Base paper for metallized paper, metallized paper, and packaging bag

The base paper for vapor-deposited paper, with a resin layer and pigment coating layer, addresses the challenges of printability and processing suitability in metallized papers by enhancing barrier properties and smoothness, ensuring effective packaging performance.

WO2024219296A1PCT designated stage expired Publication Date: 2024-10-24OJI HLDG CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014461
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-10
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional packaging materials with paper bases lack excellent printability and processing suitability for automatic packaging, particularly for metallized papers used in packaging foods and medical products, due to insufficient barrier properties and surface smoothness.

Method used

A base paper for vapor-deposited paper is developed with a resin layer on one side and a pigment coating layer on the other, featuring a clay coat layer, water-suspended polyurethane or polyester resin, and a heat-sealing layer, which enhances printability and processing suitability by improving oxygen and water vapor barrier properties and reducing dynamic friction.

Benefits of technology

The solution provides metallized paper with excellent printability and processing suitability for automatic packaging, maintaining effective barrier properties and smoothness, suitable for packaging materials like food and medical products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided are a base paper for a metallized paper, which has excellent printability and processing suitability in automatic packaging, and a metallized paper obtained using the base paper. The base paper for a metallized paper has a resin layer on one surface of a paper base material, and is for forming a vapor deposition layer on the resin layer. A pigment coating layer is provided to another surface of the paper base material, and the pigment content within the pigment coating layer is 50-85 mass%. The surface comprising the pigment coating layer has an Oken-type smoothness of 300 seconds or more and a dynamic friction coefficient of 0.35 or less with respect to stainless steel. The metallized paper comprises a vapor deposition layer on the resin layer of the base paper for a metallized paper, which has the resin layer on the one surface and the pigment coating layer on the other surface of the paper base material. The pigment content within the pigment coating layer is 50-85 mass%. The surface comprising the pigment coating layer has an Oken-type smoothness of 300 seconds or more and a dynamic friction coefficient of 0.35 or less with respect to stainless steel.
Need to check novelty before this filing date? Find Prior Art

Description

Metallized paper base paper, metallized paper, and packaging bags

[0001] The present invention relates to a base paper for metallized paper, metallized paper using the same, and a packaging bag using the metallized paper.

[0002] Conventionally, packaging materials that have been imparted with a paper base material water vapor barrier property that provides a barrier against water vapor, gas barrier property that provides a barrier against gases other than water vapor, and in particular oxygen barrier property that provides a barrier against oxygen, have been used in packaging foods, medical products, electronic components, and the like to prevent deterioration of the contents.

[0003] Metallized paper is a paper substrate on which a metallized layer made of metal or the like is provided to improve the barrier properties of the paper substrate against oxygen and water vapor.

[0004] Japanese Patent No. 6958756 discloses a base paper for metallized paper for forming a vapor-deposited layer by vapor deposition, which has a coating layer on at least one side of a paper substrate, the coating layer having, from the paper substrate side, a clay coating layer and a resin layer containing a water-dispersible polyurethane resin, in this order, wherein the Cobb water absorbency of the coating layer side is in a specific range and the contact angle with water of the coating layer surface is not more than a specific value.Japanese Patent No. 6958757 discloses a base paper for metallized paper for forming a vapor-deposited layer by vapor deposition, which has a clay coating layer and a resin layer, in this order, on at least one side of a paper substrate, the resin layer surface having a wetting tension not less than a specific value and a surface roughness not more than a specific value.

[0005] Metallized paper used as a packaging material for food and the like is required to have excellent printability on the printing surface, and particularly when used as a packaging bag, it is required to have excellent processability in automatic packaging.

[0006] Therefore, an object of the present invention is to provide a base paper for metallized paper that provides metallized paper with excellent printability and processability in automatic packaging, and to provide metallized paper made using the base paper. Another object of the present invention is to provide a packaging bag made using the metallized paper.

[0007] The present invention has the following configurations <1> to <11>. <1> A base paper for metal-deposited paper having a resin layer on one side of a paper substrate and for forming a metal-deposited layer on the resin layer, the base paper for metal-deposited paper having a pigment coating layer on the other side of the paper substrate, the pigment coating layer having a pigment content of 50% by mass or more and 85% by mass or less, and the side having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. <2> The base paper for metal-deposited paper according to <1>, which has a clay coating layer between the paper substrate and the resin layer. <3> The base paper for metal-deposited paper according to <1> or <2>, wherein the resin layer contains at least one resin selected from the group consisting of a water-dispersible polyurethane resin and a water-dispersible polyester resin. <4> The metal-deposited paper according to <1> or <2>, wherein the resin layer contains a water-soluble polyvinyl alcohol resin. <5> A metal-deposited paper having a resin layer on one side of a paper substrate and a pigment coating layer on the other side of the paper substrate, the metal-deposited paper having a metal-deposited layer on the resin layer, wherein the pigment coating layer has a pigment content of 50% by mass or more and 85% by mass or less, and the side having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. <6> The metal-deposited paper according to <5>, which has a heat-seal layer on the metal-deposited layer. <7> The metal-deposited paper according to <6>, which has an overcoat layer between the metal-deposited layer and the heat-seal layer. <8> The metal-deposited paper according to any one of <5> to <7>, which has a clay coat layer between the paper substrate and the resin layer. <9> The metal-deposited paper according to any one of <5> to <8>, wherein the resin layer contains at least one resin selected from the group consisting of a water-dispersible polyurethane resin and a water-dispersible polyester resin. <10> The metal-deposited paper according to any one of <5> to <8>, wherein the resin layer contains a water-soluble polyvinyl alcohol-based resin. <11> A packaging bag made using the metal-deposited paper according to any one of <5> to <10>.

[0008] [Metal-deposited Paper Base Paper] The metal-deposited paper base paper of this embodiment (hereinafter simply referred to as metal-deposited paper base paper) has a resin layer on one side of a paper substrate, and is a base paper for forming a metal-deposited layer on the resin layer. The metal-deposited paper base paper has a pigment coating layer on the other side of the paper substrate, and the pigment content in the pigment coating layer is 50% by mass or more and 85% by mass or less. The side with the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. The metal-deposited paper base paper of this embodiment provides metal-deposited paper with excellent printability and processability in automatic packaging. Although the reason for this is unclear, it is thought that the metal-deposited paper base paper of this embodiment provides metal-deposited paper with excellent printability and processability in automatic packaging by providing a pigment coating layer on the other side of the paper substrate, thereby increasing the smoothness of that side so that the Oken smoothness is a predetermined value or more and reducing the dynamic friction coefficient against stainless steel to a predetermined value or less. The effects of the present invention are not limited by the above mechanism.

[0009] The structure and properties of the base paper for metallized paper of this embodiment will be described in more detail below. In this specification, a numerical range represented by "X to Y" means a numerical range including X as the lower limit and Y as the upper limit. When a numerical range is described in stages, the upper and lower limits of each numerical range can be combined arbitrarily. Furthermore, "(meth)acrylic" is a generic term that includes both acrylic and methacrylic.

[0010] The base paper for metallized paper of this embodiment has a resin layer on one side of a paper substrate, on which a metallized layer can be formed, and has a pigment coating layer on the other side of the paper substrate. From the viewpoint of smoothing the surface of the paper substrate, the base paper for metallized paper of this embodiment preferably has a clay coating layer between one side of the paper substrate and the resin layer. That is, the base paper for metallized paper of this embodiment preferably has a clay coating layer on one side of the paper substrate, and a resin layer on the clay coating layer.

[0011] <Paper Base> The pulp constituting the paper base in this embodiment preferably contains plant-derived pulp as its main component, and more preferably contains wood pulp as its main component. Examples of wood pulp include hardwood pulp and softwood pulp. Examples of non-wood pulp include cotton pulp, hemp pulp, kenaf pulp, and bamboo pulp. Materials other than pulp fibers, such as synthetic fibers such as rayon fiber and nylon fiber, may also be blended as secondary paper materials as long as they do not impair the effects of the present invention.

[0012] From the viewpoints of the formation, physical properties and recyclability of the metallized paper, the proportion of hardwood pulp in the pulp constituting the paper base material is preferably 65% ​​by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be 100% by mass.

[0013] The paper base material may contain an internal sizing agent in addition to pulp, and examples of internal sizing agents include rosin-based, alkyl ketene dimer-based, alkenyl succinic anhydride-based, styrene-unsaturated carboxylic acid-based, higher fatty acid-based, petroleum resin-based, etc. The content of the internal sizing agent is not particularly limited, but is preferably 0 to 3 parts by mass per 100 parts by mass of pulp (bone dry mass) of the paper base material.

[0014] In addition to the internal sizing agent, other known internal additives may be added to the paper base material, such as fillers, paper strength agents, retention aids, pH adjusters, drainage aids, water-resistant agents, softeners, antistatic agents, antifoaming agents, slime control agents, dyes, and pigments.

[0015] Examples of fillers include titanium dioxide, kaolin, talc, calcium carbonate (heavy calcium carbonate, light calcium carbonate), calcium sulfite, gypsum, calcined kaolin, white carbon, amorphous silica, delaminated kaolin, diatomaceous earth, magnesium carbonate, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, and zinc hydroxide.

[0016] The paper base material is obtained by papermaking from a papermaking raw material mainly composed of pulp slurry. The pulp slurry can be obtained from wood or non-wood raw material chips through processes such as cooking, washing, and bleaching. There are no particular limitations on the methods used in the cooking, washing, and bleaching processes. The pulp slurry obtained through these processes is preferably further beaten in the presence of water.

[0017] In the papermaking of paper substrates, a known wet paper machine can be appropriately selected and used. Examples of paper machines include a Fourdrinier paper machine, a gap former paper machine, a cylinder paper machine, and a short wire paper machine. The paper layer formed by the paper machine is preferably transported on a felt and dried in a dryer. A multi-stage cylinder dryer may be used as a pre-dryer before drying in the dryer.

[0018] The paper substrate obtained as described above may be subjected to a surface treatment using a calendar to make the paper thickness and gloss profile uniform. For the calendar treatment, a known calendaring machine can be appropriately selected and used.

