Cathode active material, method for producing same, and cathode and lithium secondary battery each comprising same

The use of single particle lithium composite transition metal oxide with a layered structure and specific dopants addresses thermal stability and safety concerns in lithium secondary batteries, enhancing performance and stability through a two-stage firing process.

WO2024219804A1PCT designated stage expired Publication Date: 2024-10-24LG CHEM LTD

Patent Information

Application Number
PCT/KR2024/005123
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Lithium secondary batteries face issues with thermal stability and volume expansion due to the use of spherical secondary particle cathode active materials, which can lead to safety risks and performance degradation, particularly when high nickel content is used.

Method used

Development of a single particle lithium composite transition metal oxide with a layered structure, containing Ni, Co, Mn, Al, and M1 (Zr, Y, K, Sr, or Ba), which is manufactured through a two-stage firing process to achieve improved structural stability and particle strength, thereby enhancing battery capacity, efficiency, and lifespan.

Benefits of technology

The single particle lithium composite transition metal oxide exhibits excellent structural stability and particle strength, reducing particle deformation and improving battery performance metrics such as capacity, initial efficiency, and resistance, while minimizing gas generation and residual lithium by-products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention relates to a cathode active material, a method for producing same, and a cathode and a lithium secondary battery each comprising same, the cathode active material being in the form of a single particle and having an almost unchanged particle size distribution even after rolling, due to the small deformation of particles, wherein the cathode active material comprises a lithium composite transition metal oxide in the form of a single particle, and the lithium composite transition metal oxide comprises Ni, Co, Mn, Al, and M1, in which M1 is at least one selected from Zr, Y, K, Sr, and Ba, and satisfies equation 1. [Equation 1] |1-α / β| ≤ 0.1, wherein α is a value of D90-D10) / D50, and β is a value of D90-D10) / D50 after the cathode active material is rolled at 1,000 kgf / cm2 to 7,000 kgf / cm2.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material, method for producing the same, and positive electrode and lithium secondary battery including the same

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0051887, filed April 20, 2023, the entire contents of which are incorporated herein by reference.

[0003] Technology field

[0004] The present invention relates to a positive electrode active material, a method for producing the same, and a positive electrode and a lithium secondary battery comprising the same, and more particularly, to a positive electrode active material comprising a lithium composite transition metal oxide in the form of a single particle capable of improving the performance of a battery, a method for producing the same, and a positive electrode and a lithium secondary battery comprising the same.

[0005]

[0006] With the recent technological development and increasing demand for mobile devices and electric vehicles, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which boast high energy density and voltage, long cycle life, and low self-discharge rates, are commercialized and widely used.

[0007] Lithium transition metal oxides such as lithium cobalt oxide such as LiCoO2, lithium nickel oxide such as LiNiO2, lithium manganese oxide such as LiMnO2 or LiMn2O4, and lithium iron phosphate oxide such as LiFePO4 have been developed as positive electrode active materials for lithium secondary batteries, and recently, Li[Ni a Co b Mn c ]O2, Li[Ni a Co b Al c ]O2, Li[Ni a Co b Mn c Al d] Lithium composite transition metal oxides containing two or more transition metals, such as O2, have been developed and are widely used.

[0008] Lithium composite transition metal oxides containing two or more transition metals developed to date are usually manufactured in the form of spherical secondary particles in which tens to hundreds of primary particles are aggregated. However, in order to solve the structural and thermal stability problems of the secondary particle-type positive electrode active material itself, the development of single-particle positive electrode active materials is accelerating. Specifically, when the secondary particle-type positive electrode active material is applied to a lithium secondary battery, there is a problem that a large amount of gas is generated, causing the volume of the battery to expand. In addition, when the nickel content in the positive electrode material is increased for high capacity, the risk of fire also increases. Accordingly, the demand for the development of single-particle positive electrode active materials with excellent stability is increasing.

[0009] Therefore, there is a need to develop a single particle type cathode active material that has excellent stability and can improve various performances of batteries when applied to batteries.

[0010]

[0011] The present invention is an invention for solving the above problems, and aims to provide a cathode active material including a lithium composite transition metal oxide in the form of a single particle, which has excellent structural stability and can improve the capacity, initial efficiency, lifespan, resistance, etc. of a battery when applied to a battery.

[0012] In addition, the present invention aims to provide a manufacturing method for manufacturing the positive electrode active material.

[0013] In addition, the present invention aims to provide a lithium secondary battery with improved performance, including the positive electrode active material.

[0014]

[0015] To solve the above problem, the present invention provides a positive electrode active material, a method for manufacturing a positive electrode active material, a positive electrode, and a lithium secondary battery.

[0016]

[0017] (1) The present invention provides a cathode active material comprising a lithium composite transition metal oxide in the form of a single particle, wherein the lithium composite transition metal oxide comprises Ni, Co, Mn, Al and M1, wherein M1 is at least one selected from Zr, Y, K, Sr and Ba, and satisfies the following formula 1.

[0018] [Formula 1]

[0019] |1-α / β| ≤ 0.1

[0020] In the above equation 1,

[0021] α is (D 90 -D 10 ) / D 50 is the value, and β is the positive electrode active material at 1,000 kgf / cm 2 Up to 7,000 kgf / cm 2 After rolling (D 90 -D 10 ) / D 50 It's worth it.

[0022] (2) The present invention provides a positive electrode active material in the above (1), wherein the lithium composite transition metal oxide has a layered structure.

[0023] (3) In the present invention, in the above (1) or (2), the lithium composite transition metal oxide has an average particle diameter (D 50 ) provides a positive electrode active material having a diameter of 3.00㎛ to 8.00㎛.

[0024] (4) The present invention provides a positive electrode active material in any one of the above (1) to (3), wherein the lithium composite transition metal oxide is doped with Al and M1.

[0025] (5) The present invention provides a positive electrode active material in any one of the above (1) to (4), wherein Al is included in an amount of 500 ppm to 3,000 ppm based on the total weight of the lithium composite transition metal oxide.

[0026] (6) The present invention provides a positive electrode active material in any one of the above (1) to (5), wherein M1 is included in an amount of 100 ppm to 5,000 ppm based on the total weight of the lithium composite transition metal oxide.

[0027] (7) The present invention provides a positive electrode active material in any one of the above (1) to (6), wherein the lithium composite transition metal oxide contains nickel at 60 mol% or more based on the total molar number of metals excluding lithium.

[0028] (8) The present invention provides a positive electrode active material in any one of the above (1) to (7), wherein the lithium composite transition metal oxide has a composition represented by the following chemical formula 1.

[0029] [Chemical Formula 1]

[0030] Li x [Ni a Co b Mn c Al d M1 e M2 f ]O 2-y A y

[0031] In the above chemical formula 1,

[0032] M1 is at least one selected from Zr, Y, K, Sr, and Ba,

[0033] M2 is at least one selected from B, Ba, Ce, Cr, Mg, V, Ti, Fe, Zn, Si, Nb, Ga, Sn, Mo, W, and P,

[0034] A is at least one selected from F, Cl, Br, I, and S,

[0035] 1.0≤x≤1.3, 0.6≤a<1, 0.0 <b≤0.4, 0.0<c≤0.4, 0.0<d≤0.01, 0.0<e≤0.005, 0.0≤f≤0.2, a+b+c+d+e+f=1, 0≤y≤0.2이다.

