Semiconductor device and electronic apparatus

The semiconductor device achieves stable TFT characteristics and miniaturization by employing a high-indium-content oxide semiconductor layer with a boron-doped impurity region and specific layer configurations, ensuring effective channel length and mobility, thereby overcoming the miniaturization challenges of high-indium-content materials.

WO2024219464A1PCT designated stage expired Publication Date: 2024-10-24IDEMITSU KOSAN CO LTD

Patent Information

Application Number
PCT/JP2024/015420
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The challenge is to provide a semiconductor device with stable thin-film transistor (TFT) characteristics using an oxide semiconductor material with an indium content of 70 atomic % or more, while ensuring a sufficient effective channel length, as high indium content can lead to difficulties in miniaturization due to optimal state uncertainties in the low-resistance impurity region.

Method used

The semiconductor device incorporates an oxide semiconductor layer with a high indium content of 70 atomic % or more, featuring a boron-doped impurity region and a channel region, along with multiple insulating and metal layers on a substrate, ensuring a threshold voltage greater than -2.4V and linear mobility of 15cm^2/Vs or more, with specific resistance and boron concentration profiles to maintain effective channel length and stability.

Benefits of technology

This configuration enables stable TFT characteristics with high mobility and appropriate threshold voltage, facilitating the miniaturization of thin-film transistors by maintaining a sufficient effective channel length and low resistance, thus addressing the miniaturization challenges associated with high indium content oxide semiconductors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015420_24102024_PF_FP_ABST
    Figure JP2024015420_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This semiconductor device includes a thin film transistor comprising, on a substrate: an oxide semiconductor layer, which comprises an impurity region containing boron as an impurity and a channel region, and in which an atomic ratio of In to all metal elements is 70 atom % or more; a plurality of insulating film layers; and a plurality of metal layers. The linear mobility μlin of the thin film transistor is 15 cm 2 / Vs or more and the threshold voltage Vth of the thin film transistor is more than –2.4 V.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor devices and electronic equipment

[0001] The present invention relates to semiconductor devices and electronic devices.

[0002] Thin film transistors (TFTs) using oxide semiconductors in their channel layers are widely used in industry. In recent years, TFTs have tended to be miniaturized, making the performance of small TFTs important. Furthermore, for example, when driving high-definition displays, high mobility and stable TFT characteristics are required. For example, Patent Literature 1 discloses that a thin film transistor having a gate electrode and an oxide semiconductor containing impurity elements in regions not overlapping with the source and drain electrodes can be obtained, resulting in a transistor with reduced parasitic resistance and a high on-current. Meanwhile, Patent Literature 2 discloses that a thin film transistor having an oxide semiconductor with a high In content (e.g., a ratio of In to all metal elements of 92 atomic %) can continue to operate for a long period of time without a decrease in mobility.

[0003] JP 2022-169558 A JP 2015-103646 A

[0004] To date, oxide semiconductors containing less than 70 atomic % indium have been widely used in industry, providing semiconductor devices with both a low-resistance impurity region and a good switching region. Meanwhile, the present applicant has provided thin-film transistors with high mobility and good TFT characteristics using oxide semiconductor materials with a high indium content of 70 atomic % (hereinafter sometimes referred to as at %) or more. However, the optimal state of the low-resistance impurity region in a thin-film transistor having an oxide semiconductor layer with a high indium content has not been discovered. For example, thin-film transistors with an oxide semiconductor layer containing a high indium content sometimes have a small effective channel length (large difference between the gate width and the effective channel length). This has made it difficult to miniaturize thin-film transistors using an oxide semiconductor layer with a high indium content, such as those disclosed in Patent Document 2.

[0005] An object of the present invention is to provide a semiconductor device having stable TFT characteristics by using an oxide semiconductor material with an indium content of 70 atomic % or more to ensure a sufficient effective channel length.

[0006] According to the present invention, the following semiconductor device and the like are provided: 1. A semiconductor device including an oxide semiconductor layer on a substrate, the oxide semiconductor layer including an impurity region containing boron as an impurity, a channel region, and an In atomic ratio of 70 atomic % or more to all metal elements, a plurality of insulating film layers, and a plurality of metal layers, and having a linear mobility μ lin is 15cm 2 / Vs or more and a threshold voltage Vth greater than -2.4 V. 2. The semiconductor device according to 1, wherein a first insulating layer, the oxide semiconductor layer, a second insulating layer, and a first metal layer are stacked in this order on the substrate. 3. The semiconductor device according to 1 or 2, wherein the atomic ratio of In to all metal elements contained in the oxide semiconductor layer is 73 atomic % or more. 4. The semiconductor device according to any of 1 to 3, wherein the oxide semiconductor layer includes a polycrystalline region. 5. The semiconductor device according to any of 1 to 4, wherein the oxide semiconductor layer includes crystal grains with a bixbyite structure. 6. The semiconductor device according to any of 1 to 5, wherein the resistivity of the impurity region is 0.05 Ωcm or less. 7. The linear mobility μ of the channel region lin is 20cm 2 7. The semiconductor device according to any one of 1 to 6, wherein the effective channel length L eff is represented by the following formula: L eff = L - (ΔL 1 +ΔL 2 ) (wherein L is the width of the gate electrode in the source electrode-drain electrode direction, and ΔL 1 is the distance from a position where a perpendicular line drawn from one end of the gate electrode toward the oxide semiconductor layer intersects with the oxide semiconductor layer to an end of a region having a carrier concentration that functions as a channel in the oxide semiconductor layer, and ΔL 2 is the distance from the position where a perpendicular line drawn from the other end of the gate electrode toward the oxide semiconductor layer intersects with the oxide semiconductor layer to the end of a region having a carrier concentration that functions as a channel in the oxide semiconductor layer. 1 and ΔL 2 9. The semiconductor device according to any one of 1 to 7, wherein one or both of the impurity regions has an average boron concentration of 5×10 18 ~5 x 10 21 cm -310. The semiconductor device according to any one of 1 to 8, wherein the first insulating layer is in contact with the impurity region of the oxide semiconductor layer, the first insulating layer has a first impurity-doped insulating film region having a thickness of up to 100 nm from the interface with the impurity region, and the average boron concentration of the first impurity-doped insulating film region is 1×10 17 ~3 x 10 21 cm -3 11. The semiconductor device according to any one of 2 to 9, wherein the second insulating layer is in contact with the impurity region on a surface of the oxide semiconductor layer opposite to a surface in contact with the first insulating layer, the second insulating layer has a second impurity-doped insulating film region, and an average boron concentration of the second impurity-doped insulating film region is 5×10 18 ~5 x 10 21 cm -3 12. The semiconductor device according to any one of 2 to 10, wherein the average boron concentration in the channel region is 5×10 18 cm -3 13. The semiconductor device according to any one of 1 to 11, wherein the second insulating layer has the second impurity-doped insulating film region and an insulating gate insulating film region. 14. The semiconductor device according to 11 or 12, wherein the average boron concentration of the gate insulating film region is 1×10 17 ~5 x 10 20 cm -3 15. The semiconductor device according to any one of 1 to 14, which is a thin film transistor. 16. An electronic circuit comprising the semiconductor device according to any one of 1 to 15. 17. An electric device, an electronic device, a vehicle, or a power plant comprising the electronic circuit according to 16.

[0007] According to the present invention, by using an oxide semiconductor material with an indium content of 70 atomic % or more and ensuring a sufficient effective channel length, a semiconductor device with stable TFT characteristics can be provided.

[0008] FIG. 1 is a cross-sectional schematic diagram for explaining an example of the configuration of a semiconductor device according to a first embodiment of the present aspect. FIG. 2 is a cross-sectional schematic diagram for explaining a modified example of an oxide semiconductor layer constituting the semiconductor device according to the present aspect. FIG. 3 is a cross-sectional schematic diagram for explaining another example of the configuration of a semiconductor device according to the second embodiment of the present aspect. FIG. 4 is a cross-sectional schematic diagram for explaining a method for manufacturing the semiconductor device according to the first embodiment shown in FIG. 1. FIG. 5 is a cross-sectional schematic diagram for explaining a method for manufacturing the semiconductor device according to the second embodiment shown in FIG. 3. FIG. 4 is a cross-sectional schematic diagram of an example of a TFT employing the configuration shown in FIG. 1 and fabricated by employing an indirect implantation type ion implantation process. FIG. 5 is a cross-sectional schematic diagram of an example of a TFT employing the configuration shown in FIG. 3 and fabricated by employing a direct implantation type ion implantation process. FIG. 6 is a cross-sectional diagram schematically showing the configuration of another example of a TFT according to the present embodiment. FIG. 7 is a cross-sectional diagram schematically showing the configuration of an apparatus having a semiconductor device according to one embodiment of the present invention. FIG. 8 is a diagram showing depth profiles of boron concentration, silicon concentration, and indium concentration of a TFT.

[0009] The ordinal numbers "first," "second," and "third" used in this specification are used to avoid confusion between components, and components that do not specify an order are not limited to the numerical order of the ordinal numbers.

[0010] In this specification and the like, the terms "film" or "thin film" and "layer" can be used interchangeably in some cases.

[0011] In the sintered body and oxide thin film of this specification and the like, the terms "compound" and "crystalline phase" can be interchangeable in some cases.

[0012] In this specification, the “oxide sintered body” may be simply referred to as the “sintered body.” In this specification, the “sputtering target” may be simply referred to as the “target.”

[0013] In this specification, "electrically connected" includes connection via "something that has some kind of electrical function." Here, "something that has some kind of electrical function" is not particularly limited as long as it allows electrical signals to be transmitted and received between the connected objects. For example, "something that has some kind of electrical function" includes electrodes, wiring, switching elements (such as transistors), resistive elements, inductors, capacitors, and other elements with various functions.

[0014] In this specification, the functions of the source and drain of a transistor may be interchanged when transistors of different polarities are used or when the direction of current flow changes during circuit operation, etc. Therefore, in this specification, the terms source and drain may be used interchangeably.

[0015] In this specification, "x to y" represents a numerical range of "not less than x and not more than y." The upper and lower limits of the numerical ranges can be combined in any combination. In addition, a combination of two or more of the individual embodiments of the present invention described below is also an embodiment of the present invention.

[0016] 1. Semiconductor Device The semiconductor device according to this embodiment has a plurality of insulating film layers, a plurality of metal layers, and at least one oxide semiconductor layer on a substrate.

[0017] In one embodiment, the semiconductor device according to this aspect has at least a first insulating layer, the oxide semiconductor layer, a second insulating layer, and a first metal layer stacked in this order on a substrate. When the semiconductor device with this stacking order is a so-called top-gate type, which does not have a metal layer functioning as a gate electrode between the oxide semiconductor layer and the substrate, the first insulating layer generally functions as a buffer layer, the second insulating layer generally functions as a gate insulating film, and the first metal layer generally functions as a gate electrode. Also, in one embodiment, the semiconductor device according to this aspect has at least a first metal layer, the first insulating layer, the oxide semiconductor layer, and a second insulating layer stacked in this order on a substrate. When the semiconductor device with this stacking order is a so-called bottom-gate type, which does not have a metal layer functioning as a gate electrode on the opposite side of the oxide semiconductor layer from the first metal layer, the first metal layer generally functions as a gate electrode, the first insulating layer generally functions as a gate insulating film, and the second insulating layer generally functions as a buffer layer.

[0018] [First Embodiment] A semiconductor device according to a first embodiment of this aspect will be described below. FIG. 1 is a schematic cross-sectional view illustrating an example of the configuration of a semiconductor device according to the first embodiment of this aspect. The semiconductor device 100 includes, on a substrate 12, a first insulating layer 13, an oxide semiconductor layer 11 stacked in contact with the first insulating layer 13, a second insulating layer 14 stacked in contact with the oxide semiconductor layer 11, a first metal layer 15 stacked in contact with a portion of the second insulating layer 14, and a second metal layer and a third metal layer (not shown) connected to the oxide semiconductor layer 11. The second metal layer and the third metal layer may be connected to the oxide semiconductor layer 11 via, for example, contact holes formed in the second insulating layer 14 and other insulating layers (not shown). The oxide semiconductor layer 11 has a channel region 11B and an impurity region 11A, and the second insulating layer 14 is stacked in contact with both the channel region 11B and the impurity region 11A.

[0019] (Oxide Semiconductor Layer) In the present embodiment, the atomic ratio of In to all metal elements contained in the oxide semiconductor layer 11 (hereinafter simply referred to as oxide semiconductor layer) ([In] / ([In]+[all metal elements other than In])×100) is 70 at% or more. The atomic ratio of In may be 71 at% or more, 73 at% or more, or 75 at% or more. As the In content ratio increases, high mobility can be obtained in semiconductor devices. If 70 at% or more of the total number of atoms of metal elements constituting the oxide semiconductor layer are In elements, sufficiently high mobility can be achieved in semiconductor devices.

[0020] The oxide semiconductor layer may be composed of a single-crystal oxide semiconductor, a polycrystalline oxide semiconductor including a polycrystalline region, an amorphous oxide semiconductor, or a microcrystalline oxide semiconductor. The oxide semiconductor layer may have two or more structures selected from the group consisting of polycrystalline, amorphous, and microcrystalline. In one embodiment, the oxide semiconductor layer used in this embodiment is preferably composed of a polycrystalline oxide semiconductor. Amorphous oxide semiconductors containing 70 atomic % or more indium tend to make it difficult to control the threshold voltage, which is the voltage required to switch a transistor. It is often difficult to form a single crystal of a single-crystal oxide semiconductor uniformly on a substrate with a relatively large area. In contrast, polycrystalline oxide semiconductors are less likely to encounter the difficulties encountered with amorphous oxide semiconductors and single-crystal oxide semiconductors.

[0021] The impurity region 11A (hereinafter simply referred to as the impurity region) contains boron as an impurity. The impurity region 11A contains boron, resulting in a low-resistance region with a resistance of, for example, 0.05 Ωcm or less. Therefore, by including the impurity region 11A and the channel region 11B, a switching region with excellent switching characteristics can be obtained. Furthermore, an oxide semiconductor layer 11 containing a high concentration of indium tends to have an increased carrier concentration in the channel region 11B. However, in the semiconductor device of this embodiment, by separating the oxide semiconductor layer 11 into the impurity region 11A containing boron as an impurity and the channel region B, Vth can be easily controlled to the positive side when the semiconductor device is operated, resulting in stable semiconductor characteristics. Furthermore, unlike other impurity elements, when forming the impurity region 11A, it is possible to appropriately select, by adjusting the implantation conditions, whether to generate electrons derived from oxygen vacancies caused by implantation of boron into the oxide semiconductor layer as carriers or to generate electrons derived from the formation of chemical bonds between boron and oxygen as carriers (or to generate both of these). That is, in the impurity region 11A formed by implanting an element other than boron, only electrons derived from oxygen vacancies become dominant carriers, but when boron is implanted as the impurity element, as described above, it is possible to supply both electrons derived from oxygen vacancies and electrons derived from the formation of chemical bonds of boron to the impurity region 11A as carriers. As a result, the gate width (L1 in FIG. 1 ) and the effective channel length L eff (L2 in Figure 1) (ΔL 1 +ΔL 2) is suppressed, and it is possible to obtain a low-resistance impurity region that has little effect on the switching region. In this specification, "gate width" means the distance from one end of the gate electrode to the other end in the source electrode-drain electrode direction (hereinafter referred to as "gate width L"). For example, in FIG. 1, the gate width L corresponds to the distance L1 from the position where a perpendicular line drawn from one end of the first metal layer 15 (gate electrode) toward the oxide semiconductor layer 11 intersects with the oxide semiconductor layer 11 to the position where a perpendicular line drawn from the other end of the first metal layer 15 (gate electrode) toward the oxide semiconductor layer 11 intersects with the oxide semiconductor layer 11. In addition, in this specification, the effective channel length L eff The effective channel region (hereinafter referred to as "effective channel region") has a carrier concentration sufficient to function effectively as a channel region, and corresponds to L2 in FIG. 1. ... 18 cm -3 It may be 1×10 or less, 17 cm -3 It may be 1×10 or less, 16 cm -3 The effective channel length L eff Is, L eff = L1 - (ΔL 1 +ΔL 2 ) is a value defined by the structure of the channel region of the semiconductor device. 1 and ΔL 2 In some cases, the values ​​are almost the same, and in other cases, the values ​​are different. 1 and ΔL 2 As will be described later, ΔL may be a positive value, 0 μm, or a negative value. 1 +ΔL 2 If the sum of the eff is smaller than the gate width L1. 1 +ΔL 2 If the sum of the eff becomes larger than the gate width L1.

[0022] In the configuration shown in FIG. 1, the channel region 11B is located directly below the first metal layer 15, and the impurity regions 11A are formed adjacent to both sides of the channel region 11B in the horizontal direction in the figure, but the positional relationship between the channel region 11B and the impurity region 11A is not limited to the configuration shown in FIG. 1, and for example, the impurity region 11A may be formed adjacent to only one side of the channel region 11B.

[0023] In addition, in the configuration shown in FIG. 1, the channel region 11B and the impurity region 11A are adjacent to each other, but the channel region 11B and the impurity region 11A do not necessarily have to be in direct contact with each other. For example, as shown in FIG. 2, another region 11C may exist between the channel region 11B and the impurity region 11A.