[0019] Specific examples of paper substrates used in the base paper for metallized paper of this embodiment include bleached kraft paper, unbleached kraft paper, fine paper, paperboard, liner paper, coated paper, one-side glazed paper, glassine paper, graphene paper, etc. Among these, bleached kraft paper, unbleached kraft paper, fine paper, and one-side glazed paper are preferred.

[0020] (Stockigt sizing degree) The Stockigt sizing degree of the paper substrate is not particularly limited, but from the viewpoint of improving barrier properties, the Stockigt sizing degree of at least the surface on which the resin layer described below is to be formed is preferably 1 second or more, more preferably 3 seconds or more, and even more preferably 5 seconds or more. The upper limit is not particularly limited, but from the viewpoint of ease of manufacturing the paper substrate, it is preferably 100 seconds or less, more preferably 30 seconds or less. That is, the Stockigt sizing degree of the paper substrate is preferably 1 to 100 seconds, more preferably 3 to 30 seconds, and even more preferably 5 to 30 seconds. The Stockigt sizing degree of the paper substrate is measured in accordance with JIS P 8122:2004. The Stockigt sizing degree of the paper substrate can be controlled by the type and content of internal sizing agent, the type of pulp, smoothing treatment, etc.

[0021] (Basis Weight) The basis weight of the paper substrate is not particularly limited, but from the viewpoint of strength when used as a packaging bag, it is preferably 20 g / m 2 More preferably, 30 g / m 2 More preferably, 40 g / m 2 From the viewpoint of economy and ease of production, it is preferably 500 g / m 2 or less, more preferably 400 g / m 2 More preferably 200 g / m or less 2 More preferably, 100 g / m or less 2 That is, the basis weight of the paper substrate is preferably 20 to 500 g / m 2 , more preferably 20 to 400 g / m 2 , more preferably 30 to 200 g / m 2 , and even more preferably 40 to 100 g / m 2 The basis weight of the paper substrate is measured in accordance with JIS P 8124:2011.

[0022] (Thickness) The thickness of the paper substrate is not particularly limited, but from the viewpoint of strength when used as a packaging bag, it is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 30 μm or more, and even more preferably 50 μm or more, and from the viewpoint of economy and ease of production, it is preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 75 μm or less. That is, the thickness of the paper substrate is preferably 5 to 150 μm, more preferably 10 to 100 μm, even more preferably 30 to 100 μm, and even more preferably 50 to 75 μm. The thickness of the paper substrate is measured in accordance with JIS P 8118:2014.

[0023] (Density) From the viewpoint of moldability, the density of the paper substrate is preferably 0.5 g / cm 3 More preferably, 0.6 g / cm 3 More preferably, 0.7 g / cm 3 and preferably 1.2 g / cm 3 or less, more preferably 1.0 g / cm 3 That is, the density of the paper substrate is preferably 0.5 to 1.2 g / cm 3 , more preferably 0.6 to 1.2 g / cm 3 , more preferably 0.7 to 1.0 g / cm 3 The density of the paper substrate is calculated from the basis weight and thickness of the paper substrate measured by the above-mentioned method.

[0024] (Oken Smoothness) From the viewpoint of obtaining a uniform vapor-deposited layer, the Oken smoothness of the paper substrate, at least on the surface on which the vapor-deposited layer is to be formed (i.e., the resin layer surface), is preferably 5 seconds or more, more preferably 10 seconds or more, and the upper limit is not particularly limited, but is preferably 1000 seconds or less, for example. That is, the Oken smoothness of the paper substrate is preferably 5 to 1000 seconds, more preferably 10 to 1000 seconds. The Oken smoothness of the paper substrate is measured in accordance with JIS P 8155:2010.

[0025] From the above viewpoints, the paper substrate has a Stockigt sizing degree of preferably 1 to 100 seconds, more preferably 3 to 100 seconds, and even more preferably 5 to 30 seconds on the side where the resin layer is to be provided (resin layer side), and a basis weight of preferably 20 to 500 g / m 2 , more preferably 20 to 400 g / m 2 , more preferably 30 to 200 g / m 2 , and even more preferably 40 to 100 g / m 2 The thickness is preferably 5 to 150 μm, more preferably 10 to 100 μm, even more preferably 30 to 100 μm, and still more preferably 50 to 75 μm, and the density is preferably 0.5 to 1.2 g / cm 3 , more preferably 0.6 to 1.2 g / cm 3 , more preferably 0.7 to 1.0 g / cm 3 The Oken smoothness of the resin layer surface is preferably 5 to 1000 seconds, more preferably 10 to 1000 seconds.

[0026] <Resin Layer> The base paper for metallized paper of this embodiment preferably has a resin layer on one side of the paper substrate, and has a resin layer on the clay coat layer described below. By providing a resin layer, adhesion between the metallized layer of the metallized paper and the paper substrate of the base paper for metallized paper is improved, improving barrier properties. In addition, the resin layer has oxygen barrier properties and water vapor barrier properties, and therefore also functions to improve the barrier properties when made into metallized paper.

[0027] The resin layer preferably contains one or more selected from the group consisting of water-suspendable polymers and water-soluble polymers, more preferably contains primarily water-suspendable polymers or water-soluble polymers, and even more preferably contains primarily water-suspendable polymers. The phrase "the resin layer primarily contains a water-suspendable polymer" means that the content of the water-suspendable polymer in the resin layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. The phrase "the resin layer primarily contains a water-soluble polymer" means that the content of the water-soluble polymer in the resin layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. In this specification, "water-suspendable" means that the polymer is suspended in water, but has a solubility of less than 1 g in 100 g of water at 25° C. Furthermore, "water-soluble" means that the solubility is 1 g or more in 100 g of water at 25° C. The resin layer may further contain any component in addition to the water-suspendable polymer or water-soluble polymer.

[0028] (Water-Suspendable Polymer) The water-suspendable polymer contained in the resin layer is not particularly limited, and examples thereof include alkyd resins; (meth)acrylic (co)polymers, styrene-(meth)acrylic resins; olefin-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers; polyvinyl alcohol resins such as ethylene-vinyl alcohol copolymers; cellulose resins; cellulose nanofibers; cellulose nanocrystals; polyurethane resins; and polyester resins. These may be used alone or in combination of two or more. Among these, the water-suspendable polymer is preferably one or more selected from the group consisting of water-suspendable polyvinyl alcohol resins, water-suspendable polyurethane resins, and water-suspendable polyester resins, and more preferably one or more selected from the group consisting of water-suspendable polyurethane resins and water-suspendable polyester resins.

[0029] <Water-Suspendable Polyurethane Resin> The water-suspendable polyurethane resin contained in the resin layer is not particularly limited, and is preferably, for example, a resin that can be prepared into one or more selected from the group consisting of polyurethane resin dispersions and emulsions, more preferably a resin that can be prepared into a polyurethane resin dispersion or emulsion, and even more preferably a resin that can be prepared into a polyurethane resin dispersion.

[0030] The water-dispersible polyurethane resin contained in the resin layer preferably contains at least one selected from the group consisting of structural units derived from meta-xylylene diisocyanate and structural units derived from hydrogenated meta-xylylene diisocyanate. When the polyurethane resin contains at least one of structural units derived from meta-xylylene diisocyanate and structural units derived from hydrogenated meta-xylylene diisocyanate, the total content of structural units derived from meta-xylylene diisocyanate and structural units derived from hydrogenated meta-xylylene diisocyanate relative to the total amount of structural units derived from polyisocyanate is preferably 50 mol% or more. Such polyurethane resins exhibit high cohesive strength due to hydrogen bonds and the stacking effect between xylylene groups, and therefore have excellent gas barrier properties. The above content is 1 The identification can be performed using known analytical techniques such as H-NMR.

[0031] -Oxygen permeability- The water-dispersible polyurethane resin contained in the resin layer preferably has an oxygen permeability of 100 mL / (m) at 23°C and 50% RH when converted into a sheet having a thickness of 25 μm. 2 ·day·atm) or less, more preferably 50 mL / (m 2 ·day·atm) or less, more preferably 25 mL / (m 2 ·day·atm) or less, and even more preferably 10 mL / (m 2 ·day·atm) or less, and even more preferably 5 mL / (m 2 ·day·atm) or less. A low oxygen permeability of the resin layer is preferable because it imparts better gas barrier properties to the base paper for metallized paper. In this specification, oxygen permeability is measured using an oxygen permeability measuring device (OX-TRAN2 / 22, manufactured by MOCON) under conditions of 23°C and 50% RH.

[0032] —Glass Transition Temperature— The glass transition temperature of the water-dispersible polyurethane resin contained in the resin layer is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 135° C. or lower, from the viewpoint of enhancing film-formability in order to protect the vapor-deposited layer of the vapor-deposited paper described below, and the lower limit is not particularly limited, but is preferably 50° C. or higher. The glass transition temperature of the water-dispersible polyurethane resin is measured in accordance with JIS K 7122:2012.

[0033] From the above viewpoint, the water-dispersible polyurethane resin contained in the resin layer preferably has an oxygen permeability of 100 mL / (m) at 23°C and 50% RH when converted into a 25 μm thick sheet. 2 ·day·atm) or less, more preferably 50 mL / (m 2 ·day·atm) or less, more preferably 25 mL / (m 2 ·day·atm) or less, and even more preferably 10 mL / (m 2 ·day·atm) or less, and even more preferably 5 mL / (m 2 ·day·atm) or less, and the glass transition temperature is preferably 50 to 150° C., more preferably 50 to 140° C., and even more preferably 50 to 135° C. As the water-dispersible polyurethane-based resin, a synthetic product may be used, and examples thereof include the polyurethane-based resins described in WO 2015 / 016069.

[0034] As the water-dispersible polyurethane resin, commercially available products may be used, such as "Takelac W series (trade name)," "Takelac WPB series (trade name)," and "Takelac WS series (trade name)" manufactured by Mitsui Chemicals, Inc., and a specific example is "Takelac WPB-341 (trade name)." Other commercially available products include "HPU W-003 (trade name)" (hydroxyl value 235 mg KOH / g) manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.

