glass
A glass with specific composition parameters addresses the manufacturing challenges of high Young's modulus and low thermal expansion by suppressing deflection and crystallization, enabling easier production and use in semiconductor manufacturing.
Patent Information
- Application Number
- PCT/JP2024/015068
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
Glass with high Young's modulus and low coefficient of thermal expansion is difficult to manufacture due to susceptibility to crystallization, making it challenging to suppress deflection during semiconductor device manufacturing.
A glass composition with a Young's modulus of 95 GPa or more and a linear thermal expansion coefficient of 5.5 ppm/°C or less, along with a devitrification suppression parameter value A of 6.0 or more, is developed to facilitate manufacturing while suppressing deflection.
The glass composition effectively suppresses deflection and facilitates manufacturing by maintaining a low liquidus temperature and preventing crystallization, ensuring the glass can be easily produced and used as a substrate for semiconductor devices.
Smart Images

Figure JPOXMLDOC01-APPB-M000001 
Figure JPOXMLDOC01-APPB-M000002 
Figure JPOXMLDOC01-APPB-M000003
Abstract
Description
Glass
[0001] The present invention relates to glass.
[0002] Glass is sometimes used as a member for supporting semiconductor devices during the manufacturing process of the semiconductor devices. For example, Patent Document 1 describes a supporting glass substrate with a high Young's modulus to suppress deflection. In addition, the coefficient of thermal expansion may be reduced to suppress deflection due to temperature changes.
[0003] Japanese Patent Application Laid-Open No. 2021-20840
[0004] However, glass with a low thermal expansion coefficient and a high Young's modulus to suppress distortion can easily crystallize and be difficult to manufacture, so there is a demand for glass that can suppress distortion and is easy to manufacture.
[0005] An object of the present invention is to provide a glass that is easy to manufacture while suppressing warping.
[0006] The glass according to the present disclosure has a Young's modulus of 95 GPa or more, a linear thermal expansion coefficient of 5.5 ppm / °C or less, and a devitrification suppression parameter value A shown in formula (1) of 6.0 or more.
[0007]
[0008] Here, N is the number of oxides contained in the glass that are present at a content of 0.5% or more in mole percent based on oxides, and R is the gas constant [R x O y ] is the oxide R contained in the glass in mole % notation based on oxides. x O y The content is
[0009] According to the present invention, it is possible to easily manufacture the device while suppressing bending.
[0010] Fig. 1 is a schematic diagram of a glass according to this embodiment, and Fig. 2 is a schematic diagram for explaining deflection evaluation.
[0011] Preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Note that the present invention is not limited to these embodiments, and when there are multiple embodiments, the present invention also includes combinations of the embodiments. Numerical values include rounded ranges. The upper and lower limits of the numerical ranges can be combined as appropriate.
[0012] (Glass) FIG. 1 is a schematic diagram of glass according to this embodiment. As shown in FIG. 1, glass 10 according to this embodiment is used as a glass substrate for manufacturing semiconductor packages, and more specifically, is a supporting glass substrate for manufacturing FOWLPs and the like. However, the use of glass 10 is not limited to the manufacture of FOWLPs and the like and is arbitrary. It may be a glass substrate used to support components, or may be used for purposes other than supporting components. Note that FOWLPs and the like include fan-out wafer level packages (FOWLPs) and fan-out panel level packages (FOPLPs).
[0013] (Young's modulus of glass) The Young's modulus of the glass 10 is 95 GPa or more, preferably 96 GPa or more, more preferably 97 GPa or more, more preferably 98 GPa or more, more preferably 99 GPa or more, more preferably 100 GPa or more, more preferably 101 GPa or more, more preferably 102 GPa or more, more preferably 103 GPa or more, more preferably 104 GPa or more, more preferably 105 GPa or more, more preferably 106 GPa or more, more preferably 108 GPa or more, more preferably 111 GPa or more, more preferably 112 GPa or more, more preferably 113 GPa or more, more preferably 114 GPa or more, and more preferably 115 GPa or more. Furthermore, the Young's modulus of the glass 10 is preferably 100 GPa or more and 150 GPa or less, more preferably 105 GPa or more and 140 GPa or less, and even more preferably 110 GPa or more and 130 GPa or less. Having the Young's modulus within this range can suppress deflection and facilitate cutting, grinding, and polishing. The Young's modulus of the glass 10 can be measured based on the propagation of ultrasonic waves using a 38DL PLUS manufactured by Olympus Corporation.
[0014] (Linear Thermal Expansion Coefficient of Glass) The linear thermal expansion coefficient of the glass 10 is 5.5 ppm / °C or less, preferably 5.4 ppm / °C or less, more preferably 5.3 ppm / °C or less, more preferably 5.2 ppm / °C or less, more preferably 5.1 ppm / °C or less, more preferably 5.0 ppm / °C or less, more preferably 4.9 ppm / °C or less, more preferably 4.8 ppm / °C or less, more preferably 4.7 ppm / °C or less, more preferably 4.6 ppm / °C or less, more preferably 4.5 ppm / °C or less, more preferably 4.4 ppm / °C or less, more preferably 4.3 ppm / °C or less, more preferably 4.2 ppm / °C or less, and more preferably 4.1 ppm / °C or less. Furthermore, the linear thermal expansion coefficient of the glass 10 is preferably 3.0 ppm / °C or more and 5.5 ppm / °C or less, more preferably 3.3 ppm / °C or more and 5.0 ppm / °C or less, and even more preferably 3.5 ppm / °C or more and 4.5 ppm / °C or less. Such a low linear thermal expansion coefficient can suppress deflection due to temperature changes. That is, for example, when the glass 10 supports a member with a low thermal expansion coefficient, the low linear thermal expansion coefficient of the glass 10 as described above can suppress deflection when the temperature of the glass 10 and the member changes. The linear thermal expansion coefficient is the average thermal expansion coefficient in the range of 50°C to 200°C, and is a value measured in accordance with DIN-51045-1, a standard for thermal expansion measurement. For example, a thermal expansion meter DIL 402 Expedis Supreme manufactured by NETZSCH is used as the measuring device to measure in the range of 30°C to 300°C, and the average thermal expansion coefficient in the range of 50°C to 200°C may be taken as the linear thermal expansion coefficient.
