Rare earth-containing additive and preparation method therefor

By adopting a gas-solid two-phase structure and a streamlined shell design in rare earth additives, the problems of poor mixing uniformity and oxide inclusion of rare earths in molten steel are solved, achieving uniform distribution and high yield of rare earths, and improving the performance of steel. .

WO2024222341A1PCT designated stage expired Publication Date: 2024-10-31GRIREM ADVANCED MATERIALS CO LTD +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/083568
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-03-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The mixing uniformity of rare earths in molten steel is poor, resulting in serious segregation of components, and the excellent effects of rare earths cannot be fully exerted. In addition, the oxide inclusions in commercially available rare earth additives are generally large and difficult to control.

Method used

Rare earth additives with a gas-solid two-phase structure sealed inside the shell are used. The gas at a preset pressure pushes the internal solid additives when the shell becomes thinner, so that they are evenly distributed in the molten steel. The streamlined shell is used to reduce resistance and improve the collection of rare earths. yield and mixing uniformity.

Benefits of technology

It effectively solves the problems of uneven distribution of rare earths in steel and unstable composition control, improves the yield and mixing uniformity of rare earths, reduces oxide inclusions, and improves the performance of the final steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024083568_31102024_PF_FP_ABST
    Figure CN2024083568_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention is a rare earth-containing additive and a preparation method therefor. The rare earth-containing additive comprises a closed shell and a plurality of intermediate alloys arranged in the shell, wherein the intermediate alloys contain rare earth elements, and the shell is filled with a gas of preset pressure. By means of a gas-solid two-phase structure sealed in the shell of the additive, after liquid steel is added to the additive, as the wall of the shell thins, the gas will break through the shell to push the internal solid additive in every direction, improving the uniformity of rare earth distribution and the rare earth yield in a final product.
Need to check novelty before this filing date? Find Prior Art

Description

A rare earth-containing additive and preparation method thereof

[0001] Cross-references

[0002] This application is based on the Chinese patent application with application number 2023104782308 and application date April 28, 2023, and claims the priority of the Chinese patent application. The entire content of the Chinese patent application is hereby introduced into this application as a reference. Technical Field

[0003] The present invention relates to the field of rare earth alloys, and in particular to a rare earth-containing additive and a preparation method thereof. Background Art

[0004] Adding rare earth elements to steel can deoxidize and purify the molten steel, spheroidize sulfide inclusions, reduce material anisotropy, and improve the transverse impact resistance of rolled products. They can also act as microalloying elements to influence the evolution of the material's microstructure. However, due to significant differences in the density, melting point, and reactivity of rare earth elements compared to the steel matrix, evenly mixing rare earth elements into the molten steel is difficult, leading to severe component segregation and significantly diminishing their effectiveness. Therefore, how to evenly and effectively incorporate rare earth elements into the molten steel to maximize their potential remains a crucial challenge in this field.

[0005] At present, the method commonly used in industry is to put rare earth intermediate alloys in the form of solid blocks, ingots, wires, powders, rods or rare earth cored wires into molten steel, and after it melts, rely on its own diffusion and soft blowing of the molten steel to mix the rare earth and molten steel evenly. However, considering that a bag of molten steel often weighs hundreds of tons and the time from rare earth addition to casting is short, the above rare earth additives often cause uneven distribution and severe segregation after being added to molten steel, which makes it impossible to fully exert the role of rare earth. Secondly, the oxide inclusions in the rare earth additives have a great influence on the final performance of the steel. The rare earth oxide inclusions in the rare earth additives currently available on the market are generally large and difficult to control.

[0006] Summary of the Invention

[0007] The purpose of the embodiments of the present invention is to provide a rare earth-containing additive and a preparation method thereof. By adopting a gas-solid two-phase structure sealed inside a shell, after the additive is added to molten steel, as the shell wall becomes thinner, the gas breaks through the shell and pushes the solid additive inside in all directions, thereby improving the uniformity of rare earth distribution in the final product and the rare earth yield.

