Degradable polymer nanogel microsphere, and preparation method therefor and use thereof
Temperature- and pH-responsive degradable polymer nanogel microspheres prepared through free radical polymerization in non-polar solvents solve the problem of poor degradation performance in the existing technology and achieve effective applications in the field of biomedicine.
Patent Information
- Application Number
- PCT/CN2023/090597
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Existing stimuli-responsive nanogel microspheres prepared by free radical polymerization have poor degradation properties, which limits their application in tissue engineering and biomedicine.
Temperature- and pH-responsive polymers prepared by free radical polymerization of dimethylaminoethyl methacrylate, vinyl cyclic acetal monomers, dispersants, radical initiators, and cross-linking monomers in nonpolar solvents. Degradable polymer nanogel microspheres overcome the problem of poor degradation performance.
The obtained nanogel microspheres have dual response properties, can be degraded under alkaline conditions, are suitable for drug loading and responsive release, and significantly enhance the application prospects in the field of biomedicine.
Smart Images

Figure PCTCN2023090597-FTAPPB-I100001 
Figure PCTCN2023090597-FTAPPB-I100002 
Figure PCTCN2023090597-FTAPPB-I100003
Abstract
Description
Degradable polymer nanogel microspheres and their preparation method and application Technical Field
[0001] The present invention relates to the technical field of stimulus-responsive functional polymers, in particular to temperature- and pH-responsive degradable polymer nanogel microspheres, and a preparation method and application thereof. Background Art
[0002] Polymer nanogels (also known as microgels) are highly cross-linked colloidal particles with particle sizes typically ranging from 1 nm to 1 μm. Compared to traditional linear polymers, polymer nanogels offer advantages such as low viscosity and high surface area. In recent years, they have demonstrated significant potential for applications in a variety of fields, including biomedicine, food, petrochemicals, and environmental protection.
[0003] Stimuli-responsive nanogels refer to a type of microgel that can expand or shrink in volume due to swelling or solvent extrusion inside the nanogel when external environmental conditions change (such as temperature, pH, ionic strength, etc.). Because of their good application prospects in tissue engineering and biomedicine, they have been a research hotspot in the polymer field for the past decade.
[0004] Currently, stimulus-responsive nanogels are mainly prepared through free radical polymerization technology of vinyl monomers. The main chain skeleton is a CC bond and has poor degradation performance, which is a major obstacle to its practical application in tissue engineering and biomedicine.
[0005] Summary of the Invention
[0006] Based on this, the purpose of the present invention is to overcome the problem of poor degradability currently faced by the preparation of stimulus-responsive nanogels by free radical polymerization, and to provide a temperature and pH responsive degradable polymer nanogel microspheres, as well as a method for preparing the degradable nanogel microspheres by free radical polymerization technology.
[0007] In order to achieve the above-mentioned object of the invention, the present invention includes the following technical solutions.
[0008] A polymer nanogel microsphere, wherein the repeating structural unit in the polymer nanogel microsphere has a structure represented by the following formula (I):
[0009] Wherein, R1 is one of the following structures:
[0010] R2 is n-butyl or n-hexyl.
[0011] A polymer nanogel microsphere is prepared by free radical polymerization of dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer, dispersant, free radical initiator and crosslinking monomer in a non-polar solvent;
[0012] The vinyl cyclic acetal monomer is 2-methylene-4-phenyl-1,3-dioxolane and / or 5,6-benzo-2-methylene-1,3-dioxepane.
[0013] The present invention also provides a method for preparing the degradable polymer nanogel microspheres by free radical polymerization technology, which includes the following technical solutions.
[0014] A method for preparing polymer nanogel microspheres comprises the following steps:
[0015] The dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer, dispersant, free radical initiator and crosslinking monomer are added into a non-polar solvent and reacted under an inert gas atmosphere to obtain the product.
[0016] The present invention also provides an application of the polymer nanogel microspheres, including the following technical solutions.
[0017] The polymer nanogel microspheres are used as carrier materials in the preparation of pH and / or temperature responsive release drugs.