[0015] (Devitrification Suppression Parameter Value of Glass) The devitrification suppression parameter value A of the glass 10 is defined as a value shown by the following formula (1).
[0016]
[0017] In formula (1), N is the number of oxides contained in glass 10 that are present in an amount of 0.5% or more in mole percent based on oxides. R is the gas constant, R=8.31(J·K -1 ・mol -1 ). x O y] is the oxide R contained in the glass 10 in mole percent notation based on oxides. x O y The content of R x O y In the formula, R is an element constituting the oxide, and x and y are any integers. Therefore, for example, if the glass 10 contains Na in mole percent notation based on oxides, 2 O 30%, SiO 2 Assuming that the glass contains 70% of the above, the devitrification suppression parameter value A is 2·[{−R(0.3ln(0.3)+0.7ln(0.7))}] 0.4 That is, approximately 2.53.
[0018] The devitrification suppression parameter value A is a parameter calculated based on the composition of glass 10 as shown in formula (1), and is an index showing the difficulty of crystallization of glass 10. For example, the higher the N on the right side of formula (1), the greater the number of components contained in glass 10, and the components tend to interfere with each other, making it more difficult for the components to crystallize, thereby suppressing devitrification due to crystallization. Also, for example, the terms other than N on the right side of formula (1) indicate the degree of disorder of the components, and the higher the value of that term, the more disordered the components become and the more difficult they tend to crystallize, thereby suppressing devitrification due to crystallization.
[0019] The devitrification suppression parameter value A of glass 10 is 6.0 or more, preferably 6.2 or more, more preferably 6.25 or more, more preferably 6.3 or more, more preferably 6.5 or more, more preferably 6.7 or more, more preferably 6.9 or more, more preferably 7 or more, more preferably 7.7 or more, more preferably 7.9 or more, more preferably 8.1 or more, and more preferably 8.3 or more. The devitrification suppression parameter value A of glass 10 is preferably 6.0 or more and 20 or less, more preferably 6.4 or more and 15 or less, and even more preferably 7.3 or more and 10 or less. Such a high devitrification suppression parameter value A can prevent the liquidus temperature of glass 10 from becoming too high. This makes it possible to maintain a low holding temperature during the production of glass 10 to prevent crystallization of glass 10, making the production of glass 10 easier.
[0020] (Glass Composition) Next, a description will be given of a preferred composition of the glass 10. However, the glass 10 may have any composition as long as the Young's modulus, the coefficient of linear thermal expansion, and the devitrification suppression parameter value A satisfy the above ranges.
[0021] For glass 10, the value E represented by the following formula (2) is preferably 0.90 or greater, more preferably 0.95 or greater, even more preferably 1.00 or greater, and even more preferably 1.05 or greater. When the value E is within this range, the Young's modulus can be set to 95 GPa or greater, thereby appropriately suppressing deflection.
[0022] E=(124-0.54×[SiO 2 ]+0.29×[Al 2 O 3 ]−1.15×[B 2 O 3 ]+0.20×[MgO]-0.20×[CaO]-0.10×[SrO]-1.20×[BaO]+1.0×[Li 2 O]-3.0×[K 2 O]+0.05×[ZnO]+1.45×[ZrO 2 ]-0.05×[TiO 2 ]+1.60×[Y 2 O 3 ]+1.35×[Gd 2 O 3 ]+1.00×[Ta 2 O 5 ]) / 100・・・(2)
[0023] Furthermore, for glass 10, the value F expressed by the following formula (3) is preferably 1.05 or less, more preferably 1.0 or less, even more preferably 0.95 or less, and even more preferably 0.90 or less. When the value F is within this range, the thermal expansion coefficient can be kept at 5.5 ppm / K or less, thereby suppressing deflection.
