NV center-containing nanodiamond particle and method for producing same

The described method enhances nanodiamond particle ODMR contrast through specific thermal treatments and heteroatom incorporation, addressing the limitations of existing NV center nanodiamonds for advanced biosensing and bioimaging by achieving high sensitivity and precision in microenvironment detection.

WO2024219059A1PCT designated stage expired Publication Date: 2024-10-24DAICEL CORP +1

Patent Information

Application Number
PCT/JP2024/004227
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-02-08
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing nanodiamond particles with NV centers have insufficient ODMR contrast for high-precision sensing, and there is a lack of materials with color centers derived from different atoms like SiV, limiting their effectiveness in biosensing and bioimaging applications.

Method used

The production method involves gas-phase oxidation of nanodiamonds at 560-620°C followed by high-temperature mixed acid treatment to enhance ODMR contrast, achieving a 7% or more ODMR contrast in 10% of bright spots and a maximum Rabi vibration contrast of 25% or more, and optionally incorporating heteroatom-V centers like SiV.

Benefits of technology

The method results in nanodiamond particles with excellent ODMR contrast, enabling high-sensitivity optical detection of microenvironment changes, including temperature, and allows for non-invasive biological imaging with sufficient signal strength, even at the cellular level.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024004227_24102024_PF_FP_ABST
    Figure JP2024004227_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This nanodiamond particle satisfies the following conditions (i) and (ii), or (i) and (iii), or (i), (ii), and (iii), and has a fluorescence emission peak originating from nitrogen-vacancy (NV) centers: (i) for a 1 mass% aqueous suspension of the particles coated on a glass substrate, the percentage of the number of bright spots showing an at least 7% ODMR contrast, in bright spots for which NV center ODMR is observed, is at least 10%; (ii) the ODMR contrast is at least 0.12; and (iii) the contrast for the Rabi oscillation is at least 25% as the maximum value.
Need to check novelty before this filing date? Find Prior Art

Description

Nanodiamond particles having NV centers and method for producing the same

[0001] The present invention relates to nanodiamond particles having NV centers and a method for producing the same.

[0002] Fluorescent nanodiamonds have been attracting attention as fluorescent probes for biosensing, bioimaging, and other microenvironment measurements. - Optically detected magnetic resonance (ODMR) using center-containing nanodiamonds is attracting attention. - The ODMR activity of center-containing nanodiamond particles has been reported previously, but the intensity was insufficient (Patent Document 1). Furthermore, none of them also contained color centers derived from heteroatoms such as SiV. Some nanodiamonds possessed different nitrogen defects, such as NVN, but these were produced by annealing under special conditions. Non-Patent Document 1 describes the gas-phase oxidation of nanodiamond particles obtained by the detonation method at 425°C for 5 hours, followed by a mixed acid treatment at 130°C for 3 days, but the ODMR intensity was insufficient due to the low gas-phase oxidation temperature.

[0003] Patent No. 6117812

[0004] Nanoscale Adv. 2022, 4, 2268-2277

[0005] One object of the present invention is to provide an NV center-containing nanodiamond having excellent ODMR contrast.

[0006] The present invention provides the following nanodiamond particles and a method for producing the same. [1] Nanodiamond particles having a fluorescence emission peak derived from a nitrogen-vacancy (NV) center, satisfying the following condition (i): (i) When a 1% by mass aqueous suspension of the particles is applied to a glass substrate, 10% or more of the bright spots exhibiting an ODMR contrast of 7% or more are present. [2] The nanodiamond particles according to claim 1 further satisfy the following conditions (ii) and / or (iii): (ii) an ODMR contrast of 12% or more, and (iii) a maximum contrast in Rabi oscillation of 25% or more. [3] Fluorescent nanodiamond particles according to [1] or [2], further comprising a heteroatom-V center. [4] A method for producing a fluorescent nanodiamond according to any one of [1] to [3], comprising subjecting the nanodiamond raw material obtained in the detonation step to gas-phase oxidation at a temperature of 560 to 620°C, followed by a high-temperature, long-term mixed acid treatment at a temperature of 120 to 340°C for 36 to 120 hours. [5] A method for producing fluorescent nanodiamonds according to [4], which does not involve a post-treatment process.

[0007] According to the present invention, it is possible to provide nanodiamond particles (NDs) that have NV centers with excellent ODMR contrast and can perform highly accurate and highly sensitive sensing by optically detecting changes in the microenvironment, including temperature, via magnetic resonance. The NDs of the present invention have NV centers with excellent ODMR contrast, so that the NV centers in the individual NDs are small nano-sized particles and can be easily detected. - For example, the NDs of the present invention can be introduced into a living body non-invasively due to their small diameter, and can also generate sufficient signals, making them excellent probes for visualizing intracellular biological phenomena.

[0008] Configuration diagram of confocal microscope device. Example of bright spot mapping of nanodiamond particles obtained in Example 1 (undoped). Measurement results of fluorescence spectrum at a typical bright spot in fluorescence mapping of nanodiamond particles (undoped) obtained in Example 1. Measurement results of fluorescence spectrum at a typical bright spot in fluorescence mapping of nanodiamond particles (Si-doped) obtained in Example 2. MW: Sequence for microwave Rabi oscillation measurement. S: Signal. R: Reference. ODMR measurement results at a typical bright spot in fluorescence mapping of nanodiamond particles (undoped) obtained in Example 1. ODMR measurement results at a typical bright spot in fluorescence mapping of nanodiamond particles (Si-doped) obtained in Example 2. Rabi oscillation measurement results at a typical bright spot in fluorescence mapping of nanodiamond particles ((a) Si-doped, (b) undoped) obtained in Example 1 or 2. Temperature sensitivity measurement and T2 measurement for typical NV centers in Si-DNDs. All measurements shown in this figure were performed on the same bright spot (Si-DND aggregate) in the confocal image. Figures a) to d) are measurements taken in zero magnetic field (no external magnetic field applied), while e) and f) are measurements taken with a static magnetic field applied. a) Emission spectrum of the bright spot. b) The blue and red dots are ODMR spectra measured at sample temperatures T = 295 K and T = 313 K, respectively. The blue and red lines show the fitting results of the double Lorentzian function for each spectrum. c) Temperature dependence of the zero-field splitting constant D. The average value of the fitting results for the two peaks is shown. The rate of change of D with respect to sample temperature T (dD / dT) was calculated from the linear approximation (red line) of the D value obtained by fitting. The error bars were calculated from the standard error of the fitting using the double Lorentzian function. d) Integration time (t) measured at room temperature (T = 295 K). int ) Temperature uncertainty (standard deviation of sample temperature) σ T The red line is The fitting results are shown in Fig. 1. The temperature sensitivity η is int σ at = 1s T From the fitting results, e) Rabi oscillation measurement results when a static magnetic field is applied (m S = 0 ⇔ m S= -1). The diagram above shows the pulse sequence in Rabi vibration measurement (from top to bottom: laser, microwave, and luminescence detection). f) Hahn echo measurement results (T2). The measurement results are By fitting, T2 was calculated as T2 = 1.84 μs. - and SiV - a) Confocal image of Si-DND aggregates. - and SiV - The bright spots observed in both cases are circled. b) Fluorescence spectrum of the bright spot in a). NV - Zero phonon line (ZPL, 637 nm) of SiV and SiV - c) NV measured at two temperature levels, 295 K and 313 K. - ODMR spectrum of NV. - The zero-field splitting constant D of SiV measured at temperatures of 300 K and 313 K was found to vary linearly with temperature, with dD / dT = -84.4±9.1 kHz / K. - f) Emission spectrum of SiV - Temperature dependence of the ZPL peak wavelength. Peak wavelength λ p varies linearly with temperature, and Δλ p / ΔT = 0.014 ± 0.002 nm / K. g) Graph of the size distribution of Si-DNDs. Schematic of the device for temperature sensing of Si-DNDs.