[0036] (9) The present invention comprises the steps of: (A) preparing a mixture by mixing a positive electrode active material precursor containing Ni, Co and Mn, an aluminum-containing raw material, an M1-containing raw material and a first lithium-containing raw material;

[0037] (B) a step of first firing the mixture at a temperature of 800°C to 950°C to produce a first fired product; and

[0038] (C) a step of mixing a second lithium-containing raw material into the first fired product and then firing it a second time at a temperature of 680°C to 850°C to manufacture a second fired product;

[0039] The above M1 is at least one selected from Zr, Y, K, Sr and Ba,

[0040] The present invention provides a method for manufacturing a positive electrode active material, wherein the above M1-containing raw material is mixed in an amount of 100 ppm to 5,000 ppm based on the total weight of the positive electrode active material precursor.

[0041] (10) The present invention provides a method for manufacturing a positive electrode active material, which further includes, before step (C), step (B') of crushing the primary sintered product in the above (9).

[0042] (11) The present invention provides a method for manufacturing a positive electrode active material, further comprising the step of crushing the secondary sintered product (C') in the above (9) or (10).

[0043] (12) The present invention provides a positive electrode comprising a positive electrode active material according to any one of (1) to (8).

[0044] (13) The present invention provides a lithium secondary battery comprising a positive electrode according to (12); a negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

[0045]

[0046] The cathode active material of the present invention comprises a lithium composite transition metal oxide in the form of a single particle, wherein the lithium composite transition metal oxide comprises Ni, Co, Mn, Al and M1, wherein M1 is at least one selected from Zr, Y, K, Sr and Ba, and satisfies Equation 1 described in the present specification, so that particle deformation is small and the particle size distribution hardly changes even after rolling, thereby improving the capacity, initial efficiency, lifespan, resistance, etc. of a lithium secondary battery.

[0047] In addition, according to the method for manufacturing a positive electrode active material of the present invention, the positive electrode active material described above can be effectively manufactured.

[0048]

[0049] Hereinafter, the present invention will be described in more detail to help understand the present invention.

[0050] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical spirit of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best possible manner.

[0051]

[0052] It should be understood that the terms “include,” “have,” or “have” used in this specification are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0053] In this specification, the term 'on' means not only when a configuration is formed directly on the top surface of another configuration, but also when a third configuration is interposed between these configurations.

[0054] In this specification, the term "single-particle positive electrode active material" refers to a positive electrode active material composed of 10 or fewer primary particles, in contrast to a spherical secondary particle positive electrode active material formed by agglomeration of tens to hundreds of primary particles manufactured by a conventional method. Specifically, the single-particle positive electrode active material in the present invention may be a single particle composed of one primary particle, or may be a secondary particle in which several primary particles are agglomerated.

[0055] 'Primary particle' refers to the smallest particle unit recognized when observing a positive electrode active material through a scanning electron microscope, and 'secondary particle' refers to a secondary structure formed by the aggregation of multiple primary particles.

[0056] In this specification, the term 'average particle diameter (D 50 )' means the particle size at the 50% point of the volume cumulative distribution according to particle size. The above average particle size is calculated by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., S3500 from Microtrac), and measuring the difference in diffraction pattern according to particle size when the particles pass through the laser beam to calculate the particle size distribution, and calculating the particle diameter at the point where it becomes 50% of the volume cumulative distribution according to particle size in the measuring device, thereby obtaining D 50 can be measured.

[0057]

[0058] positive electrode active material

[0059] The present invention provides a cathode active material comprising a lithium composite transition metal oxide in the form of a single particle, wherein the lithium composite transition metal oxide comprises Ni, Co, Mn, Al and M1, wherein M1 is at least one selected from Zr, Y, K, Sr and Ba, and satisfies the following formula 1. The lithium composite transition metal oxide may have a layered structure.

[0060] [Formula 1]

[0061] |1-α / β| ≤ 0.1

[0062] In the above equation 1,

[0063] α is (D 90 -D 10 ) / D 50 is the value, and β is the positive electrode active material at 1,000 kgf / cm 2 Up to 7,000 kgf / cm 2 After rolling (D 90 -D 10 ) / D 50 It's worth it.

[0064]

[0065] The present inventors have found that when a positive electrode active material comprises a lithium composite transition metal oxide in the form of a single particle, and the lithium composite transition metal oxide comprises Ni, Co, Mn, Al, and M1, and satisfies Equation 1, the particle deformation of the positive electrode active material is small, thereby improving various performances of a lithium secondary battery, and have completed the present invention. Specifically, the present inventors have found that when the lithium composite transition metal oxide essentially contains Al, Al replaces the positions of some transition metal ions in the crystal structure, thereby increasing structural stability, thereby improving the performance of a lithium secondary battery, and when M1 is simultaneously included, a positive electrode active material having excellent particle strength and a large grain size can be provided. On the other hand, when the positive electrode active material does not contain Al, the thermal and structural stability of the positive electrode active material is low, and this causes problems in the performance of the battery because the oxide lattice is deformed during charge and discharge cycles. When M1 is not included, there is a problem that does not satisfy Equation 1, that is, a problem of low particle strength and / or a problem of small grain size.

[0066] According to the present invention, the M1, which is at least one selected from Zr, Y, K, Sr, and Ba, is an element capable of improving the crystallinity and single-particle degree of the positive electrode active material, and specifically, may be at least two selected from Zr, Y, K, Sr, and Ba, and more specifically, may be Zr and Y.

[0067] According to the present invention, the value according to the above formula 1 may be 0.1 or less, specifically 0.1, 0.09, 0.08, 0.07, 0.06, 0.05 or less. This means that the particle strength of the positive electrode active material is excellent, so that deformation is small even when pressure is applied to the positive electrode active material. When the value according to the above formula 1 is within the above range, the battery capacity, initial efficiency, lifespan, resistance performance, etc. of the battery including the positive electrode active material may be excellent. On the other hand, when the value according to the above formula 1 exceeds 0.1, there is a problem that the lifespan and resistance performance are inferior because the particle strength is low, which increases particle destruction in the electrode.

[0068]

[0069] According to the present invention, the lithium composite transition metal oxide has an average particle diameter (D 50 ) may be 3.00㎛ to 8.00㎛. The average particle diameter (D of the lithium composite transition metal oxide 50) Specifically, the average particle size (D) of the lithium composite transition metal oxide may be 3.00 ㎛, 3.50 ㎛ or more, 7.00 ㎛, 7.50 ㎛, or 8.00 ㎛ or less. 50 ) is within the above range, the electrochemical performance can be optimized.

[0070]

[0071] According to the present invention, the lithium composite transition metal oxide may be doped with Al and M1. In this case, that is, when the lithium composite transition metal oxide includes Al and M1 as dopants, the structural stability of the positive electrode active material is further increased, cation mixing is reduced, and the grain size is large, so that the capacity, initial efficiency, lifespan, and resistance performance of the lithium secondary battery can be further improved.

[0072] In order to increase the grain size while further improving the structural stability of the cathode active material in the form of single particles with a small average particle diameter, the lithium composite transition metal oxide may be doped with Al, Zr and Y, more specifically.

