Alumina granule
Alumina granules with specific structural and additive properties improve low-temperature sinterability and translucency, enabling efficient production of dense, translucent alumina sintered bodies at reduced energy costs for dental applications.
Patent Information
- Application Number
- PCT/JP2024/010515
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-25
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-24
AI Technical Summary
Existing alumina granules lack low-temperature sinterability, leading to high energy consumption during sintering processes, as they do not efficiently produce dense alumina sintered bodies at lower temperatures.
Alumina granules with specific properties, including a pore radius of 0.055 μm or less, primary alumina particles with a specific surface area of 90 nm to 200 nm, high circularity, and an aspect ratio of 1.40 or less, and the addition of sintering aids like magnesium oxide, which enhance low-temperature sinterability and translucency.
The alumina granules achieve sufficient densification and translucency at lower sintering temperatures (1250°C to 1350°C), reducing energy consumption and producing high-density, translucent alumina sintered bodies suitable for dental prosthetics.
Smart Images

Figure JP2024010515_24102024_PF_FP_ABST
Abstract
Description
Alumina Granules
[0001] The present disclosure relates to alumina granules.
[0002] One method for producing a sintered ceramic body involves press-molding a ceramic raw material to form a compact, and then sintering the compact. Ceramic granules are known as a ceramic raw material for press molding (see, for example, Patent Documents 1 and 2).
[0003] Patent Document 1 discloses ceramic granules containing an organic component and ceramic powder, having an average granule diameter Dp of 10 to 90 μm and a compressive fracture strength σp of 0.1 to 5 MPa, and the average granule diameter Dp and compressive fracture strength σp satisfy the following formula: 10≦Dp×σp≦45 [μm·MPa].
[0004] Patent Document 2 discloses ceramic granules for press molding that contain an organic component and ceramic powder, and are characterized in that the average granule size of the ceramic granules for press molding is 40 to 100 μm and the moisture content of the ceramic granules for press molding is 0.6 to 1.5 wt %.
[0005] JP 2006-27914 A JP 2007-197265 A
[0006] From the viewpoint of reducing energy consumption during sintering, alumina granules that can produce a dense alumina sintered body at a low sintering temperature (i.e., have excellent low-temperature sinterability) are desirable. However, Patent Documents 1 and 2 do not discuss improving the low-temperature sinterability of alumina granules.
[0007] The present disclosure has been made in view of the above circumstances, and an object of the present disclosure is to provide alumina granules that are excellent in low-temperature sintering property.
[0008] A first aspect of the present invention is an alumina granule formed by binding primary alumina particles with a binder, wherein the pores inside the granules have a pore radius that indicates the maximum value of the logarithmic differential pore volume of 0.055 μm or less.
[0009] A second aspect of the present invention is the alumina granules according to the first aspect, wherein the primary alumina particles have a specific surface area diameter of 90 nm or more and less than 200 nm.
[0010] A third aspect of the present invention is the alumina granules according to the first or second aspect, wherein the primary alumina particles have an average circularity of 0.74 or more.
[0011] A fourth aspect of the present invention is the alumina granule according to any one of the first to third aspects, wherein the primary alumina particles have an average aspect ratio of 1.40 or less.
[0012] A fifth aspect of the present invention is the alumina granules according to any one of the first to fourth aspects, further comprising a sintering aid in an amount of 10 to 3,000 ppm in terms of metal element relative to 100% by mass of the alumina content in the alumina granules.
[0013] According to the present disclosure, alumina granules having excellent low-temperature sinterability can be provided.
[0014] Fig. 1 is a graph plotting logarithmic (Log) differential pore volume against pore radius for pores of alumina granules according to an embodiment. Fig. 2 is an SEM image of alumina granules of Examples 1 and 2. Fig. 3 is an SEM image of alumina granules of Comparative Examples 1 and 2. Fig. 4 is a photograph of a sintered body for measuring translucency. Fig. 5 is a photograph of a colored alumina sintered body.
[0015] The present inventors have conducted extensive research to develop alumina granules with excellent low-temperature sinterability. As a result, they have found that it is sufficient for the pores inside the alumina granules, which are composed of primary alumina particles, to have a pore radius that indicates the maximum value of the logarithmic differential pore volume equal to or smaller than a certain value. The alumina granules according to this embodiment will be described in detail below.
[0016] [Alumina Granules] (Pores inside the granules have a pore radius of 0.055 μm or less, which indicates the maximum value of the logarithmic differential pore volume) The alumina granules are composed of primary alumina particles bound together with a binder. Inside the alumina granules, pores are present formed between a plurality of primary alumina particles. In the alumina granules of this embodiment, the pore radius of the pores inside the granules, which indicates the maximum value of the logarithmic differential pore volume (hereinafter simply referred to as the "pore radius of the alumina granules"), is 0.055 μm or less. Such alumina granules are considered to have excellent low-temperature sintering properties for the following reasons.
[0017] A small pore radius of alumina granules means that the gaps between primary alumina particles within the alumina granules are narrow. It is believed that such alumina granules promote densification during sintering. As a result of extensive research, the inventors have found that when the pore radius of alumina granules is 0.055 μm or less, sufficient densification progresses even at low sintering temperatures (e.g., 1250°C to 1350°C), and a high-density alumina sintered body can be obtained. The pore radius of the alumina granules is preferably 0.050 μm or less, more preferably 0.043 μm or less, and even more preferably 0.040 μm or less. A smaller pore radius of the alumina granules is preferable, e.g., 0.001 μm or more.
