Composite electrode and electrochemical device

By preparing a polyimide-containing porous fiber separator layer on the surface of the lithium-ion battery pole piece, the problems of lithium-ion battery separator hindering lithium ion transmission and poor thermal stability are solved, and the high dynamics and high-temperature safety performance are improved.

WO2024221144A1PCT designated stage expired Publication Date: 2024-10-31NINGDE AMPEREX TECHNOLOGY LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/090168
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators hinder the transmission of lithium ions, especially under high-rate and low-temperature conditions, resulting in reduced dynamic properties. In addition, the thermal stability of the PE or PP base film is poor, posing high-temperature safety risks.

Method used

The fiber separator layer is made of porous fibers containing polyimide and prepared on the surface of the pole piece through electrospinning or melt-blown processes to form a composite electrode with high porosity and high thermal stability, avoiding additional separators and improving lithium ion transmission and Electronic conduction properties.

Benefits of technology

It achieves the high kinetic performance and high-temperature safety performance of the composite electrode, improves the rate performance and cycle performance of lithium-ion batteries, reduces the self-discharge rate, and ensures the stability of the battery in high rate, high cycle times and low temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023090168_31102024_PF_FP_ABST
    Figure CN2023090168_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of electrode materials, and particularly relates to a composite electrode and an electrochemical device. The composite electrode of the present invention comprises an electrode sheet and a fiber separator layer, wherein the fiber separator layer is located on the surface of the electrode sheet; and the fiber separator layer comprises porous fibers, the porous fibers containing polyimide. In the present invention, the fiber separator layer is provided on a surface of an electrode sheet, such that the separator and the electrode sheet form a whole; an additional separator does not need to be used, and good heat resistance of the polyimide fibers can ensure high-temperature stability and safety performance of the electrode sheet; in addition, the structure of the porous fibers ensures high porosity of the composite electrode, which is beneficial for transporting lithium ions between the positive and negative electrode sheets via the fiber separator layer, thereby improving the dynamic performance of the composite electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Composite electrode and electrochemical device Technical Field

[0001] The present invention belongs to the technical field of electrode materials, and in particular relates to a composite electrode and an electrochemical device. Background Art

[0002] Lithium-ion batteries are widely used in consumer electronics due to their high volumetric and mass energy density, long cycle life, high nominal voltage, and low self-discharge rate. With the vigorous development of clean energy in recent years, the industry's requirements for the comprehensive performance of lithium-ion batteries have become increasingly stringent, especially in terms of fast charging performance and safety performance.

[0003] In lithium-ion batteries, the separator is a key internal component, playing a crucial role in battery interface stability, ion transport, and safety. Currently, commercial separators are mostly based on stretched polyethylene (PE) or polypropylene (PP) membranes, supplemented by ceramic coatings to enhance the separator's adhesion and thermal dimensional shrinkage, which can improve the interfacial dynamics and safety performance of lithium-ion batteries.

[0004] However, existing separators still pose certain obstacles to the transmission of lithium ions. In particular, polarization will occur in lithium-ion batteries under high-rate and / or low-temperature conditions, which will further hinder the dynamic characteristics of lithium-ion transmission across the separator, thereby reducing or directly reducing the tolerance. In addition, PE-based films or PP-based films have poor thermal stability. PE usually melts between 100 and 130°C, and PP between 150 and 170°C. This poses a great risk to the high-temperature safety performance of lithium-ion batteries.

[0005] Summary of the Invention

[0006] One of the purposes of the present invention is to provide a composite electrode having the advantages of high porosity and high thermal stability, which can ensure high dynamic performance and high-temperature safety performance.

[0007] Another object of the present invention is to provide an electrochemical device having advantages such as high kinetic performance and high temperature safety performance.

[0008] The composite electrode of the present invention adopts the following technical solutions:

[0009] A composite electrode, comprising a pole piece and a fiber diaphragm layer, wherein the fiber diaphragm layer is located on the pole piece surface; the fiber diaphragm layer comprises porous fibers; and the porous fibers comprise polyimide. The composite electrode provided by the present invention comprises a fiber diaphragm layer made of porous fibers containing polyimide. In the present invention, the fiber diaphragm layer located on the pole piece surface can be in situ generated on the pole piece surface, for example, the fiber diaphragm layer can be prepared on the pole piece surface using an electrospinning process or a melt-blowing process; the fiber diaphragm layer is arranged on the pole piece surface so that the diaphragm and the pole piece form a whole. When used as a composite electrode, no additional diaphragm is required. The high bonding performance of the two can avoid problems such as short circuits caused by particle puncture on the electrode pole piece surface. At the same time, the excellent heat resistance of the polyimide fiber can ensure the high-temperature stability and safety performance of the pole piece. In addition, the structure of the porous fibers ensures the high porosity of the composite electrode, which is conducive to the transmission of lithium ions and electron conduction between the positive and negative pole pieces through the fiber diaphragm layer, thereby improving the rate performance, cycle performance and other dynamic properties of the composite electrode.

[0010] Preferably, the porosity of the fiber separator layer is 30-80%; and / or the thickness of the fiber separator layer is 5-30 μm; and / or the average pore size of the fiber separator layer is 100-500 nm; and / or the fiber diameter of the porous fibers is 100 nm-1 μm. A lithium-ion battery separator with too low a porosity can clog the ion transmission pathway, hindering the normal circulation of the battery cell. Excessive porosity can lead to structural instability and poor mechanical strength, making it unable to resist puncture from particles on the electrode surface, easily causing localized cathode and anode short circuits, resulting in electrical performance degradation and severe self-discharge. The present invention sets an appropriate porosity of 30-80% for the fiber separator layer, ensuring efficient lithium ion transmission through the fiber separator layer. Furthermore, by controlling the relatively thin thickness of the fiber separator layer, the battery's energy density can be increased while ensuring separator strength. Combined with the porosity and fiber diameter characteristics, the puncture strength of the fiber separator layer is ensured, avoiding problems such as short circuits.

[0011] Furthermore, the porosity of the fiber diaphragm layer is 50-60%; and / or the thickness of the fiber diaphragm layer is 10-15 μm; and / or the average pore size of the fiber diaphragm layer is 100-200 nm; and / or the fiber diameter of the porous fiber is 300-600 nm.

[0012] In some preferred embodiments, the fiber separator layer further comprises an adhesive; and / or the fiber separator further comprises an inorganic filler, and the inorganic filler is a lithium ion conductor material and / or a non-lithium ion conductor material.

[0013] Exemplarily, the adhesive includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyamide, polyacrylonitrile (PAN), polyethylene glycol, polyethylene oxide, polyphenylene ether (PPO), polypropylene carbonate (PPC), polymethyl methacrylate (PMMA), polyethylene terephthalate, polychlorotrifluoroethylene-vinylidene fluoride copolymer, polyethylene oxide (PEO), polyvinylidene fluoride derivatives, polyvinylidene fluoride-hexafluoropropylene derivatives, polyamide derivatives, polyacrylonitrile derivatives, polyethylene glycol derivatives, polyethylene oxide derivatives, polyphenylene ether derivatives, polypropylene carbonate derivatives, polymethyl methacrylate derivatives, polyethylene terephthalate derivatives, polychlorotrifluoroethylene-vinylidene fluoride copolymer derivatives, and polyethylene oxide derivatives.

