Organic-inorganic composite electrolyte membrane and method for manufacturing same

The organic-inorganic composite electrolyte membrane addresses the brittleness and conductivity issues of sulfide-based electrolytes by integrating a sulfide-based solid electrolyte with a cross-linked polymer matrix and ionic liquid on a porous support, achieving flexible and high-conductivity films for all-solid-state batteries.

WO2024219785A1PCT designated stage expired Publication Date: 2024-10-24UI (UNIVERSITY IND FOUNDATION) YONSEI UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005068
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Sulfide-based solid electrolytes face challenges in manufacturing thin films due to brittleness and lack of flexibility, and polymer solid electrolytes have insufficient ionic conductivity and electrochemical stability, making them unsuitable for high-voltage anode materials.

Method used

An organic-inorganic composite electrolyte membrane is developed, integrating a sulfide-based solid electrolyte with a cross-linked polymer matrix and ionic liquid on a porous support, enhancing flexibility and ionic conductivity while maintaining interfacial stability.

Benefits of technology

The composite electrolyte membrane exhibits excellent flexibility, high ionic conductivity, and improved interfacial stability, enabling the use in all-solid-state batteries with high-capacity anode materials and maintaining 90% of its initial conductivity after 100 cycles of a 180° bending test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005068_24102024_PF_FP_ABST
    Figure KR2024005068_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an organic-inorganic composite electrolyte membrane and a method for manufacturing same. An organic-inorganic composite electrolyte membrane according to one embodiment overcomes the disadvantage of existing sulfide-based solid electrolytes of being brittle, rendering them difficult to manufacture into a thin membrane and problematic due to a lack of flexibility, and thus can exhibit excellent ion conductivity while being flexible.
Need to check novelty before this filing date? Find Prior Art

Description

Organic-inorganic composite electrolyte membrane and method for manufacturing the same

[0001] The present invention relates to an organic-inorganic composite electrolyte membrane and a method for manufacturing the same.

[0002] Recently, as the development of lithium batteries with improved energy density and safety has become a necessity, all-solid-state batteries that use solid electrolytes instead of liquid electrolytes are attracting attention as next-generation batteries.

[0003] Solid electrolytes can be classified into polymer organic solid electrolytes or inorganic solid electrolytes depending on their material, and in particular, inorganic solid electrolytes have the advantage of being able to secure high cation transport coefficients and ionic conductivity.

[0004] In particular, sulfide-based solid electrolytes, which are among the inorganic solid electrolytes, are 10 -2 10 inland -4 Although it exhibits very high ionic conductivity of about S / cm and excellent electrochemical stability, it is very difficult to manufacture into a thin film due to the rigidity and brittleness characteristic of solid electrolytes, and its flexibility is very poor, making commercialization difficult.

[0005] In addition, sulfide-based solid electrolytes are highly reactive with water when exposed to the air, forming H2S, making them unstable in air. Furthermore, because the electrolyte is solid, it has a high interfacial resistance between electrodes. Furthermore, the interface between the cathode material and the sulfide solid electrolyte is unstable, and there are problems with stability, such as dendrite growth, through voids caused by grain boundary defects between electrolyte particles.

[0006] On the other hand, polymer solid electrolytes offer advantages over inorganic solid electrolytes in terms of flexibility, lightness, and processability. However, compared to conventional liquid and inorganic solid electrolytes, polymer solid electrolytes have poor ionic conductivity and lithium ion transport rates at room temperature. Furthermore, their low electrochemical window hinders their combination with high-voltage cathode materials.

[0007] Therefore, in order to solve the above problem, there is an urgent need for research on a solid electrolyte that can secure flexibility and improve interface stability while maintaining the ionic conductivity of the sulfide-based solid electrolyte.

[0008] In order to solve the above-described problems, the present invention aims to provide an organic-inorganic composite electrolyte membrane having excellent flexibility and ionic conductivity, which includes a sulfide-based solid electrolyte.

[0009] In addition, another object of the present invention is to provide an all-solid-state battery including the organic-inorganic composite electrolyte membrane.

[0010] In order to achieve the above-described task, the inventors of the present invention have continuously conducted research to manufacture a solid electrolyte that can secure flexibility and improve interfacial stability while maintaining the ionic conductivity of a sulfide-based solid electrolyte. As a result, they discovered that when an organic-inorganic composite electrolyte including a sulfide-based solid electrolyte, a crosslinked polymer matrix, an ionic liquid, and a lithium salt is integrated into a porous support having a specific pore size, a thin, large-area electrolyte membrane can be manufactured, and has excellent flexibility and ionic conductivity, thereby completing the present invention.

[0011] The present invention provides an organic-inorganic composite electrolyte membrane comprising a porous support and an organic-inorganic composite electrolyte, wherein the organic-inorganic composite electrolyte comprises a sulfide-based solid electrolyte, a crosslinked polymer matrix, an ionic liquid, and a lithium salt, and wherein the organic-inorganic composite electrolyte is integrated with the porous support.

[0012] According to one embodiment of the present invention, the ionic liquid may include a glyme-based solvent.

[0013] According to one embodiment of the present invention, the ionic liquid to lithium salt can satisfy a molar ratio of 0.5 to 1.5:1.

[0014] According to one embodiment of the present invention, the crosslinked polymer matrix may be derived from a multifunctional monomer.

[0015] According to one embodiment of the present invention, the multifunctional monomer may be a monomer containing two or more photocurable functional groups selected from the group consisting of an acrylate group, a methacrylate group, a vinyl group, and a thiol group.

[0016] According to one embodiment of the present invention, the sum of the crosslinked polymer matrix to the ionic liquid and the lithium salt can satisfy a weight ratio of 3 to 15:85 to 97.

[0017] According to one embodiment of the present invention, the crosslinked polymer matrix may be included in an amount of 0.5 to 10 parts by weight based on 100 parts by weight of the sulfide-based solid electrolyte.

[0018] According to one embodiment of the present invention, the porous support may have an average pore size of 50 μm or more.

[0019] According to one embodiment of the present invention, the porous support may have a thickness of 5 to 40 μm.

[0020] According to one embodiment of the present invention, the organic-inorganic composite electrolyte membrane may have a thickness of 10 to 40 μm.

[0021] According to one embodiment of the present invention, the organic-inorganic composite electrolyte membrane has an ionic conductivity of 3.0 x10 -4 It may be more than S / cm.

[0022] According to one embodiment of the present invention, the organic-inorganic composite electrolyte membrane may have an ionic conductivity retention rate of 90% or more after 100 cycles of a 180° bending test.

[0023] According to one embodiment of the present invention, the organic / inorganic composite electrolyte film may have a structure in which two or more layers are laminated in the thickness direction.