[0018] The pore radius of the alumina granules is determined from a graph plotting the logarithmic (Log) differential pore volume against the pore radius obtained in the pore size analysis measurement. The pore size analysis measurement is performed using a pore size distribution measurement device (e.g., a Micromeritics AutoPore V9600 pore size distribution measurement device) at an absolute measurement pressure range of 1.07 to 59,256 psia. A graph is created in which the logarithmic (Log) differential pore volume is plotted against the pore radius obtained by the pore size distribution measurement device (see FIG. 1). The graph in FIG. 1 has two peaks, the peak with the smaller pore radius (first peak) corresponds to the pores inside the alumina granules, and the peak with the larger pore radius (second peak) corresponds to the gaps (pores) between multiple alumina granules. The position of the apex of the first peak, that is, the pore radius showing the maximum value of the logarithmic differential pore volume, is determined and is taken as the pore radius of the alumina granule.
[0019] (Specific surface area diameter of primary alumina particles is 90 nm or more and less than 200 nm) The specific surface area diameter of the primary alumina particles constituting the alumina granules is preferably 90 nm or more and less than 200 nm, which can further improve the low-temperature sintering property of the alumina granules. The specific surface area diameter of the primary alumina particles is preferably 90 nm or more, more preferably 110 nm or more, even more preferably 130 nm or more, particularly preferably 140 nm or more, and is preferably less than 200 nm, more preferably 190 nm or less, even more preferably 170 nm or less, particularly preferably 145 nm or less.
[0020] The specific surface area diameter of the primary alumina particles is calculated from the following formula (1), which is a general formula showing the relationship between the particle diameter and the specific surface area of spherical particles: A = 6 / (S × ρ) (1), where A is the specific surface area diameter of the primary alumina particles (μm), S is the specific surface area of the primary alumina particles (m 2 / g), and ρ: density of primary alumina particles (g / cm 3 ) and herein is 3.99 g / cm 3 Let's say.
[0021] The specific surface area (BET specific surface area) of the primary alumina particles is determined by the single-point nitrogen adsorption method in accordance with JIS Z 8830:2013, "Method for measuring the specific surface area of powders (solids) by gas adsorption." The specific surface area of the primary alumina particles can be measured either after calcining the alumina granules at 600°C to remove the binder, or by measuring the primary alumina particles as they are before granulation. Either measurement method yields substantially similar results. Specifically, the measurement method involves using a Macsorb fully automatic specific surface area measuring device manufactured by Mountech Co., Ltd., placing 0.1 g of a sample (calcined alumina granules or primary alumina particles before granulation) in a cell, pretreating the sample at 200°C for 20 minutes, and then measuring the specific surface area by nitrogen adsorption.
[0022] (Average circularity of primary alumina particles is 0.74 or more) The average circularity of the primary alumina particles is preferably 0.74 or more, which can further improve the low-temperature sinterability of the alumina granules. This is because the higher the average circularity of the primary alumina particles (i.e., the closer the primary alumina particles are to being spherical), the narrower the gaps between the primary alumina particles and the better the packing ability. The average circularity of the primary alumina particles is preferably 0.74 or more, more preferably 0.79 or more. The upper limit of the average circularity of the primary alumina particles is 1.00.
[0023] (Average aspect ratio of primary alumina particles is 1.40 or less) The average aspect ratio of primary alumina particles is preferably 1.40 or less, which can further improve the low-temperature sinterability of alumina granules. The aspect ratio in this specification is determined by measuring the maximum diameter of primary alumina particles and the particle size in a direction perpendicular to the direction in which the maximum diameter is measured, and then calculating the ratio of the "maximum diameter" to the "particle size in the perpendicular direction." The minimum value of the average aspect ratio of primary alumina particles defined in this manner is 1. An average aspect ratio of 1.40 or less is presumed to mean that the average aspect ratio is close to 1 and that the primary alumina particles have a shape that is close to spherical. Near-spherical primary alumina particles narrow the gaps between multiple primary alumina particles, improving packing properties.
[0024] The average aspect ratio of the primary alumina particles is preferably 1.40 or less, more preferably 1.30 or less. The average aspect ratio of the primary alumina particles may be 1.05 or more, 1.10 or more, or 1.20 or more.
[0025] The average circularity and average aspect ratio of the primary alumina particles can both be determined by image analysis of SEM images of the alumina granules.
[0026] An example of the measurement method is described below. Using a scanning electron microscope (e.g., a scanning electron microscope S-5500 manufactured by Hitachi High-Technologies Corporation), SEM images of the alumina granules are taken at an acceleration voltage of 1 keV. When obtaining SEM images of the alumina granules, the magnification is adjusted so that 100 to 300 primary alumina particles constituting the alumina granules are captured per image. For example, the magnification is 10,000 to 50,000. The SEM images of the alumina granules of Examples 1 and 2 shown in FIG. 2 were taken at 40,000 magnification, the SEM image of the alumina granules of Comparative Example 1 shown in FIG. 3 was taken at 25,000 magnification, and the SEM image of the alumina granules of Comparative Example 2 was taken at 25,000 magnification.
