Method for manufacturing relief-type diffraction grating

The method of forming silicon nitride films and using them as masks for local oxidation in the manufacturing of relief-type diffraction gratings addresses the issue of dimensional accuracy and light scattering, resulting in higher precision and efficiency of the diffraction gratings.

WO2024218966A1PCT designated stage expired Publication Date: 2024-10-24MITSUBISHI ELECTRIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/015925
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing relief-type diffraction gratings, such as those using photoresists, face challenges in maintaining dimensional accuracy as the convex portions of the periodic uneven structure become higher, leading to decreased accuracy and increased light scattering, which affects diffraction efficiency.

Method used

A method involving the formation of silicon nitride films on a silicon member, followed by local oxidation using these films as masks to create silicon oxide films with high dimensional accuracy, and subsequent selective removal to form stepped portions, enhancing the precision and smoothness of the diffraction grating surface.

Benefits of technology

This approach results in relief-type diffraction gratings with improved dimensional accuracy and diffraction efficiency, reducing light scattering and maintaining temperature stability due to the use of a single silicon material, thereby enhancing the overall performance of the diffraction grating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023015925_24102024_PF_FP_ABST
    Figure JP2023015925_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This method for manufacturing a relief-type diffraction grating (1) comprises a step for forming a first silicon nitride film (10) on a silicon member (2), a step for changing a part of the silicon member (2) into a first silicon oxide film (15) by oxidizing the silicon member (2) using the first silicon nitride film (10) as a mask, a step for removing the first silicon nitride film (10), and a step for selectively removing the first silicon oxide film (15) to form a first step part (4a) in the silicon member (2).
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a relief type diffraction grating

[0001] The present disclosure relates to a method for manufacturing a relief type diffraction grating.

[0002] Japanese Patent Laid-Open No. 2000-105307 (Patent Document 1) discloses a method for manufacturing a stepped relief type diffraction grating by etching a glass substrate using a photoresist as a mask. 2 Membrane and Al 2 O 3 A method for producing a stepped relief diffraction grating by etching a laminate with a film is disclosed.

[0003] JP 2000-105307 A JP 2000-155207 A

[0004] However, when etching using a photoresist, if the convex portions of the periodic uneven structure of the diffraction grating become tall, the dimensional accuracy of the diffraction grating decreases. The present disclosure has been made in view of the above-mentioned problems, and its purpose is to provide a method for manufacturing a relief-type diffraction grating with higher dimensional accuracy.

[0005] The method for manufacturing a relief type diffraction grating according to the present disclosure includes the steps of forming a first silicon nitride film on a silicon member, oxidizing the silicon member using the first silicon nitride film as a mask to convert a part of the silicon member into a first silicon oxide film, removing the first silicon nitride film, and selectively removing the first silicon oxide film to form a first step portion in the silicon member.

[0006] By oxidizing the silicon member using the first silicon nitride film as a mask, the first silicon oxide film can be formed with higher dimensional accuracy. Then, by selectively removing the first silicon oxide film, a relief-type diffraction grating is manufactured. According to the method for manufacturing a relief-type diffraction grating of this embodiment, a relief-type diffraction grating with higher dimensional accuracy can be manufactured.

[0007] 1 is a schematic partial cross-sectional view of a relief type diffraction grating according to a first embodiment; FIG. 2 is a schematic partial enlarged cross-sectional view of a relief type diffraction grating according to a first embodiment; FIG. 3 is a schematic partial enlarged cross-sectional view showing a step of a method for manufacturing a relief type diffraction grating according to a first embodiment; FIG. 4 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 5 in a method for manufacturing a relief type diffraction grating according to a first embodiment; FIG. 5 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 6 in a method for manufacturing a relief type diffraction grating according to a first embodiment; FIG. 7 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 8 in a method for manufacturing a relief type diffraction grating according to a first embodiment; FIG. 9 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 10 in the method for manufacturing a relief type diffraction grating according to the first embodiment. FIG. 11 in the method for manufacturing a relief type diffraction grating according to the first embodiment. FIG. 12 in the method for manufacturing a relief type diffraction grating according to the first embodiment. FIG. 13 in the method for manufacturing a relief type diffraction grating according to the first embodiment. FIG. 14 in the method for manufacturing a relief type diffraction grating according to the first embodiment. FIG. 15 in the method for manufacturing a relief type diffraction grating according to the first embodiment. FIG. 16 in the method for manufacturing a relief type diffraction grating according to the first embodiment. FIG. 17 in the method for manufacturing a relief type diffraction grating according to the second embodiment. FIG. 18 in the method for manufacturing a relief type diffraction grating according to the second embodiment.20 in the method for manufacturing a relief type diffraction grating according to the second embodiment. FIG. 21 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 21 in the method for manufacturing a relief type diffraction grating according to the second embodiment. FIG. 22 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 23 in the method for manufacturing a relief type diffraction grating according to the second embodiment. FIG. 23 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 24 in the method for manufacturing a relief type diffraction grating according to the second embodiment. FIG. 25 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 26 in the method for manufacturing a relief type diffraction grating according to the second embodiment. FIG. 27 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 28 in the method for manufacturing a relief type diffraction grating according to the second embodiment. 31 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 29 in the method for manufacturing a relief type diffraction grating according to Embodiment 2. FIG. 32 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 30 in the method for manufacturing a relief type diffraction grating according to Embodiment 2. FIG. 33 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 33 in the method for manufacturing a relief type diffraction grating according to Embodiment 2. FIG. 34 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 37 in the method for manufacturing a relief type diffraction grating according to Embodiment 3. FIG. 35 is a schematic partial enlarged cross-sectional view showing a step subsequent to the step shown in FIG. 38 in the method for manufacturing a relief type diffraction grating according to Embodiment 3.41 in the method for manufacturing a relief type diffraction grating of the third embodiment. FIG. 42 in the method for manufacturing a relief type diffraction grating of the third embodiment. FIG. 43 in the method for manufacturing a relief type diffraction grating of the third embodiment. FIG. 44 in the method for manufacturing a relief type diffraction grating of the third embodiment. FIG. 45 in the method for manufacturing a relief type diffraction grating of the third embodiment. FIG. 46 in the method for manufacturing a relief type diffraction grating of the third embodiment. FIG. 47 in the method for manufacturing a relief type diffraction grating of the third embodiment. 52. A schematic partial enlarged cross-sectional view showing the step subsequent to the step shown in Fig. 53 in the method for manufacturing a relief type diffraction grating of embodiment 4. FIG. 53 is a schematic partial enlarged cross-sectional view showing the step subsequent to the step shown in Fig. 48 in the method for manufacturing a relief type diffraction grating of embodiment 3. FIG. 54 is a schematic partial enlarged cross-sectional view showing the step subsequent to the step shown in Fig. 48 in the method for manufacturing a relief type diffraction grating of embodiment 3. FIG. 55 is a schematic partial enlarged cross-sectional view showing the step subsequent to the step shown in Fig. 52 in the method for manufacturing a relief type diffraction grating of embodiment 4. FIG. 56 is a schematic partial enlarged cross-sectional view showing the step subsequent to the step shown in Fig. 53 in the method for manufacturing a relief type diffraction grating of embodiment 4. FIG. 57 is a schematic plan view of an optical scanning device of embodiment 5.

