimethyl sulfite, butane sultone, and tris(trimethylsilyl)phosphate.

[0028] In any embodiment, the inorganic filler includes one or more of boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, magnesium aluminum silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate, and barium titanate.

[0029] In any embodiment, the volume distribution particle size Dv50 of the first inorganic component is less than or equal to 80 nm, and can be optionally 10 nm to 30 nm, thereby reducing the interfacial impedance of the battery and improving the cycle performance and / or kinetic performance of the battery.

[0030] In any embodiment, the polymer includes one or more of a polymer having high viscosity, a polymer having ion-conducting function, and a polymer capable of reacting with the first metal material.

[0031] In any embodiment, the polymer includes one or more of poly(meth)acrylate, polyurethane, natural rubber, polyisoprene, polystyrene, polyether, polyethylene oxide, polycarbonate, polymethyl methacrylate, ionomer, polyacrylonitrile, polycyanoacrylate, poly(meth)acrylic acid, hydrogenated nitrile rubber, polyvinyl alcohol, and their respective derivatives.

[0032] In any embodiment, the first substrate layer further comprises a first negative electrode active material. Optionally, the first negative electrode active material comprises a carbon-based material, and more optionally comprises one or more of graphite and hard carbon.

[0033] In any embodiment, the negative electrode substrate further includes a negative electrode current collector layer away from the organic-inorganic composite layer, and the first substrate layer is located on at least one surface of the negative electrode current collector layer.

[0034] In any embodiment, the negative electrode substrate further includes a second negative electrode active material layer located between the first substrate layer and the negative electrode current collector layer, and the second negative electrode active material layer includes a second negative electrode active material.

[0035] In any embodiment, the second negative electrode active material includes one or more of a carbon-based material, lithium titanate, and a silicon-based material.

[0036] In a second aspect, the present application provides a method for preparing a negative electrode plate, comprising the following steps: providing a negative electrode substrate, wherein the negative electrode substrate includes a first substrate layer, wherein the first substrate layer includes a first metal material, and the first metal material includes one or more of lithium element and lithium alloy; providing a first reaction component, wherein the first reaction component includes one or more of I2, S, N2, and P; causing the first reaction component to contact and react with the first metal material in the first substrate layer to in situ form a first inorganic component on the surface of the first substrate layer, wherein the first inorganic component includes one or more of LiI, LiF, Li2S, Li3N, and Li3P; providing a coating solution, wherein the coating solution includes a polymer and / or a monomer for forming a polymer; coating the coating solution on the surface of the first substrate layer, and forming an organic-inorganic composite layer after the reaction to obtain a negative electrode plate, wherein the reaction includes at least one of a reaction between the polymer and the first metal material and / or the first inorganic component and an in situ polymerization reaction of the monomer.

[0037] The first inorganic particles and polymers in the organic-inorganic composite layer formed by the preparation method provided in the embodiment of the present application can be uniformly compounded, and the formed organic-inorganic composite layer is more dense and uniform, which can reduce the formation of lithium dendrites, reduce the contact between the electrolyte and the first metal material in the negative electrode matrix, reduce side reactions, and reduce the consumption of the electrolyte and the first metal material, thereby reducing the capacity loss of the battery; it can also reduce the volume expansion of the negative electrode side during the charging process, so that the battery has high coulomb efficiency, high energy density and long cycle life; at the same time, the elastic modulus of the organic-inorganic composite layer is also improved, thereby reducing the probability of lithium dendrites penetrating the isolation membrane, reducing the probability of battery short circuit, and improving the reliability of the battery.

[0038] In any embodiment, a method of causing the first reaction component to contact and react with the first metal material in the first base layer includes evaporation, which may be vacuum evaporation or physical evaporation.

[0039] In any embodiment, the first reaction component is in vapor form.

[0040] The first inorganic component is obtained by an in-situ reaction between steam and the first metal material, thereby making the particles of the first inorganic component more nano-sized, dense and uniform.

[0041] In any embodiment, the reaction temperature when the first reactive component is contacted and reacted with the first metal material in the first base layer is 30° C.-200° C., and can be optionally 50° C.-180° C.

[0042] In any embodiment, the reaction time when the first reactive component is in contact with the first metal material in the first base layer is less than or equal to 5 hours, and can be optionally less than or equal to 2 hours.

[0043] In any embodiment, the coating solution further includes one or more of an initiator, a lithium salt, and a solid electrolyte.

[0044] A third aspect of the present application provides a battery cell, comprising an electrode assembly, wherein the electrode assembly comprises the negative electrode sheet according to the first aspect of the present application or the negative electrode sheet prepared by the method according to the second aspect of the present application.

[0045] A fourth aspect of the present application provides a battery, comprising the battery cell of the third aspect of the present application.

[0046] A fifth aspect of the present application provides an electrical device comprising the battery of the fourth aspect of the present application.

[0047] The electric device provided in the present application includes the battery provided in the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.

[0049] FIG1 is a schematic diagram of a battery cell according to an embodiment of the present application.

[0050] FIG2 is an exploded schematic diagram of an embodiment of a battery cell of the present application.

[0051] FIG3 is a schematic diagram of an embodiment of a battery module of the present application.

[0052] FIG4 is a schematic diagram of an embodiment of a battery pack of the present application.

[0053] FIG. 5 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 4 .

[0054] FIG6 is a schematic diagram of an embodiment of a negative electrode sheet of the present application.

[0055] FIG7 is a schematic diagram of another embodiment of the negative electrode sheet of the present application.

[0056] FIG8 is a schematic diagram of another embodiment of the negative electrode sheet of the present application.

[0057] FIG9 is a schematic diagram of another embodiment of the negative electrode sheet of the present application.

[0058] FIG10 is a schematic diagram of another embodiment of the negative electrode sheet of the present application.

[0059] FIG11 is a schematic diagram of an embodiment of an electric device including the battery of the present application as a power source.

[0060] In the accompanying drawings, which are not necessarily drawn to scale, the reference numerals are as follows: 1, battery pack; 2, upper housing; 3, lower housing; 4, battery module; 5, battery cell; 51, housing; 52, electrode assembly; 53, cover plate; 10, negative electrode sheet; 101, negative electrode substrate; 102, organic-inorganic composite layer; 1011, first substrate layer; 1012, negative electrode current collector layer; 1013, second negative electrode active material layer. DETAILED DESCRIPTION

[0061] Below, with appropriate reference to the accompanying drawings, the embodiments of the negative electrode sheet, its preparation method, battery cell, battery and electrical device of the present application are described in detail. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0062] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0063] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.

[0064] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.

[0065] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0066] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0067] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0068] Unless otherwise specified, in this application, the terms "first", "second", etc. are used to distinguish different objects rather than to describe a specific order or a primary-secondary relationship.

[0069] Unless otherwise specified, the terms used in this application have the common meanings that are commonly understood by those skilled in the art.

[0070] Unless otherwise specified, the values ​​of the parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods provided in this application. Unless otherwise specified, the test temperature for each parameter is 25°C.

[0071] In the present application, the term "monomers for forming a polymer" includes both monomers and oligomers.

[0072] The battery mentioned in the embodiments of this application refers to a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in this application may include a battery cell, a battery module or a battery pack.

[0073] A battery cell is the smallest unit of a battery, independently capable of charging and discharging. A battery cell can be cylindrical, flat, rectangular, or in other shapes, though this is not a limitation in the present invention. Figure 1 shows a battery cell 5 with a rectangular structure as an example.

[0074] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed series via a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a housing and battery cells, with the battery cells or battery modules housed in the housing. In some embodiments, the housing may serve as part of the vehicle's chassis structure. For example, a portion of the housing may form at least a portion of the vehicle's floor, or a portion of the housing may form at least a portion of the vehicle's crossbeam or longitudinal beam.

[0075] In some embodiments, the battery may be an energy storage device, including an energy storage container, an energy storage cabinet, and the like.

[0076] The battery cells mentioned in the embodiments of the present application include battery cells using metallic lithium and its alloys as negative electrode active materials. For example, the battery cells provided in the embodiments of the present application may include lithium metal battery cells, lithium air battery cells, lithium sulfur battery cells, etc., but the embodiments of the present application are not limited to this.

[0077] A battery cell generally includes an electrode assembly. The electrode assembly generally includes a positive electrode sheet, a negative electrode sheet, and a separator located between the positive and negative electrode sheets. The electrode assembly can be a wound structure or a laminated structure, which is not limited in the present embodiment.

[0078] The battery cell may also include an outer packaging that can be used to encapsulate the electrode assembly and electrolyte. The outer packaging can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging can also be a soft package, such as a bag-type soft package. The soft package can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0079] In some embodiments, as shown in Figure 2, the outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, which together form a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 is used to cover the opening, thereby sealing the receiving cavity. The electrode assembly 52 is enclosed in the receiving cavity. The number of electrode assemblies 52 contained in a battery cell 5 can be one or more, and can be adjusted according to needs.

[0080] In some embodiments, battery cells can be assembled into a battery module. The number of battery cells contained in a battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module. Figure 3 is a schematic diagram of a battery module 4 as an example. As shown in Figure 3, in the battery module 4, multiple battery cells 5 can be arranged in sequence along the length of the battery module 4. Of course, they can also be arranged in any other manner. The multiple battery cells 5 can further be fixed by fasteners.

[0081] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.

[0082] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0083] Figures 4 and 5 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a housing and multiple battery modules 4 disposed within the housing. The housing comprises an upper housing 2 and a lower housing 3. The upper housing 2 covers the lower housing 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the housing.

[0084] High energy density is an irreversible trend in future battery development. Lithium metal batteries have attracted widespread attention due to their high energy density. However, their large-scale application faces many challenges. For example, lithium metal is highly reactive and easily undergoes side reactions with the electrolyte, which consumes the electrolyte and lithium and produces a thick passivation layer, resulting in rapid capacity decay and a short cycle life after battery cycling. In addition, during the charging process, regional differences in ion and electron flow can easily lead to uneven deposition on the negative electrode surface, which can easily form lithium dendrites. On the one hand, lithium dendrites have a high specific surface area, which can exacerbate electrolyte consumption and even cause battery failure. On the other hand, the rapid growth of lithium dendrites can also penetrate the separator, increasing the risk of battery short circuits.

