Positive electrode active material, positive electrode sheet, secondary battery and electric device

By designing secondary particles with holes and a bimodal particle size distribution in the cathode active material, combined with the combination of different particle sizes, the problem of insufficient mechanical strength of existing materials is solved, and the high volumetric energy density and excellent performance of the battery are achieved. Power performance.

WO2024222369A1PCT designated stage expired Publication Date: 2024-10-31CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/084405
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing cathode active materials have insufficient mechanical strength during use, making it difficult to balance the power performance and mechanical strength of the battery, and cannot meet the application needs of the new generation of electrochemical systems.

Method used

Secondary particles formed by the aggregation of primary particles are used. At least some of the secondary particles have holes. The particle size distribution pattern is measured by laser diffraction method to be bimodal. The difference between the second peak position and the first peak position is 1 μm. ~13μm, combined with cathode active materials of different particle sizes, to form three-dimensional pores to shorten the solid-phase mass transfer path of lithium ions and improve the power performance and mechanical strength of the battery.

Benefits of technology

It improves the volumetric energy density, power performance and mechanical strength of the battery, reduces the risk of breakage of the positive electrode piece, and enhances the shear strength and cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024084405_31102024_PF_FP_ABST
    Figure CN2024084405_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present application are a positive electrode active material, a positive electrode sheet, a secondary battery and an electric device. The positive electrode active material is present in the form of secondary particles that are formed by means of the aggregation of primary particles, wherein at least some of the secondary particles have holes. The particle size distribution diagram of the positive electrode active material determined by means of a laser diffraction method is of a bimodal shape, and the difference between the peak position of a second peak and the peak position of a first peak is 1-13 μm, such that a battery has both good power performance and mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material, positive electrode sheet, secondary battery and electrical device

[0001] Cross-references

[0002] This application refers to Chinese patent application No. 202310473126.X filed on April 27, 2023, entitled “Positive Electrode Active Material, Positive Electrode Sheet, Secondary Battery and Electrical Device,” which is incorporated herein by reference in its entirety. Technical Field

[0003] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode active material, a positive electrode sheet, a secondary battery, and an electrical device. Background Art

[0004] In recent years, secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields.

[0005] The performance of positive electrode active materials directly affects the performance of secondary batteries. Currently, positive electrode active materials have many defects and cannot meet the application requirements of the new generation of electrochemical systems.

[0006] Summary of the Invention

[0007] The present application is made in view of the above-mentioned problems, and its purpose is to provide a positive electrode active material, in which at least part of the secondary particles have pores, and the particle size distribution diagram of the positive electrode active material is bimodal, which can take into account the power performance and mechanical strength of the battery.

[0008] In a first aspect of the present application, a positive electrode active material is provided, wherein the positive electrode active material is in the form of secondary particles formed by aggregation of primary particles, at least some of the secondary particles having pores; and

[0009] The particle size distribution of the positive electrode active material determined by laser diffraction method is bimodal, and the difference between the peak position of the second peak and the peak position of the first peak is 1 μm to 13 μm.

[0010] On the one hand, the presence of pores is conducive to the positive electrode active material having three-dimensional channels, shortening the solid-phase mass transfer path of lithium ions, and improving the power performance and energy density of the battery. On the other hand, the particle size distribution diagram of the positive electrode active material is bimodal, that is, the combination of positive electrode active materials of different particle sizes is not only conducive to improving the tap density of the positive electrode active material, but more importantly, the positive electrode active materials of different particle sizes can play a certain supporting role, which is conducive to improving its mechanical strength, reducing the risk of the positive electrode active material breaking during use, improving the shear strength of the positive electrode sheet, and improving the mechanical strength of the battery. In addition, controlling the difference between the first peak and the second peak in the particle size distribution diagram of the positive electrode active material to 1μm to 13μm is conducive to further improving the compaction density of the positive electrode sheet and the electrical performance of the battery.

[0011] In any embodiment, the first peak is located between 1 μm and 5 μm, and optionally between 1.5 μm and 4.5 μm; and / or

[0012] The second peak is located between 6 μm and 14 μm, and can be optionally between 8 μm and 12 μm.

[0013] The peak position of the first peak and the peak position of the second peak are controlled within a suitable range so that the battery has high volume energy density, excellent power performance and mechanical strength.

[0014] In any embodiment, the secondary particles include a plurality of pores formed by the spaces between the primary particles, and the inner diameter of the pores is 0.1 μm to 0.6 μm, and optionally 0.2 μm to 0.4 μm; or

[0015] The secondary particles include a single hollow hole surrounded by primary particles at the center, and the inner diameter of the hole is 0.5 μm to 3 μm, and can be optionally 0.8 μm to 1.2 μm.

[0016] Pores with different distribution forms have different inner diameters, which are beneficial to the formation of three-dimensional channels in the positive electrode active material, shortening the solid-phase mass transfer path of lithium ions and improving the power performance of the battery.

[0017] In any embodiment, the positive electrode active material has the chemical formula shown below:

[0018] Li a Ni x M1 y M2 1-x-y O2,

[0019] Among them, M1 and M2 include one or more of Co, Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, and Nb, 0.8≤a≤1.2, 0.55≤x≤1.0, 0≤y≤0.45, optionally, 0.8≤a≤1.2, 0.95≤x≤0.995, and 0≤y≤0.05.

[0020] The use of the above materials can ensure that the positive electrode active material has a high gram capacity, so that the battery has a high energy density.

[0021] In any embodiment, the average particle size D of the primary particles of the positive electrode active material is 0.1 μm to 0.8 μm, and optionally 0.2 μm to 0.5 μm.

[0022] The average particle size of the primary particles of the positive electrode active material is controlled within a suitable range, thereby forming secondary particles of the positive electrode active material with a suitable range, so as to enable the battery to have high volume energy density, excellent power performance and mechanical strength.

[0023] In any embodiment, the Dv50 of the secondary particles of the positive electrode active material is 9 μm to 15 μm, and optionally 10 μm to 12 μm.

[0024] The Dv50 of the positive electrode active material is controlled to have a suitable range so that the battery has high volume energy density, excellent power performance and mechanical strength.

[0025] In any embodiment, the specific surface area of ​​the positive electrode active material is 0.1 m 2 / g~1.0m 2 / g, optional 0.2m 2 / g~0.5m 2 / g.

[0026] The specific surface area of ​​the positive electrode active material is controlled within a suitable range so that the battery has high volume energy density, excellent power performance and mechanical strength.

[0027] In any embodiment, the positive electrode active material includes a first positive electrode material and a second positive electrode material.

[0028] The first positive electrode material and the second positive electrode material are used in combination, and there is a synergistic effect between the two, which is beneficial to improving the compaction density of the positive electrode sheet and improving the mechanical properties and cycle performance of the battery.

[0029] In any embodiment, the first cathode material has pores, and the second cathode material is a solid structure; or

[0030] The first positive electrode material is a solid structure, and the second positive electrode material has pores; or

[0031] Both the first positive electrode material and the second positive electrode material have pores.

[0032] The presence of pores can shorten the solid-phase mass transfer path of lithium ions, improve the power performance of the battery, and expose more (010) crystal planes, thereby generating more reaction active sites and improving the material's gram capacity and energy density.

[0033] In any embodiment, the mass ratio A of the first positive electrode material to the second positive electrode material and the porosity B of the positive electrode active material satisfy: 0≤|BA×0.4−(1−A)×0.2|≤1.

[0034] Controlling the mass ratio of the first positive electrode material and the second positive electrode material and the porosity of the positive electrode active material to satisfy the above relationship can not only provide sufficient pores to shorten the solid-phase mass transfer path of lithium ions and improve the power performance of the battery, but also adjust the interaction force between the first positive electrode material and the second positive electrode material to improve the mechanical properties of the battery.

[0035] In any embodiment, the mass ratio A of the first positive electrode material to the second positive electrode material is 1.5-9, and can be optionally 2-8.

[0036] The mass ratio of the first positive electrode material to the second positive electrode material is controlled within an appropriate range, taking into account both the compaction density of the positive electrode sheet and the mechanical strength of the battery.

[0037] In any embodiment, the porosity B of the positive electrode active material is 0.15% to 0.45%, and optionally 0.25% to 0.35%.

