Rotating tool for double-sided friction stir welding

The rotary tool for double-sided friction stir welding, featuring a low-friction and high-hardness tip with a spiral stepped surface, addresses the challenges of defect suppression and tool durability, achieving efficient and durable welding of structural steel by controlling friction and heat generation.

WO2024219083A1PCT designated stage expired Publication Date: 2024-10-24JFE STEEL CORP
View PDF 24 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006355
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-02-21
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Friction stir welding for structural steel faces challenges with defect suppression, welding speed, and tool durability, particularly when using rotary tools with high rotational speeds, leading to excessive frictional heat and material adhesion issues.

Method used

A rotary tool for double-sided friction stir welding is designed with a tip made from a material having a dynamic friction coefficient of less than 0.30 and a Vickers hardness of 2500 HV or more, featuring a flat, convex, or concave surface with a spiral stepped portion, and a controlled tip diameter to optimize material flow and reduce heat generation.

Benefits of technology

This design effectively suppresses defects, increases welding speed, and enhances the durability of the rotary tool, enabling high-quality joints in structural steel with reduced surface and internal defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006355_24102024_PF_FP_ABST
    Figure JP2024006355_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a rotating tool for double-sided friction stir welding, the rotating tool making it possible to simultaneously suppress the occurrence of defects during welding, increase the welding speed, and improve the durability of the rotating tool. A tip end portion of the rotating tool is made of a material having a coefficient of dynamic friction of less than 0.30 and a Vickers hardness of 2500 HV or more.
Need to check novelty before this filing date? Find Prior Art

Description

Rotary tool for double-sided friction stir welding

[0001] The present invention relates to a rotary tool for double-sided friction stir welding.

[0002] As a technology related to friction welding, for example, Patent Document 1 discloses, "A method of friction welding a pair of members (45, 46) comprising the steps of: causing relative motion between the pair of members while forcing the members together; detecting the speed of the relative motion at least toward the end of the welding cycle; and forcing the members together under a force controlled in accordance with the detected speed of the relative motion between the members."

[0003] However, the friction welding of Patent Document 1 requires the rotation of the members to be welded, such as metal plates, and therefore places limitations on the shapes and dimensions of the members to be welded, such as metal plates.

[0004] Furthermore, as a technology related to friction stir welding, for example, Patent Document 2 discloses the following: "A friction welding method comprising providing a probe made of a material harder than the material of the workpiece on a continuous or substantially continuous surface of the workpiece, causing the probe and the workpiece to come together by frictional heat generated as the probe enters the workpiece to create a flexible layer of the workpiece material around the probe, stopping the relative circular motion, and hardening the area around the probe to provide a flexible material." In this disclosure, a region where the workpieces are butted or overlapped and not yet joined is referred to as an "unjoined portion," and a region that has been joined and integrated is referred to as a "jointed portion."

[0005] As described above, friction welding as described in Patent Document 1 is a method of rotating metal plates or other workpieces and welding them using frictional heat between the workpieces. On the other hand, friction stir welding as described in Patent Document 2 is a method of joining workpieces by rotating and moving a rotating tool while the metal plates or other workpieces are fixed. Therefore, friction stir welding has the advantage of being able to continuously join workpieces that are essentially infinitely long in the joining direction. Furthermore, friction stir welding is a solid-state welding method that utilizes the flow of metal material due to frictional heat between the rotating tool and the workpieces, so it can join without melting unjoined parts. Furthermore, friction stir welding has many advantages, such as less deformation after joining due to low heating temperatures, fewer defects in the weld because the workpieces are not melted, and no filler metal is required.

[0006] Japanese Patent Publication No. 62-183979 Japanese Patent Publication No. Hei 07-505090 Japanese Patent No. 3261433 Japanese Patent No. 4838385 Japanese Patent No. 4838388 Japanese Patent No. 6825630 Japanese Patent No. 6737347 Japanese Patent No. 4827359 Japanese Patent Publication No. 2007-237258 Japanese Patent No. 5971616 Japanese Patent No. 6491363 Japanese Patent No. 5156948 International Publication No. 2018 / 030309 Japanese Patent No. 5185103 Japanese Patent Publication No. 2015-127063 Japanese Patent Publication No. 2003-181655 Japanese Patent Publication No. 2003-290936 Japanese Patent Publication No. 2004-195480 Japanese Patent Publication No. 2011-115846

[0007] The above-mentioned friction stir welding has been widely used in the fields of aircraft, ships, railway vehicles, automobiles, etc. as a method for joining low-melting-point metal materials, such as aluminum alloys and magnesium alloys. The reason for this is as follows: When joining the above-mentioned low-melting-point metal materials, it is difficult to obtain satisfactory characteristics of the joint using conventional arc welding methods. Furthermore, the application of friction stir welding improves productivity and produces high-quality joints.

