Resin component, holder member, and vehicular lighting fixture
By combining polypropylene with white pigment, light stabilizers, and heat resistance improvers in resin parts for vehicle lamps, the issue of ultraviolet-induced degradation is addressed, enhancing light and heat resistance while maintaining fluidity for complex shapes.
Patent Information
- Application Number
- PCT/JP2024/013698
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-24
AI Technical Summary
Resin parts used in vehicle lamps, particularly those made from polypropylene with white pigment, face degradation due to ultraviolet rays, leading to insufficient light resistance and potential cracking, when used instead of polycarbonate with black pigment.
Incorporating polypropylene with white pigment and a light stabilizer into the resin parts, along with a heat resistance improver and reinforcing materials like talc, to enhance reflectance and prevent ultraviolet-induced degradation, while maintaining high fluidity for complex shapes.
The solution effectively improves light resistance and heat resistance, preventing cracking and maintaining reflectance, even after prolonged exposure to ultraviolet rays, while ensuring the resin parts remain lightweight and thin.
Smart Images

Figure JP2024013698_24102024_PF_FP_ABST
Abstract
Description
Resin parts, holder members and vehicle lighting fixtures
[0001] The present invention relates to a resin part, a holder member, and a vehicle lamp.
[0002] It is known that a resin material containing polypropylene as a main component and an inorganic filler such as talc is used for a housing member of a vehicle lamp (see, for example, Patent Document 1).It is also known that a black pigment such as carbon black is added to a resin material such as polypropylene or polycarbonate that forms a lamp body in order to block light (see, for example, Patent Document 2).
[0003] Japanese Patent Publication No. 2022-135732 Japanese Patent Publication No. 2021-061107
[0004] In recent years, the interiors of vehicle lamps have become increasingly complex, resulting in a demand for complex-shaped and small-sized resin parts. For this reason, the use of polypropylene, which has higher fluidity than polycarbonate, to manufacture vehicle lamps has been considered. Furthermore, the use of light guides in vehicle lamps has become widespread to improve design, and the adoption of components with reflector functions that reflect light leaking from the light guide and increase the output efficiency of the lamp light has been considered. Such holder components are required to reflect visible light from LED light sources without transmitting or absorbing it. For this reason, the use of white pigments instead of black pigments in the resin components that make up the holder components has been considered. Meanwhile, resin materials used in vehicle lamps are required to be light-resistant enough to withstand external ultraviolet light that passes through the lens. However, using polypropylene instead of polycarbonate and white pigment instead of black pigments presents a problem: UV light scattered by the white pigment causes aging degradation of the polypropylene, resulting in insufficient light resistance.
[0005] SUMMARY OF THE INVENTION An object of the present invention is to improve the light resistance of resin parts of vehicle lamps.
[0006] A resin part for a vehicle lamp according to one aspect of the present disclosure includes polypropylene, a white pigment, and a light stabilizer.
[0007] A holder member according to one aspect of the present disclosure holds a long light guide, includes a recess configured to be able to reflect light emitted from the light guide, and is made from the resin composition described above.
[0008] A vehicle lamp according to one aspect of the present disclosure includes the holder member described above.
[0009] According to the present disclosure, the white pigment can reflect visible light from an LED light source, and the light stabilizer can repair radicals generated by the action of ultraviolet light on polypropylene, thereby improving the light resistance of the resin composition.
[0010] 1 is a diagram showing a vehicle lamp according to an embodiment of the present invention;
[0011] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. Note that, for the sake of convenience, the dimensions of each component shown in the drawings may differ from the actual dimensions of each component.
[0012] First, a vehicle lamp 1 according to an embodiment will be described with reference to Fig. 1. Fig. 1 is a partial cross-sectional view showing the vehicle lamp 1 equipped with a holder member 10. The vehicle lamp 1 includes a lamp body 22 and a transparent outer cover 24 that covers the front opening of the lamp body 22. The lamp body 22 and the outer cover 24 form a lamp chamber 26.