[0008] Hereinafter, embodiments of the present disclosure will be described. Note that the same reference numerals are used to designate the same components, and the description thereof will not be repeated.

[0009] Embodiment 1 A relief type diffraction grating 1 according to embodiment 1 will be described with reference to Figures 1 and 2. The diffraction wavelength of the relief type diffraction grating 1 is, for example, in the wavelength range from infrared to far infrared.

[0010] The relief type diffraction grating 1 includes a silicon member 2 and a periodic uneven structure 9 formed on the silicon member 2. The relief type diffraction grating 1 may further include a reflective film (not shown) provided on the surface of the periodic uneven structure 9. The reflective film is made of, for example, a metal.

[0011] The relief type diffraction grating 1 is formed on a silicon member 2. In this embodiment, the silicon member 2 is a silicon substrate 2a.

[0012] The periodic uneven structure 9 includes a plurality of periodically arranged protrusions 3. Each of the protrusions 3 includes a side surface 3a, a side surface 3b opposite to the side surface 3a, and a top surface 4t. The top surface 4t is disposed between the side surfaces 3a and 3b and is connected to the side surfaces 3a and 3b.

[0013] In this embodiment, each of the protrusions 3 has a plurality of height levels. The relief type diffraction grating 1 is a stepped diffraction grating having a plurality of height levels. Specifically, each of the protrusions 3 has, for example, four height levels. Each of the protrusions 3 includes step portions 4a, 4b, 5a, 5b, 6a, 6b, 7a, and 7b.

[0014] Step portions 4a, 5a, 6a, and 7a are provided on the side surface 3a. Step portion 4a is the uppermost step portion among the step portions 4a, 5a, 6a, and 7a. Step portion 5a is the second uppermost step portion among the step portions 4a, 5a, 6a, and 7a. Step portion 6a is the second lowermost step portion among the step portions 4a, 5a, 6a, and 7a. Step portion 7a is the lowest step portion among the step portions 4a, 5a, 6a, and 7a.

[0015] Step portions 4b, 5b, 6b, and 7b are provided on the side surface 3b. Step portion 4b is the uppermost step portion among step portions 4b, 5b, 6b, and 7b. Step portion 5b is the second uppermost step portion among step portions 4b, 5b, 6b, and 7b. Step portion 6b is the second lowermost step portion among step portions 4b, 5b, 6b, and 7b. Step portion 7b is the lowest step portion among step portions 4b, 5b, 6b, and 7b.

[0016] Step portion 4b faces step portion 4a in an in-plane direction (left-right direction in FIG. 2) perpendicular to the height direction of each of protrusions 3 (up-down direction in FIG. 2). Step portion 5b faces step portion 5a in the in-plane direction. Step portion 6b faces step portion 6a in the in-plane direction. Step portion 7b faces step portion 7a in the in-plane direction. Top surface 4t is disposed between step portion 4a and step portion 4b, and is connected to step portion 4a and step portion 4b.

[0017] The step portion 4a has a smooth edge portion 4c. The step portion 4b has a smooth edge portion 4d. The step portion 5a has a smooth edge portion 5c. The step portion 5b has a smooth edge portion 5d. The step portion 6a has a smooth edge portion 6c. The step portion 6b has a smooth edge portion 6d. The step portion 7a has a smooth edge portion 7c. The step portion 7b has a smooth edge portion 7d. In this specification, a smooth edge portion means that the minimum radius of curvature of the edge portion is one-tenth or more of the diffraction wavelength of the relief type diffraction grating 1.

[0018] A method for manufacturing the relief type diffraction grating 1 of this embodiment will be described with reference to FIGS.

[0019] 3, a silicon nitride film 10 is formed on the main surface 2s of the silicon member 2. A portion of the main surface 2s of the silicon member 2 is covered with the silicon nitride film 10. The remaining portion of the main surface 2s of the silicon member 2 is exposed from the silicon nitride film 10.

[0020] For example, a silicon nitride film is formed on the entire main surface 2s of the silicon member 2 by low-pressure chemical vapor deposition (LPCVD). A photoresist (not shown) is applied to the silicon nitride film. The photoresist is exposed and developed to pattern the photoresist. The portions of the silicon nitride film exposed by the photoresist are removed by dry etching using CF-based plasma or wet etching using hot phosphoric acid. The photoresist is removed from the silicon member 2 using oxygen plasma or an organic solvent such as acetone. In this way, a silicon nitride film 10 is formed on a portion of the main surface 2s of the silicon member 2. The silicon nitride film formed by the LPCVD method can withstand the process of oxidizing the silicon member 2 (see FIG. 4). The thickness of the silicon nitride film 10 is, for example, in the range of 0.1 μm to 0.3 μm, which is smaller than the thickness of the photoresist (1 μm or more).

[0021] Referring to FIG. 4, the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 10 as a mask, a portion of the silicon member 2 is oxidized (local oxidation), converting the portion into a silicon oxide film 15. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 10 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 10 are converted into the silicon oxide film 15. The silicon oxide film 15 is formed to extend under the peripheral edge of the silicon nitride film 10, thereby lifting the peripheral edge of the silicon nitride film 10. The extension of the silicon oxide film 15 under the peripheral edge of the silicon nitride film 10 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0022] Referring to FIG. 5, silicon nitride film 10 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0023] 6, the silicon oxide film 15 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, to form step portions 4a and 4b on the silicon member 2. The step portion 4a has a smooth edge portion 4c. The step portion 4b has a smooth edge portion 4d. The edges 4c and 4d of the step portions 4a and 4b are smoothed by the local oxidation step (see FIG. 4) and the silicon oxide film selective removal step (see FIG. 6). The top surface 4t is part of the main surface 2s (see FIG. 3) of the silicon member 2, and is flat like the main surface 2s.

[0024] 7, a silicon nitride film 11 is formed on the top surface 4t and the step portion 4a of the silicon member 2. The step portion 4b and a portion of the silicon member 2 opposite the top surface 4t with respect to the step portion 4a in the in-plane direction (the left-right direction in FIG. 7) are exposed from the silicon nitride film 11. The silicon nitride film 11 is formed by the same method as the silicon nitride film 10. The thickness of the silicon nitride film 11 is, for example, in the range of 0.1 μm to 0.3 μm.