[0008] Furthermore, in recent years, the application of friction stir welding to structural steel, which is primarily used as a material for structures such as buildings, ships, heavy machinery, pipelines, and automobiles, has also been considered. This can avoid solidification cracking and hydrogen cracking, which are issues with conventional fusion welding. It also suppresses changes in the steel's structure. As a result, improved joint performance can be expected. In addition, stirring the weld interface with a rotating tool creates a clean surface, allowing the clean surfaces to come into contact with each other. Therefore, there is also the expected benefit of not requiring the preparatory process that is required with diffusion welding. As such, the application of friction stir welding to structural steel is expected to have many advantages.

[0009] However, friction stir welding of structural steel has not been widely adopted compared to friction stir welding of low-melting-point metal materials because problems remain in the joining workability, such as suppressing the occurrence of defects during joining and increasing the joining speed. Here, the defects that occur during joining mentioned above include, in particular, shape defects and joining defects on the joint surface or inside the joint.

[0010] To solve the above problems, the application of double-sided friction stir welding to structural steel, as disclosed in, for example, Patent Documents 3 to 7, has been considered. In double-sided friction stir welding, as shown in Figures 1 and 2, a pair of opposing rotating tools presses one side and the other side of the unjoined portion of the workpieces. This ensures sufficient, uniform material flow in the thickness direction of the workpieces. This is expected to reduce the occurrence of defects during welding while increasing the welding speed.

[0011] Furthermore, in order to popularize friction stir welding of structural steel, it is also necessary to improve the durability of the rotating tool. In other words, if the durability of the rotating tool is insufficient, it is predicted that repairs will be necessary due to breakage and wear of the rotating tool, and there will be a high probability of poor welding. Therefore, even if there are advantages as described above, if the durability of the rotating tool is insufficient, it will be judged that the practical application of friction stir welding to structural steel is difficult.

[0012] Here, Patent Documents 8 to 13 disclose rotary tools made of various materials, and Patent Documents 14 to 19 disclose rotary tools that do not have probes (pins) that are subject to a large load during welding and are prone to breakage and wear (hereinafter also referred to as probe-less rotary tools).

[0013] However, even when the rotary tools disclosed in Patent Documents 8 to 19 are used in double-sided friction stir welding of structural steel, it has not been possible to simultaneously achieve the following: - Suppress the occurrence of defects during welding, particularly the following defects. When the rotation speed of the rotary tool is increased to increase the welding speed, excessive frictional heat is generated between the rotary tool and the workpieces. This causes the workpieces to seize onto the tip of the rotary tool and gouge the surface of the weld. - Increase the welding speed. - Improve the durability of the rotary tool. Therefore, there is currently a demand to simultaneously achieve the above points.

[0014] The present invention has been developed in consideration of the above-described current situation, and aims to provide a rotary tool for double-sided friction stir welding that can simultaneously suppress the occurrence of defects during welding, increase the welding speed, and improve the durability of the rotary tool.

[0015] The inventors have conducted extensive research to achieve the above object. As a result, they have found that the above object can be achieved by forming the tip of the rotary tool from a material having a dynamic friction coefficient of less than 0.30 and a Vickers hardness of 2500 HV or more. The present invention was completed based on the above finding and further research.

[0016] That is, the gist of the present invention is as follows: 1. A rotating tool for double-sided friction stir welding, wherein a tip portion of the rotating tool is made of a material having a dynamic friction coefficient of less than 0.30 and a Vickers hardness of 2500 HV or more.

[0017] 2. The rotary tool for double-sided friction stir welding according to 1, wherein the rotary tool is a probe-less rotary tool, and the tip surface of the rotary tool is a flat surface, a convex curved surface, or a concave curved surface.

[0018] 3. The rotary tool for double-sided friction stir welding according to 2 above, wherein the tip surface of the rotary tool has a spiral-shaped step portion in the direction opposite to the rotation.

[0019] 4. The rotary tool for double-sided friction stir welding according to any one of 1 to 3 above, which satisfies the relationship of the following formula (1): 4×t   ≦   D   ≦   20×t (1) where, t: thickness of the workpieces (mm), and D: diameter of the tip of the rotary tool (mm).

[0020] According to the present invention, a rotary tool for double-sided friction stir welding can be obtained that can simultaneously suppress the occurrence of defects during welding, increase the welding speed, and improve the durability of the rotary tool. Furthermore, the rotary tool for double-sided friction stir welding of the present invention can be more advantageously applied to various workpieces such as structural steel, and is therefore extremely advantageous from an industrial perspective.

[0021] 3A . FIG. 3B is a side perspective view showing an example of butt welding by double-sided friction stir welding. FIG. 3C is a side perspective view showing an example of lap welding by double-sided friction stir welding. FIG. 3D is a top view showing an example of butt welding by double-sided friction stir welding. FIG. 3E is a view taken along the arrows AA' in FIG. 3A . FIG. 3F is a schematic view showing an example of the shape of a rotary tool with a probe. FIG. 3G is a schematic view showing an example of the shape of a rotary tool with a probe. FIG. 3H is a schematic view showing an example of the shape of a flat-tip rotary tool without a probe. FIG. 3I is a schematic view showing an example of the shape of a flat-tip rotary tool without a probe. FIG. 3J is a schematic view showing an example of the shape of a convex-tip rotary tool without a probe. FIG. 3J is a schematic view showing an example of the shape of a convex-tip rotary tool without a probe. FIG. 3I is a schematic view showing an example of the shape of a concave-tip rotary tool without a probe. FIG. 3I is a schematic view showing an example of the shape of a concave-tip rotary tool without a probe. FIG. 3J is a schematic view showing an example of a convex-tip rotary tool provided with a stair-like step portion. FIG. 3J is a schematic view showing an example of a convex-tip rotary tool provided with a groove-like step portion.