[0024] When multiple impurity regions exist in a semiconductor device, the impurity region closest in electrical connection distance to the target channel region is designated as the impurity region 11A (the target for boron ion measurement). In the following description, the target channel region refers to the channel region in the semiconductor device that has the smallest value for channel width x channel length. Furthermore, when impurity regions exist on the left and right sides of the target channel region, the side containing the larger amount of boron (i.e., the side with the larger volume of the impurity region) may be designated as the impurity region 11A (the target for boron ion measurement), and the other may be designated as the impurity region 11A' (the target for boron ion measurement). Furthermore, when impurity regions exist on the left and right sides of the target channel region and there is no difference in the amount of boron contained in the left and right impurity regions, the impurity region 11A (the target for boron ion measurement) and the impurity region 11A' (the target for boron ion measurement) may be arbitrarily determined. When multiple channel regions exist, the target channel region may be arbitrarily selected from the multiple channel regions. However, when a semiconductor device contains both a structural unit A in which the channel region and the impurity region are in direct contact with each other, and a structural unit B in which the channel region and the impurity region are not in direct contact with each other but another region exists between the channel region and the impurity region, the channel region of the directly contacting structural unit A is the "target channel region," and the impurity region of the directly contacting structural unit A is the "impurity region 11A (target for measuring boron ions)."

[0025] The semiconductor device of this embodiment has a linear mobility μ lin is 15cm 2 / Vs or more. lin is 15cm 2 / Vs or more, a semiconductor device with high mobility can be provided. lin is 20cm 2 / Vs or more, 30cm 2 / Vs or more, or 40 cm 2 / Vs or more is more preferable. The linear mobility of the TFT is determined from the transfer characteristics when a drain voltage of 0.1 V is applied. The method for measuring the saturated mobility of the TFT will be explained in detail in the Examples.

[0026] The semiconductor device of this embodiment has a threshold voltage (Vth) of greater than -2.40 V (greater than -2.40 V). By providing a threshold voltage (Vth) of greater than -2.40 V (greater than -2.40 V), a Vth correction circuit can be installed in the TFT to correct Vth to 0 V. When the TFT thus obtained is installed in a panel, it is possible to drive a display without uneven brightness or burn-in. The lower limit of the threshold voltage (Vth) may be -2.3 V or more, -2.25 V or more, -2.2 V or more, -2.0 V or more, or -1.0 V or more. The upper limit of the threshold voltage (Vth) may be 2.0 V or less, less than 1.5 V, 1.4 V or less, or 1.0 V or less. The threshold voltage (Vth) is preferably −2.2 V or more and 2.0 V or less, more preferably −2.0 V or more and 2.0 V or less, more preferably −2.0 V or more and 1.4 V or less, and even more preferably −1.0 V or more and 1.0 V or less. The most preferable range of the threshold voltage (Vth) is 0 V or more and 1.0 V or less. If the threshold voltage (Vth) is 0 V or more, a normally-off transistor can be provided even without a correction circuit. A method for measuring the threshold voltage (Vth) of a TFT will be described in detail in the Examples.

[0027] The average boron concentration of the impurity region 11A (hereinafter sometimes simply referred to as the impurity region) is 5×10 18 cm -3 That's it, 5 x 10 19 cm -3 That's it, 9 x 10 19 cm -3 That's it, 3 x 10 20 cm -3 or more or 5 x 10 20 cm -3 It may be 5×10 or more. 21 cm -3 Below, 3 x 10 21 cm -3 Below, 2 x 10 21 cm -3 Below, 1 x 10 21 cm -3 Below, 6 x 10 20 cm -3 Below, 3 x 10 20 cm -3or less, or 3 x 10 19 cm -3 The impurity region 11A may have an average boron concentration of 5×10 18 ~5 x 10 21 cm -3 5×10 18 ~3 x 10 21 cm -3 5×10 19 ~1 x 10 21 cm -3 may be 1×10 20 ~5 x 10 20 cm -3 The "average boron concentration" may be expressed as the number of boron atoms per unit volume (atoms / cm 3 ) means. A method for measuring the average boron concentration of the impurity region 11A will be described in detail in the Examples. By setting the average boron concentration of the impurity region 11A to be equal to or higher than the lower limit, the resistance value of the impurity region connected to the source / drain electrodes can be, for example, 0.05 Ωcm or less (more preferably 0.005 Ωcm or less), making it a region with sufficiently low resistance. Furthermore, the higher the average boron concentration of the impurity region 11A, the lower the sheet resistance of the impurity region 11A, and therefore, it is possible to suppress interference with the operation of a high-mobility semiconductor device electrically connected to the impurity region 11A. Furthermore, by setting the average boron concentration of the impurity region 11A within the above upper limit range, the penetration of boron ions into the channel region 11B is suppressed, and the phenomenon of an increase in the difference between the gate width and the effective channel length (i.e., the effective channel length L eff Therefore, by setting the average boron concentration of the impurity region 11A to a predetermined range that is equal to or greater than the above-mentioned lower limit value and equal to or less than the above-mentioned upper limit value, the semiconductor device exhibits good semiconductor characteristics, and it is possible to achieve both the effects obtained when the average boron concentration is equal to or less than the upper limit value and the effects obtained when the average boron concentration is equal to or greater than the lower limit value.

[0028] The average boron concentration of the channel region 11B (hereinafter simply referred to as the channel region) is 5×10 18 cm -3 Below, 5 x 10 18 cm -3 Less than 4 x 10 18 cm-3 Below, 3 x 10 18 cm -3 or less, or 1 x 10 18 cm -3 or less. Boron bonds with oxygen in the oxide semiconductor to supply carriers, so by setting the average boron concentration in the channel region 11B to the upper limit or less, an appropriate amount of carriers are present in the channel region, filling electron traps and making it easier to obtain a TFT with high mobility. Furthermore, the lower the average boron concentration in the channel region 11B, the more the carrier concentration in the channel region 11B is reduced, making it easier for the channel region 11B to exhibit good on / off characteristics. Furthermore, the lower the average boron concentration in the channel region 11B, the more likely Vth is to become a positive value, and therefore the semiconductor device will exhibit good semiconductor characteristics. The average boron concentration in the channel region 11B is, for example, 5×10 18 cm -3 If the concentration is less than 1×10, no particular problems are likely to occur, and the lower limit is not particularly limited. A trace amount of boron present in the channel region 11B is effective in controlling Vth in the positive direction as a component that fills oxygen vacancies. The average boron concentration in the channel region 11B is 1×10 18 ~5 x 10 18 cm -3 2×10 18 ~5 x 10 18 cm -3 2×10 18 ~4 x 10 18 cm -3 3×10 18 ~4 x 10 18 cm -3 2×10 18 ~3 x 10 18 cm -3 The method for measuring the average boron concentration in the channel region 11B will be described in detail in Examples. The lower limit of the average boron concentration in the channel region 11B is not particularly limited, but the average boron concentration in the oxide semiconductor may be 1×10 18 cm -3 The average boron concentration in the oxide semiconductor may be 1×10 or more. 18 cm -3If the concentration is less than 1×10, the concentration may be below the lower limit of measurement and may not be measurable. Furthermore, impurity ions may diffuse from the surrounding layers of the oxide semiconductor layer 11, causing the impurity concentration (e.g., boron concentration) in the oxide semiconductor layer 11 to exceed 1×10. 18 cm -3 It may be more than that.

[0029] The resistivity of the impurity region 11A of the oxide semiconductor layer 11 may be 0.05 Ωcm or less, 0.03 Ωcm or less, 0.01 Ωcm or less, or 0.005 Ωcm or less. When the resistivity of the impurity region 11A is equal to or less than the upper limit, the wiring resistance is reduced, and therefore, when a high-mobility TFT is connected to the impurity region 11A, a decrease in the mobility of the TFT can be suppressed. The lower limit of the resistivity of the impurity region 11A is not particularly limited, but may be 0.0005 Ωcm or more, or 0.001 Ωcm or more. A method for measuring the resistivity of the impurity region 11A will be described in detail in the Examples.

[0030] The sheet resistance of the impurity region 11A of the oxide semiconductor layer 11 may be 7000 Ω / □ or less, 6000 Ω / □ or less, or 5500 Ω / □ or less. By keeping the sheet resistance of the impurity region 11A at or below the upper limit, it is possible to prevent problems such as the characteristics of other TFT regions electrically connected to the impurity region 11A not being fully exhibited. The lower limit of the sheet resistance of the impurity region 11A is not particularly limited, but may be 100 Ω / □ or more, or 200 Ω / □ or more. A method for measuring the sheet resistance of the impurity region 11A will be described in detail in the Examples.

[0031] The specific resistance of an oxide semiconductor layer having a thickness of 10 nm is 0.005 Ωcm, which means that the sheet resistance is 5000 Ω / □. The specific resistance of an oxide semiconductor layer having a thickness of 30 nm is 0.015 Ωcm, which means that the sheet resistance is 5000 Ω / □. 2When the semiconductor material of the oxide semiconductor layer 11 is a semiconductor material having a mobility of 20 cm or more, the sheet resistance of the impurity region 11A may be 10,000 Ω / □ or less, preferably 3,333 Ω / □ or less, more preferably 1,000 Ω / □ or less, and further preferably 500 Ω / □ or less. 2 When the semiconductor material has a resistivity of 0.03 Ωcm or less, preferably 0.01 Ωcm or less, more preferably 0.003 Ωcm or less, and further preferably 0.0015 Ωcm or less, and the oxide semiconductor layer has a thickness of 30 nm, the resistivity of the impurity region 11A may be 0.03 Ωcm or less, more preferably 0.01 Ωcm or less, more preferably 0.003 Ωcm or less, and further preferably 0.0015 Ωcm or less. When the sheet resistance of the impurity region 11A is equal to or less than the upper limit, it is possible to prevent problems such as the characteristics of other TFT regions electrically connected to the impurity region 11A not being fully exhibited.

[0032] In addition to In, the oxide semiconductor layer may contain one or more elements selected from the group consisting of H, B, C, N, O, F, Mg, Al, Si, O, S, Cl, Ar, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Sn, Sb, Cs, Ba, Ln, Hf, Ta, W, Re, Os, Ir, Pt, Au, Pb, and Bi.

[0033] In this embodiment, the oxide semiconductor layer may consist essentially of elements selected from In, Mg, Al, Si, Zn, Ga, Mo, Sn, Ln elements (lanthanoid elements), and O. Here, "substantially" means that the oxide semiconductor layer of the semiconductor device according to this embodiment may contain other components as long as the effects of the present invention resulting from the combination of In, Mg, Al, Si, Zn, Ga, Mo, Sn, Ln, and O are achieved.

[0034] In this embodiment, a more preferred first form of the oxide semiconductor layer is one in which the metal elements are composed of In and Ga, and the atomic ratio satisfies the following formula (11): [Ga] / ([In]+[Ga])<22 at% (11). Note that the metal elements may contain inevitable impurities, and may further contain F or H in addition to O. By setting the composition in the above range, the In ratio becomes large, and Ga can be substituted into the In site at an annealing temperature of about 300°C, allowing crystallization into a bixbyite structure. Furthermore, by adding Ga, which has a strong bond with oxygen, oxygen deficiency after annealing can be suppressed, and a stable film as a semiconductor can be formed.

[0035] In this embodiment, a more preferred second form of the oxide semiconductor layer comprises a metal element, In, and one or more elements X selected from B, Al, Sc, Mg, Zn, Ti, Y, Zr, Mo, Sn, Hf, W, Nb, Ta, Ge, Si, La, Ce, Pr, Nd, Sm, Dy, Ho, Er, Tm, Yb, and Lu, where X represents a metal element other than In, and satisfies the following atomic ratio: [X] / ([In]+[X])<15 at% (12). The metal element may contain unavoidable impurities, and may further contain F or H in addition to O. By setting the composition within the above range, the In ratio increases, allowing crystallization into a bixbyite structure in which X substitutes for the In site at an annealing temperature of approximately 300°C. Furthermore, adding an element X that has a strong bond with oxygen suppresses oxygen deficiency after annealing, resulting in the formation of a stable semiconductor film.

[0036] In the present embodiment, a more preferable third form of the oxide semiconductor layer includes metal elements In, Ga, and one or more elements X selected from B, Al, Sc, Mg, Zn, Ti, Y, Zr, Mo, Sn, Hf, W, Nb, Ta, Ge, Si, La, Ce, Pr, Nd, Sm, Dy, Ho, Er, Tm, Yb, and Lu, and when a metal element other than In and Ga is an additional element X, the atomic ratios satisfy the following formulas (13) and (14): [Ga] / ([In]+[Ga]+[X])<22.5 at % (13) [X] / ([In]+[Ga]+[X])<8.0 at % (14) The metal elements may include inevitable impurities, and may further include F or H in addition to O. By setting the composition in the above range, the In ratio becomes large, and crystallization into a bixbyite structure in which Ga substitutes for the In site can be achieved at an annealing temperature of about 300° C. Furthermore, by adding an additional element X that has a strong bond with oxygen, oxygen deficiency after annealing can be further suppressed, and a stable film as a semiconductor can be formed.

[0037] In the present embodiment, a more preferable fourth form of the oxide semiconductor layer includes metal elements In, Sn, and one or more elements X selected from B, Al, Sc, Mg, Zn, Ti, Y, Zr, Mo, Hf, W, Nb, Ta, Ge, Si, La, Ce, Pr, Nd, Sm, Dy, Ho, Er, Tm, Yb, and Lu, and when a metal element other than In and Sn is defined as element X, the atomic ratios satisfy the following formulas (15) and (16): [Sn] / ([In]+[Sn]+[X])<20 at % (15) [X] / ([In]+[Sn]+[X])<8.0 at % (16) The metal elements may include inevitable impurities and may further include F or H in addition to O. By setting the composition in this range, the In ratio becomes large, and even when annealed at a low temperature such as 300°C, crystallization can be achieved into a bixbyite structure in which Sn substitutes for the In site. Sn has a large ionic radius and a large overlap of its orbital with In, so high mobility can be maintained. Furthermore, by adding an additional element X that has a strong bond with oxygen, oxygen deficiency after annealing can be further suppressed, and a stable film can be formed as a semiconductor.

[0038] In the present embodiment, a more preferable fifth form of the oxide semiconductor layer includes metal elements In, Zn, and one or more elements X selected from B, Al, Sc, Mg, Ti, Y, Zr, Mo, Hf, W, Nb, Ta, Ge, Si, La, Ce, Pr, Nd, Sm, Dy, Ho, Er, Tm, Yb, and Lu, and when a metal element other than In and Zn is element X, the atomic ratios satisfy the following formulas (17) and (18): [Zn] / ([In]+[Zn]+[X])<12 at% (17) [X] / ([In]+[Zn]+[X])<8.0 at% (18). Note that the metal elements may contain inevitable impurities and, in addition to O, F or H. By setting the composition within the above ranges, the In ratio becomes large, and crystallization into a bixbyite structure in which Zn is substituted for the In site can be achieved at an annealing temperature of about 300° C. By adding Zn, the film can be made amorphous immediately after deposition, and can be processed without leaving any residue when semiconductors are patterned with acid in the production of semiconductor devices such as TFTs. Furthermore, by adding an additional element X, which has a strong bond with oxygen, oxygen deficiency after annealing can be suppressed, and a stable film can be formed as a semiconductor.

[0039] The content (atomic ratio) of each metal element in the oxide semiconductor layer can be measured by transmission electron microscopy-energy dispersive X-ray spectroscopy (TEM-EDX) using an electron microscope. For metal elements that cannot be detected by TEM-EDX or metal elements for which the detection sensitivity is insufficient, time-of-flight secondary ion mass spectrometry (TOF-SIMS) or SIMS analysis using a sector-type dynamic secondary ion mass spectrometer can be used. Furthermore, if the above-mentioned analysis is difficult to perform, measurement can also be performed using μXPS (micro X-ray photoelectron spectroscopy) or μRBS (microbeam Rutherford backscattering spectrometry). If the above-listed analytical methods have problems with quantitative accuracy, the analytical accuracy of each analytical method can be improved by combining the above-listed analytical methods with ICP measurement using an inductively coupled plasma optical emission spectrometer and a standard oxide thin film. For example, the metal elements in the oxide semiconductor layer are identified by cross-sectional TEM-EDX, and the composition ratio (quantitative accuracy: error range of about 10 atomic %) is identified by semi-quantitative analysis. Next, using the semi-quantitative analysis results (the composition ratio identified above) as a reference value, 10 standard samples of oxide semiconductor thin films with varying composition ratios are prepared. Regarding the change in the composition ratio, any composition ratio can be selected so that the proportion of metal elements contained in the composition falls within a range of ±20 atomic percent, centered around a reference value. It is preferable to approximate other design values, such as the film thickness, to the information on the thin film being analyzed. For example, the metal elements in the oxide semiconductor layer are identified by cross-sectional TEM-EDX, and the composition ratio is identified within an error range of approximately 10 atomic percent by semi-quantitative analysis. For standard oxide thin films, the TEM-EDX measurement results can be calibrated using values ​​measured by an inductively coupled plasma optical emission spectrometry as the absolute values ​​of the composition ratio. This calibration can also be applied to two types of measurement methods, TEM-EDX and TOF-SIMS.