[0014] In some specific embodiments, the inorganic filler is located inside the porous fibers, or in the gaps between the porous fibers, or forms a stacked structure with the fiber separator layer.

[0015] Preferably, the electrode sheet includes a positive electrode sheet or a negative electrode sheet.

[0016] Preferably, the porosity of the negative electrode plate is 20-50%; and / or, the negative electrode plate comprises a negative electrode active material layer, and the content of sodium carboxymethyl cellulose is 0-0.001wt% based on the negative electrode active material layer; and / or, the interfacial adhesion between the fiber diaphragm layer and the positive electrode plate is 5-10N / m, and the interfacial adhesion between the fiber diaphragm layer and the negative electrode plate is 13-20N / m. When the fiber diaphragm layer is integrated separately on the positive (cathode) or negative (anode) plate, the interfacial adhesion with the positive and negative plates is different. For example, when the fiber diaphragm layer is integrated on the anode plate, the adhesion between the two is greater than the adhesion between the fiber diaphragm layer and the cathode. The higher interfacial adhesion between the fiber diaphragm layer and the electrode plate is conducive to ensuring the stability of the interface.

[0017] Preferably, the fiber separator layer is prepared by a method comprising the following steps: forming a spinning membrane on the surface of the electrode using the precursor PAA through an electrospinning process; then, imidizing the PAA through a gradient temperature ramp and heat-holding operation to obtain a fiber separator layer containing polyimide. The present invention utilizes an electrospinning process to construct a high-thermal-stability fiber separator layer on the electrode surface in a single step, ensuring that the fiber separator layer has an appropriate pore size and porosity. A high-porosity porous electrode electrode is simultaneously formed through an imidization heat treatment process, thereby ensuring the high-temperature stability and transmission dynamics performance of the composite electrode.

[0018] Preferably, the electrode sheet comprises a negative electrode sheet containing a negative electrode active material layer. Prior to the gradient heating and holding operation, the negative electrode active material layer contains sodium carboxymethyl cellulose. The gradient heating and holding operation causes the sodium carboxymethyl cellulose to form carbon particles and pores. After heat treatment of the composite electrode, the sodium carboxymethyl cellulose (CMC) carbonizes and decomposes, and vaporizes to form pores, thereby increasing the porosity of the electrode sheet and promoting lithium ion transport. Furthermore, the carbon particles formed after the carbonization of the CMC contribute to electronic conductivity, further improving the dynamic performance of the battery cell.

[0019] Illustratively, the heat treatment includes a gradient temperature ramp and a holding period, wherein the end point temperature of the gradient temperature ramp and the holding period are 280-320°C and 30-90 minutes, respectively. By controlling the end point temperature and holding period of the imidization heat treatment, the imidization and carbonization processes are ensured to proceed fully, thereby improving the performance of the lithium-ion battery.

[0020] Furthermore, the gradient heating and insulation operation includes: heating from room temperature to 80-120°C at a heating rate of 2-4°C / min, and keeping warm at 80-120°C for 25-35 minutes; continuing to heat up to 180-220°C at a heating rate of 2-4°C / min, and keeping warm at 180-220°C for 25-35 minutes; continuing to heat up to 280-320°C at a heating rate of 2-4°C / min, and keeping warm at 280-320°C for 30-90 minutes.

[0021] Preferably, the pole piece includes a current collector and an active material layer; the current collector, active material layer and fiber diaphragm layer are stacked in sequence; and / or, the pole piece includes a current collector, an active material layer and a conductive primer layer; the conductive primer layer includes a conductive material and an adhesive; the conductive material includes at least one of carbon black, carbon nanotubes and graphene; the current collector, conductive primer layer, active material layer and fiber diaphragm layer are stacked in sequence; and / or, the composite electrode includes a current collector, an active material layer and an inorganic filler layer; the current collector, active material layer, fiber diaphragm layer and inorganic filler layer are stacked in sequence; and / or, the composite electrode includes a current collector, an active material layer, a conductive primer layer and an inorganic filler layer; the current collector, conductive primer layer, active material layer, fiber diaphragm layer and inorganic filler layer are stacked in sequence.

[0022] The electrochemical device of the present invention adopts the following technical solutions:

[0023] An electrochemical device comprising any of the aforementioned composite electrodes. The electrochemical device of the present invention comprises any of a battery cell, module, and battery pack. The composite electrode utilizes the excellent heat resistance of the polyimide fibers on the electrode to ensure the high-temperature stability and safety of the lithium-ion battery. Furthermore, the porous fiber structure ensures a high porosity in the composite electrode, facilitating the transmission of lithium ions and electron conduction between the positive and negative electrode sheets through the fiber separator layer, thereby improving the rate capability and other dynamic properties of the lithium-ion battery.

[0024] Preferably, the electrochemical device is without a separator.

[0025] The composite electrode and electrochemical device provided by the present invention, by compounding a fiber diaphragm layer containing polyimide on the surface of the electrode pole piece, can not only give full play to the high temperature resistance of polyimide, so that the composite electrode and electrochemical device have excellent high temperature stability, but also can simultaneously ensure the appropriate porosity of the fiber diaphragm layer and the electrode pole piece, have a lower interface impedance, thereby improving the transmission performance of lithium ions and electrons, and can ensure strong battery dynamics performance under high rate, high cycle number and low temperature environment. In addition, it also has the advantages of low self-discharge rate of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] FIG1 is a schematic structural diagram of a composite electrode provided in a specific embodiment of the present invention;

[0027] FIG2 is a schematic structural diagram of a composite electrode provided in a specific embodiment of the present invention;

[0028] FIG3 is a schematic structural diagram of a composite electrode provided in a specific embodiment of the present invention;

[0029] FIG4 is a schematic structural diagram of a composite electrode provided in a specific embodiment of the present invention;

[0030] FIG5 is a schematic structural diagram of a composite electrode provided in a specific embodiment of the present invention;

[0031] FIG6 is a schematic structural diagram of a composite electrode provided in a specific embodiment of the present invention;

[0032] FIG7 is a schematic diagram of the composite electrode structure before and after gradient temperature increase in a specific embodiment of the present invention;

[0033] FIG8 is an SEM image of the composite electrode of Example 1 before and after heat treatment. FIG8 shows an SEM image of the surface of the PAA precursor spun membrane on the left and an SEM image of the surface of the fiber separator layer after imidization on the right.

