Secondary battery and preparation method therefor
By using porous hard carbon negative electrode sheets prepared by high-temperature calcination in sodium-ion batteries, the problem of porosity control of the negative electrode sheets of sodium-ion batteries is solved, the cycle performance and first charge and discharge capability are improved, and the preparation cost is reduced.
Patent Information
- Application Number
- PCT/CN2023/141000
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2023-12-22
- Publication Date
- 2024-10-31
AI Technical Summary
It is difficult to effectively improve the cycle performance and first charge-discharge specific capacity by controlling the porosity of the negative electrode sheet of existing sodium-ion batteries, and the preparation cost of hard carbon materials is high.
Hard carbon is used as the negative active material. Plastic particles and metal compounds are uniformly mixed and calcined at high temperature to form a porous structure of the hard carbon precursor. The metal compound is removed by water washing or pickling to obtain a pore volume of 0.008 to 0.025 cm3/g. and a negative electrode sheet with a porosity of 20 to 40%, combined with a conductive agent and a binder to prepare the negative electrode sheet.
It significantly improves the long cycle performance and first discharge specific capacity of sodium-ion batteries, while reducing the preparation cost of hard carbon negative active materials, improving sodium ion transmission channels, and reducing the risk of electrolyte leakage.
Smart Images

Figure PCTCN2023141000-FTAPPB-I100001 
Figure PCTCN2023141000-FTAPPB-I100002 
Figure PCTCN2023141000-FTAPPB-I100003
Abstract
Description
Secondary battery and preparation method thereof
[0001] Citation of Related Applications
[0002] This disclosure claims all rights and interests in the invention patent application with application number 202310473844.7 and invention name “Secondary battery and its preparation method” filed with the State Intellectual Property Office of the People’s Republic of China on April 25, 2023, and incorporates its entire contents into this disclosure by reference.
[0003] field
[0004] The present disclosure relates generally to the field of secondary batteries, and more particularly to secondary batteries and methods of making the same.
[0005] background
[0006] The porosity of the negative electrode sheet directly affects the cycle performance and initial charge and discharge specific capacity of the sodium-ion battery. The porosity of the negative electrode sheet of the sodium-ion battery can be regulated based on the negative electrode active material.
[0007] Hard carbon, due to its advantages such as low cost, widespread availability, and simple synthesis, has become a promising anode active material for sodium-ion batteries. Current research generally suggests that hard carbon can effectively store sodium ions within its pores. Therefore, a suitable pore volume is more effective for sodium ion storage, significantly improving the capacity performance of hard carbon materials.
[0008] Overview
[0009] In a first aspect, the present disclosure provides a secondary battery comprising a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, wherein the negative electrode active material comprises a porous material, wherein the porous material comprises hard carbon; and wherein the pore volume of the negative electrode active material is 0.008 to 0.025 cm 3 / g; and the porosity of the negative electrode sheet is 20 to 40%.
[0010] In certain embodiments, the specific surface area of the negative electrode active material is 4 to 10 m 2 / g.
[0011] In certain embodiments, the particle size D50 of the negative electrode active material is 3.5 to 6 μm.
[0012] In certain embodiments, the pore size of the negative electrode active material is 2 to 10 nm.
[0013] In certain embodiments, the compacted density of the negative electrode active material is 0.9 to 1.3 g / cm 3 .
[0014] In certain embodiments, the negative electrode active material comprises a metal element, and the metal element includes at least one of Li, Na, K, Mg, Ca, Fe, Co, Cu, Zn, and Al.
[0015] In certain embodiments, the mass percentage of the metal element in the negative electrode active material is less than 0.2%.
[0016] In certain embodiments, the secondary battery comprises a positive electrode sheet comprising a positive electrode active material comprising a sodium-containing compound.
[0017] In a second aspect, the present disclosure provides a method for preparing the secondary battery of the present disclosure, which comprises:
[0018] The plastic particles are uniformly mixed with the metal compound, and then calcined at a high temperature of 1000 to 1800° C. for 2 to 6 hours to obtain a hard carbon precursor;
[0019] The hard carbon precursor is washed with water and / or acid-washed to remove metal compounds, thereby obtaining the negative electrode active material; and
[0020] The hard carbon porous material, the conductive agent and the binder are mixed into a slurry, the slurry is coated on a current collector, and the negative electrode sheet is obtained through roller pressing, drying and cutting.
[0021] In certain embodiments, the mass ratio of the plastic particles to the metal compound is (90-99):(1-10).