[0024] F=(14.1-0.12×[SiO 2 ]−0.13×[Al 2 O 3 ]−0.10×[B 2 O 3]-0.05×[MgO]+0.01×[CaO]+0.15×[SrO]+0.02×[BaO]+0.05×[Li 2 O]-0.07×[ZnO]-0.03×[ZrO 2 ]-0.07×[TiO 2 ]+0.04×[Y 2 O 3 ]+0.07×[Gd 2 O 3 ]−0.10×[Ta 2 O 5 ]) / 5.5・・・(3)
[0025] (SiO 2 ) The glass 10 is SiO 2 Contains (SiO 2 It is preferable that the content of SiO is higher than 0 mol %. 2 is a component that reduces the linear thermal expansion coefficient and controls the Young's modulus. In addition, SiO 2 The content of the glass 10 is preferably 60% or less. 2 The content of SiO is preferably 35% or more and 60% or less, more preferably 40% or more and 59% or less, more preferably 43% or more and 57% or less, more preferably 47% or more and 55% or less, more preferably 48% or more and 53% or less, more preferably 49% or more and 52% or less, and more preferably 50% or more and 51% or less. 2 By ensuring that the content falls within this range, the coefficient of linear thermal expansion can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0026] (Al 2 O 3 ) Al 2 O 3 has the effect of increasing the Young's modulus, suppressing deflection, and suppressing phase separation of the glass. 2 O 3 Does not contain (Al 2 O 3 The content of Al may be 0 mol %, 2 O 3 It may also contain Al2 O 3 By making the content of Al 25% or less, it is possible to prevent the liquidus temperature from becoming high. 2 O 3 The content of Al is preferably 5% or more and 25% or less, more preferably 6% or more and 20% or less, more preferably 8% or more and 19% or less, more preferably 10% or more and 18.5% or less, more preferably 11% or more and 18% or less, more preferably 12% or more and 17.5% or less, more preferably 13% or more and 17% or less, more preferably 14% or more and 16.5% or less, and more preferably 14.5% or more and 16% or less. 2 O 3 By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0027] (B 2 O 3 ) B 2 O 3 has the effect of suppressing devitrification due to crystallization of the glass, facilitating manufacturing, and controlling the Young's modulus. 2 O 3 Does not contain (B 2 O 3 The content of B may be 0 mol %, 2 O 3 The glass 10 may contain, in mole percent on an oxide basis, B 2 O 3 The content of is preferably 1% or more and 15% or less, more preferably 2% or more and 14% or less, more preferably 3% or more and 13% or less, more preferably 4% or more and 12% or less, more preferably 5% or more and 11% or less, and even more preferably 6% or more and 10% or less. 2 O 3 By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0028] (MgO) MgO increases Young's modulus without increasing density, so increasing the specific elastic modulus can suppress deflection. It also has the effect of reducing the linear thermal expansion coefficient. On the other hand, by setting the MgO content to 28% or less, the liquidus temperature can be controlled low. Therefore, glass 10 may not contain MgO (MgO content is 0 mol%), but may contain MgO. The MgO content of glass 10, expressed in mol% on an oxide basis, is preferably 13% to 28% or less, more preferably 14% to 27% or less, more preferably 17% to 25% or less, more preferably 18% to 23% or less, and even more preferably 20% to 22% or less. By setting the MgO content within this range, the Young's modulus can be increased while the linear thermal expansion coefficient is reduced, thereby suppressing deflection. Furthermore, by increasing the devitrification suppression parameter value A, manufacturing can be facilitated.
[0029] (CaO) CaO has the characteristic of increasing the specific elastic modulus second only to MgO among oxides of Group 2 elements, while not excessively reducing the linear thermal expansion coefficient. Furthermore, it also has the characteristic of being less likely to increase the liquidus temperature than MgO. Therefore, glass 10 may be CaO-free (CaO content is 0 mol%), or may contain CaO. By reducing the CaO content to 10% or less, an increase in the linear thermal expansion coefficient can be suppressed and the liquidus temperature can be controlled low. The CaO content of glass 10, expressed in mol% based on oxide, is preferably 0.5% to 10% or less, more preferably 1% to 8% or less, more preferably 2% to 5% or less, and even more preferably 3% to 4% or less. By having the CaO content within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. Furthermore, the devitrification suppression parameter value A can be increased, making production easier.
[0030] (SrO) SrO has the effect of improving the meltability of glass and lowering the liquidus temperature. Therefore, glass 10 may be free of SrO (SrO content is 0 mol%), but may contain SrO. By setting the SrO content to 10% or less, an increase in the linear thermal expansion coefficient can be suppressed and the liquidus temperature can be controlled low. In glass 10, the SrO content, expressed in mol% on an oxide basis, is preferably 0.5% to 10% or less, more preferably 1% to 8% or less, more preferably 2% to 5% or less, and even more preferably 3% to 4% or less. By setting the SrO content within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. Furthermore, the devitrification suppression parameter value A can be increased, making production easier.
[0031] (BaO) BaO has the effect of improving the meltability of glass and lowering the liquidus temperature. Therefore, the glass 10 may be BaO-free (BaO content is 0 mol%), or may contain BaO. By setting the BaO content to 10% or less, an increase in the linear thermal expansion coefficient can be suppressed and the liquidus temperature can be controlled low. The BaO content of the glass 10, expressed in mol% on an oxide basis, is preferably 0.5% to 10% or less, more preferably 1% to 8% or less, more preferably 2% to 5% or less, and even more preferably 3% to 4% or less. By setting the BaO content within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. Furthermore, the devitrification suppression parameter value A can be increased, making production easier.
[0032] (Li 2 O) Li 2 Among alkali metal oxides, O has the effect of improving the solubility without decreasing the linear thermal expansion coefficient. 2 O-free (Li 2 The content of O may be 0 mol%, but 2 It may contain O. 2By setting the O content to 5% or less, the Young's modulus can be increased and the linear thermal expansion coefficient can be prevented from increasing. 2 The O content is preferably 0.1% or more and 5% or less, more preferably 0.3% or more and 4% or less, more preferably 0.5% or more and 3% or less, more preferably 0.8% or more and 2.5% or less, and even more preferably 1% or more and 2% or less. 2 By setting the O content within this range, it is possible to increase the Young's modulus while decreasing the coefficient of linear thermal expansion, thereby suppressing deflection. In addition, it is possible to increase the devitrification suppression parameter value A, thereby facilitating production.
[0033] (Na 2 O) Na 2 Among alkali metal oxides, O has the effect of improving the solubility of glass and lowering the liquidus temperature. 2 Although it may be free of O (NaO content is 0 mol%), 2 It may contain O. 2 By keeping the O content at 5% or less, the Young's modulus can be increased and the linear thermal expansion coefficient can be prevented from increasing. 2 The O content is preferably 0.1% or more and 5% or less, more preferably 0.3% or more and 4% or less, even more preferably 0.5% or more and 3% or less, still more preferably 0.8% or more and 2.5% or less, and even more preferably 1% or more and 2% or less. 2 By setting the O content within this range, it is possible to increase the Young's modulus while decreasing the coefficient of linear thermal expansion, thereby suppressing deflection. In addition, it is possible to increase the devitrification suppression parameter value A, thereby facilitating production.
