Methods of μ-led sidewall cleaning and passivation

The method of cleaning and passivating micro LEDs with a dielectric layer addresses the issue of edge defects and self-oxidation, enhancing the luminous efficiency of micro LEDs by reducing non-radiative emissions and maintaining light transparency.

WO2024220754A1PCT designated stage expired Publication Date: 2024-10-24APPLIED MATERIALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/025335
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Micro LEDs suffer from increased edge defects and self-oxidation due to their high perimeter-to-surface area ratio during manufacturing, leading to non-radiative emissions and reduced luminous efficiency.

Method used

A method involving a cleaning process to remove sidewall defects followed by the deposition of a dielectric layer over the micro LEDs to prevent self-oxidation and enhance their performance.

Benefits of technology

The cleaning and passivation process significantly reduces edge defects, improving the luminous efficiency of micro LEDs by minimizing non-radiative emissions and maintaining transparency for light emission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024025335_24102024_PF_FP_ABST
    Figure US2024025335_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure generally includes a method for forming a light-emitting diode (LED) device that includes subjecting a plurality of micro LEDs disposed on a substrate to a cleaning process, the micro LEDs having sidewalls and a top surface, wherein sidewall defects are formed on the sidewalls, and the cleaning process removes the sidewall defects, and passivating the micro LEDs.
Need to check novelty before this filing date? Find Prior Art

Description

Methods of u-LED SIDEWALL CLEANING AND PASSIVATIONCROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This Application claims the benefit of United Stated Provisional Patent Application Serial No. 63 / 497,215 filed April 20, 2023, which is hereby incorporated by reference.BACKGROUNDField

[0002] Embodiments of the present disclosure generally relate to methods for forming light-emitting diode (LED) devices. More particularly, embodiments of the present disclosure relate to performing a cleaning and a passivation process on an LED device to remove edge defects and suppress self-oxidation of materials to improve the efficiency of an LED device.Description of the Related Art

[0003] Light-emitting diode (LED) panels use LED arrays with individual LEDs that each control individual pixel elements. LED panels may be used for computer displays, televisions, smart phone screens, and the like. An LED panel that uses micron-scale LEDs (micro LEDs) offer a variety of advantages such as higher energy efficiency, luminosity efficiency, and the like. However, the smaller surface area of micro LEDs may cause manufacturing defects hindering the luminosity of micro LEDs. Accordingly, what is needed in the art is a method to reduce defects as well as to suppress further formation of defects that hinder the performance of micro-LEDs.SUMMARY

[0004] The present disclosure generally includes a method for forming a lightemitting diode (LED) device that includes subjecting a plurality of micro LEDs disposed on a substrate to a cleaning process, the micro LEDs having sidewalls and a top surface, wherein sidewall defects are formed on the sidewalls, and the cleaning process removes the sidewall defects, and passivating the micro LEDs.

[0005] Embodiments of the present disclosure may further provide a method for forming a light-emitting diode (LED) device that includes subjecting micro LEDs disposed on a substrate to a cleaning process, the micro LEDs having sidewalls anda top surface, wherein sidewall defects are formed on the sidewalls, and the cleaning process removes the sidewall defects, and passivating the micro LEDs, wherein passivating the micro LEDs includes performing a surface treatment on the LED device, and forming a dielectric layer over the top surface and sidewalls of the micro LEDs.

[0006] Embodiments of the present disclosure may further provide a method for forming a light-emitting diode (LED) device that includes subjecting micro LEDs disposed on a substrate to a cleaning process, the micro LEDs having sidewalls and a top surface, wherein sidewall defects are formed on the sidewalls, and the cleaning process removes the sidewall defects, and passivating the micro LEDs, wherein passivating the micro LEDs includes performing a surface treatment on the LED device, and forming a dielectric layer over the top surface and sidewalls of the micro LEDs.BRIEF DESCRIPTION OF THE DRAWINGS

[0007] So that the manner in which the above recited features of the present disclosure can be understood in detail, a more particular description of the disclosure, briefly summarized above, may be had by reference to embodiments, some of which are illustrated in the appended drawings. It is to be noted, however, that the appended drawings illustrate only exemplary embodiments of the present disclosure and are therefore not to be considered limiting of its scope, and may admit to other equally effective embodiments.