[0022] In a third aspect, the present disclosure provides a sodium ion battery comprising a positive electrode sheet, a separator, an electrolyte, and a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, the negative electrode active material comprises a porous material, and the porous material comprises hard carbon; the pore volume of the negative electrode active material is 0.008 to 0.025 cm 3 / g; and the porosity of the negative electrode sheet is 20 to 40%.
[0023] In certain embodiments, the negative electrode sheet in the secondary battery of the present disclosure significantly improves the sodium ion transmission channel and enhances the sodium storage capacity, which not only improves the long cycle performance and first discharge specific capacity of the secondary battery, but also reduces the preparation cost of the hard carbon negative electrode active material of the secondary battery.
[0024] Details
[0025] The present disclosure provides a secondary battery and a method for preparing the same. Those skilled in the art can refer to the contents of this article and appropriately improve the process parameters for implementation. It is particularly important to point out that all similar replacements and modifications are obvious to those skilled in the art, and they are all deemed to be included in this disclosure. The method described in this disclosure has been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method described herein without departing from the content, spirit and scope of this disclosure to implement and apply the technology disclosed in this disclosure. Obviously, the described embodiments are part of the embodiments of this disclosure, not all of the embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this disclosure.
[0026] It should be noted that, in this document, if relational terms such as "first" and "second", "step 1" and "step 2", and "(1)" and "(2)" appear, they are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "include one..." do not exclude the presence of other identical elements in the process, method, article or device comprising the elements. At the same time, the embodiments and features in the embodiments of the present disclosure can be combined with each other in the absence of conflict.
[0027] In a first aspect, the present disclosure provides a secondary battery comprising a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, wherein the negative electrode active material comprises a porous material, wherein the porous material comprises hard carbon; and wherein the pore volume of the negative electrode active material is 0.008 to 0.025 cm 3 / g; and the porosity of the negative electrode sheet is 20 to 40%.
[0028] In certain embodiments, the pore volume of the negative electrode active material may be 0.008 cm 3 / g, 0.010cm 3 / g, 0.012cm 3 / g, 0.015cm 3 / g, 0.018cm 3 / g, 0.020cm 3 / g, 0.022cm 3 / g, 0.025cm 3 / g or the range formed by any two values thereof. The pore volume of the negative electrode active material is within the range disclosed herein, which is conducive to improving the sodium storage capacity of the negative electrode active material, thereby improving the long cycle capacity and first discharge specific capacity of the battery. Moreover, when the battery is injected with electrolyte, the porosity of the negative electrode active material is within the range disclosed herein, which is conducive to regulating the contact area between the electrolyte and the material, improving the cycle capacity of the battery, and reducing the risk of electrolyte leakage.
[0029] In certain embodiments, the porosity of the negative electrode sheet can be 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, or a range consisting of any two thereof. By using the negative electrode active material disclosed herein to prepare a negative electrode sheet, the porosity of the negative electrode sheet can be controlled between 20 and 40%, which is beneficial for improving the initial charge and discharge capacity and cycle performance of the battery.
[0030] In certain embodiments, the specific surface area of the negative electrode active material is 4 to 10 m 2 / g, for example 4m 2 / g、5m 2 / g、6m 2 / g、7m 2 / g、8m 2 / g、9m 2 / g、10m 2 The specific surface area of the negative electrode active material is within the range disclosed herein, which is beneficial to improving the first efficiency of the battery and balancing the first efficiency and specific capacity.
[0031] In certain embodiments, the particle size distribution D50 of the negative active material is 3.5 to 6 μm, for example, 3.5 μm, 4.0 μm, 4.5 μm, 5.0 μm, 5.5 μm, 6.0 μm, or a range formed by any two values therein.
[0032] In certain embodiments, the pore size of the negative electrode active material is 2 to 10 nm. In certain embodiments, the pore size of the negative electrode active material is 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or a range formed by any two of these values. The pore size affects the specific surface area of the material, and pore sizes within the range disclosed herein are beneficial for ensuring that the specific surface area is within the range disclosed herein.
[0033] In certain embodiments, the compacted density of the negative electrode active material is 0.9 to 1.3 g / cm 3 In certain embodiments, the compacted density of the negative electrode active material is 0.9 g / cm 3 , 1.0g / cm 3 , 1.1g / cm 3, 1.2g / cm 3 , 1.3g / cm 3 Or a range formed by any two of these values.
[0034] In certain embodiments, the negative electrode active material comprises a metal element, and the metal element includes at least one of Li, Na, K, Mg, Ca, Fe, Co, Cu, Zn, and Al.