[0027] Image analysis of SEM images can be performed using commercially available image analysis software (e.g., Image J (manufactured by the National Institute of Health)) or an image analysis service (e.g., DeepCle (Sakai Chemical Industry Co., Ltd.)). In the examples, automatic AI analysis was performed using Sakai Chemical Industry Co., Ltd.'s AI image analysis service DeepCle (AI model: 3.3087_2f_r). The circularity and aspect ratio of 100 to 300 primary alumina particles are determined by image analysis. The multiple circularities obtained are arithmetically averaged to determine the average circularity. Similarly, the multiple aspect ratios obtained are arithmetically averaged to determine the average aspect ratio.
[0028] (Containing 10 to 3000 ppm of sintering aid) The alumina granules may contain 10 to 3000 ppm of sintering aid, if necessary. When the alumina granules are sintered, the sintering aid contained in the alumina granules acts to promote sintering. The content (ppm) of the sintering aid is determined as the content of the sintering aid converted to metal element when the alumina content in the alumina granules is taken as 100 mass%. The content of the sintering aid is preferably 10 ppm or more, more preferably 100 ppm or more, even more preferably 200 ppm or more, and particularly preferably 300 ppm or more, and is preferably 3000 ppm or less, more preferably 2000 ppm or less, and even more preferably 1500 ppm or less.
[0029] The sintering aid to be used is one that is effective as a sintering aid during sintering in air. Examples of sintering aids suitable for this embodiment include compounds that become oxides at 1200°C or less in air, and these can function as sintering aids during low-temperature sintering (e.g., 1250°C to 1350°C). Examples of compounds include oxides, nitrates, acetates, hydroxides, and chlorides. Specifically, compounds of magnesium, titanium, scandium, yttrium, zirconium, hafnium, lanthanum, zinc, tin, and the like are suitable. Among these, magnesium compounds, particularly magnesium oxide, are preferred.
[0030] As a result of investigations by the present inventors, it was found that alumina granules containing an appropriate amount of one or more sintering aids selected from the group consisting of magnesium compounds, zinc compounds, and tin compounds (e.g., a total of 300 ppm to 1200 ppm of sintering aids) are suitable for producing an alumina sintered body with excellent translucency. In recent years, alumina sintered bodies have been considered as dental materials, and the alumina granules according to the present embodiment, which have excellent low-temperature sintering properties, have the advantage that alumina sintered bodies for prosthetic use can be sintered in a simple heating furnace. Furthermore, alumina granules containing the above-described sintering aids can produce alumina sintered bodies with excellent translucency, making them suitable as a raw material for dental prosthetic materials with a natural transparency.
[0031] The present inventors further investigated the sintering temperature when magnesium oxide is used as a sintering aid, and found that translucency is exhibited at a sintering temperature of at least 1350°C, and that the translucency is further improved at a sintering temperature of 1450°C.
[0032] The alumina granules may contain a coloring additive to control the color of the alumina sintered body. Examples of the coloring additive include one or a combination of two or more compounds of chromium, manganese, cobalt, nickel, iron, and the like. Examples of the compound include oxides, nitrates, acetates, hydroxides, and chlorides. The color of the alumina sintered body depends on the type of coloring additive. For example, a red alumina sintered body can be obtained by using a compound containing chromium or manganese, a blue alumina sintered body can be obtained by using a compound containing cobalt, a green alumina sintered body can be obtained by using a compound containing nickel, and a yellow alumina sintered body can be obtained by using a compound containing iron. By appropriately selecting the type of coloring additive, an alumina sintered body having a desired color (e.g., bright red) can be obtained.
[0033] The amount of the coloring additive added is preferably 10 to 3,000 ppm in terms of metal element when the alumina content in the alumina granules is taken as 100 mass %.
[0034] The contents of sintering aids (e.g., magnesium oxide) and coloring additives (e.g., chromium oxide) can be determined from quantitative elemental analysis (e.g., quantitative analysis of Mg and Cr) by inductively coupled plasma atomic emission spectroscopy (ICP-AES).
[0035] The alumina granules may have a particle size D50 of 30 μm or more and 150 μm or less, which is the cumulative 50% particle size from the fine particle side of the cumulative particle size distribution on a volume basis. The D50 of the alumina granules is measured by a laser diffraction / scattering method. An example of the measurement method will be described. The alumina granules are added to a 0.2% aqueous solution of sodium hexametaphosphate and dispersed by stirring with a stirrer for 30 seconds. The dispersion is placed in a measurement cell and degassed, and then measured using a Microtrac particle size distribution analyzer MT-3300 manufactured by Microtrac-Bell Corporation with a measurement time of 10 s, two measurements, a particle refractive index of 1.77, and a solvent refractive index of 1.333, to determine the D50. Note that if the alumina granules are stirred with a stirrer for a short period of time, they rarely separate into primary alumina particles.
