Organic fiber cord for tire reinforcing layer and aircraft tire using the same
A hybrid organic fiber cord with a high-tensile core and fatigue-resistant sheath strands addresses the issue of low abrasion fatigue in tire reinforcing layers, enhancing wear resistance and maintaining cord strength for improved aircraft tire performance.
Patent Information
- Application Number
- PCT/JP2023/044313
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2023-12-11
- Publication Date
- 2024-10-24
AI Technical Summary
Highly rigid organic fibers used in tire reinforcing layers, such as aramid and rayon fibers, tend to have low wear and fatigue resistance, leading to reduced strength when they come into contact with each other, compromising the abrasion fatigue resistance of the reinforcing cords.
A hybrid organic fiber cord with a core strand made of high-tensile organic fibers like aromatic polyamide or aramid fibers and a sheath strand made of aliphatic polyamide, polyester, or polyvinyl alcohol fibers, where the sheath strand is wound helically around the core to enhance wear resistance while maintaining cord strength.
The hybrid organic fiber cord improves the wear resistance of the tread portion by increasing the stiffness of the reinforcing layer without deteriorating the abrasion fatigue resistance of the reinforcing cords, making it suitable for aircraft tires.
Smart Images

Figure JP2023044313_24102024_PF_FP_ABST
Abstract
Description
Organic fiber cord for tire reinforcing layer and aircraft tire using same
[0001] The present invention relates to an organic fiber cord for a tire reinforcing layer and an aircraft tire using the same (hereinafter also simply referred to as "organic fiber cord" and "tire"). More specifically, the present invention relates to an organic fiber cord for a tire reinforcing layer used to reinforce the tread portion of a tire and an improvement in an aircraft tire using the same.
[0002] In tires such as aircraft tires, the wear resistance of the tread portion can be improved by increasing the in-plane rigidity of the tread portion. One method for increasing the in-plane rigidity of the tread portion is to use high-rigidity organic fibers for the belt cords to increase the rigidity of the belt layer.
[0003] As prior art related to belt cords for aircraft tires, for example, Patent Document 1 describes a pneumatic tire suitable for use on aircraft, in which the belt ply includes a plurality of cables including at least two yarns made of aramid filaments and at least one core yarn made of at least one filament of a material selected from the group consisting of polyamide and polyester. Patent Document 2 also describes a high-speed, heavy-load pneumatic radial tire suitable for use on aircraft, in which the main belt layer uses a belt ply including organic fiber cords in which aromatic polyamide cords and aliphatic polyamide cords are twisted together.
[0004] US Patent Publication No. 4,832,101 JP 2004-256611 A
[0005] However, highly rigid organic fibers such as aramid fibers and rayon fibers tend to have low abrasion fatigue resistance. Therefore, if highly rigid organic fibers are used for the belt cords to increase the rigidity of the belt layer, there is a risk that the strength of the belt cords will decrease due to friction when the belt cords come into contact with each other.
[0006] Therefore, an object of the present invention is to provide an organic fiber cord for a tire reinforcing layer that can suppress deterioration in the abrasion fatigue resistance of the reinforcing cord even when a high-rigidity organic fiber is applied to the reinforcing cord of a reinforcing layer such as a belt layer to increase the rigidity of the reinforcing layer and thereby improve the abrasion resistance of the tread portion, and an aircraft tire using the same.
[0007] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by using, as the reinforcing cord of the reinforcing layer, a hybrid organic fiber cord having a specific structure consisting of a combination of specific types of core strands and sheath strands, and have thus completed the present invention.
[0008] That is, the organic fiber cord for a tire reinforcing layer of the present invention is as follows.
[0009] (1) An organic fiber cord for a tire reinforcing layer, comprising a core including at least one core strand and a sheath including at least one sheath strand, the sheath being formed by spirally winding the sheath around the outer periphery of the core, wherein the core strand is made of an organic fiber having an initial tensile resistance of 55 cN / dtex or more, and the sheath strand is made of at least one fiber selected from aliphatic polyamide fibers, polyester fibers, polyvinyl alcohol fibers, and cotton. This makes it possible to suppress deterioration in the abrasion fatigue resistance of the reinforcing cord, even when a high-rigidity organic fiber is used for the reinforcing cord of the reinforcing layer, thereby increasing the rigidity of the reinforcing layer and thereby improving the abrasion resistance of the tread portion.
[0010] (2) The organic fiber cord for a tire reinforcing layer according to (1), wherein the core strand is made of an aromatic polyamide fiber, thereby further improving the wear resistance of the tread portion.
[0011] (3) The organic fiber cord for a tire reinforcing layer according to (2), wherein the core strand is made of aramid fiber, thereby further improving the wear resistance of the tread portion.
[0012] (4) The total fineness of the core is 1.4 × 10 3~1.2 × 10 4 The organic fiber cord for a tire reinforcing layer of any one of (1) to (3) is dtex, which can further improve the wear resistance of the tread portion.