[0035] In certain embodiments, the weight percentage of the metal element in the negative electrode active material is less than 0.2%. In certain embodiments, the weight percentage of the metal element is less than 0.01%, 0.05%, 0.08%, 0.1%, 0.12%, 0.14%, 0.16%, 0.18%, 0.2%, or any combination thereof. A metal element content within the above range is beneficial for increasing the specific capacity of the negative electrode active material.
[0036] In certain embodiments, the mass percentage of the metal element in the negative electrode active material is 0.05 to 0.2%.
[0037] In certain embodiments, the secondary battery comprises a positive electrode sheet comprising a positive electrode active material comprising a sodium-containing compound.
[0038] In a second aspect, the present disclosure provides a method for preparing the secondary battery of the present disclosure, which comprises:
[0039] The plastic particles are uniformly mixed with the metal compound, and then calcined at a high temperature of 1000 to 1800 degrees Celsius for 2 to 6 hours to obtain a hard carbon precursor;
[0040] The hard carbon precursor is washed with water and / or acid-washed to remove metal compounds, thereby obtaining the negative electrode active material; and
[0041] The negative electrode active material, conductive agent and binder are mixed into slurry, the slurry is coated on a current collector, and the negative electrode sheet is obtained through rolling, drying and cutting.
[0042] In certain embodiments, the carbon source for the hard carbon comprises plastic particles. Plastics are widely used in packaging bags. Once used, these plastics are destined for landfill. However, these plastic wastes remain difficult to degrade over time, significantly polluting the environment. Using plastics as a carbon source for hard carbon effectively conserves resources and reduces costs.
[0043] In some embodiments, the metal compound comprises at least one of a metal oxide, a metal chloride, a metal nitrate, and a metal sulfate, wherein the metal comprises one of Li, Na, K, Mg, Ca, Fe, Co, Cu, Zn, and Al. In some embodiments, the metal ion comprises Li + 、Na + , K + Mg 2+ , Ca 2+ 、Fe 3+ 、Co 2+ 、Cu 2+ 、Zn 2+ and Al 3+ In certain embodiments, the metal compound comprises at least one of sodium chloride, calcium oxide, magnesium oxide, and cobalt chloride.
[0044] In certain embodiments, the plastic particles include at least one of polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyisobutylene, styrene-acrylonitrile copolymer, acrylonitrile-butadiene-styrene copolymer, polymethacrylate, ethylene-vinyl acetate copolymer, polyethylene terephthalate, polyvinyl alcohol, polybutylene terephthalate, polyamide, polycarbonate, polyoxymethylene ester, polyphenylene oxide, polyphenylene sulfide, and polyurethane plastic particles. In certain embodiments, the degree of polymerization of the polymer is within the range of conventional industrial-grade products. In certain embodiments, the molecular weight of the polyethylene is 10,000 to 100,000, the molecular weight of the polyvinyl chloride is 50,000 to 110,000, the molecular weight of the polyisobutylene is 30,000 to 100,000, the molecular weight of the ethylene-vinyl acetate copolymer is 1,000 to 4,000, the molecular weight of the polyethylene terephthalate is 10,000 to 40,000, the molecular weight of the polyvinyl alcohol is 20,000 to 150,000, the molecular weight of the polyamide is 17,000 to 23,000, and the molecular weight of the polycarbonate is 10,000 to 50,000.
[0045] In certain embodiments, mixing the plastic particles with the metal compound includes mixing the plastic particles and the metal compound using an organic solvent as a medium. In certain embodiments, the organic solvent includes at least one of p-xylene, trichlorobenzene, nitrobenzene, isoamyl acetate, ethyl acetate, hexane, chloroform, carbon tetroxide, tetrahydrofuran, cyclohexanone, ketone, dimethylformamide, dimethyl sulfoxide, m-cresol, o-chlorophenol, and trichloroacetic acid. In certain embodiments, the plastic particles, metal compound, and organic solvent are mixed and fully contacted before being dried at a temperature of 100 to 200°C.
[0046] In certain embodiments, the homogeneous mixing further comprises grinding.
[0047] In certain embodiments, the mass ratio of the plastic particles to the metal compound is (90-99):(1-10). Controlling the mass ratio of the plastic particles to the metal compound within the scope of the present disclosure is beneficial for regulating the pore structure of the negative electrode active material.
[0048] In certain embodiments, the organic solvent is added in an amount of 5% to 15% of the total mass of the plastic particles and the metal compound.
[0049] In certain embodiments, the high temperature calcination temperature is 1000° C., 1100° C., 1200° C., 1300° C., 1400° C., 1500° C., 1600° C., 1700° C., 1800° C., or a range formed by any two values. In certain embodiments, the high temperature calcination temperature is increased at a rate of 2 to 20° C. / min.