[0073]

[0074] According to the present invention, the Al may be included in an amount of 500 ppm to 3,000 ppm based on the total weight of the lithium composite transition metal oxide. In this case, the internal crystal structure of the positive electrode active material may be stabilized, thereby improving the capacity and resistance performance of the battery.

[0075]

[0076] According to the present invention, the M1 may be included in an amount of 100 ppm to 5,000 ppm based on the total weight of the lithium composite transition metal oxide.

[0077] Meanwhile, when the M1 is Y and Zr, the Y may be included in an amount of 100 ppm to 2,000 ppm based on the total weight of the lithium composite transition metal oxide, and the Zr may be included in an amount of 500 ppm to 5,000 ppm based on the total weight of the lithium composite transition metal oxide. When the content of the Y is within the above range, the grain size included in one particle is large, so that the capacity and life performance of the battery may be improved, and when the content of the Zr is within the above range, the Zr is stably doped into the lithium layer, so that the structural stability is improved during the insertion and de-insertion of lithium, and as a result, the particle strength is excellent, so that the life and resistance performance of the battery may be improved.

[0078]

[0079] According to the present invention, the lithium composite transition metal oxide may contain nickel in an amount of 60 mol% or more, specifically, 80 mol% or more, and more specifically, 85 mol% or more, based on the total moles of metals excluding lithium. That is, the lithium composite transition metal oxide may be a high-nickel (High Ni) lithium composite transition metal oxide. In this case, the energy density of a lithium secondary battery can be improved.

[0080] According to the present invention, the lithium composite transition metal oxide may have a composition represented by the following chemical formula 1. In this case, the lithium composite transition metal oxide has a layered structure.

[0081] [Chemical Formula 1]

[0082] Li x [Ni a Co b Mn c Al d M1 e M2 f ]O 2-y A y

[0083] In the above chemical formula 1,

[0084] M1 is at least one selected from Zr, Y, K, Sr, and Ba,

[0085] M2 is at least one selected from B, Ba, Ce, Cr, Mg, V, Ti, Fe, Zn, Si, Nb, Ga, Sn, Mo, W, and P,

[0086] A is at least one selected from F, Cl, Br, I, and S,

[0087] 1.0≤x≤1.3, 0.6≤a<1, 0.0 <b≤0.4, 0.0<c≤0.4, 0.0<d≤0.01, 0.0<e≤0.005, 0.0≤f≤0.2, a+b+c+d+e+f=1, 0≤y≤0.2이다.

[0088] The above a refers to the atomic fraction of nickel among the metal elements in the lithium composite transition metal oxide, and may be 0.6, 0.8, 0.85 or more, 0.95, 0.98, or 1.0 or less.

[0089] The above b refers to the atomic fraction of cobalt among the metal elements in the lithium composite transition metal oxide, and may be 0.0, 0.01 or more, 0.15, 0.2, or 0.4 or less.

[0090] The above c refers to the atomic fraction of manganese among the metal elements in the lithium composite transition metal oxide, and may be 0.0, 0.01 or more, 0.15, 0.2, or 0.4 or less.

[0091] The above d refers to the atomic fraction of aluminum among the metal elements in the lithium composite transition metal oxide, and may be greater than 0.0, 0.002, 0.003 or more, 0.006, 0.008, or 0.01 or less.

[0092] The above e refers to the atomic fraction of the M1 element among the metal elements in the lithium composite transition metal oxide, and may be greater than 0.0, 0.0001, 0.0002, 0.0006 or more, and 0.002, 0.003, 0.005 or less.

[0093] The above f refers to the atomic fraction of the M2 element among the metal elements in the lithium composite transition metal oxide, and may be 0.0 or more, 0.05, 0.1, or 0.2 or less.

[0094]

[0095] According to the present invention, the positive electrode active material may further include a coating portion including Co formed on the lithium composite transition metal oxide in the form of a single particle. The coating portion may further include Al, Zr, or a combination thereof. When the positive electrode active material further includes the coating portion, the amount of residual lithium byproducts may be reduced, structural stability may be increased, and thus the lifespan and resistance performance of the battery may be improved, and the amount of gas generated may also be reduced. At this time, the coating portion may have a thin film form, and may be formed on the entire surface of the lithium composite transition metal oxide or may be formed locally.

[0096]

[0097] Co present in the above coating portion may be included in an amount of 0.5 mol% to 3 mol% based on the total moles of metals excluding lithium included in the lithium composite transition metal oxide. In this case, residual lithium byproducts can be further reduced, and lifespan and resistance performance can be further improved.

[0098] The Al present in the above coating portion may be included in an amount of 300 ppm to 10,000 ppm based on the total weight of the lithium composite transition metal oxide. In this case, structural stability may be further enhanced, thereby further improving lifespan and resistance performance.

[0099]

[0100] Method for manufacturing positive electrode active material

[0101] The present invention provides a method for producing the above-described positive electrode active material. That is, the positive electrode active material according to the present invention is produced by the following method for producing a positive electrode active material.

[0102] A method for manufacturing a positive electrode active material according to the present invention comprises the steps of: (A) mixing a positive electrode active material precursor containing Ni, Co, and Mn, an aluminum-containing raw material, an M1-containing raw material, and a first lithium-containing raw material to manufacture a mixture; (B) firing the mixture for the first time at a temperature of 800°C to 950°C to manufacture a first fired product; and (C) mixing a second lithium-containing raw material into the first fired product, and then firing the mixture for the second time at a temperature of 680°C to 850°C to manufacture a second fired product. In this case, M1 is at least one selected from Zr, Y, K, Sr, and Ba, and the M1-containing raw material is mixed in an amount of 100 ppm to 5,000 ppm based on the total weight of the positive electrode active material precursor.

[0103] The present inventors have discovered that when lithium is introduced in stages (A) and (C), sintering is performed in two stages, and M1 is introduced as a dopant in a specific amount or more before the first sintering, a lithium transition metal oxide in the form of a single particle is produced, and the particle deformation of the positive electrode active material is small, so that the particle size distribution does not change much even after rolling, thereby completing the present invention.

[0104]

[0105] The positive electrode active material precursor containing the above Ni, Co and Mn may have a composition represented by the following chemical formula 2 or chemical formula 3.

[0106] [Chemical Formula 2]

[0107] Ni a' Co b' Mn c' M2 d' (OH)2

[0108] [Chemical Formula 3]

[0109] Ni a' Co b' Mn c' M2 d' O·OH

[0110] In the above chemical formulas 2 and 3,

[0111] M2 is at least one selected from B, Ba, Ce, Cr, Mg, V, Ti, Fe, Zn, Si, Nb, Ga, Sn, Mo, W, and P,

[0112] 0.6≤a'<1, 0.0 <b'≤0.4, 0.0<c'≤0.4, 0.0≤d'≤0.2이다.

[0113]

[0114] The above aluminum-containing raw material may be at least one selected from Al(OH)3, Al2O3, AlCl3, Al(NO)3, AlSO4, and Al2S3, specifically at least one selected from Al(OH)3, Al2O3, and Al(NO)3, and more specifically Al(OH)3. The above aluminum-containing raw material may be added in an amount of 500 ppm to 3,000 ppm based on the total weight of the positive electrode active material precursor. Specifically, the content of the aluminum-containing raw material may be 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1,000 ppm, 1,100 ppm, 1,200 ppm, 1,300 ppm, 1,400 ppm or more and 2,800 ppm, 2,900 ppm or less than 3,000 ppm based on the total weight of the positive electrode active material precursor. In this case, the internal crystal structure of the positive electrode active material is stabilized, so there is an advantage of better life performance of the battery.