[0034] (K 2 O) K 2 O has the effect of improving the melting property of the glass and lowering the liquidus temperature. 2 It may be free of O (the content of KO is 0 mol%), but 2 It may contain O. 2By keeping the O content at 5% or less, the Young's modulus can be increased and the linear thermal expansion coefficient can be prevented from increasing. 2 The O content is preferably 0.1% or more and 5% or less, more preferably 0.3% or more and 4% or less, even more preferably 0.5% or more and 3% or less, still more preferably 0.8% or more and 2.5% or less, and even more preferably 1% or more and 2% or less. 2 By setting the O content within this range, it is possible to increase the Young's modulus while decreasing the coefficient of linear thermal expansion, thereby suppressing deflection. In addition, it is possible to increase the devitrification suppression parameter value A, thereby facilitating production.
[0035] (ZnO) ZnO has the effect of improving the meltability of glass and increasing the Young's modulus. Therefore, the glass 10 may be ZnO-free (ZnO content is 0 mol%), but may also contain ZnO. By reducing the ZnO content to 5% or less, an increase in the linear thermal expansion coefficient can be suppressed and the liquidus temperature can be controlled. The ZnO content of the glass 10, expressed in mole percent on an oxide basis, is preferably 0.1% to 5% or less, more preferably 0.3% to 4% or less, more preferably 0.5% to 3% or less, more preferably 0.8% to 2.5% or less, and even more preferably 1% to 2% or less. By having the ZnO content within this range, the Young's modulus can be increased while the linear thermal expansion coefficient is reduced, thereby suppressing deflection. Furthermore, the devitrification suppression parameter value A can be increased, making production easier.
[0036] (P 2 O 5 ) P 2 O 5 has the effect of improving the melting property of the glass and lowering the linear thermal expansion coefficient. 2 O 5 Does not contain (P 2 O 5 The content of P may be 0 mol %, 2 O 5 It may contain P 2 O 5By making the content of P 5% or less, it is possible to increase the Young's modulus without deteriorating the chemical resistance and to suppress an increase in the linear thermal expansion coefficient. 2 O 5 The content of P is preferably 0.1% or more and 5% or less, more preferably 0.3% or more and 4% or less, even more preferably 0.5% or more and 3% or less, still more preferably 0.8% or more and 2.5% or less, and even more preferably 1% or more and 2% or less. 2 O 5 By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0037] (ZrO 2 ) ZrO 2 can increase the Young's modulus without relatively decreasing the coefficient of linear thermal expansion. 2 Does not contain (ZrO 2 The content of ZrO may be 0 mol %, 2 It may contain ZrO 2 The liquidus temperature can be controlled by making the content of ZrO 5% or less. 2 The content of ZrO is preferably 0.1% or more and 5% or less, more preferably 0.3% or more and 4% or less, even more preferably 0.5% or more and 3% or less, still more preferably 0.8% or more and 2.5% or less, and even more preferably 1% or more and 2% or less. 2 By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0038] (TiO 2 ) TiO 2 can increase the Young's modulus without relatively decreasing the linear thermal expansion coefficient. 2 Does not contain (TiO 2 The content of TiO may be 0 mol %,2 It may contain TiO 2 The liquidus temperature can be controlled by making the content of 5% or less. 2 The content of TiO is preferably 0.1% or more and 5% or less, more preferably 0.3% or more and 4% or less, even more preferably 0.5% or more and 3% or less, still more preferably 0.8% or more and 2.5% or less, and even more preferably 1% or more and 2% or less. 2 By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0039] (Y 2 O 3 ) Y 2 O 3 has the effect of improving the melting property of the glass and increasing the Young's modulus. 2 O 3 Does not contain (Y 2 O 3 The content of Y may be 0 mol %, 2 O 3 Y 2 O 3 The linear thermal expansion coefficient can be controlled by making the content of Y 10% or less. 2 O 3 The content of Y is preferably 0.1% or more and 10% or less, more preferably 0.3% or more and 8% or less, more preferably 0.5% or more and 5% or less, more preferably 0.8% or more and 4% or less, more preferably 1% or more and 3% or less, and even more preferably 1% or more and 2% or less. 2 O 3 By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0040] (Gd 2 O 3 ) Gd 2 O3 has the effect of improving the melting property of the glass and increasing the Young's modulus. 2 O 3 Non-containing (Gd 2 O 3 The content of Gd may be 0 mol %, 2 O 3 It may contain Gd 2 O 3 The coefficient of linear thermal expansion can be controlled by making the content of Gd 10% or less. 2 O 3 The content of Gd is preferably 0.1% or more and 10% or less, more preferably 0.3% or more and 8% or less, more preferably 0.5% or more and 5% or less, more preferably 0.8% or more and 4% or less, more preferably 1% or more and 3% or less, and even more preferably 1% or more and 2% or less. 2 O 3 By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0041] (W.O. 3 ) WO 3 has the effect of improving the melting property of the glass and increasing the Young's modulus. 3 Does not contain (WO 3 The content of WO may be 0 mol %. 3 It may contain WO 3 By making the content of WO 5% or less, it is possible to suppress an increase in the linear thermal expansion coefficient and control the liquidus temperature. 3 The content of WO is preferably 0.1% or more and 5% or less, more preferably 0.3% or more and 4% or less, even more preferably 0.5% or more and 3% or less, even more preferably 0.8% or more and 2.5% or less, and even more preferably 1% or more and 2% or less. 3By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0042] (Ta 2 O 5 ) Ta 2 O 5 has the effect of decreasing the coefficient of linear thermal expansion and increasing the Young's modulus. 2 O 5 Does not contain (Ta 2 O 5 The content of Ta may be 0 mol %, 2 O 5 It may contain Ta 2 O 5 The liquidus temperature can be controlled by making the content of Ta 10% or less. 2 O 5 The content of Ta is preferably 0.5% or more and 10% or less, more preferably 1% or more and 8% or less, more preferably 1.5% or more and 6% or less, more preferably 2% or more and 5% or less, more preferably 2.5% or more and 4.2% or less, and even more preferably 3% or more and 4% or less. 2 O 5 By ensuring that the content falls within this range, the Young's modulus can be increased while the linear thermal expansion coefficient can be reduced, thereby suppressing deflection. In addition, the devitrification suppression parameter value A can be increased, thereby facilitating production.