[0025] Referring to FIG. 8 , the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 11 as a mask, a portion of the silicon member 2 is oxidized (local oxidation), converting the portion into a silicon oxide film 16. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 11 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 11 are converted into the silicon oxide film 16. The silicon oxide film 16 is formed to extend under the peripheral edge of the silicon nitride film 11, lifting the peripheral edge of the silicon nitride film 11. The extension of the silicon oxide film 16 under the peripheral edge of the silicon nitride film 11 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0026] Referring to FIG. 9, silicon nitride film 11 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0027] 10, silicon oxide film 16 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, to form step portions 5a and 5b in silicon member 2. Step portion 5a has a smooth edge portion 5c. Step portion 5b has a smooth edge portion 5d. Edge portions 5c and 5d of step portions 5a and 5b are smoothed by the local oxidation step (see FIG. 8) and the silicon oxide film selective removal step (see FIG. 10).

[0028] 11 , a silicon nitride film 12 is formed on the top surface 4t and the step portions 4a and 5a of the silicon member 2. The step portions 4b and 5b and a portion of the silicon member 2 opposite the top surface 4t with respect to the step portion 5a in the in-plane direction (the left-right direction in FIG. 11 ) are exposed from the silicon nitride film 12. The silicon nitride film 12 is formed by the same method as the silicon nitride film 10. The thickness of the silicon nitride film 12 is, for example, in the range of 0.1 μm to 0.3 μm.

[0029] 12, the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 12 as a mask, a portion of the silicon member 2 is oxidized (local oxidation) to convert that portion into a silicon oxide film 17. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 12 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 12 are converted into the silicon oxide film 17. The silicon oxide film 17 is formed to extend under the peripheral edge of the silicon nitride film 12, lifting the peripheral edge of the silicon nitride film 12. The extension of the silicon oxide film 17 under the peripheral edge of the silicon nitride film 12 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0030] Referring to FIG. 13, silicon nitride film 12 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0031] 14, silicon oxide film 17 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, to form step portions 6a and 6b in silicon member 2. Step portion 6a has a smooth edge portion 6c. Step portion 6b has a smooth edge portion 6d. Edge portions 6c and 6d of step portions 6a and 6b are smoothed by the local oxidation step (see FIG. 12) and the silicon oxide film selective removal step (see FIG. 14).

[0032] 15 , a silicon nitride film 13 is formed on the top surface 4t and the step portions 4a, 5a, and 6a of the silicon member 2. The step portions 4b, 5b, and 6b and a portion of the silicon member 2 opposite the top surface 4t with respect to the step portion 6a in the in-plane direction (the left-right direction in FIG. 15 ) are exposed from the silicon nitride film 13. The silicon nitride film 13 is formed by the same method as the silicon nitride film 10. The thickness of the silicon nitride film 13 is, for example, in the range of 0.1 μm to 0.3 μm.

[0033] 16, the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 13 as a mask, a portion of the silicon member 2 is oxidized (local oxidation) to convert that portion into a silicon oxide film 18. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 13 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 13 are converted into the silicon oxide film 18. The silicon oxide film 18 is formed so as to extend under the peripheral edge of the silicon nitride film 13, thereby lifting the peripheral edge of the silicon nitride film 13. The extension of the silicon oxide film 18 under the peripheral edge of the silicon nitride film 13 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0034] Referring to FIG. 17, silicon nitride film 13 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0035] The silicon oxide film 18 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, forming step portions 7a and 7b (see FIG. 2) on the silicon member 2. The step portion 7a has a smooth edge portion 7c. The step portion 7b has a smooth edge portion 7d. The edges 7c and 7d of the step portions 7a and 7b are smoothed by the local oxidation step (see FIG. 16) and the silicon oxide film selective removal step. In this way, the relief type diffraction grating 1 shown in FIGS. 1 and 2 is obtained.

[0036] In this embodiment, the local oxidation process and the silicon oxide film selective removal process are each performed four times to form the four step portions 4a, 5a, 6a, and 7a and the four step portions 4b, 5b, 6b, and 7b. However, the local oxidation process and the silicon oxide film selective removal process may each be performed n times to form n step portions (where n is a natural number).

[0037] The effect of the manufacturing method of the relief type diffraction grating 1 of this embodiment will be described. The manufacturing method of the relief type diffraction grating 1 of this embodiment includes the steps of forming a first silicon nitride film (e.g., silicon nitride film 10) on the silicon member 2, oxidizing the silicon member 2 using the first silicon nitride film as a mask to convert a part of the silicon member 2 into a first silicon oxide film (e.g., silicon oxide film 15), removing the first silicon nitride film, and selectively removing the first silicon oxide film to form a first step portion (e.g., step portion 4a) in the silicon member 2.

[0038] By oxidizing (locally oxidizing) the silicon member 2 using the first silicon nitride film as a mask, the first silicon oxide film (e.g., silicon oxide film 15) can be formed with higher dimensional accuracy. Then, by selectively removing the first silicon oxide film, the relief-type diffraction grating 1 is manufactured. This improves the dimensional accuracy of the diffraction grating in the height direction of the diffraction grating and in the in-plane direction of the diffraction grating perpendicular to the height direction of the diffraction grating. According to the method for manufacturing the relief-type diffraction grating 1 of this embodiment, it is possible to manufacture a relief-type diffraction grating 1 with higher dimensional accuracy.

[0039] When the surface of a diffraction grating is formed by etching or film deposition, the surface of the diffraction grating becomes rough. Light scattering occurs on the surface of the diffraction grating, reducing the diffraction efficiency of the diffraction grating. In contrast, the surface of the silicon member 2 formed by selectively removing the first silicon oxide film (e.g., silicon oxide film 15) as in this embodiment has a higher smoothness. Light scattering on the surface of the diffraction grating is suppressed. According to the method for manufacturing the relief type diffraction grating 1 of this embodiment, it is possible to manufacture a relief type diffraction grating 1 with higher diffraction efficiency.

[0040] The relief type diffraction grating 1 of this embodiment is formed on a silicon member 2 made of a single material, silicon. Therefore, according to the method for manufacturing the relief type diffraction grating 1 of this embodiment, it is possible to manufacture a relief type diffraction grating 1 that has better temperature stability of diffraction efficiency than a relief type diffraction grating of a comparative example that is made of a plurality of materials with different linear expansion coefficients.

[0041] In the method for manufacturing the relief type diffraction grating 1 of this embodiment, the first step portion (for example, step portion 4a) has a smooth edge portion (for example, edge portion 4c).

[0042] Therefore, light scattering at the edge portion (for example, edge portion 4c) is suppressed. According to the method for manufacturing the relief type diffraction grating 1 of this embodiment, it is possible to manufacture a relief type diffraction grating 1 having higher diffraction efficiency.

