Clinker material and method for producing clinker material
By applying an iron-rich surface layer onto clinker particles using industrial by-products, the formation of chromium(VI) is inhibited, reducing environmental and health risks, and lowering CO2 emissions in the cement industry, while enabling the use of chromium-containing materials in clinker production.
Patent Information
- Application Number
- PCT/FI2024/050183
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
AI Technical Summary
The cement industry faces challenges in reducing chromium(VI) formation during clinker production, which leads to environmental pollution and health risks, and also contributes to high CO2 emissions, as chromium(III) is oxidized to chromium(VI) under high temperatures and oxygen-rich conditions, necessitating costly reducing agents to limit chromium(VI) concentrations in cement.
Applying an iron-rich surface layer, primarily composed of ferrites, onto clinker particles after the sintering zone but before cooling, to inhibit chromium(VI) formation by using iron-rich materials from industrial by-products, such as pyrometallurgical slags or incinerator ash, which oxidize preferentially to chromium(III), thereby reducing oxygen exposure and chromium(VI) formation.
This method effectively reduces chromium(VI) content in clinker particles, allowing for increased use of chromium-containing by-products and decreased CO2 emissions, while maintaining fuel burning efficiency and clinker mineralogy, and enables the use of iron-rich materials as a reducing agent in cement production.
Smart Images

Figure FI2024050183_24102024_PF_FP_ABST
Abstract
Description
[0001] CLINKER MATERIAL AND METHOD FOR PRODUCING CLINKER MATERIAL
[0002] The present invention relates to a clinker material, to a method for producing clinker material and use of iron-rich material according to the preambles of the enclosed independent claims.
[0003] Common cement is made from clinker and supplementary cementitious materials. The clinker material is typically produced in a kiln, such as a rotary kiln, by high temperature calcination of raw mix made of natural materials, such as limestone (CaCOs), clay, and sand. It is possible to add by-products from different industries in the raw mix or use them for the fuel mix. In the conventional clinker production a large amount of CO2 is released due to the calcination of limestone (CaCOs + heat
[0004] CaO + CO2). This makes the cement industry one of the biggest CO2 emitters in the world. The increasing awareness of climate change compels every industry, also the cement industry, to view critically their actions and to find new effective ways to reduce carbon dioxide emissions, for example by substituting the natural resources with by-products having low CO2 emission factor. In many instances in the cement industry these by-products may be materials containing increased concentration of heavy metals, including chromium. Due to its chemical properties chromium can be present in different oxidation forms. Usually it exists predominantly as Cr(lll), such as Cr20s, in the raw materials, either natural or by-products, used for clinker production. This trivalent form of chromium is not soluble and therefore not harmful for the health, nor for the environment. However, under the high temperatures of the clinker production process, especially in an oxygen rich atmosphere at the exit end of the rotary kiln, the Cr(lll) present in the clinker material may be transformed into the Cr(VI), such as CrOs.
[0005] In the production of cement clinker, chromium is dissolved in the clinker melt at a temperature around 1450 °C. In the kiln, chromium may react with alkalis to form very soluble salts, such as Na2CrO4 and K2CrO4. After the sintering zone of the kiln, when the clinker material is cooled down to a temperature around 1150 °C, chromium which is not solidified into the clinker minerals, produces calcium oxychromite, 9CaO*4CrO3*Cr2Os. In the cooling zone of the kiln, Cr(lll) may be converted into Cr(VI) in the presence of oxygen following the reaction:
[0006] 2 Cr20s + 4 CaO + 302 — > 4CaO*CrOs
[0007] Accordingly, Cr(VI) is formed when hot clinker material is exposed to an oxygen rich atmosphere during cooling.
[0008] Cr(VI) compounds are highly water-soluble, and may cause, for example, skin irritation when contacted, as well as water and / or soil pollution. Consequently, the concentration of Cr(VI) in cement preparations is limited to a maximum of 2 ppm. To achieve this limit value, Cr(VI) reducing agents can be added to the cement to reduce Cr(VI) into insoluble and non-toxic Cr(lll) when mixed with water. However, these reducing agents are often costly and not broadly available. Thus, there is a need to reduce or inhibit formation of Cr(VI) in the production of clinker material.
