Micro optoelectronic chip and manufacturing method therefor and application thereof

By forming an ion implantation area and isolation trench in the semiconductor structure layer of the Micro-LED chip, and setting up a light-blocking structure in the isolation trench, the sidewall damage and optical crosstalk problems caused by dry etching are solved, and the optoelectronic performance of the chip is improved. Performance and display.

WO2024221574A1PCT designated stage expired Publication Date: 2024-10-31SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI

Patent Information

Application Number
PCT/CN2023/101115
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-06-19
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing Micro-LED chips have sidewall damage and optical crosstalk problems in the dry etching process, resulting in low quantum efficiency, small usable area, and poor display effects. The ion implantation isolation method cannot effectively reduce optical crosstalk, affecting color uniformity. performance and resolution.

Method used

By forming an ion implantation area and an isolation trench in the semiconductor structural layer, and setting a light-blocking structure in the isolation trench, electrical isolation and optical isolation are achieved, preventing light transmission between adjacent optoelectronic chips and eliminating optical crosstalk.

Benefits of technology

The photoelectric conversion efficiency and display effect of the micro optoelectronic chip array are improved, the quantum efficiency and effective use area of ​​the chip are enhanced, and the contrast and brightness are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023101115_31102024_PF_FP_ABST
    Figure CN2023101115_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses a micro optoelectronic chip and a manufacturing method therefor and an application thereof. The micro optoelectronic chip comprises: a semiconductor structure layer which comprises a first doped semiconductor layer, an active layer and a second doped semiconductor layer which are sequentially stacked on a substrate; ion implantation regions distributed in the semiconductor structure layer and used for electrically isolating, in the semiconductor structure layer, a plurality of optoelectronic chip structures arranged in an array; isolation grooves formed in the corresponding ion implantation regions and at least used for isolating second doped semiconductor layers of any two adjacent optoelectronic chip structures from each other; and light blocking structures arranged in the isolation grooves and at least used for preventing light from being transmitted between any two adjacent optoelectronic chip structures by means of the second doped semiconductor layers. The present application can effectively eliminate the problem of optical crosstalk of a micro optoelectronic chip array, so that excellent photoelectric conversion efficiency and display effect are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Micro optoelectronic chip and its manufacturing method and application

[0001] This application is based on and claims priority from the Chinese patent application number 2023104628269 filed on April 26, 2023, entitled “Micro-optoelectronic chip, its manufacturing method and application”. Technical Field

[0002] The present application relates to a semiconductor optoelectronic device, specifically to a micro optoelectronic chip and a manufacturing method and application thereof, belonging to the technical field of semiconductor device preparation. Background Art

[0003] Micro-LED is an ideal new micro-display technology. Through chip flip-chip or wafer-level bonding technology, the Micro-LED array can be combined with an active silicon-based display driver chip to form a self-luminous Micro-LED micro-display chip with high luminous efficiency and better color performance. Compared with LCD, the self-luminous Micro-LED micro-display chip does not require a backlight, so it does not need to be equipped with various focusing and projection optical components, which can greatly reduce the size of the optical machine. At the same time, each Micro-LED pixel switches independently, and the light efficiency and dynamic contrast can be significantly improved. Compared with OLED made of organic materials, the inorganic gallium nitride (GaN) Micro-LED has a wider operating temperature range and can withstand higher current density. The display brightness of the microchip can reach up to one million nits, which is tens to hundreds of times the brightness of OLED. It is suitable for some special application scenarios or defense and military applications.

[0004] Currently, the mainstream technology for Micro-LEDs is to first use semiconductor micro-nanofabrication technologies such as dry etching (such as RIE, ECR, and ICP) to process conventional LEDs into Micro-LED chips of tens of microns or even smaller sizes, and then combine them with massively parallel transfer technology or monolithic integration technology to achieve RGB full-color image display. However, the dry etching process will leave sidewalls at the edges of the Micro-LED chip. At the same time, high-energy etching particles will bombard the material lattice and form defective dangling bonds on the material surface. Etching particles will also be injected into the material, causing sidewall damage. The damage effect can extend several microns deep into the chip. The presence of these damages means that there are a large number of defect energy levels at the edge of the Micro-LED chip. Dangling bonds mean increased carrier leakage paths, which is unacceptable for Micro-LED micro-display devices that want to have better optical and electrical properties. Specifically, these defects and damage significantly reduce the quantum efficiency and usable area of ​​Micro-LED devices. For example, the sidewall damage effect results in the usable area of ​​a 5μm×5μm Micro-LED chip being only approximately 4% of its total size. At the same time, sidewall damage defects form deep energy levels within the material that act as non-radiative recombination centers, greatly increasing the device's non-radiative recombination rate, resulting in a peak luminous efficiency of Micro-LEDs typically below 10%. Furthermore, there is severe optical crosstalk between the etched Micro-LED chips, which seriously affects the micro-display effect during use of Micro-LED displays. For example, the emission of one Micro-LED pixel may cause the emission of an adjacent Micro-LED. When the display process requires that the surrounding area of ​​the illuminated pixel be black to improve contrast, the contrast of the micro-display will be greatly reduced due to the presence of optical crosstalk. Furthermore, due to the dispersion of light transmission caused by optical crosstalk, the brightness of local Micro-LEDs will also be significantly reduced.

[0005] In recent years, researchers have discovered that ion implantation isolation can minimize the LED light-emitting area while effectively avoiding the degradation of Micro-LED device array performance due to sidewall damage caused by the etching process, reducing the impact of trench structures on the cost and potential yield of Micro-LED device array fabrication, and potentially enabling the fabricated Micro-LED device array to achieve advantages such as planarity. However, ion implantation isolation also has significant drawbacks in the fabrication of Micro-LED device arrays. For example, Micro-LED device arrays fabricated using ion implantation isolation cannot achieve true optical isolation, which is not conducive to reducing optical crosstalk between Micro-LED devices and will affect the display quality of the final Micro-LED micro-display device. In particular, as Micro-LED chip size and adjacent spacing continue to decrease, the size of the ion implantation area must also be reduced accordingly. The lateral beam expansion will lead to more severe optical crosstalk between adjacent Micro-LED chips, further reducing the color uniformity and resolution of the Micro-LED chip.