[0008] FIG. 1A is a schematic cross-sectional view of a pixel according to embodiments.

[0009] FIG. 1 B is a schematic cross-sectional views of a pixel according to embodiments.

[0010] FIG. 2 illustrates a schematic, cross-sectional view of an LED, according to one or more embodiments.

[0011] FIG. 3 is a flow diagram of a method for forming a pixel with passivated LEDs according to one or more embodiments.

[0012] FIGS. 4A-4F are schematic, cross-sectional views of a pixel during a method according to one or more embodiments.

[0013] FIG. 5 is a flow diagram of a method for passivating LEDS according to one or more embodiments.

[0014] To facilitate understanding, identical reference numerals have been used, where possible, to designate identical elements that are common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.DETAILED DESCRIPTION

[0015] Embodiments of the present disclosure generally relate to methods for forming light-emitting diode (LED) devices. More particularly, embodiments of the present disclosure relate to performing a cleaning and a passivation process on an pixel to remove edge defects and suppress self-oxidation of materials to improve the efficiency of an LED device.

[0016] Micro LEDs are classified as LEDs having a critical dimension, i.e. , width, less than or equal to 10 microns. An advantage of using micro LEDs is that the forward and side luminescence intensities are maximized and are almost uniform in every direction.

[0017] However, when manufacturing micro LEDs, the perimeter to surface area ratio increases. Stated differently, as the surface area of the LEDs decrease, the sidewalls and the perimeter surrounding the LEDs increase. When micro LEDs are manufactured, the increase in perimeter to surface area ratio causes higher edge defects. These edge defects are formed due to sidewall damage and self-oxidation of the LED components during micro LED fabrication, which produces non-radiative emission. Embodiments described herein relate to removing the sidewall damage and depositing a dielectric layer over the micro LEDs to prevent self-oxidation of the layers.

[0018] FIG. 1A is a schematic cross-sectional view of a pixel 100a according to embodiments. The pixel 100a includes a plurality of LEDs 101 overlying a backplane 102. The LEDs 101 are integrated with backplane circuitry so that each LED 101 canbe individually addressed. For example, the circuity of the backplane 102 can include a TFT active matrix array with a thin-film transistor and a storage capacitor (not illustrated) for LEDs 101 , column address and row address lines, column and row drivers, to drive the LEDs 101 . Alternatively, the LEDs 101 can be driven by a passive matrix in the backplane circuitry. The LEDs 101 may include a first LED 101 A, a second LED 101 B, and a third LED 101 C. The LEDs 101 may be PSS micro-LEDs or planar micro-LEDs, or a combination thereof. The backplane 102 can be fabricated using conventional complementary metal-oxide silicon (CMOS) process. The LEDs 101 are connected to the backplane 102 via backplane electrodes 103, n-contacts 113, and p-contacts 115.

[0019] In certain embodiments, the backplane electrodes 103 include a first metal of a first material. The first material includes, but is not limited to, gold, indium, tin, silver, aluminum, platinum, or combinations thereof.

[0020] Subpixel isolation (SI) structures 126 are disposed over, and in some embodiments on, the backplane 102. The adjacent SI structures 126 define the respective well 118 of at least three sub-pixels 105 included in the backplane 102. An LED 101 is disposed in each well 118 between the adjacent SI structures 126. For example, a first sub-pixel 105a includes a first LED 101 A, a second sub-pixel 105b includes a second LED 101 B, and a third sub-pixel 105c includes a third LED 101 C. Although the pixel 100a is described as including three LEDs (and three subpixels), it is to be understood that the pixel 100a may have hundreds, thousands, millions, or more LEDs. Although the LEDs 101 are illustrated as micro LEDs, this is for example purposes only. The LEDs 101 may be any size including, but not limited to, mini and macro LEDs. In some embodiments, the LEDs 101 emit UV light. In other embodiments, the LEDs 101 emit light of other wavelengths. Each well 118 has a width from about 0.5 urn to about 40 urn, such as about 2 urn to about 30 urn. The SI structures 126 have a width from about 0.1 urn to about 15 urn such as 1 urn to 10 urn. The SI structures 126 may include organic material, such as epoxy-based photoresist.