[0022] The present invention will be described based on the following embodiments. [1] Rotary Tool A rotary tool according to one embodiment of the present invention has a tip made of a material having a dynamic friction coefficient of less than 0.30 and a Vickers hardness of 2500 HV or more.

[0023] Material for the tip of the rotary tool: a material with a dynamic friction coefficient of less than 0.30 and a Vickers hardness of 2500 HV or more. The inventors conducted extensive research to simultaneously suppress the occurrence of defects during joining, increase the joining speed, and improve the durability of the rotary tool in double-sided friction stir welding, particularly double-sided friction stir welding of structural steel, and obtained the following findings. Increasing the rotation speed of the rotary tool to increase the joining speed in double-sided friction stir welding of structural steel generates excessive frictional heat between the rotary tool and the workpiece. This causes the workpiece to seize at the tip of the rotary tool, gouges the surface of the weld, and causes defects. This phenomenon occurs because the workpiece is suddenly exposed to high temperatures due to excessive frictional heat, softening it, and the softened workpiece adheres to the tip of the rotary tool. Suppressing the sudden generation of frictional heat is effective in preventing this phenomenon. To achieve this, it is effective to use a material with a dynamic friction coefficient of less than 0.30 for the tip of the rotary tool. Furthermore, when the rotation speed of the rotary tool is increased to increase the joining speed, a large load is applied to the rotary tool. As a result, the rotary tool is prone to breakage and wear. To prevent this, it is effective to use a high-hardness material, specifically a material with a Vickers hardness of 2500 HV or more, at the tip of the rotary tool. For these reasons, the tip of the rotary tool is made of a material with a dynamic friction coefficient of less than 0.30 and a Vickers hardness of 2500 HV or more.

[0024] The coefficient of dynamic friction of the material of the tip of the rotary tool (hereinafter simply referred to as the coefficient of dynamic friction) is preferably 0.25 or less. There is no particular limitation on the lower limit of the coefficient of dynamic friction. The coefficient of dynamic friction is preferably, for example, 0.12 or more.

[0025] Here, the dynamic friction coefficient is measured by the ball-on-disk method in accordance with JIS (Japanese Industrial Standards) R 1613 (2010). The ball (spherical test piece) is made of the material to be measured (the same material as the material constituting the tip of the rotary tool), and the disk (disk-shaped test piece) is made of SKD11 as defined in JIS G 4404 (2015). The temperature at which the dynamic friction coefficient is measured may be room temperature (e.g., 25°C).

[0026] The Vickers hardness (hereinafter simply referred to as Vickers hardness) of the material of the tip of the rotary tool is preferably 2700 HV or more, more preferably 2900 HV or more. There is no particular upper limit to the Vickers hardness. For example, the Vickers hardness is preferably 5000 HV or less.

[0027] Here, the Vickers hardness is measured by a Vickers hardness test method in accordance with JIS R 1610 (2003). The test force is 19.61 N. The temperature when measuring the Vickers hardness may be room temperature (e.g., 25°C).

[0028] Here, a material with a dynamic friction coefficient of less than 0.30 and a Vickers hardness of 2500 HV or greater can be formed, for example, from polycrystalline cubic boron nitride (hereinafter also referred to as PCBN). PCBN can be manufactured by mixing cubic boron nitride (CBN) crystal grains with a binder under a high-pressure, high-temperature environment. Furthermore, the dynamic friction coefficient and Vickers hardness of PCBN can be adjusted in various ways by adjusting the size and content of the CBN crystal grains and the type of binder.

[0029] The tip of the rotary tool is the region that comes into contact with the workpieces and their fluidized portion (softened portion) during joining. For example, in the case of a rotary tool with a probe as shown in FIGS. 4A and 4B, the tip of the rotary tool has a probe and a shoulder. In the case of a rotary tool without a probe as shown in FIGS. 5A, 5B, 6A, 6B, 7A, and 7B, the tip of the rotary tool has a shoulder. Furthermore, it is preferable that the tip of the rotary tool include a region extending from the shoulder toward the base portion on the opposite side of the rotary tool in the direction of the rotation axis of the rotary tool, extending from 0 to 5 mm.

[0030] The shoulder has a flat shape formed by a roughly flat surface or a gently curved surface. The shoulder has the function of coming into contact with the workpieces as it rotates during welding, generating frictional heat. The shoulder also has the function of pressing the area softened by heat to prevent the material from scattering and promote plastic flow in the direction of rotation.