[0024] The present invention can provide a method for manufacturing an organic-inorganic composite electrolyte membrane, which includes a step of manufacturing an organic-inorganic composite electrolyte by applying and polymerizing a slurry composition including a sulfide-based solid electrolyte, a polyfunctional monomer, an ionic liquid, and a lithium salt on a porous support.

[0025] According to one embodiment of the present invention, the ionic liquid may include a glyme-based solvent.

[0026] According to one embodiment of the present invention, the slurry composition may be substantially free of solvent.

[0027] According to one embodiment of the present invention, the step of compressing the organic-inorganic composite electrolyte membrane may be further included.

[0028] An organic-inorganic composite electrolyte membrane according to one aspect of the present invention overcomes the shortcomings of conventional sulfide-based solid electrolytes, which were difficult to manufacture into a thin membrane due to brittleness and had problems due to lack of flexibility, and can exhibit excellent ionic conductivity while ensuring flexibility.

[0029] Figure 1 is a schematic diagram of an organic-inorganic composite electrolyte membrane according to one embodiment.

[0030] Figure 2 is a photograph showing the 180° bending test process of Evaluation Example 1.

[0031] Figure 3 is a Nyquist plot of an organic-inorganic composite electrolyte membrane according to Example 1 before and after 100 cycles of a 180° bending test.

[0032] Figure 4 is a 7Li MAS NMR spectrum of an organic-inorganic composite electrolyte membrane according to Examples 1 and 2.

[0033] Figure 5 is a graph analyzing the electrochemical characteristics (charge / discharge voltage profile) of a lithium metal battery including an organic / inorganic composite electrolyte membrane according to Examples 1 and 2. In Figure 5, the descending curve represents the initial discharge capacity, and the ascending curve represents the initial charge capacity.

[0034] Figure 6 is a graph showing the results of analyzing the life characteristics (changes in capacity and coulombic efficiency according to the number of charge / discharge cycles) of a lithium metal battery including an organic / inorganic composite electrolyte membrane according to Examples 1 and 2.

[0035] Figure 7 is a graph showing the results of analyzing the rate characteristics (change in capacity according to the number of charge / discharge cycles at each current density) of a lithium metal battery including an organic / inorganic composite electrolyte membrane according to Examples 1 and 2.

[0036] Unless otherwise defined herein, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0037] As used herein, the singular forms may be intended to include the plural forms as well, unless the context clearly indicates otherwise.

[0038] Additionally, the numerical ranges used herein include lower and upper limits and all values ​​within that range, increments logically derived from the shape and width of the defined range, all doubly defined values, and all possible combinations of upper and lower limits of numerical ranges defined in different shapes. Unless otherwise specified herein, values ​​outside the defined numerical range that may arise due to experimental error or rounding of values ​​are also included in the defined numerical range.

[0039] The term "comprises" in this specification is an open-ended description equivalent to expressions such as "includes," "contains," "has," or "characterized by," and does not exclude additional elements, materials, or processes not listed herein.

[0040] Additionally, when it is said in the present invention that a layer is located "on" another layer, this includes not only cases where a layer is in contact with another layer, but also cases where one or more other layers exist between the two layers.

[0041] Hereinafter, an organic-inorganic composite electrolyte membrane according to one embodiment of the present invention will be described in more detail.

[0042] The present invention provides an organic-inorganic composite electrolyte membrane comprising a porous support and an organic-inorganic composite electrolyte, wherein the organic-inorganic composite electrolyte comprises a sulfide-based solid electrolyte, a crosslinked polymer matrix, an ionic liquid, and a lithium salt, and wherein the organic-inorganic composite electrolyte is integrated with the porous support.

[0043] According to one embodiment of the present invention, the sulfide-based solid electrolyte may be a typical sulfide-based solid electrolyte used in the relevant technical field, and may be specifically represented by MaPNbScXd. Here, M is Li, Na, or a combination thereof, N is B, Al, Ga, In, Si, Ge, Sn, Pb, Sb, Bi, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Hf, Ta, W, X: F, Cl, Br, I, or a combination thereof, X is O, Se, Te, or a combination thereof, and 0≤a≤6, 0≤b≤6, 0≤c≤6, 0≤d≤6. Specifically, the sulfide-based solid electrolyte may be represented by Li2S-P2S5-MYf. Here, Y is O, S, Se, Te, or a combination thereof, and 0.50≤f≤4. Alternatively, the sulfide-based solid electrolyte may be represented by MaPScXd. Here, M is Li, Na, or a combination thereof, N is B, Al, Ga, In, Si, Ge, Sn, Pb, Sb, Bi, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Hf, Ta, W, or a combination thereof, X is F, Cl, Br, or I, and 0≤a≤6, 0≤b≤6, 0≤c≤6, 0≤d≤6. Specifically, the sulfide-based solid electrolyte may use LPSCl. The sulfide-based solid electrolyte may be amorphous or crystalline, and may have an average particle size of 50 nm to 50 μm, or 100 nm to 10 μm, but is not limited thereto. The above sulfide-based solid electrolyte may be included in an amount of 30 wt% or more, 40 to 80 wt% or more, 50 to 80 wt% or more, 55 to 80 wt% or more, or 55 to 80 wt% based on the total weight of the organic / inorganic composite electrolyte.

[0044] According to one embodiment of the present invention, the ionic liquid may include a glyme-based solvent. As a non-limiting example, the glyme solvent may be any one or a combination of two or more selected from the group consisting of 2-dimethoxymethane (1,2-Dimethoxymethane), 1,2-dimethoxyethane (DME), diethyleneglycol dimethyl ether (diglyme), diethylene glycol diethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, tetraethylene glycol dimethyl ether (TEGDME, Tetraglyme), tetrahydrofuran (THF), 2-methyl tetrahydrofuran, dimethyl ether, and dibutyl ether.

[0045] According to one embodiment of the present invention, the lithium salt may be a combination of lithium metal and one or more anions selected from the group consisting of bis(fluorosulfonyl)imide (FSI), bis(trifluoromethylsulfonyl)imide (TFSI), bis(pentafluoroethylsulfonyl)imide (PFSI), and hexafluorophosphate (PF6). For example, the lithium salt may be LiFSI, LiTFSI, or LiPFSI.

[0046] According to one embodiment of the present invention, the ionic liquid to lithium salt may satisfy a molar ratio of 0.1 to 5:1, or a molar ratio of 0.5 to 1.5:1, or a molar ratio of 0.8 to 1.2:1.