[0021] The sub-pixels 105 each include a color conversion material 124 formed within the well 118. For example, sub-pixels 105 include a first sub-pixel 105a with a red color conversion material 124a disposed in the well 118 of the first sub-pixel 105a,a second sub-pixel 105b with a blue color conversion material 124b disposed in the well 118 of the second sub-pixel 105b, and a third sub-pixel 105c with a green color conversion material 124c disposed in the well 118 of the third sub-pixel 105c. When the first LED 101 A of the first sub-pixel 105a is turned on the red color conversion material 124a will convert the light emitted from the first LED 101 A into red light. When the second LED 101 B of the second sub-pixel 105b is turned on the blue color conversion material 124b will convert the light emitted from the second LED 101 B into blue light. When the third LED 101 c of the third sub-pixel 105c is turned on the green color conversion material 124c will convert the light emitted from the third LED 101 C into green light. In some embodiments, the color conversion material 124 may include quantum dots (QDs). The quantum dots may be sized to produce wavelengths corresponding to different colors. In one embodiment, the red color conversion material 124a may include quantum dots approximately 6 nm in size. The blue color conversion material 124b may include quantum dots approximately 4 nm in size. The green color conversion material 124c may include quantum dots approximately 2 nm in size. In other embodiments, the color conversion material 124 may include nanostructures, photoluminescent materials, or organic substances.

[0022] The LEDs 101 include mesa 104 and a body 106. A metal contact layer 110 is disposed on an upper surface of the mesa 104. In some embodiments, the metal contact layer 110 is a transparent conductive layer (TCL). The metal contact layer 110 may include a transparent conductive oxide, such as indium tin oxide (ITO). In some embodiments, a dielectric layer 116 is formed on at least the metal contact layer 110, the body 106 of the LEDs 101A-101 C, and the sidewalls of the mesa 104 and the body 106. The dielectric layer 116 may be deposited after removing (cleaning) sidewall damage formed on the sidewall of the LEDs (i.e., the sidewall of the body 106), and performing a surface treatment process on the LEDs 101. As the LEDs 101 are manufactured, the increase in perimeter to surface area ratio causes higher edge defects. The edge defects are caused by the sidewall damage of the LEDs 101 during etching. The sidewall damage creates non-radiative emissions and causes oxidation of the active materials in the LED layers. In some embodiments, the non-radiative emissions arise around the 200 nm to 800 nm wavelength in the UV-visible range. Therefore, non-radiative emission causes an increase in the emission of yellow light from the LEDs 101 , which in turn, reduces the luminous efficiency of the LEDs due tobroad emission linewidth which offers low color gamut levels. This reduces the overall performance of the pixel 100a. The dielectric layer 116 may comprise any suitable transparent material that has a high breakdown voltage and a refractive index (Rl) from about 1.45 to about 2.16, such as aluminum oxide. The dielectric layer 116 is deposited with a thickness and an Rl such that the dielectric layer 116 prevents selfoxidation of LED materials while still being transparent to light emitted from LEDs 101 .

[0023] An n-contact opening 112 is disposed in the dielectric layer 116 on a first portion 114 of the upper surface of the body 106 adjacent to the mesa 104. A p- contact opening 117 is disposed in the dielectric layer 116 on the metal contact layer 110. A conductive material 111 is disposed in the n-contact opening 112 to contact the LEDs 101 and form an n-contact 113. The conductive material 111 is disposed in the p-contact opening 117 to contact the metal contact layer 110 to form a p-contact 115. In some embodiments, the conductive material 111 is transmissive or semi- transmissive. In certain embodiments, the conductive material 111 is a second metal of a second material. The second material includes, but is not limited to, gold, silver, aluminum, platinum, indium, or combinations thereof. The transmissive or semi- transmissive metal contact layer 110, dielectric layer 116, and conductive material 111 allow light to emit from the LEDs 101 . The metal contact layer 110 conducts current into the mesa 104 to allow the LEDs 101 to emit light. The mesa size is less than the overall LED size resulting is a smaller emission area, smaller injection area than conventional LEDs. The smaller emission area, smaller injection area increases the density of the LEDs 101. The LEDs 101 with the increased density have an increased efficiency such that the light that is emitted is brighter than conventional LEDs with the same amount of current. I.e. , more light is extracted with the injection area of the mesa 104.