[0009] The nanodiamond particles of the present invention satisfy the following essential condition (i), and preferably also satisfy the following conditions (ii) and / or (iii): (i) When a 1% by mass aqueous suspension of the particles is applied to a glass substrate, 10% or more of the bright spots where NV center ODMR is observed exhibit an ODMR contrast of 7% or more. (ii) The ODMR contrast is 12% or more. (iii) The maximum contrast in Rabi oscillation is 25% or more. The number of bright spots and ODMR contrast can be measured, for example, using a confocal microscope device configured as shown in Figure 1. A glass substrate coated with an aqueous suspension of nanodiamond particles is placed on an objective lens, and fluorescence intensity mapping (detecting emission at wavelengths longer than 645 nm) is performed on 100 x 100 points in a sample area appropriate for ODMR measurement, such as 532 nm excitation light, 100 μm x 100 μm, or 30 μm x 30 μm, to determine the number of bright spots. Microwaves are applied to each bright spot through a copper wire previously installed on the glass substrate, and NV -The resonance frequency (2870 MHz) of the center in the static magnetic field is swept within a range of ±50 MHz, and changes in fluorescence intensity (photon counts) are detected. The rate of change (decrease) of fluorescence intensity at the resonance frequency relative to the fluorescence intensity at frequencies away from the resonance frequency is called the ODMR contrast. Plotting the fluorescence intensity against the frequency sweep yields a negative peak at the resonance frequency. This peak may be split by distortion of the nanodiamond crystal. Regarding the ODMR contrast obtained in this manner, the proportion of bright spots exhibiting 7% or more ODMR contrast among those where NV center ODMR is observed is preferably 10% or more, more preferably 15% or more, even more preferably 20% or more, particularly preferably 30% or more, and most preferably 40% or more. Furthermore, the proportion of bright spots exhibiting 8% or more ODMR contrast among those where NV center ODMR is observed is preferably 5% or more, more preferably 10% or more, even more preferably 15% or more, particularly preferably 20% or more, and most preferably 30% or more. Furthermore, among the bright spots where NV center ODMR was observed, the percentage of bright spots exhibiting 10% or more ODMR contrast is preferably 2% or more, more preferably 5% or more, even more preferably 10% or more, and particularly preferably 15% or more. Furthermore, among the bright spots where NV center ODMR was observed, the percentage of bright spots exhibiting 12% or more ODMR contrast is preferably 1% or more, more preferably 2% or more, even more preferably 3% or more, and particularly preferably 5% or more. Bright spot mapping is preferably performed in a wavelength range that avoids the peak wavelength of Raman scattering of nanodiamonds, but is not particularly limited as long as the fluorescence from the NV center is detected. Furthermore, the excitation wavelength is not particularly limited within the wavelength range that excites the NV center. The contrast in Rabi oscillations can be measured using the above-mentioned confocal microscope device by pulsing the laser and microwave (resonant frequency in ODMR) according to the measurement sequence and operating the opening and closing of the observation channel (photon counting). Controlling the spin state of the NV center using pulsed lasers and microwaves allows for more accurate contrast measurements.The maximum contrast in the Rabi oscillation is preferably 25% or more, more preferably 26% or more, even more preferably 27% or more, particularly preferably 28% or more, and most preferably 29% or more. Furthermore, at randomly selected bright spots where ODMR is observed, the average contrast in the Rabi oscillation is preferably 15% or more, more preferably 16% or more, even more preferably 17% or more, particularly preferably 18% or more, particularly preferably 19% or more, or even 20% or more. If the nanodiamond particles have a heteroatom-V center other than nitrogen, further testing can be performed in a wavelength range including the ZPL of the heteroatom-V center. Since the ZPL wavelength (peak top wavelength) may vary depending on the structure of the fluorescent center, the number of bright spots emitting fluorescence at the ZPL peak within the range of "ZPL ± X nm (0≦X≦5)" is measured and the percentage is calculated. For example, in the case of SiV, both the ZPL of 738 nm (±0 nm) and a ZPL slightly different from 738 nm are conceivable. However, even if the ZPL slightly deviates, it is unlikely to deviate by more than 5 nm from the known ZPL (738 nm), so it falls within the range of ZPL ±X nm (0≦X≦5). The average primary particle size of the nanodiamond particles of the present invention is preferably 2-70 nm, more preferably 2.5-60 nm, even more preferably 3-55 nm, particularly preferably 3.5-50 nm, and most preferably 5-50 nm. The average primary particle size can be determined from the results of powder X-ray diffraction (XRD) analysis using the Scherrer equation. An example of an XRD measurement device is a fully automated multipurpose X-ray diffractometer (manufactured by Rigaku Corporation).

[0010] The sp obtained from the nanodiamond particles of the present invention by Raman spectroscopy 2 Carbon and sp 3 Carbon peak area ratio (sp 2 Carbon / sp 3 The sp2 carbon content is preferably 0.01 to 7, or 0.05 to 3, more preferably 0.1 to 1.2, or 0.1 to 1, even more preferably 0.1 to 0.5, and particularly preferably 0.1 to 0.3. The oxidation treatment of the present invention reduces the proportion of sp2 carbon, thereby increasing the fluorescence intensity. 2 Carbon and sp 3Carbon peak area ratio (sp 2 Carbon / sp 3 The carbon content can be measured by micro-Raman spectroscopy using, for example, a 325 nm laser and a micro-Raman spectrometer. 2 The carbon peak area is 1250 cm -1 and 1328cm -1 It refers to the total area of ​​two peaks that appear in the vicinity, and sp 3 The carbon peak area is 1500 cm -1 and 1590cm -1 The Raman microspectroscopy device may be, for example, a LabRAM HR Evolution microscopic laser Raman spectrophotometer (manufactured by Horiba, Ltd.).

[0011] The pH of the nanodiamond particles of the present invention when dispersed in water at a concentration of 3 wt% is preferably 1 to 12. The shape of the nanodiamond particles of the present invention is not particularly limited, but is preferably spherical, ellipsoidal, or polyhedral.

[0012] The BET specific surface area of ​​the nanodiamond particles of the present invention is preferably 20 to 900 m 2 / g, 25–800 m 2 / g, 30-700 m 2 / g, 35-600 m 2 / g, 50-500 m 2 / g or 100 to 400 m 2 / g, more preferably 150 to 250 m 2 / g. The BET specific surface area can be measured by nitrogen adsorption. An example of a device for measuring the BET specific surface area is the BELSORP-mini II (manufactured by Microtrac BEL Co., Ltd.). The BET specific surface area can be measured, for example, under the following conditions: - Amount of powder measured: 40 mg - Pre-drying: 120°C, vacuum treatment for 3 hours - Measurement temperature: -196°C (liquid nitrogen temperature)

[0013] When the nanodiamond of the present invention contains doped heteroatoms other than nitrogen, the heteroatom content is preferably 0.0001 to 10.0% by mass, more preferably 0.0001 to 5.0% by mass, and even more preferably 0.0001 to 1.0% by mass. The heteroatom content can be measured, for example, by inductively coupled plasma atomic emission spectroscopy (ICP-AES), XRF, or SIMS (secondary ion mass spectrometry). When the heteroatom is a Group 14 element such as Si, Ge, Sn, or Pb, the heteroatom content of the nanodiamond can be quantified in an acidic solution after alkali fusion. The doped heteroatom preferably forms a heteroatom-V center, and the heteroatom-V center preferably has a ZPL. The heteroatom-V center concentration in the nanodiamond particles of the present invention is preferably 1×10 10 / cm 3 More preferably, 2×10 10 ~1×10 19 / cm 3 The heteroatom-V center concentration can be determined, for example, using a confocal laser microscope or a fluorescence absorption spectrometer. For the determination of heteroatom-V center concentration by fluorescence absorption analysis, see the literature (DOI 10.1002 / pssa.201532174).