[0013] (5) The organic fiber cord for a tire reinforcing layer according to any one of (1) to (4), wherein the total fineness of the sheath strands is smaller than the total fineness of the core, thereby maximizing the effect of the core in improving the wear resistance of the tread portion and achieving weight reduction.
[0014] (6) An organic fiber cord for a tire reinforcing layer according to any one of (1) to (5) used in an aircraft tire. The organic fiber cord for a tire reinforcing layer of the present invention is useful when applied to an aircraft tire.
[0015] (7) The organic fiber cord for a tire reinforcing layer according to (6), which is used in an endless belt layer disposed in a tread portion of the aircraft tire, wherein a strip material formed by rubber-coating a reinforcing cord extends from one tire width direction end toward the other tire width direction end, is folded back at the other tire width direction end, extends from the other tire width direction end toward the one tire width direction end, and is folded back at the one tire width direction end, repeating this process, so that the reinforcing cord is spirally wound in the tire circumferential direction. The organic fiber cord for a tire reinforcing layer of the present invention is particularly useful when applied to an endless belt layer in an aircraft tire.
[0016] (8) An aircraft tire characterized in that the organic fiber cord for a tire reinforcing layer of any one of (1) to (7) is used as a reinforcing cord for a reinforcing layer that reinforces a tread portion, whereby even when the abrasion resistance of the tread portion is improved by applying a high-rigidity organic fiber to the reinforcing cord of the reinforcing layer and thereby increasing the rigidity of the reinforcing layer, deterioration of the abrasion fatigue resistance of the reinforcing cord can be suppressed.
[0017] According to the present invention, by adopting the above-described configuration, it has become possible to realize an organic fiber cord for a tire reinforcing layer, which can suppress deterioration in the abrasion fatigue resistance of the reinforcing cord, even when a high-rigidity organic fiber is applied to the reinforcing cord of a reinforcing layer of a belt layer or the like to increase the rigidity of the reinforcing layer and thereby improve the abrasion resistance of the tread portion, and an aircraft tire using the same.
[0018] Fig. 1 is a schematic view showing a width direction cross section of an example of an organic fiber cord for a tire reinforcing layer of the present invention. Fig. 2 is a width direction cross section of an example of an aircraft tire of the present invention. Fig. 3 is an explanatory view showing the configuration of an endless belt layer according to the present invention. Fig. 4 is a schematic view showing a width direction cross section of another example of an organic fiber cord for a tire reinforcing layer of the present invention. Fig. 5 is a schematic view showing a width direction cross section of yet another example of an organic fiber cord for a tire reinforcing layer of the present invention. Fig. 6 is a schematic view showing a width direction cross section of yet another example of an organic fiber cord for a tire reinforcing layer of the present invention. Fig. 7 is a schematic view showing a width direction cross section of yet another example of an organic fiber cord for a tire reinforcing layer of the present invention.
[0019] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0020] The compounds and materials described herein may be derived partially or entirely from fossil resources, biological resources such as plant resources, or recycled resources such as used tires, or may be derived from a mixture of two or more of fossil resources, biological resources, and recycled resources.
[0021] Fig. 1 shows a schematic diagram of a widthwise cross section of an example of an organic fiber cord for a tire reinforcing layer of the present invention. As shown in the figure, the organic fiber cord 10 for a tire reinforcing layer of the present invention has a core 11 including at least one core strand 1 and a sheath 12 including at least one sheath strand 2, with the sheath strand 2 spirally wound around the outer periphery of the core 11 to form the sheath 12. More specifically, the organic fiber cord 10 for a tire reinforcing layer of the present invention shown in Fig. 1 has a core 11 formed by second-twisting three core strands 1 made of a single-twisted yarn obtained by first-twisting raw yarn, and a sheath 12 made of ten sheath strands 2 made of single-twisted yarn obtained by first-twisting raw yarn, with the sheath strands 2 spirally wound around the outer periphery of the core 11 to form the sheath 12.
[0022] In the cord 10 of the present invention, the core strand 1 constituting the core 11 is made of organic fibers having an initial tensile resistance of 55 cN / dtex or more. If the initial tensile resistance of the organic fibers constituting the core strand 1 is less than 55 cN / dtex, sufficient wear resistance of the tread portion cannot be ensured when the cord is applied to a tire. The initial tensile resistance of the organic fibers constituting the core strand 1 is preferably 3.0 x 10 2 cN / dtex or more 1.1×10 3 In the present invention, the initial tensile resistance of the organic fiber can be measured in accordance with JIS L 1017.
[0023] In the cord 10 of the present invention, the sheath strands 2 constituting the sheath 12 are made of at least one material selected from aliphatic polyamide fibers such as 6-nylon, 6,6-nylon, and 4,6-nylon, polyester fibers, polyvinyl alcohol (PVA) fibers, and cotton. Examples of polyester fibers include polyethylene terephthalate (PET) fibers.