[0008] To solve the above technical problems, a first aspect of an embodiment of the present invention provides a rare earth-containing additive and a preparation method thereof, comprising: a sealed shell and a plurality of master alloys disposed inside the shell; wherein the master alloy contains rare earth elements;

[0009] The shell is filled with gas at a preset pressure.

[0010] Furthermore, the shape of the shell is one of a cuboid, a sphere, a cylinder, a frustum, a cone, and a streamline.

[0011] Furthermore, the housing includes: a front housing and a rear housing;

[0012] The front shell is integrally connected to the edge of the rear shell, and the plurality of master alloys and the gas are located in a closed space between the front shell and the rear shell.

[0013] Furthermore, the counterweight of the front shell is greater than the counterweight of the rear shell.

[0014] Furthermore, the profile of the streamlined front housing satisfies the following mathematical expression obtained by rotating one circle around the x-axis:

[0015] Wherein, x is the coordinate value of the front housing in the X-axis direction, y is the coordinate value of the Y-axis direction perpendicular to the axial direction of the front housing, the origin of the XY coordinates is at the center point of the interface between the front housing and the rear housing, R is the minor axis radius of the ellipse on which the central axis section of the front housing lies, and L is the major axis radius of the ellipse on which the central axis section of the front housing lies;

[0016] The length of the front housing along the housing length direction is greater than the length of the rear housing along the housing length direction, and the maximum diameter B of the rear housing along the Y-axis direction is less than or equal to 2R.

[0017] Furthermore, the master alloy includes: rare earth metal and iron;

[0018] The rare earth metal content is 8wt% to 90wt%, and the iron content is 10wt% to 92wt%;

[0019] Among them, the oxygen content is less than 150ppm, the maximum size of inclusions is less than 30μm, and the total amount of inclusions is less than 0.5wt%.

[0020] Furthermore, the intermediate alloy composition is RE-Fe-M, where M is a transition metal, and the transition metal includes at least one of nickel, chromium, tungsten, molybdenum, cobalt, manganese, vanadium, niobium, and titanium; preferably, the transition metal includes at least one of chromium, tungsten, molybdenum, vanadium, niobium, and titanium;

[0021] In the master alloy, the rare earth metal content is 15wt% to 70wt%, the transition metal content is 0.1wt% to 15wt%, and the iron content is 20wt% to 70wt%;

[0022] The oxygen content of the rare earth-containing additive is less than 100 ppm, the carbon content is less than 300 ppm, the maximum size of inclusions is less than 25 μm, and the total amount of inclusions is less than 0.1 wt%.

[0023] Furthermore, the rare earth metal includes at least one of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium;

[0024] Preferably, the rare earth metal includes at least one of lanthanum, cerium and yttrium.

[0025] Furthermore, the shell is made of iron alloy;

[0026] The iron content of the ferroalloy is greater than 95 wt %;

[0027] The shell wall thickness ranges from 2.5 mm to 50 mm, and the length / diameter ratio ranges from 1 to 5;

[0028] Preferably, the shell wall thickness ranges from 5 mm to 30 mm, and the length / diameter ratio ranges from 1 to 3.

[0029] Furthermore, the ratio of the sum of the volumes of the plurality of master alloys to the volume of the inner cavity of the housing is greater than or equal to a preset value;

[0030] Preferably, the preset value is 70%.

[0031] Furthermore, the gas includes at least one of argon, nitrogen, helium, neon, krypton, radon, xenon, carbon dioxide, and carbon monoxide;

[0032] Preferably, the gas includes: argon;

[0033] Furthermore, the oxygen content in the gas is ≤10 ppm.

[0034] Furthermore, the preset pressure value of the gas is 0.04MPa-0.3MPa;

[0035] Preferably, the preset pressure value of the gas is 0.08MPa-0.12MPa.

[0036] Accordingly, a second aspect of an embodiment of the present invention includes a method for preparing a rare earth-containing additive, which is used to prepare the rare earth-containing additive, comprising the following steps:

[0037] Adding iron to a vacuum induction melting furnace and filling it with inert gas to a first preset pressure value;

[0038] After the temperature reaches a first preset temperature, rare earth metal is added to the iron solution, and the solution is heated until the alloy is completely melted;

[0039] The alloy solution is poured into a mold and cooled in a furnace under the protection of an inert gas to obtain a rare earth alloy;

[0040] After the rare earth alloy is loaded into the shell, gas with a second preset pressure value is filled in, and the shell is sealed to obtain the rare earth-containing additive.