[0043] In addition, Ta 2 O 5 is a component that has a large effect on Young's modulus and the coefficient of linear thermal expansion. 2 O 5 The content of Ta may be less than 0.5%. In this case, it is preferable that the Young's modulus of the glass 10 is 105 GPa or more and the linear thermal expansion coefficient is 5.1 ppm / K or less. The glass 10 contains Ta in mole percent notation based on oxides. 2 O 5In this case, the devitrification suppression parameter value A of the glass 10 is preferably 6.4 or more, more preferably 7.0 or more, and even more preferably 7.5 or more.
[0044] (MnO) MnO has the effect of increasing the Young's modulus. However, MnO may increase the liquidus temperature, and even a small amount of MnO can cause the glass to be colored dark brown to black. Therefore, it is preferable that glass 10 does not contain MnO. The MnO content of glass 10, expressed in mole percent on an oxide basis, is preferably 0.1% or less, more preferably 0.001% to 0.05%, and even more preferably 0.005% to 0.01%. By keeping the MnO content within this range, a decrease in light transmittance can be suppressed.
[0045] (Fe 2 O 3 ) Glass 10 is Fe 2 O 3 It is preferable that the glass 10 does not contain Fe as an external percentage, expressed as mass % on an oxide basis. 2 O 3 The content of Fe is preferably 0.1% or less, more preferably 0.001% or more and 0.05% or less, and even more preferably 0.005% or more and 0.01% or less. 2 O 3 Such a low content of Fe can suppress the decrease in light transmittance. 2 O 3 By setting the content of Fe in the above range, it becomes possible to make the transmittance of the glass 10 having a thickness of 0.7 mm to 90% or more for light with a wavelength of 900 nm, and it is possible to suppress a decrease in the transmittance of infrared light. 2 O 3 The content of Fe is based on the oxide. 2 O 3 Fe contained in glass 10 relative to the total mass of all components of glass 10 excluding 2 O 3 It refers to the mass ratio of
[0046] (Value of N) In glass 10, the value of N in formula (1) (the number of oxides contained in glass 10 that have a content of 0.5% or more) is preferably 8 or more, more preferably 10 to 25, more preferably 11 to 22, more preferably 12 to 20, more preferably 13 to 18, and even more preferably 15 to 17. Such a high value of N makes it possible to increase the devitrification suppression parameter value A and facilitate production.
[0047] It is preferable that the glass 10 does not contain a sintered body. In other words, the glass 10 is preferably a glass that is not a sintered body. The term "sintered body" as used herein refers to a component in which a plurality of particles are heated at a temperature lower than the melting point to bond the particles together. Sintered bodies have a relatively high porosity due to the inclusion of pores, but the glass 10 is not a sintered body and therefore has a low porosity, typically 0%. However, the inclusion of unavoidable traces of pores is permitted. The porosity here refers to the so-called true porosity, which is the sum of the volumes of pores (voids) that are open to the outside and pores (voids) that are not open to the outside, divided by the total volume (apparent volume). The porosity can be measured, for example, according to JIS R 1634:1998, "Method for measuring the density and open porosity of sintered fine ceramics."
[0048] The glass used for the glass 10 is preferably amorphous glass, i.e., an amorphous solid. This glass may be crystallized glass containing crystals on the surface or inside, but amorphous glass is preferred from the viewpoint of density. Among ceramics, those produced by sintering methods are preferably not used because they have low transmittance and high density.
[0049] (Shape of Glass) Next, the shape of the glass 10 will be described. As shown in FIG. 1 , the glass 10 is a plate-shaped glass substrate including a surface 12, which is one main surface, and a surface 14, which is the main surface opposite to the surface 12. The surface 14 may be parallel to the surface 12, for example. The glass 10 may have a circular disk shape when viewed in a plan view, i.e., from a direction perpendicular to the surface 12. However, the shape is not limited to a disk and may be any shape, such as a polygonal plate such as a rectangle. Note that the above shapes also include those having a notch or orientation flat provided on the outer periphery.
[0050] Furthermore, the thickness D of the glass 10, i.e., the length between the surface 12 and the surface 14, is preferably 0.1 mm or more and 5.0 mm or less, more preferably 0.1 mm or more and 2.0 mm or less, and even more preferably 0.1 mm or more and 0.5 mm or more. By setting the thickness D to 0.1 mm or more, the glass 10 can be prevented from becoming too thin, thereby suppressing breakage due to bending or impact. By setting the thickness D to 2.0 mm or less, the glass can be prevented from becoming too heavy, and by setting the thickness D to 0.5 mm or less, the glass can be further prevented from becoming too heavy.
[0051] (Glass Characteristics) Next, the characteristics of the glass 10 will be described.
[0052] (Light Transmittance) The internal transmittance of glass 10 having a thickness D of 0.7 mm for light (ultraviolet light) with a wavelength of 350 nm is preferably 30% or more, more preferably 35% or more, even more preferably 40% or more, even more preferably 45% or more, even more preferably 50% or more, even more preferably 55% or more, and even more preferably 60% or more. When the transmittance for light with a wavelength of 350 nm is within this range, ultraviolet light can be appropriately transmitted. Furthermore, when the thickness D of glass 10 is 0.7 mm, the internal transmittance for light with a wavelength of 1050 nm (infrared light) is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. When the transmittance for light with a wavelength of 1050 nm is within this range, infrared light can be appropriately transmitted. The transmittance can be measured by measuring a spectral transmittance curve using a spectrophotometer or the like.