[0006] Application Contents

[0007] The main purpose of this application is to provide a micro optoelectronic chip and its manufacturing method and application to overcome the shortcomings of the existing technology.

[0008] To achieve the aforementioned application objectives, the technical solutions adopted in this application include:

[0009] One aspect of the present application provides a micro optoelectronic chip, comprising:

[0010] substrate;

[0011] A semiconductor structure layer is provided on the substrate, wherein the semiconductor structure layer comprises a first doped semiconductor layer, an active layer, and a second doped semiconductor layer sequentially stacked on the substrate;

[0012] Ion implantation regions and isolation trenches distributed within the semiconductor structure layer, wherein the ion implantation regions are used to electrically isolate a plurality of optoelectronic chip structures arranged in an array within the semiconductor structure layer;

[0013] An isolation trench is provided in the ion implantation region, wherein the isolation trench is at least used to isolate the second doped semiconductor layers of any two adjacent optoelectronic chip structures from each other;

[0014] A light-blocking structure is provided in the isolation trench, and the light-blocking structure is at least used to prevent light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer.

[0015] Another aspect of the present application provides a method for manufacturing a micro optoelectronic chip, which comprises:

[0016] forming a semiconductor structure layer on a substrate, wherein the semiconductor structure layer comprises a first doped semiconductor layer, an active layer, and a second doped semiconductor layer sequentially stacked on the substrate;

[0017] Performing ion implantation on the semiconductor structure layer to form an ion implantation region in the semiconductor structure layer, thereby electrically isolating a plurality of optoelectronic chip structures arranged in an array in the semiconductor structure layer;

[0018] Etching the ion implantation region to form an isolation trench in the ion implantation region, thereby isolating at least the second doped semiconductor layers of any two adjacent optoelectronic chip structures from each other;

[0019] A light blocking structure is provided in the isolation trench, thereby at least preventing light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer.

[0020] Another aspect of the present application provides use of the micro optoelectronic chip in preparing optoelectronic devices, including but not limited to display devices, micro display devices, etc.

[0021] Compared with the existing technology, the technical solution of this application realizes the preparation of micro-optoelectronic chip arrays through ion implantation, while eliminating the problem of optical crosstalk between chips in the array, so that the micro-optoelectronic chip array has both excellent photoelectric conversion efficiency and display effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings in the specification, which constitute a part of this application, are used to provide further understanding of this application. The illustrative embodiments of this application and their descriptions are used to explain this application and do not constitute improper limitations on this application.

[0023] FIG1 is a schematic diagram of a Micro-LED chip in Example 1;

[0024] FIG2 is a schematic structural diagram of an epitaxial wafer of a Micro-LED chip in Example 1;

[0025] FIG3 is a schematic structural diagram of a device formed after ion implantation of the epitaxial wafer shown in FIG2 ;

[0026] FIG4 is a schematic structural diagram of a device formed by etching and groove forming in the ion implantation region of the device shown in FIG3 ;

[0027] FIG5 is a schematic structural diagram of a device formed by filling a light-blocking structure in an isolation groove of the device shown in FIG4 ;

[0028] FIG6 is a schematic diagram of a Micro-LED chip in Example 3;

[0029] FIG7 is a partial enlarged schematic diagram of area A in FIG6 ;

[0030] FIG8 is a test diagram of the reflectivity of a dielectric layer for light of different wavelengths in Example 3;

[0031] FIG9 is a test diagram of the reflectivity of a dielectric layer for light of different wavelengths in Example 4;

[0032] FIG10 is a test diagram of the reflectivity of a dielectric layer for light of different wavelengths in Example 5. DETAILED DESCRIPTION

[0033] In view of the problems such as sidewall damage caused by traditional etching processes in forming micro-photonic chip arrays, and the defects such as optical crosstalk caused by ion implantation isolation in forming micro-photonic chip arrays, the applicant has proposed the technical solution of this application after long-term research and practice. This solution reduces the impact of optical crosstalk that may affect the final display effect, while maintaining the advantage of ion implantation isolation in improving electro-optical conversion efficiency, thereby improving the optoelectronic performance of the micro-photonic chip array and optimizing its display effect. The technical solution of this application will be further described in detail below.

[0034] Some embodiments of the present application provide a micro optoelectronic chip comprising:

[0035] substrate;

[0036] A semiconductor structure layer is provided on the substrate, wherein the semiconductor structure layer comprises a first doped semiconductor layer, an active layer, and a second doped semiconductor layer sequentially stacked on the substrate;

[0037] Ion implantation regions and isolation trenches distributed within the semiconductor structure layer, wherein the ion implantation regions are used to electrically isolate a plurality of optoelectronic chip structures arranged in an array within the semiconductor structure layer;

[0038] An isolation trench is provided in the ion implantation region, wherein the isolation trench is at least used to isolate the second doped semiconductor layers of any two adjacent optoelectronic chip structures from each other;

[0039] A light-blocking structure is provided in the isolation trench, and the light-blocking structure is at least used to prevent light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer.

[0040] In this application, a micro-optoelectronic chip array is realized by adopting an ion implantation isolation method, and by opening an isolation groove in the ion implantation area and setting a light-blocking structure in the isolation groove, the chip can be miniaturized better, the chip sidewall damage and dangling bonds caused by the etching process can be avoided, the quantum efficiency and effective use area of ​​the chip can be guaranteed and improved, and it can have better optical and electrical properties. At the same time, it can also effectively prevent light from being transmitted between adjacent chips in the micro-optoelectronic chip array, eliminate optical crosstalk, and thus improve the display effects such as contrast and brightness of the micro-optoelectronic chip array.