[0085] In view of this, the inventors improved the negative electrode plate.

[0086] Figures 6 to 10 are schematic diagrams of different embodiments of the negative electrode plate of the present application. Referring to Figures 6 to 10, the negative electrode plate 10 provided in the embodiment of the present application includes a negative electrode substrate 101 and an organic-inorganic composite layer 102 located on at least one surface of the negative electrode substrate 101. The negative electrode substrate 101 includes a first substrate layer 1011 adjacent to the organic-inorganic composite layer 102. The first substrate layer 1011 includes a first metal material, and the first metal material includes one or more of lithium elemental and lithium alloy. The organic-inorganic composite layer 102 includes a polymer and a first inorganic component, and the first inorganic component includes one or more of LiI, LiF, Li2S, Li3N, and Li3P. The peel strength between the organic-inorganic composite layer 102 and the negative electrode substrate 101 is greater than or equal to 500N / m.

[0087] The first inorganic component in the organic-inorganic composite layer includes one or more of LiI, LiF, Li2S, Li3N, and Li3P. These inorganic components have the function of uniform ion field and regulating lithium metal deposition behavior, thereby reducing the formation of lithium dendrites, reducing the volume expansion of the negative electrode side during the charging process, and reducing the probability of fracture or cracking of the organic-inorganic composite layer due to lithium dendrite growth or interface displacement. The first inorganic component in the organic-inorganic composite layer can also reduce the probability of sharp-shaped lithium dendrites forming during the charging and discharging process, and can reduce the probability of lithium dendrites penetrating the isolation membrane, thereby reducing the probability of battery short circuit and improving battery reliability. In addition, the first inorganic component can regulate the swelling behavior of the organic-inorganic composite layer in the electrolyte, improve the ionic conductivity of the organic-inorganic composite layer, reduce the interfacial impedance of the battery, and promote the efficient transfer of ions within the organic-inorganic composite layer and at the interface with the negative electrode substrate.

[0088] The polymer in the organic-inorganic composite layer can fill the gaps between the particles of the first inorganic component, making the organic-inorganic composite layer more dense and uniform. This can reduce contact between the electrolyte and the first metal material in the first matrix layer, reduce side reactions, and reduce the consumption of the electrolyte and the first metal material, thereby reducing the battery's capacity loss and enabling the battery to have high coulombic efficiency and high energy density. The polymer also imparts good elasticity to the organic-inorganic composite layer, which helps to accommodate the volume expansion of the negative electrode during charging and reduces the probability of fracture or cracking of the organic-inorganic composite layer. This can ensure the long-term function of the organic-inorganic composite layer and extend the battery's cycle life.

[0089] The organic-inorganic composite layer includes a polymer and a first inorganic component, thereby enabling the organic-inorganic composite layer to have a suitable electrolyte swelling rate and a high ionic conductivity, thereby facilitating the efficient transfer of ions within the organic-inorganic composite layer and at the interface with the negative electrode matrix; the organic-inorganic composite layer can also have a high elastic modulus, reducing the probability of lithium dendrites penetrating the isolation membrane, reducing the probability of battery short circuit, and improving battery reliability.

[0090] The peel strength between the organic-inorganic composite layer and the negative electrode substrate is greater than or equal to 500N / m, so that the organic-inorganic composite layer is tightly bonded to the negative electrode substrate, which can reduce the volume expansion of the negative electrode side during the charging process, and can also reduce the probability of the organic-inorganic composite layer peeling from the surface of the negative electrode substrate, thereby allowing the organic-inorganic composite layer to play its role for a long time and extending the cycle life of the battery.

[0091] The organic-inorganic composite layer of the negative electrode provided in the embodiment of the present application is dense and uniform, has a uniform ion field, and has the function of regulating the deposition behavior of lithium metal. It can be tightly combined with the negative electrode matrix, and can also have good elasticity, a suitable electrolyte swelling rate, a high ionic conductivity, and a high elastic modulus. Therefore, the negative electrode provided in the embodiment of the present application can reduce side reactions, reduce the consumption of electrolyte and the first metal material, reduce the capacity loss of the battery, and can also reduce the volume expansion of the negative electrode side during the charging process, so that the battery has high coulombic efficiency, high energy density, and long cycle life; in addition, it can also reduce the formation of lithium dendrites, reduce the probability of lithium dendrites penetrating the isolation membrane, reduce the probability of battery short circuit, and improve the reliability of the battery.

[0092] In some embodiments, the peel strength between the organic-inorganic composite layer 102 and the negative electrode substrate 101 can be 600N / m-3200N / m, optionally 800N / m-2800N / m, 800N / m-2550N / m, 800N / m-2400N / m, 1200N / m-2800N / m, 1200N / m-2550N / m, 1200N / m-2400N / m, 1500N / m-2800N / m, 1500N / m-2550N / m, 1500N / m-2400N / m, 1700N / m-2800N / m, 1700N / m-2550N / m, 1700N / m-2400N / m. This can better reduce the volume expansion of the negative electrode side during the charging process and reduce the probability of the organic-inorganic composite layer peeling off from the surface of the negative electrode substrate, so that the organic-inorganic composite layer can play its role for a long time and extend the cycle life of the battery.

[0093] In some embodiments, the elastic modulus of the organic-inorganic composite layer 102 may be 0.1 MPa-70 MPa, optionally 0.5 MPa-55 MPa, 1 MPa-55 MPa, 10 MPa-55 MPa, 15 MPa-55 MPa, 19 MPa-55 MPa, 0.5 MPa-53 MPa, 1 MPa-53 MPa, 10 MPa-53 MPa, 15 MPa-53 MPa, 19 MPa-53 MPa, 0.5 MPa-45 MPa, 1 MPa-45 MPa, 10 MPa-45 MPa, 15 MPa-45 MPa, 19 MPa-45 MPa. When the elastic modulus of the organic-inorganic composite layer is within the above range, the probability of lithium dendrites penetrating the isolation membrane can be reduced, the probability of battery short circuit can be reduced, and the reliability of the battery can be improved.

[0094] In some embodiments, the elastic deformation of the organic-inorganic composite layer 102 can be 7%-700%, optionally 9%-700%, 9%-600%, 9%-500%, 9%-400%, 9%-310%, 21%-700%, 21%-600%, 21%-500%, 21%-400%, 21%-310%, 30%-700%, 30%-600%, 30%-500%, 30%-400%, 30%-310%, 50%-700%, 50%-600%, 50%-500%, 50%-400%, 50%-310%, 80%-700%, 80%-600%, 80%-500%, 80%-400%, 80%-310%. When the elastic deformation of the organic-inorganic composite layer is within the above range, it is conducive to compatibility with the volume expansion of the negative electrode side during charging, reducing the probability of breakage or cracking of the organic-inorganic composite layer, thereby enabling the organic-inorganic composite layer to play its role for a long time and extending the cycle life of the battery.

[0095] In some embodiments, the 25°C electrolyte swelling ratio of the organic-inorganic composite layer 102 may be 9%-60%, optionally 11%-60%, 11%-50%, 11%-38%, 13%-60%, 13%-50%, 13%-38%, 15%-60%, 15%-50%, or 15%-38%. When the electrolyte swelling ratio of the organic-inorganic composite layer is within the above range, efficient ion transfer within the organic-inorganic composite layer and at the interface with the negative electrode substrate can be promoted, thereby improving the cycle performance and kinetic performance of the battery.

[0096] In some embodiments, the ionic conductivity of the organic-inorganic composite layer 102 at 25° C. may be 0.001 mS / cm-5 mS / cm, optionally 0.03 mS / cm-5 mS / cm, 0.03 mS / cm-4 mS / cm, 0.03 mS / cm-3.4 mS / cm, 0.07 mS / cm-5 mS / cm, 0.07 mS / cm-4 mS / cm, 0.07 mS / cm-3.4 mS / cm, 0.1 mS / cm-5 mS / cm, 0.1 mS / cm-4 mS / cm, or 0.1 mS / cm-3.4 mS / cm. When the ionic conductivity of the organic-inorganic composite layer is within the above range, it is beneficial to the efficient transfer of ions within the organic-inorganic composite layer and at the interface with the negative electrode substrate, thereby improving the cycle performance and kinetic performance of the battery.

[0097] In some embodiments, the thickness of the organic-inorganic composite layer 102 may be 0.005 μm-10 μm, optionally 0.02 μm-8 μm, 0.02 μm-5 μm, 0.02 μm-3 μm, 0.05 μm-8 μm, 0.05 μm-5 μm, 0.05 μm-3 μm, 0.08 μm-8 μm, 0.08 μm-5 μm, 0.08 μm-3 μm, 0.1 μm-8 μm, 0.1 μm-5 μm, 0.1 μm-3 μm. When the thickness of the organic-inorganic composite layer is within the above range, side reactions can be reduced, the consumption of the electrolyte and the first metal material can be reduced, the capacity loss of the battery can be reduced, and the battery can have high coulombic efficiency, high energy density and long cycle life. It can also regulate the effect of lithium metal deposition behavior, reduce lithium dendrite formation, reduce the probability of lithium dendrites penetrating the isolation membrane, reduce the probability of battery short circuit, and improve battery reliability; in addition, it can also make the negative electrode plate have higher ionic conductivity and lower interface impedance, which is beneficial to improving the cycle performance and kinetic performance of the battery.

[0098] The thickness of the organic-inorganic composite layer 102 refers to the thickness of the organic-inorganic composite layer 102 located on one surface of the negative electrode substrate 101 .