[0034] FIG9 shows the test results of a 140° C. hot box test on the lithium-ion batteries of Example 1 and Comparative Example 1;

[0035] FIG10 is a test result of the capacity retention rate of the lithium-ion batteries of Example 1 and Comparative Example 1 under high and low temperature conditions;

[0036] In the figure, 1-positive electrode current collector, 2-positive electrode conductive primer layer, 3-positive electrode active material layer, 4-fiber separator layer, 5-inorganic filler layer, 6-negative electrode active material layer, 7-negative electrode conductive primer layer, 8-negative electrode current collector, 11-negative electrode active material layer before heat treatment, 12-PAA precursor spinning membrane. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0038] For simplicity, the present invention only explicitly discloses certain numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and similarly, any upper limit can be combined with any other upper limit to form an unspecified range. In addition, although not explicitly stated, unless otherwise specified, each point or individual value between the endpoints of a range is included in the range. Thus, each point or individual value can serve as its own lower limit or upper limit and be combined with any other point or individual value, or with other lower limits or upper limits, to form an unspecified range.

[0039] Conventional separator materials for lithium-ion batteries in the prior art have problems such as low lithium ion permeability and poor high-temperature resistance, which will affect the dynamic performance and high-temperature safety performance of lithium-ion batteries.

[0040] In order to solve the above problems, the present invention provides a composite electrode, and the technical solution adopted is as follows:

[0041] A composite electrode comprises a pole piece and a fiber diaphragm layer, wherein the fiber diaphragm layer is located on the surface of the pole piece; the fiber diaphragm layer contains porous fibers; and the porous fibers contain polyimide.

[0042] In some embodiments, the porosity of the fiber diaphragm layer is 30-80%; exemplarily, the upper limit of the porosity of the fiber diaphragm layer is selected from any value of 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, and 80%, and the lower limit of the porosity of the fiber diaphragm layer is selected from any value of 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, and 75%. The porosity of the fiber diaphragm layer is selected from the range consisting of any value selected from the upper limit of porosity and the lower limit of porosity.

[0043] In some specific embodiments, the thickness of the fiber diaphragm layer is 5μm to 30μm; exemplarily, the upper limit of the thickness of the fiber diaphragm layer is selected from any value of 6μm, 7μm, 8μm, 10μm, 12μm, 14μm, 15μm, 17μm, 18μm, 20μm, 22μm, 24μm, 25μm, 27μm, 28μm, and 30μm, and the lower limit of the thickness of the fiber diaphragm layer is selected from any value of 5μm, 6μm, 7μm, 8μm, 10μm, 12μm, 14μm, 15μm, 17μm, 18μm, 20μm, 22μm, 24μm, 25μm, 27μm, and 28μm, and the thickness of the fiber diaphragm layer is selected from the range consisting of any one value of the upper limit and lower limit of the thickness.

[0044] In some embodiments, the average pore size of the fiber membrane layer is 100-500 nm, preferably 150 nm.

[0045] In some embodiments, the fiber diameter of the porous fiber is 100nm to 1μm; illustratively, the upper limit of the fiber diameter of the porous fiber is selected from any value of 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, and 1μm, the lower limit of the diameter of the porous fiber is selected from any value of 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, and 900nm, and the diameter of the porous fiber is selected from the range consisting of any one value of the upper diameter limit and the lower diameter limit.

[0046] In some specific embodiments, the fiber diaphragm layer further comprises an adhesive; the adhesive comprises at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyethylene glycol, polyethylene oxide, polyphenylene ether, polypropylene carbonate, polymethyl methacrylate, polyethylene terephthalate, polychlorotrifluoroethylene-vinylidene fluoride copolymer, polyethylene oxide, polyvinylidene fluoride derivatives, polyvinylidene fluoride-hexafluoropropylene derivatives, polyamide derivatives, polyacrylonitrile derivatives, polyethylene glycol derivatives, polyethylene oxide derivatives, polyphenylene ether derivatives, polypropylene carbonate derivatives, polymethyl methacrylate derivatives, polyethylene terephthalate derivatives, polychlorotrifluoroethylene-vinylidene fluoride copolymer derivatives, and polyethylene oxide derivatives.

[0047] Optionally, the adhesive can be added to the fiber membrane layer by electrospinning or coating.

[0048] In some embodiments, the fiber separator further includes an inorganic filler, and the inorganic filler is a lithium ion conductor material and / or a non-lithium ion conductor material.

[0049] Optionally, the inorganic filler is located inside the porous fiber, or in the gaps between the porous fibers, or forms a laminated structure with the fiber diaphragm layer. The inorganic filler being located inside the porous fiber means that the inorganic filler particles are inside a single fiber material and are embedded and distributed inside the single fiber; the inorganic filler being located in the gaps between the porous fibers means that the inorganic filler particles fill the space between the fibers; the inorganic filler forming a laminated structure with the fiber diaphragm layer means that the inorganic filler forms an inorganic filler layer and is stacked with the fiber diaphragm layer in sequence to form a layer by layer structure, that is, a structure with an inorganic filler layer stacked on the fiber diaphragm layer.

[0050] Specifically, the non-lithium ion conductor material is selected from at least one of metal oxides, metal hydroxides, SiO2, SrTiO3, and boehmite.

[0051] Exemplarily, the metal oxide is selected from at least one of HfO2, SnO2, CeO2, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, and TiO2;

[0052] The metal hydroxide is magnesium hydroxide and / or aluminum hydroxide;

[0053] The lithium ion conductor material is selected from at least one of Li2O, LiF, LiOH, Li2CO3, LiAlO2, Li3PO4, lithium nitrides, lithium titanium phosphates, lithium aluminum titanium phosphates, lithium lanthanum titanates, lithium germanium thiophosphate, P3O y , z , y , x , y , x , 12 , , x ,

[0056] , ,

[0055] , ,

[0054] glasses, SiS2 glass, P2S5 glass, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2 ceramics, and lithium garnet composite ceramics;

[0054] The lithium nitride is selected from at least one of the substances shown by Chemical Formula a, Chemical Formula a: Li x N y , where in the Chemical Formula a, 0 < x < 4 and 0 < y < 2;

[0055] The lithium titanium phosphate is selected from at least one of the substances shown by Chemical Formula b, Chemical Formula b: Li x Ti y (PO4)3, where in the Chemical Formula b, 0 < x < 2 and 0 < y < 3;

[0056] The lithium aluminum titanium phosphate is selected from at least one of the substances shown by Chemical Formula c, Chemical Formula c: Li x Al y Ti z(PO4)3, wherein, in the chemical formula c, 0 < x < 2, 0 < y < 1 and 0 < z < 3;

[0057] The lithium lanthanum titanate is selected from at least one of the substances having the chemical formula d, chemical formula d: Li x La y TiO3, in the chemical formula d, 0 < x < 2 and 0 < y < 3;

[0058] The lithium germanium thiophosphate is selected from at least one of the substances having the chemical formula e, chemical formula e: Li x Ge y P z S w , wherein, in the chemical formula e, 0 < x < 4, 0 < y < 1, 0 < z < 1 and 0 < w < 5;

[0059] The P3O 12 glass is selected from at least one of the substances having the chemical formula f, chemical formula f: Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 , wherein, in the chemical formula f, 0 ≤ x ≤ 1 and 0 ≤ y ≤ 1;

[0060] The SiS2 glass is selected from at least one of the substances having the chemical formula g, chemical formula g: Li x Si y S z , wherein, in the chemical formula g, 0 ≤ x < 3, 0 < y < 2 and 0 < z < 4;

[0061] The P2S5 glass is selected from at least one of the substances having the chemical formula h, chemical formula h: Li x P y S z , wherein, in the chemical formula h, 0 ≤ x < 3, 0 < y < 3 and 0 < z < 7;

[0062] The lithium garnet composite ceramic is selected from at least one of the substances having the chemical formula i, chemical formula i: Li 3+x La3M2O 12 , wherein, in the chemical formula i, 0 ≤ x ≤ 5, and M is selected from any one of Te, Nb, and Zr.