[0040] In one embodiment, the thickness of the oxide semiconductor layer is preferably 100 nm or less. A thickness of 100 nm or less makes it easier to control typical parameters of TFT characteristics, such as Vth and off-state current. The thickness of the oxide semiconductor layer is more preferably 80 nm or less, more preferably 50 nm or less, and even more preferably 30 nm or less. On the other hand, the thickness of the oxide semiconductor layer is, for example, 1 nm or more, and may be 5 nm or more, 10 nm or more, or 15 nm or more. By setting the thickness of the oxide semiconductor layer to 1 nm or more, high-quality crystals can be grown without being affected by the substrate material during annealing crystallization (during deposition of the oxide semiconductor layer). Furthermore, by setting the thickness of the oxide semiconductor layer to 1 nm or more, a low sheet resistance value can be easily obtained in the oxide semiconductor layer. In this specification, the thickness is measured based on a cross-sectional TEM observation image (sometimes referred to as a "cross-sectional TEM image").

[0041] 1 and 3 described later, the oxide semiconductor layer 11 is shown as a single layer, but the semiconductor device of this embodiment is not limited to this configuration. For example, the oxide semiconductor layer 11 may be configured as a multilayer structure of two or more layers. In this case, the layers may be configured of different materials or the same material.

[0042] In one embodiment, the oxide semiconductor layer contains crystal grains that are found to have a bixbyite structure in electron beam diffraction. Because the bixbyite crystal grains have a cubic crystal shape with good symmetry, degradation of TFT characteristics (mobility) can be suppressed even when the crystal grains straddle a grain boundary. A method for evaluating whether the crystal grains in the oxide semiconductor layer have a bixbyite structure will be described in detail in the examples.

[0043] (First Insulating Layer) In one embodiment, the first insulating layer 13 is in contact with the impurity region 11A of the oxide semiconductor layer 11 and has a first impurity-doped insulating film region 131 having a thickness d13 of up to 100 nm from the interface between the impurity region and the first insulating layer (see FIG. 1 ). The term "thickness up to 100 nm" refers to a thickness of 100 nm when the thickness of the first insulating layer is 100 nm or more, and refers to the total thickness of the first insulating layer when the thickness of the first insulating layer is less than 100 nm. Note that, when the first insulating layer is provided in contact with a substrate (e.g., a glass substrate) functioning as an insulating layer, the term refers to a thickness up to 100 nm in the total thickness of the first insulating layer and the substrate. Note that, when the oxide semiconductor layer is formed directly on a glass substrate functioning as an insulating layer, the glass substrate corresponds to the first insulating layer. Note that, when the thickness of the first insulating layer (insulating film and glass substrate) in contact with the oxide semiconductor layer is less than 100 nm, the term "thickness up to 100 nm" refers to the total thickness of the first insulating layer consisting of the insulating film and the glass substrate. When a metal layer is in contact with the first insulating layer (insulating film and / or glass substrate), the "thickness up to 100 nm" means the thickness up to the interface between the first insulating layer and the metal layer when the thickness of the first insulating layer up to the interface with the metal layer is 100 nm or less, and means the thickness up to 100 nm of the first insulating layer when the thickness of the first insulating layer up to the interface with the metal layer exceeds 100 nm. The average boron concentration of the first impurity-doped insulating film region 131 (hereinafter simply referred to as the first impurity-doped insulating film region) is 1×10 17 ~3 x 10 21 cm -3 The method for measuring the average boron concentration of the first impurity-doped insulating film region will be described in detail in the Examples.

[0044] The average boron concentration of the first impurity-doped insulating film region 131 is 1×10 17 cm -3 That's it, 1 x 10 18 cm -3 That's it, 1 x 10 19 cm -3 That's it, 1 x 10 20 cm -3 or more, or 1 x 10 21 cm -3 or more, and may be 3×10 21cm -3 Below, 3 x 10 20 cm -3 Below, 3 x 10 19 cm -3 or less, or 3 x 10 18 The average boron concentration of the first impurity-doped insulating film region 131 may be 1×10 18 ~3 x 10 21 cm -3 may be 1×10 19 ~3 x 10 21 cm -3 may be 1×10 19 ~3 x 10 20 cm -3 3×10 19 ~3 x 10 20 cm -3 may be 1×10 20 ~3 x 10 20 cm -3 Alternatively, the average boron concentration of the first impurity-doped insulating film region may be set to a value equal to or greater than the lower limit, thereby reducing the resistance of the impurity region 11A. Setting the average boron concentration of the first impurity-doped insulating film region to a value equal to or less than the upper limit can reduce the total amount of boron used in the ion implantation process, which is advantageous for shortening the processing time. Furthermore, if an excessive amount of boron is implanted, the implanted boron may become a scattering source, potentially increasing the resistance of the impurity region 11A. However, setting the average boron concentration of the first impurity-doped insulating film region to a value equal to or less than the upper limit can prevent such problems from occurring. By setting the average boron concentration of the first impurity-doped insulating film region 131 to a predetermined range equal to or greater than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, both the effects of setting the concentration below the upper limit and the effects of setting the concentration above the lower limit can be achieved. A method for measuring the average boron concentration of the first impurity-doped insulating film region will be described in detail in the Examples.

[0045] (Material of the First Insulating Layer) There is no particular limitation on the material for forming the first insulating layer, and any commonly used material can be selected, and a laminated film can also be used. For example, SiO 2 , SiNx, silicon oxynitride, Al 2 O 3 , Ta2 O 5 , TiO 2 , MgO, ZrO 2 , Ga 2 O 3 , GeO 2 , Nd 2 O 3 , La 2 O 3 , CeO 2 , K. 2 O, Li 2 O, Na 2 O, Rb 2 O, Sc 2 O 3 , Y 2 O 3 , HfO 2 , CaHfO 3 , PbTiO 3 ,BaTa 2 O 6 , SrTiO 3 , Sm 2 O 3 , AlN can be used. The oxidation number of each material may vary. The first insulating layer can be designed appropriately according to the type of substrate.

[0046] When the first insulating layer is an insulating substrate, the substrate can be considered as the first insulating layer. The extension of the first insulating layer in the direction perpendicular to the substrate surface is defined as up to a region where a metal layer or semiconductor layer appears on the lower side, assuming that the interface side with the oxide semiconductor layer is the upper side. When the lower metal layer or semiconductor layer is patterned in the in-plane direction of the substrate, and thus the first insulating layer is in contact with a lower insulating layer present further below, the first insulating layer is limited to a region up to the interface with the lower insulating layer.

[0047] The thickness of the first insulating layer is, for example, 10 nm or more, or may be 50 nm or more, 100 nm or more, 300 nm or more, or 500 nm or more. Setting the thickness of the first insulating layer to 10 nm or more makes it easier to ensure insulation between the underlying metal film or semiconductor layer and the oxide semiconductor layer. The upper limit of the thickness of the first insulating layer is not particularly limited, but may be, for example, 1000 nm or less, 500 nm or less, 200 nm or less, or 50 nm or less. Setting the thickness of the first insulating layer to 1000 nm or less allows a stable element shape to be obtained in the semiconductor device of this embodiment. Furthermore, when the first insulating layer is an insulating substrate or includes an insulating substrate, the upper limit of the thickness of the first insulating layer is also not particularly limited, but is generally 1000 nm or less. By setting the thickness of the first insulating layer to a predetermined range that is equal to or greater than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, it is possible to achieve both the effects obtained when the thickness is equal to or less than the upper limit and the effects obtained when the thickness is equal to or greater than the lower limit.

[0048] The first insulating layer may be a single layer film or a laminated film. When the first insulating layer is a laminated film, the preferred thickness mentioned for the first insulating layer is the thickness of the entire laminated film.

[0049] (Second Insulating Layer) In one embodiment, the second insulating layer 14 is formed in the same process as the gate insulating film (gate insulating film region 142 in FIG. 1 ) located at a position overlapping the channel region 11B of the oxide semiconductor layer, and is an insulating layer that contacts the impurity region 11A in a direction perpendicular to the surface. In one embodiment, the second insulating layer 14 contacts the impurity region 11A on the surface of the oxide semiconductor layer 11 opposite to the contact surface with the first insulating layer 13. The second insulating layer 14 is basically composed of the same constituent elements and has the same layer structure as the gate insulating film (gate insulating film region 142 in FIG. 1 ). However, the diffusion degree of the impurity component (e.g., boron ions) may differ between the region contacting the impurity region and the region contacting the channel region. When the gate insulating film (gate insulating film region 142 in FIG. 1 ) is partially etched, the film thicknesses of the gate insulating film (gate insulating film region 142 in FIG. 1 ) and the second insulating layer 14 may be different, and the second insulating layer 14 may be discontinuous with the channel region in the in-plane direction of the substrate. However, the second insulating layer 14 shares part of the configuration with layers formed in the same process (for example, the gate insulating film region 142 of the second insulating layer 14).

[0050] In one embodiment, the second insulating layer 14 has a second impurity-doped insulating film region 141, and the second impurity-doped insulating film region 141 has an average boron concentration of 5×10 18 ~5 x 10 21 cm -3 The method for measuring the average boron concentration of the second impurity-doped insulating film region 141 of the second insulating layer will be described in detail in the Examples.

[0051] The average boron concentration in the second impurity-doped insulating film region 141 of the second insulating layer 14 is 5×10 18 cm -3 That's it, 1 x 10 19 cm -3 That's it, 5 x 10 19 cm -3 or more, or 5 x 10 20 cm -3 It may be 5×10 or more. 21 cm -3 Below, 5 x 10 20 cm -3 or less, or 5 x 10 19 cm-3 The average boron concentration of the second impurity-doped insulating film region may be 5×10 19 ~5 x 10 21 cm -3 5×10 19 ~5 x 10 20 cm -3 By setting the average boron concentration of the second impurity-doped insulating film region to be equal to or greater than the lower limit, boron diffusion from the impurity region 11A to the second impurity-doped insulating film region can be suppressed, thereby obtaining more stable resistance characteristics in the impurity region 11A. By setting the average boron concentration of the second impurity-doped insulating film region to be equal to or less than the upper limit, boron diffusion from the second impurity-doped insulating film region to the impurity region 11A can be suppressed, thereby obtaining more stable resistance characteristics in the impurity region 11A. By setting the average boron concentration of the second impurity-doped insulating film region to be equal to or greater than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, it is possible to achieve both the effect of setting the average boron concentration below the upper limit and the effect of setting the average boron concentration above the lower limit.

[0052] (Material of the Second Insulating Layer) There is no particular limitation on the material for forming the second insulating layer, and any commonly used material can be selected, and a laminated film can also be used. For example, SiO 2 , SiNx, silicon oxynitride, Al 2 O 3 , Ta 2 O 5 , TiO 2 , MgO, ZrO 2 , Ga 2 O 3 , GeO 2 , Nd 2 O 3 , La 2 O 3 , CeO 2 , K. 2 O, Li 2 O, Na 2 O, Rb 2 O, Sc 2 O 3 , Y 2 O 3 , HfO 2 , CaHfO 3 , PbTiO3 ,BaTa 2 O 6 , SrTiO 3 , Sm 2 O 3 , AlN can be used. The oxidation number of each material may vary.

[0053] The thickness of the second insulating layer is, for example, 10 nm or more, and may be 50 nm or more, 100 nm or more, 200 nm or more, or 300 nm or more. By setting the thickness of the second insulating layer to 10 nm or more, the ion implantation process described later in the semiconductor device manufacturing process can be performed while suppressing exposure of the oxide semiconductor surface to the atmosphere, thereby stably obtaining an oxide semiconductor layer including the impurity region 11A and the channel region 11B having the above-described average boron concentration. The upper limit of the thickness of the second insulating layer is not particularly limited, but may be, for example, 300 nm or less, 200 nm or less, 150 nm or less, or 100 nm or less. By setting the thickness of the second insulating layer to 300 nm or less, a stable element shape can be obtained in the semiconductor device of this embodiment.

[0054] The second insulating layer may be a single layer film or a laminated film. When the second insulating layer is a laminated film, the preferred thickness mentioned for the second insulating layer is the thickness of the entire laminated film.

[0055] In one embodiment, the second insulating layer 14 having the second impurity-doped insulating film region 141 has a gate insulating film region 142. The gate insulating film region 142 is a region that functions as a gate insulating film. For example, in the example shown in FIG. 1 , the region of the second insulating layer 14 directly below the first metal layer 15 is a region that functions as a gate insulating film.

[0056] In one embodiment, the gate insulating film region 142 of the second insulating layer 14 has an average boron concentration of 1×10 17 ~5 x 10 20 cm -3 The method for measuring the average boron concentration in the gate insulating film region 142 will be described in detail in the Examples.

[0057] The average boron concentration in the gate insulating film region 142 is 1×10 17 cm -3 That's it, 1 x 10 18 cm -3 That's it, 1 x 10 19 cm -3 or more, or 1 x 10 20 cm -3 It may be 5×10 or more. 20 cm -3 Below, 5 x 10 19 cm -3 or less, or 5 x 10 18 cm -3 The average boron concentration in the gate insulating film region 142 may be 1×10 18 ~5 x 10 20 cm -3 may be 1×10 18 ~5 x 10 19 cm -3 5×10 18 ~5 x 10 19 cm -3 By setting the average boron concentration of the gate insulating film region 142 to be equal to or greater than the lower limit, the boron doped into the second impurity-doped insulating film region has a moderately continuous concentration gradient with the gate insulating film region, thereby providing a stable semiconductor device with little boron diffusion between the insulating films (between the second impurity-doped insulating film region of the second insulating layer and the gate insulating film region). By setting the average boron concentration of the gate insulating film region 142 to be equal to or less than the upper limit, a gate insulating film with excellent dielectric strength can be provided. By setting the average boron concentration of the second insulating layer to be equal to or greater than the above-mentioned lower limit and equal to or less than the above-mentioned upper limit, it is possible to achieve both the effect of setting the concentration below the upper limit and the effect of setting the concentration above the lower limit.

[0058] [Second Embodiment] A semiconductor device according to a second embodiment of this aspect will be described below. Figure 3 is a cross-sectional schematic diagram illustrating an example of the configuration of a semiconductor device according to the second embodiment of this aspect. The semiconductor device 200 includes a first insulating layer 13 on a substrate 12, an oxide semiconductor layer 11 stacked in contact with the first insulating layer 13 and having an impurity region 11A and a channel region 11B, and a second insulating layer 16 on the side opposite to the contact surface of the oxide semiconductor layer 11 with the first insulating layer 13 and in contact with the channel region 11B in the direction perpendicular to the surface. A first metal layer 15 is stacked on the second insulating layer 16, and the second insulating layer 16 and the first metal layer 15 have approximately the same width as the channel region 11B. The semiconductor device 200 also includes a second metal layer and a third metal layer (not shown) directly connected to the impurity region 11A of the oxide semiconductor layer 11.

[0059] 1 in that it does not have a second impurity-doped insulating film region on the impurity-doped region 11A. In the semiconductor device shown in Fig. 3, since there is no second impurity-doped insulating film region, the second and third metal layers (not shown) can be directly connected to the impurity region 11A of the oxide semiconductor layer 11. However, the semiconductor device according to the second embodiment is not necessarily limited to this form, and the second and third metal layers may be connected to the impurity region 11A of the oxide semiconductor layer 11 via contact holes formed in the insulating layer.

[0060] (2ΔL: gate width L and effective channel length L eff In one embodiment of the semiconductor device of this aspect (first embodiment and second embodiment), the difference between the gate width L (L1 in FIGS. 1 and 3) and the effective channel length L eff (L2 in Figures 1 and 3) (ΔL 1 +ΔL 2 ) is set to 2ΔL. Therefore, ΔL is the sum of (ΔL 1 +ΔL 2 ) / 2. Gate width L and effective channel length L effThe difference 2ΔL between the gate width L and the effective channel length L (the difference between L1 and L2 in FIGS. 1 and 3) is 3.4 μm or less, preferably 2.2 μm or less, and more preferably 2.0 μm or less. In the semiconductor device of this embodiment, boron implanted into the impurity region 11A of the oxide semiconductor layer 11 is unlikely to penetrate from the impurity region 11A to the channel region 11B. eff The difference can be reduced.

[0061] In one embodiment of the semiconductor device of this aspect (first embodiment and second embodiment), ΔL 1 and ΔL 2 Preferably, one or both of the above is 1.1 μm or less, more preferably 1.0 μm or less, still more preferably 0.9 μm or less, still more preferably 0.8 μm or less, and still more preferably 0.7 μm or less. eff = L - (ΔL 1 +ΔL 2 ) (wherein L eff is the effective channel length in the channel region (L2 in FIGS. 1 and 3), L is the width of the gate electrode in the source-drain electrode direction (L1 in FIGS. 1 and 3), and ΔL 1 is the distance from the position where a perpendicular line drawn from one end of the gate electrode 15 toward the oxide semiconductor layer 11 intersects with the oxide semiconductor layer 11 to the end of a region (effective channel region) having a carrier concentration that functions as a channel in the oxide semiconductor layer 11, and ΔL 2 is the distance from the position where the oxide semiconductor layer 11 intersects with a perpendicular line drawn from the other end of the gate electrode 15 toward the oxide semiconductor layer 11 to the end of a region (effective channel region) having a carrier concentration that functions as a channel in the oxide semiconductor layer 11.