[0024] FIG. 1 B is a schematic cross-sectional views of a pixel 100b according to embodiments. The pixel 100b includes at least three LEDs 101 disposed on the backplane 102. The backplane 102 includes backplane electrodes 103 disposed thereon. The LEDs 101 include the n-contacts 113 and the p-contacts 115 that are coupled to corresponding backplane electrodes 103 disposed on the backplane 102 A bonding material 152 is disposed on the backplane 102, between the backplane electrodes 103, and between the LEDs 101. The bonding material 152 may be a transparent ultraviolet (UV) material that includes an adhesive material. The adhesivematerial includes, but is not limited to, an epoxy, an acrylic material, and combinations thereof. The acrylic material may be UV transparent material.

[0025] A UV blocking material 156 may be disposed over the bonding material 152. The optical density of the UV blocking material 156 provides for color isolation between each of the LEDs 101 because the UV blocking material 156 blocks UV light. The UV blocking material 156 includes thermal curable glue, UV curable glue, black matrix epoxy, metal particles, UV absorbing materials, or combinations thereof.

[0026] The pixel 101 b further includes a substrate 150. The substrate 150 includes wells 158 defined by SI structures 126. Cured color conversion material 124 is disposed in the wells 158, which are disposed on the substrate 150. The substrate 150 is coupled to the backplane 102 as seen in FIG. 1 B. To form the arrangement seen in pixel 100b, the substrate 150 aligns with the backplane 102 where the color conversion material 124 in their respective wells 158 aligns with the LEDs 101 .

[0027] FIG. 2 illustrates a schematic, cross-sectional view of an LED 200, according to one or more embodiments. The LED 200 may correspond to the first LED 101A, the second LED 101 B, or the third LED 101 C. In one or more embodiments, the LED 200 includes the body 106. The body 106 may include a plurality of layers. The structure of the LED 200 (i.e., the body 106) overlying the backplane 102 may include any number of materials and / or layers. In some embodiments, the LED 200 may be manufactured using layers of group lll-V films. Although the LED 200 is described as including layers of group lll-V films, this is for example purposes only, and the LED 200 may be manufactured using any suitable materials.

[0028] As an example, the LED 200 may include an n-type layer 204, an active layer 206, a p-type layer 208, and the metal contact layer 110. The n-type layer 204 includes an un-doped layer 204a and a doped layer 204b disposed on the un-doped layer 204a. The un-doped layer 204a may comprise gallium nitride (GaN), indium gallium nitride (InGaN), aluminum gallium nitride (AIGaN), indium aluminum gallium nitride (InAIGaN), or the like. The doped layer 204b may comprise n-type (n-doped) gallium nitride (n-GaN), n-type indium gallium nitride (n-lnGaN), n-type aluminum gallium nitride (n-AIGaN), n-type indium aluminum gallium nitride (n-lnAIGaN), or thelike. Stated otherwise, the doped layer 204b may comprise the same material as the un-doped layer 204a that is n-type doped.

[0029] The active layer 206 may be formed on or above the n-type layer 204. The active layer 206 may be a multiple quantum well (MQW) layer composed of one or a plurality of field pairs of InGaN and / or GaN. The p-type layer 208 may be formed over the active layer 206. The p-type layer 208 may comprise p-GaN, or any other suitable p-doped material. The metal contact layer 110 may be formed over the p-type layer 208.

[0030] The n-contact opening 112 is disposed in the dielectric layer 116 and exposes a portion of the doped layer 204b of the n-type layer 204. Stated otherwise, the n-contact opening is disposed on a first portion 114 the upper surface of the body 106 adjacent to the mesa 104 (FIGS. 1 A-1 B). The p-contact opening 117 is disposed in the dielectric layer 116 on the metal contact layer 110. The conductive material 111 is disposed in the n-contact opening 112 to contact the n-type layer 204 and form the n-contact 113. The conductive material 111 is disposed in the p-contact opening 117 to contact the metal contact layer 110 to form the p-contact 115.