[0041] In one embodiment, the ion implantation region extends continuously from at least the top surface of the second doped semiconductor layer to the top surface of the active layer. The isolation trench is entirely located within the ion implantation region. The bottom surface of the isolation trench is higher than the bottom surface of the ion implantation region and is flush with or lower than the bottom surface of the second doped semiconductor layer. The top surface of the second doped semiconductor layer is the surface of the second doped semiconductor layer facing away from the substrate. By placing the isolation trench entirely within the ion implantation region, the risk of damage to the semiconductor material due to overetching during the fabrication of the isolation trench can be further reduced. Furthermore, the ion implantation region can be used to electrically isolate the conductive filler material within the isolation trench from the semiconductor material in structural layers such as the second doped semiconductor layer and the active layer, thereby ensuring the normal operation and performance of the device.

[0042] The implanted ions used to form the ion implantation region include H ions, F ions, N ions, O ions, etc., but are not limited thereto.

[0043] The ion implantation region may be one or more. Exemplarily, the ion implantation region may be arranged in a grid pattern on the surface of the semiconductor structure layer, with the area surrounded by each grid being a non-ion implantation region for fabricating an optoelectronic chip structure. Accordingly, the isolation trench may be one or more, and exemplarily, may also be arranged in a grid pattern on the surface of the semiconductor structure layer.

[0044] In the present application, the ion implantation area is arranged around the corresponding non-ion implantation area, and an optoelectronic chip structure is formed in the corresponding non-ion implantation area. The sizes of the ion implantation area and the optoelectronic chip structure can be determined according to actual needs. Exemplarily, the size of the ion implantation area and the optoelectronic chip structure is 1μm to 50μm. Among them, the size of the ion implantation area and the optoelectronic chip structure mainly refers to its size in the direction parallel to the layer plane of the semiconductor structure layer, which can also be considered as its length and width or its diameter.

[0045] Furthermore, the bottom end surface of the ion implantation region can be located within the first doped semiconductor layer; the opening of the isolation trench can be located on the top surface of the second doped semiconductor layer, with the bottom of the trench located within the first doped semiconductor layer; and the light-blocking structure is at least configured to prevent light from transmitting between any two adjacent optoelectronic chip structures through the second doped semiconductor layer and the active layer. This design can better block light transmission within the micro-optoelectronic chip array, more thoroughly overcoming the problem of optical crosstalk.

[0046] In the present application, the inner wall of the isolation trench is at a certain distance from the outer wall of the corresponding ion implantation region, that is, the ion implantation region has a certain wall thickness, which can be 100 nm to 20 μm, for example.

[0047] In one embodiment, the micro optoelectronic chip further includes at least one dielectric layer, the dielectric layer continuously covering at least the sidewalls of the isolation trench and being located between the sidewalls of the isolation trench and the light-blocking structure; and the light-blocking structure includes a metal light-isolating layer continuously covering at least the dielectric layer. The provision of the dielectric layer can, on the one hand, protect the sidewalls of the isolation trench, and, on the other hand, further electrically isolate the conductive filling material in the isolation trench from the semiconductor materials in structural layers such as the second doped semiconductor layer and the active layer. Furthermore, the dielectric layer can be used to prevent ions from ion-implanted regions from escaping when the metal light-isolating layer is produced using processes such as evaporation, thereby better ensuring the performance of the device.

[0048] The material of the dielectric layer includes, but is not limited to, silicon oxide, silicon nitride, aluminum nitride, aluminum oxide, gallium oxide, titanium oxide, or hafnium oxide.

[0049] The metal light isolation layer may be made of, but not limited to, gold, titanium, aluminum, nickel, chromium, molybdenum, or copper. Preferably, the metal light isolation layer is formed of a metal or alloy such as aluminum that has both excellent reflective and conductive properties. The metal light isolation layer may be a single layer or a multilayer structure.

[0050] Preferably, the micro-optoelectronic chip includes multiple dielectric layers with different refractive indices, which are sequentially stacked at least on the sidewalls of the isolation trench and combined with the ion implantation region to form a distributed Bragg reflector (DBR) structure. The definition of the distributed Bragg reflector structure is well known in the art and is primarily an optical thin film composed of a low-refractive index material and a high-refractive index material stacked in different combinations. For example, the low-refractive index material can be selected from, but not limited to, SiO2, and the high-refractive index material can be selected from, but not limited to, TiO2, Ta2O5, ZrO2, and the like. The greater the difference in refractive index between the materials, the smaller the thickness required to achieve the desired reflectivity.

[0051] Specifically, after ion implantation forms an ion implantation zone in a selected area of ​​the semiconductor structure layer, the refractive index of the semiconductor material therein will also change, thereby forming a light refraction interface with the semiconductor material in the chip. Then, by alternately stacking multiple dielectric layers with different refractive indices on the sidewalls of the isolation groove, a DBR structure can be formed. It can not only achieve sidewall passivation to better ensure the electrical performance stability and long-term reliability of the optoelectronic chip, but also cooperate with the light-blocking structure to optically isolate and totally reflect the light emitted from the sidewall of the optoelectronic chip, so that more light energy inside the optoelectronic chip can be emitted from the front, thereby better eliminating the problem of optical crosstalk and further improving the photoelectric conversion efficiency of the chip.

[0052] Preferably, the dielectric layer is formed of a heat-conducting dielectric material. For example, the thermal expansion coefficient of the heat-conducting dielectric material is between the thermal expansion coefficient of the material constituting the metal optical isolation layer and the thermal expansion coefficient of the material constituting the ion isolation region, and / or the heat-conducting dielectric material has good bonding properties with both the material constituting the metal optical isolation layer and the material constituting the ion isolation region. This not only facilitates faster transfer of heat generated by chip operation, but also allows the metal optical isolation layer to be more firmly bonded to the chip, preventing the metal optical isolation layer from detaching from the chip structure due to the heat generated after long-term operation of the chip. The heat-conducting dielectric material can be selected from, but is not limited to, silicon nitride, aluminum nitride, and the like.

[0053] More preferably, the dielectric layer used to form the distributed Bragg reflector structure is formed of the thermal conductive dielectric material to have both light reflection and heat conduction functions.