[0041] Furthermore, the numerical range of the first preset pressure value is 10000Pa-90000Pa;

[0042] The numerical range of the second preset pressure value is 0.04-0.3 MPa; preferably, the preset pressure value is 0.08-0.12 MPa;

[0043] The numerical range of the first preset temperature value is 1550°C-1800°C.

[0044] The above technical solutions of the embodiments of the present invention have the following beneficial technical effects:

[0045] 1. The gas in the additive generates thrust when heated and expands, thereby achieving the goal of uniform dispersion of rare earth metals in the steel. This can effectively solve the problems of unstable rare earth component control, uneven distribution, and low yield in rare earth steel;

[0046] 2. By adopting a streamlined shell with a special shape, it has a smaller resistance coefficient than ordinary rare earth additives on the market, and can achieve a deeper penetration depth in the molten steel, penetrating into the middle and lower part of the ladle, so as to achieve the purpose of uniform mixing of rare earth and molten steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] FIG1 is a schematic diagram of the structure of a rare earth-containing additive provided in an embodiment of the present invention.

[0048] 1. Front shell, 2. Rear shell, 3. Shell, 4. Master alloy, 5. Gas. DETAILED DESCRIPTION

[0049] To make the objectives, technical solutions, and advantages of the present invention more clearly understood, the present invention will be further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are merely exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present invention.

[0050] 1 , an embodiment of the present invention provides a rare earth-containing additive, comprising: a sealed shell 3 and a plurality of intermediate alloys 4 disposed inside the shell 3 ; wherein the intermediate alloys 4 contain rare earth elements; and the shell 3 is filled with a gas 5 at a preset pressure.

[0051] By making the rare earth-containing additive contain both gas and solid phases, it expands when added to the molten steel due to heat, forming a positive pressure inside. As the shell of the additive continues to melt and the shell wall becomes thinner, the internal gas pressure breaks through the shell, generating a driving force, pushing the internal solid phase rare earth additive to the surroundings, further fully mixing the rare earth additive, and significantly improving the rare earth yield.

[0052] Optionally, the wall thickness of the rare earth additive shell 3 is selected to be in the range of 2.5-50 mm, preferably 5-30 mm, and the length / diameter (width) ratio is 1-5, with the longest side being 400 mm, preferably 1-3, with the longest side being 300 mm. A rare earth additive that is too small results in an excessively long addition time, while a rare earth additive that is too large results in a prolonged melting time and increased risk. Therefore, the preferred size range is determined based on a comprehensive consideration of the rare earth additive addition time, melting time, and production safety.

[0053] Optionally, the shell 3 has a shape of a cuboid, a sphere, a cylinder, a truncated cone, a cone, or a streamlined shape.

[0054] Preferably, the housing 3 comprises a front housing 1 and a rear housing 2; the front housing 1 and rear housing 2 are integrally connected at their edges, with a plurality of master alloys 4 and a gas 5 located within the enclosed space between the front housing 1 and rear housing 2; the front housing and rear housing have different shapes. Preferably, the front housing has a greater counterweight than the rear housing.

[0055] Furthermore, the front shell 1 is a semi-ellipsoid, and the rear shell 2 is a cylinder, a cone or a semi-ellipsoid.

[0056] The front shell 1 adopts a streamlined semi-ellipsoidal structure. The streamlined shell reduces the resistance coefficient of the rare earth additive, thereby reducing the viscous resistance of the rare earth additive in the steel. Compared with ordinary blocks, it can achieve a deeper penetration depth of the molten steel and increase the uniformity of rare earth mixing.