[0014] In this specification, the heteroatom is selected from the group consisting of B, P, Si, S, Cr, Sn, Al, Ge, Li, Na, K, Cs, Mg, Ca, Sr, Ba, Ti, Zr, V, Nb, Ta, Mo, W, Mn, Fe, Ni, Cu, Ag, Zn, Cd, Hg, Ga, In, Tl, Pb, As, Sb, Bi, Se, Te, Co, Xe, F, Y, and lanthanoids, preferably selected from the group consisting of Si, Ge, Sn, B, P, Ni, Ti, Co, Xe, Cr, W, Ta, Zr, Zn, Ag, Pb, and lanthanoids, more preferably selected from the group consisting of Si, Ge, Sn, B, P, Ni, Ti, Co, Xe, Cr, W, Ta, Zr, Zn, Ag, and Pb. Preferred heteroatoms to be doped into nanodiamonds are Group 14 elements selected from the group consisting of Si, Ge, Sn and Pb, B (boron), P (phosphorus), and Ni, and more preferred heteroatoms are Si, Ge, Sn, B, and P.

[0015] In one preferred embodiment, the nanodiamond particles obtained by the manufacturing method of the present invention contain at least one element selected from the group consisting of Si, Ge, Sn, and Pb, a group consisting of B, P, and Ni, and at least one other heteroatom. In another preferred embodiment, the nanodiamond particles obtained by the manufacturing method of the present invention contain at least one element selected from the group consisting of Si, B, P, and Ni, and at least one other heteroatom. The number of heteroatoms doped into the nanodiamond particles obtained by the manufacturing method of the present invention is preferably 1 to 5, more preferably 1 to 4, and even more preferably 1, 2, or 3.

[0016] The nanodiamond raw material used in the manufacturing method of the present invention can be produced, for example, by a detonation method, which includes mixing an explosive composition containing at least one explosive and, optionally, at least one heteroatom compound, and then detonating the resulting mixture in a sealed container. The nitrogen atom of the NV center can be derived from the nitro group of the explosive, but other nitrogen compounds can also be mixed with the explosive. Examples of containers include metal containers such as stainless steel and synthetic resin containers. When using metal containers such as stainless steel, metals such as Fe, Ni, and Cr from the container may be mixed into the nanodiamond particles. These metals can be removed by high-temperature, prolonged acid treatment at 130°C for three days. The explosive and heteroatom compound are preferably formed by pressing or casting. Methods for producing particles (dry powders) of the explosive and heteroatom compound include crystallization, crushing, and spray flash evaporation. The ODMR contrast of the nanodiamond raw material can be improved by gas-phase oxidation and high-temperature, prolonged acid treatment.

[0017] The temperature is important for the gas-phase oxidation treatment; temperatures below 560°C do not reduce the sp2 carbon fraction and increase fluorescence intensity. The upper limit for the oxidation treatment temperature is 650°C. The most preferred gas-phase oxidation treatment temperature is 570-610°C. The oxygen concentration in the atmosphere during the gas-phase oxidation treatment is preferably 1-100 v / v%, 1-50 v / v%, 1-25 v / v%, and more preferably 1-10 v / v%. The duration of the gas-phase oxidation treatment depends on the oxygen concentration of the atmosphere, but is preferably 0.5-20 hours, 0.5-10 hours, 1-5 hours, or more preferably 1-3 hours. Both the temperature and duration are important for the high-temperature, long-term mixed acid treatment; temperatures below 100°C or for less than 24 hours do not reduce the sp2 carbon fraction and increase fluorescence intensity. The upper limit for the high-temperature, long-term mixed acid treatment temperature is 340°C, and the upper limit for the high-temperature, long-term mixed acid treatment time is 200 hours. The most preferred temperature for the high-temperature, long-time mixed acid treatment is 120 to 200°C, and the most preferred time for the high-temperature, long-time mixed acid treatment is 60 to 120 hours. The mixed acid is composed of nitric acid and sulfuric acid, with a nitric acid:sulfuric acid (volume ratio) of 1:4 to 2:1. A conventional mixed acid treatment can be performed before the gas-phase oxidation treatment. The conventional mixed acid treatment can be performed at 50 to 200°C for 0.5 to 24 hours. The mixed acid used in the conventional mixed acid treatment is composed of nitric acid and sulfuric acid, with a nitric acid:sulfuric acid (volume ratio) of 1:3 to 1:1.

[0018] The preferred nanodiamond particles obtained by the production method of the present invention have a fluorescence emission peak due to the NV center. The wavelength of the fluorescence emission peak of the NV center is 550 to 800 nm, with the peak apex at around 700 nm. When ZPL can be confirmed, it is confirmed around 575 nm and 637 nm, but it may not be confirmed as a clear peak. When the nanodiamond particles further contain a heteroatom-V center, for example, when the heteroatom is silicon, the fluorescence emission peak due to the SiV center is preferably 720 to 770 nm, more preferably 730 to 760 nm. When the heteroatom is germanium, the fluorescence emission peak due to GeV is preferably 580 to 630 nm, more preferably 590 to 620 nm. When the heteroatom is tin, the fluorescence emission peak due to SnV is preferably 590 to 650 nm, more preferably 600 to 640 nm. When the heteroatom is lead, the fluorescence emission peak due to PbV is preferably 540 to 600 nm, more preferably 550 to 590 nm.

[0019] In one preferred embodiment of the present invention, nanodiamond particles obtained by the manufacturing method of the present invention, which emit fluorescence from heteroatom-vacancy centers where the heteroatom is other than phosphorus or boron, may be further doped with phosphorus and / or boron. The introduction of these atoms (B and / or P) is thought to have the effect of adjusting the charge of heteroatom-V centers other than B and / or P and defects (luminescence centers) derived from other doped heteroatoms, thereby stabilizing the fluorescence. Furthermore, the NV centers of the nanodiamonds obtained by the manufacturing method of the present invention and the nanodiamond particles of the present invention are luminescence centers formed by nitrogen and vacancies (vacancies), and have a broad fluorescence spectrum with peaks due to ZPL (zero-phonon lines) near 575 nm and / or 637 nm, e.g., a broad fluorescence spectrum of approximately 550-800 nm when excited at 532 nm. For example, doping with heteroatoms not directly related to fluorescence, such as phosphorus or boron, may enhance the NV center intensity, which is preferable. In a more preferred embodiment of the present invention, the fluorescence emission peak of the Si-doped nanodiamond particles includes a sharp peak at about 738 nm, called the ZPL (Zero Phonon Line).The ZPL of Ge-V is about 602 nm, that of Sn-V is about 620 nm, and that of Pb-V is about 552 nm.

[0020] The concentration of at least one nitrogen or heteroatom V center in the nanodiamond particles obtained by the production method of the present invention is preferably 1×10 10 / cm 3 More preferably, 2×10 10 ~1×10 19 / cm 3The heteroatomic V center concentration is the total concentration when the nanodiamond contains two or more NV centers and / or heteroatomic V centers. The concentration of the NV center and / or heteroatomic V center can be determined, for example, using a confocal laser microscope or a fluorescence absorption spectroscopy device. For information on determining the concentration of the NV center and heteroatomic V center by fluorescence absorption analysis, see the literature (DOI10.1002 / pssa.201532174). A heteroatomic compound is a compound containing at least one heteroatom (atom other than carbon), and may be either an organic compound or an inorganic compound.