[0013] The vehicle lamp 1 includes a low beam unit 28 that irradiates a low beam, a holder member 10, and a light guide 20 in a lamp chamber 26. In the illustrated example, the light guide 20 functions as a DRL (Daytime Running Lamp).
[0014] The light guide 20 is a long, rod-shaped member that guides light from a light source (not shown) incident on its end face and emits a portion of the light via steps formed inside. The light guide 20 is not particularly limited, but is preferably made of a thermoplastic resin with a total light transmittance of 85% or more at a thickness of 3 mm. The light guide 20 is held in a recess provided in the holder member 10.
[0015] The holder member 10 is an elongated member extending in the left-right direction and including a support portion 12 and an opening 15. In the illustrated example, a lens of a low beam unit 28 faces forward from the opening 15.
[0016] The support portion 12 is provided at two locations, the top and bottom of the opening 15. The support portion 12 is a portion that extends in the left-right direction. As shown in FIG. 1 , the support portion 12 protrudes forward and has a recess at its tip that supports the light guide 20. The recess has a semicircular cross-sectional shape that corresponds to the circular cross-sectional shape of the light guide 20. The surface of the recess also functions as a reflective surface that reflects light emitted from the light guide 20 forward.
[0017] The vehicle lamp 1 according to the embodiment is not particularly limited as long as it includes, for example, a holder member 10 according to an embodiment described below. The vehicle lamp 1 according to the embodiment can be suitably used, for example, as a headlamp, fog lamp, position lamp, rear combination lamp, or turn signal lamp of an automobile, or as various lamps that notify pedestrians and drivers of other vehicles of the status of the vehicle (for example, that the vehicle is in autonomous driving mode).
[0018] The holder member 10 is a member made of a resin part with a reflectance of 70% or more for light with wavelengths of 400 to 700 nm. The holder member 10 holds a long light guide 20 and has a recess configured to be able to reflect light emitted from the light guide 20. Because the recess is made of a resin member with the above reflectance, it can reflect light emitted from the light guide 20 held in the recess.
[0019] The resin parts constituting the holder member 10 include polypropylene, a white pigment, and a light stabilizer. While the polypropylene may be a homopolymer, copolymer, block polymer, random polymer, or other polypropylene, a polypropylene composed of a homopolymer and a copolymer is preferred. The polypropylene preferably has a melt flow rate (MFR) of 10 g / 10 min to 60 g / 10 min when extruded at 230°C and 21 N. Resin parts containing polypropylene with such physical properties have a lower specific gravity and higher fluidity than polycarbonate, allowing for the molding of lightweight resin parts with complex shapes or large sizes.
[0020] While titanium oxide, aluminum oxide, zinc oxide, lithopone, white lead, etc. may be used as the white pigment, titanium oxide is preferred due to its excellent light-blocking properties, reflectivity, and cost-effectiveness. The preferred average primary particle diameter of the white pigment is 50 nm to 500 nm. Here, the pigment particle size is the diameter of a circle equal to the projected area of the particle (area-equivalent diameter). The volume-average diameter can be used as the average primary particle diameter. The amount of white pigment added is preferably 0.5 wt% to 10 wt% of the entire resin part, and more preferably 1 wt% to 5 wt%. By using the above formulation, the reflectance of light with wavelengths of 400 to 700 nm in the resin part can be 70% or more, preventing the transmission of visible light. Here, "reflectance" refers to the sum of specular reflectance and diffuse reflectance. The specular reflectance of light with wavelengths of 400 to 700 nm in the resin part is preferably 2% or more.
[0021] When ultraviolet light acts on polypropylene, polypropylene radicals are generated. Furthermore, when oxygen acts on the polypropylene radicals, hydroperoxides are generated, which sever the polypropylene molecular chains, depolymerize the polypropylene, and cause cracks in the resin part. On the other hand, if the resin part contains a light stabilizer, the light stabilizer reacts with the polypropylene radicals and restores the polypropylene to its original state. When a white pigment is used in the resin part, ultraviolet light is not absorbed within the resin part, but is scattered by the white pigment. This increases the impact of ultraviolet light on polypropylene degradation. The resin part of this embodiment contains a light stabilizer in addition to the white pigment, thereby reducing the impact of ultraviolet light scattered by the white pigment.