[0035] <Water-Suspendable Polyester-Based Resin> The water-suspendable polyester-based resin contained in the resin layer is not particularly limited, and is preferably, for example, a resin that can be prepared into one or more selected from the group consisting of polyester-based resin dispersions and emulsions, more preferably a resin that can be prepared into a polyester-based resin dispersion or emulsion, and even more preferably a resin that can be prepared into a polyester-based resin dispersion.

[0036] From the viewpoint of achieving superior adhesion to a vapor-deposited layer, which will be described later, the acid value of the water-dispersible polyester resin is preferably 1 mgKOH / g or more, more preferably 3 mgKOH / g or more, even more preferably 5 mgKOH / g or more, and still more preferably 6 mgKOH / g or more. The upper limit is not particularly limited, but is preferably 100 mgKOH / g or less, more preferably 50 mgKOH / g or less, even more preferably 20 mgKOH / g or less, and still more preferably 15 mgKOH / g or less. The acid value of the water-dispersible polyester resin is measured in accordance with JIS K 0700:1992.

[0037] -Hydroxyl Value- From the viewpoint of superior adhesion to a vapor-deposited layer described below, the hydroxyl value of the water-dispersible polyester resin is preferably 0.5 mgKOH / g or more, more preferably 1 mgKOH / g or more, even more preferably 1.5 mgKOH / g or more, and still more preferably 2 mgKOH / g or more. The upper limit is not particularly limited, but is preferably 100 mgKOH / g or less, more preferably 50 mgKOH / g or less, even more preferably 20 mgKOH / g or less, and still more preferably 10 mgKOH / g or less. The hydroxyl value of the water-dispersible polyester resin is measured in accordance with JIS K 0700:1992.

[0038] —Glass Transition Temperature— The glass transition temperature of the water-dispersible polyester resin contained in the resin layer is preferably 150° C. or lower, more preferably 140° C. or lower, and even more preferably 135° C. or lower, from the viewpoint of enhancing film-formability in order to protect the vapor-deposited layer of the vapor-deposited paper described below, and the lower limit is not particularly limited, but is preferably 50° C. or higher. The glass transition temperature of the water-dispersible polyester resin is measured in accordance with JIS K 7122:2012.

[0039] The water-dispersible polyester resin contained in the resin layer has an acid value of preferably 1 to 100 mgKOH / g, more preferably 3 to 50 mgKOH / g, even more preferably 5 to 20 mgKOH / g, and even more preferably 6 to 15 mgKOH / g, a hydroxyl value of preferably 0.5 to 100 mgKOH / g, more preferably 1 to 50 mgKOH / g, even more preferably 1.5 to 20 mgKOH / g, and even more preferably 2 to 10 mgKOH / g, and a glass transition temperature of preferably 50 to 150 ° C, more preferably 50 to 140 ° C, and even more preferably 50 to 135 ° C. As the water-dispersible polyester resin, commercially available products may be used, for example, "Elite KT Series (trade name)" manufactured by Unitika Ltd., and "Landy PL Series (trade name)" manufactured by Miyoshi Oil & Fats Co., Ltd., and the like. Specific examples include "Elite KT-8803 (trade name)" and "Landy PL-3000 (trade name)".

[0040] (Water-Soluble Polymer) The water-soluble polymer contained in the resin layer is not particularly limited, but examples thereof include polyvinyl alcohol, polyvinyl alcohol-based resins such as ethylene-modified polyvinyl alcohol, starch, starch derivatives, water-soluble polysaccharides such as carboxymethyl cellulose, methyl cellulose, and hydroxypropyl methyl cellulose, polyacrylic acid-based resins, polyamine resins, and polyamide resins. Among these, from the viewpoints of availability and economy, one or more selected from the group consisting of polyvinyl alcohol-based resins, water-soluble polysaccharides, and polyacrylic acid-based resins are preferred. From the viewpoint of oxygen barrier properties, polyvinyl alcohol-based resins are more preferred, and ethylene-modified polyvinyl alcohol is even more preferred. The saponification degree of the polyvinyl alcohol-based resin is preferably 95 mol% or more, more preferably 98 mol% or more, from the viewpoints of improving water resistance after film formation and stably exhibiting oxygen barrier properties. The saponification degree is measured in accordance with JIS K 6726-1994.

[0041] As the water-soluble polyvinyl alcohol-based resin, commercially available products may be used, for example, "EXCEVAL AQ-4104 (trade name)" and "EXCEVAL HR-3010 (trade name)" manufactured by Kuraray Co., Ltd., and "GOHSENOL NH-18 (trade name)" and "Nichigo G-Polymer OKS-8118 (trade name)" manufactured by Mitsubishi Chemical Corporation. As the water-soluble polysaccharide, commercially available products may be used, for example, "Cellogen F5-A (trade name)" manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., and "Metolose SM (trade name)" and "Metolose 60SH (trade name)" manufactured by Shin-Etsu Chemical Co., Ltd. As the water-soluble polyacrylic acid-based resin, commercially available products may be used, for example, "Aron A-30 (trade name)" and "Jurymer AC-10P (trade name)" manufactured by Toagosei Co., Ltd.

[0042] (Silane Coupling Agent) From the viewpoint of improving the flex resistance and processability of the resin layer, the resin layer may contain a silane coupling agent in addition to the water-dispersible polymer.

[0043] The silane coupling agent is a compound having at least one alkoxysilyl group and at least one reactive functional group other than the alkoxysilyl group in the molecule. The alkoxysilyl group may be any of a monoalkoxysilyl group, a dialkoxysilyl group, and a trialkoxysilyl group, but from the viewpoint of reactivity, a trialkoxysilyl group is preferred.

[0044] Examples of reactive functional groups other than alkoxysilyl groups include vinyl groups, epoxy groups, styryl groups, (meth)acryloyloxy groups, amino groups, isocyanato groups, ureido groups, and acid anhydride groups. Among these, amino groups, epoxy groups, and acid anhydride groups are preferred, and amino groups are more preferred.

[0045] Examples of epoxy group-containing silane coupling agents include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

[0046] Examples of amino group-containing silane coupling agents include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane, and among these, 3-aminopropyltriethoxysilane is preferred.

[0047] An example of an acid anhydride group-containing silane coupling agent is 3-trimethoxysilylpropylsuccinic anhydride.

[0048] As the silane coupling agent, commercially available products may be used, and examples thereof include KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103P, KBM-573, and X-12-967C manufactured by Shin-Etsu Chemical Co., Ltd.

[0049] The amount of the silane coupling agent is preferably 0.03 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, and particularly preferably 0.3 parts by mass or more, relative to 100 parts by mass of the water-suspendable polymer and the water-soluble polymer, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 6 parts by mass or less, and particularly preferably 5 parts by mass or less.

[0050] (Optional Components) Optional components that can be contained in the resin layer include other resins and additives, such as antifoaming agents, surfactants, pigments, antioxidants, antistatic agents, dyes, plasticizers, lubricants, and mold release agents.

[0051] The coating amount of the resin layer is not particularly limited, but is preferably 0.1 g / m in terms of solid content. 2 More preferably, 0.5 g / m 2 More preferably, 0.7 g / m 2 and preferably 10 g / m 2 Less than 5 g / m, more preferably 2 More preferably, 3 g / m or less 2 That is, the coating amount of the resin layer is preferably 0.1 to 10 g / m in terms of solid content. 2 , more preferably 0.5 to 5 g / m 2 , more preferably 0.7 to 3 g / m 2 The method for forming the resin layer is not particularly limited, but it is preferable to form the resin layer by applying an aqueous coating liquid containing a water-dispersible polymer and drying it.

[0052] <Clay Coat Layer> As described above, the base paper for metallized paper of this embodiment preferably has a clay coat layer between the paper substrate and the resin layer. This seals the paper substrate and smooths the surface on which the resin layer is to be formed, forming a flatter resin layer. As a result, when metallized paper (described later) is formed, a uniform metallized layer can be formed, improving barrier properties.

[0053] The clay coat layer preferably contains an inorganic pigment and a binder, and more preferably is mainly composed of an inorganic pigment and a binder. The phrase "the clay coat layer is mainly composed of an inorganic pigment and a binder" means that the total content of the inorganic pigment and the binder in the clay coat layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. The clay coat layer may further contain any optional components in addition to the inorganic pigment and the binder.

[0054] (Inorganic Pigment) The inorganic pigment contained in the clay coat layer is not particularly limited, but examples include kaolin, talc, mica, etc., and preferably kaolin. The content of the inorganic pigment in the clay coat layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% ​​by mass or more, and preferably 98% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less. In other words, the content of the inorganic pigment in the clay coat layer is preferably 50 to 98% by mass, more preferably 60 to 90% by mass, even more preferably 65 to 80% by mass.

[0055] <<Aspect Ratio>> From the viewpoint of forming a uniform and smooth resin layer, the aspect ratio of the inorganic pigment is preferably 50 or less, more preferably 45 or less, and the lower limit thereof is not particularly limited, but is preferably 1 or more, more preferably 5 or more. The aspect ratio of the inorganic pigment is measured by observation with an electron microscope or X-ray diffraction measurement.

[0056] <Average particle size> From the viewpoint of forming a uniform and smooth resin layer, the average particle size of the inorganic pigment is preferably 5 μm or less, more preferably 3 μm or less, even more preferably 1 μm or less, and even more preferably 0.50 μm or less, and the lower limit is not particularly limited, but is preferably 0.05 μm or more, more preferably 0.10 μm or more. The average particle size of the inorganic pigment means the median diameter (d50) measured by laser diffraction / scattering particle size distribution measurement.

[0057] From the above viewpoints, the inorganic pigment preferably has an aspect ratio of 1 to 50, more preferably 5 to 45, and an average particle size of preferably 0.05 to 5 μm, more preferably 0.05 to 3 μm, even more preferably 0.10 to 1 μm, and still more preferably 0.10 to 0.50 μm.