[0115]

[0116] The above M1-containing raw material may be, but is not limited to, M1-containing hydroxides, oxides, chlorides, nitrates, sulfur oxides, sulfides, etc.

[0117] Meanwhile, when the above M1 is Y, the yttrium (Y)-containing raw material may be at least one selected from YCl3, Y2O3, Y(NO3)3, Y(OH)3, YSZ, Y2(SO4)3, and Y2S3, specifically at least one selected from Y2O3 and Y(OH)3, and more specifically Y2O3. The yttrium-containing raw material may be added in an amount of 100 ppm to 2,000 ppm based on the total weight of the positive electrode active material precursor. Specifically, the content of the yttrium-containing raw material may be 100 ppm, 200 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1,000 ppm or more, and 2,000 ppm or less, based on the total weight of the positive electrode active material precursor. In this case, since the grain size contained in one particle is large, the capacity and life performance of the battery can be further improved.

[0118] In addition, when the above M1 is Zr, the zirconium-containing raw material is Zr(OH)4, ZrO2, Zr(NO3)4, ZrCl4, ZrS2, Zr(SO4)2 and C8H 12 It may be at least one selected from O8Zr, specifically at least one selected from Zr(OH)4 and ZrO2, and more specifically ZrO2. The zirconium-containing raw material may be added in an amount of 500 ppm to 5000 ppm based on the total weight of the positive electrode active material precursor. Specifically, the amount of the zirconium-containing raw material may be 500 ppm, 1000 ppm, 1,500 ppm or more, 3,000 ppm, 3,500 ppm, 4,000 ppm, 4,500 ppm, or 5,000 ppm or less based on the total weight of the positive electrode active material precursor. In this case, Zr is stably doped into the lithium layer, so that the structural stability is further improved during the insertion and de-insertion of lithium, and there is an advantage that the particle strength is also improved.

[0119]

[0120] When the mixture is first fired at a temperature of 800°C to 950°C, the primary particles of the positive electrode active material precursor aggregate to produce a primary fired product in the form of single particles. Specifically, the primary firing temperature may be 800°C, 810°C, 820°C, 830°C, 840°C, 850°C or higher, and 900°C, 910°C, 920°C, 930°C, 940°C, or 950°C or lower. When the primary firing temperature is within the above range, the primary particles of the positive electrode active material precursor aggregate to form a structurally stable primary fired product in the form of single particles. When the primary firing temperature is less than 800°C, there is a problem that the primary particles do not sufficiently aggregate, and when it is more than 950°C, there is a problem that a structurally unstable fired product with low crystallinity is produced.

[0121] The above first calcination may be performed under an oxygen atmosphere in order to prevent the lithium transition metal oxide from degenerating into a rock salt structure.

[0122] The above first firing may be performed for 3 to 12 hours, specifically 3 hours, 4 hours, 5 hours, 6 hours or more and 9 hours, 10 hours, 11 hours, or 12 hours or less, in order to agglomerate the primary particles and improve the crystallinity of the first fired product.

[0123]

[0124] When the above-mentioned first fired product is subjected to a second firing at a temperature of 680°C to 850°C, lithium is inserted into the first fired product, thereby producing a second fired product. At this time, the second fired product is a lithium composite transition metal oxide in the form of single particles. Specifically, the second firing temperature may be 680°C, 700°C, 720°C, 740°C, 760°C, 780°C, 800°C or higher, 840°C, or 850°C or lower. When the second firing temperature is within the above range, lithium is inserted into the rock salt structure that may be formed on the surface of the first fired product due to the high temperature during the first firing, thereby restoring it to a layered structure, and there is an advantage of reducing lithium byproducts. Meanwhile, when the secondary firing temperature is lower than 680℃, there is a problem that the lithium insertion speed is slow due to the low temperature, and when it is higher than 850℃, there is a problem that the surface of the primary firing product degenerates into a rock salt structure due to the high temperature, and lithium byproducts remain.

[0125] The above secondary calcination may be performed under an oxygen atmosphere in order to prevent the lithium transition metal oxide from degenerating into a rock salt structure.

[0126] The above secondary firing may be performed for 3 to 12 hours, specifically 3 hours, 4 hours, 5 hours, 6 hours, 9 hours or more, and 9 hours, 10 hours, 11 hours, or 12 hours or less, in order to increase the crystallinity of the internal crystal structure of the positive electrode active material.

[0127]

[0128] The method for manufacturing a cathode active material according to the present invention may further include, before step (C), a step (B') of crushing the first sintered product. In order to prevent the initial resistance from increasing, step (B') crushes the first sintered product to have an average particle diameter (D 50 ) may be ground to a size of 3.50㎛ to 6.00㎛.

[0129] The method for manufacturing a cathode active material according to the present invention may further include a step (C') of crushing the secondary sintered product. In addition, in the step (C'), the secondary sintered product is crushed to have an average particle diameter (D) in order to prevent the initial resistance from increasing. 50 ) may be ground to a size of 3.50㎛ to 6.00㎛.

[0130] The grinding of the above steps (B') and (C') can be performed using a pin mill, an ACM, a jet mill, etc. Meanwhile, the pin mill can be performed under conditions of 18,000 rpm, the ACM can be performed under conditions of 6,000 rpm for classification and 12,000 rpm for main processing using a device from Hosokawa, and the jet mill can be performed under conditions of 6 bar for grinding pressure and 3,500 rpm for classification using a device from ZM solution. In this case, the desired average particle size (D 50 ) can be easily obtained.

[0131]

[0132] The cathode active material according to the present invention is manufactured by a process in which lithium-containing raw materials are introduced in two stages. That is, the lithium-containing raw materials are introduced separately before the first firing and before the second firing. In this case, there is an advantage in that lithium is inserted into the rock salt structure that may be formed on the surface, thereby facilitating recovery into a layered structure. On the other hand, if the lithium-containing raw materials are introduced all at once before the first firing, there is a problem of deterioration in electrochemical performance due to an increase in lithium byproducts. In addition, if the lithium-containing raw materials are not introduced in the second firing stage, problems arise in that a slow reaction rate, high temperature, and long time are required.

[0133] In the case where the lithium-containing raw material is input in two portions, in the step (A), the first lithium-containing raw material may be mixed so that the ratio (M:Li) of the total mole number (M) of the transition metal included in the positive electrode active material precursor and the mole number (Li) of lithium included in the first lithium-containing raw material is 1:0.98, 1:0.99, 1:1.00, 1:1.01, 1:1.02 or more, 1:1.04, 1:1.05 or less, and in the step (C), the second lithium-containing raw material may be mixed so that the ratio (M:Li) of the total mole number (M) of the transition metal included in the positive electrode active material precursor of the step (A) and the mole number (Li) of lithium included in the second lithium-containing raw material is 1:0.01 or more, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, It can be mixed to a ratio of 1:1.10 or less.