[0031] FIG. 3 is a flow diagram of a method 300 for forming a pixel with passivated LEDs according to one or more embodiments. FIGS. 4A-4F are schematic, cross- sectional views of a pixel 400 during a method according to one or more embodiments.

[0032] At operation 302, and as illustrated in FIG. 4A, a pixel 400 is cleaned using a cleaning process. The LED pixel may include LEDs 101. In some embodiments, as noted above, the LEDs 101 are formed by depositing on a transfer substrate 402, in order, the n-type layer 204, the active layer 206, and the p-type layer 208, and etching the n-type layer 204, the active layer 206, and the p-type layer 208 to form the structures of the LEDs 101 . The LEDs 101 may be separated by gaps 414 formed by the etching of each of the layers. The metal contact layer 110 is deposited on or above each p-type layer 208 after etching.

[0033] However, as noted above, when forming the LED 101 , the perimeter to surface area ratio increases. When micro LEDs are manufactured, the increase in perimeter to surface area ratio causes higher edge defects. These edge defects are formed due to sidewall damage and self-oxidation of the LED components duringmicro LED fabrication, which produces non-radiative emission. In one more embodiments, sidewall damage to the LEDs 101 are removed by subjecting the pixel 400 to a cleaning process.

[0034] In some embodiments, the cleaning process involves a first cleaning process followed by a second cleaning process. In some embodiments, the first cleaning process is a solvent cleaning. The second cleaning process is a wet chemical cleaning. In one embodiment, the solvent cleaning includes placing the pixel 400 in a cleaning solvent. Examples of cleaning solvents include, but are not limited to, a mixture of water and isopropyl alcohol (IPA).

[0035] After the solvent cleaning, the pixel 400 may undergo a wet chemical cleaning (the second cleaning process). The wet chemical cleaning may include cleaning the pixel 400 using an acid over a first duration of time at a first temperature. In some embodiments, the acid may include, but is not limited to, oxalic acid, potassium hydroxide (KOH), or the like. The first duration of time may range from 2 to 5 minutes, and the first temperature may range from 60 to 70°C. For example, the wet chemical cleaning may include cleaning the pixel 400 using oxalic acid for 3 minutes at 65°C. In another example, the pixel 400 may be chemically cleaned using KOH at room temperature for 5 minutes.

[0036] At operation 304, as illustrated in FIG. 4B, the pixel 400 is passivated. The pixel 400 is passivated by depositing the dielectric layer 116 on the pixel 400 via a deposition process. The dielectric layer 116 is deposited such that it surrounds the sidewalls and top surface (i.e., the metal contact layer) of the LEDs 101. In some embodiments, the dielectric layer 116 is also deposited in the gaps 414. In some examples, the portions of the dielectric layer 116 disposed in the gaps 414 may or may not be removed (i.e., etched). The dielectric layer 116 may be deposited using any suitable deposition process, including but not limited to, chemical vapor deposition (CVD), physical vapor deposition (PVD), plasma enhanced CVD (PECVD), atomic layer deposition (ALD), or the like. The dielectric layer 116 may comprise any suitable transparent material that has a high breakdown voltage and a refractive index (Rl) from about 1.45 to about 2.16, such as aluminum oxide. The dielectric layer 116 is deposited with a thickness and an Rl such that the dielectric layer 116 prevents selfoxidation of LED materials while still being transparent to light emitted from LEDs 101 .Advantageously, the cleaning process and passivating of the pixel 400 results in LEDs 101 having a ratio of the intensity of UV light to yellow light from about 1 :1 to about 1 :3. Operation 304 is described in more detail in FIG. 5.

[0037] At operation 306, as illustrated in FIG. 4C, openings are formed in the dielectric layer 116 of the pixel 400. In one or more embodiments, forming the openings in the dielectric layer 116 includes forming the n-contact opening 112 and the p-contact opening 117 in the dielectric layer 116. Forming the n-contact opening 112 includes etching or otherwise removing a portion of the dielectric layer 116 on the n-type layer 204 (the first portion 114 the upper surface of the body 106 adjacent to the mesa 104 (FIGS. 1A-1 B)) to expose a portion of the n-type layer 204. Forming the p-contact opening 117 includes etching or otherwise removing a portion of the dielectric layer 116 to expose the metal contact layer 110. The openings may be formed in the dielectric layer using any suitable etching process.