[0036] (Containing 0.1 to 5.0% by mass of binder) The content of the binder contained in the alumina granules is desirably an amount sufficient to bind the primary alumina particles together while not affecting the pore radius within the alumina granules. From this perspective, the alumina granules preferably contain 0.1 to 5.0% by mass of binder, based on 100% by mass of the entire alumina granules (including the binder). The content of the binder contained in the alumina granules is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, particularly preferably 0.8% by mass or more, and is preferably 5.0% by mass or less, more preferably 4.0% by mass or less, even more preferably 2.0% by mass or less, and particularly preferably 1.8% by mass or less, based on 100% by mass of the entire alumina granules. The binder content can be determined from the weight loss in thermal analysis.
[0037] [Method for producing alumina granules] The method for producing the alumina granules of the embodiment is not particularly limited, but it is preferable to adopt the following production method because it allows alumina granules having the above physical properties to be produced with good reproducibility. Note that a person skilled in the art who has read the disclosure of the present application may arrive at a different method for producing the alumina granules of the embodiment based on the description therein.
[0038] The method for producing alumina granules includes the steps of preparing primary alumina particles, preparing an alumina slurry containing the primary alumina particles, and granulating alumina granules from the alumina slurry.
[0039] (Step of Preparing Primary Alumina Particles) The step of preparing primary alumina particles includes the steps of: preparing a seed crystal slurry in which seed crystals are dispersed; mixing the seed crystal slurry with aluminum alkoxide to obtain an aluminum hydroxide slurry; drying and firing the aluminum hydroxide slurry to obtain alumina particles (primary alumina particles); and pulverizing the obtained alumina particles.
[0040] (1. Step of preparing seed crystal slurry) Alumina particles (seed crystal raw material) are dispersed in water and then wet-pulverized in a ball mill. Then, the mixture is centrifuged in a refrigerated centrifuge (for example, CR7N manufactured by Himac) to remove precipitates. This yields a seed crystal slurry in which the seed crystals are dispersed. The seed crystals are preferably alpha alumina. By using alpha alumina seed crystals, the alpha conversion of alumina can be promoted by low-temperature sintering in the sintering step described below. The seed crystals preferably have a small particle size, and those with a particle size of 0.01 μm to 0.2 μm are usually used.
[0041] The BET specific surface area of the seed crystals can affect the physical properties of the primary alumina particles that are finally obtained. In order to set the distribution RSD of the alumina powder within the range according to the embodiment (0.25 to 0.80) and / or to set the crystallite diameter within the preferred range (650 to 1400 Å), the BET specific surface area of the seed crystals is preferably 30 m 2 / g or more, more preferably 40m 2 / g or more, more preferably 50m 2 / g or more, particularly preferably 70m 2 The BET specific surface area is measured by the same method as that for measuring the BET specific surface area of primary alumina particles.
[0042] (2. Step of mixing the seed crystal slurry and the aluminum alkoxide to obtain an aluminum hydroxide slurry) The seed crystal slurry and aluminum alkoxide are continuously supplied to a stirrer and mixed. This mixture is subjected to high-speed rotational shear stirring in the stirrer, whereby the water in the seed crystal slurry and the aluminum alkoxide undergo a hydrolysis reaction, thereby obtaining a slurry containing aluminum hydroxide particles as a hydrolyzate (aluminum hydroxide slurry).
[0043] As used herein, "high-speed rotational shear mixing" refers to mixing performed by mechanical energy such as shear force, pressure fluctuation, cavitation, collision force, and potential core that occurs between the turbine (rotor) and stator (screen) when the clearance between the turbine (rotor) and stator (screen) is small (e.g., 2 mm or less) and the turbine (rotor) rotates at high speed (e.g., peripheral speed of about 1 m / sec to about 40 m / sec). In high-speed rotational shear mixing, the rotation speed of the turbine (rotor) is 3,000 rpm to 21,500 rpm, preferably 8,000 rpm to 15,000 rpm, for example, 10,000 rpm.
[0044] (3. Step of drying and calcining the aluminum hydroxide slurry to obtain alumina particles (primary alumina particles)) The aluminum hydroxide slurry is dried by a known method, and the obtained aluminum hydroxide is calcined in a calcination furnace to obtain alumina particles (primary alumina particles). The calcination is carried out usually at 800°C or higher, preferably 900°C or higher, and usually at 1000°C or lower, preferably at 980°C or lower, and more preferably at 960°C or lower. The calcination may be carried out in the air or in an inert gas such as nitrogen gas or argon gas, and it is effective to carry out the calcination while maintaining a high water vapor partial pressure in the atmosphere (for example, a dew point of 30°C or higher).
[0045] (Step of Preparing Alumina Slurry Containing Primary Alumina Particles) The obtained primary alumina particles, binder, dispersant, and solvent are blended, and optionally appropriate amounts of plasticizer, sintering aid, and coloring additive are blended, followed by mechanical stirring and mixing. For stirring and mixing, conventional methods can be used, such as a method of stirring and mixing using a stirring blade or a stirrer while irradiating ultrasonic waves from the outside, a method using various grinding media such as a ball mill or a Dyno Mill, or a method using various agitators such as an attritor or a pin mill.
[0046] As the binder, organic binders such as polyvinyl alcohol, polyvinyl acetal, various acrylic polymers, methyl cellulose, polyvinyl acetate, polyvinyl butyral, various waxes, and various polysaccharides can be used.