[0053] (Liquidus Temperature) The liquidus temperature of the glass 10 is preferably less than 1400°C. The liquidus temperature of the glass 10 is more preferably 900°C or higher and 1390°C or lower, even more preferably 950°C or higher and 1330°C or lower, even more preferably 1000°C or higher and 1300°C or lower, and even more preferably 1050°C or higher and 1250°C or lower. The liquidus temperature of the glass 10 is preferably 1225°C or lower, more preferably 1210°C or lower, even more preferably 1185°C or lower, even more preferably 1175°C or lower, and even more preferably 1155°C or lower. Such a relatively low liquidus temperature facilitates production. The liquidus temperature can be evaluated by placing glass particles that pass through a sieve with a mesh width of 4.0 mm but not a sieve with a mesh width of 2.3 mm on a platinum dish, holding the particles in an electric furnace set at a predetermined temperature for one hour, and measuring the temperature at which crystals precipitate.
[0054] (Liquidus Viscosity) Liquidus viscosity log η of Glass 10 L The liquidus viscosity log η (dPa·s) of the glass 10 is preferably 1 or more and 6 or less, more preferably 1.1 or more and 5 or less, more preferably 1.2 or more and 4.5 or less, and even more preferably 1.4 or more and 5 or less. Lis preferably 1.6 or more, more preferably 1.8 or more, even more preferably 1.9 or more, even more preferably 2.1 or more, even more preferably 2.3 or more, even more preferably 2.5 or more, even more preferably 2.8 or more, even more preferably 3 or more, even more preferably 3.15 or more, even more preferably 3.25 or more, and even more preferably 3.35 or more. The liquidus viscosity refers to the viscosity of glass 10 at the liquidus temperature. Such a relatively high liquidus temperature makes production easier. The liquidus viscosity can be determined by measuring a temperature-viscosity curve using an inner cylinder rotation method or the like and calculating the viscosity at the liquidus temperature.
[0055] (Fracture toughness value) Fracture toughness value K of glass 10 IC is 0.88 MPa m 0.5 2.0MPa・m or more 0.5 Preferably, 0.90 MPa m or less 0.5 1.5MPa・m or more 0.5 More preferably, 1.0 MPa m 0.5 1.3MPa・m or more 0.5 The following is more preferable: Fracture toughness value K IC When the fracture toughness value K is within this range, breakage of the glass 10 can be suppressed. IC It can be measured using a pre-crack introduction fracture test method (SEPB method: Single-Edge-Precracked-Beam method) as defined in, for example, JIS R1607:2015 “Room temperature fracture toughness test method for fine ceramics”.
[0056] (Glass Transition Temperature) The glass transition temperature of the glass 10 is preferably 650°C or higher and 800°C or lower, more preferably 670°C or higher and 775°C or lower, and even more preferably 700°C or higher and 750°C or lower. The glass transition temperature can be measured according to the method specified in JIS R3103-3:2001 "Viscosity and viscosity fixed points of glass - Part 3: Method for measuring transition temperature by thermal expansion method."
[0057] (Density) The density of the glass 10 is 2.5 g / cm 3 4.0g / cm or more3 Preferably, 2.6 g / cm or less 3 3.8g / cm or more 3 More preferably, 2.7 g / cm or less 3 3.5g / cm or more 3 More preferably, 2.8 g / cm 3 3.3g / cm or more 3 More preferably, 2.9 g / cm 3 3g / cm or more 3 The following is even more preferred:
[0058] (Glass Manufacturing Method) Glass 10 may be manufactured by any method, but is manufactured by the following method, for example. First, raw materials such as silica sand and soda ash, which are the raw materials for the compounds contained in glass 10, are heated to a predetermined temperature (e.g., 1500°C to 1600°C) and melted. Then, the molten raw materials (glass) are refined and then formed into a plate shape in a forming step. The formed glass has the composition range of glass 10 described above based on oxides. Then, glass 10 is manufactured by subjecting the glass formed in the forming step to an annealing step. Note that the method for manufacturing glass 10 is not limited to the above and may be any method. For example, the annealing step is not essential. Furthermore, various methods can be adopted for the forming step when manufacturing glass 10, and examples thereof include a melt casting method, a downdraw method (e.g., an overflow downdraw method, a slot-down method, and a redraw method), a float method, a roll-out method, and a press method.
[0059] Next, an example of a manufacturing process when the glass 10 is used in FOWLP manufacturing will be described. In FOWLP manufacturing, a plurality of semiconductor chips are bonded to the glass 10, and the semiconductor chips are covered with a sealing material to form an element substrate. Then, the glass 10 and the element substrate are separated, and the side of the element substrate opposite the semiconductor chips is bonded to, for example, another piece of glass 10. Then, wiring, solder bumps, etc. are formed on the semiconductor chips, and the element substrate and the glass 10 are separated again. Then, the element substrate is cut into individual semiconductor chips to obtain semiconductor devices.
[0060] (Effects) As described above, glass 10 according to the first aspect of the present disclosure has a Young's modulus of 95 GPa or more, a linear thermal expansion coefficient of 5.5 ppm / °C or less, and a devitrification suppression parameter value A shown in formula (1) of 6.0 or more. According to the present disclosure, by setting the Young's modulus and linear thermal expansion coefficient within the above ranges, it is possible to suppress deflection. Here, glass 10 having a high Young's modulus and a low thermal expansion coefficient to suppress deflection may be particularly prone to crystallization and may be difficult to manufacture. In contrast, in the present disclosure, by setting the devitrification suppression parameter value A within the above range, it is possible to suppress an increase in the liquidus temperature and facilitate manufacture.