[0043] The method for manufacturing the relief type diffraction grating 1 of this embodiment further includes the steps of forming a second silicon nitride film (e.g., silicon nitride film 11) on the top surface 4t of the silicon member 2 connected to the first step portion (e.g., step portion 4a) and on the first step portion, oxidizing the silicon member 2 using the second silicon nitride film as a mask to convert a part of the silicon member 2 into a second silicon oxide film (e.g., silicon oxide film 16), removing the second silicon nitride film, and selectively removing the second silicon oxide film to form a second step portion (e.g., step portion 5a) connected to the first step portion in the silicon member 2. Each of the protrusions 3 of the relief type diffraction grating 1 has a plurality of height levels.

[0044] Forming the convex portions 3 having multiple height levels by etching using photoresist as a mask requires a patterned, thick photoresist. If a thick photoresist is patterned by exposure and development, the thick photoresist cannot be patterned with high precision due to defocusing of the light used for exposure. In contrast, in the method for manufacturing the relief-type diffraction grating 1 of this embodiment, a silicon nitride film thinner than the photoresist is used to form the convex portions 3 having multiple height levels. Then, by oxidizing (locally oxidizing) the silicon member 2 using the silicon nitride film as a mask, the silicon oxide film can be formed with higher dimensional precision. The relief-type diffraction grating 1 is manufactured by selectively removing the silicon oxide film. Therefore, even if each of the convex portions 3 of the relief-type diffraction grating 1 has multiple height levels, a relief-type diffraction grating 1 with higher dimensional precision can be manufactured.

[0045] In the method for manufacturing the relief type diffraction grating 1 of this embodiment, the silicon member 2 is a silicon substrate 2a.

[0046] The relief type diffraction grating 1 of this embodiment is formed on a silicon substrate 2a made of a single material, silicon. Therefore, the method for manufacturing the relief type diffraction grating 1 of this embodiment makes it possible to manufacture a relief type diffraction grating 1 that has better temperature stability of diffraction efficiency than a relief type diffraction grating of a comparative example that is made of multiple materials with different linear expansion coefficients.

[0047] Embodiment 2 A relief type diffraction grating 1 of embodiment 2 will be described with reference to Figures 18 and 19. The relief type diffraction grating 1 of this embodiment has a similar configuration to the relief type diffraction grating 1 of embodiment 1, but differs from the relief type diffraction grating 1 of embodiment 1 in the following respects.

[0048] In the relief type diffraction grating 1 of this embodiment, each of the protrusions 3 has a single height level. The relief type diffraction grating 1 is a diffraction grating having a single height level. Each of the protrusions 3 has smooth side surfaces 3a, 3b. In this specification, smooth side surfaces means that the arithmetic mean roughness Ra of the side surfaces is one-tenth or less of the diffraction wavelength of the relief type diffraction grating 1. The side surfaces 3a, 3b do not have edges.

[0049] A method for manufacturing the relief type diffraction grating 1 of this embodiment will be described with reference to FIGS.

[0050] 20 , a silicon nitride film 10 is formed on a main surface 2s of the silicon member 2. A portion of the main surface 2s of the silicon member 2 is covered with the silicon nitride film 10. The remaining portion of the main surface 2s of the silicon member 2 is exposed from the silicon nitride film 10. The process of forming the silicon nitride film 10 shown in FIG. 20 is similar to the process of forming the silicon nitride film 10 shown in FIG.

[0051] 21, a portion of the silicon member 2 is oxidized (local oxidation) using the silicon nitride film 10 as a mask to change the portion of the silicon member 2 into a silicon oxide film 15. The local oxidation step shown in FIG. 21 is similar to the local oxidation step shown in FIG.

[0052] 22, silicon nitride film 10 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like. The step of removing silicon nitride film 10 shown in Fig. 22 is similar to the step of removing silicon nitride film 10 shown in Fig. 5.

[0053] 23 , the silicon oxide film 15 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, to form step portions 4 a and 4 b in the silicon member 2. The top surface 4 t is part of the main surface 2 s (see FIG. 20 ) of the silicon member 2, and is flat like the main surface 2 s. The top surface 4 t is disposed between the step portions 4 a and 4 b, and is connected to the step portions 4 a and 4 b. The step of removing the silicon oxide film 15 shown in FIG. 23 is similar to the step of removing the silicon oxide film 15 shown in FIG. 6 .

[0054] 24, a silicon nitride film 11 is formed on top surface 4t of silicon member 2. Step portions 4a and 4b are exposed from silicon nitride film 11. Silicon nitride film 11 is formed by the same method as silicon nitride film 10.

[0055] 25, the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 11 as a mask, a portion of the silicon member 2 is oxidized (local oxidation), converting that portion into a silicon oxide film 16. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 11 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 11 are converted into the silicon oxide film 16. The silicon oxide film 16 is formed to extend under the peripheral edge of the silicon nitride film 11, lifting the peripheral edge of the silicon nitride film 11. The extension of the silicon oxide film 16 under the peripheral edge of the silicon nitride film 11 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0056] Referring to FIG. 26, silicon nitride film 11 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0057] 27, the silicon oxide film 16 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, forming step portions 5a and 5b in the silicon member 2. Through the steps shown in FIGS. 24 to 27, the step portion 4a (see FIG. 23) becomes the step portion 5a, and the step portion 4b (see FIG. 23) becomes the step portion 5b. The step portion 5a is higher or deeper than the step portion 4a. The step portion 5b is higher or deeper than the step portion 4b. The step portion 5b faces the step portion 5a in the in-plane direction (the left-right direction in FIG. 27). The top surface 4t is disposed between the step portion 5a and the step portion 5b, and is connected to the step portion 5a and the step portion 5b.

[0058] 28, silicon nitride film 12 is formed on top surface 4t of silicon member 2. Step portions 5a and 5b are exposed from silicon nitride film 12. Silicon nitride film 12 is formed by the same method as silicon nitride film 10.

[0059] Referring to FIG. 29 , the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 12 as a mask, a portion of the silicon member 2 is oxidized (local oxidation) to convert that portion into a silicon oxide film 17. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 12 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 12 are converted into the silicon oxide film 17. The silicon oxide film 17 is formed to extend under the peripheral edge of the silicon nitride film 12, lifting the peripheral edge of the silicon nitride film 12. The extension of the silicon oxide film 17 under the peripheral edge of the silicon nitride film 12 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0060] Referring to FIG. 30, silicon nitride film 12 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0061] 31 , the silicon oxide film 17 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, forming step portions 6a and 6b in the silicon member 2. Through the steps shown in FIGS. 28 to 31 , the step portion 5a (see FIG. 27 ) becomes the step portion 6a, and the step portion 5b (see FIG. 27 ) becomes the step portion 6b. The step portion 6a is higher or deeper than the step portion 5a. The step portion 6b is higher or deeper than the step portion 5b. The step portion 6b faces the step portion 6a in the in-plane direction (the left-right direction in FIG. 31 ). The top surface 4t is disposed between the step portion 6a and the step portion 6b, and is connected to the step portion 6a and the step portion 6b.