[0047] It is preferable to select a suitable solvent depending on the type of binder used and the granulation method of the alumina granules. When granulating the alumina granules using a spray dryer, an acrylic binder is suitable. In this case, water is mainly used as the solvent. Depending on the type of binder used and the granulation method, various organic solvents (acetone, ethanol, toluene, etc.) can be used.
[0048] A dispersant can be added optionally, and it is preferable to select a suitable dispersant depending on the type of solvent used. When the solvent is water, polycarboxylic acid ammonium salts (for example, trade name: SN-D5468, manufactured by San Nopco) are mainly used as dispersants. When an organic solvent is used, ethyl oleate, sorbitan monooleate, sorbitan trioleate, polycarboxylic acid-based dispersants, etc. are used. Polyester-based dispersants (trade name: Texahol 3012, manufactured by San Nopco) are also suitable. However, various dispersants can be used without being limited to these.
[0049] Depending on the organic binder used, it may be possible to prepare a slurry with lower viscosity without using a dispersant, thereby increasing the concentration of alumina granules in the slurry. In such cases, it is not necessary to add a dispersant.
[0050] A plasticizer can be added as desired, and it is preferable to select a suitable plasticizer depending on the type of binder and organic solvent used together. Plasticizers used together with organic binders include ethylene glycol, diethylene glycol, polyethylene glycol, glycerin, polyglycerin, various esters, etc. When an organic solvent is used, dibutyl phthalate, diethylhexyl phthalate, etc. are particularly used, but the present invention is not limited to these.
[0051] A sintering aid can be added as desired. The sintering aid is preferably added so that the amount of sintering aid, calculated as a metal element, is 10 to 3,000 ppm when the alumina content in the alumina granules is taken as 100 mass %.
[0052] The coloring additive may be added as desired. The coloring additive is preferably added so that the amount of the coloring additive, calculated as a metal element, is 10 to 3,000 ppm when the alumina content in the alumina granules is taken as 100 mass %.
[0053] The obtained alumina slurry may be defoamed under reduced pressure. Various antifoaming agents may also be used. Depending on the subsequent molding method, various pH adjusters and flocculants may be added to adjust the viscosity to 10 to 500 centipoise. For example, in granulation using a spray dryer, in order to produce spherical granules, it is preferable to adjust the viscosity of the alumina slurry to 30 to 300 centipoise by pH adjustment using an aqueous hydrochloric acid solution, aqueous ammonia, or the like. Furthermore, the alumina concentration in the slurry can be increased by static settling, centrifugation, vacuum concentration using a rotary evaporator, or the like.
[0054] (Step of Granulating Alumina Granules from Alumina Slurry) The obtained alumina slurry is used to granulate alumina granules. The method for granulating alumina granules from the alumina slurry can be a known spray drying granulation method or oscillating extrusion granulation method. Specifically, the alumina granules can be granulated by spray drying the obtained alumina slurry using a spray drying device (spray dryer) or the like.
[0055] (Variation: Method of directly granulating alumina granules from primary alumina particles) In the above-described method of producing alumina granules, the primary alumina particles are converted into an alumina slurry and then the alumina granules are granulated. However, the primary alumina particles may be granulated directly into alumina granules without converting them into an alumina slurry. For example, the primary alumina particles, a binder, and various additives as desired may be mixed and granulated in an agitation granulator to produce a granulated powder, and the granulated powder may be repeatedly extruded and granulated in an oscillating granulator and dried to produce alumina granules.
[0056] These granulation methods for alumina granules can be appropriately selected depending on the amount of granules for ceramic molding, the properties of the desired ceramic molded body, etc. The oscillating extrusion granulation method is a method in which particles having a particle size of, for example, about several mm are crushed on a mesh and the finer particles are allowed to fall, and the mesh is successively made finer, thereby obtaining particles having a predetermined particle size or less.
[0057] [Method for manufacturing an alumina sintered body] An example of a suitable method for manufacturing an alumina sintered body using the alumina granules according to the embodiment will be described below. The alumina granules are subjected to uniaxial press molding, cold isostatic press molding, or the like to produce a molded body. In the case of cold isostatic press molding, the alumina granules are uniaxially press molded at a pressure of 20 to 40 MPa, preferably 25 to 35 MPa, and then isotropically pressed at 98 MPa or more, preferably 150 to 200 MPa, in a cold isostatic press molding machine, and the obtained molded body is processed into a predetermined shape.
[0058] Two examples of firing conditions for producing an alumina sintered body are given below. (Condition 1) Sintering process: The compact is fired in air or an oxygen atmosphere at a temperature in the range of 1250 to 1350°C for two hours or more to obtain an alumina sintered body. The average heating rate from room temperature to the sintering temperature is, for example, 200°C / hr.
[0059] The alumina granules according to the embodiment have excellent low-temperature sintering properties due to the small radius of the internal pores. For example, even when sintered at a low temperature of 1250 to 1350°C as in Condition 1, a dense alumina sintered body can be produced.