[0047] When the ionic liquid and lithium salt are mixed in the above-described organic-inorganic composite electrolyte, the lithium metal of the lithium salt is coordinated to the oxygen of the ionic liquid, and a solvated ionic liquid in which the anion of the lithium salt exists in the surroundings can be formed. The solvated ionic liquid can be included in the organic-inorganic composite electrolyte according to one embodiment, thereby further improving the ionic conductivity of the organic-inorganic composite electrolyte.

[0048] According to one embodiment of the present invention, the crosslinked polymer matrix may be derived from a multifunctional monomer. Specifically, the crosslinked polymer matrix may be a crosslinked polymer having a three-dimensional crosslinked structure manufactured by thermal polymerization or photopolymerization of a multifunctional monomer. The multifunctional monomer may be a monomer containing two or three or more reactive functional groups selected from the group consisting of an acrylic group, a methacrylic group, a vinyl group, a thiol group, an epoxy group, an isocyanate group, a silanol group, a halogen group, a carboxyl group, a hydroxyl group, and an amine group. In addition, the weight of the crosslinked polymer matrix may be the same as the weight of the multifunctional monomer introduced during manufacture.

[0049] Specifically, the multifunctional monomer may be a monomer containing two or more photocurable functional groups selected from the group consisting of an acrylate group, a methacrylate group, a vinyl group, and a thiol group. In addition, the number average molecular weight of the multifunctional monomer may be 100 to 2000 g / mol, specifically 100 to 1000 g / mol.

[0050] Non-limiting examples of the polyfunctional monomers include diglycidyl ethers, trimethylolpropane triglycidyl ethers, pentaerythritol polyglycidyl ethers, benzyl glycidyl ethers, triglycidyl isocyanurates, polyglycidyl ethers, ethoxylated trimethylolpropane triacrylate (ETPTA), trimethylolpropane propoxylate triacrylate (TPPTA), pentaerythritol triacrylate (PETA), trimethylolpropane tris (3-mercaptopropionate) (TMPT), trimethylolpropane triacrylate (TMPTA), Examples include, but are not limited to, pentaerythritol tetrakis(3-mercaptopropionate) (PEMP) and dipentaerythritol hexakis(3-mercaptopropionate).

[0051] According to one embodiment of the present invention, the polyfunctional monomer may be a polyalkylene oxide-based polyfunctional monomer. Non-limiting examples of the polyalkylene oxide-based polyfunctional monomer include diethylene glycol diacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, dipropylene glycol diacrylate, dipropylene glycol dimethacrylate, ethylene glycol divinyl ether, ethoxylated trimethylolpropane triacrylate, diethylene glycol divinyl ether, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate (PGEDA), and polyethylene glycol dimethacrylate, and specifically, polyethylene glycol diacrylate (PGEDA), polyethylene glycol dimethacrylate, or a mixture thereof may be used, but is not limited thereto.

[0052] According to one embodiment of the present invention, the crosslinked polymer matrix may be included in an amount of 0.1 to 40 parts by weight, or 0.5 to 10 parts by weight, or 1 to 7 parts by weight, based on 100 parts by weight of the sulfide-based solid electrolyte.

[0053] According to one embodiment of the present invention, the sum of the crosslinked polymer matrix to the ionic liquid and the lithium salt can satisfy a weight ratio of 1 to 30:70 to 99, or a weight ratio of 3 to 15:85 to 97, or a weight ratio of 5 to 12:88 to 95.

[0054] According to one embodiment of the present invention, a mixture including a cross-linked polymer matrix, an ionic liquid, and a lithium salt, excluding a sulfide-based solid electrolyte in the organic-inorganic composite electrolyte, may be referred to as a gel polymer electrolyte, and a 70㎛ thick film including only the gel polymer electrolyte may have a Young's modulus measured according to ASTM D882 of 300 MPa or less, preferably 200 MPa or less, or 1 to 200 MPa, preferably 1 to 150 MPa, or 5 to 150 MPa, or 5 to 100 MPa, or 5 to 60 MPa, or 5 to 40 MPa. When the Young's modulus is satisfied, the connectivity between inorganic particles is not disturbed, so that better ionic conductivity can be exhibited.

[0055] According to one embodiment of the present invention, the porous support can be used without significant limitation as long as the organic-inorganic composite electrolyte can be integrated to form an organic-inorganic composite electrolyte membrane, and examples thereof include polyester, polyamide (aromatic, aliphatic, etc., e.g., Kevlar), cellulose, polysulfone, polyethersulfone, polyimide, polyamideimide, polytetrafluoroethylene, polyethylene, polypropylene, polyvinyl difluoride, polyethylene terephthalate, and polyacrylonitrile.

[0056] According to one embodiment of the present invention, the porous support may have an average pore size of 50 μm or more, or 50 to 150 μm, or 55 to 110 μm, or 60 to 90 μm. In the case of an organic-inorganic composite electrolyte membrane using a porous support having the above pore size, the organic-inorganic composite electrolyte can be effectively integrated with the porous support to provide flexibility and excellent ionic conductivity. In addition, when the average pore size is exceeded, insufficient ionic conductivity may be exhibited.

[0057] According to one embodiment of the present invention, the porous support may have a porosity of 10 to 99%, or 30 to 95%, or 60 to 95%, or 70 to 90%, or 80 to 90%. By using a porous support satisfying the above porosity, an organic-inorganic composite electrolyte membrane capable of simultaneously realizing superior flexibility and high ionic conductivity can be manufactured. In addition, a porous support with too low a porosity may exhibit insufficient ionic conductivity.

[0058] According to one embodiment of the present invention, the porous support may have a thickness of, but is not limited to, 5 to 100 μm, or 5 to 40 μm, or 10 to 30 μm.

[0059] According to one embodiment of the present invention, when the porous support has a thickness of 10±2㎛, the weight per unit area may be 0.05 to 2mg / cm2, or 0.1 to 1mg / cm2.

[0060] According to one embodiment of the present invention, the organic-inorganic composite electrolyte is characterized by being integrated with a porous support. Specifically, the organic-inorganic composite electrolyte may be integrated with the porous support in all volumes, or the organic-inorganic composite electrolyte may be integrated with a portion of the porous support, thereby forming (a) a portion integrated with the porous support and (b) an organic-inorganic composite electrolyte layer in which only the organic-inorganic composite electrolyte exists on the porous support.

[0061] According to one embodiment of the present invention, the organic-inorganic composite electrolyte membrane may have a thickness of 5 to 100 μm, or 10 to 60 μm, or 10 to 50 μm, or 10 to 40 μm, but can be easily adjusted depending on the intended use or properties to be manufactured.