[0031] The probe is discontinuous with the shoulder and projects almost perpendicularly toward the workpieces. The probe penetrates the softened portion of the workpieces toward the center of the thickness during welding, thereby improving the stirring ability near the center of the thickness. The probe is usually located at the center of the tip.

[0032] The portion of the rotary tool other than the tip portion may be made of the same material as the tip portion or a different material from the tip portion. The different material from the tip portion is preferably a material harder than the workpiece. Specific examples include tungsten carbide (WC) and nickel-based alloys.

[0033] The shape of the rotary tool is not particularly limited, and examples include the above-mentioned rotary tool with a probe (FIGS. 4A and 4B) and a rotary tool without a probe. However, since the probe is located in a region close to the center of the thickness direction of the workpieces during joining, it is subjected to greater stress than the shoulder, making it more susceptible to breakage and wear. Therefore, from the perspective of tool durability, a rotary tool without a probe is preferred. Suitable examples of a rotary tool without a probe include a flat-tip rotary tool with a flat tip as shown in FIGS. 5A and 5B, a convex-tip rotary tool with a convex curved tip as shown in FIGS. 6A and 6B, and a concave-tip rotary tool with a concave curved tip as shown in FIGS. 7A and 7B. Furthermore, for both the rotary tool with a probe and the rotary tool without a probe, the shape of the tip surface in a plane perpendicular to the tool rotation axis (the projected area when the tip surface of the rotary tool is projected in a direction parallel to the rotation axis) is circular.

[0034] Furthermore, from the viewpoint of further promoting material flow, it is preferable that the tip surface of the rotary tool has a spiral-shaped (helical) step portion, particularly a spiral-shaped (helical) step portion in the direction opposite to the rotation. The spiral-shaped step portion is defined by a radial curve (swirl) that starts, for example, at the center of the tip surface of the rotary tool or at the periphery of a central circle (a circle of any diameter centered at the center of the tip surface of the rotary tool) of the tip surface of the rotary tool and extends to the outer periphery of the tip surface of the rotary tool, as shown in Figures 5B, 6B, and 7B. Note that in all of Figures 5B, 6B, and 7B, the number of swirls is four.

[0035] That is, in friction stir welding, frictional heat is generated when the rotary tool presses and stirs the workpieces, softening and flowing the metal material. By providing a spiral-shaped step portion on the tip surface of the rotary tool in the direction opposite to the rotation direction of the rotary tool, frictional heat is generated from the outside to the inside of the rotary tool. This prevents the metal material from flowing out of the area pressed by the rotary tool. As a result, plastic flow in the pressed area can be promoted. In addition, it is possible to prevent the thickness of the joint from decreasing relative to the thickness of the base material. Furthermore, it is possible to form a joint surface with fewer burrs.

[0036] The number of vortices defining the step portion may be one or more. However, if the number of vortices defining the step portion exceeds six, the effect of promoting material flow will be reduced. In addition, the complicated shape may make the step portion more susceptible to breakage. Therefore, it is preferable that the number of vortices defining the step portion be six or less.

[0037] In one example, the step portion changes its height position in a step-like manner for each region between vortices. For example, when the tip surface of the rotary tool is a convex curved surface, the step portion is configured by gradually lowering from the periphery of the center toward the outer periphery of the tip surface of the rotary tool (the end of the tip surface of the rotary tool), as shown in FIG. 8A . Note that when the tip surface of the rotary tool is a concave curved surface, the step portion is configured by gradually raising from the periphery of the center toward the outer periphery of the tip surface of the rotary tool (the end of the tip surface of the rotary tool). Hereinafter, such a shape of the step portion is also referred to as a stepped portion. Furthermore, in a cross section that includes the rotation axis and is parallel to the rotation axis, each step portion may be, for example, approximately horizontal.

[0038] In another example, the step portion is formed by providing a recess (groove) or a protrusion at the position of the swirl, as shown in Figure 8B. Hereinafter, such a step portion shape will also be referred to as a recess-shaped or protrusion-shaped. Examples of the cross-sectional shape of the recess (groove) include a U-shape (including a square shape and a semicircular shape), a V-shape, and a V-shape, but any shape that can achieve the above-mentioned effect is acceptable.

[0039] It is also preferable that the relationship of the following equation (1) is satisfied: 4×t   ≦   D   ≦   20 × t (1) In the formula, t: thickness of the workpieces to be welded (mm) D: diameter of the tip of the rotary tool (mm). When the thicknesses of the workpieces to be welded are different in butt joining, t is the average value of the thicknesses of the workpieces to be welded. In the case of lap joining, t is the thickness of the overlapping portion of the workpieces to be welded (total thickness of the workpieces to be welded). Furthermore, D is the diameter of the tip of the rotary tool in a plane perpendicular to the rotation axis (the diameter of the projected area when the tip of the rotary tool is projected in a direction parallel to the rotation axis).