[0038] Controlling the porosity of the positive electrode active material within an appropriate range can not only provide sufficient pores to shorten the solid-phase mass transfer path of lithium ions and improve the power performance of the battery, but also avoid or reduce the impact of the presence of pores on the mechanical strength of the positive electrode active material.

[0039] In any embodiment, the first cathode material and the second cathode material each independently have the chemical formula shown below:

[0040] Li a Ni x M1 y M2 1-x-y O2,

[0041] Among them, M1 and M2 include one or more of Co, Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, and Nb, 0.8≤a≤1.2, 0.55≤x≤1.0, 0≤y≤0.45, optionally, 0.8≤a≤1.2, 0.95≤x≤0.995, and 0≤y≤0.05.

[0042] The first positive electrode material and the second positive electrode material having the above chemical formula can both ensure that the positive electrode active material has a high gram capacity, so that the battery has a high energy density.

[0043] In any embodiment, the Dv50 of the first positive electrode material is 8 μm to 18 μm, and can be optionally 10 μm to 12 μm.

[0044] In any embodiment, the Dv50 of the second positive electrode material is 0.8 μm to 5 μm, and can be optionally 1 μm to 3 μm.

[0045] Controlling the Dv50 of the first positive electrode material and the Dv50 of the second positive electrode material to have an appropriate range is beneficial to the synergistic effect between the first positive electrode material and the second positive electrode material, and is beneficial to improving the volume energy density and mechanical properties of the battery.

[0046] In any embodiment, the ratio of the difference between Dv90 and Dv50 of the first positive electrode material to Dv50 of the first positive electrode material satisfies 0.6 to 1.2, and may be 0.8 to 1.0; and / or

[0047] The ratio of the difference between Dv50 and Dv10 of the first positive electrode material to Dv10 of the first positive electrode material satisfies 1.2 to 2.5, and can be optionally 1.5 to 2.0.

[0048] In any embodiment, the ratio of the difference between Dv90 and Dv50 of the second positive electrode material to Dv50 of the second positive electrode material satisfies 0.8 to 1.5, and may be 1.0 to 1.3; and / or

[0049] The ratio of the difference between Dv50 and Dv10 of the second positive electrode material to Dv10 of the second positive electrode material satisfies 6-12, and can be optionally 8-10.

[0050] Controlling the particle size distribution of the first positive electrode material and the second positive electrode material within an appropriate range is beneficial to the synergistic effect between the first positive electrode material and the second positive electrode material, improving the mechanical properties of the battery, and improving the compaction density of the positive electrode sheet.

[0051] A second aspect of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode film layer arranged on at least one surface of the positive electrode collector, and the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.

[0052] In any embodiment, the thickness of the positive electrode film layer is 200 μm to 400 μm, and can be optionally 220 μm to 300 μm.

[0053] Controlling the thickness of the cathode film within an appropriate range can not only provide sufficient cathode active material to increase the battery's energy density, but also reduce the impact on lithium ion solid-phase mass transfer, thus balancing the battery's energy density and power performance.

[0054] In any embodiment, the compaction density of the positive electrode film layer is 2.9 g / m 2 ~3.5g / m 2 .

[0055] The compaction density of the positive electrode film is 2.9g / m 2 ~3.5g / m 2 , which is beneficial to improving the energy density of the battery.

[0056] A third aspect of the present application provides a secondary battery, comprising the positive electrode sheet of the second aspect.

[0057] A fourth aspect of the present application provides an electrical device comprising the secondary battery of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] FIG1 is a particle size distribution diagram of a positive electrode active material according to an embodiment of the present application;

[0059] FIG2 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0060] FIG3 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG2 ;

[0061] FIG4 is a schematic diagram of a battery module according to an embodiment of the present application;

[0062] FIG5 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0063] FIG6 is an exploded view of the battery pack shown in FIG5 according to an embodiment of the present application;

[0064] 7 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application;

[0065] Explanation of reference numerals: 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 housing; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0066] Below, the embodiments of the positive electrode active material, positive electrode sheet, secondary battery and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0067] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0068] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0069] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0070] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0071] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0072] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0073] Currently, ternary materials in the lithium battery field have become one of the most popular secondary battery cathode active materials due to their high theoretical specific capacity, high discharge platform, and low cost. Commonly used ternary materials have a solid structure that restricts the solid-phase mass transfer of metal ions. By preparing ternary materials with a porous structure, the solid-phase mass transfer path of metal ions can be shortened, thereby improving the power performance of the battery. However, ternary materials with a porous structure may be at risk of breakage during use, affecting the battery's electrical performance. Therefore, it is necessary to design a cathode active material that can balance battery power performance and mechanical strength to meet the application needs of the next generation of electrochemical systems.

[0074] [Positive electrode active material]

[0075] Based on this, the present application proposes a positive electrode active material, which exists in the form of secondary particles formed by aggregation of primary particles, and at least some of the secondary particles have pores; and the particle size distribution diagram of the positive electrode active material determined by laser diffraction method is bimodal, and the difference between the peak position of the second peak and the peak position of the first peak is 1μm~13μm.

[0076] Herein, the term "primary particles" refers to particles of the positive electrode active material before agglomeration.

[0077] Herein, the term "pores" refers to a cavity structure existing inside a secondary particle of a positive electrode active material.

[0078] It can be understood that the term "particle size distribution diagram is bimodal" means that the number of particles at the first peak and the second peak in the particle size distribution diagram is significantly greater than the number of particles at other peaks in the particle size distribution diagram, that is, there are a considerable number of particles of two particle sizes in the positive electrode active material.

[0079] In some embodiments, some of the secondary particles have pores.

[0080] In some embodiments, all of the secondary particles have pores.

[0081] In some embodiments, the inner diameter of the hole can be selected as 0.1μm, 0.2μm, 0.4μm, 0.5μm, 0.6μm, 0.8μm, 1μm, 1.2μm, 1.4μm, 1.5μm, 1.6μm, 1.8μm, 2μm, 2.2μm, 2.4μm, 2.5μm, 2.6μm, 2.8μm, 3μm or a value in the range consisting of any two of the above points.

[0082] In some embodiments, the difference between the peak position of the second peak and the peak position of the first peak in the particle size distribution diagram can be selected as 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm or a value in the range consisting of any two of the above points.

[0083] In this article, the particle size distribution diagram is constructed using data measured by laser diffraction. Referring to GB / T 19077-2016, the laser diffraction method for particle size distribution, 0.1g to 0.13g of the positive electrode active material sample to be tested is weighed into a 50mL beaker, 5g of anhydrous ethanol is added, a stirring bar approximately 2.5mm in diameter is placed, and the beaker is sealed with plastic wrap. The sample is ultrasonically treated for 5 minutes, then transferred to a magnetic stirrer and stirred at 500 rpm for at least 20 minutes. Two samples are taken from each batch for testing. Testing is performed using a Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd., UK, to generate a volume-based particle size distribution diagram.

[0084] On the one hand, the presence of pores is conducive to the positive electrode active material having three-dimensional channels, shortening the solid-phase mass transfer path of lithium ions and improving the power performance of the battery. On the other hand, the particle size distribution diagram of the positive electrode active material is bimodal, that is, the combination of positive electrode active materials of different particle sizes is not only conducive to the improvement of the tap density of the positive electrode active material, but more importantly, the positive electrode active materials of different particle sizes can play a certain supporting role, which is conducive to the improvement of its mechanical strength, reducing the risk of the positive electrode active material breaking during use, improving the shear strength of the positive electrode sheet, and improving the mechanical strength of the battery. In addition, controlling the difference between the first peak and the second peak in the particle size distribution diagram of the positive electrode active material to 3μm to 13μm is conducive to further improving the compaction density of the positive electrode sheet and the electrical performance of the battery.

[0085] In some embodiments, the first peak is located between 1 μm and 5 μm. In some embodiments, the first peak is located between 1.5 μm and 4.5 μm. In some embodiments, the first peak is located between 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, or a value in a range consisting of any two of the foregoing values.

[0086] In some embodiments, the second peak is located between 6 μm and 14 μm. In some embodiments, the second peak is located between 8 μm and 12 μm. In some embodiments, the second peak is located between 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, or a range consisting of any two of the foregoing values.

[0087] The peak position of the first peak and the peak position of the second peak are controlled within a suitable range so that the battery has high volume energy density, excellent power performance and mechanical strength.