[0009] One way to inhibit or limit Cr(VI) formation in the clinker material is to reduce the amount of oxygen after the sintering zone of the kiln. However, the presence of oxygen is necessary for the effective burning of fuel in the kiln, as well as for the proper formation of clinker minerals. Typically, oxygen is provided to the sintering zone by a secondary air, taken from the cooler and passing through the cooling zone of the kiln. There have been attempts to limit the formation of Cr(VI) in the clinker by supplying CO2 gas at the kiln outlet in order to reduce the contact of formed clinker material with oxygen. However, this approach may cause disturbances in the fuel burning efficiency and / or deviation from the normal clinker mineralogy. Alternatively, the Cr(VI) formation in the clinker material has been limited by spraying limestone powder (CaCOs) at the kiln exit to produce CO2. and to reduce oxygen contact. This method has the disadvantage of dissolving the Cr(VI) in CaO and disturbing the fuel burning.
[0010] Consequently, there is a need in the cement industry for effective reduction or even elimination of Cr(VI) formation in the clinker material. Effective reduction of Cr(VI) formation might also make it possible to increase the use of chromium containing by-products for clinker production, and thus decrease the carbon dioxide emissions of the clinker production process. These objects are attained with the invention having the characteristics presented below and in the characterizing part of the independent claim. Some preferred embodiments of the invention are presented in the dependent claims.
[0011] An object of the present invention is to provide a clinker particles comprising clinker material with a low Cr(IV) content.
[0012] Another object of the present invention is to increase the use of industrial byproducts in the production of cement clinker particles and / or reduce CO2 emissions during the production of cement clinker particles comprising clinker material.
[0013] The embodiments mentioned in this text relate, where applicable, to all aspects of the invention, even if this is not always separately mentioned.
[0014] Typical clinker particles according to the present invention for production of cement comprise clinker material comprising at least calcium silicates, calcium aluminates and iron compounds, wherein the clinker particles have a particle core of clinker material which is at least partially coated with a surface layer comprising iron-rich material, preferably in form of ferrites.
[0015] Typical method according to the present invention for producing clinker particles for cement production, especially for reducing Cr(VI) amount in the cement, the clinker particles comprising clinker material comprising at least calcium silicates, calcium aluminates as well as iron compounds, the method comprising
[0016] - feeding raw mix for the clinker particles to a kiln at a first end of the kiln, wherein the kiln has a burner in a second end of the kiln,
[0017] - sintering the raw mix into clinker particles in a sintering zone of the kiln,
[0018] - removing the clinker particles from the second end of the kiln and allowing them to cool down, wherein iron-rich material is applied on the clinker particles after the sintering zone but before clinker particles are cooled down to a temperature of <900 °C, preferably wherein the clinker particles are at least partially coated with a surface layer comprising the iron-rich material, preferably in form of ferrites.
[0019] Typical arrangement according to the present invention for producing clinker material comprises
[0020] - a kiln having a first end and a second end, wherein the first end comprises a kiln inlet and the second end comprises a kiln outlet,
[0021] - a calcining zone, a sintering zone and a cooling zone arranged between the first end and the second end of the kiln,
[0022] - a burner arranged at the second end of the kiln, wherein the arrangement further comprises feeding means arranged at the second end of the kiln below the burner, for feeding iron-rich material into the kiln, wherein the feeding means are arranged to feed the iron-rich material to the cooling zone of the kiln, preferably over a clinker bed.
[0023] Typical use according to the present invention of iron-rich material originating from a pyrometallurgical process, incinerator bottom ash, tailings from mineral and / or mining industry, mill scale, rust, banded iron formations, and any of their combinations is for coating clinker particles in the production of clinker material.
[0024] Now it has been surprisingly found that by applying iron-rich material onto the hot clinker particles it is possible to reduce the Cr(VI) formation in the clinker particles. The application of iron-rich material results in clinker particles which are at least partially coated with a surface layer comprising the iron-rich material. It is assumed, without wishing to be bound by any theory, that the iron in the iron-rich material melts and forms the surface layer, i.e. coating, which at least partially covers the particle core of the clinker particles and thus blocks or restricts the access of oxygen into the particle core comprising clinker material. The high concentration of iron in the surface layer will favour the formation of Cr(lll) instead of Cr(VI) in the presence of oxygen. In this way the problems caused by the transformation of Cr(lll) into Cr(VI) in the kiln can be effectively solved. The present invention makes it possible to use chromium containing by-products in production of clinker particles without the risk of increasing the Cr(VI) concentration in the clinker material. This is advantageous as it reduces the need for virgin raw materials from natural sources that are non-calcined, i.e. which emit CO2 in the clinker production, such as limestone (CaCOs). The present invention thus provides, inter alia, a method for manufacture of cement clinker particles with low hexavalent chromium concentration.