[0057] Specifically, the cross-sectional profile of the front housing 1 satisfies:

[0058] Wherein, x is the axial X-axis coordinate value of the front shell 1, y is the Y-axis coordinate value perpendicular to the streamlined axial direction of the front shell 1, the origin of the XY-axis coordinates is at the center point of the interface between the front shell and the rear shell, R is the minor axis radius value of the ellipse on which the central axis section of the front shell is located, and L is the major axis radius value of the ellipse on which the central axis section of the front shell is located; the maximum diameter B of the rear shell 2 along the Y-axis direction is ≤ 2R.

[0059] When R / L = 1, it is a sphere; when R / L ≠ 1, it is an ellipsoid, and the shape of the first part is ≤ semi-ellipsoid; the preferred L / R range is 1-5. The front shell shape in this range is more sharp, penetrates deeper into the molten steel, and has a better addition effect.

[0060] Preferably, the length of the front shell accounts for more than 50% of the entire rare earth additive length, achieving a "top-heavy" effect, which can ensure that the first shell is dropped downward into the molten steel.

[0061] Furthermore, the master alloy 4 includes rare earth metal and iron; the rare earth metal content is 8wt% to 90wt%, and the iron content is 10wt% to 92wt%; wherein the oxygen content is less than 150ppm, the maximum size of inclusions is less than 30μm, and the total amount of inclusions is less than 0.5wt%.

[0062] Furthermore, the rare earth metal includes at least one of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium. Preferably, the rare earth metal includes at least one of lanthanum, cerium, and yttrium. Among the rare earth metals, lanthanum, cerium, and yttrium are highly abundant, inexpensive, and have a good additive effect.

[0063] In another embodiment of the present invention, the master alloy 4 further comprises a transition metal. The transition metal comprises at least one of nickel, chromium, tungsten, molybdenum, cobalt, manganese, vanadium, niobium, and titanium. Preferably, the transition metal comprises at least one of chromium, tungsten, molybdenum, vanadium, niobium, and titanium. Transition metals are derived from common trace elements in steel and do not introduce new impurities. Furthermore, the transition metals serve to microalloy the rare earth additive and prevent oxidation of the rare earth additive.

[0064] Specifically, the rare earth metal content in master alloy 4 is 15% to 70% by weight, the transition metal content is 0.1% to 15% by weight, and the iron content is 20% to 70% by weight. At this point, the oxygen content is less than 100 ppm, the carbon content is less than 300 ppm, the maximum inclusion size is less than 25 μm, and the total inclusion content is less than 0.1% by weight. Controlling the size and quantity of inclusions significantly influences the final additive effect. Within this range, the rare earth additive achieves the best results.

[0065] Furthermore, the shell is made of an iron alloy, and the proportion of iron in the iron alloy is greater than 95wt%.

[0066] Furthermore, the ratio of the sum of the volumes of the plurality of master alloys 4 to the volume of the shell cavity is greater than or equal to a predetermined value; preferably, the predetermined value is 70%. The volume of the rare earth alloy filled internally accounts for ≥ 70% of the total volume of the entire cavity. This allows for a larger amount of additive to be added at a time, resulting in higher addition efficiency. Furthermore, a larger volume of the rare earth alloy filled internally increases the overall density of the additive, allowing it to penetrate deeper into the middle and lower portion of the ladle, achieving uniform mixing of the rare earth and molten steel.

[0067] Specifically, gas 5 includes at least one of argon, nitrogen, helium, neon, krypton, radon, xenon, carbon dioxide, and carbon monoxide. Preferably, gas 5 includes argon. Argon is preferred because it is an inert gas and does not react with rare earth metals when used as a filling gas. It is also cheaper than inert gases such as helium, neon, krypton, radon, and xenon, making it more suitable for industrial production. Nitrogen readily reacts with rare earth metals, while carbon dioxide and carbon monoxide easily increase the carburization of molten steel. Carbon monoxide can easily cause human poisoning and is therefore not within the preferred range. The oxygen content is ≤10 ppm to minimize oxygen introduction.

[0068] Optionally, the preset pressure value of the gas 5 is 0.04MPa-0.3MPa; preferably, the preset pressure value of the gas 5 is 0.08MPa-0.12MPa. The pressure of the gas 5 is determined by comprehensively considering the pressure of the molten steel, explosion feasibility and production safety.