[0088] In some embodiments, the secondary particles include a plurality of pores formed by the spaces between the primary particles, and the inner diameter of the pores is 0.1 μm to 0.6 μm. In some embodiments, the secondary particles include a plurality of pores formed by the spaces between the primary particles, and the inner diameter of the pores is 0.2 μm to 0.4 μm. In some embodiments, the secondary particles include a plurality of pores formed by the spaces between the primary particles, and the inner diameter of the pores can be 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, or a value in a range consisting of any two of the above points.

[0089] In some embodiments, the secondary particles include a plurality of pores formed by spaces between the primary particles. The plurality of pores are distributed at intervals inside the secondary particles, and in a cross section passing through the center of gravity of the secondary particles, the plurality of pores are distributed in a ring shape.

[0090] In some embodiments, the secondary particles further include pores located within the primary particles, and the inner diameter of the pores is 0.01 μm to 0.06 μm. In some embodiments, the secondary particles further include pores located within the primary particles, and the inner diameter of the pores can be 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, or a value within a range consisting of any two of the foregoing values.

[0091] In some embodiments, the secondary particles include a single hollow hole enclosed by primary particles at the center, and the inner diameter of the hole is 0.5 μm to 3 μm. In some embodiments, the secondary particles include a single hollow hole enclosed by primary particles at the center, and the inner diameter of the hole is 0.8 μm to 1.2 μm. In some embodiments, the secondary particles include a single hollow hole enclosed by primary particles at the center, and the inner diameter of the hole can be 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, or a value within a range consisting of any two of the above points.

[0092] As used herein, the term "inner diameter of a pore" refers to the longest straight-line distance between any two points on the perimeter of a single cavity inside a secondary particle of a positive electrode active material.

[0093] In this article, the inner diameter of the hole can be tested by any means known in the art. As an example, a conductive glue is attached to the sample table, a powdered sample of the positive electrode active material is spread on the conductive glue, the unadhered powder is blown away with an ear bulb, gold is sprayed, and the particles of the powdered sample are cross-sectioned using argon plasma. A scanning electron microscope is used to obtain a scanning electron microscope photo of the powdered sample at an acceleration voltage of 10kV and an emission current of 10mA. The inner diameter of the hole is measured according to the scanning electron microscope photo, at least three samples are measured, and at least 50 holes are measured for each sample. The number average value is taken as the inner diameter of the hole of the sample.

[0094] Pores with different distribution forms have different inner diameters, which are beneficial to the formation of three-dimensional channels in the positive electrode active material, shortening the solid-phase mass transfer path of lithium ions and improving the power performance of the battery.

[0095] In some embodiments, the positive electrode active material has the chemical formula shown below:

[0096] Li a Ni x M1 yM2 1-x-y O2,

[0097] Wherein, M1 and M2 include one or more of Co, Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, and Nb, 0.8≤a≤1.2, 0.55≤x≤1.0, and 0≤y≤0.45. In some embodiments, 0.8≤a≤1.2, 0.95≤x≤0.995, and 0≤y≤0.05.

[0098] The use of the above materials can ensure that the positive electrode active material has a high gram capacity, so that the battery has a high energy density.

[0099] In some embodiments, the average particle size D of the primary particles of the positive electrode active material is 0.1 μm to 0.8 μm. In some embodiments, the average particle size D of the primary particles of the positive electrode active material is 0.2 μm to 0.5 μm. In some embodiments, the average particle size D of the primary particles of the positive electrode active material can be selected from 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, or a value in a range consisting of any two of the above.

[0100] In this document, the average particle size D of the primary particles of the positive electrode active material can be measured using any method known in the art. As an example, after imaging using a scanning electron microscope (ZEISS Sigma-02-33, Germany) at 500x magnification, 200 to 600 primary particles of the positive electrode active material with intact shapes and no obstructions are randomly selected from the electron microscopic image. The longest diameter of each pore in the primary particles in the microscopic image is recorded, and the average of these values ​​is taken as the average particle size D.

[0101] The average particle size of the primary particles of the positive electrode active material is controlled within a suitable range, thereby forming secondary particles of the positive electrode active material with a suitable range, so as to enable the battery to have high volume energy density, excellent power performance and mechanical strength.

[0102] In some embodiments, the Dv50 of the positive electrode active material is 9 μm to 15 μm. In some embodiments, the Dv50 of the positive electrode active material is 10 μm to 12 μm. In some embodiments, the Dv50 of the positive electrode active material can be 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 14.5 μm, 15 μm, or a value in a range consisting of any two of the above.

[0103] In this article, the Dv50 of the positive electrode active material can be tested by any means known in the art. As an example, referring to GB / T 19077-2016 particle size distribution laser diffraction method, 0.1g to 0.13g of the positive electrode active material sample to be tested is weighed in a 50mL beaker, 5g of anhydrous ethanol is added, a stirring bar of about 2.5mm is placed, and the sample is sealed with plastic wrap. After ultrasonic treatment for 5 minutes, the sample is transferred to a magnetic stirrer and stirred at 500 rpm for more than 20 minutes. Two samples are taken from each batch of products for testing. The test is performed using the Mastersizer 2000E laser particle size analyzer of Malvern Instruments Co., Ltd. in the UK. Among them, Dv50 is the particle size corresponding to the cumulative volume distribution percentage of the secondary particles of the positive electrode active material reaching 50%.

[0104] The Dv50 of the positive electrode active material is controlled to have a suitable range so that the battery has high volume energy density, excellent power performance and mechanical strength.

[0105] In some embodiments, the specific surface area of ​​the positive electrode active material is 0.1 m 2 / g~1.0m 2 In some embodiments, the specific surface area of ​​the positive electrode active material is 0.2 m 2 / g~0.5m 2 In some embodiments, the specific surface area of ​​the positive electrode active material is 0.1 m 2 / g, 0.2m 2 / g, 0.3m 2 / g, 0.4m 2 / g, 0.5m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g or a value within the range consisting of any two of the above points.

[0106] In this article, the specific surface area of ​​the positive electrode active material can be measured using any method known in the art. As an example, refer to GB / T 19587-2017 "Determination of the specific surface area of ​​solid substances by gas adsorption BET method". The measurement is performed using a TriStar II 3020 instrument. The positive electrode active material is dispersed in a dispersant (ethanol), ultrasonicated for 30 minutes, and then dried in a vacuum drying oven. Finally, the specific surface area of ​​the positive electrode active material is measured using a specific surface area meter.

[0107] The specific surface area of ​​the positive electrode active material is controlled within a suitable range so that the battery has high volume energy density, excellent power performance and mechanical strength.

[0108] In some embodiments, the positive electrode active material includes a first positive electrode material and a second positive electrode material.

[0109] It can be understood that the first positive electrode material and the second positive electrode material have different sizes. The first positive electrode material and the second positive electrode material are used in combination, and there is a synergistic effect between the two, which is beneficial to improve the compaction density of the positive electrode sheet and improve the mechanical properties and cycle performance of the battery.

[0110] In some embodiments, the first cathode material has pores, and the second cathode material is a solid structure.

[0111] In some embodiments, the first cathode material is a solid structure, and the second cathode material has pores.

[0112] In some embodiments, both the first cathode material and the second cathode material have pores.

[0113] The presence of pores can shorten the solid-phase mass transfer path of lithium ions, improve the power performance of the battery, and expose more (010) crystal planes, thereby generating more reaction active sites and improving the material's gram capacity and energy density.

[0114] In some embodiments, the mass ratio A of the first positive electrode material to the second positive electrode material and the porosity B of the positive electrode active material satisfy the following equation: 0≤|BA×0.4-(1-A)×0.2|≤1. In some embodiments, the mass ratio A of the first positive electrode material to the second positive electrode material and the porosity B of the positive electrode active material 0≤|BA×0.4-(1-A)×0.2|≤1 may satisfy 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, or a value within a range consisting of any two of the foregoing values.

[0115] Herein, the relational expression "|BA×0.4−(1−A)×0.2|" represents the absolute value of the numerical value of BA×0.4−(1−A)×0.2.

[0116] Controlling the mass ratio of the first positive electrode material and the second positive electrode material and the porosity of the positive electrode active material to satisfy the above relationship can not only provide sufficient pores to shorten the solid-phase mass transfer path of lithium ions and improve the power performance of the battery, but also adjust the interaction force between the first positive electrode material and the second positive electrode material to improve the mechanical properties of the battery.