[0024] According to the present invention, by using a high-rigidity organic fiber that satisfies a predetermined initial tensile resistance as the core strand 1 that constitutes the core 11, it is possible to increase the rigidity of the tire reinforcing layer, and therefore, when the cord 10 of the present invention is applied to a tire, the in-plane rigidity of the tread portion can be improved and the abrasion resistance of the tread portion can be ensured. On the other hand, by using the above-mentioned predetermined organic fiber that has high resistance to abrasion fatigue as the sheath strand 2 that constitutes the sheath 12 and arranging this sheath 12 on the outer periphery of the core 11, breakage of the sheath strands due to contact or friction between the sheath strands is unlikely to occur even when the cords come into contact with each other, and as a result, it is possible to prevent a decrease in cord strength and improve cord durability.
[0025] In the cord 10 of the present invention, the desired effects can be obtained by using an organic fiber that satisfies the above-mentioned specified initial tensile resistance as the core strand 1 that constitutes the core 11, and by using the above-mentioned specified organic fiber as the sheath strand 2 that constitutes the sheath 12. However, the cord 10 is more preferably configured as follows.
[0026] For the core strand 1, examples of organic fibers that satisfy the above-mentioned initial tensile resistance include aromatic polyamide fibers and rayon fibers, and aromatic polyamide fibers are preferably used. By using aromatic polyamide fibers, the wear resistance of the tread portion can be further improved when the cord 10 of the present invention is applied to a tire. Examples of aromatic polyamide fibers include aramid fibers.
[0027] The total fineness of the core 11 is preferably 1.4×10 3 ~1.2 × 10 4 dtex, and more preferably 1.0 x 10 4 ~1.2 × 10 4 By setting the total fineness of the core within the above range, the wear resistance of the tread portion can be further improved when the cord 10 of the present invention is applied to a tire.
[0028] Furthermore, the total fineness of the sheath strands 2 is preferably lower than the total fineness of the core 11. This can further improve the wear resistance of the tread portion.
[0029] 4 to 7 are schematic views of widthwise cross sections of other examples of the organic fiber cord for a tire reinforcing layer of the present invention. The structure of the organic fiber cord for a tire reinforcing layer of the present invention is not limited to those shown in the drawings.
[0030] The organic fiber cord 110 for a tire reinforcing layer shown in FIG. 4 has a core 111 consisting of one core strand 101 made of a single-twisted yarn obtained by first twisting raw yarn, and a sheath 112 consisting of ten sheath strands 102 made of single-twisted yarn obtained by first twisting raw yarn, and has a structure in which the sheath strands 102 are wound spirally around the outer periphery of the core 111 to form the sheath 112.
[0031] The organic fiber cord 210 for a tire reinforcing layer shown in FIG. 5 has a core 211 formed by second-twisting three core strands 201 each made of a single-twist yarn obtained by first-twisting raw yarn, and a sheath 212 made of ten sheath strands 202 each made of a single-twist yarn obtained by first-twisting raw yarn, and the sheath 212 is formed by winding the sheath strands 202 spirally around the outer periphery of the core 211 to form the sheath 212.
[0032] The organic fiber cord 310 for a tire reinforcing layer shown in FIG. 6 has a core 311 consisting of one core strand 301 made of a single-twisted yarn obtained by first twisting raw yarn, and a sheath 312 consisting of eight sheath strands 302 formed by second twisting three of the single-twisted yarn obtained by first twisting raw yarn, and has a structure in which the sheath strands 302 are spirally wound around the outer periphery of the core 311 to form the sheath 312.
[0033] The organic fiber cord 410 for a tire reinforcing layer shown in FIG. 7 has a core 411 formed by second-twisting three core strands 401 each made of a single-twist yarn obtained by first-twisting raw yarn, and a sheath 412 made of eight sheath strands 402 each made of a single-twist yarn obtained by first-twisting raw yarn, and three sheath strands 402 each made of a single-twist yarn obtained by second-twisting raw yarn, and the sheath 412 is formed by winding the sheath strands 402 spirally around the outer periphery of the core 411 to form the sheath 412.
[0034] The cord 10 of the present invention is used as a reinforcing cord in a reinforcing layer of a tire, and there are no particular limitations on the type of tire or the configuration of the reinforcing layer. The cord 10 of the present invention is particularly suitable for use in aircraft tires, and is particularly preferably applied to an endless belt layer in which a strip material formed by rubber-coating a reinforcing cord arranged in the tread portion of an aircraft tire extends from one tire width direction end to the other tire width direction end, is folded back at the other tire width direction end, extends from the other tire width direction end to one tire width direction end, and is folded back at the one tire width direction end, repeating this process, so that the reinforcing cord is spirally wound around the tire circumferential direction. The cord 10 of the present invention is useful when applied to aircraft tires, and in particular, in the endless belt layer, since the cords are folded back at the tire width direction end as described above, contact between the cords occurs at this portion, which is likely to result in a decrease in cord strength, and therefore the application of the organic fiber cord for a tire reinforcing layer of the present invention is particularly useful.