[0058] (Binder) The binder contained in the clay coating layer is not particularly limited, and examples thereof include styrene-butadiene resins; (meth)acrylic (co)polymers; styrene-(meth)acrylic resins; olefin-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers; and biodegradable resins such as polylactic acid. These may be used alone or in combination of two or more. Among these, preferred are one or more selected from the group consisting of styrene-butadiene resins, styrene-(meth)acrylic resins, olefin-unsaturated carboxylic acid copolymers, and polylactic acid; more preferred are one or more selected from the group consisting of styrene-(meth)acrylic resins, ethylene-(meth)acrylic acid copolymers, and polylactic acid; and even more preferred are one or more selected from the group consisting of styrene-acrylic resins, ethylene-acrylic resins, and polylactic acid.

[0059] The (meth)acrylic (co)polymer is a (co)polymer of one or more monomers selected from (meth)acrylic acid and (meth)acrylic acid esters. The (meth)acrylic acid ester is not particularly limited, but is preferably an alkyl ester of (meth)acrylic acid having 1 to 12 carbon atoms.

[0060] The styrene-(meth)acrylic resin is a copolymer of styrene and one or more monomers selected from (meth)acrylic acid and (meth)acrylic acid esters, and is preferably a styrene-acrylic resin or a styrene-methacrylic resin, and more preferably a styrene-acrylic acid copolymer or a styrene-acrylic acid ester copolymer.

[0061] The binder content in the clay coat layer is preferably 2% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 35% by mass or less. That is, the binder content in the clay coat layer is preferably 2 to 50% by mass, more preferably 10 to 40% by mass, even more preferably 20 to 35% by mass.

[0062] From the above viewpoints, the content of the inorganic pigment in the clay coating layer is preferably 50 to 98% by mass, more preferably 60 to 90% by mass, and even more preferably 65 to 80% by mass, and the content of the binder is preferably 2 to 50% by mass, more preferably 10 to 40% by mass, and even more preferably 20 to 35% by mass.

[0063] (Optional Components) Optional components that can be contained in the clay coating layer include adhesives, dispersants, thickeners, water retention agents, antifoaming agents, water-resistant agents, colorants, surfactants, etc. Examples of adhesives include proteins such as casein, soy protein, and synthetic protein; starches such as oxidized starch, cationic starch, urea phosphate esterified starch, etherified starch such as hydroxyethyl etherified starch, and dextrin; and cellulose derivatives such as carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxymethyl cellulose.

[0064] The coating amount of the clay coating layer is not particularly limited, but is preferably 5 g / m2 in terms of solid content. 2 More preferably, 8 g / m 2 More preferably, 10 g / m 2 and preferably 30 g / m 2 or less, more preferably 20 g / m 2 More preferably 15 g / m or less 2 That is, the coating amount of the clay coating layer is preferably 5 to 30 g / m2 in terms of solid content. 2 , more preferably 8 to 20 g / m 2 , more preferably 10 to 15 g / m 2 is.

[0065] The method for forming the clay coating layer is not particularly limited, but a method of forming the clay coating layer by coating a dispersion containing an inorganic pigment and a binder on a paper substrate and drying it is preferred. The dispersion containing an inorganic pigment and a binder is preferably one that uses an aqueous medium containing water as the main component as the solvent.

[0066] <Pigment Coating Layer> The base paper for metallized paper of this embodiment has a pigment coating layer on the other side of the paper substrate, i.e., the side opposite the side bearing the resin layer. By providing a pigment coating layer and then calendering the coated surface under specified conditions, the smoothness of the coated surface can be improved and the coefficient of dynamic friction against stainless steel can be reduced, resulting in metallized paper with excellent printability and processability. The pigment coating layer is preferably composed primarily of a pigment and a binder. Note that "the pigment coating layer is composed primarily of a pigment and a binder" means that the total content of the pigment and binder in the pigment coating layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. Note that the pigment coating layer may contain any optional components in addition to the pigment and binder.

[0067] (Pigment) The pigment contained in the pigment coating layer is not particularly limited, and examples thereof include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, calcined clay, heavy calcium carbonate, light calcium carbonate, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicates, colloidal silica, and satin white; and organic pigments such as solid, hollow, and core-shell pigments. These pigments may be used alone or in combination of two or more. Among these, at least one pigment selected from the group consisting of kaolin and calcium carbonate is preferred, and a combination of kaolin and calcium carbonate is more preferred, and a combination of kaolin, heavy calcium carbonate, and light calcium carbonate is even more preferred. From the viewpoint of further improving printability, the mass ratio of kaolin to calcium carbonate in the pigment (kaolin / calcium carbonate) is preferably 10 / 90 to 50 / 50, more preferably 20 / 80 to 40 / 60.

[0068] The pigment content in the pigment coating layer is 50% by mass or more, preferably 60% by mass or more, and 85% by mass or less, preferably 83% by mass or less, from the viewpoint of preventing ink peeling and achieving excellent printability when metal-deposited paper is formed and printed on the metal-deposited paper. That is, the pigment content in the pigment coating layer is 50 to 85% by mass, preferably 60 to 83% by mass.

[0069] (Binder) The binder contained in the pigment coating layer is not particularly limited, and examples thereof include styrene-butadiene resins; acrylic resins such as methyl (meth)acrylate copolymers and styrene-(meth)acrylic copolymers; olefin-unsaturated carboxylic acid copolymers such as ethylene-(meth)acrylic acid copolymers; dextrin, mannan, chitosan, arabinogalactan, glycogen, inulin, pectin, hyaluronic acid, hydroxyethylated starch, oxidized starch, etherified starch, phosphated starch, enzyme-modified starch, and modified starches obtained by flash drying these natural polysaccharides, as well as oligomers and modified products thereof. Among these, it is preferably one or more selected from the group consisting of acrylic resins, styrene-butadiene resins, and modified starches, more preferably one or more selected from the group consisting of styrene-(meth)acrylic copolymers, styrene-butadiene resins, and oxidized starches, even more preferably one or more selected from the group consisting of styrene-butadiene resins and oxidized starches, and even more preferably a combination of styrene-butadiene resins and oxidized starches.

[0070] The content of the binder in the pigment coating layer is preferably 1% by weight or more, more preferably 2% by weight or more, even more preferably 5% by weight or more, still more preferably 10% by weight or more, even more preferably 15% by weight or more, and preferably 50% by weight or less, more preferably 45% by weight or less. When oxidized starch is used as the binder, the content of the oxidized starch in the pigment coating layer is preferably 1% by weight or more, more preferably 2% by weight or more, and preferably 12% by weight or less, more preferably 8% by weight or less. That is, the content of the binder in the pigment coating layer is preferably 1 to 50% by weight, more preferably 2 to 50% by weight, even more preferably 5 to 50% by weight, still more preferably 10 to 45% by weight, even more preferably 15 to 45% by weight. When oxidized starch is used as the binder, the content is preferably 1 to 12% by weight, more preferably 2 to 8% by weight.

[0071] (Optional Components) Optional components that may be contained in the pigment coating layer include adhesives, dispersants, thickeners, water retention agents, antifoaming agents, waterproofing agents, colorants, surfactants, and lubricants. Examples of adhesives include proteins such as casein, soy protein, and synthetic proteins; starches such as oxidized starch, cationic starch, urea phosphate esterified starch, and etherified starch such as hydroxyethyl etherified starch, and dextrin; and cellulose derivatives such as carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxymethyl cellulose. Examples of lubricants include hydrocarbon-based lubricants such as paraffin wax and synthetic polyethylene; fatty acid lubricants such as stearic acid and stearyl alcohol; higher alcohol-based lubricants; fatty acid amide-based lubricants such as stearic acid amide and oleic acid amide; metal-based lubricants such as calcium stearate and zinc stearate; ester-based lubricants such as glycerin monostearate and glycerin monooleate; and mixtures thereof. The content of the lubricant in the pigment coating layer is preferably 0.1 to 10% by mass. By including a lubricant in the pigment coating layer, it is possible to prevent sticking to the calendar and blocking during winding.

[0072] The coating amount of the pigment coating layer is not particularly limited, but is preferably 3 g / m2 in terms of solid content. 2 More preferably, 5 g / m 2 More preferably, 7 g / m 2 and preferably 30 g / m 2 or less, more preferably 20 g / m 2 More preferably 15 g / m or less 2 That is, the coating amount of the pigment coating layer is preferably 3 to 30 g / m2 in terms of solid content. 2 , more preferably 5 to 20 g / m 2 , more preferably 7 to 15 g / m 2 is.

[0073] The method for forming the pigment coating layer is not particularly limited, but a method of forming the layer by coating a dispersion containing a pigment and a binder on a paper substrate and drying it is preferred. The dispersion containing a pigment and a binder is preferably one that uses an aqueous medium containing water as the main component as the solvent.

[0074] From the above viewpoint, the coating amount of the resin layer is preferably 0.1 to 10 g / m in terms of solid content. 2 , more preferably 0.5 to 5 g / m 2 , more preferably 0.7 to 3 g / m 2 The coating amount of the clay coating layer is preferably 5 to 30 g / m in terms of solid content. 2 , more preferably 8 to 20 g / m 2 , more preferably 10 to 15 g / m 2 The coating amount of the pigment coating layer is preferably 3 to 30 g / m2 in terms of solid content. 2 , more preferably 5 to 20 g / m 2 , more preferably 7 to 15 g / m 2 is.