[0099] In some embodiments, the organic-inorganic composite layer 102 includes a first surface proximal to the negative electrode substrate 101 and a second surface distal to the negative electrode substrate 101. The mass content of the first inorganic component at the first surface is denoted as W1, and the mass content of the first inorganic component at the second surface is denoted as W2. Thus, W1>W2. This can enhance the regulatory effect of the organic-inorganic composite layer on lithium metal deposition behavior and further reduce lithium dendrite formation.

[0100] In some embodiments, based on the total weight of the organic-inorganic composite layer 102, the content of the polymer in the organic-inorganic composite layer 102 is denoted as a, and the content of the first inorganic component is denoted as b. Then, a:b can be 1:8-8:1, optionally 1:5-5:1, and more optionally 1:3-3:1. When the weight ratio of the polymer to the first inorganic component is within the above range, one or more of the elastic modulus, elastic deformation, electrolyte swelling rate, and ionic conductivity of the organic-inorganic composite layer can be adjusted, so that the organic-inorganic composite layer has a high elastic modulus, high elastic deformation, and high ionic conductivity. It can also reduce the volume expansion of the negative electrode side during the charging process, reduce the formation of lithium dendrites, and improve the cycle performance of the battery.

[0101] In some embodiments, a may be 8 wt%-80 wt%, optionally 9.5 wt%-75 wt%, 14 wt%-71 wt%.

[0102] In some embodiments, b may be 8 wt%-80 wt%, optionally 9.5 wt%-75 wt%, 14 wt%-71 wt%.

[0103] In some embodiments, the polymer may include one or more of a polymer having high viscosity, a polymer having an ion-conducting function, and a polymer that can react with the first metal material.

[0104] In some embodiments, the polymer reactive with the first metal material may include at least one functional group selected from the group consisting of -OH, -COOH, -CN, and -SO3H. This can increase the peel strength between the organic-inorganic composite layer and the negative electrode substrate, reduce volume expansion on the negative electrode side during charging, and reduce the probability of the organic-inorganic composite layer peeling from the negative electrode substrate surface, thereby ensuring the long-term function of the organic-inorganic composite layer and extending the cycle life of the battery.

[0105] In some embodiments, the polymer having high viscosity may include one or more of poly(meth)acrylate, polyurethane, natural rubber, polyisoprene, polystyrene, and derivatives thereof.

[0106] In some embodiments, the polymer having ion-conducting functionality may include one or more of polyether, polyethylene oxide, polycarbonate, polymethyl methacrylate, ionomer, and derivatives thereof.

[0107] In some embodiments, the polymer reactive with the first metal material may include one or more of polyacrylonitrile, polycyanoacrylate, poly(meth)acrylic acid, hydrogenated nitrile rubber, polyvinyl alcohol, and derivatives thereof.

[0108] Derivatives generally refer to products derived from the replacement of hydrogen atoms or atomic groups in a polymer by other atoms or atomic groups (eg, -OH, -COOH, -CN, -SO3H, etc.).

[0109] Of course, the above polymers may also have multiple functions at the same time. For example, polycyanoacrylate can react with the first metal material and also have high viscosity.

[0110] In some embodiments, the organic-inorganic composite layer 102 may further include a second inorganic component.

[0111] In some embodiments, the second inorganic component may include one or more of a lithium salt and a solid electrolyte, thereby adjusting the elastic modulus and / or ionic conductivity of the organic-inorganic composite layer, thereby improving the cycle performance and / or kinetic performance of the battery.

[0112] In some embodiments, based on the total weight of the organic-inorganic composite layer 102, the total content of the second inorganic component in the organic-inorganic composite layer 102 is denoted as c. c can be greater than 0 and less than or equal to 55 wt%, and can optionally be 3 wt%-50 wt%, 5 wt%-50 wt%, 3 wt%-40 wt%, 5 wt%-40 wt%, 3 wt%-30 wt%, 5 wt%-30 wt%, 3 wt%-20 wt%, or 5 wt%-20 wt%. When the total content of the second inorganic component is within the above range, one or more of the elastic modulus, ionic conductivity, electrolyte swelling, and elastic deformation of the organic-inorganic composite layer can be adjusted, thereby improving the cycle performance and / or kinetic performance of the battery.

[0113] In some embodiments, the lithium salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium bisoxalatoborate (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium difluorobisoxalatophosphate (LiDFOP), lithium tetrafluorooxalatophosphate (LiTFOP), lithium difluorophosphate (LiPO2F2), and lithium trifluoromethanesulfonate (LiTFS).

[0114] In some embodiments, the solid electrolyte may include one or more of an oxide-type inorganic solid electrolyte, a sulfide-type inorganic solid electrolyte, and a halide-type inorganic solid electrolyte.

[0115] In some embodiments, the oxide-type inorganic solid electrolyte may include one or more of a NASICON-type solid electrolyte, a garnet-type solid electrolyte, a perovskite-type solid electrolyte, and a LISICON-type solid electrolyte.

[0116] In some embodiments, the sulfide-based inorganic solid electrolyte may include one or more of a sulfide-based crystalline solid electrolyte and a sulfide glass-based solid electrolyte.

[0117] In some embodiments, the solid electrolyte may include lithium titanium phosphate (Li y , y , z , x , y , 16 , 10 , 12 , 11 , 12 , y , x , z , x , 14 , 12 Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, LATP, 0 < x < 2, 0 < y < 1, 0 < z < 3), lithium aluminum germanium phosphate (Li x Al y Ge z (PO4)3, LAGP, 0 < x < 2, 0 < y < 1, 0 < z < 3), lithium aluminum zirconium phosphate (Li x Al y Zr z (PO4)3, LAZP, 0 < x < , 0 < y < 1, 0 < z < 3), lithium aluminum chromium phosphate (Li<0000,012Al y Cr z (PO4)3, LACP, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y -type glass (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, < 0 < x < 2, 0 < y < 3), lithium lanthanum zirconium oxide (Li7La3Zr2O 12 , LLZO), lithium lanthanum thallium oxide (Li5La3Ta2O 12 , LLTA), lithium zinc germanium oxide (Li 14 ZnGe4O 16 ), lithium thiargyrite electrolyte Li6PS5X (X includes one or more selected from Cl, Br, I), SiS2-type glass (Li x [[ID=]]Si<00000,24S z , 0 < x < 3, 0 < y < 2, 0 < z < 4), P2S5-type glass (Li<,0000026P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7), Li3PS4, Li7P3S 11 , Li 10 GeP2S 12, and one or more of their respective dopant compounds. Dopant compounds are typically obtained by doping a compound with another element, such as a metal element. The type of dopant element is not particularly limited, as long as it does not detract from the subject matter of this application.

[0118] In some embodiments, the organic-inorganic composite layer 102 may further include a third inorganic component.

[0119] In some embodiments, the third inorganic component may include one or more of a film-forming additive and an inorganic filler. This can improve the quality of the negative electrode film and adjust one or more of the elastic modulus, ionic conductivity, electrolyte swelling, and elastic deformation of the organic-inorganic composite layer, thereby improving the battery's cycling performance and / or kinetic performance.

[0120] In some embodiments, based on the total weight of the organic-inorganic composite layer 102 , the total content of the third inorganic component in the organic-inorganic composite layer 102 is denoted as d, and d is greater than 0 and less than or equal to 20 wt %.

[0121] In some embodiments, the film-forming additive may include one or more of fluoroethylene carbonate, vinylene carbonate, vinyl ethylene carbonate, vinyl sulfate, propylene sulfite, vinyl sulfite, diethyl sulfite, dimethyl sulfite, butane sultone, and tris(trimethylsilyl)phosphate.

[0122] In some embodiments, the inorganic filler may include one or more of boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, magnesium aluminum silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate, and barium titanate.

[0123] In some embodiments, the volume distribution particle size Dv50 of the first inorganic component may be less than or equal to 80 nm, and may be 10 nm to 30 nm, thereby reducing the interfacial impedance of the battery and improving the cycle performance and / or kinetic performance of the battery.

[0124] The volume distribution particle size Dv50 is well known in the art and represents the particle size corresponding to the cumulative volume distribution percentage of a material reaching 50%. It can be measured using instruments and methods known in the art. For example, it can be measured using a laser particle size analyzer in accordance with GB / T 19077-2016. The testing instrument can be the Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd. in the UK.

[0125] In some embodiments, the first base layer 1011 may be a lithium sheet (foil) or a lithium alloy sheet (foil).

[0126] Lithium alloys may be alloys of metallic lithium and other metallic elements or non-metallic elements. For example, the other metallic elements in the lithium alloy may include one or more of silver, magnesium, aluminum, gold, platinum, zinc, tin, copper, nickel, titanium, gallium, and indium, and the non-metallic elements in the lithium alloy may include one or more of boron, carbon, and silicon.

[0127] In some embodiments, the first base layer 1011 may further include a first negative electrode active material.

[0128] In some embodiments, the first negative electrode active material may include a carbon-based material, optionally including one or more of graphite and hard carbon.

[0129] In some embodiments, the first base layer 1011 may further include a binder to bond the first metal material and the first negative electrode active material together. The present application does not particularly limit the type of binder. As an example, the binder may include one or more of styrene-butadiene rubber (SBR), acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA), polyvinylidene fluoride (PVDF), polyurethane (PU), polyvinylidene fluoride-hexafluoropropylene, polyacrylate, and polyethylene oxide.

[0130] In some embodiments, the negative electrode plate 10 includes a negative electrode substrate 101 and an organic-inorganic composite layer 102 located on at least one surface of the negative electrode substrate 101. The negative electrode substrate 101 includes a first substrate layer 1011 adjacent to the organic-inorganic composite layer 102. The first substrate layer 1011 includes a first metal material, which includes one or more of lithium and a lithium alloy. The organic-inorganic composite layer 102 includes a polymer, a first inorganic component, and a second inorganic component. The first inorganic component includes one or more of LiI, LiF, Li2S, Li3N, and Li3P. The second inorganic component includes one or more of a lithium salt and a solid electrolyte. The polymer includes one or more of a highly viscous polymer, an ion-conducting polymer, and a polymer that reacts with the first metal material. Based on the total weight of the organic-inorganic composite layer 102, the polymer content in the organic-inorganic composite layer 102 is denoted as a, and the first inorganic component content is denoted as b. The ratio of a:b is 1:5-5:1, and can optionally be 1:3-3:1. Based on the total weight of the organic-inorganic composite layer 102, the total content of the second inorganic component in the organic-inorganic composite layer 102 is denoted as c, and c is 5 wt% to 50 wt%. The peel strength between the organic-inorganic composite layer 102 and the negative electrode substrate 101 is greater than or equal to 500 N / m, thereby improving the cycle performance of the battery.