[0038] At operation 308, as illustrated in FIG. 4D, contacts are formed in the openings of the dielectric layer 116. In one or more embodiments, forming contacts includes forming the n-contact 113 in the n-contact opening 112 and forming the p- contact 115 in the p-contact opening 117. The contacts may be formed using a metallization process in which the conductive material 111 is deposited into the n- contact opening 112 and the p-contact opening 117. In one or more embodiments, a mask may be used to expose the n-contact opening 112 and the p-contact opening 117. The conductive material 111 fills the n-contact opening 112 and the p-contact opening 117 such that the n-contact 113 and the p-contact 115 extend above the dielectric layer 116.

[0039] In one or more embodiments, the conductive material 111 is disposed in the n-contact opening 112 to contact the LEDs 101 and form the n-contact 113. The conductive material 111 is disposed in the p-contact opening 117 to contact the metal contact layer 110 to form a p-contact 115. The conductive material also fills the n- type opening 112 and the p-contact opening 117 such that the n-contact 113 and the p-contact extend to a corresponding backplane electrode 103. In some embodiments, the conductive material 111 is transmissive or semi-transmissive. The transmissive or semi- transmissive metal contact layer 110, dielectric layer 116, and conductive material 111 allow light to emit from the LEDs 101 .

[0040] At operation 310, and as illustrated in FIG. 4E, a mass transfer operation is performed to bond the LEDs 101 to the backplane 102. The mass transfer operation includes disposing the backplane 102 on a bonder stage and attaching the transfer substrate 402 to a bonder head. The bonder head and the bonder stage are orientated such that the n-contacts 113 and the p-contacts 115 face and are aligned with corresponding backplane electrodes 103. In one example, as shown in FIG. 4E, the quantity of backplane electrodes 103 is equal to the quantity of n-contacts 113 plus p-contacts 115. In other examples, the quantity of n-contacts 113 plus p-contacts 115 is not equivalent to the quantity of backplane electrodes 103. When the quantity of backplane electrodes 103 and micro-LED electrodes 108 are not equivalent, at least one of the n-contacts 113 or p-contacts 115 are aligned with a backplane electrode 103.

[0041] The bonder head is then heated to a bonder temperature T1. In some embodiments, the bonder temperature T1 may be about 40°C and about 80°C. The bonder stage is heated to a stage temperature T2. In some embodiments, the stage temperature T2 may be about 150°C and about 300°C. In some embodiments, the stage temperature T2 is based on the melting point of the material of the backplane electrodes 103. In other embodiments, the stage temperature T2 is based on the coefficient of thermal expansion (CTE) of the transfer substrate 402. The bonding process is performed by applying a pressure to the bonder head. As the n-contacts 113 and p-contacts 115 come in contact with the backplane electrodes 103, the stage temperature T2 and the pressure cause the n-contacts 113 and p-contacts 115 to bond with a corresponding backplane electrode 103. The bonding process may be performed over a bonding time period from about 30 seconds to about 2 minutes. The bonder stage is cooled to the bonder temperature T1 after the bonding process. The bonder stage and the bonder head are removed.

[0042] In one or more embodiments, the transfer substrate is removed, exposing the LEDs 101. The transfer substrate may be removed using any suitable removal process such as laser-lift off (LLO).

[0043] At operation 312, and as illustrated in FIG. 4F, the SI structures 126 are formed and the color conversion material 124 is deposited and cured. The SI structures 126 are formed on the backplane 102 on each side the LEDs 101 formingwells 118. The color conversion material is deposited into each well 118 and is cured. This is repeated until color conversion material 124 is deposited in the well 118 of the first sub-pixel 105a, the well 118 of the second sub-pixel 105b, and the well 118 of the third sub-pixel 105c. For example, a red color conversion material 124a may be deposited in a well 118 of the first sub-pixel 105a and the red color conversion material 124a is cured, a blue color conversion material 124b may be deposited in a well 118 of the second sub-pixel 105b and the blue color conversion material 124b is cured, and a green color conversion material 124c may be deposited in a well 118 of the third sub-pixel 105c and the green color conversion material 124c is cured. The color conversion material 124 is cured by turning on the micro-LEDs or by exposure to a UV-light.