[0040] That is, the diameter of the tip of the rotary tool (hereinafter also referred to as tip diameter) is appropriately controlled according to the thickness of the workpieces, particularly to satisfy the above-mentioned formula (1). This allows the temperature rise due to frictional heat generated between the rotary tool and the workpieces and the shear stress due to frictional force to be effectively applied to the workpieces. Here, if D is less than 4 × t (mm), uniform material flow in the thickness direction of the workpieces may not be effectively achieved. On the other hand, if D exceeds 20 × t (mm), the region where plastic flow occurs unnecessarily expands, and excessive heat is input to the joint. This may result in excessive load on the joining device. D is preferably 5 × t (mm) or more, more preferably 6 × t (mm) or more. D is preferably 15 × t (mm) or less, more preferably 10 × t (mm) or less.

[0041] The shape of the base portion of the rotary tool opposite to the tip portion is not particularly limited as long as it can be attached to a conventionally known friction stir welding device.

[0042] The shape of the rotary tool other than the above is not particularly limited and may be a conventional one. For example, the rotary tool shown in Fig. 4A has a tip diameter of 12 mm, a probe diameter (hereinafter also referred to as pin diameter) of 4 mm, a probe length (hereinafter also referred to as pin length) of 0.5 mm, and a concave depth of 0.3 mm. The rotary tool shown in Fig. 4B has a tip diameter of 20 mm, a pin diameter of 6.7 mm, a pin length of 0.7 mm, and a concave depth of 0.3 mm.

[0043] Furthermore, in double-sided friction stir welding, a pair of rotating tools having the same shape is usually used.

[0044] [2] Friction stir welding Next, friction stir welding using a rotary tool according to one embodiment of the present invention will be described. In friction stir welding, it is sufficient to use a rotary tool according to one embodiment of the present invention, and the joint type and joining conditions may be in accordance with conventional methods.

[0045] First, suitable examples of joining types include butt joining as shown in FIG. 1 and lap joining as shown in FIG. 2. In butt joining, the end faces of the workpieces are placed opposite each other, and a rotary tool is pressed against the butt joint, including the end faces (butt joints), while rotating. Then, in this state, the rotary tool is moved in the joining direction to join the workpieces. In lap joining, at least a portion of the end portions of the workpieces are overlapped, and the rotary tool is pressed against the overlapping joint while rotating. Then, in this state, the rotary tool is moved in the joining direction to join the workpieces. In FIGS. 1 and 2, reference numeral 1-1 denotes the rotary tool (front surface side rotary tool), reference numeral 1-2 denotes the tip portion, reference numeral 2-1 denotes the rotary tool (rear surface side rotary tool), reference numeral 2-2 denotes the tip portion, reference numeral 3 denotes the workpieces, and reference numeral 4 denotes the joining portion.

[0046] Butt joining and lap joining differ only in the shape of the unjoined portion, and the other configurations of the equipment are basically the same. Therefore, here we will explain an example of butt joining by double-sided friction stir welding, as shown in Figure 1.

[0047] In double-sided friction stir welding, for example, a friction stir welding apparatus is used that includes a pair of opposing rotary tools, a drive device for the rotary tools, a gripping device, and a control device that controls the operation of the rotary tools. The control device controls, for example, the tilt angle α of the rotary tools, the distance G between the tips of the rotary tools, the welding speed, and the rotation speed of the rotary tools.

[0048] As shown in FIG. 1 , the rotary tools of the friction stir welding apparatus are placed on both sides of the workpieces. The rotary tool placed on the front side (vertically upper side) of the workpieces is sometimes referred to as the front-side rotary tool, and the rotary tool placed on the back side (vertically lower side) of the workpieces is sometimes referred to as the back-side rotary tool. The workpieces are placed parallel to the welding center line shown in the figure and are each gripped by a gripping device (not shown). The rotary tool is then rotated and pressed against both sides of the unwelded portion (region to be welded) located on the welding center line, i.e., the butt joint between the ends of the workpieces. Next, in this state, the rotary tool is moved in the welding direction. This softens the workpieces due to frictional heat between the rotary tool and the workpieces. The softened portion is then stirred with the rotary tool, causing plastic flow and joining the workpieces. A weld (butt joint) is formed where the welding is completed.

[0049] Here, it is preferable that the rotation directions of the front-side rotary tool and the back-side rotary tool are opposite when viewed from the front side (or back side) of the workpieces. This allows the rotational torques applied to the workpieces from the front-side rotary tool and the back-side rotary tool to cancel each other out. As a result, it is possible to simplify the structure of the jig that restrains the workpieces compared to one-sided friction stir welding, in which the unjoined portions are joined by pressing from one side.

[0050] If the rotation directions of the front-side rotary tool and the back-side rotary tool are the same as viewed from the front (or back) sides of the workpieces, the relative speed of one rotary tool relative to the other rotary tool approaches zero. As a result, the plastic flow of the workpieces approaches a homogeneous state, and plastic deformation also decreases. Therefore, heat generation due to plastic deformation of the material is no longer obtained, making it difficult to achieve a good joining state. Therefore, from the viewpoint of obtaining a temperature rise and shear stress sufficient to achieve a good joining state uniformly in the thickness direction of the workpieces, it is preferable to rotate the front-side rotary tool and the back-side rotary tool in opposite directions as viewed from the front (or back) sides of the workpieces.