[0075] <Physical Properties of Metal-Deposited Paper Base Paper> (Oken Smoothness) From the viewpoint of obtaining metal-deposited paper with excellent printability, the Oken smoothness of the pigment-coated surface of the metal-deposited paper base paper is 300 seconds or more, preferably 350 seconds or more, more preferably 450 seconds or more, even more preferably 650 seconds or more, and even more preferably 850 seconds or more. The upper limit is not particularly limited, but is preferably 5000 seconds or less, more preferably 3000 seconds or less. That is, the Oken smoothness of the pigment-coated surface of the metal-deposited paper base paper is preferably 350 to 5000 seconds, more preferably 450 to 5000 seconds, even more preferably 650 to 3000 seconds, and even more preferably 850 to 3000 seconds. The Oken smoothness of the pigment-coated surface of the metal-deposited paper base paper does not change even after undergoing a process such as providing a metal-deposited layer to obtain metal-deposited paper, and therefore, if it is in the above range, metal-deposited paper with excellent printability can be obtained. The Oken smoothness of the surface having the pigment coating layer is measured in accordance with JIS P 8155:2010. The Oken smoothness of the surface having the pigment coating layer can be adjusted to the above range by adjusting the Oken smoothness of the paper base material used, or by performing a calendering treatment under the following conditions after forming the pigment coating layer. As for the calendering conditions, the linear pressure is preferably 10 kg / cm or more, more preferably 30 kg / cm or more, and even more preferably 50 kg / cm or more, and is preferably 1000 kg / cm or less, more preferably 500 kg / cm or less, and even more preferably 200 kg / cm or less. That is, the linear pressure is preferably 10 to 1000 kg / cm, more preferably 30 to 500 kg / cm, and even more preferably 50 to 200 kg / cm. When heating is performed in the calendering treatment, the heating temperature is not particularly limited, but from the viewpoint of enhancing the treatment effect while preventing thermal deterioration of the paper base material or the pigment coating layer and sticking of the pigment coating layer, the heating temperature is preferably 20° C. or higher, more preferably 30° C. or higher, even more preferably 35° C. or higher, and preferably 80° C. or lower, more preferably 70° C. or lower, even more preferably 60° C. or lower. That is, the heating temperature is preferably 20 to 80° C., more preferably 30 to 70° C., even more preferably 35 to 60° C.The calendering may be carried out in one stage or multiple stages, but from the viewpoint of further improving printability and / or automatic packaging suitability, it is preferably carried out in multiple stages (two or more stages), more preferably five or more stages, even more preferably ten or more stages, and although there is no particular upper limit, it is preferably 15 or less stages. That is, the number of stages is preferably 2 to 15 stages, more preferably 5 to 15 stages, even more preferably 10 to 15 stages.

[0076] (Dynamic Friction Coefficient Against Stainless Steel) From the viewpoint of obtaining metal-deposited paper with excellent processability, the dynamic friction coefficient of the pigment-coated surface of the base paper for metal-deposited paper against stainless steel is 0.35 or less, preferably 0.32 or less. From the viewpoint of further improving processability (ease of transport in an automatic packaging machine), it is more preferably 0.22 or less, even more preferably 0.20 or less. The lower limit is not particularly limited, but is preferably 0.10 or more. That is, the dynamic friction coefficient of the pigment-coated surface of the base paper for metal-deposited paper against stainless steel is preferably 0.10 to 0.32, more preferably 0.10 to 0.22, even more preferably 0.10 to 0.20. Note that the dynamic friction coefficient of the pigment-coated surface of the base paper for metal-deposited paper against stainless steel does not change even after undergoing a process such as providing a metal-deposited layer, and therefore excellent processability is achieved when it is within the above range. The dynamic friction coefficient of the pigment-coated surface against stainless steel is measured in accordance with JIS P 8147:2010, specifically as described in the examples. The dynamic friction coefficient of the surface having the pigment coating layer against stainless steel can be adjusted to the above range by adjusting the Oken smoothness of the paper base material used, or by performing a calendar treatment under the above conditions after forming the pigment coating layer.

[0077] (Thickness) The thickness of the base paper for metallized paper is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 50 μm or more, and preferably 100 μm or less, more preferably 80 μm or less. That is, the thickness of the base paper for metallized paper is preferably 10 to 100 μm, more preferably 30 to 100 μm, even more preferably 50 to 80 μm. The thickness of the base paper for metallized paper is measured in accordance with JIS P 8118:2014.

[0078] There are no particular limitations on the method for producing the base paper for metallized paper of this embodiment, but it is preferable to, for example, coat and dry a clay coating layer coating liquid containing an inorganic pigment and a binder as needed on one side of the paper substrate, then coat and dry a resin layer coating liquid containing a water-dispersible polymer, and coat and dry a pigment coating layer coating liquid containing a pigment and a binder on the other side of the paper substrate to form the base paper, and then perform a calendering treatment under the above conditions. Note that, as long as the base paper for metallized paper of this embodiment can be obtained, after forming a pigment coating layer on one side of the paper substrate, a clay coating layer and a resin layer may be formed on the other side of the paper substrate as needed. Each layer can be formed by coating as described above.

[0079] [Metal-deposited Paper] The metal-deposited paper of this embodiment is a metal-deposited paper having a resin layer on one side of a paper substrate and a pigment coating layer on the other side of the paper substrate. The pigment content in the pigment coating layer is 50% by mass or more and 85% by mass or less. The side having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less. The metal-deposited paper of this embodiment has excellent printability and processability in automatic packaging. Although the reason for this is unclear, it is believed that the metal-deposited paper of this embodiment has excellent printability and processability in automatic packaging by providing a pigment coating layer on the other side of the paper substrate, thereby increasing the smoothness of that side so that the Oken smoothness is a predetermined value or more and reducing the dynamic friction coefficient against stainless steel to a predetermined value or less. Note that the effects of the present invention are not limited by the above mechanism. The Oken smoothness and dynamic friction coefficient against stainless steel of the pigment-coated surface of metal-deposited paper do not change even if a metal-deposited layer is provided on the resin layer of the base paper for metal-deposited paper. The preferred ranges for the Oken smoothness and dynamic friction coefficient against stainless steel of the pigment-coated surface of metal-deposited paper are the same as those for the pigment-coated surface of the base paper for metal-deposited paper described above.

[0080] The paper substrate used in the metallized paper of this embodiment can be any of the paper substrates exemplified for the base paper for metallized paper described above. The resin layer provided on one side of the paper substrate can also be any of the resin layers exemplified for the base paper for metallized paper described above. The pigment coating layer provided on the other side of the paper substrate can also be any of the pigment coating layers exemplified for the base paper for metallized paper described above.

[0081] <Vapor-deposited layer> The vapor-deposited paper of this embodiment has a vapor-deposited layer on the resin layer of the base paper for vapor-deposited paper. The vapor-deposited layer is at least one of a layer made of metal and a layer made of ceramic. That is, the vapor-deposited layer may be a layer made of metal, a layer made of ceramic, or a laminate of a metal layer and a ceramic layer. When the vapor-deposited layer is a laminate of a metal layer and a ceramic layer, the metal layer may be on the resin layer side of the base paper for vapor-deposited paper, or the ceramic layer may be on the resin layer side of the base paper for vapor-deposited paper, and there are no particular restrictions.

[0082] The vapor-deposited layer may be a layer made of a metal, a layer made of a ceramic, or a laminate thereof, but is preferably a layer made of a metal. When the vapor-deposited layer is a layer made of a metal, specific examples of the metal include aluminum and titanium. When the vapor-deposited layer is a layer made of a ceramic, specific examples of the ceramic include silicon oxide, titanium oxide, aluminum oxide, and diamond-like carbon. These may be used alone or in combination of two or more.

[0083] Among these, the vapor deposition layer is preferably a layer made of one or more materials selected from the group consisting of aluminum, aluminum oxide, silicon oxide, and diamond-like carbon, and from the viewpoint of ease of production, it is more preferably a layer made of one or more materials selected from the group consisting of aluminum, aluminum oxide, and diamond-like carbon, and even more preferably a layer made of one or more materials selected from the group consisting of aluminum and aluminum oxide.

[0084] (Thickness) The thickness of the vapor-deposited layer is preferably 1 nm or more, more preferably 2 nm or more, even more preferably 3 nm or more, and preferably 1000 nm or less, more preferably 500 nm or less, and even more preferably 100 nm or less. From the viewpoint of barrier properties, the thickness of the vapor-deposited layer is preferably 10 nm or more, more preferably 15 nm or more, and preferably 80 nm or less, more preferably 70 nm. From the viewpoints of adhesion to other layers and cost, the thickness of the vapor-deposited layer is preferably 4 nm or more, more preferably 5 nm or more, and preferably 100 nm or less, more preferably 70 nm or less, and even more preferably 60 nm or less. That is, the thickness of the vapor-deposited layer is preferably 1 to 1000 nm, more preferably 2 to 500 nm, even more preferably 3 to 100 nm, even more preferably 4 to 80 nm, even more preferably 5 to 70 nm, and even more preferably 10 to 60 nm.

[0085] <Heat Seal Layer> The metallized paper of this embodiment preferably has a heat seal layer on the metallized layer. The heat seal layer is a layer that melts and adheres by heating, ultrasonic waves, or the like. Methods for forming the heat seal layer include coating a thermoplastic resin solution or thermoplastic resin dispersion and drying, and extrusion lamination. Among these, coating a thermoplastic resin solution or thermoplastic resin dispersion and drying is preferred. The thermoplastic resin solution or thermoplastic resin dispersion used here may be a solution using an organic solvent that dissolves the thermoplastic resin, a dispersion using an organic solvent that disperses the thermoplastic resin, or a dispersion using an aqueous medium. From the standpoints of coatability and environmental impact, a dispersion using an aqueous medium is preferred.

[0086] (Thermoplastic Resin) Thermoplastic resins suitable for dispersions using aqueous media may be either natural resins or synthetic resins, and examples thereof include starch derivatives, casein, shellac, polyvinyl alcohol and its derivatives, acrylic resins, ionomer resins, maleic acid resins, urethane resins, polyester resins, styrene-butadiene resins, vinyl chloride resins, polyolefin resins, and the like. More specifically, examples of the acrylic resin include acrylic resins copolymerized with (meth)acrylic acid and its alkyl ester or styrene as monomer components, styrene-maleic acid resins, styrene-acrylic acid-maleic acid resins, water-soluble polyurethane resins, and water-soluble polyester resins. Preferred examples of the ionomer resin include ethylene-acrylic acid copolymer ionomers and ethylene-methacrylic acid ionomers. Here, the ionomer is a polymer neutralized with a cation, and examples of the cation include metal ions and ammonium ions (NH 4 + ), and organic ammonium ions. Examples of metal ions include lithium ions (Li + ), sodium ions (Na + ), potassium ions (K + ), alkali metal ions such as magnesium ions (Mg 2+ ), calcium ions (Ca 2+ ), alkaline earth metal ions such as zinc ions (Zn 2+ ), copper ions (Cu 2+) and other transition metal ions. Among these, sodium ions are preferred as the metal ion from the viewpoint of availability and the like. Among these, from the viewpoint of the stability of the coating solution and the solvent resistance of the coating layer, the thermoplastic resin is preferably one or more selected from the group consisting of starch derivatives, casein, shellac, polyvinyl alcohol and its derivatives, ionomer-based resins, acrylic resins, polyolefin-based resins, and maleic acid-based resins, more preferably one or more selected from the group consisting of starch derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer-based resins, acrylic resins, polyolefin-based resins, and maleic acid-based resins, still more preferably at least one selected from the group consisting of starch derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer-based resins, acrylic resins, and polyolefin-based resins, even more preferably one or more selected from the group consisting of polyvinyl alcohol, polyvinyl alcohol derivatives, ionomer-based resins, and polyolefin-based resins, and even more preferably one or more selected from the group consisting of ionomer-based resins and polyolefin-based resins.