[0117] In some embodiments, the mass ratio A of the first positive electrode material to the second positive electrode material is 1.5 to 9. In some embodiments, the mass ratio A of the first positive electrode material to the second positive electrode material is 2 to 8. In some embodiments, the mass ratio A of the first positive electrode material to the second positive electrode material is 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, or a value in a range consisting of any two of the foregoing.

[0118] The mass ratio of the first positive electrode material to the second positive electrode material is controlled within an appropriate range, taking into account both the compaction density of the positive electrode sheet and the mechanical strength of the battery.

[0119] In some embodiments, the porosity B of the positive electrode active material is 0.15% to 0.45%. In some embodiments, the porosity B of the positive electrode active material is 0.25% to 0.35%. In some embodiments, the porosity B of the positive electrode active material is 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, or a value in a range consisting of any two of the foregoing values.

[0120] Controlling the porosity of the positive electrode active material within an appropriate range can not only provide sufficient pores to shorten the solid-phase mass transfer path of lithium ions and improve the power performance of the battery, but also avoid or reduce the impact of the presence of pores on the mechanical strength of the positive electrode active material.

[0121] In some embodiments, the first cathode material and the second cathode material each independently have the chemical formula shown below:

[0122] Li a Ni x M1 y M2 1-x-y O2,

[0123] Wherein, M1 and M2 include one or more of Co, Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, and Nb, 0.8≤a≤1.2, 0.55≤x≤1.0, and 0≤y≤0.45. In some embodiments, 0.8≤a≤1.2, 0.95≤x≤0.995, and 0≤y≤0.05.

[0124] The first cathode material and the second cathode material having the above chemical formula both have high volume energy density.

[0125] In some embodiments, the Dv50 of the first cathode material is 8 μm to 18 μm. In some embodiments, the Dv50 of the first cathode material is 10 μm to 12 μm. In some embodiments, the Dv50 of the first cathode material is 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, or a value in a range consisting of any two of the foregoing.

[0126] In some embodiments, the Dv50 of the second cathode material is 0.8 μm to 5 μm. In some embodiments, the Dv50 of the second cathode material is 1 μm to 3 μm. In some embodiments, the Dv50 of the second cathode material is 0.8 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, or a value in a range consisting of any two of the foregoing.

[0127] Herein, the testing method of Dv50 of the first positive electrode material and the Dv50 of the second positive electrode material is the same as the testing method of Dv50 of the positive electrode active material.

[0128] Controlling the Dv50 of the first positive electrode material and the Dv50 of the second positive electrode material to have an appropriate range is beneficial to the synergistic effect between the first positive electrode material and the second positive electrode material, and is beneficial to improving the volume energy density and mechanical properties of the battery.

[0129] In some embodiments, the ratio of the difference between Dv90 and Dv50 of the first positive electrode material to the Dv50 of the first positive electrode material is 0.6 to 1.2. In some embodiments, the ratio of the difference between Dv90 and Dv50 of the first positive electrode material to the Dv50 of the first positive electrode material is 0.8 to 1.0. In some embodiments, the ratio of the difference between Dv90 and Dv50 of the first positive electrode material to the Dv50 of the first positive electrode material is 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, or a value within a range consisting of any two of the foregoing values.

[0130] In some embodiments, the ratio of the difference between Dv50 and Dv10 of the first positive electrode material to the Dv10 of the first positive electrode material satisfies 1.2 to 2.5. In some embodiments, the ratio of the difference between Dv50 and Dv10 of the first positive electrode material to the Dv10 of the first positive electrode material satisfies 1.5 to 2.0. In some embodiments, the ratio of the difference between Dv50 and Dv10 of the first positive electrode material to the Dv10 of the first positive electrode material satisfies 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, or a value in a range consisting of any two of the foregoing.

[0131] In some embodiments, the ratio of the difference between Dv90 and Dv50 of the second positive electrode material to the Dv50 of the second positive electrode material is 0.8 to 1.5. In some embodiments, the ratio of the difference between Dv90 and Dv50 of the second positive electrode material to the Dv50 of the second positive electrode material is 1.0 to 1.3. In some embodiments, the ratio of the difference between Dv90 and Dv50 of the second positive electrode material to the Dv50 of the second positive electrode material is 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, or a value within a range consisting of any two of the foregoing values.

[0132] In some embodiments, the ratio of the difference between Dv50 and Dv10 of the second positive electrode material to the Dv10 of the second positive electrode material is 6 to 12. In some embodiments, the ratio of the difference between Dv50 and Dv10 of the second positive electrode material to the Dv10 of the second positive electrode material is 8 to 10. In some embodiments, the ratio of the difference between Dv50 and Dv10 of the second positive electrode material to the Dv10 of the second positive electrode material is 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, or a value in a range consisting of any two of the foregoing.

[0133] In this article, Dv90 is the particle size corresponding to the cumulative volume distribution percentage of secondary particles of the first positive electrode material / the second positive electrode material reaches 90%, and Dv10 is the particle size corresponding to the cumulative volume distribution percentage of secondary particles of the first positive electrode material / the second positive electrode material reaches 10%.

[0134] Controlling the particle size distribution of the first positive electrode material and the second positive electrode material within an appropriate range is beneficial to the synergistic effect between the first positive electrode material and the second positive electrode material, improving the mechanical properties of the battery, and improving the compaction density of the positive electrode sheet.

[0135] [Positive electrode]

[0136] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material in some embodiments.

[0137] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0138] In some embodiments, the surface density of the positive electrode film layer is 24 mg / cm 2 ~46mg / cm 2 In some embodiments, the surface density of the positive electrode film layer can be selected to be 24 mg / cm2 , 25mg / cm 2 , 26mg / cm 2 , 28mg / cm 2 、30mg / cm 2 、32mg / cm 2 、34mg / cm 2 、35mg / cm 2 、36mg / cm 2 、38mg / cm 2 , 40mg / cm 2 , 42mg / cm 2 , 44mg / cm 2 , 45mg / cm 2 , 46mg / cm 2 Or a value within the range formed by any two of the above points.

[0139] The coating density of the positive electrode film layer is obtained by measuring the coating weight (g) of the positive electrode film layer on one side and the coating area (cm 2 Specifically, the coating area density of the positive electrode film layer = the coating weight of the positive electrode film layer on one side (g) / the coating area of ​​the positive electrode film layer (cm 2 ).

[0140] In some embodiments, the thickness of the positive electrode film layer is 200 μm to 400 μm. In some embodiments, the thickness of the positive electrode film layer is 220 μm to 300 μm. In some embodiments, the thickness of the positive electrode film layer can be selected from 200 μm, 220 μm, 240 μm, 250 μm, 260 μm, 280 μm, 300 μm, 320 μm, 340 μm, 350 μm, 360 μm, 380 μm, 400 μm, or a value in a range consisting of any two of the above points.

[0141] Controlling the thickness of the cathode film within an appropriate range can not only provide sufficient cathode active material to increase the battery's energy density, but also reduce the impact on lithium ion solid-phase mass transfer, thus balancing the battery's energy density and power performance.

[0142] In some embodiments, the compaction density of the positive electrode film layer is 2.9 g / m 2 ~3.5g / m 2 In some embodiments, the compaction density of the positive electrode film layer can be selected to be 2.9 g / m 2 3.0g / m 2 , 3.1g / m 2 3.2g / m 2 3.3g / m 2 , 3.4g / m 23.5g / m 2 Or a value within the range formed by any two of the above points.

[0143] In this article, the compaction density of the positive electrode film layer of the positive electrode sheet can be tested by any known test method. As an example, the compaction density of the positive electrode film layer of the positive electrode sheet is measured by measuring the surface density (g / cm 2 ) and the thickness of the positive electrode film on one side (cm) (the number of sampling points is greater than 14). Specifically, the compacted density of the positive electrode film = the surface density of the positive electrode film on one side (g / cm 2 ) / thickness of positive electrode film (cm).

[0144] A positive electrode sheet with a higher positive electrode film compaction density is conducive to improving the volume energy density.

[0145] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0146] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0147] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0148] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0149] [Negative electrode]

[0150] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector.

[0151] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0152] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0153] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0154] In some embodiments, the negative electrode active material includes silicon monoxide.