[0062] 32, a silicon nitride film 13 is formed on top surface 4t of silicon member 2. Step portions 6a and 6b are exposed from silicon nitride film 13. Silicon nitride film 13 is formed by the same method as silicon nitride film 10.

[0063] Referring to FIG. 33 , the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 13 as a mask, a portion of the silicon member 2 is oxidized (local oxidation), converting that portion into a silicon oxide film 18. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 13 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 13 are converted into the silicon oxide film 18. The silicon oxide film 18 is formed to extend under the peripheral edge of the silicon nitride film 13, lifting the peripheral edge of the silicon nitride film 13. The extension of the silicon oxide film 18 under the peripheral edge of the silicon nitride film 13 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0064] Referring to FIG. 34, silicon nitride film 13 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0065] The silicon oxide film 18 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, forming smooth side surfaces 3a and 3b (see FIG. 19) on the silicon member 2. The step portion 6a (see FIG. 31) becomes a smooth side surface 3a, and the step portion 6b (see FIG. 31) becomes a smooth side surface 3b. The smooth side surface 3a is higher or deeper than the step portion 6a. The smooth side surface 3b is higher or deeper than the step portion 6b. The smooth side surface 3b faces the smooth side surface 3a in the in-plane direction (the left-right direction in FIG. 19). The top surface 4t is located between the side surfaces 3a and 3b and is connected to the side surfaces 3a and 3b. In this way, the relief-type diffraction grating 1 shown in FIGS. 18 and 19 is obtained.

[0066] In this embodiment, the local oxidation step and the silicon oxide film selective removal step are each performed four times, but depending on the height of the protrusion 3, the local oxidation step and the silicon oxide film selective removal step may each be performed n times (where n is a natural number), or the thickness of the silicon oxide film produced in the local oxidation step may be adjusted.

[0067] The method for manufacturing the relief type diffraction grating 1 of this embodiment has the following advantages in addition to the advantages of the method for manufacturing the relief type diffraction grating 1 of the first embodiment.

[0068] The method for manufacturing the relief-type diffraction grating 1 of this embodiment further includes the steps of forming a second silicon nitride film (e.g., silicon nitride film 11) on the top surface 4t of the silicon member 2, oxidizing the silicon member 2 using the second silicon nitride film as a mask to convert a portion of the silicon member 2 into a second silicon oxide film (e.g., silicon oxide film 16), removing the second silicon nitride film, and selectively removing the second silicon oxide film. When the first silicon oxide film (e.g., silicon oxide film 15) is selectively removed, a second step portion (e.g., step portion 4b) facing the first step portion (e.g., step portion 4a) is formed. The top surface 4t of the silicon member 2 is connected to the first step portion and the second step portion. When the silicon member 2 is oxidized using the second silicon nitride film as a mask, the first step portion and the second step portion are exposed from the second silicon nitride film. Each of the protrusions 3 of the relief-type diffraction grating 1 has smooth side surfaces (side surfaces 3a, 3b).

[0069] The silicon oxide film can be formed with higher precision by oxidizing (locally oxidizing) the silicon member 2 using the silicon nitride film as a mask. The silicon oxide film is then selectively removed to produce the relief type diffraction grating 1. Therefore, even if the height of each of the protrusions 3 is increased, the relief type diffraction grating 1 can be produced with higher dimensional precision.

[0070] Furthermore, the relief type diffraction grating 1 of this embodiment has no edge portions on the side surfaces 3 a, 3 b of the protrusions 3, and therefore no light scattering occurs at the edge portions. According to the method for manufacturing the relief type diffraction grating 1 of this embodiment, it is possible to manufacture a relief type diffraction grating 1 having higher diffraction efficiency.

[0071] Embodiment 3 A relief type diffraction grating 1 of embodiment 3 will be described with reference to Figures 35 and 36. The relief type diffraction grating 1 of this embodiment has a similar configuration to the relief type diffraction grating 1 of embodiment 1, but differs from the relief type diffraction grating 1 of embodiment 1 in the following respects.

[0072] In the relief type diffraction grating 1 of this embodiment, the step portion 4a has an angular edge portion 4c. The step portion 5a has an angular edge portion 5c. In this specification, an angular edge portion means that the minimum radius of curvature of the edge portion is less than one-tenth of the diffraction wavelength of the relief type diffraction grating 1. The step portion 4a has a flat side surface 8a. The step portion 5a has a flat side surface 8c. The side surface 3b is a smooth side surface.

[0073] A method for manufacturing the relief type diffraction grating 1 according to the third embodiment will be described with reference to FIGS.

[0074] 37 , a photoresist 20 is formed on the main surface 2s of the silicon member 2. A portion of the main surface 2s of the silicon member 2 is covered with the photoresist 20. The remaining portion of the main surface 2s of the silicon member 2 is exposed from the photoresist 20. The thickness of the photoresist 20 is 1 μm or more. The photoresist 20 is formed by applying the photoresist to the entire main surface 2s of the silicon member 2, exposing the photoresist to light, and developing the photoresist.

[0075] Referring to FIG. 38 , using the photoresist 20 as an etching mask, dry etching such as deep reactive ion etching (DRIE) is performed to remove portions of the silicon member 2 that are exposed from the photoresist 20. Step portions 4a and 4b are formed in the silicon member 2. The step portion 4a has a flat side surface 8a and an angular edge portion 4c. The step portion 4b faces the step portion 4a in the in-plane direction (the left-right direction in FIG. 38 ). The step portion 4b has a flat side surface 8b and an angular edge portion 4d. The flat side surfaces 8a and 8b may be perpendicular to the top surface 4t. The top surface 4t is disposed between the step portions 4a and 4b and is connected to the step portions 4a and 4b.

[0076] Referring to FIG. 39, photoresist 20 is removed from silicon member 2 using oxygen plasma or an organic solvent such as acetone.

[0077] 40 , photoresist 21 is formed on top surface 4t and step portion 4a of silicon member 2. Step portion 4b and a portion of silicon member 2 on the opposite side of step portion 4a from top surface 4t in the in-plane direction (left-right direction in FIG. 40 ) are exposed from photoresist 21. Photoresist 21 is thicker than photoresist 20. Photoresist 21 is formed by the same method as photoresist 20.