[0063] In some embodiments, the electrode sheet includes a positive electrode sheet or a negative electrode sheet, and the fibrous separator layer can be located on the surface of the positive electrode sheet, or the fibrous separator layer can be located on the surface of the negative electrode sheet, or the fibrous separator layer can be located on the surfaces of both the positive electrode sheet and the negative electrode sheet simultaneously.

[0064] Referring to the structural schematic diagram of the composite electrode shown in Figure 1, in some specific embodiments, the positive electrode plate includes a positive electrode current collector 1 and a positive electrode active material layer 3; the positive electrode current collector 1, the positive electrode active material layer 3 and the fiber diaphragm layer 4 are stacked in sequence; and / or, the negative electrode plate includes a negative electrode current collector 8 and a negative electrode active material layer 6, and the negative electrode current collector 8, the negative electrode active material layer 6 and the fiber diaphragm layer 4 are stacked in sequence.

[0065] 2 , in some embodiments, the positive electrode current collector 1 , the positive electrode active material layer 3 , the fiber separator layer 4 , the negative electrode active material layer 6 and the negative electrode current collector 8 are stacked in sequence.

[0066] Referring to the structural schematic diagram of the composite electrode shown in Figure 3, the positive electrode plate includes a positive electrode current collector 1, a positive electrode active material layer 3 and a positive electrode conductive primer layer 2, and the positive electrode current collector 1, the positive electrode conductive primer layer 2, the positive electrode active material layer 3 and the fiber diaphragm layer 4 are stacked in sequence; and / or, the negative electrode plate includes a negative electrode current collector 8, a negative electrode active material layer 6 and a negative electrode conductive primer layer 7, and the negative electrode current collector 8, the negative electrode conductive primer layer 7, the negative electrode active material layer 6 and the fiber diaphragm layer 4 are stacked in sequence.

[0067] Referring to the structural schematic diagram of the composite electrode shown in Figure 4, in some embodiments, the positive electrode current collector 1, the positive electrode conductive primer layer 2, the positive electrode active material layer 3, the fiber separator layer 4, the negative electrode active material layer 6, the negative electrode conductive primer layer 7 and the negative electrode current collector 8 are stacked in sequence.

[0068] In some embodiments, the composite electrode includes a positive electrode current collector 1, a positive electrode active material layer 3 and an inorganic filler layer 5, and the positive electrode current collector 1, the positive electrode active material 3, the fiber diaphragm layer 4 and the inorganic filler layer 5 are stacked in sequence; and / or, the composite electrode includes a negative electrode current collector 8, a negative electrode active material layer 6 and an inorganic filler layer 5, and the negative electrode current collector 8, the negative electrode active material layer 6, the fiber diaphragm layer 4 and the inorganic filler layer 5 are stacked in sequence.

[0069] In some embodiments, the positive electrode current collector 1, the positive electrode active material layer 3, the fiber separator layer 4, the inorganic filler layer 5, the fiber separator layer 4, the negative electrode active material layer 6 and the negative electrode current collector 8 are stacked in sequence;

[0070] Referring to the structural schematic diagram of the composite electrode shown in Figure 5, the composite electrode includes a positive electrode current collector 1, a positive electrode active material layer 3, a positive electrode conductive primer layer 2 and an inorganic filler layer 5, and the positive electrode current collector 1, the positive electrode conductive primer layer 2, the positive electrode active material 3, the fiber diaphragm layer 4 and the inorganic filler layer 5 are stacked in sequence; and / or, the composite electrode includes a negative electrode current collector 8, a negative electrode active material layer 6, a negative electrode conductive primer layer 7 and an inorganic filler layer 5, and the negative electrode current collector 8, the negative electrode conductive primer layer 7, the negative electrode active material layer 6, the fiber diaphragm layer 4 and the inorganic filler layer 5 are stacked in sequence.

[0071] Referring to the structural schematic diagram of the composite electrode shown in Figure 6, in some embodiments, the positive electrode current collector 1, the positive electrode conductive primer layer 2, the positive electrode active material layer 3, the fiber diaphragm layer 4, the inorganic filler layer 5, the fiber diaphragm layer 4, the negative electrode active material layer 6, the negative electrode conductive primer layer 7 and the negative electrode current collector 8 are stacked in sequence.

[0072] 1 to 6 only exemplify the stacking structure of a single side of the electrode, and do not limit the composite electrode sheet of the present invention. The front and / or back sides of the electrode can be configured with reference to FIG. 1 to 6 .

[0073] In some specific embodiments, the positive electrode plate is prepared by a method comprising the following steps: the positive electrode active material lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and polyvinylidene fluoride (PVDF) are mixed according to the weight ratio of the positive electrode material formula, N-methylpyrrolidone (NMP) is added as a solvent, and a slurry with a solid content of 0.7 to 0.8 is prepared, preferably with a solid content of 0.75. After stirring evenly, it is coated on the current collector aluminum foil and dried at 85 to 95°C, preferably at 90°C. After the above steps are completed, a single-sided coated positive electrode plate is obtained. The plate can then be cut into suitable specifications for use, for example, 38mm×58mm. Finally, the coating and drying steps are repeated on the back of the single-sided coated positive electrode plate to obtain a double-sided coated positive electrode plate.

[0074] Exemplarily, the weight ratio of the positive electrode material formula of lithium cobalt oxide: conductive carbon black: polyvinylidene fluoride is (96-99): (0.5-2): (0.5-3), for example, the weight ratio of lithium cobalt oxide: conductive carbon black: polyvinylidene fluoride is 97.5:1.0:1.5.