[0131] 6 , in some embodiments, the negative electrode substrate 101 may include only the first substrate layer 1011. The organic-inorganic composite layer 102 may be located on at least one surface of the negative electrode substrate 101 (or the first substrate layer 1011).

[0132] 7 and 8 , in some embodiments, the negative electrode substrate 101 may further include a negative electrode current collector layer 1012 spaced apart from the organic-inorganic composite layer 102, and the first substrate layer 1011 is located on at least one surface of the negative electrode current collector layer 1012. The organic-inorganic composite layer 102 is located on a surface of the first substrate layer 1011.

[0133] 9 and 10 , in some embodiments, the negative electrode substrate 101 may further include a second negative electrode active material layer 1013 located between the first substrate layer 1011 and the negative electrode current collector layer 1012 , and the second negative electrode active material layer 1013 includes a second negative electrode active material.

[0134] In some embodiments, the second negative electrode active material may include one or more of a carbon-based material, lithium titanate, and a silicon-based material. As an example, the carbon-based material may include one or more of graphite (e.g., natural graphite, artificial graphite, etc.), soft carbon, and hard carbon. As an example, the silicon-based material may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy material.

[0135] The second negative electrode active material in the second negative electrode active material layer 1013 and the first negative electrode active material in the first base layer 1011 may be the same as or different from each other, and this embodiment of the present application is not limited thereto.

[0136] In some embodiments, the second negative electrode active material layer 1013 may further include a conductive agent. The present application does not particularly limit the type of the conductive agent. As examples, the conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0137] In some embodiments, the second negative electrode active material layer 1013 may further include a binder. The present application does not particularly limit the type of the binder. As examples, the binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, aqueous acrylic resins (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0138] In some embodiments, the second negative active material layer 1013 may further include other additives, such as thickeners, such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, and the like.

[0139] In some embodiments, the thickness of the first base layer 1011 may be 1 μm-100 μm, and optionally 10 μm-50 μm. The thickness of the first base layer 1011 refers to the thickness of the first base layer 1011 located on one surface of the negative electrode current collector layer 1012 .

[0140] In some embodiments, the thickness of the negative electrode current collector layer 1012 may be 0-15 μm, and may be 5 μm-12 μm. When the thickness of the negative electrode current collector layer is 0, it means that the negative electrode substrate does not include the negative electrode current collector layer.

[0141] In some embodiments, the thickness of the second negative electrode active material layer 1013 may be 0-120 μm, optionally 20 μm-100 μm. The thickness of the second negative electrode active material layer 1013 refers to the thickness of the second negative electrode active material layer 1013 located on one surface of the negative electrode current collector layer 1012. When the thickness of the second negative electrode active material layer is 0, it means that the negative electrode substrate does not include the second negative electrode active material layer.

[0142] In some embodiments, the total thickness of the negative electrode substrate 101 may be 10 μm-290 μm, optionally 20 μm-250 μm. The thickness of the negative electrode substrate refers to the total thickness of the negative electrode substrate consisting of the first substrate layer 1011 and the negative electrode current collector layer 1012 and / or the second negative electrode active material layer 1013.

[0143] In some embodiments, the negative electrode current collector layer 1012 may include a metal foil, a three-dimensional porous current collector, or a composite current collector.

[0144] Examples of the metal foil include copper foil, copper alloy foil, nickel foil, and nickel alloy foil.

[0145] As examples of the three-dimensional porous current collector, copper mesh, nickel mesh, foamed copper, and foamed nickel can be used.

[0146] The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0147] The negative electrode substrate 101 does not exclude other additional functional layers in addition to the first substrate layer 1011, the negative electrode current collector layer 1012, and the second negative electrode active material layer 1013. For example, in some embodiments, the negative electrode substrate 101 may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector layer 1012 and the second negative electrode active material layer 1013 and disposed on the surface of the negative electrode current collector layer 1012.

[0148] The thickness of the organic-inorganic composite layer is well known in the art and can be measured using instruments and methods known in the art. For example, six sets of parallel samples can be taken and the thickness of each set of samples can be measured at different locations using an optical microscope. At least 20 locations are measured for each set of samples, and the average thickness of the six sets of samples is taken as the sample thickness.

[0149] The elastic modulus of the organic-inorganic composite layer is well known in the art and can be tested using instruments and methods known in the art. The test temperature is 25°C. For example, the organic-inorganic composite layer can be cut into strips with a length L0 of 150 mm and a width of 20 mm. The strips can then be tensile tested using a universal testing machine. The tensile distance can be 100 mm and the tensile speed can be 50 mm / min. The elastic modulus is calculated based on the maximum tensile force of the organic-inorganic composite layer. The testing instrument can be an Instron 33652 tensile testing machine.

[0150] The elastic deformation of the organic-inorganic composite layer is well known in the art and can be tested using instruments and methods known in the art. The test temperature is 25°C. For example, the organic-inorganic composite layer can be cut into strips with a length L0 of 150 mm and a width of 20 mm. The strips can then be tensile tested using a universal testing machine at a tensile speed of 50 mm / min. The elastic deformation of the organic-inorganic composite layer is calculated as (L-L0) / L0×100%, assuming the length of the organic-inorganic composite layer at break is L. The testing instrument can be an Instron 33652 tensile testing machine.

[0151] The 25°C electrolyte swelling rate of the organic-inorganic composite layer is well known in the art and can be tested using instruments and methods known in the art. For example, during the test, the organic-inorganic composite layer can be cut into 30mm×30mm square samples, and the mass is recorded as m0; then the sample is placed in the electrolyte and soaked for 2 hours for a swelling experiment; the swollen sample is taken and the residual electrolyte on the surface is gently wiped with filter paper, and then the mass of the swollen sample is weighed and recorded as m. The 25°C electrolyte swelling rate of the organic-inorganic composite layer is (m-m0) / m0×100%. The electrolyte can be prepared as follows: ethylene glycol dimethyl ether (DME) is used as the solvent, and then LiFSI is added to the solvent in batches, and heated and stirred to dissolve LiFSI to prepare an electrolyte with a concentration of 1 mol / L.

[0152] The 25°C ionic conductivity of the organic-inorganic composite layer is well known in the art and can be tested using instruments and methods known in the art. For example, during the test, the organic-inorganic composite layer can be punched into a disc with a diameter of 16 mm; the organic-inorganic composite layer disc is soaked in the electrolyte for 1 hour, taken out, and the residual electrolyte on the surface is gently wiped with filter paper; the ionic conductivity of the organic-inorganic composite layer is calculated using the formula σ=d / (R×A). d is the sample thickness, which can be measured with a micrometer; A is the sample area; R is the sample impedance, which can be obtained by assembling the sample into a symmetrical battery (the electrodes can be stainless steel electrodes) and then using an electrochemical workstation for testing. The test frequency can be 10 -6 -10 -1 Hz, the voltage amplitude can be 5mV, and the intersection of the graph and the horizontal axis is taken as the sample impedance R. The electrolyte can be prepared as follows: use ethylene glycol dimethyl ether (DME) as the solvent, then add LiFSI to the solvent in batches, heat and stir to dissolve the LiFSI, and prepare an electrolyte with a concentration of 1 mol / L. The electrochemical workstation can be a Shanghai Chenhua CHI660C electrochemical workstation.

[0153] The peel strength between the organic-inorganic composite layer and the negative electrode substrate is well known in the art and can be tested using instruments and methods known in the art. For example, during the test, the negative electrode sheet (for example, if it is a negative electrode sheet with a double-sided protective layer, it can be first processed into a negative electrode sheet with a single-sided protective layer using a scraper) can be cut into a test sample of 150mm×20mm, and a flat thin steel plate is taken. A double-sided tape is pasted on the center of the steel plate (the length is slightly larger than the length of the test sample, and the width can be the same as the test sample). It is smoothed with force so that the double-sided tape fits tightly to the center of the steel plate; the negative electrode substrate side of the test sample is flatly adhered and fixed on the double-sided tape, and the organic-inorganic composite layer side of the sample is adhered to the tape (the peeling strength between the organic-inorganic composite layer and the tape is greater than the peeling strength between the organic-inorganic composite layer and the negative electrode substrate); after the sample is prepared, it is first calibrated and cleared, the test width is set, and a 180° peeling test is performed using a tensile testing machine (the peeling surface is consistent with the force line of the testing machine), the peeling speed is 50m / min, and the peeling distance is half of the sample size (for example, 75mm), and the peeling strength curve can be obtained. The peel strength between the organic-inorganic composite layer and the negative electrode substrate is calculated by taking the value of the plateau of the peel strength curve. The testing instrument can be an Instron 33652 tensile testing machine.

[0154] To ensure the accuracy of the test results, in the above tests, each sample was tested at least three times, and the average value was taken as the test result.

[0155] In the above test, the organic-inorganic composite layer can be obtained from the negative electrode sheet. For example, the first base layer can be dissolved with a solvent (such as ethanol) to obtain the organic-inorganic composite layer.

[0156] The negative electrode sheet can be sampled and tested during the preparation process, or from a prepared battery cell. For example, the battery cell can be discharged (for safety reasons, the battery cell is generally fully discharged); the battery cell can be disassembled and the negative electrode sheet removed. The negative electrode sheet is then soaked in dimethyl carbonate for a certain period of time (e.g., 2-10 hours); the negative electrode sheet is then removed and dried at a certain temperature and time (e.g., 60°C for more than 4 hours). After drying, the negative electrode sheet is removed.