[0035] 3 is an explanatory diagram showing the configuration of the endless belt layer according to the present invention. The illustrated endless belt layer 40 is formed by spirally winding a strip material 41 in the tire circumferential direction, the strip material 41 being made of rubber-coated reinforcing cords, extending from one tire width direction end to the other tire width direction end, turning back at the other tire width direction end, and then extending again from the other tire width direction end to one tire width direction end and turning back at the one tire width direction end, repeating this process.
[0036] Figure 2 shows a widthwise cross-sectional view of an example of an aircraft tire of the present invention. The illustrated aircraft tire 100 includes a tread portion 21 and a pair of sidewall portions 22 and bead portions 23 extending radially inward of the tread portion 21. A bead core 31 is embedded in each of the pair of bead portions 23, and a carcass 32 extends in a toroidal shape between the pair of bead cores 31 to form the tire skeleton. In addition, a belt 33 consisting of five or more belt layers is disposed radially outward of the carcass 32 in the tread portion 21. CL in the figure indicates the tire equator.
[0037] The aircraft tire 100 of the present invention uses the organic fiber cord for a tire reinforcing layer of the present invention as the reinforcing cord for the reinforcing layer that reinforces the tread portion 21. This increases the in-plane rigidity of the tread portion 21, improving the wear resistance of the tread portion 21, while preventing a decrease in cord strength when the cords come into contact with each other.
[0038] In the tire 100 of the present invention, the reinforcing layer to which the organic fiber cord for a tire reinforcing layer of the present invention is applied is not particularly limited as long as it is a reinforcing layer that reinforces the tread portion 21. Specifically, the organic fiber cord for a tire reinforcing layer of the present invention can be applied to the belt 33 disposed in the tread portion 21.
[0039] In the illustrated tire 100, the belt 33 is made up of six belt layers 33a to 33f. There are no particular limitations on the configuration of the six belt layers 33a to 33f, but it is preferable that the six belt layers 33a to 33f include at least one inclined belt layer in which reinforcing cords are arranged at an angle of, for example, 2 to 40 degrees with respect to the tire circumferential direction. More preferably, the inclined belt layer includes the endless belt layer described above. In the illustrated example, five belt layers 33b to 33f are endless belt layers. The endless belt layer is also called an endless belt layer because there are no cut surfaces of the reinforcing cords at both ends in the tire width direction.
[0040] The organic fiber cord for a tire reinforcing layer of the present invention is preferably applied to the endless belt layer among the belts 33. In the endless belt layer, the cords are folded back at the ends in the tire width direction as described above, and therefore contact between the cords occurs at these portions, which is likely to result in a decrease in cord strength, and therefore application of the organic fiber cord for a tire reinforcing layer of the present invention is particularly useful.
[0041] Furthermore, it is preferable that the belt 33 includes at least one spiral belt layer formed by spirally winding reinforcing cords substantially along the tire circumferential direction. In the illustrated example, the belt layer 33 a located at the innermost position in the tire radial direction of the belt 33 is a spiral belt layer.
[0042] Although several modified belt structures are exemplified below, the present invention is not limited to these belt structures. The width of each belt layer constituting the belt 33 can be set appropriately, and the relationship in width between the belt layers is not particularly limited.
[0043] (i) For example, in the above example, the number of layers of the inclined belt (e.g., endless belt layer) can be 6 to 9. Or, (ii) For example, in the above example, the carcass cord can be a hybrid cord made by twisting aramid fiber and nylon fiber. Or, (iii) For example, a configuration can be used in which spiral belt layers are arranged on the radially inner and outer sides of the inclined belt (e.g., endless belt layer). As an example, a configuration can be used in which a four-layer inclined belt (e.g., endless belt layer) is arranged on the radially outer side of a two-layer spiral belt layer, and a three-layer spiral belt layer is arranged on the radially outer side of this inclined belt layer (e.g., endless belt layer). Or, (iv) For example, a configuration can be used in which a two-layer inclined belt (e.g., endless belt layer) using reinforcing cords made of aramid fiber is arranged on the radially outer side of a six-layer spiral belt layer using reinforcing cords made of aramid fiber. Alternatively, (v) for example, a configuration may be used in which six inclined belt layers (e.g., endless belt layers) are arranged on the radially outer side of one spiral belt layer. Alternatively, (vi) for example, a configuration may be used in which four inclined belt layers (e.g., endless belt layers) are arranged on the radially outer side of two spiral belt layers. Alternatively, (vii) a configuration may be used in which two inclined belt layers (e.g., endless belt layers) are arranged on the radially outer side of six spiral belt layers. In any of the examples, the material and number of cords of the carcass are not particularly limited.