[0062] According to one embodiment of the present invention, the organic / inorganic composite electrolyte membrane may have a structure in which two or more of the unit electrolyte membranes are laminated in the thickness direction. By repeatedly laminating the unit electrolyte membranes, a flexible organic / inorganic composite electrolyte membrane with excellent ion conductivity can be manufactured. The unit electrolyte membranes may have a structure in which two, three, four, five, six, seven, eight, nine, ten, ten or more, or 2 to 15, or 4 to 12 are laminated in the thickness direction, but the present invention is not limited thereto, and may be easily controlled depending on the properties to be manufactured.

[0063] According to one embodiment of the present invention, the organic-inorganic composite electrolyte membrane has an ionic conductivity of 1.0 x10 -4 S / cm or more, or 3.0 x10 -4 S / cm or more, or 3.5 x10 -4 It may be more than S / cm.

[0064] According to one embodiment of the present invention, the organic-inorganic composite electrolyte membrane can maintain an ionic conductivity measured after 100 cycles as a result of a 180° bending test of 80% or more, 90% or more, preferably 95% or more, or 99% or more of the initially measured ionic conductivity.

[0065]

[0066] Hereinafter, a method for manufacturing an organic-inorganic composite electrolyte membrane according to one embodiment will be described in more detail.

[0067] The present invention can provide a method for producing an organic-inorganic composite electrolyte membrane, which comprises the step of applying and polymerizing a slurry composition comprising a sulfide-based solid electrolyte, a polyfunctional monomer, an ionic liquid, and a lithium salt onto a porous support to produce an organic-inorganic composite electrolyte. Here, specific descriptions of the sulfide-based solid electrolyte, the polyfunctional monomer, the ionic liquid, and the lithium salt and examples of the compounds are the same as those described above, and therefore are omitted.

[0068] According to one embodiment of the present invention, in the slurry composition, the multifunctional monomer may be included in an amount of 0.1 to 40 parts by weight, or 0.5 to 10 parts by weight, or 1 to 7 parts by weight, based on 100 parts by weight of the sulfide-based solid electrolyte.

[0069] In particular, in the present invention, when the content of the multifunctional monomer is outside the range of 0.5-10 parts by weight, it was confirmed that the continuous phase of the sulfide-based solid electrolyte may not be formed, and thus the ionic conductivity may not be maximized depending on the cell implementation conditions.

[0070] In addition, the sum of the polyfunctional monomer to the ionic liquid and the lithium salt can satisfy a weight ratio of 1 to 30:70 to 99, or a weight ratio of 3 to 15:85 to 97, or a weight ratio of 5 to 12:88 to 95.

[0071] In addition, the slurry composition may further include a known polymerization initiator widely used in the technical field. The polymerization initiator may be a thermal initiator or a photoinitiator. Non-limiting examples of the thermal initiator include azo initiators such as 2,2-azobis-2,4-dimethylvaleronitrile, 2,2-azobisisobutyronitrile, 2,2-azobis-2-methylbutyronitrile, and the like; or peroxide initiators such as amyl peroxy pivalate, hexyl peroxy dicarbonate, benzoyl peroxide, dibenzoyl peroxide, and the like; The above photoinitiator can be used without significant limitation as long as it is a compound that can generate radicals and initiate a radical reaction by irradiation with an active energy ray, and non-limiting examples thereof include alpha-ketone compounds, acetophenone compounds, ketal compounds, aromatic sulfonyl chloride compounds, photoactive oxime compounds, benzophenone compounds, thioxanthone compounds, camphorquinone compounds, halogenated ketone compounds, acylphosphinoxide compounds, and acylphosphonate compounds.

[0072] According to one embodiment of the present invention, the slurry composition may be substantially free of a solvent. Here, "substantially free" may mean that the slurry composition contains 1 wt% or less of the solvent, specifically 0.1 wt% or less, based on the total weight of the slurry composition. A method for manufacturing an organic-inorganic composite electrolyte membrane according to one embodiment is characterized by desolvation without using a separate solvent in the process. In conventional process technologies that used solvents, there were great difficulties in selecting a solvent due to the high chemical reactivity of sulfides, and further, the solvents used were highly toxic, resulting in high processing costs. However, a manufacturing method according to one embodiment is a solvent-free process, and has the advantage that the electrolyte and sulfides are not reactive and no separate solvent processing costs are incurred. In addition, since the above-mentioned organic-inorganic composite electrolyte membrane is a continuous phase exhibiting lithium ion conductivity, it can be made into a thin film and exhibits high flexibility depending on the combination of the inorganic particles, which are sulfide-based solid electrolytes, and the cross-linked polymer matrix, and above all, it can implement the effect of improving the continuous phase between the inorganic particles, which are passages for lithium ions, and thus can exhibit ion conductivity and battery characteristics that are far superior to the ion conductivity of the conventional technology, an independent sulfide-based solid electrolyte, or a cross-linked polymer matrix.

[0073] According to one embodiment of the present invention, a method for applying the slurry composition may use a conventional or known application or coating method, and for example, a coating method selected from knife casting, tape casting, doctor blade coating, bar coating, spin coating, slot die coating, dip coating, and spray coating; or a printing method selected from inkjet printing, gravure printing, gravure offset, aerosol printing, stencil printing, and screen printing, but is not limited thereto. Tape casting may be preferably used.

[0074] According to one embodiment of the present invention, a method for curing the slurry composition may utilize a conventionally used or known thermal polymerization or photocuring method. The thermal curing may be heating at a temperature of 60°C, preferably 80°C or higher for a certain period of time. In addition, the photocuring may be curing by irradiating a light source in the ultraviolet (UV) wavelength range, and for example, a lamp in the ultraviolet (UV) wavelength range of 254 nm, 300 nm, 365 nm, 385 nm, or 395 nm or a 1260 mW / cm2 Hg UV lamp may be irradiated to the substrate, but is not limited thereto. Through this, the multifunctional monomer is polymerized to form a crosslinked polymer matrix, which functions as a binder, thereby suppressing desorption of a sulfide-based solid electrolyte and producing an organic-inorganic composite electrolyte membrane with excellent durability.

[0075] According to one embodiment of the present invention, an organic-inorganic composite electrolyte membrane manufactured through a unit process including the above manufacturing step once each is used as a unit electrolyte membrane, and the unit process is performed multiple times to manufacture an organic-inorganic composite electrolyte membrane having multiple unit electrolyte membranes. Specifically, the step of repeating the manufacturing step at least once, once, twice, three times, four times, five times, or more than five times on the unit electrolyte membrane may be further included. Through this, an organic-inorganic composite electrolyte membrane having excellent ionic conductivity and flexibility and effectively suppressing desorption of a sulfide-based solid electrolyte, in which multiple unit electrolyte membranes are formed, can be manufactured.