[0087] Examples of methods for applying the thermoplastic resin solution or thermoplastic resin dispersion include bar coating, blade coating, squeeze coating, air knife coating, roll coating, gravure coating, and transfer coating, and a coating machine such as a fountain coater or a slit die coater may be used.

[0088] The coating amount of the heat seal layer is not particularly limited, but from the viewpoint of ensuring sufficient heat sealability, it is preferably 0.5 g / m 2 More preferably, 1 g / m 2 More preferably, 1.5 g / m 2 From the viewpoint of recyclability of the metallized paper, it is preferably 15 g / m 2 or less, more preferably 10 g / m 2 More preferably, 7 g / m or less 2 More preferably, 5 g / m or less 2That is, the coating amount of the heat seal layer is preferably 0.5 to 15 g / m 2 , more preferably 1 to 10 g / m 2 , and more preferably 1.5 to 7 g / m 2 , and even more preferably 1.5 to 5 g / m 2 is.

[0089] <Overcoat Layer> The metallized paper of this embodiment may have an overcoat layer between the metallized layer and the heat seal layer. The overcoat layer is a layer for protecting the metallized layer. The metallized paper of this embodiment has a certain level of barrier property due to the metallized layer, but by having an overcoat layer on the metallized layer, the oxygen barrier property can be further improved. In addition, the metallized layer is less likely to be damaged by processing such as bending, and even if it is damaged, the overcoat layer can ensure the oxygen barrier property, allowing the excellent oxygen barrier property to be maintained.

[0090] The overcoat layer is not particularly limited and may contain an organic compound, an inorganic compound, or both. That is, the overcoat layer may be an organic layer, an inorganic layer, or an organic-inorganic hybrid layer. Examples of organic compounds include vinyl alcohol-based resins such as polyvinyl alcohol, polyurethane-based resins, (meth)acryloyl compounds, and reaction products of (meth)acryloyl compounds. Examples of inorganic compounds include oxides of silicon, aluminum, and the like.

[0091] Among these, the overcoat layer is preferably one of the resins exemplified as being contained in the resin layer of the base paper for metallized paper, more preferably contains at least one resin selected from the group consisting of water-dispersible polyurethane resins and water-dispersible polyester resins, even more preferably is capable of being prepared into one or more resins selected from the group consisting of polyurethane resin dispersions and emulsions, even more preferably is capable of being prepared into a polyurethane resin dispersion or emulsion, and even more preferably is capable of being prepared into a polyurethane resin dispersion.

[0092] The water-dispersible polyurethane resin or water-dispersible polyester resin that can be contained in the overcoat layer may be the same type as or a different type from the resin contained in the resin layer of the base paper for metallized paper described above, but it is preferable that they are the same type. Furthermore, the synthetic products or commercially available products listed as usable for the resin layer of the base paper for metallized paper may also be used.

[0093] The content of the water-dispersible polyurethane resin or water-dispersible polyester resin in the overcoat layer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 99% by mass or more, and the upper limit is not particularly limited, but is 100% by mass.

[0094] The overcoat layer may contain other resins or additives as long as the effects of the present invention are not impaired. Examples of additives include surfactants, pigments, antioxidants, antistatic agents, dyes, plasticizers, lubricants, and release agents. When the polyurethane resin is used as an aqueous dispersion, it is preferable to use a dispersant to disperse the polyurethane resin in an aqueous medium and obtain a uniform overcoat layer film.

[0095] The coating amount of the overcoat layer is preferably 0.1 g / m in terms of solid content from the viewpoint of protecting the vapor deposition layer. 2 More preferably, 0.2 g / m 2 More preferably, 0.3 g / m 2 From the viewpoint of recyclability of the metallized paper, it is preferably 10 g / m 2 More preferably, 7 g / m or less 2 More preferably, 5 g / m or less 2 That is, the coating amount of the overcoat layer is preferably 0.1 to 10 g / m 2 , more preferably 0.2 to 7 g / m 2 , more preferably 0.3 to 5 g / m 2 is.

[0096] The thickness of the overcoat layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more from the viewpoint of protecting the vapor-deposited layer, and is preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 4 μm or less from the viewpoint of recyclability of the vapor-deposited paper. That is, the thickness of the overcoat layer is preferably 0.1 to 10 μm, more preferably 0.2 to 7 μm, and even more preferably 0.3 to 4 μm.

[0097] The method for forming the overcoat layer is not particularly limited, but it is preferable to form the overcoat layer by applying an aqueous medium of an organic compound or inorganic compound that constitutes the overcoat layer and drying it.

[0098] In the metallized paper of this embodiment, the overcoat layer may be the outermost layer, but even if the overcoat layer is the outermost layer, it does not impair the design of the glossy metallized layer.

[0099] [Method for manufacturing metal-deposited paper] There are no limitations on the method for manufacturing the metal-deposited paper of this embodiment, but it is preferable to include the steps of forming a metal-deposited layer by vapor-depositing at least one of metal and ceramic on the resin layer-covered side of a base paper for metal-deposited paper, which has a clay coating layer and a resin layer, in that order, as needed, on one side of the paper substrate, and applying a coating liquid for a heat-sealing layer onto the metal-deposited layer and drying it to form a heat-sealing layer. In this case, an overcoat layer may be formed on the metal-deposited layer by coating before forming the heat-sealing layer.

[0100] The preferred method for depositing metal or ceramic is to vacuum-deposit the metal or ceramic directly onto the surface of the resin layer of the base paper for metallized paper.

[0101] From the viewpoint of efficiently protecting the vapor-deposited layer and enhancing the barrier property, the overcoat layer is preferably formed directly on the vapor-deposited layer. The overcoat layer is preferably formed by applying a coating liquid for the overcoat layer and drying it. By using the method of forming the overcoat layer by applying a coating liquid for the overcoat layer, it is possible to form an overcoat layer with a relatively thin film thickness of 10 μm or less.

[0102] The coating liquid for the overcoat layer used here may be an aqueous medium for an organic compound or an inorganic compound that constitutes the overcoat layer. Among these, a solution using an organic solvent that dissolves a polyurethane resin, a dispersion using an organic solvent that disperses a polyurethane resin, or a dispersion using an aqueous medium is preferred, and from the viewpoints of coatability and environmental load, a dispersion using an aqueous medium is more preferred.

[0103] Examples of methods for applying the coating liquid for the overcoat layer include bar coating, blade coating, squeeze coating, air knife coating, roll coating, gravure coating, and transfer coating, and a coating machine such as a fountain coater or a slit die coater may be used. The coated metal-deposited paper coated with the coating liquid for the overcoat layer is dried to remove the organic solvent or aqueous medium, thereby obtaining a metal-deposited paper having an overcoat layer on the metal-deposited layer.

[0104] A heat seal layer containing a thermoplastic resin can be formed on the vapor deposition layer or the overcoat layer. Methods for forming the heat seal layer include coating a thermoplastic resin solution or a thermoplastic resin dispersion and drying it, and extrusion lamination. Among these, coating a thermoplastic resin solution or a thermoplastic resin dispersion and drying it is preferred.

[0105] The thermoplastic resin solution or thermoplastic resin dispersion used here may be a solution using an organic solvent that dissolves the thermoplastic resin, a dispersion using an organic solvent that disperses the thermoplastic resin, or a dispersion using an aqueous medium, and from the standpoints of coatability and environmental impact, a dispersion using an aqueous medium is preferred.

[0106] Examples of methods for applying the thermoplastic resin solution or thermoplastic resin dispersion include bar coating, blade coating, squeeze coating, air knife coating, roll coating, gravure coating, and transfer coating, and a coating machine such as a fountain coater or a slit die coater may be used.

[0107] The coated metallized paper coated with a thermoplastic resin solution or thermoplastic resin dispersion can be dried to remove the organic solvent or aqueous medium, thereby obtaining a metallized paper having a heat seal layer on the metallized layer or overcoat layer.

[0108] From the above viewpoints, the thickness of the base paper for the metallized paper is preferably 10 to 100 μm, more preferably 30 to 100 μm, and even more preferably 50 to 80 μm; the thickness of the metallized layer is preferably 1 to 1000 nm, more preferably 2 to 500 nm, even more preferably 3 to 100 nm, still more preferably 4 to 100 nm, still more preferably 5 to 70 nm, and even more preferably 10 to 60 nm; the thickness of the overcoat layer is preferably 0.1 to 10 μm, more preferably 0.2 to 7 μm, and even more preferably 0.3 to 4 μm; and the coating amount of the overcoat layer is preferably 0.1 to 10 g / m 2 , more preferably 0.2 to 7 g / m 2 , more preferably 0.3 to 5 g / m 2 The coating amount of the heat seal layer is preferably 0.5 to 15 g / m 2 , more preferably 1 to 10 g / m 2 , more preferably 1.5 to 7 g / m 2 , and even more preferably 1.5 to 5 g / m 2 is.