[0021] The carbon content of the nanodiamond particles obtained by the production method of the present invention is preferably 70 to 99 mass%, more preferably 75 to 98 mass%, and even more preferably 80 to 97 mass%. The hydrogen content of the nanodiamond particles obtained by the production method of the present invention is preferably 0.1 to 5 mass%, more preferably 0.2 to 4.5 mass%, and even more preferably 0.3 to 4.0 mass%.

[0022] The nitrogen content of the nanodiamond particles obtained by the production method of the present invention is preferably 0.1 to 5 mass%, more preferably 0.2 to 4.5 mass%, and even more preferably 0.3 to 4.0 mass%. The carbon, hydrogen, and nitrogen contents of the nanodiamonds obtained by the production method of the present invention can be measured by elemental analysis.

[0023] When the nanodiamonds obtained by the production method of the present invention contain heteroatoms, the heteroatom content is preferably 0.0001 to 10.0% by mass, more preferably 0.0001 to 5.0% by mass, and even more preferably 0.0001 to 1.0% by mass. The heteroatom content can be measured, for example, by inductively coupled plasma atomic emission spectroscopy (ICP-AES), XRF, or SIMS (secondary ion mass spectrometry). The nanodiamonds can be quantified as an acidic solution after alkali fusion. Furthermore, when the nanodiamonds contain two or more heteroatoms, the heteroatom content refers to the total content of those atoms.

[0024] In one preferred embodiment of the nanodiamond particles obtained by the manufacturing method of the present invention, peaks characteristic of diamond, graphite, surface hydroxyl groups (OH), and surface carbonyl groups (CO) can be identified in the Raman shift chart by Raman spectroscopy. The peak characteristic of diamond in the Raman shift chart is 1100 to 1400 cm -1 The characteristic peak of graphite is 1450-1700 cm -1 and the characteristic peak of the surface hydroxyl group (OH) is 1500-1750 cm -1 and the peak characteristic of surface carbonyl groups (CO) is 1650-1800 cm -1 The areas of the peaks characteristic of diamond, graphite, surface hydroxyl groups (OH), and surface carbonyl groups (CO) are shown by a Raman spectrometer. The laser wavelength of the Raman light source is, for example, 325 nm or 488 nm. A confocal microscopic Raman spectrometer (for example, trade name: Microscopic Laser Raman Spectrophotometer LabRAM HR Evolution, manufactured by Horiba, Ltd.) can be used as the Raman spectrometer. In one preferred embodiment of the nanodiamond particles obtained by the production method of the present invention, the ratio (D / G) of the diamond peak area (D) to the graphite peak area (G) is preferably 0.2 to 9, more preferably 0.3 to 8, and even more preferably 0.5 to 7.

[0025] In a preferred embodiment of the nanodiamond particles obtained by the production method of the present invention, the ratio (H / D) of the peak area (H) of the surface hydroxyl groups (OH) to the peak area (D) of the diamond is preferably 0.1 to 5, more preferably 0.1 to 4.0, and even more preferably 0.1 to 3.0. In a preferred embodiment of the nanodiamond particles obtained by the production method of the present invention, the ratio (C / D) of the peak area (C) of the surface carbonyl groups (CO) to the peak area (D) of the diamond is preferably 0.01 to 1.5, more preferably 0.03 to 1.2, and even more preferably 0.05 to 1.0. For Raman analysis of nanodiamond particles, see, for example, Vadym N. Mochalin et al., NATURE NANOTECHNOLOGY, 7 (2012) 11-23, especially Figure 3.

[0026] In another preferred embodiment of the present invention, the surface of the nanodiamond particles obtained by the manufacturing method of the present invention may have at least one oxygen functional group terminal and / or at least one hydrogen terminal. The oxygen functional group terminal may be OH, COOH, CONH 2 , C=O, CHO, etc., with OH, C=O, and COOH being preferred. Examples of hydrogen termination include alkyl groups having 1 to 20 carbon atoms. The presence of at least one type of oxygen functional group termination on the surface of the nanodiamond particles obtained by the production method of the present invention is preferred because it suppresses aggregation of the nanodiamond particles. The presence of at least one type of hydrogen termination on the surface of the nanodiamond particles obtained by the production method of the present invention is preferred because it gives a positive zeta potential and allows for stable and high dispersion in acidic aqueous solutions.

[0027] In another preferred embodiment of the present invention, the nanodiamond particles obtained by the manufacturing method of the present invention may have a core-shell structure. The core of the nanodiamond particles with a core-shell structure obtained by the manufacturing method of the present invention is a nanodiamond particle doped with at least one heteroatom. This core preferably has a heteroatom V center and emits fluorescence. The shell is a non-diamond coating layer, which may contain sp2 carbon and preferably further contains oxygen atoms. The shell may be a graphite layer. The shell thickness is preferably 5 nm or less, more preferably 3 nm or less, and even more preferably 1 nm or less. The shell may have hydrophilic functional groups on its surface.

[0028] The shape of the nanodiamond particles obtained by the production method of the present invention is preferably spherical, ellipsoidal, or a polyhedral shape close to these. In the production method of the present invention, the explosive and the optionally compounded heteroatom compound in the detonation method can be mixed either in the presence or absence of a solvent, and after mixing, they can be shaped by a compression method or a pouring method. The average particle size of the explosive and the heteroatom compound is preferably 10 mm or less, more preferably 5 mm or less, and even more preferably 1 mm or less. These average particle sizes can be measured by laser diffraction / scattering, optical microscopy, or Raman spectroscopy. The product obtained by explosion can be subjected to purification processes such as gas-phase oxidation treatment, high-temperature long-term mixed acid treatment, and further alkali treatment, as well as post-treatment processes.

[0029] When an explosive composition containing an explosive and, if necessary, a heteroatom compound is exploded in a container, in addition to nanodiamonds, graphite, metal impurities, heteroatom elements, heteroatom oxides, etc. are produced. Graphite and metal impurities can be removed by a long-term high-temperature mixed acid treatment. When the heteroatom is a Group 14 element such as Si, Ge, Sn, or Pb, the Group 14 element elements (Si, Ge, Sn, Pb) and Group 14 element oxides (SiO 2 , GeO 2 , SnO, SnO 2 , PbO, PbO 2The metal impurities can be removed by alkaline treatment. However, metal impurities can hardly be removed or cannot be removed at all by ordinary mixed acid treatment.

[0030] Examples of alkali include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide. The alkali treatment temperature is 30 to 150°C, and the alkali treatment time is 0.5 to 24 hours. In one preferred embodiment of the present invention, nanodiamond particles with NV centers having high ODMR contrast can be obtained without performing the vacancy formation process by ion beam or electron beam irradiation and the NV center formation process by annealing in a vacuum or inert gas atmosphere. However, the following post-treatment process may be performed if necessary. The post-treatment process may include annealing. The annealing process allows the doped nitrogen and heteroatoms in the nanodiamond to meet with defects (vacancies), forming NV centers and heteroatomic V centers. Although this is an optional process, a vacancy formation process may be performed before annealing. The vacancy formation process is performed by ion beam or electron beam irradiation. NV centers and heteroatomic V centers are formed by annealing even without the vacancy formation process, but more NV centers and heteroatomic V centers can be formed by annealing after the vacancy formation process. The upper limit of the vacancy density introduced by ion beam or electron beam irradiation is the concentration at which diamond is destroyed (>1×10 21 / cm 3 The lower limit is, for example, 1 × 10 16 / cm 3 That's it, plus 1x10 18 / cm 3The ion beam is preferably a hydrogen (H) or helium (He) ion beam. For example, the energy of the hydrogen ion beam is preferably 10 to 1500 keV, and the energy of the helium ion beam is preferably 20 to 2000 keV. The energy of the electron beam is preferably 500 to 5000 keV. The annealing temperature is 650°C or higher, preferably 800°C or higher, and the annealing time is 30 minutes or longer.