[0076] According to one embodiment of the present invention, a step of compressing the organic-inorganic composite electrolyte membrane may be further included. The compressing method may use a conventional or known method, and for example, it may be performed by applying a pressure of 1 MPa or more, preferably 3 to 10 MPa or 3 to 500 MPa for a certain period of time at room temperature or a temperature of 60°C or higher, or 80°C or higher, or by using a conventional roll press or hydraulic press. Through this, an organic-inorganic composite electrolyte membrane with higher adhesion can be manufactured.

[0077]

[0078] Hereinafter, an all-solid-state battery according to one embodiment will be described. However, except for including the organic-inorganic composite electrolyte membrane according to one embodiment, the battery can be manufactured using a manufacturing method and materials common in the art with a structure known in the art.

[0079] The present invention can provide an all-solid-state battery including the above-described organic-inorganic composite electrolyte membrane. The all-solid-state battery includes a cathode layer and a cathode layer, and includes an organic-inorganic composite electrolyte layer between the cathode layer and the anode layer, and the organic-inorganic composite electrolyte layer may include an organic-inorganic composite electrolyte membrane according to one embodiment.

[0080] According to one embodiment of the present invention, the positive electrode layer may include a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector.

[0081] According to another embodiment of the present invention, the positive electrode active material layer may be impregnated with an organic / inorganic composite electrolyte according to one aspect within the pores, and the positive electrode layer and the organic / inorganic composite electrolyte layer may be integrated with each other.

[0082] For example, the thickness of the organic-inorganic composite electrolyte layer may be 0.1 to 100 ㎛, 1 to 100 ㎛, or 5 to 40 ㎛, wherein the thickness of the organic-inorganic composite electrolyte layer means the thickness of a section where the positive electrode active material layer and the organic-inorganic composite electrolyte are not mixed and only the organic-inorganic composite electrolyte film according to one embodiment exists.

[0083] An all-solid-state battery according to one embodiment may be manufactured by including the steps of (A) applying a cathode material slurry composition to one surface of a cathode current collector, drying, and rolling to manufacture a cathode active material layer having pores; (B) impregnating the cathode active material layer with the slurry composition according to one embodiment and polymerizing it to manufacture a cathode layer impregnated with an organic-inorganic composite electrolyte and an organic-inorganic composite electrolyte layer integrated with the cathode layer; and (C) laminating the cathode layer impregnated with the organic-inorganic composite electrolyte and a cathode layer.

[0084] Non-limiting examples of the positive electrode current collector may include a foil made of aluminum, nickel, or a combination thereof, and the positive electrode material slurry composition may include a solvent, a binder, a conductive agent, a dispersant, etc., in addition to the positive electrode active material, as needed. The thickness of the positive electrode current collector is not particularly limited, but may be 3 to 500 μm.

[0085] The above cathode active material can be any cathode active material used in this technical field without limitation, as long as it is a material capable of reversible insertion and de-insertion of lithium ions, and non-limiting examples thereof include lithium cobalt oxide composite oxide (LiCoO2), spinel crystalline lithium manganate composite oxide (LiMn2O4), lithium manganate composite oxide (LiMnO2), lithium nickelate composite oxide (LiNiO2), lithium iron phosphate (LiFePO4), lithium manganese phosphate (LiMnPO4), lithium cobalt phosphate (LiCoPO4), lithium iron pyrophosphate (Li2FeP2O7), lithium niobate composite oxide (LiNbO2), lithium iron oxide composite oxide (LiFeO2), lithium magnesium oxide composite oxide (LiMgO2), lithium cuprate composite oxide (LiCuO2), lithium zincate composite oxide (LiZnO2), and molybdic acid. Lithium composite oxide (LiMoO2), lithium tantalate composite oxide (LiTaO2), lithium tungstate composite oxide (LiWO2), lithium permanganate nickel cobalt composite oxide (xLi2MnO3(1-x)LiMn1-y-zNiyCozO2), lithium nickel cobalt aluminum composite oxide (LiNi0.8Co0.15Al0.05O2), lithium nickel cobalt manganese composite oxide (LiNi0.33Co0.33Mn0.33O2, LiNi0.4Co0.2Mn0.4O2, LiNi0.5Co0.2Mn0.3O2, LiNi0.6Co0.2Mn0.2O2, LiNi0.7Co0.15Mn0.15O2, LiNi0.8Co0.1Mn0.1O2), manganese oxide Examples include, but are not limited to, nickel (LiNi0.5Mn1.5O4).

[0086] The conductive material may include, but is not limited to, carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, etc.; conductive fibers such as carbon fibers and metal fibers; metal powders such as fluorinated carbon, aluminum, and nickel powders; conductive whiskeys such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives, but is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery.

[0087] The above binder polymer may include one or more selected from the group consisting of nitrile butadiene rubber, polyethylene glycol, polyacrylonitrile, polyvinyl chloride, polymethyl methacrylate, polypropylene oxide, polydimethylsiloxane, polyvinylidene fluoride, polyvinylidene carbonate, and polyvinylpyrrolidinone, and preferably one or more selected from the group consisting of polyvinylidene fluoride, polyvinylidene carbonate, and polyethylene glycol, but is not limited thereto.

[0088] The above negative electrode layer may include a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector.

[0089] Non-limiting examples of the negative electrode current collector may be selected from a foil made of copper, gold, nickel, or a copper alloy or a combination thereof. The negative electrode active material layer may be any one or two or more selected from the group consisting of any one carbon selected from soft carbon, hard carbon, artificial graphite, natural graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, carbon nanotubes, acetylene black, Ketjen black, graphene, fullerene, activated carbon, and meso carbon microbeads; any one metal selected from silicon, tin, lithium, aluminum, silver, bismuth, indium, germanium, lead, platinum, titanium, zinc, manganese, cadmium, cerium, copper, cobalt, nickel, and iron; an alloy comprising two or more of the above metals; and an oxide of one or more of the above metals; and preferably, lithium metal, but is not limited thereto.

[0090] The above-mentioned all-solid-state battery can be manufactured in a shape commonly used in the relevant field, and there is no limitation on the external shape according to the use of the battery, and for example, it can be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.

[0091] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. However, these are provided to enable those skilled in the art to easily implement the present invention. The present invention may be implemented in various different forms, and the spirit of the present invention is not necessarily limited to the embodiments.

[0092] [Manufacturing Example 1]

[0093] An ionic liquid (1,2-dimethoxyethane) and a lithium salt (LiFSI) were mixed in a molar ratio of 1:1, and then a multifunctional monomer (ethoxylated trimethylolpropane triacrylate (ETPTA)) was added at 3.5 wt% based on the total weight, and a photoinitiator was added at 1 wt% based on 100 wt% of the ETPTA to prepare a mixture.