[0062] In addition, Figures 1 and 3 show ΔL 1 and ΔL 2 This is an example where both are positive values, but ΔL 1 and ΔL 2 may be a negative value. 1 and ΔL 2An example of a semiconductor device in which ΔL can be a negative value is shown in FIG. 1 and ΔL 2 One of the values ​​may be a positive value and the other may be a negative value. The value of ΔL can be calculated or measured by the method described in the Examples.

[0063] 4 is a schematic cross-sectional view illustrating another example of the configuration of a semiconductor device according to the second embodiment of the present invention. In the semiconductor device 201 shown in FIG. 4, the second insulating layer 16 provided between the oxide semiconductor layer 11 and the first metal layer 15 is slightly wider than the first metal layer 15, and the side edges of the second insulating layer 16 protrude outward from the end faces of the first metal layer 15.

[0064] The oxide semiconductor layer 11 of the semiconductor device 201 has a channel region 11B formed in a region that overlaps with the first metal layer 15 within a region that contacts the second insulating layer 16, a region 11C formed in a region that contacts the second insulating layer 16 and protrudes outward from an end face of the first metal layer 15 (a region that contacts the second insulating layer 16 excluding the channel region 11B), and an impurity region 11A formed adjacent to the region 11C in a region that does not contact the second insulating layer 16. The boron content of the region 11C is greater than the boron content of the channel region 11B but less than the boron content of the impurity region 11A. Other than the above, the semiconductor device 201 shown in FIG. 4 has a basic configuration similar to that of the semiconductor device 200 shown in FIG. 3.

[0065] In the semiconductor device 201 shown in FIG. eff L2, which corresponds to the above, may be the total width of the channel region 11B and the regions 11C on both sides. In this case, it is the difference (L1-L2) between the gate width L1 and the effective channel length L2 (ΔL 1 +ΔL 2 ) will have a negative value.

[0066] 2. Method for Manufacturing a Semiconductor Device (Method for Manufacturing a Semiconductor Device of the First Embodiment: Indirect Implantation) The semiconductor device according to the first embodiment can be manufactured by forming an oxide thin film primarily composed of an oxide of In on a lower layer constituting the semiconductor device, such as a substrate, a buffer layer, or an insulating layer, patterning the oxide thin film into a desired shape using photolithography, and then annealing and crystallizing the oxide thin film as necessary to form an oxide semiconductor layer having an In atomic ratio of 70 atomic % or more to all metal elements (oxide semiconductor layer formation step), forming a second insulating layer covering the entire oxide semiconductor layer (second insulating film formation step), forming a metal layer on a portion of the second insulating layer (metal layer formation step), patterning the metal layer into a desired shape using photolithography, and then irradiating the second insulating layer and the metal layer with boron ions (ion implantation process). In the method for manufacturing a semiconductor device according to the first embodiment, boron ions are implanted into a portion of the second insulating layer that does not overlap with the metal layer (ion implantation process), thereby forming a second impurity-doped insulating film region. Boron ions diffuse from the second impurity-doped insulating film region to a portion of the oxide semiconductor layer that does not overlap with the metal layer, forming an impurity region. That is, the impurity region is formed in a portion of the oxide semiconductor layer by indirectly implanting boron ions into the portion of the oxide semiconductor layer via the second insulating layer. The portion of the oxide semiconductor layer that overlaps with the metal layer forms a channel region.

[0067] The steps of a method for manufacturing a semiconductor device according to the first embodiment shown in FIG. 1 will be described below with reference to FIG. 5 . The semiconductor device according to the first embodiment can be manufactured by forming an oxide thin film primarily composed of In oxide on a lower layer, such as a substrate, buffer layer, or insulating layer, and then annealing and crystallizing the film as necessary to form an oxide semiconductor layer having an In atomic ratio of 70 atomic % or more to all metal elements (oxide semiconductor layer forming step), forming a second insulating layer in contact with the oxide semiconductor layer (second insulating layer forming step), forming a metal layer on the second insulating layer on the oxide semiconductor layer (metal layer forming step), and irradiating the oxide semiconductor layer and the metal layer with boron ions (ion implantation step). In the method for manufacturing a semiconductor device according to the first embodiment, an impurity region and a channel region are formed in the oxide semiconductor layer by indirect ion implantation, in which boron ions are implanted into the oxide semiconductor layer through the second insulating layer.

[0068] In the process shown in FIG. 5, an oxide semiconductor layer 11 is formed on a first insulating layer 13 formed on a substrate 12 (FIG. 5(a)).

[0069] [First Insulating Layer Formation Step] (Deposition of First Insulating Layer) The method for forming the first insulating layer is not particularly limited. Examples of the formation method include PE-CVD, ALD, PLD, MO-CVD, RF sputtering, ICP sputtering, reactive sputtering, ICP-CVD, ion plating, a sol-gel method, a coating method, and mist CVD. Note that the gas species used in PE-CVD include silane (SiH 4 Besides, tetraethoxysilane (TEOS) can also be used.

[0070] When a sputtering method is employed, the atomic composition ratio of the first insulating layer obtained by the sputtering method reflects the atomic composition ratio of the oxide sintered body in the sputtering target. Therefore, it is preferable to form the film using a sputtering target containing an oxide sintered body having an atomic composition ratio similar to the atomic composition ratio of the desired first insulating layer. As in the case of forming an oxide thin film described below, it is preferable to use one or more gases selected from the group consisting of argon and oxygen that are substantially free of impurity gases as the sputtering gas.

[0071] The proportion of impurity gas in the sputtering gas, the preferred range of the argon purity in the sputtering gas, and the preferred range of the oxygen purity in the sputtering gas are the same as the preferred ranges for forming an oxide thin film, which will be described later.

[0072] The gas introduced during sputtering film formation (sputtering gas) is not particularly limited, but examples thereof include argon, nitrogen, oxygen, water, hydrogen, and a mixed gas containing two or more of these gases.

[0073] (Heat Treatment of First Insulating Layer) After the first insulating layer is formed, a heat treatment (annealing treatment) may be performed.

[0074] [Oxide Semiconductor Layer Formation Step] (Oxide Thin Film Formation) The method for forming an oxide thin film having an In content of 70 atomic % or more is not particularly limited, and examples thereof include DC sputtering, AC sputtering, RF sputtering, ICP sputtering, reactive sputtering, ion plating, ALD, PLD, MO-CVD, ICP-CVD, a sol-gel method, a coating method, and mist CVD. When forming a film by sputtering, the film may be formed using a planar sputtering cathode apparatus, or may be formed using a rotary sputtering cathode apparatus.

[0075] One example of a method for forming an oxide thin film is DC sputtering using a sputtering target made of an oxide sintered body in which the atomic ratio of In to all metal elements is 70 atomic % or more. The atomic composition ratio of the oxide thin film obtained by sputtering reflects the atomic composition ratio of the oxide sintered body in the sputtering target. Therefore, it is preferable to form the film using a sputtering target containing an oxide sintered body having an atomic composition ratio similar to that of the desired oxide thin film.

[0076] The target used in the sputtering method preferably contains 500 ppm or less of impurity metals, more preferably 100 ppm or less. The content of impurity metals in the target can be measured by ICP or SIMS, as in the case of the oxide semiconductor layer. The "impurities" contained in the target refer to trace elements that are mixed in raw materials or during the manufacturing process and are not intentionally added, and do not substantially affect the performance of the target or semiconductor. The "impurity metals" refer to metal elements among the elements considered as "impurities."

[0077] In this embodiment, the sputtering target may consist essentially of In and an element selected from Mg, Al, Si, Zn, Ga, Mo, Sn, Ln (lanthanoid element), and O. Here, "substantially" means that the sputtering target may contain other components in addition to the above-mentioned In, as long as the effects of the present invention resulting from the combination of In with any of Mg, Al, Si, Zn, Ga, Mo, Sn, Ln, and O are achieved. Alternatively, the sputtering target may be indium oxide composed of In and oxygen.

[0078] Similar to the oxide semiconductor layer of the semiconductor device of the present invention described above, a more preferred first form of the sputtering target in this embodiment is an oxide containing metal elements In and Ga, and the atomic ratio satisfies the following formula (11): [Ga] / ([In]+[Ga])<22 at% (11).

[0079] A second more preferred embodiment of the sputtering target is an oxide comprising a metal element In and one or more elements X selected from B, Al, Sc, Mg, Zn, Ti, Y, Zr, Mo, Sn, Hf, W, Nb, Ta, Ge, Si, La, Ce, Pr, Nd, Sm, Dy, Ho, Er, Tm, Yb, and Lu, wherein the atomic ratio of X satisfies the following formula (12), where X is a metal element other than In: [X] / ([In]+[X])<15 at% (12).

[0080] A more preferred third embodiment of the sputtering target is an oxide comprising metal elements In, Ga, and one or more elements X selected from B, Al, Sc, Mg, Zn, Ti, Y, Zr, Mo, Sn, Hf, W, Nb, Ta, Ge, Si, La, Ce, Pr, Nd, Sm, Dy, Ho, Er, Tm, Yb, and Lu, wherein when a metal element other than In or Ga is an additional element X, the atomic ratios satisfy the following formulas (13) and (14): [Ga] / ([In]+[Ga]+[X])<22.5 at% (13) [X] / ([In]+[Ga]+[X])<8.0 at% (14).

[0081] A more preferred fourth embodiment of the sputtering target is an oxide comprising metal elements In, Sn, and one or more elements X selected from B, Al, Sc, Mg, Zn, Ti, Y, Zr, Mo, Hf, W, Nb, Ta, Ge, Si, La, Ce, Pr, Nd, Sm, Dy, Ho, Er, Tm, Yb, and Lu, wherein when a metal element other than In and Sn is defined as element X, the atomic ratios satisfy the following formulas (15) and (16): [Sn] / ([In]+[Sn]+[X])<20 at% (15) [X] / ([In]+[Sn]+[X])<8.0 at% (16).

[0082] A more preferred fifth embodiment of the sputtering target is an oxide comprising metal elements In, Zn, and one or more elements X selected from B, Al, Sc, Mg, Ti, Y, Zr, Mo, Hf, W, Nb, Ta, Ge, Si, La, Ce, Pr, Nd, Sm, Dy, Ho, Er, Tm, Yb, and Lu, wherein, when a metal element other than In and Zn is element X, the atomic ratios satisfy the following formulas (17) and (18): [Zn] / ([In]+[Zn]+[X])<12 at% (17) [X] / ([In]+[Zn]+[X])<8.0 at% (18).

[0083] The oxide thin film obtained by sputtering using a sputtering target containing indium oxide as a main component may be an amorphous oxide thin film. The amorphous oxide thin film is patterned into islands by photolithography, and then heated and crystallized before forming a protective film, thereby obtaining an oxide semiconductor layer having a crystallized oxide semiconductor.

[0084] Sputtering is preferably performed using one or more gases selected from the group consisting of argon and oxygen, which are substantially free of impurity gases, as the sputtering gas. In this process, the sputtering target is preferably mounted in an RF magnetron sputtering device or a DC magnetron sputtering device and sputtered. The phrase "substantially free of impurity gases" means that no impurity gases other than the sputtering gas are actively introduced, except for adsorbed water introduced with the gas introduction, and gases (unavoidable impurity gases) that are difficult to remove from the sputtering gas, such as gases leaking from the chamber or adsorbed gases. If possible, impurities are preferably excluded from the gas (sputtering gas) introduced during sputtering film formation.

[0085] The proportion of impurity gas in the sputtering gas is preferably 0.1% by volume or less, and more preferably 0.05% by volume or less. If the proportion of impurity gas is 0.1% by volume or less, crystallization of the oxide thin film proceeds without any problems. The purity of high-purity argon and high-purity oxygen, which are examples of sputtering gases, is preferably 99% by volume or more, more preferably 99.9% by volume or more, and even more preferably 99.99% by volume or more.

[0086] The gas (sputtering gas) introduced during sputtering deposition is not particularly limited, and examples include argon, nitrogen, oxygen, water, hydrogen, and a mixed gas containing two or more of these gases. For example, when argon and oxygen are used, the oxygen partial pressure in the mixed gas is preferably greater than 0 vol% and less than 50 vol%, more preferably greater than 0 vol% and less than 20 vol%. When the oxygen partial pressure is greater than 0 vol% and less than 50 vol%, the oxide thin film easily crystallizes and becomes a semiconductor upon heating. By changing the oxygen partial pressure, the degree of oxidation of the oxide thin film, i.e., the degree of crystallization, can be adjusted. The oxygen partial pressure can be appropriately selected as needed. For example, when argon and water are used, the water pressure in the mixed gas is preferably greater than 0.03 vol% and less than 10 vol%, more preferably greater than 0.03 vol% and less than 5 vol%. When the water pressure is greater than 0.03 vol% and less than 5 vol%, the oxide thin film easily crystallizes and becomes a semiconductor upon heating. Alternatively, a mixed gas of hydrogen and oxygen may be used instead of water.

[0087] (Heat Treatment of Oxide Thin Film) After forming the oxide thin film, heat treatment may be performed before ion implantation. This heat treatment is sometimes called annealing. By performing the heat treatment, the oxide thin film is crystallized to form an oxide semiconductor layer. The heat treatment process is not particularly limited, but a hot air oven, an IR oven, a lamp annealing device, a laser annealing device, a thermal plasma device, or the like can be used. After annealing, N 2 Plasma oxidation treatment using O or O 2Alternatively, plasma oxidation treatment may be performed using a plasma oxidizing agent. The plasma oxidation treatment device is not particularly limited, but examples include PE-CVD. Heating the oxide thin film obtained by sputtering deposition in a heat treatment process can cause crystal growth (for example, crystals extending in a columnar shape relative to the underlying layer). By applying the oxide semiconductor layer deposited as described above to a small TFT, excellent electron carrier injection properties are achieved during operation, resulting in high mobility.

[0088] The temperature for the heat treatment of the oxide thin film is preferably 250° C. or higher and 500° C. or lower, more preferably 280° C. or higher and 470° C. or lower, and even more preferably 300° C. or higher and 450° C. or lower. If the heat treatment temperature after the formation of the oxide thin film is 250° C. or higher, the oxide thin film is likely to crystallize. If the heat treatment temperature after the formation of the oxide thin film is 500° C. or lower, abnormal crystal growth and enlargement of the crystal grains can be prevented, and the crystal grain size can be controlled to be small.

[0089] The heating time in the heat treatment step of the oxide thin film is preferably 0.1 hour or more and 5 hours or less, more preferably 0.3 hour or more and 3 hours or less, and even more preferably 0.5 hour or more and 2 hours or less. If the heating time in the heat treatment step is 0.1 hour or more, regions with insufficient crystallization are unlikely to be formed, and the crystallinity of the oxide thin film is likely to be high. If the heating time in the heat treatment step is 5 hours or less, it is economically advantageous. "Heating time" refers to the time during which a predetermined maximum temperature is maintained during heat treatment (retention time).

[0090] The temperature rise rate in the heat treatment step of the oxide thin film is preferably 2°C / min or more and 40°C / min or less, and more preferably 3°C / min or more and 20°C / min or less. If the temperature rise rate in the heat treatment step of the oxide thin film is 2°C / min or more, the production efficiency of the oxide thin film is improved compared to when it is less than 1°C / min. If the temperature rise rate in the heat treatment step of the oxide thin film is 40°C / min or less, the metal elements are uniformly diffused during crystallization, and crystals without metal segregation at grain boundaries can be formed. Furthermore, the temperature rise rate in the heat treatment step is different from the value calculated from the set temperature and set time of the furnace, and is the value obtained by dividing the actual temperature of the oxide thin film by time. The actual temperature of the oxide thin film can be determined, for example, by measuring an area within 1 cm of the oxide thin film in the furnace with a thermocouple.

[0091] The heat treatment process for the oxide thin film is preferably carried out in an air atmosphere with a humidity of 10% or more at 25° C. By performing the heat treatment process in an air atmosphere with a humidity of 10% or more, hydrogen and oxygen can be diffused into the film during annealing, thereby promoting crystallization.

[0092] The heat treatment process for the oxide thin film is preferably carried out after patterning the oxide thin film. By carrying out the heat treatment after patterning, crystallization can be promoted while removing excess oxygen present in the film during film formation and organic substances that adhere during patterning. As a result, a film with few crystal defects and no organic substances or excess oxygen within the crystal grains can be formed, and an oxide thin film with few electron traps and good conductivity can be formed.

[0093] Crystal defects in oxide thin films after heat treatment can be evaluated by defect analysis such as cathodoluminescence (CL). When there are many defects due to oxygen, strong 680 nm light emission is detected. To obtain an oxide thin film with few electron traps and good conductivity, it is necessary to adjust the film formation method and annealing conditions so that a film quality in which CL emission is as low as possible is obtained.

[0094] The heat treatment process for the oxide thin film may be performed multiple times. For example, the heat treatment process (first heat treatment process) described above may be performed after patterning the oxide thin film, followed by a heat treatment process (second heat treatment process) after forming the gate insulating film, and finally a heat treatment process (third heat treatment process) may be performed as a final process after fabricating the TFT element. The third heat treatment process is preferably performed at a lower annealing temperature than the first heat treatment process.