[0054] In the present application, the thickness of the dielectric layer may be 5 nm to 500 nm.

[0055] In one embodiment, the micro-optoelectronic chip further includes a thermally conductive passivation layer, which covers the surface of the semiconductor structure layer and is thermally connected to the metal optical isolation layer. This thermally conductive passivation layer not only protects the surface of the micro-optoelectronic chip array but also forms a thermally conductive path with the metal optical isolation layer, further helping to reduce the temperature of the micro-optoelectronic chip array and ensure its operating performance and stability.

[0056] The material of the thermally conductive passivation layer includes, but is not limited to, aluminum nitride, boron nitride, or diamond.

[0057] In some cases, a local area of ​​the thermally conductive passivation layer fills the isolation groove and directly contacts the metal optical isolation layer. In some cases, the thermally conductive passivation layer may also have windows for forming electrodes that cooperate with the optoelectronic chip structures.

[0058] In one embodiment, the metal light isolation layer further extends to cover the surface of the semiconductor structure layer and forms a current spreading layer.

[0059] In the present application, the material of the semiconductor structure layer includes a III-V compound, preferably a III-V nitride, such as Al x In y Ga 1-x-y N, 1 ≥ x ≥ 0, 1 ≥ y ≥ 0, 1 ≥ (1 - xy) ≥ 0. The first doped semiconductor layer and the second doped semiconductor layer have different conductivity types. For example, the first doped semiconductor layer and the second doped semiconductor layer can be an N-type semiconductor layer and a P-type semiconductor layer, respectively, or vice versa. The active layer can be a multi-quantum well layer. In addition, the semiconductor structure layer can also include other structural layers commonly known in the art, such as a buffer layer. The materials, thicknesses, etc. of these structural layers can be selected or set in accordance with methods known in the art and will not be described in detail here.

[0060] In the present application, the substrate may include sapphire, Si, SiC, GaN substrate, etc., but is not limited thereto.

[0061] In the present application, the optoelectronic chip structure may include a Micro-LED chip structure, or may also be an LD (laser), a Mini-LED chip structure or other light-emitting semiconductor structure, but is not limited thereto.

[0062] Some embodiments of the present application provide a method for manufacturing the micro optoelectronic chip, including:

[0063] A semiconductor structure layer is formed on a substrate, wherein the semiconductor structure layer includes a first doped semiconductor layer, an active layer, and a second doped semiconductor layer sequentially stacked on the substrate; illustratively, the first doped semiconductor layer, the active layer, and the second doped semiconductor layer can be sequentially grown on the substrate using processes such as metal organic chemical vapor epitaxy (MOCVD) or molecular beam epitaxy (MBE).

[0064] The semiconductor structure layer is subjected to ion implantation treatment to form an ion implantation region in the semiconductor structure layer, thereby electrically isolating a plurality of optoelectronic chip structures arranged in an array in the semiconductor structure layer, wherein the implanted ions include but are not limited to H ions, F ions, N ions or O ions. Generally speaking, the ion implantation region is arranged around the non-ion implantation region, and the optoelectronic chip structure is made in the non-ion implantation region. The sizes of the ion implantation region and the non-ion implantation region can be set to 1μm to 50μm. In order to increase the effective utilization area of ​​the semiconductor structure layer, the size of the non-ion implantation region should be as large as possible, and the size of the ion implantation region should be as small as possible within a reasonable range. The reasonable range should meet the following conditions, namely, it can achieve electrical isolation between adjacent chip structures and is conducive to the opening of isolation grooves.

[0065] The ion implantation region is etched to form an isolation groove in the ion implantation region, thereby isolating at least the second doped semiconductor layers of any two adjacent optoelectronic chip structures from each other.

[0066] A light blocking structure is provided in the isolation trench, thereby at least preventing light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer.

[0067] In one embodiment, the manufacturing method specifically includes:

[0068] Performing ion implantation on the semiconductor structure layer at least from the top surface of the second doped semiconductor layer, and the ion implantation depth at least reaches the top surface of the active layer, thereby forming the ion implantation region;

[0069] Etching the ion implantation region to a depth less than the ion implantation depth but at least reaching the bottom surface of the second doped semiconductor layer, thereby forming the isolation trench;

[0070] The top surface of the second doped semiconductor layer is a surface of the second doped semiconductor layer away from the substrate.

[0071] In one embodiment, the manufacturing method more specifically includes:

[0072] Performing ion implantation on the semiconductor structure layer at least from the top surface of the second doped semiconductor layer, and the ion implantation depth reaches the interior of the first doped semiconductor layer, thereby forming the ion implantation region;

[0073] Etching the ion implantation region to a depth less than the ion implantation depth and reaching the interior of the first doped semiconductor layer, thereby forming the isolation trench;

[0074] Furthermore, a light blocking structure is provided in the isolation groove to prevent light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer and the active layer.

[0075] In the above embodiments of the present application, a patterned ion implantation mask can be pre-set on the surface of the semiconductor structure layer, and the ion implantation can be performed using the mask. The ion implantation mask can be pre-fabricated and then transferred to the surface of the semiconductor structure layer, or it can be formed on the surface of the semiconductor structure layer by coating a photoresist layer on the surface of the semiconductor structure layer and then using a photolithography process. The pattern and size of the ion implantation mask correspond to the shape and size of the ion implantation area, which can be determined according to actual needs. For example, the ion implantation area can be circular, square, or other regular or irregular shapes.

[0076] In the above embodiments of the present application, the ion implantation area can be etched using etching methods such as RIE, ECR, and ICP to form the isolation groove. Furthermore, by setting an etching mask on the ion implantation area and performing the etching operation using the etching mask, the position, size, and shape of the isolation groove can be more accurately controlled to avoid damage to the side wall of the chip structure. Preferably, the distance between the edge of the opening on the etching mask and the edge of the ion implantation area can be controlled to be 100nm to 20μm, so that the distance between the inner wall of the etched isolation groove and the outer wall of the corresponding ion implantation area is 100nm to 20μm. In actual production, the spacing of the high-resistance ion implantation area can be precisely adjusted by changing the size of the aforementioned ion implantation mask and etching mask, thereby flexibly defining the characteristic size of the chip and realizing the preparation of devices with sizes ranging from several microns to hundreds of microns.