[0094] In addition, to evaluate the properties of the gel polymer electrolyte (crosslinked polymer matrix, ionic liquid, and lithium salt), the prepared mixture was applied and irradiated with a 365 nm UV lamp for 1 minute to perform UV crosslinking, thereby producing a 70 μm thick gel polymer electrolyte film. The Young's modulus of the gel polymer electrolyte film was measured according to ASTM D882, and was found to be 30 MPa.

[0095] [Manufacturing Example 2]

[0096] A mixture was prepared in the same manner as in Preparation Example 1, except that diethylene glycol dimethyl ether was used as the ionic liquid.

[0097] [Manufacturing Example 3]

[0098] A mixture was prepared in the same manner as in Manufacturing Example 1, except that ETPTA was added at 5 wt%.

[0099] [Manufacturing Example 4]

[0100] A mixture was prepared in the same manner as in Manufacturing Example 1, except that ETPTA was added at 10 wt%.

[0101] [Manufacturing Example 5]

[0102] A mixture was prepared in the same manner as in Manufacturing Example 1, except that ETPTA was added at 15 wt%.

[0103] [Manufacturing Example 6]

[0104] A mixture was prepared in the same manner as in Preparation Example 1, except that diethylene glycol diethyl ether was used instead of 1,2-dimethoxyethane.

[0105] [Manufacturing Example 7]

[0106] A mixture was prepared in the same manner as in Preparation Example 1, except that triethylene glycol dimethyl ether was used instead of 1,2-dimethoxyethane.

[0107] [Manufacturing Example 8]

[0108] A mixture was prepared in the same manner as in Preparation Example 1, except that tetraethylene glycol dimethyl ether was used instead of 1,2-dimethoxyethane.

[0109] [Manufacturing Example 9]

[0110] A mixture was prepared in the same manner as in Manufacturing Example 1, except that diethylene glycol dimethyl ether (dlgyme) was used instead of 1,2-dimethoxyethane and LiTFSI was used instead of LiFSI.

[0111] [Manufacturing Example 10]

[0112] A mixture was prepared in the same manner as in Preparation Example 1, except that triethylene glycol dimethyl ether was used instead of 1,2-dimethoxyethane and LiTFSI was used instead of LiFSI.

[0113] [Manufacturing Example 11]

[0114] A mixture was prepared in the same manner as in Preparation Example 1, except that tetraethylene glycol dimethyl ether was used instead of 1,2-dimethoxyethane and LiTFSI was used instead of LiFSI.

[0115] [Comparative Manufacturing Example 1]

[0116] A mixture was prepared in the same manner as in Manufacturing Example 1, except that no multifunctional monomer was added.

[0117] [Comparative Manufacturing Example 2]

[0118] A mixture was prepared in the same manner as in Manufacturing Example 1, except that a 1:1 volume ratio mixed solvent of dimethyl ether and 1,3-dioxolane (DOL), which are common solvents, was used instead of the ionic liquid diethylene glycol dimethyl ether.

[0119] [Evaluation Example 1] Ionic Conductivity (σLi)

[0120] The gel polymer electrolyte film manufactured in the above manufacturing example was overlapped between two identical stainless steel foils to manufacture an ionic conductivity measurement cell, and the ionic conductivity was measured. Based on EIS (Electrochemical Impedance Spectroscopy) analysis, the impedance was measured by applying an AC amplitude of 10 mV and a frequency range of 0.1 mHz to 5 MHz at room temperature, and the ionic conductivity was calculated according to Equation 1 below. The results are shown in Table 1 below. In addition, the ionic conductivity of the liquid electrolyte alone, which was a mixture of the ionic liquid (1,2-dimethoxyethane) and lithium salt (LiFSI) in a molar ratio of 1:1, was found to be 2.64 mS / cm.

[0121] [Formula 1]

[0122]

[0123] (In the above equation 1, l is the thickness of the cell, R is the resistance measured through EIS analysis, and S is the working area of ​​the electrode.)

[0124] In addition, a slurry composition was prepared by mixing each of the mixtures of Manufacturing Examples 1 to 5 and a sulfide-based solid electrolyte (LPSCl (Lithium phosphorus sulfur chloride) having an average particle size of 3 μm) in a volume ratio of 3:7. In addition, in order to measure the ionic conductivity of the slurry composition, the slurry composition was applied and irradiated with a 365 nm UV lamp for 1 minute to perform UV crosslinking, thereby preparing an organic-inorganic composite electrolyte film having a thickness of approximately 450 μm. Subsequently, the ionic conductivity of the organic-inorganic composite electrolyte film was measured in the same manner as in Evaluation Example 1, and is shown in Table 1 below.

[0125] Young's modulus of gel polymer electrolyte film [MPa] Ionic conductivity of gel polymer electrolyte film [mS / cm] Ionic conductivity of organic / inorganic composite electrolyte film [mS / cm] Manufacturing example 1300.710.714 Manufacturing example 2300.630.672 Manufacturing example 3500.690.603 Manufacturing example 41300.680.564 Manufacturing example 52200.670.184 Manufacturing example 6420.690.692 Manufacturing example 7490.550.642 Manufacturing example 8530.480.523 Manufacturing example 9340.620.675 Manufacturing example 10460.560.593 Manufacturing example 11510.440.516

[0126] As shown in Table 1 above, the gel polymer electrolyte films of Manufacturing Examples 1 to 11 exhibited excellent ionic conductivity, and in particular, Manufacturing Example 1 exhibited excellent ionic conductivity.

[0127] However, the organic-inorganic composite electrolyte film according to Manufacturing Example 1 easily formed a continuous phase of a sulfide-based solid electrolyte and exhibited very high ionic conductivity, but in the case of the organic-inorganic composite electrolyte film according to Manufacturing Example 5, it was difficult to form a continuous phase of a sulfide-based solid electrolyte and exhibited insufficient ionic conductivity compared to Manufacturing Example 1.

[0128] In addition, in the case of Comparative Manufacturing Example 2, which used a 1:1 volume ratio mixed solvent of dimethyl ether (DME) and 1,3-dioxolane (DOL), which are common solvents, instead of the ionic liquid in Manufacturing Example 1, it was confirmed that the mobility of the solvated lithium ions could be greatly reduced, resulting in a rapid decrease in ionic conductivity.

[0129] In addition, in the case of Manufacturing Examples 6-11, although the ionic conductivity is somewhat inferior to that of Manufacturing Example 1, it was confirmed that the ionic conductivity of the organic-inorganic composite electrolyte film was greatly improved not only compared to Comparative Manufacturing Examples 1 or 2, but also compared to Manufacturing Example 5.