[0155] In some embodiments, the mass content of silicon oxide is 20% to 100% based on the total mass of the negative electrode active material. In some embodiments, the mass content of silicon oxide is 50% to 100% based on the total mass of the negative electrode active material.

[0156] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0157] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0158] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0159] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0160] [Isolation film]

[0161] In some embodiments, the secondary battery further includes a separator, which can be any known porous separator with good chemical and mechanical stability.

[0162] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different.

[0163] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0164] In some embodiments, a secondary battery includes a negative electrode sheet, a separator, an electrolyte, and in some embodiments, a positive electrode sheet.

[0165] In some embodiments, the secondary battery includes a lithium secondary battery.

[0166] In some embodiments, the energy density of the secondary battery is 700 Wh / L to 900 Wh / L.

[0167] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0168] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0169] The shape of the secondary battery in this application can be cylindrical, square or any other shape. For example, FIG2 shows a secondary battery 5 with a square structure as an example.

[0170] In some embodiments, referring to Figure 3, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0171] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0172] Figure 4 shows an example battery module 4. Referring to Figure 4 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0173] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0174] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0175] Figures 5 and 6 illustrate an example battery pack 1. Referring to Figures 5 and 6 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0176] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0177] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0178] Figure 7 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0179] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0180] Example

[0181] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0182] 1. Preparation method

[0183] Example 1

[0184] 1) Preparation of positive electrode active materials

[0185] Preparation of the first positive electrode material:

[0186] A nickel-cobalt-manganese solution with a molar ratio of nickel, cobalt, and manganese elements of 96:1:3 was prepared, and the concentration was adjusted to 2 mol / L, wherein the raw materials of soluble nickel-cobalt-manganese were nickel sulfate, cobalt sulfate, and manganese sulfate, respectively, and the molar concentration of manganese ions was 0.25 mol / L; a 3 mol / L sodium hydroxide solution was prepared; and a 5.5 mol / L ammonia solution was prepared.

[0187] Under a nitrogen atmosphere, the nickel-cobalt-manganese solution, sodium hydroxide solution, and ammonia solution were simultaneously added to a reactor for a coprecipitation reaction at a controlled speed of 400 rpm, a temperature of 110°C, a reaction time of 8 hours, a pH of 9.5, and an ammonia concentration of 6 mol / L. After the coprecipitation reaction, the reaction materials were transferred to a slurry tank for aging and washing. After dehydration, they were placed in a 115°C oven and dried for 9 hours. After sieving and demagnetization, a precursor with multiple ring-shaped pores was obtained.

[0188] The precursor and lithium hydroxide are uniformly mixed in a certain proportion, wherein the Li / Me molar ratio is 1.03; Me is the total molar content of nickel, cobalt and manganese.

[0189] The uniformly mixed materials are placed in a furnace for calcination with a heating rate of 3°C / min and kept at 720°C for 20 hours in an atmosphere with an oxygen content of ≥98%, and then cooled in the furnace to obtain a matrix material.

[0190] Under a nitrogen atmosphere, the base material, cobalt boride, and titanium boride were mixed in a high-pressure mixer at a mass ratio of 1:0.015:0.0041, and then calcined in a furnace at a temperature of 320°C for 5 hours in a nitrogen atmosphere to obtain a product. The product was washed with water for 30 minutes, centrifuged, filtered, and then vibrated to obtain a first positive electrode material having a plurality of pores formed by the spaces between the primary particles of the first positive electrode material.

[0191] Preparation of the second positive electrode material:

[0192] A nickel-cobalt-manganese solution having a molar ratio of nickel, cobalt, and manganese of 96:1:3 was prepared, and the concentration was adjusted to 2.0 mol / L, wherein the raw materials of soluble nickel-cobalt-manganese were nickel sulfate, cobalt sulfate, and manganese sulfate, respectively; a 2 mol / L sodium hydroxide solution was prepared; and a 6 mol / L ammonia solution was prepared.

[0193] The nickel-cobalt-manganese solution, sodium hydroxide solution, and aqueous ammonia solution were simultaneously added to a reactor for a coprecipitation reaction at a controlled speed of 850 rpm, a temperature of 55°C, and a reaction time of 5 hours. The flow rates of the three solutions were adjusted to 0.6 L / min for the sodium hydroxide solution, 0.6 L / min for the aqueous ammonia solution, and 0.3 L / min for the nickel-cobalt-manganese solution. The pH of the system was controlled at 10.3.

[0194] After the coprecipitation reaction is completed, the precipitate is transferred to a slurry tank for aging and washing, and then dehydrated and placed in an oven at 110° C. for 12 hours. The positive electrode active material precursor is obtained by sieving and demagnetizing.

[0195] The precursor and lithium hydroxide are uniformly mixed in a certain proportion, wherein the Li / Me molar ratio is 1.03; Me is the total molar content of nickel, cobalt and manganese.

[0196] The uniformly mixed materials are placed in a furnace for calcination with a heating rate of 3°C / min and kept at 700°C for 15 hours in an atmosphere with an oxygen content of ≥98%, and then cooled in the furnace to obtain a matrix material.

[0197] Under a nitrogen atmosphere, the base material, cobalt boride, and titanium boride were mixed in a high-pressure mixer at a mass ratio of 1:0.015:0.0041, and then calcined in a furnace at 300°C for 4 hours in a nitrogen atmosphere to obtain a product. The product was washed with water for 30 minutes, centrifuged, filtered, and then vibrated to obtain a second positive electrode material with a solid structure.

[0198] Preparation of positive electrode active material: The first positive electrode material and the second positive electrode material are uniformly mixed in a mass ratio of 6:1 to obtain a positive electrode active material.

[0199] 2) Preparation of positive electrode sheet

[0200] The above-mentioned positive electrode active material, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are added to N-methylpyrrolidone in a mass ratio of 97:1:2, and mixed and stirred for 0.5-6 hours to obtain a positive electrode slurry; then the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil to prepare a positive electrode film layer, which is dried, cold pressed, and cut to obtain a positive electrode sheet.

[0201] 3) Preparation of negative electrode sheet

[0202] Artificial graphite doped with silicon dioxide (SIO), conductive agent carbon black, carbon nanotubes (CNT), binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are added to deionized water in a weight ratio of 94.5:1:0.375:2.8:1.325, where the mass fraction of SIO is 30%, based on the mass of artificial graphite, and mixed and stirred for 5 hours to obtain a negative electrode active material layer slurry; the negative electrode active material layer slurry is evenly coated on the negative electrode current collector copper foil in layers, and then dried, cold pressed, and cut to obtain a negative electrode sheet.

[0203] 4) Electrolyte

[0204] In an argon atmosphere glove box (H2O <0.1ppm, O2 <0.1ppm), the lithium salt LiPF6 / LIFSI was dissolved in an organic solvent of ethylene carbonate / ethyl methyl carbonate / diethyl carbonate / fluoroethylene carbonate (volume ratio of 1:1:1:1) and stirred evenly to obtain an electrolyte with a lithium salt concentration of 1 mol / L.

[0205] 5) Isolation film

[0206] A polypropylene film is used as a base film, and 1 micron aluminum oxide (CCS) + 1 micron polyvinylidene fluoride (PCS) is coated on the base film.

[0207] 6) Preparation of batteries

[0208] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator positioned between the positive and negative electrode sheets to provide isolation. The cells are then wound to obtain a bare cell. The tabs are welded to the bare cell and placed in an aluminum shell. The cells are then baked at 80°C to remove moisture. The electrolyte is then injected and sealed to obtain an uncharged battery. The uncharged battery then undergoes a series of steps, including resting, hot and cold pressing, formation, shaping, and capacity testing, to obtain the lithium battery product of Example 1.

[0209] Examples 2 to 4

[0210] The batteries of Examples 2 to 4 were prepared in a similar manner to that of Example 1, but the preparation method of the positive electrode active material was adjusted to make the inner diameter of the pores of the first positive electrode material different. The specific parameters are shown in Table 1.