[0075] In some specific embodiments, the negative electrode sheet is prepared using a method comprising the following steps: mixing the negative electrode active material graphite, conductive carbon black (Super P), styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC) according to the weight ratio of the positive electrode material formula, adding deionized water (H2O) as a solvent, and preparing a slurry with a solid content of 0.6-0.8, preferably 0.7. After stirring evenly, the slurry is coated on a copper foil current collector and dried at 100-120°C, preferably 110°C, to obtain a single-sided coated negative electrode sheet. The sheet is then cut into suitable sizes for use, for example, 41 mm x 61 mm. Finally, the coating and drying steps are repeated on the back of the single-sided coated negative electrode sheet to obtain a double-sided coated negative electrode sheet.

[0076] In some specific embodiments, the percentage of sodium carboxymethyl cellulose in the negative electrode material to the total weight of the negative electrode active material is 0.5-3%, preferably 1.5%.

[0077] Exemplarily, the weight ratio of the negative electrode material formula is (93-98): (0.5-1.5): (0.5-3): (0.5-3), for example, the weight ratio of graphite: conductive carbon black: styrene-butadiene rubber: sodium carboxymethyl cellulose is 96:1:1.5:1.5.

[0078] In some specific embodiments, the composite electrode of the present invention is prepared by a method comprising the following steps: forming a spinning membrane on the surface of the electrode by the precursor PAA through an electrospinning process; imidizing PAA through heat treatment to obtain a fiber diaphragm layer containing polyimide, thereby obtaining the composite electrode.

[0079] In some specific embodiments, the negative electrode sheet contains a negative electrode active material layer; referring to the schematic diagram of the composite electrode structure before and after the gradient heating shown in Figure 7, before the gradient heating and insulation operation is performed, the PAA precursor spinning membrane 12 is located on the negative electrode sheet, and the negative electrode active material layer 11 before heat treatment contains sodium carboxymethyl cellulose, which has a relatively dense structure and low porosity; through the gradient heating and insulation operation, the PAA precursor undergoes an imidization reaction to form a fiber diaphragm layer 4 containing polyimide fibers, and at the same time, the sodium carboxymethyl cellulose is carbonized and decomposed to form carbon particles and pores, forming a negative electrode active material layer 6 with higher porosity.

[0080] Exemplarily, the heat treatment includes a gradient temperature rise and heat preservation operation; the gradient temperature rise and heat preservation operation includes: the end point temperature of the gradient temperature rise and heat preservation operation is 280 to 320° C., and the heat preservation at the end point temperature is 30 to 90 minutes.

[0081] Optionally, the gradient heating and insulation operation includes: heating from room temperature to 80-120°C at a heating rate of 2-4°C / min, and keeping warm at 80-120°C for 25-35 minutes; continuing to heat up to 180-220°C at a heating rate of 2-4°C / min, and keeping warm at 180-220°C for 25-35 minutes; continuing to heat up to 280-320°C at a heating rate of 2-4°C / min, and keeping warm at 280-320°C for 30-90 minutes.

[0082] Optionally, the heat treatment is performed under vacuum or inert gas conditions.

[0083] Optionally, the preparation method of the composite electrode of the present invention includes the following steps: forming a spinning membrane on the surface of the electrode piece by the precursor PAA through an electrospinning process; imidizing PAA through heat treatment to obtain a fiber diaphragm layer containing polyimide, thereby obtaining the composite electrode.

[0084] In some embodiments, the porosity of the negative electrode sheet is 20-50%. In the present invention, the porosity of the negative electrode sheet refers to the porosity of the negative electrode active material layer. For example, the upper limit of the porosity of the negative electrode sheet is selected from any value of 25%, 30%, 35%, 40%, 45%, and 50%, and the lower limit of the porosity of the negative electrode sheet is selected from any value of 20%, 25%, 30%, 35%, 40%, and 45%. The porosity of the negative electrode sheet is selected from a range consisting of any one of the upper limit and lower limit of the porosity.

[0085] In some specific embodiments, the negative electrode plate includes a negative electrode active material layer, and the content of sodium carboxymethyl cellulose is 0-0.001 wt % based on the negative electrode active material layer. Sodium carboxymethyl cellulose (CMC) is currently the main binder for negative electrode materials. The negative electrode active material layer of the negative electrode plate provided by the present invention does not contain sodium carboxymethyl cellulose or contains only a trace amount of sodium carboxymethyl cellulose. This is because when porous fibers containing polyimide (PI) are directly prepared on the negative electrode plate, the CMC in the negative electrode active material layer is carbonized and decomposed by high temperature during the heat treatment stage of the polyimide fiber preparation process.

[0086] When the porous fibers containing polyimide are prepared directly on the negative electrode plate, the interfacial adhesion between the fiber diaphragm layer and the positive electrode and the negative electrode is different. In some exemplary embodiments, the interfacial adhesion between the fiber diaphragm layer and the positive electrode plate is 5 to 10 N / m, and the interfacial adhesion between the fiber diaphragm layer and the negative electrode plate is 13 to 20 N / m.

[0087] The present invention also provides an electrochemical device comprising any one of the above composite electrodes. Optionally, the electrochemical device is any one of a cell, a module and a battery.

[0088] In some embodiments, the electrochemical device is membrane-free.

[0089] Optionally, the electrolyte in the electrochemical device has a lithium salt concentration of 1 to 2 mol / L, preferably 1.15 mol / L. The lithium salt may be lithium hexafluorophosphate (LiPF6).

[0090] The electrolyte solvent can be selected from at least one of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC); illustratively, the mass ratio of ethylene carbonate: ethyl methyl carbonate: diethyl carbonate is (20-40): (40-60): (10-30); for example, the mass ratio of ethylene carbonate: ethyl methyl carbonate: diethyl carbonate can be 30:50:20.

[0091] Exemplarily, the electrolyte is prepared by a method comprising the following steps: under an inert atmosphere, taking a dry argon atmosphere as an example, the organic solvents ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate are mixed according to a mass ratio, and then a suitable mass of lithium salt is added to the mixed solvent to dissolve and mix evenly to obtain the electrolyte.

[0092] The electrochemical device can be prepared by a method comprising the following steps: stacking and fixing the positive electrode sheet, the negative electrode sheet and the fiber separator layer, wherein the stacking method includes but is not limited to the stacking method shown in Figures 2, 4 and 6, and then placing the fixed stacked structure in an aluminum-plastic film, sealing the top and side, injecting liquid, and packaging to obtain the device.

[0093] Example

[0094] The technical solutions of the present invention are described below with reference to specific embodiments. The raw materials used in the following embodiments are all from common commercially available products, and the devices or equipment used are all purchased from conventional market sales channels.

[0095] Example 1

[0096] The composite electrode of this embodiment includes a negative electrode plate and a fiber separator layer. The fiber separator layer contains porous fibers, which include polyimide fibers. The fiber separator layer has a porosity of 60%, a thickness of 15μm, an average pore size of 150nm, and a porous fiber diameter of 300nm. The negative electrode plate has a porosity of 20% and includes a negative electrode active material layer. The content of sodium carboxymethyl cellulose is 0.001wt% based on the negative electrode active material layer. The interfacial adhesion between the fiber separator layer and the positive electrode plate is 6N / m, and the interfacial adhesion between the fiber separator layer and the negative electrode plate is 13N / m.