[0157] [Preparation method]

[0158] The embodiment of the present application also provides a method for preparing the above-mentioned negative electrode sheet.

[0159] The preparation method includes the following steps: providing a negative electrode substrate, the negative electrode substrate includes a first substrate layer, the first substrate layer includes a first metal material, and the first metal material includes one or more of lithium element and lithium alloy; providing a first reaction component, the first reaction component includes one or more of I2, S, N2, and P; allowing the first reaction component to contact and react with the first metal material in the first substrate layer to in-situ form a first inorganic component on the surface of the first substrate layer, the first inorganic component includes one or more of LiI, LiF, Li2S, Li3N, and Li3P; providing a coating solution, the coating solution includes a polymer and / or a monomer for forming a polymer; coating the coating solution on the surface of the first substrate layer, forming an organic-inorganic composite layer after reaction, and obtaining a negative electrode plate, the reaction including at least one of a reaction between the polymer and the first metal material and / or the first inorganic component and an in-situ polymerization reaction of the monomer.

[0160] In the preparation method provided in the embodiment of the present application, the organic-inorganic composite layer is formed by an in-situ reaction, thereby improving the peeling strength between the organic-inorganic composite layer and the negative electrode substrate, making the organic-inorganic composite layer tightly bonded to the negative electrode substrate, reducing the volume expansion of the negative electrode side during the charging process, and reducing the probability of the organic-inorganic composite layer peeling off from the surface of the negative electrode substrate, thereby enabling the organic-inorganic composite layer to play its role for a long time and extending the cycle life of the battery.

[0161] The first inorganic component is obtained by the in-situ contact reaction of the first reaction component with the first metal material, thereby making the particles of the first inorganic component more nano-sized, dense and uniform, which can better uniformize the ion field and regulate the lithium metal deposition behavior, thereby reducing the formation of lithium dendrites, reducing the volume expansion of the negative electrode side during the charging process, and reducing the probability of the organic-inorganic composite layer breaking or cracking due to lithium dendrite growth or interface displacement; it can also reduce the probability of forming sharp-shaped lithium dendrites during the charging and discharging process, and reduce the probability of lithium dendrites penetrating the isolation membrane, thereby reducing the probability of battery short circuit and improving battery reliability; in addition, it can also regulate the swelling behavior of the organic-inorganic composite layer in the electrolyte, improve the ionic conductivity of the organic-inorganic composite layer, reduce the interface impedance of the battery, and promote the efficient transfer of ions within the organic-inorganic composite layer and at the interface with the negative electrode matrix.

[0162] The polymer can be obtained by an in-situ polymerization reaction of a monomer or a reaction between the polymer and the first metal material and / or the first inorganic component. The polymer obtained in this way can effectively fill the gaps left by the first inorganic component particles on the surface of the first substrate layer, reduce the contact between the electrolyte and the first metal material in the first substrate layer, reduce side reactions, and reduce the consumption of the electrolyte and the first metal material; it can also make the first inorganic component particles evenly dispersed in the organic-inorganic composite layer, making the organic-inorganic composite layer more dense and uniform, and can avoid the problems of easy agglomeration of nano-inorganic particles and poor dispersion of nano-inorganic particles in the organic phase (such as polymer binder) in traditional coating methods.

[0163] Therefore, the first inorganic particles and polymers in the organic-inorganic composite layer formed by the preparation method provided in the embodiment of the present application can be uniformly compounded, and the formed organic-inorganic composite layer is more dense and uniform, which can reduce the formation of lithium dendrites, reduce the contact between the electrolyte and the first metal material in the negative electrode matrix, reduce side reactions, and reduce the consumption of the electrolyte and the first metal material, thereby reducing the capacity loss of the battery; it can also reduce the volume expansion of the negative electrode side during the charging process, so that the battery has high coulomb efficiency, high energy density and long cycle life; at the same time, the elastic modulus of the organic-inorganic composite layer is also improved, thereby reducing the probability of lithium dendrites penetrating the isolation membrane, reducing the probability of battery short circuit, and improving the reliability of the battery.

[0164] In some embodiments, the peel strength between the in-situ generated organic-inorganic composite layer and the negative electrode substrate is greater than or equal to 500N / m, for example, it can be 600N / m-3200N / m, 800N / m-2800N / m, 800N / m-2550N / m, 800N / m-2400N / m, 1200N / m-2800N / m, 1200N / m-2550N / m, 1200N / m-2400N / m, 1500N / m-2800N / m, 1500N / m-2550N / m, 1500N / m-2400N / m, 1700N / m-2800N / m, 1700N / m-2550N / m, 1700N / m-2400N / m.

[0165] In some embodiments, the method of causing the first reactive component to contact and react with the first metal material in the first base layer may include evaporation, which may be vacuum evaporation or physical evaporation.

[0166] In some embodiments, the first reactive component is in vapor form.

[0167] In some embodiments, the method includes the following steps: providing a negative electrode substrate, the negative electrode substrate includes a first substrate layer, the first substrate layer includes a first metal material, and the first metal material includes one or more of lithium element and lithium alloy; providing vapor, the vapor includes one or more of I2, S, N2, and P; allowing the vapor to contact and react with the first metal material in the first substrate layer to form a first inorganic component in situ on the surface of the first substrate layer, the first inorganic component includes one or more of LiI, LiF, Li2S, Li3N, and Li3P; providing a coating solution, the coating solution includes a polymer and / or a monomer for forming a polymer; coating the coating solution on the surface of the first substrate layer, forming an organic-inorganic composite layer after reaction, and obtaining a negative electrode plate, the reaction including at least one of a reaction between the polymer and the first metal material and / or the first inorganic component and an in situ polymerization reaction of the monomer.

[0168] The first inorganic component is obtained by an in-situ reaction between steam and the first metal material, thereby making the particles of the first inorganic component more nano-sized, dense and uniform.

[0169] In some embodiments, the reaction temperature when the first reactive component contacts and reacts with the first metal material in the first base layer may be 30° C.-200° C., and optionally 50° C.-180° C.

[0170] In some embodiments, the reaction time when the first reactive component is in contact with the first metal material in the first base layer may be less than or equal to 5 hours, and may optionally be less than or equal to 2 hours.

[0171] By adjusting the reaction temperature and / or reaction time during the reaction, the content of the first inorganic component in the organic-inorganic composite layer can be adjusted, and the thickness of the organic-inorganic composite layer can also be adjusted.

[0172] In some embodiments, the coating solution may include a polymer, wherein the polymer includes a polymer that is reactive with the first metal material. For example, the polymer may include at least one functional group selected from the group consisting of: -OH, -COOH, -CN, and -SO3H. This allows the polymer to chemically bond to the negative electrode substrate, thereby tightly bonding the organic-inorganic composite layer to the negative electrode substrate. This reduces volume expansion on the negative electrode side during charging and reduces the probability of the organic-inorganic composite layer peeling from the negative electrode substrate surface, thereby enabling the organic-inorganic composite layer to function over a long period of time and extending the cycle life of the battery.

[0173] In some embodiments, the coating solution may include monomers for forming a polymer. For example, the coating solution may be applied to the surface of a negative electrode substrate having a first inorganic component, and then an in-situ polymerization reaction of the monomers is carried out under the action of at least one of an initiator, heat, light, or a radiation source to form an organic-inorganic composite layer. The polymer in the organic-inorganic composite layer is obtained through the in-situ polymerization reaction of the monomers, thereby allowing the organic-inorganic composite layer to be tightly bonded to the negative electrode substrate, reducing volume expansion on the negative electrode side during charging and reducing the probability of the organic-inorganic composite layer peeling from the negative electrode substrate surface. This allows the organic-inorganic composite layer to function for a long time and extends the cycle life of the battery.

[0174] In some embodiments, the monomer used to form the polymer may further include at least one functional group selected from the following: -OH, -COOH, -CN, and -SO3H. This allows the formed polymer to be chemically bonded to the negative electrode substrate, thereby more tightly integrating the organic-inorganic composite layer with the negative electrode substrate. This reduces volume expansion on the negative electrode side during charging and the probability of the organic-inorganic composite layer peeling from the negative electrode substrate surface, thereby ensuring the long-term function of the organic-inorganic composite layer and extending the cycle life of the battery.

[0175] In some embodiments, the coating solution may further include an initiator. As an example, the initiator may include an initiator for free radical polymerization, such as an organic peroxide (such as benzoyl peroxide, lauroyl peroxide, isopropyl benzene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, diisopropyl benzene peroxide, tert-butyl perbenzoate, tert-butyl pervalerate, methyl ethyl ketone peroxide, cyclohexanone peroxide, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, etc.), an inorganic peroxide (such as potassium persulfate, sodium persulfate, ammonium persulfate, etc.), an azo compound (such as azobenzene), The monomers may be selected from the group consisting of diisobutyronitrile, azobisisoheptanenitrile, and the like; a photoinitiator may also be included, such as one or more of benzophenone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, and triphenylphosphine oxide derivatives; and an initiator (or catalyst) for ionic polymerization may also be included, such as one or more of lithium metal, Li2S, metal alkyl compounds (e.g., triethylaluminum), metal alkoxides, alkali metal amides, tertiary amines, and stannous octoate. Those skilled in the art can make the selection based on the monomer type and polymerization method.

[0176] Of course, in some embodiments, the coating solution may not use an initiator, and those skilled in the art may adjust it according to actual conditions.

[0177] In some embodiments, the first inorganic component and / or the first metal material may function as a polymerization catalyst or initiator to promote polymerization of the monomer.

[0178] The heating method can be a method known in the art, such as oven heating, etc. The embodiments of the present application are not limited to this, and those skilled in the art can make a choice based on actual conditions.

[0179] In some embodiments, the reaction temperature during the in-situ polymerization of the monomers may be 25° C. to 120° C., or optionally 30° C. to 100° C. Those skilled in the art may select the temperature based on actual conditions.