[0022] The light stabilizer preferably has a melting point of 120° C. or higher. The light stabilizer is not particularly limited, but examples thereof include Tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate (CAS registration number: 91788-83-9), Tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate (CAS registration number: 64022-61-3), Bis(2,2,6,6-tetramethyl-4-piperidyl)seb ceate (CAS registration number: 52829-07-9), Poly[[6-[(1,1,3,3-tetramethylbutyl) amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperid inyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl) imino]]) (CAS registration number: 71878-19-8), 2,2,6,6-tetramethylpiperidin-4-yl Examples of such stabilizers include 2,2,6,6-tetramethylpiperidine-4-yl octadecenoate (CAS Registry Number: 24860-22-8), 2,2,6,6-tetramethylpiperidine-4-yl octadecenoate, and the like. It is preferable to use at least one of the above light stabilizers in the resin part. The content of the light stabilizer is preferably 500 to 2000 ppm relative to the entire resin part. By using the stabilizer in the above range, deterioration of the resin part due to ultraviolet rays can be suppressed, light resistance can be improved, and cracks can be suppressed from occurring on the surface of the resin part while maintaining the reflectance of the resin part.
[0023] The resin parts constituting the holder member 10 preferably further contain a heat resistance improver. The heat resistance improver is not particularly limited, but an antioxidant can be used. Specifically, hindered phenol-based antioxidants such as pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) (IRGANOX® 1010 manufactured by BASF Japan Ltd.) and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (IRGANOX® 3114 manufactured by BASF Japan Ltd.) can be used. The content of the heat resistance improver is preferably 100 to 2000 ppm relative to the entire resin part. By setting the content within this range, excellent heat resistance can be ensured in the holder member 10 having reflector functions.
[0024] The resin parts constituting the holder member 10 preferably further include a reinforcing material. Examples of reinforcing materials that may be used include talc, glass fiber, calcium carbonate, mica, and wollastonite. Among these, talc is preferred because it offers improved heat resistance, improved dimensional accuracy, and cost performance. The preferred particle size of talc is a side length of 1 μm to 30 μm and a thickness of 10 nm to 500 nm. The amount of reinforcing material added is preferably 10 wt% to 40 wt%, and more preferably 20 wt% to 40 wt%, of the total weight of the resin part. The flexural modulus of the resin part is preferably 2 GPa to 5 GPa. Furthermore, the deflection temperature under load of the resin part at a bending stress of 0.45 MPa is preferably 120°C to 140°C. By using such resin parts, excellent strength and heat resistance can be ensured in the holder member 10 having reflector functionality.
[0025] The resin parts constituting the holder member 10 preferably further contain an ultraviolet absorber. By employing resin parts containing an ultraviolet absorber, excellent light resistance can be ensured in the holder member 10 having the function of a reflector. The melting point of the ultraviolet absorber is preferably 120°C or higher. By using an ultraviolet absorber with a melting point of 120°C or higher, the light resistance of the reflective material can be improved without causing fogging of the lamp lens.
[0026] The ultraviolet absorber is not particularly limited, but examples thereof include 2-(2H-Benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (CAS registration number: 70321-86-7), 2,2'-Methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol] (CAS registration number: 103597-45-1), ), 2-(5-chloro-2H-benzotriazol-2-yl)-6-tert-butyl-4-methylphenol (CAS registration number: 3896-11-5), 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine (CAS registration number: 222529-65-9), 3,5-Di-tert-butyl-4-hydroxybenzoic acid 2,4-di-tert-butylphenyl ester (CAS registration number: 4221-80-1), etc. It is preferable to use at least one of the above ultraviolet absorbers in resin parts.