[0031] The explosive is not particularly limited, and a wide variety of known explosives can be used. Specific examples include trinitrotoluene (TNT), cyclotrimethylenetrinitramine (hexogen, RDX), cyclotetramethylenetetranitramine (octogen), trinitrophenylmethylnitramine (tetryl), pentaerythritol tetranitrate (PETN), tetranitromethane (TNM), triamino-trinitrobenzene, hexanitrostilbene, and diaminodinitrobenzofuroxan, and these can be used alone or in combination of two or more. The heteroatom compounds specifically described below are merely illustrative, and a wide variety of known heteroatom compounds can be used. When the heteroatom is silicon, examples of organic silicon compounds include: silanes having a lower alkyl group such as acetoxytrimethylsilane, diacetoxydimethylsilane, triacetoxymethylsilane, acetoxytriethylsilane, diacetoxydiethylsilane, triacetoxyethylsilane, acetoxytripropylsilane, methoxytrimethylsilane, dimethoxydimethylsilane, trimethoxymethylsilane, ethoxytrimethylsilane, diethoxydimethylsilane, triethoxymethylsilane, ethoxytriethylsilane, diethoxydiethylsilane, triethoxyethylsilane, and trimethylphenoxysilane;

[0032] Trichloromethylsilane, dichlorodimethylsilane, chlorotrimethylsilane, trichloroethylsilane, dichlorodiethylsilane, chlorotriethylsilane, trichlorophenylsilane, dichlorodiphenylsilane, chlorotriphenylsilane, dichlorodiphenylsilane, dichloromethylphenylsilane, dichloroethylphenylsilane, chlorodifluoromethylsilane, dichlorofluoromethylsilane, chlorofluorodimethylsilane, chloroethyldifluorosilane, dichloroethylfluorosilane, chlorodifluoropropylsilane, dichlorofluoropropyl silanes having halogen atoms such as pyrsilane, trifluoromethylsilane, difluorodimethylsilane, fluorotrimethylsilane, ethyltrifluorosilane, diethyldifluorosilane, triethylfluorosilane, trifluoropropylsilane, fluorotripropylsilane, trifluorophenylsilane, difluorodiphenylsilane, fluorotriphenylsilane, tribromomethylsilane, dibromodimethylsilane, bromotrimethylsilane, bromotriethylsilane, bromotripropylsilane, dibromodiphenylsilane, and bromotriphenylsilane;

[0033] - Polysilanes such as hexamethyldisilane, hexaethyldisilane, hexapropyldisilane, hexaphenyldisilane, and octaphenylcyclotetrasilane. - Silazanes such as triethylsilazane, tripropylsilazane, triphenylsilazane, hexamethyldisilazane, hexaethyldisilazane, hexaphenyldisilazane, hexamethylcyclotrisilazane, octamethylcyclotetrasilazane, hexaethylcyclotrisilazane, octaethylcyclotetrasilazane, and hexaphenylcyclotrisilazane. - Aromatic silanes in which a silicon atom is incorporated into an aromatic ring, such as silabenzene and disilabenzene. - Hydroxyl group-containing silanes such as trimethylsilanol, dimethylphenylsilanol, triethylsilanol, diethylsilanediol, tripropylsilanol, dipropylsilanediol, triphenylsilanol, and diphenylsilanediol.

[0034] Alkyl- or aryl-substituted silanes such as tetramethylsilane, ethyltrimethylsilane, trimethylpropylsilane, trimethylphenylsilane, diethyldimethylsilane, triethylmethylsilane, methyltriphenylsilane, tetraethylsilane, triethylphenylsilane, diethyldiphenylsilane, ethyltriphenylsilane, and tetraphenylsilane; Carboxylic acid-containing silanes such as triphenylsilylcarboxylic acid, trimethylsilylacetic acid, trimethylsilylpropionic acid, and trimethylsilylbutyric acid;

[0035] Siloxanes such as hexamethyldisiloxane, hexaethyldisiloxane, hexapropyldisiloxane, and hexaphenyldisiloxane; Silanes having an alkyl group or an aryl group and a hydrogen atom, such as methylsilane, dimethylsilane, trimethylsilane, diethylsilane, triethylsilane, tripropylsilane, diphenylsilane, and triphenylsilane; Tetrakis(chloromethyl)silane, tetrakis(hydroxymethyl)silane, tetrakis(trimethylsilyl)silane, tetrakis(trimethylsilyl)methane, tetrakis(dimethylsilanolyl)silane, tetrakis(tri(hydroxymethyl)silyl)silane, and tetrakis(nitratemethyl)silane.

[0036] Examples of inorganic silicon compounds include silicon oxide, silicon oxynitride, silicon nitride, silicon carbide oxide, silicon carbide nitride, silane, and silicon-doped carbon materials. Examples of carbon materials doped with silicon include graphite, activated carbon, carbon black, ketjen black, coke, soft carbon, hard carbon, acetylene black, carbon fiber, and mesoporous carbon. Examples of boron compounds include inorganic boron compounds and organic boron compounds. Examples of inorganic boron compounds include orthoboric acid, diboron dioxide, diboron trioxide, tetraboron trioxide, tetraboron pentoxide, boron tribromide, tetrafluoroboric acid, ammonium borate, and magnesium borate.

[0037] Examples of organic boron compounds include triethylborane, (R)-5,5-diphenyl-2-methyl-3,4-propano-1,3,2-oxazaborolidine, triisopropyl borate, 2-isopropoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane, bis(hexylene glycolato)diboron, 4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-1H-pyrazole, tert-butyl-N-[4-(4,4,5,5-tetramethyl-1,2,3-dioxaborolan-2-yl)phenyl]carbamate, phenylboronic acid, 3-acetylphenylboronic acid, boron trifluoride acetic acid complex, boron trifluoride sulfolane complex, 2-thiopheneboronic acid, and tris(trimethylsilyl)borate. Examples of the phosphorus compound include inorganic phosphorus compounds, organic phosphorus compounds, etc. Examples of the inorganic phosphorus compound include ammonium polyphosphate.

[0038] Examples of organic phosphorus compounds include trimethyl phosphate, triethyl phosphate, tripropyl phosphate, tributyl phosphate, tripentyl phosphate, trihexyl phosphate, dimethyl ethyl phosphate, methyl dibutyl phosphate, ethyl dipropyl phosphate, 2-ethylhexyl di(p-tolyl) phosphate, bis(2-ethylhexyl) p-tolyl phosphate, tritolyl phosphate, di(dodecyl) p-tolyl phosphate, tris(2-butoxyethyl) phosphate, tricyclohexyl phosphate, triphenyl phosphate, ethyl diphenyl phosphate, dibutyl phosphoric acid esters such as phenyl phosphate, phenyl bis dodecyl phosphate, cresyl diphenyl phosphate, tricresyl phosphate, p-tolyl bis(2,5,5'-trimethylhexyl) phosphate, cresyl-2,6-xylenyl phosphate, trixylenyl phosphate, hydroxyphenyl diphenyl phosphate, tris(t-butylphenyl) phosphate, tris(i-propylphenyl) phosphate, 2-ethylhexyl diphenyl phosphate, bis(2-ethylhexyl)phenyl phosphate, tri(nonylphenyl) phosphate, and phenyl bis neopentyl phosphate; Condensed phosphate esters such as 1,3-phenylene bis(diphenyl phosphate), 1,4-phenylene bis(dixylenyl phosphate), 1,3-phenylene bis(3,5,5'-trimethylhexyl phosphate), bisphenol A bis(diphenyl phosphate), 4,4'-biphenyl bis(dixylenyl phosphate), 1,3,5-phenylene tris(dixylenyl phosphate), phosphites such as trimethyl phosphite, triethyl phosphite, triphenyl phosphite, tricresyl phosphite, 1,3-phenylene bis(diphenyl phosphite), 1,3-phenylene bis(dixylenyl phosphite), 1,4-phenylene bis(3,5,5'-trimethylhexyl phosphite), bisphenol A bis(diphenyl phosphite), 4,4'-biphenyl bis(dixylenyl phosphite), 1,3,Examples of germanium compounds include organic germanium compounds such as methyl germanium, ethyl germanium, trimethyl germanium methoxide, dimethyl germanium diacetate, tributyl germanium acetate, tetramethoxy germanium, tetraethoxy germanium, isobutyl germanium, alkyl germanium trichloride, and dimethylamino germanium trichloride. Examples of germanium compounds include nitrotriphenol complexes (Ge, 2 (ntp) 2 O), catechol complex (Ge(cat) 2 ) or aminopyrene complex (Ge 2 (ap) 2 Cl 2 and germanium alkoxides such as germanium ethoxide and germanium tetrabutoxide.