[0069] Accordingly, a second aspect of an embodiment of the present invention provides a method for preparing a rare earth-containing additive, which is used to prepare the rare earth-containing additive, comprising the following steps:

[0070] In step S100 , iron is added to a vacuum induction melting furnace, and an inert gas is filled into the furnace to a first preset pressure value.

[0071] Step S200 , adding rare earth metal to the iron solution after the temperature is raised to a first preset temperature value, and heating until the alloy is completely melted.

[0072] Step S300: pouring the alloy solution into a mold and cooling it in a furnace under the protection of an inert gas to obtain a rare earth alloy.

[0073] Step S400 , after the rare earth alloy is loaded into a shell, a gas with a second preset pressure value is filled into the shell, and the shell is sealed to obtain the rare earth-containing additive.

[0074] Furthermore, the numerical range of the first preset pressure value is 10000Pa-90000Pa; the numerical range of the second preset pressure value is 0.04-0.3MPa; preferably, the preset pressure value is 0.08-0.12MPa; the numerical range of the first preset temperature value is 1550℃-1800℃.

[0075] The following is a further description of the rare earth-containing additives using several examples:

[0076] Example 1

[0077] Pure iron and rare earth cerium obtained by thermal reduction are prepared at 92% and 8% by mass, respectively. The pure iron raw material is placed in a crucible in a vacuum induction melting furnace, and the rare earth cerium is placed in a trough in the furnace. The furnace is evacuated to below 0.2 Pa, and high-purity argon is introduced to bring the vacuum level to 10,000 Pa. High-purity argon is then added, and when the furnace vacuum is maintained at 10,000 Pa, the temperature is raised to 1,700°C. Once the metal in the crucible is completely melted, rare earth cerium is added to the molten iron through the trough. Once completely melted, the molten alloy is refined for 10 minutes. The alloy solution is poured into a mold and allowed to cool in the furnace under the protection of the argon atmosphere. After analysis, the average size of inclusions in the rare earth alloy is 20μm, the oxygen content is 66ppm, and the carbon content is 200ppm. The rare earth alloy is loaded into a streamlined (L / R=1) pure iron shell with a rare earth alloy filling ratio of 85%, a shell wall thickness of 2.5mm, a maximum (diameter) length of 100mm, and an aspect ratio of 2:1. The air in the shell is evacuated and filled with 0.04MPa Ar, which is then added to the ladle. The rare earth recovery rate in the tested product is 60.1%, the standard deviation of the rare earth composition at the edge, 1 / 4 radius, 1 / 2 radius, and middle of the slab is 4.5ppm, and the average size of inclusions in the steel is 15.1μm.

[0078] Comparative Example 1

[0079] Pure iron and rare earth cerium obtained by thermal reduction are prepared at 92% and 8% by mass, respectively. The pure iron raw material is placed in a crucible in a vacuum induction melting furnace, and the rare earth cerium is placed in a trough in the furnace. The furnace is evacuated to below 0.2 Pa, and high-purity argon is introduced to bring the vacuum level to 10,000 Pa. High-purity argon is then added, and when the furnace vacuum is maintained at 10,000 Pa, the temperature is raised to 1,700°C. Once the metal in the crucible is completely melted, rare earth cerium is added to the molten iron through the trough. Once completely melted, the molten alloy is refined for 10 minutes. The alloy solution is poured into a mold and allowed to cool in the furnace under the protection of the argon atmosphere. After analysis, the average size of inclusions in the rare earth alloy is 50μm, the oxygen content is 200ppm, and the carbon content is 200ppm. The rare earth alloy is loaded into a streamlined (L / R=1) pure iron shell with a rare earth alloy filling ratio of 85%, a shell wall thickness of 2.5mm, a maximum (diameter) length of 100mm, and an aspect ratio of 2:1. The air in the shell is evacuated and filled with 0.04MPa Ar, which is then added to the ladle. The rare earth recovery rate in the tested product is 49.5%, the standard deviation of the rare earth composition at the edge, 1 / 4 radius, 1 / 2 radius, and middle of the slab is 6ppm, and the average size of inclusions in the steel is 30.2μm.