[0078] Referring to FIG. 41 , using the photoresist 21 as an etching mask, dry etching such as deep reactive ion etching (DRIE) is performed to remove portions of the silicon member 2 that are not covered by the photoresist 21. Step portions 5a and 5b are formed in the silicon member 2. The step portion 5a has a flat side surface 8c and an angular edge portion 5c. Through the steps shown in FIGS. 40 to 42 , the step portion 4b (see FIG. 39 ) becomes the step portion 5b. The step portion 5b is higher or deeper than the step portion 4b. The step portion 5b faces the step portions 4a and 5a in the in-plane direction (the left-right direction in FIG. 41 ). The step portion 5b has a flat side surface 8d and an angular edge portion 4d. The flat side surfaces 8c and 8d may be perpendicular to the top surface 4t. The top surface 4t is disposed between the step portion 4a and the step portion 5b and is connected to the step portion 4a and the step portion 5b.

[0079] Referring to FIG. 42, photoresist 21 is removed from silicon member 2 using oxygen plasma or an organic solvent such as acetone.

[0080] 43 , a silicon nitride film 10 is formed on the top surface 4t and the step portions 4a and 5a of the silicon member 2. The step portion 5b and a portion of the silicon member 2 opposite the top surface 4t with respect to the step portion 5a in the in-plane direction (the left-right direction in FIG. 43 ) are exposed from the silicon nitride film 10. The silicon nitride film 10 of this embodiment is formed by the same method as the silicon nitride film 10 of the first embodiment. The silicon nitride film 10 is thinner than each of the photoresists 20 and 21. The thickness of the silicon nitride film 10 is, for example, in the range of 0.1 μm to 0.3 μm.

[0081] Referring to FIG. 44, the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 10 as a mask, a portion of the silicon member 2 is oxidized (local oxidation), converting that portion into a silicon oxide film 15. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 10 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 10 are converted into the silicon oxide film 15. The silicon oxide film 15 is formed to extend under the peripheral edge of the silicon nitride film 10, lifting the peripheral edge of the silicon nitride film 10. The extension of the silicon oxide film 15 under the peripheral edge of the silicon nitride film 10 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0082] Referring to FIG. 45, silicon nitride film 10 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0083] Referring to FIG. 46 , the silicon oxide film 15 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, forming step portions 6 a and 6 b in the silicon member 2. The step portion 6 a has a smooth edge portion 6 c. The edge portion 6 c of the step portion 6 a is smoothed by the local oxidation process (see FIG. 44 ) and the silicon oxide film selective removal process (see FIG. 46 ). The step portion 5 b (see FIG. 42 ) becomes the step portion 6 b by the processes shown in FIGS. 43 to 46 . The step portion 6 b is higher or deeper than the step portion 5 b. The step portion 6 b faces the step portions 4 a, 5 a, and 6 a in the in-plane direction (the left-right direction in FIG. 46 ). The step portion 6 b has a smooth side surface. The side surface of the step portion 6 b is steeper than the step portion 6 a. The top surface 4t is disposed between the step portion 4a and the step portion 6b and is connected to the step portion 4a and the step portion 6b.

[0084] 47 , a silicon nitride film 11 is formed on the top surface 4t of the silicon member 2 and on the step portions 4a, 5a, and 6a. The step portion 6b and a portion of the silicon member 2 opposite the top surface 4t with respect to the step portion 6a in the in-plane direction (the left-right direction in FIG. 47 ) are exposed from the silicon nitride film 11. The silicon nitride film 11 of this embodiment is formed by the same method as the silicon nitride film 10 of this embodiment. The silicon nitride film 11 is thinner than each of the photoresists 20 and 21. The thickness of the silicon nitride film 11 is, for example, in the range of 0.1 μm to 0.3 μm.

[0085] Referring to FIG. 48, the silicon member 2 is placed in a thermal oxidation furnace (not shown). Using the silicon nitride film 11 as a mask, a portion of the silicon member 2 is oxidized (local oxidation), converting that portion into a silicon oxide film 16. Specifically, the portion of the silicon member 2 exposed from the silicon nitride film 11 and the portion of the silicon member 2 located below the peripheral edge of the silicon nitride film 11 are converted into the silicon oxide film 16. The silicon oxide film 16 is formed to extend under the peripheral edge of the silicon nitride film 11, lifting the peripheral edge of the silicon nitride film 11. The extension of the silicon oxide film 16 under the peripheral edge of the silicon nitride film 11 can be achieved with high reproducibility and high dimensional accuracy. The silicon member 2 is then removed from the thermal oxidation furnace.

[0086] Referring to FIG. 49, silicon nitride film 11 is selectively removed by dry etching using CF-based plasma or the like, or wet etching using hot phosphoric acid or the like.

[0087] The silicon oxide film 16 is selectively removed using a hydrofluoric acid solution or hydrofluoric acid vapor, forming a step portion 7a (see FIG. 36) on the silicon member 2. The step portion 7a has a smooth edge portion 7c (see FIG. 36). The edge portion 7c of the step portion 7a is smoothed by the local oxidation process (see FIG. 48) and the selective removal process of the silicon oxide film. The step portion 6b (see FIG. 46) has a smooth side surface 3b (see FIG. 36). The side surface 3b is higher or deeper than the side surface of the step portion 6b. The side surface 3b faces the step portions 4a, 5a, 6a, and 7a in the in-plane direction (the left-right direction in FIG. 36). The side surface 3b is steeper than the step portions 6a and 7a. The side surface 3b is gentler than the side surfaces of the step portion 4a and the step portion 5a. In this way, the relief-type diffraction grating 1 shown in FIGS. 35 and 36 is obtained.

[0088] In this embodiment, the step of removing the silicon member 2 using photoresist is performed twice to form the two step portions 4a and 5a, and then the local oxidation step and the selective removal step of the silicon oxide film are each performed twice to form the two step portions 6a and 7a. However, the step of removing the silicon member 2 using photoresist may be performed m times (where m is a natural number) to form m step portions, and then the local oxidation step and the selective removal step of the silicon oxide film may be performed n times (where n is a natural number) to form n step portions below the n step portions.

[0089] The method for manufacturing the relief type diffraction grating 1 of this embodiment has the following advantages in addition to the advantages of the method for manufacturing the relief type diffraction grating 1 of the first embodiment.

[0090] The method for manufacturing the relief type diffraction grating 1 of this embodiment further includes the steps of forming a photoresist (e.g., photoresist 20) on the silicon member 2, dry etching a portion of the silicon member 2 using the photoresist as an etching mask to form a second step portion (e.g., step portion 4a) in the silicon member 2, and removing the photoresist. A first silicon nitride film (e.g., silicon nitride film 10) is formed on the second step portion and on the top surface 4t of the silicon member 2 connected to the second step portion. The first step portion (e.g., step portion 6a) is located below the second step portion. Each of the protrusions 3 of the relief type diffraction grating 1 has a plurality of height levels.