[0060] (Condition 2) Debinding step: The compact is debound by firing at a temperature in the range of 500 to 1200°C for at least one hour, preferably in the range of 600 to 800°C for at least two hours. The average temperature rise rate from room temperature to the firing temperature is, for example, 100°C / hr. Sintering step: After the debinding step, the compact is subsequently fired at a high temperature to obtain an alumina sintered body. In condition 2, the firing atmosphere is not limited. If firing is performed in an air atmosphere, the compact is fired at a temperature in the range of 1200 to 1700°C, preferably 1250 to 1450°C, for at least two hours to obtain an alumina sintered body. The sintering temperature in the sintering step is set to be equal to or higher than the sintering temperature in the debinding step. The average temperature rise rate from the firing temperature in the debinding step to the sintering temperature in the sintering step is, for example, 200°C / hr.
[0061] Condition 2 is suitable not only for obtaining an alumina sintered body by low-temperature sintering, but also for obtaining a translucent alumina sintered body using alumina granules containing a sintering aid. When obtaining a translucent alumina sintered body, the sintering step conditions are preferably such that the alumina sintered body is fired in the air or a vacuum atmosphere at a temperature in the range of 1350°C to 1700°C, and firing at a temperature in the range of 1400°C to 1450°C in particular can further improve the translucency of the alumina sintered body.
[0062] (Example 1) (Preparation of primary alumina particles) Alumina particles (seed crystal raw material) were dispersed in water and then wet-pulverized using a ball mill. The resulting mixture was then centrifuged at 4,000 rpm for 30 minutes using a refrigerated centrifuge (manufactured by Himac: CR7N) to remove precipitates. This produced a seed crystal slurry in which the seed crystals were dispersed.
[0063] Aluminum isopropoxide and the seed crystal slurry were mixed and hydrolyzed using a precision emulsifying and dispersing machine, Clearmix CLM-2.2S (manufactured by M Technique Co., Ltd.), at a rotation speed of 10,000 rpm. This produced an aluminum hydroxide slurry. The compounding ratio of aluminum isopropoxide to the seed crystal slurry was adjusted so that, in terms of metal component oxide, 10 parts by mass of the aluminum component contained in the seed crystals (hereinafter simply referred to as "parts by mass of aluminum in the seed crystals") was contained per 100 parts by mass of the total amount of aluminum isopropoxide and the aluminum component contained in the seed crystals. The content (parts by mass) of each aluminum component was calculated on the assumption that all of the aluminum isopropoxide used was converted to alumina.
[0064] The resulting aluminum hydroxide slurry was dried at 150°C to obtain aluminum hydroxide particles, which were then placed in an alumina crucible and fired in a gas furnace. The firing conditions were to raise the temperature to 965°C at a heating rate of 200°C / hr and hold the temperature for 4 hours to produce primary alumina particles. The specific surface area (BET specific surface area) of the primary alumina particles before being made into alumina granules was measured. This result can be considered to correspond to the specific surface area of the primary alumina particles after being made into alumina granules.
[0065] (Preparation of Alumina Slurry) The obtained primary alumina particles (1700 g), pure water (1054 g), a dispersant (7.95 g, manufactured by San Nopco, SND-5468), and alumina beads (3540 g, manufactured by Nikkato, φ2-SSA999W) were filled into a pot (volume 3 L) with an alumina-lined inner surface, and uniformly dispersed at 65 rpm for 6 hours to prepare an alumina slurry.
[0066] (Preparation of Alumina Granules) The obtained alumina slurry (705 g), pure water (69.6 g), binder (17.4 g, manufactured by Chuo Rika Kogyo Co., Ltd., SA-261P), and plasticizer (4.35 g, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., PEG-400) were mixed and stirred for 10 minutes. The obtained slurry was spray-dried using a spray dryer (Ohkawahara Kakoki Co., Ltd., Li-8 type) under the following conditions: flow rate 79 g / min, atomizer rotation speed 18,000 rpm, inlet temperature 180°C, outlet temperature 90°C, and hot air differential pressure 1.1 kPa to prepare alumina granules.
[0067] The obtained alumina granules were subjected to pore size analysis and SEM observation. The pore radius of the alumina granules was determined from the pore size analysis. The SEM images were analyzed to determine the average circularity and average aspect ratio of the primary alumina particles. Each measurement was performed using the measuring equipment and under the measuring conditions exemplified in the embodiment. Note that no sintering aid (MgO) was added when producing the alumina granules.
[0068] (Preparation of alumina sintered body) The obtained alumina granules (5 g) were filled into a φ20 mm cylindrical mold and subjected to uniaxial compaction at a pressure of 30 MPa for 30 seconds, followed by cold isostatic pressing (CIP) at a pressure of 98 MPa for 3 minutes to obtain an alumina compact. The compact was heated in air at a heating rate of 200 ° C / hr to 1250 ° C or 1350 ° C and held at each temperature for 2 hours to obtain an alumina sintered body. The density of the obtained alumina sintered body was measured in water at 22 ° C by the Archimedes method.
[0069] (Preparation of Sintered Body for Translucency Measurement) The obtained alumina granules (1 g) were filled into a φ20 mm cylindrical mold and subjected to uniaxial compaction at a pressure of 30 MPa for 30 seconds. Subsequently, a 3-minute cold isostatic pressing (CIP) compaction was performed five times at a pressure of 200 MPa to obtain an alumina compact. The compact was heated to 600°C in air at a heating rate of 100°C / hr and held at that temperature for 2 hours for calcination. The alumina calcined body was heated to 1350°C or 1450°C in air at a heating rate of 200°C / hr and held at each temperature for 2 hours to obtain an alumina sintered body for translucency measurement (referred to herein as a "sintered body for translucency measurement"). The surface of this sintered body for translucency measurement was polished, and then the translucency was evaluated.