[0211] Example 5

[0212] The battery of Example 5 is prepared similarly to the battery of Example 1, except that the preparation method of the first positive electrode material is adjusted so that the first positive electrode material includes a single hollow hole surrounded by primary particles of the first positive electrode active material at the center. The specific preparation method is as follows:

[0213] Prepare a nickel-cobalt-manganese solution with a molar ratio of nickel, cobalt, and manganese of 96:1:3, adjusting the concentration to 1.9 mol / L. The soluble raw materials for nickel, cobalt, and manganese are nickel sulfate, cobalt sulfate, and manganese sulfate, respectively. Prepare a 2 mol / L sodium hydroxide solution and a 6 mol / L ammonia solution. Prepare a carbon sphere dispersion with a mass concentration of 10 g / L, place it in a reactor, and stir at 850 rpm for 120 minutes until uniformly dispersed. Carbon sphere specifications: 0.20 μm diameter.

[0214] The nickel-cobalt-manganese solution, sodium hydroxide solution, and ammonia solution were simultaneously added to a reactor for a coprecipitation reaction at a controlled speed of 850 rpm, a temperature of 55°C, and a reaction time of 5 hours. The flow rates of the three solutions were adjusted to 0.6 L / min for the sodium hydroxide solution, 0.6 L / min for the ammonia solution, and 0.3 L / min for the nickel-cobalt-manganese solution. The pH of the system was controlled at 10.3. The ratio of the weight of the carbon spheres to the total weight of the nickel, cobalt, and manganese in the nickel-cobalt-manganese solution was 2:18.

[0215] After the coprecipitation reaction is completed, the reaction material overflows into the aging kettle, some washing additives are added, and stirred for 1 hour. The material is then dehydrated, washed, dehydrated twice, dried, screened, and demagnetized to obtain a positive electrode active material precursor with a carbon ball as the center.

[0216] The positive electrode active material precursor and lithium carbonate are uniformly mixed in a certain proportion, wherein the Li / Me molar ratio is 1.02; Me is the total molar content of nickel, cobalt and manganese.

[0217] The mixed materials are placed in an oxygen atmosphere furnace, the heating rate is set to 5°C / min, and the temperature is kept at 705°C for 6 hours. The atmosphere is required to have an oxygen content of ≥98%, and then cooled with the furnace.

[0218] The calcined material is subjected to roller crushing, ultracentrifugal grinding, and then sieved through a 400-mesh screen to obtain a first positive electrode material having a hollow single hole surrounded by primary particles of the first positive electrode active material at the center.

[0219] Examples 6 to 31

[0220] The preparation methods of the batteries of Examples 6 to 31 are similar to those of the battery of Example 5, but the preparation method of the positive electrode active material is adjusted. The specific parameters are shown in Table 1.

[0221] Example 32

[0222] The battery of Example 32 is prepared in a similar manner to the battery of Example 5, but the preparation method of the second positive electrode material is adjusted so that the second positive electrode material includes a hollow single hole surrounded by primary particles of the second positive electrode active material at the center position. The specific parameters are shown in Table 1.

[0223] Example 33

[0224] The battery of Example 33 is prepared in a similar manner to the battery of Example 32, but the preparation method of the second positive electrode material is adjusted so that the second positive electrode material includes a plurality of pores formed by the spaces between the primary particles of the second positive electrode material. The specific parameters are shown in Table 1.

[0225] Example 34

[0226] The battery of Example 34 is prepared in a similar manner to the battery of Example 2, but the preparation method of the second positive electrode material is adjusted so that the second positive electrode material includes a hollow single hole surrounded by primary particles of the first positive electrode active material at the center position. The specific parameters are shown in Table 1.

[0227] Example 35

[0228] The battery of Example 35 is prepared in a similar manner to the battery of Example 34, but the preparation method of the second positive electrode material is adjusted so that the second positive electrode material includes a plurality of pores formed by the spaces between the primary particles of the second positive electrode material. The specific parameters are shown in Table 1.

[0229] Example 36

[0230] The preparation method of the battery of Example 36 is similar to that of the battery of Example 32, but the preparation method of the first positive electrode material is adjusted so that the first positive electrode material has a solid structure. The specific parameters are shown in Table 1.

[0231] Example 37

[0232] The preparation method of the battery of Example 37 is similar to that of the battery of Example 33, but the preparation method of the first positive electrode material is adjusted so that the first positive electrode material has a solid structure. The specific parameters are shown in Table 1.

[0233] Comparative Example 1

[0234] The battery of Comparative Example 1 is prepared in a similar manner to the battery of Example 5, but the positive electrode active material only includes the first positive electrode material having a hollow structure and does not include the second positive electrode material. Specific parameters are shown in Table 1.

[0235] Comparative Example 2

[0236] The battery of Comparative Example 2 is prepared in a similar manner to the battery of Example 33, but the positive electrode active material only includes the second positive electrode material having pores arranged in a ring shape, and does not include the first positive electrode material. The specific parameters are shown in Table 1.

[0237] Comparative Example 3

[0238] The battery of Comparative Example 3 is prepared in a similar manner to that of Example 2, but the positive electrode active material only includes the first positive electrode material having pores arranged in a ring shape, and does not include the second positive electrode material. Specific parameters are shown in Table 1.

[0239] Comparative Example 4

[0240] The battery of Comparative Example 4 is prepared in a similar manner to the battery of Example 32, but the positive electrode active material only includes the second positive electrode material having a hollow structure, and does not include the first positive electrode material. The specific parameters are shown in Table 1.

[0241] Comparative Example 5

[0242] The battery of Comparative Example 5 was prepared in a similar manner to the battery of Example 1, but the positive electrode active material included a first positive electrode material and a second positive electrode material both having a solid structure. The specific parameters are shown in Table 1.

[0243] Comparative Example 6

[0244] The preparation method of the battery of Comparative Example 6 is similar to that of the battery of Example 1, but the parameters of the preparation method of the positive electrode active material are adjusted so that the difference between the peak position of the second peak and the peak position of the first peak in the particle size distribution diagram of the positive electrode active material is 15 μm. The specific parameters are shown in Table 1.

[0245] Comparative Example 7

[0246] The battery of Comparative Example 7 is prepared in a similar manner to that of Example 1, but the parameters of the preparation method of the positive electrode active material are adjusted so that the difference between the peak position of the second peak and the peak position of the first peak in the particle size distribution diagram of the positive electrode active material is 2 μm. The specific parameters are shown in Table 1.

[0247] 2. Performance Testing

[0248] 1. Performance test of positive electrode active materials

[0249] 1) Hole inner diameter test

[0250] A conductive adhesive was applied to the sample table. The powdered samples of the positive electrode active materials in each embodiment and comparative example were spread flat on the conductive adhesive. The unadhered powder was blown off with an ear bulb. The powdered samples were sprayed with gold. The particles of the powdered samples were cross-sectioned using argon plasma. A scanning electron microscope (e.g., a ZEISS Sigma 300) was used at an accelerating voltage of 10 kV and an emission current of 10 mA to obtain scanning electron micrographs of the powdered samples. The inner diameter of the pores was measured based on the SEM images. At least three samples were measured, and at least 50 data points were measured for each sample. The number average was taken as the inner diameter of the pores of the sample.

[0251] 2) Difference test between the first peak and the second peak

[0252] With reference to GB / T 19077-2016 / ISO 13320:2009 particle size distribution laser diffraction method, the measurement was performed using the Malvern 3000 device to obtain a particle size distribution diagram based on volume distribution, and the first peak position and the second peak position were measured from the particle size distribution diagram.

[0253] 3) Porosity test

[0254] The porosity of the positive electrode active material can be measured using any method known in the art. For example, the porosity is measured using the gas displacement method according to GB / T 24586. Porosity = (V1 - V2) / V1 * 100%, where V1 is the apparent volume of the sample and V2 is the actual volume of the sample.

[0255] 4) Average particle size D of primary particles

[0256] After imaging with a 500x scanning electron microscope (ZEISS Sigma-02-33, Germany), 200 to 600 primary particles of the positive electrode active material with complete shapes and no obstructions were randomly selected from the electron microscopic image, and the average value of the longest diameter of the primary particles in the microscopic image was recorded as the average particle size D.