[0091] When forming upper step portions (e.g., step portions 4a, 5a) by etching using photoresist as a mask, the photoresist can be made relatively thin. Therefore, even when etching using photoresist as a mask, the upper step portions can be formed with relatively high dimensional accuracy. However, when forming lower step portions (e.g., step portions 6a, 7a) by etching using photoresist as a mask, a thick, patterned photoresist is required. When a thick photoresist is patterned by exposure and development, the thick photoresist cannot be patterned with high accuracy due to defocusing of the light used for exposure. Therefore, when forming lower step portions (e.g., step portions 6a, 7a) by etching using photoresist as a mask, the dimensional accuracy of the lower step portions (e.g., step portions 6a, 7a) deteriorates.

[0092] In contrast, in this embodiment, to form the lower step portions (e.g., step portions 6a and 7a), oxidation (local oxidation) of the silicon member 2 is performed using a silicon nitride film thinner than the photoresist as a mask, and selective removal of the silicon oxide film is performed. By oxidizing the silicon member 2 using the silicon nitride film as a mask (local oxidation), the silicon oxide film can be formed with higher dimensional accuracy. The relief-type diffraction grating 1 is manufactured by selectively removing the silicon oxide film. Therefore, the dimensional accuracy of the lower step portions (e.g., step portions 6a and 7a) is improved. According to the manufacturing method of the relief-type diffraction grating 1 of this embodiment, a relief-type diffraction grating 1 with higher dimensional accuracy can be manufactured.

[0093] Furthermore, the in-plane dimensions of the convex portions 3 can be adjusted by etching using a photoresist as a mask to form the upper step portions (e.g., step portions 4a and 5a), which makes it possible to adjust the diffraction wavelength of the relief type diffraction grating 1.

[0094] In the method for manufacturing the relief type diffraction grating 1 of this embodiment, when a portion of the silicon member 2 is removed, a flat side surface (e.g., flat side surface 8b) facing the second step portion (e.g., step portion 4a) is formed in the silicon member 2. When the silicon member 2 is oxidized, the flat side surface is exposed from the first silicon nitride film (e.g., silicon nitride film 10). When the first silicon oxide film (e.g., silicon oxide film) is selectively removed, a side surface (e.g., side surface 6b) facing the first step portion (e.g., step portion 6a) and the second step portion and smoother than the first step portion and the second step portion is formed in the silicon member 2.

[0095] Therefore, it is possible to adjust the in-plane dimensions of the convex portions 3. This makes it possible to adjust the diffraction wavelength of the relief type diffraction grating 1.

[0096] Embodiment 4 A relief type diffraction grating 1 of embodiment 4 will be described with reference to Figures 50 and 51. The relief type diffraction grating 1 of this embodiment has a similar configuration to the relief type diffraction grating 1 of embodiment 1, but differs from the relief type diffraction grating 1 of embodiment 1 in the following respects.

[0097] In this embodiment, the silicon member 2 is a silicon layer 33 of a silicon-on-insulator (SOI) substrate 30. The SOI substrate 30 is made of a silicon substrate 31 and a SiO 2 It includes an insulating layer 32 and a silicon layer 33. SiO 2 The insulating layer 32 is located between the silicon substrate 31 and the silicon layer 33. The relief type diffraction grating 1 is formed in the silicon layer 33.

[0098] Each side surface 3b of the protrusion 3 is a flat side surface 8e facing the step portions 4a, 5a, 6a, and 7a. The side surface 3b may be perpendicular to the top surface 4t. The side surface 3b is made of SiO 2 It may extend to the insulating layer 32 .

[0099] A method for manufacturing the relief type diffraction grating 1 according to the fourth embodiment will be described with reference to FIGS.

[0100] 52, an SOI substrate 30 is prepared. The SOI substrate 30 is made of a silicon substrate 31 and a SiO 2 It includes an insulating layer 32 and a silicon layer 33. SiO 2 The insulating layer 32 is located between the silicon substrate 31 and the silicon layer 33. The silicon layer 33 is made of SiO 2 The main surface 2 s is on the side opposite to the insulating layer 32 .

[0101] 53 , a relief type diffraction grating 1 is formed on a silicon layer 33 by a manufacturing method similar to that of the relief type diffraction grating 1 of the first embodiment. The relief type diffraction grating 1 includes a periodic uneven structure 9. The periodic uneven structure 9 of the relief type diffraction grating 1 includes a plurality of periodically arranged protrusions 3. Each of the protrusions 3 includes a side surface 3a, a side surface 3b opposite to the side surface 3a, and a top surface 4t. Step portions 4a, 5a, 6a, and 7a are formed on the side surface 3a. Step portions 4b, 5b, 6b, and 7b are formed on the side surface 3b.

[0102] 54, photoresist 35 is formed on top surface 4t of silicon layer 33 and on step portions 4a, 5a, 6a, and 7a. Step portions 4b, 5b, 6b, and 7b are exposed from photoresist 35. Photoresist 35 is thicker than silicon nitride films 10, 11, 12, and 13 of the first embodiment. Photoresist 35 is formed by a method similar to that for photoresist 20 of the third embodiment.

[0103] Using the photoresist 35 as an etching mask, the portion of the silicon layer 33 exposed by the photoresist 35 is removed by dry etching such as deep reactive ion etching (DRIE). A flat side surface 8e, that is, a side surface 3b (see FIG. 51 ), is formed. In the etching process of the silicon layer 33, the SiO 2 The insulating layer 32 functions as an etch stop layer. Then, the photoresist 21 is removed using oxygen plasma or an organic solvent such as acetone. In this way, the relief type diffraction grating 1 shown in FIGS. 50 and 51 is obtained.

[0104] The method for manufacturing the relief type diffraction grating 1 of this embodiment has the following advantages in addition to the advantages of the method for manufacturing the relief type diffraction grating 1 of the first embodiment.

[0105] The method for manufacturing the relief type diffraction grating 1 of this embodiment further includes a step of etching the silicon member 2 (e.g., the silicon layer 33) to form a flat side surface 8e facing the first step portion (e.g., the step portion 4a).

[0106] Therefore, it is possible to adjust the in-plane dimensions of the convex portions 3. This makes it possible to adjust the diffraction wavelength of the relief type diffraction grating 1.

[0107] In the method for manufacturing the relief type diffraction grating 1 of this embodiment, the silicon member 2 is the silicon layer 33 of the silicon-on-insulator substrate 30 .