[0027] The content of the ultraviolet absorber is preferably 100 to 3000 ppm relative to the total weight of the resin part, which can maintain the reflectance of the resin part while suppressing deterioration of the resin part due to ultraviolet rays, improving light resistance, and suppressing the occurrence of cracks on the surface of the resin part.
[0028] The resin parts constituting the holder member 10 have a specific gravity of 0.89 g / cm 3 1.30g / cm or more 3Preferably, the resin part has a melt flow rate (MFR) of 3 g / 10 min or more, and more preferably 10 g / 10 min or more and 60 g / 10 min or less, when extruded at 230°C and 21 N. Resin parts with such physical properties have a lower specific gravity and higher fluidity than conventional polycarbonate materials, so that even if the resin part has a complex shape or is large, the resin part can be molded with reduced weight.
[0029] The resin components that make up the holder member 10 preferably have a color with a yellowness index YI ranging from -10 to -0.4. Furthermore, upconversion nanoparticles that absorb light with wavelengths longer than 640 nm and emit light at around 475 nm may be used as additives to reduce the yellow tint. By using such upconversion nanoparticles, the yellow tint in the reflected light can be reduced, resulting in a bluish light emission.
[0030] The resin parts constituting the holder member 10 preferably have a flexural modulus of 2 GPa or more and 5 GPa or less. The resin parts constituting the holder member 10 preferably have a molding shrinkage rate of 1.0% or more and 1.5% or less. The resin parts constituting the holder member 10 preferably have a deflection temperature under load of 120°C or more and 140°C or less at a bending stress of 0.45 MPa.
[0031] The holder member 10, which holds a long light guide 20 and has a recess configured to reflect light emitted from the light guide 20, itself becomes large in size according to the length of the light guide 20. Therefore, if a resin material with low fluidity is used, the member will be thick and heavy. If a resin material with a high specific gravity is used, the weight will also increase. However, because the resin parts that make up the holder member 10 have a low specific gravity and exhibit high fluidity during molding, the holder member 10 with reflector function can be made thin and lightweight.
[0032] Furthermore, a holder member 10 having an edge that outlines an opening 15 configured to allow insertion of another component and a recess that functions as a reflector provided along at least a portion of the edge would have a more complex shape. Therefore, if a resin material with low fluidity were used, the member would be even thicker and heavier. By using the above-mentioned specific resin parts in such a complex-shaped holder member 10, a holder member 10 that functions as a reflector and is made of a material with a low specific gravity can be suitably configured.
[0033] Polypropylene was used as the base resin, and talc, a white pigment, a light stabilizer, and a heat resistance improver were mixed and molded to produce resin parts. The contents of polypropylene, talc, white pigment, light stabilizer, and heat resistance improver are shown in Tables 1 and 2. Test pieces of the obtained resin products were evaluated for fogging resistance, long-term heat resistance, and light resistance as follows.
[0034] <Fogging property> According to the provisions of ISO 6452:2021, a plate-shaped test piece was prepared, the test piece was placed in a glass container, and the glass container was then covered with a glass plate. The glass container containing the test piece was placed in an oil bath and held at 135 ° C. for 24 hours. Thereafter, the glass plate was removed from the glass container, and the haze value (degree of cloudiness; fogging) was measured according to JIS K7136:2000. The haze value of the glass plate before the test was measured in advance, and if the change in haze value (ΔHaze) was 5% or less, it was judged to be good. The evaluation results are shown in Tables 1 and 2.
[0035] <Long-term heat resistance> The test pieces were kept at 135°C for 1000 hours. Using a spectrophotometric color difference meter (Color Computer CC-i manufactured by Suga Test Instruments Co., Ltd.), the color difference ΔE expressed in the CIE L*a*b* color system was evaluated before and after the test in accordance with the spectrophotometric colorimetric method specified in JIS Z 8722:2009. A ΔE of 3.0 or less was judged to be good. The evaluation results are shown in Tables 1 and 2.