[0044] FIG. 5 is a flow diagram of a method 500 for passivating LEDS according to one or more embodiments. The method 500 corresponds to operation 304 of method 300. The method 500 is an ALD process. FIG. 5 is described with reference to FIG. 4B.

[0045] At operation 502, as shown in FIG. 4B, the pixel 400 undergoes a surface treatment process. The surface treatment process is performed at a second temperature from about 150 to about 250 °C. For example, the surface treatment process is performed at 200°C. During the surface treatment process, a first precursor is introduced in a processing chamber for a second duration of time. Examples of the first precursor may include, but are not limited to, trimethylamine (TMA). The second duration of time may range from about 100 ms to about 10 seconds. For example, TMA may be introduced into the processing chamber for 250 ms. Then, the chamber may be purged, via a first purging process, by introducing a first purge gas into the chamber over a third duration of time. Examples of the first purge gas include, but are not limited to, nitrogen and argon. The third duration of time may range from about 100 ms to about 300 ms. For example, the chamber may be purged by introducing nitrogen into the chamber for a duration of 250 ms. The above process would comprise one cycle of the surface treatment process. The surface treatment process would include about 50 to about 500 cycles. The surface treatment process is cycled until the surface of the LEDs 101 are suitable to adhere to the dielectric layer 116. For example, the surface treatment process may be performed for 100 cycles.

[0046] At operation 504, the pixel undergoes a deposition process. The deposition process is performed at a third temperature of about 150 and to about 250 °C. For example, the deposition process is performed at 200°C. During the deposition process, a second precursor is introduced into the processing chamber for a fourth duration of time to form an absorption layer. The second precursor may comprise, but is not limited to, TMA and argon. The fourth duration may range from about 100 ms to about 1000 ms. For example, TMA may be introduced into the processing chamber for 500 ms.

[0047] Next the chamber is purged using a second purging process that includes introducing a second purging gas over a fifth duration of time. The second purging gas may be the same or different from the first purging gas. The fifth duration of time may be from about 100 ms and to about 250 ms. Then a reactant is introduced into the chamber for a sixth duration of time. Examples of the reactant include, but are not limited to, water. The sixth duration of time may be from about 100 ms to about 500 ms. For example, water may be introduced into the chamber for 250 ms. The reactant reacts with the absorption layer to form the dielectric layer 116. For example, TMA and water react, forming aluminum oxide (AIOx). After adding the reactant, the chamber is purged using a third purging process. The third purging process may be the same or different from the second purging process. For example, the third purging process may include introducing the second purging gas over the fifth duration of time. This above process would comprise one cycle of the deposition process. The deposition process is repeated until the dielectric layer 116 has a thickness from about 28 nm to about 32 nm. For example the deposition process may be repeated until an aluminum oxide layer having a thickness of about 30 nm is formed.

[0048] While the foregoing is direct to examples of the present disclosure, other and further examples of the disclosure may be devised without departing from the basic scope thereof, and the scope thereof is determined by the claims that follow.

Claims

What is claimed is:

1. A device, comprising: a backplane, the backplane including a plurality of backplane electrodes; and light emitting diodes (LEDs) disposed over the backplane, each LED includes: a mesa and a body; a metal contact layer disposed on an upper surface of the mesa; a dielectric layer disposed over a top surface and sidewalls of the LEDs, an n-contact of a conductive material disposed in an n-contact opening of the dielectric layer to contact an n-type layer; and a p-contact of the conductive material disposed in a p-contact opening of the dielectric layer to contact the metal contact layer; and subpixel isolation (SI) structures disposed over the LEDs defining wells of subpixels, each well including a respective LED between adjacent SI structures, the subpixels have a different color conversion material disposed in the wells.