[0039] Examples of tin compounds include inorganic tin compounds such as tin(II) oxide, tin(IV) oxide, tin(II) sulfide, tin(IV) sulfide, tin(II) chloride, tin(IV) chloride, tin(II) bromide, tin(II) fluoride, tin acetate, and tin sulfate; alkyl tin compounds such as tetramethyltin; monoalkyl tin oxide compounds such as monobutyltin oxide; dialkyl tin oxide compounds such as dibutyltin oxide; aryl tin compounds such as tetraphenyltin; and organic tin compounds such as dimethyltin maleate, hydroxybutyltin oxide, and monobutyltin tris(2-ethylhexanoate). Examples of lead compounds include lead monoxide (PbO), lead dioxide (PbO 2 ), red lead (Pb 3 O 4 ), white lead (2PbCO 3 Pb(OH) 2 ), lead nitrate (Pb(NO 3 ) 2 ), lead chloride (PbCl 2 ), lead sulfide (PbS), yellow lead (PbCrO 4 , Pb(SCr)O 4 , PbO・PbCrO 4 ), lead carbonate (PbCO3 ), lead sulfate (PbSO 4 ), lead fluoride (PbF 2 ), lead tetrafluoride (PbF 4 ), lead bromide (PbBr 2 ), lead iodide (PbI 2 inorganic lead compounds such as lead acetate (Pb(CH 3 COO) 2 ), lead tetracarboxylate (Pb(OCOCH 3 ) 4 ), tetraethyl lead (Pb(CH 3 CH 2 ) 4 ), tetramethyl lead (Pb(CH 3 ) 4 ), tetrabutyl lead (Pb(C 4 H 9 ) 4 ) and other organic lead compounds.

[0040] The heteroatom compound may be used alone or in combination of two or more. The proportion of the explosive in the mixture containing the explosive and the heteroatom compound is preferably 80 to 99.9999 mass%, more preferably 85 to 99.999 mass%, even more preferably 90 to 99.99 mass%, and particularly preferably 95 to 99.9 mass%, and the proportion of the heteroatom compound is preferably 0.0001 to 20 mass%, more preferably 0.001 to 15 mass%, even more preferably 0.01 to 10 mass%, and particularly preferably 0.1 to 5 mass%. The heteroatom content in the mixture containing the explosive and the heteroatom compound is preferably 0.000005 to 10 mass%, more preferably 0.00001 to 8 mass%, even more preferably 0.0001 to 5 mass%, particularly preferably 0.001 to 3 mass%, and most preferably 0.01 to 1 mass%. When the explosive and the heteroatom compound are solid, they may be mixed as powders, melted, or dissolved or dispersed in a suitable solvent. Mixing can be carried out by stirring, bead milling, ultrasonic waves, etc.

[0041] In a preferred embodiment, the explosive composition containing an explosive and a heteroatom compound further contains a cooling medium. The cooling medium may be solid, liquid, or gas. A method using a cooling medium includes detonating a mixture of an explosive and a heteroatom compound in the cooling medium. Examples of cooling mediums include inert gases (nitrogen, argon, CO), water, ice, liquid nitrogen, aqueous solutions of heteroatom-containing salts, and crystalline hydrates. Examples of heteroatom-containing salts include ammonium hexafluorosilicate, ammonium silicate, and tetramethylammonium silicate. In the case of water or ice, for example, the cooling medium is preferably used in an amount approximately five times the weight of the explosive.

[0042] In one preferred embodiment of the present invention, a mixture containing an explosive and an optional heteroatom compound is converted into diamond by compression by a shock wave under high pressure and high temperature conditions generated by the detonation of the explosive (detonation method). During the detonation of the explosive, nitrogen and optionally other heteroatoms are incorporated into the diamond lattice. The carbon source of the nanodiamonds can be the explosive and the organic heteroatom compound, but if the mixture containing the explosive and the heteroatom compound also contains a carbon material that does not contain heteroatoms, this carbon material can also be the carbon source of the nanodiamonds. The nitrogen source of the NV center can be the nitro group of the explosive.

[0043] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.

[0044] Example 1: Nanodiamonds were produced using 1 kg of explosive containing 60% trinitrotoluene (TNT) and 40% cyclotrimethylenetrinitramine (RDX) according to the standard method for nanodiamond production by detonation. The resulting nanodiamonds were subjected to the following processes. (i) Purification: 15 g of nanodiamonds obtained in the detonation test were added to 2800 g of a mixed acid mixture of concentrated sulfuric acid and concentrated nitric acid (11:1 by weight), and the mixture was stirred at 150°C for 10 hours to purify the nanodiamonds. The precipitate (containing nanodiamonds) obtained after washing with water was then dried to obtain purified nanodiamond powder. (ii) Gas-Phase Oxidation: The powder obtained in (i) was oxidized in a gas atmosphere furnace at 570°C for 1 hour in a 4% oxygen atmosphere to obtain nanodiamond powder. The yield after the 570°C oxidation process was 17.5%. (iii) High-temperature, long-term mixed acid treatment The nanodiamond powder obtained in gas-phase oxidation treatment (ii) was added to a mixed acid of concentrated sulfuric acid and concentrated nitric acid = 3:1 (weight ratio), and mixed acid treatment was carried out at 130°C for 72 hours. The mixed acid treated nanodiamonds were collected by centrifugation and washed repeatedly with pure water. After washing, the collected nanodiamonds were dried to obtain nanodiamond powder.

[0045] Example 2: Silicon-doped nanodiamonds were produced using approximately 1 kg of an explosive composition containing 100 parts by weight of an explosive containing trinitrotoluene (TNT) and cyclotrimethylenetrinitramine (RDX) and 1 part by weight of triphenylsilanol as a heteroatom compound, according to standard nanodiamond production methods. The resulting silicon-doped nanodiamonds were then subjected to the following treatments. The amount of triphenylsilanol added to the explosive was 1% by weight. (I) Mixed Acid Treatment: 15 g of nanodiamonds obtained in a detonation test were added to 2800 g of mixed acid (concentrated sulfuric acid:concentrated nitric acid = 11:1 by weight) and treated at 150 °C for 10 hours with stirring. (II) Alkali Treatment: 1 g of the mixed acid-treated nanodiamonds was added to 100 mL of 8N aqueous sodium hydroxide solution and treated at 70 °C for 8 hours with stirring. The resulting Si-doped nanodiamond raw material was subjected to gas-phase oxidation in a gas atmosphere furnace at 570 °C in a 4% oxygen atmosphere for 2 hours to obtain the Si-doped nanodiamond particles of the present invention. The yield after gas-phase oxidation at 570°C was 4.6%. (III) Gas-phase oxidation: The powder obtained in (I) was oxidized in a gas atmosphere furnace at 570°C in a 4% oxygen atmosphere for 1 hour to obtain nanodiamond powder. The yield after oxidation at 570°C was 17.5%. (IV) High-temperature, long-term mixed acid treatment: The nanodiamond powder obtained in gas-phase oxidation (III) was added to a mixed acid of concentrated sulfuric acid and concentrated nitric acid (3:1 by weight), and the mixed acid treatment was carried out at 130°C for 72 hours. The mixed acid-treated nanodiamonds were recovered by centrifugation and repeatedly washed with pure water. After washing, the recovered nanodiamonds were dried to obtain nanodiamond powder.