[0018] The present invention also provides a pH and / or temperature responsive drug release method, which includes the following technical solutions.
[0019] A pH and / or temperature responsive release drug is prepared from a drug active ingredient and an adjuvant acceptable in the drug, wherein the adjuvant comprises the polymer nanogel microspheres.
[0020] Wherein, the active pharmaceutical ingredient is a hydrophilic drug, such as heparin.
[0021] A heparin-loaded nanogel microsphere medicine is prepared from raw and auxiliary materials including the polymer nanogel microspheres and heparin.
[0022] In some embodiments, the mass ratio of the polymer nanogel microspheres to heparin is 4-6:1.
[0023] The present invention also provides a method for preparing the heparin-loaded nanogel microsphere drug, comprising the following steps:
[0024] The polymer nanogel microspheres are dispersed in tetrahydrofuran to obtain a nanogel microsphere dispersion liquid, the heparin is dissolved in water, and the solution is dropwise added into the nanogel microsphere dispersion liquid. The solution is stirred in an open air to completely volatilize the tetrahydrofuran, centrifuged, and freeze-dried to obtain the heparin-loaded nanogel microsphere drug.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention uses a free radical dispersion polymerization method, using dimethylaminoethyl methacrylate, a vinyl cyclic acetal monomer, and a crosslinking monomer as reaction materials. The copolymerization is carried out in a nonpolar solvent under the combined action of a dispersant and a free radical initiator. The resulting polymer nanogel microspheres contain degradable ester groups in the backbone, overcoming the problem of the nondegradability of current stimulus-responsive nanogel microspheres obtained through free radical polymerization. The resulting polymer nanogel microspheres exhibit dual temperature and pH responsiveness, making them suitable for drug loading and responsive release. Furthermore, they are degradable under alkaline conditions, demonstrating promising application prospects in the biomedical field. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] FIG1 is a Fourier transform infrared absorption spectrum of the nanogel microspheres prepared in Example 1.
[0028] FIG2 is a scanning electron micrograph of the nanogel microspheres prepared in Example 1.
[0029] FIG3 is a dynamic light scattering graph showing the particle size of the water-dispersible nanospheres of Example 1 at different pH values and temperatures.
[0030] FIG4 is a scanning electron micrograph of the nanogel microspheres prepared in Example 1 after hydrolysis under alkaline conditions.
[0031] FIG5 is a drug release curve of heparin-loaded nanogel microspheres prepared in Example 2 at 37° C. and different pH values.
[0032] FIG6 is a scanning electron micrograph of the nanogel microspheres prepared in Example 3.
[0033] FIG7 is a scanning electron micrograph of the nanogel microspheres prepared in Example 4.
[0034] FIG8 is a scanning electron micrograph of the nanogel microspheres prepared in Example 5. DETAILED DESCRIPTION
[0035] The technical solutions of the present invention are further illustrated by specific examples below. Those skilled in the art should understand that the examples are only for helping to understand the present invention and should not be regarded as specific limitations of the present invention.
[0036] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0037] The terms "comprise," "comprising," and "having," and any variations thereof, are intended to cover non-exclusive inclusions. For example, a process, method, apparatus, product, or device comprising a series of steps is not limited to the listed steps or modules but may optionally include steps not listed, or other steps inherent to the process, method, product, or device.
[0038] In this application, "plurality" refers to two or more. "And / or" describes the relationship between related objects, indicating that three possible relationships exist. For example, "A and / or B" can mean: A exists alone, A and B exist simultaneously, or B exists alone. The character " / " generally indicates that the related objects are in an "or" relationship.
[0039] In one embodiment of the present invention, the present invention provides a polymer nanogel microsphere, wherein the repeating structural unit in the polymer nanogel microsphere has a structure represented by the following formula (I):
[0040] Wherein, R1 is one of the following structures:
[0041] R2 is n-butyl or n-hexyl.