[0044] When applying the organic fiber cord for a tire reinforcing layer of the present invention to a tire, it is preferable to coat the cord with an adhesive composition in order to ensure adhesion to rubber. Any adhesive composition that is usually used for adhesive treatment of organic fiber cords may be used, but in the present invention, it is preferable to use the adhesive composition described below.
[0045] Examples of the adhesive composition include an adhesive composition containing a thermoplastic polymer (A) having at least one crosslinkable functional group as a pendant group and substantially no addition-reactive carbon-carbon double bonds in its main chain structure, a heat-reactive aqueous urethane resin (B), and an epoxy compound (C), and optionally further containing a rubber latex (D). Treating an organic fiber cord with such an adhesive composition can improve the adhesion between the organic fiber cord (particularly a polyethylene terephthalate cord) and an elastomer (coating rubber) at high temperatures.
[0046] Conventionally, adhesive treatment of organic fiber cords (especially polyethylene terephthalate cords) has been performed using a so-called two-bath process, in which epoxy or isocyanate is applied to the cord surface and then treated with a resin (hereinafter referred to as RFL resin) made by mixing resorcinol, formaldehyde, and latex. However, this method can cause the resin used in the first bath to become very hard, increasing the strain input to the organic fiber cord and reducing the cord fatigue resistance. Furthermore, while such RFL resins can exhibit sufficient cord-elastomer adhesive strength at room temperature, adhesive strength can be drastically reduced at temperatures above 130°C. In contrast, by using a one-bath mixed liquid (adhesive composition) containing a thermoplastic polymer (A) having at least one crosslinkable functional group as a pendant group and substantially not containing an addition-reactive carbon-carbon double bond in its main chain structure, a thermally reactive aqueous urethane resin (B), and an epoxy compound (C), it is possible to ensure sufficient adhesion to the elastomer (coating rubber) even at high temperatures of 180°C or higher without curing the organic fiber cord.
[0047] The main chain of the thermoplastic polymer (A) mainly has a linear structure, and the main chain is preferably, for example, an ethylenic addition polymer such as an acrylic polymer, a vinyl acetate polymer, or a vinyl acetate-ethylene polymer; a urethane high molecular weight polymer; etc. However, the thermoplastic polymer (A) is not limited to the above-mentioned ethylenic addition polymer and urethane high molecular weight polymer as long as it has the function of suppressing resin fluidity at high temperatures and ensuring the breaking strength of the resin by crosslinking the functional groups of the pendant groups.
[0048] The functional group of the pendant group of the thermoplastic polymer (A) is preferably an oxazolidine group, a bismaleimide group, a (blocked) isocyanate group, an aziridine group, a carbodiimide group, a hydrazino group, an epoxy group, an epithio group, or the like.
[0049] The above-mentioned thermoplastic polymer (A), heat-reactive aqueous urethane resin (B), epoxy compound (C), and rubber latex (D) can be those described in Japanese Patent Application No. 2023-040157 or Japanese Patent Application No. 2023-030762.
[0050] In the adhesive treatment of the organic fiber cord (particularly polyethylene terephthalate cord), it is preferable to use a three-type mixed liquid (adhesive composition) of the thermoplastic polymer (A), the heat-reactive aqueous urethane resin (B), and the epoxy compound (C) as a one-bath treatment liquid, and to use a normal RFL resin liquid as a two-bath treatment liquid. In the adhesive treatment, it is also possible to treat with only one bath using a mixed liquid (adhesive composition) of the thermoplastic polymer (A), the heat-reactive aqueous urethane resin (B), the epoxy compound (C), and the rubber latex (D).
[0051] In the adhesive composition, the proportion (dry mass ratio) of the thermoplastic polymer (A) is preferably 2 to 75%, the proportion (dry mass ratio) of the heat-reactive aqueous urethane resin (B) is preferably 15 to 87%, the proportion (dry mass ratio) of the epoxy compound (C) is preferably 11 to 70%, and the proportion (dry mass ratio) of the rubber latex (D) is preferably 20% or less.
[0052] On the other hand, from the viewpoint of environmental protection, it is preferable to use a dip treatment liquid that does not contain resorcinol or formalin as an adhesive composition for organic fiber cords. Examples of such dip treatment liquids include a composition containing (a) a rubber latex having an unsaturated diene and (b) one or more compounds selected from a compound having a polyether skeleton structure and an amine functional group, a compound having an acrylamide structure, a polypeptide, a polylysine, and a carbodiimide. Examples of such dip treatment liquids include a composition containing, in addition to the rubber latex having an unsaturated diene (a) and the compound (b), one or more compounds selected from (c) an aqueous compound having a (thermally dissociable blocked) isocyanate group, a polyphenol (d), and a polyvalent metal salt (e).