[0180] In some embodiments, the reaction time for the in-situ polymerization of the monomers may be less than or equal to 24 hours, optionally less than or equal to 10 hours, and more optionally less than or equal to 8 hours. Those skilled in the art may make the selection based on actual conditions.

[0181] The light may be ultraviolet light, and the radiation source may include α-rays, β-rays, γ-rays, x-rays, electron beams, etc. The embodiments of the present application are not limited to this, and those skilled in the art may make a selection according to actual circumstances.

[0182] In some embodiments, the coating solution may further include one or more of a lithium salt and a solid electrolyte. When the formed organic-inorganic composite layer contains the aforementioned components, the swelling behavior of the organic-inorganic composite layer in the electrolyte can be adjusted, resulting in a higher ionic conductivity for the swollen organic-inorganic composite layer and a lower interfacial impedance for the assembled battery cell, thereby improving the battery's cycling and kinetic performance.

[0183] In some embodiments, the coating solution may further include one or more of a film-forming additive and an inorganic filler. This can improve the quality of the negative electrode film and adjust one or more of the elastic modulus, ionic conductivity, electrolyte swelling, and elastic deformation of the organic-inorganic composite layer, thereby improving the battery's cycling performance and / or kinetic performance.

[0184] In some embodiments, the formed polymer may have a cross-linked network structure, thereby enabling the organic-inorganic composite layer to have a suitable electrolyte swelling degree, thereby promoting efficient ion transfer within the organic-inorganic composite layer and at the interface with the negative electrode matrix, thereby improving the battery's cycling performance and kinetic performance.

[0185] In some embodiments, the solvent of the coating solution may include one or more of ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF), toluene, ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), dimethoxymethane (DMM), diethylene glycol dimethyl ether (DG), and tetraethylene glycol dimethyl ether, and the embodiments of the present application are not limited to this.

[0186] In some embodiments, the coating solution may be applied by scraping, spraying, spin coating, or vapor deposition, etc., which is not limited in the embodiments of the present application.

[0187] The preparation method provided in the embodiments of this application can prepare the negative electrode sheet described above in this application. Other parameters of the negative electrode sheet can refer to the negative electrode sheet described above in this application and will not be repeated here. In the preparation process, unless otherwise specified, the instruments and reagents used are all commercially available.

[0188] [Positive electrode]

[0189] In some embodiments, the positive electrode sheet may include a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. The positive electrode film layer may include a positive electrode active material. For example, the positive electrode current collector may have two opposing surfaces in its thickness direction, and the positive electrode film layer may be disposed on either or both of the two opposing surfaces of the positive electrode current collector.

[0190] The type of positive electrode active material can be selected according to the type of battery cell, which is not limited in the embodiments of the present application.

[0191] For example, when the battery cell is a lithium metal battery cell, the positive electrode active material may include, but is not limited to, one or more of lithium transition metal oxides, lithium-containing phosphates, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of lithium-containing phosphates may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and their respective modified compounds. In some embodiments, in order to further improve the energy density of the battery cell, the positive electrode active material may include a general formula of Li a Ni b Co c M d O e A f One or more lithium transition metal oxides and modified compounds thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes one or more of N, F, S and Cl.

[0192] As an example, the positive electrode active material may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (abbreviated as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (abbreviated as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (abbreviated as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (abbreviated as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (abbreviated as NCM811), LiNi 0.96 Co 0.02 Mn 0.02 O2 (abbreviated as Ni96), LiNi0.85 Co 0.15 Al 0.05 One or more of O2, LiFePO4, LiMnPO4.

[0193] The modified compounds of the above-mentioned positive electrode active materials may be used to perform doping modification and / or surface coating modification on the positive electrode active materials.

[0194] When the battery cell is a lithium-sulfur battery cell, the positive electrode active material may include, but is not limited to, one or more of elemental sulfur, a sulfur-carbon composite material, a sulfur-conductive polymer composite material, and a sulfur-metal oxide composite material.

[0195] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. For example, the positive electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0196] In some embodiments, the positive electrode film layer may further optionally include a positive electrode binder. This application does not particularly limit the type of positive electrode binder. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.

[0197] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0198] The positive electrode film layer can be formed by coating a positive electrode slurry onto a positive electrode current collector, drying it, and cold pressing it. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional conductive agent, an optional binder, and any other components in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP).

[0199] [Electrolytes]

[0200] The electrolyte conducts ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and the electrolyte can be selected based on needs. For example, the electrolyte can include one or more selected from solid electrolytes and liquid electrolytes (i.e., electrolyte solutions).

[0201] In some embodiments, the electrolyte may be an electrolyte solution, which may include an electrolyte salt and a solvent.

[0202] For example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium bisoxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0203] The type of solvent is not particularly limited and can be selected according to actual needs.

[0204] In some embodiments, the solvent may include one or more of an ester solvent (eg, carbonate, carboxylate, sulfate, etc.), an ether solvent (eg, ether, alcohol ether, fluoroether, etc.), or a sulfone solvent.

[0205] As an example, the solvent may include, but is not limited to, one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), diethyl sulfone (ESE), dimethoxymethane (DMM), diethylene glycol dimethyl ether (DG), ethylene glycol dimethyl ether (DME), and tetraethylene glycol dimethyl ether.

[0206] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve overcharge performance, additives that improve high-temperature performance, and additives that improve low-temperature power performance.

[0207] In some embodiments, the concentration of the electrolyte salt may be 0.5 mol / L to 4 mol / L.

[0208] [Isolation film]

[0209] In some embodiments, the battery cell further includes a separator, which may be disposed between the positive and negative electrode sheets to primarily prevent internal short circuits. This application does not specifically limit the type of separator; any known porous membrane with good chemical and mechanical stability may be used.

[0210] In some embodiments, the material of the isolation membrane can include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, and polyimide. The isolation membrane can be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different.

[0211] In some embodiments, the charging current density of the battery cell can be 0.5 mA / cm 2 -12mA / cm 2 , optional 0.8mA / cm 2 -10mA / cm 2 or 1mA / cm 2 -6mA / cm 2 The negative electrode plate provided in the embodiment of the present application can enable the battery cell to withstand a larger charging current.

[0212] Electrical devices

[0213] The present application also provides an electrical device, which includes a battery provided in the present application. The battery can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.

[0214] The electrical device can select a specific type of battery, such as a battery cell, a battery module, or a battery pack, according to its usage requirements.

[0215] Figure 11 is a schematic diagram of an exemplary electrical device. This device can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the device's requirements for high power and high energy density, a battery pack or battery module can be used as a power source.

[0216] As another example, an electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a battery cell as a power source.

[0217] Example

[0218] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.

[0219] Example 1

[0220] (1) Preparation of negative electrode sheet

[0221] A 20μm-thick lithium ribbon was pressed and attached to a 10μm-thick copper current collector to form the negative electrode substrate. The coating solution was a monomer solution prepared in the following proportions: 10.54g of butyl cyanoacrylate, 2.79g of lithium bis(fluorosulfonyl)imide (LiFSI), and 12.93g of ethylene glycol dimethyl ether (DME). The thickness of the resulting organic-inorganic composite layer could be adjusted by adjusting the coating thickness of the monomer solution.

[0222] The negative electrode substrate was placed in a 70°C atmosphere of sublimated iodine vapor for 60 seconds, followed by a scraping of the monomer solution onto its surface. The substrate coated with the monomer solution was then placed horizontally at 25°C for 2 hours before being transferred to a 60°C vacuum oven and dried for 5 hours to allow the monomer to fully polymerize, resulting in a negative electrode with an organic-inorganic composite layer. The organic-inorganic composite layer includes polybutyl cyanoacrylate, LiI, and LiFSI. The contents of each component are shown in Table 1. The thickness of the organic-inorganic composite layer is 0.1 μm.

[0223] (2) Preparation of positive electrode sheet

[0224] The positive electrode active material NCM811, the conductive agent acetylene black, and the binder PVDF were mixed in a mass ratio of 98:1:1, added to the solvent NMP and stirred until the system became uniform to obtain a positive electrode slurry with a solid content of 70%; the positive electrode slurry was evenly coated on the surface of the positive electrode current collector aluminum foil, dried, and then transferred to an oven for further drying to obtain a positive electrode sheet.

[0225] (3) Preparation of electrolyte

[0226] Ethylene glycol dimethyl ether (DME) was used as a solvent, and LiFSI was added to the solvent in batches. The LiFSI was dissolved by heating and stirring to prepare an electrolyte with a concentration of 1 mol / L.

[0227] (4) Preparation of isolation membrane

[0228] A polyethylene porous membrane was used as the separator.

[0229] (5) Preparation of battery cells

[0230] The positive electrode sheet, separator, and negative electrode sheet are stacked in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, dried, and then injected with electrolyte. After vacuum packaging, standing, formation, shaping and other processes, a battery cell is obtained.

[0231] Example 2

[0232] The preparation method of the battery cell is similar to that of Example 1, except for the preparation process of the negative electrode plate.

[0233] A 20μm-thick lithium ribbon was pressed and attached to a 10μm-thick copper current collector to form the negative electrode substrate. The coating solution was a polymer solution prepared in the following proportions: 10.31g of hydrogenated nitrile rubber, 2.73g of lithium difluorooxalatoborate (LiDFOB), and 16.8g of tetrahydrofuran (THF). The thickness of the resulting organic-inorganic composite layer could be adjusted by adjusting the coating thickness of the polymer solution.

[0234] The negative electrode substrate was placed in a sublimed sulfur vapor atmosphere at 120°C for 120 seconds, followed by a scraping of a polymer solution onto its surface. The polymer solution-coated negative electrode substrate was then placed horizontally at 25°C for 30 minutes before being transferred to a 70°C vacuum oven and dried for another 4 hours. This yielded a negative electrode sheet with an organic-inorganic composite layer. The organic-inorganic composite layer consisted of hydrogenated nitrile rubber, Li2S, and LiDFOB. The content of each component is shown in Table 1. The thickness of the organic-inorganic composite layer was 0.1 μm.