[0025] In the present invention there is no need to modify the composition or oxygen content of the secondary air for the kiln, as the clinker particles are protected by the surface layer formed from the iron-rich material. This means that the effective fuel burning process is guaranteed as well as the correct formation of the clinker minerals in the sintering zone.
[0026] The clinker particles of the present invention are intended and suitable for production of cement, and they comprise clinker material comprising calcium silicates, aluminium and iron containing clinker phases, i.e. calcium aluminates and iron compounds. The clinker particles may typically have a particle diameter in a range of 1 - 100 mm, such as 1 - 50 mm or 2 - 30 mm (measured e.g. by sieving). If the particle is not spherical, the diameter is here understood as the largest distance from surface to surface via the centre of the particle. The clinker particle of the invention comprises a particle core made clinker material comprising at least calcium silicates, calcium aluminates and iron compounds, and a protective surface layer comprising iron-rich material, preferably in form of ferrites, which at least partially coats, surrounds or covers the particle core. Preferably at least 40 %, more preferably at least 50 %, even more preferably at least 60 %, of the particle core is coated or covered by the surface layer of iron-rich material. According to one embodiment, 40 - 100 %, preferably 50 - 100 %, more preferably 60 - 100 % of the surface of the particle core is coated or covered by the surface layer.
[0027] Preferably the surface layer of the clinker particle has a higher iron concentration, given as Fe2Os, than the particle core. According to one embodiment of the invention, the iron concentration in the surface layer may be at least 50 %, preferably at least 60 %, more preferably at least 70 % or at least 80 %, even more preferably at least 90 %, higher than the iron concentration of the clinker material in the particle core, given as Fe20s. For example, the clinker material in the particle core may have an iron concentration up to 5 weight-%, for example 0.1 - 5 weight-%, whereas the surface layer may have an iron concentration in range of 15 - 70 weight-%, given as Fe2C>3.
[0028] The surface layer of the clinker particle is preferably relatively thin. The thickness of the surface layer is less than 50 %, more preferably less than 30 %, of the diameter of the clinker particle. The thickness of the surface layer may be, for example, less than 0.5 mm, such as 0.01 - 0.5 mm.
[0029] The surface layer, which at least partially coats or covers the particle core comprising or consisting of clinker material, is made of iron-rich material, preferably in form of ferrites. The surface layer may essentially consist of iron-rich material. According to one preferable embodiment, the iron-rich material, used for forming the surface layer, as well as the surface layer, may comprise >15 weight-% or >20 weight-%, preferably >50 weight-%, more preferably >60 weight-%, sometimes even >70 weight-%, of iron compounds, given as Fe2Os. The iron-rich material, and the surface layer, may comprise 15 - 98 weight-% or 20 - 97 weight-%, preferably 50 - 95 weight-%, more preferably 60 - 90 weight-% or 70 - 90 weight-%, of iron compounds, given as Fe2Os. For example, the iron-rich material, and the surface layer, may comprise 7 - 95 weight-%, preferably 15 - 70 weight-%, more preferably 30 - 50 weight-%, of iron compounds, given as Fe2Os. The amount of iron / iron compounds in the iron-rich material can be measured, for example, by using X-ray fluorescence (XRF).
[0030] According to one preferable embodiment of the invention the iron-rich material used in the present invention for forming the protective surface layer for the clinker particles may originate from a pyrometallurgical process, incinerator bottom ash, tailings from mineral and / or mining industry, mill scale, rust, banded iron formations, or any of their combinations. The iron-rich material may originate from or be ferrous slags, ferroalloy slags, base metal slags, metallurgical tailings, or any of their combinations. The iron-rich material may originate from a pyrometallurgical process selected from basic oxygen furnace slags, electric arc furnace slags, induction furnace slags, Linz-Donawitz slags, ladle furnace slags, blast furnace slag, copper slag, or any of their combinations. Preferably the iron-rich material may be selected from basic oxygen furnace slags, electric arc furnace slags, induction furnace slags, Linz-Donawitz slags, ladle furnace slags, or any of their combinations. The iron-rich material may originate from the industrial pyrometallurgical production process of steel, either stainless steel or carbon steel, copper, nickel, or zinc. The material used for creating the surface layer may also be selected from municipal waste incinerator bottom ash, tailings from copper, gold or other mineral / metal industries containing wustite, hematite, magnetite, ferrite, fayalite or any of their combinations, mill scale, rust, or banded iron formations (BIF). In principle, any material that is able to oxidize easier than chromium and does not negatively affect the resulting clinker material, can be used to form the protective surface layer. Examples of such materials are tin and antimony compounds.