[0097] The composite electrode of this embodiment is prepared by a method comprising the following steps:

[0098] 1) Preparation of negative electrode sheet

[0099] The negative electrode active materials, graphite, conductive carbon black (Super P), styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC), are mixed in a weight ratio of 96:1:1.5:1.5. Deionized water is added as a solvent to form a slurry with a solid content of 0.7%. After stirring evenly, the mixture is coated on a copper foil current collector and dried at 110°C to obtain a single-sided coated negative electrode sheet. After drying, the sheet is cut into 41mm × 61mm squares for future use. After completing the above steps on one side of the negative electrode sheet, the same steps are repeated on the back side of the sheet using the same method to obtain a double-sided coated negative electrode sheet.

[0100] 2) Preparation of PAA precursor spinning membrane

[0101] A 15μm-thick PAA precursor membrane was prepared on the surface of the negative electrode sheet through electrospinning. The membrane had an average pore size of 150nm and a porosity of 60%. After spinning on one side was completed, the other side was spun under the same conditions, ultimately forming a PAA precursor membrane encapsulating the negative electrode sheet.

[0102] 3) Heat treatment of negative electrode

[0103] The PAA is imidized by a gradient heating and holding operation, and the sodium carboxymethyl cellulose contained in the negative electrode active material layer is carbonized to form carbon particles and pores. The gradient heating and holding operation includes: (1) gradually increasing the temperature from room temperature to 100°C at a heating rate of 3°C / min; (2) holding at 100°C for 30 minutes; (3) gradually increasing the temperature to 200°C at a heating rate of 3°C / min; (4) holding at 200°C for 30 minutes; (5) gradually increasing the temperature to 300°C at a heating rate of 3°C / min; (6) holding at 300°C for 30 minutes; (7) cooling the temperature to room temperature to obtain the composite electrode of this embodiment.

[0104] This embodiment also provides a lithium-ion battery using the composite electrode of this embodiment, wherein the preparation method of the positive electrode plate in the lithium-ion battery includes: mixing the positive electrode active material lithium cobalt oxide, conductive carbon black, and polyvinylidene fluoride in a weight ratio of 97.5:1.0:1.5, adding N-methylpyrrolidone (NMP) as a solvent, and preparing a slurry with a solid content of 0.75%, stirring evenly, and coating it on the current collector aluminum foil, and drying it at 90°C to obtain a single-sided coated positive electrode plate. After drying, the plate is cut into a size of (38mm×58mm) for future use. After completing the above steps, the single-sided coating of the positive electrode plate is completed. Thereafter, these steps are also completed on the back of the plate using exactly the same method, and dried at 90°C to obtain a double-sided coated positive electrode plate.

[0105] The preparation method of the electrolyte in the lithium-ion battery includes: first mixing organic solvents ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a mass ratio of 30:50:20 in a dry argon atmosphere, then adding lithium salt lithium hexafluorophosphate to the organic solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.

[0106] The preparation method of the lithium-ion battery of this embodiment includes: stacking the positive electrode sheet, the negative electrode sheet and the fiber separator layer, fixing the four corners of the entire laminate structure with tape, and then placing the fixed laminate structure in an aluminum-plastic film. After top and side sealing, electrolyte injection, and packaging, the lithium-ion battery of this embodiment is obtained.

[0107] Example 2

[0108] The composite electrode of this embodiment includes a negative electrode plate and a fiber separator layer. The fiber separator layer contains porous fibers, which include polyimide fibers. The fiber separator layer has a porosity of 60%, a thickness of 15μm, an average pore size of 150nm, and a porous fiber diameter of 300nm. The negative electrode plate has a porosity of 23% and includes a negative electrode active material layer. The content of sodium carboxymethyl cellulose is 0.0001wt% based on the negative electrode active material layer. The interfacial adhesion between the fiber separator layer and the positive electrode plate is 7N / m, and the interfacial adhesion between the fiber separator layer and the negative electrode plate is 16N / m.

[0109] The only difference between the preparation method of the composite electrode of this embodiment and that of embodiment 1 is that: during the heat treatment of the negative electrode sheet in step 3), (6) the temperature is kept at 300° C. for 60 minutes.

[0110] Example 3

[0111] The composite electrode of this embodiment includes a negative electrode sheet and a fiber separator layer. The fiber separator layer includes porous fibers, which include polyimide fibers. The fiber separator layer has a porosity of 60%, a thickness of 15μm, an average pore size of 150nm, and a porous fiber diameter of 300nm. The negative electrode sheet has a porosity of 25% and includes a negative electrode active material layer. The sodium carboxymethyl cellulose content is 0wt% based on the negative electrode active material layer. The interfacial adhesion between the fiber separator layer and the positive electrode sheet is 6N / m, and the interfacial adhesion between the fiber separator layer and the negative electrode sheet is 15N / m.

[0112] The only difference between the preparation method of the composite electrode of this embodiment and that of embodiment 1 is that: during the heat treatment of the negative electrode sheet in step 3), (6) the temperature is kept at 300° C. for 90 minutes.

[0113] Example 4

[0114] The composite electrode of this embodiment includes a negative electrode sheet and a fiber separator layer. The fiber separator layer includes porous fibers, which include polyimide fibers. The fiber separator layer has a porosity of 30%, a thickness of 15 μm, an average pore size of 300 nm, and a porous fiber diameter of 1 μm. The negative electrode sheet has a porosity of 20%, includes a negative electrode active material layer, and, based on the negative electrode active material layer, contains 0 wt% sodium carboxymethyl cellulose. The interfacial adhesion between the fiber separator layer and the positive electrode sheet is 5 N / m, and the interfacial adhesion between the fiber separator layer and the negative electrode sheet is 13 N / m.

[0115] The method for preparing the composite electrode of this embodiment differs from that of Example 1 only in that, in step 2), during the preparation of the PAA precursor spun membrane, a 15 μm thick PAA precursor spun membrane is prepared on the surface of the negative electrode sheet by electrospinning. The membrane has an average pore size of 300 nm, a fiber diameter of 1 μm, and a porosity of 30%. After spinning is completed on one side, spinning is repeated on the other side under the same conditions, ultimately forming the PAA precursor spun membrane encapsulating the negative electrode sheet.

[0116] Example 5

[0117] The composite electrode of this embodiment includes a negative electrode plate and a fiber separator layer. The fiber separator layer includes porous fibers, which include polyimide fibers. The fiber separator layer has a porosity of 80%, a thickness of 15 μm, an average pore size of 300 nm, and a porous fiber diameter of 300 nm. The negative electrode plate has a porosity of 50%, includes a negative electrode active material layer, and, based on the negative electrode active material layer, contains 0 wt% sodium carboxymethyl cellulose. The interfacial adhesion between the fiber separator layer and the positive electrode plate is 10 N / m, and the interfacial adhesion between the fiber separator layer and the negative electrode plate is 20 N / m.