[0134]

[0135] The method for manufacturing a cathode active material according to the present invention may further include the step of (D) mixing the secondary sintered product and a cobalt-containing coating material, followed by heat treatment. In this case, a coating portion containing Co is formed on the secondary sintered product (lithium composite transition metal oxide in the form of single particles).

[0136] According to the present invention, when mixing the secondary sintered product and the cobalt-containing coating material in step (D), an aluminum-containing coating material, a zirconium-containing coating material, or a combination thereof may be further mixed. In this case, the coating portion may further include Al, Zr, or a combination thereof in addition to Co.

[0137] According to the present invention, the cobalt-containing coating material may be mixed in an amount such that the ratio (B / A) of the number of moles of cobalt (B) contained in the cobalt-containing coating material to the total number of moles (A) of metals excluding lithium contained in the secondary fired product is 0.01 to 0.03. In this case, there is an advantage in that lithium byproducts can be controlled in a cathode active material manufacturing process that does not include a washing process.

[0138] The above cobalt-containing coating material may be at least one selected from Co(OH)2, Co3O4, CoO, (CH3CO2)2Co, CoCl2, and CoSO4·xH2O, and specifically may be Co(OH)2.

[0139] According to the present invention, the aluminum-containing coating material may be mixed in an amount of 0.03 to 0.10 parts by weight per 100 parts by weight of the secondary fired product. In this case, structural stability can be secured, thereby improving service life, resistance, and gas generation.

[0140] The above aluminum-containing coating material may be at least one selected from Al(OH)3, Al2(SO4)3·xH2O, Al2O3, Al(NO3)3·9H2O, AlCl3, and C2H5O4Al, and specifically may be Al(OH)3.

[0141] The above zirconium-containing coating materials are Zr(OH)4, ZrO2, Zr(NO3)4, ZrCl4, ZrS2, Zr(SO4)2 and C8H 12 It can be one or more types selected from O8Zr.

[0142]

[0143] According to the present invention, the heat treatment may be performed under an oxygen atmosphere to prevent the lithium transition metal oxide from degenerating into a rock salt structure.

[0144]

[0145] According to the present invention, the heat treatment may be performed at a temperature of 600°C, 610°C, 620°C, 630°C, 640°C, 650°C or higher and 720°C, 740°C, 760°C, 780°C, or 800°C or lower, and then the temperature may be lowered to about 450°C to 550°C, and then the heat treatment may be performed at a temperature of 450°C, 460°C, 470°C, 480°C or higher and 520°C, 530°C, 540°C, or 550°C or lower, so that the coating portion is formed to an appropriate thickness. That is, the heat treatment may be performed at 600°C to 800°C in one firing profile, and then the heat treatment may be performed at 450°C to 550°C.

[0146]

[0147] According to the present invention, the heat treatment may be performed for a time of 1 hour, 2 hours, 3 hours or more, 8 hours, 9 hours or less, or 10 hours or less in order to increase the crystallinity of the coating portion.

[0148]

[0149] anode

[0150] The present invention provides a positive electrode comprising the positive electrode active material.

[0151] The positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer may include the positive electrode active material.

[0152] The positive electrode current collector may include a highly conductive metal, and is not particularly limited as long as it is easily adhered to by the positive electrode active material layer and does not react within the voltage range of the battery. The positive electrode current collector may be made of, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode current collector may typically have a thickness of 3 ㎛ to 500 ㎛, and fine unevenness may be formed on the surface of the current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0153] The above-mentioned positive electrode active material layer may optionally include a conductive material and a binder, together with the positive electrode active material, as needed. In this case, the positive electrode active material may be included in an amount of 80 wt% to 99 wt%, more specifically 85 wt% to 98.5 wt%, based on the total weight of the positive electrode active material layer, and excellent capacity performance may be exhibited within this range.

[0154] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used. The conductive material may be included in an amount of 0.1 wt% to 15 wt% based on the total weight of the positive electrode active material layer.

[0155] The above binder serves to improve the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylalcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, polyacrylic acid, and polymers in which hydrogens of these are substituted with Li, Na, or Ca, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The above binder may be included in an amount of 0.1 wt% to 15 wt% based on the total weight of the positive electrode active material layer.

[0156] The positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the positive electrode active material described above is used. Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, which is manufactured by dissolving or dispersing the positive electrode active material and optionally a binder, a conductive agent, and a dispersant in a solvent as needed, onto a positive electrode current collector, followed by drying and rolling, or by casting the composition for forming a positive electrode active material layer onto a separate support, peeling the film from the support, and laminating the resulting film onto a positive electrode current collector.

[0157] The solvent may be a solvent generally used in the relevant technical field, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethylformamide (DMF), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, binder, and dispersant in consideration of the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0158]

[0159] lithium secondary battery

[0160] The present invention provides a lithium secondary battery comprising: the positive electrode; the negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

[0161]

[0162] The above lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, negative electrode, and separator, and a sealing member that seals the battery container.

[0163]

[0164] The above negative electrode may include a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0165] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0166] The above negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material.

[0167] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO β(0<β<2), SnO2, vanadium oxide, lithium vanadium oxide, and other metal oxides capable of doping and dedoping lithium; or composites containing the above metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical or fibrous shapes, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes. The negative electrode active material may be included in an amount of 80 wt% to 99 wt% based on the total weight of the negative electrode active material layer.

[0168] The binder of the above-described negative electrode active material layer is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 wt% to 10 wt% based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0169] The conductive material of the above-described negative electrode active material layer is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10 wt% or less, preferably 5 wt% or less, based on the total weight of the negative electrode active material layer. The conductive material is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; fluorinated carbon; metal powder such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0170] The above negative electrode can be manufactured by applying and drying a composition for forming a negative electrode active material layer prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector, or by casting the composition for forming a negative electrode active material layer on a separate support, and then laminating the film obtained by peeling it off from the support on a negative electrode current collector.

[0171] The above separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without any particular restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.

[0172] Examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries. As a specific example, the electrolyte may include an organic solvent and a lithium salt.

[0173] As the organic solvent, any solvent that can serve as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without particular limitation. Specifically, the organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylenecarbonate (EC), and propylene carbonate (PC); Alcohol solvents such as ethyl alcohol, isopropyl alcohol, etc.; nitriles such as R-CN (R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes, etc. can be used. Among these, carbonate solvents are preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferable.

[0174] The above lithium salt can be used without any special limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the anion of the above lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - At least one selected from the group consisting of may be used, and the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. It is preferable to use the concentration of the lithium salt within the range of 0.1 M to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0175] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the lifespan of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 wt% to 5 wt% based on the total weight of the electrolyte.

[0176]

[0177] Since the lithium secondary battery including the positive electrode active material according to the present invention has excellent performance, it is useful in the fields of portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs) and electric vehicles (EVs).

[0178] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.

[0179] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also be preferably used as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.

[0180] Accordingly, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.