[0031] The iron-rich material used in the present invention may have a particle size Dv50 of <500 pm, preferably <300 pm, more preferably <200 pm. The particle size Dv50 may be, for example in a range of 1 - 500 pm, preferably 5 - 300 pm, more preferably 10 - 200 pm. Particle size Dv50 indicates that 50% of the material in weight is below the given size. The particle size Dv50 as used herein is measured according to standards ISO 13320:2020 and ISO 9276-2:2014. It is possible to effectively control and / or adjust the thickness of the formed surface layer by appropriate selection of fineness, i.e. the particle size Dv50, of the iron-rich material, which is applied on the clinker particles.
[0032] Some iron-rich materials, for example fayalite tailings, may already be in the form of fine powder and have a suitable particle size Dv50. However, if the particle size of the iron-rich material is too large, the material may be comminuted to a suitable particle size as defined above, before its application to the clinker particles. Comminution can be performed by using any suitable comminution method, for example, by using an impact crusher, a high energy impact crusher, a jaw crusher, a cone crusher, a hammer crusher, a roll crusher, a ball mill, a rod mill or any combination of these. The iron rich material originating from the industrial pyrometallurgical process, industrial tailings or incinerator bottom ash may be pre-treated in order to concentrate the iron-bearing minerals while removing the elemental iron or steel.
[0033] The clinker particles are formed in any suitable kiln, preferably a rotary kiln. The kiln has a first end, i.e. kiln feed side or kiln inlet, and a second end, i.e. kiln exit side with kiln outlet. The raw mix is fed to the kiln at its first end and the kiln has a burner at the second end of the kiln. The kiln can comprise at least to a calcining zone, a sintering zone and a cooling zone, arranged between the first end and the second end, seen from the first end to the second end. The raw mix is sintered into clinker particles in the sintering zone, where the temperature may be around 1400 - 1500 °C
[0034] The raw mix fed to the kiln comprises natural raw materials, such as limestone (CaCOs), clay, and sand. The raw mix preferably further comprises calcinated calcium-containing by-products from an industrial process, e.g. pyrometallurgical process. Calcium in the by-product may be present as calcium oxides, calcium silicates, calcium carbonate or as any combination of these.
[0035] The clinker particles are removed from the kiln at the end of the cooling zone of the kiln, located at the second end of the kiln. The temperature of the clinker material in the cooling zone may be around 1000 - 1400 °C. From the cooling zone the clinker material is transferred into a cooler, where the clinker material is usually cooled to a temperature below 80 °C. The iron-rich material can be applied to the clinker particles in the cooling zone of the kiln or at the removal of the clinker material from the kiln to the cooler or in the cooler, immediately after the removal of the clinker material from the kiln.
[0036] The iron-rich material is applied on the clinker particles after the sintering zone but before the temperature of the clinker material is cooled down <900 °C, preferably <950 °C, more preferably <1000 °C. According to one embodiment the iron-rich material may be applied on the clinker particles when the temperature of the clinker material is <1500 °C, preferably <1450 °C, more preferably <1400 °C. Preferably the temperature of the clinker material may be in a range of 900 - 1500 °C, more preferably 950 - 1450 °C, even more preferably 1000 - 1400 °C. The application of the iron-rich material at these temperatures ensures that it is effectively melted and spread onto the surface of the clinker particles.
[0037] It is possible to apply iron-rich material on the clinker particles in one or several application locations. According to one embodiment, the iron-rich material can be applied by spraying at the kiln exit in order to spread and melt the iron-rich material on the clinker particles at a correct temperature, without affecting the clinker formation in the sintering zone. Alternatively, or in addition, the iron-rich material can be applied by spraying in the cooling zone of the kiln in order to spread and melt the iron-rich material on the clinker particles in a clinker bed at a correct temperature. For example, iron-rich material can be applied on the clinker particles in the cooling zone of the kiln, at the kiln exit and / or immediately after removal of clinker particles from the kiln, as long as the temperature of the clinker particles is >900 °C.