[0130] [Example 1]

[0131] A slurry composition was prepared by mixing the mixture of the above Preparation Example 1 and a sulfide-based solid electrolyte (LPSCl (Lithium phosphorus sulfur chloride) having an average particle size of 3 μm) in a weight ratio of 4:6. The slurry composition was tape-casted on one side of an aromatic aramid porous support having a thickness of about 18 μm (average pore size: about 70 μm, porosity: about 86%), and irradiated with a UV lamp of 365 nm for 1 minute to perform UV crosslinking, thereby photo-curing the multifunctional monomer and forming an organic-inorganic composite electrolyte. Subsequently, the opposite side was similarly cast and photo-cured, and then pressed at a pressure of 370 MPa to ultimately manufacture an organic-inorganic composite electrolyte membrane in which the organic-inorganic composite electrolyte and the porous support were integrated with each other and had a thickness of 35 μm. A schematic diagram of the organic-inorganic composite electrolyte membrane according to the manufactured Example 1 is shown in FIG. 1.

[0132] [Example 2]

[0133] The same procedure as Example 1 was followed, except that the mixture of Manufacturing Example 5 was used instead of the mixture of Manufacturing Example 1.

[0134] [Comparative Example 1]

[0135] A slurry composition was prepared by mixing the mixture of Comparative Manufacturing Example 1 and a sulfide-based solid electrolyte (LPSCl (Lithium phosphorus sulfur chloride) having an average particle size of 3 ㎛) in a weight ratio of 4:6. The slurry composition was pressed at a pressure of 370 MPa to produce a solid electrolyte having a final thickness of 300 ㎛. In the case of Comparative Example 1, it was impossible to produce a thin film as in the example, and therefore a thick film was produced. As a result of measuring the ionic conductivity of the solid electrolyte according to Comparative Example 1, it was 1.42 x10 -3 It was expressed as S / cm.

[0136]

[0137] [Evaluation Example 2] 180° Bending Test

[0138] In order to evaluate the flexibility of the organic / inorganic composite electrolyte membranes manufactured in Examples 1 and 2 and Comparative Example 1, a 180° bending test was performed. Specifically, a 90 mm x 80 mm sample was manufactured with the organic / inorganic composite electrolyte membrane placed in the center, and the ends of the raw sample were fixed to the head of a UTM (Universal Testing Machine) so that they were interlocked by 20 mm each, and a test of bending and unfolding the sample 180° at a speed of 200 mm / min was repeated 100 cycles. A rough outline of the experimental method is illustrated in Fig. 2.

[0139] Ionic conductivity retention after 100 cycles of bending test = (Ionic conductivity after 100 cycles of 180° bending test / Initial measured ionic conductivity) x 100

[0140]

[0141] It was confirmed that the organic-inorganic composite electrolyte membrane according to Example 1 maintained 99% of the initially measured ionic conductivity (0.4 mS / cm) after 100 cycles of a 180° bending test. In addition, the Nyquist plot analyzed by electrochemical impedance spectroscopy (EIS) using a VSP classic analyzer from Bio-Logic before and after 100 cycles of a 180° bending test of the organic-inorganic composite electrolyte membrane according to Example 1 is shown in Fig. 3, and through this, it was confirmed that Example 1 exhibited an ion transfer resistance similar to the initial charge transfer resistance without a sharp decrease even after 100 cycles of a 180° bending test.

[0142] However, in the case of Comparative Example 1, it was difficult to produce a free-standing film, and the electrolyte membrane was broken with just one bend, making it impossible to measure the physical properties.

[0143] In addition, since Example 2 used a gel polymer electrolyte with a high Young's modulus, it showed an initial ionic conductivity (0.14 mS / cm) that was inferior to Example 1, and an ionic conductivity retention rate after 100 cycles of a bending test. Specifically, Example 1 enabled the continuous phase between inorganic particles, which is a sulfide-based solid electrolyte, to be smoothly formed, and thus lithium ions could move through the continuous phase of the inorganic particles, thereby realizing excellent ionic conductivity. On the other hand, Example 2 showed more inadequate physical properties because it was difficult to secure a movement path for lithium ions because a continuous phase was not formed between the inorganic particles.

[0144]

[0145] [Evaluation Example 3] Lithium ion migration evaluation

[0146] In addition, the organic / inorganic composite electrolyte membrane (using 7Li) manufactured in Examples 1 and 2 was overlapped between two identical lithium metal (6Li) foils to manufacture a symmetric cell (6Li||organic / inorganic composite electrolyte membrane (7Li)||6Li), and the lithium ion yield (tLi+) of the symmetric cell was evaluated using the Bruce-Vincent analysis method (potentiostatic polarization method).

[0147] In addition, the organic-inorganic composite electrolyte membrane of the symmetric cell was analyzed by 7Li MAS NMR before and after 100 cycles of 180° bending test using the same method as Evaluation Example 1, and the resulting spectrum is shown in Fig. 4. Through Fig. 4, it is possible to determine the path along which the organic-inorganic composite electrolyte with 7Li dominantly moved between the sulfide-based solid electrolyte and the gel polymer electrolyte as it exchanged with 6Li.

[0148] Referring to Figure 4, in the case of Example 1, the ratio of peak intensities of the sulfide-based solid electrolyte① / gel polymer electrolyte② decreased from 9.96 to 5.26 after 100 cycles, indicating that lithium ions predominantly moved along the sulfide-based solid electrolyte path, which demonstrated that the continuous phase of sulfide-based solid electrolyte particles was well formed, and the lithium ion yield also showed a high value of 0.69.

[0149] On the other hand, in the case of Example 2, the ratio of peak intensities of the sulfide-based solid electrolyte① / gel polymer electrolyte② was measured to be increased or similar from 8.72 to 8.85, which indicates that lithium ions were dominantly transferred to the gel polymer electrolyte, and the lithium ion yield was a low value of 0.37.

[0150]

[0151] - Manufacturing of all-solid-state lithium metal batteries

[0152] A cathode material slurry composition was prepared by adding N-methylpyrrolidone to a cathode material content of 40 wt% in a weight ratio of cathode active material (LiNi0.7Co0.15Mn0.15O2 (NCM711) coated with LiNbO3 (1.4 wt. %)) / solid electrolyte (LPSCl) / binder (polybutadiene rubber) / conductive material (carbon black; Super C65) = 74.5 / 21.5 / 2.0 / 2.0 (w / w / w / w)). The cathode material slurry composition was applied to a 10 ㎛ thick aluminum (Al) thin film using a doctor blade, dried with hot air at 80°C, and then vacuum-dried at 120°C for 24 hours to form a 110 ㎛ thick cathode active material layer.