[0181] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0182]

[0183] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0184]

[0185] Examples and Comparative Examples

[0186] Example 1

[0187] A composite transition metal hydroxide in the form of secondary particles formed by the agglomeration of tens to hundreds of primary particles (composition: Ni) 0.885 Co 0.035 Mn 0.08 (OH)2, average particle size (D) 50 ): 4.20㎛) and LiOH were mixed so that the ratio of the total mole number of transition metals (Ni+Co+Mn) included in the complex transition metal hydroxide and the mole number of lithium (Li) included in LiOH ((Ni+Co+Mn):Li) was 1:1.03, and Al(OH)3 (KC Daejoo Co., Ltd.) was added in an amount of 1400 ppm based on the total weight of the complex transition metal hydroxide, Y2O3 (Neo performance Co., Ltd.) was added in an amount of 1000 ppm based on the total weight of the complex transition metal hydroxide, and ZrO2 (R&F Co., Ltd.) was added in an amount of 1500 ppm based on the total weight of the complex transition metal hydroxide, and mixed to prepare a mixture.

[0188] The above mixture was first fired at 890°C for 6 hours to obtain a first fired product, and the first fired product was subjected to a first firing at room temperature with an average particle diameter (D 50 ) was crushed to 3.80㎛.

[0189] The crushed primary calcined product and LiOH were mixed so that the ratio of the total mole number of transition metals (Ni+Co+Mn) included in the above complex transition metal hydroxide and the mole number of lithium (Li) included in LiOH ((Ni+Co+Mn):Li) was 1:0.01, and the secondary calcined product was obtained by crushing the secondary calcined product at room temperature to obtain an average particle size (D 50 ) is a lithium composite transition metal oxide in the form of a single particle with a diameter of 3.80㎛ (composition: LiNi 0.87836 Co 0.03493 Mn 0.07985 Al 0.00499 Y 0.00027 Zr 0.0016 O2) was obtained.

[0190] After uniformly mixing the lithium composite transition metal oxide in the form of a single particle with Co(OH)2 (Huayou) and Al(OH)3 (KC Daejoo), heat treatment was performed in an oxygen atmosphere at a temperature of 700°C for 5 hours and at a temperature of 500°C for 3 hours, thereby manufacturing a positive electrode active material in which a coating portion including Co and Al was formed on the lithium composite transition metal oxide in the form of a single particle. At this time, the Co(OH)2 was mixed in an amount such that the ratio (B / A) of the number of moles of cobalt (B) included in the cobalt-containing coating material to the total number of moles (A) of metals excluding lithium included in the lithium composite transition metal oxide in the form of a single particle was 0.02, and the Al(OH)3 was mixed in an amount of 0.05 part by weight per 100 parts by weight of the lithium composite transition metal oxide in the form of a single particle.

[0191]

[0192] Example 2

[0193] A composite transition metal hydroxide in the form of secondary particles formed by the agglomeration of tens to hundreds of primary particles (composition: Ni) 0.885 Co 0.035 Mn 0.08 (OH)2, average particle size (D) 50 ): 4.20㎛) and LiOH were mixed so that the ratio of the total mole number of transition metals (Ni+Co+Mn) included in the complex transition metal hydroxide and the mole number of lithium (Li) included in LiOH ((Ni+Co+Mn):Li) was 1:1.03, and Al(OH)3 (KC Daejoo Co., Ltd.) was added in an amount of 1400 ppm based on the total weight of the complex transition metal hydroxide, Y2O3 (Neo performance Co., Ltd.) was added in an amount of 2000 ppm based on the total weight of the complex transition metal hydroxide, and ZrO2 (R&F Co., Ltd.) was added in an amount of 1500 ppm based on the total weight of the complex transition metal hydroxide, and mixed to prepare a mixture.

[0194] The above mixture was first fired at 890°C for 6 hours to obtain a first fired product, and the first fired product was subjected to a first firing at room temperature with an average particle diameter (D 50 ) was crushed to 3.80㎛.

[0195] The crushed primary calcined product and LiOH were mixed so that the ratio of the total mole number of transition metals (Ni+Co+Mn) included in the above complex transition metal hydroxide and the mole number of lithium (Li) included in LiOH ((Ni+Co+Mn):Li) was 1:0.01, and the secondary calcined product was obtained by crushing the secondary calcined product at room temperature to obtain an average particle size (D 50 ) is a lithium composite transition metal oxide in the form of a single particle with a diameter of 3.80㎛ (composition: LiNi 0.87813 Co 0.03492 Mn 0.07983 Al 0.00499 Y 0.00054 Zr 0.00159 O2) was obtained.

[0196] After uniformly mixing the lithium composite transition metal oxide in the form of a single particle with Co(OH)2 (Huayou) and Al(OH)3 (KC Daejoo), heat treatment was performed in an oxygen atmosphere at a temperature of 700°C for 5 hours and at a temperature of 500°C for 3 hours, thereby manufacturing a positive electrode active material in which a coating portion including Co and Al was formed on the lithium composite transition metal oxide in the form of a single particle. At this time, the Co(OH)2 was mixed in an amount such that the ratio (B / A) of the number of moles of cobalt (B) included in the cobalt-containing coating material to the total number of moles (A) of metals excluding lithium included in the lithium composite transition metal oxide in the form of a single particle was 0.02, and the Al(OH)3 was mixed in an amount of 0.05 part by weight per 100 parts by weight of the lithium composite transition metal oxide in the form of a single particle.

[0197]

[0198] Example 3

[0199] A composite transition metal hydroxide in the form of secondary particles formed by the agglomeration of tens to hundreds of primary particles (composition: Ni) 0.885 Co 0.035 Mn 0.08 (OH)2, average particle size (D) 50 ): 4.20㎛) and LiOH were mixed so that the ratio of the total mole number of transition metals (Ni+Co+Mn) included in the complex transition metal hydroxide and the mole number of lithium (Li) included in LiOH ((Ni+Co+Mn):Li) was 1:1.03, and Al(OH)3 (KC Daejoo Co., Ltd.) was added in an amount of 2800 ppm based on the total weight of the complex transition metal hydroxide, Y2O3 (Neo performance Co., Ltd.) in an amount of 1000 ppm based on the total weight of the complex transition metal hydroxide, and ZrO2 (R&F Co., Ltd.) in an amount of 1500 ppm based on the total weight of the complex transition metal hydroxide, and mixed to prepare a mixture.

[0200] The above mixture was first fired at 890°C for 6 hours to obtain a first fired product, and the first fired product was subjected to a first firing at room temperature with an average particle diameter (D50 ) was crushed to 3.80㎛.

[0201] The crushed primary calcined product and LiOH were mixed so that the ratio of the total mole number of transition metals (Ni+Co+Mn) included in the above complex transition metal hydroxide and the mole number of lithium (Li) included in LiOH ((Ni+Co+Mn):Li) was 1:0.01, and the secondary calcined product was obtained by crushing the secondary calcined product at room temperature to obtain an average particle size (D 50 ) is a lithium composite transition metal oxide in the form of a single particle with a diameter of 3.80㎛ (composition: LiNi 0.87338 Co 0.03493 Mn 0.07985 Al 0.00998 Y 0.00027 Zr 0.00159 O2) was obtained.