[0095] [Second insulating layer forming step] A second insulating layer 14 is formed on the surface of the oxide semiconductor layer 11 (FIG. 5B). The second insulating layer 14 will become a layer having a region that functions as a gate insulating film in the final semiconductor device.

[0096] (Deposition of Second Insulating Layer) The second insulating layer can be formed by the same method as described in the step of forming the first insulating layer.

[0097] (Heat Treatment of Second Insulating Layer) After the second insulating layer is formed, a heat treatment (annealing treatment) may be performed.

[0098] The temperature of the heat treatment after the formation of the second insulating layer is not particularly limited, but may be, for example, 200 to 500°C, or 300 to 400°C.

[0099] The heating time in the heat treatment step after the formation of the second insulating layer is not particularly limited, but may be, for example, 0.1 to 5 hours, or 0.5 to 1 hour.

[0100] The temperature rise rate in the heat treatment step after the formation of the second insulating layer is preferably 2° C. / min or more and 40° C. / min or less, and more preferably 3° C. / min or more and 20° C. / min or less. The method for determining the temperature rise rate in the heat treatment step after the formation of the second insulating layer is the same as the method for determining the temperature rise rate in the heat treatment step of the oxide film described above.

[0101] The heat treatment step after the formation of the second insulating layer is preferably carried out in an air atmosphere at 25° C. and a humidity of 10% or more.

[0102] [First Metal Layer Formation Step] A first metal layer 15 is formed on a portion of the surface of the second insulating layer 14 ( FIG. 5C ). The first metal layer can be formed by depositing a layer of a metal such as Al, Ag, Cu, Cr, Ni, Co, Mo, Au, Ti, Zr, Ru, Y, Nb, Ta, or W, or an alloy containing two or more of these metals, over the entire surface of the second insulating layer by a method such as sputtering, and then patterning the layer by a method such as photolithography, to form a shape that covers only a portion of the second insulating layer 14. By forming the first metal layer 15 by patterning, regions are formed in which portions of the second insulating layer 14 and the oxide semiconductor layer 11 overlap with (cover only a portion of) the first metal layer 15.

[0103] [Ion Implantation Process] As shown in FIG. 5(d), boron ions are irradiated toward the second insulating layer 14 and the first metal layer 15. As a result, the first metal layer 15 acts as a mask, and boron ions are implanted into the region of the second insulating layer 14 that is not covered with the first metal layer 15. The boron ions are implanted through the second insulating layer 14 into the region of the oxide semiconductor layer 11 that is not covered with the first metal layer 15. Meanwhile, the implantation of boron ions into the region of the oxide semiconductor layer 11 that is covered with the first metal layer 15 is suppressed. As a result, an impurity region 11A having a predetermined average boron concentration is formed mainly in the region of the oxide semiconductor layer 11 that is not covered with the first metal layer 15, and a channel region 11B is formed in the region of the oxide semiconductor layer 11 that is mainly covered with the first metal layer 15 (FIG. 5(e)). The boron ions are implanted using, for example, BF 3 This can be done by mass-separating boron ions from an ion source (gas source) such as a gas, and irradiating the boron ions. The ion source can be, for example, BF 3 Gas, BH 3 Gaseous boron such as a gas may be used, or solid boron may be used. Preferably, BF 3 It is a gas. 3 When boron ion irradiation is performed using a gas as an ion source, a small amount of fluorine (F) may be mixed into the irradiated body (for example, the second insulating layer).

[0104] During the ion implantation process, some of the boron ions irradiated onto the surface of the second insulating layer 14 are implanted into the oxide semiconductor layer 11 to form the impurity region 11A, while some remain in the second insulating layer 14 to form the second impurity-doped insulating film region 141 (see FIG. 1).

[0105] A portion of the boron ions irradiated onto the surface of the second insulating layer 14 during the ion implantation process and implanted into the impurity region 11A of the oxide semiconductor layer 11 may diffuse into the channel region 11B of the oxide semiconductor layer 11 and the region of the second insulating layer 14 that functions as the gate insulating film 142 during the ion implantation process or the heat treatment described later. A portion of the boron ions implanted into the impurity region 11A during the ion implantation process or the heat treatment described later may diffuse into the first insulating layer 13 and form a first impurity-doped insulating film region 131 (see FIG. 1 ).

[0106] The dose of boron ions in the indirect ion implantation process is 0.05×10 15 ions / cm 2 Above, 0.1 x 10 15 ions / cm 2 Above, 0.2 x 10 15 ions / cm 2 or more, or 0.3 x 10 15 ions / cm 2 or more, 8.0 × 10 15 ions / cm 2 Below, 6.0 x 10 15 ions / cm 2 or less, or 4.0 x 10 15 ions / cm 2 By setting the dose of boron ions in the indirect ion implantation process to fall within the above range, an impurity region having an appropriate resistance value can be formed in the oxide semiconductor layer 11 .

[0107] The beam energy of the indirect ion implantation process may be 0.1 keV to 1000 keV, 1 keV to 500 keV, or 5 keV to 100 keV.

[0108] The suitable beam energy for the indirect ion implantation process can be determined depending on, for example, the material and film thickness of the second insulating layer, the material and film thickness of the impurity region 11A of the oxide semiconductor layer 11, and the interrelationship with the ion implantation species. For example, the suitable beam energy can be calculated using TRIM, which is software capable of simulating the ion implantation process by the Monte Carlo method. Specifically, when the material of the second insulating layer is SiO 2 (density 2.32g / cm 3 ), the film thickness is 50 nm, and the material forming the impurity region 11A is indium oxide (density 7.18 g / cm 3 ), when the film thickness is 30 nm, the beam energy of the boron ion implantation process is preferably about 20 keV. 2 When the film thickness is changed to 110 nm, 150 nm, and 200 nm, the beam energies suitable for the ion implantation process in each case are approximately 30 keV, 40 keV, and 50 keV, respectively.

[0109] When performing the ion implantation process, the substrate 12 of the stacked structure to be ion implanted or the entire stacked structure may be heated. The temperature of the substrate 12 of the stacked structure during the indirect ion implantation process may be 15 to 450°C, 20 to 450°C, 50 to 450°C, 100 to 400°C, 150 to 400°C, or 200 to 300°C. By performing the ion implantation of boron ions while heating the substrate 12 of the stacked structure or the entire stacked structure, the resistance value of the impurity region can be reduced to a value at which good semiconductor characteristics can be obtained with a smaller dose than at room temperature.

[0110] After the indirect ion implantation process, the stacked structure may be heat-treated. The temperature for the heat treatment of the stacked structure may be 100 to 400°C, 200 to 350°C, or 250 to 300°C. The heat treatment time may be 0.1 to 5 hours, 0.3 to 3 hours, or 0.5 to 2 hours. By performing the heat treatment at a temperature within the above range, it becomes easier to obtain a state in which boron ions are uniformly diffused throughout the entire impurity region. Furthermore, by the heat treatment (annealing) after the ion implantation process, the boron ions in the impurity region 11A diffuse and penetrate into the channel region 11B, thereby reducing the effective channel length L eff is eroded, and ΔL (gate width L and effective channel length L eff However, by setting the annealing conditions within the above range, the increase in ΔL can be suppressed.

[0111] When heat treatment is performed after the indirect ion implantation process, it is preferable to pattern a part of the second insulating layer 14 and perform the heat treatment with a part of the impurity region 11A exposed. By performing the heat treatment with a part of the impurity region 11A exposed, excess boron ions among the boron ions implanted into the impurity region 11A are released to the outside from the exposed region of the impurity region 11A, thereby suppressing the diffusion of boron ions from the impurity region 11A to the channel region 11B. Therefore, the threshold voltage V th The potential is likely to be maintained near 0 V. Alternatively, after forming contact holes before performing the indirect ion implantation process, ions may be irradiated onto regions other than the contact holes to perform the ion implantation process, and then annealing may be performed.

[0112] The heat treatment after the ion implantation process may be performed in a vacuum, in an inert gas (nitrogen, rare gas, etc.) atmosphere, or in a nitrogen atmosphere. Preferably, the heat treatment is performed in an inert gas (nitrogen, rare gas, etc.) atmosphere with an oxygen concentration of about 20%, and more preferably in an air atmosphere with a humidity of about 40%. By performing the heat treatment in an atmosphere containing a moderate amount of oxygen or water, excess boron ions implanted into each layer of the stacked structure react with oxygen or water entering from outside the stacked structure, making them more likely to be desorbed to the outside of the stacked structure. When the heat treatment is performed with a portion of the impurity region 11A exposed, the reaction between the boron ions and oxygen, water, etc., tends to proceed more easily near the exposed region of the impurity region 11A.

[0113] (Method for Manufacturing Semiconductor Device of Second Embodiment: Direct Implantation) The semiconductor device according to the second embodiment can be manufactured by, for example, forming an oxide thin film containing an oxide of In as a main component on a lower layer constituting the semiconductor device, such as a substrate, a buffer layer, or an insulating layer, patterning the oxide thin film into a desired shape using photolithography, and then annealing it as necessary to perform a crystallization treatment to form an oxide semiconductor layer in which the atomic ratio of In to all metal elements is 70 atomic % or more (oxide semiconductor layer forming step), forming a second insulating layer on the surface of the oxide semiconductor layer so as to cover the entire oxide semiconductor layer (second insulating layer forming step), forming a metal layer on a part of the second insulating layer on the oxide semiconductor layer (metal layer forming step), patterning the metal layer into a desired shape using photolithography, removing parts of the second insulating layer that do not overlap with the metal layer to expose the surface of the oxide semiconductor layer in parts that do not overlap with the metal layer (insulating layer removing step), and irradiating the oxide semiconductor layer and the metal layer with boron ions in this state (ion implantation processing step). In the method for manufacturing a semiconductor device according to the second embodiment, the surface of the oxide semiconductor layer portion exposed in the second insulating layer removal step is directly irradiated with boron ions. As a result, boron ions are directly implanted into the exposed oxide semiconductor layer portion, forming an impurity region in the oxide semiconductor layer. The portion of the oxide semiconductor layer that overlaps with the metal layer forms a channel region.

[0114] The first insulating layer forming step, the oxide semiconductor layer forming step ( FIG. 6( a) ), the second insulating layer forming step ( FIG. 6( b) ), and the metal layer forming step ( FIG. 6( c) ) in the method for manufacturing a semiconductor device according to the second embodiment can be performed in the same manner as described in the method for manufacturing a semiconductor device according to the first embodiment. Therefore, only the steps that are different from the method for manufacturing a semiconductor device according to the first embodiment will be described below. Each step in the method for manufacturing a semiconductor device according to the second embodiment shown in FIG. 3 will be described below with reference to FIG. 6 .

[0115] [Insulating Layer Removal Step] The step of removing a portion of the second insulating layer ( FIG. 6( d) ) can typically be performed by photolithographically patterning the metal layer formed on the surface of the second insulating layer 14 in the preceding metal layer formation step, and then photolithographically patterning the second insulating layer 14 using the same photoresist film. Note that a photoresist film different from the one used to pattern the metal layer may also be used. This exposes the surface of the oxide semiconductor layer in the region where the second insulating layer has been removed.

[0116] [Ion Implantation Treatment Step] Boron ions are irradiated toward the oxide semiconductor layer 11 and the metal layer 15, so that the boron ions are directly irradiated and implanted into the exposed surface regions of the oxide semiconductor layer 11 ( FIG. 6( e) ). On the other hand, the metal layer 15 acts as a mask and boron ions are not directly implanted into the regions of the oxide semiconductor layer 11 that are covered with the metal layer 15. As a result, an impurity region 11A having a predetermined average boron concentration is formed in the region of the oxide semiconductor layer 11 that is not covered with the metal layer 15, and a channel region 11B is formed in the region of the oxide semiconductor layer 11 that is covered with the metal layer 15 ( FIG. 6( f) ).

[0117] Some of the boron ions implanted into the exposed oxide semiconductor layer 11 during the ion implantation process diffuse into the first insulating layer 13 during the ion implantation process or during a heat treatment described later. The boron ions diffused into the first insulating layer 13 during the ion implantation process or during a heat treatment described later form a first impurity-doped insulating film region 131 (see FIG. 3 ).

[0118] The dose of boron ions in the direct implantation ion implantation process is 0.05×10 15 ions / cm 2 Above, 0.1 x 10 15 ions / cm 2 Above, 0.2 x 10 15 ions / cm 2 or more, or 0.3 x 10 15 ions / cm 2 or more, 6.0 × 10 15 ions / cm 2 Below, 4.0 x 10 15 ions / cm 2 or less, or 2.0 x 10 15 ions / cm 2 By setting the dose of boron ions in the direct ion implantation process to fall within the above range, an impurity region having an appropriate resistance value can be formed in the oxide semiconductor layer 11 .

[0119] The beam energy of the direct implantation ion implantation process may be between 0.1 keV and 1000 keV, between 1 keV and 500 keV, or between 5 keV and 100 keV.

[0120] The optimum beam energy for the direct implantation type ion implantation process can be determined, for example, depending on the material and film thickness of the impurity region 11A of the oxide semiconductor layer 11, and the interrelationship with the ion implantation species. For example, the optimum beam energy can be calculated using TRIM, which is software capable of simulating the ion implantation process by the Monte Carlo method. Specifically, when the material for forming the impurity region 11A is indium oxide (density 7.18 g / cm 3 ), when the film thickness is 30 nm, the beam energy of the boron ion implantation process is preferably about 5 keV.

[0121] In the case of the direct implantation type, as in the case of the indirect implantation type, the substrate 12 of the laminated structure to be ion implanted or the entire laminated structure may be heated during the ion implantation process. The temperature of the substrate 12 of the laminated structure during the direct implantation ion implantation process may be 15 to 450°C, 20 to 450°C, 50 to 450°C, 100 to 400°C, 150 to 400°C, or 200 to 300°C.

[0122] In the case of direct ion implantation, as in the case of indirect ion implantation, the stacked structure may be heat-treated after the ion implantation. The suitable temperature range, heat treatment time range, and heat treatment atmosphere for the heat treatment of the stacked structure after the ion implantation can be the same as the suitable temperature range, heat treatment time range, and heat treatment atmosphere for the heat treatment after the indirect ion implantation. The reasons why these ranges and atmospheres are suitable are also the same as those explained for the heat treatment after the indirect ion implantation.

[0123] 5 and 6, an ion implantation process is performed in which ions are irradiated onto the second insulating layer or the oxide semiconductor layer using a metal layer formed on the second insulating layer as a mask. However, the semiconductor device manufacturing method of this embodiment is not necessarily limited to this method. For example, the ion implantation process may be performed using a photolithography resist as a mask instead of a metal layer.

[0124] 3. Thin Film Transistor (TFT) The semiconductor device according to this embodiment can be suitably used for a TFT. In one embodiment, the TFT includes a buffer layer, a channel layer stacked on and in contact with the buffer layer, a source electrode and a drain electrode connected to the channel layer, and a gate electrode stacked on the channel layer via a gate insulating film, wherein the channel layer is an oxide semiconductor layer included in the semiconductor device of the present invention, the gate insulating film is a gate insulating film region of the second insulating layer included in the semiconductor device of the present invention, the buffer layer is the first insulating layer included in the semiconductor device of the present invention, the source electrode and the drain electrode are the second metal layer and the third metal layer included in the semiconductor device of the present invention, and the gate electrode is the first metal layer included in the semiconductor device of the present invention.

[0125] 7, which will be described later, shows a configuration in which a source electrode and a drain electrode are connected to the impurity regions on both ends of the oxide semiconductor layer, and a region in contact with the lower surface of the gate insulating film is a channel region. That is, a region that functions as a gate insulating film is formed on the channel region, and a source electrode and a drain electrode are formed in the impurity region.

[0126] The TFT according to this embodiment can be configured as, for example, a known configuration. The TFT according to this embodiment can be manufactured by employing the semiconductor device manufacturing method described above. Specifically, the manufacturing method includes an oxide semiconductor layer formation process including a step of forming an oxide thin film by sputtering using a sputtering target and one or more gases selected from the group consisting of argon, nitrogen, hydrogen, water, and oxygen, substantially free of impurity gases, as a sputtering gas (sometimes referred to as an oxide thin film formation process), and a step of heat-treating the oxide thin film (sometimes referred to as an oxide thin film heat-treatment process). It also includes a second insulating layer formation process of forming a second insulating layer in contact with the oxide semiconductor layer, a metal layer formation process on the oxide semiconductor layer, and a step of irradiating the oxide semiconductor layer and the metal layer with boron ions to form an impurity region and a channel region (an ion implantation process). The source electrode, the drain electrode, and the buffer layer can be formed using known materials and methods.

[0127] In this specification, the mobility when Vd = 0.1 V is applied is defined as the linear mobility. Specifically, the mobility can be calculated by creating a transfer characteristic Id-Vg graph when Vd = 0.1 V is applied, calculating the transconductance (Gm) for each Vg, and using the equation for the linear region to find the mobility. In the following description, the current Id is the current between the source electrode and the drain electrode, the voltage Vd is the voltage applied between the source electrode and the drain electrode (drain voltage), and the voltage Vg is the voltage applied between the source electrode and the gate electrode (gate voltage).