[0038] The iron-rich material can be applied by any suitable method available, e.g. by spraying iron-rich material on the clinker particles. According to one aspect of the invention, the arrangement comprises feeding means arranged at the second end of the kiln below the main burner, for feeding iron-rich material into the kiln. The feeding means are arranged to feed the iron-rich material to the cooling zone of the kiln for coating the clinker particles of the clinker bed. The iron-rich material is thus applied to the cooling zone of the kiln by using feeding means arranged at the second end of the kiln below a main burner of the kiln. According to one embodiment, the feeding means may be a feeding pipe. For example, the iron-rich material can be applied by using a feeding pipe made of refractory material, e.g. hardened steel, with two concentric channels where the iron-rich material is transported in a central inner channel and the outer channel surrounding the central inner channel is connected with a feeding means for transport gas, e.g. pressurized air. The transport gas can be used for cooling the feeding means. The transport of iron-rich material can be arranged pneumatically. The transport gas, e.g. pressurized air, used for cooling may also help in directing the iron-rich material correctly towards the clinker particles. For protecting the feed pipe from the high temperatures and from the abrasion effect of the clinker dust, the feed pipe is casted in a refractory concrete. The feed pipe is preferably positioned to face clinker material in the kiln, ideally aligned with the zero position of the kiln (without entering the kiln tube), in correlation with the direction of rotation of the kiln (on the side of the clinker movement), but without dispersing the feed material on the refractory lining.
[0039] The iron-rich material may be applied onto the clinker particles in the form of a dry powder or in the form of a suspension. If applied as a suspension, the particles of iron-rich material are suspended into a liquid continuous phase, which can be water or any other suitable liquid or liquid mixture. The iron-rich material, either in powder form or suspension form, may contain auxiliary agents, such as chemical compounds which help to handle and / or apply the iron-rich material or which help the formation of the surface layer onto the clinker particles.
[0040] According to one embodiment the iron-rich material may be applied in amount of <1 weight-%, preferably <0.9 weight-%, calculated from a total weight of the clinker particles or clinker material produced. For example, the iron-rich material may be applied in amount of 0.05 - 1 weight-%, preferably 0.1 - 0.9 weight-%, calculated from a total weight of the clinker material produced. The amount of the iron-rich material used can be controlled to provide the optimal coverage of the clinker particles without formation of an excess melt. If too much iron-rich material is fed to the kiln at the second end of, the melted iron can may stick on the refractory lining of the kiln, and cause damage to the lining as well as risk for blockage of the kiln exit.
[0041] According to one preferable embodiment of the present invention, the iron-rich material which is applied to the clinker particles comprises or consists of a particulate material originating from an industrial pyrometallurgical process, preferably from a steelmaking process. The particulate material comprises at least 10 weight-% of iron(ll) and / or iron(lll), given as Fe2Os, calculated from the dry weight of the particulate material and preferably 5 weight-% or less, more preferably 3 weight-% or less, of Fe(0). Such particulate material may be obtained by fractioning a starting particulate material from an industrial pyrometallurgical process into at least a first fraction and a second fraction, wherein the first fraction and the second fraction have different content of iron(ll) and iron(lll). The second fraction may typically comprise at least 10 weight-% of iron(ll) and / or iron(lll), given as Fe2Os, and be used as the iron-rich material in the present invention. The second fraction may comprise, for example, at least 5 weight-%, preferably at least 10 weight-%, more preferably at least 15 weight-% of iron(ll), calculated as FeO from the dry weight of the particulate material. The particulate material may comprise, for example, 5 - 20 weight-%, of iron(ll), calculated as FeO from the dry weight of the particulate material. Before and / or after the fractioning, the particulate material may be crushed and / or ground to a suitable particle size, and optionally demetallized by removal of metallic iron particles, i.e. particles of Fe(0). Suitable processes for processing, e.g. fractioning, of the particulate material from industrial pyrometallurgical process are disclosed, for example, in PCT / FI2023 / 050620.
[0042] According to one embodiment, when the iron-rich material applied to the clinker particles comprises or consists of a particulate material originating from an industrial pyrometallurgical process, obtained by fractionating as described above, it is applied to the clinker particles by feeding into the kiln through feeding means arranged at the second end of the kiln, preferably below the main burner. As described above, the feeding means are thus arranged to feed the iron-rich material to the cooling zone, where the temperature is around 1000 - 1400 °C.