[0042] In one embodiment of the present invention, the present invention provides a polymer nanogel microsphere, which is prepared by free radical polymerization of dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer, dispersant, free radical initiator and crosslinking monomer in a non-polar solvent;
[0043] The vinyl cyclic acetal monomer is 2-methylene-4-phenyl-1,3-dioxolane and / or 5,6-benzo-2-methylene-1,3-dioxepane.
[0044] The present invention prepares polymer nanogel microspheres having a main chain containing a degradable ester group by free radical dispersion copolymerization of a vinyl ring acetal monomer, dimethylaminoethyl methacrylate, and a crosslinking monomer in a non-polar solvent, thereby overcoming the problem that the stimulus-responsive nanogel microspheres currently obtained by free radical polymerization cannot be degraded. The polydimethylaminoethyl methacrylate chain segments in the polymer nanogel microspheres undergo phase transitions with changes in temperature and / or pH, resulting in a transition between hydrophilic and hydrophobic properties, which causes a volume change in the polymer nanogel microspheres. This allows the prepared polymer nanogel microspheres to have dual temperature and pH responsiveness and can be used for drug loading and responsive release. Furthermore, the copolymerization of dimethylaminoethyl methacrylate and the vinyl ring acetal monomer can insert a degradable ester group into the polymer main chain, giving the polymer good degradation properties. The polymer can be degraded under alkaline conditions, overcoming the problem that the stimulus-responsive polymer nanogel microspheres currently obtained by free radical polymerization cannot be degraded, thereby providing the polymer with foreseeable potential application prospects in the field of biomedicine.
[0045] The vinyl cyclic acetal monomers used in the present invention are 2-methylene-4-phenyl-1,3-dioxolane (MPDL) and / or 5,6-benzo-2-methylene-1,3-dioxepane (BMDO). Both vinyl cyclic acetal monomers contain benzene rings. The introduction of benzene ring side groups stabilizes the generated free radicals, resulting in high ring-opening efficiency and minimal side reactions, achieving 100% ring-opening efficiency under free radical polymerization conditions. Furthermore, the low glass transition temperature (Tg) of dimethylaminoethyl methacrylate hinders the preservation of the self-assembly morphology during polymerization. The benzene ring side groups in MPDL and BMDO can increase their Tg. Combined with the introduction of a crosslinking agent (crosslinking monomer), the stability of the resulting polymer nanogel microsphere particles can be enhanced.
[0046] In addition, since vinyl cyclic acetal monomers are sensitive to active protons and easily undergo side reactions with solvents, thereby affecting the efficiency of their copolymerization reaction with dimethylaminoethyl methacrylate and affecting the acquisition of polymer nanogel microspheres, the use of non-polar solvents for dispersion polymerization in the reaction system of the present invention can effectively avoid the above problems, achieve very excellent reaction results, and efficiently obtain stable and degradable polymer nanogel microspheres.
[0047] In some embodiments of the present invention, the cross-linking monomer is selected from one or both of 1,6-hexanediol dimethacrylate and 1,4-butanediol dimethacrylate.
[0048] In some embodiments of the present invention, the dispersant is stearic acid.
[0049] In some embodiments of the present invention, the non-polar solvent is n-heptane.
[0050] In some embodiments of the present invention, the initiator is selected from one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and diisopropyl peroxydicarbonate.
[0051] In some embodiments of the present invention, the molar ratio of dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer and cross-linking monomer is 3-7:1:0.1-0.5, more preferably 4-6:1:0.2-0.4, and more preferably 4.8-5.2:1:0.3-0.35. The amount of cross-linking agent used will affect the synthesis of the polymer. If the amount is too low, the stability of the obtained polymer nanogel microspheres cannot be maintained. If the amount is too high, cross-linking and gelation will occur during the polymerization process, and polymer nanogel microspheres cannot be obtained. The molar ratio of dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer and cross-linking monomer within the above preferred range is conducive to the acquisition of polymer nanogel microspheres and is conducive to improving the stability of the obtained polymer nanogel microspheres.