2. The device of claim 1 , wherein a bonding material is disposed over the backplane.

3. The device of claim 2, wherein an ultraviolet (UV) blocking material is disposed over the bonding material.

4. The device of claim 1 , wherein the LEDs comprise: an n-type layer; an active layer disposed over the n-type layer; a p-type layer disposed over the active layer; and a metal contact layer disposed over the p-type layer.

5. The device of claim 1 , wherein the dielectric layer comprises aluminum oxide.

6. The device of claim 4, wherein the n-type layer is in contact with the n-contact including the conductive material.

7. The device of claim 4, wherein the p-type layer is in contact with the p-contact including the conductive material.

8. A device, comprising: a backplane, the backplane including a plurality of backplane electrodes; and light emitting diodes (LEDs) disposed over the backplane, each LED includes: a mesa and a body; a metal contact layer disposed on an upper surface of the mesa; a dielectric layer disposed over a top surface and sidewalls of the LEDs, an n-contact of a conductive material disposed in an n-contact opening of the dielectric layer to contact an n-type layer; and a p-contact of the conductive material disposed in a p-contact opening of the dielectric layer to contact the metal contact layer; and subpixel isolation (SI) structures disposed over the LEDs defining wells of subpixels, each well including a respective LED between adjacent SI structures, the subpixels have a different color conversion material disposed in the wells; and a bonding material disposed below the SI structures.

9. The device of claim 8, further comprising an ultraviolet (UV) blocking material disposed over the bonding material.

10. The device of claim 8, wherein the LEDs comprise: an n-type layer; an active layer disposed over the n-type layer; a p-type layer disposed over the active layer; and a metal contact layer disposed over the p-type layer.11 . The device of claim 8, wherein the dielectric layer comprises aluminum oxide.

12. The device of claim 10, wherein the n-type layer is in contact with the n- contact including the conductive material, and the p-type layer is in contact with the p-contact including the conductive material.

13. A method for forming a pixel, comprising: subjecting a plurality of micro LEDs disposed to a cleaning process comprising a first cleaning process and a second cleaning process, the first cleaningprocess comprising a solvent cleaning and the second cleaning process comprising a wet chemical etching, the micro LEDs having sidewalls and a top surface, wherein sidewall defects are formed on the sidewalls, and the cleaning process removes the sidewall defects; and passivating the micro LEDs.

14. The method of claim 13, wherein the solvent cleaning comprises placing the plurality of micro LEDs in a cleaning solvent comprising a mixture of water and isopropyl alcohol (IPA).

15. The method of claim 13, wherein the wet chemical cleaning comprises cleaning the plurality of micro LEDs using an acid comprising oxalic acid or potassium hydroxide (KOH).

16. The method of claim 13, wherein passivating the micro LEDs comprises: performing a surface treatment on the micro LEDs; and forming a dielectric layer over the top surface and sidewalls of the micro LEDs.

17. The method of claim 16, wherein performing a surface treatment on the micro LEDs comprises: introducing trimethylamine (TMA) into a processing chamber; purging the processing chamber by performing a purging process; and cycling between the introducing of the TMA into the processing chamber and the performing the purging process for a quantity of cycles.

18. The method of claim 16, wherein forming the dielectric layer over the top surface and sidewalls of the micro LEDs comprises: forming an absorption layer by introducing TMA into a processing chamber; purging the processing chamber by performing a first purging process; forming the dielectric layer by introducing a reactant into the processing chamber; purging the processing chamber by performing a second purging process; andcycling between the introducing TMA into a processing chamber, performing the first purging process, introducing the reactant into the processing chamber, and performing the second purging process until the dielectric layer has a thickness from about 28 to about 32 nm.

19. The method of claim 16, wherein the dielectric layer surrounds each of the LEDs and is formed over gaps between each of the micro LEDs.

20. The method of claim 16, wherein the dielectric layer comprises aluminum oxide.

Citation Information

Patent Citations

  • Method for improving modulation bandwidth of micro LED by using atomic layer deposition technology

    CN113851568A

  • Method for manufacturing light emitting device

    US20140322844A1

  • Display device using semiconductor light emitting device

    US20160190105A1

  • Print process for color conversion layer using porous host or positive photoresist

    US20220293826A1

  • Optoelectronic device

    US20220310875A1