[0257] 5) Testing of Dv90, Dv50, and Dv10

[0258] According to the particle size distribution laser diffraction method specified in GB / T 19077-2016, 0.1g to 0.13g of the positive electrode active material / first positive electrode material / second positive electrode material to be tested was weighed into a 50mL beaker. 5g of anhydrous ethanol was added, and a stirring bar (approximately 2.5mm) was placed in the beaker, which was then sealed with plastic wrap. The sample was ultrasonically treated for 5 minutes, then transferred to a magnetic stirrer and stirred at 500 rpm for at least 20 minutes. Two samples were collected from each batch for testing. Testing was performed using a Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd., UK. Dv90 is the particle size at which the cumulative volume distribution percentage of secondary particles of the first positive electrode material / second positive electrode material reaches 90%, Dv50 is the particle size at which the cumulative volume distribution percentage of secondary particles of the positive electrode active material / first positive electrode material / second positive electrode material reaches 50%, and Dv10 is the particle size at which the cumulative volume distribution percentage of secondary particles of the first positive electrode material / second positive electrode material reaches 10%.

[0259] 6) Test method for tap density

[0260] The tap density test of the positive electrode active material refers to GB / T 24533-2009 "Determination of tap density of metal powders" and the equipment used is Dandong Better BT-300 tap density meter for measurement.

[0261] Tap density: The mass per unit volume of powder in a container measured after tapping under specified conditions. The calculation formula is:

[0262] Pt=(m-m0) / V, where:

[0263] Pt----tap density of powder, g / cm 3 ;

[0264] m----total mass of the measuring cylinder and sample, g;

[0265] m0----weight of the measuring cylinder, g;

[0266] V----the tapped volume of the powder, cm 3 .

[0267] 2. Positive electrode performance test

[0268] 1) Compaction density of the positive electrode film

[0269] The compaction density of the positive electrode film layer of the positive electrode sheet is measured by measuring the surface density (g / cm 2 ) and the thickness of the positive electrode film on one side (cm) (the number of sampling points is greater than 14). Specifically, the compacted density of the positive electrode film = the surface density of the positive electrode film on one side (g / cm 2 ) / thickness of positive electrode film (cm).

[0270] 2) Shear strength test

[0271] Cut a double-sided tape of about 60mm in length, stick the double-sided tape along the longitudinal direction of the electrode, and cut the electrode along the edge of the double-sided tape with a blade; select a steel plate with a smooth appearance, polish the surface of the steel plate with sandpaper, wipe the surface of the steel plate with cotton gauze dipped in alcohol, and dry it; stick the double-sided tape on the steel plate, with the distance between the bottom edge of the tape and the bottom edge of the steel plate greater than 1cm, place the steel plate in a 60-80℃ oven for 5 minutes, take out the steel plate, and gently scrape off the release paper on the top layer of the tape with a blade; stick the electrode cut earlier on the double-sided tape of the steel plate with the test surface facing down; use a 2kg pressure roller to roll back and forth 3 times; turn on the power of the Sansi tensile testing machine, the indicator light will light up, adjust the limit block to the appropriate position, fix the end of the steel plate without the electrode with the lower clamp, and clamp the end of the electrode without the steel plate with the upper clamp; then perform the test and read the value, the tensile speed is 10mm / min.

[0272] 3. Battery performance test

[0273] 1) Volume energy density test

[0274] Battery cell capacity test: Allow the battery cell to rest at 25°C for 2 hours, ensuring the cell temperature is 25°C. At 25°C, charge the battery cell at 0.1C to a charge cutoff voltage of 4.25V. Continue constant voltage charging at this charge cutoff voltage until the current reaches 0.05C, at which point charging is terminated (where C represents the rated capacity of the battery cell). Allow the battery cell to rest at 25°C for 1 hour. At 25°C, discharge the battery cell at 0.1C to a discharge cutoff voltage of 2.5V. Record the total discharge capacity (C0) and total discharge energy (E0).

[0275] Battery cell volume measurement: Use a caliper to measure the length, width and height of the battery cell, and multiply the length, width and height of the battery cell to obtain the volume V0 of the battery cell.

[0276] Calculation of volume energy density: Battery cell discharge energy E0 / battery cell volume V0 is the volume energy density of the battery cell.

[0277] 2) Battery 40% SOC discharge time test

[0278] The battery cell was discharged at a constant current of 0.33C to 2.8V and allowed to stand for 30 minutes; charged at a constant current of 0.33C to 4.25V and then at a constant voltage of 0.05C until the voltage stabilized and allowed to stand for 30 minutes; discharged at a constant current of 0.33C to 2.8V, at which time the initial capacity C0 was read and allowed to stand for 30 minutes; charged at a constant current of 0.33C to 4.25V and then at a constant voltage of 0.05C until the voltage stabilized and allowed to stand for 30 minutes; discharged at a constant current of 0.33C to 0.4C0Ah (40%) SOC and allowed to stand for 60 minutes; discharged at a constant current of 4.5C to 2.8V and recorded the discharge time.

[0279] 3) Cyclic performance test

[0280] The secondary batteries prepared in each example and comparative example were charged at a constant current rate of 0.5C to a charge cutoff voltage of 4.25V, then charged at a constant voltage rate to a current of ≤0.05C, allowed to rest for 5 minutes, and then discharged at a constant current rate of 0.33C to a discharge cutoff voltage of 2.5V, allowed to rest for 5 minutes. This constituted one charge-discharge cycle. The batteries were subjected to cyclic charge-discharge testing using this method until the battery capacity decayed to 80%. The number of cycles at this point is the battery's cycle life at 25°C.

[0281] 3. Analysis of test results of various embodiments and comparative examples

[0282] Batteries of various embodiments and comparative examples were prepared according to the above methods, and various performance parameters were measured. The results are shown in Tables 1, 2, and 3 below.

[0283] Table 1

[0284] Table 2

[0285] Table 3

[0286] According to the above table, the positive electrode active materials in Examples 1 to 37 exist in the form of secondary particles formed by aggregation of primary particles, and at least some of the secondary particles have pores; and the particle size distribution diagram of the positive electrode active materials determined by laser diffraction method is bimodal, and the difference between the peak position of the second peak and the peak position of the first peak is 1μm to 13μm.

[0287] From the comparison of Examples 1 to 29, Examples 32 to 37 and Comparative Examples 1 to 4, it can be seen that compared to the positive electrode active material with a single-peak particle size distribution, the positive electrode active material in the present application with a double-peak particle size distribution has a higher shear strength and its battery has a better volume energy density and cycle performance. From the comparison of Examples 1 to 29, Examples 32 to 37 and Comparative Example 5, it can be seen that controlling at least part of the secondary particles to have pores is beneficial to improving the discharge time of the battery and improving the power performance of the battery. From the comparison of Examples 1 to 29, Examples 32 to 37 and Comparative Examples 6 to 7, it can be seen that controlling the difference between the peak position of the second peak and the peak position of the first peak to be 1μm to 13μm is beneficial to improving the compaction density of the positive electrode sheet and the cycle performance of the battery.

[0288] As can be seen from Examples 1 to 4, the secondary particles of the positive electrode active material include multiple pores formed by the spaces between the primary particles. The inner diameter of the pores is controlled to be 0.1 μm to 0.6 μm, resulting in excellent shear strength of the positive electrode sheet and excellent volumetric energy density, discharge time, and cycle performance of the battery. Furthermore, the inner diameter of the pores is controlled to be 0.2 μm to 0.4 μm, which can improve the battery's cycle performance.

[0289] As shown in Examples 5-9, the secondary particles of the positive electrode active material include a single hollow pore surrounded by primary particles at the center. Controlling the inner diameter of the pore to 0.5 μm to 3 μm results in excellent shear strength for the positive electrode sheet and excellent volumetric energy density, discharge time, and cycle performance for the battery. Further controlling the inner diameter of the pore to 0.8 μm to 1.2 μm further improves discharge time.

[0290] As can be seen from Examples 5, 10-13, controlling the Dv50 of the first positive electrode material to 8μm-18μm enables the positive electrode sheet to have excellent shear strength and the battery to have excellent volumetric energy density, discharge time and cycle performance. As can be seen from the comparison of Examples 5, 11-12 with Examples 10 and 13, further controlling the Dv50 of the first positive electrode material to 10μm-12μm balances the shear strength of the positive electrode sheet and the volumetric energy density, discharge time and cycle performance of the battery.

[0291] It can be seen from Examples 5, 14 to 15 that the difference between Dv90 and Dv50 of the first positive electrode material is controlled, and the ratio of Dv50 to the first positive electrode material satisfies 0.6 to 1.2, so that the positive electrode sheet has excellent shear strength and the battery has excellent volume energy density, discharge time and cycle performance.