[0108] The relief type diffraction grating 1 of this embodiment is formed on a silicon layer 33 made of a single material, silicon. Therefore, according to the method for manufacturing the relief type diffraction grating 1 of this embodiment, it is possible to manufacture a relief type diffraction grating 1 that has better temperature stability of diffraction efficiency than a relief type diffraction grating of a comparative example that is made of a plurality of materials with different linear expansion coefficients.

[0109] In the etching process of the silicon layer 33, the SiO 2 The insulating layer 32 functions as an etch stop layer, which allows the height of the protrusions 3 to be accurately determined. According to the method for manufacturing the relief type diffraction grating 1 of this embodiment, it is possible to manufacture a relief type diffraction grating 1 with higher dimensional accuracy.

[0110] Fifth Embodiment An optical scanning device 40 according to a fifth embodiment will be described with reference to Fig. 55. The optical scanning device 40 is an application example of the relief type diffraction grating 1 according to the first to fourth embodiments.

[0111] The optical scanning device 40 includes a relief type diffraction grating 1, a frame 41, beams 42 and 44, an anchor 43, a coil 45, and a magnetic field generator 46.

[0112] The relief type diffraction grating 1 is coupled to a frame 41 via a beam 42. The frame 41 is coupled to an anchor 43 via a beam 44. A coil 45 is provided on the frame 41. The coil 45 is wound around the relief type diffraction grating 1. A magnetic field generator 46 generates a magnetic field 47. The magnetic field generator 46 is, for example, a permanent magnet.

[0113] When an AC current is applied to the coil 45, an electromagnetic force is applied to the frame 41 by the AC current flowing through the coil and a magnetic field 47 from the magnetic field generator 46. This electromagnetic force causes the frame 41 to oscillate around the beams 44. The relief type diffraction grating 1 oscillates together with the frame 41, scanning the light incident on the relief type diffraction grating 1.

[0114] The optical scanning device 40 of this embodiment has the following effects. The optical scanning device 40 includes a relief type diffraction grating 1. The relief type diffraction grating 1 has high dimensional accuracy. Therefore, the relief type diffraction grating 1 has high diffraction efficiency. The optical scanning device 40 of this embodiment can scan the light incident on the relief type diffraction grating 1 with low optical loss.

[0115] The presently disclosed embodiments 1 to 5 should be considered to be illustrative in all respects and not restrictive. Unless there is a contradiction, at least two of the presently disclosed embodiments 1 to 5 may be combined. For example, the relief type diffraction grating of embodiments 1 to 3 may be formed in the silicon layer 33 of the SOI substrate 30, as in embodiment 4. The scope of the present disclosure is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims.

[0116] 1 Relief type diffraction grating, 2 Silicon member, 2a Silicon substrate, 2s Main surface, 3 Convex portion, 3a, 3b, 6b Side, 4a, 4b, 5a, 5b, 6a, 6b, 7a, 7b Step portion, 4c, 4d, 5c, 5d, 6c, 6d, 7c, 7d Edge portion, 4t Top surface, 8a, 8b, 8c, 8d, 8e Flat side, 9 Periodic uneven structure, 10, 11, 12, 13 Silicon nitride film, 15, 16, 17, 18 Silicon oxide film, 20, 21, 35 Photoresist, 30 Silicon-on-insulator substrate, 31 Silicon substrate, 33 Silicon layer, 32 Insulating layer, 40 Optical scanning device, 41 Frame, 42, 44 Beam, 43 Anchor, 45 Coil, 46 Magnetic field generator, 47 Magnetic field.

Claims

1. A method for manufacturing a relief type diffraction grating, comprising the steps of: forming a first silicon nitride film on a silicon member; oxidizing the silicon member using the first silicon nitride film as a mask to convert a portion of the silicon member into a first silicon oxide film; removing the first silicon nitride film; and selectively removing the first silicon oxide film to form a first step portion in the silicon member.

2. The method for producing a relief type diffraction grating according to claim 1, wherein the first step portion has a smooth edge portion.

3. A method for manufacturing a relief type diffraction grating as claimed in claim 1 or claim 2, further comprising the steps of: forming a second silicon nitride film on a top surface of the silicon member connected to the first step portion and on the first step portion; oxidizing the silicon member using the second silicon nitride film as a mask to convert a part of the silicon member into a second silicon oxide film; removing the second silicon nitride film; and selectively removing the second silicon oxide film to form a second step portion connected to the first step portion in the silicon member, wherein each of the protrusions of the relief type diffraction grating has a plurality of height levels.

4. A method for manufacturing a relief type diffraction grating as claimed in claim 1 or claim 2, further comprising the steps of: forming a second silicon nitride film on a top surface of the silicon member; oxidizing the silicon member using the second silicon nitride film as a mask to convert a portion of the silicon member into a second silicon oxide film; removing the second silicon nitride film; and selectively removing the second silicon oxide film, wherein when the first silicon oxide film is selectively removed, a second step portion opposing the first step portion is formed, the top surface of the silicon member is connected to the first step portion and the second step portion, when the silicon member is oxidized using the second silicon nitride film as a mask, the first step portion and the second step portion are exposed from the second silicon nitride film, and each of the convex portions of the relief type diffraction grating has a smooth side surface.

5. A method for manufacturing a relief type diffraction grating as claimed in claim 1 or claim 2, further comprising the steps of: forming a photoresist on said silicon member; dry etching a part of said silicon member using said photoresist as an etching mask to form a second step portion in said silicon member; and removing said photoresist, wherein said first silicon nitride film is formed on said second step portion and on a top surface of said silicon member connected to said second step portion, said first step portion is below said second step portion, and each of said protrusions of said relief type diffraction grating has a plurality of height levels.

6. A method for manufacturing a relief type diffraction grating as described in claim 5, wherein, when removing the portion of the silicon member, a flat side surface facing the second step portion is formed on the silicon member, when the silicon member is oxidized, the flat side surface is exposed from the first silicon nitride film, and when the first silicon oxide film is selectively removed, a side surface facing the first step portion and the second step portion and smoother than the first step portion and the second step portion is formed on the silicon member.

7. A method for manufacturing a relief type diffraction grating according to any one of claims 1 to 5, further comprising the step of etching the silicon member to form a flat side surface facing the first step portion.

8. A method for producing a relief type diffraction grating according to any one of claims 1 to 7, wherein the silicon member is a silicon substrate.

9. A method for producing a relief type diffraction grating according to any one of claims 1 to 7, wherein the silicon member is a silicon layer of a silicon-on-insulator substrate.

Citation Information

Patent Citations

  • Four-step grating and preparation method thereof

    CN102495444A

  • Manufacture of digital braze diffraction grating

    JP2000105307A

  • Manufacture of element

    JP2000155207A

  • Semiconductor device

    JP2009094210A

  • Pattern formation method and pattern formation body

    JP2013077665A