[0051] Furthermore, when using a rotary tool with a probe, it is preferable that the tilt angle α of the rotary tool satisfy the relationship of the following equation (2): 0°< α≦3° (2) Here, α is the tilt angle of the rotation axis of the rotary tool (hereinafter also referred to as the rotation axis of the tool) from the thickness direction of the workpieces (direction perpendicular to the surface of the workpieces) in a plane including the joining direction and the thickness direction (direction perpendicular to the surface of the workpieces), as shown in FIG. 3B. The direction (angle) in which the tip of the rotary tool leads the joining direction is defined as +. Note that FIG. 3A is a top view showing an example of butt joining by double-sided friction stir welding, i.e., a view of the state in which double-sided friction stir welding is being performed, viewed from above in the vertical direction where the surface-side rotary tool is positioned. Also, FIG. 3B is a view taken along the arrows A-A' in FIG. 3A. In Figures 3A and 3B, reference numeral 1-1 denotes a rotary tool (front surface side rotary tool), reference numeral 1-2 denotes a tip portion, reference numeral 1-3 denotes a probe, reference numeral 2-1 denotes a rotary tool (rear surface side rotary tool), reference numeral 2-2 denotes a tip portion, reference numeral 2-3 denotes a probe, reference numeral 3 denotes a workpiece, and reference numeral 4 denotes a joining portion.

[0052] That is, the rotary tool is usually made of a material harder than the workpieces. However, when a bending force is applied to the probe, stress concentrates locally, which may lead to breakage. In this regard, if the rotation axis of the tool is tilted from the thickness direction of the workpieces and the tip of the probe is advanced in the welding direction, the load on the rotary tool is received by the rotary tool as a component of compressive force in the rotation axis direction, and the force in the bending direction can be reduced. This improves the durability of the rotary tool.

[0053] Here, when α exceeds 0°, the above-mentioned effect can be obtained. However, when the tilt angle α of the rotary tool exceeds 3°, the front and back surfaces of the joint become concave, which may have an adverse effect on the joint strength. Therefore, it is preferable to set α in the range of 0° < α ≦ 3° for both the front-side rotary tool and the back-side rotary tool.

[0054] Furthermore, when a rotary tool without a probe is used, it is preferable that α satisfies the relationship of the following formula (3): 0°≦α≦3° (3)

[0055] In other words, when using a rotary tool without a probe, there is no need to consider reducing the load of the bending force on the probe. Therefore, even if the rotation axis of the tool is parallel to the thickness direction of the workpieces, i.e., α = 0°, there is no significant effect on the durability of the rotary tool. However, as mentioned above, if the tilt angle α of the rotary tool exceeds 3°, the front and back surfaces of the joint may become concave, which may adversely affect the joint strength. Therefore, it is preferable to set α in the range of 0°≦α≦3° for both the front-side rotary tool and the back-side rotary tool.

[0056] Furthermore, it is preferable that the distance G between the tips of the rotary tools satisfies the relationship of the following equation (4): 0.25×t-0.2×D×sin α≦G≦0.8×t-0.2×D×sin α (4) Here, G corresponds to the distance (shortest distance) in the thickness direction of the workpieces between the shoulder of the front-side rotary tool and the shoulder of the back-side rotary tool, as shown in Fig. 3B. The definitions of t, D, and α are as described above.

[0057] In double-sided friction stir welding, it is advantageous to appropriately control the separation distance between the tips of the rotary tools from the viewpoint of achieving sufficient temperature rise and uniform shear stress application in the thickness direction of the workpieces during welding. Therefore, it is preferable for G to satisfy the relationship of the above formula (4). When α = 0°, that is, when the rotation axis of the tool is not tilted from the thickness direction of the workpieces, it is preferable to control G within the range of 0.25 × t to 0.8 × t. On the other hand, when the rotation axis of the tool is tilted from the thickness direction of the workpieces, it is preferable to satisfy the relationship of the above formula (4) depending on α and D.

[0058] By satisfying the relationship of Equation (4) above for G, the tips of the opposing front-side and back-side rotary tools are pressed against the workpieces with a sufficient load, sufficiently promoting heat generation and material flow. This promotes uniform material flow in the thickness direction of the workpieces, resulting in a good weld. On the other hand, if G exceeds 0.8 × t − 0.2 × D × sin α, the tips of the front-side and back-side rotary tools may not be pressed against the workpieces with a sufficient load, and the above-mentioned effect may not be achieved. Furthermore, if G is less than 0.25 × t − 0.2 × D × sin α, the front and back surfaces of the weld may become concave, which may adversely affect joint strength.

[0059] Furthermore, conditions other than those described above may also follow standard practice. For example, the rotational speed of the rotary tool is preferably 100 to 5000 r / min. Setting the rotational speed of the rotary tool within this range is advantageous because it is possible to maintain a good surface shape of the joint while suppressing deterioration of mechanical properties due to the input of excessive heat. The rotational speed of the rotary tool is more preferably 500 r / min or more. Furthermore, the rotational speed of the rotary tool is more preferably 3000 r / min or less.