[0080] Example 2

[0081] Pure iron and rare earth lanthanum obtained by molten salt electrolysis are prepared in 10% and 90% mass percentages, respectively. The pure iron raw material is placed in a crucible of a vacuum induction melting furnace, and the rare earth lanthanum is placed in a charge trough of the vacuum induction melting furnace. The furnace is evacuated to below 0.2 Pa, and high-purity argon is introduced to bring the vacuum level to 20,000 Pa. High-purity argon is added, and when the vacuum level in the furnace is maintained at 20,000 Pa, the temperature is raised to 1550°C. Once the metal in the crucible is completely melted, the rare earth lanthanum is added to the molten iron through the charge trough. Once completely melted, the alloy solution is refined for 10 minutes. The alloy solution is poured into a mold and cooled in the furnace under the protection of the argon atmosphere. After analysis, the average size of inclusions in the rare earth alloy is 12.4μm, the oxygen content is 55ppm, and the carbon content is 150ppm. The rare earth alloy is loaded into a streamlined (L / R=2) pure iron shell with a rare earth alloy filling ratio of 75%, a shell wall thickness of 50mm, a maximum (diameter) length of 180mm, and an aspect ratio of 2.5:1. The air in the shell is evacuated and filled with 0.3MPa Ar, which is then added to the ladle. The rare earth recovery rate in the tested product is 55%, the standard deviation of the rare earth composition at the edge, 1 / 4 radius, 1 / 2 radius, and middle of the slab is 4.2ppm, and the average size of inclusions in the steel is 12.4μm.

[0082] Comparative Example 2

[0083] An irregular block of lanthanum-iron alloy with the same composition as that of Comparative Example 2 was prepared, with a maximum (diameter) length of 180 mm, an aspect ratio of 2.5:1, an average size of inclusions in the rare earth alloy of 12.4 μm, an oxygen content of 55 ppm, and a carbon content of 150 ppm. It was added to a ladle, and the rare earth yield in the tested product was 35.1%. The standard deviation of the rare earth composition at the edge, 1 / 4 radius, 1 / 2 radius, and middle of the slab was 15 ppm, and the average size of inclusions in the steel was 14.6 μm.

[0084] Example 3

[0085] Pure iron and rare earth metal yttrium produced using molten salt electrolysis are prepared at 60% and 40% mass percentages, respectively. The pure iron raw material is placed in a crucible in a vacuum induction melting furnace, and the rare earth metal yttrium is placed in a trough in the furnace. The furnace is evacuated to below 0.2 Pa, and high-purity argon is introduced to bring the vacuum level to 30,000 Pa. The furnace is then heated to 1600°C while maintaining a vacuum of 30,000 Pa. Once the metal in the crucible is completely melted, the rare earth metal yttrium is added to the molten iron through the trough. Once completely melted, the alloy solution is then poured into a mold and allowed to cool within the furnace under the protection of the argon atmosphere. After analysis, the average size of inclusions in the rare earth alloy was 25μm, the oxygen content was 56ppm, and the carbon content was 180ppm. The rare earth alloy was loaded into a streamlined (L / R=3) pure iron shell with a rare earth alloy filling ratio of 80%, a shell wall thickness of 10mm, a maximum (diameter) length of 200mm, and an aspect ratio of 3.5:1. The air in the shell was evacuated and filled with 0.1MPa Ar, which was then added to the ladle. The rare earth recovery rate in the tested product was 62.2%, the standard deviation of the rare earth composition at the edge, 1 / 4 radius, 1 / 2 radius, and middle of the slab was 2.3ppm, and the average size of inclusions in the steel was 10.7μm.