[0050] In certain embodiments, during the process of water washing and / or acid washing to remove metal compounds, water washing mainly removes water-soluble metal compounds such as sodium chloride, and acid washing removes water-insoluble metal compounds or reduced metals. After washing, the negative electrode active material contains almost no metal compounds originally added. The use of metal compounds is mainly to play a role in forming pores in the negative electrode active material, forming a porous negative electrode active material with a pore volume of 0.008 to 0.025 cm 3 In some embodiments, the acid comprises at least one of sulfuric acid, nitric acid, hydrochloric acid and hydrofluoric acid. The concentration of the acid is not critical and can be selected from 1 to 3M.
[0051] In certain embodiments, the water washing and / or acid washing to remove the metal compounds further comprises drying, wherein the drying temperature is 100 to 200°C.
[0052] In a third aspect, the present disclosure provides a sodium-ion battery comprising a cathode, a separator, an electrolyte, and the anode described herein. In certain embodiments, the sodium-ion battery described herein can be a full cell, a half cell, or a symmetrical cell, or can be a button cell, a pouch cell, or the like.
[0053] In certain embodiments, the cathode material may be a transition metal layered oxide, a polyanionic compound, a Prussian blue analog, or the like. In certain embodiments, the separator may be a polyethylene, polypropylene, or the like. In certain embodiments, the electrolyte may be an electrolyte containing 1 to 1.5 M sodium hexafluorophosphate. In certain embodiments, ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 1:1:1.
[0054] In certain embodiments, the conductive agent and binder involved in the positive electrode material and the negative electrode active material described in the present disclosure may also use conventional materials. In certain embodiments, the conductive agent may include carbon black, conductive graphite, VGCF (vapor-grown carbon fiber), carbon nanotubes, and graphene, and the binder may include polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyacrylic acid (PAA) and its salts, polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), etc.
[0055] In the comparative experiments provided in this disclosure, unless otherwise specified, other experimental conditions and materials, etc., except for the differences noted in each group, were kept consistent to ensure comparability. In addition, all materials used in this disclosure can be purchased from commercial sources.
[0056] The secondary battery and its preparation method provided by the present disclosure are further described below. Example
[0057] Example 1
[0058] Polyethylene (molecular weight of 20,000) and sodium chloride powder are mixed in a mass ratio of 93:7, 10% of the total amount of the mixture is added to p-xylene, and the mixture is fully ground to obtain a mixed slurry. The mixed slurry is then dried at 150°C, and after drying, the mixed slurry is calcined at a high temperature of 1200°C for 2h with a heating rate of 5°C / min to prepare a hard carbon material precursor. The obtained precursor is washed in water, filtered, and dried to remove sodium chloride to obtain the negative electrode active material. The negative electrode active material, conductive agent acetylene black (SuperP) and binder (SBR) are mixed uniformly in a mass ratio of 80:10:10, and the mixed slurry is coated on a copper foil with a diameter of 12 mm, and a negative electrode sheet is obtained after vacuum baking. The negative electrode sheet is then placed in a 2023 button battery shell and assembled into a half-cell with sodium foil as the counter electrode.
[0059] Other Examples and Comparative Examples:
[0060] The preparation methods of the negative electrode active materials of the remaining examples and comparative examples refer to Example 1, with the differences shown in Table 1.
[0061] Table 1
[0062] Performance test results are shown in Table 2
[0063] Performance testing method:
[0064] The test method of the first discharge specific capacity is to conduct charge and discharge test at 0.1C rate, with the voltage range of 2.0V to 4.0V. First, conduct the charge test to obtain the charge specific capacity Qc , then conduct discharge test to obtain the discharge specific capacity Q d , Q d This is the first discharge specific capacity.
[0065] The calculation method of capacity retention rate is the ratio of the first discharge voltage to the first charge voltage, that is, Q d / Q c is the capacity retention rate.
[0066] Table 2
[0067] Combining the data in Table 1 and Table 2, it can be concluded that when the negative electrode active material is prepared by using a metal compound for pore formation, the pore volume of the negative electrode active material prepared is 0.008 to 0.025 cm 3 / g range, providing more suitable active sites for sodium storage in the hard carbon negative electrode active material, and at the same time, the porosity of the prepared negative electrode sheet can be controlled between 20 and 40%, which makes the first discharge specific capacity and cycle life of Examples 1 to 13 higher than those of the hard carbon negative electrode active material without using metal compounds for pore formation.