[0077] In one embodiment, the manufacturing method further comprises:

[0078] Making at least one dielectric layer, and making the dielectric layer continuously cover at least the sidewalls of the isolation trench;

[0079] A metal light isolation layer is manufactured, and the metal light isolation layer is made to at least continuously cover the dielectric layer to form the light blocking structure.

[0080] In the above embodiments of the present application, the dielectric layer may be grown by a process such as atomic layer deposition (ALD), and its thickness may be set to be 5 nm to 500 nm.

[0081] More preferably, the manufacturing method specifically includes: forming a plurality of alternately stacked dielectric layers with different refractive indices at least on the sidewalls of the isolation trench, and combining the plurality of dielectric layers with the ion implantation region to form a distributed Bragg reflector structure.

[0082] More preferably, the dielectric layer can be formed at least on the sidewalls of the isolation groove using a heat-conducting dielectric material, the thermal expansion coefficient of the heat-conducting dielectric material being between the thermal expansion coefficient of the material constituting the metal optical isolation layer and the thermal expansion coefficient of the material constituting the ion isolation region.

[0083] In one embodiment, a thermally conductive passivation layer is formed on the surface of the semiconductor structure layer, and the thermally conductive passivation layer is thermally connected to the metal optical isolation layer. The thermally conductive passivation layer can also be grown by a process such as atomic layer deposition (ALD). Preferably, the thermally conductive passivation layer can cover the entire surface of the semiconductor structure layer. Of course, if electrodes are to be formed, corresponding windows can also be opened in the thermally conductive passivation layer.

[0084] In one embodiment, the metal light isolation layer may be extended to cover the surface of the semiconductor structure layer to form a current spreading layer, which is also beneficial to improving the light emission uniformity of the micro optoelectronic chip array.

[0085] The materials of the semiconductor structure layer, dielectric layer, metal optical isolation layer, thermal conductive dielectric material and thermal conductive passivation layer are as described above and will not be described in detail here.

[0086] The manufacturing method provided in this application is simple and reliable, compatible with existing process technologies, and can take into account increasing the effective use area of ​​the chip, reducing the side wall damage effect of the material, eliminating the device optical crosstalk problem, and improving the device luminous efficiency.

[0087] Some embodiments of the present application also provide an optoelectronic device, which includes the micro optoelectronic chip.

[0088] Some embodiments of the present application further provide a method for manufacturing a photoelectric device, which includes:

[0089] manufacturing the micro optoelectronic chip;

[0090] Furthermore, electrodes are fabricated and electrically contacted with the first doped semiconductor layer and the second doped semiconductor layer in the optoelectronic chip structure, for example, to form ohmic contacts. The electrodes include P-type electrodes and N-type electrodes.

[0091] Exemplarily, the optoelectronic device may be a Micro-LED device. Using the fabrication method, it is possible to more conveniently, quickly, and cost-effectively fabricate Micro-LED chips with smaller size and improved optical and electrical properties, effectively improving their resolution and brightness, and achieving better display effects.

[0092] Furthermore, some embodiments of the present application also provide a Micro-LED device, such as a Micro-LED display device, which includes the micro optoelectronic chip.

[0093] The following describes the embodiments of the present application through specific examples. Those skilled in the art will readily understand the other advantages and benefits of the present application from the disclosure herein. The present application may also be implemented or applied through various other specific embodiments, and the details in this specification may be modified or altered based on different viewpoints and applications without departing from the spirit of the present application.

[0094] For example, when describing the embodiments of this application, cross-sectional views of device structures may be partially enlarged to a different scale for ease of explanation. Furthermore, these schematic views are merely illustrative and should not limit the scope of protection of this application. Furthermore, in actual production, three-dimensional dimensions, including length, width, and depth, should be included.

[0095] For convenience, spatially relative terms such as "under," "below," "below," "below," "above," and "on" may be used herein to describe the relationship of one element or feature to other elements or features shown in the drawings. It will be understood that these spatially relative terms are intended to encompass orientations of the device in use or operation in addition to the orientation depicted in the drawings. Additionally, when a layer is referred to as being "between" two layers, it can be the only layer between the two layers, or one or more intervening layers may also be present.

[0096] In the context of the present application, a structure described as a first feature being "above" a second feature may include embodiments where the first and second features are in direct contact, and may also include embodiments where additional features are formed between the first and second features, such that the first and second features may not be in direct contact.

[0097] It should be noted that the illustrations provided in this embodiment only illustrate the basic concept of the present application in a schematic manner. Therefore, the illustrations only show components related to the present application and are not drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component can be changed at will, and the component layout type may also be more complicated.