[0118] The preparation method of the composite electrode of this embodiment differs from that of Example 1 only in that: Step 1) the negative electrode material formula has a weight ratio of graphite: conductive carbon black: styrene-butadiene rubber: sodium carboxymethyl cellulose of 94.5:1:1.5:3; Step 2) during the preparation of the PAA precursor spinning membrane, a 15μm thick PAA precursor spinning membrane is prepared on the surface of the negative electrode sheet by electrospinning. The membrane has an average pore size of 300nm, a fiber diameter of 300nm, and a porosity of 80%. After spinning is completed on one side, spinning is repeated on the other side under the same conditions, ultimately forming a PAA precursor spinning membrane-wrapped negative electrode sheet.

[0119] Example 6

[0120] The composite electrode of this embodiment differs from that of embodiment 1 only in that the porosity of the fiber separator layer is 60%, and the porosity of the negative electrode sheet is 30%.

[0121] The preparation method of the composite electrode of this embodiment differs from that of Example 1 only in that: Step 1) the weight ratio of the negative electrode material formula is graphite: conductive carbon black: styrene-butadiene rubber: sodium carboxymethyl cellulose is 95.5:1:1.5:2.

[0122] Example 7

[0123] The composite electrode of this embodiment differs from that of embodiment 1 only in that the porosity of the fiber separator layer is 60%, and the porosity of the negative electrode sheet is 40%.

[0124] The preparation method of the composite electrode of this embodiment differs from that of Example 1 only in that: Step 1) the weight ratio of the negative electrode material formula is graphite: conductive carbon black: styrene-butadiene rubber: sodium carboxymethyl cellulose is 95:1:1.5:2.5.

[0125] Example 8

[0126] The composite electrode of this embodiment differs from that of embodiment 1 only in that the porosity of the fiber diaphragm layer is 60% and the average pore diameter is 500 nm.

[0127] The method for preparing the composite electrode of this embodiment differs from that of Example 1 only in that, during step 2) the preparation of the PAA precursor spun membrane, a 15 μm thick PAA precursor spun membrane is electrospun on the surface of the negative electrode sheet. The membrane has an average pore size of 500 nm, a fiber diameter of 300 nm, and a porosity of 60%. After spinning is completed on one side, the other side is spun under the same conditions, ultimately forming the PAA precursor spun membrane encapsulating the negative electrode sheet.

[0128] Example 9

[0129] The composite electrode of this embodiment differs from that of Example 1 only in that the fiber separator layer comprises porous fibers containing polyimide fibers and PVDF fibers. After preparing the negative electrode sheet encapsulated by the PAA precursor spinning membrane, an adhesive layer is prepared using an electrospinning process. The adhesive solution has a mass ratio of PVDF (wt%) to 20%, and the solvent is DMF.

[0130] Example 10

[0131] The composite electrode of this embodiment differs from that of embodiment 1 only in that: after the negative electrode is heat-treated, an inorganic filler layer is coated. The formula of the inorganic filler layer is: inorganic ceramic filler: PVDF = 80:20 by mass, and the solvent is NMP.

[0132] Comparative Example 1

[0133] The lithium-ion battery preparation method of this comparative example differs from that of Example 1 only in that, after the double-sided coated negative electrode sheet is prepared, the subsequent preparation of the PAA precursor spinning membrane and the heat treatment of the negative electrode sheet are omitted. A 15 μm thick polyethylene separator is used and placed between the positive and negative electrode sheets.

[0134] Comparative Example 2

[0135] The lithium-ion battery preparation method of this comparative example differs from that of Example 1 only in that, after the double-sided coated negative electrode sheet is prepared, a 15 μm thick PVDF fiber layer with an average pore size of 150 nm and a porosity of 60% is prepared on the surface of the negative electrode sheet by electrospinning. After spinning is completed on one side, the other side is spun under the same conditions, ultimately forming a fiber-wrapped negative electrode sheet. The remaining process is the same as in Comparative Example 1.

[0136] Comparative Example 3

[0137] The lithium-ion battery preparation method of this comparative example differs from that of Example 1 only in that, after the double-sided coated negative electrode sheet is prepared, a self-supporting PI fiber separator is prepared: a 15 μm-thick PAA fiber layer with an average pore size of 150 nm and a porosity of 60% is electrospun onto a silicone oil paper substrate. The PAA is then imidized using a gradient heating and holding process, similar to that of Example 1. After imidization, the resulting PI fiber separator is carefully peeled from the silicone oil paper and used as a separator to assemble with the positive and negative electrode sheets into a lithium-ion laminated battery.

[0138] Comparative Example 4

[0139] The preparation method of the lithium-ion battery in this comparative example differs from that in Example 1 only in that: electrospinning is performed on the surface of the negative electrode plate to prepare the negative electrode plate wrapped and encapsulated by the PAA precursor spinning membrane, and then the heat treatment step is omitted and the battery is directly assembled into a lithium-ion laminated battery.

[0140] Test example

[0141] The surface morphology of the composite electrode of Example 1 before and after heat treatment was observed using a scanning electron microscope (SEM). The SEM results are shown in Figure 8. The left side of Figure 8 shows an SEM image of the PAA precursor spun membrane surface, and the right side shows an SEM image of the fiber separator layer after imidization. Figure 8 shows that after the heat treatment and imidization process, the fiber morphology and structure remain stable, with no significant changes.

[0142] The lithium-ion battery of Example 1 was subjected to a 140°C hot box test. The results are shown in Figure 9. As shown in Figure 9, the Example did not experience thermal runaway at 140°C, while the battery cell of Comparative Example 1 burned and the temperature continued to rise. This shows that the composite electrode of Example 1 has high thermal stability and can ensure the thermal safety performance of the battery.

[0143] The capacity retention rates of the lithium-ion batteries of Example 1 and Comparative Example 1 under high and low temperature conditions were tested at temperatures between -20°C and 60°C, and the results are shown in Figure 10. As shown in Figure 10, the lithium-ion battery of Example 1 still has a high capacity retention rate of 70% to 90% at low temperatures between -20°C and 0°C, which is higher than the 39% to 82% of Comparative Example 1, demonstrating superior low-temperature performance.