[0070] Translucency evaluation was performed using a Nippon Denshoku Industries haze meter NDH8000, with the instrument settings conforming to the measurement method for total luminous transmittance (TT) and parallel ray transmittance (PT) of JIS K7361-1:1997. A small diameter attachment was attached, and the measurement diameter was set to the small diameter. Measurements were performed after warming up the instrument for 30 minutes after starting up. The thickness of the sintered compacts for translucency measurement after surface polishing was set to 0.9 to 1.1 mm, and total luminous transmittance TT and parallel ray transmittance PT were measured. Figure 4 is a photograph of the sintered compacts for translucency measurement produced in the examples and comparative examples.
[0071] Example 2 Primary alumina particles were produced, an alumina slurry was prepared, alumina granules were produced, and an alumina sintered body and a sintered body for translucency measurement were produced in the same manner as in Example 1, except that an aluminum hydroxide slurry was prepared at a blending ratio such that the aluminum parts by mass of the seed crystals was 5.6 parts by mass.
[0072] Example 3 An alumina slurry was prepared, alumina granules were produced, and an alumina sintered body was produced in the same manner as in Example 1, except that α-alumina powder AKP-50 (manufactured by Sumitomo Chemical Co., Ltd.) was used as the primary alumina particles.
[0073] Examples 4, 6, and 8 Primary alumina particles were produced, and an alumina slurry was prepared in the same manner as in Example 1. High-purity magnesia powder (150 g, manufactured by Ube Material Industries, Ltd., vapor-phase magnesia 500A) and pure water (2,850 g) were mixed with a disperser for 10 minutes, and then circulated once in a wet disperser (manufactured by Shinmaru Enterprises, Dynomill) under conditions of a peripheral speed of 8 m / s, a flow rate of 500 mL / min, and alumina beads φ0.5 mm (2,690 g), followed by 30 minutes of circulation for uniform dispersion, to prepare a magnesia slurry.
[0074] Alumina slurry (1250 g), magnesia slurry (12.79 g), pure water (111.25 g), binder (30.85 g, manufactured by Chuo Rika Kogyo, SA-261P), and plasticizer (7.71 g, manufactured by Fujifilm Wako Pure Chemical Industries, PEG-400) were mixed and stirred for 10 minutes. The resulting slurry was spray-dried using a spray dryer (Okawahara Kakoki, Li-8 type) under the following conditions: flow rate 79 g / min, atomizer rotation speed 18,000 rpm, inlet temperature 180°C, outlet temperature 90°C, and hot air differential pressure 1.1 kPa to produce alumina granules. The MgO content of the alumina granules is shown in Table 2 as a metal element equivalent value.
[0075] A sintered body for measuring translucency was produced from the obtained alumina granules in the same manner as in Example 1.
[0076] (Examples 5, 7, and 9) Primary alumina particles were produced and an alumina slurry was prepared in the same procedure as in Example 2. Magnesia slurry was prepared and alumina granules were produced in the same procedure as in Example 4, and a sintered body for measuring translucency was produced in the same procedure as in Example 1.
[0077] Example 10 Primary alumina particles were produced and an alumina slurry was prepared in the same manner as in Example 1. A magnesia slurry was prepared in the same manner as in Example 4. Chromium oxide powder (15 g, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and pure water (285 g) were dispersed in a ball mill for 1 hour to produce a chromium oxide slurry.
[0078] Alumina slurry (1250 g), magnesia slurry (12.79 g), pure water (111.25 g), binder (30.85 g, manufactured by Chuo Rika Kogyo, SA-261P), plasticizer (7.71 g, manufactured by Fujifilm Wako Pure Chemical Industries, PEG-400), and chromium oxide slurry (22.5 g) were mixed and stirred for 10 minutes. The resulting slurry was spray-dried using a spray dryer (Okawahara Kakoki, Li-8 type) under the following conditions: flow rate 79 g / min, atomizer rotation speed 18,000 rpm, inlet temperature 180°C, outlet temperature 90°C, and hot air differential pressure 1.1 kPa to produce alumina granules. Note that the MgO and Cr contained in the alumina granules were 2 O 3The contents are shown in Table 4 as metal element equivalent values.
[0079] (Preparation of Colored Alumina Sintered Body) The alumina granules (1 g) obtained in Example 10 were filled into a 20 mm diameter cylindrical mold and subjected to uniaxial compaction at a pressure of 30 MPa for 30 seconds. Subsequently, a 3-minute cold isostatic pressing (CIP) process was repeated five times at a pressure of 200 MPa to obtain an alumina compact. The compact was heated to 600°C in air at a heating rate of 100°C / hr and held at that temperature for 2 hours for calcination. The calcined alumina body was heated to 1450°C in air at a heating rate of 200°C / hr and held at that temperature for 2 hours to obtain a colored alumina sintered body (colored alumina sintered body). The appearance (color) of the colored alumina sintered body was observed with the naked eye. The results of the appearance observation are shown in Table 4. FIG. 5 shows photographs of the colored alumina sintered bodies produced in the examples and comparative examples.