[0098] Example 1

[0099] Referring to FIG. 1 , this embodiment provides a Micro-LED chip comprising a sapphire substrate 10 and a semiconductor structure layer 11. The semiconductor structure layer comprises an AlN buffer layer 111, an N-type GaN layer 112, a multi-quantum well active layer 113, and a P-type GaN layer 114, sequentially grown on the substrate. The semiconductor structure layer includes an ion-implanted region 115 and multiple non-ion-implanted regions distributed along the layer plane. Any two adjacent non-ion-implanted regions are electrically isolated by the ion-implanted region. A Micro-LED chip structure 116 is fabricated within each non-ion-implanted region, and each Micro-LED chip structure 116 can serve as a pixel, thereby forming a Micro-LED chip structure within the semiconductor structure layer. Furthermore, an isolation trench 117 is provided within the ion-implanted region to isolate the P-type GaN layer and the multi-quantum well active layer of two adjacent Micro-LED chip structures from each other. Furthermore, a light-blocking structure is provided within the isolation trench to prevent light from transmitting between two adjacent Micro-LED chip structures through the P-type GaN layer 114 and the multi-quantum well active layer 113. The light-blocking structure comprises one or more layers of opaque metal light-isolating layers 12, made of gold (Au), titanium (Ti), aluminum (Al), nickel (Ni), chromium (Cr), molybdenum (Mo), copper (Cu), or their alloys. The metal light-isolating layers cover the inner walls of the isolation trench and are primarily used to block and reflect light reflected by the multi-quantum well active layer, thereby interrupting the light transmission path between adjacent Micro-LED chip structures. One or more dielectric layers 13 are provided between the metal optical isolation layer and the inner wall of the isolation groove. The material of the dielectric layer includes but is not limited to silicon oxide (SiO2), silicon nitride (SiN), aluminum nitride (AlN), aluminum oxide (Al2O3), gallium oxide (Ga2O3), titanium oxide (TiO2) or hafnium oxide (HfO2), etc. Its thickness is 5nm to 500nm. It is mainly used to passivate the inner wall of the isolation groove and electrically isolate the metal optical isolation layer from the inner wall of the isolation groove. Preferably, the material of the dielectric layer can be selected from materials with high thermal conductivity such as aluminum nitride and silicon nitride. In some cases, the isolation groove can also be completely filled with the metal optical isolation layer and the dielectric layer. Preferably, the metal optical isolation layer can be continuously extended to cover the surface of the semiconductor structure layer, thereby forming a current expansion layer to improve the efficiency and uniformity of current injection. Furthermore, the surface of the semiconductor structure layer is also covered with a continuous thermally conductive passivation layer 14, which is in direct contact with the metal light isolation layer. Its material may include but is not limited to aluminum nitride (AlN), boron nitride (BN), diamond (Diamond) or a mixed material thereof. The thermally conductive passivation layer not only passivates the surface of the metal light isolation layer, but also serves as a Micro-LED thermal conductive layer.

[0100] Referring to Figures 2 to 5 , a method for manufacturing the Micro-LED chip includes the following steps:

[0101] S1. An AlN buffer layer 111, an N-type GaN layer 112, a multi-quantum well active layer 113 and a P-type GaN layer 114 are sequentially grown on a sapphire substrate by MOCVD, MBE, PECVD or the like to obtain the epitaxial wafer shown in FIG2.

[0102] S2. A patterned ion implantation mask is formed through processes such as photolithography. The materials of the ion implantation mask include, but are not limited to, photoresist, silicon oxide, silicon nitride, and metal. Using the ion implantation mask as a barrier layer, ion implantation is performed on the semiconductor structure layer of the epitaxial wafer to control the area and / or shape of the light-emitting region of the Micro-LED chip structure. The ion implantation depth must at least penetrate the P-type GaN layer and preferably reach the interior of the N-type GaN layer 112. The implanted ions include, but are not limited to, H ions, F ions, N ions, and O ions. The size of the resulting ion implantation region 115 is 1 μm to 50 μm, and the size of the non-ion implantation region 118 is 1 μm to 50 μm. From a top-down perspective, the ion implantation region 115 is preferably arranged around the non-ion implantation region 118, and each non-ion implantation region 118 is used to form a Micro-LED chip structure. The device structure obtained in this step is shown in Figure 3. This step uses ion implantation for electrical isolation, which has the advantages of less damage and higher control precision compared to the method of using an etching process for electrical isolation.

[0103] S3. An etching mask is set on the ion implantation area 115, and a through hole is opened on the etching mask. The size of the through hole is smaller than the size of the ion implantation area. Preferably, the distance between the edge of the through hole and the edge of the ion implantation area is 100nm to 20μm to minimize the damage to the side wall of the chip. Then, a dry etching process such as atomic layer etching (ALE), ion beam etching (IBE), and inductively coupled plasma etching (ICP) is used to etch the ion implantation area through the through hole of the etching mask. The etching depth is less than or equivalent to the ion implantation depth, but preferably less than the ion implantation depth, and especially preferably enters the interior of the N-type GaN layer 112, thereby forming an isolation groove 117. The device structure finally obtained in this step is shown in Figure 4. By performing dry etching in the ion implantation area, this step can not only effectively avoid the damage to the side wall caused by the etching process and improve the photoelectric conversion efficiency, but also the etched isolation area formed can be narrower, especially it can effectively isolate the light between Micro-LED pixels and eliminate the optical crosstalk effect.

[0104] S4. Form one or more dielectric layers 14 at least on the sidewalls of the isolation groove 117 by atomic layer deposition (ALD) and other processes, the thickness of which can be 5nm to 500nm. In some cases, the inner wall of the isolation groove 117 can also be completely covered by the dielectric layer. Further, one or more layers of opaque metal material are deposited on the dielectric layer to form a metal light isolation layer 12. The light-blocking structure formed mainly by the metal light isolation layer 12 can effectively reduce the light crosstalk between each pixel point. Among them, the isolation groove 117 can also be filled with the metal light isolation layer 12. The device structure finally obtained in this step is shown in Figure 5.

[0105] S5. Depositing a non-metallic thermally conductive material on the metal light-isolating layer 12 to form a thermally conductive passivation layer 14, which passivates the surface of the metal light-isolating layer 12 and also serves as a thermally conductive layer for the Micro-LED chip structure. Preferably, the thermally conductive passivation layer 14 can be continuously extended to cover the device surface, ultimately obtaining the Micro-LED chip shown in FIG1 .

[0106] Example 2

[0107] The Micro-LED chip provided in this embodiment is substantially the same as that in Example 1, differing in that the dielectric layer is formed of aluminum nitride, a material with high thermal conductivity, while the metal optical isolation layer is formed of aluminum. The dielectric layer not only serves to passivate the sidewalls of the isolation trench and electrically isolate the metal optical isolation layer from the inner walls of the isolation trench, but also serves as a transition layer between the ion-implanted region of the GaN-doped material and the metal optical isolation layer, allowing the metal optical isolation layer to be firmly bonded to the isolation trench. Together with the dielectric layer, it also forms a thermal conduction channel, facilitating the rapid transfer of heat generated by the Micro-LED chip during operation, ensuring operational stability and improving performance.