[0086] Comparative Example 3

[0087] Pure iron and rare earth metal yttrium produced using molten salt electrolysis are prepared at 60% and 40% mass percentages, respectively. The pure iron raw material is placed in a crucible in a vacuum induction melting furnace, and the rare earth metal yttrium is placed in a trough in the furnace. The furnace is evacuated to below 0.2 Pa, and high-purity argon is introduced to bring the vacuum level to 30,000 Pa. The furnace is then heated to 1600°C while maintaining a vacuum of 30,000 Pa. Once the metal in the crucible is completely melted, the rare earth metal yttrium is added to the molten iron through the trough. Once completely melted, the alloy solution is then poured into a mold and allowed to cool within the furnace under the protection of the argon atmosphere. After analysis, the average size of inclusions in the rare earth alloy is 25μm, the oxygen content is 56ppm, and the carbon content is 180ppm. The rare earth alloy is loaded into a streamlined (L / R=3) pure iron shell with a shell wall thickness of 10mm, a maximum (diameter) length of 200mm, an aspect ratio of 3.5:1, and no gas is filled. The rare earth recovery rate in the tested product is 46.4%, and the standard deviation of the rare earth composition at the edge, 1 / 4 radius, 1 / 2 radius, and middle of the slab is 14.4ppm. The average size of inclusions in the steel is 23.2μm.

[0088] All examples and comparative examples of the present invention are listed in Tables 1 and 2. The effects of adding gaseous rare earth additives to steel are significantly superior to those of conventional solid rare earth additives, as demonstrated by higher rare earth yield and improved uniformity. The average inclusion size and oxygen content of the rare earth additive significantly influence the size of inclusions in the final steel, with rare earth additives with smaller average inclusion size and lower oxygen content resulting in finer inclusions in the final steel. The rare earth-containing additives provided by the present invention offer simple preparation methods, excellent additive effects, and promise large-scale industrial production.

[0089] Table 1

[0090] Table 2

[0091] The embodiment of the present invention aims to protect a rare earth-containing additive, comprising: a sealed housing and a plurality of master alloys disposed within the housing; wherein the master alloys contain rare earth elements, and the housing is filled with a gas at a preset pressure. The above technical solution has the following effects:

[0092] 1. The gas in the additive generates thrust when heated and expands, thereby achieving the goal of uniform dispersion of rare earth metals in the steel. This can effectively solve the problems of unstable rare earth component control, uneven distribution, and low yield in rare earth steel;

[0093] 2. By adopting a streamlined shell with a special shape, it has a smaller resistance coefficient than ordinary rare earth additives on the market, and can achieve a deeper penetration depth in the molten steel, penetrating into the middle and lower part of the ladle, so as to achieve the purpose of uniform mixing of rare earth and molten steel.

[0094] It should be understood that the above-described specific embodiments of the present invention are merely illustrative or illustrative of the principles of the present invention and do not constitute limitations of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included within the scope of protection of the present invention. In addition, the appended claims are intended to cover all variations and modifications that fall within the scope and metes and bounds of the appended claims, or equivalents thereof.

Claims

1. An additive containing rare earth, It is characterized in that include: A sealed shell and a plurality of master alloys disposed inside the shell; wherein the master alloy contains rare earth elements; The shell is filled with gas at a preset pressure.

2. The rare earth-containing additive according to claim 1, It is characterized in that The shell has a shape of a cuboid, a sphere, a cylinder, a truncated cone, a cone, or a streamline.

3. The rare earth-containing additive according to claim 2, It is characterized in that The housing comprises: a front housing and a rear housing; The front shell is integrally connected with the rear shell, and the plurality of master alloys and the gas are located in a closed space between the front shell and the rear shell.

4. The rare earth-containing additive according to claim 3, It is characterized in that The counterweight of the front housing is greater than the counterweight of the rear housing.

5. The rare earth-containing additive according to claim 3, It is characterized in that The streamlined front shell profile satisfies the following mathematical expression obtained by rotating one circle around the x-axis: Wherein, x is the coordinate value of the front shell in the X-axis direction, y is the coordinate value of the Y-axis direction perpendicular to the axial direction of the front shell, the origin of the XY-axis coordinates is at the center point of the interface between the front shell and the rear shell, R is the minor axis radius value of the ellipse where the central axis section of the front shell is located, and L is the major axis radius value of the ellipse where the central axis section of the front shell is located; The length of the front shell along the length direction of the shell is greater than the length of the rear shell along the length direction of the shell, and the maximum diameter B of the rear shell along the Y-axis direction is less than or equal to 2R.