[0036] <Light resistance> Using an ultraviolet auto-fade meter (FAL-5H manufactured by Suga Test Instruments Co., Ltd.), ultraviolet light with a wavelength of 300 to 700 nm was applied at 500 W / m 2The test pieces were irradiated with light at an intensity of 1000 times for 1000 hours. Thereafter, the surfaces of the test pieces were observed with an optical microscope at a magnification of 200 times to check for the presence or absence of cracks. The evaluation results are shown in Table 1.
[0037]
[0038]
[0039] As shown in Tables 1 and 2, the fogging properties were good in all of Test Examples 1 to 11. As shown in Table 1, when the content of the light stabilizer was 500 ppm or more, no cracking occurred and light resistance was good. On the other hand, when the content of the light stabilizer was 2000 ppm or less, long-term heat resistance was good. As shown in Table 2, when the content of the heat resistance improver was 100 ppm or more, long-term heat resistance was good. On the other hand, the color difference ΔE decreased as the content of the heat resistance improver increased.
[0040] Although the embodiments of the present disclosure have been described above, it goes without saying that the technical scope of the present invention should not be construed as being limited by the description of the present embodiments. The present embodiments are merely examples, and it will be understood by those skilled in the art that various modifications of the embodiments are possible within the scope of the invention described in the claims. The technical scope of the present invention should be determined based on the scope of the invention described in the claims and its equivalents.
[0041] This disclosure is based on Japanese Patent Application No. 2023-069962, filed on April 21, 2023, the contents of which are incorporated herein by reference.
Claims
1. A resin part for a vehicle lamp, comprising: polypropylene; a white pigment; and a light stabilizer.
2. The light stabilizer is Tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, Tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, Bis(2,2,6,6,-tetramethyl-4-piperidyl)sebacate , Poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethylbutyl-4-piperidiny l)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]]), 2,2,6,6-tetramethylpiperidin-4-yl 2. The resin part for a vehicle lamp according to claim 1, wherein the resin is at least one selected from the group consisting of 2,2,6,6-tetramethylpiperidine-4-yl octadecenoate.
3. The resin part for a vehicle lamp according to claim 1, wherein the content of the light stabilizer is 500 to 2000 ppm.
4. The resin part of a vehicle lamp according to claim 1, further comprising a heat resistance improver.
5. The resin part for a vehicle lamp according to claim 4, wherein the heat resistance improver is a hindered phenol-based antioxidant.
6. The resin part for a vehicle lamp according to claim 4, wherein the content of the heat resistance improver is 100 to 2000 ppm.
7. The resin part for a vehicle lamp according to claim 1, wherein the white pigment is titanium oxide.
8. The resin part for a vehicle lamp according to claim 1, wherein the content of the white pigment is 1 to 5 mass %.
9. The resin part for a vehicle lamp according to claim 1, wherein the melt flow rate of the polypropylene is 10 to 60 g / 10 min.
10. The resin part for a vehicle lamp according to claim 1, further comprising 20 to 40 mass % of talc.
11. The resin part for a vehicle lamp according to claim 1, further comprising an ultraviolet absorbing agent.
12. The ultraviolet absorber is 2-(2H-Benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2,2'-Methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol]2-(5 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, 3,5-di-tert-butyl-4-hydroxybenzoic acid 2,4-di-tert-butylphenyl ester. The resin part of the vehicle lamp according to claim 11, which is at least one selected from the group consisting of: 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, 3,5-di-tert-butyl-4-hydroxybenzoic acid 2,4-di-tert-butylphenyl ester.
13. The resin part for a vehicle lamp according to claim 11, wherein the content of the ultraviolet absorbing agent is 100 to 3000 ppm.
14. A holder member for holding a long light guide and having a recess configured to be able to reflect light emitted from the light guide, the holder member being made of a resin part for a vehicle lamp as described in any one of claims 1 to 13.
15. A vehicle lamp comprising the holder member according to claim 14.
Citation Information
Patent Citations
Extension reflector of lighting fixture for vehicle
JP1999238401A
Thermoplastic resin composition and its molded product
JP2004137472A
Polypropylene resin composition for light-transmitting molded product and light-transmitting molded product
JP2007145909A
Light source module