[0068] The comparison between Examples 2 and 7 and Comparative Example 3 shows that when the mass ratio of plastic particles to metal compounds is controlled within the range of (90-99):(1-10), it is beneficial to maintain the pore volume of the hard carbon negative electrode active material at 0.008 to 0.025 cm 3 / g range and the porosity of the negative electrode sheet is within the range of 20 to 40%, thereby improving battery performance. In the present disclosure, the metal compound mainly plays the role of creating pores in the hard carbon negative electrode active material. Therefore, the mass ratio of the plastic particles to the metal compound has a significant impact on the pore volume of the hard carbon negative electrode active material.
[0069] The foregoing description is intended only to provide specific embodiments of the present disclosure, which will enable those skilled in the art to understand and implement the present disclosure. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure is not intended to be limited to the embodiments shown herein, but rather to be construed in the broadest manner consistent with the principles and novel features disclosed herein.
Claims
1. A secondary battery comprising a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, wherein the negative electrode active material comprises a porous material, and wherein the porous material comprises hard carbon; The pore volume of the negative electrode active material is 0.008 to 0.025 cm 3 / g; and The porosity of the negative electrode sheet is 20 to 40%.
2. The secondary battery according to claim 1, wherein the specific surface area of the negative electrode active material is 4 to 10 m 2 / g. 3 . The secondary battery according to claim 1 , wherein the particle size D50 of the negative electrode active material is 3.5 to 6 μm. 4 . The secondary battery according to claim 1 , wherein the pore size of the negative electrode active material is 2 to 10 nm.
5. The secondary battery according to claim 1, wherein the compaction density of the negative electrode active material is 0.9 to 1.3 g / cm 3 . 6 . The secondary battery according to claim 1 , wherein the negative electrode active material contains a metal element, the metal element comprising at least one of Li, Na, K, Mg, Ca, Fe, Co, Cu, Zn, and Al.
7. The secondary battery according to claim 1, wherein the mass percentage of the metal element in the negative electrode active material is less than 0.2%. 8 . The secondary battery according to claim 1 , wherein the secondary battery comprises a positive electrode sheet, the positive electrode sheet comprises a positive electrode active material, and the positive electrode active material comprises a sodium-containing compound.
9. A method for preparing a secondary battery according to any one of claims 1 to 8, comprising: The plastic particles are uniformly mixed with the metal compound, and then calcined at a high temperature of 1000 to 1800° C. for 2 to 6 hours to obtain a hard carbon precursor; The hard carbon precursor is washed with water and / or acid to remove metal compounds, thereby obtaining the negative electrode active material; as well as The negative electrode active material, the conductive agent and the binder are mixed into slurry, the slurry is coated on the current collector, and the negative electrode sheet is obtained through rolling, drying and cutting. 10 . The method for preparing a secondary battery according to claim 9 , wherein the mass ratio of the plastic particles to the metal compound is (90-99):(1-10).
11. A sodium ion battery comprising a positive electrode sheet, a separator, an electrolyte and a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, the negative electrode active material comprises a porous material, and the porous material comprises hard carbon; The pore volume of the negative electrode active material is 0.008 to 0.025 cm 3 / g; and The porosity of the negative electrode sheet is 20 to 40%.
12. The sodium ion battery according to claim 11, wherein the specific surface area of the negative electrode active material is 4 to 10 m 2 / g. 13 . The sodium ion battery according to claim 11 , wherein the particle size D50 of the negative electrode active material is 3.5 to 6 μm.
14. The sodium ion battery of claim 11, wherein the pore size of the negative electrode active material is 2 to 10 nm.
15. The sodium ion battery of claim 11, wherein the compaction density of the negative electrode active material is 0.9 to 1.3 g / cm 3 .
16. The sodium ion battery of claim 11, wherein the negative electrode active material contains a metal element, and the metal element includes at least one of Li, Na, K, Mg, Ca, Fe, Co, Cu, Zn and Al.
17. The sodium ion battery of claim 11, wherein the mass percentage of the metal element in the negative electrode active material is less than 0.2%.
18. The sodium ion battery according to any one of claims 11 to 17, wherein the secondary battery comprises a positive electrode sheet, the positive electrode sheet comprises a positive electrode active material, and the positive electrode active material comprises a sodium-containing compound.
Citation Information
Patent Citations
Negative active material, negative pole piece comprising same, electrochemical device and electric device
CN115458723A
Hard carbon material, negative pole piece and electrochemical device
CN116022771A
Secondary battery and method for manufacturing the same
CN116741991A
Particulate composite materials
US20220055906A1
Methods of passivation to control oxygen content and reactivity of silicon-carbon composite materials