[0108] Example 3

[0109] The Micro-LED chip provided in this embodiment is substantially the same as that in Example 1, except that the Micro-LED chip structure is a blue LED chip with a central wavelength of approximately 450 nm. Referring to Figures 6 and 7 , the dielectric layer 13' comprises eight pairs of TiO2 / SiO2 composite layers, with a total thickness of approximately 895.2 nm. The TiO2 and SiO2 layers are alternately stacked to form a distributed Bragg reflector structure, with each TiO2 layer having a thickness of approximately 41.1 nm and each SiO2 layer having a thickness of approximately 70.8 nm. The reflectivity of the dielectric layer 13' for light of different wavelengths is shown in Figure 8 . The dielectric layer 13' can be used in conjunction with a metal optical isolation layer (e.g., an aluminum layer) to more thoroughly eliminate optical crosstalk. It can also serve as a transition layer between the GaN-doped ion-implanted region and the metal optical isolation layer, strengthening the bonding between the metal optical isolation layer and the isolation trench walls. Furthermore, the dielectric layer 13' can collaborate with the metal optical isolation layer to create a new heat conduction channel for the Micro-LED chip.

[0110] Example 4

[0111] The Micro-LED chip provided in this embodiment is basically the same as that in Example 3, except that the Micro-LED chip structure is a green LED chip structure with a central wavelength of approximately 550 nm, and the dielectric layer is a structure of 8 pairs of TiO2 / SiO2 composite layers. The total thickness of the dielectric layer is approximately 1112.0 nm, wherein the TiO2 layer and the SiO2 layer are alternately stacked to form a distributed Bragg reflector structure, and the thickness of each TiO2 layer is approximately 46.9 nm, and the thickness of each SiO2 layer is approximately 92.1 nm. The reflectivity of the dielectric layer for light of different wavelengths is shown in FIG9. The dielectric layer can also cooperate with the metal optical isolation layer to better eliminate the problem of optical crosstalk and enhance the heat dissipation performance of the device, thereby improving the photoelectric conversion efficiency and stability of the device.

[0112] Example 5

[0113] The Micro-LED chip provided in this embodiment is basically the same as that in Example 3, except that the Micro-LED chip structure is a red light LED chip structure with a central wavelength of approximately 660 nm, and the dielectric layer is a structure of 8 pairs of TiO2 / SiO2 composite layers. The total thickness of the dielectric layer is approximately 1350.4 nm, wherein the TiO2 layer and the SiO2 layer are alternately stacked to form a distributed Bragg reflector structure, and the thickness of each TiO2 layer is approximately 54.6 nm, and the thickness of each SiO2 layer is approximately 114.2 nm. The reflectivity of the dielectric layer for light of different wavelengths is shown in Figure 10. The dielectric layer can also cooperate with the metal optical isolation layer to better eliminate the problem of optical crosstalk and enhance the heat dissipation performance of the device, thereby improving the photoelectric conversion efficiency and stability of the device.

[0114] The above embodiments are merely illustrative of the principles and effects of this application and are not intended to limit this application. Anyone skilled in the art may modify or alter the above embodiments without departing from the spirit and scope of this application. Therefore, all equivalent modifications or alterations made by one of ordinary skill in the art without departing from the spirit and technical concepts disclosed in this application shall be covered by the claims of this application.

Claims

1. A micro optoelectronic chip, characterized in that: include: substrate; A semiconductor structure layer is provided on the substrate, wherein the semiconductor structure layer comprises a first doped semiconductor layer, an active layer and a second doped semiconductor layer sequentially stacked on the substrate; Ion implantation regions and isolation grooves distributed in the semiconductor structure layer, wherein the ion implantation regions are used to electrically isolate a plurality of optoelectronic chip structures arranged in an array in the semiconductor structure layer; An isolation groove is provided in the ion implantation region, wherein the isolation groove is used to at least isolate the second doped semiconductor layers of any two adjacent optoelectronic chip structures from each other; A light blocking structure is arranged in the isolation groove, and the light blocking structure is at least used to prevent light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer.

2. The micro optoelectronic chip according to claim 1, characterized in that: The ion implantation region at least continuously extends from the top end surface of the second doped semiconductor layer to the top end surface of the active layer, the isolation groove is entirely located in the ion implantation region, the bottom surface of the isolation groove is higher than the bottom end surface of the ion implantation region and is flush with or lower than the bottom end surface of the second doped semiconductor layer, and the top end surface of the second doped semiconductor layer is a side surface of the second doped semiconductor layer away from the substrate; Preferably, the bottom end surface of the ion implantation region is located inside the first doped semiconductor layer; the notch of the isolation groove is arranged on the top end surface of the second doped semiconductor layer, and the bottom of the groove is located inside the first doped semiconductor layer; and the light blocking structure is at least used to prevent light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer and the active layer.

3. The micro optoelectronic chip according to claim 2, characterized in that It also includes at least one dielectric layer, which continuously covers at least the sidewalls of the isolation groove and is located between the sidewalls of the isolation groove and the light-blocking structure; and the light-blocking structure includes a metal light-isolating layer that continuously covers at least the dielectric layer.

4. The micro optoelectronic chip according to claim 3, characterized in that: The micro optoelectronic chip comprises a plurality of dielectric layers with different refractive indices, wherein the plurality of dielectric layers are at least sequentially stacked on the sidewalls of the isolation groove and combined with the ion implantation region to form a distributed Bragg reflector structure; and / or, the dielectric layer is formed of a heat-conducting dielectric material, the thermal expansion coefficient of the heat-conducting dielectric material is between the thermal expansion coefficient of the material constituting the metal optical isolation layer and the thermal expansion coefficient of the material constituting the ion isolation region, and / or, The thermal conductive medium material has good bonding performance with the material constituting the metal light isolation layer and the material constituting the ion isolation region; And / or, the micro optoelectronic chip further comprises a thermally conductive passivation layer, the thermally conductive passivation layer covers the surface of the semiconductor structure layer and is thermally conductively connected to the metal optical isolation layer; And / or, the metal light isolation layer also extends to cover the surface of the semiconductor structure layer and forms a current spreading layer; Preferably, the material of the dielectric layer includes silicon oxide, silicon nitride, aluminum nitride, aluminum oxide, gallium oxide, titanium oxide or hafnium oxide; Preferably, the material of the metal light isolation layer includes gold, titanium, aluminum, nickel, chromium, molybdenum or copper; Preferably, the thermal conductive medium material includes aluminum nitride, boron nitride or diamond.