[0060] From the viewpoint of improving the efficiency of construction, the joining speed is preferably 1000 mm / min or more, and more preferably 2000 mm / min or more.

[0061] [3] Joined Material The materials to be joined are not particularly limited. Examples of the joined material include high-melting-point alloys such as steel plates. Specific steel types include general structural steel and carbon steel, such as rolled steel for welded structures specified in JIS G 3106 (2020) and carbon steel for mechanical structures specified in JIS G 4051 (2016). High-strength structural steel with a tensile strength of 800 MPa or more can also be advantageously used as the joined material. Even in this case, the tensile strength at the joint can be 85% or more, even 90% or more, and even more preferably 95% or more of the tensile strength of the steel material to be joined.

[0062] The functions and effects of the present invention will be described below using examples, but the present invention is not limited to the following examples.

[0063] Steel plates having the thickness, chemical composition (the balance being Fe and unavoidable impurities), and tensile strength shown in Table 1 were butted together as the workpieces, and double-sided friction stir welding was performed using a pair of rotary tools shown in Table 2 under the following conditions (the same conditions were used for both the front-side rotary tool and the back-side rotary tool), to obtain a welded joint: α: 0° G: 0.80 mm Rotation speed of rotary tool: 1500 r / min Welding speed: 3000 mm / min Welding length: 0.5 m In addition, in the butt welding, a so-called I-groove was formed on the end faces of the two steel plates to be welded, with no groove angle applied to the edges, and the two steel plates were butted together with their surfaces in a state similar to that of milling, and the welding was performed.

[0064] The front-side rotary tool located on the upper side in the vertical direction was rotated clockwise as viewed from above, and the back-side rotary tool located on the lower side in the vertical direction was rotated counterclockwise as viewed from above. In other words, when the tip of each rotary tool was viewed from the front, both rotated counterclockwise. Furthermore, the front-side rotary tool and the back-side rotary tool used had the same cross-sectional dimensions and shape. Conditions not specified were set according to standard methods.

[0065] Next, the resulting bonded joint was checked for (I) surface defects and (II) internal defects in the following manner.

[0066] (I) Surface Defects The presence or absence of surface defects was confirmed by visually observing, in particular, the presence or absence of recesses (hereinafter also referred to as recesses) caused by gouging out of the surface of the joint. When the above recesses were confirmed, their depth D d (mm) was measured using a laser displacement meter. The presence or absence of surface defects and their significance were judged according to the following criteria. The evaluation results are also shown in Table 2. The above observations were carried out in the steady state area, that is, the area where joining was carried out when the joining speed reached 3000 mm / min. <Judgment criteria> No defects (pass, excellent): No recesses were observed. Minor defects (pass): Recesses were observed, but the D of the recesses was d / t is 0.1 or less. Significant defects (fail): D dA depression with a / t of more than 0.1 (including a groove-like unbonded state penetrating from the front surface to the back surface of the bonded portion) was confirmed. (Note that if an unbonded state penetrating from the front surface to the back surface of the bonded portion was confirmed, it was considered that the bond was not established, and the following evaluation was omitted.)

[0067] (II) Internal Defects The welded joint was cut in the thickness (vertical) direction so that the plane including the direction perpendicular to the weld and the thickness direction served as the observation surface, and three test specimens were collected. The cut positions (observation surfaces) in the joining direction were 20 mm from the end of the steady portion on the joining start side, 20 mm from the end of the steady portion on the joining end side, and the middle position of the steady portion. The test specimens were collected so that the cut surfaces at these cutting positions served as the observation surfaces. The observation surfaces of the obtained test specimens were then observed using an optical microscope (magnification: 10x). The presence or absence of internal defects and their significance were evaluated according to the following criteria. <Evaluation Criteria> No defects (pass, excellent): No tunnel-shaped unbonded state was observed in any of the three test specimens. Minor defects (pass): A tunnel-shaped unbonded state was observed in one of the three test specimens. Significant defects (fail): A tunnel-shaped unbonded state was observed in two or more of the three test specimens.

[0068] In addition, No. 1 test pieces specified in JIS Z 3121 (2013) were taken from the bonded joints, and tensile tests were performed in accordance with JIS Z 3121 (2013) to measure the tensile strength. The measurement results are also shown in Table 2.

[0069] (III) Durability of Rotary Tool Furthermore, the durability of the rotary tool was evaluated as follows. That is, when the rotary tool breaks or wears, there is a high probability that a poor weld will occur due to an internal defect. Therefore, under the same conditions as above, welding was repeatedly performed with a welding length of 0.5 m, and the obtained welded joints were judged for the presence or absence of internal defects using the judgment method shown in "(II) Presence or absence of internal defects" above. Then, the durability of the rotary tool was evaluated according to the following criteria based on the maximum number of weldings at which the number of joints judged to be free of internal defects was maintained at 90% or more of the total (hereinafter also referred to as the maximum number of weldings while maintaining 90%). The evaluation results are also shown in Table 2. Good (pass, particularly excellent): The maximum number of weldings while maintaining 90% was 200 or more. Unacceptable (fail): The maximum number of weldings while maintaining 90% was less than 200.