[0292] It can be seen from Examples 5, 16 to 17 that the difference between Dv50 and Dv10 of the first positive electrode material is controlled, and the ratio of Dv10 to the first positive electrode material satisfies 1.2 to 2.5, so that the positive electrode sheet has excellent shear strength and the battery has excellent volume energy density, discharge time and cycle performance.

[0293] A comparison of Examples 5 and 18 to 21 shows that controlling the Dv50 of the second positive electrode material to 0.8 μm to 5 μm enables the positive electrode sheet to have excellent shear strength, and the battery to have excellent volumetric energy density, discharge time, and cycle performance. A comparison of Examples 5 and 20 with Examples 18 to 19 and 21 shows that further controlling the Dv50 of the second positive electrode material to 1 μm to 3 μm further improves the volumetric energy density and cycle performance of the battery.

[0294] It can be seen from Examples 5, 22 to 23 that the difference between Dv90 and Dv50 of the first positive electrode material is controlled, and the ratio of Dv50 to the first positive electrode material satisfies 0.8 to 1.5, so that the positive electrode sheet has excellent shear strength and the battery has excellent volume energy density, discharge time and cycle performance.

[0295] It can be seen from Examples 5, 24 to 25 that the difference between Dv50 and Dv10 of the first positive electrode material is controlled, and the ratio of Dv10 of the first positive electrode material satisfies 6 to 12, so that the positive electrode sheet has excellent shear strength and the battery has excellent volume energy density, discharge time and cycle performance.

[0296] As can be seen from Examples 5, 26-29, controlling the mass ratio A of the first positive electrode material to the second positive electrode material to be 1.5-9 results in excellent shear strength of the positive electrode sheet and excellent volumetric energy density, discharge time, and cycle performance of the battery. A comparison of Examples 5, 27-28 with Examples 26 and 29 shows that further controlling the mass ratio A of the first positive electrode material to the second positive electrode material to be 2-8 can balance the shear strength of the positive electrode sheet with the volumetric energy density, discharge time, and cycle performance of the battery.

[0297] It can be seen from Examples 5 and 30 to 31 that the thickness of the positive electrode film layer is controlled to be 200 μm to 400 μm, so that the positive electrode sheet has excellent shear strength and the battery has excellent volume energy density, discharge time and cycle performance.

[0298] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A positive electrode active material, characterized in that: The positive electrode active material exists in the form of secondary particles formed by aggregation of primary particles, and at least part of the secondary particles have holes; and The particle size distribution diagram of the positive electrode active material measured by laser diffraction is bimodal, and the difference between the peak position of the second peak and the peak position of the first peak is 1 μm to 13 μm.

2. The positive electrode active material according to claim 1, characterized in that The first peak is located between 1 μm and 5 μm, and may be located between 1.5 μm and 4.5 μm; and / or The second peak is located between 6 μm and 14 μm, and can be optionally between 8 μm and 12 μm.

3. The positive electrode active material according to claim 1 or 2, characterized in that: The secondary particles include a plurality of holes formed by the spaces between the primary particles, and the inner diameter of the holes is 0.1 μm to 0.6 μm, and may be 0.2 μm to 0.4 μm; or The secondary particles include a single hollow hole surrounded by the primary particles at the center, and the inner diameter of the hole is 0.5 μm to 3 μm, and can be 0.8 μm to 1.2 μm.

4. The positive electrode active material according to any one of claims 1 to 3, characterized in that The positive electrode active material has the following chemical formula: Li a Ni x M1 y M2 1-x-y O2, Among them, M1 and M2 include one or more of Co, Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, and Nb, 0.8≤a≤1.2, 0.55≤x≤1.0, 0≤y≤0.45, and optionally, 0.8≤a≤1.2, 0.95≤x≤0.995, and 0≤y≤0.

05.

5. The positive electrode active material according to any one of claims 1 to 4, characterized in that The average particle size D of the primary particles of the positive electrode active material is 0.1 μm to 0.8 μm, and can be 0.2 μm to 0.5 μm.

6. The positive electrode active material according to any one of claims 1 to 5, characterized in that The Dv50 of the secondary particles of the positive electrode active material is 9 μm to 15 μm, and can be optionally 10 μm to 12 μm.

7. The positive electrode active material according to any one of claims 1 to 6, characterized in that The specific surface area of ​​the positive electrode active material is 0.1 m 2 / g~1.0m 2 / g, optional 0.2m 2 / g~0.5m 2 / g.

8. The positive electrode active material according to any one of claims 1 to 7, characterized in that The positive electrode active material includes a first positive electrode material and a second positive electrode material.

9. The positive electrode active material according to claim 8, characterized in that The first positive electrode material has the holes, and the second positive electrode material is a solid structure; or The first positive electrode material is a solid structure, and the second positive electrode material has the holes; or The first positive electrode material and the second positive electrode material both have the pores.

10. The positive electrode active material according to claim 8 or 9, characterized in that: The mass ratio A of the first positive electrode material to the second positive electrode material and the porosity B of the positive electrode active material satisfy the following: 0≤|BA×0.4-(1-A)×0.2|≤1.

11. The positive electrode active material according to any one of claims 8 to 10, characterized in that The mass ratio A of the first positive electrode material to the second positive electrode material is 1.5-9, and can be optionally 2-8.

12. The positive electrode active material according to any one of claims 1 to 11, characterized in that The porosity B of the positive electrode active material is 0.15% to 0.45%, and can be optionally 0.25% to 0.35%.

13. The positive electrode active material according to any one of claims 8 to 12, characterized in that the first positive electrode material and the second positive electrode material each independently have the following chemical formula: Li a Ni x M1 y M2 1-x-y O2, in, M1 and M2 include one or more of Co, Mn, Al, B, Zr, Sr, Y, Sb, W, Ti, Mg, and Nb, 0.8≤a≤1.2, 0.55≤x≤1.0, 0≤y≤0.45, and optionally, 0.8≤a≤1.2, 0.95≤x≤0.995, and 0≤y≤0.

05.

14. The positive electrode active material according to any one of claims 8 to 13, characterized in that The Dv50 of the first positive electrode material is 8 μm to 18 μm, and can be optionally 10 μm to 12 μm.

15. The positive electrode active material according to any one of claims 8 to 14, characterized in that The Dv50 of the second positive electrode material is 0.8 μm to 5 μm, and can be optionally 1 μm to 3 μm.

16. The positive electrode active material according to any one of claims 8 to 15, characterized in that The ratio of the difference between Dv90 and Dv50 of the first positive electrode material to Dv50 of the first positive electrode material satisfies 0.6 to 1.2, and may be 0.8 to 1.0; and / or The ratio of the difference between Dv50 and Dv10 of the first positive electrode material to Dv10 of the first positive electrode material satisfies 1.2 to 2.5, and can be optionally 1.5 to 2.

0.

17. The positive electrode active material according to any one of claims 8 to 16, characterized in that The ratio of the difference between Dv90 and Dv50 of the second positive electrode material to Dv50 of the second positive electrode material satisfies 0.8 to 1.5, and may be 1.0 to 1.3; and / or The ratio of the difference between Dv50 and Dv10 of the second positive electrode material to Dv10 of the second positive electrode material satisfies 6-12, and can be 8-10.

18. A positive electrode plate, characterized in that: The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes the positive electrode active material according to any one of claims 1 to 17.

19. The positive electrode sheet according to claim 18, characterized in that: The thickness of the positive electrode film layer is 200 μm to 400 μm, and can be optionally 220 μm to 300 μm.

20. The positive electrode sheet according to claim 18 or 19, characterized in that: The compaction density of the positive electrode film layer is 2.9 g / m 2 ~3.5g / m 2 .

21. A secondary battery, characterized in that: A positive electrode sheet comprising the positive electrode sheet according to any one of claims 18 to 20.

22. An electrical device, characterized in that: Includes the secondary battery as claimed in claim 21.

Citation Information

Patent Citations

  • Cathode active material for secondary battery, preparation method therefor, and lithium secondary battery comprising same

    CN111492511A

  • Positive electrode material, electrochemical device comprising same, and electronic device

    CN113224271A

  • Electrochemical device and electronic device

    CN113745452A

  • Positive electrode for lithium secondary battery and lithium secondary battery comprising same

    CN115050924A

  • Secondary battery, method for manufacturing the same, and apparatus containing the same

    US20220052321A1