5. The micro optoelectronic chip according to any one of claims 1 to 4, characterized in that: The ion implantation region is arranged around the corresponding optoelectronic chip structure, and the sizes of the ion implantation region and the optoelectronic chip structure are 1μm to 50μm; and / or, the implanted ions used to form the ion implantation region include H ions, F ions, N ions or O ions; and / or, the distance between the inner wall of the isolation groove and the outer wall of the corresponding ion implantation region is 100nm to 20μm; and / or, the material of the semiconductor structure layer includes III-V group compounds, preferably III group nitrides; and / or, the optoelectronic chip structure includes a Micro-LED chip structure.

6. A method for manufacturing a micro optoelectronic chip, characterized in that include: Forming a semiconductor structure layer on a substrate, wherein the semiconductor structure layer comprises a first doped semiconductor layer, an active layer, and a second doped semiconductor layer sequentially stacked on the substrate; Performing ion implantation on the semiconductor structure layer to form an ion implantation region in the semiconductor structure layer, thereby electrically isolating a plurality of optoelectronic chip structures arranged in an array in the semiconductor structure layer; Etching the ion implantation region to form an isolation groove in the ion implantation region, thereby isolating at least the second doped semiconductor layers of any two adjacent optoelectronic chip structures from each other; A light blocking structure is arranged in the isolation groove, so as to at least prevent light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer.

7. The manufacturing method according to claim 6, characterized in that: The production method specifically comprises: Performing ion implantation on the semiconductor structure layer at least from the top surface of the second doped semiconductor layer, and the ion implantation depth at least reaches the top surface of the active layer, thereby forming the ion implantation region; Etching the ion implantation region to a depth less than the ion implantation depth but at least reaching the bottom end surface of the second doped semiconductor layer, thereby forming the isolation groove; Wherein, the top surface of the second doped semiconductor layer is a surface of the second doped semiconductor layer away from the substrate; Preferably, the production method specifically includes: Performing ion implantation on the semiconductor structure layer at least from the top surface of the second doped semiconductor layer, and the ion implantation depth reaches the inside of the first doped semiconductor layer, thereby forming the ion implantation area; Etching the ion implantation region to a depth less than the ion implantation depth and reaching the inside of the first doped semiconductor layer, thereby forming the isolation groove; Furthermore, a light blocking structure is arranged in the isolation groove to prevent light from being transmitted between any two adjacent optoelectronic chip structures through the second doped semiconductor layer and the active layer.

8. The manufacturing method according to claim 7, characterized in that: The production method further comprises: Manufacturing at least one dielectric layer, and making the dielectric layer continuously cover at least the sidewall of the isolation trench; Making a metal light isolation layer, and making the metal light isolation layer at least continuously cover the dielectric layer to form the light blocking structure; Preferably, the production method specifically includes: Forming a plurality of alternately stacked dielectric layers with different refractive indices at least on the sidewalls of the isolation groove, and combining the plurality of dielectric layers with the ion implantation region to form a distributed Bragg reflector structure; and / or, the dielectric layer is formed at least on the sidewall of the isolation groove with a heat-conducting dielectric material, the thermal expansion coefficient of the heat-conducting dielectric material is between the thermal expansion coefficient of the material constituting the metal light isolation layer and the thermal expansion coefficient of the material constituting the ion isolation region, and / or, the heat-conducting dielectric material has good bonding performance with the material constituting the metal light isolation layer and the material constituting the ion isolation region; and / or, forming a thermally conductive passivation layer on the surface of the semiconductor structure layer, and thermally conductively connecting the thermally conductive passivation layer to the metal optical isolation layer; and / or, extending the metal light isolation layer to cover the surface of the semiconductor structure layer to form a current spreading layer; Preferably, the material of the dielectric layer includes silicon oxide, silicon nitride, aluminum nitride, aluminum oxide, gallium oxide, titanium oxide or hafnium oxide; and / or the material of the metal light isolation layer includes gold, titanium, aluminum, nickel, chromium, molybdenum or copper; and / or the material of the thermal conductive passivation layer includes aluminum nitride, boron nitride or diamond.

9. The method according to any one of claims 6 to 8, characterized in that: The ion implantation zone is arranged around the corresponding optoelectronic chip structure, wherein the size of the ion implantation zone and the optoelectronic chip structure is 1μm to 50μm; and / or, the ions used in the ion implantation treatment include H ions, F ions, N ions or O ions; and / or, the distance between the inner wall of the isolation groove and the outer wall of the corresponding ion implantation zone is 100nm to 20μm; and / or, the material of the semiconductor structure layer includes III-V group compounds, preferably III group nitrides; and / or, the optoelectronic chip structure includes a Micro-LED chip structure.

10. A Micro-LED device, characterized in that A micro optoelectronic chip comprising any one of claims 1-5.

Citation Information

Patent Citations

  • Manufacturing method of semiconductor photoelectronic device

    CN110957399A

  • Micro-light emitting diode vertical chip structure and preparation method and application thereof

    CN112599554A

  • Light emitting diode structure and manufacturing method thereof

    CN112864290A

  • Miniature light emitting diode display device and manufacturing method thereof

    CN114188459A

  • LED structure, preparation method thereof and light field display system

    CN114824043A

Cited By

  • Semiconductor laser and laser radar

    CN119944429A

  • Preparation method of LED chip structure and LED chip structure

    CN120091670A