[0053] Other examples of the dipping treatment liquid that does not contain resorcinol or formalin include a composition containing polyphenols (I) and aldehydes (II). Such a composition may further contain at least one of an isocyanate compound (III) and a rubber latex (IV) in addition to the polyphenols (I) and aldehydes (II).
[0054] The adhesive composition for treating (coating) the organic fiber cord with an adhesive contains polyphenols (I) and aldehydes (II), so that good adhesive properties can be exhibited even when resorcinol is not used in consideration of the environmental load.
[0055] [Polyphenols (I)] The adhesive composition contains polyphenols (I) as a resin component, thereby improving adhesion to organic fiber cords. The polyphenols (I) are typically water-soluble polyphenols, and are not particularly limited as long as they are polyphenols other than resorcinol (resorcinol). The number of aromatic rings or hydroxyl groups in the polyphenols (I) can be appropriately selected.
[0056] From the viewpoint of realizing better adhesive properties, the polyphenols (I) preferably have two or more hydroxyl groups, and more preferably three or more hydroxyl groups. When the polyphenols have three or more hydroxyl groups, the polyphenol or polyphenol condensate is soluble in the adhesive composition (dip treatment liquid) containing water. This allows the polyphenols to be uniformly distributed in the adhesive composition, thereby realizing better adhesive properties. Furthermore, when the polyphenols (I) are polyphenols containing multiple (two or more) aromatic rings, each of the aromatic rings has two or three hydroxyl groups at the ortho, meta, or para positions.
[0057] As the polyphenols (I), for example, those described as polyphenol compounds in WO 2022 / 130879 can be used. These polyphenols (I) may be used alone or in combination of two or more.
[0058] [Aldehydes (II)] When the adhesive composition contains aldehydes (II) as a resin component in addition to the polyphenols (I), high adhesiveness can be achieved together with the polyphenols (I). Here, the aldehydes (II) are not particularly limited and can be appropriately selected depending on the required performance. In this specification, the aldehydes (II) also include derivatives of aldehydes that are generated from aldehydes.
[0059] Examples of the aldehydes (II) include monoaldehydes such as formaldehyde, acetaldehyde, butylaldehyde, acrolein, propionaldehyde, chloral, butylaldehyde, caproaldehyde, and allylaldehyde, and aliphatic dialdehydes such as glyoxal, malonaldehyde, succinaldehyde, glutaraldehyde, and adipaldehyde, aldehydes having an aromatic ring, and dialdehyde starch. These aldehydes (II) may be used singly or in combination of two or more.
[0060] The aldehydes (II) are preferably aldehydes having an aromatic ring or contain aldehydes having an aromatic ring, because this allows for better adhesiveness to be obtained. Furthermore, the aldehydes (II) preferably do not contain formaldehyde. Here, "does not contain formaldehyde" means, for example, that the formaldehyde content of the total mass of the aldehydes is less than 0.5 mass%.
[0061] In the adhesive composition, polyphenols (I) and aldehydes (II) are in a condensed state, and the mass ratio of the polyphenols to the aldehydes having an aromatic ring (content of aldehydes having an aromatic ring / content of polyphenols) is preferably 0.1 or more and 3 or less. In this case, the hardness and adhesive properties of the resin, which is the product of the condensation reaction between the polyphenols and the aldehydes having an aromatic ring, are more suitable. From the same viewpoint, the mass ratio of the polyphenols to the aldehydes having an aromatic ring (content of aldehydes having an aromatic ring / content of polyphenols) in the adhesive composition is more preferably 0.25 or more and more preferably 2.5 or less. Note that the above mass ratio is the mass of the dry matter (solid content ratio).
[0062] The total content of polyphenols (I) and aldehydes (II) in the adhesive composition is preferably 3 to 30% by mass. This is because better adhesion can be ensured without impairing workability, etc. From the same viewpoint, the total content of polyphenols (I) and aldehydes (II) in the adhesive composition is more preferably 5% by mass or more, and more preferably 25% by mass or less. The above total content is the mass of the dry product (solid content ratio).
[0063] [Isocyanate Compound (III)] The adhesive composition preferably further contains an isocyanate compound (III) in addition to the polyphenols (I) and aldehydes (II) described above. In this case, the adhesive composition can further enhance the adhesiveness due to a synergistic effect with the polyphenols (I) and the aldehydes (II).
[0064] Here, the isocyanate compound (III) is a compound that has the effect of promoting adhesion to a resin material (e.g., a phenol / aldehyde resin obtained by condensing polyphenols (I) and aldehydes (II)) that is the adherend of the adhesive composition, and is a compound that has an isocyanate group as a polar functional group. These isocyanate compounds (III) may be used alone or in combination of two or more.
[0065] The isocyanate compound (III) is not particularly limited, but from the viewpoint of further improving adhesion, it preferably contains a (blocked) isocyanate group-containing aromatic compound. When the adhesive composition contains a (blocked) isocyanate group-containing aromatic compound, the (blocked) isocyanate group-containing aromatic compound is distributed in a position near the interface between the organic fiber cord and the adhesive composition, resulting in a further adhesion-promoting effect, and this effect can further improve the adhesion of the adhesive composition to the organic fiber cord.