[0080] (Example 11) Alumina slurry, magnesia slurry, chromium oxide slurry, alumina granules, and a colored alumina sintered body were prepared in the same manner as in Example 10, except that primary alumina particles were prepared in the same manner as in Example 2. Note that the MgO and Cr contained in the alumina granules were 2 O 3 The contents are shown in Table 4 as metal element equivalent values.
[0081] Comparative Example 1 An alumina slurry was prepared in the same manner as in Example 1, except that α-alumina powder AKP-30 (manufactured by Sumitomo Chemical Co., Ltd.) was used as the primary alumina particles. Furthermore, alumina granules were produced in the same manner as in Example 1, and an alumina sintered body was produced.
[0082] Comparative Example 2 An alumina slurry was prepared in the same manner as in Example 1, except that α-alumina powder AKP-20 (manufactured by Sumitomo Chemical Co., Ltd.) was used as the primary alumina particles. Furthermore, alumina granules were produced in the same manner as in Example 1, and an alumina sintered body was produced.
[0083] (Comparative Example 3) The same primary alumina particles as in Comparative Example 1 were prepared, and an alumina slurry was prepared in the same procedure as in Comparative Example 1. A magnesia slurry was prepared in the same procedure as in Example 4. Alumina granules were produced in the same procedure as in Example 6. A sintered body for measuring translucency was produced in the same procedure as in Example 1. The content of MgO contained in the alumina granules is shown in Table 2 as a metal element equivalent value.
[0084] (Comparative Example 4) The same primary alumina particles as in Comparative Example 2 were prepared, and an alumina slurry was prepared in the same procedure as in Comparative Example 2. A magnesia slurry was prepared in the same procedure as in Example 4. Alumina granules were produced in the same procedure as in Example 6. A sintered body for measuring translucency was produced in the same procedure as in Example 1. The content of MgO contained in the alumina granules is shown in Table 2 as a metal element equivalent value.
[0085] (Comparative Example 5) Except for preparing the same primary alumina as in Comparative Example 1, an alumina slurry, a magnesia slurry, a chromium oxide slurry, alumina granules, and a colored alumina sintered body were prepared in the same manner as in Example 10. Note that the MgO and Cr contained in the alumina granules were 2 O 3 The contents are shown in Table 4 as metal element equivalent values.
[0086] Tables 1 to 4 show the results of various measurements of the alumina granules and alumina sintered bodies according to the examples and comparative examples.
[0087]
[0088]
[0089]
[0090]
[0091] The measurement results in Tables 1 to 4 will be examined. From the results in Table 1, it was found that in sintering tests at low temperatures (1250°C, 1350°C), the alumina granules according to the examples that satisfy the requirements specified in this embodiment can produce alumina sintered bodies with higher densities than the alumina granules of the comparative examples. This confirms that the alumina granules according to this embodiment have excellent low-temperature sintering properties.
[0092] The results in Tables 2 and 3 show that alumina granules according to Examples that satisfy the requirements of this embodiment can produce alumina sintered bodies with excellent light transmittance compared to the alumina granules of Comparative Examples. Furthermore, when comparing groups of Examples that differ only in the amount of MgO added (the group consisting of Examples 1, 4, 6, and 8, and the group consisting of Examples 2, 5, 7, and 9), it was found that alumina granules with an MgO content of 500 to 1000 ppm can produce alumina sintered bodies with particularly excellent transmittance.
[0093] The results in Table 4 show that the alumina granules according to the examples, which satisfy the requirements of this embodiment, can produce an alumina sintered body with a more vivid red color than the alumina granules of the comparative examples (see FIG. 5). This confirms that the alumina granules according to this embodiment can provide a colored alumina sintered body with a vivid color.
[0094] This application claims priority to Japanese patent application No. 2023-070415, filed on April 21, 2023, and Japanese patent application No. 2023-160734, filed on September 25, 2023, all of which are incorporated herein by reference.
Claims
1. An alumina granule composed of primary alumina particles bound together with a binder, in which the pore radius showing the maximum value of the logarithmic differential pore volume in the pores inside the granule is 0.055 μm or less.
2. Alumina granules according to claim 1, wherein the specific surface area diameter of the primary alumina particles is 90 nm or more and less than 200 nm.
3. Alumina granules according to claim 1 or 2, wherein the average circularity of the primary alumina particles is 0.74 or more.
4. Alumina granules according to claim 1 or 2, wherein the average aspect ratio of the primary alumina particles is 1.40 or less.
5. Alumina granules according to claim 1 or 2, containing 10 to 3,000 ppm of a sintering aid calculated as a metal element relative to 100 mass % of the alumina content in the alumina granules.
Citation Information
Patent Citations
FINE alpha-ALUMINA PARTICLE
JP2007055888A
Amorphous mesoporous alumina having an optimized pore distribution and a method for preparing the same
JP2017523109A
Aluminum sintered body production method and aluminum sintered body
WO2020196605A1
Cited By
Alumina pre-sintered body for crown color and method for producing same, method for producing alumina molded body for crown color, and method for producing alumina granular body for crown color
WO2026203984A1
Presintered alumina body for gingival color and method for producing same, method for producing molded alumina body for gingival color, and method for producing alumina particulate material for gingival color
WO2026203986A1