[0052] In some embodiments of the present invention, the mass ratio of the dimethylaminoethyl methacrylate to the dispersant is 1:0.02-0.1, more preferably 1:0.04-0.06, and even more preferably 1:0.05. The particle size of the temperature- and pH-responsive degradable polymer nanogel microspheres of the present invention can be adjusted by the amount of dispersant added. Within a certain range, the particle size decreases as the dispersant content increases.
[0053] In some embodiments of the present invention, the molar ratio of the vinyl cyclic acetal monomer to the free radical initiator is 1:0.05-0.1, more preferably 1:0.06-0.09, and further preferably 1:0.08.
[0054] In some embodiments of the present invention, the particle size of the polymer nanogel microspheres is 200 nm-600 nm.
[0055] In some embodiments of the present invention, the particle size of the polymer nanogel microspheres is 300 nm-500 nm.
[0056] In one embodiment of the present invention, the present invention provides a method for preparing the degradable polymer nanogel microspheres by free radical polymerization technology, comprising the following steps: adding the dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer, dispersant, free radical initiator and crosslinking monomer to a non-polar solvent, and reacting under an inert gas atmosphere to obtain.
[0057] In some embodiments, the reaction temperature is 80° C.-100° C., and the reaction time is 4 h-10 h. This preferred temperature is conducive to the ring-opening polymerization of the vinyl cyclic acetal monomer and improves the reaction conversion rate.
[0058] In some embodiments, the reaction temperature is 85° C.-95° C., and the reaction time is 6 h-9 h.
[0059] In one embodiment of the present invention, the present invention also provides the use of the polymer nanogel microspheres as a carrier material in the preparation of pH and / or temperature responsive release drugs.
[0060] In one embodiment of the present invention, the present invention provides a pH and / or temperature responsive release drug, which is prepared from a pharmaceutical active ingredient and an excipient acceptable in a drug, wherein the excipient includes the polymer nanogel microspheres.
[0061] In some embodiments, the pharmaceutically active ingredient is a hydrophilic drug.
[0062] In some embodiments, the pharmaceutically active ingredient is heparin.
[0063] In one embodiment of the present invention, the present invention provides a heparin-loaded nanogel microsphere drug, which is prepared from raw materials including the polymer nanogel microspheres and heparin.
[0064] In some embodiments, the mass ratio of the polymer nanogel microspheres to heparin is 4-6:1.
[0065] In one embodiment of the present invention, the present invention provides a method for preparing the heparin-loaded nanogel microsphere drug, comprising the following steps:
[0066] The polymer nanogel microspheres are dispersed in tetrahydrofuran to obtain a nanogel microsphere dispersion liquid, the heparin is dissolved in water, and the solution is dropwise added into the nanogel microsphere dispersion liquid. The solution is stirred in an open air to completely volatilize the tetrahydrofuran, centrifuged, and freeze-dried to obtain the heparin-loaded nanogel microsphere drug.
[0067] The following are specific examples. Unless otherwise specified, the raw materials used in the following examples can be obtained from conventional commercial sources. The processes used, unless otherwise specified, are conventional processes in the art. Unless otherwise specified, room temperature or normal temperature refers to 25±5°C.
[0068] Example 1 Synthesis and Characterization of Temperature and pH Responsive Degradable Nanogel Microspheres
[0069] 1. Synthesis of Temperature- and pH-responsive Degradable Nanogel Microspheres
[0070] 2 g (12.7 mmol) of dimethylaminoethyl methacrylate, 0.4 g (2.5 mmol) of a vinyl cyclic acetal monomer (2-methylene-4-phenyl-1,3-dioxolane, MPDL), 0.1 g of stearic acid (dispersant), 32.4 mg (0.2 mmol) of azobisisobutyronitrile, and 0.2 g (0.8 mmol) of 1,6-hexanediol dimethacrylate were added to 10 mL of n-heptane and reacted at 90°C under an inert atmosphere for 8 h. Centrifugation yielded 2.6 g of nanogel microspheres.