[0109] <Physical Properties of Metal-Deposited Paper> (Thickness) The thickness of the metal-deposited paper is preferably 20 μm or more, more preferably 50 μm or more, and preferably 200 μm or less, more preferably 150 μm or less. That is, the thickness of the metal-deposited paper is preferably 20 to 200 μm, more preferably 50 to 150 μm. The thickness of the metal-deposited paper is measured in accordance with JIS P 8118:2014.

[0110] (Oxygen permeability) The oxygen permeability of the metallized paper at 23°C and 50% RH is preferably 1.5 mL / (m 2 ·day·atm) or less, more preferably 1.0 mL / (m 2 ·day·atm) or less, and the lower limit is 0 mL / (m 2The oxygen permeability of the metallized paper is measured in accordance with JIS K 7126-2:2006, specifically by the method described in the examples.

[0111] (Water vapor permeability) The water vapor permeability of the metallized paper at 40°C and 90% RH is preferably 1.0 g / (m 2 ·day) or less, more preferably 0.7 g / (m 2 · day) or less, and the lower limit is 0 g / (m 2 The water vapor permeability of the metallized paper is measured in accordance with JIS K 7129-2:2019, specifically by the method described in the examples.

[0112] Taking advantage of the excellent printability and processability, as well as the gas barrier properties, the metallized paper of this embodiment can be suitably used as a packaging material, particularly as a packaging bag, for foods such as coffee, confectionery, and milk, as well as medicines, medical supplies, and electronic components.

[0113] [Packaging Bag] A packaging bag according to another embodiment of the present disclosure is a packaging bag made using the above-described metal-deposited paper. Examples of packaging bags include a standing pouch type, a side seal type, a two-sided seal type, a three-sided seal type, a four-sided seal type, an envelope seal type, a grommed seal type (pillow seal type), a pleated seal type, a flat bottom seal type, a square bottom seal type, and a gusset type. The packaging bag of this embodiment may be formed by folding one of the above-described metal-deposited papers having a heat seal layer or by overlapping two sheets of the paper together so that the heat seal layers face each other, and then heat-sealing the peripheral edges of the paper to form the above-described shape, or by folding one of the above-described metal-deposited papers or by overlapping two sheets of the paper together and then bonding the peripheral edges of the paper together with an adhesive to form the above-described shape.

[0114] The metallized paper of this embodiment may be used for purposes other than packaging bags, such as flexible packaging materials such as lids and labels; liquid containers such as milk cartons (hereinafter also referred to as liquid paper containers); and packaging containers such as cups, trays, dishes, lids, laminated tubes, etc. In this case, the contents to be packaged may be liquids, solids (granular materials, powdery materials, etc.), or gels.

[0115] The features of the present invention will be explained in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. Furthermore, unless otherwise specified, "%" and "parts" represent "% by mass" and "parts by mass," respectively. Furthermore, the operations of the examples and comparative examples were carried out at room temperature (20-25°C) and normal humidity (40-50% RH) unless otherwise specified.

[0116] [Measurements and Evaluations] The metallized paper base paper, metallized paper (packaging material), and packaging bags according to the examples and comparative examples were analyzed and evaluated as follows.

[0117] <Base Paper for Metallized Paper> (Oken Smoothness) The Oken Smoothness of the surface having the pigment coating layer was measured in accordance with JIS P 8155:2010.

[0118] (Dynamic friction coefficient against stainless steel) The dynamic friction coefficient of the surface having a pigment coating layer against stainless steel was measured in accordance with JIS P 8147:2010 by fixing a stainless steel plate to the sled side and placing a test piece on the table side so that the surface having the pigment coating layer was in contact with the stainless steel.

[0119] <Metal-deposited paper> (Oxygen permeability) The oxygen permeability of the metal-deposited paper was measured using an oxygen permeability measuring device (trade name "OX-TRAN2 / 22" manufactured by MOCON Corporation) under conditions of a temperature of 23°C and a relative humidity of 50%. Specifically, an isocyanate-based adhesive (manufactured by DIC Corporation, a mixture of 10 parts by mass of Dickdry LX-500 and 1 part by mass of Dickdry KW-75) was applied at 5 g / m2 to the surface of the heat-seal layer of the metal-deposited paper obtained in the examples and comparative examples. 2 After coating, a 20 μm thick CPP film (GP-32, manufactured by Hokuetsu Chemicals Co., Ltd.) was attached to form a laminate sheet. The oxygen permeability of the laminate sheet was measured at a temperature of 23° C. and a relative humidity of 50% in accordance with JIS K7126-2:2006. The lower the oxygen permeability value, the better the oxygen barrier property.

[0120] (Water vapor permeability) The water vapor permeability of metallized paper was measured in accordance with JIS Z 7129-2:2019 (temperature 40°C ± 0.5°C, relative humidity 90% ± 2%) by positioning the metallized paper so that the overcoat layer or metallized layer was on the inner side (low humidity side). The lower the water vapor permeability value, the better the water vapor barrier property.

[0121] (Printability) Test printing was carried out using a gravure printing machine with four colors, and the print density was evaluated using a Gretag Macbeth portable reflection densitometer RD-19A. A: Print density of 1.0 or more for all four colors. B: Print density of less than 1.0 for one or more colors, but white voids are not noticeable. C: Print density of less than 1.0 for one or more colors, and white voids are noticeable.

[0122] (Processability) <Cracks and abrasions in pigment coating layer> Using a horizontal pillow packaging machine (trade name "α8 series FW3410" manufactured by Fujikikai Co., Ltd.), empty bags with a width of 150 mm and a length of 250 mm were continuously produced without any contents at a speed of 60 bags / minute, and the condition of the pigment coating layer of the resulting empty bags was evaluated according to the following criteria: A: No cracks or abrasions. B: Cracks or abrasions present but barely noticeable. C: Cracks or abrasions present and noticeable.

[0123] <<Transportability in an Automatic Packaging Machine>> Using a horizontal pillow packaging machine (trade name "α8 Series FW3410" manufactured by Fujikikai Co., Ltd.), empty bags measuring 150 mm in width and 250 mm in length were continuously produced at a speed of 60 bags per minute without any contents inside. The transportability of the packaging material unwound from the reel before being made into packaging bags was evaluated according to the following criteria: A: The packaging material was pulled smoothly and did not meander. B: The packaging material caught slightly but did not meander. C: The packaging material could not be pulled continuously or meandered.

[0124] <Packaging Bag> (Appearance) The appearance of the empty packaging bags produced in the above-mentioned evaluation of processability was evaluated according to the following criteria. A: The bag is not distorted and there are no sealing defects. B: The bag is slightly distorted, but there are no sealing defects. C: The bag is significantly distorted or there are sealing defects.

[0125] (Gas barrier properties) The empty packaging bags produced in the above-mentioned evaluation of processability were measured using an oxygen transmission rate measuring device (trade name "OX-TRAN2 / 22" manufactured by MOCON Corporation) under conditions of a temperature of 23°C and a relative humidity of 50%, and evaluated according to the following criteria. Note that "pkg" means "package". A: Oxygen transmission rate is less than 0.1 mL / (day pkg 0.2 atm) B: Oxygen transmission rate is 0.1 mL / (day pkg 0.2 atm) or more and less than 1 mL / (day pkg 0.2 atm) C: Oxygen transmission rate is 1 mL / (day pkg 0.2 atm) or more

[0126] Example 1 <Preparation of base paper for metallized paper> 70 parts of kaolin (trade name "Contour Xtreme" manufactured by Imerys, aspect ratio 33, average particle size d50: 0.26 μm) and 30 parts (solid content) of a styrene-acrylic copolymer aqueous dispersion (trade name "ACRONAL S504" manufactured by BASF) were mixed to prepare a coating liquid for a clay coat layer. 2 , thickness 60 μm, density 0.83 g / cm 3 The clay coating layer coating solution was applied to the glossy surface of the substrate (12 g / m2, Stockigt sizing degree (glossy surface) 9 seconds, Oken smoothness (glossy surface) 430 seconds) with a Mayer bar, and dried at 120°C for 1 minute to form a clay coating layer (12 g / m2). 2 Next, a 25 μm thick film having an oxygen permeability (23° C., 50% RH) of 2.0 mL / (m 2 An aqueous dispersion of a water-dispersible polyurethane resin binder (trade name "Takelac WPB-341" manufactured by Mitsui Chemicals, Inc., glass transition temperature 130°C, solid content 30%) was diluted with water to a solid content of 10%, and then coated with a Mayer bar and dried at 120°C for 1 minute to form a resin layer (1 g / m 2Next, 0.1 parts of sodium polyacrylate (trade name "Aron T-50" manufactured by Toagosei Co., Ltd.) was added as a dispersant to an aqueous solution per 100 parts of kaolin to be dispersed, and 30 parts of fine kaolin (trade name "Milagros J" manufactured by BASF), 40 parts of light calcium carbonate (trade name "TP-123CS" manufactured by Okutama Kogyo Co., Ltd.), and 30 parts of heavy calcium carbonate (trade name "Hydrocarb 90" manufactured by Bihoku Funka Kogyo Co., Ltd.) were added as solids, and the mixture was dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (trade name "Oji Ace A" manufactured by Oji Cornstarch Co., Ltd.) and 25 parts (solids) of styrene-butadiene copolymer latex (trade name "OJ1000H" manufactured by JSR Corporation) were added as a binder relative to 70 parts (solids) of pigment, to prepare Coating Solution A for the pigment coating layer, which had a final solids concentration of 60%. This was applied to the surface opposite the resin layer in an amount of 10 g / m2 in terms of solids. 2 After coating using a Mayer bar so that the coating was as follows, the coated paper was dried for 1 minute in a 120°C air dryer. Finally, a linear pressure of 90 kg / cm was applied, with a chilled roll in contact with the resin layer coated surface and a cotton roll in contact with the pigment layer coated surface. The rolls were heated to 40°C and a 12-stage supercalendering treatment was performed to obtain a base paper for metallized paper (thickness 65 μm, smoothness of the resin layer side: 7000 seconds, smoothness of the reverse pigment coating layer side: 2400 seconds, dynamic friction coefficient of the pigment coating layer side against stainless steel: 0.188). The obtained base paper for metallized paper was subjected to the above-mentioned analyses and evaluations. The results are shown in Table 1. <Preparation of Metallized Paper> An aluminum vapor-deposited layer (thickness 50 nm) was formed on the resin layer of the above base paper for metallized paper using a batch-type vacuum vapor deposition device. Next, an aqueous dispersion of ethylene-methacrylic acid copolymer sodium salt (active ingredient 35% by mass, trade name "Chemipearl S-300" manufactured by Mitsui Chemicals, Inc.) was diluted with water so that the active ingredient content was 20% by mass to prepare a coating liquid for the heat seal layer. The coating liquid was applied with a Mayer bar and dried at 120°C for 1 minute to form a heat seal layer (3 g / m 2 The metallized paper thus obtained was subjected to the above-described analysis and evaluation. The results are shown in Table 1.