[0235] Example 3

[0236] The preparation method of the battery cell is similar to that of Example 1, except for the preparation process of the negative electrode plate.

[0237] A 50μm-thick lithium ribbon was used as the negative electrode substrate. The coating solution was a monomer solution prepared in the following proportions: 10.64g of isoprene, 0.21g of azobisisobutyronitrile (AIBN), 2.81g of lithium bis(oxalatoborate) (LiBOB), 6.33g of toluene, and 6.30g of ethylene glycol dimethyl ether (DME). The thickness of the resulting organic-inorganic composite layer can be adjusted by adjusting the coating thickness of the monomer solution.

[0238] The negative electrode substrate was placed in a nitrogen atmosphere at 100°C for 120 seconds, followed by a scraping coat of the monomer solution. The substrate coated with the monomer solution was then cured in a vacuum oven at 65°C for 5 hours to obtain a negative electrode sheet with an organic-inorganic composite layer. The organic-inorganic composite layer includes polyisoprene, Li3N, and LiBOB. The content of each component is shown in Table 1. The thickness of the organic-inorganic composite layer is 0.1 μm.

[0239] Example 4

[0240] The preparation method of the battery cell is similar to that of Example 1, except for the preparation process of the negative electrode plate.

[0241] A 50μm-thick lithium ribbon was used as the negative electrode substrate. The coating solution was a monomer solution prepared in the following proportions: 11.74g styrene, 0.21g benzophenone, 3.10g lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and 9.60g tetrahydrofuran (THF). The thickness of the resulting organic-inorganic composite layer can be adjusted by adjusting the coating thickness of the monomer solution.

[0242] The negative electrode substrate was placed on a surface of black phosphorus powder at 180°C for 30 minutes, followed by a scraping of a monomer solution. The substrate coated with the monomer solution was then placed horizontally and irradiated under a 50W UV lamp for 40 seconds to produce a negative electrode sheet with an organic-inorganic composite layer. The organic-inorganic composite layer includes polystyrene, Li3P, and LiTFSI. The content of each component is shown in Table 1. The thickness of the organic-inorganic composite layer is 0.1μm.

[0243] Example 5

[0244] The preparation method of the battery cell is similar to that of Example 1, except for the preparation process of the negative electrode plate.

[0245] A 20μm-thick lithium ribbon was pressed and attached to a 10μm-thick copper current collector to form the negative electrode substrate. The coating solution was a monomer solution prepared in the following proportions: 10.74g of trimethylene carbonate, 0.21g of stannous octoate, 2.84g of lithium bis(fluorosulfonyl)imide (LiFSI), and 13.48g of ethyl methyl carbonate (EMC). The thickness of the resulting organic-inorganic composite layer could be adjusted by adjusting the coating thickness of the monomer solution.

[0246] The negative electrode substrate was placed in a 70°C atmosphere of sublimated iodine vapor for 60 seconds, followed by a scraping of a monomer solution onto its surface. The substrate coated with the monomer solution was then cured in a vacuum oven at 100°C for 5 hours to obtain a negative electrode sheet with an organic-inorganic composite layer. The organic-inorganic composite layer includes polytrimethylene carbonate, LiI, and LiFSI. The contents of each component are shown in Table 1. The thickness of the organic-inorganic composite layer is 0.1 μm.

[0247] Example 6

[0248] The preparation method of the battery cell is similar to that of Example 1, except for the preparation process of the negative electrode plate.

[0249] A 20μm-thick lithium-magnesium alloy was pressed and attached to a 10μm-thick copper current collector to form the negative electrode substrate. The coating solution was a monomer solution prepared in the following proportions: 9.61g propylene oxide, 0.19g triethylaluminum, 2.54g lithium tetrafluoroborate (LiBF4), and 23.44g ethylene glycol dimethyl ether (DME). The thickness of the resulting organic-inorganic composite layer could be adjusted by adjusting the coating thickness of the monomer solution.

[0250] The negative electrode substrate was placed in a sublimed sulfur vapor atmosphere at 120°C for 120 seconds, followed by a scraping coat of the monomer solution. The substrate coated with the monomer solution was then cured in a vacuum oven at 80°C for 4 hours, yielding a negative electrode sheet with an organic-inorganic composite layer. The organic-inorganic composite layer consisted of polypropylene oxide, Li2S, and LiBF4, with the contents of each component listed in Table 1. The thickness of the organic-inorganic composite layer was 0.1 μm.

[0251] Examples 7-15

[0252] The preparation method for the battery cells was similar to that of Example 1, except that the composition of the organic-inorganic composite layer was different, as detailed in Table 1. The organic-inorganic composite layers of Examples 7-15 were prepared by adjusting the contact time between the negative electrode substrate and the iodine vapor, the composition of the monomer solution, and the coating thickness of the monomer solution.

[0253] Examples 16-21

[0254] The preparation method for the battery cells was similar to that of Example 1, except that the thickness of the organic-inorganic composite layer was different, as detailed in Table 1. The organic-inorganic composite layers of Examples 16-21 were prepared by adjusting the contact time between the negative electrode substrate and the iodine vapor, the composition of the monomer solution, and the coating thickness of the monomer solution.

[0255] Comparative Example 1

[0256] The preparation method of the battery cell is similar to that of Example 1, except that the negative electrode plate does not have an organic-inorganic composite layer.

[0257] Comparative Example 2

[0258] The preparation method of the battery cell is similar to that of Example 1, except that the preparation process of the negative electrode plate is different.

[0259] A 20μm-thick lithium ribbon was pressed and attached to a 10μm-thick copper current collector to form the negative electrode substrate. The negative electrode substrate was then placed in a sublimated iodine vapor atmosphere at 70°C for 60 seconds to obtain the negative electrode sheet with an inorganic coating.

[0260] Comparative Example 3

[0261] The preparation method of the battery cell is similar to that of Example 1, except that the preparation process of the negative electrode plate is different.

[0262] A 20μm-thick lithium ribbon was pressed and attached to a 10μm-thick copper current collector to form the negative electrode substrate. A solution of polybutylcyanoacrylate and lithium bis(fluorosulfonyl)imide (85:15 by mass) was added to ethylene glycol dimethyl ether. The solution was then applied to the negative electrode substrate and dried to obtain the negative electrode sheet with an organic coating.

[0263] Comparative Example 4

[0264] The preparation method of the battery cell is similar to that of Example 1, except that the preparation process of the negative electrode plate is different.

[0265] A 20μm-thick lithium ribbon was pressed and attached to a 10μm-thick copper current collector to obtain the negative electrode substrate. A solution of polybutylcyanoacrylate, LiI, and lithium bis(fluorosulfonyl)imide (mass ratio of 56.7:28.3:15) was added to ethylene glycol dimethyl ether. The solution was then coated on the negative electrode substrate and dried to obtain a negative electrode sheet with an organic-inorganic composite layer.

[0266] Test section

[0267] The elastic modulus, elastic deformation, 25° C. electrolyte swelling ratio, 25° C. ionic conductivity, and peel strength between the organic-inorganic composite layer and the negative electrode substrate were tested according to the above-described methods.

[0268] (1) Cyclic performance test

[0269] The test temperature is 25°C. The prepared battery cell is charged to 4.25V at a constant current as shown in Table 1, and then discharged to 3.0V at a constant current of 0.33C to obtain the first-cycle discharge capacity, which is recorded as Cd1. The above method is repeated for 50 cycles, and the discharge capacity of the battery cell after 50 cycles is recorded as Cd 50 The capacity retention rate of the battery cell after 50 cycles (%) = the discharge capacity after 50 cycles (Cd 50 ) / first cycle discharge capacity (Cd1)×100%.

[0270] (2) Lithium deposition test

[0271] After the battery cells were adjusted to a fully discharged state after 50 cycles, the battery cells were disassembled to obtain the negative electrode plates. The lithium deposition on the surface of the negative electrode plates was observed under an optical microscope. The results are shown in Table 1. "Minor" indicates that the area of ​​lithium dendrites observed under an optical microscope is less than 1 / 4 of the area of ​​the negative electrode plate. "Moderate" indicates that the area of ​​lithium dendrites observed under an optical microscope is between 1 / 4 and 2 / 3 of the area of ​​the negative electrode plate. "Severe" indicates that the area of ​​lithium dendrites observed under an optical microscope is greater than 2 / 3 of the area of ​​the negative electrode plate.

[0272] (3) Thickness expansion test of negative electrode

[0273] The test temperature was 25°C. The thickness of the negative electrode sheet after rolling was measured using an optical microscope and recorded as d1. After 50 cycles, the battery cell was adjusted to a fully discharged state, then disassembled to obtain the negative electrode sheet. The thickness of the negative electrode sheet was measured again using an optical microscope and recorded as d2. The thickness expansion ratio (%) of the negative electrode sheet is (d2 - d1) / d1 × 100%.

[0274] The test results are shown in Table 1.

[0275] As can be seen from Table 1, by in-situ setting of an organic-inorganic composite layer on the surface of the negative electrode substrate, the volume expansion of the negative electrode sheet can be reduced, the formation of lithium dendrites can be reduced, and the cycle performance of the battery can be improved.

[0276] It can be seen from the test results of Examples 1-21 and Comparative Example 4 that by in-situ forming an organic-inorganic composite layer on the surface of the negative electrode substrate, the peeling strength between the organic-inorganic composite layer and the negative electrode substrate can be improved, the organic-inorganic composite layer and the negative electrode substrate can be tightly combined, and the volume expansion of the negative electrode plate can be further reduced; at the same time, the first inorganic component particles can be evenly dispersed in the organic-inorganic composite layer, making the organic-inorganic composite layer more dense and uniform, thereby better regulating the lithium metal deposition behavior, further reducing the formation of lithium dendrites, reducing side reactions, and thereby further reducing the capacity loss of the battery and improving the cycle performance of the battery.