[0061] The glass 10 according to the second aspect of the present disclosure is the glass 10 according to the first aspect, 2 O 5 It is preferable that the content of is less than 0.5%. According to the present disclosure, it is possible to easily manufacture the steel while suppressing warping.
[0062] Glass 10 according to a third aspect of the present disclosure is glass 10 according to the second aspect, and preferably has a Young's modulus of 105 GPa or more and a linear thermal expansion coefficient of 5.1 ppm / ° C. or less. According to the present disclosure, it is possible to facilitate production while suppressing deflection.
[0063] The glass 10 according to a fourth aspect of the present disclosure is the glass 10 according to the first aspect, and further contains, in mole percent on an oxide basis, Ta 2 O 5 It is preferable that the content of is 0.5% or more and the devitrification suppression parameter value A is 6.4 or more. According to the present disclosure, it is possible to easily manufacture the glass while suppressing warping.
[0064] Glass 10 according to a fifth aspect of the present disclosure is glass 10 according to any one of the first to fourth aspects, comprising, in mol % on an oxide basis, SiO 2 :35%~60%, Al 2 O 3It is preferable that the resin contains: 6% to 20% of SiO2; and 13% to 28% of MgO. By ensuring that the content of each component falls within this range, the Young's modulus can be set to 95 GPa or more and the linear thermal expansion coefficient to 5.5 ppm / °C or less, thereby suppressing deflection. Note that a numerical range expressed as "to" means a numerical range that includes the numerical values before and after "to" as the lower and upper limits, and the same meaning will be used hereinafter when "to" is used.
[0065] Glass 10 according to a sixth aspect of the present disclosure is glass 10 according to any one of the first to fifth aspects, and preferably has a transmittance of 30% or more at a thickness of 0.7 mm for light with a wavelength of 350 nm. According to the present disclosure, ultraviolet light can be appropriately transmitted.
[0066] Glass 10 according to a seventh aspect of the present disclosure is glass 10 according to any one of the first to sixth aspects, and preferably has a transmittance of 80% or more at a thickness of 0.7 mm for light with a wavelength of 1,050 nm. According to the present disclosure, infrared rays can be appropriately transmitted.
[0067] Glass 10 according to an eighth aspect of the present disclosure is glass 10 according to any one of the first to seventh aspects, and preferably has N equal to or greater than 8. According to the present disclosure, such a high number of N makes it possible to increase the devitrification suppression parameter value A and facilitate production.
[0068] The glass 10 according to a ninth aspect of the present disclosure is the glass 10 according to any one of the first to eighth aspects, and is preferably used as a substrate. The glass 10 according to the present disclosure is suitably used as a substrate.
[0069] The glass 10 according to a tenth aspect of the present disclosure is the glass 10 according to the ninth aspect, and is preferably used in the manufacture of at least one of a fan-out wafer-level package and a fan-out panel-level package. The glass 10 is suitable for these applications.
[0070] Examples Next, examples will be described. Tables 1 to 5 show the properties of the glass of each example. Note that the embodiment may be modified as long as the effects of the invention are achieved.
[0071]
[0072] Example 1 In Example 1, a glass having the composition shown in Table 1 was produced. In Example 1, a raw plate having a diameter of 320 mm and a thickness of 6 mm was produced using a melt-casting method. Next, multiple plates having a diameter of 300 mm and a thickness of 3 mm were cut out from the center of the raw plate. Both sides of these plates were polished using cerium oxide as an abrasive to obtain glass having a thickness of 0.7 mm.
[0073] The glass transition temperature (°C) of the glass of Example 1 was measured. The glass transition temperature was measured by obtaining an expansion curve until the glass softened using a thermal expansion measuring device. The density (g / cm 3 ) was measured. Density was measured by the Archimedes method. Young's modulus was measured for the glass of Example 1. Young's modulus was measured based on ultrasonic propagation using an Olympus 38DL PLUS. The linear thermal expansion coefficient CTE (ppm / °C) for the glass of Example 1 was measured. Measurements were made using a NETZSCH dilatometer (DIL 402 Expedis Supreme) over a temperature range of 30°C to 300°C, and the average thermal expansion coefficient over a temperature range of 50°C to 200°C was taken as the linear thermal expansion coefficient CTE. The liquidus temperature (°C) for the glass of Example 1 was measured. The liquidus temperature was measured by placing glass particles that passed through a 4.0 mm mesh sieve but not a 2.3 mm mesh sieve on a platinum dish, holding the dish in an electric furnace set at a predetermined temperature for 1 hour, and measuring the temperature at which crystals precipitated. The liquidus viscosity for the glass of Example 1 was measured. The liquidus viscosity was measured by measuring the temperature-viscosity curve by the inner cylinder rotation method and calculating the viscosity at the liquidus temperature. IC (MPa m 0.5 The fracture toughness value K ICwas measured using the single-edge precracked beam (SEPB) method, as defined in JIS R1607:2015 "Room temperature fracture toughness test method for fine ceramics." For the glass of Example 1, the devitrification suppression parameter value A was calculated based on the composition using the above-mentioned formula (1). The number of oxides (number of components N) contained in the glass of Example 1 with a content of 0.5% or more was calculated. For the glass of Example 1, the transmittance for light with a wavelength of 350 nm and the transmittance for light with a wavelength of 1050 nm were measured. The transmittance was measured by measuring the spectral transmittance curve using an ultraviolet-visible spectrophotometer (UH4150 model, manufactured by Hitachi High-Tech Corporation). The measurement results and calculation results are shown in Table 1.