[0071] The reaction formula is as follows:
[0072] Among them, R1 is (* indicates the connection site), R2 is n-hexyl.
[0073] 2. Test Characterization
[0074] (1) The obtained nanogel microspheres were characterized by infrared spectroscopy, as shown in Figure 1. -1 The stretching vibration characteristic absorption peak of the C=O bond in the MPDL unit appears at 1720 cm -1 The characteristic absorption peak of stretching vibration of C=O bond in dimethylaminoethyl methacrylate unit appeared, indicating that MPDL and dimethylaminoethyl methacrylate achieved copolymerization.
[0075] (2) The obtained nanogel microspheres were characterized by scanning electron microscopy. As shown in FIG2 , the nanogel microspheres prepared in this example were spherical in shape with a particle size of ∼400 nm.
[0076] (3) The resulting nanogel microspheres were dispersed in water, and their particle size at different pH values and temperatures was measured using dynamic light scattering. As shown in Figure 3, within the test range, the particle size decreased with increasing temperature, indicating that the polydimethylaminoethyl methacrylate chain segments underwent a phase transition from hydrophilic to hydrophobic, resulting in a shrinkage of the microsphere volume. Furthermore, as the pH increased, the phase transition temperature decreased. This is because as the pH increased, the amino group deprotonated, resulting in a stronger hydrophobicity, which in turn led to a lower phase transition temperature.
[0077] (4) 10 mg of the obtained nanogel microspheres were dispersed in 1 mL of sodium hydroxide solution at a pH of 10 and stirred for 6 h. The obtained sample was observed using a scanning electron microscope. As shown in FIG4 , the results showed that the morphology of the gel microspheres had changed to irregular granules with a size of 60-100 nm, indicating that the nanogel microspheres had degraded.
[0078] Example 2 Preparation and drug release of heparin-loaded nanogel microspheres
[0079] 1. Preparation of heparin-loaded nanogel microspheres
[0080] 100 mg of the nanogel microspheres prepared in Example 1 were dispersed in 10 mL of tetrahydrofuran to obtain a nanogel microsphere dispersion. 20 mg of heparin was dissolved in 2 mL of water and added dropwise to the nanogel microsphere dispersion. The mixture was stirred open for 24 hours to allow the tetrahydrofuran to evaporate completely. The supernatant and nanogel microspheres were separated by centrifugation, and the gel microspheres were freeze-dried to obtain heparin-loaded nanogel microspheres. The heparin content in the supernatant was determined by ultraviolet absorption spectroscopy, and the heparin loading in the nanogel microspheres was calculated to be 13.2% (Method reference: Int. J. Nanomed., 2016, 11, 6149-6159).
[0081] 2. Heparin release rate of nanogel microspheres at different pH
[0082] Take 50 mg of the prepared heparin-loaded nanogel microspheres and disperse them in 1 mL of PBS buffer with a specific pH at 37°C with stirring; use a pipette to aspirate 10 uL of the supernatant and dilute it to 1 mL at different time periods, and determine the heparin content released from the solution using the UV-Vis spectral standard curve method to calculate the release rate.
[0083] The test results are shown in Figure 5. As the pH increases, the time required for heparin to reach 50% release rate is 21 hours (pH = 6), 12.5 hours (pH = 7), and 7.5 hours (pH = 8), respectively. That is, the higher the pH, the faster the release rate of heparin. This is because the higher the pH, the higher the degree of deprotonation of the amino group, the stronger the hydrophobicity, and the more conducive to the release of hydrophilic heparin. This shows that the degradable nanogel microspheres prepared by the present invention can be used as carriers for hydrophilic drugs such as heparin to prepare pH and / or temperature-responsive release drugs, and can achieve the effect of different drug release rates at different pH and / or temperatures.