[0043] According to one embodiment, the particle diameter of the particulate material originating from an industrial pyrometallurgical process, used as the iron-rich material, may be up to 5 mm. The particulate material thus comprises a coarse fraction with a particle diameter from 1 mm to 5 mm and a fine fraction with a particle diameter of less than 1 mm, for example from 0.01 to less than 1 mm. When the particulate material is applied through the feeding means arranged at the cooling zone at the second end of the kiln, the coarse fraction of the particulate material falls down to the clinker bed due to the gravity and is taken out of the kiln together with the clinker particles. The coarse fraction is thus mixed with the clinker particles. The fine fraction of the particulate material is carried by a secondary air flow, passing through the cooling zone of the kiln, where it is applied to the clinker particles for forming the surface layer. The particulate material originating from an industrial pyrometallurgical process may be applied in an amount up to 20 weight-%, calculated from the weight of clinker particles before addition of the iron-rich material. For example, it can be applied in an amount of 1 - 20 weight-%, preferably 2 - 15 weight-%, more preferably 3 - 13 weight-%.
[0044] The clinker particles according to the present invention are typically used in preparation of cement, preferably as a Cr(VI) reducing agent. The clinker material according to the present invention is suitable for use as a Cr(VI) reducing agent in preparation of cement. The clinker material, i.e. clinker particles, can be subjected to fine grinding in different types of cement mills commonly employed in the art. In case there is Cr(VI) present in the cement mix, the iron-rich surface layer can be used as a source for Fe(ll) that will act as chromium reducing compound. Fe(ll) present in the surface layer can be dissolved by an activator, e.g. carboxylic acid, added to during preparation of cement, e.g. during grinding or postgrinding. This present invention will thus lead to the effective reduction or complete elimination of Cr(VI) in cement and open a wide range of possibilities to utilize more by-products in the cement industry.
[0045] Some embodiments of the invention are shown in the following schematical drawings, where
[0046] Figure 1 shows an arrangement for producing clinker particles, according to one embodiment of the present invention, seen from the side of the kiln, and
[0047] Figure 2 shows the embodiment of Figure 1 , seen from the second end of the kiln.
[0048] Figure 1 shows an arrangement for producing clinker particles according to one embodiment of the present invention seen from the side of the kiln. The arrangement comprises a kiln 1 , having a first end (not shown) and a second end 1 ’. A burner 2 with a flame 3 is arranged in a kiln hood 11 , located at the second end 1 ’ of the kiln 1. Clinker bed movement from the first end towards the second end is generally indicated with arrow A. At the second end 1 ’ of the kiln 1 the clinker bed comprises clinker particles 4, some of which are schematically indicated in Figure 1 .
[0049] A cooling zone 5, indicated with a dashed ellipse, is located at the second end 1 ’ under the burner 2. The temperature of the clinker particles 4 in the cooling zone 5 is around 1000 - 1400 °C. The clinker particles 4 are removed from the cooling zone 5 of the kiln 1 through a kiln exit 6, and transferred into a cooler 7, where the clinker particles 4 are usually cooled to a temperature below 80 °C. Secondary air, indicated with dashed arrows B, is taken from the cooler 7 and fed through the kiln exit 6 to the cooling zone 5 of the kiln 1 .
[0050] Iron-rich material is applied on the clinker particles 4 in the cooling zone 5 and / or at the kiln exit 6 by using a feeding means 8, i.e. feeding pipe. The feeding means 8 for the iron-rich material are located below the burner 2, so that the feeding of iron- rich material does not disturb the burner functions. The feeding means 8 are positioned to direct the iron-rich material correctly towards the clinker particles, wherein the clinker particles become at least partly coated by the iron-rich material. At the temperatures prevailing at the second end 1 ’ of the kiln 1 , the iron melts and forms at least a partial coating for the clinker particles 4.
[0051] Figure 2 shows the embodiment of Figure 1 , seen from the second end 1 ’ of the kiln 1 , through the kiln hood 11. It is seen that the feeding means 8 for the iron-rich material is located below the burner 2, slightly on the side of the burner 2.
[0052] Even if the invention was described with reference to what at present seems to be the most practical and preferred embodiments, it is appreciated that the invention shall not be limited to the embodiments described above, but the invention is intended to cover also different modifications and equivalent technical solutions within the scope of the enclosed claims.
Claims
CLAIMS1 . Clinker particles for production of cement, which clinker particles comprise clinker material comprising at least calcium silicates, calcium aluminates and iron compounds, characterised in that the clinker particles have a particle core of clinker material which is at least partially coated with a surface layer comprising iron-rich material, preferably in form of ferrites.