[0128] The shape of the thin film transistor according to this embodiment is not particularly limited, but is preferably a top gate type transistor, a back channel etch type transistor, an etch stopper type transistor, etc. Furthermore, these transistors may be self-aligned type.

[0129] Hereinafter, embodiments will be described with reference to the drawings, etc. However, it will be readily understood by those skilled in the art that the embodiments can be implemented in many different ways and that various changes in form and details can be made without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the following description of the embodiments.

[0130] In the drawings, sizes, layer thicknesses, regions, etc. may be exaggerated for clarity. Therefore, the present invention is not limited to the illustrated sizes, layer thicknesses, regions, etc. Note that the drawings are schematic illustrations of ideal examples, and the present invention is not limited to the shapes, values, etc. shown in the drawings.

[0131] 7 is a schematic cross-sectional view of an example of a TFT having the configuration shown in FIG. 1 and fabricated using an indirect ion implantation process. The TFT 60 is a top-gate TFT and includes a substrate 21, a buffer layer (first insulating layer) 22, a channel layer (oxide semiconductor layer) 11, a second insulating layer 26-1 having a gate insulating film (gate insulating film region) 24, a gate electrode (first metal layer) 25, an interlayer insulating film 26-2, a source electrode 27, a drain electrode 28, and a protective film 29. In the TFT shown in FIG. 7, the region of the second insulating layer 26-1 below the gate electrode (first metal layer) 25 corresponds to the gate insulating film.

[0132] The TFT 60 has a structure in which a substrate 21, a buffer layer 22 (first insulating layer), and a channel layer (oxide semiconductor layer) 11 are stacked in this order. A channel region 11B is located in the center of the channel layer 11, and a gate insulating film (gate insulating film region) 24 and a gate electrode (first metal layer) 25 are stacked in this order on the channel region 11B. The gate insulating film (gate insulating film region) 24 is an insulating film that blocks conduction between the gate electrode (first metal layer) 25 and the channel layer (oxide semiconductor layer) 11. Impurity regions 11A-1 and 11A-2 are located on both sides of the channel region 11B in the oxide semiconductor layer 11. The impurity regions 11A-1 and 11A-2 are covered with a second insulating layer 26-1, and the gate electrode (first metal layer) 25 is covered with an interlayer insulating film 26-2. Specifically, ions are implanted into the oxide semiconductor layer 11 through a second insulating layer 26-1 formed in the same process as the gate insulating film, thereby forming impurity regions 11A-1 and 11A-2 in which the ion-implanted portions of the oxide semiconductor layer 11 have low resistance. Ions are less likely to be implanted into the region of the oxide semiconductor layer 11 that overlaps with the gate electrode (first metal layer) 25, resulting in a channel region 11B that does not have low resistance. A source electrode 27 is connected to the impurity region 11A-2, and a drain electrode 28 is connected to the impurity region 11A-1 through contact holes provided in the second insulating layer 26-1 and the interlayer insulating film 26-2. The source electrode 27 and the drain electrode 28 are conductive terminals for passing source current and drain current through the channel layer 11. A protective film 29 is provided to cover the TFT constituent layers, such as the interlayer insulating film 26-2, the source electrode 27, and the drain electrode 28.

[0133] 8 is a schematic cross-sectional view of an example of a TFT fabricated using a direct ion implantation process and employing the configuration shown in FIG. 3 . The TFT 52 has the same configuration as the TFT 60 shown in FIG. 7 , except that the gate insulating film 24 is configured as an independent layer between the gate electrode (first metal layer) 25 and the channel layer (oxide semiconductor layer) 11. In the TFT 52 fabricated by direct ion implantation shown in FIG. 8 , the impurity regions 11A-1 and 11A-2 are formed by ion implantation directly into the oxide semiconductor layer 11 without an interlayer insulating film, thereby forming low-resistance impurity regions 11A-1 and 11A-2 in the ion-implanted portions of the oxide semiconductor layer 11. Ions are not implanted into the region of the oxide semiconductor layer 11 that overlaps with the gate electrode (first metal layer) 25, resulting in a channel region 11B that is not low-resistance.

[0134] The TFT of this embodiment can be improved by a known configuration. For example, although not shown, in the TFTs 60 and 52, a write shield layer may be formed between the substrate 21 and the buffer layer 22, or a write shield layer may be formed as an intermediate layer in the buffer layer 22, which is made up of multiple laminated layers.

[0135] The TFTs 60 and 52 may have a second gate electrode (fourth metal layer) between the substrate 21 and the buffer layer 22, or may have the second gate electrode (fourth metal layer) as an intermediate layer in the buffer layer 22, which is formed by stacking multiple layers. Figures 9 and 10 are schematic structural diagrams of other examples of TFTs according to this embodiment. The TFTs 70 and 71 have the same structure as the TFT 60, except that a second gate electrode (fourth metal layer) 81 is provided between the substrate 21 and the oxide semiconductor layer 11. As shown in Figure 9, the second gate electrode (fourth metal layer) 81 may be provided so as not to overlap the source electrode 27 and the drain electrode 28, or as shown in Figure 10, the second gate electrode (fourth metal layer) 81 may be provided so as to overlap the source electrode 27 and the drain electrode 28 and to overlap the entire region of the oxide semiconductor layer 11 in the source electrode 27-drain electrode 28 direction. The second gate electrode (fourth metal layer) 81 may be electrically connected to the source electrode 27 or the gate electrode (first metal layer) 25, which is the first gate electrode. The second gate electrode (fourth metal layer) 81 may be a floating electrode that is not electrically connected to other metal layers, and any configuration may be used for the electrical connection between the second gate electrode (fourth metal layer) 81 and other metal layers.

[0136] 11A and 11B are schematic diagrams illustrating another example of the configuration of a TFT according to this embodiment. The TFT 72 shown in FIGS. 11A and 11B has a gate electrode (first metal layer) 25 having a laminated structure made up of a first conductive layer 25-1 and a second conductive layer 25-2, and the gate insulating film 24 and the protective film 26 have a portion of their end shapes that are curvature. The basic configuration of the TFT 72 is the same as that of the TFT 52 shown in FIG. 8.

[0137] A gate insulating film 24 and a gate electrode (first metal layer) 25 are laminated in this order on a channel region 11B in the center of the channel layer (oxide semiconductor layer) 11 of the TFT 72. A source electrode 27 and a drain electrode 28 are directly connected to impurity regions 11A-1 and 11A-2 provided on both sides of the channel region 11B in the oxide semiconductor layer 11, and a protective film 26 is provided to cover the source electrode 27, the drain electrode 28, the gate insulating film 24, and the gate electrode (first metal layer) 25.

[0138] The gate electrode (first metal layer) 25 has a structure in which the side edges of the second conductive layer 25-2 protrude outward beyond the side edges of the first conductive layer 25-1. The materials described as the material for the first metal layer can be used to form the first conductive layer 25-1 and the second conductive layer 25-2. The first conductive layer 25-1 and the second conductive layer 25-2 may be formed of different materials or the same material.

[0139] In one embodiment, the crystalline oxide semiconductor layer serving as a channel layer for the source electrode and the drain electrode has a channel length (the length in the source electrode 27-drain electrode 28 direction in the contact region between the oxide semiconductor layer 11 and the gate insulating film (gate insulating film region) 24 in FIGS. 7 and 8 ) of 1 μm or more and 50 μm or less, and a channel width (the length in the direction perpendicular to the source electrode 27-drain electrode 28 direction in the contact region between the oxide semiconductor layer 11 and the gate insulating film (gate insulating film region) 24 in FIGS. 7 and 8 ) of 1 μm or more and 80 μm or less.

[0140] The TFT of this embodiment can be improved with a known configuration.

[0141] The material for forming the substrate is not particularly limited, and any commonly used material can be selected. For example, a glass substrate, a ceramic substrate, a quartz substrate, or a sapphire substrate can be used. Alternatively, a single-crystal semiconductor substrate such as silicon or silicon carbide, a polycrystalline semiconductor substrate, a compound semiconductor substrate such as silicon germanium, or an SIO (Silicon In Insulator) substrate can also be used. These substrates on which semiconductor elements are provided may also be used as the substrate.

[0142] A flexible substrate may also be used as the substrate. As a method for providing a TFT on a flexible substrate, in addition to a method for directly fabricating a TFT on a flexible substrate, there is also a method for fabricating a TFT on a non-flexible substrate, and then peeling the TFT and placing it on a flexible substrate. In this case, it is preferable to provide a peeling layer between the non-flexible substrate and the TFT.

[0143] Various types of substrates can be used as the substrate, and are not limited to specific ones. Examples of substrates include semiconductor substrates (e.g., single crystal substrates or silicon substrates), SOI substrates, glass substrates, quartz substrates, plastic substrates, metal substrates, stainless steel substrates, substrates having stainless steel foil, tungsten substrates, substrates having tungsten foil, flexible substrates, laminated films, paper containing fibrous materials, or base films. Examples of glass substrates include barium borosilicate glass, aluminoborosilicate glass, or soda-lime glass. Examples of flexible substrates, laminated films, and base films include plastics such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polyethersulfone (PES). Examples of substrate materials include synthetic resins such as acrylic. Examples of substrate materials include polypropylene, polyester, polyvinyl fluoride, and polyvinyl chloride. Examples of substrate materials include polyamide, polyimide, aramid, epoxy, inorganic vapor-deposited film, and paper. In particular, by manufacturing transistors using a semiconductor substrate, a single-crystal substrate, an SOI substrate, or the like, it is possible to manufacture transistors with small size, high current capability, and little variation in characteristics, size, or shape. Constructing a circuit using such transistors can reduce the power consumption of the circuit or increase the circuit integration.

[0144] Alternatively, a flexible substrate may be used as the substrate, and transistors may be formed directly on the flexible substrate. Alternatively, a release layer may be provided between the substrate and the transistor. The release layer can be used to separate a semiconductor device, after it has been partially or entirely completed, from the substrate and transfer it to another substrate. In this case, the transistor can also be transferred to a substrate with poor heat resistance or a flexible substrate. The release layer may be, for example, a laminated structure of an inorganic film such as a tungsten film and a silicon oxide film, or a structure in which an organic resin film such as polyimide is formed on a substrate. Examples of substrates on which transistors may be transferred include, in addition to the substrates on which the transistors can be formed, paper substrates, cellophane substrates, aramid film substrates, polyimide film substrates, stone substrates, wood substrates, cloth substrates (including natural fibers (silk, cotton, hemp), synthetic fibers (nylon, polyurethane, polyester), or regenerated fibers (acetate, cupra, rayon, regenerated polyester), etc.), leather substrates, and rubber substrates. By using these substrates, it is possible to form transistors with good characteristics, to form transistors with low power consumption, to manufacture devices that are less likely to break, to impart heat resistance, and to reduce the weight or thickness of devices.

[0145] The buffer layer 22 may be composed of a single layer or two or more layers. A metal layer may be provided between the buffer layer 22 and the substrate 21. However, the channel layer 11 and the buffer layer 22 are preferably in direct contact with each other as shown in FIGS. 7 and 8 , and the buffer layer 22 in direct contact with the channel layer 11 corresponds to the first insulating layer. When the buffer layer 22 is composed of two or more layers, the layer of the buffer layer 22 in direct contact with the channel layer (oxide semiconductor layer) 11 is the first insulating layer.

[0146] The material for forming the buffer layer that is in direct contact with the channel layer (oxide semiconductor layer) 11 can be any of the materials described as the material for the first insulating layer.

[0147] There is no particular limitation on the material for forming the buffer layer that is not in direct contact with the channel layer (oxide semiconductor layer) 11, and any commonly used material can be selected. Also, a laminated film can be used as the buffer layer. For example, SiO 2, SiN x , silicon oxynitride, Al 2 O 3 , Ta 2 O 5 , TiO 2 , MgO, ZrO 2 , Ga 2 O 3 , GeO 2 , Nd 2 O 3 , La 2 O 3 , CeO 2 , K. 2 O, Li 2 O, Na 2 O, Rb 2 O, Sc 2 O 3 , Y 2 O 3 , HfO 2 , CaHfO 3 , PbTiO 3 ,BaTa 2 O 6 , SrTiO 3 , Sm 2 O 3 , AlN, etc. The oxidation number of each material may vary. Flexible organic resins, polyimides, etc. may also be used.

[0148] The write shield layer may be connected to either the source electrode 27 or the gate electrode 25. There are no particular restrictions on the material from which the write shield layer is formed, and any commonly used material can be selected. Specific examples include metal electrodes made of Al, Ag, Cu, Cr, Ni, Co, Mo, Au, Ti, Zr, Ru, Y, Nb, Ta, W, etc., and metal electrodes made of alloys containing two or more of these metals. A laminated electrode with two or more layers can also be used.

[0149] A second buffer layer may be provided between the write shield layer and the substrate 21. There are no particular restrictions on the material for forming the second buffer layer, and any commonly used material may be selected. A laminated film may also be used as the second buffer layer. Examples of materials for the second buffer layer include SiO 2, SiNx, silicon oxynitride, Al 2 O 3 , Ta 2 O 5 , TiO 2 , MgO, ZrO 2 , Ga 2 O 3 , GeO 2 , Nd 2 O 3 , La 2 O 3 , CeO 2 , K. 2 O, Li 2 O, Na 2 O, Rb 2 O, Sc 2 O 3 , Y 2 O 3 , HfO 2 , CaHfO 3 , PbTiO 3 ,BaTa 2 O 6 , SrTiO 3 , Sm 2 O 3 , AlN can be used. The oxidation number of each material may vary.

[0150] The material for forming the gate insulating film can be the same as that described as the material for the second insulating layer.

[0151] There is no particular limitation on the materials for forming the drain electrode, source electrode, and gate electrode, and any commonly used material can be selected. Specifically, ITO, IZO, ZnO, SnO 2 Examples of the material include transparent electrodes such as those made of Al, Ag, Cu, Cr, Ni, Co, Mo, Au, Ti, Zr, Ru, Y, Nb, Ta, and W, and metal electrodes made of an alloy containing two or more of these metals. Also, a laminated electrode having two or more layers can be used.

[0152] There is no particular limitation on the material for forming each interlayer insulating film, and any commonly used material can be selected. Also, a laminated film can be used as the interlayer insulating film. For example, SiO 2 , SiN x , silicon oxynitride, Al 2 O3 , Ta 2 O 5 , TiO 2 , MgO, ZrO 2 , Ga 2 O 3 , GeO 2 , Nd 2 O 3 , La 2 O 3 , CeO 2 , K. 2 O, Li 2 O, Na 2 O, Rb 2 O, Sc 2 O 3 , Y 2 O 3 , HfO 2 , CaHfO 3 , PbTiO 3 ,BaTa 2 O 6 , SrTiO 3 , Sm 2 O 3 , AlN, etc. The oxidation number of each material may be varied.

[0153] Regardless of the TFT structure, it is preferable to provide a protective film on the drain electrode, source electrode, and conductive region. Furthermore, in the case of a bottom gate type, it is preferable to provide a protective film on the channel layer. By providing a protective film, the durability of the TFT tends to improve even when driven for a long time.

[0154] There is no particular limitation on the method for producing the insulating films of the buffer layer, gate insulating film, interlayer insulating film, and protective film. Examples of the production method include PE-CVD, ALD, PLD, MO-CVD, RF sputtering, ICP sputtering, reactive sputtering, ICP-CVD, ion plating, the sol-gel method, the coating method, and mist CVD. The gas species used in PE-CVD include silane (SiH 4 Besides, tetraethoxysilane (TEOS) can also be used.

[0155] For example, when forming the protective film or insulating film by PE-CVD, the process may require high temperatures. Furthermore, the protective film or insulating film often contains impurity gases immediately after film formation, so it is preferable to perform a heat treatment (annealing treatment). Removing the impurity gases through heat treatment results in a stable protective film or insulating film, making it easier to form highly durable TFTs.

[0156] The S value (swing factor) is a value that indicates how steeply the drain current rises from the off state to the on state when the gate voltage is increased from the off state. The smaller the S value, the steeper the rise. If the S value is large, a high gate voltage must be applied when switching from on to off, which may increase power consumption.

[0157] The S value of the TFT is preferably 0.8 V / dec or less, more preferably 0.6 V / dec or less, more preferably 0.5 V / dec or less, and even more preferably 0.3 V / dec or less. If the S value is 0.8 V / dec or less, the driving voltage can be reduced, potentially reducing power consumption. In particular, when used in an organic EL display, which is driven by DC, an S value of 0.3 V / dec or less is preferred because it can significantly reduce power consumption. The method for measuring the S value will be described in detail in the Examples.

[0158] On-off ratio is 10 6 More than 10 is preferable. 7 More preferably, 10 or more 8 More preferably, the on-off ratio is 10 or more. 6 If the on-off ratio is 10 or more, the liquid crystal display can be driven. 8 When the on-off ratio is 10 or more, an organic EL element with high contrast can be driven. 10 or more, and the off-current is 10 -12 If the value can be reduced to A or less, it is possible to provide a display element that can be driven at a low frequency of about 1 Hz and has excellent low power consumption.