[0046] Example 3: Fluorescence mapping, fluorescence spectra, and ODMR (optically detected magnetic resonance) measurements of the nanodiamond particles obtained in Examples 1 and 2 were performed using the confocal microscope shown in Figure 1. The nanodiamond powder obtained by the high-temperature, long-term mixed acid treatment (iii) in Example 1 was added to pure water and sonicated for 10 minutes to prepare a nanodiamond aqueous dispersion with a concentration of 0.03 mg / mL. 5 μL of the dispersion was then dropped onto a cover glass and allowed to air-dry. A 30 μm diameter copper wire was then attached to the cover glass surface (for microwave application). After attaching the copper wire, the measurement set was sandwiched between two cover glasses to form a measurement set. The measurement set was fixed onto the objective lens of the confocal microscope (Figure 1), and a microwave generator was connected to the copper wire. Fluorescence mapping, fluorescence spectra, and ODMR measurements were performed. For fluorescence mapping measurements, the measurement set was fixed onto an oil-immersion objective lens, and excitation light was focused onto the nanodiamond layer. The fluorescence emitted from the nanodiamonds was collected using the same oil-immersion objective, passed through a pinhole and a long-pass filter, and focused onto a detector for measurement. High-speed fluorescence mapping measurements were performed by moving the objective lens mounted on a piezo stage (plane movement range: 100 μm square, optical axis movement range: 25 μm) (Figure 2). An avalanche photodiode (APD) was used as the detector. The measurement conditions were excitation wavelength: 532 nm, excitation power: 100 μW, pixel count: 200 × 200 pixels, exposure time: 3 ms / pixel, number of integrations: 1, and measurement area: 30 × 30 μm. A neutral density filter (optical density 1.0) was attached in front of the APD. The fluorescence spectrum and fluorescence mapping measurements confirmed multiple bright spots. The fluorescence spectrum of the nanodiamond particles obtained in Example 1 was measured by focusing the excitation light at one bright spot (Figure 3) (excitation light wavelength: 532 nm, excitation light power: 100 μW, exposure time: 0.1 s, number of integrations: 100). The fluorescence spectrum was obtained using a spectrometer and a CCD camera. Furthermore, the fluorescence spectrum of the Si-doped nanodiamond particles obtained in Example 2 was obtained in the same manner as above (Figure 4).For ODMR measurements, excitation light was focused on a single bright spot, and the fluorescence intensity emitted from the nanodiamond particles obtained in Example 1 or Example 2 was confirmed. After confirming the fluorescence intensity, the microwave generator output was turned on, electricity was applied to the stretched copper wire, the microwave frequency was swept, and the ODMR spectrum was measured (Table 1, Figures 6 and 7). An APD was used as the detector. The measurement conditions were: microwave frequency (MW Frequency / MHz) sweep range: 2820-2920 MHz, microwave power: 25 dBm (estimated after amplification), excitation light wavelength: 532 nm, excitation light power: 100 μW, and number of integrations: 10.

[0047] Example 4: Rabi Oscillation Measurement After determining the resonant frequency of the NV center from the ODMR spectrum of the nanodiamond particles obtained in Example 1 or Example 2, the frequency of the microwave generator was set to match the resonant frequency of the NV center. The measurement sequence shown in Figure 5 was then set up. First, a laser was applied to initialize the spin state of the NV center. After a certain period of time, microwaves were applied to change the spin state. Since the NV center's luminescence intensity changes depending on the spin state, the laser was applied again and the luminescence intensity was read using a detector. However, since continued laser irradiation will initialize the spin state, the luminescence intensity was read only for a certain period of time after the laser irradiation. This is referred to as Signal (S). Meanwhile, in the time domain where the spin state has been initialized by continuing to apply the laser for a sufficient period of time, the luminescence intensity is detected for the same period as S. This is referred to as Reference (R). For Rabi oscillations, by plotting the Signal / Reference value while varying the microwave application time τ, oscillations corresponding to τ can be observed, which is the Rabi oscillation. The measurement conditions were: excitation light wavelength: 532 nm, excitation light power: 100 μW, and set frequency: 2870 MHz (determined from the ODMR spectrum). In Fig. 5, t1 = 20000 ns, t 2 = 1000 ns, t3 = 100 ns, and t4 = 600 ns. τ was typically measured by increasing it in 10 ns increments from 0 ns. Signal / Reference (intensity) was plotted against τ, and fitting was performed using the fitting function shown in Equation 1. Each parameter was determined by fitting, and the value of 2 × b was taken as the contrast in the Rabi oscillation (Figure 8, Table 2).

[0048] Example 5: Si-doped nanodiamond particles (hereinafter abbreviated as "Si-DND") obtained by the same manufacturing method as in Example 2 were used to perform NV - The average particle size of the Si-DNDs used in Example 5 was 11.2 nm based on the particle size distribution measured by a transmission electron microscope, and it was confirmed that this particle size was sufficient for introduction into the cell nucleus. In addition, electron spin resonance was used to measure the NV in the Si-DNDs. - The concentration was estimated to be about 0.35 ppm, which is the same as the NV concentration in NDs that were not subjected to electron beam irradiation or annealing treatment. - The concentration was more than three times higher than the conventional concentration. On the other hand, when ODMR was measured for the luminescent spots (aggregates) of Si-DND, the contrast was at most 0.4%. This is due to the sp remaining in the ND. 2 This is thought to be due to the influence of non-diamond carbon, etc. In order to remove these residues, the film was heated with mixed acid for 72 hours, and as a result, NV films with a contrast of 10% or more were obtained. - A large number of Si-DNDs were identified, and ODMR signals were confirmed in approximately 50% of the measured DND light-emitting spots. Temperature measurements were performed on Si-DNDs using CW-ODMR (Continuous wave optically detected magnetic resonance). First, several bright spots (Si-DND aggregates) with PL spectra derived from NV centers were identified using a confocal microscope, and measurements were performed on 10 of these bright spots. Figure 9 shows data on one of these bright spots. Figure 9a shows the PL spectrum, with NV centers at around 637 nm. -ZPL (Zero Phonon Line) at the center and NV around 575 nm 0 A central ZPL was confirmed. The temperature dependence of the ODMR spectrum for this bright spot was investigated. The sample temperature was varied using a thermoplate in contact with the sample glass substrate and a lens heater on the objective lens side. The sample temperature, T, was measured using a temperature sensor (thermistor) attached immediately adjacent to the sample. Figure 9b shows ODMR measured at 295 K and 313 K under zero magnetic field (no external magnetic field applied). The zero-field splitting constant (D) shifts to lower frequencies with increasing temperature. The spectrum was fitted with a double Lorentzian function, and D was obtained by averaging the two centers of the two Lorentzian curves. Figure 9c shows the plot of D for different temperatures, T. D varies linearly with T, and the rate of change, dD / dT, was fitted with a straight line, yielding dD / dT = -72.2 ± 1.3 kHz / K. The average dD / dT value for 10 different origins was -71.2 kHz / K, which is in close agreement with the dD / dT commonly reported for other diamonds.