[0066] As the (blocked) isocyanate group-containing aromatic compound, those described in Japanese Patent Application No. 2023-040157 and those described in Japanese Patent Application No. 2023-030762 can be used.
[0067] The content of the isocyanate compound (III) in the adhesive composition is not particularly limited, but from the viewpoint of more reliably ensuring excellent adhesion, it is preferably 5 to 65% by mass. From the same viewpoint, the content of the isocyanate compound (III) in the adhesive composition is more preferably 10% by mass or more, and more preferably 45% by mass or less. The above content is the mass of the dry product (solid content ratio).
[0068] [Rubber Latex (IV)] The adhesive composition may further contain substantially rubber latex (IV) in addition to the polyphenols (I), aldehydes (II), and isocyanate compound (III) described above, which can further enhance the adhesiveness of the adhesive composition to rubber members.
[0069] Here, the rubber latex (IV) is not particularly limited, and examples thereof include natural rubber (NR), as well as synthetic rubbers such as polyisoprene rubber (IR), styrene-butadiene copolymer rubber (SBR), polybutadiene rubber (BR), ethylene-propylene-diene rubber (EPDM), chloroprene rubber (CR), halogenated butyl rubber, acrylonitrile-butadiene rubber (NBR), and vinylpyridine-styrene-butadiene copolymer rubber (Vp). These rubber latexes (IV) may be used alone or in combination of two or more.
[0070] When preparing the adhesive composition containing the rubber latex (IV), it is preferable to mix the rubber latex (IV) with the phenol (I) and the aldehyde (II) before compounding the isocyanate compound (III).
[0071] The content of the rubber latex (IV) in the adhesive composition is preferably 20% by mass or more, more preferably 25% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less.
[0072] The method for producing the adhesive composition is not particularly limited, and examples thereof include a method of mixing raw materials such as polyphenols (I), aldehydes (II), and rubber latex (IV) and aging the mixture, or a method of mixing polyphenols (I) and aldehydes (II) and aging the mixture, and then adding rubber latex (IV) and aging the mixture. When an isocyanate compound (III) is contained in the raw materials, the method for producing the adhesive composition may also be a method of adding rubber latex (IV), aging the mixture, and then adding the isocyanate compound (III).
[0073] In the tire of the present invention, although not shown, a protective layer can be disposed on the radially outer side of the belt 33. The protective layer is formed by arranging a plurality of cords extending in a wavy pattern in the tire circumferential direction in parallel with each other and covering them with a coating rubber. The cords in the protective layer can be, for example, organic fiber cords made of aromatic polyamide fiber (aramid fiber) or the like.
[0074] In the tire of the present invention, the carcass 32 can be a radial carcass consisting of two or more carcass plies. The number of carcass plies is not particularly limited as long as it is two or more, and can be, for example, 3 to 8, preferably 6 to 8, or more. In the example shown, the carcass ply constituting the carcass 32 has a carcass ply main body extending in a toroidal shape between a pair of bead cores 31, and a carcass ply turn-up portion extending from the carcass ply main body and folded back around the bead cores 31 from the inner side to the outer side in the tire width direction. One or more carcass plies can also be a down ply consisting only of a carcass ply main body extending in a toroidal shape between a pair of bead cores 31. Although not shown, the radial positions of the ends of two or more carcass plies are preferably different from the viewpoint of preventing end-related failures, but can also be the same. Organic fiber cords can be used as ply cords reinforcing the carcass ply, and the cord 10 of the present invention can also be used.
[0075] In the illustrated example, a bead filler 34 is disposed on the radially outer side of the bead core 31. The illustrated bead filler 34 has a generally triangular cross section whose width in the tire width direction tapers from the radially inner side to the radially outer side of the tire, but is not limited thereto and the bead filler 34 may have various cross-sectional shapes. For example, one or more types of known hard rubber may be used for the bead filler 34. Although not illustrated, the tire 100 also has an inner liner disposed to cover its inner surface.
[0076] The present invention will be described in more detail below using specific examples.
[0077] [Test Method for Abrasion Fatigue Resistance of Organic Fibers] 6,6-nylon, aramid fiber, and rayon fiber yarns were prepared, and a test to evaluate abrasion fatigue resistance was conducted by rubbing the two yarns together. Specifically, both ends of one yarn (A) were clamped in a chuck, and the other yarn (B) was crossed with the yarn (A) and hung from the front to the back. A load (0.018 gf / dtex) corresponding to the fineness of the yarn (B) was applied to one end of the yarn (B), and the other end of the yarn (B) was clamped in the chuck. The angle between the front yarn and the back yarn of the yarn (B) was 40 degrees. The chuck clamping the other end of the yarn (B) was moved up and down 6 mm back and forth 2,500 times at a frequency of 2 Hz, and the strength of the yarn (B) was measured before the test (0 times), after 1,500 times, and after 2,500 times, and the strength of each fiber was expressed as an index, with the strength at 0 times being 100. The results are shown in Table 1 below.