[0159] The on-off ratio is calculated by determining the ratio [on current value / off current value], where the value of Id when Vd = 10 V and Vg = -10 V is the off current value, and the value of Id when Vd = 10 V and Vg = 20 V is the on current value. -10 A or less is preferable, and 10 -11 A or less is more preferable, and 10 -12 A or less is more preferable. -10 When the resistance is A or less, it is possible to drive an organic EL device with high contrast. Furthermore, when used in the transfer transistor or reset transistor of a CMOS image sensor, it is possible to extend the image retention time and improve the sensitivity.

[0160] 12 is a cross-sectional view schematically illustrating the configuration of an apparatus having a semiconductor device according to one embodiment of the present invention. In FIG. 12, the apparatus 500 has a structure in which a storage capacitor 520 and an oxide semiconductor TFT 530 are formed in a stacked structure 510 in which insulating films 501 and 502 corresponding to a first insulating layer, an insulating film 503 corresponding to a second insulating layer, an interlayer insulating film 504, and a planarizing film 505 are stacked in this order on a substrate (not shown). The oxide semiconductor TFT 530 corresponds to the semiconductor device of this embodiment.

[0161] The storage capacitor 520 has a lower electrode 521 provided on the insulating film 501, an upper electrode 522 provided on the insulating film 502 opposite the lower electrode 521, and an insulating region formed by the portion of the insulating film 502 between the upper electrode 522 and the lower electrode 521.

[0162] The oxide semiconductor TFT 530 includes an oxide semiconductor layer 531 provided on an insulating film 502, a gate electrode 535 provided on an insulating film 503, source / drain electrodes 536 and 537 provided to penetrate the interlayer insulating film 504 and the insulating film 503, and a gate insulating region that blocks conduction between the oxide semiconductor layer 531 and the gate electrode 535. The source / drain electrodes 536 and 537 are connected to impurity regions 533 and 534 provided on both sides of a channel region 532 of the oxide semiconductor layer 531, respectively, via contact holes provided in the third insulating film 503 and the fourth insulating film 504. The gate insulating region is formed by a portion of the third insulating film 503 between the gate electrode 535 and the channel region 532.

[0163] The source electrode / drain electrode 536, 537 of the oxide semiconductor layer 531 are provided on one end side of a series of conductor layers provided on the fourth insulating film 504, and the remaining portions of the conductor layers form a connection portion 540. The connection portion 540 is connected to the upper electrode 522 of the storage capacitor 520 via contact holes formed in the third insulating film 503 and the fourth insulating film 504. In other words, the source electrode / drain electrode 537 of the oxide semiconductor TFT 530 and the upper electrode 522 of the storage capacitor 520 are connected to each other by the connection portion 540.

[0164] The materials described as the substrate materials can be used as materials for forming the substrate (not shown). The materials described as the materials for each interlayer insulating film can be used as materials for forming the first insulating film 501, the second insulating film 502, the third insulating film 503, the fourth insulating film 504, and the planarizing film 505. The conductor layers constituting the gate electrode 535 and the lower electrode 521, and the conductor layers constituting the source / drain electrodes 536, 537, and the connecting portion 540 can be formed using the materials described as the materials for the drain electrode, source electrode, and gate electrode. The upper electrode 522 is typically formed using the materials described as the materials for the drain electrode, source electrode, and gate electrode. However, it is also possible to form the upper electrode 522 using the same material as the oxide semiconductor layer 531 and enable it to function as an electrode by ion implanting boron.

[0165] The TFT according to this embodiment can be suitably used in display elements such as solar cells, liquid crystal elements, organic electroluminescence elements, and inorganic electroluminescence elements, power semiconductor elements, touch panels, and other electronic devices.

[0166] The thin film transistor according to this embodiment can be applied to various integrated circuits such as field-effect transistors (MOSFETs, MESFETs), logic circuits, memory circuits, and differential amplifier circuits, and can be applied to electronic devices, electric devices, vehicles, powertrains, and the like. Furthermore, the thin film transistor according to this embodiment can also be applied to static induction transistors and Schottky barrier transistors in addition to field-effect transistors. The thin film transistor according to this embodiment can be suitably used in display devices such as portable or in-vehicle display devices, solid-state imaging devices, and the like. Furthermore, the thin film transistor according to this embodiment can also be suitably used as a transistor for flat panel detectors for X-ray image sensors in medical applications. The oxide semiconductor layer according to this embodiment can also be applied to Schottky diodes, resistance-change memories, and resistor elements.

[0167] The present invention will be described in detail below based on specific examples of semiconductor devices, but the present invention is not limited to these examples.

[0168] <Manufacturing of small self-aligned top-gate structure TFTs> [Examples of manufacturing TFT elements by indirect ion implantation] Examples 1 to 8, Comparative Examples 1 to 7 Thin film transistors (TFTs) were manufactured by the following process. The thin film transistors (TFTs) manufactured by the following process have the same configuration as the thin film transistor (TFT) 60 shown in FIG. 7 except that they do not have the protective film 29, and therefore will be described below using the symbols shown in FIG. 7. (1) Formation of buffer layer (first insulating layer) 22 SiO 2 A 300 nm thick SiO film was deposited on a 4-inch diameter non-alkali glass substrate 21 by sputtering using a sputtering target of x A layer (buffer layer 22) was formed.

[0169] (2) Formation of Oxide Thin Film Next, oxide thin films having the film thicknesses shown in Tables 1 to 3 were formed by sputtering using oxide sputtering targets. Materials A and B shown in the column "Materials for Oxide Semiconductor Layer" in Tables 1 to 3 were used as the oxide sputtering targets. Materials A and B are oxide sputtering targets made of oxides containing at least In and Ga.

[0170] (3) Formation of Oxide Semiconductor Layer 11 Next, the oxide thin film was patterned into islands by photolithography to form the oxide semiconductor layer 11. First, a photoresist film was formed on the oxide thin film. AZ1500 (manufactured by AZ Electronic Materials) was used as the photoresist. Exposure was performed through a photomask on which a pattern of 50 μm in width and 20 μm in length was formed. After exposure, development was performed with tetramethylammonium hydroxide (TMAH). After development, the oxide thin film was etched with oxalic acid (ITO-06N, manufactured by Kanto Chemical). After etching, the photoresist was peeled off to obtain a substrate 21 with a patterned oxide thin film (oxide semiconductor layer 11).

[0171] (4) Annealing Next, the substrate 21 on which the oxide semiconductor layer 11 was formed was placed in a furnace, and the temperature was raised to 350°C at a rate of 10°C / min in the atmosphere, and then held at that temperature for 1 hour. After the inside of the furnace was held at 350°C for 1 hour, the inside of the furnace was allowed to cool naturally, and after the temperature inside the furnace returned to room temperature, the substrate 21 was taken out of the furnace.

[0172] (5) Deposition of the second insulating layer (layer including a gate insulating film) 26-1. Next, SiO 2 The sputtering was performed using a sputtering target of 100 nm thick. x A layer (second insulating layer 26-1) was formed.

[0173] (6) Annealing of Second Insulating Layer 26-1 Next, the substrate 21 on which the second insulating layer 26-1 was formed was placed in a furnace, and the temperature was raised to 400°C at a heating rate of 10°C / min in the atmosphere, and then held for 1 hour. The inside of the furnace was held at 400°C for 1 hour, and then naturally cooled. After the temperature inside the furnace returned to room temperature, the substrate 21 was removed from the furnace.

[0174] (7) Formation of Gate Electrode 25 Next, a Mo film having a thickness of 150 nm was formed by sputtering using a Mo sputtering target.

[0175] (8) Patterning of the Gate Electrode 25 Next, the Mo film was patterned into islands by photolithography. First, a photoresist film was formed on the channel layer. AZ1500 (manufactured by AZ Electronic Materials) was used as the photoresist. Exposure was performed through a photomask with a pattern of 10 μm wide x 28 μm long. After exposure, development was performed with tetramethylammonium hydroxide (TMAH). After development, the Mo film was etched with PAN (a mixed acid of phosphoric acid, nitric acid, and acetic acid) to form the gate electrode 25.

[0176] (9) Ion Implantation Treatment Boron ions were implanted into the oxide semiconductor layer 11. The substrate on which the gate electrode 25 had been formed was placed on a sample stage of an ion implantation device, and BF ions were injected as a gas source toward the second insulating layer 26-1 and the gate electrode 25 by the ion implantation device. 3 The implantation was performed by irradiating boron ions mass-separated from a gas. The beam energy and sample stage temperature (substrate temperature) during the ion implantation process are shown in the "Beam Energy" and "Substrate Temperature During Ion Implantation" columns of Tables 1 to 3, respectively. The dose of boron ions implanted is shown in the "Dose" column of Tables 1 to 3.

[0177] Next, the substrate after the ion implantation process was placed in a furnace and annealed in the atmosphere at 300° C. for 1 hour.

[0178] (10) Formation of Interlayer Insulating Film 26-2 Next, SiO 2 A sputtering target of 150 nm thick was used for sputtering. x A layer (interlayer insulating film 26-2) was formed.

[0179] (11) Formation of Contact Holes in Second Insulating Layer 26-1 and Interlayer Insulating Film 26-2 The substrate on which the second insulating layer 26-1 and interlayer insulating film 26-2 were formed was exposed to light through a photomask using photoresist AZ1500 (manufactured by AZ Electronic Materials), and then developed with tetramethylammonium hydroxide (TMAH). After development, contact holes were formed in the second insulating layer 26-1 and interlayer insulating film 26-2 using buffered hydrofluoric acid (BHF).

[0180] (12) Formation of Source Electrode 27 and Drain Electrode 28 Next, a Mo layer having a thickness of 150 nm was formed by sputtering and patterned.

[0181] (13) Final annealing Finally, N 2 The resulting substrate was annealed at 200° C. for 1 hour in a high-temperature atmosphere to obtain a small self-aligned top-gate structure TFT device 1. Tables 1 to 3 show a summary of the TFT fabrication conditions.

[0182] Comparative Example 8 "(9) Ion Implantation Process" was performed in the same manner as in Examples 1 to 8 and Comparative Examples 1 to 7 (Examples of Manufacturing TFT Elements by Indirect Ion Implantation), except that the ions irradiated by the ion implantation device toward the second insulating layer 26-1 and the gate electrode 25 were changed from boron ions to argon ions. Otherwise, TFT elements were manufactured in the same manner as described in Examples 1 to 8 and Comparative Examples 1 to 7 (Examples of Manufacturing TFT Elements by Indirect Ion Implantation).

[0183] [Examples of TFT Element Fabrication by Direct Ion Implantation] Examples 9 to 11 and Comparative Examples 9 to 13 Thin film transistors (TFTs) were fabricated by the following process. The thin film transistors (TFTs) fabricated by the following process had the same configuration as the thin film transistor (TFT) 52 shown in FIG. 8 , except that they did not have the protective film 29. In "(8) Patterning of Gate Electrode 25," after etching the Mo film to form the gate electrode 25 and before peeling off the photoresist, the second insulating layer 26-1 was etched with buffered hydrofluoric acid (BHF) to pattern the second insulating layer 26-1. This exposed the surface of the oxide semiconductor layer 11 in a region not overlapping with the gate electrode 25, and a gate insulating film 24 consisting of the remainder of the second insulating layer 26-1 after patterning was formed between the gate electrode 25 and the oxide semiconductor layer 11. Other than this, "(8) Patterning of the gate electrode 25" was carried out in the same manner as in Examples 1 to 8 and Comparative Examples 1 to 8 (examples of manufacturing TFT elements by indirect ion implantation). Next, in "(9) Ion implantation treatment", BF as a gas source was injected by an ion implantation apparatus toward the oxide semiconductor layer 11 and the gate electrode 25 whose surfaces were partially exposed. 3 Boron ions mass-separated from a gas were irradiated onto the oxide semiconductor layer 11, thereby implanting boron ions into the oxide semiconductor layer 11. The beam energy and sample stage temperature (substrate temperature) during the ion implantation process were changed as shown in the "Beam Energy" and "Substrate Temperature During Ion Implantation" columns of Table 3, respectively, and the dose of boron ions during ion implantation was changed as shown in the "Dose" column of the table, respectively. Except for this, "(9) Ion Implantation Process" was performed in the same manner as in Examples 1 to 8 and Comparative Examples 1 to 7 (Examples of Manufacturing TFT Elements by Indirect Ion Implantation). Otherwise, TFT elements were manufactured in the same manner as described in Examples 1 to 8 and Comparative Examples 1 to 7 (Examples of Manufacturing TFT Elements by Indirect Ion Implantation).

[0184] Comparative Example 14 "(9) Ion implantation treatment" was performed in the same manner as in Examples 9 to 11 and Comparative Examples 9 to 13 (Examples of manufacturing TFT elements by direct ion implantation), except that the ions irradiated by the ion implantation device toward the oxide semiconductor layer 11 with a partially exposed surface and the gate electrode 25 were changed from boron ions to argon ions in "(9) Ion implantation treatment". In other respects, TFT elements were manufactured in the same manner as described in Examples 9 to 11 and Comparative Examples 9 to 13 (Examples of manufacturing TFT elements by direct ion implantation).

[0185] [Characteristics Evaluation] The TFTs obtained in the examples and comparative examples were evaluated as follows. The results are shown in Tables 1 to 3. In the tables, "E+XX" means "×10 XX " means.

[0186] (A) Evaluation of the oxide semiconductor layer of the TFT (a) Crystallinity (polycrystalline / amorphous) of the oxide semiconductor layer after fabrication of the TFT The crystalline state of the cross section of the oxide semiconductor layer in the TFT was evaluated by pretreating the oxide semiconductor layer using a focused ion beam (FIB) and observing the cross section of the oxide semiconductor layer with a transmission electron microscope (TEM).

[0187] Specifically, first, an ion beam was applied perpendicularly to the surface of the oxide semiconductor layer using an FIB (Hitachi High-Technologies Corporation "FB2100") device, and a 16 μm × 4 μm test piece was sampled. Then, from the sampled test piece, two samples were extracted: one from a 3 μm region extending in the channel length direction (horizontal direction in the drawing) from the edge of the region where the source electrode or drain electrode and the impurity region of the oxide semiconductor layer overlap toward the non-overlapping region, and one from a 3 μm region extending in the channel length direction (horizontal direction in the drawing) from the edge of the region where the gate electrode and the channel region of the oxide semiconductor layer overlap toward the overlapping region. The two extracted samples were subjected to Ar ion milling in the channel width direction (depth direction in the drawing), perpendicular to the channel length direction and film thickness direction, until the thickness of the flakes reached approximately 100 nm, thereby thinning the thickness of the two extracted samples. When crystal grains could not be confirmed due to ion sputter damage during FIB processing, etching was repeated using Ar ion milling (Gatan "Model 691") with an ion gun voltage of 4 keV until crystal grains could be confirmed. Cross-sectional TEM images were observed using a transmission electron microscope (JEOL "JEM-2800") with an acceleration voltage of 200 kV and a magnification of 100,000 times (an area of ​​approximately 4 μm square).

[0188] The crystalline state was determined by observing the electron beam diffraction pattern of the sample obtained by observing the cross-sectional TEM image. Specifically, using an electron microscope (JEOL "JEM-2800" model), the oxide thin film area observed in the cross-sectional TEM image was irradiated with an electron beam at an irradiation area of ​​approximately 100 nmφ and an acceleration voltage of 200 kV using a selected area aperture, and the diffraction pattern was measured with the camera length set to 2 m. An oxide thin film that did not show clear diffraction spots in any three fields of view selected so that the observation points did not overlap in the channel length direction of the cross-sectional TEM image sample was judged to be "amorphous." On the other hand, an oxide thin film in which symmetrical diffraction spots were observed in the diffraction pattern was judged to be "crystalline." Furthermore, if an oxide semiconductor layer existing parallel to the substrate surface had grain boundaries perpendicular to the substrate surface, it was judged to be "polycrystalline." As a result of the above measurements, it was confirmed that the oxide semiconductor layers of the TFTs obtained in Examples 1 to 11 and Comparative Examples 1 to 14 were polycrystalline.

[0189] (b) Identification of Crystal Structure by Electron Beam Diffraction Whether the crystal structure of the oxide semiconductor layer in the TFT is a bixbyite structure was evaluated by observing the electron beam diffraction pattern of the sample obtained by observing the cross-sectional TEM image. Specifically, using an electron microscope (JEOL Ltd. "JEM-2800 type"), the oxide thin film area observed in the cross-sectional TEM image was irradiated with an electron beam using a selected area aperture at an irradiation area of ​​approximately 100 nmφ and an acceleration voltage of 200 kV, and the camera length was set to 2 m to measure the diffraction pattern. Furthermore, to identify the crystal structure, electron beam diffraction simulation software ReciPro (free software ver. 4.641 (2019 / 03 / 04)) was used to measure the In 2 O 3A simulation of the electron diffraction pattern of the bixbyite structure was carried out. In the simulation, the crystal structure data of the bixbyite structure was 14388 from the Inorganic Crystal Structure Database (ICSD: Chemical Information Association), with a space group of Ia-3, a lattice constant of a = 10.17700 Å, and atomic coordinates of In site (0.250, 0.250, 0.250), In site (0.466, 0.000, 0.250), and O site (0.391, 0.156, 0.380). Furthermore, with a camera length of 2 m, simulations were performed using 11 types of reciprocal lattice vectors (100), (111), (110), (211), (311), (221), (331), (210), (310), (321), and (230) as the incident electron beam direction. The electron beam diffraction pattern of the oxide thin film was compared with the diffraction spot results for the obtained simulation pattern, and if it matched any of the 11 types of simulation patterns, it was determined that the oxide thin film contained crystal grains with a bixbyite structure. As a result of the above measurements, it was confirmed that the oxide thin films of the TFTs obtained in Examples 1 to 11 and Comparative Examples 1 to 14 contained crystal grains with a bixbyite structure.