[0070] Here, the maximum number of weldings with 90% maintenance is the maximum value of N that satisfies the following formula (a), where the presence or absence of internal defects in the welded joints obtained in the order of welding is checked, and the number of welded joints for which the presence or absence of internal defects is checked is N: [Number of welded joints determined to be free of internal defects among the welded joints for which the presence or absence of internal defects was checked]÷[Number of welded joints for which the presence or absence of internal defects was checked]×100≧90 ... formula (a)

[0071] For example, if the welded joints obtained in the first to fourth welding attempts are determined to be free of internal defects, and the welded joint obtained in the fifth welding attempt is determined to have an internal defect, then when N = 4, [Total number of welded joints without internal defects among the welded joints checked for the presence or absence of internal defects] ÷ [Number N of welded joints checked for internal defects] × 100 = 4 ÷ 4 × 100 = 100 ≧ 90, and when N = 5, [Total number of welded joints without internal defects among the welded joints checked for the presence or absence of internal defects] ÷ [Number N of welded joints checked for internal defects] × 100 = 4 ÷ 5 × 100 = 80 < 90. That is, in this case, formula (a) is satisfied up to N = 4, and formula (a) is no longer satisfied for the first time at N = 5, so the maximum number of welding attempts while maintaining 90% is 4.

[0072] Furthermore, if the welded joints obtained after the 1st to 10th and 12th to 19th weldings are determined to be free of internal defects, and the welded joints obtained after the 11th, 20th, and 21st weldings are determined to have internal defects, then, when N = 11, [Total number of welded joints without internal defects among welded joints checked for the presence or absence of internal defects] ÷ [Number N of welded joints where internal defects were confirmed] × 100 = 10 ÷ 11 × 100 ≒ 90.9 ≧ 90, when N = 20, [Total number of welded joints without internal defects among welded joints checked for the presence or absence of internal defects] ÷ [Number N of welded joints where internal defects were confirmed] × 100 = 18 ÷ 20 × 100 = 90 ≧ 90, and when N = 21, [Total number of welded joints without internal defects among welded joints checked for the presence or absence of internal defects] ÷ [Number N of welded joints where internal defects were confirmed] × 100 = 18 ÷ 21 × 100 = 85.7 < 90. That is, in this case, the formula (a) is satisfied up to N=20, and the formula (a) is not satisfied until N=21. Therefore, the maximum number of joinings while maintaining 90% is 20.

[0073]

[0074]

[0075] As shown in Table 2, in all of the inventive examples, the occurrence of defects during joining was suppressed even when the joining speed was increased to 3000 mm / min and the tool rotation speed was increased to a high rotation speed of 1500 r / min. The durability of the rotary tool was also excellent. Furthermore, in all of the inventive examples, the tensile strength of the joint was 95% or more of the tensile strength of the joined materials, and sufficient joint strength was obtained. On the other hand, in all of the comparative examples, the durability of the rotary tool was insufficient. Furthermore, significant surface defects were confirmed in comparative examples 6 and 7.

[0076] Furthermore, when the rotary tool of the above-mentioned invention was used to perform double-sided friction stir welding of various workpiece materials under various welding conditions, with butt joints or lap joints as the joint type, it was possible to simultaneously achieve the suppression of defect occurrence during welding, an increase in welding speed, and an improvement in the durability of the rotary tool, as described above. Furthermore, sufficient joint strength was obtained at the welded joint.

[0077] 1-1: Rotating tool (front side rotating tool) 1-2: Tip 1-3: Probe 2-1: Rotating tool (rear side rotating tool) 2-2: Tip 2-3: Probe 3: Workpiece 4: Joint

Claims

1. A rotating tool for double-sided friction stir welding, the tip of which is made of a material having a dynamic friction coefficient of less than 0.30 and a Vickers hardness of 2500 HV or more.

2. A rotating tool for double-sided friction stir welding as described in claim 1, wherein the rotating tool is a probe-less rotating tool, and the tip surface of the rotating tool is a flat surface, a convex curved surface, or a concave curved surface.

3. A rotating tool for double-sided friction stir welding as described in claim 2, wherein the tip surface of the rotating tool has a spiral-shaped step portion facing in the opposite direction to the rotation direction.

4. The rotary tool for double-sided friction stir welding according to any one of claims 1 to 3, which satisfies the following formula (1): 4×t   <   D   <   20×t (1) where, t is the thickness of the workpieces (mm), and D is the diameter of the tip of the rotary tool (mm).

Citation Information

Patent Citations

  • Friction welding method and device thereof

    JP1987183979A

  • friction welding method

    JP1995505090A

  • Friction stir welding method

    JP2003181655A

  • Surface friction joining device, and surface friction tool

    JP2003290936A

  • Method for joining thin plate

    JP2004195480A