[0202] After uniformly mixing the lithium composite transition metal oxide in the form of a single particle with Co(OH)2 (Huayou) and Al(OH)3 (KC Daejoo), heat treatment was performed in an oxygen atmosphere at a temperature of 700°C for 5 hours and at a temperature of 500°C for 3 hours, thereby manufacturing a positive electrode active material in which a coating portion including Co and Al was formed on the lithium composite transition metal oxide in the form of a single particle. At this time, the Co(OH)2 was mixed in an amount such that the ratio (B / A) of the number of moles of cobalt (B) included in the cobalt-containing coating material to the total number of moles (A) of metals excluding lithium included in the lithium composite transition metal oxide in the form of a single particle was 0.02, and the Al(OH)3 was mixed in an amount of 0.05 part by weight per 100 parts by weight of the lithium composite transition metal oxide in the form of a single particle.

[0203]

[0204] Example 4

[0205] A composite transition metal hydroxide in the form of secondary particles formed by the agglomeration of tens to hundreds of primary particles (composition: Ni) 0.885 Co 0.035 Mn 0.08(OH)2, average particle size (D) 50 ): 4.20㎛) and LiOH were mixed so that the ratio of the total mole number of transition metals (Ni+Co+Mn) included in the complex transition metal hydroxide and the mole number of lithium (Li) included in LiOH ((Ni+Co+Mn):Li) was 1:1.03, and Al(OH)3 (KC Daejoo Co., Ltd.) was added in an amount of 1400 ppm based on the total weight of the complex transition metal hydroxide, Y2O3 (Neo performance Co., Ltd.) was added in an amount of 1000 ppm based on the total weight of the complex transition metal hydroxide, and ZrO2 (R&F Co., Ltd.) was added in an amount of 3000 ppm based on the total weight of the complex transition metal hydroxide, and mixed to prepare a mixture.

[0206] The above mixture was first fired at 890°C for 6 hours to obtain a first fired product, and the first fired product was subjected to a first firing at room temperature with an average particle diameter (D 50 ) was crushed to 3.80㎛.

[0207] The crushed primary calcined product and LiOH were mixed so that the ratio of the total mole number of transition metals (Ni+Co+Mn) included in the above complex transition metal hydroxide and the mole number of lithium (Li) included in LiOH ((Ni+Co+Mn):Li) was 1:0.01, and the secondary calcined product was obtained by crushing the secondary calcined product at room temperature to obtain an average particle size (D 50 ) is a lithium composite transition metal oxide in the form of a single particle with a diameter of 3.80㎛ (composition: LiNi 0.87651 Co 0.03486 Mn 0.07968 Al 0.00498 Y 0.00027 Zr 0.0037 O2) was obtained.

[0208] After uniformly mixing the lithium composite transition metal oxide in the form of a single particle with Co(OH)2 (Huayou) and Al(OH)3 (KC Daejoo), heat treatment was performed in an oxygen atmosphere at a temperature of 700°C for 5 hours and at a temperature of 500°C for 3 hours, thereby manufacturing a positive electrode active material in which a coating portion including Co and Al was formed on the lithium composite transition metal oxide in the form of a single particle. At this time, the Co(OH)2 was mixed in an amount such that the ratio (B / A) of the number of moles of cobalt (B) included in the cobalt-containing coating material to the total number of moles (A) of metals excluding lithium included in the lithium composite transition metal oxide in the form of a single particle was 0.02, and the Al(OH)3 was mixed in an amount of 0.05 parts by weight per 100 parts by weight of the lithium composite transition metal oxide in the form of a single particle.

[0209]

[0210] Comparative Example 1

[0211] Lithium composite transition metal oxide in single particle form (composition: LiNi) was prepared in the same manner as in Example 1, except that Y2O3 was not added during the preparation of the mixture. 0.8786 Co 0.03494 Mn 0.07987 Al 0.00499 Zr 0.0016 A positive electrode active material having a coating portion including Co and Al formed on O2) was manufactured.

[0212]

[0213] Comparative Example 2

[0214] Lithium composite transition metal oxide in single particle form (composition: LiNi) was prepared in the same manner as in Example 1, except that Al(OH)3 was not added during the preparation of the mixture. 0.88336 Co 0.03493 Mn 0.07985 Y 0.00027 Zr 0.00159 A positive electrode active material having a coating portion including Co and Al formed on O2) was manufactured.

[0215]

[0216] Comparative Example 3

[0217] Lithium composite transition metal oxide in single particle form (composition: LiNi) was prepared in the same manner as in Example 1, except that ZrO2 was not added during the preparation of the mixture. 0.87976 Co 0.03499 Mn 0.07998 Al 0.005 Y 0.00027 A positive electrode active material having a coating portion including Co and Al formed on O2) was manufactured.

[0218]

[0219] Experimental example

[0220] Experimental Example 1: Particle Size Analysis of Positive Electrode Active Material

[0221] After taking 0.01 g of each of the positive electrode active materials (powder) manufactured in Examples 1 to 4 and Comparative Examples 1 to 3, put them in a vial containing 30 ml of ultrapure water and 500 μl of dispersant, disperse the positive electrode active materials for 1 minute using a sonicator, and then put them in a particle size analyzer (PSA) (Microtrac, S3500), and the D of each positive electrode active material 10 , D 50 , D 90 Obtain the value, α = (D 90 -D 10 ) / D 50 The value was calculated. At this time, D 10 , D 50 , D 90 refers to the particle size at 10%, 50%, and 90% of the cumulative volume distribution according to particle size.

[0222]

[0223] Then, 3g of each of the positive electrode active materials (powder) manufactured in Examples 1 to 4 and Comparative Examples 1 to 3 was taken, and then 6,780.6kgf / cm was used using an automatic pellet press (Auto Pellet Press) (Carver, 3887.4). 2The pellets were manufactured by rolling under pressure (3 g of positive electrode active material (powder) was placed in a circular pellet holder with a diameter of 13 mm and a force was applied until a force equivalent to 9,000 kgf was applied to manufacture them), and the pellets were crushed for 1 minute using a mortar and pestle to make them into powder again. After taking 0.01 g of the crushed positive electrode active material, they were placed in a vial containing 30 ml of ultrapure water and 500 ㎕ of a dispersant, and the positive electrode active material was dispersed for 1 minute using a sonicator, and then placed in a particle size analyzer (PSA) (Microtrac, S3500), and the D of each positive electrode active material 10 , D 50 , D 90 Obtain the value, β = (D 90 -D 10 ) / D 50 The value was calculated.

[0224] For reference, disintegration using a mortar and pestle does not affect the average particle size of the positive electrode active material.

[0225]

[0226] By substituting the above α and β values ​​into Equation 1 below, the values ​​according to Equation 1 are calculated and shown in Table 1 below.

[0227] Classification αβ|1-α / β|Example 10.98840.97230.0166Example 20.98420.95950.0256Example 31.03501.06760.0305Example 40.98320.94140.0444Comparative Example 11.02701.23480.1683Comparative Example 20.94430.97210.0286Comparative Example 31.02491.28890.2048

[0228]

[0229] Experimental Example 2: Battery Performance Evaluation

[0230] Each of the positive electrode active materials, carbon black conductive agent, and polyvinylidene fluoride (PVDF) binder prepared in Examples 1 to 4 and Comparative Examples 1 to 3 was mixed in an N-methylpyrrolidone (NMP) solvent at a ratio of 96:2:2 to prepare a positive electrode slurry. The positive electrode slurry was applied to one surface of an aluminum current collector, dried at 150°C, and rolled to prepare a positive electrode.