[0084] Example 3 Synthesis and Characterization of Temperature and pH Responsive Degradable Nanogel Microspheres
[0085] 2 g (12.7 mmol) of dimethylaminoethyl methacrylate, 0.4 g (2.5 mmol) of a vinyl cyclic acetal monomer (5,6-benzo-2-methylene-1,3-dioxepane, BMDO), 0.1 g of stearic acid (dispersant), 32.4 mg (0.2 mmol) of azobisisobutyronitrile, and 0.2 g (0.8 mmol) of 1,6-hexanediol dimethacrylate were added to 10 mL of n-heptane and reacted at 90°C under an inert atmosphere for 8 h. Centrifugation yielded 2.6 g of nanogel microspheres.
[0086] The reaction formula is as follows:
[0087] Among them, R1 is (* indicates the connection site), R2 is n-hexyl.
[0088] The obtained nanogel microspheres were characterized by scanning electron microscopy. As shown in FIG6 , the nanogel microspheres prepared in this example were spherical in shape with a particle size of ˜400 nm.
[0089] Example 4 Synthesis and Characterization of Temperature and pH Responsive Degradable Nanogel Microspheres
[0090] 2 g (12.7 mmol) of dimethylaminoethyl methacrylate, 0.4 g (2.5 mmol) of a vinyl cyclic acetal monomer (2-methylene-4-phenyl-1,3-dioxolane, MPDL), 0.05 g of stearic acid (dispersant), 32.4 mg (0.2 mmol) of azobisisobutyronitrile, and 0.2 g (0.8 mmol) of 1,6-hexanediol dimethacrylate were added to 10 mL of n-heptane and reacted at 90°C under an inert atmosphere for 8 h. Centrifugation yielded 2.5 g of nanogel microspheres.
[0091] The obtained nanogel microspheres were characterized by scanning electron microscopy. As shown in FIG7 , the nanogel microspheres prepared in this example were spherical in shape with a particle size of ˜500 nm.
[0092] Example 5 Synthesis and Characterization of Temperature and pH Responsive Degradable Nanogel Microspheres
[0093] 2 g (12.7 mmol) of dimethylaminoethyl methacrylate, 0.4 g (2.5 mmol) of a vinyl cyclic acetal monomer (2-methylene-4-phenyl-1,3-dioxolane, MPDL), 0.2 g of stearic acid (dispersant), 32.4 mg (0.2 mmol) of azobisisobutyronitrile, and 0.2 g (0.8 mmol) of 1,6-hexanediol dimethacrylate were added to 10 mL of n-heptane and reacted at 90°C under an inert atmosphere for 8 h. Centrifugation yielded 2.4 g of nanogel microspheres.
[0094] The obtained nanogel microspheres were characterized by scanning electron microscopy. As shown in FIG8 , the nanogel microspheres prepared in this example were spherical in shape with a particle size of ∼300 nm.
[0095] Comparative Example 1 Synthesis of Temperature and pH Responsive Degradable Nanogel Microspheres
[0096] 2 g (12.7 mmol) of dimethylaminoethyl methacrylate, 0.4 g (2.5 mmol) of vinyl cyclic acetal monomer (2-methylene-4-phenyl-1,3-dioxolane, MPDL), 0.1 g of stearic acid as a dispersant, 32.4 mg (0.2 mmol) of azobisisobutyronitrile, and 0.64 g (2.5 mmol) of 1,6-hexanediol dimethacrylate were added to 10 mL of n-heptane and reacted at 90 ° C for 2 h under an inert gas atmosphere. The system gelled and could not continue.
[0097] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0098] The above-described embodiments merely represent several implementation methods of the present invention. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that a person skilled in the art would be able to make various modifications and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be determined by the appended claims.
Claims
1. A polymer nanogel microsphere, characterized in that: The repeating structural unit in the polymer nanogel microsphere has a structure shown in the following formula (I): Wherein, R1 is one of the following structures: R2 is n-butyl or n-hexyl.
2. A polymer nanogel microsphere, characterized in that: It is prepared by free radical polymerization of dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer, dispersant, free radical initiator and crosslinking monomer in a non-polar solvent; The vinyl cyclic acetal monomer is 2-methylene-4-phenyl-1,3-dioxolane and / or 5,6-benzo-2-methylene-1,3-dioxepane.