[0074] (Examples 2 to 47) In Examples 2 to 47, glasses were produced in the same manner as in Example 1, except that the glass compositions were as shown in Table 1. The measurement results and calculation results for each example are shown in Tables 1 to 5.
[0075] (Evaluation) The deflection and manufacturability of each glass example were evaluated. The deflection evaluation was performed based on the Bi-Metal warpage calculation defined in the literature by S. Timoshenko, "Analysis of Bi-Metal Thermostats," J. Opt. Soc. Am. 11 (1925) 233. FIG. 2 is a schematic diagram for explaining the deflection evaluation. Here, the amount of warpage δ is defined as the amount of vertical displacement of the edge of the glass 10, with the center of the second surface 14 used as the height reference, when the glass 10 is cooled from a high temperature of 200°C to a low temperature of 20°C during the process of molding and bonding a semiconductor substrate with resin to the first surface 12 side of the glass 10 processed into the shape of FIG. 1, as shown in FIG. 2. Specifically, the amount of warpage δ is calculated using the following equation (4):
[0076]
[0077] Here, as shown in FIG. 2, L is the length of the glass 10 in the warp direction (the horizontal direction in FIG. 2), and α 1 is the linear thermal expansion coefficient of the resin substrate 20, and α 2is the linear thermal expansion coefficient of the glass 10, and T 2 is the temperature after cooling (here 20°C), and T 1 is the temperature before cooling (here, 200°C). 1 / a 2 and h is a 1 +a 2 and n is Y 1 / Y 2 Here, a 1 is the thickness of the resin substrate 20, and a 2 is the thickness of the glass 10, and Y 1 is the Young's modulus of the resin substrate 20, and Y 2 is the Young's modulus of the glass 10. For the deflection evaluation, the resin substrate 20 to be bonded to the glass 10 was assumed to have a thickness of 0.3 mm and a Young's modulus of 31.5 GPa, taking into consideration the implementation of semiconductors. Four linear thermal expansion coefficients were assumed: 3.0 ppm / °C, 4.0 ppm / °C, 5.0 ppm / °C, and 5.5 ppm / °C. The amount of warpage δ was calculated for each case when the thickness of the glass 10 was 0.7 mm and the length L = 300 mm. The deflection was evaluated as follows: ◯ if the average absolute value of the calculated value δ for the four patterns was less than 1.672 mm; ⊚ if it was less than 1.60 mm; and × if it was 1.672 mm or greater. Furthermore, manufacturability refers to ease of manufacturing, with a liquidus temperature of less than 1400°C being evaluated as ◯ and a liquidus temperature of 1400°C or greater being evaluated as ×.
[0078] As shown in Tables 1 and 2, Examples 1 to 36, which are working examples having a Young's modulus of 95 GPa or more, a linear thermal expansion coefficient of 5.5 ppm / °C or less, and a devitrification suppression parameter value A of 6.0 or more, were evaluated as ◯ to ◎ in terms of deflection and manufacturability, indicating that they can be easily manufactured while suppressing deflection. On the other hand, Examples 37 to 47, which are comparative examples, do not satisfy the requirement of a devitrification suppression parameter value A of 6.0 or more, and therefore were evaluated as × in terms of manufacturability, indicating that they cannot be easily manufactured. Furthermore, Examples 37, 42, 43, and 45 to 48 were also evaluated as × in terms of deflection.
[0079] Although the embodiments of the present invention have been described above, the embodiments are not limited to the contents of these embodiments. Furthermore, the above-described components include those that can be easily imagined by a person skilled in the art, those that are substantially the same, and those that are within the scope of what is called equivalents. Furthermore, the above-described components can be combined as appropriate. Furthermore, various omissions, substitutions, or modifications of the components can be made without departing from the spirit of the above-described embodiments.
[0080] 10. Glass
Claims
1. A glass having a Young's modulus of 95 GPa or more, a linear thermal expansion coefficient of 5.5 ppm / °C or less, and a devitrification suppression parameter value A represented by formula (1) of 6.0 or more. Here, N is the number of oxides contained in the glass that are present at a content of 0.5% or more in mole percent based on oxides, R is the gas constant, [R x O y ] is the oxide R contained in the glass in mole percent based on oxide. x O y is the content.
2. Ta in mole percent notation based on oxide 2 O 5 The glass of claim 1 , wherein the content is less than 0.5%.
3. The glass according to claim 2, wherein the Young's modulus is 105 GPa or more and the linear thermal expansion coefficient is 5.1 ppm / °C or less.
4. Ta in mole percent notation based on oxide 2 O 5 The glass according to claim 1 , wherein the content of is 0.5% or more and the devitrification suppression parameter value A is 6.4 or more.
5. In terms of oxide mole percent, SiO 2 :35%~60%, Al 2 O 3 5. The glass according to claim 1, comprising: ZnO: 6% to 20%; MgO: 13% to 28%.
6. The glass according to any one of claims 1 to 4, which has a transmittance of light with a wavelength of 350 nm of 30% or more when the glass has a thickness of 0.7 mm.
7. The glass according to any one of claims 1 to 4, which has a transmittance of light with a wavelength of 1,050 nm of 80% or more when the glass has a thickness of 0.7 mm.
8. The glass according to any one of claims 1 to 4, wherein N is 8 or more.
9. The glass according to any one of claims 1 to 4, which is used as a substrate.
10. The glass of claim 9 for use in the manufacture of at least one of a fan-out wafer level package and a fan-out panel level package.
Citation Information
Patent Citations
Glass for information recording medium substrate
JP2000159539A
Glass composition, substrate for information recording medium using the same, information recording medium and information recorder
JP2001114531A
glass
JP2009203154A
Glass for magnetic recording medium substrates, magnetic recording medium substrate, magnetic recording medium, and glass spacer for magnetic recording / reproducing apparatuses
WO2018088563A1