[0153] Thereafter, the aromatic aramid porous support of Example 1 was placed on the positive electrode active material layer, and the slurry composition of Example 1 was impregnated into the porous support and the positive electrode active material layer, and a pressure of 370 MPa (5 tons) was applied for 2 minutes at room temperature using a hydraulic press (Hefei Kejing Materials Technology Co., Ltd.) to form a film. The film was irradiated with a 365 nm UV lamp for 1 minute, thereby manufacturing a positive electrode layer impregnated with an organic-inorganic composite electrolyte and a 40 μm thick solid electrolyte layer integrated with the positive electrode layer.

[0154] Afterwards, a graphite negative electrode was manufactured from a negative electrode active material composition containing negative electrode active material (Graphite / solid electrolyte (LPSCl) / binder (polybutadiene rubber) / conductive material (carbon black; Super C65) in a weight ratio of 75.0 / 22.0 / 3.0 / 0.0 (w / w / w / w)), and then the 106 ㎛ thick graphite negative electrode was rolled onto a 9 ㎛ thick copper foil current collector to manufacture an all-solid-state lithium metal battery.

[0155]

[0156] [Evaluation Example 4] Evaluation of Lifetime Characteristics and Rate-Dependent Characteristics

[0157] The room temperature life characteristics and rate characteristics of the manufactured all-solid-state battery were analyzed. The charge / discharge conditions were a current density of 0.05 C (= 0.088 mA / cm2) at room temperature (25℃) and a voltage range of 2.5 to 4.3 V, and a 100-cycle life test was conducted, and the results are shown in Figs. 5 and 6. In addition, in order to measure the rate characteristics, several cycle tests were conducted by changing the current density from 20, 0.05 C (= 0.088 mA / cm2) to 2.0 C (= 3.2 mA / cm2) in a voltage range of 2.5 to 4.3 V, and the results are shown in Fig. 7.

[0158] Referring to FIGS. 5 to 7, it can be seen that the all-solid-state lithium metal battery to which the organic-inorganic composite electrolyte membrane of Example 1 is applied exhibits excellent initial charge-discharge capacity, and also exhibits an excellent capacity retention rate of 80% or more even after 100 cycles. Specifically, when the Young's modulus of the organic-inorganic composite electrolyte satisfies 5 to 100 MPa, or 5 to 40 MPa, the connectivity between inorganic particles is not disturbed, so that the inorganic particles can form a continuous phase, thereby exhibiting ionic conductivity superior to that of Example 2, which is an organic-inorganic composite electrolyte with a high Young's modulus.

[0159] Accordingly, it can be seen that the organic-inorganic composite electrolyte membrane according to one aspect of the present invention can be manufactured into a thin film, exhibits excellent flexibility, has high ionic conductivity that enables operation at room temperature, and has excellent interfacial stability with a high-capacity positive electrode material or a graphite negative electrode, so that it has excellent life characteristics and rate characteristics.

[0160] As described above, the present invention has been described by limited embodiments, but these are provided only to help a more general understanding of the present invention, and the present invention is not limited to the above embodiments, and those skilled in the art to which the present invention pertains can make various modifications and variations based on this description.

[0161] Therefore, the idea of ​​the present invention should not be limited to the described embodiments, and all things that are equivalent or equivalent to the following claims as well as the claims are considered to fall within the scope of the idea of ​​the present invention.

Claims

1. Contains a porous support and an organic-inorganic composite electrolyte, An organic-inorganic composite electrolyte membrane characterized in that the organic-inorganic composite electrolyte comprises a sulfide-based solid electrolyte, a crosslinked polymer matrix, an ionic liquid, and a lithium salt, and the organic-inorganic composite electrolyte is integrated with a porous support.

2. In paragraph 1, The above ionic liquid is an organic-inorganic composite electrolyte membrane containing a glyme solvent.

3. In paragraph 1, An organic-inorganic composite electrolyte membrane in which the above ionic liquid and lithium salt satisfy a molar ratio of 0.5 to 1.5:

1.

4. In paragraph 1, An organic-inorganic composite electrolyte membrane wherein the above cross-linked polymer matrix is ​​derived from a multifunctional monomer.

5. In paragraph 4, An organic-inorganic composite electrolyte membrane wherein the above multifunctional monomer is a monomer containing two or more photocurable functional groups selected from the group consisting of an acrylate group, a methacrylate group, a vinyl group, and a thiol group.

6. In paragraph 1, An organic-inorganic composite electrolyte membrane in which the sum of the crosslinked polymer matrix, the ionic liquid, and the lithium salt satisfies a weight ratio of 3 to 15:85 to 97.

7. In paragraph 1, An organic-inorganic composite electrolyte membrane in which the cross-linked polymer matrix is ​​included in an amount of 0.5 to 10 parts by weight relative to 100 parts by weight of the sulfide-based solid electrolyte.

8. In paragraph 1, The above porous support is an organic-inorganic composite electrolyte membrane having an average pore size of 50㎛ or more.

9. In paragraph 8, The above porous support is an organic / inorganic composite electrolyte membrane having a thickness of 5 to 40 μm.

10. In paragraph 1, An organic-inorganic composite electrolyte membrane having a thickness of 10 to 40 μm.

11. In paragraph 1, Ionic conductivity is 3.0 x10 -4 Organic / inorganic composite electrolyte membrane with a density of S / cm or more.

12. In paragraph 1, An organic-inorganic composite electrolyte membrane with an ionic conductivity retention rate of 90% or higher after 100 cycles of a 180° bending test.

13. In paragraph 1, An organic / inorganic composite electrolyte membrane having a structure in which two or more organic / inorganic composite electrolyte membranes are laminated in the thickness direction.

14. A method for producing an organic-inorganic composite electrolyte membrane, comprising the step of applying and polymerizing a slurry composition containing a sulfide-based solid electrolyte, a polyfunctional monomer, an ionic liquid, and a lithium salt on a porous support to produce an organic-inorganic composite electrolyte.

15. In paragraph 14, The above ionic liquid is a method for manufacturing an organic-inorganic composite electrolyte membrane including a glyme-based solvent.

16. In paragraph 14, A method for producing an organic-inorganic composite electrolyte membrane, wherein the above slurry composition substantially does not contain a solvent.

17. In paragraph 14, A method for manufacturing an organic-inorganic composite electrolyte membrane, further comprising a step of compressing the organic-inorganic composite electrolyte membrane.

Citation Information

Patent Citations

  • Lithium metal battery

    JP2020526909A

  • All-solid secondary battery

    JP2021077643A

  • Composite electolyte, method for manufacturing the same, and rechargeable battery comprising the same

    KR1020180000195A

  • Cold roll forming method for ultra high strength material

    KR1020240074182A

  • Method and apparatus for generating NFT (Non-Fungible Token) for cosmetics

    KR102503842B1