3. The polymer nanogel microspheres according to claim 2, characterized in that: The cross-linking monomer is selected from one or both of 1,6-hexanediol dimethacrylate and 1,4-butanediol dimethacrylate; and / or, The dispersant is stearic acid; and / or, The non-polar solvent is n-heptane; and / or, The initiator is selected from azobisisobutyronitrile, azobisisoheptanenitrile, diisopropyl peroxydicarbonate One or more of.
4. The polymer nanogel microspheres according to claim 2 or 3, characterized in that: The molar ratio of dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer and crosslinking monomer is 3-7:1:0.1-0.
5.
5. The polymer nanogel microsphere according to claim 4, characterized in that: The molar ratio of dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer and crosslinking monomer is 4-6:1:0.2-0.
4.
6. The polymer nanogel microspheres according to claim 2 or 3, characterized in that: The mass ratio of the dimethylaminoethyl methacrylate to the dispersant is 1:0.02-0.1; and / or, The molar ratio of the vinyl cyclic acetal monomer to the free radical initiator is 1:0.05-0.
1.
7. The polymer nanogel microspheres according to claim 6, characterized in that: The mass ratio of the dimethylaminoethyl methacrylate to the dispersant is 1:0.04-0.06; and / or, The molar ratio of the vinyl cyclic acetal monomer to the free radical initiator is 1:0.06-0.
09.
8. The polymer nanogel microsphere according to any one of claims 1 to 3, characterized in that: Its particle size is 200nm-600nm.
9. A method for preparing polymer nanogel microspheres according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: adding dimethylaminoethyl methacrylate, vinyl cyclic acetal monomer, dispersant, free radical initiator and crosslinking monomer into a non-polar solvent, and reacting them under an inert gas atmosphere to obtain the product.
10. The method for preparing polymer nanogel microspheres according to claim 9, characterized in that: The reaction temperature is 80°C-100°C, and the reaction time is 4h-10h.
11. Use of the polymer nanogel microspheres according to any one of claims 1 to 8 as carrier materials in the preparation of pH and / or temperature responsive release drugs.
12. A pH and / or temperature responsive release drug, characterized in that: The microspheres are prepared from active pharmaceutical ingredients and adjuvants acceptable in pharmaceuticals, wherein the adjuvants include the polymer nanogel microspheres.
13. The pH and / or temperature responsive release drug according to claim 12, characterized in that: The active ingredient of the medicine is a hydrophilic drug.
14. The pH and / or temperature responsive release drug according to claim 13, characterized in that: The active ingredient of the medicine is heparin.
15. A heparin-loaded nanogel microsphere drug, characterized in that: The nanogel microspheres are prepared from raw and auxiliary materials including the polymer nanogel microspheres according to any one of claims 1 to 8 and heparin.
16. The heparin-loaded nanogel microsphere drug according to claim 15, characterized in that: The mass ratio of the polymer nanogel microspheres to heparin is 4-6:
1.
17. A method for preparing the heparin-loaded nanogel microsphere drug according to claim 15 or 16, characterized in that: The steps include: The polymer nanogel microspheres are dispersed in tetrahydrofuran to obtain a nanogel microsphere dispersion, the heparin is dissolved in water, and then added dropwise to the nanogel microsphere dispersion, stirred in an open air to completely volatilize the tetrahydrofuran, centrifuged, and freeze-dried to obtain the heparin-loaded nanogel microsphere drug.
Citation Information
Patent Citations
Microgel with nanometer grade sensitivity of temperature and PH value and preparation method thereof
CN101037494A
Polyacrylic acid nano-gel microspheres, preparation method and application thereof
CN101836970A
Temperature-pH dual-sensitivity gel microsphere as well as preparation method and application thereof
CN102311945A
High-efficiency and antibacterial polymeric micelle with high pH sensibility and biocompatibility and preparation method thereof
CN102702451A
Preparation method of degradable environmental sensitive polymer nano hydrogel and application
CN103304733A