[0231] A lithium metal electrode was used as the negative electrode, and a porous polyethylene separator was interposed between the positive and negative electrodes to manufacture an electrode assembly. The electrode assembly was then placed inside a battery case, and an electrolyte was injected into the case to manufacture a half-cell. At this time, the electrolyte was prepared by dissolving 1.0 M LiPF6 in an organic solvent containing ethylene carbonate (EC): ethyl methyl carbonate (EMC): diethyl carbonate (DEC) in a volume ratio of 3:4:3.

[0232] For each half cell manufactured in this way, the initial charge capacity and initial discharge capacity were measured while charging to 4.3 V at 0.1 C in CC-CV mode at 25°C and discharging to 3.0 V at a constant current of 0.1 C, and the initial efficiency and direct current internal resistance (DCIR) were calculated, which are shown in Table 2 below. For reference, the initial efficiency value is a percentage value of the initial discharge capacity to the initial charge capacity, and the DCIR value is a value calculated by dividing the difference between the voltage at 60 seconds and the initial voltage while discharging at a constant current of 0.1 C by the applied current.

[0233] Then, the capacity of the lithium secondary battery was measured by repeating the charge / discharge cycle 50 times at a constant current of 0.33 C in the range of 3.0 to 4.25 V at 45℃, and the percentage of the discharge capacity of the 50th cycle to the discharge capacity of the 1st cycle was defined as the capacity retention rate, and this is shown in Table 2 below. In addition, the percentage of the DICR, which was calculated by dividing the voltage drop (△V) for 60 seconds in the 1st discharge cycle by the current, to the DCIR, which was calculated by dividing the voltage drop (△V) for 60 seconds in the 50th discharge cycle by the current, was defined as the resistance increase rate, and this is shown in Table 2 below.

[0234] ClassificationInitial charge capacity (mAh / g)Initial discharge capacity (mAh / g)Initial efficiency (%)DCIR (Ω)Capacity retention rate (%)Resistance increase rate (%)Example 1231.2206.389.216.294.747.0Example 2230.8206.289.316.294.049.6Example 3230.1204.989.016.994.151.8Example 4229.4204.189.014.793.943.1Comparative example 1231.1203.488.016.793.556.3Comparative example 2228.6202.688.615.792.152.5Comparative example 3230.9205.889.116.693.857.2

[0235]

[0236] Referring to Tables 1 and 2, it can be confirmed that the batteries including the positive electrode active materials of Examples 1 to 4 include Ni, Co, Mn, Al, Zr, and Y, and satisfy Equation 1 described herein, so that the capacity, initial efficiency, lifespan, and resistance performance of the batteries are all excellent.

[0237] Meanwhile, it can be confirmed that the batteries including the positive electrode active materials of Comparative Examples 1 to 3 have inferior initial discharge capacities compared to the battery including the positive electrode active material of Example 1, and that the initial efficiency, lifespan, and resistance performance are all reduced. The positive electrode active material of Comparative Example 1 does not contain Y, so there is a problem with grain growth, and thus does not satisfy Equation 1 described herein, resulting in reduced performance of the battery including it. In addition, the positive electrode active material of Comparative Example 2 does not contain Al, so the bonding (defect) is high, resulting in increased cation mixing, and thus the performance of the battery including it is reduced. In addition, the positive electrode active material of Comparative Example 3 does not contain Zr, which improves particle strength, and thus does not satisfy Equation 1 described herein, resulting in reduced performance of the battery including it.

Claims

1. Contains a lithium composite transition metal oxide in the form of a single particle, The above lithium composite transition metal oxide comprises Ni, Co, Mn, Al and M1, The above M1 is at least one selected from Zr, Y, K, Sr and Ba, A positive electrode active material satisfying the following equation 1: [Formula 1] |1-α / β| ≤ 0.1 In the above equation 1, α is (D 90 -D 10 ) / D 50 is the value, and β is the positive electrode active material at 1,000 kgf / cm 2 Up to 7,000 kgf / cm 2 After rolling (D 90 -D 10 ) / D 50 It's worth it.

2. In claim 1, The above lithium composite transition metal oxide is a positive electrode active material having a layered structure.

3. In claim 1, The above lithium composite transition metal oxide has an average particle diameter (D 50 ) is a positive electrode active material having a diameter of 3.00㎛ to 8.00㎛.

4. In claim 1, The above lithium composite transition metal oxide is a cathode active material doped with Al and M1.

5. In claim 1, A cathode active material in which the above Al is included in an amount of 500 ppm to 3,000 ppm based on the total weight of the above lithium composite transition metal oxide.

6. In claim 1, The above M1 is a positive electrode active material, which is included in a content of 100 ppm to 5,000 ppm based on the total weight of the lithium composite transition metal oxide.

7. In claim 1, The above lithium composite transition metal oxide is a cathode active material containing nickel in an amount of 60 mol% or more based on the total molar number of metals other than lithium.

8. In claim 1, The above lithium composite transition metal oxide is a positive electrode active material having a composition represented by the following chemical formula 1: [Chemical Formula 1] Li x [Ni a Co b Mr c Al d M1 e M2 f ]O 2-y A y In the above chemical formula 1, M1 is at least one selected from Zr, Y, K, Sr, and Ba, M2 is at least one selected from B, Ba, Ce, Cr, Mg, V, Ti, Fe, Zn, Si, Nb, Ga, Sn, Mo, W, and P, A is at least one selected from F, Cl, Br, I, and S, 1.0≤x≤1.3, 0.6≤a<1, 0.0 <b≤0.4, 0.0<c≤0.4, 0.0<d≤0.01, 0.0<e≤0.005, 0.0≤f≤0.2, a+b+c+d+e+f=1, 0≤y≤0.2이다. 9.(A) A step of preparing a mixture by mixing a positive electrode active material precursor including Ni, Co and Mn, an aluminum-containing raw material, an M1-containing raw material and a first lithium-containing raw material; (B) a step of first firing the mixture at a temperature of 800°C to 950°C to produce a first fired product; and (C) a step of mixing a second lithium-containing raw material into the first fired product and then firing it a second time at a temperature of 680°C to 850°C to manufacture a second fired product; The above M1 is at least one selected from Zr, Y, K, Sr and Ba, A method for manufacturing a positive electrode active material, wherein the above M1-containing raw material is mixed in an amount of 100 ppm to 5,000 ppm based on the total weight of the positive electrode active material precursor.

10. In claim 9, A method for producing a positive electrode active material, further comprising, prior to step (C), a step (B') of crushing the primary sintered product.

11. In claim 9, (C') A method for manufacturing a positive electrode active material, further comprising a step of crushing the above secondary sintered product.

12. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 8.

13. The anode according to claim 12; cathode; a separator interposed between the anode and the cathode; and A lithium secondary battery comprising an electrolyte.

Citation Information

Patent Citations

  • Positive electrode active material for secondary battery, method for preparing the same, and secondary battery comprising the same

    KR1020160149162A

  • Bombproof shutter appartus

    KR1020210128726A

  • Antibacterial panel structure of freight car loading box

    KR1020220060147A

  • A cathode active material, method of preparing the same, and lithium secondary battery comprising a cathode comprising the cathode active material

    KR102195187B1

Cited By

  • Coated positive electrode active material

    WO2026119991A1