6. The rare earth-containing additive according to claim 1, It is characterized in that The master alloy comprises: rare earth metal and iron; The rare earth metal content is 8wt% to 90wt%, and the iron content is 10wt% to 92wt%; Among them, oxygen content <150ppm, maximum size of inclusions <30μm, total amount of inclusions <0.5 wt%.

7. The rare earth-containing additive according to claim 6, It is characterized in that The intermediate alloy composition is RE-Fe-M, where M is a transition metal, and the transition metal includes at least one of nickel, chromium, tungsten, molybdenum, cobalt, manganese, vanadium, niobium, and titanium; preferably, the transition metal includes at least one of chromium, tungsten, molybdenum, vanadium, niobium, and titanium; In the master alloy, the rare earth metal content is 15wt% to 70wt%, the transition metal content is 0.1wt% to 15wt%, and the iron content is 20wt% to 70wt%; The oxygen content of the rare earth-containing additive is less than 100 ppm, the carbon content is less than 300 ppm, the maximum size of inclusions is less than 25 μm, and the total amount of inclusions is less than 0.1 wt%.

8. The rare earth-containing additive according to claim 6, It is characterized in that The rare earth metal includes at least one of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium; Preferably, the rare earth metal includes at least one of lanthanum, cerium and yttrium.

9. The rare earth-containing additive according to any one of claims 1 to 8, It is characterized in that The material of the shell is iron alloy; The proportion of iron in the ferroalloy is greater than 95wt%; The shell wall thickness has a numerical range of 2.5 mm to 50 mm, and a length / diameter ratio of 1 to 5; Preferably, the shell wall thickness has a value ranging from 5 mm to 30 mm, and a length / diameter ratio of 1 to 3.

10. The rare earth-containing additive according to any one of claims 1 to 8, It is characterized in that The ratio of the sum of the volumes of the plurality of master alloys to the volume of the inner cavity of the housing is greater than or equal to a preset value; Preferably, the preset value is 70%.

11. The rare earth-containing additive according to any one of claims 1 to 8, It is characterized in that The gas includes at least one of argon, nitrogen, helium, neon, krypton, radon, xenon, carbon dioxide and carbon monoxide; Preferably, the gas includes: argon; Furthermore, the oxygen in the gas is ≤10ppm.

12. The rare earth-containing additive according to claim 11, It is characterized in that The preset pressure value of the gas is 0.04-0.3MPa; Preferably, the preset pressure value of the gas is 0.08-0.12 MPa.

13. A method for preparing a rare earth-containing additive, It is characterized in that The method for preparing the rare earth-containing additive according to any one of claims 1 to 12 comprises the following steps: Adding iron to a vacuum induction melting furnace and filling it with inert gas to a first preset pressure value; After the temperature reaches a first preset temperature, rare earth metal is added to the iron solution, and the temperature is heated until the alloy is completely melted; The alloy solution is poured into a mold and cooled in a furnace under the protection of an inert gas to obtain a rare earth alloy; After the rare earth alloy is loaded into the shell, a gas with a second preset pressure value is charged into the shell, and the shell is sealed to obtain the rare earth-containing additive.

14. The method for preparing a rare earth-containing additive according to claim 13, It is characterized in that The numerical range of the first preset pressure value is 10000Pa-90000Pa; The numerical range of the second preset pressure value is 0.04-0.3MPa; preferably, the preset pressure value is 0.08-0.12MPa; The numerical range of the first preset temperature value is 1550°C-1800°C.

Citation Information

Patent Citations

  • Rare earth iron intermediate alloy and application thereof

    CN103820698A

  • Iron-copper-rare earth intermediate alloy and preparation method thereof

    CN115896603A

  • Rare earth-containing additive and preparation method thereof

    CN116574864A

  • Process and apparatus for encapsulated articles

    GB2097022A

  • Formation of bubble casting and additive

    JP1995155930A