[0049] Next, the temperature sensitivity of the 10 bright spots was examined. The temperature sensitivity measurement was based on the method used to measure AC magnetic field sensitivity. The frequency position where the ODMR spectrum had the maximum gradient relative to the microwave frequency was selected from double Lorentzian fitting and used to evaluate the temperature sensitivity. The emission intensity was traced while irradiating microwaves at the frequency position where the gradient was the steepest. The integration time t required for one measurement of the emission intensity was int The emission intensity was measured 100 times and the standard deviation of the emission intensity was calculated. Next, the maximum frequency-intensity gradient was used to convert it into the standard deviation of microwaves. Finally, dD / dT was used to convert it into the standard deviation of temperature, which was then used to calculate the temperature uncertainty σ. T The cumulative time t int A int  Varying σ = 0.003 - 2 seconds T As a result of measuring σ T Generally, This decays according to σ T This means that in this time domain, N is affected almost exclusively by shot noise. phis the number of detected photons, where η T represents the temperature sensitivity, and the unit integration time t int σ at = 1 s T In the case of the bright spot in Figure 9, However, in this measurement, in order to reduce saturation of the avalanche photodiode (APD), a neutral density (ND) filter with an optical density (OD) of 1.0 was used in front of the APD, and the emission intensity was reduced to one-tenth. If the ND filter was not used and the effect of APD saturation could be ignored, the number of detected photons would be 10 times higher, so η T is improved by 1 / √10. As a result, the temperature sensitivity at the bright spot is The bright spot was estimated to be a multiple NV (Fig. 9(d)). - Due to the contribution from a single NV - To estimate the sensitivity at is applied, where η ensemble is NV - Ensemble sensitivity, η single is a single NV - is the sensitivity of the NV in the range observed by the confocal microscope. - NV - is the number of single NVs in bulk diamond measured with the same optical system. - In the case of Figure 9, there are 23 NVs in the bright spot. - From the above, it was estimated that a single NV - The temperature sensitivity is It was estimated that:

[0050] NV - To investigate the spin properties of DND, Rabi oscillation and spin Hahn echo measurements were performed in the presence of an external magnetic field applied from a permanent magnet. The results of these measurements are shown in Figures 9e and 9f. The spin coherence time (T2) measured from the Hahn echo experiment was found to be 1.8 μs, which is consistent with the time commonly reported for DNDs. The experimental procedure shown in Figures 9b to 9d was repeated for 10 different bright spots. From the obtained data, the average temperature sensitivity was In addition, a single NV - When converted to Among these measurements, the NV of the Si-DND aggregates was determined to be - The maximum temperature sensitivity of the ensemble is Single NV - The highest observed sensitivity is Furthermore, the NV of the above Si-DND - and SiV - The results of temperature sensing using this method are shown in Figure 10. A diagram of the device used for temperature sensing is shown in Figure 11.

[0051] In Figure 10a, a confocal image of Si-DND aggregates shows NVs. - Center and SiV - The spots where both were observed are circled in white. Figure 10b shows the fluorescence spectrum of the spots in Figure 10a. NV - (637 nm) and SiV - The zero-phonon line at (737 nm) is also observed. - The ODMR spectrum of the center was measured at two temperatures, 295 K and 313 K (Fig. 10c). The ODMR contrast improved with increasing measurement temperature. Figure 10d shows the temperature dependence of the ODMR zero-field splitting constant (D). The average of the two peaks fitted with a double Lorentzian function was plotted, and the error bars were calculated from the standard error of each. The peak sensitivity to temperature (dD / dT) was calculated to be -84.4 ± 9.1 kHz / K. The SiV at two temperature levels, 300 K and 313 K, - The ZPL spectrum is shown in Fig. 10e. At 300 K and 313 K, the relative intensity decreases with increasing temperature. - The temperature dependence of the ZPL peak wavelength λ is shown in Figure 10f. p varies linearly with temperature, and Δλ p / ΔT = 0.014 ± 0.002 nm / K. Figure 10g shows a graph of the size distribution of Si-DNDs.- Center and SiV - The simultaneous presence of NV center for temperature sensing - The versatility of the center could be expanded. NV - The ODMR resonance frequency (zero-field splitting constant D) of NV is affected by both temperature and electric field. - On the other hand, it is difficult to distinguish between the electric field-induced shift and the temperature-induced shift. - If temperature measurement using SiV is possible, - and NV - It is also noteworthy that the ODMR contrast increased with increasing temperature, which contradicts the finding that the ODMR contrast decreased with increasing temperature. However, this increase in ODMR contrast is due to the SiV, as shown in Figure 10e. - Since the fluorescence of SiV becomes the background during ODMR measurements, - This may be due to a decrease in the fluorescence intensity from SiV. - This background from the NV - The relative fluorescence ratio of SiV increases, resulting in an increase in ODMR contrast. - The ODMR contrast was further improved by using a short-pass filter near the ZPL of SiV during ODMR measurements. - This suggests that the fluorescence is effectively reduced, further improving the sensitivity of ODMR-based techniques.

[0052] NV - Temperature sensing using the ODMR characteristics of the center can improve temperature sensitivity with sub-Kelvin accuracy, and by using nanodiamonds with a size of 10 nm, it is possible to perform measurements that are very important for measuring living cells, such as distinguishing the difference in temperature distribution between the nucleus and cytoplasm and monitoring the temperature change of mitochondria after activation (a rise of about 10 K at 20 nm). In addition, NV measurements can be performed within the same confocal volume. - and SiV -We demonstrate multimodal temperature sensing using both DNDs and Pb-DNDs, suggesting their high compatibility and the potential versatility of quantum sensing for DNDs doped with group 14 elements, such as GeV-DNDs, Sn-DNDs, and Pb-DNDs.

Claims

1. Fluorescent nanodiamond particles having a fluorescent emission peak derived from a nitrogen-vacancy (NV) center, which satisfies the following condition (i): (i) when a 1 mass% aqueous suspension of the particles is applied to a glass substrate, the proportion of bright spots showing an ODMR contrast of 7% or more among the bright spots where ODMR of the NV center is observed is 10% or more.

2. A fluorescent nanodiamond particle as described in claim 1, further satisfying the following conditions (ii) and / or (iii): (ii) the ODMR contrast is 12% or more; (iii) the maximum contrast in the Rabi oscillation is 25% or more.

3. A fluorescent nanodiamond particle as described in claim 1 or 2, further comprising a heteroatom-V center.

4. A method for producing fluorescent nanodiamonds as described in any one of claims 1 to 3, which comprises subjecting the nanodiamond raw material obtained in the detonation process to gas-phase oxidation at a temperature of 560 to 620°C, and then subjecting it to a high-temperature, long-term mixed acid treatment at a temperature of 120 to 340°C for 36 to 120 hours.

5. A method for producing fluorescent nanodiamonds as described in claim 4, which does not involve a post-treatment process.

Citation Information

Patent Citations

  • Nanodiamond particles, method for producing the same, fluorescent molecular probe, and method for analyzing protein structure

    JP6117812B2

  • Diamond composite particles

    JP2014095025A

  • Method for manufacturing fluorescent NANO diamond

    JP2021134127A

  • Nano-diamond particle and method for producing same, and fluorescent molecular probe and method for analyzing structure of protein

    WO2014058012A1

  • Heteroatom-doped nanodiamond particles and method for producing heteroatom-doped nanodiamond particles

    WO2023013659A1

Cited By

  • Solid-state spin sensor with a compliant head

    US12724091B2