[0277] Comparative Example 4 uses a traditional coating method to form an organic-inorganic composite layer. The peeling strength between the organic-inorganic composite layer and the negative electrode substrate is low. At the same time, the nano-inorganic particles also have problems such as easy agglomeration and poor dispersion in the organic phase. As a result, the negative electrode plate prepared in Comparative Example 4 has a large volume expansion, severe lithium plating, and the battery's cycle performance is not excellent enough.

[0278] It can also be seen from the test results of Examples 1-21 and Comparative Examples 1-4 that the negative electrode plates provided in the embodiments of the present application can also enable the battery to withstand a larger charging current, and the battery also has good cycle performance under a large charging current.

[0279] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and within the scope of the technical solution of the present application, embodiments having substantially the same structure as the technical idea and exerting the same effects are all included in the technical scope of the present application. In addition, within the scope of the subject matter of the present application, various modifications that can be conceived by those skilled in the art to the embodiments, and other methods constructed by combining some of the constituent elements in the embodiments are also included in the scope of the present application.

[0280]

Claims

1. A negative electrode sheet, in, The negative electrode plate comprises a negative electrode substrate and an organic-inorganic composite layer located on at least one surface of the negative electrode substrate; The negative electrode substrate comprises a first substrate layer close to the organic-inorganic composite layer, the first substrate layer comprises a first metal material, and the first metal material comprises one or more of lithium element and lithium alloy; The organic-inorganic composite layer includes a polymer and a first inorganic component, wherein the first inorganic component includes LiI, LiF, Li 2 S. Li 3 N.Li 3 One or more of P; The peel strength between the organic-inorganic composite layer and the negative electrode substrate is greater than or equal to 500 N / m.

2. The negative electrode sheet according to claim 1, in, The peeling strength between the organic-inorganic composite layer and the negative electrode substrate is 600N / m-3200N / m, and can be optionally 800N / m-2800N / m.

3. The negative electrode sheet according to claim 1 or 2, in, The organic-inorganic composite layer satisfies at least one of the following conditions (1) to (5): (1) The elastic modulus of the organic-inorganic composite layer is 0.1 MPa-70 MPa, and can be optionally 19 MPa-53 MPa; (2) The elastic deformation of the organic-inorganic composite layer is 7%-700%, and can be optionally 9%-310%; (3) The swelling rate of the organic-inorganic composite layer in the electrolyte at 25°C is 9%-60%, and can be optionally 11%-38%; (4) The ionic conductivity of the organic-inorganic composite layer at 25° C. is 0.001 mS / cm-5 mS / cm, and can be optionally 0.03 mS / cm-3.4 mS / cm; (5) The thickness of the organic-inorganic composite layer is 0.005 μm-10 μm, and can be optionally 0.02 μm-5 μm.

4. The negative electrode sheet according to any one of claims 1 to 3, in, The organic-inorganic composite layer includes a first surface close to the negative electrode substrate and a second surface away from the negative electrode substrate. The mass content of the first inorganic component at the first surface is recorded as W. 1 , the mass content of the first inorganic component at the second surface is recorded as W 2 , then W 1 >W 2 .

5. The negative electrode sheet according to any one of claims 1 to 4, in, Based on the total weight of the organic-inorganic composite layer, the content of the polymer in the organic-inorganic composite layer is recorded as a, and the content of the first inorganic component is recorded as b, then a:b is 1:5-5:1, and can be optionally 1:3-3:1; Optionally, a is 8wt%-80wt%, more preferably 14wt%-71wt%; Optionally, b is 8wt%-80wt%, more preferably 14wt%-71wt%.

6. The negative electrode sheet according to any one of claims 1 to 5, in, The organic-inorganic composite layer further includes a second inorganic component; Optionally, the second inorganic component includes one or more of a lithium salt and a solid electrolyte; and / or, Optionally, based on the total weight of the organic-inorganic composite layer, the total content of the second inorganic component in the organic-inorganic composite layer is denoted as c, and c is greater than 0 and less than or equal to 55 wt %, and may be 5 wt %-50 wt %.

7. The negative electrode sheet according to claim 6, in, The lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalato)borate, lithium difluorooxalatoborate, lithium difluorobis(oxalato)phosphate, lithium tetrafluorooxalatophosphate, lithium difluorophosphate, and lithium trifluoromethanesulfonate; and / or, The solid electrolyte includes an oxide-type inorganic solid electrolyte, a sulfide-type inorganic solid electrolyte and a halide Optionally, the oxide-type inorganic solid electrolyte includes one or more of a NASICON-type solid electrolyte, a garnet-type solid electrolyte, a perovskite-type solid electrolyte, and a LISICON-type solid electrolyte. Optionally, the sulfide-type inorganic solid electrolyte includes one or more of a sulfide-type crystalline solid electrolyte and a sulfide glass-type solid electrolyte.

8. The negative electrode sheet according to claim 6 or 7, in, The organic-inorganic composite layer further includes a third inorganic component; Optionally, the third inorganic component includes one or more of a film-forming additive and an inorganic filler; and / or, Optionally, based on the total weight of the organic-inorganic composite layer, the total content of the third inorganic component in the organic-inorganic composite layer is recorded as d, and d is greater than 0 and less than or equal to 20 wt %.

9. The negative electrode sheet according to claim 8, in, The film-forming additive includes one or more of fluoroethylene carbonate, vinylene carbonate, vinyl ethylene carbonate, vinyl sulfate, propylene sulfite, vinyl sulfite, diethyl sulfite, dimethyl sulfite, butane sultone, tris(trimethylsilyl)phosphate; and / or, The inorganic filler includes one or more of boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, aluminum magnesium silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate, and barium titanate.

10. The negative electrode sheet according to any one of claims 1 to 9, in, The volume distribution particle size Dv50 of the first inorganic component is less than or equal to 80 nm, and can be optionally 10 nm-30 nm.

11. The negative electrode sheet according to any one of claims 1 to 10, in, The polymer includes one or more of a polymer having high viscosity, a polymer having ion conduction function, and a polymer that can react with the first metal material; Optionally, the polymer includes one or more of poly(meth)acrylate, polyurethane, natural rubber, polyisoprene, polystyrene, polyether, polyethylene oxide, polycarbonate, polymethyl methacrylate, ionomer, polyacrylonitrile, polycyanoacrylate, poly(meth)acrylic acid, hydrogenated nitrile rubber, polyvinyl alcohol, and their respective derivatives.

12. The negative electrode sheet according to any one of claims 1 to 11, in, The first substrate layer also includes a first negative electrode active material; Optionally, the first negative electrode active material includes a carbon-based material, and more optionally includes one or more of graphite and hard carbon.

13. The negative electrode sheet according to any one of claims 1 to 12, in, The negative electrode substrate further includes a negative electrode current collector layer away from the organic-inorganic composite layer, and the first substrate layer is located on at least one surface of the negative electrode current collector layer.

14. The negative electrode sheet according to claim 13, in, The negative electrode substrate further comprises a second negative electrode active material layer located between the first substrate layer and the negative electrode current collector layer, wherein the second negative electrode active material layer comprises a second negative electrode active material; Optionally, the second negative electrode active material includes one or more of carbon-based materials, lithium titanate, and silicon-based materials.

15. A method for preparing a negative electrode sheet, comprising the following steps: Providing a negative electrode substrate, the negative electrode substrate comprising a first substrate layer, the first substrate layer comprising a first metal material, the first metal material comprising one or more of lithium element and lithium alloy; Providing a first reaction component, the first reaction component comprising I 2 , S, N 2 , one or more of P; The first reaction component is contacted with the first metal material in the first base layer to react, so as to form a first inorganic component in situ on the surface of the first base layer, wherein the first inorganic component includes LiI, LiF, Li 2 S. Li 3 N.Li 3 One or more of P; providing a coating solution, the coating solution comprising a polymer and / or a monomer for forming a polymer; The coating solution is coated on the surface of the first substrate layer, and an organic-inorganic composite layer is formed after reaction to obtain a negative electrode plate. The reaction includes at least one of a reaction between the polymer and the first metal material and / or the first inorganic component and an in-situ polymerization reaction of the monomer.

16. The method according to claim 15, in, The method of making the first reaction component contact and react with the first metal material in the first base layer comprises evaporation, which may be vacuum evaporation or physical evaporation; and / or, The reaction temperature when the first reaction component contacts and reacts with the first metal material in the first substrate layer is 30° C.-200° C., and can be 50° C.-180° C.; and / or, The reaction time of the first reaction component and the first metal material in the first substrate layer in contact reaction is less than or equal to 5 hours, and can be less than or equal to 2 hours; and / or, The first reaction component is in vapor form.

17. The method according to claim 15 or 16, in, The coating solution further comprises one or more of an initiator, a lithium salt, and a solid electrolyte.

18. A battery cell, comprising an electrode assembly, wherein the electrode assembly comprises the negative electrode sheet according to any one of claims 1 to 14 or the negative electrode sheet prepared by the method according to any one of claims 15 to 17.

19. A battery comprising the battery cell according to claim 18.

20. An electrical device comprising the battery according to claim 19.

Citation Information

Patent Citations

  • NEGATIVE ELECTRODE FOR LITHIUM METAL BATTERY, METHOD OF PREPARING NEGATIVE ELECTRODE, LITHIUM METAL BATTERY INCLUDING THE SAME, AND composite electrolyte

    CN108807851A

  • All-solid-state lithium metal battery and preparation process thereof

    CN109818048A

  • Pre-lithiated silicon negative electrode as well as preparation method and application thereof

    CN111864181A

  • Negative pole piece and lithium metal battery

    CN112563461A

  • Lithium metal negative pole piece, electrochemical device and electronic device

    CN113437257A

Cited By

  • Three-dimensional porous lithium metal material, secondary battery, and electric device

    WO2026137501A1

  • Battery cell and manufacturing method therefor, negative electrode sheet, battery device, and electric device

    WO2026156806A1