[0144] The lithium ion batteries of Examples 1 to 9 and Comparative Examples 1 to 4 were tested for adhesion between the fiber separator layer and the negative electrode, self-discharge rate of the battery cell, 2C discharge capacity / 0.1C discharge capacity, capacity after 500 cycles / initial discharge capacity, and 140°C hot box test. The performance data are shown in Table 1 below:

[0145] Table 1 Lithium ion battery performance test results of Examples 1 to 9 and Comparative Examples 1 to 4

[0146] As can be seen from Table 1, the fiber diaphragm layer of Examples 1 to 10 has a strong bonding force with the negative electrode, reaching 13 to 20 N / m. In addition, the diaphragms of Comparative Examples 2 and Comparative Examples 4 using the electrospinning process also have a strong bonding force with the negative electrode. It can be seen that the fiber diaphragm prepared by the electrospinning process has a high bonding force with the substrate electrode. The lithium ion batteries of Examples 1 to 10 have a low self-discharge rate of only 0.032 to 0.060 mV / h, especially in Examples 2 and 3 which are subjected to a 60 to 90 min heat treatment at about 300°C. The self-discharge rate of the battery cell is only 0.032 to 0.038 mV / h, which is conducive to long-term stable storage and service. In addition, the lithium ion batteries of Examples 1 to 10 exhibit a high discharge specific capacity at a high rate, with a 2C discharge specific capacity / 0.1C discharge specific capacity of 92.3 to 93.8%, which is much higher than 86.2 to 88.6% of Comparative Examples 1 to 4. The porosity of the fiber diaphragm layer is 2C. The 2C discharge specific capacity / 0.1C discharge specific capacity of Examples 1 to 4 and 6 to 8 with a negative electrode porosity of 20 to 40% all reached more than 93.0%, showing strong rate performance. Moreover, the lithium ion batteries of Examples 1 to 10 can also ensure strong cycle performance. After 500 cycles, the discharge capacity can still reach 88.3 to 92.7% of the initial discharge capacity, which is higher than 85.6 to 87.6% of Comparative Examples 1 to 4. The lithium ion batteries of Examples 1 to 4 and 6 with a fiber diaphragm layer porosity of 30 to 80%, an average pore size of 150 to 300 nm, and a negative electrode porosity of 20 to 30% can still reach more than 90.3% of the initial discharge capacity after 500 cycles, showing excellent cycle stability. In addition, the lithium ion batteries of Examples 1 to 10 all passed the 140°C hot box test, which shows that the composite electrode and electrochemical device provided by the present invention can ensure extremely high thermal stability.

[0147] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent replacements, and improvements made within the spirit and principles of the present application should be included in the scope of protection of the present application.

Claims

1. A composite electrode, characterized in that: The composite electrode comprises a pole piece and a fiber diaphragm layer, wherein the fiber diaphragm layer is located on the surface of the pole piece; The fiber diaphragm layer comprises porous fibers; The porous fiber contains polyimide.

2. The composite electrode according to claim 1, characterized in that The porosity of the fiber diaphragm layer is 30-80%; and / or, The thickness of the fiber diaphragm layer is 5 to 30 μm; and / or, The average pore size of the fiber diaphragm layer is 100 to 500 nm; and / or, The fiber diameter of the porous fiber is 100 nm to 1 μm; and / or, The fiber diaphragm layer further comprises an adhesive; the adhesive comprises at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyethylene glycol, polyethylene oxide, polyphenylene ether, polypropylene carbonate, polymethyl methacrylate, polyethylene terephthalate, polychlorotrifluoroethylene-vinylidene fluoride copolymer, polyethylene oxide, polyvinylidene fluoride derivatives, polyvinylidene fluoride-hexafluoropropylene derivatives, polyamide derivatives, polyacrylonitrile derivatives, polyethylene glycol derivatives, polyethylene oxide derivatives, polyphenylene ether derivatives, polypropylene carbonate derivatives, polymethyl methacrylate derivatives, polyethylene terephthalate derivatives, polychlorotrifluoroethylene-vinylidene fluoride copolymer derivatives, and polyethylene oxide derivatives; and / or, The fiber diaphragm also includes an inorganic filler, which is a lithium ion conductor material and / or a non-lithium ion conductor material; the inorganic filler is located in the porous fibers, or in the gaps between the porous fibers, or forms a stacked structure with the fiber diaphragm layer.

3. The composite electrode according to claim 2, characterized in that: The porosity of the fiber diaphragm layer is 50-60%; and / or, The thickness of the fiber diaphragm layer is 10 to 15 μm; and / or, The average pore size of the fiber diaphragm layer is 100-200 nm; and / or, The fiber diameter of the porous fiber is 300-600 nm.

4. The composite electrode according to claim 1, characterized in that: The electrode sheet includes a positive electrode sheet or a negative electrode sheet.

5. The composite electrode according to claim 4, characterized in that The porosity of the negative electrode sheet is 20-50%; and / or, The negative electrode plate comprises a negative electrode active material layer, and the content of sodium carboxymethyl cellulose is 0 to 0.001 wt % based on the negative electrode active material layer; and / or, The interfacial bonding force between the fiber diaphragm layer and the positive electrode plate is 5 to 10 N / m, and the interfacial bonding force between the fiber diaphragm layer and the negative electrode plate is 13 to 20 N / m.

6. The composite electrode according to claim 1, characterized in that: The fiber diaphragm layer is prepared by a method comprising the following steps: Through an electrospinning process, the precursor PAA is formed into a spinning film on the surface of the electrode; Afterwards, the PAA is imidized by a gradient temperature increase and heat preservation operation, thereby obtaining a fiber diaphragm layer containing polyimide.

7. The composite electrode according to claim 6, characterized in that: The electrode sheet includes a negative electrode sheet, and the negative electrode sheet contains a negative electrode active material layer; Before the gradient temperature rise and heat preservation operation is performed, the negative electrode active material layer contains sodium carboxymethyl cellulose; The sodium carboxymethyl cellulose is formed into carbon particles and pores through gradient temperature increase and heat preservation operation.

8. The composite electrode according to claim 1, characterized in that: The pole piece comprises a current collector and an active material layer; the current collector, the active material layer and the fiber separator layer are stacked in sequence; and / or, The pole piece comprises a current collector, an active material layer and a conductive primer layer; the conductive primer layer comprises a conductive material and an adhesive; the conductive material comprises at least one of carbon black, carbon nanotubes and graphene; the current collector, the conductive primer layer, the active material layer and the fiber separator layer are stacked in sequence; and / or, The composite electrode comprises a current collector, an active material layer and an inorganic filler layer; the current collector, the active material layer, the fiber separator layer and the inorganic filler layer are stacked in sequence; and / or, The composite electrode comprises a current collector, an active material layer, a conductive primer layer and an inorganic filler layer; the current collector, the conductive primer layer, the active material layer, the fiber separator layer and the inorganic filler layer are stacked in sequence.

9. An electrochemical device, characterized in that: A composite electrode comprising any one of claims 1 to 8.

10. The electrochemical device according to claim 9, characterized in that The electrochemical device has no diaphragm.

Citation Information

Patent Citations

  • Composite negative plate for lithium ion battery as well as preparation method of composite negative plate and lithium ion battery

    CN103682247A

  • Composite electrode plate of lithium ion battery, preparation method of composite electrode plate and lithium ion battery

    CN104124414A

  • High-temperature-resistant integrated electrode for lithium ion battery and preparation method of high-temperature-resistant integrated electrode

    CN113422060A

  • Electrochemical device and electronic device

    CN113540699A

  • Electrochemical device

    CN115380430A