2. Clinker particles according to claim 1 , characterised in that the surface layer has a higher iron concentration than the particle core.
3. Clinker particles according to claim 2, characterised in that the iron concentration in the surface layer is at least 50 %, preferably at least 60 %, more preferably at least 70%, even more preferably at least 90 %, higher than the iron concentration of the clinker material in the particle core.
4. Clinker particles according to claim 1 , 2 or 3, characterised in that the surface layer comprises 15 - 98 weight-%, preferably 50 - 95 weight-%, more preferably 60- 90 weight-% or 70 - 90 weight-%, of iron compounds, given as Fe2Os.
5. Use of clinker particles according to any of claims 1 - 4 in preparation of cement, preferably as a Cr(VI) reducing agent.
6. Use according to claim 5, characterised in that Fe(ll) present in the surface layer of the clinker particles is dissolved by an activator, e.g. carboxylic acid, added to during preparation of cement.
7. Method for producing clinker particles for cement production, especially for reducing Cr(VI) formation in production of the clinker particles, the clinker particles comprising clinker material comprising at least calcium silicates, calcium aluminates as well as iron compounds, the method comprising- feeding raw mix for the clinker particles to a kiln at a first end of the kiln, wherein the kiln has a burner in a second end of the kiln,- sintering the raw mix into clinker particles in a sintering zone of the kiln,- removing the clinker particles from the second end of the kiln and allowing them to cool down, characterised in iron-rich material is applied on the clinker particles after the sintering zone but before clinker particles are cooled down to a temperature of <900 °C, wherein the clinker particles are at least partially coated with a surface layer comprising the iron-rich material, preferably in form of ferrites.
8. Method according to claim 7, characterised in that the iron-rich material originating from a pyrometallurgical process, incinerator bottom ash, tailings from mineral and / or mining industry, mill scale, rust, banded iron formations, or any of their combinations, is used as the iron-rich material.
9. Method according to claim 8, characterised in that the iron-rich material originating from a pyrometallurgical process is selected from basic oxygen furnace slags, electric arc furnace slags, induction furnace slags, Linz-Donawitz slags, ladle furnace slags, blast furnace slag, copper slag, or any of their combinations.
10. Method according to claim 7, 8 or 9, characterised in that the iron-rich material is applied on the clinker particles when the temperature of the clinker material is <1500 °C, preferably <1450 °C, more preferably <1400 °C.11 . Method according to any of preceding claims 7 - 10, characterised in that the iron-rich material is applied in form of a dry powder or in form of a suspension.
12. Method according to any of preceding claims 7 - 11 , characterised in that the iron-rich material is applied to the cooling zone of the kiln by using feeding means arranged at the second end of the kiln below a main burner of the kiln.
13. Method according to any of preceding claims 7 - 11 , characterised in that the iron-rich material has a particle size Dv50 of <500 pm, preferably <300 pm, more preferably <200 pm.
14. Method according to any of preceding claims 7 - 13, characterised in that the iron-rich material comprises >20 weight-%, preferably >50 weight-%, more preferably >70 weight-%, of iron compounds, given as Fe2Os.
15. Method according to any of preceding claims 7 - 14, characterised in that the iron-rich material is applied in amount of <1 weight-%, preferably <0.9 weight-%, calculated from a total weight of the clinker material produced.
16. Arrangement for producing clinker material according to any of claims 1 - 4, the arrangement comprising- a kiln having a first end and a second end, wherein the first end comprises a kiln inlet and the second end comprises a kiln outlet,- a calcining zone, a sintering zone and a cooling zone arranged between the first end and the second end of the kiln- a burner arranged at the second end of the kiln, characterised in that the arrangement comprises feeding means arranged at the second end of the kiln below the burner, for feeding iron-rich material into the kiln, wherein the feeding means are arranged to feed the iron-rich material to the cooling zone of the kiln, preferably over a clinker bed.
17. Arrangement according to claim 16, characterised in that the feeding means is a feeding pipe, preferably with two concentric channels where the iron-rich material is transported in an inner channel surrounded by an outer channel connected with a feeding means for transport gas.
Citation Information
Patent Citations
Dispersion comprising tin sulfate or ferrous sulfate for reducing chromate in cement
EP1533287A1
Process for producing cement clinker containing blast furnace slag
US5976243A