[0078]
[0079] From the results shown in the above table, it was confirmed that high-rigidity organic fibers such as aramid fiber and rayon fiber have poor abrasion fatigue resistance compared to nylon, which has lower rigidity.
[0080] [Evaluation of Tire Wear Resistance] The wear performance was evaluated for tires of Reference Examples 1 to 3, in which the organic fiber cords shown in the table below were used as reinforcing cords for the endless belt layer having the structure shown in Figure 3 among the belts of aircraft tires. In all Reference Examples, the end count of the reinforcing cords in the endless belt layer, the arrangement angle of the reinforcing cords in the endless belt layer relative to the tire circumferential direction, and the tire structure were the same. The results were expressed as an index, with the evaluation result of Reference Example 1 being set to 100. The smaller the value, the less wear there was and the better the result.
[0081]
[0082] *1) The initial tensile resistance value measured for each organic fiber in accordance with JIS L 1017. *2) The tensile rigidity under a load of 200 N was determined for the dipped cord obtained by dipping each reinforcing cord in the adhesive composition, and this value is expressed as an index with the tensile rigidity of the dipped cord of Reference Example 1 set to 100. *3) The treat rigidity calculated based on the following formula is expressed as an index with the treat rigidity of Reference Example 1 set to 100. Treat rigidity = Cord rigidity × Number of cord ends in treat *4) The evaluation result of the circumferential wear resistance of Reference Example 3 is an estimated value.
[0083] From the results shown in the table above, it was confirmed that when rayon fiber or aramid fiber, which have high initial tensile resistance, are used as the reinforcing cords of the endless belt layer, high treat rigidity is obtained and the tire's wear resistance performance is excellent. Also, it was confirmed that 6,6-nylon, an aliphatic polyamide fiber, is superior to rayon fiber and aramid fiber in terms of abrasion fatigue resistance. Therefore, it can be expected that the abrasion resistance and durability of the tire can be improved by using a fiber with high initial tensile resistance for the core strand and a fiber with high abrasion fatigue resistance for the sheath strand.
[0084] REFERENCE SIGNS LIST 1,101,201,301,401 Core strand 2,102,202,302,402 Sheath strand 10,110,210,310,410 Organic fiber cord for tire reinforcing layer 11,111,211,311,411 Core 12,112,212,312,412 Sheath 21 Tread portion 22 Sidewall portion 23 Bead portion 31 Bead core 32 Carcass 33 Belt 33a to 33f Belt layer 34 Bead filler 40 Endless belt layer 41 Strip material 100 Aircraft tire
Claims
1. An organic fiber cord for a tire reinforcing layer, comprising a core including at least one core strand and a sheath including at least one sheath strand, the sheath being wound in a spiral shape around the outer periphery of the core to form the sheath, wherein the core strand is made of an organic fiber having an initial tensile resistance of 55 cN / dtex or more, and the sheath strand is made of at least one type selected from the group consisting of aliphatic polyamide fiber, polyester fiber, polyvinyl alcohol fiber and cotton.
2. The organic fiber cord for a tire reinforcing layer according to claim 1, wherein said core strand is made of aromatic polyamide fiber.
3. The organic fiber cord for a tire reinforcing layer according to claim 2, wherein the core strand is made of aramid fiber.
4. The total fineness of the core is 1.4 x 10 3 ~1.2 x 10 4 2. The organic fiber cord for a tire reinforcing layer according to claim 1, which is dtex.
5. The organic fiber cord for a tire reinforcing layer according to claim 1, wherein the total fineness of said sheath strands is smaller than the total fineness of said core.
6. The organic fiber cord for a tire reinforcing layer according to claim 1, which is used in aircraft tires.
7. The organic fiber cord for a tire reinforcing layer according to claim 6, which is used in an endless belt layer in which a strip material formed by rubber-coating a reinforcing cord is arranged in the tread portion of the aircraft tire, extends from one end in the tire width direction to the other end in the tire width direction, is folded back at the other end in the tire width direction, extends from the other end in the tire width direction to one end in the tire width direction, and is folded back at the one end in the tire width direction, repeating this process so that the reinforcing cord is wound spirally in the circumferential direction of the tire.
8. An aircraft tire, comprising the organic fiber cord for tire reinforcing layers according to claim 1 as a reinforcing cord for a reinforcing layer for reinforcing the tread portion.
Citation Information
Patent Citations
Tire for bicycle
JP1989164604A
JP1989170001U
Hybrid cord with high tensile strength and high elongation at break
JP2014500413A
Elevator rope and manufacturing method therefor
WO2017138228A1