[0190] (c) Average In Concentration (In Content Ratio) in Oxide Semiconductor Layer The In concentration (average concentration of In (indium) relative to all detectable metal atoms contained in the oxide semiconductor layer) in the oxide semiconductor layer of the TFTs obtained in Examples and Comparative Examples was measured by transmission electron microscopy-energy dispersive X-ray spectroscopy (TEM-EDX).

[0191] Measurement of the average In concentration in the oxide semiconductor layer by TEM-EDX was performed as follows. First, the TFTs obtained in each example and comparative example were processed with a focused ion beam (FIB) at an acceleration voltage of 20 to 30 kV using a composite beam processing and observation system (manufactured by JEOL Ltd., "JIB-4700F"), and then thin film samples for cross-sectional TEM observation were picked up by a microsampling method using a focused ion beam processing and observation system (FIB) (manufactured by Hitachi High-Tech Corporation, "FB-2100") at an acceleration voltage of 40 kV. The thin film samples for cross-sectional TEM observation by TEM-EDX were prepared as thin films that included the entire region in the thickness direction of the oxide semiconductor layer (the stacking direction of the TFT), and were prepared so that the sample thickness was the same in all examples and comparative examples (thickness: 60 to 80 nm).

[0192] Next, the thin film sample for cross-sectional TEM observation was subjected to cross-sectional TEM observation, and EDX line analysis was performed in the film thickness direction from the first insulating layer 13 side to the second insulating layer 14 side for the field of view including the oxide semiconductor layer, in the field of view at the center of the channel region. The EDX analysis was performed using an energy dispersive X-ray analyzer (manufactured by JEOL Ltd., "JED-2300T") under the following conditions: acceleration voltage: 200 kV, measurement mode: STEM mode, spot diameter: 0.16 nm, measurement interval: 1 nm. The EDX analysis was performed by selecting, as the elements to be detected (detectable elements), In, as well as all metal elements that were constituent elements of the oxide semiconductor layer, the second insulating layer, and the first insulating layer and that could be detected by the analyzer, and performing line analysis in the film thickness direction of the oxide semiconductor layer. The EDX spectral intensity obtained by EDX line analysis was automatically calculated using initial setting values ​​using the dedicated software of the energy dispersive X-ray analyzer (manufactured by JEOL Ltd., "JED-2300T"). The average In concentration was calculated by arithmetically averaging the In concentrations in the region in the film thickness direction where In is the main component, calculated based on the amount of In obtained at each measurement point in the EDX line analysis described above.

[0193] (d) Resistance of Impurity Region The resistance of the impurity region 11A of the oxide semiconductor layer 11 of the TFT obtained in the Examples and Comparative Examples was measured as follows. First, a pair of probes of a resistance measuring instrument was inserted into the impurity region of the TFT element obtained in the Examples and Comparative Examples, and the resistance R was measured. If it is not possible to insert the probes into the sample, and if there is a semiconductor device to be measured in which three or more types of TFTs have a fixed channel width and different channel lengths, the resistance R calculated by the TLM (Transmission Line Method) analysis shown in item (e) below may be used. 0 The value of may be regarded as the above-mentioned resistance value R. Based on the obtained measured resistance value R, the sheet resistance and specific resistance were calculated based on the formulas (2) and (3) calculated from the following relational expression (1). ρ=R×L / W×d (1) Rsh=R×L / W (2) ρ=Rsh×d (3) In the above formulas (1) to (3), ρ is the specific resistance, Rsh is the sheet resistance, d is the film thickness of the oxide semiconductor layer, R is the measured resistance value measured by a resistance meter, the channel length L is the length of the oxide semiconductor layer in the source-drain direction, and the channel width W is the width of the oxide semiconductor layer (the width relative to the length L). Note that when the region formed by L and W is not rectangular, the specific resistance is calculated by applying a method that can exclude the shape factor, such as the van der Pauw method.

[0194] (e) ΔL (gate width L and effective channel length L eff The TLM (Transmission Line Method) analysis was performed on the TFT elements obtained in the examples and comparative examples to calculate ΔL in the oxide semiconductor layer. Tables 1 to 3 show the values ​​of ΔL. In the TLM analysis, when three or more types of TFTs having the same gate length W and three or more gate widths L are present on a semiconductor device, characteristic information on the resistance value (R) and gate width (L) of the TFT element (thin film transistor) is obtained for each of a plurality of gate voltages (Vg) for each TFT, and the coordinates of the intersections of the graphs obtained based on the following relational expressions (A) and (B) are calculated to calculate the effective channel length (L eff) and the external resistance. T The relationship between R and the gate width (L) is given by the following equations (A) and (B): T =V DS / I D =2R 0 +r ch ・L eff (A) L eff = L - 2ΔL (B) In the above formulas (A) and (B), R T is the total resistance, and R 0 is the external resistance, and L eff is the effective channel length (hereinafter referred to as the effective channel length), L is the gate width, and ΔL is the ratio of the gate width L to the effective channel length L eff It is half the difference between r ch is the channel resistance divided by the unit length, and the gate voltage (V g In formulas (A) and (B), V DS is the source-drain voltage, and I D is the drain current. Note that the "gate width L" in equations (A) and (B) is shown as gate width L1 in FIGS. 1 and 3, and the "effective channel length L eff " is shown as L2 in Figures 1 and 3. Also, "ΔL" in formulas (A) and (B) is the same as ΔL in Figures 1 and 3. 1 and ΔL 2 In Examples 1 to 11 and Comparative Examples 1 to 14, the ΔL 1 and ΔL 2 In addition, when the above-mentioned TLM analysis is performed, the effective channel length L is calculated from the gate width L in the formula (B). eff The value 2ΔL obtained by subtracting L−L is obtained. eff is ΔL 1 +ΔL 2 Also expresses ΔL 1 = ΔL 2 In this case, ΔL is ΔL 1 will be consistent with

[0195] As mentioned above, multiple gate voltages (V g The resistance value (R; R) of the TFT element (thin film transistor) obtained for each T ) and gate width (L) characteristic information is expressed as (x, y) = (gate width L, total resistance R of the TFT element) T ) and obtained multiple graphs were plotted. The x value of the intersection coordinate of the graphs coincides with 2ΔL. The y value of the intersection coordinate is the external resistance (2R 0 ) The TLM method, which is the method for calculating ΔL described above, can be applied only when three or more types of TFTs having the same gate length W and three or more gate widths L are present on a semiconductor device and the above graph can be created. Therefore, when the above graph cannot be created (for example, when reverse engineering is performed), ΔL (ΔL 1 and / or ΔL 2 The ΔL value determined by the TLM method and the ΔL value measured by a method using SSRM or SCM are almost the same, but by further correcting using a standard sample, the ΔL value can be corrected to the TLM standard value.

[0196] (B) Average boron concentration in the oxide semiconductor layer (impurity region / channel region), first impurity-doped insulating film region, second impurity-doped insulating film region, and gate insulating film region Each layer of the TFT elements obtained in the examples and comparative examples was etched without pretreatment, and a time-of-flight secondary ion mass spectrometry (ToF-SIMS) depth profile analysis was performed using a time-of-flight secondary ion mass spectrometer (manufactured by ION-TOF, "TOF-SIMS5") to detect the intensity of secondary ions to analyze the elements present in the depth direction, thereby measuring the boron concentration in the impurity region and channel region of the oxide semiconductor layer, and the first impurity-doped insulating film region, second impurity-doped insulating film region, and gate insulating film region of the first insulating layer. Etching ion source: O 2 + (for secondary positive ions) and Cs + (For secondary negative ions) Acceleration energy of etching ions: 1 keV Primary ions: Bi + Primary ion acceleration energy: 25 keV. Secondary ions detected were B, Si, In, and Mo as negative ions, and H, F, O, Si, In, and O as positive ions. The mass resolution was set to normal resolution, and charge correction was performed using the electron gun. For secondary ions B and H, SiO 2 For the region, the standard sample is SiO 2 The concentration was converted as follows: for the oxide semiconductor region (channel region and impurity region), the standard sample was In 2 O 3 The boron concentration distribution was obtained for each region or layer by the above-described SIMS depth profile analysis. The obtained boron concentration distribution was integrated and averaged over the film thickness of each region or layer to calculate the average boron concentration.

[0197] (C) Evaluation of TFT Performance The TFTs obtained in the examples and comparative examples were measured at room temperature in a light-shielded environment (inside a shielded box) using a semiconductor parameter analyzer (Agilent Technologies' "B1500"). A drain voltage (Vd) of 0.1 V or 20 V was applied. For each Vd applied, the gate voltage (Vg) was varied from -10 V to 20 V in 0.2 V steps to measure the current value Id, thereby obtaining the Id-Vg characteristics. Tables 1 to 3 show various parameters calculated from the Id-Vg characteristics. The calculation method for each parameter is as follows:

[0198] (a) Maximum value of linear mobility (μlin Max) The maximum value of linear mobility when Vd = 0.1 V was determined by creating a graph of Id-Vg characteristics, calculating the transconductance (Gm) for each Vg, and deriving the linear mobility (μlin) using the equation for the linear region. Specifically, Gm was calculated by ∂(Id) / ∂(Vg). Furthermore, μlin was calculated using the following equation (c) for the linear region: μlin = (Gm L) / (W Ci Vd) ... (c) In equation (c), Ci is the capacitance of the gate insulating film, and is determined by the gate insulating film thickness, SiO 2 The relative dielectric constant of 3.9 and the dielectric constant of vacuum is 8.85 x 10 -14 Ci [F / cm] calculated based on [F / cm] 2 In formula (c), L is the channel length (L length), and W is the channel width (W length). Furthermore, the maximum value of μlin at Vg = 0 to 20 V was calculated from each Vg-μlin graph and designated as "μlin Max."

[0199] (b) S value and threshold voltage Vth The S value and threshold voltage (Vth) were evaluated from the graph of each Id-Vg characteristic. -11 ~10 -10 In the [A] region, the value obtained by the following formula (d) was calculated as the S value. -10 The value of Vg at [A] was calculated as the threshold voltage (Vth).

[0200]

[0201] (Depth Profile) Using the time-of-flight secondary ion mass spectrometer (manufactured by ION-TOF, "TOF-SIMS5") described in the above section (B), an area of ​​approximately 20 μm × 20 μm was specified for the channel region and the impurity region, and SIMS depth profile analysis was performed. As an example, for a TFT element having a configuration similar to that of the thin film transistor (TFT) 60 shown in FIG. 7 and obtained by indirect injection ion implantation processing, the interlayer insulating film 26-2 - the second insulating layer 26-1 - the impurity region 11A-1 of the oxide semiconductor layer 11 - the buffer layer (first insulating layer) 22 region was analyzed by the SIMS depth profile analysis described above. When the impurity region was further identified, the depth profiles of the boron (B) concentration, silicon (Si) concentration, and indium (In) concentration are shown in FIG. 13. In the graph of FIG. 13, the left vertical axis, Concentration (atoms / cc), indicates the average boron concentration (number of boron atoms per unit volume), and the right vertical axis, Intensity (counts), indicates the Si + ions and In + 13 shows the secondary ion intensity of the ions, and Depth (μm) on the horizontal axis indicates depth. In Fig. 13, 0.22 to 0.26 μm is the depth profile of each of the above elements in the impurity region 11A-1 of the oxide semiconductor layer 11. The analysis range of the channel region or the impurity region is specified to be about 1 μm away from the boundary between the channel region and the impurity region in order to avoid detection of components derived from regions other than the analysis range.

[0202]

[0203]

[0204]

[0205] In Tables 1 to 3, a "-" in the column for average boron concentration indicates that the concentration was below the measurement limit, and a "-" in the columns for conductive region characteristics and TFT characteristics indicates that the characteristic value could not be calculated or that the characteristics were so poor that they could not be quantified. The TFTs fabricated in Examples 9 to 11 and Comparative Examples 9 to 14 did not have a second impurity-doped insulating film region, and are therefore denoted as "wo" (abbreviation for "without").

[0206] From the results shown in Tables 1 to 3, in Examples 1 to 11 in which the atomic ratio of In contained in the oxide semiconductor layer was 70 atomic % or more and boron ions were contained in the impurity region of the oxide semiconductor layer, the linear mobility was 15 cm 2 It was confirmed that the material exhibited high mobility of 1.5V or more, a high threshold voltage (Vth) of over -2.4V, a small ΔL of 1.7 μm or less, and good switching characteristics were obtained, and that the material operated well as a TFT.

[0207] Although several embodiments and / or examples of the present invention have been described in detail above, those skilled in the art will readily be able to make numerous modifications to these exemplary embodiments and / or examples without substantially departing from the novel teachings and advantages of the present invention. Accordingly, these numerous modifications are within the scope of the present invention. The contents of all documents cited in this specification and of the applications from which this application claims priority under the Paris Convention are incorporated by reference in their entirety.

Claims

1. A semiconductor device comprising: an impurity region containing boron as an impurity; a channel region; an oxide semiconductor layer having an atomic ratio of In of 70 atomic % or more to all metal elements; a plurality of insulating film layers; and a plurality of metal layers on a substrate; and a linear mobility μ lin is 15cm 2 / Vs or more and a threshold voltage Vth exceeding -2.4V.

2. The semiconductor device according to claim 1, further comprising: a first insulating layer; the oxide semiconductor layer; a second insulating layer; and a first metal layer stacked in this order on the substrate.

3. The semiconductor device according to claim 1 or 2, wherein the atomic ratio of In to all metal elements contained in the oxide semiconductor layer is 73 atomic % or more.

4. The semiconductor device according to claim 1, wherein the oxide semiconductor layer includes a polycrystalline region.

5. The semiconductor device according to claim 1, wherein the oxide semiconductor layer contains crystal grains having a bixbyite structure.

6. The semiconductor device according to claim 1, wherein the impurity region has a resistivity of 0.05 Ωcm or less.

7. Linear mobility μ of the channel region lin is 20cm 2 The semiconductor device according to any one of claims 1 to 6, wherein the Vref is 0.1 V or more.

8. Effective channel length L in the channel region eff is represented by the following formula: L eff = L - (ΔL 1 +ΔL 2 ) (wherein, L is the width of the gate electrode in the source electrode-drain electrode direction, and ΔL 1 is the distance from a position where a perpendicular line drawn from one end of the gate electrode toward the oxide semiconductor layer intersects with the oxide semiconductor layer to an end of a region having a carrier concentration functioning as a channel in the oxide semiconductor layer, 2 is the distance from a position where a perpendicular line drawn from the other end of the gate electrode toward the oxide semiconductor layer intersects with the oxide semiconductor layer to an end of a region having a carrier concentration functioning as a channel in the oxide semiconductor layer. 1 and ΔL 2 8. The semiconductor device according to claim 1, wherein one or both of the above is 1.1 μm or less.

9. The average boron concentration of the impurity region is 5×10 18 ~5×10 21 cm -3 The semiconductor device according to any one of claims 1 to 8, 10. The first insulating layer is in contact with the impurity region of the oxide semiconductor layer, the first insulating layer has a first impurity-doped insulating film region having a thickness of up to 100 nm from an interface with the impurity region, and an average boron concentration of the first impurity-doped insulating film region is 1×10 17 ~3×10 21 cm -3 The semiconductor device according to any one of claims 2 to 9, 11. The second insulating layer is in contact with the impurity region on a surface of the oxide semiconductor layer opposite to a contact surface with the first insulating layer, the second insulating layer has a second impurity-doped insulating film region, and an average boron concentration of the second impurity-doped insulating film region is 5×10 18 ~5×10 21 cm -3 The semiconductor device according to any one of claims 2 to 10, 12. The average boron concentration in the channel region is 5×10 18 cm -3 The semiconductor device according to any one of claims 1 to 11, wherein the semiconductor device has a resistance of less than 100 Ω / s.

13. The semiconductor device according to claim 11 or 12, wherein the second insulating layer has the second impurity doped insulating film region and an insulating gate insulating film region.

14. The average boron concentration in the gate insulating film region is 1×10 17 ~5×10 20 cm -3 14. The semiconductor device of claim 13, wherein:

15. The semiconductor device according to any one of claims 1 to 14, which is a thin film transistor.

16. An electronic circuit comprising a semiconductor device according to any one of claims 1 to 15.

17. An electrical device, electronic device, vehicle, or power plant comprising an electronic circuit according to claim 16.

Citation Information

Patent Citations

  • Semiconductor device

    JP2013048216A

  • Semiconductor device and manufacturing method of the same

    JP2014232867A

  • Field-effect transistor, method for manufacturing field-effect transistor, display device using field-effect transistor, and semiconductor device

    WO2009093625A1

  • Oxide sintered body and sputtering target

    WO2010032422A1

  • Thin film transistor having crystalline indium oxide semiconductor film

    WO2010032431A1

Cited By

  • Semiconductor device and display device

    WO2026176963A1