[0127] Example 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that Coating Solution B for pigment coating layer was used in the same amounts as in Example 1, with 80 parts pigment, 5 parts oxidized starch, and 15 parts by mass of styrene-butadiene copolymer latex, each in terms of solid content.

[0128] Example 3 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that Coating Solution C for pigment coating layer was used in the same amounts as in Example 1, with the pigment, oxidized starch, and styrene-butadiene copolymer latex being 60 parts, 5 parts, and 35 parts by mass, respectively, in terms of solid content.

[0129] Example 4 To an aqueous solution prepared by adding 0.1 parts of sodium polyacrylate (manufactured by Toagosei Co., Ltd. under the trade name "Aron T-50") as a dispersant relative to 100 parts of kaolin to be dispersed, 30 parts of fine kaolin (manufactured by BASF under the trade name "Milagros J"), 40 parts of light calcium carbonate (manufactured by Okutama Kogyo Co., Ltd. under the trade name "TP-123CS"), and 30 parts of heavy calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd. under the trade name "Hydrocarb 90") were added as solid contents, and the mixture was dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (trade name "Oji Ace A" manufactured by Oji Cornstarch Co., Ltd.) and 15 parts (solids) of styrene-butadiene copolymer latex (trade name "OJ1000H" manufactured by JSR Corporation) were added as binders relative to 80 parts (solids) of pigment, to prepare Coating Solution D for the pigment coating layer having a final solids concentration of 60%. 2 to 10 g / m 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that the thickness was changed to 3.8 μm.

[0130] Example 5 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that instead of using aluminum as the deposition source, a mixture of aluminum and oxygen was vacuum-deposited, and the deposited layer was made of alumina (AlOx) and had a thickness of 20 nm.

[0131] Example 6 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that instead of aluminum as the deposition source, silica (SiOx) was deposited using electron beam deposition to form a deposited layer with a thickness of 20 nm.

[0132] Example 7 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that chemical vapor deposition was carried out using acetylene instead of aluminum as the deposition source, and the deposited layer was made of diamond-like carbon (DLC) and had a thickness of 20 nm.

[0133] Example 8 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the coating liquid for the heat seal layer was changed to a polyolefin dispersion (active content 43 mass%, product name "Rhobarr 320" manufactured by Dow Chemical Japan Ltd.).

[0134] Example 9 After aluminum deposition, the oxygen permeability (23°C, 50% RH) of a 25 μm thick film was 2.0 mL / (m 2 An aqueous dispersion of a polyurethane resin binder (trade name "Takelac WPB-341" manufactured by Mitsui Chemicals, Inc., glass transition temperature 130°C, solid content 30%) was diluted with water to a solid content of 10%, and then coated with a Mayer bar. The coating was dried at 120°C for 1 minute to form an overcoat layer (0.5 g / m 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that a metallized paper having a thickness of 0.5 μm was formed.

[0135] Example 10 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the number of stages in the supercalender was changed from 12 stages to 6 stages.

[0136] Example 11 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that the number of stages in the supercalender was changed from 12 stages to 2 stages.

[0137] Example 12 On the clay coating layer, an aqueous dispersion of a water-dispersible polyester resin (trade name "Eliteru KT-8803" manufactured by Unitika Ltd., acid value 8 mgKOH / g, hydroxyl value 3 mgKOH / g, glass transition temperature 65°C, solid content 30%) was diluted with water to a solid content of 10%, and then coated with a Mayer bar and dried at 120°C for 1 minute to form a resin layer (1 g / m 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that a metallized paper (thickness: 1 μm) was formed.

[0138] Example 13 On a clay coating layer, a water-soluble polyvinyl alcohol resin (trade name "EXCEVAL HR-3010" manufactured by Kuraray Co., Ltd., ethylene-modified polyvinyl alcohol, saponification degree 99.00 to 99.40 mol%) was dissolved in water, and then further diluted with water to a solid content concentration of 8%, followed by Mayer bar coating and drying at 120°C for 1 minute to form a resin layer (1 g / m 2 The base paper for metallized paper and metallized paper were obtained in the same manner as in Example 4, except that a metallized paper (1 μm thick) was formed. The results of Examples 1 to 13 are shown in Table 1 below.

[0139]

[0140] Comparative Example 1 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that the pigment coating layer was not formed.

[0141] Comparative Example 2 A base paper for metallized paper and metallized paper were obtained in the same manner as in Comparative Example 1, except that the 12-stage supercalendering was not carried out.

[0142] Comparative Example 3 A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that a resin coating solution containing 100 parts by mass (solid content) of a styrene-(meth)acrylic resin (trade name "ACRONAL S504" manufactured by BASF) was used instead of Coating Solution A for the pigment coating layer.

[0143] Comparative Example 4 To an aqueous solution prepared by adding 0.1 parts of sodium polyacrylate (manufactured by Toagosei Co., Ltd. under the trade name "Aron T-50") as a dispersant relative to 100 parts of kaolin to be dispersed, 30 parts of fine kaolin (manufactured by BASF under the trade name "Milagros J"), 40 parts of light calcium carbonate (manufactured by Okutama Kogyo Co., Ltd. under the trade name "TP-123CS"), and 30 parts of heavy calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd. under the trade name "Hydrocarb 90") were added as solid contents, and the mixture was dispersed using a Coles disperser to prepare a pigment slurry. A base paper for metallized paper and metallized paper were obtained in the same manner as in Example 1, except that 20 parts (solid content) of the pigment slurry was used as coating solution E for the pigment coating layer by adding 5 parts (solid content) of oxidized starch (trade name "Oji Ace A" manufactured by Oji Cornstarch Co., Ltd.) and 75 parts (solid content) of styrene-butadiene copolymer latex (trade name "OJ1000H" manufactured by JSR Corporation) as binders.

[0144] Comparative Example 5 To an aqueous solution prepared by adding 0.1 parts of sodium polyacrylate (manufactured by Toagosei Co., Ltd. under the trade name "Aron T-50") as a dispersant relative to 100 parts of kaolin to be dispersed, 30 parts of fine kaolin (manufactured by BASF under the trade name "Milagros J"), 40 parts of light calcium carbonate (manufactured by Okutama Kogyo Co., Ltd. under the trade name "TP-123CS"), and 30 parts of heavy calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd. under the trade name "Hydrocarb 90") were added as solid contents, and the mixture was dispersed using a Coles disperser to prepare a pigment slurry. To this pigment slurry, 5 parts (solids) of oxidized starch (trade name "Oji Ace A" manufactured by Oji Cornstarch Co., Ltd.) and 5 parts (solids) of styrene-butadiene copolymer latex (trade name "OJ1000H" manufactured by JSR Corporation) were added as binders per 90 parts (solids) of pigment to prepare Coating Solution F for the pigment coating layer, which had a final solids concentration of 60%, and the same procedures as in Example 1 were used to obtain base paper for metallized paper and metallized paper. The results of Comparative Examples 1 to 5 are shown in Table 2.

[0145]

[0146] The metallized paper produced using the base paper for metallized paper of the examples was excellent in printability and processability. In addition, the metallized paper produced using the base paper for metallized paper of the examples also produced packaging bags with good appearance.

Claims

1. A base paper for metallized paper having a resin layer on one side of a paper substrate, for forming a metallized layer on the resin layer, and having a pigment coating layer on the other side of the paper substrate, the pigment coating layer having a pigment content of 50% by mass or more and 85% by mass or less, and the surface having the pigment coating layer has an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less.

2. The base paper for metallized paper according to claim 1, further comprising a clay coating layer between the paper substrate and the resin layer.

3. The base paper for metallized paper according to claim 1 or 2, wherein the resin layer contains at least one resin selected from the group consisting of water-dispersible polyurethane resins and water-dispersible polyester resins.

4. The metal-deposited paper according to claim 1 or 2, wherein the resin layer contains a water-soluble polyvinyl alcohol resin.

5. A metal-deposited paper having a resin layer on one side of a paper substrate and a pigment coating layer on the other side of the paper substrate, the metal-deposited paper having a metal-deposited layer on the resin layer, the pigment coating layer having a pigment content of 50% by mass or more and 85% by mass or less, the surface having the pigment coating layer having an Oken smoothness of 300 seconds or more and a dynamic friction coefficient against stainless steel of 0.35 or less.

6. The metal-deposited paper according to claim 5, which has a heat seal layer on said metal-deposited layer.

7. The metallized paper according to claim 6, further comprising an overcoat layer between said metallized layer and said heat seal layer.

8. The metal-deposited paper according to any one of claims 5 to 7, further comprising a clay coating layer between the paper substrate and the resin layer.

9. The metal-deposited paper according to any one of claims 5 to 8, wherein the resin layer contains at least one resin selected from the group consisting of water-dispersible polyurethane resins and water-dispersible polyester resins.

10. The metal-deposited paper according to any one of claims 5 to 8, wherein the resin layer contains a water-soluble polyvinyl alcohol resin.

11. A packaging bag made using the metallized paper according to any one of claims 5 to 10.

Citation Information

Patent Citations

  • Metallized paper base paper and metallized paper

    JP6958756B1

  • Metallized paper base paper and metallized paper

    JP6958757B1

  • Polyurethane dispersion and polyurethane laminate

    WO2015016069A1

  • Paper for metal vacuum deposited label and production thereof

    JP1989221593A

  • Biodegradable paper sheet and paper container

    JP2003013391A